Polymer particle group and method for producing the same, and resin composition
A polymer particle group with controlled siloxane units and vinyl monomers forms a core-shell structure to enhance transparency and impact strength in molded articles, addressing the transparency and strength issues of polyorganosiloxane-based compositions.
Patent Information
- Application Number
- JP2023212138
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2023-12-15
- Publication Date
- 2024-10-11
AI Technical Summary
Existing polymer compositions containing polyorganosiloxane suffer from inadequate transparency and impact strength, particularly when blended with resins having a higher refractive index, leading to decreased transparency in molded products.
A polymer particle group comprising polyorganosiloxane with aryl groups and controlled particle size, combined with a specific mass ratio of siloxane units and vinyl monomers, forms a core-shell or sea-island structure to enhance transparency and impact strength.
The solution achieves both improved transparency and impact strength in molded articles by optimizing the composition and structure of the polymer particles, resulting in better mechanical properties and appearance.
Smart Images

Figure 2024144078000001 
Figure 2024144078000002 
Figure 2024144078000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polymer particle group, a production method thereof, and a resin composition. [Background technology]
[0002] Rubber-containing polymers, in which vinyl monomers are polymerized on rubber polymers, can be dispersed in a wide variety of resins while maintaining a specified rubber particle size and rubber structure, and are therefore suitable for use in resins requiring impact strength. In general, it is preferable to use a rubbery polymer with a low elastic modulus and a high Poisson's ratio in terms of improving impact strength. Butadiene rubber and silicone rubber are preferably used as rubbery polymers because they have an extremely high Poisson's ratio of 0.5 and a low elastic modulus. Among them, silicone rubber is less susceptible to hardening or coloring due to heat or ultraviolet rays and has excellent durability compared to butadiene rubber, and is therefore preferably used in applications requiring long-term maintenance of mechanical properties such as building materials and automobile parts, etc. Polyorganosiloxanes, typified by polydimethylsiloxane, are used as silicone rubbers.
[0003] However, polyorganosiloxane is more expensive than butadiene rubber, and when a polyorganosiloxane-containing polymer is blended with a resin (such as polycarbonate, polymethyl methacrylate, or styrene-acrylonitrile copolymer) having a higher refractive index than the polyorganosiloxane-containing polymer to form a molded article, there is a problem that the transparency of the molded article decreases.
[0004] In Patent Document 1, the transparency of the resulting molded article is improved by using a polymer particle group (C) characterized in that at least one monomer unit (B') selected from a vinyl cyanide monomer unit, an aromatic alkenyl unit, and an alkyl (meth)acrylate unit is graft polymerized onto an aryl group-containing polyorganosiloxane (A). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2002-20438 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, in Patent Document 1, there is a problem in that the obtained molded article does not sufficiently achieve both transparency and impact strength. An object of the present invention is to provide a polymer particle group capable of giving a molded article having both transparency and impact strength, a method for producing the same, and a resin composition. [Means for solving the problem]
[0007] The present invention has the following aspects. [1] A polymer particle group containing a polyorganosiloxane having a siloxane unit containing an aryl group, A group of polymer particles having an average particle size of 200 nm or less as measured by absorbance method. [2] The group of polymer particles according to [1], wherein the aryl group-containing siloxane unit is represented by the following general formula (1):
[0008] [ka]
[0009] In formula (1), Ar is an aryl group, and R is a hydrogen atom, a halogen atom, an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, an aryl group having 5 to 12 carbon atoms, or a halogenated alkyl group having 1 to 3 carbon atoms. [3] The group of polymer particles according to [1] or [2], wherein the polyorganosiloxane further contains a siloxane unit that does not contain an aryl group. [4] The group of polymer particles according to [3], wherein the content of the siloxane units containing an aryl group is 5 to 80 parts by mass, and the content of the siloxane units not containing an aryl group is 20 to 95 parts by mass, based on the total content of the siloxane units containing an aryl group and the siloxane units not containing an aryl group. [5] The group of polymer particles according to any one of [1] to [4], which contains a structural unit derived from a vinyl monomer (a). [6] The group of polymer particles according to [3] or [4], wherein a mass ratio of [the total content of the siloxane units containing an aryl group and the siloxane units not containing an aryl group] / [the content of the structural units derived from the vinyl monomer (a)] is 3 / 97 to 50 / 50. [7] The group of polymer particles according to any one of [1] to [6], wherein the polyorganosiloxane has a refractive index of 1.410 to 1.560. [8] A polymer particle group obtained by polymerizing a vinyl monomer (a) in the presence of a latex of a polymer having a siloxane unit containing an aryl group to obtain a polymer complex, and then polymerizing a vinyl monomer (b) thereto, A group of polymer particles having an average particle size of 200 nm or less as measured by absorbance method. [9] A step of polymerizing an organosiloxane containing an aryl group to obtain a polyorganosiloxane; and polymerizing the polyorganosiloxane with a vinyl monomer (a) to obtain a polymer composite.
[10] A method for producing polymer particles, comprising the step of polymerizing the polymer complex obtained by the method according to [9] with a vinyl monomer (b) to obtain polymer particles.
[11] The method for producing a polymer particle group according to
[10] , wherein the organosiloxane containing an aryl group has a viscosity at 15° C. of 0.5 to 35.0 mPa s.
[12] The method for producing a polymer particle group according to
[10] or
[11] , wherein the organosiloxane containing an aryl group is represented by the following general formula (2):
[0010] [ka]
[0011] In formula (2), Ar is an aryl group, and R1, R2, and R3 each independently represent a hydrogen atom, a halogen atom, an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, an aryl group having 5 to 12 carbon atoms, or a halogenated alkyl group having 1 to 3 carbon atoms.
[13] A resin composition comprising the polymer particles according to any one of [1] to [8] and a thermoplastic resin.
[14] The resin composition according to
[13] , wherein a mass ratio represented by [content of the polymer particle group] / [content of the thermoplastic resin] is 10 / 90 to 50 / 50.
[15] The resin composition according to
[13] or
[14] , wherein the thermoplastic resin is an acrylic resin or an aliphatic polyester resin. Effect of the Invention
[0012] According to the present invention, it is possible to provide a polymer particle group capable of giving a molded article having both transparency and impact strength, a production method thereof, and a resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an embodiment of the present invention will be described in detail. In the present invention, the vinyl monomer is a compound having a polymerizable double bond. "(Meth)acrylate" means acrylate or methacrylate.
[0014] [Polymer Particle Group] The polymer particle group according to one embodiment of the present invention (hereinafter, also simply referred to as "polymer particle group (C)") is obtained by graft polymerizing a second vinyl monomer (b) to a polymer complex (hereinafter, also simply referred to as "polymer (A)"), and includes a graft copolymer (C1) in which a constitutional unit derived from the second vinyl monomer (b) forms a covalent bond with the polymer (A). The polymer particle group (C) of the present invention may further include a polymer complex (C2) containing a free polymer composed of the second vinyl monomer (b) and the polymer (A) in addition to the graft copolymer (C1), in which the free polymer is physically adsorbed on the outer surface of the polymer (A) without forming a covalent bond with the polymer (A). Hereinafter, the graft layer containing the constitutional unit derived from the second vinyl monomer (b) in the graft copolymer (C1) and the free polymer containing the constitutional unit derived from the second vinyl monomer (b) in the polymer complex (C2) are collectively referred to as "vinyl polymer (B)".
[0015] The polymer particle group (C) contains a polyorganosiloxane having a siloxane unit containing an aryl group (hereinafter, also referred to as "polyorganosiloxane (A1)").
[0016] The particle size of the polymer particle group (C) measured by the absorbance method is 200 nm or less, preferably 10 nm to 150 nm, more preferably 50 nm to 120 nm. If the particle size measured by the absorbance method is not less than the lower limit, the impact strength of the molded article is superior, and if it is not more than the upper limit, the colored appearance and transparency of the molded article are superior. The particle size of the polymer particles (C) measured by the absorbance method is not particularly limited, and can be measured, for example, by the method described in the Examples.
[0017] When the cross section of a resin piece obtained by dispersing the polymer particles (C) in a resin is observed by TEM, the polymer (A) preferably has an island-sea structure with the polyorganosiloxane (A1) as the sea component and the vinyl polymer (A2) as the island component. By adopting such an island-sea structure in which the polyorganosiloxane (A1) and the vinyl polymer (A2) are combined, the impact strength, colored appearance, transparency and weather resistance of a molded article containing the polymer particles (C) are more excellent.
[0018] When the cross section of the resin piece is observed by TEM, the polymer particles (C) preferably have a core-shell structure in which the polymer (A) constitutes the core and the constitutional unit derived from the second vinyl monomer (b) constitutes the shell. By forming the core-shell structure, the impact strength, colored appearance, transparency and weather resistance of a molded article containing the polymer particles (C) are more excellent.
[0019] Each particle of the polymer particle group (C) preferably has an island-sea structure in which the polyorganosiloxane (A1) is a sea component, the vinyl polymer (A2) is a first island component, and the vinyl polymer (B) is a second island component when the cross section of the resin piece is observed by TEM. By having such an island-sea structure in which the polyorganosiloxane (A1), the vinyl polymer (A2), and the vinyl polymer (B) are combined, the impact strength, colored appearance, and transparency of the molded article are more excellent.
[0020] The sea-island structure in which the polyorganosiloxane (A1), the vinyl polymer (A2), and the vinyl polymer (B) are combined as described above can be formed, for example, by impregnating the polymer (A) with at least a portion of the vinyl monomer component (b) constituting the vinyl polymer (B) during the production of the polymer particle group (C) and polymerizing the polymer. In order to impregnate at least a portion of the vinyl monomer component (b) into the polymer (A), for example, a vinyl monomer having a solubility in water at 30° C. of 1.0 g / L or less may be used as at least a portion of the vinyl monomer component (b). Examples of vinyl monomers having a solubility in water of 1.0 g / L or less at 30° C. include, among the vinyl monomers described below, styrene, alkyl-substituted styrene, alkyl-substituted isopropenylbenzene, 1,1-diphenylethylene, and the like. Methods for distinguishing the first island component from the second island component include, for example, TEM observation under adjusted dyeing conditions (specifically, dye type and dyeing time), and elemental analysis using energy dispersive X-ray spectroscopy, electron energy loss spectroscopy, etc. Each particle of the polymer particle group (C) may contain a vinyl polymer (B') that does not form the second island component. The vinyl polymer (B') that does not form the second island component (vinyl polymer obtained by polymerizing the vinyl monomer component (b) that has not been impregnated into the polymer (A)) exists on the outer surface of the polymer (A) in each particle of the polymer particle group (C) as a graft polymer (polymer covalently bonded to the polymer (A)) or a free polymer (polymer that is not covalently bonded to the polymer (A) and is physically adsorbed thereto).
[0021] Specifically, the TEM image of the cross section of the resin piece can be obtained according to the following procedure. (1) First, the polymer particles (C) are placed at the tip of a polyethylene capsule, and liquid uncured epoxy resin is poured into it. The capsule is left to stand at 25° C. for 12 hours to cure, and a resin piece is obtained. (2) Next, the obtained resin piece is stained with an aqueous osmium tetroxide solution (23°C, 12 hours). (3) Next, the resin piece that has been dyed with the osmium tetroxide aqueous solution is dyed with a ruthenium tetroxide aqueous solution (23°C, 5 hours). (4) Next, sections are cut out from the resin pieces stained with the ruthenium tetroxide aqueous solution using a microtome and collected on copper grids with a supporting membrane. The thickness of the sections is 50 nm. (5) Next, a randomly selected 0.5 μm area on the surface of the section (cross section of the resin piece) was analyzed by TEM. 2 An image (TEM image) of the above range is acquired at a magnification of 200,000 times.
[0022] The ratio of polyorganosiloxane (A1) to 100% by mass of polymer particle group (C) is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less, even more preferably 20% by mass or less, particularly preferably 10% by mass or less, and most preferably 6% by mass or less, while it is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more. If the ratio of polyorganosiloxane (A1) is the lower limit or more, the impact strength of the molded article is superior, and if it is the upper limit or less, the colored appearance and transparency of the molded article are superior.
[0023] The ratio of the polymer (A) to 100% by mass of the polymer particle group (C) is preferably 60% by mass or more, more preferably 65% by mass or more, and is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less. If the content of the polymer (A) is equal to or more than the lower limit, the impact strength of the molded article is superior, and if it is equal to or less than the upper limit, the dispersibility of the polymer particle group (C) in the thermoplastic resin is superior, and the appearance of the obtained molded article is superior. The ratio of the polymer (A) to 100% by mass of the polymer particle group (C) may be, for example, 60 to 95% by mass, 60 to 90% by mass, 65 to 90% by mass, or 65 to 85% by mass.
[0024] The ratio of the vinyl polymer (B) to 100% by mass of the polymer particle group (C) is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, while it is preferably 40% by mass or less, and more preferably 35% by mass or less. If the content of the vinyl polymer (B) is equal to or more than the lower limit, the dispersibility of the polymer particle group (C) in the thermoplastic resin is superior, and the appearance of the obtained molded article is superior, and if it is equal to or less than the upper limit, the impact strength of the molded article is superior. The ratio of the vinyl polymer (B) to 100% by mass of the polymer particle group (C) may be, for example, 5 to 40% by mass, 10 to 40% by mass, 10 to 35% by mass, or 15 to 35% by mass.
[0025] The refractive index of the polymer particles (C) is preferably from 1.470 to 1.560, and more preferably from 1.480 to 1.500. In this specification, the refractive index can be measured by the method described in the examples.
[0026] The absorbance of the polymer particles (C) is preferably from 0.01 to 0.06, and more preferably from 0.02 to 0.05. In this specification, absorbance can be measured by the method described in the Examples.
[0027] Typically, a portion of each particle of the polymer particle group (C) is insoluble in acetone, in other words, a portion of each particle of the polymer particle group (C) is soluble in acetone. Hereinafter, the acetone-insoluble portion of each particle of the polymer particle group (C) is also referred to as the "acetone-insoluble portion", and the acetone-soluble portion is also referred to as the "acetone-soluble portion".
