Laminated structure, cured product and image display device light emitting element substrate
The laminated structure with specific resin layers addresses color variation and concealability issues in image display devices by optimizing light transmission and opacity, ensuring consistent color and effective hiding of light emitting elements.
Patent Information
- Application Number
- JP2024056418
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-11
AI Technical Summary
Existing image display devices with multilayered coating layers exhibit color differences when viewed from different angles and struggle with concealability of light emitting elements when turned off, particularly due to variations in light emission intensity and increased element count.
A laminated structure comprising a first thermosetting resin layer with specific haze and temperature properties, and a second thermosetting resin layer containing an inorganic filler, which reduces color variation and enhances concealability by optimizing light transmission and opacity.
The laminated structure improves color consistency across viewing angles and enhances the concealability of light emitting elements when turned off, providing a coating layer with improved properties for image display devices.
Smart Images

Figure 2024144396000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate structure, a cured product, and a light emitting element substrate for an image display device (hereinafter, also simply referred to as a light emitting element substrate). [Background technology]
[0002] Conventionally, image display devices have been developed that include a light-emitting element substrate on which light-emitting elements such as LEDs are mounted. A coating layer made of a transparent curable resin composition is formed on the surface of the light-emitting element substrate in order to protect the light-emitting elements such as LEDs (for example, Patent Documents 1 and 2).
[0003] In recent years, from the viewpoint of market needs such as versatility and high performance of image display devices, there is a demand for improvement of the coating layer. One of the means for improving the coating layer is to make the coating layer multi-layered. For example, Patent Document 3 discloses a multi-layered laminate structure in which a resin layer made of an encapsulant composition having a haze of 10% or less after curing is laminated with a resin layer made of an encapsulant composition containing an epoxy resin and dicyandiamide. The laminate structure described in Patent Document 3 does not inhibit the emission of the light emitter, and can conceal the light emitter when the light is turned off. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 8-283385 [Patent Document 2] JP 2011-42762 A [Patent Document 3] JP 2021-161413 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, it was found that the coating layer obtained by curing the laminated structure as described in Patent Document 3 has a problem in that the color of light emitted differs when the image display device having the light-emitting element is viewed from the front and when viewed from a 45° angle. In addition, since the number of light-emitting elements mounted is increasing due to the increase in size and high definition of the image display device, there was also a problem of improving the concealment of the light-emitting elements when they are turned off.
[0006] Therefore, an object of the present invention is to provide a laminated structure capable of forming a coating layer that improves the change in color during emission of light from a light-emitting element when the image display device is viewed from the front and from a 45° oblique direction and improves the concealment of the light-emitting element when the light is turned off, a cured product of the laminated structure, and a light-emitting element substrate for an image display device. [Means for solving the problem]
[0007] As a result of intensive research into the realization of the above object, the present inventors have found that the reason for the difference in color during light emission is that the intensity distribution of the light emitted by each color light-emitting element is different, for example, the red light-emitting element emits light uniformly in all directions, while the blue and green light-emitting elements emit light in the horizontal direction, so that when viewed from a 45° diagonal direction, the blue and green light emission may appear stronger than when viewed from the front. Therefore, as a result of further intensive research into a configuration for simultaneously improving the concealment of the light-emitting element when turned off, it has been found that in a laminated structure in which multiple thermosetting resin layers are laminated, it is necessary that the haze of the first thermosetting resin layer at a light wavelength of 450 to 750 nm after heat treatment at 150° C. for 60 minutes is set to a specific value or more, and that the second thermosetting resin layer contains an inorganic filler, and thus the present invention has been completed.
[0008] That is, the laminate structure of the present invention is a laminate structure having a first thermosetting resin layer and a second thermosetting resin layer, wherein the first thermosetting resin layer has a haze of 12% or more at a light wavelength of 450 to 750 nm after heat treatment at 150°C for 60 minutes, and the second thermosetting resin layer contains an inorganic filler. The laminate structure of the present invention may be a laminate structure having a first thermosetting resin layer and a second thermosetting resin layer, wherein the first thermosetting resin layer contains at least one of carbon black and titanium black, an epoxy resin having an alicyclic skeleton, and a thermoplastic resin, and when the first thermosetting resin layer contains the carbon black, the content thereof is 0.07 mass% or less based on the total solid content in the first thermosetting resin layer, and when the first thermosetting resin layer contains the titanium black, the content thereof is 0.70 mass% or more based on the total solid content in the first thermosetting resin layer, and the second thermosetting resin layer may contain an inorganic filler. The laminate structure of the present invention is preferably used for forming a covering layer for a light emitting element in a light emitting element substrate for an image display device.
[0009] In the laminate structure of the present invention, the first thermosetting resin layer preferably has a total light transmittance of 30 to 80% at a light wavelength of 450 to 750 nm after heat treatment at 150° C. for 60 minutes.
[0010] In the laminate structure of the present invention, the second thermosetting resin layer preferably contains 1 to 20 mass % of an inorganic filler based on the total solid content of the second thermosetting resin layer.
[0011] In the laminate structure of the present invention, the inorganic filler is preferably silica.
[0012] In the laminate structure of the present invention, the first thermosetting resin layer preferably contains a black colorant.
[0013] In the laminated structure of the present invention, at least one surface of the laminated structure is preferably supported or protected by a film.
[0014] The cured product of the present invention is characterized in that it is obtained by curing the first thermosetting resin layer and the second thermosetting resin layer that constitute the laminate structure.
[0015] The light emitting element substrate for an image display device of the present invention is characterized in that a light emitting element is covered with a covering layer containing the above-mentioned cured product.
