Honeycomb structure, electric heating type carrier and exhaust gas purification device

By optimizing the composition and resistivity of silicon and silicon carbide in honeycomb structures with controlled dopant concentrations, the issue of non-uniform heat distribution and excessive current flow is addressed, resulting in a more reliable catalyst carrier for exhaust gas purification.

JP2024143853AActive Publication Date: 2024-10-11NGK CORP

Patent Information

Application Number
JP2023056766
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

Existing honeycomb structures for exhaust gas purification systems face issues with non-uniform heat generation distribution and excessive current flow, leading to potential damage and uneven heating, particularly at low voltage levels.

Method used

The honeycomb structure is designed with specific compositions of silicon and silicon carbide, controlled dopant concentrations, and adjusted electrical resistivity to mitigate NTC thermistor characteristics, ensuring uniform heat distribution and preventing excessive current flow.

Benefits of technology

The improved honeycomb structure achieves enhanced uniformity in heat generation, reducing the risk of cracks and damage, and can be effectively used as a catalyst carrier in exhaust gas purification devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143853000001_ABST
    Figure 2024143853000001_ABST
Patent Text Reader

Abstract

To provide a honeycomb structure with improved uniformity of calorific distribution.SOLUTION: A honeycomb structure comprises: a ceramic honeycomb structure part; and a pair of electrode layers provided on an external surface of an outer peripheral wall, extending in a band shape in an extension direction of cells, and provided so as to face each other across a central axis of the honeycomb structure part, where the ceramic contains at least silicon and silicon carbide, and satisfies one or both of the following conditions (1) and (2): (1) a silicon content in the ceramic is 21 to 30 mass%; silicon contains P and B; and a value (P-B amount) obtained by subtracting a B concentration from a P concentration in the silicon is 20 ppm by mass or more; (2) a silicon carbide content in the ceramic is 50 mass% or more; silicon carbide contains Al and N; and the value (Al-N amount) obtained by subtracting an N concentration from an Al concentration in the silicon carbide is 130 ppm by mass or more and 450 ppm by mass or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a honeycomb structure. The present invention also relates to an electrically heated carrier having a honeycomb structure. The present invention also relates to an exhaust gas purification device having an electrically heated carrier. [Background technology]

[0002] Conventionally, catalysts supported on honeycomb structures made of cordierite or silicon carbide have been used to treat harmful substances in exhaust gases emitted from automobile engines. When treating exhaust gases with a catalyst supported on a honeycomb structure, the catalyst needs to be heated to a specified temperature. However, a problem has existed in the past where exhaust gases are not sufficiently purified at engine start-up because the catalyst temperature is low. To address this problem, a system called an electrically heated catalyst (EHC) has been developed in which electrodes are provided on a honeycomb structure made of conductive ceramics, and the honeycomb structure itself is heated by passing electricity through it, thereby heating the catalyst supported on the honeycomb structure to its activation temperature before or at engine start-up.

[0003] An EHC generally includes an outer peripheral wall, a conductive honeycomb structure having partition walls disposed inside the outer peripheral wall to define a plurality of cells that form a flow path from a first end face to a second end face, and a pair of electrode layers disposed on the outer peripheral wall of the honeycomb structure. When an EHC is mounted on an automobile or the like for use, the power source used for the electrical system of the automobile or the like is shared. For this reason, if an excessive current flows through the EHC, the power supply circuit may be damaged. Since various voltages are used for the power source for the EHC, it is important to adjust the resistance of the honeycomb structure for the EHC for each voltage to be used and control it so that an excessive current does not flow.

[0004] Patent Document 1 describes a honeycomb structure in which the partition walls and the outer peripheral wall contain silicon carbide particles as aggregates and silicon as a binder for binding the silicon carbide particles, and the honeycomb structure has a volume electrical resistance of 1 to 40 Ωcm at 400° C. Patent Document 1 describes that the volume electrical resistance of the honeycomb structure at 400° C. can be set to 1 to 40 Ωcm by setting the average particle size of the silicon carbide particles to 3 to 40 μm. It also describes that since the honeycomb structure has a volume electrical resistance of 1 to 40 Ωcm at 400° C., even if a current is passed through it using a high-voltage power source, an excessive current does not flow, and the honeycomb structure can be suitably used as a heater.

[0005] However, a very wide range of voltages is used for the power source of the EHC, depending on, for example, the type of vehicle in which it is installed. In particular, when a low voltage of 60 V or less, for example 48 V, is used for the power source of the EHC, the appropriate volume resistivity for suppressing the generation of excess current is around 0.1 Ω cm. Thus, in recent EHCs that use a wide range of voltages, there is a need for research and development of technology that effectively suppresses the generation of excess current even when used at a low voltage.

[0006] Therefore, Patent Documents 2 and 3 specify the range of the amount of dopant contained in the silicon constituting the EHC. In Patent Documents 2 and 3, the concentration of the dopant in the silicon in the ceramic constituting the partition walls and the outer peripheral wall of the honeycomb structure is set to 1×10 16 ~5×10 20 pieces / cm 3 It is stated that:

[0007] Uniformity of heat generation distribution is also an issue with EHC. Normally, the honeycomb structure has a higher electrical resistivity than the electrode layer, so the current from the terminal connected to the electrode layer tends to be spread in the electrode layer before flowing to the honeycomb structure. This causes a lot of current to flow near the ends of the electrode layer, where the distance it passes through the honeycomb structure is shorter, resulting in uneven heat generation distribution in the honeycomb structure and uneven catalyst heating. Poor heat generation distribution tends to increase the occurrence of cracks, as parts of the EHC generate excessive heat.

[0008] Therefore, Patent Document 4 proposes controlling the distribution of electrical resistivity in end regions near a pair of electrodes of a honeycomb structure and in a central region excluding the end regions. Specifically, it proposes improving the uniformity of heat distribution in the honeycomb structure by making the average electrical resistivity of the material constituting the end regions lower than the average electrical resistivity of the material constituting the central region. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Patent No. 5735428 [Patent Document 2] JP 2020-204300 A [Patent Document 3] JP 2022-142543 A [Patent Document 4] JP 2019-173662 A Summary of the Invention [Problem to be solved by the invention]

[0010] As proposed in Patent Documents 2 and 3, controlling the concentration of dopant in silicon in the ceramics constituting the partition walls and outer peripheral wall of the honeycomb structure is useful for adjusting the volume resistivity of the honeycomb structure. In addition, as proposed in Patent Document 4, controlling the distribution of electrical resistivity within the honeycomb structure is also useful for improving the uniformity of heat generation distribution. However, in a honeycomb structure containing a dopant, there is still room for improving the uniformity of heat generation distribution by a method different from that used up to now.

[0011] The present invention has been made in view of the above circumstances, and an object of one embodiment is to provide a honeycomb structure in which the uniformity of heat distribution is improved by a method different from that of the conventional method. [Means for solving the problem]

[0012] The present inventors conducted extensive research to solve the above problems and found that the non-uniformity of heat generation distribution in a honeycomb structure is due to the cell structure of the honeycomb structure known in the art, as well as the NTC thermistor properties of the materials constituting the honeycomb structure, such as silicon carbide and silicon. In other words, the electrode layer ends of the honeycomb structure, which are prone to heat generation, have a further reduced electrical resistance due to the NTC thermistor properties of silicon and silicon carbide, making it easier for electricity to flow (=easier to generate heat). It was found that if this is repeated, it leads to a large deviation in the heat generation distribution in a cross section perpendicular to the extension direction of the cells of the honeycomb structure, increasing the probability of crack occurrence.

