Method for manufacturing silicon carbide single crystal ingot

The novel method of using a molten silicon-SiO composition with a carbon source at 1400°C for SiC deposition addresses the challenges of high energy costs and slow growth in existing methods, producing high-purity SiC single crystals efficiently.

JP2024142437AInactive Publication Date: 2024-10-11村川 纪博
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023054574
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for manufacturing silicon carbide (SiC) single crystal ingots face high energy costs, difficulty in producing long crystals, and the presence of micropipes, while solution methods suffer from slow growth rates and contamination from foreign elements.

Method used

A novel solution method involving a molten composition of metallic silicon and SiO at 1400°C or higher, stirred with a carbon source to disperse or dissolve SiC at a high concentration, allowing SiC to be deposited on a seed crystal for continuous growth.

Benefits of technology

This method enables high-purity, high-quality SiC single crystal ingots with reduced manufacturing costs and eliminates the need for mixing foreign elements, achieving faster growth rates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142437000001_ABST
    Figure 2024142437000001_ABST
Patent Text Reader

Abstract

To provide a method for manufacturing a high purity SiC single crystal ingot by a solution method having a low process temperature without intentionally mixing different elements with metal silicon like the conventional solution method.SOLUTION: A method for manufacturing a SiC single crystal ingot comprises steps of: bringing a molten composition 10 including metal silicon and silicon monoxide and having a temperature of 1400°C or more into contact with a carbon source under stirring to form silicon carbide in the molten composition; and depositing the silicon carbide on a silicon carbide seed crystal 14 immersed in the molten composition. The molten composition including the metal silicon and the silicon monoxide and having the temperature of 1400°C or more is prepared by mixing molten metal silicon and particulate silicon monoxide, by mixing molten metal silicon and particulate silica dioxide, or by supplying a silicon compound including a Si-O bond to an upper space 12 of the molten metal silicon in a vapor phase.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a method for producing a silicon carbide single crystal ingot for preparing silicon carbide single crystal wafers. [Background technology]

[0002] Silicon carbide (SiC) has excellent inherent properties as a semiconductor material, and if it were to replace silicon (Si), the current power device semiconductor material used for controlling and converting electricity, it would be possible to significantly reduce energy loss and is expected to make a significant contribution to reducing carbon dioxide, a greenhouse gas.

[0003] SiC single crystal wafers are manufactured using SiC single crystal ingots as the starting material, which go through a series of processes including cutting, polishing, cleaning, and inspection. Here, SiC single crystal ingots are commercially produced by a sublimation method known as the modified Lely process, in which SiC powder is sublimated at approximately 2300°C to precipitate a SiC single crystal on a seed crystal at approximately 2200°C.

[0004] This sublimation method has the drawbacks of extremely high manufacturing costs due to the excessive energy costs required for heating, the difficulty of producing long SiC single crystals, and the inevitable presence of fine, continuous pores known as micropipes in the deposited SiC single crystals.

[0005] In view of these problems, methods for producing SiC single crystal ingots using the so-called solution method have also been investigated. As an example of this solution method, a method has been proposed in which a seed SiC single crystal substrate and a polycrystalline SiC substrate are placed face to face with an extremely thin layer of molten silicon interposed therebetween, and SiC is dissolved and transferred into the molten silicon to epitaxially grow SiC on the SiC seed crystal (see, for example, Patent Document 1).

[0006] Because this solution method is a growth method close to thermodynamic equilibrium, it is expected to grow crystals with extremely low crystal defect densities. It also has the advantage of significantly lower process temperatures than sublimation methods, and the ability to grow long crystals. However, the extremely low SiC concentration in the molten silicon results in an extremely slow growth rate of SiC single crystals.

