Imprint mold and method for manufacturing same, and method for manufacturing article
The imprint mold with a low Young's modulus pattern layer and stress relaxation layer addresses the challenges of substrate unevenness and foreign matter, ensuring precise and defect-free pattern transfer.
Patent Information
- Application Number
- JP2023054917
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing nanoimprint molds face challenges in transferring precise concavo-convex patterns due to substrate surface unevenness and foreign matter, leading to unfilled defects and pattern damage.
The development of an imprint mold with a base material and a pattern layer having a lower Young's modulus than the base material, combined with a stress relaxation layer, allows for deformation and recovery, minimizing defects and damage during the imprinting process.
The solution effectively suppresses unfilled defects and pattern damage by enabling precise transfer of concavo-convex patterns even on uneven substrates with foreign matter, extending the mold's life and ensuring high-quality pattern formation.
Smart Images

Figure 2024142676000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an imprint mold and a method for making the same, and a method for making an article. [Background technology]
[0002] Nanoimprint technology, known as a microfabrication technology, is a pattern formation technology that uses an imprint mold having a concave-convex pattern formed on the surface of a base material, and transfers the concave-convex pattern to a workpiece such as a transfer substrate at the same magnification. In particular, with the further miniaturization of wiring patterns in semiconductor devices, nanoimprint technology has been attracting attention as one means in the manufacturing process thereof.
[0003] In nanoimprint technology, an imprint mold with a transfer pattern of fine projections and recesses formed on its pattern surface is brought into contact with resin supplied to the surface of a transfer substrate such as a semiconductor wafer, filling the transfer pattern with the resin, and hardening the resin in this state to form a projection-and-recess pattern in which the projection-and-recess shape of the transfer pattern of the imprint mold is transferred to the resin. The projection-and-recess pattern formed on the transfer substrate using the imprint mold is used as it is as a part of the components of a product, or is used to process the transfer substrate, etc. For this reason, it is necessary to transfer the projection-and-recess shape of the transfer pattern of the imprint mold to the resin with high precision.
[0004] On the other hand, in order to transfer the uneven shape of the transfer pattern of the imprint mold to the resin with high accuracy, it is necessary to make the surface of the transfer substrate to which the resin is supplied parallel to the pattern surface on which the transfer pattern is formed. If the surface of the transfer substrate is not flat, even if the surface of the transfer substrate and the pattern surface are made parallel, the resin supplied to the surface of the transfer substrate may not fill the transfer pattern, causing an unfilled defect in part of the uneven pattern. In addition, if a foreign object is present on the surface of the transfer substrate, the transfer pattern may be damaged if the foreign object comes into contact with the transfer pattern.
[0005] Conventionally, a mold for nanoimprinting has been proposed which includes a mold base portion, a mold main body portion having a first surface and a second surface opposite the first surface, and an elastic body portion fixed between the first surface of the mold main body portion and the mold base portion, with a pattern formed on the second surface of the mold main body portion, and the bulk modulus of the elastic body portion being smaller than the bulk modulus of the mold main body portion (see Patent Document 1). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2012-11728 A Summary of the Invention [Problem to be solved by the invention]
[0007] In the nanoimprint mold described in Patent Document 1, even if there is a height distribution on the surface of the transfer substrate, the elastic portion deforms in accordance with the height distribution, thereby reducing the variation in the shape of the uneven pattern formed on the surface of the transfer substrate due to the height distribution.
[0008] However, since the elastic body portion in the nanoimprinting mold described in Patent Document 1 is made of a resin material such as polyethylene terephthalate (PET), polyethylene, polypropylene, etc., it cannot be said to have a sufficient elastic modulus, and there is a risk that it will be difficult to prevent unfilled defects in the uneven pattern and damage to the transfer pattern of the mold due to the flatness of the surface of the transfer substrate and foreign matter present on the surface.
[0009] Furthermore, since the elastic portion is made of a resin material such as polyethylene terephthalate (PET), polyethylene, or polypropylene, there is also the problem that even if it deforms in accordance with the height distribution of the surface of the transferred substrate, it is difficult to restore the elastic portion from the deformation.
[0010] In view of the above problems, the present disclosure aims to provide an imprint mold and a manufacturing method thereof that can suppress the occurrence of unfilled defects and damage to the unevenness pattern due to unevenness or the presence of foreign matter on the surface of a transfer substrate or other object to be imprinted, as well as a manufacturing method of an article using the imprint mold. [Means for solving the problem]
[0011] In order to achieve this objective, one embodiment of the present disclosure provides an imprint mold comprising: a substrate having a first surface and a second surface located opposite the first surface; and a pattern layer provided on the first surface side of the substrate and having a concave-convex pattern including concave portions and convex portions, wherein the pattern layer has a function of deforming due to stress in the thickness direction of the substrate and a function of recovering when the stress is released, wherein the Young's modulus of a constituent material of the pattern layer is smaller than that of a constituent material of the substrate, the elastic recovery rate of the constituent material of the pattern layer is greater than that of a constituent material of the substrate, and the Young's modulus of the constituent material of the substrate is 70 GPa or less.
[0012] As one embodiment of the present disclosure, there is provided an imprint mold comprising: a substrate having a first surface and a second surface located opposite to the first surface; and a pattern layer provided on the first surface side of the substrate, the pattern layer having an uneven pattern including recesses and protrusions, the pattern layer including a stress relaxation layer provided on the first surface side of the substrate, and an uneven pattern layer provided on the stress relaxation layer, the uneven pattern having the uneven pattern, wherein the Young's modulus of a constituent material of the stress relaxation layer is smaller than the Young's modulus of a constituent material of the substrate, the elastic recovery modulus of the constituent material of the stress relaxation layer is greater than the elastic recovery modulus of a constituent material of the substrate, and the Young's modulus of the constituent material of the substrate is 70 GPa or less.
[0013] As one embodiment of the present disclosure, there is provided a method for manufacturing an imprint mold, the method including the steps of: applying a pattern layer forming material for forming the pattern layer to the first surface of the substrate; preparing a master mold having a pattern corresponding to the uneven pattern, and contacting the pattern of the master mold with the pattern layer forming material to fill the pattern with the pattern layer forming material; hardening the pattern layer forming material filled in the pattern of the master mold; and separating the master mold from the hardened pattern layer forming material.
[0014] As one embodiment of the present disclosure, there is provided a method for manufacturing an imprint mold, the method including the steps of forming the stress relaxation layer on the first surface of the substrate, applying a pattern layer forming material for forming the concave-convex pattern layer on the stress relaxation layer, preparing a master mold having a pattern corresponding to the concave-convex pattern, and filling the pattern with the pattern layer forming material by contacting the pattern of the master mold with the pattern layer forming material, hardening the pattern layer forming material filled in the pattern of the master mold, and separating the master mold from the hardened pattern layer forming material.