[0016] A preferred light-emitting element substrate for an image display device of the present invention is a light-emitting element substrate for an image display device in which a light-emitting element is covered with a covering layer including a first resin-cured product layer and a second resin-cured product layer, the second resin-cured product layer and the first resin-cured product layer being laminated in this order from the light-emitting element side, the first resin-cured product layer having a haze of 12% or more at a light wavelength of 450 to 750 nm, and the second resin-cured product layer containing an inorganic filler. Effect of the Invention
[0017] According to the present invention, it is possible to provide a laminate structure capable of forming a coating layer that improves the change in color of the light-emitting element when the image display device is viewed from the front and from a 45° oblique direction and improves the concealment of the light-emitting element when the light is turned off, a cured product of the laminate structure, and a light-emitting element substrate for an image display device. Also, according to the present invention, it is possible to provide a laminate structure capable of forming a coating layer that is excellent in blackness when the light-emitting element is turned off, a cured product of the laminate structure, and a light-emitting element substrate for an image display device. [Brief description of the drawings]
[0018] [Figure 1] 1 is a schematic cross-sectional view showing an embodiment of a laminated structure of the present invention. [Diagram 2] 1 is a schematic cross-sectional view showing an embodiment of a light-emitting element substrate for an image display device according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] [Laminated structure] The laminated structure of the present invention is a laminated structure having a first thermosetting resin layer and a second thermosetting resin layer, characterized in that the first thermosetting resin layer has a haze of 12% or more at a light wavelength of 450 to 750 nm after heat treatment at 150° C. for 60 minutes, and the second thermosetting resin layer contains an inorganic filler. Since the first thermosetting resin layer has a haze of 12% or more at a light wavelength of 450 to 750 nm, i.e., in the visible light region, after heat treatment at 150° C. for 60 minutes, and the second thermosetting resin layer contains an inorganic filler, it is possible to reduce the change in color during emission of light from the light-emitting element when the image display device is viewed from the front and from a 45° oblique direction, and at the same time improve the concealment of the light-emitting element when it is turned off.
[0020] FIG. 1 is a schematic cross-sectional view showing an embodiment of the laminated structure of the present invention. In FIG. 1, the laminated structure 1 of the present invention has a laminated structure in which a first thermosetting resin layer 10 and a second thermosetting resin layer 20 are laminated. In FIG. 1, the second thermosetting resin layer 20 is thicker than the first thermosetting resin layer 10. The laminated structure of the present invention is suitably used for forming a covering layer for a light-emitting element in a light-emitting element substrate for an image display device. In this application, it is preferable that the second thermosetting resin layer is positioned on the light-emitting element side, that is, the second thermosetting resin layer is positioned so as to directly cover the light-emitting element, and the first thermosetting resin layer is positioned on the opposite side of the second thermosetting resin layer to the light-emitting element.
[0021] The total thickness of the first thermosetting resin layer and the second thermosetting resin layer constituting the laminated structure of the present invention is, for example, 50 to 500 μm, and preferably 100 to 400 μm. In applications in which a coating layer for a light-emitting element such as a micro LED is formed, the total thickness should be thicker than the height of the light-emitting element, and the total thickness may be appropriately set according to the height of the light-emitting element.
[0022] [First thermosetting resin layer] The haze is 12% or more, preferably 13% or more, and more preferably 14% or more. The higher the haze, the less the color change of the light emitting element when the image display device is viewed from the front and from a 45° angle can be reduced, and the concealment of the light emitting element when the light is turned off can be improved at the same time, and the blackness when the light is turned off can be excellent. On the other hand, the haze is preferably 50% or less, and more preferably 40% or less. By setting the haze to 50% or less, the inconvenience of the cured product of the first thermosetting resin layer becoming cloudy can be suppressed. Therefore, the blackness of the light emitting element when the light is turned off can be further improved. The haze means the haze of the first thermosetting resin layer at a light wavelength of 450 to 750 nm after heat treatment at 150° C. for 60 minutes. Here, the first thermosetting resin layer preferably has a total light transmittance of 30 to 80% at a light wavelength of 450 to 750 nm after heat treatment for 60 minutes at 150° C. When the haze is equal to or greater than the specific value and the total light transmittance is 30 to 80%, the change in color during emission of the light emitting element when the image display device is viewed from the front and from a 45° oblique direction can be reduced, the concealment of the light emitting element when turned off can be improved, and the blackness when turned off can be improved. The haze and total light transmittance of the first thermosetting resin layer are values measured as follows. That is, the thermosetting resin composition for forming the first thermosetting resin layer is applied to a film (PET film; TN-200 manufactured by Toyobo Co., Ltd., thickness 38 μm, size 30 cm × 30 cm) (hereinafter referred to as film A) using a bar coater so that the thickness of the thermosetting resin layer becomes a specific thickness after drying. Next, it is dried at 70 to 120 ° C (average 100 ° C) for 5 to 10 minutes in a hot air circulation drying oven so that the organic solvent remaining in the first thermosetting resin layer is 0.5 to 2.5 mass %, and the first thermosetting resin layer is formed on the film A. Next, a film (biaxially oriented polypropylene film, OPP, Alphan FG-201, Fish Eyeless, manufactured by Oji F-Tex Co., Ltd.) (hereinafter referred to as Film B) is laminated to the surface of the first thermosetting resin layer using a roll laminator set to a temperature of 80°C to prepare a laminated structure for evaluation consisting of Film A / first thermosetting resin layer / Film B. Film B (OPP) of the prepared laminated structure for evaluation is peeled off, and the laminate is laminated on a slide glass having a thickness of 1 mm using a vacuum laminator MVLP-500 (manufactured by Meiki Seisakusho Co., Ltd.). The conditions are a lamination temperature of 50 to 80°C and a pressure of 0.3 MPa. Next, the laminate is heated in a hot air circulation drying oven at 150°C for 60 minutes to cure the thermosetting resin layer and obtain a cured product. Then, film A is peeled off from the surface of the cured product to obtain an evaluation substrate having a cured product on the slide glass. The total light transmittance and haze of the cured product formed on the evaluation substrate are measured at a light wavelength of 450 to 750 nm using a hazemeter NDH7000II (manufactured by Nippon Denshoku Industries Co., Ltd.) The thickness of the first thermosetting resin layer in the evaluation laminate structure is the same as the thickness of the first thermosetting resin layer in the laminate structure of the present invention.
