Composition, undercoat layer, electrode, and lithium ion secondary battery
A conductive carbon and acrylic resin-based undercoat layer composition addresses safety and resistance issues in lithium-ion batteries, ensuring low initial DC resistance and resistance suppression in high-temperature conditions, thereby enhancing battery performance and lifespan.
Patent Information
- Application Number
- JP2023054387
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Lithium-ion secondary batteries face challenges in maintaining safety and suppressing DC resistance during charging and discharging, especially in high-temperature environments and after long-term storage, which affects their performance and lifespan.
A composition comprising a conductive carbon material, an olefin resin, and an acrylic resin, with specific ratios and properties, is used to form an undercoat layer that reduces initial DC resistance and prevents resistance increase in high-temperature conditions, enhancing battery safety and performance.
The composition effectively suppresses DC resistance at the initial stage of charging and discharging, and in high-temperature environments, leading to improved safety and extended lifespan of lithium-ion secondary batteries.
Smart Images

Figure 2024142265000006 
Figure 2024142265000007 
Figure 2024142265000008
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a composition, an undercoat layer, an electrode, and a lithium ion secondary battery. [Background technology]
[0002] In recent years, lithium ion secondary batteries have been widely used as power sources for electronic devices, electric vehicles, and electricity storage. In particular, there has been a demand for batteries with high capacity, high output, and high energy density that can be installed in hybrid vehicles and the like. Such lithium ion secondary batteries have the advantage of having high energy density. On the other hand, sufficient safety measures are required because they use lithium metal and lithium ions.
[0003] Patent Document 1 discloses a positive electrode for a lithium ion secondary battery that improves the safety of the lithium ion secondary battery. The positive electrode disclosed in Patent Document 1 includes a positive electrode current collector and a positive electrode mixture layer. The positive electrode mixture layer is laminated on at least one side of the positive electrode current collector. The positive electrode mixture layer includes a positive electrode mixture layer and an undercoat layer. The undercoat layer is formed between the positive electrode current collector and the positive electrode mixture layer. The undercoat layer includes a conductive assistant, a binder, and a thermally expandable microcapsule. The thermally expandable microcapsule has a maximum volume expansion temperature of 70°C or more and 180°C or less.
[0004] Patent Document 2 discloses a secondary battery having an intermediate layer containing a cured product of a curable resin having a specific functional group and a conductive material between a positive electrode current collector and a positive electrode mixture layer in order to suppress an increase in battery temperature when an internal short circuit occurs. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2019 / 189866 [Patent Document 2] International Publication No. 2018 / 198689 Summary of the Invention [Problem to be solved by the invention]
[0006] There is a demand for a lithium ion secondary battery that is excellent in safety and excellent in battery performance in which the DC resistance at the initial stage of charging and discharging and the increase in the DC resistance of the lithium ion secondary battery in a high-temperature environment (particularly after long-term storage) are suppressed. The output of a lithium ion secondary battery in which the DC resistance at the initial stage of charging and discharging is suppressed is superior to the output of a lithium ion secondary battery in which the DC resistance at the initial stage of charging and discharging is not suppressed. The life of a lithium ion secondary battery in which the increase in the DC resistance in a high-temperature environment (particularly after long-term storage) is suppressed is superior to the life of a lithium ion secondary battery in which the increase in the DC resistance in a high-temperature environment (particularly after long-term storage) is not suppressed.
[0007] The problem to be solved by one embodiment of the present disclosure is to provide a composition (preferably an undercoat composition) and an undercoat layer suitable for forming an electrode that is safe, has low DC resistance during initial charging and discharging, and is suppressed from increasing in DC resistance under high temperature environments (especially after long-term storage). The problem to be solved by another embodiment of the present disclosure is to provide an electrode and a lithium ion secondary battery that are highly safe, have low DC resistance during initial charging and discharging, and are suppressed from increasing in DC resistance under high temperature environments (especially after long-term storage), and can stably provide excellent battery performance. [Means for solving the problem]
[0008] Specific means for solving the problems include the following aspects. <1> The composition comprises a conductive carbon material (A), an olefin-based resin (B) and an acrylic-based resin (C), the acrylic resin (C) comprising a first polymer obtained by polymerizing a first monomer component containing a (meth)acrylic acid ester and (meth)acrylonitrile, and a second polymer obtained by polymerizing a second monomer component containing (meth)acrylamide, and the ratio of the mass of the second polymer to the mass of the first polymer is 0.1 or more and less than 100. <2> the content of the conductive carbon material (A) is 1 mass% to 30 mass% based on the total mass of the composition, the content of the olefin-based resin (B) is 30 mass% to 90 mass% based on the total mass of the composition, and the content of the acrylic resin (C) is 1 mass% to 20 mass% based on the total mass of the composition; <1> The composition according to claim 1, <3> The olefin resin (B) contains an ethylene resin or a propylene resin. <1> or <2> The composition according to claim 1, <4> The olefin resin (B) is particulate, has a particle size of 0.1 μm to 9.0 μm, and has a softening point of 70° C. or higher. <1> ~ <3> The composition according to any one of claims 1 to 5, <5> The second monomer component in the acrylic resin (C) further contains a carboxyl group-containing vinyl monomer and a hydroxyl group-containing vinyl monomer. <1> ~ <4> The composition according to any one of claims 1 to 5, <6> The composition further contains an additive (D), and the content of the additive (D) is 1% by mass to 50% by mass based on the total mass of the composition. <1> ~ <5> The composition according to any one of claims 1 to 5, <7> The additive (D) contains carboxymethyl cellulose. <6> The composition according to claim 1, <8> The additive (D) contains at least one of a thermally expandable microcapsule having a maximum volume expansion temperature of 70° C. or more and 180° C. or less and an inorganic oxide filler. <6> or <7> The composition according to claim 1, <9> The ratio of particle size distribution D99 to particle size distribution D10 (D99 / D10), measured by the laser light diffraction scattering method, is 35 or less. <1> ~ <8> The composition according to any one of claims 1 to 5, <10> The particle size distribution D99 measured by the laser light diffraction scattering method is 20 μm or less. <1> ~ <9> The composition according to any one of claims 1 to 5, <11> The ratio of particle size distribution D99 to particle size distribution D50 (D99 / D50), measured by the laser light diffraction scattering method, is 20 or less. <1> ~ <10> The composition according to any one of claims 1 to 5, <12> <1> ~ <11> 1. An undercoat layer comprising the composition according to any one of claims 1 to 9. <13> A current collector; <12> and a composite layer. <14> The current collector, the undercoat layer, and the composite layer are provided in this order. <13> 2 is an electrode according to the above. <15> <13> or <14> A lithium ion secondary battery comprising the electrode according to the present invention. Effect of the Invention
[0009] According to the present disclosure, there is provided a composition (preferably an undercoat composition) and an undercoat layer suitable for forming an electrode that is safe, has low DC resistance during initial charging and discharging, and is suppressed from increasing in DC resistance under high temperature environments (especially after long-term storage). In addition, according to other embodiments of the present disclosure, there are provided an electrode and a lithium ion secondary battery that are highly safe, have low DC resistance during initial charging and discharging, and are suppressed from increasing in DC resistance under high temperature environments (especially after long-term storage), and can stably provide excellent battery performance. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a laminated battery, which is an example of a lithium ion secondary battery according to the present disclosure. [Diagram 2] FIG. 2 is a schematic cross-sectional view of a positive electrode in a lithium-ion secondary battery according to an embodiment of the present disclosure. [Diagram 3] FIG. 2 is a schematic cross-sectional view of a negative electrode in a lithium-ion secondary battery according to an embodiment of the present disclosure. [Figure 4] FIG. 1 is a schematic side view showing an example of a three-roll mill. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The contents of the present disclosure will be described in detail below. The following description of the components may be based on a representative embodiment of the present disclosure, but the present disclosure is not limited to such an embodiment.
[0012] In the present disclosure, a numerical range indicated using "~" indicates a range including the numerical value described before "~" as the lower limit and the numerical value described before "~" as the upper limit. In the numerical ranges described in stages in the present disclosure, the upper limit or lower limit described in a certain numerical range may be replaced with the upper limit or lower limit of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper limit or lower limit described in a certain numerical range may be replaced with a value shown in the examples.
[0013] In the description of groups (atomic groups) in this specification, when there is no indication of whether they are substituted or unsubstituted, the term encompasses both unsubstituted groups (atomic groups) and substituted groups (atomic groups). For example, the term "alkyl group" encompasses not only alkyl groups without a substituent (unsubstituted alkyl groups) but also alkyl groups with a substituent (substituted alkyl groups).
[0014] In this specification, "(meth)acrylate" refers to both or either of acrylate and methacrylate, "(meth)acryl" refers to both or either of acryl and methacryl, and "(meth)acryloyl" refers to both or either of acryloyl and methacryloyl.
[0015] In this specification, the term "process" refers not only to an independent process, but also to a process that cannot be clearly distinguished from other processes, as long as the intended effect of the process is achieved. The present disclosure will be described in detail below.
[0016] (1) Composition The composition of the present disclosure contains a conductive carbon material (A), an olefin resin (B) and an acrylic resin (C), and preferably contains an additive (D), and may further contain other components as necessary. The acrylic resin (C) of the present disclosure contains a first polymer obtained by polymerizing a first monomer component containing a (meth)acrylic acid ester and (meth)acrylonitrile, and a second polymer obtained by polymerizing a second monomer component containing a (meth)acrylamide, and the ratio of the mass of the second polymer to the mass of the first polymer (amount of the second polymer / amount of the first polymer) is in the range of 0.1 or more and less than 100.
[0017] In the present disclosure, the term "conductive carbon material" refers to a carbon material having a volume resistivity at 20° C. of less than 40 Ω·cm, preferably less than 3 Ω·cm. In the present disclosure, the term "olefin-based resin" refers to a resin containing structural units derived from an olefin. Specifically, the term "olefin-based resin" includes a homopolymer of an olefin, a copolymer of two or more kinds of olefins, or a copolymer of an olefin and another monomer. In the present disclosure, the term "acrylic resin" refers to a resin containing a structural unit derived from a monomer having a (meth)acryloyl group (hereinafter also referred to as a (meth)acrylic monomer). In more detail, the term "acrylic resin" includes a homopolymer of a (meth)acrylic monomer and a copolymer of two or more kinds of (meth)acrylic monomers.
[0018] In the present disclosure, the term "additive" refers to components other than the conductive carbon material (A), the olefin-based resin (B), and the acrylic resin (C). In the present disclosure, the terms "content" and "addition amount" are considered to be substantially the same.
[0019] The composition of the present disclosure contains a conductive carbon material (A), an olefin resin (B), and an acrylic resin (C), and the ratio of the mass of the second polymer to the mass of the first polymer in the acrylic resin (C) (amount of second polymer / amount of first polymer) satisfies a specific range, thereby making it possible to form an electrode that is excellent in safety, has low DC resistance during initial charging and discharging, and is suppressed from increasing in DC resistance under high temperature conditions (especially after long-term storage). In other words, when the composition of the present disclosure is applied to a lithium ion secondary battery equipped with an electrode, it is possible to obtain a lithium ion secondary battery that has a good balance between safety and battery performance (i.e., output and life).
[0020] The reason why the present disclosure has an effect is not necessarily clear, but is presumed to be as follows. Among the resin components contained in the composition of the present disclosure, one of the water-dispersible olefin resins (B) has the function of melting in a lower temperature range. In other words, it is advantageous for the manifestation of the shutdown function during heat generation. On the other hand, the acrylic resin (C) is configured (preferably in a core-shell structure) containing a first polymer obtained by polymerizing a first monomer component containing a (meth)acrylic acid ester and (meth)acrylonitrile, and a second polymer obtained by polymerizing a second monomer component containing a (meth)acrylamide, and the ratio of the amount of the second polymer to the amount of the first polymer is in the range of 0.1 or more and less than 100. For example, a core-shell structure is formed in which the core component contains a first polymer containing electrolyte-resistant (meth)acrylonitrile, and the shell component containing the core contains a second polymer containing heat-resistant (meth)acrylamide. That is, the second polymer, which is relatively hydrophilic to the first polymer, which is hydrophobic, is present on the surface of the acrylic resin, and the above-mentioned ratio of the amount of the second polymer to the amount of the first polymer is obtained. This allows the heat resistance, electrolyte resistance, and ion permeability to be improved in a well-balanced manner. Therefore, an electrode can be obtained that is excellent in safety, and not only has low DC resistance during initial charging and discharging, but also has a significantly suppressed increase in DC resistance under high temperature conditions (especially after long-term storage). As a result, when a lithium ion secondary battery is produced, it can have a good balance between safety and battery performance (i.e., output and life).
[0021] The composition of the present disclosure is preferably used for, for example, electrode components of lithium ion secondary batteries. In particular, the composition of the present disclosure is preferably used to form an undercoat layer included in an electrode of a lithium ion secondary battery having an electrode in which an undercoat layer and a composite layer are laminated in this order on at least one main surface of a current collector. In particular, the composition of the present disclosure is more preferably used to form an undercoat layer included in a positive electrode of a lithium ion secondary battery having a positive electrode in which an undercoat layer and a composite layer are laminated in this order on at least one main surface of a current collector.
[0022] In this disclosure, the term "current collector" refers to a sheet-like object for collecting electrons generated from an active material in a lithium-ion secondary battery and supplying the electrons to the active material. The term "main surfaces of a current collector" refers to a pair of opposing surfaces having the largest area among a plurality of pairs of opposing surfaces.
[0023] (1.1) Conductive carbon material (A) The composition of the present disclosure includes at least one conductive carbon material, which reduces the electrical resistance of the composition of the present disclosure.
[0024] Examples of the conductive carbon material include graphite, carbon black, conductive carbon fiber, and fullerene. Examples of graphite include artificial graphite and natural graphite (e.g., flake graphite, lump graphite, and amorphous graphite). Examples of the conductive carbon fiber include carbon nanotubes, carbon nanofibers, and carbon fibers. The conductive carbon material may be used alone or in combination of two or more.
[0025] The shape of the conductive carbon material is not particularly limited, and may be particulate. When the conductive carbon material is particulate, the particle size of the conductive carbon material is not particularly limited. From the viewpoint of dispersing the conductive carbon material between the particles contained in the undercoat layer and functioning as a conductive assistant, the particle size of the conductive carbon material is preferably 5 μm or less, more preferably 1 μm to 4 μm. In this case, the primary particle size of the particles of the conductive carbon material is preferably 0.5 μm or less, more preferably 0.1 μm to 0.4 μm. The particle size of the conductive carbon material is the particle size (particle size distribution D50, median diameter) that corresponds to 50% by volume cumulative from the fine particle side in the volume-based particle size distribution measured by a particle size distribution measuring device based on the laser light diffraction scattering method.
[0026] The conductive carbon material may be a commercially available product. Examples of commercially available carbon black products include "Super P" (manufactured by TIMCAL). Examples of commercially available flake graphite products include "KS-6" (manufactured by TIMREX).
[0027] The content of the conductive carbon material is preferably 1% by mass to 30% by mass with respect to the total amount of the composition. If the content of the conductive carbon material is within the above range, the number of contact points between the conductive carbon materials in the composition of the present disclosure is large, and the electrical resistance of the composition of the present disclosure at room temperature can be reduced by the percolation effect. Furthermore, when the temperature of the lithium ion secondary battery increases rapidly, the contact between the conductive carbon materials is difficult to maintain, and the electrical resistance of the undercoat layer increases, so that the resulting lithium ion secondary battery can exhibit a shutdown function. In other words, the safety of the lithium ion secondary battery is excellent. The shutdown function includes preventing the progress of the battery reaction of the lithium ion secondary battery. The "battery reaction" refers to the insertion reaction and desorption reaction of lithium ions that occur between the positive electrode and the negative electrode. The higher the content of the conductive carbon material, the better the battery performance of the lithium ion secondary battery tends to be. The content of the conductive carbon material is preferably 25% by mass or less, more preferably 20% by mass or less, based on the total amount of the composition, from the viewpoint of ensuring the shutdown function. The content of the conductive carbon material is preferably 5% by mass or more, more preferably 10% by mass or more, based on the total amount of the composition, from the viewpoint of ensuring the battery performance.
[0028] (1.2) Olefin resin (B) The composition of the present disclosure contains at least one olefin-based resin, and when the composition of the present disclosure is used as a raw material for an undercoat layer, the lithium ion secondary battery is less likely to experience thermal runaway, and the safety of the lithium ion secondary battery can be further improved.
[0029] The material of the olefin resin (B) is not particularly limited. The softening point of the olefin resin is preferably 150°C or less, more preferably 140°C or less, and even more preferably 135°C or less, from the viewpoint of more effectively exerting the shutdown function by melting the olefin resin in a lower temperature range during a sudden temperature rise of the lithium ion secondary battery (hereinafter referred to as "effective exertion of the shutdown function"). The softening point of the olefin resin is preferably 70°C or more, more preferably 90°C or more, even more preferably 110°C or more, and particularly preferably 120°C or more, from the viewpoint of maintaining the shape of the olefin resin before and after the drying process performed in the manufacturing process of the positive electrode (hereinafter referred to as "shape maintenance of the olefin resin (B) during the positive electrode drying process"). The softening point of the olefin resin (B) is preferably 70°C to 150°C. The softening point of the olefin resin (B) is a value measured according to JIS K 2207-2015 (ring and ball method).
