Polymer-attached particle, target substance detection reagent, target substance detection kit, and method for detecting target substance

Surface-modified polymer-coated particles address the sensitivity limitations of latex immunoagglutination by enhancing adhesion and dispersibility, leading to improved target substance detection accuracy.

JP2024143335AInactive Publication Date: 2024-10-11SUMITOMO BAKELITE CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023055956
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The sensitivity of latex particles used in latex immunoagglutination methods for target substance detection is limited, necessitating improvements for more accurate and sensitive detection.

Method used

Surface-treating core particles with a surface-modified polymer to form polymer-coated particles, ensuring a specific amount of reactive functional groups for enhanced adhesion, within a predetermined range, to improve detection sensitivity.

Benefits of technology

The polymer-coated particles enhance detection sensitivity by promoting target substance aggregation while maintaining dispersibility, thereby improving the accuracy of target substance detection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143335000001_ABST
    Figure 2024143335000001_ABST
Patent Text Reader

Abstract

To provide a polymer-attached particle that excels in sensitivity.SOLUTION: A polymer-attached particle according to the present invention includes a core particle, and a surface-modified polymer formed on at least a portion of the surface of the core particle. The surface-modified polymer includes a structural unit A1 including a reactive functional group (A1) capable of binding to a ligand that has the ability to specifically bind to a target substance. The coating weight of the surface-modified polymer in the polymer-attached particle is 0.01 mg or greater per 1 mg of the polymer-attached particle.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polymer-attached particle, a target substance detection reagent, a target substance detection kit, and a method for detecting a target substance. [Background technology]

[0002] The latex immunoagglutination method is known as a method for measuring a target substance in a sample. The latex immunoagglutination method is a measurement method in which, for example, latex particles carrying antibodies against a target substance are used, and the degree of agglutination (turbidity) of the latex particles caused by binding between the target substance, an antigen, and the antibody-carrying latex particles is detected by optical means or the like. Known examples of this type of technology include the technology described in Patent Document 1. Patent Document 1 describes a reagent for measuring a target substance in a sample using a latex immunoagglutination method, which includes latex particles carrying an antibody that specifically recognizes the target substance in the sample (e.g., claim 7 of Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2021-162593 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, as a result of investigations conducted by the present inventors, it was found that the latex particles described in Patent Document 1 above leave room for improvement in terms of sensitivity. [Means for solving the problem]

[0005] After further investigation, the inventors found that the sensitivity of detecting the aggregation of polymer-attached particles can be improved by surface-treating the surface of core particles such as latex particles with a surface-modifying polymer to form polymer-attached particles, and then setting the amount of attached surface-modifying polymer calculated using infrared absorption spectroscopy to a predetermined amount or more, thereby completing the present invention.

[0006] According to one aspect of the present invention, there are provided the following polymer-attached particles, target substance detection reagent, target substance detection kit, and target substance detection method. 1. A polymer-attached particle comprising a core particle and a surface-modifying polymer formed on at least a portion of the surface of the core particle, The surface-modifying polymer includes a structural unit A1 including a reactive functional group (A1) capable of binding to a ligand having specific binding ability to a target substance, A polymer-attached particle, in which the amount of the surface-modifying polymer attached to the polymer-attached particle, as measured according to the procedure described below, is 0.01 mg or more per 1 mg of the polymer-attached particle. (procedure) The infrared absorption spectrum of the polymer-attached particles is obtained by infrared spectroscopy. From the obtained infrared absorption spectrum, the peak area of ​​the absorption peak derived from a predetermined functional group of the surface-modified polymer is calculated. Based on a calibration curve prepared in advance, the adhesion amount (mg) of the surface modifying polymer is calculated from the obtained peak area. 2. The polymer-attached particles according to 1., The amount of the surface-modifying polymer attached to the particles is 0.3 mg or less per 1 mg of the particles. 3. The polymer-attached particle according to 1. or 2., The reactive functional group (A1) includes one or more groups selected from the group consisting of a carboxy group, a phenolic hydroxy group, an amino group, a thiol group, an epoxy group, a maleimide group, an acryl group, a methacryl group, and an acid anhydride group. 4. A polymer-attached particle according to any one of 1. to 3., The surface-modifying polymer comprises a structural unit A2 containing a salt formed by an acidic functional group (A2) and an organic base, the polymer-attached particle comprising the structural unit A2. 5. The polymer-attached particles according to 4., The acidic functional group (A2) includes one or more groups selected from the group consisting of a carboxy group, a sulfo group, a phosphate group, and a hydroxyl group. 6. A polymer-attached particle according to any one of 1. to 5., The organic base comprises a nitrogen-containing base and / or a phosphorus-containing base. 7. The polymer-attached particle according to 4, The surface-modifying polymer has a weight average molecular weight of 1,000 or more and 10,000,000 or less. 8. A polymer-attached particle according to any one of 1. to 7., The polymer-attached particle, wherein the core particle is an organic particle or an inorganic particle. 9. A polymer-attached particle according to any one of 1. to 8., A polymer-attached particle comprising the ligand bonded to at least a portion of the plurality of reactive functional groups (A1). 10. A polymer-attached particle according to any one of 1. to 9., The polymer-attached particle, wherein the ligand is any one of an antibody, an antigen, a protein, and a nucleic acid. 11. A polymer-attached particle according to any one of 1. to 10., The polymer-attached particles are used for detecting the target substance by an agglutination method. 12. A target substance detection reagent comprising a polymer-attached particle according to any one of 1. to 11. and a dispersion medium. 13. A target substance detection kit comprising a reagent container containing the target substance detection reagent described in 12. 14. A method for detecting a target substance, comprising the step of mixing a target substance with the target substance detection reagent described in 12. Effect of the Invention

[0007] According to the present invention, there are provided polymer-attached particles having excellent sensitivity, and a target substance detection reagent, a target substance detection kit, and a target substance detection method using the same. [Brief description of the drawings]

[0008] [Figure 1] FIG. 2 is a cross-sectional view illustrating an example of the configuration of a polymer-attached particle according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In all drawings, similar components are given similar reference numerals and their explanations will be omitted as appropriate. Also, the drawings are schematic diagrams and do not correspond to the actual dimensional ratios.

[0010] The polymer-attached particles of this embodiment will be outlined below.

[0011] The polymer-attached particle of this embodiment includes a core particle and a surface-modifying polymer formed on at least a part of the surface of the core particle. The surface-modifying polymer formed on the surface of the polymer-attached particle includes a structural unit A1 including a reactive functional group (A1) capable of binding to a ligand having specific binding ability to a target substance. In such a polymer-attached particle, the amount of the surface-modifying polymer attached to the polymer-attached particle, measured according to the procedure described below, is configured to be 0.01 mg or more per 1 mg of the polymer-attached particle.

