Liquid curable composition, layer of curable composition, method for forming layer of curable composition, and method for fixing semiconductor element

A liquid curable composition with a curable organopolysiloxane compound addresses adhesion issues by ensuring secure and upright fixation of semiconductor elements, enhancing device performance and appearance.

JP2024142048APending Publication Date: 2024-10-10LINTEC CORP
View PDF 6 Cites -1 Cited by

Patent Information

Application Number
JP2023054013
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Semiconductor elements sometimes peel off or are fixed in an inclined manner after being mounted on a coating layer, leading to adhesion issues and improper posture.

Method used

A liquid curable composition containing a curable organopolysiloxane compound with specific tack force and mass reduction rate properties, allowing for proper attachment and fixation of semiconductor elements to a cured material layer.

Benefits of technology

The composition ensures secure attachment and appropriate posture of semiconductor elements, reducing bubble formation and improving adhesiveness, resulting in improved appearance and functionality of light-emitting devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142048000001
    Figure 2024142048000001
  • Figure 2024142048000002
    Figure 2024142048000002
  • Figure 2024142048000003
    Figure 2024142048000003
Patent Text Reader

Abstract

To provide a liquid curable composition which enables a semiconductor element to stick appropriately to a layer of the curable composition and enables the semiconductor element to be fixed in an appropriate position to a cured material layer.SOLUTION: A liquid curable composition comprises a curable organopolysiloxane compound, where a layer having a thickness of 50 μm±7 μm obtained by heating the liquid curable composition at 100°C for 20 minutes has a tack strength of 1000 mN or more, and the layer obtained by heating the liquid curable composition at 100°C for 20 minutes has a mass reduction rate of 13% or less after heating at 150°C for 4 hours.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a liquid curable composition, a layer of the curable composition, a method for forming a layer of the curable composition, and a method for fixing a semiconductor element. [Background technology]

[0002] Liquid curable compositions are improved in various ways depending on the application, and are widely used as raw materials for optical parts and molded bodies, adhesives, coating agents, etc. Patent Document 1 discloses an adhesive sheet having a liquid curable composition. Such an adhesive sheet having a liquid curable composition may be used to fix a semiconductor element.

[0003] Semiconductor elements include optical semiconductor elements such as light-emitting elements such as lasers and light-emitting diodes (LEDs) and light-receiving elements such as solar cells, transistors, sensors such as temperature sensors and pressure sensors, integrated circuits, etc. The semiconductor element may be mounted on a layer of the curable composition (hereinafter sometimes referred to as a "coating layer") formed by applying a liquid curable composition (hereinafter sometimes referred to as a "coating liquid") to a release sheet and drying the applied coating liquid, and then the coating layer is cured, and the semiconductor element may be fixed to the cured layer. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2022-039836 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, after the semiconductor element is mounted on the coating layer, the semiconductor element may peel off, or the semiconductor element may be fixed at an angle to the cured layer.

[0006] An object of the present invention is to provide a liquid curable composition that enables a semiconductor element to be appropriately attached to a layer of the curable composition and enables the semiconductor element to be fixed in an appropriate posture to a cured layer. [Means for solving the problem]

[0007] According to the present invention, A liquid curable composition containing a curable organopolysiloxane compound, The liquid curable composition is heated at 100° C. for 20 minutes to obtain a layer having a thickness of 50 μm±7 μm, which layer has a tack strength of 1000 mN or more, The liquid curable composition is provided, wherein a layer obtained by heating the liquid curable composition at 100° C. for 20 minutes has a mass loss rate of 13% or less after heating at 150° C. for 4 hours. Effect of the Invention

[0008] According to the present invention, it is possible to provide a liquid curable composition that allows a semiconductor element to be appropriately attached to a layer of the curable composition and that allows the semiconductor element to be fixed in an appropriate posture to the cured layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The following embodiments do not limit the invention according to the claims, and not all combinations of features described in the embodiments are essential to the invention. Two or more features among the multiple features described in the embodiments may be arbitrarily combined.

[0010] <Liquid curable composition according to this embodiment> The liquid curable composition according to this embodiment contains a curable organopolysiloxane compound. The liquid curable composition is heated at 100° C. for 20 minutes to obtain a layer having a thickness of 50 μm±7 μm, which has a tack strength (specifically, a probe tack value) of 1000 mN or more. As described above, the liquid curable composition according to this embodiment has excellent adhesion to instantaneous surface contact, so that a semiconductor element can be appropriately or sufficiently attached (i.e., mounted) to the layer of the curable composition.

[0011] Furthermore, the liquid curable composition according to this embodiment is one in which the mass loss rate of the layer obtained by heating the liquid curable composition at 100°C for 20 minutes is 13% or less after heating at 150°C for 4 hours. As described above, the liquid curable composition according to this embodiment is one in which the mass loss is small when the layer of the curable composition obtained by the liquid curable composition is cured, so that there are few bubbles (voids) generated during the mass loss, and the bubbles remaining in the cured layer are reduced or eliminated. Therefore, the semiconductor element can be fixed to the cured layer in an appropriate position, the adhesion between the semiconductor element and the cured layer is improved, and the appearance is also improved. In addition, when a light-emitting element such as an LED chip is fixed by the cured layer, the light-emitting element is not fixed at an angle, so that a light-emitting device with the desired brightness can be obtained.

[0012] A "liquid curable composition" refers to a composition that is a viscous liquid at room temperature and has flowability. Here, room temperature refers to 23°C. A liquid curable composition has the properties of this state, and therefore has excellent workability in the coating process. Here, "excellent workability in the coating process" refers to the absence of repelling (collection of a spreading liquid) and roughness of the coated surface, or the presence of little repelling and roughness of the coated surface.

[0013] (tack strength) The liquid curable composition according to this embodiment is such that a layer having a thickness of 50 μm±7 μm obtained by heating the liquid curable composition at 100° C. for 20 minutes has a tack strength of 1000 mN or more.

[0014] In one embodiment, the tack force can be 1000 mN or more, in another embodiment, 2000 mN or more, in yet another embodiment, 4000 mN or more, and in yet another embodiment, 6000 mN or more, which allows the semiconductor element to be properly or sufficiently attached to the layer of the curable composition obtained from the liquid curable composition.

[0015] On the other hand, the upper limit of the tack force is not particularly limited, but in one embodiment, it can be 15000 mN or less, in another embodiment, it can be 12000 mN or less, in yet another embodiment, it can be 10000 mN or less, and in yet another embodiment, it can be 8000 mN or less. As a result, when the layer of the curable composition obtained by the liquid curable composition is peeled off from the release sheet, the occurrence of linear marks (zipping marks) is suppressed. The range of the tack force can be 1000 mN or more and 15000 mN or less in one embodiment, 2000 mN or more and 12000 mN or less in another embodiment, 4000 mN or more and 10000 mN or less in yet another embodiment, and 6000 mN or more and 8000 mN or less in yet another embodiment. As a result, the semiconductor element can be appropriately or sufficiently attached to the layer of the curable composition obtained by the liquid curable composition, and when the layer of the curable composition is peeled off from the release sheet, the occurrence of linear marks is suppressed.

[0016] The tackiness of the layer obtained by heating and drying the liquid curable composition can be confirmed, for example, as follows. The liquid curable composition is applied to the release surface of a release sheet so that the thickness after drying is 50 μm±7 μm, and heated at 100° C. for 20 minutes to prepare a layer. The prepared layer is placed in a tester for testing by the probe tack method, and the force (probe tack value) when a probe is brought into contact with the layer for a certain period of time at 23° C. and then peeled off is measured, thereby obtaining the tackiness of the layer. A more specific method for measuring the tackiness will be described in the Examples.

[0017] (mass reduction rate) The liquid curable composition according to the present embodiment is one in which a layer (after heat drying) obtained by heating the liquid curable composition at 100°C for 20 minutes has a mass reduction rate (mass reduction rate of the cured layer after curing relative to the layer of the liquid curable composition after heat drying) of 13% or less after heating at 150°C for 4 hours (after curing).

[0018] The mass reduction rate of the cured layer after curing relative to the layer after heating and drying of the liquid curable composition can be 13% or less in one embodiment, 12% or less in another embodiment, 10% or less in yet another embodiment, and 8% or less in yet another embodiment. This reduces or eliminates air bubbles (voids) remaining in the cured layer, allowing the semiconductor element to be fixed to the cured layer in an appropriate position. Furthermore, the adhesion between the semiconductor element and the cured layer is also improved.

[0019] On the other hand, the lower limit of the mass reduction rate of the cured material layer after curing relative to the layer after heat drying of the liquid curable composition is not particularly limited, but in one embodiment, it can be 0.1% or more, in another embodiment, 0.5% or more, in yet another embodiment, 1% or more, and in yet another embodiment, 2% or more. The range of the mass reduction rate of the cured material layer after curing relative to the layer after heat drying of the liquid curable composition can be 13% or less and 0.1% or more, in another embodiment, 12% or less and 0.5% or more, in yet another embodiment, 10% or less and 1% or more, and in yet another embodiment, 8% or less and 2% or more. As a result, the air bubbles (voids) remaining in the cured material layer are reduced or eliminated, the semiconductor element can be fixed to the cured material layer in an appropriate position, and the adhesion between the semiconductor element and the cured material layer is improved.

[0020] The mass reduction rate of the cured layer after curing relative to the layer after heat drying of the liquid curable composition can be confirmed, for example, as follows. The liquid curable composition is applied to a measurement sample pan and placed in a simultaneous differential thermal and thermogravimetric analyzer. After the temperature reaches 100°C, the temperature is maintained for 20 minutes, and the mass of the layer after heat drying is measured. Subsequently, the layer after heat drying is heated, and after the temperature reaches 150°C, the temperature is maintained for 4 hours, and the mass of the cured layer is measured. The mass reduction rate [%] of the cured layer after curing relative to the layer after heat drying of the liquid curable composition is calculated from the mass of the layer after heat drying and the mass of the cured layer by the following formula. Mass reduction rate [%] = {{(mass of layer after heating and drying) - (mass of hardened layer)} / (mass of layer after heating and drying)} × 100

[0021] (viscosity) The liquid curable composition according to one embodiment has a viscosity of 5 Pa·s or more at 23° C. The viscosity of the liquid curable composition can be 5 Pa·s or more in one embodiment, 10 Pa·s or more in another embodiment, 20 Pa·s or more in yet another embodiment, and 30 Pa·s or more in yet another embodiment. This can suppress repelling and allow the liquid curable composition to be uniformly formed on the coating surface.

[0022] On the other hand, the upper limit of the viscosity of the liquid curable composition is not particularly limited, but in one embodiment, it can be less than 65 Pa·s, in another embodiment, less than 60 Pa·s, in yet another embodiment, less than 55 Pa·s, and in yet another embodiment, less than 50 Pa·s. This improves the workability in forming the layer of the curable composition. The range of the viscosity of the liquid curable composition can be 5 Pa·s or more and less than 65 Pa·s in one embodiment, 10 Pa·s or more and less than 60 Pa·s in another embodiment, 20 Pa·s or more and less than 55 Pa·s in yet another embodiment, and 30 Pa·s or more and less than 50 Pa·s in yet another embodiment. This suppresses repelling, allows the liquid curable composition to be uniformly formed on the coating surface, and improves the workability in forming the layer of the curable composition.

[0023] The viscosity of the liquid curable composition can be confirmed, for example, as follows. Using a rheometer, a cone plate with a radius of 50 mm and a cone angle of 0.5° is used, and the viscosity is measured at a shear rate of 2 s at 23° C. -1 At this time, the viscosity is measured.

[0024] (Curable organopolysiloxane compound (A)) The liquid curable composition according to the present embodiment contains a curable organopolysiloxane compound (A) (hereinafter, sometimes referred to as "component (A)"). By containing component (A), the liquid curable composition can more easily achieve the tackiness in the above-mentioned range, and can more easily obtain a layer of the curable composition that gives a cured product with superior adhesion.

[0025] The curable organopolysiloxane compound (A) is a compound having a carbon-silicon bond and a siloxane bond (-Si-O-Si-) in the molecule. The component (A) is a thermosetting compound, and therefore can have at least one functional group selected from the group consisting of functional groups capable of undergoing a condensation reaction by heating and functional groups capable of undergoing a condensation reaction via hydrolysis. Such a functional group can be at least one selected from the group consisting of a hydroxyl group and an alkoxy group, for example, a hydroxyl group or an alkoxy group having 1 to 10 carbon atoms.

[0026] The main chain structure of the curable organopolysiloxane compound (A) is not limited, and may be any of linear, ladder, and cage structures. For example, the linear main chain structure may be the structure represented by the following formula (a-1), the ladder main chain structure may be the structure represented by the following formula (a-2), and the cage main chain structure may be the structure represented by the following formula (a-3).

[0027] [ka]

[0028] [ka]

[0029] [ka]

[0030] In formulas (a-1) to (a-3), Rx, Ry, and Rz each independently represent a hydrogen atom or an organic group, and the organic group can be an unsubstituted or substituted alkyl group, an unsubstituted or substituted cycloalkyl group, an unsubstituted or substituted alkenyl group, an unsubstituted or substituted aryl group, or an alkylsilyl group. The multiple Rx in formula (a-1), the multiple Ry in formula (a-2), and the multiple Rz in formula (a-3) may be the same or different. However, the two Rx in formula (a-1) are not both hydrogen atoms.

[0031] Examples of the alkyl group of the unsubstituted or substituted alkyl group include alkyl groups having 1 to 10 carbon atoms, such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a t-butyl group, an n-pentyl group, an isopentyl group, a neopentyl group, an n-hexyl group, an n-heptyl group, and an n-octyl group.