[0030] Examples of olefin-based resins include ethylene-based resins (e.g., polyethylene, ethylene-vinyl acetate copolymer (EVA), polyethylene oxide), propylene-based resins (e.g., polypropylene), polyvinyl chloride, polyvinylidene chloride, polyvinyl fluoride, polyvinylidene fluoride, polyamide, polystyrene, polyacrylonitrile, and polymethyl (meth)acrylate. Among them, the olefin-based resin preferably contains a polyethylene-based resin or a polypropylene-based resin from the viewpoint of achieving both effective shutdown function and shape retention of the olefin-based resin during the positive electrode drying step.
[0031] An "ethylene-based resin" is a resin whose main component is ethylene, and a "propylene-based resin" is a resin whose main component is propylene. Here, the term "main component" refers to the component that is contained in the resin in the greatest amount. The ethylene-based resin may be a homopolymer or copolymer of ethylene. Among them, the ethylene-based resin is preferably a copolymer of ethylene and at least one α-olefin. The propylene-based resin may be a homopolymer or copolymer of propylene.
[0032] The olefin resin preferably contains a water-dispersible olefin resin, whereby when the composition of the present disclosure is used as a raw material for the undercoat layer, the lithium ion secondary battery is less susceptible to thermal runaway, and the safety of the lithium ion secondary battery is improved. The term "water-dispersible olefin resin" refers to an olefin resin that is dispersible in water without the addition of at least one of a surfactant and an organic solvent.
[0033] Examples of the water-dispersible olefin resin material include polyethylene, polyethylene elastomers, polyolefin ionomers, and EVA.
[0034] The content of the water-dispersible olefin resin is not particularly limited, and is preferably 20% by mass or more, more preferably 50% by mass or more, and may be 100% by mass, based on the total amount of the olefin resin (B).
[0035] As the olefin-based resin (B), a commercially available product may be used. Commercially available olefin resins include the Chemipearl (registered trademark) series (polyolefin aqueous dispersions) manufactured by Mitsui Chemicals, Inc. Examples of finely divided aqueous dispersions of polyethylene or polypropylene include WP100, W100, W200, W300, W308, W310, W400, W401, W410, W4005, W500, WF640, W700, W800, W900, W950, P301W, and WH201.
[0036] The shape of the olefin resin (B) is not particularly limited, and may be particulate. When the olefin resin (B) is particulate, the particle size is not particularly limited. The upper limit of the particle size of the olefin resin (B) is preferably 9.0 μm, more preferably 4.0 or less, and even more preferably 2.0 μm, as the average primary particle size, from the viewpoint of adjusting the particle size of the olefin resin so as to fall within the optimum film thickness range of the undercoat layer. The lower limit of the particle size of the olefin resin (B) is preferably 0.1 μm, more preferably 0.5 μm, from the viewpoint of the processability of the composition (e.g., slurry for the undercoat layer). The particle size of the olefin resin (B) is preferably 0.1 μm to 9.0 μm. The smaller the particle size of the olefin resin (B), the more likely the olefin resin (B) is to aggregate. The particle size of the olefin resin (B) is the average primary particle size measured by a Coal counter method.
[0037] The olefin resin (B) is preferably particulate, has a particle size of 0.1 μm to 9.0 μm, and has a softening point of 70° C. or higher. As a result, when the composition of the present disclosure is used as a raw material for the undercoat layer, the lithium ion secondary battery is less susceptible to thermal runaway, and the safety of the lithium ion secondary battery is further improved.
[0038] The olefin-based resin (B) may be used alone or in combination of two or more kinds. The content of the olefin resin (B) is preferably 30% by mass to 90% by mass based on the total amount of the composition. When the content of the olefin resin (B) is within the above range, the shutdown function can be satisfactorily ensured. The higher the content of the olefin resin (B), the better the safety of the lithium ion secondary battery becomes, whereas the battery performance of the lithium ion secondary battery tends to decrease. In other words, there is a trade-off between the safety of the lithium ion secondary battery and the battery performance of the lithium ion secondary battery. From this viewpoint, the content of the olefin resin (B) is preferably 80 mass% or less, more preferably 75 mass% or less, based on the total amount of the composition, from the viewpoint of reducing the resistance of the undercoat layer. Also, the content of the olefin resin (B) is preferably 35 mass% or more, more preferably 40 mass% or more, even more preferably 50 mass% or more, and particularly preferably 60 mass% based on the total amount of the composition, from the viewpoint of effectively exerting the shutdown function.
[0039] (1.3) Acrylic resin (C) The composition of the present disclosure contains at least one acrylic resin. The acrylic resin (C) in the present disclosure contains a first polymer and a second polymer, and the ratio of the mass of the second polymer to the mass of the first polymer (amount of second polymer / amount of first polymer) is in the range of 0.1 or more and less than 100. The first polymer is a polymer obtained by a polymerization reaction of a first monomer component containing a (meth)acrylic acid ester and (meth)acrylonitrile. The second polymer is a polymer obtained by a polymerization reaction of a second monomer component containing (meth)acrylamide.
[0040] (1.3.1) First polymer The first polymer is a polymer obtained by a polymerization reaction of a first monomer component containing a (meth)acrylic acid ester and (meth)acrylonitrile.
[0041] When the first monomer component contains (meth)acrylonitrile, an electrode using the composition of the present disclosure exhibits excellent electrolyte resistance, and as a result, a lithium ion secondary battery with an excellent balance between safety and battery performance (i.e., output and life) can be obtained.
[0042] The (meth)acrylic acid ester is a main unit among the structural units forming the first polymer. Being a main unit means that it accounts for 45 mass % or more of all structural units of the first polymer.
[0043] Examples of the (meth)acrylic acid ester include alkyl esters having 1 to 12 carbon atoms of (meth)acrylic acid such as methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-amyl (meth)acrylate, isoamyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, octadecyl (meth)acrylate, cyclohexyl (meth)acrylate, phenyl (meth)acrylate, and benzyl (meth)acrylate. Preferred are methyl (meth)acrylate and n-butyl (meth)acrylate, and more preferred are methyl methacrylate and n-butyl acrylate.
[0044] The (meth)acrylonitrile is preferably acrylonitrile, that is, the first monomer component preferably contains acrylonitrile.
[0045] The first monomer component may contain, as an optional component, a copolymerizable monomer copolymerizable with the (meth)acrylic acid ester and (meth)acrylonitrile (hereinafter also referred to as the first copolymerizable monomer).
[0046] Examples of the first copolymerizable monomer include functional group-containing vinyl monomers, vinyl esters, aromatic vinyl monomers, N-substituted unsaturated carboxylic acid amides, heterocyclic vinyl compounds, vinylidene halide compounds, α-olefins, and dienes.
[0047] Examples of functional group-containing vinyl monomers include carboxy group-containing vinyl monomers, hydroxyl group-containing vinyl monomers, amino group-containing vinyl monomers, glycidyl group-containing vinyl monomers, sulfonic acid group-containing vinyl monomers and salts thereof, acetoacetoxy group-containing vinyl monomers, and phosphoric acid group-containing compounds. Examples of the carboxy group-containing vinyl monomer include monocarboxylic acids (such as (meth)acrylic acid, etc.), dicarboxylic acids (such as itaconic acid, maleic acid, fumaric acid, itaconic anhydride, maleic anhydride, fumaric anhydride, etc.), and salts thereof. Examples of hydroxyl group-containing vinyl monomers include 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate. Examples of amino group-containing vinyl monomers include 2-aminoethyl (meth)acrylate, 2-(N-methylamino)ethyl (meth)acrylate, and 2-(N,N-dimethylamino)ethyl (meth)acrylate. An example of the glycidyl group-containing vinyl monomer is glycidyl (meth)acrylate. Examples of the sulfonic acid group-containing vinyl monomer include allylsulfonic acid, methallylsulfonic acid, and acrylamido t-butylsulfonic acid. Examples of the salts include alkali metal salts (e.g., sodium salts, potassium salts, etc.) and ammonium salts of the sulfonic acid group-containing vinyl monomer. Specific examples include sodium allylsulfonate, sodium methallylsulfonate, and ammonium methallylsulfonate. An example of an acetoacetoxy group-containing vinyl monomer is acetoacetoxyethyl (meth)acrylate. An example of the phosphate group-containing compound is 2-methacryloyloxyethyl acid phosphate.
[0048] Furthermore, examples of vinyl esters include vinyl acetate and vinyl propionate. Examples of aromatic vinyl monomers include styrene and α-methylstyrene. An example of the N-substituted unsaturated carboxylic acid amide is N-methylol (meth)acrylamide. An example of the heterocyclic vinyl compound is vinylpyrrolidone. Examples of the vinylidene halide compound include vinylidene chloride and vinylidene fluoride. Examples of the α-olefins include ethylene and propylene. An example of the dienes is butadiene.
[0049] The first copolymerizable monomer can also include a crosslinkable vinyl monomer. Examples of crosslinkable vinyl monomers include compounds having two or more vinyl groups, such as methylene bis(meth)acrylamide, divinylbenzene, polyethylene glycol chain-containing di(meth)acrylate, trimethylolpropane tetraacrylate, pentaerythritol triacrylate, and pentaerythritol tetraacrylate.
[0050] The first copolymerizable monomer may be used alone or in combination of two or more kinds.
[0051] As the first copolymerizable monomer, a functional group-containing vinyl monomer, an N-substituted unsaturated carboxylic acid amide or a combination thereof is preferable, a carboxy group-containing vinyl monomer, a hydroxy group-containing vinyl monomer, an N-substituted unsaturated carboxylic acid amide or a combination thereof is more preferable, and a combination of a carboxy group-containing vinyl monomer, a hydroxy group-containing vinyl monomer and an N-substituted unsaturated carboxylic acid amide, or a combination of a carboxy group-containing vinyl monomer and a hydroxy group-containing vinyl monomer is even more preferable.
[0052] The combined use of a carboxyl group-containing vinyl monomer, a hydroxyl group-containing vinyl monomer, and an N-substituted unsaturated carboxylic acid amide improves dispersion stability, and the functional groups are condensed intermolecularly to increase the molecular weight, thereby improving solvent resistance. Particularly preferred is the combined use of methacrylic acid, 2-hydroxyethyl methacrylate, and N-methylolacrylamide, or the combined use of methacrylic acid and 2-hydroxyethyl methacrylate.
[0053] When the first copolymerizable monomer contains a carboxyl group-containing vinyl monomer, a hydroxyl group-containing vinyl monomer, and an N-substituted unsaturated carboxylic acid amide, the content of the carboxyl group-containing vinyl monomer is, for example, 25 parts by mass or more and 50 parts by mass or less relative to 100 parts by mass of the first copolymerizable monomer. The content of the carboxyl group-containing vinyl monomer is, for example, 0.5 parts by mass or more and 12 parts by mass or less relative to 100 parts by mass of the first monomer component. The content of the hydroxyl group-containing vinyl monomer is, for example, 35 parts by mass or more and 50 parts by mass or less relative to 100 parts by mass of the first copolymerizable monomer, and the content of the hydroxyl group-containing vinyl monomer is, for example, 0.5 parts by mass or more and 12 parts by mass or less relative to 100 parts by mass of the first monomer component. The content of the N-substituted unsaturated carboxylic acid amide is, for example, 3 parts by mass or more and 30 parts by mass or less relative to 100 parts by mass of the first copolymerizable monomer, and the content of the N-substituted unsaturated carboxylic acid amide is, for example, 0.1 parts by mass or more and 5 parts by mass or less relative to 100 parts by mass of the first monomer component.
[0054] When the first copolymerizable monomer contains a carboxy group-containing vinyl monomer and a hydroxyl group-containing vinyl monomer, the content of the carboxy group-containing vinyl monomer is, for example, 15 parts by mass or more and 80 parts by mass or less per 100 parts by mass of the first copolymerizable monomer, and is, for example, 0.5 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the first monomer component. The content of the hydroxyl group-containing vinyl monomer is, for example, 20 parts by mass or more and 85 parts by mass or less per 100 parts by mass of the first copolymerizable monomer, and is, for example, 0.5 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the first monomer component.
[0055] The content of the (meth)acrylic acid ester in the first monomer component is, relative to 100 parts by mass of the total amount of the (meth)acrylic acid ester and (meth)acrylonitrile, for example, 15 parts by mass or more, preferably 20 parts by mass or more, more preferably 34 parts by mass or more, and for example, 85 parts by mass or less, preferably 80 parts by mass or less, more preferably 66 parts by mass or less. The content of the (meth)acrylic acid ester is, for example, 20 parts by mass or more, preferably 30 parts by mass or more, and for example, 80 parts by mass or less, preferably 70 parts by mass or less, and more preferably 65 parts by mass or less, relative to 100 parts by mass of the first monomer component.
[0056] The content of (meth)acrylonitrile in the first monomer component is, relative to 100 parts by mass of the total amount of the (meth)acrylic acid ester and (meth)acrylonitrile, for example, 15 parts by mass or more, preferably 20 parts by mass or more, more preferably 34 parts by mass or more, and for example, 85 parts by mass or less, preferably 80 parts by mass or less, more preferably 66 parts by mass or less. The content of (meth)acrylonitrile is, for example, 20 parts by mass or more, preferably 30 parts by mass or more, and more preferably 35 parts by mass or more, and is, for example, 80 parts by mass or less, and preferably 70 parts by mass or less, relative to 100 parts by mass of the first monomer component.
[0057] When the content of (meth)acrylonitrile is equal to or greater than the lower limit, the electrode using the composition of the present disclosure exhibits excellent electrolyte resistance, and as a result, a lithium ion secondary battery having an excellent balance between safety and battery performance (i.e., output and life) can be obtained. When the content of (meth)acrylonitrile is equal to or less than the upper limit, the film-forming property is improved, and the adhesion to the substrate (e.g., positive electrode current collector) is improved.
[0058] The first monomer component may be only a (meth)acrylic acid ester and (meth)acrylonitrile without containing the first copolymerizable monomer, or a combination of a (meth)acrylic acid ester, (meth)acrylonitrile, and the first copolymerizable monomer may be used. When the first monomer component contains a first copolymerizable monomer, the content of the first copolymerizable monomer is preferably 0.5 parts by mass or more, more preferably 2 parts by mass or more, relative to 100 parts by mass of the total amount of (meth)acrylic acid ester and (meth)acrylonitrile. Also, for example, it is 30 parts by mass or less, preferably 22 parts by mass or less. Also, the content of the first copolymerizable monomer is, for example, 0.5 parts by mass or more, preferably 3 parts by mass or more, and for example, 30 parts by mass or less, preferably 24 parts by mass or less, relative to 100 parts by mass of the first monomer component. As the first monomer component, a preferred embodiment is one in which a (meth)acrylic acid ester, (meth)acrylonitrile, and a first copolymerizable monomer are used in combination in the above ratio.
[0059] The first polymer is relatively hydrophobic with respect to the second polymer described below.
[0060] (1.3.2) Second polymer The second polymer is a polymer obtained by a polymerization reaction of a second monomer component containing (meth)acrylamide.
[0061] When the second monomer component contains (meth)acrylamide, an electrode using the composition of the present disclosure exhibits excellent heat resistance, resulting in a secondary battery with an excellent balance between safety and battery performance (i.e., output and life).
[0062] The (meth)acrylamide is preferably methacrylamide, that is, the second monomer component preferably contains methacrylamide.
[0063] If the second monomer component contains methacrylamide, a secondary battery separator (described below) obtained using a coating material for a secondary battery separator (described below) containing this raw material for a coating material for a secondary battery separator has even more excellent heat resistance.
[0064] Furthermore, the second monomer component may contain, as an optional component, a copolymerizable monomer copolymerizable with (meth)acrylamide (hereinafter also referred to as a second copolymerizable monomer).
[0065] Examples of the second copolymerizable monomer include the (meth)acrylic acid esters, functional group-containing vinyl monomers, vinyl esters, aromatic vinyl monomers, N-substituted unsaturated carboxylic acid amides, heterocyclic vinyl compounds, vinylidene halide compounds, α-olefins, dienes, and crosslinkable vinyl monomers described above in the section on the first copolymerizable monomer.
[0066] Furthermore, the second copolymerizable monomer may further include a functional group-containing vinyl monomer, such as a cyano group-containing vinyl monomer, for example, (meth)acrylonitrile.
[0067] The second copolymerizable monomer may be used alone or in combination of two or more kinds.
[0068] As the second copolymerizable monomer, a functional group-containing vinyl monomer, a crosslinkable vinyl monomer or a combination thereof is preferred, a carboxy group-containing vinyl monomer, a hydroxy group-containing vinyl monomer, a crosslinkable vinyl monomer or a combination thereof is more preferred, a combination of a carboxy group-containing vinyl monomer and a hydroxy group-containing vinyl monomer, or a combination of a carboxy group-containing vinyl monomer, a hydroxy group-containing vinyl monomer and a crosslinkable vinyl monomer is even more preferred.
[0069] The second monomer component in the acrylic resin (C) preferably contains a carboxyl group-containing vinyl monomer and a hydroxyl group-containing vinyl monomer.
[0070] When the second monomer component contains a carboxyl group-containing vinyl monomer and a hydroxyl group-containing vinyl monomer, the dispersion stability is improved.
