Glass adhesive, and fixture for burning or drying having junction part composed of burned product of glass adhesive
A glass adhesive with a specific composition and viscosity range addresses the issues of heat resistance and dimensional accuracy in bonding ceramic members, enhancing the performance of baking or drying jigs by improving adhesion and thermal stability.
Patent Information
- Application Number
- JP2023056527
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing baking or drying jigs face challenges in achieving suitable heat resistance and dimensional accuracy, particularly when bonding ceramic members using adhesives.
A glass adhesive with a specific composition and viscosity range is used to bond members, containing 95 mol% or more of a glass composition with defined oxide ratios of MgO, CaO, BaO, ZnO, B2O3, Al2O3, SiO2, Fe2O3, Bi2O3, CuO, and Y2O3, and a rotational viscosity of 10 Pa·s to 2000 Pa·s, which improves heat resistance and dimensional accuracy.
The glass adhesive enables the creation of jigs with enhanced heat resistance and dimensional accuracy, suitable for bonding ceramic materials like alumina, mullite, forsterite, and stabilized zirconia, with improved adhesion and thermal stability.
Smart Images

Figure 2024143721000006 
Figure 2024143721000007 
Figure 2024143721000008
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a glass adhesive and to a baking or drying jig having a joint that is a baked product of such a glass adhesive. [Background technology]
[0002] For example, Patent Document 1 discloses an alumina adhesive that is placed between a pair of alumina ceramic members and heated to bond the pair of alumina ceramic members, and also discloses a firing jig having a joint formed by sintering the alumina adhesive. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2018-168050 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, according to the inventor's research, it was found that when the members constituting a firing (or drying) jig are bonded together with an adhesive and then fired to join them, there is still room for improvement in terms of the heat resistance, dimensional accuracy, etc. of the firing (or drying) jig. In other words, there is a demand for further development of technology to obtain a firing or drying jig with favorably improved heat resistance and dimensional accuracy.
[0005] The present disclosure has been made in consideration of the above circumstances, and its main objective is to provide a technique for obtaining a firing or drying jig having favorably improved heat resistance and dimensional accuracy. [Means for solving the problem]
[0006] In order to achieve this object, the present disclosure provides a glass adhesive prepared in a paste form for bonding members constituting a firing or drying jig, the glass adhesive having a viscosity of 10 Pa·s to 2000 Pa·s as measured at a rotational speed of 100 rpm using a rotational viscometer in an environment of 25° C., and containing a glass composition as a main component, wherein, when the entire glass composition is taken as 100 mol %, 95 mol % or more of the glass composition has the following composition in molar ratio calculated as oxides: MgO: 0 mol % to 40 mol %, CaO: 0 mol % to 30 mol %, BaO: 0 mol % to 50 mol %, ZnO: 0 mol % to 50 mol %, B 2 O 3 : 0 mol% to 50 mol%, Al 2 O 3 : 1 mol% to 20 mol%, SiO 2 : 5 mol% to 50 mol%, Fe 2 O 3 : 0 mol% to 3 mol%, Bi 2 O 3 : 0 mol% to 20 mol%, CuO: 0 mol% to 5 mol%, Y 2 O 3 The present invention provides a glass adhesive comprising: 0 mol % to 3 mol % of a glass component. Although details will be described later, a glass adhesive having such a composition can provide a firing or drying jig having favorably improved heat resistance and dimensional accuracy.
[0007] In a preferred embodiment of the glass adhesive disclosed herein, the glass composition contains Mg, Ca, and Ba in a total molar ratio of 3 mol % to 60 mol % calculated as oxides when the entire glass composition is taken as 100 mol %. With this configuration, a firing or drying jig with more favorably improved heat resistance and dimensional accuracy can be obtained.
[0008] In a preferred embodiment of the glass adhesive disclosed herein, the thermal expansion coefficient from 30° C. to 500° C. is 6×10 ―6 K ―1 ~12×10 ―6 K ―1 and the glass softening point is 500° C. to 850° C. With this configuration, it is possible to obtain a firing or drying jig with more suitably improved heat resistance and dimensional accuracy.
[0009] In addition, for example, when the members to be joined are made of at least one selected from the group consisting of alumina, mullite, forsterite, stabilized zirconia, and magnesia, the difference in thermal expansion coefficient between the members to be joined and the members to be joined from 30° C. to 500° C. is 3×10 ―6 K ―1 In this configuration, it is possible to obtain a firing or drying jig having favorably improved heat resistance and dimensional accuracy.
[0010] In a preferred embodiment of the glass adhesive disclosed herein, the glass composition does not contain Pb, Te, As, or Cd. This is preferable because it is possible to prevent the generation of substances that may have adverse effects on the human body and the environment during firing.
[0011] From another aspect, the present disclosure provides a firing or drying jig (hereinafter, also simply referred to as a "jig") having a joint that is a fired product of any of the glass adhesives disclosed herein. Since such a firing or drying jig has a joint that is a fired product of any of the glass adhesives disclosed herein, it can be said to be a jig with favorably improved heat resistance and dimensional accuracy. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a schematic diagram illustrating a configuration of a jig according to an embodiment. [Diagram 2] FIG. 2 is a schematic diagram illustrating a configuration of a jig according to an embodiment. [Diagram 3] FIG. 1 is a schematic diagram showing a base material according to a test example. [Figure 4] FIG. 1 is a schematic diagram showing a member according to a test example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] A preferred embodiment of the present disclosure will be described below. Matters other than those specifically mentioned in this specification and necessary for the implementation of the present disclosure can be understood as design matters of a person skilled in the art based on the conventional technology in the field. The present disclosure can be implemented based on the contents disclosed in this specification and the technical common sense in the field. The following embodiments are not intended to limit the technology disclosed herein to such embodiments. In addition, in the following drawings, dimensional relationships (length, width, thickness, etc.) do not reflect actual dimensional relationships, and do not limit the present disclosure unless specifically mentioned. And, the symbols X, Y, and Z in the drawings respectively represent the vertical direction of the jig or member, the horizontal direction perpendicular to the vertical direction, and the height direction. However, these are merely directions for convenience of explanation, and do not limit the installation form of the jig or member in any way. In addition, in this specification and claims, when a certain numerical range is described as A to B (A and B are arbitrary numerical values), it means A or more and B or less. Therefore, it includes the case where it is greater than A and less than B. In addition, "paste-like" can be a concept that includes ink-like and slurry-like.