[0007] To solve the problem of the slow growth rate associated with the solution method, a solution method has been proposed in which a process of dissolving carbon or carbon and Si in molten silicon is introduced, and dissimilar elements such as Ti, Cr, and La are added to the molten silicon to further increase the solubility of carbon and increase the growth rate of SiC on SiC seed crystals (see, for example, Patent Documents 2, 3, and 4). However, there is a problem in that even trace amounts of dissimilar elements remaining in the resulting SiC ingot have an unacceptable adverse effect on the performance of the SiC semiconductor. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] WO2002 / 099169 [Patent Document 2] Japanese Patent Application Laid-Open No. 2015-212215 [Patent Document 3] Japanese Patent Publication No. 2022-89311 [Patent Document 4] Japanese Patent Publication No. 2023-24315 Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention aims to provide a method for producing high-purity SiC single crystal ingots by a novel solution process, which uses a process temperature significantly lower than that of the conventional modified Lely process and does not require intentional mixing of different elements into metallic silicon as in the conventional solution process. [Means for solving the problem]

[0010] The above-mentioned object can be achieved by a method for producing a SiC single crystal ingot, comprising the steps of: bringing a molten composition containing metallic silicon and SiO and having a temperature of 1400°C or higher into contact with a carbon source under stirring to produce SiC in the molten composition; and precipitating the SiC on a SiC seed crystal immersed in the molten composition.

[0011] The present inventors have discovered that by contacting a molten composition containing high-temperature metallic silicon and SiO, i.e., a molten composition containing metallic silicon and SiO and having a temperature of 1400°C or higher, with a carbon source under stirring, it is possible to obtain a metallic silicon-containing molten composition in which SiC is dispersed or dissolved at a concentration far higher than that previously known.

[0012] Specifically, the present inventors have found that when the SiC concentration in a molten composition obtained by contacting molten metal silicon without containing SiO with a carbon source for a certain period of time is compared with the SiC concentration in a molten composition obtained by contacting molten metal silicon containing SiO with a carbon source for a certain period of time, the latter has a significantly higher SiC concentration, at least 10 times that of the former.

[0013] The reason for this is not entirely clear, but the inventors speculate that if SiO is present, the interaction between SiO and Si present in the molten silicon metal generates active SiO, which promotes the reaction with the carbon source to generate SiC, and furthermore, SiO becomes a monomolecular gas in the molten silicon at 1400°C or higher and comes into contact with the carbon source, and SiC generated by the reaction between SiO and the carbon source is also generated in a monomolecular state.

[0014] Furthermore, since the monomolecular SiC produced in the molten silicon metal has high mobility, the bonding between the SiC molecules becomes extremely low, and it is presumed that this results in a metal silicon-containing molten composition in which SiC is dispersed or dissolved at a concentration significantly higher than the solubility of solid SiC in the molten silicon metal.

[0015] Furthermore, the inventors have found that when a SiC seed crystal is immersed in a molten composition in which SiC is dispersed or dissolved at such a high concentration, a SiC single crystal precipitates on the seed crystal, and that by gradually and continuously withdrawing the seed crystal, a SiC single crystal can be continuously grown. Here, the concentration of dispersed or dissolved SiC at this high concentration is at least 1 wt %, preferably 5 to 20 wt %, and more preferably 10 to 40 wt %, based on the total weight of the molten composition.

[0016] The temperature of the molten composition is not particularly limited as long as it is 1400°C or higher and in a molten state, but temperatures as high as 1700°C or higher are not appropriate because the vapor pressure of metallic silicon in the molten composition would increase.

[0017] In a preferred embodiment, the molten composition containing metallic silicon and SiO and having a temperature of 1400°C or higher is prepared from molten metallic silicon and powdered or granular SiO. For example, it can be prepared by heating a mixture of granular or chunky metallic silicon and powdered or granular SiO in an inert atmosphere to a temperature equal to or higher than the melting temperature of the metallic silicon and mixing by stirring or the like.

[0018] In another preferred embodiment, the above-mentioned molten composition containing metallic silicon and SiO and having a temperature of 1400°C or higher is prepared from molten metallic silicon and powdered or granular silicon dioxide. For example, a molten composition containing metallic silicon and SiO in a predetermined content can be prepared by heating a mixture of granular or chunky metallic silicon and powdered or granular silicon dioxide in a predetermined ratio in an inert atmosphere to a temperature equal to or higher than the melting temperature of the metallic silicon and mixing by stirring or the like, thereby generating SiO through a reaction between the metallic silicon and silicon dioxide.