[0013] Therefore, the present inventors believed that alleviating the NTC thermistor characteristics is important for improving the uniformity of the heat generation distribution of the honeycomb structure, and conducted extensive research. As a result, the present inventors found that the NTC thermistor characteristics can be alleviated by appropriately controlling the contents of silicon carbide and silicon, and the predetermined dopant concentration, and the uniformity of the heat generation distribution of the honeycomb structure can be significantly improved. The present invention was completed based on this knowledge, and is exemplified below. [Aspect 1] a ceramic honeycomb structure having an outer peripheral wall and partition walls disposed inside the outer peripheral wall and partitioning a plurality of cells that form a fluid flow path from a first end surface to a second end surface; A pair of electrode layers are provided on the outer surface of the outer peripheral wall, extend in a band shape in the extending direction of the cells, and are provided so as to face each other across the central axis of the honeycomb structure section; Equipped with The honeycomb structure is characterized in that the ceramic contains at least silicon and silicon carbide and satisfies one or both of the following conditions (1) and (2): (1) The ceramic has a silicon content of 21 to 30 mass %, the silicon contains P and B, and the value obtained by subtracting the B concentration from the P concentration in the silicon (PB amount) is 20 mass ppm or more. (2) The ceramic has a silicon carbide content of 50 mass% or more, the silicon carbide contains Al and N, and the value obtained by subtracting the N concentration from the Al concentration in the silicon carbide (Al-N amount) is 130 mass ppm or more and 450 mass ppm or less. [Aspect 2] The honeycomb structure according to embodiment 1, which satisfies both of the above conditions (1) and (2). [Aspect 3] 3. The honeycomb structure according to embodiment 1 or 2, wherein the ceramic satisfies one or both of the following conditions (3) and (4): (3) The ceramic has a silicon content of 21 to 30 mass %, the silicon contains P and B, and the value obtained by subtracting the B concentration from the P concentration in the silicon (PB amount) is 20 mass ppm or more. (4) The ceramic has a silicon carbide content of 50 mass% or more, the silicon carbide contains Al and N, and the value obtained by subtracting the N concentration from the Al concentration in the silicon carbide (Al-N amount) is 300 ppm by mass or more and 450 ppm by mass or less. [Aspect 4] The honeycomb structure according to embodiment 3, which satisfies both of the above conditions (3) and (4). [Aspect 5] 5. The honeycomb structure according to any one of aspects 1 to 4, wherein the total content of silicon and silicon carbide in the ceramic is 80 to 95 mass %. [Aspect 6] 6. The honeycomb structure according to any one of aspects 1 to 5, wherein the ceramic further contains 5 to 20 mass % of silicon oxide. [Aspect 7] 7. The honeycomb structure according to any one of aspects 1 to 6, wherein the partition walls of the honeycomb structure portion have a porosity of 30% or more. [Aspect 8] The volume resistivity (ρ v50 ) versus volume resistivity at 500°C (ρ v500 ) ratio (ρ v500 / ρ v50 8. The honeycomb structure according to any one of aspects 1 to 7, wherein the ratio of the surface roughness to the surface roughness is 0.30 to 0.80. [Aspect 9] A honeycomb structure according to any one of aspects 1 to 8, a metal terminal joined to each of the outer surfaces of the pair of electrode layers; An electrically heated carrier comprising: [Aspect 10] An electrically heated carrier according to embodiment 9; A metal tube containing the electrically heated carrier; An exhaust gas purification device comprising: Effect of the Invention

[0014] According to one embodiment of the present invention, a honeycomb structure with improved uniformity of heat distribution can be provided. By combining with other conventionally known techniques, further improvement in uniformity of heat distribution can be expected. By joining a metal terminal to this honeycomb structure, an electrically heated carrier can be produced. The electrically heated carrier can be suitably used, for example, as a catalyst carrier for an exhaust gas purification device. [Brief description of the drawings]

[0015] [Figure 1] 1 is a schematic diagram of an electrically heated carrier according to an embodiment of the present invention, as viewed from a first end surface. [Diagram 2] FIG. 1 is a schematic perspective view of an electrically heated carrier according to an embodiment of the present invention. [Diagram 3]1 is a schematic cross-sectional view showing an exhaust gas purification device according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Next, the embodiments of the present invention will be described in detail with reference to the drawings. It should be understood that the present invention is not limited to the following embodiments, and that appropriate changes and improvements in the design may be made based on the ordinary knowledge of those skilled in the art without departing from the spirit of the present invention.

[0017] (1. Electrically heated carrier) Fig. 1 is a schematic diagram of an electrically heated support 100 according to an embodiment of the present invention when viewed from a first end surface 116. Fig. 2 is a schematic perspective view of the electrically heated support 100 according to an embodiment of the present invention.

[0018] The electrically heated carrier 100 includes a honeycomb structure 110 and a metal terminal 130. By supporting a catalyst on the electrically heated carrier 100, the electrically heated carrier 100 can be used as a catalyst body. Examples of the catalyst include precious metal catalysts and other catalysts. Precious metal catalysts include three-way catalysts and oxidation catalysts in which precious metals such as platinum (Pt), palladium (Pd), and rhodium (Rh) are supported on the surface of alumina pores and include co-catalysts such as ceria and zirconia, or alkaline earth metals and platinum are used to reduce nitrogen oxides (NO x ) as a storage component of NO x Examples of catalysts that do not use precious metals include NOx storage reduction catalysts (LNT catalysts). x Examples of the catalyst include selective catalytic reduction catalysts (SCR catalysts). Two or more catalysts selected from these catalysts may be used. There is no particular limitation on the method of supporting the catalyst, and any known method for supporting a catalyst on a honeycomb structure may be used.

[0019] (1-1. Honeycomb structure) In one embodiment, the honeycomb structure 110 is a ceramic honeycomb structure having an outer peripheral wall 114 and partition walls 113 disposed inside the outer peripheral wall 114 and partitioning a plurality of cells 115 that form flow paths from a first end surface 116 to a second end surface 118; a first electrode layer 112a provided on the outer surface of the outer peripheral wall 114 and extending in a strip shape in the extension direction of the cells 115; and A second electrode layer 112b is provided on the outer surface of the outer peripheral wall 114, extends in a strip shape in the extending direction of the cells 115, and is provided so as to face the first electrode layer 112a across the central axis O of the honeycomb structure portion. Equipped with.

[0020] The outer shape of the honeycomb structure 110 is not particularly limited, and may be, for example, a columnar body whose end faces are round, such as circular, oval, elliptical, racetrack, or oval, a columnar body whose end faces are polygonal, such as triangular or rectangular, or a columnar body whose end faces have other irregular shapes. The illustrated honeycomb structure 110 has a circular end face shape and is cylindrical as a whole.

[0021] There is no particular limit to the height of the honeycomb structure 110 (the length from one end face to the other end face), and it may be set appropriately depending on the application and required performance. There is also no particular limit to the relationship between the height of the honeycomb structure 110 and the maximum diameter of each end face (the maximum length of the diameters passing through the center of gravity of each end face of the honeycomb structure). Therefore, the height of the honeycomb structure 110 may be longer than the maximum diameter of each end face, or the height of the honeycomb structure 110 may be shorter than the maximum diameter of each end face.

[0022] The size of the honeycomb structure 110 is set to 2,000 to 20,000 mm2 in order to enhance heat resistance (suppress cracks in the circumferential direction of the outer peripheral wall). 2 It is preferable that the thickness is 5000 to 15000 mm. 2 It is more preferable that:

[0023] <Honeycomb structure> The ceramic honeycomb structure portion has a higher volume resistivity than the electrode layers 112a and 112b, but is conductive. The volume resistivity of the honeycomb structure portion is not particularly limited as long as it can generate heat by Joule heat when current is applied, and may be set appropriately according to the voltage to be applied. For example, when measured at 25°C, the volume resistivity may be 0.001 to 500 Ω·cm. For high voltages of more than 60V, the volume resistivity may be 2 to 100 Ω·cm, typically 5 to 100 Ω·cm. For low voltages of 60V or less, such as 48V, the volume resistivity may be 0.001 to 2 Ω·cm, typically 0.001 to 1 Ω·cm, and more typically 0.01 to 1 Ω·cm.

