Nanostructure dispersion liquid

The nanostructure dispersion liquid with controlled particle size and water-based medium addresses dispersibility and stability issues, ensuring consistent quality and preventing aggregation, particularly in storage and processing.

JP2024142191AInactive Publication Date: 2024-10-10ZEON CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023054246
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing nanostructure dispersions face challenges with dispersibility and stability, particularly in containers during storage and transportation, leading to potential aggregation and clogging issues.

Method used

A nanostructure dispersion liquid containing fibrous carbon nanostructures with a specific Z-average particle diameter of 45.0 nm to 70.0 nm, using water as the dispersion medium, and optionally including functional groups and additives, which enhances dispersion stability through controlled aggregation and clogging prevention.

Benefits of technology

The solution provides a nanostructure dispersion with improved stability, effectively suppressing aggregation and clogging, especially during storage and processing, thereby maintaining consistent dispersibility and quality for applications like electronic devices.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a nanostructure dispersion liquid excellent in dispersion stability.SOLUTION: A nanostructure dispersion liquid includes: a fibrous nanostructure whose Z-average particle diameter according to dynamic light scattering method is 45.0-70.0 nm; and a dispersion medium containing water.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a nanostructure dispersion liquid. [Background technology]

[0002] In recent years, various nanostructures such as nanocarbons, nanofibers, and nanowires have been attracting attention as materials with various excellent properties such as mechanical properties. Among them, nanocarbons, particularly fibrous carbon nanostructures such as carbon nanotubes (hereinafter sometimes referred to as "CNTs"), have been attracting attention as materials with excellent electrical conductivity, thermal conductivity, and mechanical properties.

[0003] However, nanostructures such as CNTs are fine structures with a diameter of nanometers, and therefore are difficult to handle and process when used alone. Thus, nanostructures are used for various purposes after forming an assembly in which a plurality of nanostructures are assembled into a film, or after forming a composite material by combining with a polymeric material such as resin or rubber, or a metal. As a method for forming an assembly of nanostructures, a method has been proposed in which the dispersion medium is removed from a nanostructure dispersion liquid in which nanostructures are dispersed. As a method for forming a composite material containing nanostructures, a method has been proposed in which the composite material is precipitated or sedimented from a composite material composition formed by mixing a matrix material such as a polymeric material with a nanostructure dispersion liquid.

[0004] Here, from the viewpoint of making the nanostructure aggregate and composite material exhibit excellent properties, a nanostructure dispersion liquid used for forming the aggregate and composite material is required in which the nanostructures are well dispersed in the dispersion medium. For example, Patent Document 1 discloses the finding that by filling a predetermined amount or more of the nanostructure dispersion liquid in a sealed container used for storing or transporting the nanostructure dispersion liquid, it is possible to reduce the effects of environmental changes during storage and vibrations during transport, and to prevent the dispersibility of the nanostructures from decreasing. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2017 / 115707 Summary of the Invention [Problem to be solved by the invention]

[0006] According to the technology disclosed in Patent Document 1, it is possible to provide a container containing a nanostructure dispersion liquid that can prevent the dispersibility of the nanostructures contained in the nanostructure dispersion liquid in the container from decreasing even when the container is stored or transported.

[0007] Here, in the technology disclosed in the above Patent Document 1, there is room for further improvement in the dispersibility of nanostructures in the nanostructure dispersion liquid. Therefore, an object of the present invention is to provide a nanostructure dispersion liquid having excellent dispersion stability. [Means for solving the problem]

[0008] The present inventors have conducted extensive research with the aim of solving the above problems, and have found that a nanostructure dispersion liquid containing a fibrous nanostructure having a Z-average particle size of 45.0 nm to 70.0 nm based on a dynamic light scattering method and a dispersion medium containing water has excellent dispersion stability, thereby completing the present invention.

[0009] That is, the present invention aims to advantageously solve the above problems, and [1] the nanostructure dispersion of the present invention is a nanostructure dispersion containing nanostructures and a dispersion medium, wherein the nanostructures contain fibrous carbon nanostructures having functional groups, and further, the Z-average particle size based on dynamic light scattering is 45.0 nm or more and 70.0 nm or less, and the dispersion medium contains water. A nanostructure dispersion containing nanostructures that satisfy such a predetermined Z-average particle size has excellent dispersion stability. Here, the Z-average particle size based on dynamic light scattering can be measured according to the method described in the examples of this specification. In addition, in this specification, "fibrous" refers to an aspect ratio of 10 or more.

[0010] [2] In the nanostructure dispersion liquid of the present invention, the nanostructures preferably include carbon nanotubes.

[0011] [3] In the nanostructure dispersion liquid of [2] above, the carbon nanotubes preferably include single-walled carbon nanotubes.

[0012] [4] In the nanostructure dispersion liquid of [2] or [3] above, it is preferable that the carbon nanotubes have an upwardly convex t-plot obtained from an adsorption isotherm. Effect of the Invention

[0013] According to the present invention, it is possible to provide a nanostructure dispersion liquid having excellent dispersion stability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The nanostructure dispersion of the present invention can be used for a desired purpose after being subjected to a treatment such as purification as necessary.