[0019] In another preferred embodiment, the molten composition containing metallic silicon and SiO and having a temperature of 1400°C or higher is prepared by supplying a silicon compound containing an Si-O bond in a vapor phase to the headspace above molten metallic silicon. For example, a molten composition containing predetermined contents of metallic silicon and SiO can be prepared by converting a compound selected from the group consisting of SiO, silicon alkoxides such as silicon tetraethoxide, and siloxane compounds such as disiloxane into a vapor phase at an appropriate temperature and supplying the vaporized compound to the headspace above molten metallic silicon under stirring for an appropriate period of time.

[0020] The ratio of metallic silicon to SiO present in the molten composition containing metallic silicon and SiO thus prepared is not particularly limited, but a rough guideline is 1 to 30 parts by weight, more preferably 3 to 20 parts by weight, of SiO per 100 parts by weight of metallic silicon.

[0021] The carbon source for producing SiC upon contact with the molten composition may be carbon in various forms, such as powder, granule, or lump carbonaceous materials, and these carbon sources can be mixed with and contacted with the molten composition by stirring or other means. Alternatively, the carbon container that contains the molten composition may itself be used as the carbon source, and the molten composition may be stirred in the container to contact the carbon source. Alternatively, a carbon-containing compound may be supplied in a vapor phase to the space above the molten composition, and the carbon-containing compound may be brought into contact with the surface of the molten composition under stirring.

[0022] Here, the carbon compound is preferably a compound having 1 to 16 carbon atoms in one molecule, i.e., a C1 to C16 compound, and specific examples include CO, CH4, C2H6, C2H4, C2H2, C3H8, C3H6, and mixtures thereof.

[0023] In the present invention, such a carbon source is brought into contact with a molten composition having a temperature of 1400°C or higher under stirring. Such stirring can be performed by rotating a stirring blade in the molten composition, applying vibration to the molten composition by an ultrasonic vibrator or a mechanical vibrator, rotating the container of the molten composition, or a combination thereof.

[0024] As described above, by bringing a molten composition containing metal silicon and SiO and having a temperature of 1400°C or higher into contact with a carbon source, SiC is generated in the molten composition, and the generated SiC is deposited on a SiC seed crystal. The step of generating SiC in such a molten composition and the step of depositing the generated SiC on a SiC seed crystal may be performed simultaneously or alternately.

[0025] Note that silicon monoxide (SiO) in the present invention does not necessarily have x = 1 when represented by SiOx, and those with 0.7 < x < 1.5 when represented by SiOx are also included in silicon monoxide in the present invention.

Advantages of the Invention

[0026] In the method for producing a SiC single crystal ingot by a solution method, there is no need to intentionally mix a foreign element into metallic silicon to increase the solubility of SiC, and since it is a method of continuously pulling up a SiC single crystal, it is possible to provide a method for producing a high purity and high quality SiC single crystal ingot with reduced production costs.

Brief Description of the Drawings

[0027] [Figure 1] It is a schematic diagram of a manufacturing apparatus used in the method for producing a silicon carbide single crystal according to the present invention.

Embodiments for Carrying Out the Invention

[0028] The method for producing a SiC single crystal ingot of the present invention includes the steps of: bringing a molten composition containing metallic silicon and SiO and having a temperature of 1400°C or higher into contact with a carbon source while stirring to produce silicon carbide in the molten composition; and precipitating the silicon carbide on a silicon carbide seed crystal immersed in the molten composition.

[0029] 1 is a schematic diagram showing one embodiment of an apparatus used in this method. Molten composition 10 is contained in a heat-resistant container 11, and an upper space 12 exists above the surface of molten composition 10. Molten composition 10 is heated through the side wall of heat-resistant container 11 by a heater 13, and the heating temperature of heater 13 is controlled to an appropriate temperature of 1400°C or higher.