[0024] In one embodiment, the volume resistivity (ρ v50 ) versus volume resistivity at 500°C (ρ v500 ) ratio (ρ v500 / ρ v50 ) is 0.30 or more. v500 / ρ v50 A ρ of 0.30 or more means that the NTC thermistor characteristics are relaxed, and the uniformity of the heat distribution is significantly improved. v500 / ρ v50 is preferably 0.35 or more, more preferably 0.40 or more. In addition, since a silicon-silicon carbide composite material or a ceramic material mainly composed of silicon carbide is used for the honeycomb structure, ρ v500 / ρ v50 The upper limit of is preferably 0.80 or less, more preferably 0.75 or less, and even more preferably 0.70 or less. v500 / ρ v50 is, for example, preferably from 0.30 to 0.80, more preferably from 0.35 to 0.75, and even more preferably from 0.40 to 0.70.

[0025] In this specification, the volume resistivity of the honeycomb structure part is measured by the following procedure. A total of five partition wall samples, each measuring 5 mm x 5 mm x 50 mm (in the cell extension direction), are taken from the honeycomb structure part, and the volume resistivity of each is measured at 25°C by the four-terminal method unless otherwise specified, and the average value of the five samples is regarded as the volume resistivity of the honeycomb structure part. The partition wall samples are taken from near the center in the height direction and radial direction of the honeycomb structure part.

[0026] In one embodiment, the ceramics constituting the honeycomb structure part having the outer peripheral wall 114 and the partition wall 113 contain at least (metallic) silicon and silicon carbide, and preferably the total content of silicon and silicon carbide in the ceramics is 80 to 95 mass%. Typically, the ceramics contain a silicon carbide-silicon composite. From the viewpoint of achieving both heat resistance and electrical conductivity, the ceramics preferably contain a silicon carbide-silicon composite as a main component. When the ceramics are said to contain a silicon carbide-silicon composite as a main component, it means that the silicon carbide-silicon composite (total mass) in the ceramics accounts for 70 mass% or more of the total, and preferably accounts for 80 to 95 mass%. From the viewpoint of alleviating the NTC thermistor characteristics, it is advantageous to adjust the content of silicon and silicon carbide in the ceramics constituting the honeycomb structure part.

[0027] Here, the silicon carbide-silicon composite material contains silicon carbide particles as an aggregate, and (metallic) silicon as a binder for binding the silicon carbide particles. The ceramic may contain one or two aggregates selected from silicon nitride particles and aluminum nitride particles in addition to silicon carbide particles. It may also contain one or more other aggregates. Examples of the other aggregates include oxide ceramics such as alumina, mullite, zirconia, and cordierite.

[0028] However, it is preferable that the main component of the aggregate is silicon carbide, since the thermal conductivity is higher and the difference in thermal expansion coefficient with silicon is smaller. When the main component of the aggregate is silicon carbide, it means that silicon carbide (total mass) accounts for 80 mass% or more of the aggregate, and more preferably accounts for 90 mass% or more of the aggregate.

[0029] The silicon and silicon carbide in the ceramics constituting the honeycomb structure portion may contain one or more dopants. The dopant in silicon and silicon carbide may be, for example, one or more selected from group 13 elements and group 15 elements of the periodic table. For example, group 13 elements include boron (B), aluminum (Al), gallium (Ga), indium (In), etc., and group 15 elements include nitrogen (N), phosphorus (P), arsenic (As), antimony (Sb), bismuth (Bi), etc. Among these, from the viewpoint of alleviating the NTC thermistor characteristics, it is preferable to control at least one of the value obtained by subtracting the B concentration from the P concentration in silicon (PB amount) and the value obtained by subtracting the N concentration from the Al concentration in silicon carbide (Al-N amount), and more preferably to control both.

[0030] Therefore, in the honeycomb structure according to one embodiment of the present invention, the silicon content, the silicon carbide content, the value obtained by subtracting the B concentration from the P concentration in silicon (PB amount), and the value obtained by subtracting the N concentration from the Al concentration in silicon carbide (Al-N amount) in the ceramics constituting the honeycomb structure part preferably satisfy at least one of the following conditions (1) and (2), and more preferably satisfy both conditions. (1) The ceramic has a silicon content of 21 to 30 mass %, the silicon contains P and B, and the amount of PB in the silicon is 20 ppm by mass or more. (2) The ceramic has a silicon carbide content of 50% by mass or more, the silicon carbide contains Al and N, and the amount of Al-N in the silicon carbide is 130 ppm by mass or more and 450 ppm by mass or less.

[0031] It is more preferable that the ceramic satisfies at least one of the following conditions (3) and (4), and it is even more preferable that the ceramic satisfies both conditions. (3) The ceramic has a silicon content of 21 to 30 mass %, the silicon contains P and B, and the amount of PB in the silicon is 20 ppm by mass or more. (4) The ceramic has a silicon carbide content of 50 mass % or more, the silicon carbide contains Al and N, and the amount of Al-N in the silicon carbide is 300 ppm by mass or more and 450 ppm by mass or less.

[0032] The amount of PB in silicon contained in the ceramics may be 20 mass ppm or more, and is preferably 25 mass ppm or more. The upper limit of the amount of PB in silicon contained in the ceramics is not particularly set, but considering the concentration of P and B generally added as dopants in silicon, it is usually 100 mass ppm or less, and typically 90 mass ppm or less. Therefore, the amount of PB in silicon contained in the ceramics is preferably, for example, 20 to 100 mass ppm, more preferably 25 to 90 mass ppm, and can be, for example, 20 to 50 mass ppm.

[0033] From the viewpoint of making the volume resistivity of silicon uniform, the upper limit of the B concentration in silicon contained in the ceramic is preferably 60 mass ppm or less, more preferably 50 mass ppm or less. In addition, even in high purity silicon, a small amount of B is generally added as a dopant, and is 10 mass ppm or more. Therefore, the B concentration in silicon contained in the ceramic is, for example, preferably 10 to 60 mass ppm, more preferably 10 to 50 mass ppm, and can be, for example, 10 to 20 mass ppm.

[0034] As the N dopant concentration in silicon carbide increases, the electrical resistance of the honeycomb structure tends to decrease. From the viewpoint of keeping the electrical resistance of the honeycomb structure within a predetermined range, the N concentration in silicon carbide is, for example, preferably 50 to 500 ppm by mass, more preferably 50 to 450 ppm by mass, and can be, for example, 50 to 200 ppm by mass, or can be 60 to 120 ppm by mass.

[0035] From the viewpoint of alleviating the NTC thermistor characteristics, it is preferable to also control the silicon oxide content in the ceramics constituting the honeycomb structure part. The silicon oxide content in the ceramics is preferably 5 to 20 mass %, for example, 10 to 15 mass %.

[0036] The contents of Si (silicon), SiC (silicon carbide), and SiO2 (silicon oxide) in the ceramics constituting the honeycomb structure can be measured by the following method. In the following method, a calculation method when (doped) silicon and silicon carbide are used as ceramic raw materials will be described. When silicon and silicon carbide are used as ceramic raw materials, the ceramics constituting the honeycomb structure are composed of silicon (Si), silicon carbide (SiC), and silicon oxide (SiO2). The contents of Si (silicon), SiC (silicon carbide), and SiO2 (silicon oxide) in the ceramics can be measured by measuring the amount of silicon element and the amount of oxygen element by the fluorescent X-ray method, and measuring the amount of carbon element by the resistance heating infrared absorption method. Measurement samples are taken from near the center in the height direction and the radial direction of the honeycomb structure. The mass of one sample is 10 g. The average value of the contents of each component in the five samples is regarded as the contents of Si (silicon), SiC (silicon carbide), and SiO2 (silicon oxide) in the ceramic.

