Photosensitive resin composition, transparent substrate with frame member, and semiconductor device
The photosensitive resin composition, featuring an alkali-soluble resin with epoxy groups and 1,2-epoxidized polybutadiene, addresses the challenge of balancing developability and heat resistance, enhancing the performance of semiconductor device components.
Patent Information
- Application Number
- JP2023054086
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-03-29
AI Technical Summary
Existing photosensitive resin compositions used in semiconductor devices face challenges in achieving both developability and heat resistance, as well as sufficient compressive strength in the cured product.
A photosensitive resin composition containing an alkali-soluble resin with an epoxy group, 1,2-epoxidized polybutadiene, and a photoacid generator, with specific weight ratios and inclusion of polysiloxane compounds, particularly those with cyclic siloxane structures, to enhance heat resistance and compressive strength while maintaining developability.
The composition achieves both high developability and heat resistance, along with improved compressive strength, making it suitable for semiconductor device manufacturing processes.
Smart Images

Figure 00000019_0000 
Figure 00000019_0001 
Figure 00000019_0002
Abstract
Description
[Technical field]
[0001] The present invention relates to a photosensitive resin composition, a transparent substrate with a frame-shaped member, and a semiconductor device. [Background technology]
[0002] Conventionally, semiconductor devices having imaging elements such as CMOS image sensors and CCD image sensors are applied to imaging devices such as digital cameras and smartphones. In the semiconductor device, for example, a rib material is arranged around the imaging element, and an active area of the imaging element is covered with a seal glass fixed on the rib material, forming a hollow structure. In addition, the semiconductor device is sealed with resin.
[0003] Patent Document 1 describes a method for manufacturing semiconductor devices in which a protective area defined on a seal glass covering an active area of an imaging element of each semiconductor device is protected with a release film, and multiple semiconductor devices are collectively sealed with resin. Here, a movable core provided in a mold for each semiconductor device adjusts the pressing force of the release film against the semiconductor device.
[0004] On the other hand, Patent Document 2 describes a photosensitive composition containing a polysiloxane compound, a photoacid generator, a colorant, and a solvent, in which the colorant content is 5% by weight or more of the total solid content. Here, the polysiloxane compound contains a cyclic polysiloxane structure and a cationic polymerizable functional group. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2014-225619 A [Patent Document 2] International Publication No. 2018 / 061988 Summary of the Invention [Problem to be solved by the invention]
[0006] Here, it is conceivable to place a rib material using the photosensitive composition described in Patent Document 2, and then seal it with resin using the semiconductor device manufacturing method described in Patent Document 1. However, it is necessary to achieve both the developability of the photosensitive composition and the heat resistance and compressive strength of the cured product of the photosensitive composition.
[0007] An object of the present invention is to provide a photosensitive resin composition that can achieve both developability and heat resistance and compressive strength of a cured product. [Means for solving the problem]
[0008] (1) A photosensitive resin composition comprising an alkali-soluble resin having an epoxy group, an epoxidized 1,2-polybutadiene, and a photoacid generator, wherein the weight ratio of the epoxidized 1,2-polybutadiene to the alkali-soluble resin is 0.20 or more and 1.10 or less.
[0009] (2) The photosensitive resin composition according to (1), wherein the alkali-soluble resin is a polysiloxane compound.
[0010] (3) The photosensitive resin composition according to (2), wherein the polysiloxane compound has a cyclic siloxane structure.
[0011] (4) The photosensitive resin composition according to any one of (1) to (3), wherein the alkali-soluble resin has an alicyclic epoxy group and / or a glycidyl group.
[0012] (5) The photosensitive resin composition according to any one of (1) to (4), wherein the alkali-soluble resin has a group represented by the following formula (Ia) and / or a group represented by the following formula (Ib): [ka]
[0013] (6) The photosensitive resin composition according to any one of (1) to (5), further comprising a pigment, the weight ratio of the pigment to the alkali-soluble resin being 0.01 or more and 0.30 or less.
[0014] (7) A transparent substrate with a frame-shaped member, comprising a frame-shaped member including a cured product of the photosensitive resin composition according to any one of (1) to (6) above provided on the transparent substrate.
[0015] (8) A semiconductor device comprising: a transparent substrate with a frame-shaped member as described in (7); and a semiconductor substrate on which a light-receiving element is mounted, the transparent substrate with a frame-shaped member being disposed opposite the semiconductor substrate, and the frame-shaped member being disposed around the light-receiving element.
[0016] (9) A semiconductor device comprising: a transparent substrate with a frame-shaped member as described in (7); and a semiconductor substrate on which a light-receiving element is mounted, the transparent substrate with a frame-shaped member being disposed opposite the semiconductor substrate via a frame-shaped spacer, the spacer being disposed on the opposite side of the transparent substrate to the frame-shaped member, and the spacer being disposed around the light-receiving element. Effect of the Invention
[0017] According to the present invention, it is possible to provide a photosensitive resin composition that can achieve both developability and heat resistance and compressive strength of a cured product. [Brief description of the drawings]
[0018] [Figure 1] 1 is a cross-sectional view showing an example of a frame-shaped member-attached transparent substrate of the present embodiment. [Diagram 2] 1 is a cross-sectional view showing an example of a semiconductor device according to an embodiment of the present invention. [Diagram 3] 10 is a cross-sectional view showing another example of the semiconductor device according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, an embodiment of the present invention will be described.
[0020] (Photosensitive resin composition) The photosensitive resin composition of the present embodiment contains an alkali-soluble resin having an epoxy group, 1,2-epoxidized polybutadiene, and a photoacid generator, and therefore has high heat resistance.
[0021] In the present specification and claims, 1,2-epoxidized polybutadiene means an epoxidized product of a 1,2-adduct of 1,3-butadiene.
[0022] The weight ratio of 1,2-epoxidized polybutadiene to the alkali-soluble resin is from 0.20 to 1.10, and preferably from 0.3 to 1.0. If the weight ratio of 1,2-epoxidized polybutadiene to the alkali-soluble resin is less than 0.20, the compressive strength of the cured product of the photosensitive resin composition decreases, whereas if it exceeds 1.10, the developability of the photosensitive resin composition decreases.
[0023] The alkali-soluble resin is not particularly limited as long as it has an alkali-soluble group, and examples thereof include polysiloxane compounds.
[0024] Examples of the alkali-soluble group include a phenolic hydroxyl group, a carboxyl group, a group represented by the following formula (Ia), and a group represented by the following formula (Ib). From the viewpoint of the heat resistance of the cured product of the photosensitive resin composition, the group represented by the following formula (Ia) and / or the group represented by the following formula (Ib) is preferred.