[0012] In this embodiment, the lower limit of the amount of the surface-modifying polymer attached is 0.01 mg or more, preferably 0.02 mg or more, and more preferably 0.05 mg or more per 1 mg of the polymer-attached particles, which can improve the coagulation properties of the polymer-attached particles. Although the detailed mechanism is unclear, it is believed that the polymer-attached particles, in which the above-mentioned surface-modifying polymer has been introduced onto the surface of the core particle, contain a predetermined or greater amount of reactive functional groups (A1) and ligand bonds, which promotes aggregation in a dispersion medium containing a target substance, thereby improving the sensitivity of detecting the aggregation of polymer-attached particles as described above.

[0013] On the other hand, in this embodiment, the upper limit of the amount of the surface-modifying polymer attached is, for example, 0.3 mg or less, preferably 0.2 mg or less, and more preferably 0.1 mg or less per 1 mg of the polymer-attached particles, which can improve the sensitivity of the polymer-attached particles. Although the detailed mechanism is unclear, it is believed that the polymer-attached particles in which the above-mentioned surface-modifying polymer has been introduced onto the surface of the core particle can have an appropriate amount of reactive functional group (A1) bonded to the ligand, thereby suppressing self-aggregation in a dispersion medium that does not contain the target substance, thereby improving dispersibility as described above. Furthermore, by setting the upper limit to 0.2 mg or less, it is possible to prevent a decrease in the coating efficiency of the surface-modifying polymer during particle preparation. Furthermore, by setting the upper limit at 0.1 mg or less, the amount of the surface modifying polymer used can be reduced from an economical point of view.

[0014] In this embodiment, for example, it is possible to control the amount of adhesion of the surface-modified polymer by appropriately selecting the type and amount of each component contained in the surface-modified polymer, the preparation method of the surface-modified polymer, etc. Among these, for example, in the manufacturing process of the polymer-attached particles, appropriately controlling the supply amount of the surface-modified polymer is cited as an element for setting the amount of adhesion of the surface-modified polymer to a desired numerical range.

[0015] Here, the procedure for calculating the adhesion amount of the surface modification polymer will be described. First, an infrared absorption spectrum of the polymer-attached particles is obtained by infrared spectroscopy such as Fourier transform infrared spectroscopy (FIIR) (step 1). From the obtained infrared absorption spectrum, the peak area of ​​the absorption peak derived from a predetermined functional group of the surface-modified polymer is calculated (step 2). Based on a previously prepared calibration curve, the adhesion amount (mg) of the surface modifying polymer is calculated from the obtained peak area (step 3).

[0016] Step 1: Obtaining an infrared absorption spectrum The infrared absorption spectrum is measured using an infrared spectrophotometer such as a Fourier transform infrared spectrophotometer. The sample for measuring the infrared absorption spectrum is prepared by the KBr pellet method or the like. As a pretreatment, the peak intensity of the infrared absorption spectrum is normalized using the absorption peaks of the aromatic ring overtones derived from the core particles, and the infrared absorption spectrum (peak area) of the core particles (single particles) is subtracted to obtain the infrared absorption spectrum of 1400 to 2000 cm. -1 It is preferable to perform baseline correction so that the base is horizontal in the measurement wavenumber range such as above.

[0017] Step 2: Waveform separation of infrared absorption spectrum and acquisition of peak areas of absorption peaks derived from specific functional groups It is preferable to perform waveform separation on the preprocessed infrared absorption spectrum and calculate the peak area of ​​the absorption peak derived from a predetermined functional group of the surface-modified polymer. In the waveform separation process, for example, the aromatic ring absorption from the core particle is fixed at the peak (center position, half-width, height) obtained by the waveform separation result of the particle alone, and the peaks from various functional groups having C=O absorption (unsaturated ester group, saturated ester group, carboxylic acid group, cyclic anhydride group, etc.) are each fitted with a Gaussian function. In addition, when the core particle is made of an organic material, the peak obtained by waveform separation of a single particle means a peak corresponding to an aromatic overtone among the infrared absorption spectrum of the single core particle after normalization, which is fitted by a Gaussian function or the like. From the infrared spectrum subjected to waveform separation, the peak area corresponding to the absorption peak of a specific functional group (unsaturated ester group, saturated ester group, carboxylic acid group, cyclic anhydride group, etc.) derived from the surface modified polymer is obtained.

[0018] Step 3: Calculate the amount of surface-modifying polymer attached from the calibration curve The calibration curve shows the relationship between the polymer concentration of the surface-modifying polymer and the peak area corresponding to a given functional group of the surface-modifying polymer. The calibration curve can be obtained using a measurement sample containing core particles and a surface-modified polymer, based on the measurement results of multiple samples with different polymer concentrations, i.e., multiple measurement results of the peak area corresponding to a specified functional group for a specified polymer concentration. For this calibration curve, the formula polymer concentration = (mass of polymer / mass of particle sample alone) x 100 is transformed to derive a function that uses the peak area as a variable to calculate the "amount of polymer attached (mg) per 1 mg of polymer-attached particles." Then, by inserting the peak area value obtained from the infrared absorption spectrum of the polymer-attached particles as the measurement sample into the function derived above, the "amount of polymer attached (mg) per 1 mg of polymer-attached particles" can be calculated.

[0019] The configuration of the polymer-attached particles of this embodiment will be described in detail below.

[0020] FIG. 1 is a cross-sectional view that illustrates an example of the configuration of a polymer-attached particle 10 according to this embodiment. An example of the polymer-attached particle 10 has at least a core particle 1 and a surface-modifying polymer 2 formed on at least a portion of the surface of the core particle 1 .

[0021] The polymer-attached particles 10 of this embodiment can be used as particles for an agglutination method used in detecting a target substance by an agglutination method. The polymer-attached particles 10 used in the aggregation method have ligands 3 chemically fixed to the surface.

[0022] The agglutination method is a method in which a sample containing a target substance (e.g., an antigen) is contacted in a dispersion medium with polymer-attached particles 10 carrying a ligand 3 (e.g., an antibody) that specifically recognizes (binds to) the target substance, causing the ligand 3 to bind to the target substance, forming a complex between the target substance, the ligand 3, and the polymer-attached particles 10, and selectively agglutinating the polymer-attached particles 10. The immunoagglutination method (also called immunoturbidimetry), which is one of the agglutination methods, utilizes an antigen-antibody reaction to react an antigen with an antibody present on the surface of the polymer-attached particles 10, thereby agglutinating the polymer-attached particles 10. In a method for detecting a target substance using an agglutination method, the degree of agglutination of the polymer-attached particles 10 can be characterized and quantified by optical measurement such as absorbance, scattered light intensity, or transmitted light intensity.

[0023] According to the present embodiment, the dispersibility of the polymer-attached particles 10 in the dispersion medium can be increased. This makes it possible to suppress the polymer-attached particles 10 from aggregating with each other in the dispersion medium before reacting with the target substance, i.e., to suppress non-specific reactions.

[0024] Furthermore, according to this embodiment, the dispersibility of the polymer-attached particles 10 can be improved, so that the change in the degree of aggregation of the polymer-attached particles 10 before and after the reaction with the target substance can be increased. In other words, when comparing the presence and absence of the target substance, the difference in optical measurement values ​​such as absorbance in a dispersion medium containing the polymer-attached particles 10 becomes large, so that it is possible to improve the sensitivity of the polymer-attached particles 10, i.e., the detection sensitivity of the target substance.