[0015] (Nanostructure dispersion) The nanostructure dispersion of the present invention is a nanostructure dispersion containing nanostructures and a dispersion medium, the nanostructures being fibrous carbon nanostructures having functional groups, the Z-average particle size based on dynamic light scattering being 45.0 nm to 70.0 nm, and the dispersion medium being water. A nanostructure dispersion containing nanostructures having such a predetermined Z-average particle size has excellent dispersion stability. Here, when the nanostructure dispersion of the present invention is used for a desired purpose, an ion exchange process may be carried out as necessary for the purpose of removing impurities such as metals from the nanostructure dispersion. In this ion exchange process, the nanostructure dispersion may be brought into contact with a strongly acidic ion exchange resin. In this ion exchange process, the strongly acidic ion exchange resin may be brought into contact with the nanostructure dispersion. If the nanostructure dispersion used in the ion exchange process has excellent dispersion stability, it is possible to effectively suppress the aggregation of the nanostructures and the clogging of the ion exchange resin by the nanostructures in the ion exchange process.

[0016] The nanostructure dispersion liquid contains nanostructures and a dispersion medium, and may further contain optional additives such as dispersants, molecular additives, ionic particles, etc. Each component contained in the nanostructure dispersion liquid will be described below in order.

[0017] <Nanostructures> The nanostructure must include a fibrous carbon nanostructure having a functional group, and must have a Z-average particle size based on dynamic light scattering of 45.0 nm or more and 70.0 nm or less.

[0018] Examples of nanostructures include, but are not limited to, nanocarbons such as fullerene, graphene, and fibrous carbon nanostructures, nanofibers such as cellulose nanofibers, nanowires such as silver nanowires, and boron nitride nanotubes. These may be used alone or in combination of two or more.

[0019] Among the above, the nanostructure is preferably a nanocarbon, and more preferably a fibrous carbon nanostructure. Here, the fibrous carbon nanostructure is not particularly limited, and examples thereof include carbon nanotubes, carbon nanofibers, carbon nanohorns, and vapor-grown carbon fibers. These may be used alone or in combination of two or more. Among them, it is more preferable to use carbon nanotubes as the fibrous carbon nanostructure. This is because carbon nanotubes have excellent electrical conductivity, thermal conductivity, and mechanical properties.

[0020] Here, the carbon nanotubes that can be suitably used as the nanostructure may consist of carbon nanotubes alone, or may be a mixture of carbon nanotubes and fibrous carbon nanostructures other than carbon nanotubes. The carbon nanotube is not particularly limited, and single-walled carbon nanotubes and / or multi-walled carbon nanotubes can be used, but the carbon nanotubes are preferably single-walled to five-walled carbon nanotubes, and more preferably single-walled carbon nanotubes, because single-walled carbon nanotubes are superior in electrical conductivity, thermal conductivity, and mechanical properties compared to multi-walled carbon nanotubes.

[0021] In addition, as the fibrous carbon nanostructure, it is preferable to use a carbon nanostructure having a ratio (3σ / Av) of the value (3σ) obtained by multiplying the standard deviation (σ) of the diameter by 3 to the average diameter (Av) of more than 0.20 and less than 0.60, more preferably a carbon nanostructure having a 3σ / Av of more than 0.25, and even more preferably a carbon nanostructure having a 3σ / Av of more than 0.50. This is because the fibrous carbon nanostructure having a 3σ / Av of more than 0.20 and less than 0.60 has excellent electrical conductivity, thermal conductivity, and mechanical properties. The "average diameter (Av) of fibrous carbon nanostructures" and the "standard deviation of diameters of fibrous carbon nanostructures (σ: sample standard deviation)" can each be determined by measuring the diameter (outer diameter) of 100 randomly selected fibrous carbon nanostructures using a transmission electron microscope. The average diameter (Av) and standard deviation (σ) of the fibrous carbon nanostructures may be adjusted by changing the manufacturing method or manufacturing conditions of the fibrous carbon nanostructures, or by combining multiple types of fibrous carbon nanostructures obtained by different manufacturing methods.

[0022] The fibrous carbon nanostructures that are usually used are those that show a normal distribution when the diameter measured as described above is plotted on the horizontal axis and the frequency on the vertical axis and approximated with a Gaussian.

[0023] Furthermore, the fibrous carbon nanostructure preferably has a radial breathing mode (RBM) peak when evaluated by Raman spectroscopy. Note that the Raman spectrum of a fibrous carbon nanostructure consisting only of multi-walled carbon nanotubes having three or more walls does not have an RBM.

[0024] Furthermore, the fibrous carbon nanostructure preferably has a ratio of G band peak intensity to D band peak intensity in a Raman spectrum (G / D ratio) of 1 to 20. This is because a fibrous carbon nanostructure having a G / D ratio of 1 to 20 has excellent electrical conductivity, thermal conductivity and mechanical properties.

[0025] Furthermore, the average diameter (Av) of the fibrous carbon nanostructures is preferably 0.5 nm or more, more preferably 1 nm or more, and preferably 15 nm or less, and more preferably 10 nm or less. If the average diameter (Av) of the fibrous carbon nanostructures is 0.5 nm or more, the aggregation of the fibrous carbon nanostructures can be suppressed and the dispersibility of the fibrous carbon nanostructures in the dispersion liquid can be increased. In addition, the fibrous carbon nanostructures having an average diameter (Av) of 15 nm or less have excellent electrical conductivity, thermal conductivity and mechanical properties.