[0014] <Glass adhesive> The glass adhesive disclosed herein is a glass adhesive (which may also be called a glass paste) prepared in a paste form for bonding members constituting a firing or drying jig. The glass adhesive has a viscosity of 10 Pa·s to 2000 Pa·s measured at a rotational speed of 100 rpm using a rotational viscometer in an environment of 25° C. The glass adhesive contains a glass composition as a main component, and when the entire glass composition is taken as 100 mol %, 95 mol % or more (preferably 99 mol % or more, and may be, for example, 100 mol %) of the glass composition has the following composition in molar ratio calculated as oxides: MgO: 0 mol % to 40 mol %, CaO: 0 mol % to 30 mol %, BaO: 0 mol % to 50 mol %, ZnO: 0 mol % to 50 mol %, B 2 O 3 : 0 mol% to 50 mol%, Al 2 O 3 : 1 mol% to 20 mol%, SiO 2: 5 mol% to 50 mol%, Fe 2 O 3 : 0 mol% to 3 mol%, Bi 2 O 3 : 0 mol% to 20 mol%, CuO: 0 mol% to 5 mol%, Y 2 O 3 The glass adhesive is characterized in that it contains 0 mol% to 3 mol%. Note that "containing a glass composition as a main component" can mean that, when the entire glass adhesive is taken as 100 mass%, the glass composition is contained in an amount of, for example, 50 mass% or more, 60 mass% or more, 70 mass% or more, or 80 mass% or more. The upper limit of the glass composition may be, for example, 99 mass% or less, 95 mass% or less, or 90 mass% or less.
[0015] As a result of intensive research, the present inventors have found that when a glass adhesive having the above-mentioned composition of the glass composition and adjusted to have a viscosity within an appropriate range is used to bond components constituting a firing (or drying) jig, the heat resistance of the joint is suitably improved. It has also been found that when such a glass adhesive is used, the dimensional change rate of the firing (or drying) jig falls within an appropriate range. In other words, the glass adhesive disclosed herein makes it possible to obtain a firing or drying jig with suitably improved heat resistance and dimensional accuracy. Each of the components of the above glass adhesive will be described below.
[0016] (1) Magnesium content As described above, the glass adhesive disclosed herein may not contain a magnesium component (typically, magnesium oxide (MgO)) (i.e., 0 mol%) when the entire glass composition is taken as 100 mol%), and if it does contain one, the molar ratio calculated as oxide is specified as 40 mol% or less. The magnesium component (MgO) is a component that adjusts the thermal expansion coefficient within an appropriate range and can increase the hardness of the glass matrix to improve the wear resistance. From the viewpoint of suitably obtaining such an effect, the content of the magnesium component (MgO) in the glass adhesive disclosed herein is preferably 5 mol% or more, and may be 10 mol% or more (e.g., 11 mol% or more), or 15 mol% or more. The upper limit of the content of the magnesium component (MgO) is preferably 30 mol% or less, and may be 21 mol% or less. The lower limit and upper limit of the content of the magnesium component (MgO) can be combined without any particular restriction.
[0017] (2) Calcium content As described above, the glass adhesive disclosed herein may not contain a calcium component (typically calcium oxide (CaO)) (i.e., 0 mol%) when the entire glass composition is taken as 100 mol%), and if it does contain a calcium component, the molar ratio calculated as oxide is specified to be 30 mol% or less. The calcium component (CaO) is a component that adjusts the thermal expansion coefficient within an appropriate range and can increase the hardness of the glass matrix to improve the wear resistance. From the viewpoint of preferably obtaining such an effect, the content of the calcium component (CaO) in the glass adhesive disclosed herein is preferably 5 mol% or more, and may be 10 mol% or more, or 15 mol% or more (e.g., 16 mol% or more). The upper limit of the content of the calcium component (CaO) is preferably 25 mol% or less (e.g., 24 mol% or less), and may be 22 mol% or less. The lower limit and upper limit of the content of the calcium component (CaO) can be combined without any particular restriction.
[0018] (3) Barium component As described above, the glass adhesive disclosed herein may not contain a barium component (typically, barium oxide (BaO)) (i.e., 0 mol%) when the entire glass composition is taken as 100 mol%), and if it does contain a barium component, the molar ratio calculated as oxide is specified to be 50 mol% or less. The barium component (BaO) can significantly reduce the viscosity of the glass component after melting, making it easier to adjust the viscosity of the glass adhesive to an appropriate range. From the viewpoint of optimally obtaining such effects, the content of the barium component (typically, barium oxide (BaO)) in the glass adhesive disclosed herein is preferably 3 mol% or more, and may be 5 mol% or more, 10 mol% or more, 15 mol% or more, or 20 mol% or more (e.g., 21 mol% or more). The upper limit of the content of the barium component (BaO) is preferably 45 mol% or less (e.g., 43 mol% or less), and may be 40 mol% or less, 30 mol% or less, or 25 mol% or less. The lower and upper limits of the content of the barium component (BaO) can be combined without any particular restriction.
[0019] (4) Zinc content As described above, the glass adhesive disclosed herein may not contain a zinc component (typically, zinc oxide (ZnO)) (i.e., 0 mol%) when the entire glass composition is taken as 100 mol%), and if it does contain a zinc component, the molar ratio calculated as oxide is specified to be 50 mol% or less. The zinc component (ZnO) can adjust the viscosity of the glass adhesive during firing and can have the function of improving the airtightness and stability of the joint formed after firing. From the viewpoint of preferably obtaining such an effect, the content of the zinc component (ZnO) in the glass adhesive disclosed herein is preferably 3 mol% or more (e.g., 3.5 mol% or more), and may be 6 mol% or more, 8 mol% or more (e.g., 9 mol% or more), or 10 mol% or more. The upper limit of the content of the zinc component (ZnO) is preferably 40 mol% or less, and may be 30 mol% or less, or 20 mol% or less. The lower limit and upper limit of the content of the zinc component (ZnO) can be combined without any particular restriction.
[0020] (5) Boron component As described above, the glass adhesive disclosed herein contains a boron component (typically, boron oxide (B 2 O 3 Boron (B) may not be included (i.e., 0 mol%), but if it is included, it is specified that the molar ratio of the oxide is 50 mol% or less. 2 O 3 ) is a component capable of forming a glass skeleton. From the viewpoint of obtaining such an effect, the boron component (B 2 O 3 The content of the boron component (B) is preferably 10 mol% or more, and may be 12 mol% or more, 14 mol% or more, 19 mol% or more, or 20 mol% or more. 2 O 3 The upper limit of the content of the boron component (B) is preferably 45 mol % or less (for example, 44 mol % or less), and may be 40 mol % or less, or 30 mol % or less. 2 O 3 The lower and upper limits of the contents of the components (a) and (b) can be combined without any particular limitation.