[0025] [ka]
[0026] The polysiloxane compound preferably has a cyclic siloxane structure, which improves the film-forming properties of the photosensitive resin composition of the present embodiment and the heat resistance of the cured product.
[0027] In this specification and claims, a cyclic siloxane structure means a cyclic structure having a siloxane bond (-Si-O-).
[0028] The polysiloxane compound may have a cyclic siloxane structure in a side chain, but preferably has a cyclic siloxane structure in a main chain, which increases the heat resistance of the cured product of the photosensitive resin composition of the present embodiment.
[0029] The cyclic siloxane structure may be a monocyclic structure or a polycyclic structure. Here, the polycyclic structure may be a polyhedral structure. When the cyclic siloxane structure has a high content of T units (XSiO3 / 2) or Q units (SiO4 / 2), the hardness and heat resistance of the cured product of the photosensitive resin composition of this embodiment are high. In addition, when the cyclic siloxane structure has a high content of M units (X3SiO1 / 2) or D units (X2SiO2 / 2), the flexibility of the cured product of the photosensitive resin composition of this embodiment is high.
[0030] The epoxy group contained in the alkali-soluble resin functions as a photocationically polymerizable group and undergoes ring-opening polymerization.
[0031] From the viewpoint of stability, the alkali-soluble resin preferably has an alicyclic epoxy group or a glycidyl group, and from the viewpoint of photocationic polymerizability, it is particularly preferable that the alkali-soluble resin has an alicyclic epoxy group.
[0032] The alkali-soluble resin may have a plurality of epoxy groups, which increases the crosslink density of the cured product of the photosensitive resin composition of the present embodiment, and as a result, increases the heat resistance of the cured product of the photosensitive resin composition of the present embodiment.
[0033] The multiple epoxy groups contained in the alkali-soluble resin may be the same or different.
[0034] The alkali-soluble resin can be synthesized by a known method. The polysiloxane compound can be obtained, for example, by hydrosilylation reaction of a compound (α) having one or more alkenyl groups and an alkali-soluble group, a cyclic siloxane (β) having multiple hydrosilyl groups, and a compound (γ) having one or more alkenyl groups and an epoxy group. At this time, a compound (δ) having multiple alkenyl groups and no alkali-soluble group or epoxy group may be hydrosilylated. As a result, crosslinking occurs between the compounds (β), so that the molecular weight of the polysiloxane compound is increased, and the film-forming property of the photosensitive resin composition of this embodiment and the heat resistance of the cured film are improved. In addition, a compound (ε) having a single hydrosilyl group or alkenyl group and no alkali-soluble group or epoxy group may be hydrosilylated. As a result, a specific functional group can be introduced to the end of the polysiloxane compound. Furthermore, a chain polysiloxane having multiple hydrosilyl groups may be hydrosilylated.
[0035] Examples of the alkenyl group in the compound (α) include a vinyl group, an allyl group, and a methallyl group. Among these, the vinyl group and the allyl group are preferred from the viewpoint of reactivity in the hydrosilylation reaction.
[0036] Examples of the compound (α) include diallyl isocyanuric acid, monoallyl isocyanuric acid, diallyl bisphenol A, diallyl bisphenol S, vinylphenol, allylphenol, butenoic acid, pentenoic acid, hexenoic acid, heptenoic acid, and undecylenic acid. Among these, from the viewpoint of the heat resistance of the cured product of the photosensitive resin composition of the present embodiment, diallyl isocyanuric acid, monoallyl isocyanuric acid, diallyl bisphenol A, diallyl bisphenol S, vinylphenol, and allylphenol are preferred. In addition, from the viewpoint of the electrical properties of the cured product of the photosensitive resin composition of the present embodiment, diallyl isocyanuric acid and monoallyl isocyanuric acid are particularly preferred.
[0037] When diallyl isocyanuric acid and monoallyl isocyanuric acid are used as the compound (α), a group represented by formula (Ia) and a group represented by formula (Ib) are introduced into the polysiloxane compound, respectively. The group represented by formula (Ib) has a higher acidity (smaller pKa) than the group represented by formula (Ia). Therefore, when monoallyl isocyanuric acid is used as the compound (α), the developability of the photosensitive resin composition of this embodiment is improved.
[0038] When monoallyl isocyanuric acid is used as the compound (α), it is preferable to use a compound (δ) having multiple alkenyl groups in combination in order to increase the molecular weight and crosslink density of the polysiloxane compound. Also, diallyl isocyanuric acid and monoallyl isocyanuric acid may be used in combination as the compound (α).
[0039] The cyclic siloxane (β) has a plurality of hydrosilyl groups (see, for example, International Publication No. 96 / 15194). The cyclic siloxane (β) preferably has three or more hydrosilyl groups. From the viewpoint of the heat resistance and light resistance of the cured product of the photosensitive resin composition of the present embodiment, the group bonded to the silicon atom is preferably a hydrogen atom or a methyl group.
[0040] The cyclic siloxane (β) is represented, for example, by the following general formula (III).
[0041] [ka] (In the formula, R 4 , R 5 and R 6 are each independently an organic group having 1 to 20 carbon atoms. m is an integer of 2 to 10, and preferably an integer of 3 to 10. n is an integer of 0 to 10, and preferably an integer of 3 to 10. The sum of m and n is preferably an integer of 3 to 12.
[0042] R 4 , R 5 and R6 Examples of R include alkyl groups, hydroxyalkyl groups, alkoxyalkyl groups, and aryl groups. Among these, chain alkyl groups such as methyl groups, ethyl groups, propyl groups, hexyl groups, octyl groups, decyl groups, and dodecyl groups, cyclic alkyl groups such as cyclohexyl groups and norbornyl groups, and phenyl groups are preferred. From the viewpoint of availability of cyclic siloxane (β), R 4 , R 5 and R 6 is preferably a methyl group, a propyl group, a hexyl group, or a phenyl group. 4 and R 5 is more preferably a chain alkyl group having 1 to 6 carbon atoms, and particularly preferably a methyl group.
[0043] Examples of the compound represented by general formula (III) include 1,3,5,7-tetrahydrogen-1,3,5,7-tetramethylcyclotetrasiloxane, 1-propyl-3,5,7-trihydrogen-1,3,5,7-tetramethylcyclotetrasiloxane, 1,5-dihydrogen-3,7-dihexyl-1,3,5,7-tetramethylcyclotetrasiloxane, 1,3,5-trihydrogen-1,3,5-trimethylcyclosiloxane, 1,3,5,7,9-pentahydrogen-1,3,5,7,9-pentamethylcyclosiloxane, and 1,3,5,7,9,11-hexahydrogen-1,3,5,7,9,11-hexamethylcyclosiloxane. Among these, 1,3,5,7-tetrahydrogen-1,3,5,7-tetramethylcyclotetrasiloxane is preferred from the standpoints of availability and reactivity in the hydrosilylation reaction.