[0026] Furthermore, the BET specific surface area of ​​the fibrous carbon nanostructure is 400m 2 / g or more, and 2 / g or more is more preferable, and 2500m 2 / g or less, and 2 / g or less. 2 This is because the fibrous carbon nanostructures with a BET specific surface area of ​​2500 m / g or more have excellent electrical conductivity, thermal conductivity and mechanical properties. 2 If the molecular weight is 1 / g or less, the dispersibility of the fibrous carbon nanostructure in the dispersion liquid can be further improved. In the present invention, the term "BET specific surface area" refers to a nitrogen adsorption specific surface area measured by the BET method.

[0027] Furthermore, the fibrous carbon nanostructure preferably has a plurality of micropores. The fibrous carbon nanostructure preferably has micropores with a pore diameter of less than 2 nm, and the amount of the micropores is preferably 0.40 mL / g or more, more preferably 0.43 mL / g or more, and the upper limit is usually about 0.65 mL / g, as determined by the following method. When the fibrous carbon nanostructure has the above-mentioned micropores, the aggregation of the fibrous carbon nanostructure in the dispersion liquid is suppressed, and the dispersibility of the fibrous carbon nanostructure in the dispersion liquid can be further improved. The micropore volume can be adjusted, for example, by appropriately changing the preparation method and preparation conditions of the fibrous carbon nanostructure. Here, the "micropore volume (Vp)" can be calculated by measuring the nitrogen adsorption isotherm of the fibrous carbon nanostructure at the liquid nitrogen temperature (77K), and using the amount of nitrogen adsorption at a relative pressure P / P0 = 0.19 as V, from the formula (I): Vp = (V / 22414) × (M / ρ). Note that P is the measurement pressure at the time of adsorption equilibrium, P0 is the saturated vapor pressure of liquid nitrogen at the time of measurement, and in the formula (I), M is the molecular weight of the adsorbate (nitrogen) of 28.010, and ρ is the density of the adsorbate (nitrogen) at 77K of 0.808 g / cm. 3The micropore volume can be determined, for example, by using "BELSORP (registered trademark)-mini" (manufactured by BEL Japan Co., Ltd.).

[0028] In addition, it is preferable that the fibrous carbon nanostructure has a t-plot obtained from the adsorption isotherm that shows an upwardly convex shape. In particular, it is more preferable that the fibrous carbon nanostructure has not been subjected to an opening treatment and shows an upwardly convex t-plot. This is because the fibrous carbon nanostructure showing an upwardly convex t-plot has excellent electrical conductivity, thermal conductivity, and mechanical properties. The "t-plot" can be obtained by converting the relative pressure into the average thickness t (nm) of the nitrogen gas adsorption layer in the adsorption isotherm of the fibrous carbon nanostructure measured by the nitrogen gas adsorption method. That is, the t-plot of the fibrous carbon nanostructure can be obtained by determining the average thickness t of the nitrogen gas adsorption layer corresponding to the relative pressure from a known standard isotherm in which the average thickness t of the nitrogen gas adsorption layer is plotted against the relative pressure P / P0, and performing the above conversion (t-plot method by de Boer et al.).

[0029] Here, in a material having pores on the surface, the growth of a nitrogen gas adsorption layer is classified into the following processes (1) to (3). The slope of the t-plot changes depending on the processes (1) to (3) below. (1) The process of forming a monolayer of nitrogen molecules on the entire surface (2) Formation of multilayer adsorption and the associated capillary condensation filling process in the pores (3) The formation of multilayer adsorption on an apparently non-porous surface whose pores are filled with nitrogen

[0030] In the t-plot showing an upward convex shape, the plot is located on a straight line passing through the origin in the region where the average thickness t of the nitrogen gas adsorption layer is small, whereas as t increases, the plot shifts downward from the straight line. Fibrous carbon nanostructures having such a t-plot shape have a large ratio of the internal specific surface area to the total specific surface area of ​​the fibrous carbon nanostructure, indicating that a large number of openings are formed in the carbon nanostructures that make up the fibrous carbon nanostructure.

[0031] Furthermore, the inflection point of the t-plot of the fibrous carbon nanostructure is preferably in the range satisfying 0.2≦t(nm)≦1.5, more preferably in the range of 0.45≦t(nm)≦1.5, and even more preferably in the range of 0.55≦t(nm)≦1.0. The "position of the bending point" is the intersection of the approximation line A in the above-mentioned process (1) and the approximation line B in the above-mentioned process (3).

[0032] Furthermore, the fibrous carbon nanostructure preferably has a ratio (S2 / S1) of the internal specific surface area S2 to the total specific surface area S1 obtained from a t-plot of 0.05 or more and 0.30 or less. The total specific surface area S1 and the internal specific surface area S2 of the fibrous carbon nanostructure are not particularly limited. 2 / g or more 2500m 2 / g or less, and 2 / g or more 1200m 2 / g or less. 2 / g or more 540m 2 It is preferable that the molecular weight is not more than 1 / g. Here, the total specific surface area S1 and the internal specific surface area S2 of the fibrous carbon nanostructure can be obtained from the t-plot. Specifically, first, the total specific surface area S1 can be obtained from the slope of the approximation line in step (1), and the external specific surface area S3 can be obtained from the slope of the approximation line in step (3). Then, the internal specific surface area S2 can be calculated by subtracting the external specific surface area S3 from the total specific surface area S1.