[0025] The sample is not particularly limited as long as it may contain the target substance, and examples thereof include any one or more biological samples selected from the group consisting of whole blood, plasma, serum, urine, cerebrospinal fluid, saliva, amniotic fluid, urine, sweat, and pancreatic juice. The sample is preferably whole blood, plasma, serum, or urine. The sample may be an aqueous medium containing the target substance, for example the target substance diluted in phosphate buffered saline or the like.

[0026] The aqueous solvent is not particularly limited as long as it is an aqueous solvent that allows the aggregation method, and examples thereof include deionized water, distilled water, and buffer solutions, with buffer solutions being preferred. Examples of the buffering agent contained in the buffer solution include phosphate-based, acetate-based, Tris-based, borate-based, carbonate-based, glycine-based, and Gut-based buffer solutions. As the Good's buffer, for example, HEPES, PIPES, MOPS, etc. are preferably used. The buffering agent may be used alone or in combination of two or more kinds. In addition, acids that can be used to adjust the pH of a buffer solution containing a buffer component include ordinary hydrochloric acid, sulfuric acid, nitric acid, and organic acids such as acetic acid, and alkalis that can be used include sodium hydroxide, potassium hydroxide, lithium hydroxide, ammonium hydroxide, and the like.

[0027] The target substance is not particularly limited as long as it is a target substance that allows for the agglutination method, and examples thereof include CRP (C-reactive protein); prostate-specific antigen (PSA); ferritin; α2-macroglobulin; β2-microglobulin; myoglobin; fibrin; fibrinogen degradation products; D-dimer; thrombin-antithrombin III complex (TAT); soluble fibrin (SF); soluble interleukin-2 receptor (sIL-2R); and sodium diuretic peptides such as atrial natriuretic peptide (ANP), brain natriuretic peptide (BNP), and C-type natriuretic peptide (CNP). These include urinary peptides; N-terminal pro-brain natriuretic peptide (NT-proBNP); antistreptolysin O; rheumatoid factor; transferrin; haptoglobin; α1-antitrypsin; α1-acidoglycoprotein; hemopexin; antithrombin-III; α-fetoprotein; CEA (carcinoembrionic antigen); HBs-Ag (hepatitis B envelope antigen); Anti-HBs (anti-hepatitis B envelope antibody); HBe-Ag (hepatitis B e antigen); Anti-HBe (anti-hepatitis B e antibody); Anti-HBc (anti-hepatitis B core antibody); IgG; IgA; IgM, etc. The target substance is not particularly limited as long as it is in a form that allows binding to an antibody, and may be, for example, in a free form as a simple substance, or in a complexed form with another substance (such as a protein).

[0028] The ligand 3 is a compound that specifically binds to a receptor of a specific target substance. The site at which a ligand binds to a target substance is fixed, and the ligand has a high affinity selectively or specifically. Examples of ligands include, but are not limited to, antigens and antibodies, enzyme proteins and their substrates, signal substances such as hormones and neurotransmitters and their receptors, and nucleic acids. Ligands include, for example, full length antibodies, antigen-binding fragments (e.g., Fab, F(ab') 2 Examples of the antibody that specifically recognizes a target substance include antibodies such as antibodies, antigens, nucleic acids such as naturally occurring nucleic acids and artificial nucleic acids, proteins such as aptamers, peptide aptamers, oligopeptides, enzymes, and coenzymes, etc. In addition, commercially available antibodies can be used as the antibody that specifically recognizes a target substance.

[0029] The core particle 1 is a particle that becomes the nucleus of the polymer-attached particle 10, and may be composed of either an organic particle or an inorganic particle. According to this embodiment, it is possible to improve the dispersibility of the polymer-attached particle 10 while taking advantage of the core particle characteristics (e.g., particle characteristics such as specific gravity and particle distribution) derived from the organic particle / inorganic particle.

[0030] As the organic particles, particles made of an organic polymer can be used. Examples of organic polymers include synthetic resins such as polystyrene, polyvinyl chloride, polypropylene, (meth)acrylic resins, polymethyl methacrylate, and silicone rubber; cellulose derivatives such as nitrocellulose, cellulose, and methylcellulose; phenolic resins, polylactic acid, polyethylene, and melamine phenol; copolymers containing one of these as a main component (for example, copolymers containing styrene as a main component); and copolymers containing two or more of these. The organic polymer may be used alone or in combination of two or more. The organic polymer constituting the organic particles is not particularly limited as long as it is composed of a polymer different from the surface-modifying polymer 2.

[0031] As the organic particles, known latex particles can be used, for example, styrene-based latex particles such as polystyrene latex, acrylic acid-based latex particles, various modified latex particles (for example, carboxylic acid-modified latex particles in which a carboxyl group is introduced into the above-mentioned polystyrene), colored latex particles, fluorescent latex particles, and the like. The latex particles can be produced by a known method, or may be commercially available. Two or more kinds of the latex particles may be used in combination.

[0032] Examples of methods for producing organic particles (resin particles) include a method in which raw material monomers (styrene, methacrylic acid, etc.) are polymerized with a polymerization initiator (radical polymerization initiator, etc.) to form a granular organic polymer in a solvent (water, etc.). The method for forming the granular organic polymer can be a radical polymerization method such as emulsion polymerization, soap-free emulsion polymerization, or suspension polymerization, but is not limited to radical polymerization.

[0033] As the inorganic particles, particles made of an inorganic substance can be used. Examples of inorganic substances include inorganic materials such as metals, ceramics, and glass. Specific examples of inorganic substances include silica. These may be used alone or in combination of two or more. In addition, inorganic materials having magnetic properties may be used as inorganic substances. In this way, the inorganic particles may be non-magnetic particles or magnetic particles.

[0034] The shape of the core particle 1 is not particularly limited, but examples thereof include a spherical shape, an elliptical shape, and an irregular shape.

[0035] The average particle diameter (D50) of the core particles 1 may be, for example, 0.01 μm to 1.0 μm, 0.02 μm to 0.8 μm, or 0.03 μm to 0.6 μm. The particle size of the core particle 1 can be measured, for example, by a laser diffraction particle size distribution analyzer. The average particle size (D50) is defined as the particle size at which the integrated value from the small particle side in the volume-based particle size distribution is 50%.

[0036] The surface modifying polymer 2 may be formed on at least a part of the surface of the core particle 1, and may form a polymer coating layer that covers a part or the entire surface of the core particle 1.

