Carburizing steel

The carburizing steel composition optimizes element ratios to suppress grain boundary oxidation, enhancing both bending and surface fatigue strengths while controlling Mo content for cost-effectiveness.

JP2024142650APending Publication Date: 2024-10-11DAIDO STEEL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023054887
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing carburizing steels face challenges in achieving both high bending fatigue strength and surface fatigue strength due to the formation of grain boundary oxidation layers, which are exacerbated by high Mo content, leading to increased material costs.

Method used

A carburizing steel composition with controlled amounts of C, Si, Mn, Cr, Mo, and Al, satisfying specific ratios (Cr/Mn-0.6Si >= 2.0 and Cr-1.82Si >= -0.7, limits Mo to 0.40% or less, thereby suppressing grain boundary oxidation and enhancing temper softening resistance.

Benefits of technology

The steel achieves both high bending fatigue strength and surface fatigue strength while reducing material costs by minimizing Mo content and optimizing carbon concentration, ensuring a shallow grain boundary oxidation layer and improved surface hardness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a carburizing steel capable of achieving both high flexure fatigue strength and surface fatigue strength, through gas carburization, at low cost.SOLUTION: A carburizing steel containing, by mass%, 0.10%≤C≤0.30%, 0.50%≤Si≤1.20%, 0.05%≤Mn≤0.80%, 0.30%≤Cr≤2.00%, 0.01%≤Mo≤0.40%, 0.02%≤Al≤0.10%, P≤0.030%, S≤0.030%, Cu≤0.3%, with the balance being Fe and unavoidable impurities, and satisfying the following formulas (1) and (2). Cr / Mn-0.6Si≥2.0 (1) Cr-1.82Si≥-0.7 (2) In formulas (1) and (2), the symbols of the elements indicate the content of each element in units of mass%.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a carburizing steel. [Background technology]

[0002] Steel materials that compose parts that require mechanical strength, such as gears, may be carburized and quenched to improve mechanical properties such as fatigue strength and pitting resistance. Currently, gas carburizing is the most widely used carburizing method. In gas carburizing, carburizing gas such as acetylene, propane, or ethanol is introduced into an atmospheric furnace to heat the steel material, and the carbon monoxide generated by the incomplete combustion of the carburizing gas causes carbon to be absorbed on the surface of the steel material, increasing the carbon concentration on the surface. Gas carburizing improves the surface quenching hardness and tempered hardness, resulting in high mechanical properties.

[0003] As explained in the following Patent Document 1, when gas carburizing is performed, oxygen atoms derived from moisture and oxygen molecules in the carburizing furnace form oxides along the prior austenite grain boundaries from the steel surface, generating a grain boundary oxide layer. The grain boundary oxide layer becomes the starting point of fracture and reduces the bending fatigue strength of the carburized steel. Furthermore, when the grain boundary oxide layer absorbs alloy elements in the steel, it becomes difficult to obtain a martensite structure during quenching, and a pearlite or bainite structure is generated, and a carburized abnormal layer with reduced hardness may be formed. The carburized abnormal layer acts as a defect and deteriorates the mechanical properties of the steel. One of the measures to suppress the generation of the grain boundary oxide layer is to reduce the content of Si, an element that reacts with oxygen, in the carburizing steel.

[0004] On the other hand, when hardened steel is used in applications such as gears where the surface generates heat due to friction, the surface of the steel may be pseudo-tempered due to the heat generated. By increasing the Si and Mo content in carburizing steel, the decrease in hardness during tempering can be minimized. In other words, tempering softening resistance can be increased. Improved tempering softening resistance increases the surface fatigue strength of the steel. Conversely, if the Si and Mo content is low, the surface fatigue strength is likely to be low.

[0005] Thus, in the case of a steel for carburizing which is used after gas carburizing, if the content of Si is reduced, the generation of the grain boundary oxide layer is suppressed, which is effective in improving the bending fatigue strength, but on the other hand, the tempering softening resistance is reduced, making it difficult to obtain high surface fatigue strength. Therefore, a method of suppressing the generation of the grain boundary oxide layer and increasing the content of Mo while suppressing the generation of the grain boundary oxide layer and increasing the tempering softening resistance can be considered. In addition, from the viewpoint of preventing the generation of the grain boundary oxide layer from leading to the generation of the carburizing abnormal layer even if the grain boundary oxide layer is generated, a method of adding a large amount of Mo or Cr, which has the effect of suppressing the precipitation of pearlite and bainite (enhancing hardenability), to the steel for carburizing can be considered. In each example of Patent Document 1, about 0.5 mass % of Mo is added to the steel. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2003-27142 A Summary of the Invention [Problem to be solved by the invention]

[0007] As described above, in the case of carburizing steel subjected to gas carburizing, if the Si content is kept low and the Mo content is increased, the generation of the grain boundary oxide layer can be suppressed to increase the bending fatigue strength, and the surface fatigue strength can be increased by increasing the tempering softening resistance. However, since Mo is an expensive metal, if a large amount of Mo is added to the carburizing steel to suppress the decrease in tempering softening resistance and improve hardenability, the material cost will increase.