[0032] Examples of the cycloalkyl group of the unsubstituted or substituted cycloalkyl group include cycloalkyl groups having 3 to 10 carbon atoms, such as a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, and a cycloheptyl group.

[0033] Examples of the alkenyl group of the unsubstituted or substituted alkenyl group include alkenyl groups having 2 to 10 carbon atoms, such as a vinyl group, a 1-propenyl group, a 2-propenyl group, a 1-butenyl group, a 2-butenyl group, and a 3-butenyl group.

[0034] Examples of the substituent on the alkyl group, cycloalkyl group, and alkenyl group include halogen atoms such as a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom; a hydroxyl group; a thiol group; an epoxy group; a glycidoxy group; a (meth)acryloyloxy group; and unsubstituted or substituted aryl groups such as a phenyl group, a 4-methylphenyl group, and a 4-chlorophenyl group.

[0035] Examples of the aryl group of the unsubstituted or substituted aryl group include aryl groups having 6 to 10 carbon atoms, such as a phenyl group, a 1-naphthyl group, and a 2-naphthyl group.

[0036] The lower limit of the number ratio of aryl groups in Rx, Ry, and Rz (organic group) can be 20% or more in one embodiment, 50% or more in another embodiment, 70% or more in yet another embodiment, and 90% or more in yet another embodiment. This makes it easier to obtain a layer of the curable composition that gives a cured product with excellent adhesion, and also makes it easier to obtain a cured product with a high refractive index, and makes it easier to use in devices that require a high refractive index. In addition, the upper limit of the number ratio of aryl groups in the organic group is not particularly limited, but can be 100% or less in one embodiment. The range of the number ratio of aryl groups can be 20% or more and 100% or less in one embodiment, 50% or more and 100% or less in another embodiment, 70% or more and 100% or less in yet another embodiment, and 90% or more and 100% or less in yet another embodiment.

[0037] Examples of the substituent on the aryl group include halogen atoms such as a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom; alkyl groups having 1 to 6 carbon atoms such as a methyl group and an ethyl group; alkoxy groups having 1 to 6 carbon atoms such as a methoxy group and an ethoxy group; a nitro group; a cyano group; a hydroxyl group; a thiol group; an epoxy group; a glycidoxy group; a (meth)acryloyloxy group; and unsubstituted or substituted aryl groups such as a phenyl group, a 4-methylphenyl group, and a 4-chlorophenyl group.

[0038] Examples of the alkylsilyl group include a trimethylsilyl group, a triethylsilyl group, a triisopropylsilyl group, a tri-t-butylsilyl group, a methyldiethylsilyl group, a dimethylsilyl group, a diethylsilyl group, a methylsilyl group, and an ethylsilyl group.

[0039] Among these, Rx, Ry, and Rz can be a hydrogen atom, an unsubstituted or substituted alkyl group having 1 to 6 carbon atoms, or a phenyl group, and an example of such an alkyl group is an unsubstituted or substituted alkyl group having 1 to 6 carbon atoms.

[0040] In addition, Rx, Ry, and Rz can be a fluoro group, which is a substituent having a fluorine atom. Examples of the fluoro group include a fluoroalkyl group, a fluorocycloalkyl group, a fluoroalkenyl group, and a fluoroaryl group. The fluoro group may be a group that has or does not have a hydrogen atom.

[0041] The lower limit of the number ratio of fluoro groups in Rx, Ry, and Rz (organic group) can be 10% or more in one embodiment, 20% or more in another embodiment, 30% or more in yet another embodiment, and 40% or more in yet another embodiment. This makes it easier to obtain a layer of the curable composition that gives a cured product with excellent adhesion, and also makes it easier to obtain a cured product with a low refractive index, and makes it easier to use in devices that require a low refractive index. In addition, the upper limit of the number ratio of fluoro groups in the organic group is not particularly limited, but can be 90% or less in one embodiment, 80% or less in another embodiment, 70% or less in yet another embodiment, and 60% or less in yet another embodiment. This makes it easier to prepare the curable organopolysiloxane compound (A) more stably, and makes it easier to prepare a liquid curable composition with stable performance. The range of the proportion of the number of fluoro groups can be, in one embodiment, 10% or more and 90% or less, in another embodiment, 20% or more and 80% or less, in yet another embodiment, 30% or more and 70% or less, and in yet another embodiment, 40% or more and 60% or less. By using a curable organopolysiloxane compound (A) in which the range of the proportion of the number of fluoro groups is within the above range, it becomes easier to obtain a layer of the curable composition that gives a cured product with excellent adhesiveness.

[0042] In one embodiment, the organic group can be a fluoro group and a methyl group. In one embodiment, the number ratio of the fluoro group can be 10% or more and the methyl group can be 90% or less, in another embodiment, the number ratio of the fluoro group can be 20% or more and the methyl group can be 80% or less, in yet another embodiment, the number ratio of the fluoro group can be 30% or more and the methyl group can be 70% or less, in yet another embodiment, the number ratio of the fluoro group can be 40% or more and the methyl group can be 60% or less, and in yet another embodiment, the number ratio of the fluoro group can be 50% and the methyl group can be 50%.

[0043] The curable organopolysiloxane compound (A) can be obtained by a known production method, for example, by polycondensing a silane compound having a hydrolyzable functional group (alkoxy group, halogen atom, etc.).

[0044] The silane compound to be used may be appropriately selected according to the structure of the desired curable organopolysiloxane compound (A). For example, bifunctional silane compounds such as dimethyldimethoxysilane, dimethyldiethoxysilane, diethyldimethoxysilane, and diethyldiethoxysilane; trifunctional silane compounds such as methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, n-propyltrimethoxysilane, n-butyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, and phenyldiethoxymethoxysilane; tetrafunctional silane compounds such as tetramethoxysilane, tetraethoxysilane, tetra-n-propoxysilane, tetraisopropoxysilane, tetra-n-butoxysilane, tetra-t-butoxysilane, tetra-s-butoxysilane, methoxytriethoxysilane, dimethoxydiethoxysilane, and trimethoxyethoxysilane; and the like.

[0045] The mass average molecular weight (Mw) of the curable organopolysiloxane compound (A) can be 800 or more in one embodiment, 1,000 or more in another embodiment, 1,200 or more in yet another embodiment, and 3,000 or more in one embodiment, 30,000 or less in one embodiment, 20,000 or less in another embodiment, 15,000 or less in yet another embodiment, and 10,000 or less in yet another embodiment. The mass average molecular weight (Mw) of the curable organopolysiloxane compound (A) can be in the range of 800 or more and 30,000 or less in one embodiment, 1,000 or more and 20,000 or less in another embodiment, 1,200 or more and 15,000 or less in yet another embodiment, and 3,000 or more and 10,000 or less in yet another embodiment. By using a curable organopolysiloxane compound (A) having a mass average molecular weight (Mw) within the above range, it becomes easier to adjust the tackiness to the above range, and it becomes easier to obtain a layer of the curable composition that gives a cured product with excellent adhesion.

[0046] The molecular weight distribution (Mw / Mn) of the curable organopolysiloxane compound (A) is not particularly limited, but in one embodiment, it can be 1.0 or more, in another embodiment, it can be 1.1 or more, in one embodiment, it can be 10.0 or less, and in another embodiment, it can be 6.0 or less. In one embodiment, the molecular weight distribution (Mw / Mn) of the curable organopolysiloxane compound (A) can be in the range of 1.0 or more and 10.0 or less, and in another embodiment, it can be 1.1 or more and 6.0 or less. By using the curable organopolysiloxane compound (A) having a molecular weight distribution (Mw / Mn) within the above range, it becomes easier to obtain a layer of the curable composition that gives a cured product with better adhesion.

[0047] The mass average molecular weight (Mw) and number average molecular weight (Mn) of the curable organopolysiloxane compound (A) can be determined, for example, as values ​​converted into standard polystyrene by gel permeation chromatography (GPC) using tetrahydrofuran (THF) as a solvent.

[0048] The content of the curable organopolysiloxane compound (A) is not particularly limited, but the amount can be 40 parts by mass or more, 60 parts by mass or more, and 70 parts by mass or more in one embodiment, less than 98 parts by mass, less than 94 parts by mass, and less than 90 parts by mass in one embodiment, less than 94 parts by mass, and less than 90 parts by mass in another embodiment, relative to 100 parts by mass of the solid content of the liquid curable composition (i.e., the active ingredient). The amount of the (A) component can be in the range of 40 parts by mass or more and less than 98 parts by mass, 60 parts by mass or more and less than 94 parts by mass, and less than 70 parts by mass or more and less than 90 parts by mass in another embodiment, relative to 100 parts by mass of the solid content of the liquid curable composition. By using the (A) component in the above range, the effect of adding the (A) component can be more effectively expressed.

[0049] Polysilsesquioxane Compounds In one embodiment, the curable organopolysiloxane compound (A) can be a polysilsesquioxane compound obtained by polycondensing a trifunctional organosilane compound. By containing a polysilsesquioxane compound as component (A) in the liquid curable composition, the tackiness and the mass reduction rate can be more easily set within the above-mentioned ranges, and a layer of the curable composition that gives a cured product with superior adhesiveness can be easily obtained.

[0050] The polysilsesquioxane compound can be a compound having a repeating unit represented by the following formula (a-4): When the liquid curable composition contains a polysilsesquioxane compound having a repeating unit represented by the following formula (a-4) as component (A), the tackiness and the mass reduction rate are more easily adjusted to the above-mentioned ranges, and a layer of the curable composition that gives a cured product with superior adhesion is more easily obtained.

[0051] [ka]

[0052] In formula (a-4), R 1 represents an organic group. The organic group can be selected from the group consisting of an unsubstituted alkyl group, an alkyl group having a substituent, an unsubstituted cycloalkyl group, a cycloalkyl group having a substituent, an unsubstituted alkenyl group, an alkenyl group having a substituent, an unsubstituted aryl group, an aryl group having a substituent, and an alkylsilyl group, and can be selected from the group consisting of, for example, an unsubstituted alkyl group having 1 to 10 carbon atoms, an alkyl group having 1 to 10 carbon atoms having a substituent, an unsubstituted aryl group having 6 to 12 carbon atoms, and an aryl group having 6 to 12 carbon atoms having a substituent.

[0053] Examples of the "unsubstituted alkyl group having 1 to 10 carbon atoms" include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a s-butyl group, a t-butyl group, an n-pentyl group, an n-hexyl group, an n-octyl group, an n-nonyl group, and an n-decyl group. 1 The number of carbon atoms in the "unsubstituted alkyl group having 1 to 10 carbon atoms" represented by the following formula can be 1 to 6 in one embodiment, and 1 to 3 in another embodiment.

[0054] R 1 The number of carbon atoms in the "alkyl group having 1 to 10 carbon atoms and having a substituent" represented by the formula (I) can be 1 to 6 in one embodiment, and 1 to 3 in another embodiment. Note that this number of carbon atoms refers to the number of carbon atoms in the portion excluding the substituent (the alkyl group portion). Therefore, R 1 is a "substituted alkyl group having 1 to 10 carbon atoms", R 1 The number of carbon atoms may exceed 10. Examples of the alkyl group of the "substituted alkyl group having 1 to 10 carbon atoms" include the same as those listed as the "unsubstituted alkyl group having 1 to 10 carbon atoms".

[0055] Examples of the substituent of the "substituted alkyl group having 1 to 10 carbon atoms" include halogen atoms such as fluorine atom, chlorine atom, and bromine atom; cyano group; and a group represented by the formula OG. The number of atoms (excluding the number of hydrogen atoms) of the substituent of the "substituted alkyl group having 1 to 10 carbon atoms" can be 1 to 30 in one embodiment, and 1 to 20 in another embodiment. Here, G represents a protecting group for a hydroxyl group. The protecting group for a hydroxyl group is not particularly limited, and examples thereof include known protecting groups known as protecting groups for a hydroxyl group. Examples of such groups include acyl groups; silyl groups such as trimethylsilyl group, triethylsilyl group, t-butyldimethylsilyl group, and t-butyldiphenylsilyl group; acetal groups such as methoxymethyl group, methoxyethoxymethyl group, 1-ethoxyethyl group, tetrahydropyran-2-yl group, and tetrahydrofuran-2-yl group; alkoxycarbonyl groups such as t-butoxycarbonyl group; and ether groups such as methyl group, ethyl group, t-butyl group, octyl group, allyl group, triphenylmethyl group, benzyl group, p-methoxybenzyl group, fluorenyl group, trityl group, and benzhydryl group.

[0056] Examples of the "unsubstituted aryl group having 6 to 12 carbon atoms" include a phenyl group, a 1-naphthyl group, and a 2-naphthyl group. 1 The number of carbon atoms in the "unsubstituted aryl group having 6 to 12 carbon atoms" represented by the following formula can be 6.

[0057] R 1 The number of carbon atoms in the "aryl group having 6 to 12 carbon atoms and a substituent" represented by the formula (1) can be 6. Note that this number of carbon atoms refers to the number of carbon atoms in the portion excluding the substituent (the aryl group portion). Therefore, R 1 When R is a "substituted aryl group having 6 to 12 carbon atoms", 1 The number of carbon atoms may exceed 12. Examples of the aryl group in the "substituted aryl group having 6 to 12 carbon atoms" include the same groups as those listed as the "unsubstituted aryl group having 6 to 12 carbon atoms".