[0071] When the second copolymerizable monomer contains a carboxyl-containing vinyl monomer and a hydroxyl-containing vinyl monomer, the content of the carboxyl-containing vinyl monomer is, for example, 35 parts by mass or more, preferably 45 parts by mass or more, and, for example, 85 parts by mass or less, preferably 80 parts by mass or less, relative to 100 parts by mass of the total amount of the carboxyl-containing vinyl monomer and the hydroxyl-containing vinyl monomer. The content of the carboxyl-containing vinyl monomer is, for example, 0.5 parts by mass or more, preferably 3 parts by mass or more, and, for example, 40 parts by mass or less, preferably 30 parts by mass or less, and more preferably 25 parts by mass or less, relative to 100 parts by mass of the second monomer component. The content of the hydroxyl group-containing vinyl monomer is, for example, 15 parts by mass or more, preferably 20 parts by mass or more, and for example, 65 parts by mass or less, preferably 55 parts by mass or less, relative to 100 parts by mass of the total amount of the carboxyl group-containing vinyl monomer and the hydroxyl group-containing vinyl monomer. The content of the hydroxyl group-containing vinyl monomer is, for example, 0.5 parts by mass or more, preferably 3 parts by mass or more, and for example, 30 parts by mass or less, preferably 20 parts by mass or less, more preferably 15 parts by mass or less, relative to 100 parts by mass of the second monomer component.
[0072] When the second copolymerizable monomer contains a carboxyl group-containing vinyl monomer, a hydroxyl group-containing vinyl monomer, and a crosslinkable vinyl monomer, the content of the carboxyl group-containing vinyl monomer is, for example, 20 parts by mass or more, preferably 40 parts by mass or more, and, for example, 48 parts by mass or less, preferably 45 parts by mass or less, relative to 100 parts by mass of the total amount of the carboxyl group-containing vinyl monomer, the hydroxyl group-containing vinyl monomer, and the crosslinkable vinyl monomer. The content of the carboxyl group-containing vinyl monomer is, for example, 0.5 parts by mass or more, preferably 3 parts by mass or more, and, for example, 20 parts by mass or less, preferably 10 parts by mass or less, relative to 100 parts by mass of the second monomer component. The content of the hydroxyl group-containing vinyl monomer is, for example, 20 parts by mass or more, preferably 40 parts by mass or more, and for example, 48 parts by mass or less, preferably 45 parts by mass or less, relative to 100 parts by mass of the total amount of the carboxyl group-containing vinyl monomer, the hydroxyl group-containing vinyl monomer, and the crosslinkable vinyl monomer. The content of the hydroxyl group-containing vinyl monomer is, for example, 0.5 parts by mass or more, preferably 3 parts by mass or more, and for example, 20 parts by mass or less, preferably 10 parts by mass or less, relative to 100 parts by mass of the second monomer component. The content of the crosslinkable vinyl monomer is, for example, 4 parts by mass or more, preferably 10 parts by mass or more, and for example, 60 parts by mass or less, preferably 20 parts by mass or less, relative to 100 parts by mass of the total amount of the carboxyl group-containing vinyl monomer, the hydroxyl group-containing vinyl monomer, and the crosslinkable vinyl monomer. The content of the crosslinkable vinyl monomer is, for example, 0.1 parts by mass or more, preferably 1 part by mass or more, and for example, 5 parts by mass or less, relative to 100 parts by mass of the second monomer component. As the second copolymerizable monomer, a combination of methacrylic acid and 2-hydroxyethyl methacrylate, a combination of methacrylic acid, 2-hydroxyethyl methacrylate and methylenebisacrylamide, or a combination of methacrylic acid, 2-hydroxyethyl methacrylate and polyethylene glycol dimethacrylate is particularly preferred.
[0073] In the second monomer component, the content of (meth)acrylamide is, relative to 100 parts by mass of the second monomer component, for example, 60 parts by mass or more, preferably 70 parts by mass or more, and for example, 100 parts by mass or less, preferably 99 parts by mass or less, more preferably 95 parts by mass or less, even more preferably 90 parts by mass or less, and particularly preferably 80 parts by mass or less. When the content of (meth)acrylamide is equal to or higher than the lower limit, the electrode using the composition of the present disclosure exhibits excellent heat resistance, and as a result, a secondary battery having an excellent balance between safety and battery performance (i.e., output and life) can be obtained. When the content of (meth)acrylamide is equal to or lower than the upper limit, a functional group-containing vinyl monomer can be introduced into the second monomer component, improving dispersion stability.
[0074] The second monomer component may be only (meth)acrylamide without containing the second copolymerizable monomer, or may be a combination of (meth)acrylamide and the second copolymerizable monomer in the above ratio. When the second monomer component contains a second copolymerizable monomer, the content of the second copolymerizable monomer is, for example, 0.5 parts by mass or more, preferably 2 parts by mass or more, and for example, 70 parts by mass or less, relative to 100 parts by mass of (meth)acrylamide. The content of the second copolymerizable monomer is, for example, 0.5 parts by mass or more, preferably 2 parts by mass or more, and for example, 50 parts by mass or less, preferably 45 parts by mass or less, relative to 100 parts by mass of the second monomer component. The second monomer component is preferably a combination of (meth)acrylamide and the second copolymerizable monomer in the above ratio.
[0075] The second polymer is relatively hydrophilic with respect to the first polymer.
[0076] (1.3.3) Synthesis method Next, a method for synthesizing the acrylic resin (C) will be described. The acrylic resin (C) in the present disclosure can be prepared by a method (first method) in which a first monomer component is polymerized to synthesize a first polymer, and then a second monomer component is polymerized in the presence of the first polymer; or a method (second method) in which a second monomer component is polymerized to synthesize a second polymer, and then the first monomer component is polymerized in the presence of the second polymer.
[0077] (1.3.3.1) First method The first method includes a step (first step) of obtaining a first polymer by polymerizing a first monomer component containing a (meth)acrylic acid ester and (meth)acrylonitrile, and a step (second step) of obtaining a second polymer by polymerizing a second monomer component containing (meth)acrylamide in the presence of the first polymer.
[0078] In the first step, the first monomer component is polymerized. Specifically, the first monomer component and a polymerization initiator are mixed into water, and the first monomer component is polymerized in the water.
[0079] Examples of the polymerization initiator include water-soluble initiators such as persulfates (ammonium persulfate, potassium persulfate, etc.), hydrogen peroxide, organic hydroperoxides, and 4,4'-azobis(4-cyanovaleric) acid; oil-soluble initiators such as benzoyl peroxide and azobisisobutyronitrile; and redox initiators.
[0080] The polymerization initiator may be used alone or in combination of two or more kinds. The blending ratio of the polymerization initiator may be appropriately set depending on the purpose and application, and is, for example, 0.05 parts by mass or more and, for example, 10 parts by mass or less, preferably 5 parts by mass or less, relative to 100 parts by mass of the first monomer component.
[0081] The polymerization conditions are, for example, at normal pressure, a polymerization temperature of 30° C. or higher (preferably 50° C. or higher). The polymerization temperature is, for example, 95° C. or lower (preferably 85° C. or lower). The polymerization time is, for example, 1 hour or higher (preferably 2 hours or higher), and, for example, 30 hours or lower (preferably 20 hours or lower).
[0082] In the polymerization of the first polymer, an emulsifier (surfactant) can be blended as necessary from the viewpoint of improving the production stability. Examples of the emulsifier include anionic surfactants such as sulfate esters of higher alcohols, alkylbenzenesulfonates (dodecylbenzenesulfonates, etc.), aliphatic sulfonates, alkyldiphenylethersulfonates, and ammonium lauryl sulfate; and nonionic surfactants such as alkyl esters, alkylphenylethers, and alkylethers of polyethylene glycol. A preferred emulsifier is an anionic surfactant, and more preferably ammonium lauryl sulfate.
[0083] When an emulsifier is used, the blending ratio of the emulsifier may be appropriately set depending on the purpose and application, and is, for example, 0.01 parts by mass or more and, for example, 5 parts by mass or less, and preferably 1 part by mass or less, relative to 100 parts by mass of the first monomer component.
[0084] In the polymerization of the first polymer, from the viewpoint of improving production stability, known additives such as, for example, a pH adjuster, a metal ion sequestering agent (e.g., ethylenediaminetetraacetic acid and its salts), and a molecular weight regulator (a chain transfer agent, for example, mercaptans and low molecular weight halogen compounds) may be blended in an appropriate ratio.
[0085] Before or after polymerization of the first polymer, the pH can be adjusted to within the range of 7 to 11 by adding a neutralizing agent (ammonia, etc.).
[0086] The first polymer can be obtained as a dispersion in water. The solid content concentration of the first polymer in the dispersion is, for example, 5% by mass or more and, for example, 50% by mass or less.
[0087] In the next second step, the second monomer component is polymerized in the presence of the first polymer. Specifically, the second monomer component and the above-mentioned polymerization initiator are mixed into an aqueous dispersion containing the first polymer. Preferably, the mixture is then aged.
[0088] The polymerization initiator may be the same as that used in the polymerization of the first monomer component described above. The polymerization initiator may be used alone or in combination of two or more kinds. The mixing ratio of the polymerization initiator may be appropriately set depending on the purpose and application, and is, for example, 0.05 parts by mass or more and 5 parts by mass or less relative to 100 parts by mass of the second monomer component.
[0089] The polymerization conditions are, for example, at normal pressure, a polymerization temperature of 30° C. or higher (preferably 50° C. or higher). The polymerization temperature is, for example, 95° C. or lower (preferably 85° C. or lower). The polymerization time is, for example, 0.5 hours or higher (preferably 1.5 hours or higher), and, for example, 20 hours or lower (preferably 10 hours or lower). The maturation time is, for example, 0.5 hours or more (preferably 1.5 hours or more) and, for example, 6 hours or less (preferably 3 hours or less).
[0090] In the polymerization of the second polymer, from the viewpoint of improving production stability, the above-mentioned emulsifier (surfactant) and additives may be blended in an appropriate ratio, if necessary.
[0091] Before or after polymerization of the second polymer, the pH can be adjusted to within the range of 7 to 11 by adding a neutralizing agent (such as ammonia).
[0092] Through the first and second steps, a dispersion liquid containing a first polymer and a second polymer is obtained. In the first method, when the second monomer component is polymerized on the surface of the first polymer, core-shell particles in which the first polymer as a core component is covered with the second polymer (shell) can be obtained. The solid content concentration of the dispersion liquid is, for example, 5% by mass to 50% by mass. The pH value of the dispersion is, for example, 6 to 11. When the pH value is within the above range, the dispersion stability is improved.
[0093] In this disclosure, pH is a value measured using a pH meter with the temperature adjusted to 25°C.
[0094] (1.3.3.2) Second method The second method includes a step (third step) of obtaining a second polymer by polymerizing a second monomer component containing (meth)acrylamide, and a step (fourth step) of obtaining a first polymer by polymerizing a first monomer component containing a (meth)acrylic acid ester and (meth)acrylonitrile in the presence of the second polymer.
[0095] In the third step, the second monomer component is polymerized. Specifically, the second monomer component and the above-mentioned polymerization initiator are mixed into water, and the second monomer component is polymerized in the water.
[0096] The polymerization initiator is preferably a water-soluble initiator, more preferably 4,4'-azobis(4-cyanovaleric acid). The polymerization initiator may be used alone or in combination of two or more kinds. The mixing ratio of the polymerization initiator may be appropriately set depending on the purpose and application, and is, for example, from 0.05 parts by mass to 10 parts by mass (preferably 5 parts by mass or less) per 100 parts by mass of the second monomer component.
[0097] The polymerization conditions are, for example, at normal pressure, a polymerization temperature of 30° C. or higher (preferably 50° C. or higher). The polymerization temperature is, for example, 95° C. or lower (preferably 85° C. or lower). The polymerization time is, for example, 0.5 hours or higher (preferably 1.5 hours or higher), and, for example, 20 hours or lower (preferably 10 hours or lower).
[0098] In the polymerization of the second polymer, the above-mentioned emulsifier (surfactant) may be added as necessary from the viewpoint of improving the production stability. The mixing ratio of the emulsifier may be appropriately set depending on the purpose and application.
[0099] In the polymerization of the second polymer, from the viewpoint of improving production stability, known additives such as, for example, a pH adjuster, a metal ion sequestering agent (e.g., ethylenediaminetetraacetic acid and its salts), and a molecular weight regulator (a chain transfer agent, for example, mercaptans and low molecular weight halogen compounds) may be blended in an appropriate ratio.
[0100] Before or after polymerization of the second polymer, the pH can be adjusted to within the range of 7 to 11 by adding a neutralizing agent (such as ammonia).
[0101] The second polymer may be provided as an aqueous solution. The solids concentration of the aqueous solution containing the second polymer is, for example, 5% by mass to 50% by mass.
[0102] In the next fourth step, the first monomer component is polymerized in the presence of the second polymer. Specifically, the first monomer component and the above-mentioned polymerization initiator are mixed into an aqueous solution containing the second polymer. Preferably, the mixture is then aged.
[0103] The polymerization initiator is preferably a water-soluble initiator, more preferably 4,4'-azobis(4-cyanovaleric acid).
[0104] The polymerization initiator may be used alone or in combination of two or more kinds. The mixing ratio of the polymerization initiator may be appropriately set depending on the purpose and application, and is, for example, 0.05 to 10 parts by mass relative to 100 parts by mass of the first monomer component.
[0105] The polymerization conditions are, for example, at normal pressure, a polymerization temperature of 30° C. or higher (preferably 50° C. or higher), for example, a polymerization temperature of 95° C. or lower (preferably 85° C. or lower), and a polymerization time of, for example, 0.5 hours or more and 20 hours or less (preferably 10 hours or less). The maturation time is, for example, 0.5 hours or more (preferably 1.5 hours or more), and, for example, 6 hours or less.
[0106] In the polymerization of the first polymer, from the viewpoint of improving production stability, the above-mentioned emulsifier (surfactant) and additives may be blended in an appropriate ratio, if necessary. The emulsifier is preferably an anionic surfactant, more preferably ammonium lauryl sulfate. The emulsifier may be used alone or in combination of two or more. The blending ratio of the emulsifier may be appropriately set according to the purpose and application, and is, for example, 0.1 to 5 parts by mass with respect to 100 parts by mass of the first monomer component.
[0107] Before or after polymerization of the first polymer, the pH can be adjusted to within the range of 7 to 11 by adding a neutralizing agent (such as ammonia).
[0108] A dispersion liquid containing the first polymer and the second polymer can be obtained through the third and fourth steps. Also, by polymerizing the relatively hydrophobic first polymer in the presence of the second polymer previously formed in water, it is possible to obtain core-shell particles in which the first polymer is coated with the second polymer (shell) as the core component. The solid content concentration of the dispersion is, for example, 5% by mass to 50% by mass. The pH of the dispersion is, for example, 6 to 11. When the pH is within the above range, the dispersion stability is improved.
[0109] The acrylic resin (C) can also be obtained by separately synthesizing the first polymer and the second polymer using the same method as above and then mixing them. The acrylic resin (C) is preferably synthesized by the above-mentioned first method or second method, and more preferably is a core-shell particle synthesized by the above-mentioned first method or second method. The acrylic resin (C) in the present disclosure is a polymer including a first polymer obtained by polymerizing at least a (meth)acrylic acid ester and (meth)acrylonitrile, and a second polymer obtained by polymerizing at least (meth)acrylamide. Therefore, if (meth)acrylonitrile and (meth)acrylamide are not used, the electrolyte resistance and heat resistance cannot be improved satisfactorily. It is also possible to start the polymerization reaction by blending the first and second monomer components together, but when they are blended together and polymerized, a random polymer of (meth)acrylonitrile and (meth)acrylamide may be formed. If the acrylic resin is a random polymer, it tends to have lower electrolyte resistance than the first polymer and lower heat resistance than the second polymer, so it is preferable to synthesize it by the above-mentioned first or second method.
[0110] In the acrylic resin (C) of the present disclosure, the ratio of the mass of the second polymer to the mass of the first polymer (amount of the second polymer / amount of the first polymer) is in the range of 0.1 or more and less than 100. The ratio of the amount of the second polymer / amount of the first polymer is preferably 0.2 or more, more preferably 0.3 or more. The ratio of the amount of the second polymer / amount of the first polymer is preferably 50 or less, more preferably 20 or less, even more preferably 15 or less, even more preferably 5 or less, even more preferably 2.5 or less, even more preferably 2.0 or less, and particularly preferably 1.5 or less. If the ratio of the amount of the second polymer / the amount of the first polymer is less than the lower limit, the heat resistance and electrolyte resistance are likely to decrease, and the battery performance (particularly the performance after high-temperature storage) when a secondary battery is produced is decreased, and the balance between safety and battery performance (i.e., output and life) is decreased. If the ratio of the amount of the second polymer / the amount of the first polymer is more than the upper limit, the ion permeability is likely to decrease, and the balance between safety and battery performance (i.e., output and life) is decreased when a secondary battery is produced.