[0037] Regarding the amount of SiC (silicon carbide), all carbon elements are assumed to be SiC, and the amount of SiC in the ceramic is calculated by molecular weight calculation. Regarding the amount of SiO2 (silicon oxide), all oxygen elements are assumed to be SiO2, and the amount of SiO2 in the ceramic is calculated by molecular weight calculation. The amount of Si (silicon) can be calculated by subtracting the total amount of Si in SiC and the total amount of Si in SiO2 from the total amount of silicon element from the amount of SiC and SiO2 calculated above. Note that when a ceramic raw material other than silicon carbide is used, the composition of the ceramics that make up the honeycomb structure part based on the ceramic raw material is confirmed, and then the amount of elements can be measured by X-ray fluorescence method or resistance heating infrared absorption method, and the amount of elements can be calculated in the same manner.

[0038] Regarding the P concentration and B concentration in silicon in the ceramics constituting the honeycomb structure, a total of five partition wall samples, each weighing 10 g, were taken from near the center in the height direction and radial direction of the honeycomb structure, and the P concentration and B concentration in silicon of each were measured using the following procedure, and the average value was calculated to obtain the measured value.

[0039] The method for measuring the P and B concentrations in silicon (Si) in the partition wall sample is as follows. According to the silicon separation ICP emission spectroscopy specified in JIS G1322-3:2010 "Metallic Silicon Analysis Method", the partition wall sample is decomposed with nitric acid and hydrofluoric acid, perchloric acid is added, and the sample is heated to generate white smoke of perchloric acid, and silicon is volatilized as silicon tetrafluoride and separated, and then the salts are dissolved in water. Next, the P and B contained in the solution are measured by ICP emission spectroscopy, and the concentrations in the silicon are calculated.

[0040] The Al concentration and N concentration in silicon carbide in the ceramics constituting the honeycomb structure can be measured by the following method. First, a total of five partition wall samples are taken from the honeycomb structure near the center in the height direction and the radial direction of the honeycomb structure. The size of one sample is 1 cm. 3The size is 1 cm x 1 cm x 1 cm cube. The sample is observed with a SEM (scanning electron microscope) (magnification 1000x) and the areas with dark contrast are visually identified as silicon carbide parts. The silicon carbide parts are then analyzed by SIMS (secondary ion mass spectrometry) to determine the Al concentration and N concentration in the silicon carbide. The average values ​​of the Al concentration and N concentration in the five samples are regarded as the Al concentration and N concentration in the silicon carbide of the ceramic.

[0041] The partition walls 113 of the honeycomb structure may be dense, such as in the form of Si-impregnated SiC, but are preferably porous. If the porosity of the partition walls 113 is 30% or more, deformation during firing is more easily suppressed. If the porosity of the partition walls 113 is 60% or less, the strength of the honeycomb structure is sufficiently maintained. Therefore, the porosity of the partition walls 113 is preferably, for example, 30% or more, more preferably 35 to 60% in order to keep the thermistor characteristics within a predetermined range, and even more preferably 37 to 45%. The porosity is a value measured by a mercury porosimeter. Note that dense refers to a porosity of 5% or less.

[0042] The thickness of the partition walls 113 that define the cells 115 is preferably 0.1 to 0.3 mm, and more preferably 0.1 to 0.2 mm. When the thickness of the partition walls 113 is 0.1 mm or more, it is possible to suppress a decrease in the strength of the honeycomb structure section. When the thickness of the partition walls 113 is 0.3 mm or less, it is possible to suppress an increase in pressure loss when exhaust gas is passed through the honeycomb structure section when the honeycomb structure section is used as a catalyst carrier to support a catalyst. In the present invention, the thickness of the partition walls 113 is defined as the length of a portion that passes through the partition walls 113, of a line segment that connects the centers of gravity of adjacent cells 115 in a cross section perpendicular to the extension direction of the cells 115.

[0043] Providing the outer peripheral wall 114 on the honeycomb structure portion is useful from the viewpoint of ensuring the structural strength of the honeycomb structure portion and suppressing leakage of the fluid flowing through the cells 115 from the outer peripheral wall 114. In this respect, the thickness of the outer peripheral wall 114 is preferably 0.1 mm or more, more preferably 0.15 mm or more, and even more preferably 0.2 mm or more. However, if the outer peripheral wall 114 is made too thick, the strength becomes too high, and the strength balance with the partition walls 113 is lost, and the thermal shock resistance is reduced. Therefore, the thickness of the outer peripheral wall 114 is preferably 1.0 mm or less, more preferably 0.7 mm or less, and even more preferably 0.5 mm or less. Therefore, the thickness of the outer peripheral wall 114 is preferably, for example, 0.1 to 1.0 mm, more preferably 0.15 to 0.7 mm, and even more preferably 0.2 to 0.5 mm. Here, the thickness of the outer peripheral wall 114 is defined as the thickness in the normal direction to the tangent to the outer surface of the outer peripheral wall 114 at the measurement point when the portion of the outer peripheral wall 114 where the thickness is to be measured is observed in a cross section perpendicular to the extension direction of the cells 115. preferable.

[0044] The honeycomb structure has a cell density of 40 to 150 cells / cm in a cross section perpendicular to the extension direction of the cells 115. 2 Preferably, the cell density is 70 to 100 cells / cm. 2 By setting the cell density in this range, it is possible to increase the purification performance of the catalyst while reducing the pressure loss when exhaust gas flows through the honeycomb structure. 2 If the cell density is 150 cells / cm or more, the catalyst carrying area is sufficiently secured. 2 When the honeycomb structure 110 is used as a catalyst carrier to support a catalyst, the pressure loss caused by the exhaust gas flowing therethrough is prevented from becoming too large if the honeycomb structure 110 is used as a catalyst carrier to support a catalyst, and the cell density is a value obtained by dividing the number of cells by the area of ​​one end face of the honeycomb structure part on the inner peripheral side than the outer peripheral wall 114.

[0045] Although there is no limitation on the shape of the cells in a cross section perpendicular to the extension direction of the cells 115, a rectangle, a hexagon, an octagon, or a combination of these is preferable. Among these, a rectangle and a hexagon are more preferable. By using such a cell shape, the pressure loss when exhaust gas flows through the honeycomb structure 110 is reduced, and the purification performance of the catalyst is improved. From the viewpoint of easily achieving both structural strength and heating uniformity, a hexagon is particularly preferable.

[0046] The cells 115 may penetrate from the first end face 116 to the second end face 118. In this case, the cells 115 may be open at both the first end face 116 and the second end face 118. Alternatively, a first cell having a plugged first end face 116 and an opening at the second end face 118 and a second cell having an opening at the first end face 116 and a plugged second end face 118 may be alternately arranged adjacent to each other with the partition wall 113 in between.

[0047] <Electrode layer> A first electrode layer 112a and a second electrode layer 112b facing the first electrode layer 112a across the central axis O of the honeycomb structure part can be provided on the outer surface of the outer peripheral wall 114. By disposing the electrode layers 112a and 112b having a lower volume resistivity than the outer peripheral wall 114, the current spreads easily in the circumferential direction of the honeycomb structure 110 and in the extending direction of the cells 115, so that the uniform heat generation of the honeycomb structure 110 can be improved. Referring to FIG. 1, in a cross section perpendicular to the extending direction of the cells 115, the angle θ (0°≦θ≦180°) formed by two line segments extending from the circumferential centers of the pair of electrode layers 112a and 112b to the central axis O (center of gravity) of the honeycomb structure 110 is preferably 150°≦θ≦180°, more preferably 160°≦θ≦180°, even more preferably 170°≦θ≦180°, and most preferably 180°.

