Laminate, display device including the same, and adhesive layer
The laminate structure with specific adhesive layer stress reduction rates and bending stiffness addresses the flexibility issues of conventional laminates, ensuring robust performance under thermal and low-temperature bending conditions.
Patent Information
- Application Number
- JP2023055716
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Conventional laminates lack sufficient thermal shock flexibility and low-temperature flexibility, especially when bent with the front plate side inward, necessitating improvements in these areas.
A laminate structure comprising a front plate, first and second adhesive layers, a polarizer layer, and a back plate, where the first adhesive layer has a stress reduction rate of 40% to 70% and satisfies the relationship R1 ≤ R2, with bending stiffness between 1000 gf·m and 2000 gf·m at -20°C, and specific thickness and composition ratios of the adhesive layers to enhance flexibility.
The laminate exhibits excellent thermal shock flexibility and low-temperature flexibility when bent with the front plate side inward, minimizing air bubbles and peeling between layers under extreme temperature changes.
Smart Images

Figure 2024143182000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate and a display device including the same, as well as an adhesive layer for a flexible display device. [Background technology]
[0002] Patent Document 1 describes a laminate including, in this order, a front plate, a first pressure-sensitive adhesive layer, a polarizer layer, a second pressure-sensitive adhesive layer, and a back plate. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-154308 A Summary of the Invention [Problem to be solved by the invention]
[0004] A conventional laminate such as that described in Patent Document 1 has good flexibility. However, the thermal shock flexibility and low-temperature flexibility of the conventional laminate are not necessarily sufficient, and there is room for improvement.
[0005] Depending on the application, the laminate may be bent so that the front panel side faces inward. In such applications, the laminate is required to have improved thermal shock bending properties and low-temperature bending properties when bent so that the front panel side faces inward.
[0006] Therefore, the present invention aims to provide a laminate that has excellent thermal shock bending properties and low-temperature bending properties when bent with the front panel side on the inside, a display device including the laminate, and an adhesive layer for a flexible display device. [Means for solving the problem]
[0007] The present invention provides the following laminate, display device, and pressure-sensitive adhesive layer. [1] A laminate comprising, in this order, a front panel, a first pressure-sensitive adhesive layer, a polarizer layer, a second pressure-sensitive adhesive layer, and a back panel, wherein the stress reduction rate of the first pressure-sensitive adhesive layer calculated by the following formula (1) is 40% or more and 70% or less, and the stress reduction rate R1 of the first pressure-sensitive adhesive layer and the stress reduction rate R2 of the second pressure-sensitive adhesive layer satisfy the relationship of the following formula (2). Stress reduction rate=100-{(RB / RA)×100} …(1) R1≦R2 …(2) [In formula (1), RA represents the stress (unit: Pa) when a 400% strain is applied to the adhesive layer at -20°C for the first time after the start of the strain cycle test, and RB represents the stress (unit: Pa) when a 400% strain is applied to the adhesive layer at 60°C for the last time in the 10th cycle of the strain cycle test.] [Strain Repeated Loading Test] The repeated strain test is performed by adhering an adhesive layer adjusted to a thickness of 150 μm to the measurement chip of a viscoelasticity measuring device, and repeatedly applying 0% strain and 400% strain under normal force free conditions and a frequency of 1 Hz, while maintaining the temperature at -20°C for 2 minutes, and then raising the temperature to 60°C at a heating rate of 10°C / min and maintaining the temperature for 2 minutes, which constitutes one cycle. This cycle is repeated for a total of 10 cycles. [2] The laminate according to [1] above, wherein the bending stiffness of the laminate at a temperature of -20°C is 1000 gf·m or more and 2000 gf·m or less. [3] The laminate according to [1] or [2] above, wherein the thickness of the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer are both 10 μm or more and 100 μm or less. [4] The laminate according to any one of the above [1] to [3], wherein the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer are both layers formed from a pressure-sensitive adhesive composition containing a (meth)acrylic polymer. [5] The laminate according to [4] above, wherein the (meth)acrylic polymer contains 20% by mass or more and 30% by mass or less of structural units derived from nitrogen-containing monomers, based on the total amount of structural units. [6] The laminate according to any one of [1] to [5] above, wherein the first pressure-sensitive adhesive layer is a layer formed from a first pressure-sensitive adhesive composition containing a fluorine atom-containing compound, and the content of the fluorine atom-containing compound is 5 mass% or less based on the total solid content of the first pressure-sensitive adhesive composition. [7] The laminate according to any one of the above [1] to [6], wherein a stress reduction rate R1 of the first pressure-sensitive adhesive layer and a stress reduction rate R2 of the second pressure-sensitive adhesive layer satisfy the relationship of the following formula (3). 0 Pa ≦ (R2-R1) ≦ 20 Pa … (3) [8] The laminate according to any one of the above [1] to [7], wherein the stress reduction rate of the second pressure-sensitive adhesive layer is 40% or more and 70% or less. [9] The laminate according to any one of the above [1] to [8], wherein a thickness T1 of the first pressure-sensitive adhesive layer and a thickness T2 of the second pressure-sensitive adhesive layer satisfy the relationship of the following formula (4): 0.1≦(T1 / T2)≦4 …(4)
[10] A display device comprising the laminate according to any one of the above [1] to [9].
[11] An adhesive layer disposed between a front panel and a polarizer layer of a flexible display device, the adhesive layer having a stress reduction rate calculated by the following formula (1) of 40% or more and 70% or less. Stress reduction rate=100-{(RB / RA)×100} …(1) [In formula (1), RA represents the stress (unit: Pa) when a 400% strain is applied to the adhesive layer at -20°C for the first time after the start of the strain cycle test, and RB represents the stress (unit: Pa) when a 400% strain is applied to the adhesive layer at 60°C for the last time in the 10th cycle of the strain cycle test.] [Strain Repeated Loading Test] The repeated strain test is performed by adhering an adhesive layer adjusted to a thickness of 150 μm to the measurement chip of a viscoelasticity measuring device, and repeatedly applying 0% strain and 400% strain under normal force free conditions and a frequency of 1 Hz, while maintaining the temperature at -20°C for 2 minutes, and then raising the temperature to 60°C at a heating rate of 10°C / min and maintaining the temperature for 2 minutes, which constitutes one cycle. This cycle is repeated for a total of 10 cycles. Effect of the Invention
[0008] According to the present invention, it is possible to provide a laminate having excellent thermal shock bending properties and low-temperature bending properties when bent with the front panel side on the inside, a display device including the laminate, and an adhesive layer for a flexible display device. [Brief description of the drawings]
[0009] [Figure 1] 1 is a schematic cross-sectional view showing one embodiment of a laminate according to the present invention. [Diagram 2] FIG. 4 is a schematic cross-sectional view showing another embodiment of the laminate according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, a laminate according to one embodiment of the present invention (hereinafter, simply referred to as a "laminate") will be described with reference to the drawings.
[0011] <Laminate> 1 shows a schematic cross-sectional view of a laminate according to one embodiment of the present invention. The laminate 100 includes, in this order, a front plate 101, a first adhesive layer 102, a polarizer layer 103, a second adhesive layer 104, and a back plate 105. Hereinafter, the first adhesive layer 102 and the second adhesive layer 104 may be collectively referred to as the "adhesive layer."
[0012] The laminate 100 according to this embodiment preferably has a bending stiffness S1 of 1000 gf·m or more and 2000 gf·m or less at -20°C. When the bending stiffness at -20°C is 1000 gf·m or more and 2000 gf·m or less, the laminate 100 has excellent flexibility and durability as well as moderate hardness, and when the laminate 100 is applied to a flexible display, for example, the display can be easily bent even in a low-temperature environment. In this embodiment, the bending stiffness of the laminate 100 is more preferably 1200 gf·m or more and 1800 gf·m or less, and even more preferably 1400 gf·m or more and 1600 gf·m or less. The bending stiffness is a value measured according to the method described in the examples.
[0013] The bending stiffness of the laminate 100 can be adjusted to a desired range, for example, by controlling the thickness of each layer constituting the laminate 100, the stress reduction rate of the adhesive layer, etc. Specifically, for example, the bending stiffness can be increased by increasing the thickness of the adhesive layer or the stress reduction rate.
[0014] The thickness of the laminate 100 is not particularly limited as it varies depending on the function required of the laminate and the use of the laminate, but is, for example, 30 μm or more and 1500 μm or less, preferably 40 μm or more and 1000 μm or less, and more preferably 50 μm or more and 500 μm or less.
[0015] The planar shape of the laminate 100 may be, for example, a square shape, preferably a square shape having long sides and short sides, and more preferably a rectangle. When the shape of the surface direction of the laminate 100 is a rectangle, the length of the long side may be, for example, 10 mm or more and 1400 mm or less, and preferably 50 mm or more and 600 mm or less. The length of the short side may be, for example, 5 mm or more and 800 mm or less, preferably 30 mm or more and 500 mm or less, and more preferably 50 mm or more and 300 mm or less. Each layer constituting the laminate may have rounded corners, notched ends, or holes.
[0016] The laminate 100 can be applied to, for example, a display device. The display device is not particularly limited, and examples thereof include an organic electroluminescence (organic EL) display device, an inorganic electroluminescence (inorganic EL) display device, a liquid crystal display device, and an electroluminescence display device. The display device may have a touch panel function. Furthermore, the display device to which the laminate 100 is applied can be used as a flexible display that can be bent or rolled. It is preferable that the display device is bendable with the front panel 101 side on the inside. The display device including the laminate 100 according to this embodiment is particularly excellent in thermal shock bending property and low-temperature bending property when bent with the front panel 101 side on the inside. However, the laminate 100 may be bendable with the front panel 101 side on the outside.
[0017] <Adhesive Layer (First Adhesive Layer and Second Adhesive Layer)> As described above, the laminate 100 includes the first adhesive layer 102 and the second adhesive layer 104. In the laminate 100, the stress reduction rate of the first adhesive layer 102 is 40% or more and 70% or less. The stress reduction rate is represented by the following formula (1). Stress reduction rate=100-{(RB / RA)×100} …(1) In formula (1), RA represents the stress (unit: Pa) when a 400% strain is first applied to the adhesive layer at -20°C after the start of the strain cycle test, and RB represents the stress (unit: Pa) when a 400% strain is finally applied at 60°C in the 10th cycle of the strain cycle test.
[0018] Furthermore, in the laminate 100, the stress reduction rate R1 of the first pressure-sensitive adhesive layer 102 and the stress reduction rate R2 of the second pressure-sensitive adhesive layer 104 satisfy the relationship of the following formula (2). R1≦R2 …(2)
[0019] The strain repetitive loading test is performed by adhering the adhesive layer adjusted to a thickness of 150 μm to the measuring chip of a viscoelasticity measuring device, repeatedly applying 0% strain and 400% strain under the conditions of normal force free and frequency of 1 Hz, and holding the temperature at -20°C for 2 minutes, then heating to 60°C at a heating rate of 10°C / min and holding for 2 minutes, which is one cycle, and repeating this cycle for a total of 10 cycles. The above temperature indicates the temperature of the adhesive layer. The stress RA and the stress RB can be determined according to the measurement method described in the Examples section below.