[0033] Incidentally, the measurement of the adsorption isotherm of the fibrous carbon nanostructure, the creation of t-plots, and the calculation of the total specific surface area S1 and the internal specific surface area S2 based on the analysis of the t-plots can be performed, for example, using a commercially available measuring device, "BELSORP (registered trademark)-mini" (manufactured by BEL Japan Co., Ltd.).

[0034] The fibrous carbon nanostructure having a functional group can be efficiently produced by acid treatment of the fibrous carbon nanostructure produced by the method that can be called the super growth method disclosed in International Publication No. 2006 / 011655. The above-mentioned preferred attributes described for the fibrous carbon nanostructure, particularly the number of layers of CNT, 3σ / Av, the plot shape when the plot obtained by taking the diameter on the horizontal axis and the frequency on the vertical axis is Gaussian-approximated, the peak position and G / D ratio of the Raman spectrum, the average diameter (Av), the BET specific surface area, and the micropore volume, are also applicable to the fibrous carbon nanostructure having a functional group. In the super growth method, when a raw material compound and a carrier gas are supplied onto a substrate having a catalyst layer for producing carbon nanotubes on its surface to synthesize CNTs by chemical vapor deposition (CVD), a trace amount of an oxidizing agent (catalyst activation material) is present in the system, thereby dramatically improving the catalytic activity of the catalyst layer. Hereinafter, the carbon nanotubes as the above-mentioned fibrous carbon nanostructures obtained by the super-growth method may be referred to as "SGCNTs".

[0035] The fibrous carbon nanostructure may be composed of only SGCNTs, or may be composed of SGCNTs and non-cylindrical carbon nanostructures. Specifically, the fibrous carbon nanostructure may include a single-layer or multi-layer flat cylindrical carbon nanostructure (sometimes called "graphene nanotape (GNT)") having tape-shaped portions over its entire length in which the inner walls are close to or bonded to each other.

[0036] The functional group of the fibrous carbon nanostructure having a functional group may be selected from the group consisting of a hydroxyl group, an aldehyde group, a carbonyl group, and a carboxyl group. The method for introducing these functional groups into the fibrous carbon nanostructure is not particularly limited, and any method can be used. For example, the fibrous carbon nanostructure can be oxidized with an oxidizing acid such as nitric acid to form the above-mentioned functional group on the fibrous carbon nanostructure. If the fibrous carbon nanostructure has a functional group, it is possible to improve the dispersibility in the dispersion liquid. In addition, whether or not the fibrous carbon nanostructure has a functional group can be determined by quantitatively analyzing the amount of oxygen element by X-ray photoelectron spectroscopy (XPS) on the solid content after solid-liquid separation of the dispersion liquid.

[0037] For example, the method of oxidizing the fibrous carbon nanostructure with nitric acid is not particularly limited, but may be, for example, a method of mixing an oxidizing acid such as nitric acid with the fibrous carbon nanostructure to obtain a mixture, and reacting the mixture with stirring for 1 hour to 13 hours at a temperature condition of 83°C to 120°C. Thereafter, it is preferable to carry out a step (purification step) of removing impurities by filtration such as cross-flow filtration while adjusting the pH to about pH 7.0, after optionally adding water or the like to reduce the acid concentration. The temperature during the purification step is not particularly limited, but may be 20°C to 35°C.

[0038] In the above purification step, metal impurities that are inevitably mixed in during the production of nanostructures can be removed. Here, examples of metal impurities include metal catalysts used during the production of nanostructures, such as alkali metals, alkaline earth metals, metal elements belonging to groups 3 to 13, and lanthanoids, metal elements such as Si, Sb, As, Pb, Sn, and Bi, and metal compounds containing these. More specifically, examples of metal elements include Al, Sb, As, Ba, Be, Bi, B, Cd, Ca, Cr, Co, Cu, Ga, Ge, Fe, Pb, Li, Mg, Mn, Mo, Ni, K, Na, Sr, Sn, Ti, W, V, Zn, and Zr, and metal compounds containing these. The concentration of metal impurities in the fibrous carbon nanostructures having functional groups is 1×10 from the viewpoint of further increasing the dispersion stability of the dispersion liquid. 18 atoms / cm 3 Preferably less than 15 x 10 10 atoms / cm 3 It is more preferable that it is less than 1000 .mu.m. The concentration of metal impurities can be measured, for example, by a transmission electron microscope (TEM), a scanning electron microscope (SEM), an energy dispersive X-ray analyzer (EDAX), a gas phase decomposition apparatus, and an inductively coupled plasma (ICP) mass spectrometry (VPD, ICP / MS), but since this method allows for high accuracy, it is usually used for measurement by inductively coupled plasma (ICP / MS).

[0039] The Z-average particle size of the nanostructure based on the dynamic light scattering method must be 45.0 nm to 70.0 nm, preferably 45.1 nm to 69.5 nm, and more preferably 45.2 nm to 69.0 nm. If the Z-average particle size of the nanostructure based on the dynamic light scattering method is within the above range, the generation of aggregates in the dispersion can be effectively suppressed, and the dispersion stability is excellent.