[0111] The acrylic resin (C) preferably contains a first polymer obtained by polymerizing a first monomer component containing a (meth)acrylic acid ester, (meth)acrylonitrile, a carboxyl group-containing vinyl monomer, a hydroxyl group-containing vinyl monomer, and an N-substituted unsaturated carboxylic acid amide, and a second polymer obtained by polymerizing a second monomer component containing a (meth)acrylamide, a carboxyl group-containing vinyl monomer, and a hydroxyl group-containing vinyl monomer. In this case, the ratio of the mass of the second polymer to the mass of the first polymer (amount of second polymer / amount of first polymer) is preferably 0.2 or more, more preferably 0.3 or more, and is preferably 5 or less, more preferably 2.5 or less, even more preferably 2.0 or less, and particularly preferably 1.5 or less.
[0112] The mass of the first polymer and the mass of the second polymer can be calculated by identifying the first monomer component and the second monomer component constituting each polymer, and based on the ratio of the identified monomers or the amount of each monomer charged.
[0113] When the acrylic resin (C) is in a particulate form, the average particle size is, for example, 10 nm or more (preferably 100 nm or more, more preferably 300 nm or more) and, for example, 3000 nm or less (preferably 2000 nm or less). The average particle size refers to the average primary particle size, and is a value determined by measurement using a particle size measuring device (for example, FPAR1000 manufactured by Otsuka Electronics Co., Ltd.).
[0114] Regarding the content ratios of the above-mentioned conductive carbon material (A), olefin resin (B) and acrylic resin (C), from the viewpoint of the balance between safety when a secondary battery is produced and battery performance (i.e., output and life), it is preferable that the content of the conductive carbon material (A) is 1 mass% to 30 mass% relative to the total mass of the composition, the content of the olefin resin (B) is 30 mass% to 90 mass% relative to the total mass of the composition, and the content of the acrylic resin (C) is 1 mass% to 20 mass% relative to the total mass of the composition.
[0115] (1.4) Additives (D) The composition of the present disclosure may contain an additive (D) as necessary. Depending on the type of additive (D), various functions can be imparted to the composition of the present disclosure.
[0116] Examples of additives (D) include thermally expandable microcapsules having a maximum volume expansion temperature of 70°C or more and 180°C or less (hereinafter simply referred to as "thermally expandable microcapsules"), inorganic oxide fillers, curable resin fillers, scaly fillers, binder resins, synthetic rubbers, non-solid contents, etc.
[0117] Among them, from the viewpoint of assisting the shutdown function of the olefin resin (B), it is preferable to contain carboxymethyl cellulose (CMC) as the additive (D).For the same reason, it is preferable to contain at least one of a thermally expandable microcapsule having a maximum volume expansion temperature of 70°C or more and 180°C or less and an inorganic oxide filler (particularly aluminum oxide) as the additive (D).
[0118] The term "thermally expandable microcapsule" refers to a particle having an outer shell made of a thermoplastic resin and a volatile expanding agent, which is a core component, encapsulated in the outer shell. In detail, the thermally expandable microcapsule is preferably one that, in contact with an electrolyte solution described below, softens and foams to cause a volume expansion when exposed to a temperature (e.g., 70°C to 160°C) immediately before the onset of thermal runaway due to abnormal heat generation in a lithium ion secondary battery. The "maximum volume expansion temperature" refers to the temperature at which the expanded volume of the thermally expandable microcapsule becomes maximum when the volatile expanding agent contained in the thermally expandable microcapsule gasifies and the thermally expandable microcapsule expands in volume. The temperature at which the volatile expanding agent contained in the thermally expandable microcapsule gasifies and the thermally expandable microcapsule starts to expand in volume is called the "volume expansion start temperature."
[0119] When additive (D) is contained, the content of additive (D) is preferably 1 mass % to 50 mass % relative to the total mass of the composition. When the content of additive (D) is within the above range, the shutdown function due to the properties of additive (D) can be more effectively exhibited. The content of the additive (D) has a small effect on the content ratio of the conductive carbon material (A) and the olefin resin (B), and is preferably 40 mass% or less, more preferably 30 mass% or less, based on the total mass of the composition, from the viewpoint of effectively exerting the shutdown function and maintaining the battery performance. Also, the content of the additive (D) is preferably 5 mass% or more, more preferably 10 mass% or more, based on the total mass of the composition, from the viewpoint of effectively exerting the shutdown function.
[0120] (1.4.1) Viscosity stabilizers The composition of the present disclosure may contain a thickening stabilizer. The composition of the present disclosure may not contain a thickening stabilizer. When the composition of the present disclosure contains a thickening stabilizer and is used as a raw material for the undercoat layer, it becomes possible to stably disperse particles when preparing a slurry for the undercoat layer.
[0121] Examples of thickening stabilizers include carboxymethylcellulose (CMC), polyvinyl alcohol (PVA), methylcellulose (MC), hydroxypropylcellulose (HPC), polyethylene glycol (PEG), polyethylene oxide (PEO), polyvinylpyrrolidone (PVP), polyacrylic acid (PAA), polycarboxylate ammonium salts, sugars exemplified by glycosides such as lecithin and saponin, and polysaccharides such as xanthan gum, polyether polyols such as sucrose polyether polyol, polyoxypropylene sorbitol ether, trimethylolpropane polyether polyol, and pentaerythritol polyether polyol, oxidized starch, starch phosphate, casein, and various modified starches.
[0122] The content of the thickening stabilizer is preferably 1% by mass to 50% by mass relative to the total amount of the composition. From the viewpoint of effectively exerting the shutdown function and maintaining the battery performance, the content of the thickening stabilizer is preferably 15% by mass or less, more preferably 10% by mass or less, relative to the total amount of the composition. From the viewpoint of more effectively dispersing particles when preparing the slurry for the undercoat layer, the content of the thickening stabilizer is preferably 2% by mass or more, more preferably 3% by mass or more, relative to the total amount of the composition.
[0123] Commercially available CMC products include "1130", "1140", "1240", "1250", "1260", "1330", "2200", and "DL100L" manufactured by Daicel Miraize Co., Ltd.
[0124] (1.4.2) Thermally expandable microcapsules The composition of the present disclosure preferably contains thermally expandable microcapsules. When the composition of the present disclosure contains thermally expandable microcapsules and is used as a raw material for an undercoat layer, the thermally expandable microcapsules undergo volumetric expansion due to abnormal heat generation in the lithium ion secondary battery, efficiently increasing the DC resistance of the electrode and improving the safety of the lithium ion secondary battery.
[0125] The volume expansion starting temperature of the thermally expandable microcapsules is preferably 120°C to 130°C. The maximum volume expansion temperature of the thermally expandable microcapsules is preferably 145°C to 155°C.
[0126] The thermoplastic resin constituting the outer shell preferably contains a (co)polymer containing vinylidene chloride and a (co)polymer containing (meth)acrylonitrile. This allows the thermoplastic resin constituting the outer shell to have excellent electrolyte resistance, thermoplasticity, and excellent gas barrier properties. In particular, from the viewpoint of electrolyte resistance, the thermoplastic resin constituting the outer shell is preferably a (co)polymer containing (meth)acrylonitrile as the main component (51 mass% or more). The raw material of the thermoplastic resin constituting the outer shell may contain a crosslinkable monomer in addition to a polymerizable monomer in order to improve the foaming properties and heat resistance of the resulting thermally expandable microcapsule.
[0127] The boiling point of the volatile expanding agent is preferably selected so that the maximum volume expansion temperature of the thermally expandable microcapsules is higher than the softening point of the olefin resin (B). The boiling point is preferably selected so that the volume expansion start temperature of the thermally expandable microcapsules is equal to the softening point of the olefin resin (B). This allows the DC resistance of the electrode to increase efficiently when the temperature of the undercoat layer rises above the softening point of the olefin resin (B) due to heat generation in the lithium ion secondary battery. As a result, the safety of the lithium ion secondary battery is further improved. Examples of the volatile expanding agent include low molecular weight hydrocarbons having a boiling point of 100°C or less, non-flammable or flame-retardant compounds, etc. As the low molecular weight hydrocarbons having a boiling point of 100°C or less, low molecular weight hydrocarbons are preferably used. Examples of the low molecular weight hydrocarbons include propane, propylene, n-butane, isobutane, butene, isobutene, isopentane, neopentane, n-pentane, n-hexane, isohexane, heptane, and petroleum ether. Examples of the non-flammable or flame-retardant compounds include halogenated hydrocarbons (e.g., methyl chloride, methylene chloride, fluorotrichloromethane, difluorodichloromethane, chlorotrifluoromethane, etc.), and chlorofluorocarbons. The volatile expanding agent may be used alone or in combination of two or more.
[0128] The particle size of the thermally expandable microcapsules is not particularly limited, and is preferably from 1 μm to 40 μm, more preferably from 3 μm to 30 μm, and further preferably from 5 μm to 25 μm.
[0129] The particle size of the thermally expandable microcapsules is the particle size (particle size distribution D50, median diameter) equivalent to 50% cumulative volume from the fine particle side in the volume-based particle size distribution measured using a particle size distribution measuring device based on the laser light diffraction scattering method.
[0130] The content of the thermally expandable microcapsules is preferably 0% by mass to 50% by mass with respect to the total mass of the composition. The content of the thermally expandable microcapsules has a small effect on the content ratio of the conductive carbon material (A) and the olefin resin (B), and is preferably 50% by mass or less, more preferably 40% by mass or less, with respect to the total mass of the composition, from the viewpoint of maintaining the shutdown function and battery performance. The content of the thermally expandable microcapsules is preferably 5% by mass or more, more preferably 10% by mass or more, with respect to the total mass of the composition, from the viewpoint of enhancing the shutdown function due to the thermal expansion of the thermally expandable microcapsules during abnormal heat generation.
[0131] As the thermally expandable microcapsules, commercially available products may be used. Commercially available thermally expandable microcapsules include the "Matsumoto Microsphere (registered trademark)" series manufactured by Matsumoto Yushi Pharmaceutical Co., Ltd., the "EXPANCEL (registered trademark)" series manufactured by Akzo Nobel, and the "ADVANCELL (registered trademark)" series manufactured by Sekisui Chemical Co., Ltd.
[0132] (1.4.3) Inorganic oxide fillers The composition of the present disclosure may contain an inorganic oxide filler. The composition of the present disclosure may not contain an inorganic oxide filler. When the composition of the present disclosure contains an inorganic oxide filler, the inorganic oxide filler functions as a filler. Increasing the content of the inorganic oxide filler contributes to improving the heat resistance of the positive electrode, while minimizing the content of the inorganic oxide filler forms an undercoat layer that adheres closely to the positive electrode mixture layer, and the undercoat layer melts in the event of an internal short circuit, contributing to improving safety. Furthermore, by selecting the type and physical properties of the inorganic oxide filler, it is also possible to decompose the electrolyte and generate gas when the battery is overcharged.
[0133] Examples of inorganic oxide fillers include aluminum oxide (α-Al2O3, γ-Al2O3), aluminum hydroxide (Al(OH)3), boehmite (AlOOH)), magnesia (magnesium oxide: MgO), magnesium hydroxide (Mg(OH)2), zirconia (ZrO2), titania (TiO2), silica (SiO2), silicon dioxide (SiO2), silicon carbide (SiC), aluminum nitride (AlN), boron nitride (BN), mica, and graphite oxide (e.g., expanded graphite). The inorganic oxide filler may be used alone or in combination of two or more. Among them, it is preferable that the inorganic oxide filler contains aluminum oxide.
[0134] The shape of the inorganic oxide filler is not particularly limited, and examples thereof include a spherical shape, a needle shape, an ellipsoid shape, a plate shape, a scale shape, etc. The particle size of the inorganic oxide filler is not particularly limited, and is preferably 0.01 μm to 5 μm. The particle size of the inorganic oxide filler is the particle size (particle size distribution D50, median diameter) that corresponds to 50% by volume cumulative from the fine particle side in the volume-based particle size distribution measured by a particle size distribution measuring device based on the laser light diffraction scattering method.
[0135] The content of the inorganic oxide filler is preferably 0% by mass to 50% by mass relative to the total mass of the composition. The content of the inorganic oxide filler has a small effect on the content ratio of the conductive carbon material (A) and the olefin resin (B), and from the viewpoint of maintaining the shutdown function and battery performance, the content is preferably 40% by mass or less, more preferably 30% by mass or less, relative to the total mass of the composition. In addition, the content of the inorganic oxide filler is preferably 5% by mass or more, more preferably 10% by mass or more, relative to the total mass of the composition, from the viewpoint of suppressing the fluidity of the olefin resin (B) dissolved in the undercoat layer at high temperatures and maintaining the shutdown function for a long period of time.
[0136] (1.4.4) Binder resin The composition of the present disclosure may contain a binder resin other than the above-mentioned olefin-based resin (B) and acrylic-based resin (C). In this way, when the composition of the present disclosure is used as a raw material for the undercoat layer, the binder resin can improve the physical properties (e.g., electrolyte permeability and peel strength) of the undercoat layer and can also improve the battery performance of the lithium ion secondary battery.
[0137] Examples of the binder resin include polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF copolymer, polyvinyl alcohol, hydroxypropyl cellulose, and diacetyl cellulose. The PVDF copolymer is a copolymer of vinylidene fluoride and other monomers, and examples of the PVDF copolymer include PVDF-HFP (hexafluoropropylene) and PVDF-PEO (polyoxyethylene). Among these, the binder resin preferably contains PVDF from the viewpoint of reducing the resistance of the undercoat layer.
[0138] As the binder resin, a commercially available product may be used. Commercially available PVDF products include the Kureha (registered trademark) KF Polymer series manufactured by Kureha Corporation, such as "W#1100", "W#1300", "W#1700", "W#7200", and "W#7300".
[0139] The binder resin may be used alone or in combination of two or more kinds. The content of the binder resin is preferably 1% by mass to 30% by mass with respect to the total mass of the composition. The shutdown function depends on the balance between the content of the binder resin and the total content of the olefin resin (B) and the acrylic resin (C). When the content ratio of the binder resin to the total mass of the composition is high, the content ratio of the olefin resin (B) and the acrylic resin to the total mass of the composition is low, and therefore the shutdown function may be reduced. When the content of the binder resin is within the above range, it is possible to achieve both the processability of the composition (e.g., slurry for the undercoat layer) and the assurance of the shutdown function. The content of the binder resin is preferably 15% by mass or less, more preferably 10% by mass or less, based on the total mass of the composition, from the viewpoint of ensuring the shutdown function in relation to the contents of the olefin resin (B) and the acrylic resin (C). Also, the content of the binder resin is preferably 2% by mass or more, more preferably 3% by mass or more, based on the total mass of the composition, from the viewpoint of the processability of the composition (e.g., slurry for the undercoat layer).
[0140] (1.4.5) Synthetic rubber The composition of the present disclosure may contain a synthetic rubber. When the composition of the present disclosure is used as a raw material for an undercoat layer, the adhesion between the undercoat layer and the current collector is improved, and the battery resistance can be further reduced.
[0141] Examples of synthetic rubbers include styrene butadiene rubber (SBR), acrylonitrile-butadiene rubber, acrylonitrile-butadiene-styrene rubber, hydrogenated styrene butadiene rubber (HSBR), butylene rubber, polybutadiene, polyisoprene rubber, etc. Among them, from the viewpoint of low resistance of the undercoat layer, it is preferable for the synthetic rubber to be appropriately mixed with a water-dispersible binder such as an emulsion of SBR, and it is more preferable for it to contain SBR.
[0142] The shape of the synthetic rubber is not particularly limited, and it may be in the form of particles. As the synthetic rubber, commercially available products may be used. Examples of commercially available synthetic rubber products include "TRD2001" (aqueous dispersion of styrene butadiene rubber particles) manufactured by JSR Corporation.
[0143] (1.4.6) Non-solids The composition of the present disclosure may contain non-solid contents. Examples of the non-solid contents include various blending components derived from the slurry for the undercoat layer (e.g., surfactants, dispersants, wetting agents, defoamers, etc.), water, etc.
[0144] (1.5) Properties of the composition Various physical properties of the composition of the present disclosure will be described.
[0145] From the viewpoint of forming an electrode which is excellent in safety, has low DC resistance during initial charge / discharge, and is suppressed from increasing in DC resistance in a high-temperature environment, the composition of the present disclosure preferably has a ratio of particle size distribution D99 to particle size distribution D10 (D99 / D10) of 35 or less, as measured by a laser light diffraction scattering method.
[0146] "Particle size distribution D99 measured by laser light diffraction scattering method" refers to the particle size corresponding to the cumulative 99% by volume from the fine particle side in the volume-based particle size distribution measured by a particle size distribution measuring device based on the laser light diffraction scattering method. The method for measuring D99 is the same as that described in the Examples. "Particle size distribution D10 measured by laser light diffraction scattering method" refers to the particle size corresponding to 10% by volume cumulative from the fine particle side in the volume-based particle size distribution measured by a particle size distribution measuring device based on laser light diffraction scattering method. The method for measuring D10 is the same as that described in the Examples.
[0147] The ratio (D99 / D10) of 35 or less indicates that the number of aggregates of the components in the composition is small (in other words, the number of components dispersed in the composition is large). That is, the lower the ratio (D99 / D10), the fewer the number of aggregates of the components in the composition. The conductive carbon material (A) in the composition is uniformly dispersed, and a uniform conductive path is easily formed in the undercoat layer. This makes it possible to suppress the initial DC resistance of the battery charge / discharge and the increase in DC resistance after long-term storage in a high-temperature environment. Furthermore, the olefin resin (B) and the acrylic resin (C) in the composition are uniformly dispersed, making it easier to efficiently exert the shutdown function. As a result, the composition of the present disclosure is excellent in safety, and makes it possible to form an electrode in which the DC resistance at the initial stage of charge / discharge is kept low and the increase in DC resistance in a high-temperature environment is significantly suppressed. Therefore, a lithium-ion secondary battery with excellent battery performance is obtained.