[0037] The method of forming the surface-modifying polymer 2 on the surface of the core particle 1 uses, for example, a polymer introduction step in which the surface-modifying polymer 2 is introduced onto the surface of the core particle 1 by a chemical reaction. For the chemical reaction, an immobilization method using a carboxy group or an immobilization method using an amino group, which are known as methods for immobilizing antibodies, can be used. These chemical reactions may involve the use of condensing agents, if desired, such as carbodiimide-based crosslinkers and amine-reactive crosslinkers. Carboxy groups and amino groups can be reacted with each other by using a carbodiimide crosslinking agent such as EDC (1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride, also known as EDAC or WSC). Amine-reactive crosslinkers can also be used to react primary or secondary amino groups with synthetic chemical groups such as isothiocyanates, isocyanates, acyl azides, NHS esters, sulfonyl chlorides, aldehydes, glyoxals, epoxides, oxiranes, carbonates, aryl halides, imidoesters, carbodiimides, anhydrides, fluoroesters, and the like.

[0038] When the core particle 1 is an organic particle (resin particle), a method is used in which a polymer reactive group (such as a carboxy group or an amino group) contained in the raw material monomer of the organic particle is reacted with a predetermined reactive group contained in the surface-modifying polymer 2. For example, in the manufacturing process of the organic particle, it becomes possible to include a polymer reactive group in the organic polymer during polymerization of the raw material monomer. Note that, as the core particle 1, a commercially available polystyrene particle containing a carboxy group may be used. As a specific example, when a surface-modifying polymer 2 containing a carboxy group is fixed to a core particle 1 containing a carboxy group, a part of the carboxy group in the core particle 1 is converted to a primary amino group (-NH 2 ) may be introduced (amino treatment). Then, a method of chemically reacting a primary amino group (polymer reactive group) in the core particle 1 after the amino treatment with a predetermined reactive group in the surface-modifying polymer 2 by adding the above-mentioned condensing agent as necessary can be mentioned. When the surface-modifying polymer 2 contains an acrylic group / methacrylic group, it is possible to react a primary amino group (polymer reactive group) with a carboxy group (predetermined reactive group) contained in the acrylic group / methacrylic group via the above-mentioned condensing agent. In another embodiment, when the surface modifying polymer 2 contains an anhydride group, it is possible to react a primary amino group (polymer reactive group) with an anhydride group (predetermined reactive group) such as a maleic anhydride group without using the above-mentioned condensing agent. On the other hand, when the core particle 1 is an inorganic particle, a method is used in which a polymer reactive group is introduced onto the surface of the inorganic particle, if necessary, using coupling or the like, and then the polymer reactive group is reacted with a specific reactive group contained in the surface-modifying polymer 2.

[0039] In addition, the reactive functional group (A1) such as a carboxy group remaining after the introduction step of the surface-modifying polymer 2 can be bonded by chemical reaction with a functional group such as an amino group possessed by the ligand 3 during sensitization. In addition, a functional group similar to the reactive functional group (A1) present in the surface-modifying polymer 2 can also chemically react with a functional group such as an amino group possessed by the ligand 3 during sensitization.

[0040] The surface modifying polymer 2 may be composed of a (meth)acrylic polymer, a maleic anhydride polymer, a methylene malonate polymer, a phenol resin, an epoxy resin, etc. These may be used alone or in combination of two or more kinds. According to this embodiment, by using the surface-modifying polymer 2 in addition to the core particle 1, a wide variety of molecular designs are possible for the surface-modifying polymer 2, and the degree of freedom in molecular design is increased.

[0041] Examples of the (meth)acrylic polymer include methacrylic polymers and acrylic polymers. Examples of maleic anhydride polymers include maleic anhydride-norbornene copolymers, styrene-maleic anhydride copolymers, maleic anhydride homopolymers, methyl vinyl ether-maleic anhydride copolymers, and olefin-maleic anhydride copolymers.

[0042] The surface-modifying polymer 2 may be any of a homopolymer, a random copolymer, an alternating copolymer, a block copolymer, and a periodic copolymer.

[0043] The weight average molecular weight of the surface modifying polymer 2 is, for example, 1,000 or more and 10,000,000 or less, preferably 2,000 or more and 5,000,000 or less, and more preferably 3,000 or more and 1,000,000 or less. The weight average molecular weight can be determined using a polystyrene equivalent value from a calibration curve of standard polystyrene (PS) obtained by gel permeation chromatography measurement.

[0044] The surface modifying polymer 2 comprises a structural unit A1 that includes a reactive functional group (A1) capable of binding with a ligand 3.

[0045] The polymer-attached particles 10 used in the aggregation method may contain a ligand 3 bonded to at least a portion of the reactive functional groups (A1). The polymer-attached particles 10 having the ligand 3 are called sensitized particles. A conventionally known method can be applied as a method of chemical reaction for chemically fixing the reactive functional group (A1) and the ligand 3. The above-mentioned carbodiimide-mediated reaction, NHS ester activation reaction, etc. can be used as a chemical reaction method, but are not limited thereto. If necessary, a condensing agent may be used. For example, in order to bind (support) the ligand 3 to the polymer-attached particle 10, the ligand 3 (antibody) and the polymer-attached particle 10 may be suspended in a buffer solution and reacted for a predetermined time at about 20 to 37°C, followed by a washing process and a blocking process. If necessary, other operational processes such as centrifugation, ultrasonication, and heating (aging) may be performed at an appropriate timing. Sensitized particles can be obtained by including one or more processes that are usually used in the technical field of sensitized particles, such as a sensitization process, a washing process, and a blocking process.

[0046] The reactive functional group (A1) may contain one or more selected from the group consisting of nucleophilic groups such as carboxyl groups, phenolic hydroxyl groups, amino groups, and thiol groups, and electrophilic groups such as epoxy groups, maleimide groups, acrylic groups, methacrylic groups, and acid anhydride groups. Examples of the acid anhydride groups include maleic anhydride groups and succinic anhydride groups. Among these, the reactive functional group (A1) may contain a carboxyl group.

[0047] The surface modifying polymer 2 also contains a structural unit A2 that includes a salt formed by an acidic functional group (A2) and an organic base. The acidic functional group (A2) constitutes a part of a side chain bonded to the main chain of the surface modification polymer 2. The acidic functional group (A2) may be bonded directly to the main chain of the surface modification polymer 2, or may be bonded, for example, without the intervention of a spacer having 5 or more carbon atoms. When bonded directly to the main chain without the intervention of the spacer, the ionic bond strength of the salt can be appropriately adjusted due to the steric hindrance of the surrounding side chains.

[0048] In the salt of the structural unit A2, the acidic functional group (A2) is H + (proton) is removed to form an anion (conjugate base), and the organic base is H + (proton) is accepted and the structure unit A2 is in a cationic (conjugate acid) state. It is presumed that the salt in the structural unit A2 is in an ionic bond between the anion of the acidic functional group (A2) and the cation of the organic base.

[0049] The acidic functional group (A2) includes, for example, one or more groups selected from the group consisting of a carboxy group, a sulfo group, a phosphate group, and a hydroxyl group. A part or all of the acidic functional group (A2) may be composed of the same group as the reactive functional group (A1), or may be composed of a group different from the reactive functional group (A1). For example, when the acidic functional group (A2) is a carboxyl group, the reactive functional group (A1) may be a carboxyl group, but may also be a different group selected from the above-mentioned groups other than the carboxyl group. When the acidic functional group (A2) and the reactive functional group (A1) contain the same group, at least a part of the other identical groups that do not form a chemical bond with an organic base among the multiple identical groups contained in the surface modification polymer 2 functions as the reactive functional group (A1). However, all of the other identical groups do not have to function as reactive functional groups (A1), and may be functional groups having other functions (functions other than ligand binding and salt formation) such as hydrophilic groups.