[0015] As one embodiment of the present disclosure, there is provided a method for manufacturing an article, including the steps of: preparing a substrate having a first surface and a second surface opposite to the first surface; applying an imprint resin to the first surface of the substrate; filling the imprint resin into the concave-convex pattern by contacting an imprint mold with the imprint resin; hardening the imprint resin filled into the concave-convex pattern; and separating the imprint mold from the hardened imprint resin. Effect of the Invention
[0016] According to the present disclosure, it is possible to provide an imprint mold and a manufacturing method thereof that can suppress the occurrence of unfilled defects and damage to the unevenness pattern due to unevenness or the presence of foreign matter on the surface of a transfer substrate or other object to be imprinted, as well as a manufacturing method for an article using the imprint mold. [Brief description of the drawings]
[0017] [Figure 1A] FIG. 1A is a schematic cut-away end view of an imprint mold according to one embodiment of the present disclosure. [Figure 1B] FIG. 1B is a schematic cut-away end view of an imprint mold according to one embodiment of the present disclosure. [Figure 1C] FIG. 1C is a schematic cut-away end view of an imprint mold according to one embodiment of the present disclosure. [Figure 1D] FIG. 1D is a schematic cut-away end view of an imprint mold according to one embodiment of the present disclosure. [Figure 1E] FIG. 1E is a schematic cut-away end view of an imprint mold according to one embodiment of the present disclosure. [Diagram 2] FIG. 2 is a partially enlarged cutaway end view that illustrates a schematic projection and recess pattern of an imprint mold according to an embodiment of the present disclosure. [Figure 3A] FIG. 3A is a cut-away end view that illustrates a schematic diagram of a step in a method for making a master mold used to produce an imprint mold according to an embodiment of the present disclosure. [Figure 3B] FIG. 3B is a cutaway end view that illustrates a schematic diagram of a step in a method for making a master mold used to produce an imprint mold according to an embodiment of the present disclosure, the step continuing from FIG. 3A. [Figure 3C] FIG. 3C is a cutaway end view that illustrates a schematic diagram of a step in a method for making a master mold used to produce an imprint mold according to an embodiment of the present disclosure, the step continuing from FIG. 3B. [Figure 3D]FIG. 3D is a cutaway end view that illustrates a schematic diagram of a step in a method for making a master mold used to produce an imprint mold according to an embodiment of the present disclosure, the step following FIG. 3C. [Figure 4A] FIG. 4A is a cut-away end view that illustrates a schematic diagram of a step in a method for manufacturing the imprint mold shown in FIG. 1A. [Figure 4B] FIG. 4B is a cutaway end view that diagrammatically illustrates a step in the method for manufacturing the imprint mold shown in FIG. 1A, the step following FIG. 4A. [Figure 4C] FIG. 4C is a cutaway end view that illustrates a schematic diagram of a step in the method for manufacturing the imprint mold shown in FIG. 1A, the step following that shown in FIG. 4B. [Figure 4D] FIG. 4D is a cross-sectional end view that illustrates a schematic diagram of a step in the method for manufacturing the imprint mold shown in FIG. 1A, the step following that shown in FIG. 4C. [Figure 4E] FIG. 4E is a cutaway end view that diagrammatically illustrates a step in the method for manufacturing the imprint mold shown in FIG. 1A, the step following that shown in FIG. 4D. [Figure 5A] FIG. 5A is a cutaway end view that illustrates a schematic diagram of a step in a method for manufacturing the imprint mold shown in FIG. 1B. [Figure 5B] FIG. 5B is a cutaway end view that illustrates a schematic diagram of a step in the method for manufacturing the imprint mold shown in FIG. 1B, the step following FIG. 5A. [Figure 5C] FIG. 5C is a cutaway end view that diagrammatically illustrates a step in the method for manufacturing the imprint mold shown in FIG. 1B, the step following FIG. 5B. [Figure 5D] FIG. 5D is a cross-sectional end view that illustrates a step in the method for manufacturing the imprint mold shown in FIG. 1B, the step following FIG. 5C. [Figure 5E] FIG. 5E is a cutaway end view that diagrammatically illustrates a step in the method for manufacturing the imprint mold shown in FIG. 1B, the step following FIG. 5D. [Figure 6A] FIG. 6A is a cutaway end view that illustrates a schematic diagram of a step in a method for manufacturing the imprint mold shown in FIG. 1C. [Figure 6B] FIG. 6B is a cross-sectional end view that illustrates a step in the method for manufacturing the imprint mold shown in FIG. 1C, the step following FIG. 6A. [Figure 6C] FIG. 6C is a cutaway end view that diagrammatically illustrates a step in the method for manufacturing the imprint mold shown in FIG. 1C, the step following FIG. 6B. [Figure 6D] FIG. 6D is a cutaway end view that diagrammatically illustrates a step in the method for manufacturing the imprint mold shown in FIG. 1C, the step following that shown in FIG. 6C. [Figure 6E] FIG. 6E is a cutaway end view that diagrammatically illustrates a step in the method for manufacturing the imprint mold shown in FIG. 1C, the step following that shown in FIG. 6D. [Figure 7A] FIG. 7A is a cutaway end view that illustrates a schematic diagram of a step in a method for manufacturing the imprint mold shown in FIG. 1D. [Figure 7B] FIG. 7B is a cross-sectional end view that illustrates a schematic diagram of a step in the method for manufacturing the imprint mold shown in FIG. 1D, the step following FIG. 7A. [Figure 7C] FIG. 7C is a cutaway end view that diagrammatically illustrates a step in the method for manufacturing the imprint mold shown in FIG. 1D, the step following that shown in FIG. 7B. [Figure 7D] FIG. 7D is a cross-sectional end view that illustrates a schematic diagram of a step in the method for manufacturing the imprint mold shown in FIG. 1D, the step following that shown in FIG. 7C. [Figure 7E] FIG. 7E is a cutaway end view that diagrammatically illustrates a step in the method for manufacturing the imprint mold shown in FIG. 1D, the step following that shown in FIG. 7D. [Figure 8A] FIG. 8A is a cut-away end view that illustrates a schematic diagram of a step of an imprinting method using an imprint mold according to an embodiment of the present disclosure. [Figure 8B] FIG. 8B is a cut-away end view that illustrates a schematic diagram of a step following FIG. 8A in a method of imprinting using an imprint mold according to an embodiment of the present disclosure. [Figure 8C]FIG. 8C is a cut-away end view that illustrates a schematic diagram of a step following FIG. 8B in an imprinting method using an imprint mold according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] An embodiment of the present disclosure will be described with reference to the drawings. In the drawings, the shape, scale, aspect ratio, etc. of each part may be shown modified or exaggerated from the actual product to facilitate understanding. In this specification, etc., a numerical range expressed using "~" means that the range includes the numerical values written before and after "~" as the lower and upper limits, respectively. In this specification, etc., terms such as "film," "sheet," and "plate" are not distinguished from each other based on differences in names. For example, "plate" is a concept that includes members that can be generally called "sheet" and "film."
[0019] A first aspect of this embodiment is an imprint mold comprising a substrate having a first surface and a second surface located opposite to the first surface, and a pattern layer provided on the first surface side of the substrate and having an uneven pattern including concave and convex portions, the pattern layer having a function of deforming due to stress in the thickness direction of the substrate and a function of recovering when the stress is released, the Young's modulus of a constituent material of the pattern layer is smaller than that of a constituent material of the substrate, the elastic recovery rate of the constituent material of the pattern layer is greater than that of the constituent material of the substrate, and the Young's modulus of the constituent material of the substrate is 70 GPa or less.
[0020] A second aspect of this embodiment is an imprint mold comprising a substrate having a first surface and a second surface located opposite to the first surface, and a pattern layer provided on the first surface side of the substrate, the pattern layer having an uneven pattern including concave and convex portions, the pattern layer including a stress relaxation layer provided on the first surface side of the substrate, and an uneven pattern layer provided on the stress relaxation layer, the uneven pattern having the concave and convex pattern, wherein the Young's modulus of a constituent material of the stress relaxation layer is smaller than the Young's modulus of a constituent material of the substrate, the elastic recovery modulus of the constituent material of the stress relaxation layer is greater than the elastic recovery modulus of a constituent material of the substrate, and the Young's modulus of the constituent material of the substrate is 70 GPa or less.
[0021] A third aspect of this embodiment is the imprint mold of the first aspect, wherein the Young's modulus of the outermost surface of the concave-convex pattern is greater than the Young's modulus of a constituent material of the pattern layer.
[0022] A fourth aspect of the present embodiment is an imprint mold according to any one of the first to third aspects, further comprising a protective layer covering the surface of the concave-convex pattern, the Young's modulus of the material constituting the protective layer being greater than the Young's modulus of the material constituting the pattern layer.
[0023] A fifth aspect of this embodiment is the above-mentioned fourth aspect, wherein the protective layer is an imprint mold containing SiO2. A sixth aspect of the present embodiment is the imprint mold according to the fourth or fifth aspect, wherein the protective layer has a thickness of 1 nm to 100 nm.
[0024] A seventh aspect of this embodiment is an imprint mold according to any one of the first to sixth aspects, wherein, when viewed in a cross section along the thickness direction of the substrate, the angle of the side wall portion of the convex portion relative to the bottom surface of the concave portion of the concave-convex pattern is less than 90°.
[0025] An eighth aspect of the present embodiment is the imprint mold of the first aspect, further comprising a planarization layer provided between the first surface of the substrate and the pattern layer. A ninth aspect of the present embodiment is the imprint mold of the second aspect, further comprising a planarizing layer provided between the stress relaxation layer and the concave-convex pattern layer.
[0026] A tenth aspect of the present embodiment is the above-mentioned first aspect, wherein the material constituting the pattern layer is a curable resin containing a polymerizable compound having an organic component and an inorganic component in the molecule, and the inorganic component is SiO X (X is 1 or more).
[0027] An eleventh aspect of the present embodiment is the above-mentioned second aspect, wherein the material constituting the stress relaxation layer is a curable resin containing a polymerizable compound having an organic component and an inorganic component in the molecule, and the inorganic component is SiO X (X is 1 or more).
[0028] A twelfth aspect of the present embodiment is an imprint mold according to the tenth or eleventh aspect, wherein the polymerizable compound has a siloxane bond as the inorganic component, and among the oxygen atoms bonded to silicon atoms contained in the polymerizable compound, a ratio of oxygen atoms bonded to a single silicon atom is 10 mol % or less.
[0029] A thirteenth aspect of this embodiment is any one of the tenth to twelfth aspects, wherein the polymerizable compound is an imprint mold having a spherical structure.
[0030] A fourteenth aspect of the present embodiment is the imprint mold according to any one of the first to thirteenth aspects, wherein the recesses and / or protrusions of the concave-convex pattern have dimensions of 8 nm to 1000 nm.
[0031] A fifteenth aspect of the present embodiment is a method for producing the imprint mold of the first aspect above, comprising the steps of: applying a pattern layer forming material for forming the pattern layer to the first surface of the substrate; preparing a master mold having a pattern corresponding to the uneven pattern, and contacting the pattern of the master mold with the pattern layer forming material to fill the pattern with the pattern layer forming material; hardening the pattern layer forming material filled in the pattern of the master mold; and separating the master mold from the hardened pattern layer forming material.
[0032] A sixteenth aspect of the present embodiment is a method for producing the imprint mold of the second aspect above, comprising the steps of forming the stress relaxation layer on the first surface of the substrate, applying a pattern layer forming material for forming the concave-convex pattern layer on the stress relaxation layer, preparing a master mold having a pattern corresponding to the concave-convex pattern, and contacting the pattern of the master mold with the pattern layer forming material to fill the pattern with the pattern layer forming material, hardening the pattern layer forming material filled in the pattern of the master mold, and separating the master mold from the hardened pattern layer forming material.
[0033] A seventeenth aspect of the present embodiment is a method for producing an imprint mold according to the fifteenth or sixteenth aspect, comprising a step of forming a protective layer on a surface of the concave-convex pattern formed by peeling off the master mold.
[0034] An 18th aspect of the present embodiment is a method for manufacturing an article, including the steps of preparing a substrate having a first surface and a second surface opposite to the first surface, applying an imprint resin to the first surface of the substrate, contacting the imprint resin with an imprint mold of any of the above-mentioned 1st to 14th aspects to fill the imprint resin into the concave-convex pattern, curing the imprint resin filled into the concave-convex pattern, and detaching the imprint mold from the cured imprint resin.