[0021] (6) Aluminum content As described above, the glass adhesive disclosed herein contains an aluminum component (typically, aluminum oxide (Al 2 O 3 The aluminum content (Al) is specified to be 1 mol % or more and 20 mol % or less in terms of oxide molar ratio. 2 O 3 ) is a component capable of forming a glass skeleton. From the viewpoint of preferably obtaining such an effect, the aluminum component (Al 2 O 3 The content of the aluminum component (Al) is preferably 1.5 mol % or more, and may be 2 mol % or more (for example, 2.5 mol % or more), 3 mol % or more, or 5 mol % or more. 2 O 3 The upper limit of the content of the aluminum component (Al) is preferably 15 mol % or less, and may be 10 mol % or less.2 O 3 The lower and upper limits of the contents of the components (a) and (b) can be combined without any particular limitation.
[0022] (7) Silicon component As described above, the glass adhesive disclosed herein contains a silicon component (typically, silicon oxide (SiO 2 The silicon component (SiO 2 ) is a component capable of forming a glass skeleton. In addition, since it is possible to prevent the softening point of the glass adhesive from becoming too high, it is possible to bond members to each other even at relatively low temperatures (for example, about 500°C). In addition, it is said that the silicon component can improve at least one of water resistance, chemical resistance, and thermal shock resistance. From the viewpoint of preferably obtaining such effects, the silicon component (SiO 2 The content of the silicon component (SiO ) is preferably 10 mol% or more (for example, 11 mol% or more), and may be 15 mol% or more, 18 mol% or more (for example, 19 mol% or more), or 20 mol% or more. 2 The upper limit of the content of the silicon component (SiO 2 The lower and upper limits of the contents of the components (a) and (b) can be combined without any particular limitation.
[0023] (8) Iron As described above, the glass adhesive disclosed herein contains an iron component (typically, iron oxide (Fe 2 O 3 It is not necessary for the steel to contain iron (Fe) (i.e., 0 mol%), but if it does contain iron, the molar ratio of the oxide is regulated to 3 mol% or less. 2 O 3) is a component that makes it easy to adjust the thermal expansion coefficient within an appropriate range. From the viewpoint of obtaining such an effect, the iron component (Fe 2 O 3 The content of the iron component (Fe) is preferably 0.1 mol % or more, and may be 0.4 mol % or more. 2 O 3 The upper limit of the content of the iron component (Fe) is preferably 2 mol % or less, and may be 1 mol % or less. 2 O 3 The lower and upper limits of the contents of the components (a) and (b) can be combined without any particular limitation.
[0024] (9) Bismuth component As described above, the glass adhesive disclosed herein contains a bismuth component (typically, bismuth oxide (Bi 2 O 3 Bismuth component (Bi) may not be included (i.e., 0 mol%), but if it is included, it is specified that the molar ratio of the oxide is 20 mol% or less. 2 O 3 ) is a component that adjusts the thermal expansion coefficient and is highly effective in lowering the softening point of the glass matrix. From the viewpoint of obtaining such effects, the bismuth component (Bi 2 O 3 The content of the bismuth component (Bi) is preferably 5 mol % or more, and may be 10 mol % or more. 2 O 3 The upper limit of the content of the bismuth component (Bi) is preferably 18 mol % or less, and may be 15 mol % or less. 2 O 3 The lower and upper limits of the contents of the components (a) and (b) can be combined without any particular limitation.
[0025] (10) Copper Content As described above, the glass adhesive disclosed herein may not contain a copper component (typically, copper oxide (CuO)) (i.e., 0 mol%) when the entire glass composition is taken as 100 mol%), and if it does contain a copper component, the molar ratio calculated as oxide is specified to be 5 mol% or less. The copper component (CuO) is a component that adjusts the thermal expansion coefficient and is highly effective in lowering the softening point of the glass matrix. From the viewpoint of preferably obtaining such an effect, the content of the copper component (typically, copper oxide (CuO) in the glass adhesive disclosed herein is preferably 1 mol% or more, and may be 2 mol% or more. The upper limit of the content of the copper component (typically, copper oxide (CuO) is preferably 4 mol% or less, and may be 3 mol% or less. The lower limit and upper limit of the content of the copper component (typically, copper oxide (CuO) can be combined without any particular restriction.
[0026] (11) Yttrium component As described above, the glass adhesive disclosed herein contains a yttrium component (typically, yttrium oxide (Y 2 O 3 The yttrium component (Y) may not be contained (i.e., 0 mol%), but if it is contained, it is specified that the molar ratio of the oxide is 3 mol% or less. 2 O 3 ) is a component that makes it easy to adjust the thermal expansion coefficient. From the viewpoint of obtaining such an effect, the yttrium component (Y 2 O 3 The content of the yttrium component (Y 2 O 3 The upper limit of the content of the yttrium component (Y 2 O 3 The lower and upper limits of the contents of the components (a) and (b) can be combined without any particular limitation.
[0027] In a preferred embodiment, the glass composition contains Mg, Ca, and Ba in a total molar ratio calculated as oxides of 3 mol% or more (e.g., 3.5 mol% or more), 10 mol% or more, 20 mol% or more, or 30 mol% or more (e.g., 32 mol% or more) when the entire glass composition is taken as 100 mol%. The upper limit of the total molar ratio calculated as oxides of Mg, Ca, and Ba is preferably 60 mol% or less, 57 mol% or less, 52 mol% or less, or 43 mol% or less. That is, when the entire glass composition is taken as 100 mol%, the glass composition preferably contains Mg, Ca, and Ba in a total molar ratio calculated as oxides within a range of 3 mol% to 60 mol%. With this configuration, a firing or drying jig having more suitably improved heat resistance and dimensional accuracy can be obtained.
[0028] In addition, the glass adhesive disclosed herein may contain optional components other than the above 11 types of components, so long as the effects of the technology disclosed herein are exhibited. An example of such an optional component is a copper component (typically, Cu 2 O), iron components (typically FeO,Fe 3 O 4 ), nickel component (typically NiO), zirconium component (typically ZrO 2 ), niobium content (typically Nb 2 O 5 ), tin components (typically SnO, SnO 2 ), lanthanum component (typically, La 2 O 3 ), cerium component (typically CeO 2 ), titanium component (typically TiO 2 ), vanadium components (typically V 2 O 5 ), phosphorus content (typically P 2 O 5 ), Group 1 element components (typically oxides of Group 1 elements: M 2Examples of the optional components include O and M, which can be selected from Li, Na, K, Rb, Cs, and Fr, and Group 2 element components (typically, oxides of Group 2 elements: M', O and M', which can be selected from Be, Sr, and Ra). By adding these optional components to form a multi-component glass composition, the physical stability of the glass joint after firing can be improved. When these optional components are added, the ratio of the optional components in the entire glass adhesive can be about 0.01 mol % to 5 mol %, preferably about 0.05 mol % to 3 mol %, and more preferably about 0.1 mol % to 1 mol %, in terms of oxide, when the entire glass composition is taken as 100 mol %.