[0008] The problem to be solved by the present invention is to provide carburizing steel that is inexpensive and can achieve both high bending fatigue strength and surface fatigue strength after gas carburizing.

Means for Solving the Problem

[0009] To solve the above problems, the carburizing steel according to the present invention has the following configuration. [1] The carburizing steel according to the present invention contains, in mass%, 0.10% ≤ C ≤ 0.30%, 0.50% ≤ Si ≤ 1.20%, 0.05% ≤ Mn ≤ 0.80%, 0.30% ≤ Cr ≤ 2.00%, 0.01% ≤ Mo ≤ 0.40%, 0.02% ≤ Al ≤ 0.10%, P ≤ 0.030%, S ≤ 0.030%, Cu ≤ 0.3%, and the balance consists of Fe and inevitable impurities, and satisfies the following formulas (1) and (2). Cr / Mn - 0.6Si ≥ 2.0 (1) Cr - 1.82Si ≥ -0.7 (2) In the above formulas (1) and (2), each element symbol indicates the content of each element in mass%.

[0010] [2] In the aspect of [1] above, the carburizing steel may further contain at least one of 0% < Ni ≤ 0.30%, 0% < Nb ≤ 0.05%, 0% < Ti ≤ 0.05%, 0% < B ≤ 0.005% in mass%.

[0011] [3] In the aspect of [1] or [2] above, it is preferable that the depth of the grain boundary oxide layer after gas carburizing is less than 7.0 μm.

Effect of the Invention

[0012] [1] The carburizing steel according to the present invention contains each of the component elements in the above-mentioned predetermined contents, and the contents of Cr, Mn, and Si satisfy the relationship of the above formula (1). This allows the steel to contain only a small amount of Mo, 0.40 mass% or less, thereby suppressing material costs, and simultaneously improves bending fatigue strength by suppressing the formation of grain boundary oxide layers and improves surface fatigue strength by improving temper softening resistance. In addition, by satisfying formula (2), it becomes easier to increase the carbon concentration on the surface during carburizing, and the high hardness is highly effective in improving bending fatigue strength. Furthermore, the cost required for carburizing can be kept low by reducing the amount of carburizing gas used.

[0013] In the above aspect [2], the carburizing steel further contains at least one of Ni, Nb, B, and Ti in the above-mentioned predetermined amount, thereby further improving the material properties of the carburizing steel after carburization. Ni contributes to improving toughness, and Nb and Ti act to suppress the deterioration of mechanical properties due to grain coarsening during carburization. In addition, B has the effect of improving hardenability.

[0014] In the above embodiment [3], the depth of the grain boundary oxide layer after gas carburization is suppressed to 7.0 μm or less, thereby obtaining high bending fatigue strength. [Brief description of the drawings]

[0015] [Figure 1] 1 is a diagram for explaining a bending fatigue test, in which (a) shows the conditions of the carburizing treatment before the test, and (b) is a schematic diagram showing the test method (left: side view, right: front view). [Diagram 2] Fig. 1 is a diagram explaining the surface fatigue test, in which (a) shows the conditions of the carburizing heat treatment before the test, and (b) is a schematic diagram showing the test method (left: side view, right: front view). [Diagram 3] As an example of a sample cross section on which an intergranular oxide layer is formed, an optical microscope image of the sample cross section of Comparative Example 7 is shown. In the image, the region where the intergranular oxide layer exists is indicated by a dashed line. [Figure 4]Graphs showing test results. (a) shows the relationship between Cr / Mn-0.6Si and the depth of the grain boundary oxide layer. (b) shows the relationship between Cr / Mn-0.6Si and bending fatigue strength. (c) shows the relationship between the Si content and the surface fatigue strength. (d) shows the relationship between Cr-1.82Si and the surface carbon content. Examples are indicated with circles, and comparative examples are indicated with triangles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] A carburizing steel according to one embodiment of the present invention will be described in detail below. In this specification, the content of each element is expressed in mass% in a state without carburization. In addition, in this specification, each property is a value evaluated at room temperature (approximately 25°C) unless otherwise specified.