[0148] From the viewpoint of improving the safety and battery performance of the lithium ion secondary battery, the ratio (D99 / D10) is more preferably from 3.0 to 30.0, further preferably from 3.0 to 22.0, and particularly preferably from 3.0 to 15.0.
[0149] Methods for adjusting the ratio (D99 / D10) within the above range include a kneader, a two-roll mill, a three-roll mill, a planetary mixer, a ball mill, a horizontal sand mill, a vertical sand mill, an annular bead mill, an attritor, a high shear mixer, a disperser, a film mix, ultrasonic waves, and a high-pressure homogenizer.
[0150] The composition of the present disclosure preferably has a particle size distribution D99 of 20 μm or less as measured by a laser light diffraction scattering method. The smaller the aggregates of fine particles, the better the dispersibility of the materials contained in the composition. When D99 is 20 μm or less, it is easier to improve the safety and battery performance of a lithium ion secondary battery compared to when D99 exceeds 20 μm. From the viewpoint of improving the safety and battery performance of a lithium ion secondary battery, D99 of the composition is more preferably 2.0 μm to 20.0 μm, further preferably 2.0 μm to 15.0 μm, and particularly preferably 2.0 μm to 10.0 μm.
[0151] Methods for adjusting the D99 of the composition to within the above range include a kneader, a two-roll mill, a three-roll mill, a planetary mixer, a ball mill, a horizontal sand mill, a vertical sand mill, an annular bead mill, an attritor, a high shear mixer, a Disper, a Filmix, ultrasonic waves, and a high-pressure homogenizer.
[0152] The composition of the present disclosure has a particle size distribution D10 measured by a laser light diffraction scattering method of preferably 0.1 μm to 1.5 μm, more preferably 0.1 μm to 1.0 μm, and even more preferably 0.1 μm to 0.7 μm. When D10 is within the above range, the dispersibility of the materials contained in the composition is excellent, and the safety and battery performance of the lithium ion secondary battery are more easily improved than when D10 is not within the above range.
[0153] Methods for adjusting D10 within the above range include a kneader, a two-roll mill, a three-roll mill, a planetary mixer, a ball mill, a horizontal sand mill, a vertical sand mill, an annular bead mill, an attritor, a high shear mixer, a disperser, a filmix, ultrasonic waves, and a high-pressure homogenizer.
[0154] The composition of the present disclosure preferably has a ratio (D99 / D50) of particle size distribution D99 to particle size distribution D50 (also simply referred to as "D50") of 20 or less, as measured by a laser light diffraction scattering method. The ratio (D99 / D50) of 20 or less indicates that the size of aggregates is suppressed relative to the median diameter of fine particles in the composition. The ratio (D99 / D50) of 20 or less provides excellent dispersibility of the composition. This makes it easier to improve the safety and battery performance of a lithium ion secondary battery compared to a case where the ratio (D99 / D50) is more than 20. From the viewpoint of improving the safety and battery performance of a lithium ion secondary battery, the ratio (D99 / D50) is more preferably 2.0 to 16.0, even more preferably 2.0 to 10.0, and particularly preferably 2.0 to 6.0.
[0155] "Particle size distribution D50 measured by laser light diffraction scattering method" refers to the particle size corresponding to cumulative 50 volume % from the fine particle side in the volume-based particle size distribution measured by a particle size distribution measuring device based on laser light diffraction scattering method. The method for measuring D50 is the same as the method described in the Examples.
[0156] Methods for adjusting the ratio (D99 / D50) within the above range include a kneader, a two-roll mill, a three-roll mill, a planetary mixer, a ball mill, a horizontal sand mill, a vertical sand mill, an annular bead mill, an attritor, a high shear mixer, a disperser, a filmix, an ultrasonic wave, and a high-pressure homogenizer.
[0157] The particle size distribution D50 of the composition of the present disclosure measured by a laser light diffraction scattering method is not particularly limited, and is preferably 0.5 μm to 5.0 μm, more preferably 0.5 μm to 3.0 μm, and further preferably 0.5 μm to 2.0 μm. If D50 is within the above range, the dispersibility of the composition is excellent, and the safety and battery performance of the lithium ion secondary battery are likely to be improved.
[0158] Methods for adjusting D50 within the above range include a kneader, a two-roll mill, a three-roll mill, a planetary mixer, a ball mill, a horizontal sand mill, a vertical sand mill, an annular bead mill, an attritor, a high shear mixer, a disperser, a filmix, ultrasonic waves, and a high-pressure homogenizer.
[0159] The composition of the present disclosure has a particle size distribution D90 (also simply referred to as "D90") measured by a laser light diffraction scattering method of preferably 1.0 μm to 10.0 μm, more preferably 1.0 μm to 7.0 μm, and even more preferably 1.0 μm to 4.0 μm. When D90 is within the above range, the composition has excellent dispersibility, and the safety and battery performance of the lithium ion secondary battery are easily improved. "Particle size distribution D90 measured by laser light diffraction scattering method" refers to the particle size corresponding to cumulative 90 volume % from the fine particle side in the volume-based particle size distribution measured by a particle size distribution measuring device based on laser light diffraction scattering method. The method for measuring D90 is the same as the method described in the Examples.
[0160] Methods for adjusting D90 within the above range include a kneader, a two-roll mill, a three-roll mill, a planetary mixer, a ball mill, a horizontal sand mill, a vertical sand mill, an annular bead mill, an attritor, a high shear mixer, a disperser, a filmix, ultrasonic waves, and a high-pressure homogenizer.
[0161] (1.6) Method for producing the composition The method for producing the composition of the present disclosure preferably includes mixing the conductive carbon material (A), the olefin resin (B), and the acrylic resin (C) to prepare a mixture (hereinafter also referred to as the "mixing step"), and dispersing the mixture using a dispersion roll (hereinafter also referred to as the "dispersing step"). The mixing step and the dispersing step can be performed in this order, and when performed in this order, another step (for example, a step of kneading the mixture) may be included between the mixing step and the dispersing step.
[0162] (1.6.1) Mixing process In the mixing step, the conductive carbon material (A), the olefin resin (B), and the acrylic resin (C) are mixed to prepare a mixture. The mixing method is not particularly limited and may be any known method. The amounts of the conductive carbon material (A), the olefin-based resin (B), and the acrylic resin (C) are the same as the ranges already described for the contents of the conductive carbon material (A), the olefin-based resin (B), and the acrylic resin (C) in the composition of the present disclosure.
[0163] (1.6.2) Dispersion process In the dispersion step, the mixture is dispersed using a dispersion roll. This results in a composition in which the raw materials are more dispersed than in the mixture before the dispersion step. As a result, when the electrode thus prepared is provided in a secondary battery, the obtained composition can not only reduce the DC resistance during initial charging and discharging, but also effectively suppress an increase in DC resistance in a high-temperature environment, compared to a case in which the dispersion step is not performed. The treatment of dispersing the mixture using a dispersing roll is also called a “dispersion treatment.” The mixture may be kneaded in advance before the dispersion treatment.
[0164] The dispersion method is not particularly limited, and examples thereof include a method using a kneading device. Examples of the kneading device include a kneader, a two-roll mill, a three-roll mill, a planetary mixer, a ball mill, a horizontal sand mill, a vertical sand mill, an annular bead mill, an attritor, a high shear mixer, a disperser, a film mix, an ultrasonic wave, and a high-pressure homogenizer. Among them, the kneading device is preferably a three-roll mill from the viewpoint of dispersing the fine particles more uniformly in the mixture. When a kneading device is used, the method of dispersing the mixture includes batch dispersion, pass dispersion, and circulation dispersion. The method of dispersing the mixture may be a combination of two or more methods. "Batch dispersion" refers to a method of dispersing the mixture using only a kneading device without using piping or the like. "Pass dispersion" refers to a method of dispersing the mixture by passing the mixture through the kneading device using a kneading system. The kneading system includes a kneading device, a first tank that supplies the mixture to the kneading device through piping, and a second tank that receives the mixture after the kneading process. "Circulation dispersion" refers to a method of dispersing the mixture by returning the mixture after the kneading process in the second tank to the first tank and circulating it.
[0165] The three-roll mill will be described with reference to Fig. 4. In Fig. 4, the reference character D1 indicates the rotation direction of the first roll 91 (hereinafter also referred to as the "feed roll 91"). The reference character D2 indicates the rotation direction of the second roll 92 (hereinafter also referred to as the "intermediate roll 92"). The reference character D3 indicates the rotation direction of the third roll 93 (hereinafter also referred to as the "finishing roll 93").
[0166] As shown in Fig. 4, the three-roll mill 90 includes a feed roll 91, an intermediate roll 92, a finishing roll 93, and a blade 94. The feed roll 91 and the intermediate roll 92 are disposed with a first distance L1 (see Fig. 4) between them. The intermediate roll 92 and the finishing roll 93 are disposed with a second distance L2 (see Fig. 4) between them. The blade 94 is disposed so as to come into contact with the surface of the finishing roll 93.
[0167] In the three-roll mill 90, as shown in Fig. 4, the mixture 1110 is stored in the upper space formed by the feed roll 91 and the intermediate roll 92. The mixture 1110 attached to the surface of the feed roll 91 is transferred to the surface of the intermediate roll 92. The mixture 1110 attached to the surface of the intermediate roll 92 is transferred to the surface of the finishing roll 93. The mixture 1110 attached to the surface of the finishing roll 93 is scraped off by the blade 94.
[0168] Each of the feed roll 91, the intermediate roll 92, and the finishing roll 93 may be a roll used in a known three-roll mill. The feed roll 91, the intermediate roll 92, and the finishing roll 93 each have approximately the same diameter. The blade 94 may be, for example, a doctor blade.
[0169] The rotation speeds of the feed roll 91, the intermediate roll 92, and the finishing roll 93 are not particularly limited, and may be in the order of speed from the feed roll 91, the intermediate roll 92, to the finishing roll 93. The rotation speed of the feed roll 91 is not particularly limited, but is preferably 5 rpm (revolutions per minute) to 84 rpm, and more preferably 16 rpm to 56 rpm. The rotation speed of the intermediate roll 92 is not particularly limited, but is preferably 16 rpm to 240 rpm, and more preferably 50 rpm to 160 rpm. The rotation speed of the finishing roll 93 is not particularly limited, but is preferably 50 rpm to 600 rpm, and more preferably 150 rpm to 400 rpm. The ratio of the rotation speed of the intermediate roll 92 to the rotation speed of the charge roll 91 (rotation speed of the intermediate roll 92 / rotation speed of the charge roll 91) is preferably 2.0 to 4.0, more preferably 2.5 to 3.5, from the viewpoint of uniformly dispersing the fine particles in the mixture. The ratio of the rotation speed of the finishing roll 93 to the rotation speed of the charge roll 91 (rotation speed of the finishing roll 93 / rotation speed of the charge roll 91) is preferably 5.0 to 12.0, more preferably 6.5 to 10.0, from the viewpoint of uniformly dispersing the fine particles in the mixture.
[0170] The first interval L1 is not particularly limited, and from the viewpoint of uniformly dispersing the fine particles in the mixture, it is preferably 0 mm to 0.05 mm, and more preferably 0 mm to 0.02 mm. The second distance L2 is not particularly limited, and is preferably 0 mm to 0.05 mm, and more preferably 0 mm to 0.02 mm, from the viewpoint of uniformly dispersing the fine particles in the mixture.
[0171] The number of dispersion treatments (hereinafter also referred to as the "number of treatments") may be one or more. In particular, the number of treatments is preferably three. When the number of treatments is three, the conductive carbon material (A) and the olefin resin (B) in the mixture are more likely to be uniformly dispersed than when the number of treatments is two or less or four or more. As a result, a composition is obtained that can be used to form a lithium ion secondary battery in which the DC resistance at the beginning of charging and discharging and the increase in the DC resistance under a high-temperature environment (especially after long-term storage) are more effectively suppressed.
[0172] (2) Undercoat layer The undercoat layer of the present disclosure contains the composition of the present disclosure described above. The composition of the present disclosure is as described above, so a description thereof will be omitted here.
[0173] The thickness of the undercoat layer is not particularly limited. The thickness of the undercoat layer is preferably 50 μm or less, more preferably 20 μm or less, from the viewpoint of suppressing the DC resistance of the lithium ion secondary battery in normal operation. The thickness of the undercoat layer is preferably 0.1 μm or more, more preferably 0.2 μm or more, from the viewpoint of increasing the DC resistance when the lithium ion secondary battery is abnormally heated and more reliably exhibiting the shutdown function.
[0174] The position where the undercoat layer is formed is preferably at least a part of at least one of the main surfaces of the positive electrode current collector, and may be appropriately selected depending on the coating pattern of the positive electrode mixture layer (for example, intermittent coating, stripe coating, etc.).
[0175] (3) Electrode The electrode of the present disclosure includes a current collector, the undercoat layer of the present disclosure described above, and a composite layer. The term "electrode" refers to at least one of the positive electrode and the negative electrode of a lithium ion secondary battery.
[0176] Since the electrode of the present disclosure has the above-mentioned configuration, it is possible to fabricate a lithium ion secondary battery that is excellent in safety and in which an increase in DC resistance is suppressed during the initial charge / discharge period and in high-temperature environments (especially after long-term storage).
[0177] In the electrode of the present disclosure, it is preferable that the electrode has a current collector, an undercoat layer, and a composite layer laminated in this order. As a result, the electrode of the present disclosure increases the electrical resistance between the current collector and the composite layer when the temperature of the lithium ion secondary battery rises suddenly. This suppresses overheating of the lithium ion secondary battery. Therefore, the electrode of the present disclosure can improve the safety of the lithium ion secondary battery. Furthermore, the electrode of the present disclosure can suppress an increase in the DC resistance of the lithium ion secondary battery even if the lithium ion secondary battery is stored for a long period of time in a high-temperature environment.
[0178] The electrode of the present disclosure may be a positive electrode or a negative electrode. Among them, the electrode of the present disclosure is preferably a positive electrode. When the electrode of the present disclosure is a positive electrode, the electric resistance of the positive electrode increases, so that the resulting lithium ion secondary battery can exhibit a good shutdown function.
[0179] (3.1) Positive electrode The positive electrode of the present disclosure may include a current collector (hereinafter also referred to as a "positive electrode current collector"), an undercoat layer, and a mixture layer (hereinafter also referred to as a "positive electrode mixture layer").
[0180] Positive electrodes of the present disclosure include a first positive electrode configuration, a second positive electrode configuration, a third positive electrode configuration, and a fourth positive electrode configuration. The first positive electrode configuration indicates a configuration in which an undercoat layer and a positive electrode mixture layer are laminated in this order on both main surfaces of a current collector. The second positive electrode configuration indicates a configuration in which an undercoat layer and a positive electrode mixture layer are laminated in this order on one main surface of a current collector, and an undercoat layer is laminated on the other main surface of the current collector. The third positive electrode configuration indicates a configuration in which an undercoat layer and a positive electrode mixture layer are laminated in this order on one main surface of a current collector, and a positive electrode mixture layer is laminated on the other main surface of the current collector. The fourth positive electrode configuration indicates a configuration in which an undercoat layer and a positive electrode composite layer are laminated in this order on one main surface of a current collector, and neither the undercoat layer nor the positive electrode composite layer is laminated on the other main surface of the current collector.
[0181] (3.1.1) Positive electrode current collector Examples of the material of the positive electrode current collector include aluminum, nickel, stainless steel (SUS), copper, etc. "Aluminum" includes pure aluminum and aluminum alloys.
[0182] (3.1.2) Undercoat layer The details of the undercoat layer and the composition forming it have been described above, and therefore a detailed description thereof will be omitted here.
[0183] (3.1.3) Positive electrode composite layer The positive electrode mixture layer contains a positive electrode active material and a binder.
[0184] (3.1.3.1) Positive electrode active material The positive electrode active material is not particularly limited as long as it is a material capable of absorbing and releasing lithium ions, and can be appropriately adjusted depending on the application of the lithium ion secondary battery.
[0185] Examples of the positive electrode active material include a first oxide and a second oxide. The first oxide contains lithium (Li) and nickel (Ni) as constituent metal elements. The second oxide contains Li, Ni, and at least one metal element other than Li and Ni as constituent metal elements. Examples of metal elements other than Li and Ni include transition metal elements and typical metal elements. The second oxide preferably contains the metal elements other than Li and Ni in an amount equivalent to or less than Ni in terms of atomic number. The metal elements other than Li and Ni may be, for example, at least one selected from the group consisting of Co, Mn, Al, Cr, Fe, V, Mg, Ca, Na, Ti, Zr, Nb, Mo, W, Cu, Zn, Ga, In, Sn, La, and Ce. The positive electrode active material may be used alone or in combination of two or more.
[0186] The positive electrode active material preferably contains a lithium-containing composite oxide (hereinafter, sometimes referred to as "NCM") represented by the following formula (X). The lithium-containing composite oxide (X) has the advantages of high energy density per unit volume and excellent thermal stability.