[0023] The thickness of the first thermosetting resin layer is not particularly limited, but is preferably, for example, 5 to 150 μm, and more preferably 5 to 100 μm.
[0024] (Coloring agent) The first thermosetting resin layer preferably contains a colorant. By containing a colorant, the haze can be easily set to 12% or more. Examples of the colorant include black colorants, blue colorants, red colorants, yellow colorants, green colorants, purple colorants, orange colorants, and brown colorants. The colorants can be used alone or in combination of two or more.
[0025] Among the colorants, black colorants such as carbon black, titanium black, iron oxide, cobalt oxide, and perylene-based black colorants are preferred. In particular, the colorant contained in the first thermosetting resin layer is more preferably at least one of carbon black and titanium black. By containing a black colorant in the first thermosetting resin layer, the haze can be easily set to 12% or more. Therefore, the change in color during emission of the light-emitting element when the image display device is viewed from the front and from a 45° angle can be reduced, and the concealment of the light-emitting element when turned off can be improved, resulting in excellent blackness when turned off.
[0026] As the carbon black, one or more of known carbon blacks such as channel black, furnace black, thermal black, and lamp black can be used. Resin-coated carbon black may also be used. When carbon black is blended, carbon black powder or a carbon black dispersion may be added. Examples of commercially available carbon black products include MA-100 (manufactured by Mitsubishi Chemical Corporation).
[0027] Examples of commercially available titanium black products include Titanium Black 10S, 12S, 13R, 13M, 13M-C, 13R, 13R-N, and 13M-T (product names: manufactured by Mitsubishi Materials Corporation), Tilack D TM-F, TM-A, TM-B, TS-A, TM-F, TS-M, TM-A-CSM, TS-A-CSM, TM-F-CSM, and TS-M-CSM (product names: manufactured by Ako Kasei Co., Ltd.).
[0028] When a colorant is contained, the content thereof in the first thermosetting resin layer is preferably 0.01 to 10 mass %, more preferably 0.02 to 8 mass %, and further preferably 0.03 to 7 mass %, based on the total solid content. Since the colorant contained in the first thermosetting resin layer is preferably a black colorant, the preferred content of the black colorant in the first thermosetting resin layer is the same as above.
[0029] (thermosetting resin) The first thermosetting resin layer preferably contains an epoxy resin as a thermosetting resin. However, the thermosetting resin contained in the first thermosetting resin layer may be other than the epoxy resin as long as it is a transparent thermosetting resin. The epoxy resin is a resin having an epoxy group, and any conventionally known epoxy resin can be used. Examples of the epoxy resin include a bifunctional epoxy resin having two epoxy groups in a molecule and a multifunctional epoxy resin having three or more epoxy groups in a molecule. The epoxy resin may be any of a solid epoxy resin, a semi-solid epoxy resin, and a liquid epoxy resin. In this specification, a solid epoxy resin refers to an epoxy resin that is solid at 40°C, a semi-solid epoxy resin refers to an epoxy resin that is solid at 20°C and liquid at 40°C, and a liquid epoxy resin refers to an epoxy resin that is liquid at 20°C. The liquid state is determined in accordance with the "Method of Confirming Liquid State" in Appendix 2 of the Ministerial Ordinance on the Testing and Properties of Hazardous Materials (Ministry of Home Affairs Ordinance No. 1 of 1989). For example, the method described in paragraphs 23 to 25 of JP 2016-079384 A can be used.
[0030] Examples of epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AF type epoxy resins, phenol novolac type epoxy resins, tert-butyl-catechol type epoxy resins, glycidylamine type epoxy resins, aminophenol type epoxy resins, alicyclic epoxy resins, etc. Examples of commercially available epoxy resins include N-740 manufactured by DIC Corporation.
[0031] Among epoxy resins, it is preferable to contain an epoxy resin having an alicyclic skeleton in order to reduce coloration of the cured product so as not to inhibit light emission. The epoxy resin having an alicyclic skeleton may be a hydrogenated epoxy resin of an epoxy resin having an aromatic ring, such as a bisphenol A type epoxy resin. Examples of the alicyclic skeleton include a cyclopentane ring, a dicyclopentadiene ring, and a cyclohexane ring. Examples of commercially available epoxy resins having an alicyclic skeleton include ST-6100 manufactured by Nippon Steel Chemical & Material Co., Ltd. and YX8000 manufactured by Mitsubishi Chemical Corporation.
[0032] The epoxy resin may be used alone or in combination of two or more kinds. When the epoxy resin is contained, the content thereof is, for example, 10 to 60 mass % based on the total solid content of the first thermosetting resin layer.
[0033] In the present invention, when an epoxy resin having an alicyclic skeleton is contained, the content thereof is, for example, 10 to 50 mass % based on the total solid content of the first thermosetting resin layer.
[0034] (thermoplastic resin) The first thermosetting resin layer may contain a thermoplastic resin. By containing a thermoplastic resin, it becomes easier to manufacture a laminated structure having a thick first thermosetting resin layer and a thick second thermosetting resin layer. Examples of the thermoplastic resin include a thermoplastic polyhydroxypolyether resin, a phenoxy resin, a polyvinyl acetal resin, a polyamide resin, a polyamideimide resin, a block copolymer, a polymer resin having a glass transition point of 20°C or less and a weight average molecular weight of 10,000 or more, and the like. The thermoplastic resin is preferably a phenoxy resin. Examples of the phenoxy resin include a phenoxy resin which is a condensation product of epichlorohydrin and various bifunctional phenolic compounds, and a hydroxyl group of a hydroxyether part present in the skeleton of the phenoxy resin is esterified using various acid anhydrides or acid chlorides.
[0035] Specific examples of phenoxy resins include FX280 and FX293 manufactured by Nippon Steel Chemical & Material Co., Ltd., and YX8100, YX6954, YL6954, and YL6974 manufactured by Mitsubishi Chemical Corporation. Specific examples of polyvinyl acetal resins include the S-LEC KS series manufactured by Sekisui Chemical Co., Ltd., specific examples of polyamide resins include the KS5000 series manufactured by Resonac Corporation and the BP series manufactured by Nippon Kayaku Co., Ltd., and specific examples of polyamideimide resins include the KS9000 series manufactured by Resonac Corporation.