[0040] <Dispersion medium> The dispersion medium for dispersing the nanostructure is not particularly limited, and examples thereof include water; alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, t-butanol, pentanol, hexanol, heptanol, octanol, nonanol, decanol, amyl alcohol, methoxypropanol, propylene glycol, and ethylene glycol; ketones such as acetone, methyl ethyl ketone, and cyclohexanone; ethyl acetate, butyl acetate, ethyl lactate, esters of α-hydroxycarboxylic acids, and benzyl benzoate. Examples of the solvent include esters such as benzyl benzoate; ethers such as diethyl ether, dioxane, tetrahydrofuran, and monomethyl ether; amide-based polar organic solvents such as N,N-dimethylformamide, dimethyl sulfoxide, dimethylacetamide, and N-methylpyrrolidone; aromatic hydrocarbons such as toluene, xylene, chlorobenzene, orthodichlorobenzene, and paradichlorobenzene; salicylaldehyde, dimethyl sulfoxide, 4-methyl-2-pentanone, N-methylpyrrolidone, γ-butyrolactone, and tetramethylammonium hydroxide. Among these, water and dimethylacetamide are preferred, and water is more preferred, from the viewpoint of particularly excellent dispersibility of nanostructures. These may be used alone or in combination of two or more.

[0041] <Additives> Additives that can be optionally blended into the nanostructure dispersion include, but are not limited to, dispersants, molecular additives, and pH adjusters. Examples of dispersants and molecular additives include, but are not limited to, those described in International Publication No. 2017 / 115707. Examples of pH adjusters include, but are not limited to, ammonia water and ammonium nitrate water. For example, from the viewpoint of improving the characteristics (particularly, conductivity, etc.) of an electronic device formed using the nanostructure dispersion liquid, it is preferable that the concentration of the additive contained in the nanostructure dispersion liquid be 1 mass % or less.

[0042] <pH of nanostructure dispersion> The pH of the nanostructure dispersion is preferably 5.5 or more, preferably 8.0 or less, and more preferably 7.5 or less. If the pH of the nanostructure dispersion is 5.5 or more, the dispersion stability of the nanostructures can be improved. As a result, when an electronic device is manufactured using the nanostructure dispersion, the quality of the obtained electronic device can be improved. In addition, if the pH of the nanostructure dispersion is 7.5 or less even at the manufacturing stage, for example, the elution of metal components from a ceramic filtration membrane or the like used in the process of manufacturing the nanostructure dispersion can be suppressed, and the amount of metal as an impurity contained in the nanostructure dispersion can be reduced. As a result, the quality of the obtained electronic device can be improved.

[0043] <Method of preparing nanostructure dispersion> The nanostructure dispersion liquid can be prepared through a step (dispersion step) of dispersing a mixture containing fibrous carbon nanostructures having functional groups as nanostructures, a dispersion medium, and any additives to obtain a dispersion liquid. Furthermore, the dispersion liquid obtained through the dispersion step is filled into a sealed container as necessary (filling step). Then, the dispersion liquid filled into the sealed container is subjected to a dispersion treatment as necessary (dispersion step of container-filled dispersion liquid). Here, the dispersion liquid filled into the sealed container can be stored in that state for a predetermined period of time (storage step). As described above, the filling step, the container-filled dispersion step, and the storage step are optional steps. Among them, only one of the filling step, the container-filled dispersion step, and the storage step may be performed, or both may be performed. When both the container-filled dispersion step and the storage step are performed, the order of performing these steps is not particularly limited, and (i) the container-filled dispersion step may be performed immediately after the filling step and then the storage step, or (ii) the container-filled dispersion step may be performed after the storage step. Furthermore, in the above case (i), the container-filled dispersion step may be further performed after the storage step.

[0044] In the dispersion step, a mixture containing a fibrous carbon nanostructure having a functional group, a dispersion medium, and an optional additive is dispersed to obtain a dispersion liquid. It is preferable to adopt a dispersion method without any particular limitation. The dispersion temperature at this time may be, for example, 5°C or more and 35°C or less from the viewpoint of improving dispersibility. In addition, the dispersion time is preferably 0.5 hours or more and 4 hours or less from the viewpoint of improving dispersibility and dispersion stability. By setting the dispersion time within the above range, the Z-average particle size of the nanostructure based on the dynamic light scattering method can be appropriately controlled.

[0045] In the filling step, the dispersion liquid obtained through the dispersing step is filled into a sealed container as necessary. As the sealed container, it is preferable to use a container whose inner surface portion that comes into contact with the dispersion liquid is formed of a resin. The resin preferably contains at least one selected from high-density polyethylene, low-density polyethylene, polystyrene, polypropylene, and fluororesins. Among them, fluororesins such as polytetrafluoroethylene (PTFE), fluorinated ethylene propylene (FEP), perfluoroalkoxyalkane (PFA), ethylene tetrafluoroethylene (ETFE), chlorotrifluoroethylene (CTFE), and polyvinylidene fluoride (PVDF) are more preferable, and ETFE and PVDF are particularly preferable. By storing the dispersion liquid in a sealed container whose inner surface portion is made of at least one of the above resins, it is possible to effectively suppress the aggregation of the fibrous carbon nanostructures having functional groups, and as a result, it is possible to further increase the dispersion stability of the dispersion liquid. In this specification, "high-density polyethylene" refers to a polyethylene having a density of 942 kg / m 3 "Low density polyethylene" means polyethylene with a density of 910 kg / m 3 More than 930kg / m 3The term "polyethylene having a thickness of less than 100 mm" means polyethylene having a thickness of less than 100 mm. In addition, "at least the inner surface portion" of the sealed container is made of at least one of the specified resins, and includes not only the case where the entire sealed container is made of the specified resin, but also the case where the inner surface of the sealed container is lined with the specified resin. In this case, the material constituting the sealed container body (e.g., exterior) is not particularly limited, and may be glass or metal. The shape of the sealed container is not particularly limited, and may be any sealed container having, for example, an injection port that can be sealed after being filled with the nanostructure dispersion. Specifically, the sealed container may be, for example, a bottle with a lid.