[0029] In addition, it is preferable that the glass adhesive does not contain lead (Pb), tellurium (Te), arsenic (As), cadmium (Cd), etc. By not containing these components, it is possible to prevent the generation of substances that may have adverse effects on the human body and the environment, which is preferable. In this specification and claims, "not containing" means that the above-mentioned components are not intentionally added. Therefore, it does not strictly exclude unavoidable substances that may be contained in small amounts due to raw materials, manufacturing processes, etc. For example, when the entire glass composition is 100 mol%, it is preferable that the molar ratio in terms of oxide is less than 0.1 mol%.
[0030] As described above, the viscosity of the glass adhesive is specified to be within the range of 10 Pa·s to 2000 Pa·s when measured at a rotational speed of 100 rpm using a rotational viscometer in an environment of 25°C. With this configuration, when members constituting a firing (or drying) jig are bonded together, the heat resistance of the joint can be suitably improved. Also, the dimensional change rate of the firing (or drying) jig can be set within an appropriate range. From the viewpoint of improving the dimensional accuracy of the members, the viscosity is preferably 10 Pa·s to 1000 Pa·s, and may be, for example, 20 Pa·s to 1000 Pa·s or 100 Pa·s to 1000 Pa·s. Also, from the viewpoint of particularly improving the dimensional accuracy, the viscosity is more preferably within the range of 10 Pa·s to 100 Pa·s (for example, 20 Pa·s to 100 Pa·s). The viscosity may be, for example, within the range of 50 Pa·s to 500 Pa·s. The viscosity can be measured using a commercially available viscometer, such as a Brookfield HB viscometer. The viscosity of the glass adhesive can be easily adjusted by adjusting the amounts of glass powder, solvent, and additives.
[0031] The thermal expansion coefficient of the glass adhesive is not particularly limited as long as the effects of the technology disclosed herein can be obtained, but from the viewpoint of suitably preventing damage to the members to be joined (preferably ceramic members made of a ceramic material), it is preferable that the thermal expansion coefficient of the glass adhesive is close to that of the objects to be joined. From this viewpoint, the thermal expansion coefficient of the glass adhesive is preferably 6.0×10 -6 K -1 ~12.0×10 -6 K -1 (More preferably 6.5×10 -6 K -1 ~11.5×10 -6 K -1In this specification, the term "thermal expansion coefficient" refers to the average expansion coefficient (average linear expansion coefficient) measured using a thermomechanical analysis (TMA) in the temperature range from 30°C to 500°C, and refers to the value obtained by dividing the amount of change in sample length relative to the initial length of the sample by the temperature difference. The thermal expansion coefficient can be measured, for example, in accordance with JIS R3102:1995 or the like.
[0032] The glass softening point of the glass adhesive is not particularly limited as long as the effects of the technology disclosed herein can be obtained, but is preferably 500°C to 850°C. In this configuration, a firing or drying jig with more favorably improved heat resistance and dimensional accuracy can be obtained. Note that the "glass softening point" approximately means the temperature below which most molding operations of the glass adhesive become impossible, and may be, for example, 10 7.6 The glass softening point may refer to the temperature corresponding to a viscosity of dPa·s. The glass softening point can be measured, for example, by the method described in the test examples below.
[0033] Although not particularly limited, the thermal expansion coefficient of the joined members is, for example, 6×10 ―6 K ―1 ~13×10 ―6 K ―1 For example, it is preferable that the members to be joined are made of alumina, mullite, forsterite, stabilized zirconia, magnesia, a mixture of these, or the like. In such a case, the difference in thermal expansion coefficient between the members to be joined and the members to be joined from 30° C. to 500° C. is within the range of 3×10 ―6 K ―1 It is preferable that the difference in the linear thermal expansion coefficient is 3×10 ―6 K ―1 By making the difference in thermal expansion coefficient to be less than or equal to 2.5×10, a jig for firing or drying having favorably improved heat resistance and dimensional accuracy can be obtained. ―6 K ―1 Less than (e.g., 2.2×10 ―6 K ―1 (less than 1.0×10―6 K ―1 Here, a suitable example of stabilized zirconia is yttrium oxide (Y 2 O 3 Examples of suitable zirconia include yttria-stabilized zirconia (YSZ) stabilized with yttria (also called "yttria") and calcia-stabilized zirconia (CSZ) stabilized with calcia (CaO). Among these, YSZ is particularly suitable, and YSZ having yttria dissolved therein in an amount of 1 mol % to 15 mol % (preferably 3 mol % to 10 mol %) of the total amount can be preferably used.
[0034] Although not particularly limited, the adhesive force (bonding strength) between the members (for example, in this embodiment, the support member 2 and the setter 3) when bonded with the glass adhesive can be, for example, 1.0 MPa or more (preferably, 5.0 MPa or more). The upper limit of the bonding strength can be, for example, 100 MPa or less or 80 MPa or less. The bonding strength test can be measured, for example, by the following method. First, the members to be bonded are cut into a cube with one side of about 10 mm to 15 mm, and the cut members are overlapped (bonded) with about 0.1 g of the glass adhesive interposed therebetween. Then, for example, at room temperature (20°C ± 10°C), a force is applied to one of the members in the shear direction at a compression speed of 0.5 mm / min using a compression tester or the like, and the maximum breaking load when the two are peeled off is measured, and the value obtained by dividing the value by the bonding area is regarded as the bonding strength.
[0035] <How to prepare glass adhesive> The method for preparing such a glass adhesive is not particularly limited, but for example, first, a glass raw material powder is prepared. In the preparation of the glass raw material powder, for example, industrial products, reagents, or various mineral raw materials containing oxides, carbonates, nitrates, composite oxides, etc. containing each of the above-mentioned components are prepared, and these are mixed to obtain a desired composition. The preparation of such glass raw material powder can be performed, for example, by putting the above-mentioned raw materials into a mixer such as a ball mill and mixing them for several hours to several tens of hours.
[0036] Next, the glass raw material powder obtained as described above is dried, heated and melted under high temperature conditions (typically about 900 to 1400°C), and then cooled or quenched to vitrify. In a preferred embodiment, the obtained glass (vitreous intermediate) is pulverized to an appropriate size (particle size) to produce glass powder. The average particle size of the vitreous intermediate is preferably, for example, 0.5 μm to 50 μm (typically, 1 μm to 10 μm). The "average particle size" (also referred to as D50 particle size) may mean a particle size equivalent to 50% of the cumulative value from the small particle size side in a volume-based particle size distribution based on a laser diffraction / scattering method.