[0017] [Content of each component element] The carburizing steel according to this embodiment contains predetermined amounts of C, Si, Mn, Cr, Mo, and Al, with the balance being Fe and unavoidable impurities. The types, contents, and reasons for limiting the additive elements are as follows:

[0018] 0.10%≦C≦0.30% C contributes to improving the hardness deep inside the steel material by forming carbides with Cr etc. To fully obtain the effect of improving hardness, the C content is set to 0.10% or less.

[0019] On the other hand, if the C content is excessive, it will cause a decrease in workability in carburizing steel. From the viewpoint of ensuring workability, C is set to 0.30% or less.

[0020] 0.50%≦Si≦1.20% Silicon has the effect of increasing the pitting resistance and improving the surface fatigue strength of steel materials after carburization. From the viewpoint of fully obtaining these effects, the Si content is set to 0.50% or less.

[0021] On the other hand, if the Si content is excessive, the grain boundary oxide layer is easily formed through carburization, which leads to a decrease in bending fatigue strength. From the viewpoint of suppressing the formation of the grain boundary oxide layer, the Si content is set to be ≦ 1.20%, and preferably, Si ≦ 0.90%.

[0022] 0.05%≦Mn≦0.80% Mn plays a role in improving the hardenability of steel. From the viewpoint of fully obtaining the effect of improving hardenability, the Mn content is set to 0.05% or less, and preferably 0.30% or less.

[0023] On the other hand, if a large amount of Mn is contained, it becomes difficult to satisfy formula (1) described later, and it becomes difficult to obtain the effect of improving bending fatigue strength after carburization, which is a phenomenon that is highly correlated with the satisfaction of formula (1).From this viewpoint, Mn≦0.80% is specified.

[0024] 0.30%≦Cr≦2.00% Cr increases the equilibrium carbon concentration during carburization and is highly effective in improving surface hardness. It also works to improve hardenability. Furthermore, Cr satisfies formula (1) in balance with the Mn content, suppressing the formation of grain boundary oxide layers and showing an effect on improving bending fatigue strength. From the viewpoint of fully obtaining these effects, the Cr content is set to 0.30%≦Cr. It is preferably set to 1.00%≦Cr.

[0025] On the other hand, from the viewpoint of reducing material costs, Cr≦2.00%, and preferably Cr≦1.60%.

[0026] 0.01%≦Mo≦0.40% Mo improves the hardenability of steel materials. It also increases the temper softening resistance. To fully obtain these effects, the Mo content is set to 0.01% or less.

[0027] On the other hand, Mo is an expensive metal, and from the viewpoint of obtaining an inexpensive carburizing steel by suppressing material costs, Mo≦0.40%, preferably Mo≦0.30%.

[0028] 0.02%≦Al≦0.10% Al suppresses the coarsening of crystal grains during carburizing. To obtain this effect sufficiently, the Al content is set at 0.02% or less.

[0029] On the other hand, Al forms inclusions that deteriorate the mechanical properties of steel materials. From the viewpoint of suppressing the formation of inclusions, the Al content is set at 0.10% or less.

[0030] The carburizing steel according to this embodiment may contain P, S, and Cu in addition to the above-mentioned predetermined amounts of C, Si, Mn, Cr, Mo, and Al, but the contents of each are restricted to the following upper limits or less. However, these elements do not have any positive effect when contained in the carburizing steel, and therefore may not be contained.

[0031] P≦0.030% P deteriorates the mechanical properties of steel materials by grain boundary segregation. From the viewpoint of suppressing grain boundary segregation, the P content is controlled within the range of P≦0.030%, and preferably P≦0.015%.

[0032] S≦0.030% S forms coarse MnS grains, which deteriorates the mechanical properties of the steel material. From the viewpoint of suppressing the formation of coarse MnS grains, the S content is controlled to within the range of S≦0.030%, and preferably S≦0.015%.

[0033] Cu≦0.30% Cu is an element that is added to many steel materials, but in the carburizing steel according to this embodiment, the addition of Cu has almost no positive effect. Even if Cu is added, it is limited to Cu≦0.30% from the viewpoint of reducing material costs. Preferably, Cu≦0.16%.

[0034] Examples of unavoidable impurities other than P, S, and Cu that may be contained in the steel material according to this embodiment include V≦0.1%, Co≦0.1%, O≦0.01%, N≦0.03%, Sn≦0.01%, Sb≦0.01%, etc. It is preferable that the total amount of unavoidable impurities is suppressed to 0.1% or less.