[0187] LiNi a Co b Mn c O2… Formula (X)
[0188] In formula (X), a, b and c each independently represent more than 0 and less than 1, and the sum of a, b and c is 0.99 or more and 1.00 or less.
[0189] A specific example of NCM is LiNi 0.33 Co 0.33 Mn 0.33 O2, LiNi 0.5 Co 0.3 Mn 0.2 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.8 Co 0.1 Mn 0.1 Examples include O2.
[0190] The positive electrode active material may contain a lithium-containing composite oxide (hereinafter sometimes referred to as "NCA") represented by the following formula (Y).
[0191] Li t Ni 1-x-y Co x Al y O2… Formula (Y)
[0192] In formula (Y), t is 0.95 or more and 1.15 or less, x is 0 or more and 0.3 or less, y is 0.01 or more and 0.2 or less, and the sum of x and y is less than 0.5.
[0193] A specific example of NCA is LiNi 0.8 Co0.15 Al 0.05 Examples include O2.
[0194] The content of the positive electrode active material is preferably 10 mass % or more, more preferably 30 mass % or more, still more preferably 50 mass % or more, and particularly preferably 70 mass % or more, based on the total amount of the positive electrode mixture layer. The content of the positive electrode active material is preferably 99.9 mass % or less, and more preferably 99 mass % or less, based on the total amount of the positive electrode mixture layer.
[0195] (3.1.3.2) Binder Examples of the binder include polyvinyl acetate, polymethyl methacrylate, nitrocellulose, fluororesin, and rubber particles. Examples of fluororesins include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), vinylidene fluoride-hexafluoropropylene copolymer, and the like. Examples of the rubber particles include styrene-butadiene rubber particles and acrylonitrile rubber particles. Among these, from the viewpoint of improving the oxidation resistance of the positive electrode mixture layer, it is preferable that the binder contains a fluororesin. The binder may be used alone or in combination of two or more kinds. The content of the binder is preferably 0.1% by mass or more and 4% by mass or less based on the total amount of the positive electrode mixture layer from the viewpoint of achieving both the physical properties of the positive electrode mixture layer (eg, electrolyte permeability, peel strength, etc.) and the battery performance.
[0196] (3.1.3.3) Conductive additives The positive electrode mixture layer may further contain a conductive assistant. As the conductive assistant, a known conductive assistant can be used. As the known conductive assistant, a conductive carbon material is preferable. As the conductive carbon material, graphite, carbon black, conductive carbon fiber, fullerene, etc. can be mentioned. As the conductive carbon fiber, carbon nanotube, carbon nanofiber, carbon fiber, etc. can be mentioned. As the graphite, for example, artificial graphite, natural graphite, etc. can be mentioned. As the natural graphite, for example, flake graphite, lump graphite, and earthy graphite can be mentioned. The conductive assistant may be used alone or in combination of two or more kinds. The material of the conductive assistant may be a commercially available product.
[0197] (3.1.3.4) Other ingredients The positive electrode mixture layer may contain other components such as a thickener, a surfactant, a dispersant, a wetting agent, and a defoamer.
[0198] (3.2) Negative electrode The negative electrode of the present disclosure includes a current collector (hereinafter also referred to as a "negative electrode current collector") and a mixture layer (hereinafter also referred to as a "negative electrode mixture layer"), and may also include an undercoat layer.
[0199] Negative electrodes of the present disclosure may include a first negative electrode configuration, a second negative electrode configuration, a third negative electrode configuration, and a fourth negative electrode configuration. The first negative electrode configuration indicates a configuration in which an undercoat layer and a negative electrode mixture layer are laminated in this order on both main surfaces of a current collector. The second negative electrode configuration indicates a configuration in which an undercoat layer and a negative electrode mixture layer are laminated in this order on one main surface of a current collector, and an undercoat layer is laminated on the other main surface of the current collector. The third negative electrode configuration shows a configuration in which an undercoat layer and a negative electrode mixture layer are laminated in this order on one main surface of a current collector, and a negative electrode mixture layer is laminated on the other main surface of the current collector. The fourth negative electrode configuration indicates a configuration in which an undercoat layer and a negative electrode composite layer are laminated in this order on one main surface of a current collector, and neither the undercoat layer nor the negative electrode composite layer is laminated on the other main surface of the current collector.
[0200] (3.2.1) Negative electrode current collector Examples of the material for the negative electrode current collector include copper, aluminum, nickel, stainless steel (SUS), and nickel-plated steel.
[0201] (3.2.2) Undercoat layer The undercoat layer is the same as that exemplified as the undercoat layer of the positive electrode.
[0202] (3.2.3) Negative electrode composite layer The negative electrode mixture layer contains a negative electrode active material and a binder.
[0203] (3.2.3.1) Negative electrode active material The negative electrode active material is not particularly limited as long as it is a material capable of absorbing and releasing lithium ions. The negative electrode active material is preferably at least one selected from the group consisting of, for example, metallic lithium, lithium-containing alloys, metals or alloys capable of alloying with lithium, oxides capable of doping and dedoping lithium ions, transition metal nitrides capable of doping and dedoping lithium ions, and carbon materials capable of doping and dedoping lithium ions. Among these, the negative electrode active material is preferably a carbon material capable of doping and dedoping lithium ions (hereinafter referred to as "carbon material").
[0204] Examples of carbon materials include carbon black, activated carbon, graphite materials, and amorphous carbon materials. These carbon materials may be used alone or in combination of two or more. The form of the carbon material is not particularly limited, and may be, for example, fibrous, spherical, or flaky. The particle size of the carbon material is not particularly limited, and is preferably 5 μm or more and 50 μm or less, more preferably 20 μm or more and 30 μm or less. Examples of amorphous carbon materials include hard carbon, coke, mesocarbon microbeads (MCMB) calcined at 1500° C. or less, and mesophase pitch carbon fiber (MCF). Examples of the graphite material include natural graphite and artificial graphite. Examples of the artificial graphite include graphitized MCMB and graphitized MCF. The graphite material may contain boron. The graphite material may be coated with a metal or amorphous carbon. Examples of the metal material that coats the graphite material include gold, platinum, silver, copper, and tin. The graphite material may be a mixture of amorphous carbon and graphite.
[0205] (3.2.3.2) Binder Examples of the binder contained in the negative electrode mixture layer include the same binders as those exemplified as the binder contained in the positive electrode mixture layer. The binder contained in the negative electrode mixture layer may be the same as or different from the binder contained in the positive electrode mixture layer. The content of the binder contained in the negative electrode mixture layer is not particularly limited, and may be the same as the exemplified content of the binder contained in the positive electrode mixture layer.
[0206] (3.2.3.3) Conductive additives The negative electrode mixture layer preferably contains a conductive assistant. Examples of the conductive assistant include the same conductive assistants as those exemplified as the conductive assistants that can be contained in the positive electrode mixture layer.
[0207] (3.2.3.4) Other ingredients The negative electrode mixture layer may contain other components in addition to the above components, such as a thickener, a surfactant, a dispersant, a wetting agent, and a defoamer.
[0208] The electrode of the present disclosure preferably has a structure having a current collector, an undercoat layer, and a composite layer in this order.
[0209] (4) Lithium-ion secondary battery The lithium ion secondary battery of the present disclosure includes the above-described electrode of the present disclosure. A lithium ion secondary battery generally includes an exterior body, electrodes (positive and negative electrodes), a separator, and an electrolyte. The exterior body accommodates the electrodes (positive and negative electrodes), the separator, and the non-aqueous electrolyte.
[0210] Hereinafter, an example will be described in which the positive electrode and the negative electrode are the electrodes of the present disclosure.
[0211] (4.1) Exterior body Examples of the exterior body include an exterior body including a laminate film, an exterior body consisting of a battery can and a battery can lid, etc. The shape of the exterior body is not particularly limited and is appropriately selected depending on the application of the lithium ion secondary battery, etc.
[0212] (4.2) Electrode The battery includes a positive electrode and a negative electrode as electrodes. The positive electrode is capable of absorbing and releasing lithium ions. The negative electrode is capable of absorbing and releasing lithium ions. In the lithium ion secondary battery of the present disclosure, at least one of the positive electrode and the negative electrode is the electrode of the present disclosure. When one of the positive electrode and the negative electrode of the lithium ion secondary battery of the present disclosure is the electrode of the present disclosure, the other of the positive electrode and the negative electrode may be a known electrode used in lithium ion secondary batteries.
[0213] (4.3) Separator The separator separates the positive electrode and the negative electrode. For example, a porous resin plate can be used as the separator. The material of the porous resin plate can be resin or nonwoven fabric containing the resin. The resin can be polyethylene (PE), polypropylene (PP), polymethylpentene (PMP), polyester, cellulose, polyamide, or the like. Among them, the separator is preferably a porous resin sheet having a single layer or multilayer structure. The material of the porous resin sheet is mainly composed of one or more polyolefin resins. The thickness of the separator is preferably 5 μm or more and 30 μm or less. The separator is preferably disposed between the positive electrode and the negative electrode.
[0214] (4.4) Non-aqueous electrolyte The non-aqueous electrolyte contains an electrolyte and a non-aqueous solvent. (4.4.1) Electrolyte The electrolyte preferably contains at least one of a fluorine-containing lithium salt (hereinafter also referred to as a "fluorine-containing lithium salt") and a fluorine-free lithium salt.
[0215] Examples of the fluorine-containing lithium salt include inorganic acid anion salts and organic acid anion salts. Examples of inorganic acid anion salts include lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), and lithium hexafluorotantalate (LiTaF6). Examples of organic acid anion salts include lithium trifluoromethanesulfonate (LiCF3SO3). Among them, LiPF6 is particularly preferred as a fluorine-containing lithium salt. Examples of fluorine-free lithium salts include lithium perchlorate (LiClO4), lithium tetrachloroaluminate (LiAlCl4), and lithium decachlorodecaborate (Li2B 10 Cl 10 ) are mentioned.
[0216] When the electrolyte contains a fluorine-containing lithium salt, the content of the fluorine-containing lithium salt is preferably 50 mass % or more and 100 mass % or less, more preferably 60 mass % or more and 100 mass % or less, and even more preferably 80 mass % or more and 100 mass % or less, based on the total amount of the electrolyte. When the fluorine-containing lithium salt contains lithium hexafluorophosphate (LiPF6), the content of lithium hexafluorophosphate (LiPF6) is preferably 50 mass% or more and 100 mass% or less, more preferably 60 mass% or more and 100 mass% or less, and even more preferably 80 mass% or more and 100 mass% or less, based on the total amount of the electrolyte.
[0217] When the non-aqueous electrolyte contains an electrolyte, the concentration of the electrolyte in the non-aqueous electrolyte is preferably 0.1 mol / L or more and 3 mol / L or less, and more preferably 0.5 mol / L or more and 2 mol / L or less. When the non-aqueous electrolyte contains lithium hexafluorophosphate (LiPF6), the concentration of lithium hexafluorophosphate (LiPF6) in the non-aqueous electrolyte is preferably 0.1 mol / L or more and 3 mol / L or less, more preferably 0.5 mol / L or more and 2 mol / L or less.
[0218] (4.4.2) Nonaqueous solvents The non-aqueous electrolyte generally contains a non-aqueous solvent. Examples of non-aqueous solvents include cyclic carbonates, fluorine-containing cyclic carbonates, chain carbonates, fluorine-containing chain carbonates, aliphatic carboxylic acid esters, fluorine-containing aliphatic carboxylic acid esters, γ-lactones, fluorine-containing γ-lactones, cyclic ethers, fluorine-containing cyclic ethers, chain ethers, fluorine-containing chain ethers, nitriles, amides, lactams, nitromethane, nitroethane, sulfolane, trimethyl phosphate, dimethyl sulfoxide, and dimethyl sulfoxide phosphate. The non-aqueous solvents may be used alone or in combination of two or more.
[0219] Examples of cyclic carbonates include ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC). Examples of fluorine-containing cyclic carbonates include fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), and trifluoropropylene carbonate. Examples of chain carbonates include dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), and dipropyl carbonate (DPC). An example of the fluorine-containing chain carbonates is methyl 2,2,2-trifluoroethyl carbonate. Examples of the aliphatic carboxylate esters include methyl formate, methyl acetate, methyl propionate, methyl butyrate, methyl isobutyrate, methyl trimethylbutyrate, ethyl formate, ethyl acetate, ethyl propionate, ethyl butyrate, ethyl isobutyrate, and ethyl trimethylbutyrate. Examples of the fluorine-containing aliphatic carboxylates include methyl difluoroacetate, methyl 3,3,3-trifluoropropionate, ethyl difluoroacetate, and 2,2,2-trifluoroethyl acetate. Examples of γ-lactones include γ-butyrolactone and γ-valerolactone. Examples of cyclic ethers include tetrahydrofuran, 2-methyltetrahydrofuran, tetrahydropyran, 1,3-dioxolane, 4-methyl-1,3-dioxolane, 1,3-dioxane, and 1,4-dioxane. Examples of chain ethers include 1,2-ethoxyethane (DEE), ethoxymethoxyethane (EME), diethyl ether, 1,2-dimethoxyethane, and 1,2-dibutoxyethane. Examples of fluorine-containing chain ethers include HCF2CF2CH2OCF2CF2H, CF3CF2CH2OCF2CF2H, HCF2CF2CH2OCF2CFHCF3, CF3CF2CH2OCF2CFHCF3, and C6F 13 OCH3, C6F 13 OC2H5, C8F 17 OCH3, C8F 17 Examples include OC2H5, CF3CFHCF2CH(CH3)OCF2CFHCF3, HCF2CF2OCH(C2H5)2, HCF2CF2OC4H9, HCF2CF2OCH2CH(C2H5)2, and HCF2CF2OCH2CH(CH3)2. Examples of nitriles include acetonitrile, glutaronitrile, adiponitrile, methoxyacetonitrile, and 3-methoxypropionitrile. An example of the amides is N,N-dimethylformamide. Examples of lactams include N-methylpyrrolidinone, N-methyloxazolidinone, and N,N'-dimethylimidazolidinone.
[0220] The non-aqueous solvent preferably contains at least one selected from the group consisting of cyclic carbonates, fluorine-containing cyclic carbonates, chain carbonates, and fluorine-containing chain carbonates. In this case, the total proportion of the cyclic carbonates, fluorine-containing cyclic carbonates, chain carbonates, and fluorine-containing chain carbonates is preferably 50% by mass or more and 100% by mass or less, more preferably 60% by mass or more and 100% by mass or less, and even more preferably 80% by mass or more and 100% by mass or less, based on the total amount of the non-aqueous solvent.
[0221] The non-aqueous solvent preferably contains at least one selected from the group consisting of cyclic carbonates and chain carbonates. In this case, the total proportion of the cyclic carbonates and chain carbonates in the non-aqueous solvent is preferably 50% by mass or more and 100% by mass or less, more preferably 60% by mass or more and 100% by mass or less, and even more preferably 80% by mass or more and 100% by mass or less, based on the total amount of the non-aqueous solvent.
[0222] The content of the nonaqueous solvent is preferably 99% by mass or less, more preferably 97% by mass or less, and even more preferably 90% by mass or less, based on the total amount of the nonaqueous electrolyte. The content of the nonaqueous solvent is preferably 60% by mass or more, and even more preferably 70% by mass or more, based on the total amount of the nonaqueous electrolyte.
[0223] The intrinsic viscosity of the nonaqueous solvent is preferably 10.0 mPa·s or less at 25° C., from the viewpoint of further improving the dissociation property of the electrolyte and the mobility of ions.
[0224] (4.4.3) Electrolyte Additives The non-aqueous solvent may contain an electrolyte additive. This makes it possible to make it difficult for side reactions that are not the original battery reaction to proceed during the charge / discharge cycle of the lithium ion secondary battery. The battery reaction is a reaction in which lithium ions enter and leave (intercalate) the positive electrode and the negative electrode. The side reactions include a reductive decomposition reaction of the non-aqueous electrolyte by the negative electrode, an oxidative decomposition reaction of the non-aqueous electrolyte by the positive electrode, and elution of metal elements in the positive electrode active material. The electrolyte additive is not particularly limited, and any known additive can be used. For example, the additives described in JP-A-2019-153443 can be used.
[0225] (5) An example of a lithium-ion secondary battery An example of a lithium ion secondary battery according to an embodiment of the present disclosure will be specifically described with reference to Fig. 1 and Fig. 2. Fig. 1 is a schematic cross-sectional view of a lithium ion secondary battery 1 according to an embodiment of the present disclosure. Fig. 2 is a schematic cross-sectional view of a positive electrode 11 in the lithium ion secondary battery 1 according to an embodiment of the present disclosure. Fig. 3 is a schematic cross-sectional view of a negative electrode 12 in the lithium ion secondary battery 1 according to an embodiment of the present disclosure.
[0226] The lithium ion secondary battery 1 according to the embodiment of the present disclosure is a laminated type. As shown in FIG. 1, the lithium ion secondary battery 1 includes a battery element 10, a positive electrode lead 21, a negative electrode lead 22, and an exterior body 30. The battery element 10 is enclosed inside the exterior body 30. The exterior body 30 is formed of a laminate film. The positive electrode lead 21 and the negative electrode lead 22 are attached to the battery element 10. The positive electrode lead 21 and the negative electrode lead 22 are led out in opposite directions from the inside to the outside of the exterior body 30.