[0020] When the stress reduction rate of the first adhesive layer 102 is 40% or more and 70% or less, and the stress reduction rate R1 of the first adhesive layer 102 and the stress reduction rate R2 of the second adhesive layer 104 satisfy the relationship of the above formula (2), the laminate 100 can improve its durability by suppressing the generation of air bubbles in the first adhesive layer 102 under a thermal shock test (thermal shock bending test) environment in which the laminate 100 is bent with the front panel 101 side facing inward. Specifically, as shown in the examples described later, the laminate 100 is wrapped around a mandrel so that the front plate 101, which is the inner side when folded, is on the inner side, and is left at -20°C for 2 minutes, then left at 25°C for 2 minutes, and then left at 60°C for 2 minutes, for a total of 10 cycles. Then, even when the laminate is taken out to an environment of 25°C, the generation of bubbles in the first adhesive layer 102 and the occurrence of peeling between the first adhesive layer 102 and the front plate 101 can be suppressed (hereinafter, such performance is also referred to as "excellent bending durability in a thermal shock test environment"). When the laminate 100 is bent so that the front plate 101 side is on the inner side and thermal shock is applied, compared to the second adhesive layer 104, the first adhesive layer 102 located on the inner side (the side closer to the mandrel) of the second adhesive layer 104 is more likely to generate bubbles and peeling from the adjacent layer, but by satisfying the above conditions, the occurrence of bubbles in the first adhesive layer 102 and peeling from the adjacent layer can be suppressed.
[0021] In addition, when the stress reduction rate of the first adhesive layer 102 is 40% or more and 70% or less, and the stress reduction rate R1 of the first adhesive layer 102 and the stress reduction rate R2 of the second adhesive layer 104 satisfy the relationship of the above formula (2), the laminate 100 can improve durability by suppressing the generation of bubbles in the first adhesive layer 102 in a low-temperature bending test when the laminate 100 is bent so that the front panel 101 side is on the inside. Specifically, as shown in the examples described later, even when the laminate 100 is wrapped around a mandrel so that the front panel 101, which is on the inside when folded, is on the inside, left in an environment of -20°C for 24 hours, and taken out into an environment of 25°C, it can suppress the generation of bubbles in the first adhesive layer 102 and the occurrence of peeling between the first adhesive layer 102 and the front panel 101 (hereinafter, such performance is also referred to as excellent "low-temperature bending property"). When the laminate 100 is bent so that the front panel 101 side is on the inside and placed in a low-temperature environment, the first adhesive layer 102, which is located on the inside (closer to the core) of the second adhesive layer 104, is more likely to develop air bubbles or peeling off from adjacent layers than the second adhesive layer 104. However, by satisfying the above conditions, the occurrence of air bubbles in the first adhesive layer 102 or peeling off from adjacent layers can be suppressed.
[0022] In this embodiment, the stress reduction rate of the first adhesive layer 102 is preferably 45% or more and 65% or less, and even more preferably 50% or more and 60% or less, from the viewpoint of further improving the thermal shock bending resistance and low-temperature bending resistance when bending the front panel 101 side inward.
[0023] In this embodiment, it is preferable that the stress reduction rate R1 of the first adhesive layer 102 and the stress reduction rate R2 of the second adhesive layer 104 satisfy the relationship of the following formula (3). When R1 and R2 satisfy the relationship of the following formula (3), it is possible to further improve the thermal shock bending property and the low-temperature bending property when bending with the front panel 101 side on the inside. From the viewpoint of further enhancing the above effect, the value of R2-R1 may be 18 Pa or less, or may be 16 Pa or less. 0 Pa ≦ (R2-R1) ≦ 20 Pa … (3)
[0024] In the laminate 100, the stress reduction rate of the second pressure-sensitive adhesive layer 104 is not particularly limited as long as it satisfies the condition of the above formula (2), but is preferably 40% to 70%, more preferably 45% to 70%, and even more preferably 50% to 70%. When the stress reduction rate of the second pressure-sensitive adhesive layer 104 is within the above range, the generation of air bubbles in the first pressure-sensitive adhesive layer 102 and peeling from adjacent layers can be further suppressed in the thermal shock test and the low-temperature bending test.
[0025] Here, "bending" in this specification includes a folding form in which a curved surface is formed at the bent portion. In the folding form, the radius of curvature of the inner surface of the folded portion is not limited unless otherwise specified. In addition, "bending" includes a bending form in which the refraction angle of the inner surface is greater than 0 degrees and less than 180 degrees unless otherwise specified, and also includes a folding form in which the radius of curvature of the inner surface is close to zero or the refraction angle of the inner surface is 0 degrees.
[0026] The laminate 100 can be used in a laminate of a type in which the front panel 101 side is bent inward (so-called in-folding type), and a display device including the laminate (flexible display device). The laminate 100 can also be bent with the front panel 101 side facing outward. Therefore, the laminate 100 can be applied not only to a laminate that can be bent with the front panel 101 side facing inward, but also to a laminate that can be bent with the front panel 101 side facing outward, and a display device including the laminate.
[0027] The gel fraction of the pressure-sensitive adhesive layer can be from 40 to 90%, and may be from 50 to 80%.
[0028] The thickness of the pressure-sensitive adhesive layer is not particularly limited, but is preferably from 10 μm to 150 μm, more preferably from 10 μm to 100 μm, even more preferably from 15 μm to 80 μm, and particularly preferably from 20 μm to 75 μm.
[0029] It is preferable that the thickness T1 of the first adhesive layer 102 and the thickness T2 of the second adhesive layer 104 satisfy the relationship of the following formula (4). When T1 and T2 satisfy the relationship of the following formula (4), the thermal shock bending property and the low-temperature bending property can be further improved when bending with the front panel 101 side on the inside. From the viewpoint of further enhancing the above effect, the value of T1 / T2 may be 0.5 or more and 3.5 or less. 0.1≦(T1 / T2)≦4 …(4)
[0030] Here, examples of methods for preparing the first and second pressure-sensitive adhesive compositions constituting the first and second pressure-sensitive adhesive layers in this embodiment include a method of constituting them from a pressure-sensitive adhesive composition A described below, a method of changing the type of monomer constituting the (meth)acrylic polymer A described below, a method of adjusting the molecular weight of the (meth)acrylic polymer A, etc. The pressure-sensitive adhesive composition will be specifically described below.
[0031] <Adhesive composition A> The first pressure-sensitive adhesive layer 102 and the second pressure-sensitive adhesive layer 104 may have the same composition or different compositions, but each of them can be formed from a pressure-sensitive adhesive composition containing a (meth)acrylic polymer in one form (hereinafter also referred to as "pressure-sensitive adhesive composition A"). The pressure-sensitive adhesive composition A may be an active energy ray curable type or a heat curable type. In this specification, "(meth)acrylic polymer" refers to at least one selected from the group consisting of acrylic polymers and methacrylic polymers. The same applies to other terms with "(meth)". Regarding the first pressure-sensitive adhesive composition forming the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive composition forming the second pressure-sensitive adhesive layer, when both contain a (meth)acrylic polymer, the (meth)acrylic polymer may be the same or different. Hereinafter, the (meth)acrylic polymer contained in the pressure-sensitive adhesive composition A is also referred to as "(meth)acrylic polymer A".
[0032] The (meth)acrylic polymer A in this embodiment may contain a nitrogen atom-containing monomer as a monomer unit constituting the polymer. Examples of the nitrogen atom-containing monomer include a monomer having an amino group, a monomer having an amide group, and a monomer having a nitrogen-containing heterocycle. Among them, from the viewpoint of the bending durability of the obtained pressure-sensitive adhesive layer, a monomer having an amide group (amide group-containing monomer) is preferable. These may be used alone or in combination of two or more kinds. Note that the reactive functional group-containing monomer described below is excluded from the nitrogen atom-containing monomer referred to here.
[0033] Examples of the amide group-containing monomer include (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N-butyl(meth)acrylamide, N-dodecyl(meth)acrylamide, N-methylol(meth)acrylamide, N-methylolpropane(meth)acrylamide, alkoxyalkyl(meth)acrylamides such as N-methoxymethyl(meth)acrylamide and N-butoxymethyl(meth)acrylamide, etc. Among them, N-dodecyl(meth)acrylamide is preferred from the viewpoint of the bending durability of the obtained pressure-sensitive adhesive layer.
[0034] When the (meth)acrylic polymer A contains a nitrogen atom-containing monomer (particularly an amide group-containing monomer) as a monomer unit constituting the polymer, the content is preferably 20% by mass or more and 30% by mass or less, more preferably 22% by mass or more and 28% by mass or less, and even more preferably 24% by mass or more and 26% by mass or less, based on 100% by mass of all constituent units. By controlling the content of the constituent unit derived from the nitrogen atom-containing monomer, the stress reduction rate of the pressure-sensitive adhesive layer can be adjusted to a desired range. Specifically, by increasing the content of the constituent unit derived from the nitrogen atom-containing monomer, the flexibility of the pressure-sensitive adhesive layer can be reduced and the stress reduction rate can be increased.
[0035] The pressure-sensitive adhesive composition A preferably contains a fluorine atom-containing compound as an additive in addition to the (meth)acrylic polymer A. Examples of the fluorine atom-containing compound include 2,2,2-trifluoroethyl (meth)acrylate and 2,2,3,3-tetrafluoropropyl (meth)acrylate, and among them, 2,2,2-trifluoroethyl methacrylate and 2,2,3,3-tetrafluoropropyl acrylate are preferred from the viewpoint of improving the heat resistance of the resulting pressure-sensitive adhesive layer. These may be used alone or in combination of two or more.
[0036] When the pressure-sensitive adhesive composition A contains a fluorine atom-containing compound, the content is preferably 5 mass% or less, more preferably 4 mass% or less, and even more preferably 3 mass% or less, based on 100 mass% of the solid content of the pressure-sensitive adhesive composition A. The content of the fluorine atom-containing compound is preferably 1 mass% or more, based on 100 mass% of the solid content of the pressure-sensitive adhesive composition A. By controlling the content of the fluorine atom-containing compound, the heat resistance of the pressure-sensitive adhesive layer can be adjusted, and the bending durability of the laminate in a thermal shock test environment can be improved.
[0037] (Active energy ray-curable pressure-sensitive adhesive composition) When the adhesive composition A is an active energy ray curable adhesive composition, the content of the structural unit derived from a monomer having a reactive functional group in the (meth)acrylic polymer A contained in the adhesive composition A is preferably 1 mass% or less based on the total mass of the (meth)acrylic polymer A. Examples of the reactive functional group include a hydroxyl group, a carboxyl group, and an epoxy group. This tends to improve the flexibility of the adhesive layer and to easily suppress the generation of bubbles in the adhesive layer under a thermal shock test environment. In the (meth)acrylic polymer A, from the viewpoint of suppressing the generation of bubbles when bending, the content of the structural unit derived from a monomer having a reactive functional group is more preferably 0.01 mass% or less based on the total mass of the (meth)acrylic polymer A, and further preferably does not have a structural unit derived from a monomer having a reactive functional group, and particularly preferably does not have a hydroxyl group, a carboxyl group, or an epoxy group.