[0035] In addition to the essential elements described above, the steel material according to this embodiment may further contain at least one selected from Ni, Nb, Ti, and B. The contents of each element and the reasons for limiting them are as follows.

[0036] 0% <Ni≦0.30% Ni improves the toughness of steel. Even a small amount of Ni added has a high effect on improving toughness, so there is no particular lower limit for the Ni content.

[0037] On the other hand, Ni is an expensive element, and from the viewpoint of reducing material costs, Ni≦0.30% is set. More preferably, Ni≦0.1% is set. Note that Ni of about 0.05% or less can be contained in the carburizing steel as an unavoidable impurity.

[0038] 0% <Nb≦0.05% Nb contributes to suppressing the coarsening of crystal grains and the resulting deterioration of mechanical properties when carburizing is performed under high temperature conditions or conditions where carburizing progresses quickly. Since even a small amount of Nb exerts this effect, there is no particular lower limit for the content. From the viewpoint of obtaining a particularly high effect, it is preferable that the Nb content is 0.01% or less.

[0039] However, Nb reduces the mechanical strength of steel by forming coarse carbides. From the viewpoint of suppressing such phenomena, the Nb content is set to 0.05% or less. More preferably, Nb is set to 0.03% or less.

[0040] 0% <Ti≦0.05% Ti contributes to suppressing the coarsening of crystal grains and the resulting deterioration of mechanical properties when carburizing is performed under high temperature conditions or conditions where carburizing progresses rapidly. Since even a small amount of Ti exerts this effect, there is no particular lower limit for the content. From the viewpoint of obtaining a particularly high effect, it is preferable that the Ti content is 0.01% or less.

[0041] However, Ti reduces the mechanical strength of steel by forming coarse nitrides and carbides. From the viewpoint of suppressing these phenomena, Ti≦0.05% is set, and more preferably Ti≦0.03%.

[0042] 0% <B≦0.005% B contributes to improving the hardenability of steel. Even a small amount of B has a significant effect of improving hardenability, so there is no particular lower limit for the B content. From the viewpoint of obtaining a particularly high effect, it is preferable that the B content is 0.001% or less.

[0043] However, B generates coarse nitrides, which reduces the mechanical strength of the steel material. From the viewpoint of suppressing this phenomenon, B≦0.005% is set, and more preferably, B≦0.003%.

[0044] [Relationship between the content of component elements] Next, the relationship between the contents of the component elements will be described. In the formulas that define the relationship between the contents of the component elements, each element symbol indicates the content of each element in units of mass%.

[0045] In the carburizing steel according to this embodiment, the contents of Si, Mn, and Cr satisfy the following formula (1), and the contents of Cr and Si satisfy the following formula (2).

[0046] Cr / Mn-0.6Si≧2.0 (1) When gas carburizing steel is subjected to gas carburization, Si easily bonds with oxygen atoms derived from moisture and oxygen molecules in the furnace to form a grain boundary oxide layer. Therefore, when the Si content in the steel for carburizing is reduced, the formation of the grain boundary oxide layer can be suppressed. On the other hand, according to the findings obtained by the inventors through experiments, although the reason is not clear, the formation of the grain boundary oxide layer during carburization can be suppressed by increasing the Cr / Mn ratio. In other words, when the value of the left side of formula (1) increases due to an increase in Cr / Mn and / or a decrease in Si, the formation of the grain boundary oxide layer during carburization can be suppressed. If the contents of Si, Mn, and Cr are set so that the value is 2.0 or more as shown in formula (1), the depth of the grain boundary oxide layer formed when gas carburizing is performed under general conditions can be suppressed to a shallow depth of less than 7.0 μm.

[0047] The grain boundary oxide layer forms an uneven structure on the surface of the steel material, and may become the starting point of fracture, thereby reducing the bending fatigue strength of the steel material. Therefore, by suppressing the formation of the grain boundary oxide layer, the bending fatigue strength of the steel material can be increased. In addition, the formation of the grain boundary oxide layer also leads to the formation of the carburized abnormal layer, which also causes the mechanical properties of the steel material to deteriorate. Therefore, it is preferable to suppress the formation of the grain boundary oxide layer from the viewpoint of suppressing the formation of the carburized abnormal layer. If the above formula (1) is satisfied by sufficiently increasing Cr / Mn and / or suppressing Si to a sufficiently low value, the formation of the grain boundary oxide layer and the associated formation of the carburized abnormal layer can be effectively suppressed, and the mechanical properties of the steel material, including the bending fatigue strength, can be improved.