[0035] [Imprint mold] The imprint mold 1 according to this embodiment includes a substrate 2 having a first surface 2A and a second surface 2B located on the opposite side to the first surface 2A, and a pattern layer 3 provided on the first surface 2A side of the substrate 2 (see FIGS. 1A to 1D). The imprint mold 1 according to this embodiment may also include a convex structure 8 protruding from the first surface 2A of the substrate 2, and a recessed portion 9 formed on the second surface 2B side (see FIG. 1E). In the imprint mold 1 shown in FIG. 1E, the pattern layer 3 may be formed on the upper surface of the convex structure 8.
[0036] The substrate 2 is a typical substrate for imprint molds, and may be, for example, a glass substrate such as a quartz glass substrate, a soda glass substrate, a fluorite substrate, a calcium fluoride substrate, a magnesium fluoride substrate, an alkali-free glass substrate such as barium borosilicate glass, amino borosilicate glass, or aluminosilicate glass, a resin substrate such as a polycarbonate substrate, a polypropylene substrate, a polyethylene substrate, a polymethyl methacrylate substrate, or a polyethylene terephthalate substrate, or a laminate substrate formed by laminating two or more substrates arbitrarily selected from the above. In this embodiment, "transparent" means that the substrate can transmit light having a wavelength capable of curing the imprint resin, and has a transmittance of 60% or more for light having a wavelength of 150 nm to 400 nm, preferably 90% or more, and particularly preferably 95% or more.
[0037] The planar shape of the substrate 2 is not particularly limited, and may be, for example, a substantially rectangular shape. When the substrate 2 is made of a quartz glass substrate that is generally used for photoimprinting, the substrate 2 usually has a substantially rectangular shape in plan view. When the imprint mold 1 is used for imprint processing by a roll-to-roll method, the substrate 2 may have a substantially cylindrical shape or the like, and the imprint mold 1 may include the substantially cylindrical substrate 2 and the pattern layer 3 provided on the surface of the substrate 2.
[0038] The size of the base material 2 (size in plan view) is not particularly limited, but when the base material 2 is made of the above-mentioned quartz glass substrate, the size of the base material 2 is, for example, about 152 mm × 152 mm. The thickness of the base material 2 can be appropriately set, for example, in the range of about 300 μm to 10 mm, taking into consideration strength, handling suitability, and the like.
[0039] The pattern layer 3 provided on the first surface 2A side of the substrate 2 has a function of deforming due to stress in the thickness direction of the substrate 2 and a function of restoring when the stress is released. Specifically, the pattern layer 3 may be a single-layer structure made of a material having the above function (see Figs. 1A and 1C), or may be a two-layer structure made of a material having the above function, a stress relaxation layer 31, and a concave-convex pattern layer 32 (see Figs. 1B and 1D). The stress in the thickness direction of the substrate 2 means that the stress on the pattern layer 3 has a vector component in the thickness direction of the substrate 2. For example, even if the stress on the pattern layer 3 is inclined with respect to the thickness direction of the substrate 2, the stress can be said to be a stress in the thickness direction of the substrate 2.
[0040] The pattern layer 3 (the pattern layer 3 shown in FIG. 1A and FIG. 1C, and the concave-convex pattern layer 32 shown in FIG. 1B and FIG. 1D) has a concave-convex pattern 4 including recesses 41 and protrusions 42. The shape, dimensions, etc. of the concave-convex pattern 4 can be appropriately set according to the shape, dimensions, etc. required for the product manufactured using the imprint mold 1 according to this embodiment. For example, the shape of the concave-convex pattern 4 can be a line-and-space shape, a pillar shape, a hole shape, a lattice shape, a staircase shape, etc. In addition, the dimensions of the concave-convex pattern 4 can be set to, for example, about 8 nm to 1000 nm. The dimensions of the concave-convex pattern 4 are defined by the shape of the concave-convex pattern 4. For example, the dimension of the uneven pattern 4 is, in the case of a line-and-space shape, the short-side (width) length of the space-shaped recess 41 or the line-shaped protrusion 42; in the case of a pillar shape, the diameter or diagonal length of the pillar-shaped protrusion 42; in the case of a hole shape, the diameter or diagonal length of the hole-shaped recess 41; in the case of a lattice shape, the short-side (width) length of the lattice-shaped protrusion 42; and in the case of a staircase shape, the short-side length of the step surface of each step of the staircase-shaped recess 41 or protrusion 42.
[0041] When viewed in a cross section along the thickness direction of the substrate 2, the angle θ of the sidewall portion 44 of the convex portion 42 with respect to the bottom surface 43 of the recess 41 of the concave-convex pattern 4 (the rising angle of the convex portion 42) is preferably less than 90°, and particularly preferably 89° or less. That is, the cross-sectional shape of the convex portion 42 is preferably tapered. When the angle θ of the sidewall portion 44 is less than 90° and the cross-sectional shape of the convex portion 42 is tapered, the mechanical strength of the convex portion 42 of the concave-convex pattern 4 can be improved, and therefore, damage to the concave-convex pattern 4 due to foreign matter present on the transfer substrate during the imprint process using the imprint mold 1 can be suppressed.
[0042] The elastic modulus (Young's modulus) of the material constituting the pattern layer 3 shown in FIG. 1A and FIG. 1C and the stress relaxation layer 31 shown in FIG. 1B and FIG. 1D is smaller than the elastic modulus (Young's modulus) of the material constituting the substrate 2. If the elastic modulus (Young's modulus) of the material constituting the pattern layer 3 and the stress relaxation layer 31 is equal to or greater than the elastic modulus (Young's modulus) of the material constituting the substrate 2, when stress is applied to the pattern layer 3 or the concave-convex pattern layer 32 due to foreign matter or the like present on the substrate during imprint processing using the imprint mold 1, the pattern layer 3 and the stress relaxation layer 31 are less likely to deform, so that the imprint resin on the substrate may not be sufficiently filled into the concave-convex pattern 4, or the concave-convex pattern 4 may be damaged. However, since the elastic modulus (Young's modulus) of the material constituting the pattern layer 3 and the stress relaxation layer 31 is smaller than the elastic modulus (Young's modulus) of the material constituting the substrate 2, it is possible to suppress the occurrence of defects due to non-filling of the imprint resin, damage to the concave-convex pattern 4, etc.
[0043] The difference between the elastic modulus (Young's modulus) of the constituent material of the pattern layer 3 (see FIGS. 1A and 1C) and the stress relaxation layer 31 (see FIGS. 1B and 1D) and the elastic modulus (Young's modulus) of the constituent material of the substrate 2 is not particularly limited as long as it is possible to suppress the occurrence of defects due to non-filling of the imprint resin and damage to the uneven pattern 4. The elastic modulus (Young's modulus) of the constituent material of the substrate 2 may be 70 GPa or less. Note that the elastic modulus (Young's modulus) in this embodiment can be determined by a nanoindentation method using a microhardness tester (e.g., PICODENTOR HM500 (product name), manufactured by Fisher Instruments) under conditions of a measurement environment temperature of 25° C. and a measurement environment humidity of 50%.
[0044] The elastic recovery rate of the constituent materials of the pattern layer 3 (see FIGS. 1A and 1C) and the stress relaxation layer 31 (see FIGS. 1B and 1D) is greater than that of the constituent material of the substrate 2. Since the elastic recovery rate of the constituent materials of the pattern layer 3 and the stress relaxation layer 31 is greater than that of the substrate 2, the pattern layer 3 and the stress relaxation layer 31 are restored (do not undergo plastic deformation) when the stress is released after they are deformed by the stress in the thickness direction of the substrate 2, and therefore the parallelism of the concave-convex pattern 4 can be maintained.
[0045] The elastic recovery rate of the constituent materials of the pattern layer 3 (see Figs. 1A and 1C) and the stress relaxation layer 31 (see Figs. 1B and 1D) is not particularly limited as long as they can be restored when the stress on the pattern layer 3 and the stress relaxation layer 31 is released, but may be, for example, 80% or more, preferably 90% or more, and particularly preferably 95% or more. The elastic recovery rate in this embodiment is determined from the indentation depth and indentation force (load) of an indenter against a material formed on a silicon wafer by a microhardness test measurement using a microhardness tester (for example, PICODENTOR HM500 (product name), manufactured by Fisher Instruments). When the load is removed from the maximum indentation depth position, the elastic recovery rate is 100% when the initial depth is completely returned. The elastic recovery rate can be determined under the conditions of a measurement environment temperature of 25°C and a measurement environment humidity of 50%, with the measurement load conditions being a maximum load of 0.05 mN, a hold time of 3 seconds, and a film thickness of 1 μm.
[0046] The constituent materials of the pattern layer 3 (see Figures 1A and 1C) and the stress relaxation layer 31 (see Figures 1B and 1D) may be any material that satisfies the above elastic modulus (Young's modulus) and elastic recovery rate conditions, such as polyurethane resin, polyamide resin, or a predetermined curable resin containing Si.
[0047] The Si-containing curable resin, which is one of the materials constituting the pattern layer 3 shown in Figures 1A and 1C and the stress relaxation layer 31 shown in Figures 1B and 1D, may be any polymerizable compound having an organic component and an inorganic component (an inorganic component containing a siloxane polymerized portion as a main component) in the molecule. The inorganic component is SiO X (X is 1 or more), and the polymerizable compound may be any compound having a siloxane bond as an inorganic component and having at least one polymerizable functional group.
[0048] The polymerizable compound contained in the curable resin may have a ratio of oxygen atoms bonded to a single silicon atom of 10 mol% or less among oxygen atoms bonded to silicon atoms contained in the polymerizable compound. As the polymerizable compound, a polymer or oligomer having a tetrafunctional silane, a trifunctional silane, a bifunctional silane, or a monofunctional silane as a constituent unit may be used alone or in combination.