[0036] The thermoplastic resin may be used alone or in combination of two or more. When the thermoplastic resin is contained, the content thereof is, for example, 10 to 50 mass % based on the total solid content of the first thermosetting resin layer.
[0037] (hardening agent) The first thermosetting resin layer preferably contains a curing agent. The curing agent may be any agent that reacts with the thermosetting resin contained in the first thermosetting resin layer, and examples of the curing agent include dicyandiamide, a compound having a phenolic hydroxyl group, an acid anhydride, a compound having a thiol group, and a carboxyl group-containing resin. Among these, the curing agent is preferably dicyandiamide.
[0038] Examples of the compound having a phenolic hydroxyl group include conventionally known compounds such as phenol novolac resins, alkylphenol novolac resins, bisphenol A novolac resins, dicyclopentadiene-type phenolic resins, Xylok-type phenolic resins, terpene-modified phenolic resins, cresol / naphthol resins, polyvinyl phenols, phenol / naphthol resins, α-naphthol skeleton-containing phenolic resins, triazine skeleton-containing cresol novolac resins, biphenylaralkyl-type phenolic resins, and Xylok-type phenolic novolac resins.
[0039] Examples of the acid anhydride include alicyclic dibasic acid anhydrides such as methyltetrahydrophthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, nadic anhydride, 3,6-endomethylenetetrahydrophthalic anhydride, methylendomethylenetetrahydrophthalic anhydride, and tetrabromophthalic anhydride; aliphatic or aromatic dibasic acid anhydrides such as succinic anhydride, maleic anhydride, itaconic anhydride, octenylsuccinic anhydride, pentadodecenylsuccinic anhydride, phthalic anhydride, and trimellitic anhydride; and aliphatic or aromatic tetrabasic acid dianhydrides such as biphenyltetracarboxylic dianhydride, diphenylethertetracarboxylic dianhydride, butanetetracarboxylic dianhydride, cyclopentanetetracarboxylic dianhydride, pyromellitic anhydride, and benzophenonetetracarboxylic dianhydride.
[0040] The compound having a thiol group is a compound having two or more thiol groups in one molecule. Any of the conventionally known compounds having a thiol group can be used. Examples of the compound having a thiol group include TMMP; trimethylolpropane tris(3-mercaptopropionate), PEMP; pentaerythritol tetrakis(3-mercaptopropionate), DPMP; dipentaerythritol hexaneth(3-mercaptopropionate), etc.
[0041] Examples of the carboxyl group-containing resin include a copolymer resin having a carboxyl group, a urethane resin having a carboxyl group, a carboxyl group-containing resin having an alicyclic structure, etc. The carboxyl group-containing resin may be any of a monomer, an oligomer, and a polymer.
[0042] The curing agent may be used alone or in combination of two or more. When the curing agent is contained, the content thereof is, for example, 1 to 70 mass % based on the total solid content of the first thermosetting resin layer.
[0043] (Cure accelerator) The first thermosetting resin layer may contain a curing accelerator. The curing accelerator accelerates the thermosetting reaction and is used to further improve properties such as adhesion, chemical resistance, and heat resistance. Specific examples of the curing accelerator include imidazole and imidazole derivatives such as imidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 4-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole; guanamines such as acetoguanamine and benzoguanamine; diaminodiphenylmethane, m-phenylene; Polyamines such as diamine, m-xylylenediamine, diaminodiphenylsulfone, urea, urea derivatives, melamine, polybasic hydrazides; their organic acid salts and / or epoxy adducts; amine complexes of boron trifluoride; triazine derivatives such as ethyldiamino-S-triazine, 2,4-diamino-S-triazine, 2,4-diamino-6-xylyl-S-triazine; trimethylamine, triethanolamine, N,N-dimethyloctylamine, N-benzoxamine, etc. Tertiary amines such as diethyldimethylamine, pyridine, 4-dimethylaminopyridine, N-methylmorpholine, hexa(N-methyl)melamine, 2,4,6-tris(dimethylaminophenol), and tetramethylguanidine; aminophenols such as m-aminophenol; organic phosphines such as tributylphosphine, triphenylphosphine, and tris-2-cyanoethylphosphine; phosphonium salts such as tri-n-butyl(2,5-dihydroxyphenyl)phosphonium bromide and hexadecyltributylphosphonium chloride; quaternary ammonium salts such as benzyltrimethylammonium chloride and phenyltributylammonium chloride; styrene-maleic anhydride resin; equimolar reaction product of phenylisocyanate and dimethylamine, equimolar reaction product of organic polyisocyanate such as tolylene diisocyanate and isophorone diisocyanate and dimethylamine, and conventionally known curing accelerators such as metal catalysts can be mentioned. As the curing accelerator, imidazole and its derivatives are preferable.
[0044] The curing accelerator can be used alone or in combination of two or more. When the curing accelerator is contained, the content thereof can be, for example, in the range of 0.1 to 10 parts by mass per 100 parts by mass of the thermosetting resin, particularly when it is desired to accelerate the curing. In the case of a metal catalyst, the content is, for example, 10 to 550 ppm in terms of metal per 100 parts by mass of the thermosetting resin.
[0045] (Inorganic filler) The first thermosetting resin layer may contain an inorganic filler. Examples of the inorganic filler include barium sulfate, barium titanate, silica such as amorphous silica, crystalline silica, fused silica, and spherical silica, talc, clay, Neuburg silica particles, boehmite, magnesium carbonate, calcium carbonate, aluminum oxide, aluminum hydroxide, silicon nitride, aluminum nitride, and calcium zirconate. When the first thermosetting resin layer contains an inorganic filler, the inorganic filler is preferably silica.