[0038] The (meth)acrylic polymer A may contain a structural unit derived from a (meth)acrylic monomer having a linear or branched alkyl group having 1 to 24 carbon atoms. The (meth)acrylic monomer having a linear or branched alkyl group having 1 to 24 carbon atoms may be, for example, a (meth)acrylic acid alkyl ester, and examples thereof include butyl (meth)acrylate, methyl (meth)acrylate, ethyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, lauryl (meth)acrylate, isooctyl (meth)acrylate, isodecyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and isobornyl (meth)acrylate. The (meth)acrylic polymer A may be a polymer or copolymer containing one or more of the above-mentioned (meth)acrylic acid alkyl esters as monomers.
[0039] The content of the (meth)acrylic polymer A in the pressure-sensitive adhesive composition A may be, for example, 50% by mass or more and 100% by mass or less, preferably 80% by mass or more and 99.5% by mass or less, and more preferably 90% by mass or more and 99% by mass or less, relative to 100% by mass of the solid content of the pressure-sensitive adhesive composition A.
[0040] The weight average molecular weight (Mw) of the (meth)acrylic polymer A may be, for example, from 100,000 to 2,000,000, and is preferably from 500,000 to 1,500,000 from the viewpoint of suppressing bubbles during bending. The weight average molecular weight in this specification can be determined based on a value calculated in terms of standard polystyrene measured by gel permeation chromatography (GPC) as described in the Examples section below.
[0041] The pressure-sensitive adhesive composition A may contain one or more (meth)acrylic polymers A. Furthermore, the pressure-sensitive adhesive composition A may contain only the (meth)acrylic polymer A as a constituent, or may further contain a crosslinking agent. Examples of the crosslinking agent include divalent or higher metal ions that form a carboxylate metal salt with a carboxyl group; polyamine compounds that form an amide bond with a carboxyl group; polyepoxy compounds or polyols that form an ester bond with a carboxyl group; and polyisocyanate compounds that form an amide bond with a carboxyl group. Among these, polyisocyanate compounds are preferred. When the pressure-sensitive adhesive composition A contains a crosslinking agent, the content of the crosslinking agent may be, for example, 5 parts by mass or less, preferably 3 parts by mass or less, more preferably 1 part by mass or less, and even more preferably 0.5 parts by mass or less, relative to 100 parts by mass of the (meth)acrylic polymer A. The pressure-sensitive adhesive composition A may not contain a crosslinking agent.
[0042] The active energy ray-curable pressure-sensitive adhesive composition is a pressure-sensitive adhesive composition that has the property of being cured by irradiation with active energy rays such as ultraviolet rays or electron beams, that has adhesiveness even before irradiation with active energy rays and can be adhered to an adherend such as a film, and that has the property of being cured by irradiation with active energy rays and allowing adjustment of adhesion, etc. The active energy ray-curable pressure-sensitive adhesive composition is preferably an ultraviolet ray-curable type.
[0043] When the pressure-sensitive adhesive composition A is an active energy ray-curable pressure-sensitive adhesive composition, the pressure-sensitive adhesive composition A may further contain an active energy ray-polymerizable compound, a photopolymerization initiator, a photosensitizer, and the like.
[0044] Examples of the active energy ray polymerizable compound include (meth)acrylic compounds such as (meth)acryloyloxy group-containing compounds. Examples of the (meth)acryloyloxy group-containing compound include (meth)acrylate monomers having at least one (meth)acryloyloxy group in the molecule; (meth)acrylate oligomers obtained by reacting two or more functional group-containing compounds and having at least two (meth)acryloyloxy groups in the molecule. The pressure-sensitive adhesive composition A can contain 0.1% by mass or more and 10% by mass or less of the active energy ray polymerizable compound relative to 100% by mass of the solid content of the pressure-sensitive adhesive composition A.
[0045] Examples of photopolymerization initiators include benzophenone, benzyl dimethyl ketal, and 1-hydroxycyclohexyl ketone. When the pressure-sensitive adhesive composition A contains a photopolymerization initiator, it may contain one or more kinds. When the pressure-sensitive adhesive composition A contains a photopolymerization initiator, the total content thereof may be, for example, 0.01% by mass or more and 1.0% by mass or less relative to 100% by mass of the solid content of the pressure-sensitive adhesive composition A.
[0046] The pressure-sensitive adhesive composition A may contain additives such as fine particles for imparting light scattering properties, beads (resin beads, glass beads, etc.), glass fibers, resins other than the base polymer, tackifiers, fillers (metal powders or other inorganic powders, etc.), antioxidants, UV absorbers, dyes, pigments, colorants, defoamers, corrosion inhibitors, etc. From the viewpoint of preventing the problem of reduced durability due to residual solvents, the pressure-sensitive adhesive composition A preferably does not contain an organic solvent.
[0047] When the pressure-sensitive adhesive layer is formed from the pressure-sensitive adhesive composition A, the pressure-sensitive adhesive layer can be formed by applying the pressure-sensitive adhesive composition A onto a substrate. When an active energy ray-curable pressure-sensitive adhesive composition is used, the formed pressure-sensitive adhesive layer can be irradiated with active energy rays to form a cured product having a desired degree of cure.
[0048] (Thermosetting adhesive composition) When the pressure-sensitive adhesive composition A is a thermosetting pressure-sensitive adhesive composition, the (meth)acrylic polymer A preferably contains, as monomer units constituting the polymer, a (meth)acrylic acid alkyl ester having an alkyl group with a carbon number of 2 to 20 and a monomer having a reactive functional group in the molecule (reactive functional group-containing monomer).When the pressure-sensitive adhesive composition A is a thermosetting pressure-sensitive adhesive composition, it preferably further contains a thermal crosslinking agent.
[0049] The (meth)acrylic polymer A can exhibit preferable adhesiveness by containing a (meth)acrylic acid alkyl ester having an alkyl group with 2 to 20 carbon atoms as a monomer unit constituting the polymer. The (meth)acrylic acid alkyl ester having an alkyl group with 2 to 20 carbon atoms preferably contains, for example, a (meth)acrylic acid alkyl ester (hereinafter sometimes referred to as a "low Tg alkyl acrylate") that, when formed into a homopolymer, has a Tg of -40°C or less. By containing the low Tg alkyl acrylate as a constituent monomer unit, the flexibility of the adhesive layer is improved, and thus the generation of bubbles during bending can be more easily suppressed.
[0050] Examples of low Tg alkyl acrylates include n-butyl acrylate (Tg-54°C), n-octyl acrylate (Tg-65°C), isooctyl acrylate (Tg-58°C), 2-ethylhexyl acrylate (Tg-70°C), isononyl acrylate (Tg-58°C), isodecyl acrylate (Tg-60°C), isodecyl methacrylate (Tg-41°C), n-lauryl methacrylate (Tg-65°C), tridecyl acrylate (Tg-55°C), and tridecyl methacrylate (Tg-40°C). Among them, the low Tg alkyl acrylate is more preferably one having a homopolymer Tg of -45°C or less, and particularly preferably one having a homopolymer Tg of -50°C or less. Specifically, n-butyl acrylate and 2-ethylhexyl acrylate are particularly preferred. These may be used alone or in combination of two or more.
[0051] The (meth)acrylic polymer A preferably contains low Tg alkyl acrylate as a monomer unit constituting the polymer in a lower limit of 85% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more.
[0052] Furthermore, the (meth)acrylic polymer A preferably contains the low Tg alkyl acrylate as a monomer unit constituting the polymer in an amount of 99.9% by mass or less, more preferably 99.5% by mass or less, and even more preferably 99% by mass or less. By containing 99.9% by mass or less of the low Tg alkyl acrylate, a suitable amount of other monomer components (particularly reactive functional group-containing monomers) can be introduced into the (meth)acrylic polymer A.
[0053] From the viewpoint of further achieving the effects of the present invention, it is preferable that the (meth)acrylic polymer A contains as little as possible a monomer having a glass transition temperature (Tg) of more than 0°C as a homopolymer (hereinafter, sometimes referred to as "hard monomer"). Specifically, the (meth)acrylic polymer A contains, as a monomer unit constituting the polymer, a hard monomer, the upper limit of which is preferably 15% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less. The hard monomer also includes a reactive functional group-containing monomer, which will be described later.
[0054] Examples of the hard monomer include methyl acrylate (Tg 10° C.), methyl methacrylate (Tg 105° C.), ethyl methacrylate (Tg 65° C.), n-butyl methacrylate (Tg 20° C.), isobutyl methacrylate (Tg 48° C.), t-butyl methacrylate (Tg 107° C.), n-stearyl acrylate (Tg 30° C.), n-stearyl methacrylate (Tg 38° C.), cyclohexyl acrylate (Tg 15° C.), cyclohexyl methacrylate (Tg 66° C.), phenoxyethyl acrylate (Tg 5° C.), meth ... Examples of such monomers include acrylic monomers such as phenoxyethyl acrylate (Tg 54° C.), benzyl methacrylate (Tg 54° C.), isobornyl acrylate (Tg 94° C.), isobornyl methacrylate (Tg 180° C.), acryloylmorpholine (Tg 145° C.), adamantyl acrylate (Tg 115° C.), adamantyl methacrylate (Tg 141° C.), acrylic acid (Tg 105° C.), dimethylacrylamide (Tg 89° C.), and acrylamide (Tg 165° C.), vinyl acetate (Tg 32° C.), and styrene (Tg 80° C.).
[0055] The (meth)acrylic polymer A contains a reactive functional group-containing monomer as a monomer unit constituting the polymer, and reacts with a thermal crosslinking agent described below via the reactive functional group derived from the reactive functional group-containing monomer, thereby forming a crosslinked structure (three-dimensional network structure) as a whole, and thus a pressure-sensitive adhesive having the desired cohesive strength can be obtained.
[0056] Preferred reactive functional group-containing monomers contained in the (meth)acrylic polymer A as monomer units constituting the polymer include monomers having a hydroxyl group in the molecule (hydroxyl group-containing monomers), monomers having a carboxyl group in the molecule (carboxyl group-containing monomers), monomers having an amino group in the molecule (amino group-containing monomers), etc. Among these, hydroxyl group-containing monomers are particularly preferred since many of them have a glass transition temperature (Tg) of 0°C or less.
[0057] Examples of hydroxyl group-containing monomers include (meth)acrylic acid hydroxyalkyl esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. Among them, from the viewpoints of glass transition temperature (Tg), reactivity of the hydroxyl group in the resulting (meth)acrylic polymer A with a thermal crosslinking agent, and copolymerizability with other monomers, at least one of 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 3-hydroxypropyl acrylate, and 4-hydroxybutyl acrylate is preferred. These may be used alone or in combination of two or more.
[0058] Examples of the carboxyl group-containing monomer include ethylenically unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, itaconic acid, citraconic acid, etc. These may be used alone or in combination of two or more kinds.
[0059] Examples of the amino group-containing monomer include aminoethyl (meth)acrylate, n-butylaminoethyl (meth)acrylate, etc. These may be used alone or in combination of two or more.