[0037] Next, the obtained glass powder is mixed with a solvent (typically an organic solvent) and a binder (typically an organic binder) to prepare a paste. As the organic solvent, for example, terpineol, an ether-based solvent, an ester-based solvent, various glycols, etc. can be used. These may be used alone or in combination of two or more. In addition, as the organic binder, various binders that are usually used in this type of glass paste can be used. For example, cellulose-based polymers such as methyl cellulose, ethyl cellulose, and nitrocellulose, acrylic resins, epoxy resins, amine resins, etc. can be used. These may be used alone or in combination of two or more. In addition, as the above-mentioned solvent and binder, commercially available products can be used without particular restrictions. Here, when the entire glass adhesive is taken as 100 mass%, the above-mentioned glass powder can be added in an amount of about 50 to 90 mass% (for example, 60 to 80 mass%). Furthermore, when the entire glass adhesive is taken as 100% by mass, the solvent can be added in an amount of about 1 to 50% by mass (for example, 5 to 45% by mass). When the entire glass adhesive is taken as 100% by mass, the binder can be added in an amount of about 1 to 20% by mass (for example, 10 to 15% by mass). The paste-like glass adhesive can be applied to a member to be joined (for example, a ceramic member, etc.) in the form of coating or printing by adjusting the viscosity to an appropriate value according to the desired application. The method of dispersing and mixing the paste is not particularly limited, and can be carried out, for example, using a conventionally known three-roll mill. In this manner, the glass adhesive can be prepared.
[0038] In addition, when preparing the glass adhesive, any component may be added as necessary as long as the effect of the technology disclosed herein is exhibited. Examples of such optional components include dispersants, plasticizers, antioxidants, defoamers, leveling agents, and the like. For example, dispersants that are usually used in glass pastes can be used, and examples of such dispersants include polyamine-based polymer dispersants, polycarboxylic acid-based polymer surfactants, modified acrylic block copolymers, acrylic copolymers having pigment affinity groups, block copolymers having basic or acidic pigment adsorption groups, modified polyalkoxylates having pigment affinity groups, polyaminoamide salts and polyesters, combinations of polar acid esters and polymer alcohols, alkyl ammonium salts of acidic polymers, copolymers and alkyl ammonium salts containing acid groups, high molecular weight block copolymers having pigment affinity groups, special modified ureas, and the like. One or more of these can be appropriately selected and used. In addition, when the entire glass adhesive is taken as 100% by mass, the above-mentioned optional components can be added in an amount of about 0.1 to 5% by mass (for example, 1 to 3% by mass).
[0039] <Jig> Next, with reference to FIG. 1 and FIG. 2, a jig for firing or drying according to this embodiment will be described. Here, the term "jig for firing" refers to a jig used when firing an object to be fired, and the term "jig for drying" refers to a jig used when drying an object to be dried. The jig for firing or drying includes, for example, one or more setters on which the object to be fired or dried is placed, and a support member for holding the setter. Such a support member includes various shapes such as a geta (for example, a platform for supporting one or more setters), a shelf (for example, a rack for placing one or more setters), and a pillar (for example, a support for supporting one or more setters). Below, a jig according to this embodiment will be described, but it is not intended to limit the jig to such a configuration.
[0040] 1 and 2 are schematic diagrams showing the configuration of the jig according to the present embodiment. First, as shown in FIG. 1, the jig 1 according to the present embodiment includes a setter 3 and a support member 2 that supports the setter 3. A workpiece 4 can be placed on the setter 3. The workpiece 4 may be an object to be dried or an object to be fired. As shown in FIG. 2, the jig 1 according to the present embodiment has a joint 5 that joins the support member 2 and the setter 3. The joint 5 is a fired product of the glass adhesive disclosed herein. Since the jig 1 has the joint 5 that is a fired product of any of the glass adhesives disclosed herein, it can be said that the jig has favorably improved heat resistance and dimensional accuracy. Each component will be described below.
[0041] (A) Setter As shown in FIG. 1, the setter 3 according to this embodiment is plate-shaped. The setter 3 is rectangular here. A workpiece 4 is placed on the setter 3. The setter 3 is preferably made of, for example, a ceramic material. Here, "made of a ceramic material" means that, when the total mass of the setter is 100 mass%, for example, the ceramic material is contained at 50 mass% or more, 60 mass% or more, 70 mass% or more, 80 mass% or more, or 90 mass% or more (may be 100 mass%) (the same applies below). Examples of such ceramic materials include alumina, silica, mullite, forsterite, stabilized zirconia, magnesia, etc. Examples of stabilized zirconia include YSZ and CSZ as described above, and YSZ can be particularly preferably used. Examples of the dimensions of the setter 3 include a length of 10 cm to 30 cm, a width of 10 cm to 30 cm, and a thickness of 0.1 cm to 5 cm. Here, the length, width, and thickness of the setter 3 refer to, for example, the lengths in the X direction, Y direction, and Z direction in Fig. 1, respectively. In other embodiments, the setter may not be plate-shaped, but may be box-shaped so as to accommodate a workpiece. In other embodiments, the setter may not be rectangular, but may be circular, elliptical, polygonal, or any other shape.
[0042] (B) Support member As shown in FIG. 1, the support member 2 according to this embodiment has a cubic shape. The support member 2 is a member that supports the setter 3, and is a getter in this embodiment. The support member 2 is preferably made of, for example, a ceramic material. Examples of such ceramic materials include those listed in the description of the setter (A) above. The material constituting the support member 2 and the material constituting the setter 3 may be the same or different. An example of the dimensions of the support member 2 is one in which the length of one side is about 5 mm to 20 mm (for example, about 10 mm to 15 mm). Note that in other embodiments, the support member may have a rectangular parallelepiped shape, a cylindrical shape, an elliptical cylinder shape, a polygonal cylinder shape, or various other shapes, instead of a cube shape.
[0043] (C) Work As shown in FIG. 1, the workpiece 4 according to this embodiment is plate-shaped. The workpiece 4 is rectangular here. The workpiece 4 is placed on the setter 3. The workpiece 4 is preferably made of, for example, a ceramic material. Examples of such ceramic materials include those listed in the description of the setter (A) above. In other embodiments, the workpiece may not be rectangular, but may be circular, elliptical, or of various other shapes.
[0044] When the jig 1 is for firing, a reaction-preventing setter may be further disposed between the setter 3 and the work 4 to prevent side reactions from occurring between the setter 3 and the work 4 during firing.