[0044] The cyclic siloxane (β) may have a polycyclic structure. In this case, the cyclic siloxane (β) may have a polyhedral skeleton. The number of silicon atoms constituting the polyhedral skeleton is preferably 6 to 24, more preferably 6 to 10.
[0045] The cyclic siloxane (β) may be a polysiloxane having a polyhedral skeleton.
[0046] The cyclic siloxane (β) may be a silylated silicic acid having a polyhedral framework.
[0047] In the silylated silicic acid having a polyhedral skeleton, the silicon atoms and hydrosilyl groups constituting the polyhedral skeleton are bonded via siloxane bonds, and therefore the flexibility of the cured product of the photosensitive resin composition of this embodiment is increased.
[0048] Cyclic siloxane (β) is synthesized by known methods.For example, the compound represented by general formula (III) is synthesized by the method described in International Publication No. 96 / 15194.The polysiloxane having a polyhedral skeleton and the silylated silicic acid are synthesized by the method described in Japanese Patent Application Laid-Open No. 2004-359933, Japanese Patent Application Laid-Open No. 2004-143449, and Japanese Patent Application Laid-Open No. 2006-269402.
[0049] As the cyclic siloxane (β), a commercially available cyclic siloxane may be used.
[0050] The alkenyl group in compound (γ) is the same as the alkenyl group in compound (α).
[0051] Examples of the compound (γ) include vinylcyclohexene oxide, allyl glycidyl ether, diallyl monoglycidyl isocyanurate, and monoallyl diglycidyl isocyanurate. Among these, from the viewpoint of photocationic polymerization, a compound having an alicyclic epoxy group is preferred, and vinylcyclohexene oxide is particularly preferred.
[0052] The compound (δ) may be either a polymeric compound or a low molecular weight compound. Examples of the polymeric compound include polyether compounds, polyester compounds, polyarylate compounds, polycarbonate compounds, saturated hydrocarbon compounds, unsaturated hydrocarbon compounds, polyacrylic acid ester compounds, polyamide compounds, phenol-formaldehyde (phenolic resin) compounds, and polyimide compounds. Examples of the low molecular weight compound include phenolic compounds, bisphenolic compounds, aromatic hydrocarbon compounds such as benzene and naphthalene, linear compounds, aliphatic hydrocarbon compounds such as alicyclic compounds, and heterocyclic compounds.
[0053] From the viewpoint of the heat resistance and light resistance of the cured product of the photosensitive resin composition of the present embodiment, the compound (δ) is preferably a compound represented by the following general formula (VI), and more preferably triallyl isocyanurate or diallyl monomethyl isocyanurate.
[0054] [ka] (In the formula, R 1 and R 2 are each independently an alkenyl group; R 3 is an organic group having 1 to 50 carbon atoms.
[0055] R 1 and R 2 The alkenyl group in R is the same as the alkenyl group in compound (α), but is preferably a vinyl group or an allyl group, and is particularly preferably an allyl group. 3 From the viewpoint of heat resistance of the cured product of the photosensitive resin composition of this embodiment, the number of carbon atoms in R is preferably 1 or more and 20 or less, and more preferably 1 or more and 10 or less. 3is a group selected from chain alkyl groups (e.g., methyl, ethyl, propyl, butyl, etc.), cycloalkyl groups (e.g., cyclohexyl), aryl groups (e.g., phenyl, tolyl), groups in which at least a portion of the hydrogen atoms bonded to the carbon atoms of these groups have been substituted with halogen atoms or cyano groups (e.g., chloromethyl, trifluoropropyl, cyanoethyl), alkenyl groups (e.g., vinyl, allyl, butenyl, hexenyl), (meth)acryloyl groups, epoxy groups, and organic groups having a mercapto group or an amino group.
[0056] When a polysiloxane having a single hydrosilyl group as the compound (ε) is subjected to a hydrosilylation reaction, a polysiloxane structure can be introduced into the terminal of the polysiloxane compound. An example of the polysiloxane having a single hydrosilyl group is a compound in which m is 1 in the general formula (III). The polysiloxane having a single hydrosilyl group may be a chain siloxane.
[0057] When a compound having a single alkenyl group as the compound (ε) is subjected to a hydrosilylation reaction, a desired functional group can be introduced at the end of the polysiloxane compound.
[0058] In addition, instead of the compound (α) having one or more alkenyl groups and an alkali-soluble group, a compound having one or more hydrosilyl groups and an alkali-soluble group may be used. Also, instead of the cyclic siloxane (β) having multiple hydrosilyl groups, a cyclic siloxane having multiple alkenyl groups may be used. Furthermore, instead of the compound (γ) having one or more alkenyl groups and an epoxy group, a compound having one or more hydrosilyl groups and an epoxy group may be used.
[0059] Examples of cyclic siloxanes having an alkenyl group include 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasiloxane, 1-propyl-3,5,7-trivinyl-1,3,5,7-tetramethylcyclotetrasiloxane, 1,5-divinyl-3,7-dihexyl-1,3,5,7-tetramethylcyclotetrasiloxane, 1,3,5-trivinyl-1,3,5-trimethylcyclosiloxane, 1,3,5,7,9-pentavinyl-1,3,5,7,9-pentamethylcyclosiloxane, and 1,3,5,7,9,11-hexavinyl-1,3,5,7,9,11-hexamethylcyclosiloxane. In the cyclic siloxane having an alkenyl group, from the viewpoint of the heat resistance and light resistance of the cured product of the photosensitive resin composition of this embodiment, the organic group bonded to the silicon atom is preferably a vinyl group or a methyl group.
[0060] The order and method of the hydrosilylation reaction are not particularly limited. For example, a polysiloxane compound can be obtained by a hydrosilylation reaction according to the method described in International Publication No. 2009 / 075233. From the viewpoint of suppressing the generation of low molecular weight substances, it is preferable to carry out the introduction of an alkali-soluble group and the introduction of an epoxy group in a stepwise manner into the cyclic siloxane (β). For example, a compound having an excess amount of multiple alkenyl groups (e.g., compound (α) and / or compound (δ)) and a compound having multiple hydrosilyl groups (β) are subjected to a hydrosilylation reaction, and then a compound having a single epoxy group (e.g., compound (γ) and / or compound (ε)) is added to carry out a hydrosilylation reaction.