[0060] The (meth)acrylic polymer A preferably contains reactive functional group-containing monomers as monomer units constituting the polymer in an amount of 0.1% by mass or more as a lower limit, particularly preferably 0.5% by mass or more, and more preferably 1% by mass or more. The (meth)acrylic polymer A preferably contains reactive functional group-containing monomers in an amount of 10% by mass or less as an upper limit, particularly preferably 8% by mass or less, and more preferably 5% by mass or less. This tends to make it easier to suppress the generation of bubbles when bending.
[0061] The (meth)acrylic polymer A may not contain a carboxyl group-containing monomer, particularly acrylic acid, which is also a hard monomer, as a monomer unit constituting the polymer. Since a carboxyl group is an acid component, by not containing a carboxyl group-containing monomer, even if the target to which the pressure-sensitive adhesive is applied includes a transparent conductive film such as tin-doped indium oxide (ITO), a metal film, or a metal mesh, the acid-induced defects (corrosion, change in resistance, etc.) can be suppressed.
[0062] The (meth)acrylic polymer A may contain other monomers as monomer units constituting the polymer, if desired. The other monomers are preferably monomers that do not contain reactive functional groups so as not to interfere with the action of the reactive functional group-containing monomer. Examples of the other monomers include (meth)acrylic acid alkoxyalkyl esters such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate, as well as monomers having a glass transition temperature (Tg) as a homopolymer of more than -40°C and not more than 0°C (hereinafter sometimes referred to as "middle Tg alkyl acrylates"). Examples of the middle Tg alkyl acrylates include ethyl acrylate (Tg-20°C), isobutyl acrylate (Tg-26°C), 2-ethylhexyl methacrylate (Tg-10°C), n-lauryl acrylate (Tg-23°C), isostearyl acrylate (Tg-18°C), and the like. These may be used alone or in combination of two or more.
[0063] The polymerization mode of the (meth)acrylic polymer A may be a random copolymer or a block copolymer.
[0064] The lower limit of the weight average molecular weight of the (meth)acrylic polymer A is preferably 200,000 or more, particularly preferably 300,000 or more, and more preferably 400,000 or more. When the lower limit of the weight average molecular weight of the (meth)acrylic polymer A is above the above, problems such as bleeding of the adhesive are suppressed. The weight average molecular weight in this specification can be determined based on a value calculated in terms of standard polystyrene measured by gel permeation chromatography (GPC) as described in the Examples section below.
[0065] The upper limit of the weight average molecular weight of the (meth)acrylic polymer A is preferably not more than 2 million, particularly preferably not more than 1.5 million, and further preferably not more than 1.3 million. When the upper limit of the weight average molecular weight of the (meth)acrylic acid ester polymer (A) is the above-mentioned or less, the flexibility of the pressure-sensitive adhesive layer can be ensured, and therefore the effects of the present invention can be easily achieved.
[0066] In the pressure-sensitive adhesive composition A, the (meth)acrylic polymer A may be used either alone or in combination of two or more.
[0067] When the pressure-sensitive adhesive composition A containing the thermal crosslinking agent is heated, the thermal crosslinking agent crosslinks the (meth)acrylic polymer A to form a three-dimensional network structure, which improves the cohesive strength while maintaining the flexibility of the pressure-sensitive adhesive, and when applied to a laminate, can provide a hardness that can improve the surface hardness of the laminate.
[0068] The thermal crosslinking agent may be any one that reacts with the reactive group of the (meth)acrylic polymer A, and examples thereof include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, amine-based crosslinking agents, melamine-based crosslinking agents, aziridine-based crosslinking agents, hydrazine-based crosslinking agents, aldehyde-based crosslinking agents, oxazoline-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, and ammonium salt-based crosslinking agents. Among the above, when the reactive group of the (meth)acrylic polymer A is a hydroxyl group, it is preferable to use an isocyanate-based crosslinking agent that has excellent reactivity with the hydroxyl group. The thermal crosslinking agent may be used alone or in combination of two or more.
[0069] The isocyanate-based crosslinking agent contains at least a polyisocyanate compound. Examples of the polyisocyanate compound include aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, and xylylene diisocyanate, aliphatic polyisocyanates such as hexamethylene diisocyanate, alicyclic polyisocyanates such as isophorone diisocyanate and hydrogenated diphenylmethane diisocyanate, and their biuret and isocyanurate forms, as well as adducts which are reactants with low-molecular active hydrogen-containing compounds such as ethylene glycol, propylene glycol, neopentyl glycol, trimethylolpropane, and castor oil. Among these, trimethylolpropane-modified aromatic polyisocyanates, particularly trimethylolpropane-modified tolylene diisocyanate and trimethylolpropane-modified xylylene diisocyanate, are preferred from the viewpoint of reactivity with hydroxyl groups.
[0070] Examples of epoxy crosslinking agents include 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-m-xylylenediamine, ethylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane diglycidyl ether, diglycidyl aniline, and diglycidylamine.
[0071] The content of the thermal crosslinking agent in the pressure-sensitive adhesive composition A is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more, based on 100 parts by mass of the (meth)acrylic polymer A. Furthermore, the content is preferably 1 part by mass or less, more preferably 0.8 parts by mass or less, and even more preferably 0.5 parts by mass or less. By having the content of the thermal crosslinking agent in the above range, it is possible to more easily obtain an appropriate hardness by improving the cohesive force.
[0072] The pressure-sensitive adhesive composition A may contain a silane coupling agent, which improves the adhesion of the resulting pressure-sensitive adhesive layer to each member in the laminate that serves as the adherend, and improves durability against bending.
[0073] The silane coupling (SC) agent is preferably an organosilicon compound having at least one alkoxysilyl group in the molecule, which has good compatibility with the (meth)acrylic polymer A and has optical transparency.
[0074] Examples of the silane coupling agent include polymerizable unsaturated group-containing silicon compounds such as vinyltrimethoxysilane, vinyltriethoxysilane, and methacryloxypropyltrimethoxysilane; epoxy structure-containing silicon compounds such as 3-glycidoxypropyltrimethoxysilane and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; mercapto group-containing silicon compounds such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, and 3-mercaptopropyldimethoxymethylsilane; Examples of the silane include amino group-containing silicon compounds such as N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, and N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-chloropropyltrimethoxysilane, and 3-isocyanatepropyltriethoxysilane, and condensates of at least one of these with alkyl group-containing silicon compounds such as methyltriethoxysilane, ethyltriethoxysilane, methyltrimethoxysilane, and ethyltrimethoxysilane. These may be used alone or in combination of two or more.
[0075] The content of the silane coupling agent in the pressure-sensitive adhesive composition A is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more, based on 100 parts by mass of the (meth)acrylic polymer A. Furthermore, the content is preferably 1 part by mass or less, more preferably 0.5 parts by mass or less, and even more preferably 0.3 parts by mass or less. By having the content of the silane coupling agent in the above range, the adhesion between each member in the laminate can be further improved.
[0076] If desired, various additives may be added to the pressure-sensitive adhesive composition A. In this specification, the additives constituting the pressure-sensitive adhesive composition A do not include polymerization solvents and diluent solvents.
[0077] The (meth)acrylic polymer A can be produced by polymerizing a mixture of monomers constituting the polymer by a normal radical polymerization method. The polymerization of the (meth)acrylic polymer A is preferably carried out by a solution polymerization method using a polymerization initiator as desired. Examples of the polymerization solvent include ethyl acetate, n-butyl acetate, isobutyl acetate, toluene, acetone, hexane, and methyl ethyl ketone, and two or more of them may be used in combination.
[0078] Examples of the polymerization initiator include azo compounds and organic peroxides, and two or more of them may be used in combination. Examples of the azo compounds include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane 1-carbonitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethyl-4-methoxyvaleronitrile), dimethyl 2,2'-azobis(2-methylpropionate), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-hydroxymethylpropionitrile), and 2,2'-azobis[2-(2-imidazolin-2-yl)propane].
[0079] Examples of organic peroxides include benzoyl peroxide, t-butyl perbenzoate, cumene hydroperoxide, diisopropyl peroxydicarbonate, di-n-propyl peroxydicarbonate, di(2-ethoxyethyl)peroxydicarbonate, t-butyl peroxyneodecanoate, t-butyl peroxypivalate, (3,5,5-trimethylhexanoyl)peroxide, dipropionyl peroxide, and diacetyl peroxide.
[0080] In the above polymerization step, the weight average molecular weight of the resulting polymer can be adjusted by adding a chain transfer agent such as 2-mercaptoethanol.
[0081] When the (meth)acrylic polymer A is obtained, a thermal crosslinking agent, a silane coupling agent, and optionally an additive and a dilution solvent are added to the solution of the (meth)acrylic polymer A, and mixed thoroughly to obtain a solvent-diluted adhesive composition A (coating solution). The adhesive composition A can be produced by a known method, for example, by mixing the components together using a mixer or the like. Furthermore, the first adhesive composition and the second adhesive composition can be prepared from the adhesive composition A thus obtained.
[0082] When any of the above components is used in a solid state, or when precipitation occurs when the component is mixed with other components in an undiluted state, the component may be dissolved or diluted in a dilution solvent before being mixed with the other components.
[0083] Examples of the dilution solvent include aliphatic hydrocarbons such as hexane, heptane, and cyclohexane; aromatic hydrocarbons such as toluene and xylene; halogenated hydrocarbons such as methylene chloride and ethylene chloride; alcohols such as methanol, ethanol, propanol, butanol, and 1-methoxy-2-propanol; ketones such as acetone, methyl ethyl ketone, 2-pentanone, isophorone, and cyclohexanone; esters such as ethyl acetate and butyl acetate; and cellosolve-based solvents such as ethyl cellosolve.
[0084] The concentration and viscosity of the adhesive composition A (coating solution) thus prepared may be within a range that allows coating, and are not particularly limited, and may be appropriately selected depending on the situation. For example, the concentration of the adhesive composition A can be prepared to be 10 to 60 mass% in the solution. When obtaining the coating solution, the addition of a dilution solvent or the like is not a necessary condition, and if the adhesive composition A has a viscosity that allows coating, it is not necessary to add a dilution solvent. In this case, the adhesive composition A becomes a coating solution in which the polymerization solvent of the (meth)acrylic polymer A is used as the dilution solvent itself.
[0085] The pressure-sensitive adhesive layer can be obtained by crosslinking the pressure-sensitive adhesive composition A. The crosslinking of the pressure-sensitive adhesive composition A can be carried out by a heat treatment. The heat treatment can also serve as a drying treatment for volatilizing a diluting solvent and the like from a coating film of the pressure-sensitive adhesive composition A applied to a desired object.
[0086] The heating temperature in the heat treatment is preferably 50 to 150° C., and more preferably 70 to 120° C. The heating time in the heat treatment is preferably 10 seconds to 10 minutes, and more preferably 50 seconds to 2 minutes.
[0087] After the heat treatment, a curing period of about 1 to 2 weeks can be provided at room temperature (e.g., 23°C, 50% RH) as necessary. If this curing period is necessary, the adhesive layer can be formed after the curing period has elapsed. If no curing period is necessary, the adhesive layer can be formed after the above-mentioned heat treatment is completed.