[0045] (D)Joint part As shown in FIG. 1, the joint 5 according to this embodiment is a portion that joins the support member 2 and the setter 3. The joint 5 can be a fired product of any of the glass adhesives disclosed herein. The thickness of the joint 5 (thickness in the Z direction in FIG. 2) can be, for example, about 0.01 cm to 1 cm (preferably, about 0.05 cm to 0.5 cm). With the glass adhesive disclosed herein, the strength of the joint 5 can be suitably ensured even in an embodiment in which the thickness of the joint 5 is made thin.
[0046] <Method of manufacturing jig> Next, an example of a method for manufacturing the jig 1 according to this embodiment will be described. Below, a method for manufacturing the jig according to this embodiment will be described, but it is not intended that the jig be limited to such a configuration.
[0047] First, a predetermined amount (generally about 0.1 g to 1 g, for example, about 0.1 g to 0.5 g) of any of the glass adhesives disclosed herein is applied to the surface of the support member 2 that contacts the setter 3. Such application can be performed using a metal spatula, a dispenser, or the like. Then, the support member 2 and the setter 3 are assembled into a configuration as shown in FIG. 1. Subsequently, such an assembly is dried at a predetermined temperature (for example, about 50 to 100° C.) for a predetermined time (for example, about 0.5 to 2 hours), and then fired at a predetermined temperature (for example, about 500 to 1500° C.) for a predetermined time (for example, about 1 to 2 hours), thereby manufacturing the jig 1.
[0048] The jig 1 thus obtained can be used as a drying jig for drying the workpiece 4, or as a firing jig for firing the workpiece 4. For example, when the jig 1 is a drying jig, the workpiece 4 placed on the setter 3 can be placed in a dryer or the like to dry the workpiece 4 at a predetermined temperature (for example, about 50 to 300°C). When the jig 1 is a firing jig, the workpiece 4 placed on the setter 3 can be placed in a firing furnace or the like to fire the workpiece 4 at a predetermined temperature (for example, about 500 to 1500°C).
[0049] [Test example A] Hereinafter, a test example related to the present disclosure will be described with reference to Fig. 3 and Fig. 4, but it is not intended that the present disclosure be limited to such a test example. Here, Fig. 3 is a schematic diagram showing a base material related to the test example. Fig. 4 is a schematic diagram showing a member related to the test example.
[0050] <Preparation of glass adhesive according to each example> First, the glass raw material powder was prepared and mixed to have the composition shown in Tables 1 and 2, and then melted at 900°C to 1400°C for about 1 hour, and quenched to 25°C to vitrify. Then, pulverization and classification were performed to prepare glass powder with an average particle size of about 5 μm. Then, the glass powder prepared as described above, a binder, a dispersant, and a solvent were kneaded by a three-roll mill to prepare glass pastes (glass adhesives) according to each example. Here, the content of each component was such that, when the glass paste was taken as 100% by mass, the glass powder was 50 to 90% by mass, the binder was 1 to 20% by mass, the dispersant was 1 to 5% by mass, and the remainder was the solvent (5 to 45% by mass). Then, an ethyl cellulose-based binder manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. was used as the binder, a polyamine-based polymer dispersant manufactured by Croda Japan Co., Ltd. was used as the dispersant, and terpineol manufactured by Nippon Terpene Chemical Co., Ltd. was used as the solvent. In this manner, the glass adhesives according to the respective examples were obtained.
[0051] [Table 1]
[0052] [Table 2]
[0053] <Evaluation test> (1) Measurement of the thermal expansion coefficient of glass adhesive The glass adhesives according to the examples prepared as described above were press-molded into a rectangular column of about φ20 mm×7 mm, and heat-treated at 500°C to 1000°C for about 0.5 to 2 hours to obtain a disk-shaped fired body. The fired body was cut into a size of about 15 mm×5 mm×5 mm with a diamond cutter to prepare a test piece for measurement. The test piece was then evaluated using a thermomechanical analyzer (TMA8310, manufactured by Rigaku Corporation). Specifically, the thermal expansion coefficient was calculated from the average linear expansion amount between 30°C and 500°C when the temperature was raised from room temperature (25°C) to 1000°C at a constant rate of 10°C / min. The results are shown in the "Thermal expansion coefficient of glass adhesive" column in Tables 3 and 4.
[0054] The thermal expansion coefficient of each base material was measured by cutting each base material into a test piece of about 15 mm x 5 mm x 5 mm using a diamond cutter. The test piece was evaluated using a thermomechanical analyzer (TMA8310, manufactured by Rigaku Corporation). Specifically, the thermal expansion coefficient was calculated from the average linear expansion amount between 30 ° C and 500 ° C when the temperature was raised from room temperature (25 ° C) to 1000 ° C at a constant rate of 10 ° C / min. The results are shown in the column "Thermal expansion coefficient of base material" in Tables 3 and 4.
[0055] (2) Measurement of glass softening point The glass powder used in the above glass adhesive was press-molded into a cylindrical shape of about 7 to 10 mm in diameter and 5 to 7 mm in height, and then calcined at 500 to 850°C for 10 minutes. The calcined test piece was then heated again, and the amount of deformation in the height direction was measured from room temperature (25°C) to a maximum of 900°C using a glass parallel plate viscosity measuring device. The glass viscosity was then calculated based on the deformation rate of the measured sample according to the Gent formula. 7.6 The temperature at which the glass softening point is reached is taken as the glass softening point. The results are shown in the "glass softening point" column of Tables 1 and 2. Gent's formula: η = 2πMgH 5 / 3V(-dH / dt)(2πH 3 +V) (where η is viscosity (Poise), M is load (g), H is sample height (cm), g is gravitational acceleration (cm / s 2 ), V: sample volume (cm 3), dH / dt: sample deformation speed (cm / s).
[0056] (3) Measurement of viscosity of glass adhesive The viscosity of each of the glass adhesives prepared as described above was measured using a rotational viscometer at a rotation speed of 100 rpm in an environment of 25°C. The measurement was performed using a Brookfield HB type viscometer, spindle: SC-4-14, and small cup. The results are shown in the "Viscosity of glass adhesive" column in Tables 1 and 2.
[0057] (4) Evaluation of adhesiveness of components First, as shown in Figure 3, cubic alumina (manufactured by AS ONE Corporation) with sides of about 10 to 12 mm, mullite (manufactured in-house, fired at 1300°C), forsterite (manufactured in-house, fired at 1400°C), and stabilized zirconia (3 mol% Y 2 O 3 Two base materials 10 made of stabilized zirconia (manufactured by AS ONE Corporation) and magnesia (manufactured by Nikkato Corporation) were prepared, and 0.1 g to 0.5 g of the glass adhesive according to each example prepared as described above was applied to the bonding surface (corresponding to the shaded area in FIG. 3) with a metal spatula, and the glass adhesive was assembled and dried at 80°C for 0.5 to 2 hours. Then, heat treatment was performed at 600°C to 1400°C for about 1 to 2 hours to obtain a member 20 as shown in FIG. 4. In the evaluation of "adhesion of the member", the adhesion of the member was indicated as "x" when the base materials were not bonded to each other during the formation of the member, or when cracks occurred at the joint 15 after heat treatment, and the adhesion of the member was indicated as "◯" when the base materials were bonded to each other. The results are shown in the "adhesion of the member" column in Tables 3 and 4.