[0048] On the other hand, in the left side of formula (1), Cr / Mn and Si contribute in opposite directions, and if the Cr / Mn value is large enough, even if the Si content is increased to a certain extent, formula (1) is satisfied and the formation of the grain boundary oxide layer can be suppressed. Increasing the Si content increases the temper softening resistance of the steel after carburization, and accordingly, the surface fatigue strength is increased and high pitting resistance can be obtained. In other words, by satisfying formula (1) through the balance between Cr / Mn and Si, it is possible to achieve both high bending fatigue strength and high surface fatigue strength.

[0049] Cr-1.82Si≧-0.7 (2) When gas carburizing is performed, if the carbon potential determined by the carburizing gas concentration is the same, Cr has a positive contribution to the equilibrium carbon concentration, that is, the carbon concentration on the steel surface, and Si has a negative contribution. In other words, the equilibrium carbon concentration increases as the Cr content in the carburizing steel increases and as the Si content decreases. When the equilibrium carbon concentration increases, the surface carbon concentration after carburizing increases. Therefore, the larger the value of the left side of formula (2), the higher the surface carbon concentration after carburizing. In other words, when the value of the left side of formula (2) increases, carburizing can be effectively promoted. If the Si and Cr contents are set so that the value is -0.7 or more as shown in formula (2), when gas carburizing is performed under general conditions, for example, at 930 to 950°C, carburizing is performed with a carburizing gas concentration that makes the surface carbon concentration of pure iron 0.80%, and then oil quenching is performed at 900°C and tempering is performed at 180°C, the surface carbon concentration can be increased to 0.74% or more.

[0050] In steel after carburization, increasing the surface carbon concentration can improve the surface hardness. Improving the surface hardness increases the bending fatigue strength of the steel. Satisfying formula (2) has an excellent effect on improving bending fatigue strength, in addition to the effect of suppressing the formation of grain boundary oxide layers by satisfying formula (1). Furthermore, satisfying formula (2) allows the carbon potential for achieving the desired equilibrium carbon concentration to be set low, so the amount of carburizing gas used can be reduced. This makes it possible to keep the cost required for carburization low.

[0051] [Steel characteristics] The carburizing steel according to this embodiment contains each of the component elements in the above-mentioned predetermined amounts and further satisfies formula (1) and formula (2), thereby making it possible to simultaneously achieve an improvement in bending fatigue strength due to the effect of suppressing the formation of grain boundary oxide layers and improving surface hardness, and an improvement in surface fatigue strength due to an improvement in temper softening resistance. Mo is an element that is highly effective in improving surface fatigue strength by improving temper softening resistance, and in the carburizing steel according to this embodiment, by particularly satisfying formula (1), it is possible to obtain high surface fatigue strength while keeping the Mo content to a small amount of 0.40% or less. In other words, it is possible to obtain a carburizing steel that is inexpensive yet achieves both bending fatigue strength and surface fatigue strength. In addition to reducing the material cost by reducing the Mo content, the cost required for carburizing can also be reduced by reducing the amount of carburizing gas used due to the effect of further satisfying formula (2).

[0052] The carburizing steel according to this embodiment preferably has the following surface condition and physical properties when gas carburized under typical conditions, for example, at 930 to 950°C with a carburizing gas concentration such that the surface carbon concentration of pure iron is 0.80%, and then oil quenched at 900°C and tempered at 180°C. Depth of grain boundary oxide layer: less than 7.0μm. Surface carbon concentration: 0.74% or more. -Surface hardness: 735HV or higher. Bending fatigue strength: a value evaluated by a bending fatigue strength test shown in the examples below, of 9.0 kN or more, and more preferably 9.5 kN or more. Surface fatigue strength: The roller pitting life evaluated by the surface fatigue test shown in the examples below is 11.5 x 10 6 More preferably, 14.1×10 6 More than once.

[0053] The use of the carburizing steel according to this embodiment is not particularly limited. However, since it has high bending fatigue strength and surface fatigue strength as described above, it can be suitably applied to members to which a large mechanical load is applied. In particular, it can be suitably used to form members that undergo (pseudo) tempering during operation due to heat generation caused by friction or the like. Examples of such members include gears and pulleys. In particular, the carburizing steel according to this embodiment can be suitably used to form transmission gears and CVT pulleys in automobiles.