[0061] The ratio of starting materials in the hydrosilylation reaction is not particularly limited. The molar ratio of the total amount of hydrosilyl groups to the total amount of alkenyl groups of the starting materials is preferably 1 to 30, more preferably 1 to 10. If the molar ratio of the total amount of hydrosilyl groups to the total amount of alkenyl groups of the starting materials is 1 or more, the alkenyl groups are less likely to remain, and if it is 30 or less, the hydrosilyl groups are less likely to remain.
[0062] In carrying out the hydrosilylation reaction, a hydrosilylation catalyst may be used, or a co-catalyst may be used in combination.
[0063] Examples of hydrosilylation catalysts include chloroplatinic acid, platinum-olefin complexes, and platinum-vinylsiloxane complexes.
[0064] The molar ratio of the hydrosilylation catalyst to the total amount of alkenyl groups in the starting material was 1×10 -8 More than 1×10 -1 It is preferable that the value is less than 1×10 -6 More than 1×10 -2 It is more preferable that:
[0065] The reaction temperature for the hydrosilylation reaction is preferably 30°C or higher and 200°C or lower, and more preferably 50°C or higher and 150°C or lower.
[0066] The oxygen concentration in the environment for the hydrosilylation reaction is preferably 0.1% by volume or more and 3% by volume or less.
[0067] The hydrosilylation reaction may be carried out in the presence of a solvent and, optionally, in the presence of a gelation inhibitor.
[0068] Examples of the solvent include hydrocarbon solvents such as benzene, toluene, hexane, and heptane; ether solvents such as tetrahydrofuran, 1,4-dioxane, 1,3-dioxolane, and diethyl ether; ketone solvents such as acetone and methyl ethyl ketone; and halogen solvents such as chloroform, methylene chloride, and 1,2-dichloroethane. Among these, toluene, tetrahydrofuran, 1,4-dioxane, 1,3-dioxolane, and chloroform are preferred because they are easy to remove by distillation.
[0069] The epoxy groups contained in the 1,2-epoxidized polybutadiene function as photocationically polymerizable groups and undergo ring-opening polymerization.
[0070] The number average molecular weight of the 1,2-epoxidized polybutadiene is not particularly limited, but is, for example, 500 or more and 8,000 or less, and preferably 1,000 or more and 6,000 or less.
[0071] The epoxy equivalent of the 1,2-epoxidized polybutadiene is not particularly limited, but is, for example, from 50 eq / g to 300 eq / g, and preferably from 100 eq / g to 250 eq / g.
[0072] The photoacid generator functions as a photocationic polymerization initiator, and when irradiated with light, an acid is generated, and the epoxy groups of the alkali-soluble resin and the 1,2-epoxidized polybutadiene undergo ring-opening polymerization. Examples of light include visible light, ultraviolet light, infrared light, X-rays, α-rays, β-rays, and γ-rays.
[0073] The photoacid generator is not particularly limited as long as it is capable of ring-opening polymerization of an epoxy group, and examples thereof include sulfonate esters, carboxylate esters, and onium salts. Among these, onium salts are preferred.
[0074] Examples of the onium salt include sulfonium salts and iodonium salts. Among these, sulfonium salts are preferred, and aromatic sulfonium salts are particularly preferred.
[0075] The counter ion of the onium salt is, for example, tetrafluoroborate (BF 4 - ), hexafluorophosphate (PF 6 - ), hexafluoroantimonate (SbF 6 - ), hexafluoroarsenate (AsF 6 - ), hexachloroantimonate (SbCl 6 - ), tetraphenylborate, tetrakis(trifluoromethylphenyl)borate, tetrakis(pentafluoromethylphenyl)borate, fluoroalkyl fluorophosphate, perchlorate ion (ClO4 - ), trifluoromethanesulfonate ion (CF 3 SO 3 - ), fluorosulfonate ion (FSO 3 - ), toluenesulfonate ion, trinitrobenzenesulfonate ion, and trinitrotoluenesulfonate ion.
[0076] The weight ratio of the photoacid generator to the alkali-soluble resin is not particularly limited, but is, for example, from 0.01 to 0.1.
[0077] The photosensitive resin composition of the present embodiment may further contain a pigment, which enhances the light shielding properties of the cured product of the photosensitive resin composition of the present embodiment.
[0078] The pigment may be an organic pigment, but is preferably an inorganic pigment from the viewpoint of the heat resistance of the cured product of the photosensitive resin composition of this embodiment.
[0079] Examples of organic pigments include anthraquinone-based black pigments, perylene-based black pigments, azo-based black pigments, and lactam-based black pigments. Among these, perylene-based black pigments and lactam-based black pigments are preferred from the viewpoint of light shielding properties.
[0080] Examples of inorganic pigments include composite metal oxide pigments, carbon black, black low-order titanium oxynitride, titanium oxide, barium sulfate, zinc white, lead sulfate, yellow lead, red ocher, ultramarine, Prussian blue, chromium oxide, antimony white, iron black, red lead, zinc sulfide, cadmium yellow, cadmium red, zinc, manganese purple, cobalt purple, barium sulfate, and magnesium carbonate.
[0081] The weight ratio of the pigment to the alkali-soluble resin is preferably 0.01 to 0.30, more preferably 0.015 to 0.2. When the weight ratio of the pigment to the alkali-soluble resin is 0.01 or more, the light shielding property of the cured product of the photosensitive resin composition of this embodiment is high, and when it is 0.30 or less, the film formability of the photosensitive resin composition of this embodiment is high.
[0082] The optical density (OD value) per 30 μm of the film thickness of the cured product of the photosensitive resin composition of this embodiment is preferably 0.8 to 1.1, and more preferably 0.9 to 1.0. When the optical density (OD value) per 30 μm of the film thickness of the cured product of the photosensitive resin composition of this embodiment is 0.8 or more, the light shielding property of the cured product of the photosensitive resin composition of this embodiment is high, and when it is 1.1 or less, the film formability of the photosensitive resin composition of this embodiment is high.
[0083] The compressive strength of the cured product of the photosensitive resin composition of this embodiment is 100 N / mm 2 It is preferable that the resistance is 150N / mm or more. 2 It is more preferable that the compressive strength of the cured product of the photosensitive resin composition of the present embodiment is 100 N / mm 2 As described above, when a semiconductor device is manufactured using a cured product of the photosensitive resin composition of this embodiment as a frame-shaped member, it is easy to seal with resin by a transfer molding method, as described later.
[0084] The photosensitive resin composition of the present embodiment may further contain a polyfunctional epoxy compound as a reactive diluent.