[0058] Examples of the substituent of the "substituted aryl group having 6 to 12 carbon atoms" include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, s-butyl, isobutyl, t-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, and isooctyl; halogen atoms such as fluorine, chlorine, and bromine; alkoxy groups such as methoxy and ethoxy. The number of atoms (excluding the number of hydrogen atoms) of the substituent of the "substituted aryl group having 6 to 12 carbon atoms" can be 1 to 30 in one embodiment, and 1 to 20 in another embodiment.

[0059] Among these, R 1 From the viewpoints of facilitating the production of a polysilsesquioxane compound having a stable structure and of providing a liquid curable composition with more stable performance, R may be at least one selected from the group consisting of an unsubstituted alkyl group having 1 to 10 carbon atoms, an alkyl group having 1 to 10 carbon atoms and a fluorine atom, and an unsubstituted aryl group having 6 to 12 carbon atoms. 1 However, by using a polysilsesquioxane compound having an unsubstituted alkyl group having 1 to 10 carbon atoms, it becomes easier to obtain a layer of a curable composition that gives a cured product with excellent adhesiveness.

[0060] Among these, R 1 can be at least one selected from the group consisting of unsubstituted aryl groups having 6 to 12 carbon atoms and substituted aryl groups having 6 to 12 carbon atoms, since this makes it easier to efficiently obtain a curable polysilsesquioxane compound having a high refractive index and makes it easier to use the compound in devices that require a high refractive index. For example, R 1 can be a phenyl group.

[0061] R 1However, by using a polysilsesquioxane compound having an alkyl group (fluoro group) having 1 to 10 carbon atoms and a fluorine atom, the adhesiveness is improved, and a cured product having a low refractive index can be easily obtained from the curable composition layer, which can be easily used in devices requiring a low refractive index. m H (2m-n+1) F n (wherein m is an integer of 1 to 10, and n is an integer of 1 or more and (2m+1) or less). Among these, a 3,3,3-trifluoropropyl group is exemplified.

[0062] In addition, polysilsesquioxane compounds are a type of R 1 (homopolymer), and may have two or more R 1 The copolymer may be one having the above formula (a copolymer).

[0063] R 1 When (organic group) has an alkyl group having 1 to 10 carbon atoms and a fluorine atom (fluoro group), R 1 The lower limit of the proportion of the number of fluoro groups in R can be 10% or more in one embodiment, 20% or more in another embodiment, 30% or more in yet another embodiment, and 40% or more in yet another embodiment. This makes it easier to obtain a layer of the curable composition that has improved adhesiveness and gives a cured product with a low refractive index. 1The upper limit of the number ratio of fluoro groups in the fluoro group is not particularly limited, but in one embodiment, it can be 90% or less, in another embodiment, 80% or less, in yet another embodiment, 70% or less, and in yet another embodiment, 60% or less. This makes it easier to prepare a polysilsesquioxane compound more stably, and easier to prepare a liquid curable composition with stable performance. In one embodiment, the number ratio of fluoro groups can be 10% or more and 90% or less, in another embodiment, 20% or more and 80% or less, in yet another embodiment, 30% or more and 70% or less, and in yet another embodiment, 40% or more and 60% or less. By using a polysilsesquioxane compound having a number ratio of fluoro groups within the above range, it becomes easier to obtain a liquid curable composition with excellent long-term static stability, and it becomes easier to obtain a layer of a curable composition that gives a cured product with improved adhesion and a low refractive index.

[0064] In one embodiment, R 1 can be fluoro groups and methyl groups. In one embodiment, the number ratio of fluoro groups can be 10% or more and methyl groups can be 90% or less, in another embodiment, the number ratio of fluoro groups can be 20% or more and methyl groups can be 80% or less, and in yet another embodiment, the number ratio of fluoro groups can be 30% or more and methyl groups can be 70% or less.

[0065] The content ratio of the repeating unit represented by the formula (a-4) in the polysilsesquioxane compound (i.e., the T site described below) can be 50 mol% or more in one embodiment, 70 mol% or more in another embodiment, and 90 mol% or more in yet another embodiment, based on all repeating units. The content ratio of the repeating unit represented by the formula (a-4) in the polysilsesquioxane compound (i.e., the T site described below) can be 50 to 100 mol% in one embodiment, 70 to 100 mol% in another embodiment, and 90 to 100 mol% in yet another embodiment, based on all repeating units. As an example, the content ratio of the repeating unit represented by the formula (a-4) in the polysilsesquioxane compound (i.e., the T site described below) can be 100 mol%. By using a polysilsesquioxane compound in which the content ratio of the repeating unit represented by the formula (a-4) (T site) is the above ratio, a layer of a curable composition that gives a cured product with excellent light resistance can be easily obtained. The content of the repeating unit (T site) represented by the formula (a-4) in the polysilsesquioxane compound can be calculated, for example, by the following formula when NMR peak assignment and area integration are possible: 29 Si-NMR and 1 It can be determined by measuring H-NMR.

[0066] Polysilsesquioxane compounds are soluble in various organic solvents, such as ketone solvents such as acetone, aromatic hydrocarbon solvents such as benzene, sulfur-containing solvents such as dimethyl sulfoxide, ether solvents such as tetrahydrofuran, ester solvents such as ethyl acetate, halogen-containing solvents such as chloroform, and mixed solvents consisting of two or more of these. Therefore, the polysilsesquioxane compounds in a solution state can be dissolved in these solvents. 29 Si-NMR and 1 H-NMR can be measured.

[0067] The repeating unit represented by the formula (a-4) can be one represented by the following formula (a-5).

[0068] [ka]

[0069] As shown in formula (a-5), polysilsesquioxane compounds have a structure in which three oxygen atoms are bonded to a silicon atom, generally collectively referred to as a T site, and other groups (R 1 ) is bonded to the partial structure.

[0070] In formula (a-5), R 1 is R in the formula (a-4) 1 It has the same meaning as above. * represents a Si atom, a hydrogen atom, or an alkyl group having 1 to 10 carbon atoms, and at least one of the three * is a Si atom. Examples of the alkyl group having 1 to 10 carbon atoms represented by * include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an s-butyl group, an isobutyl group, and a t-butyl group. The multiple *s may be the same or different from each other.

[0071] In addition, the polysilsesquioxane compound is a thermosetting compound, and is a compound that can undergo a condensation reaction and / or hydrolysis by heating. Therefore, at least one of the * in the formula (a-5) of the multiple repeating units (T sites) of the polysilsesquioxane compound can be a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and can be a hydrogen atom as an example.

[0072] In addition, when the polysilsesquioxane compound is soluble in the solvent used for measurement, 29 By measuring Si-NMR, it is possible to confirm the presence of a hydrogen atom or an alkyl group having 1 to 10 carbon atoms at * in the formula (a-5) and whether all three * in the formula (a-5) are repeating units each being a Si atom. 29When the assignment of the Si-NMR peak and the integration of the area are possible, the total number of repeating units in which all three * in the formula (a-5) are Si atoms relative to the total number of repeating units (T sites) represented by the formula (a-4) in the polysilsesquioxane compound can be roughly calculated. The total number of repeating units in which all three * in the formula (a-5) are Si atoms relative to the total number of repeating units (T sites) represented by the formula (a-4) in the polysilsesquioxane compound can be 30 mol% or more in one embodiment, 40 mol% or more in another embodiment, and 95 mol% or less in one embodiment, and 90 mol% or less in another embodiment, from the viewpoint of easily obtaining a layer of a curable composition that gives a cured product with stable productivity and stable performance. The range of the total number of repeating units in which all three * in the formula (a-5) are Si atoms relative to the total number of repeating units (T sites) represented by the formula (a-4) in the polysilsesquioxane compound can be 30 to 95 mol% in one embodiment, and 40 to 90 mol% in another embodiment.

[0073] When the polysilsesquioxane compound is a copolymer, the polysilsesquioxane compound may be any of a random copolymer, a block copolymer, a graft copolymer, an alternating copolymer, etc., but may be a random copolymer from the viewpoint of ease of production, etc. The structure of the polysilsesquioxane compound may be any of a ladder structure, a double-decker structure, a cage structure, a partially cleaved cage structure, a cyclic structure, and a random structure.

[0074] The polysilsesquioxane compound may be solid at room temperature, but may be liquid. The term "liquid" refers to a state having fluidity, for example, a state in which the viscosity is 10,000 Pa·s or less at room temperature, and room temperature refers to 23°C. The liquid polysilsesquioxane compound can reduce the amount of solvent in the liquid curable composition, and can increase the concentration of the polysilsesquioxane compound in the liquid curable composition.

[0075] The polysilsesquioxane compounds can be used alone or in combination of two or more.

[0076] The method for producing the polysilsesquioxane compound is not particularly limited. For example, the polysilsesquioxane compound represented by the following formula (a-6) can be used

[0077] [ka]

[0078] (In the formula, R 1 is R in the formula (a-4) 1 It has the same meaning as R 2 represents an alkyl group having 1 to 10 carbon atoms, and X 1 represents a halogen atom, and p represents an integer of 0 to 3. 2 , and multiple X 1 R may be the same as or different from each other. A polysilsesquioxane compound can be produced by polycondensing at least one of the silane compounds (1) represented by the following formula: 2 Examples of the alkyl group having 1 to 10 carbon atoms in X include the same as those shown as the alkyl group having 1 to 10 carbon atoms in * in the above formula (a-5). 1 Examples of the halogen atom include a chlorine atom and a bromine atom.

[0079] Specific examples of the silane compound (1) include alkyltrialkoxysilane compounds such as methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, and ethyltripoxysilane; and alkylhalogenoalkoxysilane compounds such as methylchlorodimethoxysilane, methylchlorodiethoxysilane, methyldichloromethoxysilane, methylbromodimethoxysilane, ethylchlorodimethoxysilane, ethylchlorodiethoxysilane, ethyldichloromethoxysilane, and ethylbromodimethoxysilane. alkyltrihalogenosilane compounds such as methyltrichlorosilane, methyltribromosilane, ethyltrichlorosilane, and ethyltribromosilane; substituted alkyltrialkoxysilane compounds such as 3,3,3-trifluoropropyltrimethoxysilane, 3,3,3-trifluoropropyltriethoxysilane, 2-cyanoethyltrimethoxysilane, and 2-cyanoethyltriethoxysilane; 3,3,3-trifluoropropylchlorodimethoxysilane, 3,3,3-trifluoropropylchlorodiethoxysilane, and 3,3,3-trifluoropropylchlorodimethoxysilane; Substituted alkyl halide alkoxysilane compounds such as trifluoropropyl dichloromethoxysilane, 3,3,3-trifluoropropyl dichloroethoxysilane, 2-cyanoethyl chlorodimethoxysilane, 2-cyanoethyl chlorodiethoxysilane, 2-cyanoethyl dichloromethoxysilane, and 2-cyanoethyl dichloroethoxysilane; substituted alkyl trihalogenosilane compounds such as 3,3,3-trifluoropropyl trichlorosilane and 2-cyanoethyl trichlorosilane; phenyl trimethoxysilane, 4-methoxyphenyl trimethoxysilane, and 5-methoxyphenyl trimethoxysilane; phenyltrialkoxysilane compounds having or without a substituent, such as phenylchlorodimethoxysilane, phenyldichloromethoxysilane, 4-methoxyphenylchlorodimethoxysilane, 4-methoxyphenyldichloromethoxysilane, etc.; phenyltrihalogenosilane compounds having or without a substituent, such as phenyltrichlorosilane, 4-methoxyphenyltrichlorosilane, etc.; and the like.These silane compounds (1) can be used either individually or in combination of two or more.

[0080] The method of polycondensing the silane compound (1) is not particularly limited. For example, a method of adding a predetermined amount of a polycondensation catalyst to the silane compound (1) in a solvent or without a solvent and stirring at a predetermined temperature can be mentioned. Specifically, (a) a method of adding a predetermined amount of an acid catalyst to the silane compound (1) and stirring at a predetermined temperature, (b) a method of adding a predetermined amount of a base catalyst to the silane compound (1) and stirring at a predetermined temperature, (c) a method of adding a predetermined amount of an acid catalyst to the silane compound (1), stirring at a predetermined temperature, and then adding an excess amount of a base catalyst to make the reaction system basic and stirring at a predetermined temperature can be mentioned. Among these, the polycondensation can be carried out by the method (a) or (c) since the desired polysilsesquioxane compound can be efficiently obtained.

[0081] The polycondensation catalyst used may be either an acid catalyst or a base catalyst. Two or more polycondensation catalysts may be used in combination, and at least an acid catalyst may be used. Examples of the acid catalyst include inorganic acids such as phosphoric acid, hydrochloric acid, boric acid, sulfuric acid, and nitric acid; and organic acids such as citric acid, acetic acid, methanesulfonic acid, trifluoromethanesulfonic acid, benzenesulfonic acid, and p-toluenesulfonic acid. Among these, at least one selected from phosphoric acid, hydrochloric acid, boric acid, sulfuric acid, citric acid, acetic acid, and methanesulfonic acid may be used.

[0082] Examples of the base catalyst include aqueous ammonia; organic bases such as trimethylamine, triethylamine, lithium diisopropylamide, lithium bis(trimethylsilyl)amide, pyridine, 1,8-diazabicyclo[5.4.0]-7-undecene, aniline, picoline, 1,4-diazabicyclo[2.2.2]octane, and imidazole; organic salt hydroxides such as tetramethylammonium hydroxide and tetraethylammonium hydroxide; metal alkoxides such as sodium methoxide, sodium ethoxide, sodium t-butoxide, and potassium t-butoxide; metal hydrides such as sodium hydride and calcium hydride; metal hydroxides such as sodium hydroxide, potassium hydroxide, and calcium hydroxide; metal carbonates such as sodium carbonate, potassium carbonate, and magnesium carbonate; and metal hydrogen carbonates such as sodium hydrogen carbonate and potassium hydrogen carbonate.