[0058] (5) Evaluation of heat resistance of components The members obtained by the same method as in (4) above were held at each temperature in 50°C intervals in the range from 200°C to 1600°C for 30 minutes, and the maximum temperature at which it was confirmed that no peeling occurred at the joint 15 was determined as the heat resistance temperature of the member. The heat resistance temperatures of each member are shown in the "heat resistance temperature of member" column of Tables 3 and 4. In addition, in the evaluation of "heat resistance of member", the heat resistance of the member was shown as "x" when the maximum temperature was less than 400°C, the heat resistance of the member was shown as "◯" when the maximum temperature was 400°C or more and less than 1000°C, and the heat resistance of the member was shown as "◎" when the maximum temperature was 1000°C or more. The results are shown in the "heat resistance of member" column of Tables 3 and 4.
[0059] (6) Evaluation of heat cycle resistance The members obtained by the same method as in (4) above were subjected to a heat cycle between the maximum temperature determined in (5) above and room temperature (for example, about 25°C), and the maximum number of heat cycles at which it was confirmed that no peeling or cracking occurred in the joint 15 was defined as the number of heat cycles resistance. The number of heat cycles resistance for each member is shown in the "number of heat cycles resistance" column of Tables 3 and 4. Here, in the heat cycle, the temperature rise was 10°C / min, the maximum temperature was held for 30 minutes, and the maximum temperature was held for 30 minutes, after which the temperature was lowered to 25°C and the furnace was cooled. For those members for which peeling or cracking was not confirmed after 10 heat cycles, "10 times or more" was written in the "number of heat cycles resistance" column. In addition, in the evaluation of "heat cycle resistance", a heat cycle resistance of less than 10 times was indicated as "x", and a heat cycle resistance of 10 times or more was indicated as "◯". The results are shown in the "heat cycle resistance" column of Tables 3 and 4.
[0060] (7) Evaluation of dimensional accuracy First, the length (in other words, the dimension before forming into a component) of the two base materials shown in FIG. 3 in the direction perpendicular to the adhesive surface (corresponding to the Z direction in FIG. 3) was measured using a commercially available micrometer. In addition, the length (length in the Z direction in FIG. 4, also referred to as the dimension after forming into a component) of the component obtained by the same method as in (4) above was measured. The dimensions before forming into a component and the dimensions after forming into a component of each component are shown in the "dimension before forming into a component" and "dimension after forming into a component" columns of Tables 3 and 4, respectively. Then, the "dimensional change rate" was calculated from the following formula (I): dimensional change rate = {(dimension after forming into a component - dimension before forming into a component) / dimension after forming into a component} x 100 (%). In addition, in the evaluation of "dimensional accuracy", when the dimensional change rate is smaller than -3% or larger than +3%, the dimensional accuracy is indicated as "x", when the dimensional change rate is -3% or more but less than -1% or more than +1% or less than +3%, the dimensional accuracy is indicated as "〇", and when the dimensional change rate is -1% or more but +1% or less, the dimensional accuracy is indicated as "◎". The results are shown in the "Dimensional Accuracy" column of Tables 3 and 4.
[0061] For each evaluation item, items that received all "◎" were marked as "◎", items that received no "×" were marked as "◯", and items that received at least one "×" were marked as "×".
[0062] In Table 4, samples 15, 18, 21, 23, and 25, which used glass adhesive containing glass A, had a very high glass softening point and could not be bonded to the base materials below the heat resistance temperature of the base materials, so "-" was written in the columns "Heat resistance temperature of the component", "Heat resistance of the component", "Number of heat cycles", "Heat cycle resistance", "Dimensions before componentization", "Dimensions after componentization", "Dimensional change rate before and after componentization", and "Dimensional accuracy". In addition, samples 16, 19, 22, 24, and 26, which used glass adhesive containing glass B and glass E, had a very low glass softening point and could not be bonded to the base materials at the specified firing temperature, so "-" was written in the columns "Number of heat cycles", "Heat cycle resistance", "Dimensions before componentization", "Dimensions after componentization", and "Dimensional accuracy". In samples 22 and 24, the heat resistance temperature of the component could not be measured, so "-" was written in the column "Heat resistance temperature of the component". In addition, for samples 17, 20, and 27, which used glass adhesives containing glass C, glass D, and glass F, respectively, there was a large difference in the thermal expansion coefficients of the base material and the glass adhesive. Furthermore, in the case of samples 20 and 27, the glass softening point was high, so cracks occurred at the joint when the components were made and proper joining was not possible. Therefore, a "-" was entered in the columns for "heat resistance temperature of component," "heat resistance of component," "number of heat cycles," "heat cycle resistance," "dimensions before componentization," "dimensions after componentization," "dimensions before and after componentization," and "dimensional precision."
[0063] [Table 3]
[0064] [Table 4]
[0065] [Test Example B] Next, in Test Example B, evaluation was performed with the viscosity of the glass adhesive changed. Hereinafter, this Test Example will be described.
[0066] <Preparation of glass adhesives according to samples 28 to 33> Glass adhesives according to Samples 28 to 33 were prepared in the same manner as Sample 14, except that the viscosity of the glass adhesive (here, the glass adhesive containing glass 7) was changed.
[0067] <Evaluation test> Each evaluation test in Table 5 was performed in the same manner as described in [Test Example A]. The evaluation criteria were also the same as those described in [Test Example A]. The results are shown in the corresponding columns in Table 5.
[0068] In addition, for sample 28, the viscosity of the glass adhesive was very low and the adhesive strength was insufficient, so the base materials did not bond together, and so "adhesion of components" was marked as "x". Also, since no other evaluations could be performed, they were marked as "-". And for sample 33, the viscosity of the glass adhesive was very high, so it did not wet and spread well on the base materials, and the dimensional accuracy after firing was poor, so "dimensional accuracy" was marked as "x".