[0046] The average particle size of the inorganic filler is preferably 0.1 to 10 μm, more preferably 0.2 to 1 μm. When the average particle size of the inorganic filler is in the above range, the haze can be set to 12% or more. Therefore, the change in color of the light-emitting element when the image display device is viewed from the front and from a 45° angle can be easily reduced, and the concealment of the light-emitting element when the image display device is turned off can be improved, and the blackness when the image display device is turned off is also excellent. Here, the average particle size refers to the value of D50 when the particle size distribution is prepared on a volume basis, and can be determined by a laser diffraction particle size distribution measuring device or a measuring device using a dynamic light scattering method. As a measuring device using the laser diffraction method, Microtrac MT3300EXII manufactured by Microtrac-Bell Co., Ltd. can be mentioned, and as a measuring device using the dynamic light scattering method, Nanotrac Wave II UT151 manufactured by Microtrac-Bell Co., Ltd. can be mentioned. As the measurement sample, a sample in which the inorganic filler is dispersed in PMA (propylene glycol monomethyl ether acetate) can be preferably used.
[0047] The inorganic filler may be used alone or in combination of two or more. When the inorganic filler is contained, the content thereof is, for example, 0.1 to 10 mass % based on the total solid content of the first thermosetting resin layer.
[0048] (Organic solvent) The first thermosetting resin layer may contain an organic solvent. Examples of the organic solvent include ketones, aromatic hydrocarbons, glycol ethers, glycol ether acetates, esters, alcohols, aliphatic hydrocarbons, and petroleum-based solvents. Specific examples of the organic solvent include ketones such as methyl ethyl ketone, cyclohexanone, methyl butyl ketone, and methyl isobutyl ketone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as cellosolve, methyl cellosolve, butyl cellosolve, carbitol, methyl carbitol, butyl carbitol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; ethyl acetate, butyl acetate, and acetic acid. Examples of the solvent include esters such as isobutyl acetate, ethylene glycol monoethyl ether acetate, dipropylene glycol methyl ether acetate, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, and propylene glycol butyl ether acetate; alcohols such as ethanol, propanol, 2-methoxypropanol, n-butanol, isobutyl alcohol, isopentyl alcohol, ethylene glycol, and propylene glycol; aliphatic hydrocarbons such as octane and decane; petroleum solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha, as well as tetrachloroethylene and turpentine. In addition, organic solvents such as Swazol 1000 and Swazol 1500 manufactured by Maruzen Petrochemical Co., Ltd., Solvent #100 and Solvent #150 manufactured by Sankyo Chemical Co., Ltd., Shellsol A100 and Shellsol A150 manufactured by Shell Chemicals Japan Co., Ltd., and Ipzol 100 and Ipzol 150 manufactured by Idemitsu Kosan Co., Ltd. may also be used. The organic solvent may be used alone or in combination of two or more kinds.
[0049] When the organic solvent is contained, the content thereof in the first thermosetting resin layer is, for example, 0.1 to 5% by mass.
[0050] (Other Ingredients) The first thermosetting resin layer may contain conventional additives such as acrylic, fluorine-based, or silicone-based defoamers, leveling agents, surface conditioners, antioxidants, UV absorbers, antistatic agents, flame retardants, surfactants, plasticizers, lubricants, flow control agents, thickeners, film-building agents, adhesion promoters, release agents, organic fillers, rubber particles, ion adsorbents, and reactive diluents.
[0051] [Second thermosetting resin layer] The second thermosetting resin layer contains an inorganic filler, which can improve the concealment of the light-emitting element when the light is turned off. The second thermosetting resin layer preferably has a haze of 80% or more, more preferably 82% or more, after the heat treatment. The higher the haze, the less the color change of the light emitting element when the image display device is viewed from the front and from a 45° angle, and the more the concealment of the light emitting element when the light is off is improved, and the blackness when the light is off is also superior. Here, the method and conditions for measuring the haze after the heat treatment, i.e., the heat treatment temperature, time, and light wavelength, are the same as those described above.
[0052] The thickness of the second thermosetting resin layer is not particularly limited, but is preferably from 45 to 350 μm, and more preferably from 95 to 300 μm.
[0053] (Inorganic filler) The second thermosetting resin layer contains an inorganic filler. Examples of the inorganic filler include those mentioned above, and one type may be used alone or two or more types may be used in combination. Among the inorganic fillers, silica is preferred.
[0054] The average particle size of the inorganic filler is preferably 0.1 to 10 μm, more preferably 0.2 to 1 μm. Here, the average particle size and the method for measuring it are the same as those described above. When the average particle size of the inorganic filler contained in the second thermosetting resin layer is within the above range, the haze of the cured product of the second thermosetting resin layer can be easily set to 80% or more. Therefore, the change in color during emission of the light-emitting element when the image display device is viewed from the front and from a 45° angle can be easily reduced, and the concealment of the light-emitting element when the light is turned off can be improved, resulting in excellent blackness when the light is turned off.
[0055] The content of the inorganic filler in the second thermosetting resin layer is preferably 1 to 20 mass %, more preferably 3 to 15 mass %, and particularly preferably 7 to 15 mass %, based on the total solid content of the second thermosetting resin layer.
[0056] (Coloring agent) The second thermosetting resin layer may contain a colorant, preferably together with an inorganic filler. In addition to the above, the colorant may be a white colorant, and one type may be used alone or two or more types may be used in combination. When the second thermosetting resin layer contains a colorant, the colorant is preferably a black colorant such as carbon black, titanium black, iron oxide, cobalt oxide, or a perylene-based black colorant.
[0057] When a colorant is contained, the content thereof is preferably 0.01 to 3 mass % based on the total solid content of the second thermosetting resin layer, and more preferably 0.01 to 2 mass %. Since the colorant contained in the second thermosetting resin layer is preferably a black colorant, the preferred content of the black colorant in the second thermosetting resin layer is the same as above.