[0054] [Manufacturing method of carburizing steel and carburizing method] To manufacture the carburizing steel according to the present embodiment, first, an alloy having a predetermined composition is melted and an ingot is manufactured. The melting may be performed by a method such as a vacuum induction melting method (VIF), an arc melting method (AF), or a blast furnace-converter method. A bloom may be manufactured by continuous casting. After that, the steel material may be forged and rolled. For example, the cast piece may be heated to a temperature equal to or higher than the A3 transformation point, and then forged and rolled. Furthermore, it is preferable to appropriately perform a softening heat treatment on the obtained forged and rolled piece in order to increase the ease of machining. Specific examples of the softening heat treatment include annealing, in which the forged and rolled piece is heated to the A3 transformation point or higher and then furnace-cooled, normalizing, in which the forged and rolled piece is heated to the A3 transformation point or higher and then air-cooled, and spheroidizing annealing, in which the piece is heated between the A1 transformation point and the A3 transformation point and then furnace-cooled, depending on the required degree of softening. The obtained steel material may then be subjected to cutting, hot or cold forging, or other processes as appropriate, and processed into a desired product shape, such as a gear.

[0055] The carburizing steel processed into the product shape as described above may be carburized. The carburizing is preferably carried out by gas carburizing. As conditions for the gas carburizing, for example, a form in which carburizing is carried out at a temperature of 900 to 980°C and with a carburizing gas concentration that results in a surface carbon concentration of 0.65 to 0.85% for pure iron can be suitably applied. In addition, after carburizing, it is preferable to carry out oil quenching at 830 to 980°C and further tempering at 150 to 200°C. EXAMPLES

[0056] The present invention will now be described more specifically with reference to examples.

[0057] [Sample preparation] As samples, carburizing steels according to Examples 1 to 21, Comparative Examples 1 to 10, and Reference Example 1 were prepared. Alloys containing the metal elements in the ratios shown in Table 1 were melted by VIF and cast into ingots weighing 150 kg. The concentrations of C and S in the obtained ingots were investigated by combustion and infrared absorption spectroscopy, and the concentrations of other component elements were investigated by optical emission spectroscopy, confirming that they had the composition (unit: mass%) shown in Table 1.

[0058] The ingots obtained above were heated to 1250°C and forged. At this time, the specimens for the bending fatigue test described below were forged into round bars with a diameter of 22 mm, and the specimens for the surface fatigue test were forged into round bars with a diameter of 32 mm. Furthermore, the obtained forged pieces were subjected to softening heat treatment. That is, the specimens were heated to 950°C and then cooled in a furnace to be softened. The carburizing steel obtained in this manner was machined into the shapes of the test specimens to be used in each test.

[0059] After that, the bending fatigue test specimen and the surface fatigue test specimen were subjected to gas carburizing. For the bending fatigue test specimen, the test piece with the shape shown in FIG. 1(b) was carburized under the conditions shown in FIG. 1(a). That is, the carburizing gas (gas type: acetylene) concentration was controlled to a concentration where the surface carbon concentration of pure iron was 0.80% at 930°C, and carburizing was performed for 130 minutes. Then, the specimen was oil quenched at 900°C, and tempered in oil at 180°C for 2 hours to prevent cracking. For the surface fatigue test specimen, the hollow cylindrical test piece (indicated by symbol A) shown in FIG. 2(b) was used as a test roller, and carburized under the conditions shown in FIG. 2(a). That is, the carburizing was performed for 420 minutes at 950°C, and the surface carbon concentration of pure iron was controlled to a concentration where 0.80% was. Then, the specimen was oil quenched at 900°C, and tempered in oil at 180°C for 2 hours to prevent cracking.

[0060] [Evaluation method] (depth of grain boundary oxide layer) The specimen for bending fatigue test was cut, the cross section was polished, and the cross section was observed by an optical microscope. The depth of the grain boundary oxide layer was estimated from the observed image. FIG. 3 shows an observed image of the cross section of the sample of Comparative Example 7 as an example of a microscope image. The dark needle-like region corresponds to the grain boundary oxide layer, and the depth (length) of the grain boundary oxide layer was estimated from the observed image as shown by the range indicated by the dashed line in the image. In FIG. 3, the depth of the grain boundary oxide layer is 7.0 μm. In the observed image, the outermost layer covering the surface of the region where the grain boundary oxide layer exists is a Ni plating layer formed for preparing the cross section sample.