[0069] [Table 5]
[0070] As shown in Tables 3 and 4, the viscosity measured at a rotational speed of 100 rpm using a rotational viscometer in an environment of 25° C. is 10 Pa·s to 2000 Pa·s, and the glass composition contains a glass composition as a main component, and when the entire glass composition is taken as 100 mol %, 95 mol % or more of the glass composition has the following composition in molar ratio calculated as oxides: MgO: 0 mol % to 40 mol %, CaO: 0 mol % to 30 mol %, BaO: 0 mol % to 50 mol %, ZnO: 0 mol % to 50 mol %, B 2 O 3 : 0 mol% to 50 mol%, Al 2 O 3 : 1 mol% to 20 mol%, SiO 2 : 5 mol% to 50 mol%, Fe 2 O 3 : 0 mol% to 3 mol%, Bi 2 O 3: 0 mol% to 20 mol%, CuO: 0 mol% to 5 mol%, Y 2 O 3 It was confirmed that Samples 1 to 14, which used glass adhesives containing 0 mol % to 3 mol %, had superior heat resistance and dimensional accuracy of the members compared to Samples 15 to 27, which used glass adhesives not satisfying the above-mentioned configuration. In addition to the above-mentioned effects, Samples 1 to 14 were also confirmed to have superior adhesion and heat cycle resistance of the members.
[0071] Furthermore, as shown in Table 3, when the glass composition contains Mg, Ca, and Ba in a total molar ratio of 3 mol % to 60 mol % calculated as oxides, assuming the entire glass composition to be 100 mol %, it was confirmed that the heat resistance and dimensional accuracy of the component were excellent.
[0072] As shown in Table 3, in an embodiment in which the members to be joined (corresponding to the base material here) are made of alumina, mullite, forsterite, stabilized zirconia, or magnesia, the difference in thermal expansion coefficient between the members to be joined and the base material from 30° C. to 500° C. is 3×10 ―6 K ―1 Less than (e.g., 2.5×10 ―6 K ―1 It was confirmed that when the above conditions are met, the heat resistance and dimensional accuracy of the components are excellent.
[0073] Also, as shown in Table 5, it was confirmed that samples 28 and 33, in which the viscosity of the glass adhesive was outside the range of 10 Pa·s to 2000 Pa·s, did not have excellent heat resistance and / or dimensional accuracy of the members. Also, it was confirmed that samples 14, 29 to 32 had better dimensional accuracy when the viscosity of the glass adhesive was within the range of 10 Pa·s to 1000 Pa·s, for example. Furthermore, it was confirmed that the dimensional accuracy was particularly excellent when the viscosity of the glass adhesive was within the range of 10 Pa·s to 100 Pa·s (e.g., 20 Pa·s to 100 Pa·s).
[0074] Although specific examples of the present disclosure have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and alterations of the specific examples exemplified above.
[0075] As described above, specific aspects of the technology disclosed herein include those described in the following items. Item 1: A glass adhesive prepared in a paste form for bonding members constituting a firing or drying jig, the glass adhesive having a viscosity of 10 Pa·s to 2000 Pa·s measured at a rotational speed of 100 rpm using a rotational viscometer in an environment of 25°C, containing a glass composition as a main component, wherein, when the entire glass composition is taken as 100 mol%, 95 mol% or more of the glass composition has the following composition in molar ratio calculated as oxides: MgO: 0 mol% to 40 mol%, CaO: 0 mol% to 30 mol%, BaO: 0 mol% to 50 mol%, ZnO: 0 mol% to 50 mol%, B 2 O 3 : 0 mol% to 50 mol%, Al 2 O 3 : 1 mol% to 20 mol%, SiO 2 : 5 mol% to 50 mol%, Fe 2 O 3 : 0 mol% to 3 mol%, Bi 2 O 3 : 0 mol% to 20 mol%, CuO: 0 mol% to 5 mol%, Y 2 O 3 : 0 mol% to 3 mol%, including glass adhesive. Item 2: The glass adhesive according to item 1, wherein the glass composition contains Mg, Ca, and Ba in a total molar ratio of 3 mol % to 60 mol % calculated as oxides when the entire glass composition is taken as 100 mol %. Item 3: The thermal expansion coefficient from 30°C to 500°C is 6×10 ―6 K ―1 ~12×10 ―6 K ―1 Item 3. The glass adhesive according to item 1 or 2, having a glass softening point of 500°C to 850°C. Item 4: The joined members are made of at least one selected from the group consisting of alumina, mullite, forsterite, stabilized zirconia, and magnesia, and the difference in thermal expansion coefficient between the joined members and the joined members from 30°C to 500°C is 3×10 ―6 K ―1 Item 4. A glass adhesive according to any one of items 1 to 3, which is as follows: Item 5: The glass adhesive according to any one of Items 1 to 4, wherein the glass composition does not contain B, Pb, Te, or As. Item 6: A firing or drying jig having a joint which is a fired product of the glass adhesive according to any one of items 1 to 5. [Explanation of symbols]
[0076] 1 Jig 2 Supporting member 3. Setter 4 Work 5,15 Joint 10 Base material 20 Materials
Claims
1. A glass adhesive prepared in a paste form for bonding members constituting a firing or drying jig, The viscosity measured at a rotational speed of 100 rpm using a rotational viscometer in an environment of 25° C. is 10 Pa·s to 2000 Pa·s, The glass composition is included as a main component, When the entire glass composition is taken as 100 mol %, 95 mol % or more of the glass composition has the following composition in terms of oxide molar ratio: MgO: 0 mol% to 40 mol% CaO: 0 mol% to 30 mol% BaO: 0 mol% to 50 mol% ZnO: 0 mol% to 50 mol% B 2 O 3 : 0 mol% to 50 mol% A 2 O 3 : 1 mol% to 20 mol% SiO 2 : 5 mol% to 50 mol% Fe 2 O 3 : 0 mol% to 3 mol% Bi 2 O 3 : 0 mol% to 20 mol% CuO: 0 mol% to 5 mol% Y 2 O 3 : 0 mol% to 3 mol% Including, glass adhesive.
2. The glass adhesive according to claim 1, wherein the glass composition contains Mg, Ca, and Ba in a total molar ratio of 3 mol% to 60 mol% calculated as oxides, when the entire glass composition is taken as 100 mol%.
3. The thermal expansion coefficient from 30°C to 500°C is 6 x 10 ―6 K ―1 ~12×10 ―6 K ―1 and a glass softening point is 500°C to 850°C.
4. the members to be joined are made of at least one selected from the group consisting of alumina, mullite, forsterite, stabilized zirconia, and magnesia; The difference in thermal expansion coefficient between the joined members from 30°C to 500°C is 3×10 ―6 K ―1 3. The glass adhesive according to claim 1 or 2, wherein:
5. The glass adhesive according to claim 1 or 2, wherein the glass composition does not contain Pb, Te, As, or Cd.
6. A firing or drying jig having a joint which is a fired product of the glass adhesive according to claim 1 or 2.
Citation Information
Patent Citations
Adhesive for alumina, burning tool and manufacturing method therefor
JP2018168050A