[0028] The ratio of the acetone insoluble matter to 100% by mass of the polymer particle group (C) is preferably 80% by mass or more, more preferably 85% by mass or more, even more preferably 90% by mass or more, and particularly preferably 93% by mass or more, while it is preferably less than 100% by mass, and more preferably 99% by mass or less. If the ratio of the acetone insoluble matter is equal to or more than the lower limit, the dispersibility of the polymer particle group (C) in the thermoplastic resin is better, and the impact strength and appearance of the obtained molded article are better. If the ratio of the acetone insoluble matter is less than 100% by mass, the balance between impact strength and color development is better, and if it is 99% by mass or less, the melt flowability when added to the thermoplastic resin is better. The ratio of the acetone insoluble matter to 100% by mass of the polymer particle group (C) may be 80% by mass or more and less than 100% by mass, 85% by mass or more and less than 100% by mass, 90% by mass or more and 99% by mass or less, or 93% by mass or more and 99% by mass or less. The ratio of the acetone soluble content to 100% by mass of the polymer particle group (C) may be 10% by mass or less, 8% by mass or less, or 5% by mass or less.
[0029] The acetone insoluble matter is measured by carrying out the following procedures (1-1) to (1-5). (1-1) 0.5 g of a sample (polymer particle group (C)) is added to 50 mL (44.5 g) of acetone to prepare a mixed solution, which is then allowed to stand at 25°C for 8 hours and then stirred with a stirrer for 30 minutes to dissolve the acetone-soluble components. (1-2) The mixed solution is placed in a centrifuge tube whose mass has been measured, and the liquid containing the acetone insoluble matter and the acetone soluble matter is separated by centrifugation (16,000 rpm, 4 hours). (1-3) After removing the supernatant, fresh acetone is added and stirred, and then centrifugal separation is performed again in the same manner as in (1-2) above to wash off the acetone-insoluble matter. (1-4) After repeating (1-3) twice, the supernatant is removed. The centrifuge tube with the acetone-insoluble matter remaining is immersed in a hot water bath (80°C, 8 hours) to volatilize the acetone, and then vacuum-dried at 65°C for 6 hours to obtain a dry sample (acetone-insoluble matter adhering to the centrifuge tube). (1-5) Measure the mass of the obtained dried sample (acetone insolubles + centrifuge tube) and calculate the ratio of acetone insolubles w by the following formula. ais Calculate the percentage. w ais =(w c1 -w as ) / wt×100 wt: mass of polymer particle group (C) subjected to measurement w as : Mass of the centrifuge tube w c1 : Mass of acetone insoluble matter (including centrifuge tube)
[0030] From the viewpoint of making the ratio of acetone insoluble matter in the polymer particle group (C) fall within the above-mentioned range, it is preferable that the vinyl polymer (A2) is sufficiently crosslinked and that the polyorganosiloxane (A1) and the vinyl polymer (A2) are covalently bonded. It is also preferable that the vinyl polymer (B) is covalently bonded to the polymer (A), and it is more preferable that the vinyl polymer (B) is covalently bonded to the vinyl polymer (A2) in the polymer (A).
[0031] The weight average molecular weight of the acetone soluble matter of the polymer particle group (C) is preferably 20,000 or more, and more preferably 50,000 or more, and on the other hand, is preferably 500,000 or less, more preferably 350,000 or less, even more preferably 200,000 or less, and particularly preferably 150,000 or less. When the weight average molecular weight of the acetone soluble portion is 20,000 or more and 500,000 or less, the dispersibility of the polymer particles (C) in the thermoplastic resin is excellent, and the impact strength and appearance of the obtained molded article are excellent. In particular, when the weight average molecular weight of the acetone soluble portion is 50,000 or more and 150,000 or less, the dispersibility of the polymer particles (C) in the thermoplastic resin is particularly good, and the impact strength and appearance of the obtained molded article are excellent under a wide range of molding conditions, including those with a low kneading level. The weight average molecular weight of the acetone soluble portion of the polymer particle group (C) may be 20,000 or more and 500,000 or less, 20,000 or more and 350,000 or less, 50,000 or more and 200,000 or less, or 50,000 or more and 150,000 or less.
[0032] The weight average molecular weight of the acetone soluble matter is measured by carrying out the following procedures (2-1) to (2-3). (2-1) From the liquid containing the acetone soluble matter collected in the above-mentioned measurement of the ratio of the acetone insoluble matter, acetone is distilled off under reduced pressure using a rotary evaporator to obtain the acetone soluble matter. (2-2) The acetone soluble fraction obtained in (2-1) is dissolved again in THF to a sample concentration of 0.1 to 0.3% by mass to obtain a THF solution of the acetone soluble fraction. (2-3) The THF solution of the acetone soluble fraction obtained in (2-2) above is subjected to gel permeation chromatography (GPC) measurement, and the weight average molecular weight (Mw) is determined from a calibration curve using standard polystyrene. The measurement conditions for GPC are as described in the Examples below.
[0033] The weight average molecular weight of the acetone soluble portion can be adjusted by the amount of initiator, the amount of reducing agent, the polymerization temperature, and the use of a chain transfer agent when polymerizing the vinyl monomer component (b) constituting the vinyl polymer (B). For example, the weight average molecular weight of the acetone soluble portion decreases due to the promotion of radical generation by increasing the amount of initiator or reducing agent or raising the polymerization temperature, or the promotion of chain transfer reaction by adding or increasing the amount of a chain transfer agent.
[0034] (Polyorganosiloxane (A1)) The polyorganosiloxane (A1) is a polymer containing organosiloxane units having aryl groups. The polyorganosiloxane (A1) can be obtained by polymerizing an organosiloxane mixture containing an organosiloxane having an aryl group. The organosiloxane mixture may further contain components that are used as necessary. The optional components include at least one selected from the group consisting of a siloxane crosslinking agent, a siloxane crosslinking agent, and a siloxane oligomer having a terminal blocking group.
[0035] The polyorganosiloxane (A1) preferably contains a constituent unit represented by the following general formula (1) as the aryl group-containing siloxane unit.
[0036] [ka]
[0037] In formula (1), Ar is an aryl group, and R is a hydrogen atom, a halogen atom, an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, an aryl group having 5 to 12 carbon atoms, or a halogenated alkyl group having 1 to 3 carbon atoms.
[0038] The organosiloxane having an aryl group includes a monomer represented by the following general formula (2).
[0039] [ka]
[0040] In formula (2), Ar is an aryl group, and R1, R2, and R3 are each independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, an aryl group having 5 to 12 carbon atoms, or a halogenated alkyl group having 1 to 3 carbon atoms.
[0041] The organosiloxane having an aryl group is not particularly limited as long as it has an aryl group, and examples thereof include linear organosiloxanes and cyclic organosiloxanes, any of which can be used. Among these, linear organosiloxanes are preferred.
[0042] The chain organosiloxane having an aryl group is preferably one having two hydrocarbon groups containing an aryl group, more preferably one having two hydrocarbon groups containing an aryl group and two alkoxy groups.The chain organosiloxane may be dimethoxydiphenylsilane, diethoxydiphenylsilane, dimethoxymethylphenylsilane, diethoxymethylphenylsilane, etc.These may be used alone or in combination of two or more.
[0043] The cyclic organosiloxane having an aryl group is preferably one having a 3- to 7-membered ring, and examples thereof include trimethyltriphenylcyclotrisiloxane, tetramethyltetraphenylcyclotetrasiloxane, octaphenylcyclotetrasiloxane, etc. These may be used alone or in combination of two or more.
[0044] The polyorganosiloxane (A1) may contain, in addition to organosiloxane units having an aryl group, organosiloxane units having no aryl group. The chain organosiloxane not having an aryl group is not particularly limited, and examples thereof include chain organosiloxanes, alkoxysilane compounds, cyclic organosiloxanes, etc., any of which can be used. Among these, alkoxysilane compounds and cyclic organosiloxanes are preferred, and cyclic organosiloxanes are particularly preferred because of their high polymerization stability and high polymerization rate.
[0045] The alkoxysilane compound not having an aryl group is preferably a bifunctional alkoxysilane compound, such as dimethoxydimethylsilane, diethoxydimethylsilane, diethoxydiethylsilane, dipropoxydimethylsilane, etc. These may be used alone or in combination of two or more.
[0046] The cyclic organosiloxane not having an aryl group is preferably one having a 3- to 7-membered ring, and examples thereof include hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, and dodecamethylcyclohexasiloxane. These may be used alone or in combination of two or more. Among these, octamethylcyclotetrasiloxane is preferred because it is easy to control the particle size distribution.
[0047] The content of the aryl group-containing siloxane units relative to the total content of the aryl group-containing siloxane units and the aryl group-free siloxane units is preferably 5 to 80 parts by mass, more preferably 7 to 77 parts by mass, and even more preferably 10 to 75 parts by mass. When the content of the siloxane unit containing an aryl group is equal to or more than the above lower limit, the transparency of the molded article is easily improved.When the content of the siloxane unit containing an aryl group is equal to or less than the above upper limit, the impact strength of the molded article is easily improved. The content of the siloxane units not containing an aryl group relative to the total content of the siloxane units containing an aryl group and the siloxane units not containing an aryl group is preferably 20 to 95 parts by mass, more preferably 25 to 93 parts by mass, and even more preferably 27 to 92 parts by mass. When the content of the siloxane units not containing an aryl group is equal to or greater than the lower limit, the impact strength of the molded article is easily improved.When the content of the siloxane units containing an aryl group is equal to or less than the upper limit, the transparency of the molded article is easily improved.
[0048] The siloxane crosslinking agent is preferably one having a siloxy group. Examples of the siloxane crosslinking agent include trifunctional or tetrafunctional silane crosslinking agents such as trimethoxymethylsilane, triethoxyphenylsilane, tetramethoxysilane, tetraethoxysilane, tetra-n-propoxysilane, and tetrabutoxysilane. Among them, tetrafunctional crosslinking agents are preferred, and tetraethoxysilane is more preferred.
[0049] The ratio of the siloxane crosslinking agent to 100% by mass of the organosiloxane mixture is preferably 10% by mass or less, more preferably 5% by mass or less, and may be 0% by mass. If the content of the siloxane crosslinking agent is 10% by mass or less, it is possible to obtain polymer particles (C) that can improve the impact strength of the molded article.
[0050] The siloxane crosslinking agent has a siloxy group (-Si-O-) and a functional group capable of polymerizing with a vinyl monomer. Examples of the siloxane crosslinking agent include siloxanes represented by the following formula (I). R-Si(R 1 ) n (OR 2 ) (3-n) (I) In formula (I), R 1 R represents a methyl group, an ethyl group, a propyl group, or a phenyl group. 2 represents an organic group such as a hydrocarbon group, and is preferably, for example, a methyl group, an ethyl group, a propyl group, or a phenyl group. n represents 0, 1, or 2. R represents a functional group represented by any one of the following formulas (I-1) to (I-4). CH2=C(R 3 )-COO-(CH2) p - (I-1) CH2=C(R 4 )-C6H4- (I-2) CH2=CH- (I-3) HS-(CH2) p - (I-4) In these formulas, R 3 and R 4 each independently represents a hydrogen atom or a methyl group, and p represents an integer of 1 to 6.
[0051] The functional group represented by formula (I-1) may be, for example, a methacryloyloxyalkyl group. Examples of siloxanes having this group include the following: β-methacryloyloxyethyldimethoxymethylsilane, γ-methacryloyloxypropylmethoxydimethylsilane, γ-methacryloyloxypropyldimethoxymethylsilane, γ-methacryloyloxypropyltrimethoxysilane, γ-methacryloyloxypropylethoxydiethylsilane, γ-methacryloyloxypropyldiethoxymethylsilane, δ-methacryloyloxybutyldiethoxymethylsilane, etc.
[0052] An example of the functional group represented by formula (I-2) is a vinylphenyl group. An example of a siloxane having this group is vinylphenylethyldimethoxysilane. Examples of siloxanes having a functional group represented by formula (I-3) include vinyltrimethoxysilane and vinyltriethoxysilane.
[0053] The functional group represented by formula (I-4) may be a mercaptoalkyl group. Examples of siloxanes having this group include the following: γ-mercaptopropyl dimethoxymethylsilane, γ-mercaptopropyl methoxydimethylsilane, γ-mercaptopropyl diethoxymethylsilane, γ-mercaptopropyl ethoxydimethylsilane, γ-mercaptopropyl trimethoxysilane, etc.
[0054] The siloxane-based crosslinking agent may be used alone or in combination of two or more kinds. As the siloxane crosslinking agent, 3-methacryloxypropylmethyldimethoxysilane is preferred because it is easy to form an island structure when the polyorganosiloxane (A1) and the vinyl polymer (A2) are composited.
[0055] The ratio of the siloxane-based crosslinking agent to 100% by mass of the organosiloxane mixture is preferably 0.05% by mass or more, more preferably 0.1% by mass or more, and even more preferably 0.5% by mass or more, while it is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less. If the ratio of the siloxane-based graft crosslinking agent is within the range of the upper limit value and the lower limit value, the covalent bond between the polyorganosiloxane (A1) and the vinyl polymer (A2) can be sufficiently formed, and a polymer particle group (C) having good impact strength can be obtained. The ratio of the siloxane-based crosslinking agent to 100% by mass of the organosiloxane mixture may be, for example, 0.05 to 20% by mass, 0.1 to 10% by mass, or 0.5 to 5% by mass.
[0056] The viscosity of the aryl group-containing organosiloxane at 15° C. is preferably from 0.5 to 35.0 mPa·s, more preferably from 1.0 to 20.0 mPa·s, and even more preferably from 1.5 to 15.0 mPa·s. In this specification, the viscosity can be measured by the method described in the Examples.
[0057] The refractive index of the polyorganosiloxane (A1) is preferably 1.410 or more, more preferably 1.440 or more, while it is preferably 1.560 or less, more preferably 1,520 or less. If the refractive index of the polyorganosiloxane is within the above range, the refractive index of the polymer particle group is easily adjusted, and the transparency of the molded article is excellent. In this specification, the refractive index can be measured by the method described in the examples.
[0058] <Method for producing polyorganosiloxane (A1)> The method for producing the polyorganosiloxane (A1) is not particularly limited, and for example, the following production method can be used. First, an organosiloxane mixture containing an organosiloxane, and optionally a siloxane-based crosslinking agent, optionally a siloxane-based crosslinking agent, and optionally a siloxane oligomer having a terminal blocking group is emulsified with an emulsifier and water to prepare an emulsion, and in this emulsion, the organosiloxane mixture is polymerized at high temperature in the presence of an acid catalyst, and then the acid catalyst is neutralized with an alkaline substance to obtain a polyorganosiloxane latex. In the following description of the manufacturing method, an example will be described in which an "organosiloxane mixture" is used as the raw material for polymerization, but the same manufacturing process can also be applied when an "organosiloxane" is used.