[0030] The volume, shape, etc. of heat-resistant vessel 11 are designed appropriately depending on the size of the SiC single crystal to be precipitated, etc. Although not limited thereto, as a rough guide, when a SiC single crystal with a diameter of 6 inches is to be produced, heat-resistant vessel 11 is cylindrical with an inner diameter of 20 to 50 cm and an inner height of 10 to 60 cm, and the size of the SiC seed crystal is 3 to 5 inches in diameter.

[0031] In one embodiment, the molten composition of the present invention, which contains metallic silicon and SiO and has a temperature of 1400°C or higher, can be prepared using a heat-resistant container 11. For example, a mixture of granular or chunky metallic silicon and powdered or granular SiO is charged into heat-resistant container 11, an inert atmosphere such as argon is created in headspace 12, and the mixture of metallic silicon and SiO is heated to a temperature of 1400°C or higher by heating using heater 13 while stirring by rotating stirring blade 14, thereby preparing molten composition 10.

[0032] In another embodiment, molten composition 10 can also be prepared from metallic silicon and granular silicon dioxide. For example, similar to the above, molten composition 10 can be prepared by charging a mixture of granular or chunky metallic silicon and powdered or granular silicon dioxide into heat-resistant container 11, filling head space 12 with an inert atmosphere such as argon, and heating the mixture of metallic silicon and silicon dioxide to a temperature of 1400°C or higher using heater 13 while rotating stirring blade 14, thereby reacting at least a portion of the silicon dioxide with the metallic silicon to produce SiO.

[0033] In another embodiment, the molten composition can be prepared by supplying a silicon compound containing Si-O bonds in a vapor phase to the space above molten metallic silicon. For example, metallic silicon is loaded into heat-resistant container 11 shown in FIG. 1, and the metallic silicon is heated to a melting temperature or higher using heater 13. Then, compounds selected from the group consisting of, for example, SiO, silicon alkoxides such as silicon tetraethoxide, and siloxane compounds such as disiloxane are supplied in a vapor phase at appropriate temperatures through inlet channel 15, thereby preparing molten composition 10 containing metallic silicon and SiO. Note that, if decomposition gases are generated from the silicon compound, they can be discharged through exhaust gas channel 17.

[0034] The resulting molten composition 10, which contains silicon metal and SiO and has a temperature of 1400°C or higher, is then brought into contact with a carbon source under stirring. Stirring means for this molten composition include rotating a stirring blade 14 attached to a stirring rod 16 in the molten composition, immersing an ultrasonic vibrator or mechanical vibrator in the molten composition to impart vibration, or rotating a heat-resistant container containing the molten composition. These stirring means may also be combined.

[0035] To bring the molten composition under stirring into contact with the carbon source, if the carbon source is a powder, granule, or lump solid carbon substance, the carbon source is added to the molten composition to form a mixture, and then a stirring means such as the stirring blade 14 described above is applied to this mixture.

[0036] Furthermore, when the carbon source is the heat-resistant carbon container itself that contains the molten composition, the above-mentioned stirring means may be applied to the molten composition in the container, and when the carbon source is a gaseous carbon compound, for example, a carbon-containing compound may be supplied in gaseous phase to the space above the molten composition and brought into contact with the surface of the molten composition while a stirring means such as the stirring blade 14 is applied to the molten composition. Note that, when decomposition gas is generated from the silicon compound, it can be discharged from the exhaust gas flow path 17.

[0037] In this way, by bringing molten composition 10, which contains metallic silicon and SiO and has a temperature of 1400°C or higher, into contact with a carbon source under stirring, SiC can be produced by reaction in molten composition 10. As described above, the reaction that produces SiC is presumably due to the reaction between SiO activated by the molten metallic silicon and the carbon source, and therefore SiC is produced in a monomolecular state.