[0083] The amount of the polycondensation catalyst used may be 0.05 mol% or more in one embodiment, 0.1 mol% or more in another embodiment, and 10 mol% or less in one embodiment, and 5 mol% or less in another embodiment, based on the total molar amount of the silane compound (1). The amount of the polycondensation catalyst used may be in the range of 0.05 to 10 mol% in one embodiment, and 0.1 to 5 mol% in another embodiment, based on the total molar amount of the silane compound (1).

[0084] When a solvent is used during polycondensation, the solvent to be used can be appropriately selected depending on the type of silane compound (1). For example, water; aromatic hydrocarbons such as benzene, toluene, and xylene; esters such as methyl acetate, ethyl acetate, propyl acetate, butyl acetate, and methyl propionate; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; alcohols such as methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, isobutyl alcohol, s-butyl alcohol, and t-butyl alcohol; and the like. These solvents can be used alone or in combination of two or more. In addition, when the above method (c) is adopted, after polycondensation reaction is carried out in an aqueous system in the presence of an acid catalyst, an organic solvent and a base catalyst (such as aqueous ammonia) may be added to the reaction liquid, and further polycondensation reaction may be carried out under neutral or basic conditions.

[0085] The amount of the solvent used may be 0.001 L or more in one embodiment, 0.01 L or more in another embodiment, and 10 L or less in one embodiment, and 0.9 L or less in another embodiment, per 1 mole of the total amount of the silane compound (1). The amount of the solvent used may be in the range of 0.001 L or more and 10 L or less in one embodiment, and 0.01 L or more and 0.9 L or less in another embodiment, per 1 mole of the total amount of the silane compound (1).

[0086] The temperature when polycondensing the silane compound (1) is usually in the range from 0°C to the boiling point of the solvent used, and in one embodiment, it can be 20°C or higher, in another embodiment, 30°C or higher, in one embodiment, 100°C or lower, and in another embodiment, 95°C or lower. The temperature when polycondensing the silane compound (1) can be in the range of 20°C or higher and 100°C or lower, in one embodiment, 30°C or higher and 95°C or lower. By setting the reaction temperature at or above the lower limit of this reaction temperature, the polycondensation reaction proceeds sufficiently. On the other hand, by setting the reaction temperature at or below the upper limit of this reaction temperature, gelation is suppressed. In addition, the reaction is completed in 30 minutes to 30 hours.

[0087] Depending on the type of monomer used, it may be difficult to increase the molecular weight. For example, R 1 is an alkyl group having a fluorine atom, R 1 In such a case, a polysilsesquioxane compound having a desired molecular weight can be easily obtained by reducing the amount of catalyst and carrying out the reaction for a long period of time under mild conditions.

[0088] After completion of the reaction, neutralization can be carried out by adding an aqueous alkali solution such as sodium bicarbonate to the reaction solution when an acid catalyst was used, or by adding an acid such as hydrochloric acid to the reaction solution when a base catalyst was used, and the salt generated during this process can be removed by filtration or washing with water, etc., to obtain the desired polysilsesquioxane compound.

[0089] When producing a polysilsesquioxane compound by the above method, the OR of the silane compound (1) 2 or X 1 Of these, the portion that has not undergone hydrolysis and the subsequent condensation reaction remains in the polysilsesquioxane compound.

[0090] When the component (A) is, for example, a polysilsesquioxane compound obtained by a polycondensation reaction of a silane compound (1), curing proceeds by a condensation reaction, including the reaction with a silane coupling agent described later. Therefore, the liquid curable composition of this embodiment is different from a general heat-curable silicone adhesive that cures by an addition reaction in the presence of a precious metal catalyst such as a platinum catalyst. Therefore, the liquid curable composition containing a polysilsesquioxane compound does not substantially contain a precious metal catalyst or has a low content of the precious metal catalyst. Here, "substantially does not contain a precious metal catalyst" means "not intentionally adding a component that can be interpreted as a precious metal catalyst, and the content of the precious metal catalyst is, for example, less than 1 mass ppm in terms of the mass of the catalytic metal element with respect to the amount of the active component in the liquid curable composition." Here, the "active component" refers to "a component excluding the solvent (S) (described later) contained in the liquid curable composition." The liquid curable composition may be one that is substantially free of a precious metal catalyst or has a low content of a precious metal catalyst from the viewpoints of stable production taking into consideration formulation variations and the like, long-term static stability, and the fact that precious metal catalysts are expensive.

[0091] The liquid curable composition of the present embodiment contains the curable organopolysiloxane compound (A), and may contain the components described below.

[0092] (Silane coupling agent (B)) The liquid curable composition of the present embodiment may contain a silane coupling agent (B) (hereinafter, sometimes referred to as "(B) component"). By containing the silane coupling agent (B), the viscosity of the liquid curable composition is easily set to the above-mentioned range, and the layer of the curable composition is easily obtained, which is excellent in workability in the coating process, and is excellent in curability due to condensation reaction with the (A) component when heated, and gives a cured product with excellent adhesiveness. Examples of the silane coupling agent (B) include a silane coupling agent (B1) (hereinafter, sometimes referred to as "(B1) component") having a nitrogen atom in the molecule and a silane coupling agent (B2) (hereinafter, sometimes referred to as "(B2) component") having an acid anhydride structure in the molecule. The liquid curable composition may contain the silane coupling agent (B1), or the silane coupling agent (B2), or both the silane coupling agent (B1) and the silane coupling agent (B2).

[0093] Silane coupling agent (B1) By incorporating the silane coupling agent (B1), it becomes easier to obtain a layer of the curable composition that gives a cured product with superior adhesiveness.

[0094] The silane coupling agent (B1) is not particularly limited as long as it is a silane coupling agent having a nitrogen atom in the molecule. For example, a trialkoxysilane compound represented by the following formula (b-1), a dialkoxyalkylsilane compound represented by the following formula (b-2), or a dialkoxyarylsilane compound can be mentioned.

[0095] [ka] JPEG2024142048000008.jpg1266

[0096] In the above formula, R a represents an alkoxy group having 1 to 6 carbon atoms, such as a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, or a t-butoxy group. a R may be the same or different.b represents an alkyl group having 1 to 6 carbon atoms, such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, or a t-butyl group; or an aryl group having or having no substituent, such as a phenyl group, a 4-chlorophenyl group, a 4-methylphenyl group, or a 1-naphthyl group.

[0097] R c represents an organic group having 1 to 10 carbon atoms and a nitrogen atom. c R may further be bonded to another silicon-containing group. c Specific examples of the organic group having 1 to 10 carbon atoms include an N-2-(aminoethyl)-3-aminopropyl group, a 3-aminopropyl group, an N-(1,3-dimethyl-butylidene)aminopropyl group, a 3-ureidopropyl group, and an N-phenyl-aminopropyl group.

[0098] Among the compounds represented by the above formula (b-1) or (b-2), R c In the case where the organic group is bonded to a group containing another silicon atom, examples of the compound include those which are bonded to other silicon atoms via an isocyanurate skeleton to form an isocyanurate-based silane coupling agent, and those which are bonded to other silicon atoms via a urea skeleton to form a urea-based silane coupling agent.

[0099] Among these, the silane coupling agent (B1) can be an isocyanurate-based silane coupling agent or a urea-based silane coupling agent, since it is easy to obtain a layer of the curable composition that gives a cured product with excellent adhesion, and can further be one having four or more alkoxy groups bonded to silicon atoms in the molecule. Having four or more alkoxy groups bonded to silicon atoms means that the total number of alkoxy groups bonded to the same silicon atom and alkoxy groups bonded to different silicon atoms is four or more.

[0100] An example of an isocyanurate-based silane coupling agent having four or more alkoxy groups bonded to a silicon atom is a compound represented by the following formula (b-3), and an example of a urea-based silane coupling agent having four or more alkoxy groups bonded to a silicon atom is a compound represented by the following formula (b-4).

[0101] [ka] JPEG2024142048000010.jpg26131

[0102] In the formula, R a R in the formulas (b-1) and (b-2) a Each of t1 to t5 independently represents an integer of 1 to 10, and can be an integer of 1 to 6, for example, 3.

[0103] Specific examples of the compound represented by formula (b-3) include 1,3,5-N-tris[(tri(C1 to C6)alkoxy)silyl(C1 to C10)alkyl]isocyanurates such as 1,3,5-N-tris(3-trimethoxysilylpropyl)isocyanurate, 1,3,5-N-tris(3-triethoxysilylpropyl)isocyanurate, 1,3,5-N-tris(3-tri-i-propoxysilylpropyl)isocyanurate, and 1,3,5-N-tris(3-tributoxysilylpropyl)isocyanurate;1,3,5-N-tris(3-dimethoxymethylsilylpropyl)isocyanurate, 1,3,5-N-tris(3-dimethoxyethylsilylpropyl)isocyanurate, 1,3,5-N-tris(3-dimethoxyi-propylsilylpropyl)isocyanurate, 1,3,5-N-tris(3-dimethoxyn-propylsilylpropyl)isocyanurate, 1,3,5-N-tris(3-dimethoxyphenylsilylpropyl)isocyanurate, 1,3,5-N-tris(3-diethoxymethylsilylpropyl)isocyanurate 1,3,5-N-tris(3-diethoxyethylsilylpropyl)isocyanurate, 1,3,5-N-tris(3-diethoxy-i-propylsilylpropyl)isocyanurate, 1,3,5-N-tris(3-diethoxy-n-propylsilylpropyl)isocyanurate, 1,3,5-N-tris(3-diethoxyphenylsilylpropyl)isocyanurate, 1,3,5-N-tris(3-di-i-propoxymethylsilylpropyl)isocyanurate , 1,3,5-N-tris(3-di-i-propoxyethylsilylpropyl)isocyanurate, 1,3,5-N-tris(3-di-i-propoxyi-propylsilylpropyl)isocyanurate, 1,3,5-N-tris(3-di-i-propoxyn-propylsilylpropyl)isocyanurate, 1,3,5-N-tris(3-di-i-propoxyphenylsilylpropyl)isocyanurate, 1,3,5-N-tris(3-dibutoxymethylsilylpropyl)isocyanurate, 1,3,5- 1,3,5-N-tris[(di(C1 to C6)alkoxy)silyl(C1 to C10)alkyl]isocyanurates such as N-tris(3-dibutoxyethylsilylpropyl)isocyanurate, 1,3,5-N-tris(3-dibutoxyi-propylsilylpropyl)isocyanurate, 1,3,5-N-tris(3-dibutoxyn-propylsilylpropyl)isocyanurate, and 1,3,5-N-tris(3-dibutoxyphenylsilylpropyl)isocyanurate; and the like.

[0104] Specific examples of the compound represented by formula (b-4) include N,N'-bis[(tri(carbon number 1 to 6)alkoxysilyl)(carbon number 1 to 10)alkyl]ureas such as N,N'-bis(3-trimethoxysilylpropyl)urea, N,N'-bis(3-triethoxysilylpropyl)urea, N,N'-bis(3-tripropoxysilylpropyl)urea, N,N'-bis(3-tributoxysilylpropyl)urea, and N,N'-bis(2-trimethoxysilylethyl)urea; N,N'-bis(3-dimethoxymethylsilylpropyl)urea; N,N'-bis[(di(carbon number 1 to 6)alkoxy(carbon number 1 to 6)alkylsilyl(carbon number 1 to 10)alkyl)ureas such as N,N'-bis(3-dimethoxyethylsilylpropyl)urea and N,N'-bis(3-diethoxymethylsilylpropyl)urea; and N,N'-bis[(di(carbon number 1 to 6)alkoxy(carbon number 6 to 20)arylsilyl(carbon number 1 to 10)alkyl)ureas such as N,N'-bis(3-dimethoxyphenylsilylpropyl)urea and N,N'-bis(3-diethoxyphenylsilylpropyl)urea. The silane coupling agent (B1) can be used alone or in combination of two or more kinds.

[0105] Among these, the silane coupling agent (B1) that can be used is 1,3,5-N-tris(3-trimethoxysilylpropyl)isocyanurate, 1,3,5-N-tris(3-triethoxysilylpropyl)isocyanurate (hereinafter, the two are referred to as "isocyanurate compounds"), N,N'-bis(3-trimethoxysilylpropyl)urea, N,N'-bis(3-triethoxysilylpropyl)urea (hereinafter, the two are referred to as "urea compounds"), or a combination of the above-mentioned isocyanurate compounds and urea compounds.

[0106] When the liquid curable composition contains a silane coupling agent (B1) [(B1) component], the content of the (B1) component is not particularly limited, but the amount can be 2 parts by mass or more in one embodiment, 4 parts by mass or more in another embodiment, 7 parts by mass or more in yet another embodiment, 10 parts by mass or more in yet another embodiment, less than 40 parts by mass in one embodiment, less than 30 parts by mass in another embodiment, less than 25 parts by mass in yet another embodiment, and less than 20 parts by mass in yet another embodiment, relative to 100 parts by mass of the solid content of the liquid curable composition (i.e., active ingredient). The amount of the silane coupling agent (B1) can be in the range of 2 parts by mass or more and less than 40 parts by mass in one embodiment, 4 parts by mass or more and less than 30 parts by mass in another embodiment, 7 parts by mass or more and less than 25 parts by mass in yet another embodiment, and 10 parts by mass or more and less than 20 parts by mass in yet another embodiment, relative to 100 parts by mass of the solid content (i.e., active ingredient) of the liquid curable composition.