[0059] In this manufacturing method, the method of preparing the emulsion includes a method using a homomixer that uses shear force due to high speed rotation to atomize; a method using a homogenizer that uses the ejection force of a high pressure generator to atomize, etc., and mixing by high speed stirring. Among these, the method using a homogenizer is preferred because it narrows the particle size distribution of the polyorganosiloxane latex.
[0060] Examples of the method for mixing the acid catalyst during polymerization include (1) adding the acid catalyst together with the organosiloxane mixture, emulsifier, and water all at once and mixing, (2) adding the acid catalyst aqueous solution all at once to the emulsion of the organosiloxane mixture, and (3) dropping the emulsion of the organosiloxane mixture into a high-temperature aqueous acid catalyst solution at a constant speed and mixing it, etc. Among these, the method of dropping the emulsion of the organosiloxane mixture into a high-temperature aqueous acid catalyst solution at a constant speed and mixing it is preferred because it is easy to control the particle size of the polyorganosiloxane.
[0061] The polymerization temperature is preferably 50° C. or higher, more preferably 70° C. or higher. The upper limit of the polymerization temperature is, for example, 100° C. When polymerization is carried out by dropping an emulsion of an organosiloxane mixture into a hot aqueous acid catalyst solution at a constant rate, the polymerization time is usually 2 hours or more, and preferably 5 hours or more.
[0062] Furthermore, since the crosslinking reaction between silanols proceeds at temperatures of 30°C or lower, in order to increase the crosslinking density of the polyorganosiloxane, the latex formed after polymerization at a high temperature of 50°C or higher can be kept at a temperature of 30°C or lower for about 5 to 100 hours.
[0063] The polymerization reaction of the organosiloxane mixture can be terminated by neutralizing the reaction system containing the latex to a pH of 6 to 8 with an alkaline substance such as sodium hydroxide, potassium hydroxide, or an aqueous ammonia solution.
[0064] The emulsifier used in the above production method is not particularly limited as long as it is capable of emulsifying the organosiloxane mixture, but anionic emulsifiers or nonionic emulsifiers are preferred. Examples of the anionic emulsifier include sodium alkylbenzene sulfonate, sodium alkyl diphenyl ether disulfonate, sodium alkyl sulfate, sodium polyoxyethylene alkyl sulfate, and sodium polyoxyethylene nonylphenyl ether sulfate. Examples of the nonionic emulsifier include polyoxyethylene alkyl ether, polyoxyethylene alkylene alkyl ether, polyoxyethylene distyrenated phenyl ether, polyoxyethylene tribenzyl phenyl ether, polyoxyethylene polyoxypropylene glycol, and the like. These emulsifiers can be used alone or in combination of two or more.
[0065] The amount of emulsifier used is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, and more preferably 20 parts by mass or less, more preferably 10 parts by mass or less, based on 100 parts by mass of the organosiloxane mixture. The particle size of the polyorganosiloxane latex can be adjusted to a desired value by adjusting the amount of emulsifier used. If the amount of emulsifier used is equal to or more than the lower limit, the emulsion stability of the organosiloxane mixture emulsion can be improved. If the amount of emulsifier used is equal to or less than the upper limit, the heat discoloration resistance and surface appearance of the molded product are better.
[0066] Examples of acid catalysts used in the polymerization of the organosiloxane mixture include sulfonic acids such as aliphatic sulfonic acid, aliphatic-substituted benzenesulfonic acid, and aliphatic-substituted naphthalenesulfonic acid, and mineral acids such as sulfuric acid, hydrochloric acid, and nitric acid. These acid catalysts can be used alone or in combination of two or more. Among these, the use of mineral acids such as sulfuric acid, hydrochloric acid, and nitric acid can narrow the particle size distribution of the polyorganosiloxane latex, and further suppress the occurrence of problems (such as a decrease in the thermal decomposition resistance of the molded product and poor appearance) caused by the emulsifier component in the polyorganosiloxane latex.
[0067] The amount of the acid catalyst used is preferably 0.005 parts by mass or more and 40 parts by mass or less per 100 parts by mass of the organosiloxane. If the amount of the acid catalyst used is 0.005 parts by mass or more, the organosiloxane mixture can be polymerized in a short time. If the amount of the acid catalyst used is 40 parts by mass or less, the heat discoloration resistance and surface appearance of the molded product are more excellent.
[0068] In addition, since the amount of the acid catalyst used is a factor that determines the particle size of the polyorganosiloxane (A1), in order to obtain polyorganosiloxane (A1) having a particle size described below, it is more preferable to use an amount of the acid catalyst of 1 part by mass or more and 30 parts by mass or less per 100 parts by mass of the organosiloxane.
[0069] To the polyorganosiloxane latex obtained by the above method, an emulsifier may be added as necessary for the purpose of improving mechanical stability. As the emulsifier, the same anionic emulsifiers and nonionic emulsifiers as those exemplified above are preferable.
[0070] (Vinyl polymer (A2)) The polymer particles (C) of the present invention preferably have structural units derived from a vinyl monomer (a). The polymer particles (C) of the present invention preferably contain a vinyl polymer (A2) having a structural unit derived from a vinyl monomer (a). The vinyl monomer component (a) constituting the vinyl polymer (A2) comprises one or more kinds of vinyl monomers.
[0071] From the viewpoint of the impact strength of a molded article, the vinyl monomer component (a) preferably contains a monofunctional (meth)acrylate monomer (hereinafter also referred to as "monomer (a1-1)"). The vinyl monomer component (a) may further contain, in addition to the monomer (a1-1), at least one selected from the group consisting of another monofunctional monomer (hereinafter also referred to as "monomer (a1-2)") different from the monomer (a1-1) that can be copolymerized with the monomer (a1-1), and a polyfunctional monomer (hereinafter also referred to as "monomer (a1-3)") that can be copolymerized with the monomer (a1-1). From the viewpoint of the impact strength of the molded article and the viewpoint of keeping the ratio of the THF insoluble matter in the polymer particle group (C) within the above-mentioned range, it is preferable that the vinyl monomer component (a) contains the monomer (a1-1) and the monomer (a1-3).
[0072] Examples of the monomer (a1-1) include alkyl acrylates such as methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, 2-ethylhexyl acrylate, and n-octyl acrylate; and alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, n-butyl methacrylate, i-butyl methacrylate, t-butyl methacrylate, hexyl methacrylate, 2-ethylhexyl methacrylate, lauryl methacrylate, tridecyl methacrylate, and stearyl methacrylate. Among these, since the impact strength of the molded body becomes better, it is preferable that the monomer (a1-1) contains at least one monomer selected from the group consisting of ethyl acrylate, n-butyl acrylate, 2-ethylhexyl acrylate, and n-octyl acrylate, and it is more preferable that the monomer (a1-1) contains n-butyl acrylate. These monomers (a1-1) can be used alone or in combination of two or more.
[0073] Examples of the monomer (a1-2) include various vinyl monomers such as aromatic vinyl monomers such as styrene and α-methylstyrene, cyanide vinyl monomers such as acrylonitrile and methacrylonitrile, and (meth)acrylic group-modified silicones. These monomers (a1-2) can be used alone or in combination of two or more.
[0074] As the monomer (a1-3), those having reactive groups such as nucleophilic groups such as hydroxyl groups, carboxy groups, amino groups, and mercapto groups; electrophilic groups such as halogen atoms and isocyanate groups; cationic polymerizable groups such as epoxy groups and oxetane groups; and radical polymerizable groups such as vinyl groups, allyl groups, and (meth)acryloyl groups are preferred. Examples of the monomer (a1-3) include ethylene glycol dimethacrylate, propylene glycol dimethacrylate, 1,3-butylene glycol dimethacrylate, 1,4-butylene glycol dimethacrylate, ethylene glycol diacrylate, propylene glycol diacrylate, 1,3-butylene glycol diacrylate, 1,4-butylene glycol diacrylate, 1,6-hexanediol diacrylate, divinylbenzene, polyfunctional (meth)acrylic group-modified silicone, allyl methacrylate, allyl acrylate, triallyl cyanurate, triallyl isocyanurate, and triallyl trimellitate. Among these, the monomer (a1-3) is preferably at least one selected from the group consisting of allyl methacrylate, allyl acrylate, triallyl cyanurate, and triallyl isocyanurate, more preferably allyl methacrylate and allyl acrylate, and even more preferably allyl methacrylate, because this leads to better impact strength of the molded article and facilitates the formation of a chemical bond with the vinyl monomer component (b) described below. These monomers (a1-3) can be used alone or in combination of two or more.
[0075] The ratio of the monomer (a1-1) to 100% by mass of the vinyl monomer component (a) is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more, from the viewpoint of the impact strength of the molded article. The ratio of the monomer (a1-1) to 100% by mass of the vinyl monomer component (a) may be 100% by mass, but is preferably 99.9% by mass or less.
[0076] The ratio of the monomer (a1-2) to 100% by mass of the vinyl monomer component (a) is preferably 40% by mass or less, more preferably 30% by mass or less, even more preferably 25% by mass or less, particularly preferably 20% by mass or less, and may be 0% by mass, from the viewpoint of the impact strength of the molded article. From the viewpoint of transparency, the ratio of the monomer (a1-2) to 100% by mass of the vinyl monomer component (a) is preferably 5% by mass or more, more preferably 8% by mass or more, and even more preferably 10% by mass or more.
[0077] The ratio of the monomer (a1-3) relative to 100% by mass of the vinyl monomer component (a) is preferably from 0.1 to 10% by mass, more preferably from 0.3 to 5.0% by mass, even more preferably from 0.3 to 3.0% by mass, and particularly preferably from 0.3 to 1.0% by mass, from the viewpoints of melt fluidity during molding and of a balance between the colored appearance or transparency and impact strength of the molded article.
[0078] (Polymer (A)) The polymer (A) is a complex of a polyorganosiloxane (A1) and a first vinyl polymer (A2), and the polyorganosiloxane (A1) and the first vinyl polymer (A2) may form a covalent bond, or the polyorganosiloxane (A1) and the first vinyl polymer (A2) may not form a covalent bond.
[0079] In the polymer (A), the mass ratio represented by [the total content of the siloxane units containing an aryl group and the siloxane units not containing an aryl group] / [the content of the structural units derived from the vinyl monomer (a)] is preferably 3 / 97 to 50 / 50, more preferably 5 / 95 to 30 / 70, and further preferably 6 / 94 to 20 / 80.
[0080] In the polymer (A), the mass ratio represented by [total mass of structural units constituting the polyorganosiloxane (A1)] / [total mass of structural units constituting the vinyl polymer (A2)] (hereinafter also referred to as "A1 / A2") is preferably from 3 / 97 to 50 / 50, more preferably from 5 / 95 to 30 / 70, and even more preferably from 6 / 94 to 20 / 80, from the viewpoint of the impact strength of the molded article.
[0081] <Method for producing polymer (A)> The method for producing the polymer (A) is not particularly limited, but a method in which the vinyl monomer component (a) constituting the vinyl polymer (A2) is polymerized in the presence of a latex containing the polyorganosiloxane (A1) is preferred, since the impact strength of the molded product is superior.
[0082] The method of polymerizing the vinyl monomer component (a) in the presence of a latex containing polyorganosiloxane (A1) is not particularly limited, and examples thereof include (i) a method of dropping the vinyl monomer component (a) into a latex containing polyorganosiloxane (A1) and polymerizing it, (ii) a method of adding a part of the vinyl monomer component (a) to a latex containing polyorganosiloxane (A1) under conditions in which polymerization does not start, impregnating the particles of polyorganosiloxane (A1), initiating polymerization, and then dropping or adding the remainder of the vinyl monomer component (a) all at once and polymerizing it, and (iii) a method of adding the entire amount of the vinyl monomer component (a) to a latex containing polyorganosiloxane (A1) under conditions in which polymerization does not start, impregnating the particles of polyorganosiloxane (A1), and then polymerizing it.
[0083] As the method for producing the polymer (A), among the above, a method in which the entire amount of the vinyl monomer component (a) is added to a latex containing the polyorganosiloxane (A1) under conditions in which polymerization does not start, the vinyl monomer component (a) is impregnated into the particles of the polyorganosiloxane (A1), and then polymerization is performed is preferred, because the impact strength of the molded article is superior.
[0084] As a method for producing the polymer (A), a production method having the following steps i to iv is particularly preferred.
[0085] Process i: A latex of polyorganosiloxane (A1) is prepared under any conditions. The latex of polyorganosiloxane (A1) can be produced by the method described above. In this case, the polyorganosiloxane (A1) preferably comprises an organosiloxane and a siloxane-based crosslinking agent.
[0086] Step ii: The total amount of the vinyl monomer component (a) and a radical polymerization initiator are added to the latex of the polyorganosiloxane (A1) obtained in step i under conditions in which polymerization of the vinyl monomer component (a) does not start, and the particles of the polyorganosiloxane (A1) are impregnated with the vinyl monomer component (a). At this time, by adding the entire amount of the vinyl monomer component (a), the impact strength of the molded article becomes superior.
[0087] When the vinyl monomer component (a) contains a plurality of vinyl monomers, for example, when it contains the monomer (a1-1) and at least one selected from the group consisting of the monomer (a1-2) and the monomer (a1-3), the method of adding these monomers is not particularly limited. For example, the monomer (a1-1) and the monomer (a1-2) and / or the monomer (a1-3) may be added simultaneously, or the monomer (a1-1) and the monomer (a1-2) and / or the monomer (a1-3) may be added separately. When the vinyl monomer component (a) contains the monomer (a1-3), it is preferable to mix it with the monomer (a1-1) and / or the monomer (a1-2) before adding it, in order to obtain an appropriate crosslinked structure.
[0088] The radical polymerization initiator is not particularly limited, but examples thereof include azo compounds, peroxides, dihalogens, etc. These can be used alone or in combination of two or more.
[0089] Examples of the azo compound include the following: Oil-soluble azo initiators such as 2,2'-azobisisobutyronitrile, dimethyl 2,2'-azobis(2-methylpropionate), 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobis(2-butyronitrile); water-soluble azo initiators such as 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis[N-(2-carboxymethyl)-2-methylpropionamidine]hydrate, 2,2'-azobis-(N,N'-dimethyleneisobutylamidine)dihydrochloride, and 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride. These may be used alone or in combination of two or more.