[0058] (thermosetting resin) The second thermosetting resin layer preferably contains an epoxy resin as a thermosetting resin. However, the thermosetting resin contained in the second thermosetting resin layer may be a transparent thermosetting resin other than an epoxy resin. The epoxy resin may be any of the above-mentioned, and may be used alone or in combination of two or more. In order to reduce coloring of the cured product so as not to inhibit light emission, it is preferable to contain an epoxy resin having an alicyclic skeleton.
[0059] When an epoxy resin is contained, the content thereof is, for example, 10 to 50 mass % based on the total solid content of the second thermosetting resin layer. In the present invention, when an epoxy resin having an alicyclic skeleton is contained, the content thereof is, for example, 10 to 50 mass % based on the total solid content of the second thermosetting resin layer.
[0060] (thermoplastic resin) The second thermosetting resin layer may contain a thermoplastic resin. The thermoplastic resin may be any of the above-mentioned, and may be used alone or in combination of two or more. The thermoplastic resin is preferably a phenoxy resin.
[0061] When the thermoplastic resin is contained, the content thereof is, for example, 10 to 50 mass % based on the total solid content of the second thermosetting resin layer.
[0062] (hardening agent) The second thermosetting resin layer may contain a curing agent. The curing agent may be any of the above-mentioned, and may be used alone or in combination of two or more. The curing agent is preferably dicyandiamide.
[0063] When the curing agent is contained, the content thereof is, for example, 1 to 70 mass % based on the total solid content of the second thermosetting resin layer.
[0064] (Cure accelerator) The second thermosetting resin layer may contain a curing accelerator. The curing accelerator may be any of the above-mentioned, and may be used alone or in combination of two or more. The curing accelerator is preferably imidazole or its derivatives.
[0065] When a curing accelerator is contained, the content thereof may be, for example, 0.1 to 10 parts by mass relative to 100 parts by mass of the thermosetting resin, particularly when it is desired to accelerate curing. In the case of a metal catalyst, the content is, for example, 10 to 550 ppm in terms of metal relative to 100 parts by mass of the thermosetting resin.
[0066] (Organic solvent) The second thermosetting resin layer may contain an organic solvent. Examples of the organic solvent include those mentioned above, and one type may be used alone or two or more types may be used in combination.
[0067] When the organic solvent is contained, the content thereof in the second thermosetting resin layer is, for example, 0.1 to 5% by mass.
[0068] (Other Ingredients) The second thermosetting resin layer may contain other components, which are the same as those described above.
[0069] A preferred laminate structure of the present invention is a laminate structure having a first thermosetting resin layer and a second thermosetting resin layer, wherein the first thermosetting resin layer contains at least one of carbon black and titanium black, an epoxy resin having an alicyclic skeleton, and a thermoplastic resin, and when the first thermosetting resin layer contains carbon black, the content thereof is 0.07 mass% or less based on the total solid content in the first thermosetting resin layer, and when the first thermosetting resin layer contains titanium black, the content thereof is 0.70 mass% or more based on the total solid content in the first thermosetting resin layer, and the second thermosetting resin layer contains an inorganic filler.
[0070] In the preferred laminated structure of the present invention, the first thermosetting resin layer preferably contains at least one of carbon black and titanium black. When the first thermosetting resin layer contains carbon black, the content of the carbon black is preferably 0.07% by mass or less, and more preferably 0.01% by mass or more, based on the total solid content in the first thermosetting resin layer. When the first thermosetting resin layer contains titanium black, the content of the titanium black is preferably 0.70% by mass or more, and more preferably 10% by mass or less, more preferably 8% by mass or less, and particularly preferably 7% by mass or less, based on the total solid content in the first thermosetting resin layer.
[0071] The laminated structure of the present invention can be preferably used to form a coating layer for a light-emitting element. Examples of the light-emitting element include light-emitting bodies such as LEDs and organic ELs. In particular, the laminated structure can be preferably used to seal micro LEDs. The light-emitting color of the light-emitting element is not particularly limited, but the effects of the present invention can be preferably achieved in the case of red, green, or blue.
[0072] The laminated structure of the present invention may have at least one surface supported or protected by a film, which may be the first film or the second film described below.
[0073] The first film has a role of supporting the first thermosetting resin layer and the second thermosetting resin layer of the laminated structure. As the first film, for example, polyester films such as polyethylene terephthalate and polyethylene naphthalate, films made of thermoplastic resins such as polyimide films, polyamideimide films, polyethylene films, polytetrafluoroethylene films, polypropylene films, and polystyrene films, and surface-treated paper can be used. Among these, polyester films can be preferably used from the viewpoints of heat resistance, mechanical strength, and handling. The thickness of the first film is not particularly limited, but is appropriately selected in the range of about 10 to 150 μm depending on the application. The surfaces of the first film on the first thermosetting resin layer and second thermosetting resin layer side may be subjected to a release treatment.
[0074] The second film is provided on the surface of the first thermosetting resin layer and the second thermosetting resin layer opposite to the first film for the purpose of protecting the first thermosetting resin layer and the second thermosetting resin layer of the laminated structure. As the second film, for example, a film made of a thermoplastic resin exemplified in the first film, surface-treated paper, etc. can be used, among which polyester film, polyethylene film, and polypropylene film are preferable. The thickness of the second film is not particularly limited, but is appropriately selected in the range of about 10 to 150 μm depending on the application. The surface of the second film on the side of the first thermosetting resin layer and the second thermosetting resin layer may be subjected to a release treatment.