[0085] The polyfunctional epoxy compound has a plurality of epoxy groups, and preferably has a plurality of alicyclic epoxy groups.
[0086] Commercially available polyfunctional epoxy compounds having multiple alicyclic epoxy groups include, for example, Celloxide 2021P (3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexanecarboxylate), Celloxide 2081 (ε-caprolactone-modified 3',4'-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate) (all manufactured by Daicel), bis(3,4-epoxycyclohexylmethyl)adipate, X-40-2669 (epoxy-modified linear siloxane compound), and KR-470 (epoxy-modified cyclic siloxane compound) (all manufactured by Shin-Etsu Chemical).
[0087] The content of the reactive diluent in the total solid content of the photosensitive resin composition of the present embodiment is not particularly limited, but is, for example, from 1% by weight to 50% by weight.
[0088] The photosensitive resin composition of the present embodiment may further contain a solvent.
[0089] The solvent is not particularly limited, but examples thereof include hydrocarbon solvents such as benzene, toluene, hexane, and heptane; ether solvents such as tetrahydrofuran, 1,4-dioxane, 1,3-dioxolane, and diethyl ether; ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; glycol solvents such as propylene glycol-1-monomethyl ether-2-acetate (PGMEA), diethylene glycol dimethyl ether, diethylene glycol ethyl methyl ether, and ethylene glycol diethyl ether; and halogen-based solvents such as chloroform, methylene chloride, and 1,2-dichloroethane. From the viewpoint of the film formation stability of the photosensitive resin composition of this embodiment, propylene glycol-1-monomethyl ether-2-acetate and diethylene glycol dimethyl ether are preferred.
[0090] The photosensitive resin composition of the present embodiment may further contain additives such as a sensitizer, a polymer dispersant, a thermoplastic resin, a filler, an adhesion improver, a silane coupling agent, an anti-degradation agent, a radical inhibitor, a release agent, a flame retardant, a flame retardant auxiliary, a surfactant, an antifoaming agent, an emulsifier, a leveling agent, an anti-repellent agent, an ion trapping agent, a thixotropy imparting agent, a tackifier, a storage stability improver, an ozone deterioration inhibitor, a light stabilizer, a thickener, a plasticizer, an antioxidant, a heat stabilizer, an electrical conductivity imparting agent, an antistatic agent, a radiation shielding agent, a nucleating agent, a phosphorus-based peroxide decomposer, a lubricant, a metal deactivator, a thermal conductivity imparting agent, and a physical property adjuster.
[0091] (Transparent substrate with frame-shaped member) FIG. 1 shows an example of a transparent substrate with a frame-shaped member of this embodiment.
[0092] The transparent substrate 10 with a frame-shaped member has a frame-shaped member 12 disposed on a transparent substrate 11 .
[0093] The material constituting the transparent substrate 11 is not particularly limited, but may be, for example, glass.
[0094] The frame-shaped member 12 is a cured product of the photosensitive resin composition of this embodiment, and is patterned by a known method (see, for example, Patent Document 2). The frame-shaped member 12 is patterned, for example, through a coating step, a pre-baking step, an exposure step, an alkali developing step, and a post-baking step. Specifically, the cured product of the photosensitive resin composition of this embodiment is patterned on a large-sized transparent substrate, and then the substrate is divided into individual pieces, thereby obtaining the transparent substrate 10 with the frame-shaped member.
[0095] The shape of the frame member 12 when viewed from above is not particularly limited, but may be, for example, a rectangular shape.
[0096] (Semiconductor Device) FIG. 2 shows an example of the semiconductor device of this embodiment.
[0097] The semiconductor device 20 includes a transparent substrate 10 with a frame-shaped member and a semiconductor substrate 22 on which a light-receiving element (photoelectric conversion element) 21 is mounted. Here, the transparent substrate 10 with a frame-shaped member (transparent substrate 11) is disposed facing the semiconductor substrate 22, and the frame-shaped member 12 is disposed around the light-receiving element 21. At this time, the transparent substrate 10 with a frame-shaped member is fixed to the semiconductor substrate 22 by an adhesive. The semiconductor substrate 22 on which the light-receiving element 21 is mounted is fixed to the wiring substrate 23 by a die-bonding material. Electrode pads 24 and 25 are provided on the semiconductor substrate 22 and the wiring substrate 23, respectively, and are electrically connected via a bonding wire 26. At this time, the electrode pad 24 is electrically connected to the light-receiving element 21, and the bonding wire 26 is sealed with a resin 27.
[0098] The light receiving element 21 may be, for example, an imaging element such as a CMOS image sensor or a CCD image sensor.
[0099] The semiconductor substrate 22 may be, for example, an image sensor substrate.
[0100] Examples of the adhesive include an epoxy adhesive and an acrylic adhesive.
[0101] The die bond material may be, for example, a thermosetting resin such as an epoxy resin or a silicone resin.
[0102] The wiring board 23 is a multi-layer wiring board in which vias and solder balls are formed.
[0103] The resin 27 may be, for example, a thermosetting resin such as an epoxy resin, an acrylic resin, or a silicone resin.
[0104] Next, an example of a method for manufacturing the semiconductor device 20 will be described. First, a semiconductor substrate 22 on which a plurality of light receiving elements 21 are mounted is fixed to a large wiring board, and then a plurality of transparent substrates 10 with frame-shaped members are fixed to each semiconductor substrate 22. Next, a resin 27 is supplied to the cavity by a transfer molding method to seal the bonding wires 26 (see, for example, Patent Document 1), and then the semiconductor device 20 is divided into individual pieces.
[0105] The semiconductor device 20 can be applied to imaging devices such as digital cameras and smartphones.
[0106] FIG. 3 shows another example of the semiconductor device according to this embodiment.
[0107] The semiconductor device 30 is similar to the semiconductor device 20, except that the transparent substrate 10 with the frame-shaped member is turned upside down, and a frame-shaped spacer 31 is disposed around the light receiving element 21 between the transparent substrate 11 and the semiconductor substrate 22. At this time, the spacer 31 is formed by patterning a thermosetting resin composition. The transparent substrate 11 is fixed to the spacer 31 by an adhesive.
[0108] The method for patterning the spacers 31 is not particularly limited, but examples thereof include a dispensing method, a screen printing method, and a 3D printing method.
[0109] The thermosetting resin constituting the thermosetting resin composition is not particularly limited as long as it is a resin that can be cured by any heating method, and examples thereof include silicone resin, epoxy resin, alkyd resin, polyimide resin, acrylic resin, polyamide resin, polyaramid resin, and phenol resin, and two or more of them may be used in combination. Among these, from the viewpoint of the heat resistance and light resistance of the spacer 31, silicone resin, epoxy resin, and polyimide resin are preferable, and silicone-based resin is more preferable.