[0061] (surface carbon concentration) A test piece for the bending fatigue test was cut, and the cross section was polished, and then the carbon concentration in the surface portion was evaluated by a wavelength dispersive X-ray analyzer (EPMA1600 manufactured by JEOL).

[0062] (Surface hardness) The test piece for the bending fatigue test was cut and the cross section was polished, after which the surface hardness was measured at a position 0.05 mm from the surface of the test piece for the bending fatigue test using a Vickers hardness tester with a test force of 300 gf.

[0063] (Bending fatigue strength) The bending fatigue strength was evaluated by four-point bending. That is, as shown in Fig. 1(b), a round bar-shaped bending fatigue test specimen (total diameter: 19 mm, diameter of the neck: 13 mm, curvature of the neck: 1.5 mm) with a neck in the center and flat notches at the top and bottom was supported from below by a cylindrical jig at two points 80 mm apart symmetrically across the neck. In addition, a jig of the same shape was abutted from above at two points 10 mm apart symmetrically across the neck. Then, as shown by the arrows in the figure, a downward load was applied to the upper jig, and fatigue tests were repeated until at least two of the three test specimens had a fatigue strength of 2×10 6The load at which the specimen did not break after repeated fatigue tests was recorded and used as the result of the bending fatigue test. The higher the load value obtained, the higher the bending fatigue strength is indicated, and a load value of 9.0 kN or more can be considered to have a sufficiently high bending fatigue strength.

[0064] (surface fatigue strength) A surface fatigue test was carried out to measure the roller pitting life and evaluate the surface fatigue strength. That is, as shown in Fig. 2(b), a hollow cylindrical test piece for surface fatigue test (test roller; A in the figure) with a diameter of 26 mm was placed in contact with a road roller (B in the figure) made of SUJ2 tempered material (hardness 58-60HRC), with a diameter of 130 mm, and a crowning radius of 150 mm. Then, assuming use in the gears of an automobile transmission, automatic transmission fluid with a viscosity equivalent to engine oil SAE 0W-8 was poured at a flow rate of 2 L / min at 80°C while the test roller was rotated at a speed of 2000 rpm and the road roller at 560 rpm in the opposite directions (arrows in the figure). The rollers were rotated with a load of 16.9 kN applied to the contact area between the two rollers, and the life (number of rotations) was measured until the surface of the test roller peeled off and vibration occurred during rotation. The longer the measured life, the higher the surface fatigue strength of the steel material. 6 If the number of cycles is more than 1, the contact fatigue strength can be considered to be sufficiently high.

[0065] [Test Results] Table 1 shows the content of each component for Examples 1 to 21, Comparative Examples 1 to 10, and Reference Example 1. Table 2 shows the results of each evaluation together with the calculated values ​​of Cr / Mn-0.6Si and Cr-1.82Si. Furthermore, FIG. 4 illustrates the relationship between the component composition and various properties for each Example and Comparative Example.

[0066] [Table 1] [Table 2]

[0067] First, the correlation between Cr / Mn-0.6Si and the properties of steel materials is examined. Figure 4(a) shows the relationship between Cr / Mn-0.6Si and the depth of the grain boundary oxide layer, and Figure 4(b) shows the relationship between Cr / Mn-0.6Si and the results of the bending fatigue test (however, as described later, Comparative Example 3 in which the grain boundary oxide layer is thin due to the high content of Si alone is excluded). Figure 4(a) shows a negative correlation between Cr / Mn-0.6Si and the depth of the grain boundary oxide layer, and Figure 4(b) shows a positive correlation between Cr / Mn-0.6Si and the bending fatigue strength. These results show that as Cr / Mn-0.6Si increases, the formation of the grain boundary oxide layer is suppressed, and the bending fatigue strength increases accordingly. Looking at Tables 1 and 2 together, it can be seen that even if the individual contents of Si, Mn, and Cr are different, as long as the Cr / Mn-0.6Si is approximately the same, the depth of the grain boundary oxide layer and the bending fatigue strength are approximately the same, for example, in Examples 2, 6, and 7. In other words, Cr / Mn-0.6Si is a good indicator for increasing bending fatigue strength by suppressing the formation of the grain boundary oxide layer.