[0088] Through the above-mentioned heating treatment (and curing), the (meth)acrylic polymer A is sufficiently crosslinked via the crosslinking agent to form a crosslinked structure, thereby obtaining the adhesive layer (first adhesive layer 102 and second adhesive layer 104).
[0089] <Adhesive sheet> The pressure-sensitive adhesive sheet may include a pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition A. The pressure-sensitive adhesive layer may be formed by applying the pressure-sensitive adhesive composition A onto a substrate. When an active energy ray-curable pressure-sensitive adhesive composition is used as the pressure-sensitive adhesive composition A, the formed pressure-sensitive adhesive layer may be irradiated with active energy rays to form a cured product having a desired degree of cure. When a heat-curable pressure-sensitive adhesive composition is used as the pressure-sensitive adhesive composition, the formed pressure-sensitive adhesive layer may be subjected to a heat treatment (and curing) to form a cured product having a desired degree of cure.
[0090] The substrate may be a release film that has been subjected to a release treatment. The pressure-sensitive adhesive sheet can be produced by forming a sheet-shaped pressure-sensitive adhesive layer by applying the pressure-sensitive adhesive composition A onto a release film, and then laminating another release film onto the pressure-sensitive adhesive layer.
[0091] The coating solution of the pressure-sensitive adhesive composition A can be applied by, for example, bar coating, knife coating, roll coating, blade coating, die coating, gravure coating, or the like.
[0092] <Front plate> The front panel 101 is not limited in material and thickness as long as it is a plate-like body that can transmit light, and may be composed of only one layer or two or more layers. Examples include a resin plate-like body (e.g., a resin plate, a resin sheet, a resin film, etc.), a glass plate-like body (e.g., a glass plate, a glass film, etc.), and a touch sensor panel described later. The front panel can be the outermost surface of the display device.
[0093] The thickness of the front panel 101 may be, for example, from 10 μm to 1000 μm, preferably from 20 μm to 500 μm, and more preferably from 30 μm to 300 μm. In the present invention, the thickness of each layer can be measured according to the thickness measurement method described in the examples below.
[0094] When the front panel 101 is a resin plate, the resin plate is not limited as long as it is light-transmitting. Examples of resins constituting a resin plate such as a resin film include films formed of polymers such as triacetyl cellulose, acetyl cellulose butyrate, ethylene-vinyl acetate copolymer, propionyl cellulose, butyryl cellulose, acetyl propionyl cellulose, polyester, polystyrene, polyamide, polyetherimide, poly(meth)acrylic, polyimide, polyethersulfone, polysulfone, polyethylene, polypropylene, polymethylpentene, polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, polyvinyl acetal, polyether ketone, polyether ether ketone, polyethersulfone, polymethyl methacrylate, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polycarbonate, and polyamideimide. These polymers can be used alone or in combination of two or more. From the viewpoint of improving strength and transparency, a resin film formed of a polymer such as polyimide, polyamide, or polyamideimide is preferable.
[0095] From the viewpoint of hardness, the front panel 101 is preferably a film having a hard coat layer provided on at least one side of the substrate film. As the substrate film, a film made of the above resin can be used. The hard coat layer may be formed on one side of the substrate film, or on both sides. By providing the hard coat layer, a resin film having improved hardness and scratch resistance can be obtained. The hard coat layer is, for example, a cured layer of an ultraviolet curing resin. Examples of the ultraviolet curing resin include acrylic resin, silicone resin, polyester resin, urethane resin, amide resin, and epoxy resin. The hard coat layer may contain an additive to improve strength. The additive is not limited, and examples thereof include inorganic fine particles, organic fine particles, and mixtures thereof.
[0096] When the front panel 101 is a glass plate, the glass plate is preferably a tempered glass for a display. The thickness of the glass plate may be, for example, 10 μm or more and 1000 μm or less, or 50 μm or more and 500 μm or less. By using a glass plate, the front panel 101 having excellent mechanical strength and surface hardness can be formed.
[0097] When the laminate 100 is used in a display device, the front panel 101 not only has the function of protecting the front surface (screen) of the display device (functioning as a window film), but may also have functions as a touch sensor, a blue light cut function, a viewing angle adjustment function, etc.
[0098] <First adhesive layer> The first adhesive layer 102 is a layer interposed between the front plate 101 and the polarizer layer 103 to bond them together, and may be, for example, a layer made of an adhesive or a layer obtained by performing some treatment on the layer. The first adhesive layer 102 may be an adhesive layer that is disposed closest to the front plate 101 among the adhesive layers that constitute the laminate 100. Here, in this specification, the term "adhesive" is also called a pressure-sensitive adhesive. Furthermore, in this specification, the term "adhesive" refers to an adhesive other than an adhesive (pressure-sensitive adhesive) and is clearly distinguished from an adhesive. The first adhesive layer 102 may be a single layer or may be composed of two or more layers, but is preferably a single layer.
[0099] The first adhesive layer 102 is formed using the first adhesive composition as described above. The first adhesive composition can be formed using the adhesive composition A as described above. The first adhesive layer 102 is a layer having a stress reduction rate of 40% or more and 70% or less, calculated by the above formula (1), and is a layer formed so that the stress reduction rate R1 of the first adhesive layer 102 and the stress reduction rate R2 of the second adhesive layer 104 satisfy the relationship of the above formula (2). As long as the above conditions are satisfied, the first adhesive composition is not limited to the adhesive composition A, and can be formed directly from any adhesive composition, or can be formed using an adhesive sheet having an adhesive layer formed using any adhesive composition. However, the first adhesive composition is preferably formed from the above adhesive composition A, or is also preferably formed using an adhesive sheet formed by applying the above adhesive composition A onto a substrate.
[0100] That is, the first adhesive layer 102 may be as described above in the section <Adhesive Layer (First Adhesive Layer and Second Adhesive Layer)> with respect to the composition and blended components of the first adhesive composition constituting it, the type of the first adhesive composition (active energy ray curable, heat curable, etc.), additives that may be blended into the first adhesive composition, the method for producing the first adhesive layer, and the thickness of the first adhesive layer, etc.
[0101] <Polarizer layer> Examples of the polarizer layer 103 include a stretched film or layer having a dichroic dye adsorbed thereon, and a layer formed by applying and curing a composition containing a dichroic dye and a polymerizable compound. Specific examples of the dichroic dye include iodine or a dichroic organic dye. Examples of the dichroic organic dye include dichroic direct dyes made of disazo compounds such as CIDIRECT RED 39, and dichroic direct dyes made of compounds such as trisazo and tetrakisazo.
[0102] Examples of the polarizer layer formed by applying and curing a composition containing a dichroic dye and a polymerizable compound include a polarizer layer containing a cured product of a polymerizable liquid crystal compound, such as a layer obtained by applying and curing a composition containing a dichroic dye having liquid crystal properties or a composition containing a dichroic dye and a polymerizable liquid crystal. A polarizer layer formed by applying and curing a composition containing a dichroic dye and a polymerizable compound is preferable because there is no restriction on the bending direction compared to a stretched film or stretched layer having a dichroic dye adsorbed thereon.
[0103] In the laminate 100, the polarizer layer 103 can function as a circular polarizer, for example, in combination with a retardation layer described later.
[0104] (Polarizer layer which is a stretched film or layer) The polarizer layer, which is a stretched film having a dichroic dye adsorbed thereon, can usually be produced through a process of uniaxially stretching a polyvinyl alcohol-based resin film, a process of dyeing the polyvinyl alcohol-based resin film with a dichroic dye to adsorb the dichroic dye, a process of treating the polyvinyl alcohol-based resin film having the dichroic dye adsorbed thereon with an aqueous boric acid solution, and a process of washing the film with water after the treatment with the aqueous boric acid solution. The thickness of the polarizer layer 103 is, for example, 2 μm or more and 40 μm or less. The thickness of the polarizer layer 103 may be 5 μm or more, 20 μm or less, further 15 μm or less, and further 10 μm or less.
[0105] Polyvinyl alcohol resins are obtained by saponifying polyvinyl acetate resins. Polyvinyl acetate resins include polyvinyl acetate, which is a homopolymer of vinyl acetate, and copolymers of vinyl acetate and other monomers that can be copolymerized with vinyl acetate. Examples of other monomers that can be copolymerized with vinyl acetate include unsaturated carboxylic acids, olefins, vinyl ethers, unsaturated sulfonic acids, and (meth)acrylamides having an ammonium group.
[0106] The degree of saponification of the polyvinyl alcohol resin is usually 85 mol% or more and 100 mol% or less, preferably 98 mol% or more. The polyvinyl alcohol resin may be modified, for example, polyvinyl formal or polyvinyl acetal modified with aldehydes can be used. The degree of polymerization of the polyvinyl alcohol resin is usually 1000 or more and 10000 or less, preferably 1500 or more and 5000 or less.
[0107] The polarizer layer, which is a stretched layer having a dichroic dye adsorbed thereon, can be produced by the steps of: applying a coating solution containing the polyvinyl alcohol resin onto a substrate film; uniaxially stretching the resulting laminated film; dyeing the polyvinyl alcohol resin layer of the uniaxially stretched laminated film with a dichroic dye to adsorb the dichroic dye to form a polarizer layer; treating the film having the dichroic dye adsorbed thereon with an aqueous boric acid solution; and washing the film with water after the treatment with the aqueous boric acid solution. The polarizer layer, which is a stretched layer having a dichroic dye adsorbed thereon, may be produced by peeling off the substrate film from the polarizer layer as necessary. The material and thickness of the substrate film may be the same as the material and thickness of the thermoplastic resin film described below.
[0108] The polarizer layer, which is a stretched film or layer, may be incorporated into the laminate in a form in which a thermoplastic resin film is attached to one or both sides of the polarizer layer. This thermoplastic resin film can function as a protective film or a retardation film for the polarizer layer 103. The thermoplastic resin film can be, for example, a film made of a polyolefin resin such as a chain polyolefin resin (such as a polypropylene resin) or a cyclic polyolefin resin (such as a norbornene resin); a cellulose resin such as triacetyl cellulose; a polyester resin such as polyethylene terephthalate, polyethylene naphthalate, or polybutylene terephthalate; a polycarbonate resin; a (meth)acrylic resin; or a mixture thereof.
[0109] The thermoplastic resin film may or may not have a phase difference. From the viewpoint of thinning, the thickness of the thermoplastic resin film is usually 300 μm or less, preferably 200 μm or less, more preferably 100 μm or less, even more preferably 80 μm or less, and even more preferably 60 μm or less. The thickness of the thermoplastic resin film is usually 5 μm or more, preferably 20 μm or more. The thermoplastic resin film can be attached to the polarizer layer 103 using, for example, an adhesive layer.
[0110] (Polarizer layer obtained by applying and curing a composition containing a dichroic dye and a polymerizable compound) Examples of polarizer layers formed by applying and curing a composition containing a dichroic dye and a polymerizable compound include polarizer layers containing a cured product of a polymerizable liquid crystal compound, such as a layer obtained by applying a composition containing a polymerizable dichroic dye having liquid crystal properties or a composition containing a dichroic dye and a polymerizable liquid crystal to a substrate film and curing the composition.