[0107] By using the component (B1) in the above range, the effect of adding the component (B1) can be more effectively exhibited, making it easier to obtain a layer of the curable composition that gives a cured product with superior adhesion.

[0108] Silane coupling agent (B2) By incorporating the silane coupling agent (B2), it becomes easier to obtain a layer of the curable composition that gives a cured product with superior adhesiveness.

[0109] Examples of the silane coupling agent (B2) include tri(C1 to C6)alkoxysilyl(C2 to C8)alkyl succinic anhydrides such as 2-(trimethoxysilyl)ethyl succinic anhydride, 2-(triethoxysilyl)ethyl succinic anhydride, 3-(trimethoxysilyl)propyl succinic anhydride, and 3-(triethoxysilyl)propyl succinic anhydride; di(C1 to C6)alkoxymethylsilyl(C2 to C8)alkyl succinic anhydrides such as 2-(dimethoxymethylsilyl)ethyl succinic anhydride; and 2-(methoxydimethylsilyl)ethyl succinic anhydride. Examples of the silane coupling agent (B2) include (C1 to C6) alkoxydimethylsilyl (C2 to C8) alkyl succinic anhydrides such as succinic acid; trihalogenosilyl (C2 to C8) alkyl succinic anhydrides such as 2-(trichlorosilyl)ethyl succinic anhydride and 2-(tribromosilyl)ethyl succinic anhydride; dihalogenomethylsilyl (C2 to C8) alkyl succinic anhydrides such as 2-(dichloromethylsilyl)ethyl succinic anhydride; halogenodimethylsilyl (C2 to C8) alkyl succinic anhydrides such as 2-(chlorodimethylsilyl)ethyl succinic anhydride; and the like. The silane coupling agent (B2) may be used alone or in combination of two or more.

[0110] Among these, the silane coupling agent (B2) may be a tri(C1 to C6)alkoxysilyl(C2 to C8)alkyl succinic anhydride, such as 3-(trimethoxysilyl)propyl succinic anhydride or 3-(triethoxysilyl)propyl succinic anhydride.

[0111] When the liquid curable composition contains a silane coupling agent (B2) [(B2) component], the content of the (B2) component is not particularly limited, but the amount can be 0.1 parts by mass or more in one embodiment, 0.5 parts by mass or more in another embodiment, and 1.5 parts by mass or more in yet another embodiment, and less than 10 parts by mass in one embodiment, less than 6 parts by mass in another embodiment, and less than 4 parts by mass in yet another embodiment, relative to 100 parts by mass of the solid content of the liquid curable composition. The amount of the silane coupling agent (B2) can be in the range of 0.1 parts by mass or more and less than 10 parts by mass in one embodiment, 0.5 parts by mass or more and less than 6 parts by mass in another embodiment, and 1.5 parts by mass or more and less than 4 parts by mass in yet another embodiment, relative to 100 parts by mass of the solid content of the liquid curable composition.

[0112] By using the component (B2) within the above range, the effect of adding the component (B2) can be more effectively exhibited, and the hydrolysis reaction and subsequent condensation reaction of the components (A) and (B) due to the presence of an acid anhydride structure is promoted, making it easier to obtain a layer of the curable composition that gives a cured product with superior adhesion.

[0113] When the liquid curable composition contains the (B) component, the total content of the (B) component is not particularly limited, but the amount can be 2% by mass or more in one embodiment, 3% by mass or more in another embodiment, 4% by mass or more in yet another embodiment, and 15% by mass or more in yet another embodiment, and can be less than 45% by mass in one embodiment, less than 35% by mass in another embodiment, less than 30% by mass in yet another embodiment, and less than 25% by mass in yet another embodiment. The range of the total content of the (B) component can be 2% by mass or more and less than 45% by mass in one embodiment, 3% by mass or more and less than 35% by mass in another embodiment, 4% by mass or more and less than 30% by mass in yet another embodiment, and 15% by mass or more and less than 25% by mass in yet another embodiment, in the solid content of the liquid curable composition. By using the (B) component in this range, the adhesive strength is improved, and a cured product of the layer of the curable composition having a low refractive index is easily obtained, and it is easily used in devices where a low refractive index is required.

[0114] (Silicone Oligomer (C)) The liquid curable composition of this embodiment may contain a silicone oligomer (C) (hereinafter, sometimes referred to as "component (C)") that is liquid at room temperature 23°C as an additional material in addition to components (A) and (B). The silicone oligomer (C) is an oligomer that has a carbon-silicon bond and a siloxane bond (-Si-O-Si-) in the molecule and has an organic group in the side chain. The silicone oligomer (C) is easily mixed with the curable organopolysiloxane compound (A), and can improve the tackiness without lowering the solids concentration of the liquid curable composition.

[0115] There are no limitations on the structure of the silicone oligomer (C), and it can be a compound having repeating units represented by the following formulae (c-1), (c-2), and (c-3).

[0116] [ka]

[0117] [ka]

[0118] [ka]

[0119] In formulas (c-1) to (c-3), R 3 Each of R independently represents an organic group, and the organic group may be an unsubstituted or substituted alkyl group, an unsubstituted or substituted phenyl group, an unsubstituted or substituted cycloalkyl group, or a vinyl group. 4 can be an alkoxy group, an alkoxy-substituted alkoxy group, an acyloxy group, an alkenyloxy group, a ketoxime group, an amino group, an aminooxy group, an amide group, a hydroxy group, and an epoxy group. In the formulas (c-1) to (c-3), n can be an integer of 2 to 50. The silicone oligomer (C) can be linear or branched. In one embodiment, the number ratio of the alkoxy group in the silicone oligomer (C) can be 2 to 50%.

[0120] The viscosity of the silicone oligomer (C) at 23° C. can be, in one embodiment, 100,000 mPa·s or less, in another embodiment, 10,000 mPa·s or less, in yet another embodiment, 1,000 mPa·s or less, and in yet another embodiment, 500 mPa·s or less, or 5 mPa·s or more.

[0121] The molecular weight of the silicone oligomer (C) can be, in one embodiment, 1200 or less, in another embodiment, 1000 or less, in yet another embodiment, 800 or less, and in yet another embodiment, 750 or less and 100 or more, and the silicone oligomer (C) can be a dimer or trimer of the monomer that constitutes the repeating unit.

[0122] The content of the silicone oligomer (C) is not particularly limited, but the amount can be 2 parts by mass or more in one embodiment, 5 parts by mass or more in another embodiment, 10 parts by mass or more in yet another embodiment, and less than 25 parts by mass, less than 20 parts by mass, and less than 15 parts by mass, relative to 100 parts by mass of the solid content (i.e., active ingredient) of the liquid curable composition. The amount of the (C) component can be in the range of 2 parts by mass or more and less than 25 parts by mass, in another embodiment, 5 parts by mass or more and less than 20 parts by mass, and in yet another embodiment, 10 parts by mass or more and less than 15 parts by mass, relative to 100 parts by mass of the solid content of the liquid curable composition. By using the (A) component in the above range, the effect of adding the (C) component can be more effectively expressed.

[0123] (Solvent (S)) The liquid curable composition of the present embodiment may contain a solvent (S). The solvent (S) is not particularly limited as long as it can dissolve or disperse the components of the liquid curable composition. The solvent (S) may contain an organic solvent having a boiling point of 254°C or higher (hereinafter, may be referred to as "organic solvent (SH)"). Here, the "boiling point" refers to the "boiling point at 1013 hPa". The boiling point of the organic solvent (SH) may be 254°C or higher, and may be 254°C or higher and 300°C or lower.

[0124] Specific examples of the organic solvent (SH) include tripropylene glycol-n-butyl ether (boiling point 274°C), 1,6-hexanediol diacrylate (boiling point 260°C), diethylene glycol dibutyl ether (boiling point 256°C), triethylene glycol butyl methyl ether (boiling point 261°C), polyethylene glycol dimethyl ether (boiling point 264 to 294°C), tetraethylene glycol dimethyl ether (boiling point 275°C), and polyethylene glycol monomethyl ether (boiling point 290 to 310°C). Among these, the organic solvent (SH) may be tripropylene glycol-n-butyl ether or 1,6-hexanediol diacrylate, from the viewpoint of easy mixing of the active ingredient. The organic solvent (SH) may be used alone or in combination of two or more.

[0125] The liquid curable composition may contain a solvent other than the organic solvent (SH). The solvent other than the organic solvent (SH) may be a solvent having a boiling point of 70° C. or more and less than 254° C. (hereinafter, this may be referred to as an "organic solvent (SL)"). The organic solvent (SL) is not particularly limited as long as it has a boiling point of 70° C. or more and less than 254° C. and can dissolve or disperse the components of the liquid curable composition. In one embodiment, the organic solvent (SL) may have a boiling point of 70° C. or more and less than 200° C., and in another embodiment, the boiling point may be 70° C. or more and less than 170° C., which further suppresses the generation of bubbles (voids) in the cured layer and allows the semiconductor element to be fixed in an appropriate position by the cured layer.

[0126] Specific examples of the organic solvent (SL) include diethylene glycol monobutyl ether acetate (boiling point 247°C), dipropylene glycol-n-butyl ether (boiling point 229°C), dipropylene glycol methyl ether acetate (boiling point 209°C), diethylene glycol butyl methyl ether (boiling point 212°C), dipropylene glycol-n-propyl ether (boiling point 212°C), tripropylene glycol dimethyl ether (boiling point 215°C), ), triethylene glycol dimethyl ether (boiling point 216°C), diethylene glycol monoethyl ether acetate (boiling point 218°C), diethylene glycol-n-butyl ether (boiling point 230°C), ethylene glycol monophenyl ether (boiling point 245°C), tripropylene glycol methyl ether (boiling point 242°C), propylene glycol phenyl ether (boiling point 243°C), triethylene glycol monomethyl ether (boiling point 249°C), benzyl alcohol (boiling point 204.9°C), phenethyl alcohol (boiling point 219 to 221°C), ethylene glycol Examples of the organic solvent include diethylene glycol monobutyl ether acetate (boiling point 192°C), ethylene glycol monoethyl ether (boiling point 134.8°C), ethylene glycol monomethyl ether (boiling point 124.5°C), propylene glycol monomethyl ether acetate (boiling point 146°C), cyclopentanone (boiling point 130°C), cyclohexanone (boiling point 157°C), cycloheptanone (boiling point 180°C), cyclooctanone (boiling point 195 to 197°C), cyclohexanol (boiling point 161°C), cyclohexadienone (boiling point 104 to 104.5°C), and methyl ethyl ketone (boiling point 80°C). Among these, the organic solvent (SL) may be diethylene glycol monobutyl ether acetate, cyclohexanone, or methyl ethyl ketone, from the viewpoint of easy mixing of the active ingredient.

[0127] The liquid curable composition may contain the solvent (S) in an amount such that the solid content (i.e., active ingredient) concentration is 80% by mass or more in one embodiment, and 85% by mass or more in another embodiment, and may contain the solvent (S) in an amount such that the solid content concentration is less than 95% by mass in one embodiment, and less than 90% by mass in another embodiment. The liquid curable composition may contain the solvent (S) in an amount such that the solid content concentration is in the range of 80% by mass or more and less than 95% by mass in one embodiment, and 85% by mass or more and less than 90% by mass in another embodiment. This makes it easier to adjust the viscosity of the liquid curable composition, and further suppresses the generation of bubbles (voids) in the cured material layer, allowing the semiconductor element to be fixed in an appropriate position by the cured material layer.

[0128] When the solid content concentration is within this range, the active ingredient can be mixed well and the workability in the coating process is excellent. Furthermore, the liquid curable composition can be stored in a container such as a 18 liter can, a pail can, or a drum can, and when the solid content concentration is within this range, the liquid curable composition can be easily filled into the container.

[0129] (Fine particles (D)) The liquid curable composition of the present embodiment may contain fine particles (D). Examples of the fine particles (D) include fine particles (D) having an average primary particle diameter of 0.005 μm or more and 7 μm or less.

[0130] By including the fine particles (D), it becomes easier to obtain a layer of the curable composition that gives a cured product with better adhesion and heat resistance. Since this effect is easier to obtain, the average primary particle size of the fine particles (D) can be 0.005 μm or more in one embodiment, 0.006 μm or more in another embodiment, and 0.007 μm or more in yet another embodiment, and can be 7 μm or less in one embodiment, 2 μm or less in another embodiment, 0.1 μm or less in yet another embodiment, and 0.05 μm or less in yet another embodiment. The average primary particle size of the fine particles (D) can be in the range of 0.005 μm or more and 7 μm or less in one embodiment, 0.006 μm or more and 2 μm or less in another embodiment, 0.007 μm or more and 0.1 μm or less in yet another embodiment, and 0.007 μm or more and 0.05 μm or less in yet another embodiment. The average primary particle size of the fine particles (D) can be determined by observing the shape of the fine particles using a transmission electron microscope.

[0131] In one embodiment, the specific surface area of ​​the fine particles (D) is 0.1 m 2 / g or more, in another embodiment, 0.5 m 2 / g or more, and in yet another embodiment, 1m 2 / g or more, and in yet another embodiment, 50 2 / g or more, and in one embodiment, 500 m 2 / g or less, in another embodiment, 400 m 2 / g or less, and in yet another embodiment, 300 m 2 / g or less, and in yet another embodiment, 220m 2 In one embodiment, the specific surface area of ​​the fine particles (D) can be in the range of 0.1 m 2 / g or more 500m 2 / g or less, in another embodiment, 0.5 m 2 / g or more 400m 2 / g or less, and in yet another embodiment, 1m 2 / g or more 300m 2 / g or less, and in yet another embodiment, 50m 2 / g or more 220m 2 When the specific surface area is within the above range, a liquid curable composition having excellent workability in the coating step can be easily obtained.