[0046] The reason why the above-mentioned various resins are suitable as the constituent material of the sealed container is thought to be that they have low gas permeability. If the gas permeability of the resin, which is the constituent material of the sealed container, is low, it is possible to effectively suppress the intrusion of gas into the sealed container, and as a result, it is possible to effectively suppress the promotion of aggregation due to the reaction between, for example, CO2 that has invaded the sealed container and the functional groups on the surface of the fibrous carbon nanostructure. In addition, if the gas permeability of the resin, which is the constituent material of the sealed container, is low, it is possible to suppress the leakage of gas from inside the sealed container to the outside of the container, and from this aspect, it is possible to suppress the detachment of the functional groups on the surface of the fibrous carbon nanostructure, thereby improving the dispersion stability. From the viewpoint of suppressing the flow of gas inside and outside the sealed container, it is also effective to seal the sealed container in a gas barrier bag and store it. The material of such a gas barrier bag is not particularly limited, but the above-listed resins can be used as the resins constituting the inner surface part of the sealed container that comes into contact with the dispersion liquid.

[0047] Here, when filling the closed container with the nanostructure dispersion, the filling rate of the container containing the dispersion is preferably 90.0% by volume or more, more preferably 94.0% by volume or more, preferably less than 98.0% by volume, and more preferably 97.0% by volume or less. If the filling rate of the container containing the dispersion is equal to or more than the above lower limit, the dispersibility of the nanostructures contained in the nanostructure dispersion in the container can be effectively prevented from decreasing. On the other hand, if the filling rate is equal to or less than the above upper limit, the possibility of the nanostructure dispersion spilling out of the container or the container bursting during use of the nanostructure dispersion can be effectively prevented. Note that the filling of the nanostructure dispersion into the closed container is preferably performed in a nitrogen gas atmosphere or argon gas atmosphere (i.e., an inert gas atmosphere), or in a clean environment of class 10 or more.

[0048] In the container-filled dispersion step, the dispersion filled in the sealed container is subjected to dispersion treatment as necessary. Ultrasonic treatment can be used as a dispersion method for such dispersion treatment. The ultrasonic treatment conditions can be an output of 2.0 amperes or more, 5.0 amperes or less, 5°C or more and 35°C or less, and 0.5 hours or more and 2 hours or less. The longer the dispersion time, the smaller the Z-average particle size of the nanostructure based on the dynamic light scattering method can be, and the shorter the dispersion time, the larger the Z-average particle size of the nanostructure based on the dynamic light scattering method can be. Therefore, by appropriately controlling the dispersion time, the Z-average particle size of the nanostructure based on the dynamic light scattering method can be appropriately controlled.

[0049] In the storage step, the dispersion liquid filled in the sealed container is left to stand in that state and stored for a predetermined period of time. In this case, it is preferable to store the sealed container in a storage cabinet. The storage temperature in the storage cabinet is preferably 25°C or lower from the viewpoint of dispersion stability, and is preferably higher than 0°C from the viewpoint of avoiding freezing. It is presumed that if the storage temperature is 25°C or lower, Brownian motion in the dispersion liquid can be suppressed, and aggregation between nanostructures can be effectively suppressed.

[0050] The storage period is not particularly limited, but since there is a risk that the Z-average particle diameter of the nanostructures based on dynamic light scattering may increase due to long-term storage, the storage period is preferably such that the Z-average particle diameter becomes 70 nm or less, and more specifically, is preferably 370 days or less.

[0051] In addition, the pressure of the atmosphere supplementing the sealed container in the storage step (hereinafter also referred to as "storage pressure") is preferably 0 kPa or more and 100 kPa or less in gauge pressure. If the storage pressure is 0 kPa or more, the pH of the nanostructure dispersion liquid itself can be prevented from decreasing. This is presumably because the storage pressure is 0 kPa or more in gauge pressure, in other words, the storage pressure is not a reduced pressure condition, and therefore the compounds derived from the functional groups of the nanostructures and the compounds derived from any additives contained in the nanostructure dispersion liquid can be prevented from vaporizing. As a result of being able to prevent the pH of the nanostructure dispersion liquid itself from decreasing, the nanostructures can be prevented from aggregating, and thus, when an electronic device is manufactured using the nanostructure dispersion liquid, the uniformity of the electronic device can be improved. In addition, if the storage pressure is 100 kPa or less, the viscosity of the nanostructure dispersion liquid due to pressure can be prevented. As a result, when an electronic device is manufactured using the nanostructure dispersion liquid, for example, when a coating process is performed, the occurrence of coating spots can be effectively prevented. In addition, if the storage pressure is 100 kPa or less, when a gas barrier bag is used to increase the storage pressure, the breakage of the bag can be prevented.