[0049] In this embodiment, it is preferable to use a curable resin having mainly trifunctional silanes and difunctional silanes as structural units, depending on the properties desired for the curable resin.
[0050] In the above polymerizable compound, the proportion of oxygen atoms bonded to a single silicon atom among the oxygen atoms bonded to silicon atoms contained in the polymerizable compound is 10 mol % or less, preferably 7 mol % or less, and particularly preferably 5 mol % or less.
[0051] An oxygen atom bonded to a single silicon atom means an oxygen atom in which one of the two bonds of the oxygen atom is bonded to silicon, and does not mean an oxygen atom in which both of the two bonds of the oxygen atom are bonded to silicon atoms. The other bond of the oxygen atom is not particularly limited as long as it is bonded to something other than silicon, but is preferably bonded to hydrogen or an alkyl group having 1 to 4 carbon atoms.
[0052] In the present embodiment, the ratio of oxygen atoms bonded to a single silicon atom as described above, i.e., the ratio of highly reactive functional groups having high reactivity, such as hydroxyl groups (-OH) and alkoxy groups (-OR, R is an alkyl group having 1 to 4 carbon atoms) bonded to silicon atoms, is within the above range, whereby the temporal stability of the curable resin can be improved and thickening during storage can be suppressed.
[0053] The reason why the highly reactive functional group exists in a certain proportion in the polymerizable compound is presumably due to unreacted oxygen atoms remaining in the manufacturing process of the polymerizable compound. The reason why such unreacted oxygen atoms remain is considered to be that when the highly reactive functional group is an alkoxy group (-OR, R is an alkyl group having 1 to 4 carbon atoms), hydrolysis of the alkoxy group of the raw material does not proceed, and when it is a hydroxyl group (-OH), polymerization reaction does not proceed completely due to steric hindrance, etc.
[0054] In this embodiment, the ratio of oxygen atoms bonded to a single silicon atom refers to the number of oxygen atoms bonded to a single silicon atom when the number of oxygen atoms bonded to silicon atoms in the polymerizable compound is taken as 100. The method for measuring this ratio is as follows: 29 It can be calculated by analyzing the spectrum by Si-NMR.
[0055] Specifically, when a polymerizable compound containing a siloxane structure having a trifunctional silane as a constituent unit is analyzed by NMR, four peaks are observed: a component in which none of the three oxygen atoms bonded to the silicon atom are bonded to other silicon atoms, a component in which one of the three oxygen atoms bonded to the silicon atom is bonded to other silicon atoms, a component in which two of the three oxygen atoms bonded to the silicon atom are bonded to other silicon atoms, and a component in which all of the three oxygen atoms bonded to the silicon atom are bonded to other silicon atoms.
[0056] The integral of these four peaks, that is, the ratio of their areas, is called T 0 ~T 3In this case, the ratio (mol %) of oxygen atoms bonded to the single silicon atom can be calculated from the following formula (1).
[0057]
number
[0058] Furthermore, when the polymerizable compound contains a siloxane structure having a bifunctional silane as a constituent unit, three peaks are observed: a component in which none of the two oxygen atoms bonded to a silicon atom are bonded to another silicon atom, a component in which one of the two oxygen atoms bonded to a silicon atom is bonded to another silicon atom, and a component in which all of the two oxygen atoms bonded to a silicon atom are bonded to other silicon atoms.
[0059] The integral of these three peaks, that is, the ratio of their areas, is D 0 ~D 2 In this case, the ratio (mol %) of oxygen atoms bonded to the single silicon atom can be calculated from the following formula (2).
[0060]
number
[0061] Furthermore, when the polymerizable compound contains a siloxane structure having a tetrafunctional silane as a constituent unit, five peaks are observed: a component in which none of the four oxygen atoms bonded to the silicon atom are bonded to other silicon atoms, a component in which one of the four oxygen atoms bonded to the silicon atom is bonded to other silicon atoms, a component in which two of the four oxygen atoms bonded to the silicon atom are bonded to other silicon atoms, a component in which three of the four oxygen atoms bonded to the silicon atom are bonded to other silicon atoms, and a component in which all of the four oxygen atoms bonded to the silicon atom are bonded to other silicon atoms.
[0062] The integral of these five peaks, that is, the ratio of their areas, is Q 0 ~Q 4In this case, the ratio (mol %) of oxygen atoms bonded to a single silicon atom can be calculated from the following formula (3).
[0063]
number
[0064] For example, when the above-mentioned polymerizable compound having two types of constituent units, trifunctional silane and bifunctional silane, is contained in the above-mentioned curable resin, the proportion (mol%) of oxygen atoms bonded to a single silicon atom can be calculated from the following formula (4).
[0065]
number
[0066] The weight average molecular weight (Mw) of the polymerizable compound may be within the range of 500 to 100,000, preferably within the range of 600 to 50,000, and particularly preferably within the range of 700 to 20,000.
[0067] The weight average molecular weight (Mw) is a polystyrene-equivalent molecular weight measured by gel permeation chromatography (GPC), and is a value measured under the following conditions after pressure filtration through a membrane filter having a pore size of 0.2 μm.
[0068] (conditions) Equipment: Water 2695 Sample amount: Approximately 10 mg of sample per 3 mL of solvent ·Injection volume: 5μL Guard column: LF-G (Shodex) Column: GPC LF-804 x 3 (Shodex) Column temperature: 40℃ Mobile phase: Tetrahydrofuran ·Flow rate: 1.0mL / min Detector: Differential refractometer (Water 2414) Molecular weight calibration: Polystyrene equivalent
[0069] The polymerizable compound has a polymerizable functional group constituting at least a part of the organic component. The polymerizable functional group is not particularly limited as long as it is a functional group capable of undergoing a polymerization reaction and the polymerization reaction proceeds due to an external stimulus, and for example, an acryloyl group, a methacryloyl group, an acryloyloxy group, a methacryloyloxy group, an epoxy group, an oxetane group, a vinyl ether group, etc., which undergo a polymerization reaction due to light irradiation, heat, heat accompanying light irradiation, the action of a photoacid generator, etc., can be used. Such a polymerizable functional group has good stability during synthesis and storage, good reactivity during curing, and is easy to obtain as a raw material.
[0070] In this embodiment, acryloyl groups and methacryloyl groups are particularly preferred because of the wide range of options available for curing speed and physical properties.
[0071] In the polymerizable compound, when the polymerizable group directly bonded to the silicon atom is bulky, the reactivity may change due to steric hindrance, and the curability may be affected. In consideration of this, the molecular weight of the polymerizable group directly bonded to the silicon atom may be within the range of 20 to 500, and preferably within the range of 25 to 400. In this embodiment, the polymerizable group refers to a group containing a polymerizable functional group. As such a polymerizable group, the following structure is preferable.
[0072] [ka]
[0073] R1 represents a "substituted or unsubstituted alkyl chain having 1 to 10 carbon atoms," and R2 represents a "substituted or unsubstituted alkyl chain having 1 to 3 carbon atoms, or a hydrogen atom." In addition, both R1 and R2 may be linear or branched.
[0074] It is sufficient that at least one of the polymerizable functional groups is bonded to the structural unit of the polymerizable compound, but this is not limiting, and two or more of the polymerizable functional groups may be bonded to the structural unit of the polymerizable compound.
[0075] Examples of the structural unit having a polymerizable group of the polymerizable compound in this embodiment include the following.
[0076] Examples of trifunctional silanes include 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, allyltrimethoxysilane, allyltriethoxysilane, styryltrimethoxysilane, styryltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, 3-ethyl-3-[3'-(trimethoxysilyl)propyl]methyloxetane, 3-ethyl-3-[3'-(triethoxysilyl)propyl]methyloxetane, and 3-ethyl-3-[3'-(triethoxysilyl)propyl]methyloxetane. Among these, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, 3-ethyl-3-[3'-(trimethoxysilyl)propyl]methyloxetane, 3-ethyl-3-[3'-(triethoxysilyl)propyl]methyloxetane, and the like can be preferably used.
[0077] Examples of bifunctional silanes include 3-acryloxypropyl(methyl)dimethoxysilane, 3-acryloxypropyl(methyl)diethoxysilane, 3-methacryloxypropyl(methyl)dimethoxysilane, 3-methacryloxypropyl(methyl)diethoxysilane, vinyl(methyl)dimethoxysilane, vinyl(methyl)diethoxysilane, allyl(methyl)dimethoxysilane, allyl(methyl)diethoxysilane, styryl(methyl)dimethoxysilane, styryl(methyl)diethoxysilane, 3-glycidoxysilane, Examples of the silane include dipropylmethyldiethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyl(methyl)dimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyl(methyl)diethoxysilane, 3-ethyl-3-[3'-(methyldimethoxysilyl)propyl]methyloxetane, 3-ethyl-3-[3'-(methyldiethoxysilyl)propyl]methyloxetane, dimethoxymethylvinylsilane, and diethoxymethylvinylsilane. Of these, 3-acryloxypropyl(methyl)dimethoxysilane, 3-acryloxypropyl(methyl)diethoxysilane, 3-methacryloxypropyl(methyl)dimethoxysilane, 3-methacryloxypropyl(methyl)diethoxysilane, vinyl(methyl)dimethoxysilane, vinyl(methyl)diethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyl(methyl)dimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyl(methyl)diethoxysilane, 3-ethyl-3-[3'-(methyldimethoxysilyl)propyl]methyloxetane, 3-ethyl-3-[3'-(methyldiethoxysilyl)propyl]methyloxetane, and the like can be preferably used.