[0048] Although there is no particular restriction on the formation region of the pair of electrode layers 112a, 112b, from the viewpoint of improving the uniform heat generation of the honeycomb structure 110, it is preferable that the pair of electrode layers 112a, 112b are each provided in a band shape extending in the circumferential direction of the honeycomb structure 110 and in the extension direction of the cells 115 on the outer surface of the outer peripheral wall 114. Specifically, in a cross section perpendicular to the extension direction of the cells 115, the central angle α formed by two line segments connecting both side ends in the circumferential direction of each electrode layer 112a, 112b and the central axis O (center of gravity) is preferably 30° or more, more preferably 40° or more, and even more preferably 60° or more from the viewpoint of spreading the current in the circumferential direction and improving the uniform heat generation (see FIG. 1). However, if the central angle α is too large, the current passing through the inside of the honeycomb structure 110 decreases, and the current passing through the vicinity of the outer peripheral wall 114 increases. Therefore, from the viewpoint of uniform heat generation of the honeycomb structure 110, the central angle α is preferably 140° or less, more preferably 130° or less, and even more preferably 120° or less. Moreover, it is desirable that each of the electrode layers 112a and 112b extends over 80% or more of the length between both end faces of the honeycomb structure 110, preferably over 90% or more, and more preferably over the entire length. The electrode layers 112a and 112b may be composed of a single layer, or may have a laminated structure in which multiple layers are laminated.

[0049] The thickness of the electrode layers 112a, 112b is preferably 0.01 to 5 mm, and more preferably 0.01 to 3 mm. By setting the thickness in this range, the uniform heat generation can be improved. When the thickness of the electrode layers 112a, 112b is 0.01 mm or more, the electrical resistance is appropriately controlled, and the heat can be generated more uniformly. When the thickness of the electrode layers 112a, 112b is 5 mm or less, the risk of breakage during canning is reduced. The thickness of the electrode layers 112a, 112b is defined as the thickness in the normal direction to the tangent of the outer surface of the electrode layers 112a, 112b at the measurement point when the part of the electrode layers 112a, 112b to be measured for thickness is observed in a cross section perpendicular to the extension direction of the cell 115.

[0050] By making the volume resistivity of the electrode layers 112a, 112b lower than that of the partition walls 113 and the outer peripheral wall 114, electricity flows preferentially through the electrode layers 112a, 112b, and electricity spreads easily in the circumferential direction of the honeycomb structure 110 and in the extension direction of the cells 115 when electricity is applied. The volume resistivity of the electrode layers 112a, 112b is preferably 1 / 10 or less of the volume resistivity of the partition walls 113 and the outer peripheral wall 114, more preferably 1 / 20 or less, and even more preferably 1 / 30 or less. However, if the difference between the volume resistivities of the two becomes too large, current is concentrated between the ends of the opposing electrode layers 112a and 112b, and heat generation in the honeycomb structure 110 is biased, so the volume resistivities of the electrode layers 112a and 112b are preferably 1 / 200 or more, more preferably 1 / 150 or more, and even more preferably 1 / 100 or more of the volume resistivities of the partition walls 113 and the outer peripheral wall 114. Therefore, the volume resistivities of the electrode layers 112a and 112b are, for example, preferably 1 / 200 to 1 / 10 of the volume resistivities of the partition walls 113 and the outer peripheral wall 114, more preferably 1 / 150 to 1 / 20, and even more preferably 1 / 100 to 1 / 30. The volume resistivities of the electrode layers, partition walls, and outer peripheral wall here are values ​​measured at 25°C by a four-terminal method.

[0051] The material of the electrode layers 112a and 112b is not limited, but a composite material (cermet) of metal and ceramic (particularly conductive ceramic) can be used. Examples of metals include, for example, simple metals such as Cr, Fe, Co, Ni, Si, or Ti, or alloys containing at least one metal selected from these metals. Examples of ceramics include, but are not limited to, silicon carbide (SiC), as well as metal compounds such as metal silicides such as tantalum silicide (TaSi2) and chromium silicide (CrSi2). Specific examples of composite materials (cermets) of metal and ceramics include composite materials of silicon and silicon carbide, composite materials of metal silicides such as tantalum silicide and chromium silicide, and silicon and silicon carbide, and composite materials in which one or more of the above metals are added with one or more insulating ceramics such as alumina, mullite, zirconia, cordierite, silicon nitride, and aluminum nitride from the viewpoint of reducing thermal expansion. As the material for the electrode layers 112a, 112b, among the various metals and ceramics mentioned above, a composite material of a metal silicide such as tantalum silicide or chromium silicide, silicon, and silicon carbide is preferable because it can be fired simultaneously with the partition wall and the outer peripheral wall, which contributes to simplifying the manufacturing process.

[0052] (1-2. Metal terminal) The metal terminal 130 can be directly or indirectly joined to the outer surfaces of the pair of electrode layers 112a, 112b. When a voltage is applied to the honeycomb structure 110 via the metal terminal 130, electricity is passed through the honeycomb structure 110, and the honeycomb structure 110 can generate heat by Joule heat. Therefore, the honeycomb structure 110 can be suitably used as a heater. This makes it possible to improve the uniform heat generation of the honeycomb structure 110. The voltage to be applied is preferably 12 to 900 V, more preferably 48 to 600 V, but the voltage to be applied can be changed as appropriate.

[0053] The metal terminal 130 and the electrode layers 112a, 112b may be directly bonded to each other, or may be bonded to each other via one or more base layers 120 in order to reduce the thermal expansion difference between the electrode layers 112a, 112b and the metal terminal 130 and improve the bonding reliability of the metal terminal 130. Therefore, in a preferred embodiment, the honeycomb structure 110 has a first electrode layer 112a and a second electrode layer 112b disposed on the outer peripheral wall 114 so as to face each other across the central axis O (center of gravity) of the honeycomb structure 110, and one or more metal terminals 130 are bonded to each of the electrode layers 112a, 112b via the base layers 120.

[0054] From the viewpoint of improving the bonding reliability, it is preferable that the thermal expansion coefficient gradually decreases in the order of metal terminal 130 → (underlying layer 120) → electrode layers 112a, 112b → outer peripheral wall 114. Note that the "thermal expansion coefficient" here means the linear expansion coefficient measured according to JIS R1618:2002 when the temperature is changed from 25°C to 800°C.

[0055] The material of the metal terminal 130 is not particularly limited as long as it is a metal, and a single metal or an alloy can be adopted, but from the viewpoint of corrosion resistance, volume resistivity, and linear expansion coefficient, for example, an alloy containing at least one selected from the group consisting of Cr, Fe, Co, Ni, and Ti is preferable, and stainless steel and an Fe-Ni alloy are more preferable. The number, shape, and size of the metal terminal 130 are not particularly limited, and can be appropriately designed depending on the size and current-carrying performance of the honeycomb structure 110.

[0056] The material of the underlayer 120 is not limited, but may be a composite material (cermet) of metal and ceramics (particularly conductive ceramics). The thermal expansion coefficient of the underlayer 120 can be controlled by adjusting the compounding ratio of the metal and ceramics, for example.

[0057] The underlayer 120 preferably contains, but is not limited to, one or more metals selected from a Ni-based alloy, an Fe-based alloy, a Ti-based alloy, a Co-based alloy, silicon, and Cr.

[0058] The underlayer 120 preferably contains one or more ceramics selected from oxide ceramics such as alumina, mullite, zirconia, glass, and cordierite, and non-oxide ceramics such as silicon carbide, silicon nitride, and aluminum nitride, although this is not limited thereto.

[0059] The thickness of the underlayer 120 is not particularly limited, but is preferably 0.1 to 1.5 mm, and more preferably 0.3 to 0.5 mm, from the viewpoint of crack suppression. The thickness of the underlayer 120 is defined as the thickness in the normal direction to the tangent of the outer surface of the underlayer 120 at the measurement point when the underlayer 120 whose thickness is to be measured is observed in a cross section perpendicular to the cell extension direction.

[0060] The method for joining the metal terminal 130 to the electrode layers 112a, 112b or the underlayer 120 is not particularly limited, but examples thereof include thermal spraying, welding, and brazing.