[0110] The thermosetting resin composition may contain an adhesion improver, a filler, an anti-aging agent, etc., as necessary.
[0111] The manufacturing method of the semiconductor device 30 is the same as the manufacturing method of the semiconductor device 20, except that a plurality of transparent substrates 10 with frame-shaped members are fixed to each semiconductor substrate 22 via spacers 31. At this time, since the frame-shaped members 12 protrude from the transparent substrate 11, adhesion of the resin 27 to the upper surface of the transparent substrate 11 is suppressed when the resin 27 is supplied to the cavity by the transfer molding method.
[0112] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and the above embodiment may be modified as appropriate within the scope of the spirit of the present invention. EXAMPLES
[0113] Examples of the present invention will be described below, but the present invention is not limited to these examples.
[0114] (Solution A containing Resin A) 40 g of diallyl isocyanuric acid and 29 g of diallyl monomethyl isocyanuric acid were dissolved in 264 g of dioxane to obtain a dissolved product.
[0115] Next, 143 μL of a xylene solution of platinum vinylsiloxane complex Pt-VTSC-3X (manufactured by Umicore Precious Metals Japan) containing 3 wt % platinum was added to the dissolved matter to obtain solution 1.
[0116] Furthermore, solution 2 was obtained by dissolving 88 g of 1,3,5,7-tetrahydrogen-1,3,5,7-tetramethylcyclotetrasiloxane in 176 g of toluene.
[0117] Then, in a nitrogen atmosphere containing 3% by volume of oxygen, solution 2 was heated to 105° C., and solution 1 was added dropwise to solution 2 over a period of 3 hours. After completion of the dropwise addition, the mixture was maintained for 30 minutes to obtain solution 3.
[0118] The reaction rate of the alkenyl group in the compound in solution 3 is 1 The reaction rate was determined to be 95% or more by 1 H-NMR.
[0119] Furthermore, solution 4 was obtained by dissolving 62 g of 1-vinyl-3,4-epoxycyclohexane in 62 g of toluene.
[0120] Then, in a nitrogen atmosphere containing 3% by volume of oxygen, solution 3 was heated to 105° C., and solution 4 was added dropwise to solution 3 over one hour in that state. After completion of the addition, the mixture was maintained for 30 minutes to obtain solution 5.
[0121] After confirming in the same manner as above that the reaction rate of the alkenyl groups in the compound contained in solution 5 was 95% or more, solution 5 was cooled to terminate the reaction.
[0122] Next, the solvents (toluene and dioxane) were distilled off from Solution 5 under reduced pressure to obtain a solid content, and then propylene glycol-1-monomethyl ether-2-acetate was added to the solid content to obtain Solution A containing Resin A.
[0123] Resin A is a polysiloxane compound having an alkali-soluble group represented by the above formula (Ia), an alicyclic epoxy group, and a cyclic siloxane structure. Solution A is colorless and transparent, and contains 70% by weight of Resin A.
[0124] Example 1 Photosensitive resin composition A, sample B, and sample C were prepared as follows.
[0125] (Photosensitive resin composition A) 143g of solution A (100g of resin A), 30g of reactive diluent (multifunctional epoxy compound) CELLOXIDE 2081 (manufactured by DAICEL), 1.0g of photoacid generator (aromatic sulfonium salt) CPI-310FG (manufactured by SAN-APRO), 30g of 1,2-epoxidized polybutadiene BF-1000 (manufactured by ADEKA), and 21.8g of propylene glycol monomethyl ether acetate (manufactured by KH NEOCHEM) were mixed to obtain photosensitive resin composition A. Here, BF-1000 has a number average molecular weight of 1300 and an epoxy equivalent of 200g / eq.
[0126] (Sample B) Photosensitive resin composition A was applied to the surface of a glass substrate using a spin coater, and then dried using a hot plate at 80°C for 10 minutes and 120°C for 10 minutes to form a coating film with a thickness of 30 μm. Then, using a manual exposure machine (manufactured by Dai Nippon Kagaku Kenkyusho) equipped with a high-pressure mercury lamp, the coating film was exposed to an exposure dose of 2000 mJ / cm by soft contact exposure through a soda glass photomask designed to form a lattice pattern with a line width of 150 μm. 2 The coating film was exposed under the above conditions. The exposed coating film was heated on a hot plate heated to 120°C for 5 minutes. The heated coating film was left for 1 minute, and then immersed in an alkaline developer for 5 minutes. Here, the alkaline developer had a tetramethylammonium hydroxide (TMAH) content of 2.38% by weight. The coating film immersed in the alkaline developer was then washed with water for 30 seconds. Next, moisture on the surface of the washed coating film was removed with compressed air. Then, the coating film from which moisture had been removed was heated on a hot plate heated to 200°C for 30 minutes to cure the exposed portion of the coating film, thereby forming a lattice-shaped pattern of the cured product of the photosensitive resin composition A. The glass substrate on which the lattice-shaped pattern of the cured product of the photosensitive resin composition A was formed was cut using a dicing device to obtain individual pieces of sample B (9.5 mm x 9.0 mm).
[0127] (Sample C) Photosensitive resin composition A was applied to the surface of a glass substrate using a spin coater, and then dried using a hot plate at 80°C for 10 minutes and at 120°C for 10 minutes to form a coating film with a thickness of 30 μm. Then, using a manual exposure machine (manufactured by Dai Nippon Kagaku Kenkyusho) equipped with a high-pressure mercury lamp, the coating film was exposed to light at a dose of 2000 mJ / cm. 2The entire surface of the coating film was exposed under the above conditions. The exposed coating film was heated on a hot plate heated to 120°C for 5 minutes. The heated coating film was left for 1 minute, and then immersed in an alkaline developer for 5 minutes. Here, the alkaline developer had a tetramethylammonium hydroxide (TMAH) content of 2.38% by weight. The coating film immersed in the alkaline developer was then washed with water for 30 seconds. Next, moisture on the surface of the washed coating film was removed with compressed air. Then, the coating film from which moisture had been removed was heated on a hot plate heated to 200°C for 30 minutes to harden the coating film, thereby forming a cured product of the photosensitive resin composition A. The glass substrate on which the cured product of the photosensitive resin composition A had been formed was cut using a dicing device to obtain individual pieces of sample C (9.5 mm x 9.0 mm).