[0068] In Examples 1 to 21, which are in the region where Cr / Mn-0.6Si≧2.0, as shown by the dotted line and arrow in Fig. 4(a) and (b), the depth of the grain boundary oxide layer is suppressed to less than 7.0 μm, and the load obtained in the bending fatigue test is 9.0 kN or more. In all of these Examples, the Mo content is suppressed to 0.40% or less, but a high bending fatigue strength is obtained that is similar to that of Reference Example 1 containing 0.49% Mo (9.5 kN; shown by the solid line in Fig. 4(b)). On the other hand, in Comparative Examples 1 and 6, due to the balance of the contents of Si, Mn, and Cr, in Comparative Example 4, the Cr content is mainly too low, and in Comparative Examples 5, 8 to 10, the Mn content is mainly too high, so that Cr / Mn-0.6Si<2.0. In each of these Comparative Examples, the depth of the grain boundary oxide layer is 7.0 μm or more, and the result of the bending fatigue test is less than 9.0 kN, and sufficient bending fatigue strength is not obtained.

[0069] Here, the relationship between the Si content and mechanical strength will be examined. In Comparative Example 7, the Si content is low, but Cr / Mn-0.6Si<2.0. Correspondingly, the depth of the grain boundary oxide layer is 7.0 μm or more, and the result of the bending fatigue test is less than 9.0 kN, so that sufficient bending fatigue strength is not obtained. In Comparative Example 3, although Cr / Mn-0.6Si≧2.0, the Si content is too high, so that the depth of the grain boundary oxide layer is 7.0 μm or more, and the result of the bending fatigue test is less than 9.0 kN.

[0070] Furthermore, Fig. 4(c) shows the relationship between the Si content and the contact fatigue strength. According to this, there is a tendency for the contact fatigue strength to improve with an increase in the Si content. As shown by the dotted line and arrow in the figure, by increasing the Si content to 0.50% or more, the roller pitting life is increased by 11.5×10 6 In Comparative Examples 2 and 7, in which the Si content was less than 0.50%, the roller pitting life was 11.5×10 6 From the results so far, it can be said that by increasing the Si content within the range satisfying Cr / Mn-0.6Si≧2.0, it is possible to achieve both high bending fatigue strength and high surface fatigue strength.

[0071] Next, we will examine the correlation between Cr-1.82Si and steel properties. Figure 4(d) shows the relationship between Cr-1.82Si and surface carbon concentration. This shows that there is a positive correlation between Cr-1.82Si and surface carbon concentration. Furthermore, according to Table 1, in general, when the surface carbon concentration is high, the surface hardness is high. This shows that as Cr-1.82Si increases, the surface carbon concentration increases, and therefore the surface hardness increases.

[0072] In Examples 1 to 21, which are in the region of Cr-1.82Si≧-0.7 as indicated by the dotted line and arrow in the figure, the surface carbon concentration is 0.74% or more and the surface hardness is 735HV or more. On the other hand, in Comparative Example 4, the Cr content is too low, and in Comparative Examples 8 and 9, the balance between the Cr and Si contents results in Cr-1.82Si<-0.7, and in these Comparative Examples 4, 8, and 9, the surface carbon concentration is less than 0.74% and the surface hardness is less than 735HV.

[0073] From the above test results, it can be seen that by setting the component composition of the carburizing steel so that the individual content of each component falls within the range of the present invention and the relationships Cr / Mn-0.6Si≧2.0 and Cr-1.82Si≧-0.7 are satisfied, it is possible to obtain a steel material that has both high bending fatigue strength and surface fatigue strength after carburizing, and also has high surface hardness, while keeping the Mo content low.

[0074] The present invention has been described above with reference to the embodiments and examples thereof, but the present invention is not limited to these embodiments and examples and can be modified in various ways.

Claims

1. In mass percent, 0.10%≦C≦0.30%, 0.50%≦Si≦1.20%, 0.05%≦Mn≦0.80%, 0.30%≦Cr≦2.00%, 0.01%≦Mo≦0.40%, Contains 0.02%≦Al≦0.10%; P≦0.030%, S≦0.030%, Cu≦0.3%; The balance is Fe and unavoidable impurities, A carburizing steel that satisfies the following formulas (1) and (2): Cr / Mn-0.6Si≧2.0 (1) Cr-1.82Si≧-0.7 (2) In the formulas (1) and (2), each element symbol indicates the content of each element in units of mass %.

2. Further, in mass%, 0%<Ni≦0.30%, 0%<Nb≦0.05%, 0%<Ti≦0.05%, 0%<B≦0.005% The carburizing steel according to claim 1, which contains at least one of the following:

3. 3. The carburizing steel according to claim 1, wherein the depth of the grain boundary oxide layer after gas carburizing is less than 7.0 μm.

Citation Information

Patent Citations

  • High strength gear having excellent bending strength of dedendum and pitting resistance, and production method therefor

    JP2003027142A