[0132] The shape of the fine particles (D) may be any of spherical, chain-like, needle-like, plate-like, flake-like, rod-like, fibrous, etc., and may be spherical. Here, "spherical" means "almost spherical, including true spherical, spheroidal, ovoid, confetti-like, cocoon-like, and other polyhedral shapes that can approximate a sphere."

[0133] The components of the fine particles (D) are not particularly limited, and examples thereof include metals, metal oxides, minerals, metal carbonates, metal sulfates, metal hydroxides, metal silicates, inorganic components, organic components, silicones, etc. The fine particles (D) used may be surface-modified.

[0134] Metal refers to an element belonging to Group 1 (excluding H), Group 2 to 11, Group 12 (excluding Hg), Group 13 (excluding B), Group 14 (excluding C and Si), Group 15 (excluding N, P, As and Sb), or Group 16 (excluding O, S, Se, Te and Po) in the periodic table.

[0135] Examples of metal oxides include titanium oxide, alumina, boehmite, chromium oxide, nickel oxide, copper oxide, zirconium oxide, indium oxide, zinc oxide, and composite oxides thereof. The fine particles of metal oxides also include sol particles made of these metal oxides.

[0136] Examples of the minerals include smectite, bentonite, etc. Examples of the smectite include montmorillonite, beidellite, hectorite, saponite, stevensite, nontronite, and sauconite.

[0137] Examples of metal carbonates include calcium carbonate and magnesium carbonate, examples of metal sulfates include calcium sulfate and barium sulfate, examples of metal hydroxides include aluminum hydroxide, and examples of metal silicates include aluminum silicate, calcium silicate, and magnesium silicate. Examples of inorganic components include silica. Examples of silica include dry silica, wet silica, and surface-modified silica (surface-modified silica). Examples of organic components include acrylic polymers.

[0138] Silicone refers to an artificial polymer compound having a main skeleton formed by siloxane bonds, such as dimethylpolysiloxane, diphenylpolysiloxane, and methylphenylpolysiloxane.

[0139] The fine particles (D) may be used alone or in combination of two or more. Among these, the fine particles (D) may be silica, metal oxides, or minerals, and may be exemplified by silica, since it is easy to obtain a liquid curable composition having excellent transparency.

[0140] Silica can be surface-modified silica because it is relatively easy to mix as a liquid curable composition and because it is easy to obtain a liquid curable composition with excellent workability in the coating process, and it can be surface-modified hydrophobic silica. Examples of hydrophobic surface-modified silica include silica having a trialkylsilyl group having 1 to 20 tricarbons such as a trimethylsilyl group, an alkylsilyl group having 1 to 20 dicarbons such as a dimethylsilyl group, an alkylsilyl group having 1 to 20 carbons such as an octylsilyl group, and the like bonded to the surface; silica having a surface treated with silicone oil; and the like. Hydrophobic surface-modified silica can be obtained, for example, by surface-modifying silica particles with a silane coupling agent having a trialkylsilyl group having 1 to 20 tricarbons, an alkylsilyl group having 1 to 20 dicarbons, an alkylsilyl group having 1 to 20 carbons, or the like, or by treating silica particles with silicone oil.

[0141] When the liquid curable composition contains fine particles (D) [(D) component], the content of the (D) component is not particularly limited, but the amount of the (D) component in the liquid curable composition can be 0.5% by mass or more in one embodiment, 1% by mass or more in another embodiment, 2% by mass or more in another embodiment, less than 30% by mass in one embodiment, less than 20% by mass in another embodiment, and less than 10% by mass in yet another embodiment. The range of the amount of the fine particles (D) in the liquid curable composition can be 0.5% by mass or more and less than 30% by mass in one embodiment, 1% by mass or more and less than 10% by mass in another embodiment, and 2% by mass or more and less than 10% by mass in yet another embodiment. By using the (D) component in the above range, the effect of adding the (D) component can be more effectively expressed.

[0142] (Other ingredients (E)) The liquid curable composition of the present embodiment may contain another component (E). Examples of the component (E) include an antioxidant, an ultraviolet absorber, and a light stabilizer. The antioxidant is added for the purpose of preventing oxidative deterioration during heating. Examples of the antioxidant include a phosphorus-based antioxidant, a phenol-based antioxidant, and a sulfur-based antioxidant.

[0143] Examples of phosphorus-based antioxidants include phosphites, oxaphosphaphenanthrene oxides, etc. Examples of phenol-based antioxidants include monophenols, bisphenols, polymeric phenols, etc. Examples of sulfur-based antioxidants include dilauryl-3,3'-thiodipropionate, dimyristyl-3,3'-thiodipropionate, distearyl-3,3'-thiodipropionate, etc.

[0144] These antioxidants may be used alone or in combination of two or more. The amount of the antioxidant used may be up to 10% by mass based on the component (A).

[0145] The ultraviolet absorber is added for the purpose of improving the light resistance of the resulting liquid curable composition. Examples of the ultraviolet absorber include salicylic acids, benzophenones, benzotriazoles, and hindered amines. These ultraviolet absorbers can be used alone or in combination of two or more. The amount of the ultraviolet absorber used can be 10% by mass or less based on the (A) component.

[0146] The light stabilizer is added for the purpose of improving the light resistance of the resulting liquid curable composition. Examples of the light stabilizer include hindered amines such as poly[{6-(1,1,3,3,-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidine)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidine)imino}]. These light stabilizers can be used alone or in combination of two or more. The total amount of the (E) component used can be 20% by mass or less relative to the (A) component.

[0147] <Layer of Curable Composition According to this Embodiment> The layer of the curable composition according to this embodiment contains a curable organopolysiloxane compound. The layer of the curable composition has a tack strength of 1000 mN or more. The layer of the curable composition according to this embodiment has excellent adhesion, so that a semiconductor element can be appropriately or sufficiently attached (i.e., mounted) to the layer of the curable composition.

[0148] Furthermore, the layer of the curable composition according to this embodiment is a layer of the curable composition having a mass reduction rate of 13% or less after heating at 150°C for 4 hours. In this way, the layer of the curable composition according to this embodiment is such that the mass reduction of the cured layer is small when cured, so that there are few bubbles (voids) generated during mass reduction, and the bubbles remaining in the cured layer are reduced or eliminated. Therefore, the semiconductor element can be fixed to the cured layer in an appropriate position, the adhesion between the semiconductor element and the cured layer is improved, and the appearance is also improved. In addition, when a light-emitting element such as an LED chip is fixed by the cured layer, the light-emitting element is not fixed at an angle, so that a light-emitting device with the desired brightness can be obtained.

[0149] The "layer of the curable composition" refers to a layer of the liquid curable composition before it is completely cured, and is obtained by heating and drying the liquid curable composition. The "layer of the curable composition" is in a state in which it has shape retention at room temperature. Here, room temperature refers to 23°C. The "layer of the curable composition" may be a self-supporting layer or a layer disposed on a release sheet, as long as a semiconductor element can be disposed thereon.

[0150] (tack strength) The layer of the curable composition according to this embodiment is a layer of the curable composition having a tack strength of 1000 mN or more. The range of the tack strength and the method for confirming the tack strength can be the same as those exemplified in the section <Liquid curable composition according to this embodiment>.

[0151] (mass reduction rate) The layer of the curable composition according to this embodiment is a layer of the curable composition having a mass loss rate of 13% or less after heating (curing) for 4 hours at 150° C. The range of the mass loss rate of the cured layer after curing relative to the layer of the liquid curable composition after heating and drying, and the method for confirming the mass loss rate, etc., can be the same range and confirmation method as those exemplified in the section <Liquid curable composition according to this embodiment>.

[0152] (Curable organopolysiloxane compound (A)) The layer of the curable composition according to this embodiment contains a curable organopolysiloxane compound (A). In one embodiment, the curable organopolysiloxane compound is a polysilsesquioxane compound. The structure and functional group of the curable organopolysiloxane compound (A) can be the same structure and functional group as those exemplified in the section <Liquid curable composition according to this embodiment>.

[0153] (Components (B) to (E), and (S)) The layer of the curable composition according to this embodiment contains a silane coupling agent (B), a silicone oligomer (C), fine particles (D), and other components (E). The structure, functional group, content, physical properties, etc. of the silane coupling agent (B), the silicone oligomer (C), the fine particles (D), and other components (E) can be the same as those exemplified in the section <Liquid curable composition according to this embodiment>.

[0154] (Component (S)) The layer of the curable composition according to this embodiment may contain a solvent (S). The compound of the solvent (S) may be the same compound as that exemplified in the section <Liquid curable composition according to this embodiment>. However, since the layer of the curable composition is a liquid curable composition that has been heated and dried, a part of the solvent (S) contained in the liquid curable composition has volatilized, and the amount of the solvent (S) contained in the layer of the curable composition is less than the amount of the solvent (S) contained in the liquid curable composition.

[0155] The layer of the curable composition may contain an amount of solvent (S) such that the solid content (i.e., active ingredient) concentration is, in one embodiment, 90% by mass or more, in another embodiment, 93% by mass or more, and in yet another embodiment, 95% by mass or more, and in one embodiment, less than 100% by mass, in another embodiment, less than 99.5% by mass, and in yet another embodiment, less than 99% by mass. The layer of the curable composition may contain an amount of solvent (S) such that the solid content concentration is, in one embodiment, 90% by mass or more and less than 100% by mass, in another embodiment, 93% by mass or more and less than 99.5% by mass, and in yet another embodiment, 95% by mass or more and less than 99% by mass. This suppresses the generation of bubbles (voids) in the cured layer, and the semiconductor element can be fixed to the cured layer in an appropriate position.

[0156] (Thickness of the layer of the curable composition) The thickness of the layer of the curable composition according to this embodiment is not particularly limited, and can be determined according to the semiconductor element to be bonded and the use of the semiconductor element, etc., as long as the semiconductor element can be arranged. The thickness of the layer of the curable composition can be 1 μm or more in one embodiment, 5 μm or more in another embodiment, 10 μm or more in yet another embodiment, 30 μm or more in yet another embodiment, 40 μm or more in yet another embodiment, and can be 100 μm or less in one embodiment, 80 μm or less in another embodiment, and 60 μm or less in yet another embodiment. The range of the thickness of the layer of the curable composition can be 50 μm ± 7 μm in one embodiment. The thickness of the layer of the curable composition can also be determined from the thickness after the layer of the curable composition has been cured.

[0157] <Method for producing the liquid curable composition according to this embodiment> The liquid curable composition of the present embodiment can be produced, for example, by a production method including the following steps (AI) and (AII).

[0158] (Process (AI)) The step (AI) is a step of polycondensing at least one compound represented by the above formula (a-6) in the presence of a polycondensation catalyst to obtain a polysilsesquioxane compound.

[0159] (Process (AII)) The step (AII) is a step of obtaining a liquid curable composition by using the polysilsesquioxane compound obtained in the step (AI).

[0160] Examples of the method for obtaining a polysilsesquioxane compound by polycondensing at least one of the compounds represented by the above formula (a-6) in the presence of a polycondensation catalyst in step (AI) include the same methods as those exemplified in the section <Liquid curable composition according to the present embodiment>.

[0161] In step (AII), the method of obtaining a liquid curable composition using a polysilsesquioxane compound includes, for example, a method of mixing the polysilsesquioxane compound, and optionally the (B), (C), and (D) components with a solvent (S), degassing, and dissolving. The mixing method and degassing method are not particularly limited, and known methods can be used. The order of mixing is not particularly limited. According to the production method having the above steps (AI) and (AII), the liquid curable composition of the present embodiment can be efficiently and simply produced.

[0162] <Method for forming a layer of a curable composition according to this embodiment> The layer of the curable composition of the present embodiment can be formed, for example, by a method including the following steps (BI) and (BII). (Process (BI)) Step (BI) is a step of applying the liquid curable composition of this embodiment obtained in <Production method of liquid curable composition according to this embodiment> onto a release sheet.

[0163] (Process (BII)) The step (BII) is a step of heating and drying the coating film of the liquid curable composition obtained in the step (BI) to obtain a layer of the curable composition.

[0164] In step (BI), the liquid curable composition obtained in step (AII) is applied to a release sheet. The release sheet to which the liquid curable composition is applied is not particularly limited, and may be, for example, a film having a release agent formed thereon. The film is not particularly limited, and may be made of an organic material or an inorganic material. Resins may be used as organic materials, and ceramics, glass, metals, and the like may be used as inorganic materials. In one embodiment, examples of the film include polyester films such as polyethylene terephthalate film and polybutylene terephthalate film, polyolefin films such as polypropylene film and polymethylpentene film, plastic films such as polycarbonate film, metal foils such as aluminum and stainless steel, paper such as glassine paper, fine paper, coated paper, impregnated paper, and synthetic paper, and laminates thereof.

[0165] The thickness of the release sheet is not particularly limited, and in one embodiment, it can be 20 μm or more, and in another embodiment, it can be 25 μm or more, and in one embodiment, it can be less than 200 μm, and in another embodiment, it can be less than 100 μm.

[0166] The release agent is not particularly limited and is composed of a resin. In one embodiment, examples of the release agent include polyolefins such as polyethylene resins, thermoplastic elastomers such as olefin-based thermoplastic elastomers, fluororesins such as tetrafluoroethylene, and silicone resins such as silicones having dimethylpolysiloxane as a basic skeleton.