[0111] The polarizer layer formed by applying and curing a composition containing a dichroic dye and a polymerizable compound may have a substrate film peeled off from the polarizer layer as necessary. The material and thickness of the substrate film may be the same as those of the thermoplastic resin film described above. The polarizer layer may have an alignment film. The alignment film may be peeled off.
[0112] The polarizer layer formed by applying and curing a composition containing a dichroic dye and a polymerizable compound may be incorporated into an optical laminate in a form in which a thermoplastic resin film is attached to one or both sides of the polarizer layer. As the thermoplastic resin film, a thermoplastic resin film similar to that usable for the polarizer layer, which is a stretched film or layer, can be used. The thermoplastic resin film can be attached to the polarizer layer, for example, by using an adhesive layer.
[0113] The polarizer layer formed by applying and curing a composition containing a dichroic dye and a polymerizable compound may have an overcoat (OC) layer formed on one or both sides as a protective layer. Examples of the OC layer include a cured layer of a photocurable resin or a water-soluble polymer. Examples of the photocurable resin include a (meth)acrylic resin, a urethane resin, a (meth)acrylic urethane resin, an epoxy resin, and a silicone resin. Examples of the water-soluble polymer include a poly(meth)acrylamide polymer; polyvinyl alcohol, and a vinyl alcohol polymer such as an ethylene-vinyl alcohol copolymer, an ethylene-vinyl acetate copolymer, and a (meth)acrylic acid or its anhydride-vinyl alcohol copolymer; a carboxyvinyl polymer; polyvinylpyrrolidone; starches; sodium alginate; and a polyethylene oxide polymer. The thickness of the OC layer is preferably 20 μm or less, more preferably 15 μm or less, and even more preferably 10 μm or less, and may be 5 μm or less, or may be 0.05 μm or more, or may be 0.5 μm or more.
[0114] The thickness of the polarizer layer obtained by applying and curing a composition containing a dichroic dye and a polymerizable compound is usually 10 μm or less, preferably 0.5 μm or more and 8 μm or less, and more preferably 1 μm or more and 5 μm or less.
[0115] <Second adhesive layer> The second pressure-sensitive adhesive layer 104 is an adhesive layer disposed between the polarizer layer 103 and the back plate 105. The second pressure-sensitive adhesive layer can be an adhesive layer disposed closest to the back plate 105 among the adhesive layers constituting the laminate 100. The second pressure-sensitive adhesive layer 104 may be a single layer or may be composed of two or more layers, but is preferably a single layer.
[0116] The second adhesive layer 104 is formed using the second adhesive composition as described above. The second adhesive composition can be formed using the adhesive composition A as described above. The second adhesive layer 104 is a layer formed so that the stress reduction rate R1 of the first adhesive layer 102 and the stress reduction rate R2 of the second adhesive layer 104 satisfy the relationship of the above formula (2). As long as the above conditions are satisfied, the second adhesive composition is not limited to the adhesive composition A and can be formed directly from any adhesive composition, or can be formed using an adhesive sheet having an adhesive layer formed using any adhesive composition. However, the second adhesive composition is preferably formed from the above-mentioned adhesive composition A, or is also preferably formed using an adhesive sheet formed by applying the above-mentioned adhesive composition A onto a substrate.
[0117] That is, the second pressure-sensitive adhesive layer 104 may have the same composition as or different from the first pressure-sensitive adhesive layer 102, but is common in that it is preferably formed from pressure-sensitive adhesive composition A. For this reason, the second pressure-sensitive adhesive layer 104 may be as described above in the section <Pressure-sensitive adhesive layer (first pressure-sensitive adhesive layer and second pressure-sensitive adhesive layer)> with respect to the composition and blending components of the second pressure-sensitive adhesive composition constituting it, the type of the second pressure-sensitive adhesive composition (whether it is active energy ray curable or heat curable, etc.), additives that may be blended in the second pressure-sensitive adhesive composition, the method for producing the second pressure-sensitive adhesive layer, the thickness of the second pressure-sensitive adhesive layer, etc.
[0118] <Back plate> The back panel 105 may be a light-transmitting plate or a component used in a typical display device.
[0119] The thickness of rear panel 105 may be, for example, 5 μm or more and 2000 μm or less, preferably 10 μm or more and 1000 μm or less, and more preferably 15 μm or more and 500 μm or less.
[0120] The plate-like material used for rear panel 105 may be composed of only one layer, or may be composed of two or more layers, and the examples of the plate-like material described for front panel 101 can be used.
[0121] Examples of components used in a normal display device and used for rear panel 105 include a separator, a touch sensor panel, an organic EL display element, etc. Examples of the stacking order of components in a display device include front panel / circular polarizer / separator, front panel / circular polarizer / organic EL display device, front panel / circular polarizer / touch sensor panel / organic EL display element, front panel / touch sensor panel / circular polarizer / organic EL display element, etc. Rear panel 105 is preferably a touch sensor panel.
[0122] (Touch sensor panel) The touch sensor panel is not limited to a detection type as long as it has a sensor capable of detecting a touched position, and examples of such touch sensor panels include resistive film type, electrostatic capacitance coupling type, optical sensor type, ultrasonic type, electromagnetic induction coupling type, surface acoustic wave type, etc. Resistive film type and electrostatic capacitance coupling type touch sensor panels are preferably used because of their low cost.
[0123] An example of a resistive touch sensor panel is composed of a pair of substrates arranged opposite each other, an insulating spacer sandwiched between the pair of substrates, a transparent conductive film provided as a resistive film on the entire inner surface of each substrate, and a touch position detection circuit. In an image display device equipped with a resistive touch sensor panel, when the surface of the front panel is touched, the opposing resistive films are short-circuited and a current flows through the resistive films. The touch position detection circuit detects the voltage change at this time and detects the touched position.
[0124] An example of a capacitive touch sensor panel is composed of a substrate, a transparent electrode for position detection provided on the entire surface of the substrate, and a touch position detection circuit. In an image display device provided with a capacitive touch sensor panel, when the surface of the front panel is touched, the transparent electrode is grounded at the touched point via the electrostatic capacitance of the human body. The touch position detection circuit detects the grounding of the transparent electrode, and detects the touched position.
[0125] The thickness of the touch sensor panel may be, for example, 5 μm or more and 2000 μm or less, or may be 5 μm or more and 100 μm or less.
[0126] <Retardation layer> The laminate 100 can have one or more retardation layers between the polarizer layer 103 and the back plate 105. The retardation layer can be laminated on another layer (including another retardation layer) via the first adhesive layer 102, the second adhesive layer 104, or a layer made of an adhesive or bonding agent other than these layers (hereinafter also referred to as an attachment layer).
[0127] Examples of the retardation layer include positive A plates such as λ / 4 plates and λ / 2 plates, and positive C plates. The retardation layer may be a retardation film that can be formed from the above-mentioned thermoplastic resin film, or a layer formed by curing a polymerizable liquid crystal compound, that is, a layer containing a cured product of a polymerizable liquid crystal compound, but the latter is preferred. The thickness of the retardation film may be the same as that of the above-mentioned thermoplastic resin film. The thickness of the retardation layer formed by curing a polymerizable liquid crystal compound is, for example, 0.1 μm or more and 10 μm or less, preferably 0.5 μm or more and 8 μm or less, and more preferably 1 μm or more and 6 μm or less.
[0128] The retardation layer formed by curing a polymerizable liquid crystal compound can be formed by applying a composition containing a polymerizable liquid crystal compound to a substrate film and curing the composition. An alignment layer may be formed between the substrate film and the coating layer. The material and thickness of the substrate film may be the same as the material and thickness of the thermoplastic resin film described above. The retardation layer formed by curing a polymerizable liquid crystal compound may be incorporated into the laminate 100 in a form having an alignment layer and / or a substrate film. The back plate 105 may be a substrate film to which the composition is applied.
[0129] <Laminating layer> The attachment layer is a layer disposed between the first adhesive layer 102 and the second adhesive layer 104, and is a layer composed of an adhesive or a bonding agent. The adhesive constituting the attachment layer may be the same adhesive as those exemplified for the adhesive composition constituting the first adhesive layer 102 and the second adhesive layer 104, or may be another adhesive, such as a (meth)acrylic adhesive, a styrene adhesive, a silicone adhesive, a rubber adhesive, a urethane adhesive, a polyester adhesive, an epoxy copolymer adhesive, or the like.
[0130] The adhesive constituting the lamination layer can be formed by combining one or more of water-based adhesives, active energy ray curing adhesives, pressure sensitive adhesives, etc. Examples of water-based adhesives include polyvinyl alcohol resin aqueous solutions and water-based two-liquid urethane emulsion adhesives. Examples of active energy ray curing adhesives are adhesives that are cured by irradiation with active energy rays such as ultraviolet rays, and examples of such adhesives include those containing a polymerizable compound and a photopolymerization initiator, those containing a photoreactive resin, and those containing a binder resin and a photoreactive crosslinking agent. Examples of the polymerizable compound include photopolymerizable monomers such as photocurable epoxy monomers, photocurable acrylic monomers, and photocurable urethane monomers, and oligomers derived from these monomers. Examples of the photopolymerization initiator include those containing a substance that generates active species such as neutral radicals, anion radicals, and cation radicals when irradiated with active energy rays such as ultraviolet rays.
[0131] The thickness of the laminating layer may be, for example, 1 μm or more, preferably 1 μm or more and 25 μm or less, more preferably 2 μm or more and 15 μm or less, and further preferably 2.5 μm or more and 5 μm or less.
[0132] A laminate 200 according to another embodiment of the present invention includes a front plate 101, a first adhesive layer 102, a polarizer layer 103, a second adhesive layer 104, and a back plate 105, and may further include an attachment layer 108, a first retardation layer 106, an attachment layer 109, and a second retardation layer 107, as shown in FIG.
[0133] <Method of manufacturing laminate> The laminates 100 and 200 can be produced by a method including a step of bonding the layers constituting the laminates 100 and 200 together via a pressure-sensitive adhesive layer or, further, an adhesive layer. When bonding the layers together via a pressure-sensitive adhesive layer or an adhesive layer, it is preferable to subject one or both of the bonding surfaces to a surface activation treatment such as a corona treatment in order to enhance adhesion.
[0134] The polarizer layer 103 can be formed directly on a thermoplastic film or substrate film, which may be incorporated into the laminate 100, 200, or which may be peeled away from the polarizer layer 103 and not become a component of the laminate.
[0135] <Display device> A display device according to an embodiment of the present invention includes the laminate 100, 200. The display device is not particularly limited, and examples thereof include image display devices such as organic EL display devices, inorganic EL display devices, liquid crystal display devices, and electroluminescence display devices. The display device may have a touch panel function. The laminate 100, 200 has improved durability by suppressing the generation of bubbles in the adhesive layer, and is therefore suitable for a flexible display device that can be bent or folded.