[0075] The method for producing the laminated structure of the present invention is not particularly limited, and it may be produced by a known, conventional method. In the case of a laminated structure in which at least one side of the laminated structure is supported or protected by a film, for example, a first film is coated with either a thermosetting resin composition for the first or second thermosetting resin layer, and then the other thermosetting resin composition is coated thereon and dried to produce a laminated structure. A second film may be further laminated on the side opposite to the first film of this laminated structure. As an example of another production method, a dry film having a first thermosetting resin layer formed on a film and a dry film having a second thermosetting resin layer formed on a film are each previously produced. After that, these dry films are laminated so that the first thermosetting resin layer and the second thermosetting resin layer are in contact with each other, thereby forming a laminated structure in which both sides are supported or protected by a film. Alternatively, a laminated structure may be directly manufactured on a light-emitting element substrate. For example, a thermosetting resin composition for the second thermosetting resin layer is applied to a light-emitting element substrate and dried to form a second thermosetting resin layer. Then, a thermosetting resin composition for the first thermosetting resin layer is applied to the second thermosetting resin layer and dried. This allows a laminated structure having the first thermosetting resin layer and the second thermosetting resin layer of the present invention to be directly manufactured on a light-emitting element substrate. Also, two kinds of dry films may be used to manufacture a laminated structure on a light emitting element substrate. That is, a dry film having a first thermosetting resin layer formed on a film and a dry film having a second thermosetting resin layer formed on a film are each prepared in advance. After this, a dry film having a second thermosetting resin layer is laminated so that the second thermosetting resin layer covers the light emitting element substrate. After peeling off the film on the second thermosetting resin layer, a dry film having a first thermosetting resin layer is laminated on the surface of the second thermosetting resin layer. In this way, a laminated structure having the first thermosetting resin layer and the second thermosetting resin layer of the present invention can be manufactured on a light emitting element substrate using two kinds of dry films.
[0076] [Cured product] The cured product of the present invention is obtained by curing the first thermosetting resin layer and the second thermosetting resin layer constituting the laminated structure. The curing conditions may be, for example, heating at a temperature of 120 to 200°C for 30 to 90 minutes, preferably heating at 150°C for 60 minutes. As the heating method, a known and commonly used method may be used, for example, a hot air circulation drying furnace, an oven, or a hot plate press. The cured product of the present invention may be suitably used as a coating layer for coating the light emitting element of the light emitting element substrate.
[0077] [Light emitting element substrate for image display device] The light emitting element substrate for an image display device of the present invention is characterized in that the light emitting element is covered with a covering layer containing the cured product of the laminated structure of the present invention. The covering layer may further contain a cured product of a curable resin composition other than the cured product of the laminated structure of the present invention within the range in which the effects of the present invention are exhibited.
[0078] A preferred light-emitting element substrate for an image display device of the present invention is a light-emitting element substrate in which a light-emitting element is covered with a covering layer including a first cured resin layer and a second cured resin layer, characterized in that the second cured resin layer and the first cured resin layer are laminated in this order from the light-emitting element side, the first cured resin layer has a haze of 12% or more at a light wavelength of 450 to 750 nm, and the second cured resin layer contains an inorganic filler. The first resin cured product layer and the second resin cured product layer are preferably the cured products of the first thermosetting resin layer and the second thermosetting resin layer of the laminated structure of the present invention, respectively. The total thickness of the first resin cured product layer and the second resin cured product layer may be thicker than the height of the light emitting element, for example, 50 to 500 μm, preferably 100 to 400 μm. The total thickness of the first resin cured product layer and the second resin cured product layer may be appropriately set according to the height of the light emitting element. The haze of the first cured resin layer at a light wavelength of 450 to 750 nm is 12% or more, preferably 13% or more, more preferably 14% or more. On the other hand, the haze is preferably 50% or less, more preferably 40% or less. The total light transmittance of the first cured resin layer at a light wavelength of 450 to 750 nm is preferably 30 to 80%. The thickness of the first thermosetting resin layer is not particularly limited, but is preferably 5 to 150 μm, and more preferably 5 to 100 μm. The haze of the second cured resin layer at a light wavelength of 450 to 750 nm is preferably 80% or more, and more preferably 82% or more. The thickness of the second thermosetting resin layer is not particularly limited, but is preferably 45 to 350 μm, and more preferably 95 to 300 μm. A preferred light emitting element substrate of the present invention can be easily manufactured using a laminated structure having the first thermosetting resin layer and the second thermosetting resin layer of the present invention. That is, when the laminated structure of the present invention has a first film, a first thermosetting resin layer, a second thermosetting resin layer, and a second film in this order, the second film is peeled off from the surface of the second thermosetting resin layer, and the second thermosetting resin layer is laminated on the light emitting element substrate so that the second thermosetting resin layer covers the light emitting element, and then cured. This forms a coating layer including the first resin cured material layer and the second resin cured material layer. Then, the first film is peeled off. In this way, a light emitting element substrate in which the light emitting element is covered with a coating layer including the first resin cured material layer and the second resin cured material layer can be manufactured. Note that a preferred light emitting element substrate of the present invention may be manufactured by another manufacturing method. That is, a thermosetting resin composition is applied to the light emitting element substrate and dried to form a second thermosetting resin layer so as to cover the light emitting element. After that, a thermosetting resin composition is applied and dried on the second thermosetting resin layer to form a first thermosetting resin layer. Then, the first thermosetting resin layer and the second thermosetting resin layer are cured simultaneously to form a coating layer. This makes it possible to manufacture a light emitting element substrate in which the light emitting element is covered with a coating layer including a first resin cured material layer and a second resin cured material layer. In addition, a light emitting element substrate in which the light emitting element is covered with a coating layer may be manufactured using two types of dry films. That is, a dry film having a first thermosetting resin layer formed on a film and a dry film having a second thermosetting resin layer formed on a film are each previously prepared. After that, a dry film having a second thermosetting resin layer is laminated so that the second thermosetting resin layer covers the light emitting element. After peeling off the film on this second thermosetting resin layer, a dry film having a first thermosetting resin layer is laminated on the surface of the second thermosetting resin layer. Then, the first thermosetting resin layer and the second thermosetting resin layer are cured simultaneously to form a coating layer including the first cured resin layer and the second cured resin layer. Next, the film on the coating layer is peeled off. In this way, a light emitting element substrate can be manufactured in which the light emitting element is coated with a coating layer including the first cured resin layer and the second cured resin layer using two types of dry films.