[0050] The organic base may include, for example, a nitrogen-containing base and / or a phosphorus-containing base, which may be used alone or in combination of two or more kinds. The nitrogen-containing base is not limited as long as it is a nitrogen-containing compound in which the nitrogen element easily accepts a proton to become a cation, and for example, an organic amine compound is used. Examples of the organic amine compound include aliphatic amines, aliphatic cyclic amines, aromatic amines, and heterocyclic amines. The aliphatic amines, aliphatic cyclic amines, and aromatic amines are preferably tertiary amines. In addition, a part of the group bonded to the nitrogen atom of the organic amine compound may be substituted with a substituent such as a hydroxyl group. The phosphorus-containing base is not limited as long as it is a phosphorus-containing compound in which the phosphorus element easily accepts a proton to become a cation, and for example, an organic phosphorus compound is used. The organic phosphorus may be, for example, a tertiary phosphine. The three groups bonded to the phosphorus atom in the tertiary phosphine are preferably either an aromatic group or a cyclic hydrocarbon group.

[0051] The organic base may include, for example, at least one of the nitrogen-containing bases and phosphorus-containing bases exemplified below. These may be used alone or in combination of two or more.

[0052] [ka]

[0053] Here, an example of a process for producing the polymer-attached particles 10 will be described. The above-mentioned production process includes a step of preparing the above-mentioned core particle 1, and a step of forming the above-mentioned surface-modifying polymer 2 on the surface of the core particle 1. The step of forming a surface modifying polymer 2 on the surface of a core particle 1 includes the steps of: a base introduction step of forming a salt between the acidic functional group (A2) of the surface-modifying polymer 2 and the organic base; It may also include the above-mentioned polymer introduction step of chemically reacting the above-mentioned polymer reactive group of the core particle 1 with a predetermined reactive group (functional group capable of reacting with the polymer reactive group) of the surface modifying polymer 2. Here, the order of the base introduction step and the polymer introduction step is not particularly limited, but the base introduction step may be performed after the polymer introduction step, or the base introduction step may be performed after the polymer introduction step. Note that one or more known treatments such as purification may be included between these steps.

[0054] When the base introduction step is performed after the polymer introduction step, the base introduction step is performed by mixing the above-mentioned nitrogen-containing compound and / or organic amine compound (organic base) with a surface-modified polymer precursor having an acidic functional group (A2) but no organic base to form a salt.

[0055] On the other hand, when the base introduction step is performed after the polymer introduction step, the base introduction step is performed by mixing the above-mentioned organic base with core particles 1 on whose surface a surface-modified polymer precursor having an acidic functional group (A2) but no organic base is formed, to form a salt-containing surface-modified polymer 2. The above-mentioned core particles 1 can be used in the form of a dispersion liquid in which they are dispersed in a dispersion medium such as water.

[0056] The above nitrogen-containing compound and / or organic amine compound (organic base) may be used in the form of a compound, or in the form of a solution containing the compound. The concentration of the organic base in the solution is, for example, 0.1 wt % to 90 wt %, preferably 0.2 wt % to 80 wt %, and more preferably 0.3 wt % to 70 wt %. The pH of the solution containing the organic base is, for example, 4 to 10, preferably 5 to 9, and more preferably 6 to 8. The solution containing an organic base preferably contains a solvent that does not dissolve the core particles 1 but dissolves the surface-modified polymer 2. From the viewpoint of such dissolution selectivity, it is preferable to use an alcohol solvent such as methanol, ethanol, isopropanol, etc. The solution may contain other additives such as a buffer, if necessary.

[0057] The manufacturing process of the polymer-attached particle 10 of this embodiment may, if necessary, include a step of reacting the reactive functional group (A1) of the surface-modifying polymer 2 with a ligand after the step of forming the surface-modifying polymer 2 on the surface of the core particle 1.

[0058] Here, an example of a method for synthesizing the surface modifying polymer 2 will be described. The method for synthesizing the surface-modified polymer 2 can include a polymer precursor production step of producing a surface-modified polymer precursor by polymerizing one or more raw material monomers, and an organic base introduction step of mixing the surface-modified polymer precursor with the above-mentioned organic base to form a salt.

[0059] The raw material monomers used in the polymer precursor production process can be one or more of raw material monomer A containing a diene compound and a diene parent compound, and raw material monomer B containing a functional group and an unsaturated group such as a double bond.

[0060] For the polymer of a diene compound and a parent diene compound, (i) if an anhydride group is contained, the anhydride group may be ring-opened to introduce a reactive functional group (A1), an acidic functional group (A2), or other functional groups (functional functional groups) into the side chain, (ii) if a carboxy group is contained, various functional groups may be introduced into the side chain by a condensation reaction or the like, and (iii) if an unsaturated group such as a double bond is contained, the above-mentioned various functional groups may be introduced into the side chain by an addition reaction or the like. Examples of the other functional groups mentioned above include known functional groups such as various reactive groups, hydrophobic groups, hydrophilic groups (water-soluble groups), and acidic groups. In addition, (i) when an anhydride group is included, the anhydride group may be ring-opened by water, alcohol, or the like, or the anhydride group may be ring-opened by the above-mentioned organic base. By ring-opening the anhydride group by an organic base, an organic base introduction step can be realized. In addition, the functional functional group described above may be introduced into the side chain of the polymer precursor by a condensation reaction or the like as in (ii) above for a functional group such as a carboxyl group formed by ring-opening the anhydride group.

[0061] In synthesizing a polymer precursor of a maleic anhydride-based polymer, for example, a norbornene-based monomer such as norbornene can be used as the diene compound, and an unsaturated carboxylic acid anhydride having a cyclic structure in the molecule such as maleic anhydride can be used as the new diene compound.

[0062] On the other hand, the raw material monomer B may be a raw material monomer B1 having a reactive functional group (A1) and an acidic functional group (A2), or a combination of a raw material monomer B2 having a reactive functional group (A1) and a raw material monomer B2 having an acidic functional group (A2), etc. If necessary, in addition to these, a raw material monomer B3 having a functional group other than the reactive functional group (A1) and the acidic functional group (A2) may be used.

[0063] For the synthesis of the polymer precursor of the (meth)acrylic polymer, for example, (meth)acrylic acid such as acrylic acid, methacrylic acid, (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, hexyl (meth)acrylate, and ethylhexyl (meth)acrylate are used. One or more of these (meth)acrylic monomers can be used.