[0090] When an azo compound is used as a radical polymerization initiator, the amount of the azo compound used is preferably 0.01% by mass or more relative to 100% by mass of the total of the monomers to be polymerized, and is preferably 3% by mass or less, more preferably 1% by mass or less, and even more preferably 0.5% by mass or less. By setting the amount of the azo compound used within the range between the upper limit and the lower limit, the polymerization rate can be prevented from increasing excessively, and the sea-island structure can be easily constructed.
[0091] Examples of peroxides include the following: Inorganic peroxides such as hydrogen peroxide, potassium persulfate, and ammonium persulfate; organic peroxides such as diisopropylbenzene hydroperoxide, p-menthane hydroperoxide, cumene hydroperoxide, t-butyl hydroperoxide, succinic acid peroxide, t-butyl peroxy neodecanoate, t-butyl peroxy neoheptanoate, t-butyl peroxy pivalate, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, and t-butyl peroxy-2-ethylhexanoate. These can be used alone or in combination of two or more. Among them, it is preferable that the 10-hour half-life temperature is between 25°C and 105°C because it is easy to handle during emulsion polymerization.
[0092] When a peroxide is used as a radical polymerization initiator, the amount of the peroxide used is preferably 0.01% by mass or more relative to 100% by mass of the total of the monomers to be polymerized, and is preferably 1% by mass or less, more preferably 0.5% by mass or less, and even more preferably 0.2% by mass or less. By setting the amount of the peroxide used within the range between the upper limit and the lower limit, an excessive increase in the polymerization rate can be suppressed, and the above-mentioned sea-island structure can be easily constructed.
[0093] As the radical polymerization initiator, a peroxide is preferred since the polymerization rate can be easily controlled and the impact strength of the molded article is superior.
[0094] When a peroxide is used as the radical polymerization initiator, a reducing agent can be used in combination for the purpose of promoting the decomposition of the peroxide.
[0095] Examples of reducing agents include sulfur compounds such as sulfite, hydrogen sulfite, alkali metal bisulfite, acetone bisulfite, alkali metal disulfite, metabisulfite and salts thereof; organic sulfur compounds such as thiosulfate, sulfinic acid, hydroxyl alkyl sulfinic acid, hydroxyl methyl sulfinic acid, 2-hydroxy-2-sulfinic acid, formazine sulfinic acid, propyl sulfinic acid, isopropyl sulfinic acid, phenyl sulfinic acid; reducing nitrogen compounds such as formaldehyde sulfoxylate and salts thereof, hydroxylamine, hydroxylamine hydrosulfate, hydroxyl ammonium salts, polyamines, dimethylaniline; reducing sugars such as sorbose, fructose, glucose, lactose, dextrose; and enediols such as ascorbic acid and isoascorbic acid. Examples of "salts" include sodium ions, potassium ions, ammonium ions, and zinc ions.
[0096] In addition, sulfates, nitrates, acetates, carbonates, and chlorides of transition metals existing in Groups 3 to 11 of the periodic table are also useful as reducing agents. Examples of transition metals include Ce and the like in Group 3, Ti and the like in Group 4, V and the like in Group 5, Cr and Mo and the like in Group 6, Mn and the like in Group 7, Fe and the like in Group 8, Co and the like in Group 9, Ni and the like in Group 10, and Cu and Ag and the like in Group 11.
[0097] The reducing agent is preferably at least one selected from the group consisting of sodium formaldehyde sulfoxylate, L(+)-tartaric acid, sodium disulfite, sodium isoascorbate, L-ascorbic acid, and ferrous sulfate, because it is industrially easily available and provides better heat discoloration resistance and surface appearance of the molded product.
[0098] The amount of the reducing agent used is preferably 2.0 molar equivalents or less of the peroxide used in the polymerization of the vinyl monomer component (a), more preferably 1.0 molar equivalents or less, further preferably 0.6 molar equivalents or less, and may be 0. By keeping the amount of the reducing agent used at or below the upper limit, it is possible to prevent the polymerization rate from increasing excessively, and it becomes easier to form the above-mentioned sea-island structure.
[0099] When a transition metal salt is used as a reducing agent, a chelating agent can be used in combination with the transition metal salt in order to increase its reactivity. As the chelating agent, a compound containing two or more electron donor atoms capable of forming a coordinate bond with the target transition metal atom can be used, such as ethylenediaminetetraacetic acid, hydroxyethylethylenediaminetriacetic acid, nitrilotriacetic acid, citric acid, tartaric acid, gluconic acid, 5-sulfosalicylic acid, ethylenediamine, diethylenetriamine, triethylenetetramine, triaminotriethylamine, triethanolamine, N-hydroxyethylethylenediamine, sodium oxalate, and metal salts thereof. Among these, ethylenediaminetetraacetic acid and its metal salts are preferred because of their excellent polymerization stability.
[0100] From the viewpoint of controlling the polymerization reactivity, the amount of the chelating agent used is preferably 0.5 molar equivalents or more relative to the reducing agent, and more preferably 1.0 equivalents or more, while it is preferably 5.0 molar equivalents or less, and more preferably 2.5 molar equivalents or less.
[0101] In the step ii, an aqueous medium may be added to the latex of the polyorganosiloxane (A1), if necessary. The aqueous medium includes water and a mixed medium of water and an organic solvent. The organic solvent in the mixed medium may be any solvent that is miscible with water, such as methanol and ethanol.
[0102] In step ii, an emulsifier may be added to the latex of polyorganosiloxane (A1), if necessary. The emulsifier is not particularly limited, and the same emulsifiers as those used in the production of the polyorganosiloxane (A1) can be used. Among them, anionic emulsifiers or nonionic emulsifiers are preferred. In the step ii, the polymerization may be carried out using only the emulsifier contained in the latex of the polyorganosiloxane (A1) without adding any emulsifier.
[0103] A chain transfer agent may be used when polymerizing the vinyl monomer component (a). Examples of the chain transfer agent include mercaptans such as n-dodecyl mercaptan, t-dodecyl mercaptan, n-octyl mercaptan, n-tetradecyl mercaptan, n-hexyl mercaptan, and n-butyl mercaptan; halogen compounds such as carbon tetrachloride and ethylene bromide; α-methylstyrene dimer, etc. These chain transfer agents may be used alone or in combination of two or more.
[0104] The amount of the chain transfer agent used is preferably 1.0% by mass or less, and may be 0% by mass, based on 100% by mass of the vinyl monomer component (a). By setting the amount of the chain transfer agent used to 1.0% by mass or less, the decrease in the THF insoluble content ratio of the polymer particle group (C) is suppressed, and the impact strength of the molded article is more excellent.
[0105] Step iii: In step ii, for the latex of polyorganosiloxane (A1) to which the vinyl monomer component (a) and the radical polymerization initiator have been added, polymerization of the vinyl monomer component (a) is initiated under conditions that satisfy the following formula (a). T 10 >(T in +10) ···(A) Here, T 10 represents the 10-hour half-life temperature of the radical polymerization initiator used, and T in represents the temperature at which the polymerization of the vinyl monomer component (a) is initiated. When multiple radical polymerization initiators are used in combination, the T 10 Use the value.
[0106] Formula (a) is satisfied, in other words, the temperature T at which the polymerization of the vinyl monomer component (a) is initiated in (Hereinafter, polymerization temperature (T in ) is taken as the 10-hour half-life temperature T 10 By setting the temperature at least 10°C lower than the above, the polymerization rate can be suppressed, and it becomes easier to form a sea-island structure in which the polyorganosiloxane (A1) and the vinyl polymer (A2) are combined, thereby obtaining polymer particle groups (C) that can improve the impact strength of the obtained molded product. Polymerization temperature (T in ) is the 10-hour half-life temperature T 10 It is more preferable that the temperature is 15° C. or more lower, and more preferable that the temperature is 20° C. or more lower. Polymerization temperature (T in ) is not particularly limited, but from the viewpoint of the stability of polymerization initiation, the lower limit of the 10-hour half-life temperature T 10 It is preferable that the temperature is not lower than 50°C from the above. The polymerization time is determined by the polymerization temperature (T in ) depending on the time, but for example, it is 0.1 to 30 hours.
[0107] 10-hour half-life temperature T 10 is the temperature at which 50 mol% of the radical polymerization initiator used is thermally decomposed in 10 hours. For example, by substituting the conversion rate X of the radical polymerization initiator = 50 [%], time t = 36000 [s] (= 10 hours), gas constant R = 8.314 [J / Kmol], and literature values or calculated values for the frequency factor A and activation energy E into the following formula (a) and formula (c), the 10-hour half-life temperature T 10 The 10-hour half-life temperature T 10 Literature values may be used.
[0108] X = 100 × exp(-kdt) (a) kd = A × exp(-E / RT) (c) (X[%]: conversion rate, kd[1 / S]: reaction rate, t[s]: time, A[1 / S]: frequency factor, E[J / mol]: activation energy, R[J / Kmol]: gas constant, T[K]: temperature) For example, the 10-hour half-life temperature of potassium persulfate is 67°C, and the 10-hour half-life temperature of t-butyl hydroperoxide (product name Perbutyl H69, manufactured by Nippon Oil & Fats Co., Ltd.) is 167°C.
[0109] Step iv: In the polymerization behavior after the polymerization is started in step iii, the maximum temperature in the system reached in the polymerization of the vinyl monomer component (a) is T p (℃), the temperature in the system is T in After reaching +1(℃), T in +{(T p -T in ) / 3}(℃) is defined as the time required for p (seconds) (Hereinafter, polymerization rate (S p )), polymerization is carried out so as to satisfy the following formula (E). S p ≧80 (E)
[0110] Polymerization rate (S p By setting the polymerization rate (S) to 80 seconds or more, it becomes easy to construct an island-sea structure in which the polyorganosiloxane (A1) and the vinyl polymer (A2) are combined, and it is possible to obtain polymer particle group (C) that can improve the impact strength of the obtained molded article. p ) is more preferably 100 seconds or more, even more preferably 120 seconds or more, and particularly preferably 150 seconds or more. Polymerization rate (S p ) is the type and amount of the radical polymerization initiator, the polymerization initiation temperature T in In addition, it can be adjusted by the heat removal system during polymerization.
[0111] (Vinyl polymer (B)) The vinyl polymer (B) has a structure formed by polymerizing a vinyl monomer (b), and is composed of units based on the vinyl monomer. The vinyl polymer (B) refers to both the graft layer containing a structural unit derived from the second vinyl monomer (b) in the graft copolymer (C1), and the free polymer containing a structural unit derived from the second vinyl monomer (b) in the polymer complex (C2). The vinyl monomer component (b) constituting the vinyl polymer (B) comprises one or more vinyl monomers. The vinyl monomer constituting the vinyl monomer component (b) is not particularly limited, but examples thereof include various vinyl-based monomers such as (meth)acrylate monomers, aromatic vinyl monomers, and vinyl cyanide monomers.
[0112] Examples of the (meth)acrylate monomer include alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, and i-butyl methacrylate; and alkyl acrylates such as methyl acrylate, ethyl acrylate, and n-butyl acrylate. Examples of aromatic vinyl monomers include styrene, alkyl-substituted styrenes (p-methylstyrene, m-methylstyrene, o-methylstyrene, 2,4-dimethylstyrene, 2,5-dimethylstyrene, 3,4-dimethylstyrene, 3,5-dimethylstyrene, p-ethylstyrene, m-ethylstyrene, o-ethylstyrene, etc.), alkyl-substituted isopropenylbenzenes (isopropenylbenzene (α-methylstyrene), isopropenyltoluene, isopropenylethylbenzene, isopropenylpropylbenzene, isopropenylbutylbenzene, isopropenylpentylbenzene, isopropenylhexylbenzene, isopropenyloctylbenzene, etc.), 1,1-diphenylethylene, etc. Among them, styrene and α-methylstyrene are preferred because they can suppress the generation of cullets. Examples of the vinyl cyanide monomer include acrylonitrile and methacrylonitrile. These may be used alone or in combination of two or more.
[0113] In terms of obtaining a molded article with better weather resistance, the vinyl monomer component (b) preferably contains at least one selected from the group consisting of (meth)acrylate monomers and aromatic vinyl monomers. The total ratio of the (meth)acrylate monomer and the aromatic vinyl monomer to 100 mass% of the vinyl monomer component (b) is preferably 50 mass% or more, more preferably 70 mass% or more and 100 mass% or less, and even more preferably 90 mass% or more and 100 mass% or less.
[0114] Among (meth)acrylate monomers and aromatic vinyl monomers, the vinyl monomer component (b) more preferably contains either or both of methyl methacrylate and styrene, since these give molded articles with particularly excellent weather resistance. The total ratio of methyl methacrylate and styrene to 100% by mass of the vinyl monomer component (b) is preferably 50% by mass or more.
[0115] The vinyl monomer component (b) preferably contains a (meth)acrylate monomer, in terms of improving the dispersibility of the polymer particles (C) in the thermoplastic resin and improving the weather resistance of the molded article. The ratio of the (meth)acrylate monomer to 100% by mass of the vinyl monomer component (b) is preferably 50% by mass or more, more preferably 70% by mass or more and 100% by mass or less, and even more preferably 90% by mass or more and 100% by mass or less.
[0116] It is more preferable that the vinyl monomer component (b) contains methyl methacrylate among (meth)acrylate monomers, since this provides particularly excellent dispersibility of the polymer particle group (C) in the thermoplastic resin and excellent weather resistance of the molded article. The ratio of methyl methacrylate to 100% by mass of the vinyl monomer component (b) is preferably 50% by mass or more, more preferably 70% by mass or more and 100% by mass or less, and even more preferably 90% by mass or more and 100% by mass or less.
[0117] The glass transition temperature (hereinafter, also referred to as "Tg") of the vinyl polymer (B) is preferably 70° C. or higher, more preferably 80° C. or higher, and even more preferably 90° C. or higher, and is preferably 105° C. or lower. When the Tg of the vinyl polymer (B) is equal to or higher than the lower limit, the powder properties (powder flowability and particle size) of the polymer particle group (C) become good. The Tg of the vinyl polymer (B) can be adjusted by the types and ratio of the vinyl monomers constituting the vinyl monomer component (b).