[0078] A structural unit having a polymerizable group can also be used in combination with a structural unit having no polymerizable group. As a structural unit having no polymerizable group, trifunctional ones include trimethoxy(methyl)silane, triethoxy(methyl)silane, methyltrippropoxysilane, tributoxy(methyl)silane, methyltriphenoxysilane, ethyltrimethoxysilane, triethoxy(ethyl)silane, ethyltrippropoxysilane, tributoxy(ethyl)silane, ethyltriphenoxysilane, trimethoxy(propyl)silane, triethoxy(propyl)silane, tripropoxy(propyl)silane, tributoxy(propyl)silane, triphen ... Silane, butyltrimethoxysilane, butyltriethoxysilane, butyltrippropoxysilane, tributoxy(butyl)silane, butyltriphenoxysilane, trimethoxy(phenyl)silane, triethoxy(phenyl)silane, phenyltrippropoxysilane, tributoxy(phenyl)silane, triphenoxy(phenyl)silane, cyclohexyltrimethoxysilane, cyclohexyltriethoxysilane, cyclohexyltrippropoxysilane, cyclohexyltributoxysilane, cyclohexyltriphenoxysilane, etc. can be used. Among these, trimethoxy(methyl)silane, triethoxy(methyl)silane, ethyltrimethoxysilane, triethoxy(ethyl)silane, trimethoxy(phenyl)silane, triethoxy(phenyl)silane, cyclohexyltrimethoxysilane, cyclohexyltriethoxysilane, etc. can be preferably used.
[0079] As bifunctional silanes, dimethoxydimethylsilane, diethoxydimethylsilane, methylphenyldimethoxysilane, methylphenyldiethoxysilane, cyclohexyl(dimethoxy)methylsilane, cyclohexyldiethoxymethylsilane, dimethoxydiphenylsilane, diethoxydiphenylsilane, dimethoxymethylvinylsilane, diethoxymethylvinylsilane, and the like can be preferably used.
[0080] In this embodiment, the structure of the polymerizable compound is not particularly limited.However, if the polymerizable compound has a spherical structure as described below, or if the polyhedral siloxane oligomer has an incompletely condensed skeleton, it is preferable because it can be made into a curable resin with sufficiently low viscosity even if it does not substantially contain a solvent.In particular, if the polymerizable compound has a spherical structure, it is preferable from the viewpoint of thermal stability, processing uniformity, etc.
[0081] The spherical structure means a structure in which the polymerizable functional group extends outward from the polymerized part with a high degree of polymerization. For example, in the case of a polymerizable compound having a spherical structure such as a dendrimer, the ratio of oxygen atoms bonded to a single silicon atom among oxygen atoms bonded to silicon atoms contained in the polymerizable compound is 10 mol % or less, and the viscosity of the curable resin can be sufficiently reduced by simply adding a small amount of a solvent or low-viscosity material.
[0082] Examples of the polymerizable compound having a spherical structure include those having trifunctional silane as a constituent unit. Among them, those having only trifunctional silane as a constituent unit are preferable. Examples of the polymerizable compound having such a spherical structure include one or a mixture of two or more hexamers to 36amers (molecular weight 1000 to 6300) of trifunctional silane having a polymerizable functional group. The molecular weight of the polymerizable compound having a spherical structure may be in the range of 2000 to 6000, preferably in the range of 2000 to 3000.
[0083] In the case of trifunctional siloxanes, SiO 3 / 2 The polymerizable compound has a structure in which polymerizable functional groups extend outward from a siloxane polymerization part having a high degree of siloxane polymerization, which is composed of units. In the polymerizable compound having such a spherical structure, the degree of siloxane polymerization in the siloxane polymerization part is higher than 90%, and can be particularly 95% or more, and further 97% or more, so that the proportion of oxygen atoms bonded to a single silicon atom among the oxygen atoms bonded to silicon atoms contained in the polymerizable compound is 10 mol% or less.
[0084] This is presumably due to the following reason. That is, when a hydrolysis reaction of a trifunctional silane is carried out under basic conditions, OH groups are bonded to the Si atom. - A nucleophilic reaction occurs. As one hydrolyzable group (alkoxy group) is hydrolyzed, the steric hindrance of the Si atom decreases, increasing the hydrolysis reaction rate, and all three hydrolyzable groups (alkoxy groups) are hydrolyzed to produce -Si(OH)3. As all OH groups in -Si(OH)3 are capable of condensation polymerization, a three-dimensional siloxane structure with high density and high degree of polymerization is formed.
[0085] Specifically, it has a spherical structure represented by the following formula: The following formula is a schematic diagram showing a polymerizable compound having a spherical structure, which is composed of an octamer of trifunctional silane having an acryloxypropyl group and a 3-methacryloxypropyl group as the polymerizable group.
[0086] [ka] In the formula, SiO 1.5 SiO 3 / 2 The siloxane polymer moiety is composed of units.
[0087] In the present disclosure, the polymerizable compound having the spherical structure may be one that does not have an oxygen atom, a nitrogen atom, a phosphorus atom, or a sulfur atom in the bond between the siloxane polymerized portion constituting the main skeleton of the spherical structure and the polymerizable functional group, and the silicon atom (e.g., SiO 3 / 2 There may be no oxygen atom, nitrogen atom, phosphorus atom or sulfur atom between the silicon atom of the unit and the polymerizable functional group.
[0088] The bonding group between the silicon atom and the polymerizable functional group in the siloxane polymerization portion may be, for example, a divalent hydrocarbon group that does not contain an oxygen atom, a nitrogen atom, a phosphorus atom, or a sulfur atom, preferably a linear alkylene group, more preferably -(CH2) n -(n is an integer from 1 to 9).
[0089] The polymerizable compound having a spherical structure can be obtained by subjecting a hydrolyzable silane composition containing at least a hydrolyzable silane to a hydrolysis condensation reaction under basic conditions.
[0090] Specifically, the reaction can be carried out by placing a solvent and silane as the raw material in a reactor, adding a basic catalyst, and adding water dropwise while stirring. Examples of basic catalysts include sodium hydroxide, potassium hydroxide, lithium hydroxide, potassium carbonate (K2CO3), sodium carbonate, and ammonia. The reaction can be carried out at a pH of 8 to 13, typically at room temperature to 100°C.
[0091] The silane as the raw material may be any one or more of tetrafunctional hydrolyzable silane, trifunctional hydrolyzable silane, bifunctional hydrolyzable silane, and monofunctional hydrolyzable silane, but it is preferable to use tetrafunctional hydrolyzable silane or trifunctional hydrolyzable silane, especially trifunctional hydrolyzable silane. Also, only one type of hydrolyzable silane may be used, or two or more types may be used in combination.
[0092] In this way, by using a basic catalyst as the catalyst in the synthesis step, the polymerizable compound obtained by the hydrolysis condensation reaction has a high degree of condensation, and therefore, it is possible to easily obtain a polymerizable compound having a spherical structure in which the ratio of oxygen atoms bonded to a single silicon atom among oxygen atoms bonded to silicon atoms is reduced, particularly to 10 mol % or less.
[0093] In addition, the polymerizable compound may be a polyhedral siloxane oligomer having an incompletely condensed skeleton.Since such a polymerizable compound has a regular structure, the ratio of oxygen atoms bonded to a single silicon atom among the oxygen atoms bonded to silicon atoms contained in the polymerizable compound is 10 mol% or less.In addition, the viscosity of the curable resin can be sufficiently reduced.
[0094] The polyhedral siloxane oligomer having a skeleton that is incompletely condensed and has a polymerizable functional group bonded thereto may be an incompletely condensed type of the polyhedral siloxane oligomer having a skeleton that is completely condensed, in which one vertex, one side, or one face is missing.The polyhedral siloxane oligomer having a skeleton that is incompletely condensed and has a polymerizable functional group bonded thereto is particularly preferably one represented by the following formula:
[0095] [ka]
[0096] In the formula, R 3 is a monovalent hydrocarbon group, R 4 R is a -Si-polymerizable group bonded to the oxygen atom in the formula, a hydrogen atom, a metal ion such as Na or Li, or a tetraalkylammonium ion (the alkyl group is methyl, ethyl, propyl, butyl, etc.). 3 is a monovalent hydrocarbon group, preferably an alkyl group having 1 to 5 carbon atoms, or a phenyl group, specifically an ethyl group, a butyl group, or a phenyl group.
[0097] The polymerizable compound can be obtained by reacting a polyhedral siloxane oligomer having an incompletely condensed skeleton in which a hydrogen atom, a hydroxyl group, or an organic group other than a polymerizable functional group is bonded to a silicon atom, with a polymerizable functional group-containing compound.
[0098] The raw material, a polyhedral siloxane oligomer having an incompletely condensed skeleton, has a silicon atom at its vertex bonded to a hydrogen atom, a hydroxyl group, or an organic group other than a polymerizable functional group, such as an alkoxy group, an alkyl group, or a phenyl group.
[0099] The reaction between the above-mentioned raw material and the polymerizable functional group-containing compound may be a conventionally known reaction. For example, the addition reaction between a hydrogen atom directly bonded to silicon and a polymerizable functional group-containing compound having an unsaturated double bond, or the reaction between a hydroxyl group (OH group) or an alkoxy group (OR group) directly bonded to silicon and a polymerizable functional group-containing compound capable of forming a siloxane bond may be included.
[0100] The curable resin may contain a polymerization initiator. Examples of the polymerization initiator include a photopolymerization initiator and a thermal polymerization initiator, with a photopolymerization initiator being particularly preferred.