[0064] The polymerization may be, but is not limited to, addition polymerization and / or condensation polymerization. For example, addition polymerization may be carried out by radical polymerization. In addition, the reactive functional group (A1), the acidic functional group (A2), or other functional groups (functional functional groups) may be introduced into the side chains of the obtained polymer precursor by ring-opening reaction, condensation reaction, addition reaction, or the like. A specific example will be described. First, one or more raw material monomers and a polymerization initiator are dissolved in a solvent, and then the solution is polymerized by heating for a predetermined time. The heating temperature can be, for example, 50°C to 80°C. The heating time can be, for example, 1 hour to 20 hours. It is more preferable to remove dissolved oxygen in the solvent by nitrogen bubbling before carrying out the solution polymerization.

[0065] As the polymerization initiator, for example, an azo compound, an organic peroxide, etc. can be used. Specific examples of the azo compound include azobisisobutyronitrile (AIBN), dimethyl 2,2'-azobis(2-methylpropionate), and 1,1'-azobis(cyclohexanecarbonitrile) (ABCN). Examples of organic peroxides include hydrogen peroxide, di-tertiary butyl peroxide (DTBP), benzoyl peroxide (benzoyl peroxide, BPO), and methyl ethyl ketone peroxide (MEKP). As for the polymerization initiator, only one type may be used, or two or more types may be used in combination.

[0066] In addition, a molecular weight regulator or a chain transfer agent can be used as necessary. Examples of the chain transfer agent include thiol compounds such as dodecyl mercaptan, mercaptoethanol, and 4,4-bis(trifluoromethyl)-4-hydroxy-1-mercaptobutane. These chain transfer agents may be used alone or in combination of two or more.

[0067] As the solvent used in the polymerization reaction, for example, one or more of esters such as methyl ethyl ketone (MEK), propylene glycol monomethyl ether, diethyl ether, tetrahydrofuran (THF), toluene, ethyl acetate, and butyl acetate can be used. As the polymerization initiator, one or more of azo compounds and organic peroxides can be used. As the azo compound, for example, azobisisobutyronitrile (AIBN), dimethyl 2,2'-azobis(2-methylpropionate), and 1,1'-azobis(cyclohexanecarbonitrile) (ABCN) can be used. As the organic peroxide, for example, hydrogen peroxide, ditertiary butyl peroxide (DTBP), benzoyl peroxide (benzoyl peroxide (BPO)), and methyl ethyl ketone peroxide (MEKP) can be used.

[0068] The reaction liquid containing the (co)polymer thus obtained is added to an alcohol or ether such as hexane or methanol to precipitate the polymer. The polymer is then filtered, washed with an alcohol such as hexane or methanol, and then dried. In this manner, the polymer can be synthesized. This makes it possible to remove low molecular weight components such as residual monomers, oligomers, and polymerization initiators.

[0069] The target substance detection reagent of this embodiment contains a particle group of the polymer-attached particles 10 and a dispersion medium. The concentration (wt %) of the polymer-attached particles 10 in the dispersion medium can be appropriately set. As the dispersion medium, for example, the above-mentioned aqueous solvents are preferably used. The aqueous solvent may contain, within the scope of the invention, a third substance such as a buffer, a preservative (e.g., sodium azide), a blocking agent such as a protein (albumin), a sensitizer such as a water-soluble polymer (e.g., sugar, polyethylene glycol, dextran), a salt (e.g., sodium chloride, amino acid), a surfactant, etc. These may be used alone or in combination of two or more kinds. The polymer-attached particles 10 in the reagent may be subjected to a blocking treatment using a blocking agent such as bovine serum albumin (BSA).

[0070] (kit) The target substance detection reagent of this embodiment may be in the form of a kit from the viewpoints of storage, transportation, distribution, etc. The form of the kit is not particularly limited as long as it is a form that enables the measurement method of the present invention. The target substance detection kit of the present embodiment includes a reagent container containing the above-mentioned target substance detection reagent.

[0071] The kit can take various forms, such as the following: The kit of the first type includes a particle group of polymer-attached particles 10 and a first reagent container containing a dispersion medium. The kit of the second embodiment includes a second reagent container A containing a particle group of the polymer-attached particles 10, and a second reagent container B containing a dispersion medium. The first reagent container of the kit of the first embodiment and the second reagent container A and second reagent container B of the kit of the second embodiment may each contain at least one or more of the third substances exemplified above. Furthermore, each of the kits of the first and second embodiments may further include a third reagent container containing at least one of the third substances. In addition, each of the kits of the first and second forms may include, in addition to the above-mentioned reagent container, a fourth reagent container containing one or more of a positive control, a negative control, a diluent, a washing solution, instructions for use, etc. As the media for the positive and negative controls, serum, physiological saline, solvents, etc. that do not contain a measurable target substance are used.

[0072] (Method for detecting target substances) The method for detecting a target substance of the present embodiment includes a contacting step of mixing a target substance with a target substance detection reagent. In the contact step, a sample containing the target substance and the polymer-attached particles 10 having the ligand 3 are added to the same reaction vessel and allowed to coexist, allowing the ligand 3 bound to the polymer-attached particles 10 to come into contact with the target substance. The sample containing the standard substance and the target substance reagent containing the polymer-attached particles 10 may be added in any order. Furthermore, the target substance and the polymer-attached particles 10 may be mixed at a pH of about 3.0 or more and about 11.0 or less, and the temperature of the mixture may be about 20° C. or more and 50° C. or less.

[0073] The target substance is contacted with the ligand 3 and reacted with each other, so that the substance to be measured in the sample reacts with the antibody supported on the latex particles, forming a complex between the target substance, the ligand 3, and the polymer-attached particles 10, and causing aggregation of the polymer-attached particles 10 due to the formation of the complex.

[0074] The method for detecting a target substance may include, after the contact step, a detection step of optically measuring the agglutination of the polymer-attached particles 10. Examples of the method for optically measuring the agglutination include a method of measuring absorbance, scattered light intensity, or transmitted light intensity with an optical instrument. The wavelength for measuring absorbance is usually 340 nm to 1000 nm, and preferably 500 nm to 900 nm. The time for measuring the agglutination reaction can be measured based on the rate of change per unit time during which the agglutination reaction is occurring, or the amount of change per unit time. For example, when measuring absorbance, the time can be measured based on the rate of change in absorbance per unit time from 30 seconds to 5 minutes after the start of the agglutination reaction, or the amount of change in absorbance per unit time.

[0075] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. EXAMPLES

[0076] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the descriptions of these examples.

[0077] <Synthesis of surface-modifying polymer> (Maleic anhydride polymer) Norbornene and maleic anhydride were reacted by radical polymerization at a predetermined ratio using an azo compound (polymerization initiator), to obtain polymer precursor A. Subsequently, various functional monomers having the following functional groups 1 to 3 were subjected to a ring-opening reaction in the presence of an organic base (triethylamine) at a predetermined ratio, and introduced into the side chains (ring-opened maleic anhydride groups) of each polymer precursor A (organic base introduction treatment), followed by reprecipitation with hexane or diethyl ether to obtain maleic anhydride-based polymers (polymers A1 to A4 shown in Table 1).