[0038] The target SiC single crystal ingot can be precipitated on a SiC seed crystal 14 by immersing the seed crystal in the SiC-containing molten composition 10 obtained by the above process, and a long SiC single crystal ingot can be produced by continuously pulling up the SiC seed crystal 14 using a pulling rod 16. In Fig. 1, the SiC seed crystal and the stirring blade are labeled 14 in the same position, and the pulling rod and the stirring rod are labeled 16 in the same position, but this is merely for convenience in drawing, and it should be understood that the two are separate entities with separate functions. [Example]

[0039] 50 g of metallic silicon granules were placed in a 50 mL double-layered heat-resistant container (inside: quartz, outside: isotropic graphite) as shown in Figure 1, and the metallic silicon was heated to 1550°C by electrical heating using a heater to melt it. Next, while the heat-resistant container was vibrated by a mechanical vibrator, 20 g of SiO powder was dropped onto the surface of the molten metallic silicon from an inlet channel over a period of 10 minutes, and the mixture of molten metallic silicon and SiO powder was stirred by vibrating for 1 hour, yielding a molten composition containing SiO and metallic silicon.

[0040] Next, the temperature of the molten composition was maintained at 1550°C while stirring with a mechanical vibrator. Propane gas was supplied to the upper space at 1 atmosphere pressure through the inlet passage at a flow rate of 0.5 mol / h together with argon gas at a flow rate of 2 mol / h. The exhaust gas, including the thermal decomposition gas of the propane gas, was discharged through the exhaust gas passage leading to the atmosphere. This condition was maintained for 5 hours to generate SiC in the molten composition, resulting in the preparation of a molten composition containing 9.5 wt% SiC.

[0041] Next, stirring was stopped while the temperature of the molten composition was maintained at 1550°C, and a 4H-SiC seed crystal was immersed in the molten composition as shown in Figure 1. The seed crystal, immersed to a depth of 5 mm in the molten composition, had a 10 x 10 mm diameter and its bottom surface was pulled up at a rate of 1 mm / h and observed. As a result, it was confirmed that a 4H-SiC single crystal had formed on the bottom surface of the 4H-SiC seed crystal, and the growth rate of this single crystal was 190 µm / h. Comparative Example 1

[0042] In the same manner as in Example 1, except that no SiO powder was used, metallic silicon was heated to 1550°C using a heat-resistant container as shown in FIG. 1 to melt it, and the molten metallic silicon was exposed to propane gas while stirring to generate SiC in the molten metallic silicon, thereby preparing a molten composition containing 0.25 wt% SiC.

[0043] Next, stirring was stopped while maintaining the temperature of the molten composition at 1550°C, and the bottom surface of the 4H—SiC seed crystal was immersed in the molten composition to a depth of 5 mm and then pulled up at a rate of 1 mm / h. As a result, it was confirmed that a 4H—SiC single crystal had formed on the bottom surface of the 4H—SiC seed crystal, and the growth rate of this single crystal was less than 10 μm / h. [Example]

[0044] 1, 50 g of metal silicon granules were heated to 1550°C and melted. Next, 20 g of SiO powder was heated to 1400°C and gradually sublimated, and argon was used as a carrier gas at a flow rate of 0.3 mol / h to accompany the SiO sublimation gas. This was introduced into the upper space through the inlet channel over 1 hour, and the SiO was brought into contact with the molten metal silicon under stirring to obtain a molten composition.

[0045] Next, the temperature of the molten composition under stirring using a mechanical vibrator was maintained at 1550°C, and 15 g of fine carbon powder was supplied through the inlet channel. This state was maintained for 5 hours to generate SiC in the molten composition, thereby preparing a molten composition containing 15.3 wt% SiC.

[0046] Next, stirring was stopped while maintaining the temperature of the molten composition at 1550°C, and the bottom surface of a 10 × 10 mm 4H—SiC seed crystal was immersed in the molten composition to a depth of 5 mm, as shown in Figure 1, and then pulled up at a rate of 1 mm / h. As a result, it was confirmed that a 4H—SiC single crystal had formed on the bottom surface of the 4H—SiC seed crystal, and the growth rate of this single crystal was 230 μm / h. [Example]

[0047] As in Example 1, 50 g of metallic silicon granules were heated to 1550°C and melted using the heat-resistant container shown in Figure 1. Next, 10 g of SiO2 fine powder was introduced into the upper space through the inlet channel over a period of 1 hour, and the SiO2 fine powder and molten metallic silicon were stirred for 5 hours to obtain a molten composition containing SiO2 and metallic silicon.