[0227] As shown in FIG. 1, the battery element 10 is formed by laminating a positive electrode 11, a separator 13, and a negative electrode 12. 2, the positive electrode 11 is formed by forming a positive electrode composite layer 11B on both main surfaces of a positive electrode collector 11A with an undercoat layer. The positive electrode collector 11A with an undercoat layer is formed by forming an undercoat layer 111 on both main surfaces of a positive electrode collector 110. 3, negative electrode 12 is formed by forming negative electrode composite layer 12B on both main surfaces of undercoat layer-attached negative electrode current collector 12A. Undercoat layer-attached negative electrode current collector 12A is formed by forming undercoat layer 121 on both main surfaces of negative electrode current collector 120. As shown in FIG. 1, a positive electrode composite layer 11B formed on one main surface of a positive electrode collector 11A with an undercoat layer of a positive electrode 11 and a negative electrode composite layer 12B formed on one main surface of a negative electrode collector 12A with an undercoat layer of a negative electrode 12 adjacent to the positive electrode 11 are opposed to each other via a separator 13.
[0228] A non-aqueous electrolyte is injected into the interior of the exterior body 30. The non-aqueous electrolyte permeates the positive electrode mixture layer 11B, the separator 13, and the negative electrode mixture layer 12B. In the lithium-ion secondary battery 1, one unit cell layer 14 is formed by the adjacent positive electrode mixture layer 11B, the separator 13, and the negative electrode mixture layer 12B.
[0229] In this embodiment, the lithium ion secondary battery 1 is a laminated type, but the present disclosure is not limited thereto, and the lithium ion secondary battery 1 may be, for example, a wound type. The wound type is formed by stacking a positive electrode, a separator, a negative electrode, and a separator in this order and winding them into a layered shape. The wound type includes a cylindrical type and a rectangular type. 1, the directions in which the positive electrode lead 21 and the negative electrode lead 22 protrude from the inside of the exterior body 30 to the outside are opposite directions relative to the exterior body 30, but the present disclosure is not limited thereto. For example, the directions in which the positive electrode lead and the negative electrode lead protrude from the inside of the exterior body 30 to the outside may be the same direction relative to the exterior body 30. EXAMPLES
[0230] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention.
[0231] Details of the components used in the examples and comparative examples are as follows. The physical properties of the products of the components are shown in the catalog values.
[0232] <Conductive carbon material (A)> Super-P: "Super-P" manufactured by TIMCAL (conductive carbon black, solid content: 100% by mass) KS-6: TIMREX's "KS-6" (flake graphite, solid content: 100% by mass)
[0233] <Olefin resin (B)> W300: "Chemipearl (registered trademark) W300" manufactured by Mitsui Chemicals, Inc. (water dispersion of low molecular weight polyethylene, solid content concentration: 40% by mass, particle size (average primary particle size measured by the Cole counter method; the same applies below): 3.0 μm, softening point (ring and ball method): 132°C) W700: "Chemipearl (registered trademark) W700" manufactured by Mitsui Chemicals, Inc. (water dispersion of low molecular weight polyethylene, solid content concentration: 40% by mass, particle size: 1.0 μm, softening point (ring and ball method): 132°C) W900: "Chemipearl (registered trademark) W900" manufactured by Mitsui Chemicals, Inc. (water dispersion of low molecular weight polyethylene, solid content concentration: 40% by mass, particle size: 0.6 μm, softening point (ring and ball method): 132°C) W950: "Chemipearl (registered trademark) W950" manufactured by Mitsui Chemicals, Inc. (water dispersion of low molecular weight polyethylene, solid content concentration: 40% by mass, particle size: 0.6 μm, softening point (ring and ball method): 113°C) WP100: "Chemipearl (registered trademark) WP100" manufactured by Mitsui Chemicals, Inc. (water dispersion of low molecular weight polypropylene, solid content concentration: 40% by mass, particle size: 1.0 μm, softening point (ring and ball method): 148°C)
[0234] <Acrylic resin (C)> As the acrylic resin (C), acrylic resins (C-1) to (C-4) synthesized by the following method were used.
[0235] -Synthesis of acrylic resin (C-1)- A separable flask equipped with a stirrer and reflux condenser was charged with 360.9 parts by mass of distilled water, and the mixture was replaced with nitrogen gas and then heated to 80°C. Next, 0.5 parts by mass of ammonium persulfate was added, and the following first monomer component, emulsifier, and water were continuously added over 3 hours, and the mixture was maintained for another 3 hours, and the pH was adjusted to 9.0 with aqueous ammonia to complete the polymerization. An appropriate amount of water was added to obtain a dispersion containing a first polymer with a solid content of 20.0% by mass.
[0236] <First monomer component> n-Butyl acrylate 45.0 parts by mass Acrylonitrile 35.0 parts by mass Methyl methacrylate 8.0 parts by weight 2-Hydroxyethyl methacrylate 5.0 parts by mass Methacrylic acid 5.0 parts by mass N-Methylolacrylamide 2.0 parts by weight Ammonium lauryl sulfate 0.4 parts by weight Distilled water 40.0 parts by weight
[0237] 40 parts by mass of distilled water was added to 500 parts by mass of the obtained dispersion containing the first polymer, and the mixture was replaced with nitrogen gas, and then heated to 80°C. Next, 0.5 parts by mass of ammonium persulfate was added, and then a mixture of the second monomer component and water described below was continuously added over 2 hours while stirring, and then the mixture was aged at the same temperature for 2 hours, and the pH was adjusted to 9.0 with aqueous ammonia to complete the polymerization of the second monomer component. Then, an appropriate amount of water was added to obtain a dispersion containing the first polymer and the second polymer (raw material for undercoat). The solid content concentration of the dispersion was 20.0% by mass.
[0238] <Second monomer component> Methacrylamide 17.5 parts by mass Methacrylic acid 5.0 parts by mass 2-Hydroxyethyl methacrylate 2.5 parts by mass Distilled water 52.5 parts by weight
[0239] -Synthesis of acrylic resins (C-2) and (C-4)- The acrylic resin (C-1) was synthesized in the same manner as in the synthesis of the acrylic resin (C-1), except that the compounding recipe was changed according to the description in Table 1.
[0240] -Synthesis of acrylic resin (C-3)- A separable flask equipped with a stirrer and reflux condenser was charged with 229.2 parts by mass of distilled water, and the mixture was replaced with nitrogen gas and then heated to 80°C. Next, 1.1 parts by mass of 4,4'-azobis(4-cyanovaleric acid) dissolved in 12.1 parts by mass of 2.3% by mass aqueous ammonia was added, and then the second monomer component described below, 25% by mass aqueous ammonia, and water were continuously added over 3 hours, and the mixture was maintained for another 4 hours to complete the polymerization. An appropriate amount of water was added to obtain an aqueous solution containing a second polymer with a solid content of 15.0% by mass.
[0241] <Second monomer component> Methacrylamide 90.0 parts by mass Methacrylic acid 5.0 parts by mass 2-Hydroxyethyl methacrylate 5.0 parts by mass 25% ammonia water 1.8 parts by mass Distilled water 333.3 parts by weight
[0242] 1.1 parts by mass of sodium lauryl sulfate was added to 6587.7 parts by mass of the obtained aqueous solution containing the second polymer, and the mixture was replaced with nitrogen gas and then heated to 80°C. 5.4 parts by mass of 4,4'-azobis(4-cyanovaleric acid) dissolved in 203.3 parts by mass of 0.49% by mass aqueous ammonia was added, and then the following first monomer component, emulsifier and water were added continuously over 1 hour, and the mixture was aged at the same temperature for 5 hours, and the pH was adjusted to 8.0 with aqueous ammonia to complete the polymerization of the second monomer component. Then, an appropriate amount of water was added to obtain a dispersion containing the first polymer and the second polymer (raw material for undercoat). The solid content concentration of the dispersion was 15.0% by mass.
[0243] <First monomer component> Acrylonitrile 45.0 parts by mass n-Butyl acrylate 45.0 parts by mass 2-Hydroxyethyl methacrylate 7.0 parts by mass Methacrylic acid 3.0 parts by mass Sodium lauryl sulfate 0.3 parts by weight Distilled water 40.0 parts by weight
[0244] <Other acrylic resins> As acrylic resins other than the acrylic resin (C), the following acrylic resins (C'-5) and (C'-6) were used.
[0245] -Synthesis of acrylic resin (C'-5)- The acrylic resin (C-1) was synthesized in the same manner as in the synthesis of the acrylic resin (C-1), except that the compounding recipe was changed according to the description in Table 1.
[0246] -Synthesis of acrylic resin (C'-6)- The acrylic resin (C-3) was synthesized in the same manner as in the synthesis of the acrylic resin (C-3), except that the compounding recipe was changed according to the description in Table 1.
[0247] [Table 1]
[0248] <Additives (D)> Polyacrylic acid: "Polyacrylic acid" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. (polyacrylic acid aqueous solution, solids concentration: approximately 25% by mass) Polyacrylamide: "Polyacrylamide" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. (polyacrylamide aqueous solution, solids concentration: approximately 10% by mass) CMC: "2200" manufactured by Daicel Miraize Co., Ltd. (sodium carboxymethylcellulose, solid content: 100% by mass) PVDF: Kureha Corporation's "W#7200" (vinylidene fluoride resin, solid content: 100% by mass) SBR: JSR Corporation's "TRD2001" (aqueous dispersion of styrene butadiene rubber particles, solid content: 50% by mass) MC: Matsumoto Microsphere (registered trademark) FN-100SS manufactured by Matsumoto Yushi Pharmaceutical Co., Ltd. (microcapsule, solid content concentration: 100% by mass, maximum volume expansion temperature 180°C) Al2O3: "Aluminum oxide" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. (average particle size: 2 μm, solid content: 100% by mass)
[0249] Specific numerical values of the blending ratios (content ratios), physical property values, parameters, etc. used in the following description can be replaced with the upper limit values (numerical values defined as "not more than" or "less than") or lower limit values (numerical values defined as "not less than" or "exceeding") of the corresponding blending ratios (content ratios), physical property values, parameters, etc. described in the above "Form for implementing the invention." In the following description, unless otherwise specified, "parts" and "%" are by mass.
[0250] Example 1 [1] Preparation of positive electrode current collector with undercoat layer [1.1] Preparation of slurry for undercoat layer A 5 L (liter; the same applies below) planetary dispersion was used to prepare the undercoat layer slurry. A three-roll mill (BR-300HCVIII, manufactured by Imex Co., Ltd.) was used to disperse the undercoat layer slurry.
[0251] 58 parts by mass of "Super-P" (A) was pre-mixed for 5 minutes (preparation step A). Then, 229.0 parts by mass of "CMC aqueous solution" (D) was added to the "Super-P" (A) powder and mixed for another 20 minutes to obtain a first mixture (preparation step B). The "CMC aqueous solution" (D) was prepared by adding "CMC" (D) to distilled water so that the content of "CMC" (D) was 1.5% by mass relative to the total amount of the "CMC aqueous solution" (D). Next, 568.1 parts by mass of "CMC aqueous solution" (D) was added to the first mixed solution, and the addition operation of mixing for 20 minutes was repeated three times to obtain a second mixed solution (preparation step C). The total amount of "CMC aqueous solution" (D) added to the first mixed solution was 1704.3 parts by mass. Next, 72.5 parts by mass of "acrylic resin (C-1)" and 471.3 parts by mass of "W700" (B) were added to the obtained second mixed liquid, and the mixture was kneaded for 20 minutes, and then vacuum degassed for 30 minutes to obtain a third mixed liquid (preparation process D).
[0252] The third mixed liquid was subjected to dispersion processing twice (preparation step E) using a three-roll mill shown in Fig. 4 under conditions of a roll gap of 10 µm and a roll rotation speed of 300 rpm (gear ratio 1:3:9). That is, the rotation speed of the charge roll 91 was 33.3 rpm, the rotation speed of the intermediate roll 92 was 100 rpm, the rotation speed of the finishing roll 93 was 300 rpm, the first gap L1 was 10 µm, and the second gap L2 was 10 µm. In this manner, a slurry (composition) for the undercoat layer having a solid content concentration of 12.0 mass % was prepared.
[0253] [1.2] Coating and drying of undercoat layer The undercoat layer slurry was applied using a die coater. The coating thickness after drying is 3 μm (coating weight is about 0.2 mg / cm 2The slurry for the undercoat layer was applied to one main surface of an aluminum foil (thickness 20 μm, width 200 mm, positive electrode current collector) and dried so that the thickness of the coating after drying was 3 μm. Next, the slurry for the undercoat layer was similarly applied to the other main surface (uncoated surface) of the aluminum foil and dried so that the coating thickness after drying was 3 μm. In this way, an aluminum foil roll (positive electrode current collector with an undercoat layer) was obtained in which the undercoat layer was coated on both sides.
[0254] [3] Positive electrode preparation [3.1] Preparation of positive electrode mixture slurry A 5 L planetary dispenser was used to prepare the positive electrode mixture slurry. "NCM523" (Umicore, composition formula: LiNi 0.5 Co 0.2 Mn 0.3 O2), 30 parts by mass of "Super-P" (conductive carbon manufactured by TIMCAL) as a conductive additive, and 30 parts by mass of "KS-6" (flake graphite manufactured by TIMREX) as a conductive additive were mixed for 10 minutes to obtain a mixture for the positive electrode.
[0255] 50 parts by mass of "NMP" was added to the positive electrode mixture and mixed for 20 minutes to obtain a first positive electrode mixture. 350 parts by mass of "PVDF solution" was added to the first positive electrode mixture and mixed for 30 minutes, then 260 parts by mass of "PVDF solution" was added and mixed for 15 minutes, and 220 parts by mass of "PVDF solution" was added and mixed for 15 minutes to obtain a second positive electrode mixture. The "PVDF solution" was prepared by adding "PVDF" to "NMP" so that the "PVDF" content was 8 mass% relative to the total amount of the "PVDF solution." To adjust the viscosity, 80 parts by mass of "NMP" was added to the second positive electrode mixture and mixed for 30 minutes, followed by vacuum degassing for 30 minutes. In this manner, a positive electrode mixture slurry having a solid content of 65 mass % was prepared.
[0256] [3.2] Coating and drying The positive electrode mixture slurry was applied using a die coater. The mass of the positive electrode mixture layer (coating film after drying) is 19.0 mg / cm 2 The positive electrode mixture slurry was applied onto one main surface (i.e., the undercoat layer) of a positive electrode current collector with an undercoat layer (aluminum foil thickness: 20 μm, thickness of one undercoat layer: 3 μm, width: 200 mm) and dried so that the mass of the positive electrode mixture layer (coated film after drying) became 19.0 mg / cm 2 The positive electrode mixture slurry was similarly applied onto the other main surface (that is, the undercoat layer) of the positive electrode current collector with the undercoat layer so that the positive electrode mixture slurry became equal to or larger than the undercoat layer, and then dried. The positive electrode roll thus obtained was coated on both sides (the total amount of coating on both sides was 38.0 mg / cm2). 2 ) was dried in a vacuum drying oven at 130°C for 12 hours.
[0257] [3.3] Press A 35-ton press was used to press the positive electrode roll. The gap between the upper and lower rolls was adjusted to press the positive electrode to a density of 2.9±0.05 g / cm. 3 The mixture was pressed using a 35 ton press so that the thickness became
[0258] [3.4] Slit The positive electrode roll was slit so as to obtain the area of the positive electrode composite layer (front surface: 56 mm × 334 mm, back surface: 56 mm × 408 mm) and an area for tab welding margins, thereby obtaining a positive electrode in which an undercoat layer was laminated on the aluminum foil.
[0259] [4] Negative electrode production [4.1] Preparation of negative electrode mixture slurry A 5 L planetary dispenser was used to prepare the negative electrode mixture slurry. The negative electrode active material is 1,050 parts by mass of "natural graphite" and the conductive additive is "Super-P" (conductive carbon, BET specific surface area 62 m 211 parts by mass of 100% cellulose acetate / g) was mixed for 10 minutes to obtain a mixture for a negative electrode. 450 parts by mass of "CMC aqueous solution" was added to the mixture for a negative electrode, and the mixture was further mixed for 20 minutes to obtain a mixture for a first negative electrode. 150 parts by mass of "CMC aqueous solution" was added to the mixture for the first negative electrode, and the mixture was further mixed for 30 minutes, and 293.5 parts by mass of "CMC aqueous solution" was further added and mixed for 30 minutes. Next, 450 parts by mass of water as a solvent was added and mixed for 15 minutes to obtain a mixture for a second negative electrode. 45 parts by mass of "SBR aqueous solution" (manufactured by JSR Corporation, solid content concentration: 50% by mass) was added to the mixture for the second negative electrode, and the mixture was kneaded for 15 minutes and vacuum degassed for 10 minutes. In this manner, a negative electrode mixture slurry having a solid content concentration of 45 mass % was prepared.
[0260] [4.2] Coating and drying The negative electrode mixture slurry was applied using a die coater. The mass of the negative electrode mixture layer (coating film after drying) is 11.0 mg / cm 2 The negative electrode mixture slurry was applied to one main surface of a copper foil (thickness 10 μm, negative electrode current collector) and dried so that the mass of the negative electrode mixture layer (coated film after drying) was 11.0 mg / cm. 2 The negative electrode composite slurry was applied to the other main surface of the copper foil and dried so that the negative electrode composite slurry was applied to the other main surface of the copper foil. 2 ) was dried in a vacuum drying oven at 120°C for 12 hours.