[0052] The nanostructure dispersion of the present invention described above can be taken out of the sealed container and (1) used to produce an assembly of nanostructures by removing the dispersion medium, or (2) mixed with a matrix material to produce a composite material composition, and used in any manner to produce a composite material. In this case, prior to removing the dispersion medium or mixing with the matrix material, an ion exchange process may be carried out, as necessary, to remove impurities such as metals from the nanostructure dispersion. As described above, the nanostructure dispersion of the present invention has excellent dispersion stability, and therefore can effectively suppress the aggregation of nanostructures and the clogging of ion exchange resins by the nanostructures during the ion exchange process. EXAMPLES

[0053] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples. The carbon nanotubes used in the examples and comparative examples were synthesized by the following method. Various evaluations in the examples and comparative examples were performed by the following methods.

[0054] (Synthesis of Carbon Nanotubes) CNTs (SGCNT-1) were prepared by the super-growth method in accordance with the description in International Publication No. 2006 / 011655. Note that, when preparing SGCNT-1, a catalyst layer was formed on the substrate surface by a wet process, and a raw material gas containing acetylene as the main component was used. The obtained SGCNT-1 has a BET specific surface area of ​​1050 m 2 / g (unopened), the micropore volume is 0.44mL / g, and when measured with a Raman spectrophotometer, the pore volume is 100-300cm, which is characteristic of single-walled CNTs. -1A radial breathing mode (RBM) spectrum was observed in the low wavenumber region of 100 SGCNT-1. Furthermore, using a transmission electron microscope, the diameter and length of 100 randomly selected SGCNT-1 were measured, and the average diameter (Av) was 3.3 nm, the value (3σ) obtained by multiplying the standard deviation (σ) of the diameter by 3 was 1.9 nm, the ratio thereof (3σ / Av) was 0.58, and the average length was 500 μm. Furthermore, the adsorption isotherm of SGCNT-1 was measured using a fully automatic specific surface area measuring device (manufactured by Mountec Co., Ltd., product name "Macsorb (registered trademark) HM model-1210"), and when a t-plot was created by converting the relative pressure in the obtained adsorption isotherm to the average thickness t (nm) of the nitrogen gas adsorption layer, the t-plot showed an upwardly convex shape.

[0055] (Z average particle size) 0.085 g of the carbon nanotube dispersion (solid concentration 0.3%) was diluted with 15 g of ultrapure water in a polypropylene container, and then stirred for 5 seconds with a vortex mixer (manufactured by AS ONE, product name: Vortex Mixer GHW-3000). Then, the Z-average particle size was measured using dynamic light scattering (DLS) (manufactured by Malvern Panalytical, product name: Zetasizer Nano ZS) according to the following procedure. (1) Pre-measurement pretreatment 0.085 g of the carbon nanotube dispersion (solid concentration 0.3%) was diluted with 15 g of ultrapure water in a PP container, and then stirred for 5 seconds with a vortex mixer (manufactured by AS ONE Corporation, product name: Vortex Mixer GHW-3000). (2) Measurement The carbon nanotube dispersion obtained above was added to a polystyrene cell (manufactured by Malvern Panalytical, product name: 12 mm square polystyrene cell DTS0012), and DLS measurement was carried out under sample conditions (refractive index: 1.12, absorptivity: 39.2, dispersion medium: water, measurement temperature: 25.0°C, equilibration time: 240 seconds) and measurement conditions (measurement angle: 173° backscattering) to measure the Z-average particle size.

[0056] (dispersion stability) 0.165 g of carbon nanotube dispersion 1 (solid concentration 0.3%) was diluted with 9.835 g of 0.1 mol / L nitric acid in a polypropylene container, and then stirred for 5 seconds with a vortex mixer (manufactured by AS ONE Corporation, product name: Vortex Mixer GHW-3000). After leaving it to stand for 5 hours in a room temperature environment, the presence or absence of aggregates in the dispersion in the container was visually confirmed. The results of visually confirming aggregates were evaluated according to the following criteria. A: The presence or absence of aggregates in the dispersion was checked, but no visible aggregates or particles were found. B: The presence or absence of aggregates in the dispersion was confirmed, and visible particles were found to be present.

[0057] Example 1 The SGCNT-1 (80 g) obtained as described above as a nanostructure was stirred in 12 L of 10.4 M nitric acid for 2 hours, then diluted to a nitric acid concentration of 9.1 M using ultrapure water, and purified by refluxing at 120 ° C. for 12.5 hours. After that, it was diluted to a nitric acid concentration of 1.7 M using ultrapure water, and cross-flow filtration was performed using a 0.01 μm ceramic membrane until the pH became 6.5. The liquid that passed through the ceramic membrane was discarded as the permeate, and the liquid that did not pass through the filter holes was collected as the retentate. Then, ammonia water and ammonium nitrate water were added to the retentate to adjust the pH of the retentate to 7.9 and the nitrate ion concentration to 100 ppm. Then, ultrasonic treatment was performed for 2 hours under conditions of 3.5 amperes and a temperature of 12.3 ° C. using an ultrasonic irradiation machine (Tokyo Ultrasonic Engineering Co., Ltd., product name: PUC-1415). As a result, carbon nanotube dispersion 1 was obtained. Carbon nanotube dispersion 1 (4.00 L) was filled in a polyethylene airtight container (manufactured by Aicello, product name: Clean Barrier Bottle SGL(G)PR, made of high density polyethylene) with a volume of 4 L (actual capacity: 4.20 L) in a class 100 clean booth. This resulted in carbon nanotube dispersion 2. The filling rate of the CNT dispersion in the airtight container was 95.2 volume %. The carbon nanotube dispersion 1 obtained as described above was subjected to DLS measurement as described above. As a result, the Z average particle size was 54.2 nm. Furthermore, the carbon nanotube dispersion 2 obtained as described above was subjected to the dispersion stability evaluation as described above. As a result, the presence or absence of aggregates in the dispersion was confirmed, but no visible aggregates or particles were found (dispersion stability evaluation: A).