[0167] The thickness of the release agent is not particularly limited, and in one embodiment, can be 30 nm or more, and in another embodiment, 50 nm or more, and in one embodiment, can be less than 300 nm, and in another embodiment, can be less than 200 nm.

[0168] The method for applying the liquid curable composition onto the release sheet is not particularly limited, and examples thereof include knife coating, blade coating, roll coating, etc. The liquid curable composition is stored in a container such as a 18L can, a pail can, or a drum can, and is used by supplying the liquid curable composition to a coating device.

[0169] The applied liquid curable composition is dried by heating, for example, to volatilize a part of the solvent (S), thereby obtaining a layer of the curable composition. The heating temperature may be 80° C. or higher in one embodiment, 90° C. or higher in another embodiment, and 120° C. or lower in one embodiment, and 110° C. or lower in another embodiment. The heating temperature may be in the range of 80 to 120° C. in one embodiment, and 90 to 110° C. in another embodiment. The heating time may be in the range of 10 minutes to 1 hour in one embodiment, and 20 minutes to 30 minutes in another embodiment. As an example, a coating of the liquid curable composition is heated at 100° C. for 20 minutes to form a layer of the curable composition.

[0170] <Method of Fixing Semiconductor Element According to the Present Embodiment> The method for fixing the semiconductor element in this embodiment can be, for example, a method including the following steps (CI) and (CII). (Process (CI)) Step (CI) is a step of disposing a semiconductor element on the layer of the curable composition of this embodiment obtained in step (BII).

[0171] (Process (CII)) Step (CII) is a step of thermally curing the layer of the curable composition containing the semiconductor element obtained in step (CI).

[0172] In step (CI), a semiconductor element is attached to the layer of the curable composition obtained in step (BII) and arranged (mounted). The semiconductor element is not particularly limited, and examples thereof include optical semiconductor elements such as light-emitting elements such as lasers and light-emitting diodes (LEDs) and light-receiving elements such as solar cells, transistors, sensors such as temperature sensors and pressure sensors, and integrated circuits. Among these, the semiconductor element can be an optical semiconductor element from the viewpoint of easily exerting the effects of using the liquid curable composition and the layer of the curable composition according to this embodiment. The method of arranging the semiconductor element on the layer of the curable composition is not particularly limited, and for example, the semiconductor element can be arranged on the layer of the curable composition by facing the semiconductor element to a part of the adhesive surface of the layer of the curable composition and pressing the semiconductor element. Thereafter, the release sheet may be peeled off, and the exposed layer of the curable composition may be attached to another adherend (for example, a substrate such as a glass substrate).

[0173] In addition, for example, the layer of the curable composition obtained in step (BII) can be first attached to another adherend (e.g., a substrate such as a glass substrate), and then the release sheet can be peeled off, and the semiconductor element can be placed against a portion of the adhesive surface of the exposed layer of the curable composition and pressed against the semiconductor element, thereby placing the semiconductor element on the layer of the curable composition.

[0174] In step (CII), the layer of the curable composition containing the semiconductor element obtained in step (CI) is thermally cured. The layer of the curable composition is heated to volatilize the solvent (S) and cure, thereby fixing the semiconductor element to the cured layer. The heating temperature during curing can be 100° C. or higher in one embodiment, 120° C. or higher in another embodiment, 180° C. or lower in one embodiment, and 160° C. or lower in another embodiment. The heating temperature during curing can be in the range of 100 to 180° C. in one embodiment, and 120 to 160° C. in another embodiment. The heating time during curing can be in the range of 30 minutes to 10 hours in one embodiment, 1 hour to 7 hours in another embodiment, and 3 hours to 5 hours in yet another embodiment. As an example, the layer of the curable composition containing the semiconductor element is heated at 150° C. for 4 hours to fix the semiconductor element to the cured layer. This allows the semiconductor element to be fixed to the cured material layer in an appropriate posture, and when a light-emitting element such as an LED chip is fixed to the cured material layer, the light-emitting element is not fixed at an angle, resulting in a light-emitting device with the desired brightness.

[0175] The thickness of the cured layer is not particularly limited, and may be any thickness that can firmly fix the semiconductor element by curing. The thickness of the cured layer may be 1 μm or more in one embodiment, 5 μm or more in another embodiment, 10 μm or more in yet another embodiment, 30 μm or more in yet another embodiment, 40 μm or more in yet another embodiment, and may be 100 μm or less in one embodiment, 80 μm or less in another embodiment, and 60 μm or less in yet another embodiment. The thickness range of the cured layer may be 1 μm or more and 100 μm or less in one embodiment, 5 μm or more and 80 μm or less in another embodiment, 10 μm or more and 80 μm or less in yet another embodiment, 30 μm or more and 60 μm or less in yet another embodiment, and 40 μm or more and 60 μm or less in yet another embodiment.

[0176] <Summary of the embodiment> The disclosure of the present specification includes the following liquid curable composition, a layer of the curable composition, a method for forming a layer of the curable composition, and a method for fixing a semiconductor element.

[0177] (Item 1) A liquid curable composition containing a curable organopolysiloxane compound, The liquid curable composition is heated at 100° C. for 20 minutes to obtain a layer having a thickness of 50 μm±7 μm, which layer has a tack strength of 1000 mN or more, The liquid curable composition is heated at 100°C for 20 minutes, and the layer obtained has a mass loss rate of 13% or less after heating at 150°C for 4 hours.

[0178] (Item 2) 2. The liquid curable composition according to item 1, wherein the curable organopolysiloxane compound is a polysilsesquioxane compound.

[0179] (Item 3) 3. The liquid curable composition according to item 1 or 2, wherein the liquid curable composition has a viscosity of 5 Pa·s or more.

[0180] (Item 4) 4. The liquid curable composition according to any one of items 1 to 3, further comprising a silicone oligomer that is liquid at 23° C.

[0181] (Item 5) 5. The liquid curable composition according to any one of items 1 to 4, further comprising a solvent having a boiling point of 70° C. or higher and lower than 200° C.

[0182] (Item 6) 6. The liquid curable composition according to any one of items 1 to 5, wherein the layer having a thickness of 50 μm±7 μm obtained by heating the liquid curable composition at 100° C. for 20 minutes has a tack strength of 10,000 mN or less.

[0183] (Item 7) Applying the liquid curable composition according to any one of items 1 to 6 to a release sheet; drying the liquid curable composition by heating; A method for forming a layer of a curable composition comprising:

[0184] (Item 8) A layer of a curable composition containing a curable organopolysiloxane compound, It has a tack strength of 1000mN or more. A layer of a curable composition, which has a mass loss of 13% or less after heating at 150°C for 4 hours.

[0185] (Item 9) 9. The layer of curable composition according to item 8, wherein the curable organopolysiloxane compound is a polysilsesquioxane compound.

[0186] (Item 10) 10. The layer of curable composition according to claim 8 or 9, wherein the layer of curable composition has a tack force of 10,000 mN or less.

[0187] (Item 11) Arranging a semiconductor element on a layer of the curable composition according to any one of items 8 to 10; thermally curing the layer of curable composition; and A method for fixing a semiconductor element, comprising: EXAMPLES

[0188] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples. In each example, parts and percentages are by weight unless otherwise specified.

[0189] (average molecular weight measurement) The mass average molecular weight (Mw) and number average molecular weight (Mn) of the curable organopolysiloxane compound (A) obtained in the Production Examples were measured using the following apparatus and conditions, expressed as standard polystyrene equivalent values. Device name: HLC-8220GPC, manufactured by Tosoh Corporation Column: TSKgel GMHXL, TSKgel GMHXL, and TSKgel 2000HXL connected in sequence Solvent: Tetrahydrofuran Injection volume: 20μl Measurement temperature: 40℃ Flow rate: 1ml / min Detector: Differential refractometer

[0190] (IR spectrum measurement) The IR spectrum of the curable organopolysiloxane compound (A) obtained in the Production Examples was measured using a Fourier transform infrared spectrophotometer (Spectrum 100, manufactured by PerkinElmer).

[0191] (Production Example 1) A 300 ml eggplant-shaped flask was charged with 28.91 g (145.8 mmol) of phenyltrimethoxysilane (Shin-Etsu Chemical Co., Ltd.), and then an aqueous solution of 0.0376 g of 35% hydrochloric acid (0.25 mol% relative to the total amount of silane compounds) dissolved in 7.874 ml of distilled water was added while stirring, and the total volume was stirred at 30°C for 2 hours, then heated to 70°C and stirred for 5 hours. Thereafter, the reaction liquid was returned to room temperature (23°C), and 50 g of propyl acetate and 100 g of water were added to perform a liquid separation treatment, and an organic layer containing a reaction product was obtained. Magnesium sulfate was added to this organic layer and dried. After filtering and removing magnesium sulfate, the organic layer was concentrated with an evaporator, and the concentrate was vacuum dried to obtain 17.0 g of a curable organopolysiloxane compound (A1). The curable organopolysiloxane compound (A1) had a mass average molecular weight (Mw) of 1,100 and a molecular weight distribution (Mw / Mn) of 1.2. The IR spectrum data of the curable organopolysiloxane compound (A1) is shown below. Si-C6H5: 698cm -1 ,Si-O:1132cm -1

[0192] (Production Example 2) After 71.37g (400mmol) of methyltriethoxysilane was charged into a 300mL eggplant-shaped flask, 0.10g of 35% hydrochloric acid (0.25mol% relative to the total amount of silane compounds) was dissolved in 21.6ml of distilled water and added with stirring, and the entire volume was stirred at 30°C for 2 hours, then heated to 70°C and stirred for 5 hours. Then, 140g of propyl acetate was added and stirred. 0.12g of 28% ammonia water (0.5mol% relative to the total amount of silane compounds) was added with stirring, and the entire volume was heated to 70°C and further stirred for 3 hours. Purified water was added to the reaction solution, and the solution was separated. This operation was repeated until the pH of the aqueous layer reached 7. The organic layer was concentrated with an evaporator, and the concentrate was vacuum dried to obtain 55.7g of a curable organopolysiloxane compound (A2). The curable organopolysiloxane compound (A2) had a mass average molecular weight (Mw) of 7,800 and a molecular weight distribution (Mw / Mn) of 4.52. The IR spectrum data of the curable organopolysiloxane compound (A2) is shown below. Si-CH3: 1272cm -1 ,1409cm -1 ,Si-O:1132cm -1

[0193] (Production Example 3) In a 300mL eggplant-shaped flask, 17.0g (77.7mmol) of 3,3,3-trifluoropropyltrimethoxysilane (Shin-Etsu Chemical Co., Ltd.) and 32.33g (181.3mmol) of methyltriethoxysilane (Shin-Etsu Chemical Co., Ltd.) were charged, and an aqueous solution of 0.0675g of 35% hydrochloric acid (0.65mmol amount of HCl, 0.25mol% relative to the total amount of silane compounds) dissolved in 14.0ml of distilled water was added with stirring, and the total volume was stirred at 30°C for 2 hours, then heated to 70°C and stirred for 20 hours. While continuing to stir the contents, a mixed solution of 0.0394g of 28% ammonia water (0.65mmol amount of NH3) and 46.1g of propyl acetate was added thereto to adjust the pH of the reaction solution to 6.9, and the mixture was stirred at 70°C for 40 minutes. After the reaction solution was cooled to room temperature (23°C), 50g of propyl acetate and 100g of water were added thereto and separated to obtain an organic layer containing a reaction product. Magnesium sulfate was added to this organic layer and dried. After filtering and removing magnesium sulfate, the organic layer was concentrated with an evaporator, and the concentrate was vacuum dried to obtain 22.3g of a curable organopolysiloxane compound (A3). The mass average molecular weight (Mw) of the curable organopolysiloxane compound (A3) was 5,500, and the molecular weight distribution (Mw / Mn) was 3.40. The IR spectrum data of the curable organopolysiloxane compound (A3) is shown below. Si-CH3: 1272cm -1 ,1409cm -1 ,Si-O:1132cm -1 ,CF:1213cm -1

[0194] The compounds used in the examples and comparative examples are shown below. (Component (A)) Curable organopolysiloxane compound (A1): Organopolysiloxane compound obtained in Production Example 1 (solid at 23°C) Curable organopolysiloxane compound (A2): Organopolysiloxane compound obtained in Production Example 2 (solid at 23°C) Curable organopolysiloxane compound (A3): Organopolysiloxane compound obtained in Production Example 3 (solid at 23°C)

[0195] ((B) component) Silane coupling agent (B1): 1,3,5-N-tris[3-(trimethoxysilyl)propyl]isocyanurate (manufactured by Shin-Etsu Chemical Co., Ltd., product name "KBM-9659") Silane coupling agent (B2): 3-(trimethoxysilyl)propylsuccinic anhydride (manufactured by Shin-Etsu Chemical Co., Ltd., product name "X-12-967C")

[0196] ((C) component) Silicone oligomer (C): Alkoxy group-containing silicone oligomer (manufactured by Shin-Etsu Chemical Co., Ltd., product name "KR-9218", viscosity at 23°C is 50 mPa·s (measurement method: same as for viscosity evaluation of liquid curable composition described later))

[0197] ((D) component) Fine particles (D1): Silica fine particles surface-treated with trimethylsilyl groups (manufactured by Nippon Aerosil Co., Ltd., product name "AEROSIL RX300", average primary particle diameter: 7 nm, specific surface area: 210 m 2 / g) Microparticles (D2): Silicone-based microparticles (manufactured by Nikko Rica Corporation, product name "MSP-SN08", average primary particle diameter: 0.8 μm, shape: spherical)

[0198] (Solvent (S)) Solvent (S1): Methyl ethyl ketone (SL) (boiling point: 80°C) Solvent (S2): Cyclohexanone (SL) (boiling point: 157°C) Solvent (S3): Tripropylene glycol-n-butyl ether (TPnB) (SH) (Dow Chemical Company, boiling point: 274°C) Solvent (S4): Diethylene glycol monobutyl ether acetate (BDGAC) (SL) (Tokyo Chemical Industry Co., Ltd., boiling point: 247°C)

[0199] (Preparation of Liquid Curable Composition) Example 1 In terms of solid content (active ingredient) mass ratio, 100 parts by mass of the curable organopolysiloxane compound (A1) was mixed with 2 parts by mass of the silane coupling agent (B1), 5 parts by mass of the silane coupling agent (B2), 10 parts by mass of the silicone oligomer (C), and 5 parts by mass of the microparticles (D1), and further solvent (S1) was added to adjust the solid content concentration to 90%, and the entire content was thoroughly mixed and degassed to obtain a liquid curable composition.