[0101] A photopolymerization initiator is a substance that generates reactive species that cause a polymerization reaction of a polymerizable compound by light stimulation. Specific examples include photoradical generators that generate radicals by light stimulation and photoacid generators that generate protons by light stimulation. A photoradical generator is a polymerization initiator that generates radicals by light (radiation such as infrared rays, visible light, ultraviolet rays, far ultraviolet rays, charged particle rays such as X-rays and electron beams), and is mainly used when the polymerizable compound is a radical polymerizable compound. On the other hand, a photoacid generator is a polymerization initiator that generates acid (protons) by light, and is mainly used when the polymerizable compound is a cationic polymerizable compound.
[0102] Examples of photoradical generators include, but are not limited to, 2,4,6-trimethyldiphenylphosphine oxide, 2,2-dimethoxy-2-phenylacetophenone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, and 2-hydroxy-2-methyl-1-phenyl-propan-1-one. These photoradical generators may be used alone or in combination of two or more.
[0103] Examples of photoacid generators include, but are not limited to, onium salt compounds, sulfone compounds, sulfonate ester compounds, sulfonimide compounds, and diazomethane compounds.
[0104] The thermal polymerization initiator is a compound that generates the above-mentioned polymerization factors (radicals, cations, etc.) by heat. Specifically, the thermal polymerization initiator is a thermal radical generator that generates radicals by heat, a compound that generates protons (H + Thermal radical generators are mainly used when the polymerizable compound is a radical polymerizable compound. On the other hand, thermal acid generators are mainly used when the polymerizable compound is a cationically polymerizable compound.
[0105] Examples of the thermal radical generator include organic peroxides and azo compounds. Examples of the organic peroxides include peroxyesters such as t-hexylperoxyisopropyl monocarbonate, t-hexylperoxy-2-ethylhexanoate, t-butylperoxy-3,5,5-trimethylhexanoate, and t-butylperoxyisopropyl carbonates, peroxyketals such as 1,1-bis(t-hexylperoxy)3,3,5-trimethylcyclohexane, and diacyl peroxides such as lauroyl peroxide, but are not limited thereto. Examples of the azo compounds include azonitriles such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), and 1,1'-azobis(cyclohexane-1-carbonitrile), but are not limited thereto.
[0106] Examples of the thermal acid generator include known iodonium salts, sulfonium salts, phosphonium salts, ferrocenes, etc. Specific examples include diphenyliodonium hexafluoroantimonate, diphenyliodonium hexafluorophosphate, diphenyliodonium hexafluoroborate, triphenylsulfonium hexafluoroantimonate, triphenylsulfonium hexafluorophosphate, and triphenylsulfonium hexafluoroborate, but are not limited thereto.
[0107] The content of the polymerization initiator in the curable resin is not particularly limited, and can be in the range of 0.5% by mass to 20% by mass, or in the range of 1% by mass to 10% by mass, relative to the polymerizable compound.
[0108] The curable resin may be substantially free of solvent. By substantially free of solvent, it is possible to suppress deterioration of flatness and poor curing caused by the solvent floating to the surface during curing. Here, "substantially free of solvent" means that it does not contain any solvent other than impurities and other solvents that are unintentionally contained. That is, for example, the content of the solvent in the curable resin is preferably 0.01% by mass or less, more preferably 0.001% by mass or less, based on the entire curable resin. The solvent means a solvent used in general resin compositions, photoresists, etc. That is, the type of solvent is not particularly limited as long as it dissolves and uniformly disperses the curable resin and does not react with the curable resin.
[0109] The curable resin may contain a reactive crosslinking agent. The reactive crosslinking agent may have a polymerizable functional group, for example, two or more polymerizable functional groups. Examples of the polymerizable functional group include an ethylenically unsaturated bond-containing group and an epoxy group, and the ethylenically unsaturated bond-containing group is preferable. Examples of the ethylenically unsaturated bond-containing group include a (meth)acrylic group and a vinyl group, and the (meth)acrylic group is more preferable, and the acrylic group is even more preferable. In addition, the (meth)acrylic group is preferably a (meth)acryloyloxy group. Two or more types of polymerizable groups may be contained in one molecule, or two or more of the same type of polymerizable groups may be contained.
[0110] Examples of photopolymerizable monomers (bifunctional monomers) having two polymerizable functional groups include trimethylolpropane di(meth)acrylate, ethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, and bis(hydroxymethyl)tricyclodecane di(meth)acrylate. Examples of commercially available products of the bifunctional monomer include Light Acrylate 3EG-A, 4EG-A, 9EG-A, NP-A, DCP-A, BP-4EAL, and BP-4PA (all manufactured by Kyoeisha Chemical Co., Ltd.). In addition, polyfunctional monomers having a siloxane structure are preferred from the viewpoint of compatibility.
[0111] The content of the reactive crosslinking agent is not particularly limited, and can be within the range of 0% by mass to 99% by mass in the curable resin, and is preferably within the range of 5% by mass to 80% by mass.
[0112] The curable resin may contain other components in addition to the above-mentioned polymerizable compound, polymerization initiator, and reactive crosslinking agent. Examples of other components include surfactants, release agents, silane coupling agents, photosensitizers, antioxidants, organometallic coupling agents, polymerization inhibitors, ultraviolet absorbers, light stabilizers, antiaging agents, plasticizers, adhesion promoters, photobase generators, colorants, elastomer particles, photoacid multipliers, basic compounds, other flow regulators, antifoamers, dispersants, and other components, as necessary. The content of other components is not particularly limited, but is preferably 5% by mass or less, and particularly preferably 3% by mass or less, in the curable resin.
[0113] The viscosity of the curable resin may be 20 cPs or less, preferably 10 cPs or less, more preferably 7 cPs or less. On the other hand, the lower limit of the viscosity is not particularly limited, but may be 1 cPs or more, preferably 1.5 cPs or more. Since the viscosity of the curable resin is very low, it can be applied to the concave-convex structure with good filling properties while suppressing the generation of bubbles. In addition, such a low viscosity makes it possible to apply the resin by an inkjet method. The viscosity of the curable resin is the value at 25°C and 1000 (1 / s) when the curable resin is dropped onto a disk plate using AR-G2 manufactured by TA Instruments in a measurement environment of 25°C and 40% RH, and a standard steel cone with a diameter of 40 mm is changed to a shear rate of 10 to 1000 (1 / s).
[0114] The contact angle of the curable resin with respect to the surface of the standard resist is preferably 20° or less, and more preferably 15° or less. Specifically, the contact angle can be measured by dropping the curable resin onto the surface of the standard resist layer in normal atmospheric pressure at a temperature of 25° C. and a humidity of 33%, and then using a contact angle measuring device (automatic contact angle meter DM-501, manufactured by Kyowa Interface Science Co., Ltd.) 5 seconds later. The standard resist layer may be formed, for example, using an acrylic-styrene copolymer (organic resist resin) as the base resin.
[0115] If the curable resin has a contact angle with respect to the standard resist layer, when it is used as a reversal layer material in a reversal process, for example, the curable resin has good wettability with respect to the core pattern formed from the resist composition, and can be applied with good filling properties. When the curable resin has the above contact angle with respect to the standard resist, it exhibits good wettability even if the composition of the organic resist material actually used for the core pattern is different from the composition of the standard resist.
[0116] The surface free energy of the curable resin is 20 mJ / m 2 More than 70mJ / m 2 It is preferable that the ion exchange coefficient is equal to or less than 25 mJ / m 2 More than 50mJ / m 2 If it is in the above range, for example, compatibility with the core pattern made of an organic resist material can be suppressed, and the resin can be sufficiently wetted and spread on the core pattern, which is preferable.
[0117] 1B and 1D is not particularly limited, and may be, for example, a material having a modulus of elasticity (Young's modulus) greater than that of the material constituting the stress relaxation layer 31. When the modulus of elasticity (Young's modulus) of the material constituting the uneven pattern layer 32 is greater than that of the material constituting the stress relaxation layer 31, the stress relaxation layer 31 can relax the stress in the thickness direction of the base material 2, and suppress deformation of the uneven pattern layer 32 (uneven pattern 4).
[0118] Examples of materials that can be used to form the uneven pattern layer 32 include resin materials such as thermoplastic resins, such as acrylic resins, styrene resins, olefin resins, polycarbonate resins, polyester resins, and epoxy resins, thermosetting resins, and ultraviolet-curing resins.
[0119] The imprint mold 1 according to this embodiment may have a protective layer 5 that covers the surface of the concave-convex pattern 4 of the pattern layer 3 shown in Figures 1A and 1C and the concave-convex pattern 4 of the concave-convex pattern layer 32 shown in Figures 1B and 1D. The resin material constituting the pattern layer 3 shown in Figures 1A and 1C and the concave-convex pattern layer 32 shown in Figures 1B and 1D has low resistance to solvents contained in the imprint resin 91 (see Figure 8A) to which the concave-convex pattern 4 of the imprint mold 1 according to this embodiment is transferred. Therefore, the pattern layer 3 and the concave-convex pattern layer 32 may swell due to the solvents contained in the imprint resin, and the dimensions of the concave-convex pattern 4 may change. In addition, the resin material constituting the pattern layer 3 and the concave-convex pattern layer 32 may be dissolved in a cleaning liquid (cleaning liquid for cleaning the imprint mold 1) such as sulfuric acid, hydrogen peroxide water, and ammonia water, or in the imprint resin. In this embodiment, a protective layer 5 is provided to cover the concave-convex pattern 4, thereby preventing the pattern layer 3 and the concave-convex pattern layer 32 from swelling due to the solvent contained in the imprint resin, or from dissolving in the cleaning liquid or the imprint resin.