[0061] (2. Exhaust gas purification equipment) The electrically heated carrier according to one embodiment of the present invention can be used in an exhaust gas purification device. Referring to Fig. 3, an exhaust gas purification device 200 has an electrically heated carrier 100 and a metal tube 220 that houses the electrically heated carrier 100. An electric wire 240 for power supply can be connected to a metal terminal 130 of the electrically heated carrier 100. Metals constituting the metal tube 220 include, but are not limited to, various stainless steels such as chromium-based stainless steel. By using these metals, an exhaust gas purification device having high heat resistance and corrosion resistance can be obtained.

[0062] In the exhaust gas purification device 200, the electrically heated carrier 100 can be installed in the middle of a flow path of a fluid such as automobile exhaust gas. The electrically heated carrier 100 can be fixed in the metal tube 220 by, for example, push-in canning, in which the electrically heated carrier 100 is pushed into the metal tube 220 and fitted in a positional relationship in which the extension direction of the cells and the extension direction of the metal tube 220 coincide. It is preferable to dispose a retaining material (mat) 260 between the metal tube 220 and the electrically heated carrier 100. The material constituting the retaining material (mat) 260 is not limited, but examples thereof include ceramics such as alumina fiber, mullite fiber, and ceramic fiber mainly composed of alumina-silica.

[0063] (3. Manufacturing method) Next, a method for manufacturing a honeycomb structure according to one embodiment of the present invention will be described. The honeycomb structure can be manufactured by a manufacturing method including a step 1 of preparing a clay, a step 2 of forming the clay to obtain a honeycomb molded body, a step 3 of applying a pair of electrode layer forming pastes to the outer surface of the outer peripheral wall so as to extend in a band shape in the cell extension direction across the central axis of the honeycomb molded body, thereby preparing a honeycomb molded body with electrode layer forming paste, and a step 4 of firing the honeycomb molded body to prepare a honeycomb fired body.

[0064] (Process 1) In step 1, a molding raw material containing silicon carbide powder and (metallic) silicon powder is kneaded to prepare a clay. One or both of the silicon carbide powder and silicon powder can be appropriately doped with a dopant such as B, Al, N, or P. The dopant concentration in the silicon carbide powder and silicon powder can be adjusted, for example, by adding a small amount of a dopant element when producing the molding raw material, or by mixing molding raw materials having different dopant amounts in any ratio. In addition, for doping P and B into silicon, a method of incorporating the dopant source in the clay by kneading an aqueous solution containing a predetermined amount of a dopant source (such as a water-soluble inorganic salt or a water-soluble organic compound) with the molding raw material and doping the dopant source during firing can also be mentioned.

[0065] The mass of the metal silicon powder in the forming raw material is preferably 20 to 80 parts by mass, more preferably 25 to 60 parts by mass, and even more preferably 25 to 45 parts by mass, when the total mass of the silicon carbide powder and the metal silicon powder is 100 parts by mass. The average particle size of the silicon carbide particles in the silicon carbide powder is preferably 3 to 50 μm, more preferably 3 to 40 μm. The average particle size of the metal silicon particles in the metal silicon powder is preferably 2 to 35 μm, more preferably 2 to 25 μm. The average particle size of the silicon carbide particles and the metal silicon particles refers to the arithmetic mean diameter based on the volume when the frequency distribution of the particle size is measured by a laser diffraction method. The silicon carbide particles are fine particles of silicon carbide that constitute the silicon carbide powder, and the metal silicon particles are fine particles of metal silicon that constitute the metal silicon powder.

[0066] The content of water in the forming raw material is, for example, preferably 20 to 60 parts by mass, and more preferably 25 to 50 parts by mass, when the total mass of the silicon carbide powder and the metallic silicon powder is taken as 100 parts by mass.

[0067] In step 1, the forming raw materials are kneaded to prepare a clay. Any appropriate device or mechanism can be used as the kneading means. Specific examples include a kneader and a vacuum clay kneader.

[0068] The forming raw material may contain a binder, a surfactant, and a pore former in addition to the silicon carbide powder and the silicon powder.

[0069] Examples of the binder include methyl cellulose, hydroxypropyl methyl cellulose, hydroxypropoxyl cellulose, hydroxyethyl cellulose, carboxymethyl cellulose, polyvinyl alcohol, etc. Among these, it is preferable to use methyl cellulose and hydroxypropoxyl cellulose in combination. The content of the binder is preferably 2.0 to 10.0 parts by mass when the total mass of the silicon carbide powder and the silicon powder is 100 parts by mass.

[0070] The surfactant may be ethylene glycol, dextrin, fatty acid soap, polyalcohol, etc. These may be used alone or in combination of two or more. The content of the surfactant is preferably 0.1 to 2.0 parts by mass when the total mass of the silicon carbide powder and the silicon powder is 100 parts by mass.

[0071] The pore-forming material is not particularly limited as long as it becomes pores after firing, and examples thereof include graphite, starch, foamed resin, water-absorbent resin, silica gel, etc. The content of the pore-forming material is preferably 0.5 to 10.0 parts by mass when the total mass of the silicon carbide powder and the silicon powder is 100 parts by mass. The average particle diameter of the pore-forming material is preferably 10 to 30 μm. The average particle diameter of the pore-forming material refers to the arithmetic mean diameter based on volume when the frequency distribution of particle size is measured by a laser diffraction method. When the pore-forming material is a water-absorbent resin, the average particle diameter of the pore-forming material refers to the average particle diameter after water absorption.

[0072] (Process 2) In step 2, the clay produced in step 1 is molded to obtain a honeycomb molded body. Specifically, the clay is extrusion molded to produce a columnar honeycomb molded body having an outer peripheral wall and partition walls. A die having a desired overall shape, cell shape, partition wall thickness, cell density, etc. can be used during extrusion molding. Next, it is preferable to dry the obtained honeycomb molded body. If the length of the honeycomb molded body in the cell extension direction is not the desired length, both ends of the honeycomb molded body can be cut to the desired length. The honeycomb molded body after drying is called a honeycomb dried body.

[0073] The honeycomb formed body may be fired once as a modified example of step 2. That is, in this modified example, the honeycomb formed body is fired to prepare a honeycomb fired body, and step 3 is then carried out on the honeycomb fired body.

[0074] (Step 3) Step 3 is a step of applying a pair of electrode layer forming pastes to the outer surface of the outer peripheral wall of the honeycomb molded body so as to extend in a band shape in the extending direction of the cells across the central axis of the honeycomb molded body, thereby producing a honeycomb molded body with the electrode layer forming paste. The electrode layer forming paste can be formed by appropriately adding various additives to raw material powders (metal powders, ceramic powders, etc.) mixed according to the required characteristics of the electrode layer, and kneading them. The average particle diameter of the raw material powders is not limited, but is preferably, for example, 5 to 50 μm, and more preferably 10 to 30 μm. The average particle diameter of the raw material powders refers to the arithmetic mean diameter based on volume when the frequency distribution of particle size is measured by a laser diffraction method.

[0075] Next, the obtained electrode layer forming paste is applied to required locations on the outer surface of the outer peripheral wall of a honeycomb formed body (typically a dried honeycomb body) to obtain a honeycomb formed body with the electrode layer forming paste. The method of preparing the electrode layer forming paste and the method of applying the electrode layer forming paste to the honeycomb formed body can be performed in accordance with a known method for manufacturing a honeycomb structure, but in order to give the electrode layer a lower volume resistivity than the outer peripheral wall and the partition walls, the metal content can be made higher than that of the outer peripheral wall and the partition walls, or the particle size of the metal particles in the raw material powder can be made smaller. After application, it is preferable to dry the electrode layer forming paste.

[0076] (Step 4) Step 4 is a step of firing the honeycomb molded body with the electrode layer forming paste to obtain a honeycomb fired body, i.e., the desired honeycomb structure. Before firing, degreasing may be performed to remove binders and the like. The method of degreasing and firing is not particularly limited, and firing can be performed using an electric furnace, a gas furnace, or the like. The firing conditions vary depending on the material of the honeycomb structure, but are preferably heated at 1400 to 1500°C for 1 to 20 hours in an inert atmosphere such as nitrogen or argon.