[0261] [4.3] Press A small press was used to press the negative electrode roll. The gap between the upper and lower rolls was adjusted to press the negative electrode roll to a density of 1.45±0.05g / cm. 3 The mixture was pressed using a small press so that the thickness became
[0262] [4.4] Slit The negative electrode roll was slit so as to obtain the area of the negative electrode mixture layer (front surface: 58 mm×372 mm, back surface: 58 mm×431 mm) and an area for a tab welding margin, thereby obtaining a negative electrode.
[0263] [5] Fabrication of a wound battery (design capacity 1Ah) [5.1] Winding The separator used was a polyethylene porous film (60.5 mm×450 mm) with a porosity of 45% by volume and a thickness of 25 μm. The negative electrode, separator, positive electrode with an undercoat layer, and separator obtained above were stacked and wound, and then press-molded. Next, an aluminum tab was bonded to the margin of the positive electrode with the undercoat layer by an ultrasonic bonding machine, and a nickel tab was bonded to the margin of the negative electrode by an ultrasonic bonding machine. This was sandwiched between laminate films, and three sides were heat-sealed. This resulted in an exterior body having an opening (hereinafter referred to as the "first exterior body").
[0264] [5.2] Injection of non-aqueous electrolyte A mixed solvent was obtained by mixing ethylene carbonate (EC), methyl ethyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of EC:EMC:DMC=3:3:4. LiPF6 was dissolved in the mixed solvent to a concentration of 1.0 mol / L to prepare a non-aqueous electrolyte. Before the injection of the non-aqueous electrolyte, the first exterior body was dried under reduced pressure at 70° C. for 12 hours in a vacuum dryer. After the reduced pressure drying, 4.7±0.1 g of electrolyte was injected into the first exterior body. Then, the opening of the first exterior body was heat-sealed while drawing a vacuum. In this manner, a lithium ion secondary battery precursor was obtained.
[0265] [5.3] Activation process The lithium ion secondary battery precursor was kept at room temperature (25°C) for 24 hours. Next, the lithium ion secondary battery precursor was charged at a constant current (0.05C-CC) at 0.05C for 4 hours, and then rested for 12 hours. Then, it was charged at a constant current and constant voltage (0.1C-CCCV) at 0.1C to 4.2V, rested for 30 minutes, and then discharged at a constant current (0.1C-CC) at 0.1C to 2.8V. Furthermore, the charge-discharge cycle (charging to 4.2V at 0.1C-CCCV and discharging to 2.8V at 0.1C-CC) was repeated five times. Then, the lithium ion secondary battery precursor was stored at 25°C for five days in a fully charged state of 4.2V (SOC100%). In this manner, a wound type battery (lithium ion secondary battery) was produced.
[0266] [6] Evaluation method The prepared undercoat layer slurry was subjected to the following particle size distribution measurement. The prepared wound battery was also subjected to the following heating resistance test, forced internal short circuit test, initial DCIR measurement, and DCIR evaluation after high temperature storage. The evaluation results are shown in Table 5.
[0267] [6.1] Particle size distribution 1.0 g of the prepared undercoat layer slurry (hereinafter also referred to as "sample") and 50 ml of water were placed in a 100 ml beaker, and the lumps of the sample were crushed with a spatula and lightly mixed with a dropper. Next, the sample was dispersed in water using a tabletop ultrasonic cleaner (Honda Electronics Co., Ltd., W-113 model). At this time, the tabletop ultrasonic cleaner was set to an output of 100 W and 28 kHz, and dispersion was performed for 60 seconds. After that, bubbles formed on the surface of the aqueous solution in the beaker were removed, and the volume-based particle size distribution of the sample was measured using a particle size distribution measuring device (Microtrac-Bell Co., Ltd., Microtrac MT3300EXII) by a laser light diffraction scattering method. From this measurement, D10, D50, D90 and D99 in the volume particle size distribution were obtained. The measurement results of D10, D50, D90 and D99 are shown in Table 4.
[0268] [6.2] Heating resistance test A wound battery (design capacity 1 Ah) was charged at a constant current and constant voltage (0.1C-CCCV) to 4.2 V in a temperature environment of 25 ° C., and a heating resistance test was performed. The measurement cell was placed in a thermostatic chamber whose temperature had been raised to 50 ° C., and the AC resistance was measured at 1 kHz (amplitude 10 mV) while the thermostatic chamber was heated at 5 ° C. / min. The cell temperature was recorded as the temperature obtained by a temperature measurement terminal installed on the upper surface of the cell. The AC resistance measurement was performed using a ModuLab XM ECS electrochemical measurement system manufactured by Solartron. The resistance rise start temperature and resistance change ratio were calculated from the measured resistance value. The resistance rise start temperature was calculated as the temperature at which the resistance value reached 1.5 times the resistance value at 50 ° C., assuming that the resistance value at 50 ° C. was 1. The resistance change ratio was calculated as the relative ratio of the resistance value at 150 ° C., assuming that the resistance value at 50 ° C. was 1. The nail penetration test was performed on the same level of batteries multiple times (3 to 5 times) and the total number of test batteries was evaluated according to the following criteria. Acceptable evaluations for the nail penetration test are "A" and "B". <Evaluation criteria> A: The resistance rise starting temperature is 90°C or less, and the resistance change rate is 20 times or more. B: The resistance rise starting temperature is higher than 90° C. and the resistance change rate is 20 times or more, or the resistance rise starting temperature is 90° C. or less and the resistance change rate is less than 20 times. C: The resistance increase starting temperature is higher than 90° C., and the resistance change rate is less than 20 times.
[0269] [6.3] Forced internal short circuit test (nail penetration test) A wound battery (design capacity 1 Ah) was charged at a constant current and constant voltage (0.1C-CCCV) to 4.2 V at 0.1 C in a temperature environment of 25°C, and a nail penetration test (nail diameter 3 mm, nail penetration speed 1.0 mm / sec) was performed. A nail with a diameter of 3 mm was inserted into the center of the wound battery (cell) at a speed of 1.0 mm / sec, short-circuiting the positive and negative electrodes inside the battery container. The short-circuit behavior of the battery at this time was observed. The nail penetration test was performed on the battery multiple times (3 to 6 times) at the same level, and the total number of test batteries was evaluated according to the following criteria. Acceptable evaluations for the nail penetration test are "A" and "B". <Evaluation criteria> A: The percentage of batteries whose internal temperature exceeded 300°C was less than 10% of the total number of tested batteries. B: The percentage of batteries whose internal temperature exceeded 300°C was more than 10% but less than 60% of the total number of test batteries. C: The percentage of batteries whose internal temperature exceeded 300°C was 60% or more of the total number of test batteries.
[0270] [6.4] Initial DCIR Assessment [6.4.1] Initial DCIR measurement A wound battery (design capacity 1 Ah) was charged at a constant current and constant voltage (0.1C-CCCV) up to 4.2 V in a temperature environment of 25°C, and the initial DCIR was measured. The battery was discharged at a constant current of 0.1C for 10 seconds (0.1C-CC-10s) and then charged at a constant current of 0.1C for 10 seconds (0.1C-CC-10s). Next, the battery was discharged at a constant current of 0.2 C for 10 seconds (0.2C-CC-10s), and then charged at a constant current of 0.2 C for 10 seconds (0.2C-CC-10s). Next, the battery was discharged at a constant current of 0.5 C for 10 seconds (0.5C-CC-10s), and then charged at a constant current of 0.5 C for 10 seconds (0.5C-CC-10s). Next, the battery was discharged at a constant current of 1.0 C for 10 seconds (1.0 C-CC-10 s), and then charged at a constant current of 1.0 C for 10 seconds (1.0 C-CC-10 s). Next, the battery was discharged at a constant current of 2.0 C for 10 seconds (2.0C-CC-10s), and then charged at a constant current of 2.0 C for 10 seconds (2.0-CC-10s). The first direct current resistance (DCIR; unit Ω) was calculated based on each voltage drop (= voltage before the start of discharge - voltage 10 seconds after the start of discharge) due to "CC10s discharge" at each discharge rate of 0.1C to 2.0C and each current value (i.e., each current value corresponding to the discharge rates of 0.1C to 2.0C).
[0271] [6.4.2] Evaluation Based on the above measured values, a first relative value was calculated by normalizing the measured value of the first direct current resistance (DCIR; unit Ω) of the reference example (without an undercoat layer) to 100, and an initial DCIR evaluation was performed according to the following criteria. The measured values of the first direct current resistance and the first relative value are shown in Table 5. Acceptable evaluations of the initial DCIR evaluation are "A" and "B". <Evaluation criteria> A: The first relative value is 100 or less. B: The first relative value is greater than 100 and is 105 or less. C: The first relative value exceeds 105.
[0272] [6.5] DCIR evaluation after high temperature storage [6.5.1] DCIR measurement after high temperature storage A wound battery (design capacity 1 Ah) was charged at 0.1 C to 4.2 V at a constant current and constant voltage (0.1 C-CCCV) in a temperature environment of 25°C, and then left in a charged state in an atmosphere of 60°C for 28 days. In this way, a battery after high-temperature storage was obtained. A DCIR evaluation process similar to the initial DCIR evaluation process described above was performed to determine the second DC resistance (DCIR; unit Ω).
[0273] [6.5.2] Evaluation Based on the above measured values, a second relative value was calculated by normalizing the measured value of the second direct current resistance (DCIR; unit Ω) of the reference example (without an undercoat layer) to 100, and the DCIR after high-temperature storage was evaluated according to the following criteria. The measured values of the second direct current resistance and the second relative value are shown in Table 5. Acceptable evaluations of the DCIR after high-temperature storage are "A" and "B". <Evaluation criteria> A: The second relative value is 105 or less. B: The second relative value is greater than 105 and is 110 or less. C: The second relative value exceeds 110.
[0274] (Examples 2 to 9, Comparative Examples 1 to 5) Except for changing the additive materials, additive amounts, and triple roll mill conditions of the triple roll mill in each of the preparation steps A to E as shown in Tables 2 and 4, a slurry (composition) for the undercoat layer was prepared in the same manner as in Example 1. Then, using the prepared slurry (composition) for the undercoat layer, a positive electrode current collector with an undercoat layer was produced in the same manner as in Example 1, and a wound-type battery was produced, and similar measurements and evaluations were performed. The results of the measurements and evaluations are shown in Tables 4 and 5.
[0275] [Table 2]
[0276] Example 10 A 5 L planetary dispersion was used to prepare the undercoat layer slurry. A three-roll mill (BR-300HCVIII, manufactured by Imex Co., Ltd.) was used to disperse the undercoat layer slurry. Table 3 shows the additive materials, additive amounts, and three-roll mill conditions for each of the preparation steps A to E.
[0277] 58 parts by mass of "Super-P" (A) and 87.0 parts by mass of "Al2O3" (D) were mixed for 10 minutes to obtain a mixture (Preparation Step A). 550.0 parts by mass of "CMC aqueous solution" was added to the obtained mixture and mixed for an additional 20 minutes to obtain a first mixed liquid (Preparation Step B). The "CMC aqueous solution" was prepared by adding "CMC" (D) to distilled water so that the content of "CMC" (D) was 1.0% by mass relative to the total amount of the "CMC aqueous solution." Next, 300.0 parts by mass of the "CMC aqueous solution" was added to the first mixed solution and mixed for 20 minutes. This addition operation was repeated three times to obtain a second mixed solution (preparation step C). The total amount of the "CMC aqueous solution" added to the first mixed solution was 900.0 parts by mass. Next, 72.5 parts by mass of "acrylic resin (C-4)" and 290.0 parts by mass of "W700" (B) were added to the second mixed liquid, and the mixture was kneaded for 20 minutes, and vacuum degassed for 30 minutes to obtain a third mixed liquid (preparation step D). The third mixed liquid was then dispersed twice using a three-roll mill shown in FIG. 4 under the conditions of a roll gap of 10 μm and a roll rotation speed of 300 rpm (gear ratio 1:3:9) (preparation step E). That is, the rotation speed of the feed roll 91 was 33.3 rpm, the rotation speed of the intermediate roll 92 was 100 rpm, the rotation speed of the finishing roll 93 was 300 rpm, the first interval L1 was 10 μm, and the second interval L2 was 10 μm. In this manner, a slurry (composition) for the undercoat layer having a solid content concentration of 15.3 mass % was prepared.
[0278] Then, using the prepared undercoat layer slurry (composition), a positive electrode current collector with an undercoat layer was produced, and a wound type battery was produced, and similar measurements and evaluations were performed in the same manner as in Example 1. The results of the measurements and evaluations are shown in Tables 4 and 5.
[0279] Example 11 A slurry (composition) for an undercoat layer was prepared in the same manner as in Example 10, except that the additive materials, additive amounts, and three-roll mill conditions of the three-roll mill in each of the preparation steps A to E were changed as shown in Table 3. Then, a positive electrode current collector with an undercoat layer was prepared in the same manner as in Example 1 using the prepared slurry (composition) for an undercoat layer, and a wound-type battery was also prepared, and similar measurements and evaluations were performed. The results of the measurements and evaluations are shown in Tables 4 and 5.
[0280] [Table 3]
[0281] [Table 4]
[0282] [Table 5]
[0283] In the examples, safety was maintained well compared to the comparative examples, the DC resistance at the initial stage of charging and discharging was kept low, and the increase in the DC resistance after exposure to a high-temperature environment was suppressed. As a result, an electrode and a lithium-ion secondary battery with stable and excellent battery performance can be provided. [Explanation of symbols]
[0284] 1. Lithium-ion secondary battery 10 Battery element 11 Positive electrode 11A Positive electrode current collector with undercoat layer 11B Positive electrode composite layer 12 Negative electrode 12A Negative electrode current collector with undercoat layer 12B Negative electrode composite layer 13 Separator 14 Cell Layer 21 Positive lead 22 Negative lead 30 Exterior body 110 Positive electrode current collector 111,121 Undercoat layer 120 Negative electrode current collector
Claims
1. The conductive carbon material (A), the olefin-based resin (B), and the acrylic resin (C) are contained, The composition, wherein the acrylic resin (C) comprises a first polymer obtained by polymerizing a first monomer component containing a (meth)acrylic acid ester and (meth)acrylonitrile, and a second polymer obtained by polymerizing a second monomer component containing (meth)acrylamide, and a ratio of the mass of the second polymer to the mass of the first polymer is 0.1 or more and less than 100.
2. The content of the conductive carbon material (A) is 1% by mass to 30% by mass based on the total mass of the composition, The content of the olefin-based resin (B) is 30% by mass to 90% by mass based on the total mass of the composition, The composition according to claim 1, wherein the content of the acrylic resin (C) is 1% by mass to 20% by mass based on the total mass of the composition.
3. The composition according to claim 1 , wherein the olefin-based resin (B) comprises an ethylene-based resin or a propylene-based resin.
4. 2. The composition according to claim 1, wherein the olefin resin (B) is in a particulate form, has a particle size of 0.1 μm to 9.0 μm, and has a softening point of 70° C. or higher.
5. The composition according to claim 1 , wherein the second monomer component in the acrylic resin (C) further contains a carboxyl group-containing vinyl monomer and a hydroxyl group-containing vinyl monomer.
6. Further, it contains an additive (D), The composition according to claim 1, wherein the content of the additive (D) is 1 mass% to 50 mass% based on the total mass of the composition.
7. The composition of claim 6 , wherein the additive (D) comprises carboxymethyl cellulose.
8. The composition according to claim 6, wherein the additive (D) comprises at least one of a thermally expandable microcapsule having a maximum volume expansion temperature of 70°C or more and 180°C or less and an inorganic oxide filler.
9. 2. The composition according to claim 1, wherein the ratio of particle size distribution D99 to particle size distribution D10 (D99 / D10) measured by a laser light diffraction scattering method is 35 or less.
10. 2. The composition according to claim 1, wherein the particle size distribution D99 measured by a laser light diffraction scattering method is 20 μm or less.
11. 2. The composition according to claim 1, wherein the ratio of particle size distribution D99 to particle size distribution D50 (D99 / D50) measured by a laser light diffraction scattering method is 20 or less.
12. An undercoat layer comprising the composition according to any one of claims 1 to 11.
13. An electrode comprising a current collector, the undercoat layer according to claim 12, and a mixture layer.
14. The electrode according to claim 13 , comprising the current collector, the undercoat layer, and the composite layer in this order.
15. A lithium ion secondary battery comprising the electrode according to claim 13.
Citation Information
Patent Citations
Electrochemical cell acrylic water dispersion and aqueous paste and manufacturing method of electrode and battery consisting of the same
JP2012151108A
conductive adhesive
JP2012532942A
Raw material of coating material for secondary battery separator, method for manufacturing raw material of coating material for secondary battery separator, coating material for secondary battery separator, secondary battery separator, method for manufacturing secondary battery separator, and secondary battery
JP2020087591A
Carbon material dispersion for underlayer, conductive composition for underlayer using the same, current collector with underlayer for power storage device, electrode for power storage device, power storage device
JP2022165797A
Electrically conductive composition, under layer-attached current collector for electric storage devices, electrode for electric storage devices, and electric storage device
WO2016158480A1