[0078] [Table 1]

[0079] [ka]

[0080] [ka]

[0081] The weight average molecular weight (Mw) of each of the maleic anhydride polymers obtained above was calculated based on a calibration curve of a standard PEG sample using GPC (gel permeation chromatography) under the following measurement conditions. The results are shown in Table 1 or Table 2.

[0082] The maleic anhydride polymer obtained above was subjected to the following measurement conditions: 13 The C-NMR spectrum was measured. Based on the obtained NMR spectrum results, the composition ratio (content of structural units having functional groups) in each polymer was calculated. The results are shown in Table 1 or Table 2. Table 1 also shows the ring-opening rate (%) of maleic anhydride groups. It was also found that the maleic anhydride polymer contains a structural unit having each functional group represented by the above general formula (A). R in the general formula (A) is represented by one or two of the functional groups 1 to 3 exemplified above.

[0083] The above polymer precursor A and the above polymers A1 to A4 were each measured under the following measurement conditions. 13 The C-NMR spectrum was measured. From the results of the NMR spectrum, a peak shift occurred between the polymer precursor A and the corresponding polymers A1 to A4, so it was confirmed that a salt was formed by ionic bonding between the carboxyl group in the maleic anhydride polymer (surface-modified polymer) obtained above and an organic base. Here, in the above general formula (A), it is presumed that a carboxy group and / or two adjacent or neighboring carboxy groups are ionic-bonded to an organic base.

[0084] (NMR measurement conditions) NMR measurements were performed using a JEOL ECA500 with deuterated dimethyl sulfoxide or deuterated ethanol as the solvent. (GPC measurement conditions) For the GPC measurements, one Tosoh TSKgel SuperAWM-H, one TSKgel SuperAW2500, and one TSKgel guardcolumn SuperAW-H were used, and 70% methanol / H 2 The conditions used were 30% O 2 (with 10 mM LiBr added), a column temperature of 40°C, and a flow rate of 0.6 ml / min.

[0085] <Preparation of particles with polymer> [Examples 1 to 13] Diamine was mixed into the following latex liquid A, and the carboxyl groups of the polystyrene latex particles were reacted with the diamine to introduce primary amino groups, followed by purification (amino treatment). Next, the surface-modifying polymers (polymers A1 to A4) shown in Table 2 were mixed in a predetermined mixing ratio into a solution containing polystyrene latex particles having primary amino groups to react the primary amino groups with maleic anhydride groups, and the mixture was purified to obtain a dispersion containing core particles with the surface-modifying polymer introduced onto their surfaces (polymer introduction treatment).

[0086] [Comparative Example 1] A dispersion liquid containing latex particles (latex liquid A below) was used.

[0087] [Comparative Example 2] A dispersion liquid in which TEA was mixed with the following latex liquid A was used.

[0088] Latex solution A: Carboxyl-modified polystyrene latex particles (manufactured by JSR, product name: IMMUNTEX, average particle size: 351 nm, solid content: 10%) Condensation agent: Carbodiimide crosslinking agent (EDC, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride, also known as WSC)

[0089] (Calculation of polymer adhesion amount) First, a calibration curve for the surface-modified polymer was prepared according to the following (1) to (5). (1) Preparation of samples for FT-IR measurement 10 μL of the above-mentioned latex particle dispersion (polystyrene latex particles, manufactured by JSR, product name: IMMUNTEX, average particle diameter: 351 nm, solid content: 10% by mass) was placed in a mortar and dried in vacuum at 40° C. overnight to obtain a “single particle sample.” Next, methanol solutions containing each of the polymers obtained above were added to the above particle samples so that the polymer concentrations were 0, 1, 2.5, 5, 7.1, 8.5, 10, 11.5, 12.5, 13, 15, 17.5, and 20 mass%, and the methanol was evaporated at room temperature to obtain several "composite samples" with different polymer concentrations. The polymer concentration was calculated from (mass of polymer / mass of single particle sample)×100. Next, the KBr powder and the composite sample were mixed and pressed to prepare tablets with different polymer concentrations (samples for FT-IR measurement). (2) FI-IR measurement Using a Fourier transform infrared spectrophotometer (manufactured by JASCO Corporation, product name: FT-IR6100), infrared absorption spectra (as) were obtained for the multiple samples for FT-IR measurement obtained above. However, for the infrared absorption spectrum (as), the peak intensity is normalized using the absorption peak of the overtone of the aromatic ring derived from the latex particle (base material), and the infrared absorption spectrum (peak area) of the latex particle (single particle) is subtracted, and the 1400 to 2000 cm -1 The baseline was corrected so that the base was horizontal in the measurement wavenumber range of 1000 nm to 1000 nm. (3) Waveform separation processing For the normalized infrared absorption spectrum (as), the aromatic ring absorption derived from the substrate was fixed at the peak (center position, half-width, height) obtained by waveform separation of the particle alone, and the peaks derived from various functional groups having C=O absorption (unsaturated ester group, saturated ester group, carboxylic acid group, cyclic anhydride group, etc.) were each fitted with a Gaussian function (waveform separation processing). (4) Obtaining the peak area (s) corresponding to the absorption peak of each functional group derived from the polymer For each of the multiple FT-IR measurement samples, the peak area (s) corresponding to the absorption peak of each functional group derived from the polymer (unsaturated ester group, saturated ester group, carboxylic acid group, cyclic anhydride group, etc.) was obtained. (5) Preparation of calibration curve The horizontal axis is the polymer concentration, and the vertical axis is the peak area (s) corresponding to the absorption peaks of the unsaturated ester group, the saturated ester group, the carboxylic acid group, and the cyclic anhydride group, and a calibration curve showing the relationship between the polymer concentration and the peak area (s) was created by the least squares method. A calibration curve was prepared for each of the above polymers A1 to A4. Based on the prepared calibration curve, the formula polymer concentration = (mass of polymer / mass of particle sample alone) × 100 was transformed to derive a function for calculating the "amount of polymer attached (mg) per 1 mg of polymer-attached particles" using the peak area (s) as a variable.

[0090] Next, for the polymer-attached particles of Examples 1 to 13, the peak areas (S) corresponding to the absorption peaks of each functional group derived from the polymer (unsaturated ester group, saturated ester group, carboxylic acid group, cyclic anhydride group, etc.) were obtained according to (2) to (4) above. The obtained peak area (S) was introduced into the function derived above to calculate the "amount of polymer attached (mg) per 1 mg of polymer-attached particles." However, in Examples 1 to 13, unsaturated ester groups were used for the peak areas (s) and peak areas (S) of the above calibration curves.

[0091] [Table 2]

[0092] In Tables 1 to 3, TEA stands for triethylamine.

[0093] The polymer-attached particles obtained above were evaluated for the following items.