[0118] The Tg of the vinyl polymer (B) is determined by the FOX formula. In this case, the Tg of the homopolymer of the vinyl monomer constituting the vinyl monomer component (b) can be, for example, the value described in "POLYMER HANDBOOK" (Wiley Interscience / 1999). The Tg of the homopolymer of the vinyl monomer not described in this document can be calculated using Bicerano's method "Prediction of Polymer Properties" (MARCEL DEKKER / 2002).
[0119] (Method for Producing Polymer Particles (C)) The polymer particle group (C) is obtained by polymerizing a vinyl monomer (a) in the presence of a latex of a polymer having a siloxane unit containing an aryl group to obtain a polymer (A), and then polymerizing the polymer with a vinyl monomer (b). The latex is obtained by polymerizing an organosiloxane containing an aryl group to produce a polyorganosiloxane. The polymer particle group (C) can be produced, for example, by a method of polymerizing (graft polymerizing) the vinyl monomer component (b) in the presence of the polymer (A). This produces a polymer (C1) in which the vinyl monomer component (b) is grafted to the polymer (A). The vinyl monomer component (b) is polymerized alone without being grafted to the polymer (A) to produce a vinyl polymer (B), which is physically adsorbed to the outer surface of the polymer (A) to produce a polymer complex (C2).
[0120] The polymer particles (C) are preferably produced by adding the vinyl monomer component (b) to a latex of the polymer (A) and polymerizing the vinyl monomer component (b) in the latex. As described above, the latex of the polymer (A) is preferably produced by polymerizing the vinyl monomer component (a) in the presence of a latex containing the polyorganosiloxane (A1).
[0121] The temperature at which the vinyl monomer component (b) is polymerized (hereinafter referred to as "polymerization temperature (T b The polymerization temperature is not particularly limited, and conventional conditions can be used, for example, at 45 to 95° C. and for a polymerization time of 0.1 to 10 hours.
[0122] The method of adding the vinyl monomer component (b) to the latex of the polymer (A) is not particularly limited, but it is preferable to add it dropwise, since this suppresses the generation of cullets and improves the grafting rate between the polymer (A) and the vinyl monomer component (b). At this time, the entire amount of the vinyl monomer component (b) may be added dropwise continuously, or it may be added dropwise in several portions with a holding time during which the vinyl monomer component (b) is not added dropwise. When the vinyl monomer component (b) is composed of multiple types of vinyl monomers, the method of continuously dropping the entire amount of the vinyl monomer component (b) is not particularly limited, and examples thereof include a method of continuously adding a mixture of the same composition, a method of adding while continuously changing the composition as in power feed polymerization, etc. When the vinyl monomer component (b) is composed of multiple types of vinyl monomers, examples of a method of adding dropwise in multiple portions with a holding time in between include a method of adding a mixture of the same composition in multiple portions, and a method of adding each component alone and / or a mixture of different compositions in multiple portions.
[0123] When the vinyl monomer component (b) contains a (meth)acrylate monomer, an aromatic vinyl monomer, and a vinyl cyanide monomer, it is preferable to polymerize the (meth)acrylate monomer and then polymerize the aromatic vinyl monomer and the vinyl cyanide monomer. By carrying out the polymerization in this manner, the powder properties (powder flowability and particle size) of the polymer particle group (C) obtained by carrying out a powder recovery step after the polymerization become good.
[0124] The vinyl monomer component (b) easily forms a graft copolymer (C1) with the polymer (A) by chemically bonding with units based on the siloxane-based crosslinking agent contained in the polyorganosiloxane (A1) and / or units based on the monomer (a1-3) contained in the vinyl polymer (A2).
[0125] In order to improve the efficiency of this grafting, a polyfunctional monomer such as ethylene glycol dimethacrylate, propylene glycol dimethacrylate, 1,3-butylene glycol dimethacrylate, 1,4-butylene glycol dimethacrylate, ethylene glycol diacrylate, propylene glycol diacrylate, 1,3-butylene glycol diacrylate, 1,4-butylene glycol diacrylate, 1,6-hexanediol diacrylate, divinylbenzene, polyfunctional (meth)acrylic group-modified silicone, allyl methacrylate, triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, etc. can be polymerized in advance before the addition of the vinyl monomer component (b).
[0126] The emulsifier used when polymerizing the vinyl monomer component (b) is not particularly limited, and the same emulsifier as that used in the production of the polyorganosiloxane (A1) and / or the production of the vinyl polymer (A2) can be used, with anionic emulsifiers or nonionic emulsifiers being preferred. Furthermore, when polymerizing the vinyl monomer component (b), no particular emulsifier is added, and the polymerization may be carried out using only the emulsifier contained in the vinyl polymer (A2) latex.
[0127] The total amount of emulsifier used in the production of polyorganosiloxane (A1), the production of vinyl polymer (A2) and the polymerization of vinyl monomer component (b) is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, and more preferably 10 parts by mass or less, more preferably 5 parts by mass or less, based on 100 parts by mass of the total of all monomers forming polymer particle group (C). The particle size of the latex of polymer particle group (C) can be adjusted to a desired value by the total amount of emulsifier. If the total amount of emulsifier is equal to or more than the lower limit, the stability of each of the latex of polyorganosiloxane (A1), the latex of polymer (A), and the latex of polymer (C) can be sufficiently increased. If the total amount of emulsifier is equal to or less than the upper limit, the amount of emulsifier remaining in the powder of polymer particle group (C) can be sufficiently reduced, and the deterioration of the thermal decomposition resistance and surface appearance of a molded body using a resin composition containing polymer particle group (C) and a thermoplastic resin can be suppressed.
[0128] When polymerizing the vinyl monomer component (b), a chain transfer agent may be used for the purpose of adjusting the acetone soluble portion, adjusting the molecular weight, etc. Examples of the chain transfer agent include mercaptans such as n-dodecyl mercaptan, t-dodecyl mercaptan, n-octyl mercaptan, n-tetradecyl mercaptan, n-hexyl mercaptan, and n-butyl mercaptan; halogen compounds such as carbon tetrachloride and ethylene bromide; α-methylstyrene dimer, etc. These chain transfer agents may be used alone or in combination of two or more.
[0129] The amount of the chain transfer agent used is preferably 2.0% by mass or less, and may be 0% by mass, based on 100% by mass of the vinyl monomer component (b). By setting the amount of the chain transfer agent used to 2.0% by mass or less, a decrease in the ratio of THF insoluble matter in the polymer particle group (C) is suppressed, and the impact strength of the molded article is more excellent.
[0130] After polymerizing the vinyl monomer component (b), the polymer particles (C) may be recovered as a powder from the resulting latex of the polymer particles (C). When the polymer particles (C) are recovered as a powder, a direct drying method such as a spray drying method or a coagulation method can be used. In the coagulation method, the amount of polymerization aid residues contained in the obtained powder, such as the emulsifier and its coagulation salt used during polymerization, and the initiator, can be reduced in the washing step after coagulation. On the other hand, in the direct drying method, the aids added during polymerization can be generally left in the obtained powder. These powder recovery methods can be appropriately selected to make the polymer particles (C) remain in a preferred state when added to a thermoplastic resin.
[0131] The spray drying method is a method in which the latex of the polymer particle group (C) is sprayed in the form of fine droplets in a dryer, and then heated gas for drying is applied to the droplets to dry them. Examples of methods for generating fine droplets include a rotating disk type, a pressure nozzle type, a two-fluid nozzle type, and a pressurized two-fluid nozzle type. The capacity of the dryer may be any of a small capacity for laboratory use and a large capacity for industrial use. The temperature of the heating gas for drying is preferably 200°C or less, more preferably 120 to 180°C. Two or more types of graft copolymer latexes produced separately can also be spray-dried together. Furthermore, in order to improve powder properties such as blocking during spray drying and bulk density, an optional component such as silica can be added to the latex of the polymer particle group (C) and spray-dried.
[0132] The coagulation method is a method in which the latex of the polymer particles (C) is coagulated, and the polymer particles (C) are separated, recovered, and dried. First, the latex of the polymer (C) is put into hot water in which a coagulant is dissolved, and the polymer particles (C) are separated by salting out and coagulation. Next, the separated wet polymer particles (C) are dehydrated, etc., and the polymer particles (C) with a reduced water content are recovered. The recovered polymer particles (C) are dried using a squeeze dehydrator or a hot air dryer.
[0133] Examples of the coagulant include inorganic salts such as aluminum chloride, aluminum sulfate, sodium sulfate, magnesium sulfate, sodium nitrate, and calcium acetate, and acids such as sulfuric acid, with calcium acetate being particularly preferred. These coagulants may be used alone or in combination of two or more.
[0134] The coagulant is usually used as an aqueous solution. The concentration of the aqueous coagulant solution is preferably 0.1% by mass or more, particularly 1% by mass or more, from the viewpoint of stably coagulating and recovering the polymer particles (C). In addition, from the viewpoint of reducing the amount of coagulant remaining in the recovered polymer particles (C) and preventing deterioration of the molded appearance of the molded product, the concentration of the aqueous coagulant solution is preferably 20% by mass or less, particularly 15% by mass or less. The amount of the aqueous coagulant solution is not particularly limited, but is preferably 10 parts by mass or more and 500 parts by mass or less per 100 parts by mass of the latex of the polymer particle group (C).
[0135] The method for contacting the latex of the polymer particles (C) with the aqueous coagulant solution is not particularly limited, but typically includes the following methods. (1) A method in which latex is continuously added to an aqueous coagulant solution while stirring it and maintaining the solution for a certain period of time. (2) A method in which an aqueous coagulant solution and latex are continuously poured into a vessel equipped with a stirrer at a constant ratio and brought into contact with each other, and a mixture containing the coagulated polymer and water is continuously withdrawn from the vessel. The temperature when the latex is contacted with the aqueous coagulant solution is not particularly limited, but is preferably 30° C. or higher and 100° C. or lower. The contact time is not particularly limited.
[0136] The coagulated polymer particles (C) are washed with water in an amount of about 1 to 100 times by mass of the polymer particles (C) and filtered. The filtered wet polymer particles (C) are dried using a fluidized bed dryer or a squeeze dehydrator. The drying temperature and drying time may be appropriately determined depending on the polymer particles (C) to be obtained. It is also possible to directly send the polymer particles (C) discharged from the squeeze dehydrator or extruder to an extruder or molding machine for producing a resin composition without recovering them, and mix them with a thermoplastic resin to obtain a molded product.
[0137] [Resin composition] A resin composition according to one embodiment of the present invention (hereinafter also referred to as "the resin composition") contains polymer particles (C) and a thermoplastic resin (hereinafter also referred to as "thermoplastic resin (E)").
[0138] The thermoplastic resin (E) is not particularly limited, and examples thereof include engineering plastics (e.g., aromatic polycarbonate), styrene-based resins, aromatic polyester resins, olefin-based resins (e.g., polyethylene), thermoplastic elastomers, biodegradable resins (e.g., polylactic acid), halogen-based resins (e.g., vinyl chloride resins), and acrylic resins.
[0139] As the engineering plastic, various known thermoplastic engineering plastics can be used without any particular limitation. Examples of engineering plastics include polyphenylene ether, polycarbonate, polyester polymers (polyethylene terephthalate, polybutylene terephthalate, etc.), syndiotactic polystyrene, nylon polymers (6-nylon, 6,6-nylon, etc.), polyarylate, polyphenylene sulfide, polyether ketone, polyether ether ketone, polysulfone, polyether sulfone, polyamide imide, polyether imide, and polyacetal.
[0140] In addition, special styrene-based resins such as heat-resistant ABS, which are required to have excellent heat resistance and melt fluidity, and heat-resistant acrylic resins can also be exemplified as engineering plastics in the present invention. Among these, when strength expression is more important, aromatic polycarbonate and polybutylene terephthalate are more preferable. Examples of aromatic polycarbonates include 4,4'-dioxydiarylalkane-based polycarbonates such as 4,4'-dihydroxydiphenyl-2,2-propane (ie, bisphenol A)-based polycarbonates.
[0141] Examples of olefin resins include high density polyethylene, medium density polyethylene, low density polyethylene, copolymers of ethylene and other α-olefins; polypropylene, copolymers of propylene and other α-olefins; polybutene, poly-4-methylpentene-1, and the like.
[0142] Examples of the thermoplastic elastomer include styrene-based elastomers, urethane-based elastomers, polyolefin-based elastomers, polyamide-based elastomers, fluorine-based elastomers, chlorinated PE-based elastomers, and acrylic-based elastomers.
[0143] Styrene-based elastomers include styrene-butadiene-styrene copolymer (SBS), styrene-isoprene-styrene copolymer (SIS), styrene-ethylene-butene copolymer (SEB), styrene-ethylene-propylene copolymer (SEP), styrene-ethylene-butene-styrene copolymer (SEBS), styrene-ethylene-propylene-styrene copolymer (SEPS), styrene-ethylene-ethylene-propylene-styrene copolymer (SEEPS), styrene-butadiene-butylene-styrene copolymer (partially hydrogenated styrene-butadiene-styrene copolymer: SBBS), partially hydrogenated styrene-isoprene-styrene copolymer, partially hydrogenated styrene-isoprene-butadiene-styrene copolymer, etc. "-" indicates that the monomers that form the units connected by "-" are copolymerized, and "·" indicates that they are randomly modified by hydrogenation or other methods after copolymerization.
[0144] Urethane-based elastomers include reaction products of polymeric diols, organic diisocyanates, and chain extenders. Examples of the polymer diol include polyester diol, polyether diol, polyester ether diol, polycarbonate diol, and polyester polycarbonate diol. Examples of organic diisocyanates include 4,4'-diphenylmethane diisocyanate, toluene diisocyanate, p-phenylene diisocyanate, xylylene diisocyanate, naphthalene diisocyanate, hydrogenated 4,4'-diphenylmethane diisocyanate (4,4'-dicyclohexylmethane diisocyanate), isophorone diisocyanate, hexamethylene diisocyanate, etc. Among these organic diisocyanates, 4,4'-diphenylmethane diisocyanate is preferred. Chain extenders include ethylene glycol, diethylene glycol, 1,4-butanediol, 1,5-pentanediol, 2-methyl-1,3-propanediol, 1,6-hexanediol, neopentyl glycol, 1,9-nonanediol, cyclohexanediol, 1,4-bis(β-hydroxyethoxy)benzene, and the like.