[0048] Next, the temperature of the molten composition, which was being stirred by a mechanical vibrator, was maintained at 1550°C, and methane gas was supplied to the upper space at a pressure of 0.1 MPa through the inlet passage at a flow rate of 1.5 mol / h together with argon gas at a flow rate of 2 mol / h. Exhaust gas containing methane pyrolysis gas was discharged through the exhaust gas passage leading to the atmosphere. This condition was maintained for 5 hours to generate SiC in the molten composition, resulting in a molten composition containing 7.3 wt% SiC.

[0049] Next, stirring was stopped while maintaining the temperature of the molten composition at 1550°C, and the bottom surface of a 10 × 10 mm 4H—SiC seed crystal was immersed in the molten composition to a depth of 5 mm, as shown in Figure 1, and then pulled up at a rate of 1 mm / h. As a result, it was confirmed that a 4H—SiC single crystal had formed on the bottom surface of the 4H—SiC seed crystal, and the growth rate of this single crystal was 150 μm / h. [Industrial Applicability]

[0050] This provides a novel solution method for producing high-purity SiC single crystal ingots, which uses a process temperature significantly lower than that of the conventional modified Lely process and does not require intentional mixing of different elements into metallic silicon as in the conventional solution process. [Explanation of symbols]

[0051] 10. Molten composition 11. Heat-resistant container 12‥Upper space 13. Heater 14. SiC seed crystal or stirring blade 15. Inlet channel 16. Pulling rod or stirring rod 17. Exhaust gas flow path

Claims

1. 1. A method for producing a silicon carbide single crystal ingot, comprising the steps of: contacting a molten composition containing metallic silicon and silicon monoxide and having a temperature of 1400°C or higher with a carbon source under stirring to produce silicon carbide in the molten composition; and precipitating the silicon carbide on a silicon carbide seed crystal immersed in the molten composition.

2. 2. The method for producing a silicon carbide single crystal ingot according to claim 1, wherein the molten composition containing silicon metal and silicon monoxide and having a temperature of 1400°C or higher is prepared by mixing molten silicon metal and granular silicon monoxide.

3. 2. The method for producing a silicon carbide single crystal ingot according to claim 1, wherein the molten composition containing silicon metal and silicon monoxide and having a temperature of 1400°C or higher is prepared by mixing molten silicon metal with granular silicon dioxide.

4. 2. The method for producing a silicon carbide single crystal ingot according to claim 1, wherein the molten composition containing silicon metal and silicon monoxide and having a temperature of 1400° C. or higher is prepared by supplying a silicon compound containing Si—O bonds in a gas phase to a head space of molten silicon metal.

5. 5. The method for producing a silicon carbide single crystal ingot according to claim 1, wherein the carbon source is at least one of powdered carbon added to the molten composition, a carbon container that contains the molten composition, and a carbon-containing compound supplied to an upper space above the molten composition.

6. The method for producing a silicon carbide single crystal ingot according to any one of claims 1 to 5, wherein the step of generating silicon carbide in the molten composition and the step of precipitating silicon carbide on the silicon carbide seed crystal are carried out simultaneously.

7. The method for producing a silicon carbide single crystal ingot according to any one of claims 1 to 5, wherein the step of generating silicon carbide in the molten composition and the step of precipitating silicon carbide on the silicon carbide seed crystal are performed alternately.

Citation Information

Patent Citations

  • Process of producing ceramic matrix composites, and ceramic matrix composites formed thereby

    JP2015212215A

  • Production method of silicon carbide single crystal

    JP2022089311A

  • METHOD FOR MANUFACTURING SiC SINGLE CRYSTAL

    JP2023024315A

  • Single crystal silicon carbide and method for producing the same

    WO2002099169A1