[0094] <Production of Sensitized Particle Dispersion> (Sensitization treatment) 600 μL of the dispersion liquid (0.4% w / vol) of the polymer-attached particles of Examples 1 to 13 obtained above containing the condensing agent or the dispersion liquid (0.4% w / vol) containing the latex particles of Comparative Examples 1 and 2 above was mixed with 600 μL of the antibody A solution (0.27 mg / mL) described below, and the mixture was shaken and stirred at 20°C for 180 minutes to obtain a mixture. Antibody A solution: Ferritin antibody (Mikuri Immuno Research Institute, Ferritin clone No. 7 or No. 14), 10 mM MES (pH 6.5)

[0095] (Cleaning process) The resulting mixture was centrifuged at 10,000 rpm for 15 minutes at 10° C. using a centrifuge (rotor: R15A (HI antibody ACH)). The supernatant was decanted, and 3.5 mL of the following HEPES buffer was added to the resulting sediment, which was then dispersed by sonication. Subsequently, the mixture was centrifuged at 10,000 rpm for 15 minutes at 10° C. using the above centrifuge. The supernatant was decanted, and 3.5 mL of the following HEPES buffer was added to the resulting sediment, which was then dispersed by sonication to obtain a suspension. HEPES buffer: 0.1% BSA, 10 mM HEPES (4-(2-hydroxyethyl)-1-piperazineethanesulfonic acid, pH 7.2), 0.1% Tween 20, 0.05% NaN 3

[0096] (Blocking process) To the resulting suspension, 3.5 mL of the blocking solution described below was added, thoroughly dispersed, and then stirred for 1 hour at 37° C. Then, the mixture was centrifuged at 10,000 rpm and 10° C. for 15 minutes using the above centrifuge to obtain ligand-sensitized particles. Blocking solution: Bovine serum albumin (BSA) solution (1% BSA, 20 mM MES buffer (pH 6.0), 0.05% NaN 3 )

[0097] (Reagent processing) The following components were mixed in a given mixing ratio and uniformly dispersed by ultrasonic treatment (dispersion treatment) to prepare a reagent (sensitized particle dispersion) with a solid content of 0.1%. The ligand-sensitized particles obtained above · HEPES buffer containing 0.5% bovine serum albumin (BSA) 100mM NaCl 0.09% NaN 3 ·100mM HEPES buffer (pH7.0)

[0098] <Absorbance> Using an automatic analyzer TBA-120FR (manufactured by Canon Medical Systems Inc.), the absorbance at a wavelength of 700 nm was measured for each of the reagents of each Example and Comparative Example, the measurement reagents listed below, and the target substance (ferritin antigen solution) held at 10°C. Next, 20 μL of each of the reagents from each Example and Comparative Example was mixed with 80 μL of the measurement reagent described below and 4 μL of the target substance (antigen amount 0 ng / mL or 1,000 ng / mL), and the mixture was stirred uniformly and kept at 37°C. The absorbance at a wavelength of 700 nm was measured immediately after adding the measurement reagent and after 5 minutes had passed. The absorbance of each reagent when the antigen amount was 0 ng / mL and 1,000 ng / mL was calculated by subtracting the absorbance immediately after adding the measurement reagent from the absorbance after 5 minutes. As an index of sensitivity, the difference in absorbance (ΔAbs) between the presence and absence of added target substance was calculated by subtracting the absorbance at a wavelength of 700 nm when the antigen amount was 0 ng / mL from the absorbance at a wavelength of 700 nm when the antigen amount was 1,000 ng / mL.

[0099] (Measuring Reagents) The following components were mixed in a given ratio to prepare a measuring reagent. 0.1% Tween20 Polyethylene glycol (PEG) (5000~50000) ·1% bovine serum albumin (BSA) in HEPES buffer 150mM NaCl 0.09% NaN 3 ·100mM HEPES buffer (pH7.6)

[0100] The polymer-attached particles of Examples 1 to 13 showed higher absorbance differences (ΔAbs) between the presence and absence of added target substances than those of Comparative Examples 1 and 2, and therefore showed excellent sensitivity. It was found that such polymer-attached particles of Examples 1 to 13 can be suitably used as sensitized particle dispersions (reagents) for use in immune agglutination methods. [Explanation of symbols]

[0101] 1. Core Particle 2. Surface Modification Polymers 3. Ligand 10. Particles with polymer

Claims

1. A polymer-attached particle comprising a core particle and a surface-modifying polymer formed on at least a portion of the surface of the core particle, The surface-modifying polymer includes a structural unit A1 including a reactive functional group (A1) capable of binding to a ligand having specific binding ability to a target substance, A polymer-attached particle, in which the amount of the surface-modifying polymer attached to the polymer-attached particle, as measured according to the procedure described below, is 0.01 mg or more per 1 mg of the polymer-attached particle. (procedure) The infrared absorption spectrum of the polymer-attached particles is obtained by infrared spectroscopy. From the obtained infrared absorption spectrum, the peak area of ​​the absorption peak derived from a predetermined functional group of the surface-modified polymer is calculated. Based on a calibration curve prepared in advance, the adhesion amount (mg) of the surface modifying polymer is calculated from the obtained peak area.

2. The polymer-attached particle according to claim 1 , The amount of the surface-modifying polymer attached to the particles is 0.3 mg or less per 1 mg of the particles.

3. The polymer-attached particle according to claim 1 , The reactive functional group (A1) includes one or more groups selected from the group consisting of a carboxy group, a phenolic hydroxy group, an amino group, a thiol group, an epoxy group, a maleimide group, an acrylic group, a methacrylic group, and an acid anhydride group.

4. The polymer-attached particle according to claim 1 , The surface-modifying polymer comprises a structural unit A2 containing a salt formed by an acidic functional group (A2) and an organic base, the polymer-attached particle comprising the structural unit A2.

5. The polymer-attached particle according to claim 4, The acidic functional group (A2) includes one or more groups selected from the group consisting of a carboxy group, a sulfo group, a phosphate group, and a hydroxyl group.

6. The polymer-attached particle according to claim 4, The polymer-attached particles, wherein the organic base comprises a nitrogen-containing base and / or a phosphorus-containing base.

7. The polymer-attached particle according to claim 1 , The surface-modifying polymer has a weight average molecular weight of 1,000 or more and 10,000,000 or less.

8. The polymer-attached particle according to claim 1 , The polymer-attached particle, wherein the core particle is an organic particle or an inorganic particle.

9. The polymer-attached particle according to claim 1 , A polymer-attached particle comprising the ligand bonded to at least a portion of the plurality of reactive functional groups (A1).

10. The polymer-attached particle according to claim 1 , The polymer-attached particle, wherein the ligand is any one of an antibody, an antigen, a protein, and a nucleic acid.

11. The polymer-attached particle according to claim 1 , The polymer-attached particles are used for detecting the target substance by an agglutination method.

12. A target substance detection reagent comprising the polymer-attached particle according to any one of claims 1 to 11 and a dispersion medium.

13. A target substance detection kit comprising a reagent container containing the target substance detection reagent according to claim 12.

14. A method for detecting a target substance, comprising the step of mixing a target substance with the target substance detection reagent according to claim 12.

Citation Information

Patent Citations

  • Measurement method using latex immunoagglutination method, reagent, and kit

    JP2021162593A