[0058] Example 2 The carbon nanotube dispersion 2 (i.e., the CNT dispersion filled in a sealed container) obtained in the same manner as in Example 1 was placed in a thermo-hygrostat (manufactured by ESPEC, product name: SH-241) which was a storage cabinet set at 25°C. After a storage period of 305 days, starting from the day of placement, the CNT dispersion 2, which was the CNT dispersion filled in a sealed container, was taken out and subjected to DLS measurement. As a result, the Z-average particle size was 68.9 nm. In the dispersion stability evaluation, the presence or absence of aggregates in the dispersion was confirmed, but no visible aggregates or particles were found (dispersion stability evaluation: A).

[0059] Example 3 100 g of carbon nanotube dispersion 1 obtained in the same manner as in Example 1 was filled into a glass screw vial, and the vial was set in an ultrasonic irradiator (manufactured by Emerson Japan, product name: Bransonic tabletop ultrasonic cleaner 5510), and ultrasonic waves were irradiated for 8.8 minutes under conditions of 3.5 amperes and a temperature of 13.7°C. DLS measurement was performed on the obtained CNT dispersion. As a result, the Z-average particle size was 52.2 nm. In the dispersion stability evaluation, the presence or absence of aggregates in the dispersion was confirmed, but no visible aggregates or particles were found (dispersion stability evaluation: A).

[0060] Example 4 The same operation as in Example 3 was carried out, except that the ultrasonic irradiation time was set to 21 minutes. DLS measurement was carried out on the obtained CNT dispersion liquid. As a result, the Z-average particle diameter was 49.0 nm. In the dispersion stability evaluation, the presence or absence of aggregates in the dispersion liquid was confirmed, but no visible aggregates or particles were found (dispersion stability evaluation: A).

[0061] Example 5 The same operation as in Example 3 was carried out, except that the ultrasonic irradiation time was set to 63.4 minutes. DLS measurement was carried out on the obtained CNT dispersion liquid. As a result, the Z-average particle diameter was 45.4 nm. In the dispersion stability evaluation, the presence or absence of aggregates in the dispersion liquid was confirmed, but no visible aggregates or particles were found (dispersion stability evaluation: A).

[0062] Comparative Example 1 The carbon nanotube dispersion 2 (i.e., the CNT dispersion filled in a sealed container) obtained in the same manner as in Example 1 was placed in a thermo-hygrostat (manufactured by ESPEC, product name: SH-241) which was a storage cabinet set at 25°C. After a storage period of 452 days, starting from the day of placement, the CNT dispersion 2, which was the CNT dispersion filled in a sealed container, was taken out and subjected to DLS measurement. As a result, the Z-average particle size was 72.2 nm. In the dispersion stability evaluation, the presence or absence of aggregates in the dispersion was confirmed, and a large number of visible particles were present (dispersion stability evaluation: B).

[0063] Comparative Example 2 The same operation as in Example 3 was carried out, except that the ultrasonic irradiation time was 70 minutes. DLS measurement was carried out on the obtained CNT dispersion liquid. As a result, the Z-average particle diameter was 44.4 nm. In the dispersion stability evaluation, the presence or absence of aggregates in the dispersion liquid was confirmed, and as a result, many visible particles were present (dispersion stability evaluation: B).

[0064] Comparative Example 3 The same operation as in Example 3 was carried out, except that the ultrasonic irradiation time was 84 minutes. DLS measurement was carried out on the obtained CNT dispersion liquid. As a result, the Z-average particle diameter was 41.1 nm. In the dispersion stability evaluation, the presence or absence of aggregates in the dispersion liquid was confirmed, and as a result, many visible particles were present (dispersion stability evaluation: B). [Industrial Applicability]

[0065] According to the present invention, it is possible to provide a nanostructure dispersion liquid having excellent dispersion stability.

Claims

1. A nanostructure dispersion liquid containing a nanostructure and a dispersion medium, the nanostructure includes a fibrous carbon nanostructure having a functional group, and further has a Z-average particle size based on a dynamic light scattering method of 45.0 nm or more and 70.0 nm or less; The dispersion medium comprises water. Nanostructure dispersion.

2. The nanostructure dispersion of claim 1 , wherein the nanostructures comprise carbon nanotubes.

3. The nanostructure dispersion liquid according to claim 2 , wherein the carbon nanotubes include single-walled carbon nanotubes.

4. 4. The nanostructure dispersion liquid according to claim 2, wherein the carbon nanotubes exhibit an upwardly convex t-plot obtained from an adsorption isotherm.

Citation Information

Patent Citations

  • Container holding nanostructure liquid dispersion, method for storing and method for transporting nanostructure liquid dispersion, and method for producing aggregate and composition for composite material using nanostructure liquid dispersion

    WO2017115707A1