[0145] Examples of polyolefin elastomers include ethylene-propylene rubber, ethylene-propylene-diene rubber, ethylene-vinyl acetate copolymer, butyl rubber, butadiene rubber, propylene-butene copolymer, and ethylene-acrylic acid ester copolymer.
[0146] Examples of styrene-based resins include polystyrene, acrylonitrile-styrene copolymers, acrylonitrile-styrene-α-methylstyrene copolymers, acrylonitrile-methyl methacrylate-styrene-α-methylstyrene copolymers, ABS resins, AS resins, MABS resins, MBS resins, AAS resins, AES resins, acrylonitrile-butadiene-styrene-α-methylstyrene copolymers, acrylonitrile-methyl methacrylate-butadiene-styrene-α-methylstyrene copolymers, styrene-maleic anhydride copolymers, styrene-maleimide copolymers, styrene-N-substituted maleimide copolymers, acrylonitrile-styrene-N-substituted maleimide copolymers, acrylonitrile-butadiene-styrene-β-isopropenylnaphthalene copolymers, and acrylonitrile-methyl methacrylate-butadiene-styrene-α-methylstyrene-maleimide copolymers.
[0147] The aromatic polyester resin is a polymer of a polybasic acid and a polyhydric alcohol, and is not particularly limited as long as it has thermoplastic properties. Examples of the polybasic acid include terephthalic acid, naphthalic dicarboxylic acid, cyclohexyl dicarboxylic acid, and esters thereof. Examples of the polyhydric alcohol include ethylene glycol, propylene glycol, butanediol, pentanediol, neopentyl glycol, hexanediol, octanediol, decanediol, cyclohexane dimethanol, hydroquinone, bisphenol A, 2,2-bis(4-hydroxyethoxyphenyl)propane, 1,4-dimethyloltetrabromobenzene, and tetrabromobisphenol A bis(2-hydroxyethyl)ether (TBA-EO). The polyester resin may be a homopolymer, a copolymer, or a blend of two or more of these. As the polyester-based resin, a commercially available product such as "PETG" manufactured by Eastman Chemical may be used.
[0148] Examples of biodegradable resins include microbial polymers, chemically synthesized polymers, and natural polymers. Examples of microbial polymers include biopolyesters such as polyhydroxybutyrate / valerate (PHB / V), bacterial cellulose, and microbial polysaccharides (pullulan, curdlan, etc.). Examples of chemically synthesized polymers include aliphatic polyester resins (polycaprolactone, polybutylene succinate, polyethylene succinate, polyglycolic acid, polylactic acid, etc.), polyvinyl alcohol, and polyamino acids (PMLG, etc.). Examples of natural polymers include chitosan, cellulose, starch, and cellulose acetate.
[0149] Examples of halogen-based resins include vinyl chloride resins such as vinyl chloride homopolymers, copolymers containing 80% or more by mass of vinyl chloride, and highly chlorinated polyvinyl chloride. Examples of copolymer components include monovinylidene compounds such as ethylene, vinyl acetate, methyl methacrylate, and butyl acrylate, in addition to vinyl chloride. The copolymer may contain these compounds in a total amount of 20% or less by mass. Examples of halogen-based resins include vinyl chloride resins, as well as fluorinated polymers, brominated polymers, and iodinated polymers.
[0150] Examples of the acrylic resin include copolymers of methyl methacrylate and a copolymerizable vinyl monomer. Examples of the copolymerizable vinyl monomer include alkyl acrylates such as methyl acrylate, ethyl acrylate, i-propyl acrylate, n-butyl acrylate, and 2-ethylhexyl acrylate, alkyl methacrylates such as ethyl methacrylate, propyl methacrylate, and n-butyl methacrylate, and aromatic vinyl compounds such as styrene, α-methylstyrene, and vinyl toluene.
[0151] The thermoplastic resin (E) of the present invention also includes polymer alloys of engineering plastics, such as polyester resins such as polyphenylene ether, polycarbonate, polyethylene terephthalate, and polybutylene terephthalate, polyamide resins such as syndiotactic polystyrene, 6-nylon and 6,6-nylon, polyarylate, polyphenylene sulfide, polyether ketone, polyether ether ketone, polysulfone, polyether sulfone, polyamide imide, polyether imide, and polyacetal, with other thermoplastic resins.
[0152] These thermoplastic resins (E) can be used alone or in combination of two or more. The thermoplastic resin (E) is preferably at least one selected from the group consisting of aromatic polycarbonate, acrylic resin, aliphatic polyester resin, styrene-acrylonitrile copolymer, polyethylene terephthalate, polybutylene terephthalate, polyvinyl chloride, polyphenylene sulfide, and polyacetal, more preferably at least one selected from the group consisting of acrylic resin, aliphatic polyester resin, and styrene-acrylonitrile copolymer, even more preferably at least one selected from the group consisting of acrylic resin and aliphatic polyester resin, and particularly preferably at least one selected from the group consisting of polymethyl methacrylate and polylactic acid, because it is industrially easily available and has an excellent balance between the impact strength and colorability of the molded product.
[0153] The ratio of the polymer particle group (C) to 100% by mass of the present resin composition is preferably 0.5% by mass or more, more preferably 1% by mass or more, and even more preferably 2% by mass or more, while it is preferably 60% by mass or less, and more preferably 50% by mass or less. If the ratio of the polymer particle group (C) is equal to or more than the lower limit, the impact strength of the obtained molded article is superior, and if it is equal to or less than the upper limit, the decrease in the flowability and heat distortion temperature of the resin composition can be suppressed.
[0154] The ratio of the thermoplastic resin (E) to 100% by mass of the resin composition is preferably 40% by mass or more, more preferably 50% by mass or more, and is preferably 99.5% by mass or less, more preferably 99% by mass or less, and even more preferably 98% by mass or less. If the ratio of the thermoplastic resin (E) is equal to or more than the lower limit, the decrease in the flowability and heat distortion temperature of the resin composition can be suppressed, and if it is equal to or less than the upper limit, the impact strength of the obtained molded article is superior.
[0155] The present resin composition may further contain at least one component selected from the group consisting of phosphoric acid compounds and alkali metal salts thereof (hereinafter also referred to as "component (D)"). Component (D) plasticizes the resin composition containing the polymer particles (C) and improves the flowability of the resin composition during molding. It also inhibits the molecular weight of the resin composition from decreasing, improving molding stability.
[0156] Examples of the phosphoric acid compound in component (D) include alkyl phosphoric acids such as polyoxyalkylene alkyl ether phosphoric acids; and alkylaryl phosphoric acids such as polyoxyalkylene alkyl phenyl ether phosphates. In the polyoxyalkylene alkylphenyl ether phosphate and the polyoxyalkylene alkyl ether phosphate, examples of the polyoxyalkylene group include polyoxyethylene groups, and polyoxyethylene groups are preferred. The number of oxyethylene units in the polyoxyethylene group is, for example, 2 to 14, preferably 2 to 10, more preferably 2 to 8, and even more preferably 2 to 6. The number of carbon atoms in the alkyl group is, for example, 1 to 20, preferably 5 to 18, more preferably 7 to 16, and even more preferably 10 to 16. Examples of the alkali metal salt include sodium salts and potassium salts.
[0157] As component (D), from the viewpoint of easy adjustment of the phosphorus atom content described later, an alkali metal salt of a phosphoric acid compound is preferred, and an alkali metal salt of an alkyl phosphoric acid and an alkali metal salt of an alkylaryl phosphoric acid are more preferred. Among them, from the viewpoint of the fluidity and molding stability of the resin composition during molding, an alkali metal salt of a polyoxyalkylene alkylphenyl ether phosphoric acid and an alkali metal salt of a polyoxyalkylene alkyl ether phosphoric acid are preferred, and an alkali metal salt of a polyoxyalkylene alkyl ether phosphoric acid is more preferred. As the alkali metal salt of polyoxyalkylene alkylphenyl ether phosphate, an alkali metal salt of polyoxyethylene alkylphenyl ether phosphate is preferred. As the alkali metal salt of polyoxyalkylene alkyl ether phosphate, an alkali metal salt of polyoxyethylene alkyl ether phosphate is preferred. Among these, alkali metal salts of polyoxyethylene alkyl ether phosphates are preferred. These compounds can be used alone or in combination of two or more.
[0158] When the present resin composition contains component (D), the content of component (D) in the present resin composition is set taking into consideration the ratio of phosphorus atoms contained in component (D) (hereinafter also referred to as the "phosphorus content") to the total of 100 mass% of the polymer particle group (C) and component (D). From the viewpoint of the fluidity and molding stability of the resin composition during molding, the phosphorus content is preferably 10 ppm by mass or more, more preferably 50 ppm by mass or more, even more preferably 100 ppm by mass or more, particularly preferably 200 ppm by mass or more, and most preferably 300 ppm by mass or more. The upper limit of the phosphorus atom content is not particularly limited, but is, for example, 2000 ppm by mass or less, preferably 1500 ppm by mass or less.
[0159] The resin composition may further contain an emulsifier other than the component (D). The emulsifier is not particularly limited, and for example, the same emulsifier as that used in the production of the polymer particles (C) can be used. When the present resin composition contains component (D), the total ratio of the polymer particle group (C) and component (D) to 100% by mass of the present resin composition is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 98% by mass or more.
[0160] A preferred embodiment of the present resin composition contains the polymer particles (C) and an emulsifier, at least a part of which is recovered in powder form from a latex which is the alkali metal salt of the phosphoric acid compound. Such a composition can be produced, for example, by adding an alkali metal salt of a phosphoric acid compound to the latex of the polymer particles (C) (which may contain other emulsifiers) and recovering the powder, or by adding an alkali metal salt of a phosphoric acid compound during the polymerization process of the polymer particles (C) (when polymerizing the polymer (A) or the vinyl polymer (B)) and recovering the powder. Examples of the powder recovery method include the same method as the method of recovering the polymer particles (C) as a powder from the latex of the polymer particles (C).
[0161] In addition to the above, the present resin composition may contain various well-known additives within the scope of not impairing the object of the present invention. Examples of additives include flame retardants (phosphorus-based, bromine-based, silicone-based, organometallic salt-based, etc.), anti-drip agents (e.g., fluorinated polyolefin, silicone, and aramid fiber), lubricants (e.g., long-chain fatty acid metal salts such as magnesium stearate, etc.), release agents (e.g., pentaerythritol tetrastearate, etc.), nucleating agents, antistatic agents, stabilizers (e.g., phenol-based stabilizers, sulfur-based stabilizers, phosphorus-based stabilizers, ultraviolet absorbers, amine-based light stabilizers, etc.), fillers (titanium oxide, talc, mica, kaolin, calcium carbonate, glass flakes, etc.), plasticizers, reinforcing agents (e.g., glass fiber, carbon fiber, etc.), colorants, pigments, etc.
[0162] The phenol-based stabilizer is a stabilizer having a phenolic hydroxyl group, and among them, a hindered phenol-based antioxidant in which one or two carbon atoms adjacent to the carbon atom of the aromatic ring to which the phenolic hydroxyl group is bonded are substituted with a substituent having 4 or more carbon atoms can be preferably used. In this case, the substituent having 4 or more carbon atoms can be bonded to the carbon atom of the aromatic ring via a carbon-carbon bond or via an atom other than carbon.
[0163] Examples of phenol-based stabilizers include non-hindered phenol-based antioxidants such as p-cyclohexylphenol, 3-t-butyl-4-methoxyphenol, 4,4'-isopropylidenediphenol, and 1,1-bis(4-hydroxyphenyl)cyclohexane, 2-t-butyl-4-methoxyphenol, 2,6-di-t-butyl-p-cresol, 2,4,6-tri-t-butylphenol, 4-hydroxymethyl-2,6-di-t-butylphenol, styrenated phenol, 2,5-di-t-butylhydroquinone, and octyl phenol. Tadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, triethylene glycol bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,2'-methylene bis(4-methyl-6-t-butylphenol), 2,2'-methylene bis(6 -t-butyl-4-ethylphenol), 2,2'-methylenebis[4-methyl-6-(1,3,5-trimethylhexyl)phenol], 4,4'-methylenebis(2,6-di-t-butylphenol), 4,4'-butylidenebis(3-methyl-6-t-butylphenol), 2,6-bis(2-hydroxy-3-t-butyl-5-methylbenzyl)-4-methylphenol, 1,1,3-tris[2-methyl-4-hydroxy-5-t-butylphenyl]butane, 1,3,5-trimethyl-2,4,6-tris[3,5-di-t [3-(3,5-di-t-butyl-4-hydroxybenzyl)benzene, tris[3-(3,5-di-t-butyl-4-hydroxybenzyl)isocyanurate, tris[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionyloxyethyl]isocyanurate, 4,4'-thiobis(3-methyl-6-t-butylphenol), 2,2'-thiobis(4-methyl-6-t-butylphenol), 4,4'-thiobis(2-methyl-6-t-butylphenol), and thiobis(β-naphthol).In particular, the hindered phenol-based antioxidants themselves tend to form stable radicals, and therefore can be suitably used as radical trapping agents. These phenol-based stabilizers can be used alone or in combination of two or more kinds.
[0164] The content of the phenol-based stabilizer relative to 100% by mass of the present resin composition is preferably 0.001% by mass or more, more preferably 0.003% by mass or more, and is preferably 2% by mass or less, more preferably 1% by mass or less. If the content of the phenol-based stabilizer is equal to or more than the lower limit, the oxidation prevention effect is excellent, and if it is equal to or less than the upper limit, the oxidation heat stability of the resin composition and the resin decomposition during melt kneading can be further suppressed.
[0165] The sulfur-based stabilizer is a stabilizer that does not have a phenolic hydroxyl group but has a sulfur atom, and acts as a decomposer of hydroperoxides generated by deterioration of thermoplastic resins, thereby improving the heat aging resistance of the resin composition and improving the retention of color tone, tensile strength, elongation, etc. The sulfur-based stabilizer can be used alone, but by using it in combination with the phenol-based stabilizer, it is possible to further improve the long-term thermal stability.
[0166] Examples of sulfur-based stabilizers include didodecylthiodipropionate, ditetradecylthiodipropionate, dioctadecylthiodipropionate, pentaerythritol tetrakis (3-dodecylthiopropionate), thiobis (N-phenyl-β-naphthylamine), 2-mercaptobenzothiazole, 2-mercaptobenzimidazole, tetramethylthiuram monosulfide, tetramethylthiuram disulfide, nickel dibutyldithiocarbamate, nickel isopropylxanthate, and trilauryltrithiophosphite. In particular, thioether-based stabilizers having a thioether structure can be preferably used because they receive oxygen from an oxidized substance and reduce it. These sulfur-based stabilizers can be used alone or in combination of two or more.