[0136] In the display device, the laminate 100, 200 is disposed on the viewing side of the display element of the display device with the front plate facing outward (the side opposite to the display element, i.e., the viewing side). The display device is preferably bendable with the front plate 101 side of the laminate 100, 200 facing inward.
[0137] The display device according to the present invention can be used as mobile devices such as smartphones and tablets, televisions, digital photo frames, electronic signs, measuring instruments, gauges, office equipment, medical equipment, computing equipment, and the like. EXAMPLES
[0138] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In these examples, "%" and "parts" mean "% by mass" and "parts by mass", respectively, unless otherwise specified.
[0139] [Measurement of weight average molecular weight (Mw)] The weight average molecular weight (Mw) of the (meth)acrylic polymer described later was determined as the weight average molecular weight (Mw) converted to polystyrene by size exclusion chromatography (SEC) using tetrahydrofuran as the mobile phase. Specifically, the (meth)acrylic polymer to be measured was dissolved in tetrahydrofuran to a concentration of about 0.05% by mass, and 10 μL was injected into the SEC. The mobile phase was run at a flow rate of 1.0 mL / min. PLgel MIXED-B (manufactured by Polymer Laboratories) was used as the column. A UV-VIS detector (product name: Agilent GPC) was used as the detector.
[0140] [Thickness measurement] The thickness was measured using a contact type film thickness measuring device (product name "ZC-101", manufactured by Nikon Corporation).
[0141] [Measurement of bending stiffness] The laminates obtained in each Example and Comparative Example were left in an environment at -20°C for 24 hours, and then taken out into an environment at 25°C. Within 5 minutes, the bending stiffness was measured under a load of 25 g using a bending stiffness evaluation device (GURLEY STIFFNESS TESTER, manufactured by Kumagai Riki Kogyo Co., Ltd.).
[0142] [Strain Repeated Loading Test] A reference adhesive layer having a thickness of 150 μm was prepared by laminating the adhesive layer of the adhesive sheet described later. The adhesive layer of the adhesive sheet C7 had a thickness of 150 μm, so it was used as the reference adhesive layer without laminating it. Next, this reference adhesive layer was cut to a width of 20 mm and a length of 20 mm, and attached to the stage of a viscoelasticity measuring device (trade name "MCR-301", manufactured by Anton Paar), and the surface of the reference adhesive layer was attached to a measuring chip having a diameter of 8 mm. In this state, 0% strain and 400% strain were repeatedly applied under the conditions of normal force free and frequency of 1 Hz. The application of strain was performed under the temperature conditions that the reference adhesive layer was cooled to -20°C, then held at -20°C for 2 minutes, and then heated to 60°C at a heating rate of 10°C / min, and held at 60°C for 2 minutes, which was one cycle, and this operation was repeated 10 times in total. The temperature drop rate when moving to the next cycle was 10° C. / min. From the stress measured during the test, the stress reduction rate (unit: %) was calculated according to the following formula (1). Stress reduction rate=100-{(RB / RA)×100} …(1) [In formula (1), RA represents the stress (unit: Pa) when a 400% strain is applied to the adhesive layer at -20°C for the first time after the start of the strain cycle test, and RB represents the stress (unit: Pa) when a 400% strain is applied to the adhesive layer at 60°C for the last time in the 10th cycle of the strain cycle test.]
[0143] [Low temperature bending test] The laminates obtained in each Example and Comparative Example were cut into a width of 10 mm and a length of 100 mm using a super cutter to prepare test pieces. Using a bending resistance tester (cylindrical mandrel method) manufactured by TP Giken Co., Ltd., the test pieces were wound around a cylindrical mandrel so that the front panel side of the test pieces was on the inside. In this state, the test pieces were left in an environment at a temperature of -20°C for 24 hours, and within 5 minutes after being taken out to an environment at 25°C, the test pieces were checked for the presence or absence of bubbles in the first and second adhesive layers, and for the presence or absence of peeling between the first adhesive layer and the front layer and the second adhesive layer and the back layer.
[0144] The above operation was carried out with the mandrel diameter varied between 30 mm, 20 mm, 15 mm, 10 mm, and 5 mm, and the minimum diameter of the mandrel was determined when no air bubbles were generated in the first and second adhesive layers, and no peeling occurred between the first adhesive layer and the front layer, and between the second adhesive layer and the back layer, and the evaluation was carried out according to the following criteria. In the low-temperature bending test, the smaller the determined minimum diameter of the mandrel, the better the low-temperature bending property of the laminate. In all test pieces, air bubbles or peeling from the adjacent layer occurred only in the first adhesive layer. A: The minimum diameter of the mandrel determined was 10 mm or less. B: The minimum diameter of the mandrel was determined to be 15 mm. C: The minimum diameter of the determined mandrel was 20 mm or more.
[0145] [Thermal shock bending test] The laminate obtained in each Example and Comparative Example was cut into a width of 10 mm x length of 100 mm using a super cutter to prepare a test specimen. Using a bending resistance tester (cylindrical mandrel method) manufactured by TP Giken Co., Ltd., the test specimen was wound around a cylindrical mandrel so that the front panel side of the test specimen was on the inside. In this state, the test specimen was held in an environment at a temperature of -20°C for 2 minutes, and then the environmental temperature was raised to 60°C at a heating rate of 10°C / min, and the test specimen was held in an environment at 60°C for 2 minutes. This operation constituted one cycle, and was repeated for a total of 10 cycles. The temperature drop rate when moving to the next cycle was 10°C / min. After the 10 cycles, the test specimen was taken out into an environment at 25°C, and within 5 minutes, the presence or absence of bubbles in the first adhesive layer and the second adhesive layer of the test specimen, and the presence or absence of peeling between the first adhesive layer and the front layer and the second adhesive layer and the back layer were confirmed.
[0146] The above operation was carried out by changing the diameter of the mandrel between 30 mm, 20 mm, 15 mm, 10 mm, and 5 mmm, and the minimum diameter of the mandrel was determined when no air bubbles were generated in the first and second adhesive layers, and no peeling occurred between the first adhesive layer and the front layer, and between the second adhesive layer and the back layer, and the evaluation was carried out according to the following criteria. In the impact bending resistance test, the smaller the determined minimum diameter of the mandrel, the better the thermal shock bending resistance of the laminate. In all test pieces, air bubbles or peeling from the adjacent layer occurred only in the first adhesive layer. A: The minimum diameter of the mandrel determined was 10 mm or less. B: The minimum diameter of the mandrel was determined to be 15 mm. C: The minimum diameter of the determined mandrel was 20 mm or more.
[0147] <Preparation of (Meth)acrylic Polymers A1 to A10> A 1L reactor equipped with a cooling device was prepared. A mixture of the monomer components shown in Table 1 in the amounts shown in Table 1 was added to this reactor while flowing nitrogen gas. Next, while stirring the mixture, nitrogen gas was refluxed in the reactor for 1 hour to remove oxygen, and then the temperature of the mixture was raised to 60°C. After the mixture was mixed uniformly while maintaining the temperature at 60°C, the polymerization initiator shown in Table 1 was added in the amounts shown in Table 1, and the mixture was irradiated with a UV lamp (10mW) while stirring to cause a polymerization reaction to proceed, thereby obtaining (meth)acrylic polymers A1 to A10. The amounts shown in Table 1 indicate the mass ratios (mass%) based on the total mass of the monomer components and the photopolymerization initiator. The weight average molecular weights (Mw) of the (meth)acrylic polymers A1 to A10 are shown in Table 1.
[0148] [Table 1]
[0149] <Preparation of Pressure-Sensitive Adhesive Compositions B1 to B10> Pressure-sensitive adhesive compositions B1 to B10 were obtained by mixing the (meth)acrylic polymers A1 to A10, monomer components, fluorine atom-containing compounds, and photopolymerization initiators shown in Table 2 in the amounts shown in Table 2. The amounts shown in Table 2 indicate mass percentages (mass%) based on the total mass of the (meth)acrylic polymers, monomer components, fluorine atom-containing compounds, and photopolymerization initiators.
[0150] [Table 2]
[0151] The abbreviations in Tables 1 and 2 are as follows. (Monomer component) BA: butyl acrylate (obtained from Tokyo Chemical Industry Co., Ltd.) n-DAM: N-dodecylacrylamide (nitrogen atom-containing monomer, obtained from Tokyo Chemical Industry Co., Ltd.) 4-HBA: 4-hydroxybutyl acrylate (obtained from Tokyo Chemical Industry Co., Ltd.) MA: Methyl acrylate (obtained from Tokyo Chemical Industry Co., Ltd.) IBOA: isobornyl acrylate (obtained from Tokyo Chemical Industry Co., Ltd.) LA: lauryl acrylate (obtained from Tokyo Chemical Industry Co., Ltd.) 2-PEA: 2-phenoxyethyl acrylate (obtained from Tokyo Chemical Industry Co., Ltd.) C22A: Behenyl acrylate (obtained from Tokyo Chemical Industry Co., Ltd.) n-OA: n-octyl acrylate (obtained from Tokyo Chemical Industry Co., Ltd.) 2-EHA: 2-ethylhexyl acrylate (obtained from Tokyo Chemical Industry Co., Ltd.) IDA: isodecyl acrylate (obtained from Tokyo Chemical Industry Co., Ltd.) (Fluorine atom-containing compounds) TFEA: 2,2,2-trifluoroethyl acrylate (obtained from Tokyo Chemical Industry Co., Ltd.) (Photopolymerization initiator) I-184: 1-Hydroxycyclohexyl phenyl ketone (obtained from Tokyo Chemical Industry Co., Ltd.)
[0152] <Preparation of adhesive sheets C1 to C10> The adhesive composition shown in Table 3 was applied to the release-treated surface of release film A (polyethylene terephthalate film coated with a release agent containing a silicone compound) so that the thickness of the adhesive layer was as shown in Table 3. Release film B (polyethylene terephthalate film coated with a release agent containing a silicone compound) was laminated on the coating layer so that the release-treated surface side was the coating layer side, and then UV irradiation was performed to obtain adhesive sheets C1 to C10 having a layer structure of release film A / adhesive layer / release film B. The UV irradiation was performed with an integrated light amount of 400 mJ / cm. 2 , illuminance is 1.8mW / cm 2 (UVV standard). A strain repetition test was carried out using the pressure-sensitive adhesive layers of the obtained pressure-sensitive adhesive sheets C1 to C10, and the stress reduction rate was measured. The measurement results are shown in Table 3.
[0153] [Table 3]
[0154] [Examples 1-2 and Comparative Example 2] (Preparation of front layer (1)) A front panel was prepared as the front layer (1), in which a hard coat layer (thickness 10 μm) was formed on one side of a resin film (polyimide resin film, thickness 40 μm) as a first base layer. The hard coat layer was a layer formed from a composition containing an acrylic compound having a dendrimer structure with a polyfunctional acrylic group at the end.
[0155] (Preparation of Circular Polarizing Plate (1)) A protective film (cycloolefin resin film, thickness 18 μm) as a protective layer and a linear polarizing layer (thickness 8 μm) were bonded together using a water-based adhesive to obtain a linear polarizing plate (1) having a layer structure of protective layer / adhesive layer / linear polarizing layer.