[0128] (Examples 2 and 3) Photosensitive resin composition A, sample B, and sample C were obtained in the same manner as in Example 1, except that the amount of BF-1000 used in preparing photosensitive resin composition A was changed to 60 g and 100 g, respectively.
[0129] Example 4 Photosensitive resin composition A, sample B, and sample C were obtained in the same manner as in Example 2, except that 1.8 g of carbon black MA100 (manufactured by Mitsubishi Chemical) was added when preparing photosensitive resin composition A.
[0130] Example 5 Using the photosensitive resin composition A of Example 2, samples B and C were prepared as follows.
[0131] (Sample B) Photosensitive resin composition A was applied to the surface of a glass substrate using a spin coater, and then dried using a hot plate at 80°C for 10 minutes and 120°C for 10 minutes to form a coating film with a thickness of 30 μm. Photosensitive resin composition A was further applied to the surface of a glass substrate using a spin coater, and then dried using a hot plate at 80°C for 10 minutes and 120°C for 10 minutes to form a coating film with a thickness of 60 μm. Then, using a manual exposure machine (manufactured by Dai Nippon Kagaku Kenkyusho) equipped with a high-pressure mercury lamp, the substrate was exposed to an exposure dose of 2000 mJ / cm by soft contact exposure through a soda glass photomask designed to form a lattice pattern with a line width of 150 μm. 2 The coating film was exposed under the above conditions. The exposed coating film was heated on a hot plate heated to 120°C for 5 minutes. The heated coating film was left for 1 minute, and then immersed in an alkaline developer for 8 minutes. Here, the alkaline developer had a tetramethylammonium hydroxide (TMAH) content of 2.38% by weight. The coating film immersed in the alkaline developer was then washed with water for 30 seconds. Next, moisture on the surface of the washed coating film was removed with compressed air. Then, the coating film from which moisture had been removed was heated on a hot plate heated to 200°C for 30 minutes to cure the exposed portion of the coating film, thereby forming a lattice-shaped pattern of the cured product of the photosensitive resin composition A. The glass substrate on which the lattice-shaped pattern of the cured product of the photosensitive resin composition A was formed was cut using a dicing device to obtain individual pieces of sample B (9.5 mm x 9.0 mm).
[0132] (Sample C) Photosensitive resin composition A was applied to the surface of a glass substrate using a spin coater, and then dried using a hot plate at 80°C for 10 minutes and 120°C for 10 minutes to form a coating film with a thickness of 30 μm. Photosensitive resin composition A was further applied to the surface of a glass substrate using a spin coater, and then dried using a hot plate at 80°C for 10 minutes and 120°C for 10 minutes to form a coating film with a thickness of 60 μm. Then, a manual exposure machine (manufactured by Dai Nippon Kagaku Kenkyusho) equipped with a high-pressure mercury lamp was used to expose the coating film to a thickness of 2000 mJ / cm. 2The entire surface of the coating film was exposed under the above conditions. The exposed coating film was heated on a hot plate heated to 120°C for 5 minutes. The heated coating film was left for 1 minute, and then immersed in an alkaline developer for 8 minutes. Here, the alkaline developer had a tetramethylammonium hydroxide (TMAH) content of 2.38% by weight. The coating film immersed in the alkaline developer was then washed with water for 30 seconds. Next, moisture on the surface of the washed coating film was removed with compressed air. Then, the coating film from which moisture had been removed was heated on a hot plate heated to 200°C for 30 minutes to harden the coating film, thereby forming a cured product of the photosensitive resin composition A. The glass substrate on which the cured product of the photosensitive resin composition A had been formed was cut using a dicing device to obtain individual pieces of sample C (9.5 mm x 9.0 mm).
[0133] Example 6 Using the photosensitive resin composition A of Example 4, Samples B and C were prepared in the same manner as in Example 5.
[0134] (Examples 7, 9, and 11) Photosensitive resin composition A, sample B, and sample C were obtained in the same manner as in Example 1, except that BF-1000 was changed to JP100, JP200 (both manufactured by Nippon Soda), and RICON657 (manufactured by Cray Valley), respectively.
[0135] Here, JP100 has a number average molecular weight of 2200 and an epoxy equivalent of 190 to 210 g / eq. JP200 has a number average molecular weight of 1300 and an epoxy equivalent of 210 to 240 g / eq. RICON657 has a number average molecular weight of 3200 and an epoxy equivalent of 160 g / eq.
[0136] (Examples 8, 10, and 12) Photosensitive resin composition A, sample B, and sample C were obtained in the same manner as in Example 1, except that BF-1000 was changed to JP100, JP200 (both manufactured by Nippon Soda), and RICON657 (manufactured by Cray Valley), respectively.
[0137] (Comparative Examples 1 and 2) Photosensitive resin composition A, sample B, and sample C were obtained in the same manner as in Examples 1 and 4, respectively, except that BF-1000 was not added when photosensitive resin composition A was prepared.
[0138] (Comparative Examples 3 and 4) Photosensitive resin composition A, sample B, and sample C were obtained in the same manner as in Example 1, except that the amount of BF-1000 used when preparing photosensitive resin composition A was changed to 10 g and 120 g, respectively.
[0139] (Comparative Examples 5 to 7) Photosensitive resin composition A, sample B, and sample C were obtained in the same manner as in Examples 1 to 3, except that 1,4-epoxidized polybutadiene PB4700 (manufactured by Daicel) was added instead of BF-1000 when preparing photosensitive resin composition A.
[0140] Here, PB4700 has a number average molecular weight of 2,000 to 3,500.
[0141] Comparative Example 8 Photosensitive resin composition A, sample B, and sample C were obtained in the same manner as in Example 1, except that BF-1000 was not added and the amount of Celloxide 2081 was changed to 60 g.
[0142] (Number average molecular weight of epoxidized polybutadiene) Tetrahydrofuran was used as a developing solvent, and the retention time (retention volume) measured with a gel permeation chromatograph HLC8220GPC (manufactured by Tosoh Corporation) was converted based on the number average molecular weight of polystyrene to measure the number average molecular weight of the epoxidized polybutadiene.