[0167] The content of the sulfur-based stabilizer relative to 100% by mass of the present resin composition is preferably 0.001% by mass or more, more preferably 0.003% by mass or more, and is preferably 2% by mass or less, more preferably 1% by mass or less. If the content of the sulfur-based stabilizer is equal to or more than the lower limit, the thermal stabilization effect is excellent, and if it is equal to or less than the upper limit, resin decomposition during melt-kneading of the resin composition can be further suppressed.
[0168] The phosphorus-based stabilizer is a stabilizer having a phosphorus atom, and is a phosphite compound having a P(OR)3 structure. Here, R is an alkyl group, an alkylene group, an aryl group, an arylene group, etc., and the three Rs may be the same or different, and two Rs may form a ring structure. Furthermore, one molecule may have a plurality of P(OR)3 structures. The phosphorus-based stabilizer acts as a decomposer of hydroperoxides generated by the deterioration of thermoplastic resins, thereby improving the heat aging resistance of the resin composition and improving the retention of color tone, tensile strength, elongation, etc. The phosphorus-based stabilizer can be used alone, but by using it in combination with the phenol-based stabilizer, it is possible to improve the long-term heat stability in particular and suppress the yellowing caused by the phenol-based stabilizer.
[0169] Examples of the phosphite ester compound include triaryl phosphites (triphenyl phosphite, tricresyl phosphite, trixylenyl phosphite, trinaphthyl phosphite, etc.), diaryl alkyl phosphites (diaryl C1-18 alkyl phosphites such as diphenyl isooctyl phosphite, diphenyl decyl phosphite, etc.), aryl dialkyl phosphites (aryl C1-18 dialkyl phosphites such as phenyl diisooctyl phosphite, etc.), trialkyl phosphites (trimethyl phosphite, phosphites containing alkylaryl units [tris(2,4-t-butylphenyl)phosphite, tris(nonylphenyl)phosphite, tris(dinonylphenyl)phosphite, dinonylphenyl-o-biphenyl phosphite, etc.], dialkyl phosphites (di-C1-18 alkyl phosphites such as dilauryl phosphite, etc.), tris(2,4-t-butylphenyl)phosphite, tris(nonylphenyl)phosphite, tris(dinonylphenyl)phosphite, dinonylphenyl-o-biphenyl phosphite, etc.], Tris(C1-18 alkyl-aryl)phosphite, 2,2-methylenebis(4,6-di-t-butylphenyl)octylphosphite, etc.], aliphatic carboxylic acid phosphite (C1-18 aliphatic carboxylic acid phosphite such as tristearyl phosphite, etc.), phosphites containing alkylene oxide units (polydipropylene glycol nonylphenyl phosphate, tetraphenyl dipropylene glycol phosphite, etc.), phosphites containing cyclic neopentane units [cyclic neopentane tetraylbis(octa decyl) phosphite, cyclic neopentanetetraylbis(2,4-di-t-butylphenyl) phosphite, cyclic neopentanetetraylbis(2,6-di-t-butyl-4-methylphenyl) phosphite, etc.], diphosphites (diisodecyl pentaerythritol diphosphite, didodecyl pentaerythritol diphosphite, 4,4'-isopropylidenediphenyl didodecyl diphosphite, etc.), triphosphites [hepta-cis-dipropylene glycol triphosphite, hexa-tridecyl-1,1,3-tri(3-t-butyl-6-methyl-4-oxyphenyl)-3-methylpropane triphosphite, etc. These phosphite compounds can be used alone or in combination of two or more.
[0170] Among these, when using, as the thermoplastic resin (E), a resin containing a carbonate bond, an ester bond, an amide bond or an acetal bond in the polymer structural unit, such as a polycarbonate resin, a polyester resin, an acrylic resin, a polyamide resin or a polyacetal resin, it is preferable to use a phosphorus-based stabilizer having high hydrolysis resistance, from the viewpoint of suppressing a decrease in the resistance to moist heat decomposition of these thermoplastic resins. Among these, preferred are phosphite compounds having one phosphorus atom in one molecule and each ester moiety having 8 or more carbon atoms (when multiple ester moieties form a ring, the total number of carbon atoms in the region sandwiched between the ester bonds is the carbon number for each), or phosphite compounds having multiple phosphorus atoms in one molecule and each ester moiety having 8 or more carbon atoms between each phosphorus element. Examples of such phosphite compounds include triC6-18 alkyl phosphites (triisodecyl phosphite, etc.), phosphites containing branched C3-6 alkyl groups (t-butyl groups, etc.) [tris(2,4-t-butylphenyl)phosphite, 2,2-methylenebis(4,6-di-t-butylphenyl)octyl phosphite, etc.], and tetraalkyl(C12-15)-4,4'-isopropylidenediphenyl diphosphites.
[0171] The content of the phosphorus-based stabilizer relative to 100% by mass of the present resin composition is preferably 0.001% by mass or more, more preferably 0.003% by mass or more, and is preferably 2% by mass or less, more preferably 1% by mass or less. If the content of the phosphorus-based stabilizer is equal to or more than the lower limit, the thermal stabilization effect is excellent, and if it is equal to or less than the upper limit, the resin decomposition during melt-kneading of the resin composition and the decrease in resistance to moist heat decomposition can be further suppressed.
[0172] In the present resin composition, when a phenol-based stabilizer is used in combination with a sulfur-based stabilizer and / or a phosphorus-based stabilizer, the total added mass of the sulfur-based stabilizer and the phosphorus-based stabilizer is preferably 0.1 times or more, more preferably 0.2 times or more, relative to the added mass of the phenol-based stabilizer, and is preferably 5 times or less, more preferably 3 times or less. If the content of the sulfur-based stabilizer and the phosphorus-based stabilizer is equal to or more than the lower limit, the effect of improving heat aging resistance is excellent, and if it is equal to or less than the upper limit, resin decomposition during melt-kneading of the resin composition can be further suppressed.
[0173] In the present resin composition, when a phenol-based stabilizer and a sulfur-based stabilizer and / or a phosphorus-based stabilizer are contained, the total content of the stabilizers is preferably 2% by mass or less relative to 100% by mass of the resin composition. By making the total content of the stabilizers 2% by mass or less, decomposition of the resin during melt kneading can be further suppressed.
[0174] Examples of the dye or pigment include inorganic pigments such as iron oxide, ultramarine, titanium oxide, and carbon black. Examples of organic pigments include blue pigments such as phthalocyanine and anthraquinone, red pigments such as perylene and quinacridone, and yellow pigments such as isoindolinone. Examples of special pigments include fluorescent pigments, metal powder pigments, and pearl pigments. Examples of dyes include nigrosine, perinone, and anthraquinone dyes. These dyes and pigments are commercially available in various grades according to the required color, and they can be used. These can be used alone or in combination of two or more.
[0175] (Method of producing resin composition) The resin composition can be produced by mixing the polymer particles (C), the thermoplastic resin (E), and, if necessary, additives. The method for mixing the materials is not particularly limited and may be any known blending method, such as a method of mixing and kneading using a tumbler, a V-type blender, a super mixer, a Nauta mixer, a Banbury mixer, a kneading roll, an extruder, or the like. An example of a method for producing the resin composition of the present invention is a method in which the polymer particle group (C), the pellet-like thermoplastic resin (E), and, if necessary, additives are mixed using an extruder, extruded into a strand shape, and cut into pellets using a rotary cutter, etc. By this method, a pellet-like resin composition can be obtained.
[0176] [Molded body] The molded article according to one embodiment of the present invention (hereinafter also referred to as "the present molded article") contains polymer particles (C) and a thermoplastic resin (E). The present molded article may further contain component (D). The present molded article is preferably made of the present resin composition described above.
[0177] The present molded article can be produced, for example, by molding the present resin composition. The molding method may be any molding method commonly used for molding thermoplastic resin compositions, such as injection molding, extrusion molding, blow molding, calendar molding, etc.
[0178] In a molded article produced from a resin composition containing polymer particles (C) and a thermoplastic resin (E), the Δ haze value is a value obtained by subtracting the haze value of the resin composition containing polymer particles (C) and a thermoplastic resin (E) from the haze value of the resin alone. The Δ haze value is preferably less than 14%, more preferably less than 13%, even more preferably less than 12%, and particularly preferably 8% or less. In this specification, the haze value can be measured by the method described in the examples. In addition, in a molded article produced from a resin composition containing the polymer particle group (C) and the thermoplastic resin (E), the total light transmittance is preferably 80% or more, more preferably 82% or more, and even more preferably 85% or more. In this specification, the total light transmittance can be measured by the method described in the examples.
[0179] In a molded article produced from a resin composition containing polymer particles (C) and a thermoplastic resin (E), the Charpy impact strength at -30°C is 0.5 kJ / m 2 It is preferable that the concentration is 1.0 kJ / m or more. 2 More preferably, it is 1.2 kJ / m or more. 2 The higher the Charpy impact strength at -30°C, the better. There is no particular upper limit, but for example, 7.0 kJ / m 2 Less than 5.0 kJ / m is preferable. 2 The following is more preferred: A molded article produced from a resin composition containing polymer particles (C) and a thermoplastic resin (E) has a Charpy impact strength at 23°C of 0.5 kJ / m 2 It is preferable that the concentration is 1.0 kJ / m or more. 2 More preferably, it is 1.5 kJ / m or more. 2 The Charpy impact strength at 23° C. is preferably as high as possible, and the upper limit is not particularly limited. For example, the Charpy impact strength at 23° C. is preferably 25 kJ / m 2 Less than 10 kJ / m is preferable. 2 The following is more preferred: In this specification, the Charpy impact strength can be measured by the method described in the Examples.
[0180] The molded article can be widely used industrially as various materials in the fields of automobiles, office automation equipment, home appliances, electrical and electronics, architecture, lifestyle and cosmetics, medical supplies, etc. More specifically, it can be used as housings for electronic devices, various parts, coating materials, automobile structural members, automobile interior parts, light reflectors, building structural members, fittings, etc. More specifically, it can be used as interior and exterior members for personal computer housings, mobile phone housings, portable information terminal housings, portable game machine housings, printers, copiers, etc., conductor coating materials, automobile interior and exterior members, building exterior members, resin window frame members, flooring materials, piping members, etc. EXAMPLES
[0181] The present invention will be described in more detail below with reference to Production Examples and Examples. Production Examples 1-1 to 1-10 are production examples of polyorganosiloxane (A1), Production Examples 2-1 to 2-13 are production examples of polymer composite (A), and Examples 1 to 9 and Comparative Examples 1 to 4 are production examples of polymer particle group (C). Note that "parts" means "parts by mass", "%" means "% by mass", and "ppm" means "ppm by mass". Various measurement methods are described below.
[0182] (1) Solids A mass w1 of the graft copolymer latex was dried in a hot air dryer at 180° C. for 30 minutes, and the mass w2 of the residue after drying was measured, and the solid content [%] was calculated by the following formula (1). Solid content [%] = w2 / w1 × 100 (1) (2) Polymerization rate The polymerization rate was calculated from the mass w3 of the total monomers charged when producing the polymer and the mass w4 of the solid content obtained after polymerization according to the following formula (2). Polymerization rate [%]=w4 / w3×100 (2)
[0183] (3) Particle size of graft copolymer measured by spectrophotometric method The concentration (solid content) of the graft copolymer latex was diluted with deionized water to 0.5 g / L, and the absorbance DA at a wavelength of 700 nm was measured using a UV-visible spectrophotometer (Shimadzu UV-mini1240). The particle size was calculated using the following formula (3).
[0184]
number
[0185] (4) Charpy impact strength In accordance with JIS K 7111-1 / 1eA, the Charpy impact strength of the test pieces (length 80.0 mm, width 10.0 mm, thickness 4 mm, with a V-notch) was measured at temperatures of 23°C and -30°C.
[0186] (5) Evaluation of molded appearance characteristics (total light transmittance, haze) In accordance with JIS K 7375, the total light transmittance and haze of a test piece (length 100 mm, width 50 mm, thickness 2 mm) were measured under a D65 light source using a Haze Meter NDH4000 manufactured by Nippon Denshoku Industries Co., Ltd.
[0187] (6) Refractive index of polyorganosiloxane (A1) and polymer particle group (C) The weight ratios of the charged raw materials, polydimethylsiloxane (refractive index: 1.40, specific gravity: 0.97), polydiphenylsiloxane (refractive index: 1.61, specific gravity: 1.08), polymethylphenylsiloxane (refractive index: 1.53, specific gravity: 1.01), polymethylmethacrylate (refractive index 1.49, specific gravity: 1.20), polystyrene (refractive index 1.59, specific gravity: 1.05), and poly-n-butylacrylate (refractive index 1.47, specific gravity: 1.09), were converted to polymer volume ratios and multiplied by each refractive index to calculate the refractive index of polyorganosiloxane (A1) and polymer particle group (C).
[0188] (7) Viscosity of aryl group-containing organosiloxane The viscosity was measured at 15°C in accordance with JIS K 8803 using a Toki Sangyo TVB10M model and a low viscosity adapter.