[0077] By joining a metal terminal to the electrode layer of the honeycomb structure thus obtained, an electrically heated carrier can be manufactured. The joining method is not particularly limited, and examples thereof include thermal spraying, welding, and brazing. In order to improve the joining property between the electrode layer and the metal terminal, a base layer may be formed by a method such as thermal spraying.

[0078] An appropriate catalyst may be supported on the electrically heated carrier depending on the application. An example of a method for supporting a catalyst on a honeycomb structure is a method in which a catalyst slurry is introduced into cells by a conventionally known suction method or the like, and is attached to the surfaces and pores of the partition walls, and then a high-temperature treatment is performed to bake the catalyst contained in the catalyst slurry onto the partition walls and support the catalyst. EXAMPLES

[0079] The following examples are provided to better understand the present invention and its advantages, but the present invention is not limited to these examples.

[0080] <Example 1> (1. Making cylindrical clay pots) 30 g of phosphoric acid ester salt and 12.5 g of boric acid were added to 30 kg of pure water and stirred for 20 minutes to obtain an aqueous solution containing P and B. Next, silicon carbide (SiC) powder doped with Al and N and silicon (Si) powder were mixed in a mass ratio of 65:35 to prepare a ceramic raw material. The amount of Al and N to be doped into SiC (silicon carbide) was adjusted by mixing SiC (silicon carbide) with different doping amounts of Al and N. Hydroxypropyl methylcellulose as a binder and a water-absorbent resin as a pore former were added to this ceramic raw material, and the aqueous solution containing P and B was added to prepare a molding raw material. Next, the molding raw material was kneaded using a vacuum kneader to prepare a cylindrical clay.

[0081] In the molding raw material, the content of the binder was 7 parts by mass when the total of the silicon carbide (SiC) powder and the silicon (Si) powder was 100 parts by mass. The content of the pore former was 3 parts by mass when the total of the silicon carbide (SiC) powder and the silicon (Si) powder was 100 parts by mass. The content of the aqueous solution was 30 parts by mass when the total of the silicon carbide (SiC) powder and the silicon (Si) powder was 100 parts by mass. The average particle diameter of the silicon carbide powder was 20 μm, and the average particle diameter of the silicon powder was 6 μm. The average particle diameter of the pore former was 20 μm. The average particle diameters of the silicon carbide powder, the silicon powder, and the pore former refer to the arithmetic mean diameter based on the volume when the frequency distribution of the particle size is measured by the laser diffraction method.

[0082] (2. Preparation of dried honeycomb body) The obtained cylindrical clay was molded using an extrusion molding machine with a predetermined die structure to obtain a cylindrical honeycomb molded body in which each cell shape in a cross section perpendicular to the cell extension direction is hexagonal. This honeycomb molded body was dried by high-frequency dielectric heating, and then further dried in an air atmosphere at 120°C for 2 hours using a hot air dryer, and both end faces were cut by a predetermined amount to produce a dried honeycomb body.

[0083] (3. Preparation of electrode layer forming paste) Silicon (Si) powder, silicon carbide (SiC) powder, methyl cellulose, glycerin, and water were mixed with a centrifugal mixer to prepare an electrode layer forming paste. The Si powder and the SiC powder were mixed so that the volume ratio of the Si powder:SiC powder was 40:60. In addition, when the total of the Si powder and the SiC powder was 100 parts by mass, the amount of the methyl cellulose was 0.5 parts by mass, the amount of the glycerin was 10 parts by mass, and the amount of the water was 38 parts by mass. The average particle diameter of the silicon powder was 6 μm. The average particle diameter of the silicon carbide powder was 35 μm. These average particle diameters refer to the arithmetic mean diameter based on the volume when the frequency distribution of the particle size was measured by the laser diffraction method.

[0084] (4. Application of electrode layer forming paste) The electrode layer forming paste was applied to two locations on the outer surface of the outer peripheral wall of the honeycomb dried body by a curved surface printer so as to face each other across the central axis. Each application was formed in a strip shape over the entire length between both end faces of the honeycomb dried body (angle θ=180°, central angle α=127°). Next, the electrode layer forming paste applied to the honeycomb dried body was dried to obtain a honeycomb dried body with the electrode layer forming paste. The drying temperature was 70°C.

[0085] (5. Firing) The obtained honeycomb dried body with the electrode layer forming paste was degreased in an air atmosphere at 550°C for 3 hours. Next, the degreased honeycomb dried body was fired in an argon atmosphere at 1450°C for 2 hours to obtain a cylindrical honeycomb structure. The honeycomb structures were manufactured in the number required for the following tests.

[0086] (6. Specifications of honeycomb structure) The honeycomb structure obtained above had a circular end face with a diameter of 80 mm, a height (length in the cell extension direction) of 80 mm, a partition wall thickness of 125 mm, an outer peripheral wall thickness of 0.5 mm, and a cell density of 90 cells / cm. 2 The porosity of the partition walls was 38%.

[0087] (7. Content of Si, SiC, and SiO2) The contents of Si (silicon), SiC (silicon carbide), and SiO2 (silicon oxide) in the ceramics constituting the honeycomb structure part of the honeycomb structure obtained above were measured according to the above-mentioned method. The results are shown in Table 1.

[0088] (8. Dopant Concentration in Silicon) The P concentration and B concentration in silicon (Si) in the ceramics constituting the honeycomb structure part of the honeycomb structure obtained above were measured according to the method described above. The ICP (inductively coupled plasma) analyzer used was a Hitachi High-Technologies Corporation model PS3510DD. The results are shown in Table 1.

[0089] (9. Dopant Concentration in Silicon Carbide) The Al concentration and N concentration in silicon carbide (SiC) in the ceramics constituting the honeycomb structure part of the honeycomb structure obtained above were measured according to the method described above. As the SEM, Hitachi High-Technologies Corporation's model S-3400N was used, and as the SIMS, CAMECA Corporation's model NanoSIMS 50L was used. The results are shown in Table 1.

[0090] (10. Volume resistivity measurement) The volume resistivity of the honeycomb structure part of the honeycomb structure obtained above at 25° C. was measured according to the above-mentioned method. The results are shown in Table 1.

[0091] (11. NTC thermistor characteristics: ρ v500 / ρ v50 ) Volume resistivity of honeycomb structure at 50℃ (ρ v50 ) versus volume resistivity at 500°C (ρ v500 ) ratio (ρ v500 / ρ v50 ) was measured according to the method described above, and the results are shown in Table 1.

[0092] (12. Porosity) A partition wall sample was taken from the honeycomb structure portion of the honeycomb structure obtained above, and the porosity was measured by a mercury porosimeter. The results are shown in Table 1.

[0093] (13. Heat distribution) A voltage of 400 V was applied to the center of the surface of each of the pair of electrode layers of the honeycomb structure obtained above for 20 seconds, and the temperature distribution on both end faces and the outer wall of the honeycomb structure was observed by thermography to evaluate the uniformity of the heat generation distribution. The evaluation criteria were as follows. The results are shown in Table 1. A: When electricity is applied to the honeycomb structure, the difference between the maximum and minimum temperatures is within +150° C. compared with the difference between the maximum and minimum temperatures in Example 1. B: When electricity is applied to the honeycomb structure, the difference between the maximum and minimum temperatures is greater than +150° C. and within +250° C. as compared with the difference between the maximum and minimum temperatures in Example 1. C: When electricity was applied to the honeycomb structure, the difference between the maximum and minimum temperatures was more than +250° C. compared to the difference between the maximum and minimum temperatures in Example 1, and there was concern about the effect on cracks.