[0120] The thickness of the protective layer 5 is not particularly limited, but may be, for example, about 1 nm to 100 nm, or about 1 nm to 10 nm. A protective layer 5 having a thickness of 1 nm or more can suppress swelling due to a solvent contained in the imprint resin, or dissolution in a cleaning liquid or the imprint resin. In the optical imprint process using the imprint mold 1 according to this embodiment, if the protective layer 5 has a thickness of 100 nm or less, there is no effect on the transmission of light (ultraviolet light) for curing the imprint resin.
[0121] The elastic modulus (Young's modulus) of the material constituting the protective layer 5 is preferably larger than the elastic modulus (Young's modulus) of the material constituting the pattern layer 3 shown in Figures 1A and 1C and the stress relaxation layer 31 shown in Figures 1B and 1D in order to realize the effects produced by the pattern layer 3 and the stress relaxation layer 31 (effects due to deformation of the pattern layer 3 and the stress relaxation layer 31 caused by stress).
[0122] The elastic modulus (Young's modulus) of the material constituting the protective layer 5 is preferably equal to or greater than the elastic modulus (Young's modulus) of the material constituting the base material 2. In addition, the elastic modulus (Young's modulus) of the material constituting the protective layer 5 is preferably equal to or greater than the elastic modulus (Young's modulus) of the material constituting the concave-convex pattern layer 32 shown in Figures 1B and 1D. During the imprint process using the imprint mold 1 according to this embodiment, when the concave-convex pattern 4 is pressed against the imprint resin supplied onto the transfer substrate, damage to the concave-convex pattern 4 due to foreign matter or the like on the transfer substrate can be suppressed.
[0123] Examples of the protective layer 5 include, but are not limited to, a SiO2 layer, a SiN layer, a Cr layer, a CrN layer, a Ti layer, a Ta layer, and a TaO layer.
[0124] In the imprint mold 1 shown in FIG. 1A and FIG. 1C, the surface of the pattern layer 3 (concave-convex pattern 4) may be modified without providing the protective layer 5. The protective layer 5 can improve resistance to the solvent contained in the imprint resin and can suppress damage to the concave-convex pattern 4. The same effect, particularly the effect of suppressing damage to the concave-convex pattern 4, can be expected by modifying the surface of the pattern layer 3. Examples of a method for modifying the surface of the pattern layer 3 include a method of subjecting the surface of the pattern layer 3 to a plasma treatment or an electron beam irradiation treatment. By subjecting the surface of the pattern layer 3 to a plasma treatment or an electron beam irradiation treatment, the elastic modulus (Young's modulus) near the surface of the pattern layer 3 can be made larger than the elastic modulus (Young's modulus) inside the pattern layer 3, so that damage to the concave-convex pattern 4 can be suppressed. That is, the pattern layer 3 may have a gradient of elastic modulus (Young's modulus) so that the elastic modulus (Young's modulus) gradually decreases from the surface of the pattern layer 3 toward the first surface 2A side of the substrate 2.
[0125] In this embodiment, a release layer 6 may be provided to cover the protective layer 5 (see FIGS. 1A to 1D). By providing the release layer 6, the imprint mold 1 can be easily separated from the imprint resin during the imprint process using the imprint mold 1 according to this embodiment. Examples of materials constituting the release layer 6 include a fluorine alkyl-containing silane coupling agent and a long-chain alkyl-containing silane coupling agent. The thickness of the release layer 6 may be, for example, about 0.1 nm to 3 nm.
[0126] In this embodiment, as shown in Fig. 1C, a planarizing layer 7 may be provided between the pattern layer 3 and the first surface 2A of the substrate 2. Also, as shown in Fig. 1D, a planarizing layer 7 may be provided between the concave-convex pattern layer 32 and the stress relaxation layer 31. As in the imprint mold 1 shown in Figs. 1C and 1D, the provision of the planarizing layer 7 can ensure the parallelism of the concave-convex pattern 4 of the pattern layer 3 (see Fig. 1C) and the concave-convex pattern layer 32 (see Fig. 1D).
[0127] The material constituting the planarization layer 7 is not particularly limited, and examples thereof include acrylic resins, styrene resins, olefin resins, polycarbonate resins, polyester resins, and epoxy resins. The elastic modulus (Young's modulus) of the material constituting the planarization layer 7 may be larger than the elastic modulus (Young's modulus) of the material constituting the pattern layer 3 (see FIG. 1C) and the stress relaxation layer 31 (see FIG. 1D). The material constituting the planarization layer 7 may be a polyurethane resin, a polyamide resin, a curable resin containing Si, or the like, which may be used as the material constituting the pattern layer 3 (see FIG. 1C) and the stress relaxation layer 31 (see FIG. 1D). In this case, for example, the planarization layer 7 may have a relatively large molecular weight, and the cross-linking rate may be increased by adjusting the film formation conditions of the planarization layer 7, so that the planarization layer 7 has a larger elastic modulus (Young's modulus) than the pattern layer 3 (see FIG. 1C) and the stress relaxation layer 31 (see FIG. 1D).
[0128] [Imprint mold manufacturing method] A method for manufacturing the imprint mold 1 shown in FIGS. 1A and 1C will be described. First, the master mold 10 used to manufacture the imprint mold 1 is prepared.
[0129] When manufacturing the master mold 10, first, a master mold substrate 11 is prepared, which has a first surface 11A and a second surface 11B located opposite to the first surface 11A, and a resist layer 20 formed on the first surface 11A (see FIG. 3A). Note that a hard mask layer may be formed on the first surface 11A, and the master mold substrate 11 may be prepared in such a way that the resist layer 20 is formed on the hard mask layer.
[0130] Next, the resist layer 20 is subjected to an electron beam lithography process or an exposure process through a photomask having predetermined openings, and a development process, to form a resist pattern 21 corresponding to the concave-convex pattern 12 of the master mold 10 (see FIG. 3B).
[0131] Using the resist pattern 21 formed as described above as an etching mask, the first surface 11A of the master mold substrate 11 is etched (see Figure 3C) and the last remaining resist pattern 21 is removed to produce a master mold 10 having a concave-convex pattern 12 including a concave pattern 121 corresponding to the concave portions 41 of the imprint mold 1 and a convex pattern 122 corresponding to the convex portions 42 (see Figure 3D).
[0132] Next, a base material 2 is prepared as an imprint mold substrate having a first surface 2A and a second surface 2B located on the opposite side of the first surface 2A, and a pattern layer-forming resin layer 30 (see FIG. 4A) or a planarizing layer 7 and a pattern layer-forming resin layer 30 (see FIG. 6A) formed on the first surface 2A (see FIGS. 4A and 6A). The planarizing layer 7 can be formed by applying a material constituting the planarizing layer 7 to the first surface 2A of the base material 2 by a spin coating method or the like, and pressing a flat mold (not shown) against it to harden it.
[0133] Next, the master mold 10 manufactured as described above is prepared, and the master mold 10 is brought into contact with the resin layer 30 for forming a pattern layer formed on the first surface 2A of the substrate 2, so that the resin layer 30 for forming a pattern layer fills the uneven pattern 12 of the master mold 10, and the resin layer 30 for forming a pattern layer is hardened in this state (see Figures 4B and 6B).
[0134] The method for curing the resin layer 30 for forming a pattern layer may be appropriately selected depending on the curing type of the curable resin constituting the resin layer 30 for forming a pattern layer. For example, if the curable resin is a photocurable type, the resin layer 30 for forming a pattern layer (curable resin) may be irradiated with light (e.g., ultraviolet light, electron beam, etc.) through the master mold 10. If the curable resin is a thermosetting type, heat may be applied to the resin layer 30 for forming a pattern layer (curable resin). If the curable resin is a thermoplastic type, the resin layer 30 for forming a pattern layer that has been softened by heating may be brought into contact with the master mold 10, and then cooled to cure the resin layer 30 for forming a pattern layer.
[0135] Then, the master mold 10 is separated from the cured resin layer 30 for forming a pattern layer (see FIGS. 4C and 6C). As a result, a pattern layer 3 having a concave-convex pattern 4 is formed on the first surface 2A of the substrate 2.
[0136] Next, a protective layer 5 is formed on the surface of the pattern layer 3 (concave-convex pattern 4) (see FIGS. 4D and 6D). The protective layer 5 can be formed, for example, by depositing a material constituting the protective layer 5 (e.g., SiO2, etc.) by a CVD method or the like. Then, a release layer 6 is formed on the surface of the protective layer 5, thereby producing the imprint mold 1 according to this embodiment (see FIGS. 4E and 6E).
[0137] Next, a method for manufacturing the imprint mold 1 shown in FIGS. 1B and 1D will be described. First, a substrate 2 is prepared, which has a first surface 2A and a second surface 2B located opposite the first surface 2A, and in which a resin layer 310 for forming a stress relaxation layer and a resin layer 320 for forming a concave-convex pattern layer (see Figure 5A), or a resin layer 310 for forming a stress relaxation layer, a planarizing layer 7 and a resin layer 320 for forming a concave-convex pattern layer (see Figure 7A) are formed on the first surface 2A (see Figures 5A and 7A).
[0138] Next, the master mold 10 manufactured as described above is prepared, and the master mold 10 is brought into contact with the resin layer 320 for forming the concave-convex pattern layer formed on the first surface 2A of the substrate 2, so that the resin layer 320 for forming the concave-convex pattern layer fills the concave-convex pattern 12 of the master mold 10, and the resin layer 320 for forming the concave-convex pattern layer is hardened in this state (see Figures 5B and 7B).
[0139] Then, the master mold 10 is separated from the cured resin layer 320 for forming a concave-convex pattern layer (see FIGS. 5C and 7C). As a result, a concave-convex pattern layer 32 having a concave-convex pattern 4 is formed on the first surface 2A of the substrate 2.