[0189] (8) Acetone insoluble and soluble matter The acetone soluble matter is measured by carrying out the following procedures (1-1) to (1-5). (1-1) 0.5 g of a sample (polymer particle group (C)) is added to 50 mL (44.5 g) of acetone to prepare a mixed solution, which is then allowed to stand at 25°C for 8 hours and then stirred with a stirrer for 30 minutes to dissolve the acetone-soluble components. (1-2) The mixed solution is placed in a centrifuge tube whose mass has been measured, and the liquid containing the acetone insoluble matter and the acetone soluble matter is separated by centrifugation (16,000 rpm, 4 hours). (1-3) After removing the supernatant, fresh acetone is added and stirred, and then centrifugal separation is performed again in the same manner as in (1-2) above to wash off the acetone-insoluble matter. (1-4) After repeating (1-3) twice, the supernatant is removed. The centrifuge tube with the acetone-insoluble matter remaining is immersed in a hot water bath (80°C, 8 hours) to volatilize the acetone, and then vacuum-dried at 65°C for 6 hours to obtain a dry sample (acetone-insoluble matter adhering to the centrifuge tube). (1-5) Measure the mass of the obtained dried sample (acetone insolubles + centrifuge tube), and calculate the ratio of acetone solubles w by the following formula: s Calculate the percentage. w s =1-(w c1 -w as ) / wt×100 wt: mass of polymer particle group (C) subjected to measurement w as : Mass of the centrifuge tube w c1 : Mass of acetone insoluble matter (including centrifuge tube)
[0190] [Production Example 1-1] 2 parts of 3-methacryloxypropyldimethoxymethylsilane (KBM502, manufactured by Shin-Etsu Silicone Co., Ltd., product name: KBM-502), 57 parts of a cyclic organosiloxane mixture (DMC, manufactured by Shin-Etsu Silicone Co., Ltd., product name: DMC, a mixture of cyclic organosiloxanes with 3 to 6 membered rings), and 43 parts of dimethoxydiphenylsilane (DMODPS, manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed to obtain 100 parts of an organosiloxane mixture. An aqueous solution of 0.7 parts of sodium dodecylbenzenesulfonate (Neopelex G15, manufactured by Kao Corporation, product name: Neopelex G-15, solid content equivalent) dissolved in 310 parts of deionized water was added to the mixture and stirred at 12,000 rpm for 5 minutes with an Ultra Turrax to obtain a stable premixed emulsion.
[0191] Next, an aqueous solution of 10 parts of dodecylbenzenesulfonic acid (Neopelex GS, manufactured by Kao Corporation, product name: Neopelex GS) dissolved in 90 parts of deionized water was placed in a 5-liter separable flask equipped with a cooling condenser, and the aqueous solution was heated to a temperature of 80°C. The above emulsion was then continuously added over a period of 240 minutes to cause a polymerization reaction, after which the solution was cooled to 25°C and a 5% aqueous sodium hydroxide solution was added to neutralize the reaction solution to a pH of 7.0, to obtain a polyorganosiloxane latex (A-1).
[0192] The refractive index of this latex was 1.485, the solid content was 17.4%, and the absorbance was 0.014. Table 1 shows the mixture ratio and the evaluation results.
[0193] [Production Examples 1-2 to 1-8, and 1-10] Polyorganosiloxane latexes (A-2) to (A-8) and (A-10) were obtained in the same manner as in Production Example 1-1, except that the types and amounts of each raw material used in Production Example 1-1 were changed as shown in Table 1. Table 1 shows the raw materials and the evaluation results.
[0194] [Production Example 1-9] 2 parts of tetraethoxysilane (TEOS, Dow Toray Co., Ltd., product name: DOWSIL Z-6697), 2 parts of 3-methacryloxypropyldimethoxymethylsilane (KBM502, Shin-Etsu Silicone Co., Ltd., product name: KBM-502), 57 parts of cyclic organosiloxane mixture (DMC, Shin-Etsu Silicone Co., Ltd., product name: DMC, mixture of cyclic organosiloxanes with 3 to 6 membered rings), and 43 parts of dimethoxydiphenylsilane (DMODPS, Tokyo Chemical Industry Co., Ltd.) were mixed to obtain 100 parts of organosiloxane mixture. An aqueous solution of 1 part of sodium dodecylbenzenesulfonate (Neopelex G15, Kao Corporation, product name: Neopelex G-15, solid content equivalent) dissolved in 220 parts of deionized water was added to the mixture, and the mixture was stirred at 12,000 rpm for 5 minutes with an Ultra Turrax to obtain a premixed emulsion.
[0195] The emulsion was then placed in a 5-liter separable flask equipped with a cooling condenser. The emulsion was heated to 80°C, and then a mixture of 0.20 parts of sulfuric acid and 2 parts of distilled water was added. The mixture was kept heated to 80°C for 6 hours to polymerize, then cooled to room temperature (25°C), and the resulting reaction liquid was kept at room temperature for 7 hours. Then, a 5% aqueous sodium hydroxide solution was added to neutralize the reaction liquid to pH 7.0, to obtain a polyorganosiloxane rubber latex (A-9).
[0196] The refractive index of this latex was 1.485, the solid content was 24.1%, and the absorbance was 0.740. Table 1 shows the raw materials and the evaluation results.
[0197] The abbreviations in Table 1 represent the following compounds: DMODPS: Dimethoxydiphenylsilane, manufactured by Tokyo Chemical Industry Co., Ltd. DMOMPS: Dimethoxymethylphenylsilane, manufactured by Tokyo Chemical Industry Co., Ltd. DMC: A mixture of cyclic organosiloxanes with 3 to 6 membered rings, manufactured by Shin-Etsu Silicones, product name: DMC KBM502: 3-Methacryloxypropyldimethoxymethylsilane, manufactured by Shin-Etsu Silicone Co., Ltd., Product name: KBM-502 TEOS: Tetraethoxysilane, manufactured by Dow Toray, product name: DOWSIL Z-6697 Neopelex G15: Sodium dodecylbenzenesulfonate, manufactured by Kao Corporation, product name: Neopelex G-15, values in the table are calculated as solid content. Neopelex GS: Dodecylbenzenesulfonic acid, manufactured by Kao Corporation, product name: Neopelex GS, values in the table are converted to solid content. The viscosity of dimethoxydiphenylsilane (DMODPS) was 11.1 mPa·s, and the viscosity of dimethoxymethylphenylsilane (DMOMPS) was 1.9 mPa·s.
[0198] [Table 1]
[0199] [Production Example 2-1] The polyorganosiloxane rubber latex (A-1) obtained in Production Example 1-1 was collected in a 5-liter separable flask in a polymer equivalent amount of 7 parts, and 155 parts of deionized water were added and mixed. Next, 13.4 parts of styrene (St), 58.9 parts of n-butyl acrylate (n-BA), 0.7 parts of allyl methacrylate (AMA), and 0.3 parts of sodium dodecylbenzenesulfonate (Neopelex G15, Kao Corporation, product name: Neopelex G-15, solid content equivalent) were added to the separable flask, and the atmosphere in the flask was replaced with nitrogen by passing a nitrogen gas flow through the flask, and the liquid temperature was raised to 45°C and stirred for 90 minutes. An aqueous solution of 0.08 parts of potassium persulfate (KPS, Nacalai Tesque) dissolved in 2 parts of deionized water was added to initiate radical polymerization. Thereafter, the liquid temperature was raised to 80° C. and maintained at that temperature for 1 hour to complete the polymerization, thereby obtaining a composite rubber latex containing a vinyl polymer (A2-1).
[0200] While maintaining the temperature of the composite rubber latex at 80° C., 20 parts of methyl methacrylate (MMA) was added dropwise to the latex over 30 minutes to polymerize. After the addition was completed, the liquid temperature was maintained at 80° C. for 1 hour and then cooled to 25° C. to obtain a latex of polyorganosiloxane-containing graft copolymer (G-1) as polymer (A1-1).
[0201] The refractive index of the latex was 1.488, the solid content was 32%, and the polymerization rate was 99%. The absorbance was 0.025, and the particle size calculated from the absorbance was 76 nm.
[0202] Next, 500 parts of an aqueous solution with a calcium acetate concentration of 1% by mass was kept at a temperature of 60° C., and 300 parts of the latex of the graft copolymer (G-1) was gradually dropped into the solution while stirring to solidify. The obtained graft copolymer (G-1) was filtered and dehydrated. Furthermore, 10 times the amount of water was added to 100 parts of the graft copolymer, and the mixture was washed for 10 minutes in a flask equipped with a stirrer, filtered, and dehydrated. This operation was repeated twice, and then dried to obtain a powder of polyorganosiloxane-containing graft copolymer (G-1). Table 2 shows the raw materials and evaluation results.
[0203] [Manufacturing Examples 2-2 to 2-13] Except for changing the type and amount of each raw material used in Production Example 2-1 to the conditions shown in the table, the same procedure as in Production Example 2-1 was used to produce polyorganosiloxane-containing graft copolymers (G-2) to (G-13) as polymers (A1-2) to (A1-10), and further obtain powders of polyorganosiloxane-containing graft copolymers. Table 2 shows the raw materials and the evaluation results.
[0204] The abbreviations in Table 2 represent the following compounds: ·BA: n-Butyl acrylate St: styrene ·AMA: Allyl methacrylate Neopelex G15: Sodium dodecylbenzenesulfonate, product name: Neopelex G-15, manufactured by Kao Corporation. The values in the table are calculated based on the solid content. KPS: Potassium persulfate (KPS, manufactured by Nacalai Tesque) MMA: Methyl methacrylate
[0205] [Table 2]
[0206] [Examples 1 to 8 and Comparative Examples 1 to 3] 30 parts by mass of the polyorganosiloxane-containing graft polymers (G-1) to (G-8), and (G-10) to (G-12) obtained in Production Examples 2-1 to 2-8, and 2-10 to 2-12, and 70 parts by mass of polymethyl methacrylate (manufactured by Mitsubishi Chemical Corporation, "VH5-001" (trade name)) were blended to obtain a mixture. This mixture was fed to a devolatilizing twin-screw extruder (manufactured by Ikegai Iron Works, PCM-30 (trade name)) heated to a barrel temperature of 250 ° C. and kneaded to produce pellets of a resin composition blended with 30% by mass of the polyorganosiloxane-containing graft polymer. Each pellet was separately fed to a Sumitomo injection molding machine SE100DU (product name) (manufactured by Sumitomo Heavy Industries, Ltd.) and molded bodies (test pieces for impact testing) measuring 80 mm in length, 10 mm in width, and 4 mm in thickness were obtained at a cylinder temperature of 250° C. and a mold temperature of 60° C., and molded bodies (test pieces for evaluating appearance characteristics) measuring 100 mm in length, 50 mm in width, and 2 mm in thickness were obtained. The results of the Charpy impact test and the haze measurement are shown in Table 3.
[0207] [Example 9 and Comparative Example 4] Except for changing the types and amounts of the raw materials used in Example 1 to the conditions shown in the table, Example 9 and Comparative Example 4 were produced and evaluated in the same manner as Example 1. The results are shown in Table 3.
[0208] [Reference Examples 1 and 2] Except for not adding 30% by mass of the polyorganosiloxane-containing graft polymer, production and evaluation were carried out in the same manner as in Example 1 or 9. The results are shown in Table 3.
[0209] The abbreviations in Table 3 represent the following compounds: VH5-001: Polymethyl methacrylate, manufactured by Mitsubishi Chemical Corporation, "VH5-001" (product name) INGEO-4032D: Polylactic acid, NatureWorks, "INGEO Biopolymer 4032D" (product name)
[0210] [Table 3]
[0211] The polyorganosiloxane-containing polymers (G-1) to (G-9) of Examples 1 to 9 contain siloxane units containing an aryl group and have an average particle size of 200 nm or less. Therefore, molded articles containing these have excellent impact resistance and transparency, and are highly industrially useful. On the other hand, since the polyorganosiloxane-containing polymer (G-10) of Comparative Example 1 does not contain a siloxane unit containing an aryl group, the molded article containing it had excellent impact strength but low transparency. Also, since the polyorganosiloxane-containing polymers (G-11) to (G-13) of Comparative Examples 2 to 4 had an average particle size exceeding 200 nm, the molded article containing them had excellent impact strength but low transparency.
Claims
1. A polymer particle group containing a polyorganosiloxane having a siloxane unit containing an aryl group, A group of polymer particles having an average particle size of 200 nm or less as measured by absorbance method.
2. 2. The polymer particle group according to claim 1, wherein the aryl group-containing siloxane unit is represented by the following general formula (1): 【Chemistry 1】 In formula (1), Ar is an aryl group, and R is a hydrogen atom, a halogen atom, an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, an aryl group having 5 to 12 carbon atoms, or a halogenated alkyl group having 1 to 3 carbon atoms.
3. The group of polymer particles according to claim 1 , wherein the polyorganosiloxane further contains a siloxane unit that does not contain an aryl group.
4. 4. The polymer particle group according to claim 3, wherein the content of the siloxane units containing an aryl group is 5 to 80 parts by mass, and the content of the siloxane units not containing an aryl group is 20 to 95 parts by mass, based on the total content of the siloxane units containing an aryl group and the siloxane units not containing an aryl group.
5. 2. The group of polymer particles according to claim 1, which contains structural units derived from a vinyl monomer (a).
6. The polymer particle group according to claim 3, wherein a mass ratio of [the total content of the siloxane units containing an aryl group and the siloxane units not containing an aryl group] / [the content of the structural units derived from the vinyl monomer (a)] is 3 / 97 to 50 / 50.
7. The polymer particle group according to claim 1, wherein the refractive index of the polyorganosiloxane is 1.410 to 1.
560.
8. A polymer particle group obtained by polymerizing a vinyl monomer (a) in the presence of a latex of a polymer having a siloxane unit containing an aryl group, and then polymerizing a vinyl monomer (b) to the polymer complex obtained, A group of polymer particles having an average particle size of 200 nm or less as measured by absorbance method.
9. A step of polymerizing an aryl group-containing organosiloxane to obtain a polyorganosiloxane; and polymerizing the polyorganosiloxane with a vinyl monomer (a) to obtain a polymer composite.
10. A method for producing polymer particles, comprising a step of polymerizing the polymer complex obtained by the method for producing polymer particles according to claim 9 with a vinyl monomer (b) to obtain polymer particles.
11. The method for producing a polymer particle group according to claim 10, wherein the viscosity of the organosiloxane containing an aryl group at 15° C. is 0.5 to 35.0 mPa·s.
12. The method for producing a polymer particle group according to claim 10, wherein the organosiloxane containing an aryl group is represented by the following general formula (2): 【Chemistry 2】 In formula (2), Ar is an aryl group, R 1 , R 2 , and R 3 are each independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, an aryl group having 5 to 12 carbon atoms, or a halogenated alkyl group having 1 to 3 carbon atoms.
13. A resin composition comprising the polymer particles according to any one of claims 1 to 8 and a thermoplastic resin.
14. The resin composition according to claim 13, wherein a mass ratio represented by [content of said polymer particle group] / [content of said thermoplastic resin] is 10 / 90 to 50 / 50.
15. The resin composition according to claim 13, wherein the thermoplastic resin is an acrylic resin or an aliphatic polyester resin.
Citation Information
Patent Citations
Graft copolymer, thermoplastic resin composition containing the same, and molded item thereof
JP2002020438A