[0143] (Developability of Photosensitive Resin Composition A) In the process of preparing sample B, the developability of photosensitive resin composition A was evaluated. Specifically, after removing the moisture on the surface of the coating film washed with water with compressed air, the presence or absence of foreign matter adhering to the glass substrate and the size of the foreign matter were confirmed at a magnification of 10 times using a 3D measuring laser microscope LEXT OLS4000 (manufactured by Olympus). The evaluation criteria for the developability of photosensitive resin composition A are as follows. A: When there are no foreign objects with a size of 50 μm or more attached to the glass substrate B: When foreign matter with a size of 50 μm or more and less than 100 μm is attached to the glass substrate C: When foreign matter with a size of 100 μm or more is attached to the glass substrate
[0144] (Heat resistance of the cured product of photosensitive resin composition A) Using a nanoindentation tester ENT-NEXUS (manufactured by Elionix), the amount of displacement of sample C due to a temperature change in the measurement environment from 40° C. to 240° C. was measured. At this time, the amount of displacement of the initial sample C and that of sample C heat-treated at 150° C. for 1 hour were measured, and the rate of change in the amount of displacement before and after the heat treatment was calculated using the following formula to evaluate the heat resistance of the cured product of photosensitive resin composition A. The closer the obtained value is to 100, the smaller the difference in the amount of displacement before and after the heat treatment and the higher the heat resistance. (Displacement of heat-treated sample C) / (Initial displacement of sample C)×100 The conditions for measuring the displacement of Sample C are as follows: Indenter approach speed: 100 nm / sec Maximum load: 3mN Load application acceleration: 0.6mN / sec Maximum load holding time: 5 seconds Unloading speed: 0.6mN / sec Stiffness calculation: When 10% of the maximum load is removed Drift measurement: When 90% of the maximum load is removed
[0145] (Compressive strength of cured product of photosensitive resin composition A) Using a precision press tester CYPF-10 (manufactured by Shinto Kogyo), sample B was heated and compressed to evaluate the compressive strength of the cured product of photosensitive resin composition A. Specifically, sample B was placed in a precision press tester heated to 180°C with the side on which the cured product of photosensitive resin composition A was formed facing up, and a load was applied to the cured product of photosensitive resin composition A to compress it for 3 minutes, after which the appearance of the cured product of photosensitive resin composition A was observed under a microscope. At this time, a load of 10 N / mm 2 , 50N / mm 2 , 100N / mm 2 , 150N / mm 2 , 200N / mm 2 , 250N / mm 2 , 300N / mm 2 , 350N / mm 2 The load before the load at which the appearance changed was taken as the compressive strength. 2 When the appearance does not change even if a load of >300N / mm is applied, the compressive strength is 2 In addition, when evaluating the compressive strength of the cured product of the photosensitive resin composition A, the influence of the glass substrate constituting the sample B was ignored.
[0146] (Optical Density of Cured Product of Photosensitive Resin Composition A) Using a transmission densitometer X-rite361T (manufactured by X-rite), the optical density (OD value) per 30 μm of film thickness of the cured product of the photosensitive resin composition A in the sample C was measured. The optical density was measured in accordance with ISO 5-2, and the influence of the glass substrate constituting the sample C was eliminated.
[0147] Tables 1 and 2 show the evaluation results of the developability of the photosensitive resin composition A, and the heat resistance, compressive strength, and optical density of the cured product of the photosensitive resin composition A. Note that EPB and CB stand for epoxidized polybutadiene and carbon black, respectively.
[0148] [Table 1]
[0149] [Table 2]
[0150] From Table 1, it can be seen that Examples 1 to 12 achieve both the developability of Photosensitive Resin Composition A and the heat resistance and compressive strength of the cured product of Photosensitive Resin Composition A, regardless of the presence or absence of a pigment and the thickness of the coating film.
[0151] In contrast, in Comparative Examples 1 to 3, the weight ratio of EPB to resin A is 0 or 0.10, so the compressive strength of the cured product of the photosensitive resin composition A is low. In Comparative Example 4, the weight ratio of EPB to resin A is 1.20, so the developability of the photosensitive resin composition A is low. In Comparative Examples 5 to 7, 1,4-EPB is used instead of 1,2-EPB, so the developability of the photosensitive resin composition A and the heat resistance of the cured product of the photosensitive resin composition A are low. In particular, in Comparative Examples 6 and 7, a lattice pattern could not be formed. In Comparative Example 8, an epoxy compound is used instead of EPB, so the photosensitive resin composition A is dissolved in an alkaline developer, and a lattice pattern could not be formed. [Explanation of symbols]
[0152] 10 Transparent substrate with frame-shaped member 11 Transparent substrate 12 Frame-shaped member 20, 30 Semiconductor device 21 Photodetector 22 Semiconductor substrate 23 Wiring board 24, 25 Electrode pads 26 Bonding Wire 27 Resin 31 Spacer
Claims
1. The composition comprises an alkali-soluble resin having an epoxy group, 1,2-epoxidized polybutadiene, and a photoacid generator, a weight ratio of the 1,2-epoxidized polybutadiene to the alkali-soluble resin is 0.20 or more and 1.10 or less.
2. The photosensitive resin composition according to claim 1 , wherein the alkali-soluble resin is a polysiloxane compound.
3. The photosensitive resin composition according to claim 2 , wherein the polysiloxane compound has a cyclic siloxane structure.
4. The photosensitive resin composition according to claim 1 , wherein the alkali-soluble resin has an alicyclic epoxy group and / or a glycidyl group.
5. The photosensitive resin composition according to claim 1 , wherein the alkali-soluble resin has a group represented by the following formula (Ia) and / or a group represented by the following formula (Ib): 【Chemistry 1】
6. Further comprising a pigment, 2. The photosensitive resin composition according to claim 1, wherein a weight ratio of the pigment to the alkali-soluble resin is 0.01 or more and 0.30 or less.
7. A transparent substrate with a frame-shaped member, comprising a frame-shaped member comprising the cured product of the photosensitive resin composition according to claim 1 provided on the transparent substrate.
8. A semiconductor substrate having a frame-shaped member and a light-receiving element mounted thereon, the frame-shaped member-attached transparent substrate is disposed opposite the semiconductor substrate, The frame member is disposed around the light receiving element.
9. A semiconductor substrate having a frame-shaped member and a light-receiving element mounted thereon, the transparent substrate with a frame-shaped member is disposed opposite the semiconductor substrate via a frame-shaped spacer, the spacer is disposed on an opposite side of the transparent substrate from the frame member, The spacer is disposed around the light receiving element.
Citation Information
Patent Citations
Photocurable composition
JP1986192724A
Resist resin composition and its cured body
JP1998232494A
Photosensitive adhesive composition, method for manufacturing laminated body or solid-state imaging element using the composition, and solid-state imaging element
JP2012042601A
Liquid crystal element, radiation-sensitive resin composition, spacer forming method and spacer
JP2013221954A
Photosensitive resin composition, photosensitive resin film, multilayer printed board and semiconductor package, and method for manufacturing multilayer printed board and method for producing photosensitive resin composition
JP2020166033A