[0140] Next, a protective layer 5 is formed on the surface of the concave-convex pattern layer 32 (convex pattern 4) (see FIGS. 5D and 7D). Then, a release layer 6 is formed on the surface of the protective layer 5, thereby producing the imprint mold 1 according to this embodiment (see FIGS. 5E and 7E).
[0141] [Imprint method] An imprint method using the imprint mold 1 according to this embodiment will be described. An imprint mold 1 and a transferee substrate 90 having a first surface 90A and a second surface 90B located on the opposite side of the first surface 90A are prepared, and an imprint resin 91 is supplied to the first surface 90A of the transferee substrate 90 (see FIG. 8A). The method of supplying the imprint resin 91 to the first surface 90A of the transferee substrate 90 is not particularly limited, and for example, the imprint resin 91 may be discretely supplied to the first surface 90A of the transferee substrate 90 by an inkjet method, or the imprint resin may be applied to the first surface 90A of the transferee substrate 90 by using a coating machine such as a spin coater or a spray coater. Note that, as an example of the imprint method in this embodiment, a mode in which a foreign object 100 exists on the first surface 90A of the transferee substrate 90 is given.
[0142] The imprint mold 1 is brought close to the imprint resin 91 supplied to the first surface 90A of the transfer substrate 90, and the imprint resin 91 is spread between the first surface 90A of the transfer substrate 90 and the imprint mold 1 to form a molded resin layer 92 (see Figure 8B).
[0143] When the imprint mold 1 is brought into contact with the molded resin layer 92, at least one of the convex portions 42 of the imprint mold 1 comes into contact due to the presence of the foreign object 100 on the first surface 90A of the transfer substrate 90. When the imprint mold 1 is pressed toward the transfer substrate 90 side with the convex portion 42 in contact with the foreign object 100, stress is applied in the thickness direction of the substrate 2 to the convex portion 42 in contact with the foreign object 100. In the imprint mold 1 according to this embodiment, the elastic modulus (Young's modulus) of the material constituting the pattern layer 3 and the stress relaxation layer 31 is sufficiently small, so that the pattern layer 3 or the stress relaxation layer 31 located near the convex portion 42 to which stress is applied and below the convex portion 42 (on the first surface 2A side of the substrate 2) is deformed so as to contract. Therefore, defects due to non-filling of the imprint resin 91 may occur near the convex portion 42 with which the foreign object 100 is in contact, but the concave-convex pattern 4 of the imprint mold 1 can be transferred with high accuracy in the area adjacent to the convex portion 42. If the elastic modulus (Young's modulus) is relatively large, the amount of deformation of the pattern layer 3 or the stress relaxation layer 31 is small, and the imprint resin 91 is not sufficiently filled in the convex portion 42 with which the foreign matter 100 comes into contact and the concave portion 41 and the convex portion 42 around it, resulting in a relatively large area where unfilled defects occur. However, according to the imprint mold 1 according to this embodiment, the amount of deformation of the pattern layer 3 or the stress relaxation layer 31 can be made sufficiently large, so that the area where unfilled defects caused by the foreign matter 100 occur can be minimized. In addition, it is also possible to prevent the convex portion 42 with which the foreign matter 100 comes into contact from being damaged due to the deformation of the pattern layer 3 or the stress relaxation layer 31. Furthermore, since the cross-sectional shape of the convex portion 42 is tapered, the strength of the convex portion 42 itself is improved, so that it is also possible to prevent the convex portion 42 from collapsing due to the contact of the foreign matter 100 or the imprint resin 91 not being filled.
[0144] While the imprint mold 1 is in contact with the molded resin layer 92 (imprinted resin 91), the molded resin layer 92 (imprinted resin 91) is irradiated with light (e.g., ultraviolet light, electron beam, etc.) through the imprint mold 1 to harden the molded resin layer 92. Thereafter, the imprint mold 1 is separated from the hardened molded resin layer 92 (see FIG. 8C). When the imprint mold 1 is separated, the pattern layer 3 or the stress relaxation layer 31 that has been deformed by the stress caused by the foreign matter 100 recovers without plastic deformation due to the high elastic recovery rate of the constituent material. Therefore, according to this embodiment, the life of the imprint mold 1 can be extended.
[0145] In this manner, a transfer pattern 93 in which the concave-convex pattern 4 of the imprint mold 1 is transferred can be formed on the first surface 90A of the transfer substrate 90. As described above, the transfer substrate 90 on which the transfer pattern 93 is formed, or a concave-convex structure obtained by performing an etching process on the first surface 90A of the transfer substrate 90 using the transfer pattern 93 as an etching mask can be manufactured as an article such as an optical product or an aerospace product.
[0146] The above-described embodiments are described for the purpose of facilitating understanding of the present invention, and are not described for the purpose of limiting the present invention. Therefore, each element disclosed in the above embodiment is intended to include all design modifications and equivalents that fall within the technical scope of the present invention. [Explanation of symbols]
[0147] 1. Imprint mold 2...Base material 3...Pattern layer 31...Stress relief layer 32…Concave and convex pattern layer 4…Concave and convex pattern 5…Protective layer
Claims
1. a substrate having a first surface and a second surface opposite the first surface; a pattern layer provided on the first surface side of the substrate and having a concave-convex pattern including concave portions and convex portions; Equipped with The pattern layer has a function of being deformed by a stress in a thickness direction of the base material and a function of being restored when the stress is released, The Young's modulus of the material of the pattern layer is smaller than the Young's modulus of the material of the base material; The elastic recovery rate of the material of the pattern layer is greater than the elastic recovery rate of the material of the base material; The Young's modulus of the material constituting the substrate is 70 GPa or less. Imprint mold.
2. a substrate having a first surface and a second surface opposite the first surface; a pattern layer provided on the first surface side of the substrate and having a concave-convex pattern including concave portions and convex portions; Equipped with the pattern layer includes a stress relief layer provided on the first surface side of the base material, and a concave-convex pattern layer provided on the stress relief layer and having the concave-convex pattern, the Young's modulus of the material constituting the stress relaxation layer is smaller than the Young's modulus of the material constituting the base material; The elastic recovery rate of the constituent material of the stress relaxation layer is greater than the elastic recovery rate of the constituent material of the base material, The Young's modulus of the material constituting the substrate is 70 GPa or less. Imprint mold.
3. The Young's modulus of the outermost surface of the concave-convex pattern is greater than the Young's modulus of the material constituting the pattern layer. The imprint mold of claim 1 .
4. a protective layer covering the surface of the concave-convex pattern; The Young's modulus of the material constituting the protective layer is greater than the Young's modulus of the material constituting the pattern layer. The imprint mold of claim 3 .
5. The protective layer is made of SiO 2 Includes The imprint mold of claim 4 .
6. The thickness of the protective layer is 1 nm to 100 nm. The imprint mold of claim 4 .
7. When viewed in a cross section along the thickness direction of the substrate, an angle between a bottom surface of the recess of the concave-convex pattern and a side wall of the convex portion is less than 90°. The imprint mold according to claim 1 or 2.
8. a planarization layer disposed between the first surface of the substrate and the pattern layer; The imprint mold of claim 1 .
9. A planarization layer is provided between the stress relaxation layer and the concave-convex pattern layer. The imprint mold of claim 2 .
10. a material constituting the pattern layer is a curable resin containing a polymerizable compound having an organic component and an inorganic component in a molecule; The inorganic component is SiO X (X is 1 or more) The imprint mold of claim 1 .
11. the material constituting the stress relaxation layer is a curable resin containing a polymerizable compound having an organic component and an inorganic component in its molecule, The inorganic component is SiO X (X is 1 or more) The imprint mold of claim 2 .
12. The polymerizable compound has a siloxane bond as the inorganic component, Among the oxygen atoms bonded to silicon atoms contained in the polymerizable compound, the ratio of oxygen atoms bonded to a single silicon atom is 10 mol % or less. The imprint mold according to claim 10 or 11.
13. The polymerizable compound has a spherical structure. The imprint mold according to claim 10 or 11.
14. The recesses and / or protrusions of the uneven pattern have a size of 8 nm to 1000 nm. The imprint mold according to claim 1 or 2.
15. 13. A method for manufacturing the imprint mold of claim 1, comprising the steps of: applying a pattern layer forming material to the first surface of the substrate to form the pattern layer; preparing a master mold having a pattern corresponding to the concave-convex pattern, and contacting the pattern of the master mold with the pattern layer forming material to fill the pattern with the pattern layer forming material; curing the pattern layer forming material filled in the pattern of the master mold; Releasing the master mold from the hardened pattern layer forming material; A method for manufacturing an imprint mold having the following features.
16. A method for manufacturing the imprint mold of claim 2, comprising the steps of: forming the stress relief layer on the first surface of the base material; A step of applying a pattern layer forming material for forming the concave-convex pattern layer on the stress relaxation layer; preparing a master mold having a pattern corresponding to the concave-convex pattern, and contacting the pattern of the master mold with the pattern layer forming material to fill the pattern with the pattern layer forming material; curing the pattern layer forming material filled in the pattern of the master mold; Releasing the master mold from the hardened pattern layer forming material; A method for manufacturing an imprint mold having the following features.
17. The method for producing an imprint mold according to claim 15 or 16, further comprising a step of forming a protective layer on a surface of the concave-convex pattern formed by separating the master mold.
18. providing a substrate having a first side and a second side opposite the first side; applying an imprint resin to the first surface of the substrate; a step of contacting the imprinting mold according to claim 1 or 2 with the imprinting resin to fill the concave-convex pattern with the imprinting resin; curing the imprint resin filled in the concave-convex pattern; Releasing the imprint mold from the hardened imprint resin. A method for manufacturing an article comprising the steps of:
Citation Information
Patent Citations
Mold for nanoimprint
JP2012011728A