[0200] Examples 2 to 6 and Comparative Examples 1 to 5 The types of compounds ((A) component, (B) component, (C) component, (D) component) and the blending ratios (solid content (active ingredient) mass ratios) were changed to those shown in Table 1 below, and the mass ratios of each solvent (S1, S2, S3, S4) relative to 100 parts by mass of the total solvent contained in each composition were changed to those shown in Table 1 below. Except for this, the liquid curable compositions of Examples 2 to 6 and Comparative Examples 1 to 5 were obtained in the same manner as in Example 1. In Comparative Example 1, the liquid curable composition was prepared so that the solid content concentration was 85%, and in Comparative Example 2, the liquid curable composition was prepared so that the solid content concentration was 80%.

[0201] (Viscosity evaluation) The liquid curable composition obtained in Example 1 was subjected to a shear rate of 2 s at 23° C. using a rheometer (manufactured by Anton Paar, product name “MCR301”) with a cone plate having a radius of 50 mm and a cone angle of 0.5°. -1 The viscosity was measured at 100° C. for 1 hour. The viscosity of the liquid curable compositions obtained in Examples 2 to 6 and Comparative Examples 1 to 5 was also measured in the same manner as in Example 1 above.

[0202] [Table 1]

[0203] (Preparation of a layer of a curable composition) The liquid curable composition obtained in Example 1 was applied to the release-treated surface of a release sheet (manufactured by Lintec Corporation, product name "SP-PET381031", thickness: 38 μm) in which one side of a polyethylene terephthalate film was treated for release with a silicone-based release agent, using an applicator so that the thickness after heating and drying was 50 μm ± 7 μm. The applied layer was heat-treated at 100° C. for 20 minutes to obtain a layer of the curable composition. In the same manner as in Example 1, the layers of the curable compositions of Examples 2 to 6 and Comparative Examples 1 to 5 were obtained from the liquid curable compositions obtained in Examples 2 to 6 and Comparative Examples 1 to 5 (more specifically, a layer of the curable composition with a release sheet was obtained).

[0204] (Coatability evaluation) In producing the layer of the curable composition, the surface of the layer of the curable composition of Example 1, measuring 100 mm in length and 20 mm in width, was visually observed and the coatability was evaluated according to the following criteria. ○: No repelling (collection of spreading liquid) and no roughness of the coating surface △: At least one of repelling and coating surface roughness is observed. In the same manner as in Example 1, the coatability of the layers of the curable compositions of Examples 2 to 6 and Comparative Examples 1 to 5 was evaluated.

[0205] (tack strength) In the preparation of the layer of the curable composition, the layer of the curable composition of Example 1 was placed on a probe tack tester (manufactured by Tester Sangyo Co., Ltd., stainless steel probe), and the force (probe tack value) when the probe was brought into contact with the layer at 23°C for a certain period of time and then peeled off was measured, thereby measuring the tackiness of the layer of the curable composition. In addition, the probe was wiped and washed with ethyl acetate before the measurement. This measurement was performed seven times by changing the contact position of the probe on the layer of the curable composition, and the first and second smallest values ​​of the seven measured values ​​were omitted, and the average value of the remaining five measured values ​​was taken as the probe tack value (mN). The tackiness was measured under the following conditions. Contact load: 600gf Contact speed: 10mm / sec Probe Area: 5mmΦ Contact time: 1 second Peeling speed: 10mm / sec In the same manner as in Example 1, the tack strength of the layers of the curable compositions of Examples 2 to 6 and Comparative Examples 1 to 5 was measured.

[0206] (mass reduction rate) In the preparation of the liquid curable composition, 20 mg ± 1 mg of the liquid curable composition of Example 1 was applied to a sample pan for measurement and placed in a differential thermal and thermogravimetric simultaneous analyzer (manufactured by Shimadzu Corporation, product name "DTG-60"). The temperature inside the furnace was increased at a heating rate of 10 ° C. / min, and the mass at the time when the temperature reached 40 ° C. was measured as the initial mass, and then the temperature inside the furnace was increased at a heating rate of 10 ° C. / min, and after the temperature reached 100 ° C., it was maintained for 20 minutes, and the mass of the layer after heating and drying was measured. The mass reduction rate [%] of the liquid curable composition after heating is calculated from the initial mass and the mass of the layer after heating and drying by the following formula. Mass reduction rate of liquid curable composition after heating [%] = {{(initial mass) - (mass of layer after heating and drying)} / (initial mass)} × 100

[0207] Following measurement of the mass of the layer after heating and drying, the temperature inside the furnace was increased at a rate of 10° C. / min, and after the temperature reached 150° C., the temperature was maintained for 4 hours, and the mass of the resulting cured layer was measured. The mass reduction rate [%] of the cured layer after curing relative to the layer after heating and drying of the liquid curable composition was calculated from the mass of the layer after heating and drying and the mass of the cured layer according to the following formula. Mass reduction rate of the curable composition layer after heating [%] = {{(mass of layer after heating and drying) - (mass of cured layer)} / (mass of layer after heating and drying)} × 100

[0208] In the same manner as in Example 1, the mass loss rate of the liquid curable composition after heating and the mass loss rate of the curable composition layer after heating were also determined for the liquid curable compositions of Examples 2 to 6 and Comparative Examples 1 to 5.

[0209] (Zipping (peel marks left after peeling off release sheet) evaluation) In preparing the curable composition layer, the curable composition layer of Example 1 (more specifically, the curable composition layer in the curable composition layer with release sheet) was laminated to a polyethylene terephthalate film having a thickness of 50 μm at 23° C. with a hand roller to obtain a laminate having the order release sheet / curable composition layer / polyethylene terephthalate film. The release sheet was peeled from the laminate at 23° C. at a peel speed of 10 m / min and a peel angle of 180°. The surface condition of the peeled surface of the curable composition layer was visually observed, and zipping was evaluated according to the following criteria. ○: The surface of the layer of the curable composition in contact with the release sheet was not deformed and the surface condition was smooth. Δ: Deformation occurred on the surface of the layer of the curable composition that was in contact with the release sheet, and streaks or the like were visually confirmed. In the same manner as in Example 1, zipping of the layers of the curable compositions of Examples 2 to 6 and Comparative Examples 1 to 5 was evaluated.

[0210] (Mountability evaluation) In preparing the layer of the curable composition, the layer of the curable composition of Example 1 (more specifically, the layer of the curable composition in the layer of the curable composition with a release sheet) was placed facing up, and one silicon chip of length 1 mm x width 1 mm x thickness 0.35 mm was mounted on the exposed layer of the curable composition with a load of 0.49 N. Within 3 seconds after mounting, the layer of the curable composition with the silicon chip obtained was turned upside down (with the coating layer facing vertically downward), and the mounting property was evaluated according to the following criteria. The same evaluation was performed five times (i.e., five chips) by changing the mounting position. ○: None of the chips fell ×: One or more chips fell off In the same manner as in Example 1, the mounting properties of the layers of the curable compositions of Examples 2 to 6 and Comparative Examples 1 to 5 were evaluated.

[0211] (Void evaluation of the cured layer) In the preparation of the layer of the curable composition, the layer of the curable composition of Example 1 (more specifically, the layer of the curable composition in the layer of the curable composition with a release sheet) was attached to an adherend of colorless and transparent glass (length 50 mm x width 50 mm x thickness 1 mm), and the release sheet was peeled off to obtain a laminate in the order of the layer of the curable composition / colorless and transparent glass. Five glass chips with a length of 10 mm x width 10 mm x thickness of 0.35 mm were mounted on the exposed layer of the curable composition of the laminate with a load of 0.49 N, and the presence or absence of bubbles before the heat treatment was observed and recorded. Thereafter, the layer was heat-treated at 150°C for 4 hours to obtain a cured layer with glass chips fixed to the colorless and transparent glass. The cured layer with glass chips fixed to the colorless and transparent glass was visually observed for the presence or absence of voids at the interface between the cured layer and the glass chip (i.e., bubbles increased after the heat treatment compared to before the heat treatment), and the voids in the cured layer were evaluated according to the following criteria. ◎: No voids were observed in any of the five mounted chips. ○: Of the five mounted chips, some had voids with a diameter of less than 1 mm, but none had voids with a diameter of 1 mm or more. ×: Among the five mounted chips, there was a chip in which a void with a diameter of 1 mm or more occurred. In the same manner as in Example 1, the layers of the curable compositions of Examples 2 to 6 and Comparative Examples 1 to 5 were evaluated for voids.

[0212] Table 2 shows the results of the tack strength, mass reduction rate, coatability evaluation, zipping evaluation, mounting property evaluation, and void evaluation for Examples 1 to 6 and Comparative Examples 1 to 5.

[0213] [Table 2]

[0214] The liquid curable compositions of Examples 1 to 6 were heated at 100° C. for 20 minutes to obtain a layer of the curable composition (layer after heat drying) having a tack strength of 1000 mN or more. In addition, the liquid curable compositions of Examples 1 to 6 were heated at 100° C. for 20 minutes to obtain a layer after heat drying, and the reduction rate of the mass of the cured layer after the layer after heat drying was further heated at 150° C. for 4 hours was 13% or less relative to the mass of the layer after heat drying. Thus, the liquid curable compositions of Examples 1 to 6 were capable of appropriately attaching a semiconductor element to the layer of the curable composition obtained therefrom, and capable of fixing the semiconductor element to the cured layer in an appropriate position.

[0215] On the other hand, the liquid curable compositions of Comparative Examples 3 and 5 were heated at 100° C. for 20 minutes to obtain a layer of the curable composition (layer after heating and drying) with a tack strength of less than 1000 mN. In addition, the liquid curable compositions of Comparative Examples 1, 2, and 4 were heated at 100° C. for 20 minutes to obtain a layer after heating and drying, and the reduction rate of the mass of the cured layer after further heating the heated and dried layer at 150° C. for 4 hours was more than 13%. Thus, the liquid curable compositions of Comparative Examples 1 to 5 were not capable of properly attaching a semiconductor element to the layer of the curable composition obtained therefrom, and were not capable of fixing the semiconductor element to the cured layer in an appropriate position.

[0216] Although the embodiment of the invention has been described above, the invention is not limited to the above embodiment, and various modifications and variations are possible within the scope of the gist of the invention.

Claims

1. A liquid curable composition containing a curable organopolysiloxane compound, the liquid curable composition is heated at 100° C. for 20 minutes to obtain a layer having a thickness of 50 μm±7 μm, which layer has a tack strength of 1000 mN or more; The liquid curable composition, wherein the layer obtained by heating the liquid curable composition at 100°C for 20 minutes has a mass reduction rate of 13% or less after heating at 150°C for 4 hours.

2. The liquid curable composition according to claim 1 , wherein the curable organopolysiloxane compound is a polysilsesquioxane compound.

3. The liquid curable composition according to claim 1 , wherein the liquid curable composition has a viscosity of 5 Pa·s or more.

4. The liquid curable composition according to claim 1 , further comprising a silicone oligomer that is liquid at 23° C.

5. The liquid curable composition according to claim 1 , further comprising a solvent having a boiling point of 70° C. or higher and lower than 200° C.

6. 2. The liquid curable composition according to claim 1, wherein the layer having a thickness of 50 μm±7 μm obtained by heating the liquid curable composition at 100° C. for 20 minutes has a tack strength of 10,000 mN or less.

7. Applying the liquid curable composition according to claim 1 to a release sheet; drying the liquid curable composition by heating; A method for forming a layer of a curable composition comprising:

8. A layer of a curable composition containing a curable organopolysiloxane compound, It has a tack strength of 1000 mN or more, A layer of a curable composition having a mass loss of 13% or less after heating at 150°C for 4 hours.

9. 9. The layer of curable composition of claim 8, wherein the curable organopolysiloxane compound is a polysilsesquioxane compound.

10. 9. The layer of curable composition of claim 8, wherein the layer of curable composition has a tack force of 10,000 mN or less.

11. disposing a semiconductor element on a layer of the curable composition of claim 8; thermally curing the layer of curable composition; and A method for fixing a semiconductor element, comprising:

Citation Information

Patent Citations

  • Silicone adhesive and adhesive film

    JP2004075918A

  • Thermosetting organopolysiloxane composition and adhesive

    JP2005053966A

  • Curable hot-melt silicone composition, cured material thereof, and laminate containing the composition or cured material

    JP2021107550A

  • Polyorganosilsesquisoxane, curable composition, cured material, hard coat film, adhesive sheet, and laminate

    JP2022039836A

  • Curable composition, method for producing curable composition, cured object, method for using curable composition, and optical device

    WO2016031728A1