[0094] <Examples 2 to 3> The compounding ratio of silicon carbide (SiC) powder and silicon (Si) powder in the forming raw material was changed so that the contents of Si (silicon), SiC (silicon carbide), and SiO2 (silicon oxide) in the ceramics constituting the honeycomb structure part of the honeycomb structure became the values ​​shown in Table 1. In addition, the concentrations of P and B in the aqueous solution containing P and B were adjusted so that the B concentration and P concentration in Si became the same as in Example 1. A honeycomb structure was produced in the same manner as in Example 1 except for the above. The obtained honeycomb structure was subjected to the same characteristic evaluation as in Example 1. The results are shown in Table 1.

[0095] <Example 4> A honeycomb structure was produced in the same manner as in Example 2, except that the amounts of P and B doped into Si (silicon) were changed by changing the concentrations of P and B in the aqueous solution containing P and B. The obtained honeycomb structure was subjected to the same characteristic evaluation as in Example 1. The results are shown in Table 1.

[0096] <Examples 5, 6, and 8> A honeycomb structure was produced in the same manner as in Example 1, except that the amounts of P and B doped into Si (silicon) were changed by changing the concentrations of P and B in the aqueous solution containing P and B. The obtained honeycomb structure was subjected to the same characteristic evaluation as in Example 1. The results are shown in Table 1.

[0097] <Example 7> The compounding ratio of silicon carbide (SiC) powder and silicon (Si) powder in the raw material was changed so that the contents of Si (silicon), SiC (silicon carbide), and SiO2 (silicon oxide) in the ceramics constituting the honeycomb structure part of the honeycomb structure were the values ​​shown in Table 1. In addition, the concentrations of P and B in the aqueous solution containing P and B were adjusted so that the B concentration and P concentration in Si were the same as in Example 6. A honeycomb structure was produced in the same manner as in Example 6 except for the above. The obtained honeycomb structure was subjected to the same characteristic evaluation as in Example 1. The results are shown in Table 1.

[0098] <Example 9> A honeycomb structure was produced in the same manner as in Example 3, except that the amount of P and B doped into Si (silicon) was changed by changing the concentration of P and B in the aqueous solution containing P and B. The obtained honeycomb structure was subjected to the same characteristic evaluation as in Example 1. The results are shown in Table 1.

[0099] <Example 10> A honeycomb structure was produced in the same manner as in Example 2, except that the amount of Al and N doped in SiC (silicon carbide) was changed by mixing SiC (silicon carbide) with different doping amounts of Al and N. The obtained honeycomb structure was subjected to the same characteristic evaluation as in Example 1. The results are shown in Table 1.

[0100] <Examples 11 to 18> A honeycomb structure was produced in the same manner as in Example 1, except that the amount of Al and N doped in SiC (silicon carbide) was changed by mixing SiC (silicon carbide) with different doping amounts of Al and N. The obtained honeycomb structure was subjected to the same characteristic evaluation as in Example 1. The results are shown in Table 1.

[0101] <Comparative Example 1> A honeycomb structure was produced in the same manner as in Example 1, except that the amount of P and B doped into Si (silicon) was changed by changing the concentration of P and B in an aqueous solution containing P and B, and the amount of Al and N doped into SiC (silicon carbide) was changed by mixing SiC (silicon carbide) with different doping amounts of Al and N. The obtained honeycomb structure was subjected to the same characteristic evaluation as in Example 1. The results are shown in Table 1.

[0102] <Comparative Example 2> The compounding ratio of silicon carbide (SiC) powder and silicon (Si) powder in the forming raw material was changed so that the contents of Si (silicon), SiC (silicon carbide), and SiO2 (silicon oxide) in the ceramics constituting the honeycomb structure part of the honeycomb structure were the values ​​shown in Table 1. The amount of P and B doped in Si (silicon) was changed by changing the concentrations of P and B in the aqueous solution containing P and B, and the amount of Al and N doped in SiC (silicon carbide) was changed by mixing SiC (silicon carbide) with different doping amounts of Al and N. The honeycomb structure was otherwise manufactured in the same manner as in Example 1. The obtained honeycomb structure was subjected to the same characteristic evaluation as in Example 1. The results are shown in Table 1.

[0103] [Table 1]

[0104] As can be seen from the above examples and comparative examples, by appropriately controlling the silicon carbide and silicon contents, PB amount, and Al-N amount in the ceramics constituting the honeycomb structure portion, the NTC thermistor characteristics are mitigated and the uniformity of the heat distribution of the honeycomb structure is significantly improved. [Explanation of symbols]

[0105] 100: Electrically heated carrier 110: Honeycomb structure 112a: First electrode layer 112b: Second electrode layer 113: Bulkhead 114:Outer wall 115: Cell 116: First end surface 118: Second end face 120: Base layer 130: Metal terminal 200: Exhaust gas purification equipment 220: Metal tube 240: Electric wire

Claims

1. a ceramic honeycomb structure having an outer peripheral wall and partition walls disposed inside the outer peripheral wall and partitioning a plurality of cells that form a fluid flow path from a first end surface to a second end surface; A pair of electrode layers are provided on the outer surface of the outer peripheral wall, extend in a band shape in the extending direction of the cells, and are provided so as to face each other across the central axis of the honeycomb structure section; Equipped with The ceramics contain at least silicon and silicon carbide, and the honeycomb structure satisfies one or both of the following conditions (1) and (2): (1) The silicon content in the ceramic is 21 to 30 mass %, the silicon contains P and B, and the value obtained by subtracting the B concentration from the P concentration in the silicon (P-B amount) is 20 mass ppm or more. (2) The ceramic has a silicon carbide content of 50 mass% or more, the silicon carbide contains Al and N, and the value obtained by subtracting the N concentration from the Al concentration in the silicon carbide (Al-N amount) is 130 ppm by mass or more and 450 ppm by mass or less.

2. 2. The honeycomb structure according to claim 1, which satisfies both of the conditions (1) and (2).

3. 3. The honeycomb structure according to claim 1, wherein the ceramic satisfies one or both of the following conditions (3) and (4): (3) The silicon content in the ceramic is 21 to 30 mass %, the silicon contains P and B, and the value obtained by subtracting the B concentration from the P concentration in the silicon (P-B amount) is 20 mass ppm or more. (4) The ceramic has a silicon carbide content of 50 mass % or more, the silicon carbide contains Al and N, and the value obtained by subtracting the N concentration from the Al concentration in the silicon carbide (Al-N amount) is 300 ppm by mass or more and 450 ppm by mass or less.

4. 4. The honeycomb structure according to claim 3, which satisfies both of the conditions (3) and (4).

5. 3. The honeycomb structure according to claim 1, wherein the total content of silicon and silicon carbide in said ceramic is 80 to 95 mass %.

6. 3. The honeycomb structure according to claim 1, wherein the ceramic further contains 5 to 20 mass % of silicon oxide.

7. 3. The honeycomb structure according to claim 1, wherein the partition walls of the honeycomb structure portion have a porosity of 30% or more.

8. The volume resistivity (ρ v50 ) versus volume resistivity at 500°C (ρ v500 ) ratio (ρ v500 / ρ v50 3. The honeycomb structure according to claim 1, wherein the ratio of the surface roughness to the surface roughness is 0.30 to 0.

80.

9. The honeycomb structure according to claim 1 or 2, a metal terminal joined to each of the outer surfaces of the pair of electrode layers; An electrically heated carrier comprising:

10. An electrically heated carrier according to claim 9; A metal tube containing the electrically heated carrier; An exhaust gas purification device comprising:

Citation Information

Patent Citations

  • Method for producing conductive ceramic sintered compact

    JP2012214306A

  • Honey-comb structure and electric heating carrier

    JP2022142543A

  • Single side band radio receiver

    JP1982035428A

  • Honeycomb structure body

    JP2019173662A

  • Honeycomb structure, electric heating-type honeycomb structure, electric heating-type carrier and exhaust emission control device

    JP2020204300A

Cited By

  • Honeycomb structure

    WO2026204348A1

  • Honeycomb structure

    WO2026204349A1