[0156] Next, a retardation laminate (1) was obtained in which a first retardation layer (thickness 3 μm), an adhesive layer (thickness 1 μm), and a second retardation layer (thickness 2 μm) were laminated in this order. The first retardation layer was a λ / 4 retardation layer, and was a cured layer of a polymerizable liquid crystal compound. The adhesive layer was a cured layer of an epoxy adhesive, which is a photocurable adhesive composition. The second retardation layer was a positive C layer, and was a cured layer of a polymerizable liquid crystal compound.
[0157] The linear polarizing layer side of the linear polarizing plate (1) obtained above and the first retardation layer side of the retardation laminate (1) were bonded together using an attachment layer (an adhesive layer using an acrylic adhesive, thickness 5 μm) to obtain a circular polarizing plate (1) as a polarizing plate. The layer structure of the circular polarizing plate (1) was linear polarizing plate (1) (protective layer / adhesive layer / linear polarizing layer) / attachment layer / retardation laminate (1) (first retardation layer / adhesive layer / second retardation layer).
[0158] (Preparation of Laminate) The first base layer (resin film) side of the front layer (1) obtained above and the linear polarizing plate (1) side of the circular polarizing plate (1) were bonded together using the first adhesive layer shown in Table 4, and the second adhesive layer and a separator (50 μm) as a back layer shown in Table 4 were laminated on the retardation laminate (1) side of the circular polarizing plate to produce laminates of Examples 1 to 2 and Comparative Example 2. The layer structure of these laminates was front layer (1) (hard coat layer / first base layer) / first adhesive layer / linear polarizing plate (1) (protective layer / adhesive layer / linear polarizing layer) / attaching layer / retardation laminate (1) (first retardation layer / adhesive layer / second retardation layer) / second adhesive layer / back layer. The obtained laminates were subjected to bending stiffness measurement, low-temperature bending test, and thermal shock bending test. The results are shown in Table 4.
[0159] [Example 3 and Comparative Example 1] (Preparation of circular polarizing plate (2)) A retardation laminate (2) was obtained in which a first retardation layer (thickness 2 μm), an adhesive layer (thickness 2 μm), and a second retardation layer (thickness 1 μm) were laminated in this order. The first retardation layer was a λ / 2 retardation layer, and was a cured layer of a polymerizable liquid crystal compound. The adhesive layer was a cured layer of an epoxy adhesive, which is a photocurable adhesive composition. The second retardation layer was a λ / 4 retardation layer, and was a cured layer of a polymerizable liquid crystal compound.
[0160] The linear polarizing layer side of the linear polarizing plate (1) obtained by the procedure described in Example 1 and the first retardation layer side of the retardation laminate (2) obtained above were bonded together using an attachment layer (an adhesive layer using an acrylic adhesive, thickness 5 μm) to obtain a circular polarizing plate (2) as a polarizing plate. The layer structure of the circular polarizing plate (2) was linear polarizing plate (1) (protective layer / adhesive layer / linear polarizing layer) / attachment layer / retardation laminate (2) (first retardation layer / adhesive layer / second retardation layer).
[0161] (Preparation of Laminate) The first base layer (resin film) side of the front layer (1) obtained by the procedure described in Example 1 and the linear polarizing plate (1) side of the circular polarizing plate (2) were bonded together using the first adhesive layer shown in Table 4, and the second adhesive layer shown in Table 4 and a separator (thickness 50 μm) as a back layer were laminated on the retardation laminate (2) side of the circular polarizing plate to produce laminates of Example 3 and Comparative Example 1. The layer structure of these laminates was front layer (1) (hard coat layer / first base layer) / first adhesive layer / linear polarizing plate (1) (protective layer / adhesive layer / linear polarizing layer) / attaching layer / retardation laminate (2) (first retardation layer / adhesive layer / second retardation layer) / second adhesive layer / back layer. The obtained laminates were subjected to bending stiffness measurement, low-temperature bending test, and thermal shock bending test. The results are shown in Table 4.
[0162] [Examples 4 to 6] (Preparation of front layer (2)) A front panel was prepared as the front layer (2), in which a hard coat layer (thickness 5 μm) was formed on one side of a resin film (polyimide resin film, thickness 40 μm) as a first base layer. The hard coat layer was a layer formed from a composition containing an acrylic compound having a dendrimer structure with a polyfunctional acrylic group at the end.
[0163] (Preparation of circular polarizing plate (3)) According to the procedure of [Preparation of Linear Polarizing Plate B] in the example of JP 2022-185418 A, a linear polarizing plate (2) having a hard coat layer as a protective layer, a linear polarizing layer which is a cured layer of a polymerizable liquid crystal compound, and an overcoat layer as a protective layer was prepared. The layer structure of the linear polarizing plate (2) was a protective layer (hard coat layer) / alignment film / linear polarizing layer / protective layer (overcoat layer).
[0164] The protective layer (overcoat layer) side of the linear polarizing plate (2) obtained above and the first retardation layer side of the retardation laminate (1) obtained by the procedure described in Example 1 were bonded together using an attachment layer (an adhesive layer using an acrylic adhesive, thickness 5 μm) to obtain a circular polarizing plate (3) as a polarizing plate. The layer structure of the circular polarizing plate (3) was linear polarizing plate (2) (protective layer (hard coat layer) / alignment film / linear polarizing layer / protective layer (overcoat layer)) / attachment layer / retardation laminate (1) (first retardation layer / adhesive layer / second retardation layer).
[0165] (Preparation of Laminate) The first base layer (resin film) side of the front layer (2) obtained above and the linear polarizing plate (2) side of the circular polarizing plate (3) were bonded together using the first adhesive layer shown in Table 4, and the second adhesive layer shown in Table 4 and a separator (thickness 50 μm) as a back layer were laminated on the retardation laminate (1) side of the circular polarizing plate to produce laminates of Examples 4 to 6. The layer structure of these laminates was front layer (2) (hard coat layer / first base layer) / first adhesive layer / linear polarizing plate (2) (protective layer (hard coat layer) / alignment film / linear polarizing layer / protective layer (overcoat layer)) / attachment layer / retardation laminate (1) (first retardation layer / adhesive layer / second retardation layer) / second adhesive layer / back layer. The obtained laminates were subjected to bending stiffness measurement, low-temperature bending test, and thermal shock bending test. The results are shown in Table 4.
[0166] [Table 4] [Explanation of symbols]
[0167] 100,200... Laminate, 101... Front plate, 102... First adhesive layer, 103... Polarizer layer, 104... Second adhesive layer, 105... Back plate, 106... First retardation layer, 107... Second retardation layer, 108,109... Lamination layer.
Claims
1. A laminate including, in this order, a front plate, a first pressure-sensitive adhesive layer, a polarizer layer, a second pressure-sensitive adhesive layer, and a back plate, the stress reduction rate of the first pressure-sensitive adhesive layer calculated by the following formula (1) is 40% or more and 70% or less, A laminate, wherein a stress reduction rate R1 of the first pressure-sensitive adhesive layer and a stress reduction rate R2 of the second pressure-sensitive adhesive layer satisfy the relationship of the following formula (2). Stress reduction rate=100-{(RB / RA)×100}...(1) R1≦R2 (2) [In formula (1), RA represents the stress (unit: Pa) when a 400% strain is applied to the adhesive layer at −20° C. for the first time after the start of the strain cycle test, and RB represents the stress (unit: Pa) when a 400% strain is applied to the adhesive layer at 60° C. for the last time in the 10th cycle of the strain cycle test.] [Strain Repeated Loading Test] The repeated strain application test is performed by adhering an adhesive layer adjusted to a thickness of 150 μm to a measurement chip of a viscoelasticity measuring device, and repeatedly applying 0% strain and 400% strain under normal force free conditions and a frequency of 1 Hz while maintaining the temperature at -20°C for 2 minutes, and then heating the temperature to 60°C at a heating rate of 10°C / min and maintaining the temperature for 2 minutes, with this cycle being repeated a total of 10 cycles.
2. 2. The laminate according to claim 1, wherein the bending stiffness of the laminate at a temperature of -20°C is 1000 gf·m or more and 2000 gf·m or less.
3. The laminate according to claim 1 , wherein the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer each have a thickness of 10 μm or more and 100 μm or less.
4. The laminate according to claim 1 , wherein the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer are both layers formed from a pressure-sensitive adhesive composition containing a (meth)acrylic polymer.
5. The laminate according to claim 4 , wherein the (meth)acrylic polymer contains 20% by mass or more and 30% by mass or less of a constituent unit derived from a nitrogen atom-containing monomer based on the total amount of the constituent units.
6. the first pressure-sensitive adhesive layer is a layer formed from a first pressure-sensitive adhesive composition containing a fluorine atom-containing compound, The laminate according to claim 1 , wherein the content of the fluorine atom-containing compound is 5 mass % or less based on the total solid content of the first pressure-sensitive adhesive composition.
7. The laminate according to claim 1 , wherein a stress reduction rate R1 of the first pressure-sensitive adhesive layer and a stress reduction rate R2 of the second pressure-sensitive adhesive layer satisfy the relationship of the following formula (3). 0Pa≦(R2-R1)≦20Pa...(3)
8. The laminate according to claim 1 , wherein the stress reduction rate of the second pressure-sensitive adhesive layer is 40% or more and 70% or less.
9. The laminate according to claim 1 , wherein a thickness T1 of the first pressure-sensitive adhesive layer and a thickness T2 of the second pressure-sensitive adhesive layer satisfy the relationship of the following formula (4). 0.1≦(T1 / T2)≦4…(4)
10. A display device comprising the laminate according to any one of claims 1 to 9.
11. An adhesive layer disposed between a front plate and a polarizer layer of a flexible display device, A pressure-sensitive adhesive layer having a stress reduction rate calculated by the following formula (1) of 40% or more and 70% or less. Stress reduction rate=100-{(RB / RA)×100}...(1) [In formula (1), RA represents the stress (unit: Pa) when a 400% strain is applied to the adhesive layer at −20° C. for the first time after the start of the strain cycle test, and RB represents the stress (unit: Pa) when a 400% strain is applied to the adhesive layer at 60° C. for the last time in the 10th cycle of the strain cycle test.] [Strain Repeated Loading Test] The repeated strain application test is performed by adhering an adhesive layer adjusted to a thickness of 150 μm to a measurement chip of a viscoelasticity measuring device, and repeatedly applying 0% strain and 400% strain under normal force free conditions and a frequency of 1 Hz while maintaining the temperature at -20°C for 2 minutes, and then heating the temperature to 60°C at a heating rate of 10°C / min and maintaining the temperature for 2 minutes, with this cycle being repeated a total of 10 cycles.
Citation Information
Patent Citations
Pressure sensitive adhesive and pressure sensitive adhesive film
JP2017082166A
Adhesive tape and double-sided adhesive tape for fixing abrasive material
JP2018002999A
Tackifier resin, acrylic adhesive and adhesive tape
JP2019085572A
Optical laminate and display device
JP2020060708A
Laminate and display device comprising the same
JP2020154308A