[0079] Fig. 2 is a schematic cross-sectional view showing an embodiment of the light-emitting element substrate for an image display device of the present invention. The light-emitting element substrate 3 of Fig. 2 is a substrate 40 on which red, green and blue light-emitting elements 30, 31 and 32 are coated with a coating layer including a first resin cured layer 11 formed by curing the first thermosetting resin layer of the laminated structure of the present invention and a second resin cured layer 21 formed by curing the second thermosetting resin layer. In Fig. 2, the second resin cured layer 21 is thicker than the first resin cured layer 11. The second resin cured layer 21 is also thicker than the red, green and blue light-emitting elements 30, 31 and 32, and covers the surfaces of the light-emitting elements 30, 31 and 32. EXAMPLES
[0080] The present invention will be specifically described below with reference to examples, comparative examples, and test examples of the present invention, but it goes without saying that the present invention is not limited to the following examples. Note that all parts are by weight unless otherwise specified.
[0081] (Formulation examples 1-18) The components were mixed according to the formulations shown in Tables 1 and 2 below, and dispersed using a three-roll mill to obtain thermosetting resin compositions of Mixture Examples 1-18.
[0082] <Method of Producing the Laminated Structure of Example 1> The thermosetting resin composition of Formulation Example 3 was applied to a film (PET film; Toyobo Co., Ltd. TN-200, thickness 38 μm, size 30 cm × 30 cm) (hereinafter referred to as film A) using a bar coater so that the thickness of the first thermosetting resin layer after drying would be 50 μm. Next, the film was dried in a hot air circulation drying oven at 70 to 120 ° C (average 100 ° C) for 5 to 10 minutes so that the organic solvent remaining in the first thermosetting resin layer was 0.5 to 2.5 mass %, to produce a dry film having a first thermosetting resin layer on film A. Next, a film (biaxially oriented polypropylene film, OPP, Alphan FG-201, Fish Eyeless, manufactured by Oji F-Tex Co., Ltd.) (hereinafter referred to as Film B) was laminated to the surface of the prepared dry film using a roll laminator set to a temperature of 80°C to prepare a dry film with a three-layer structure of Film A / first thermosetting resin layer (thickness: 50 μm) / Film B. The thermosetting resin composition of Formulation Example 13 was applied to a film (PET film; Toyobo Co., Ltd. TN-200, thickness 38 μm, size 30 cm × 30 cm) (hereinafter referred to as film C) using a bar coater so that the thickness of the second thermosetting resin layer after drying was 150 μm. Next, it was dried in a hot air circulation drying oven at 70 to 120 ° C (average 100 ° C) for 5 to 10 minutes so that the organic solvent remaining in the second thermosetting resin layer was 0.5 to 2.5 mass %, and a dry film having a second thermosetting resin layer on film C was produced. Next, a film (biaxially oriented polypropylene film, OPP, Alphan FG-201, Fish Eyeless, manufactured by Oji F-Tex Co., Ltd.) (hereinafter referred to as Film D) was laminated to the surface of the prepared dry film using a roll laminator set to a temperature of 80°C to prepare a dry film with a three-layer structure of Film C / second thermosetting resin layer (thickness: 150 μm) / Film D. Film B of the dry film obtained using Formulation Example 3 and Film D of the dry film obtained using Formulation Example 13 were peeled off, and the first thermosetting resin layer and the second thermosetting resin layer were laminated together at 50°C using a roll laminator. This resulted in a four-layer laminate structure of film A / first thermosetting resin layer (resin layer not in contact with the light-emitting element) / second thermosetting resin layer (resin layer in contact with the light-emitting element) / film C.
[0083] <Methods for producing stacked structures and light-emitting element substrates of Examples 2 to 10 and Comparative Examples 1 to 6> A laminate structure was produced in the same manner as in Example 1, except that the formulations of the thermosetting resin compositions and the thicknesses of the thermosetting resin layers shown in Tables 3 and 4 were used.
[0084] <Preparation of substrate for evaluation of haze and total light transmittance> The thermosetting resin composition of Blending Example 3 was applied to a film (PET film; Toyobo Co., Ltd. TN-200, thickness 38 μm, size 30 cm × 30 cm) (hereinafter referred to as film A) using a bar coater so that the thickness of the thermosetting resin layer after drying was 50 μm. Next, it was dried for 5 to 10 minutes at 70 to 120 ° C (average 100 ° C) in a hot air circulation drying oven so that the solvent remaining in the thermosetting resin layer was 0.5 to 2.5 mass %, forming a thermosetting resin layer on the film A. Next, a film (biaxially oriented polypropylene film, OPP, Alphan FG-201, Fish Eyeless, Oji F-Tex Co., Ltd.) (hereinafter referred to as film B) was laminated to the surface of the thermosetting resin layer using a roll laminator set to a temperature of 80 ° C, and an evaluation laminate structure consisting of film A / thermosetting resin layer (thickness: 50 μm) / film B was prepared. Film B (OPP) of the prepared laminated structure for evaluation was peeled off, and the laminate was laminated on a slide glass having a thickness of 1 mm using a vacuum laminator MVLP-500 (manufactured by Meiki Seisakusho Co., Ltd.). The conditions were a lamination temperature of 50 to 80°C and a pressure of 0.3 MPa. Next, the laminate was heated in a hot air circulation drying oven at 100°C for 30 minutes, and then further heated at 150°C for 60 minutes to cure the thermosetting resin layer and obtain a cured product. Then, film A was peeled off from the surface of the cured product to obtain a substrate for evaluation having a cured product on the slide glass. The reason for heating at 100°C for 30 minutes is that if there is a large amount of organic solvent remaining in the thermosetting resin layer, foaming may occur when heating at 150°C for 60 minutes to cure, and the condition of heating at 100°C for 30 minutes is not a necessary condition. Laminated structures for evaluation were prepared from the thermosetting resin compositions of Formulation Examples 1 to 18 in the same manner as above, except that the formulation examples of the thermosetting resin compositions and the thicknesses of the thermosetting resin layers were set as shown in Tables 3 and 4. Furthermore, evaluation substrates having a cured product on a slide glass were obtained in the same manner as above using the laminated structures for evaluation.
[0085] <Method of measuring haze and total light transmittance> The total light transmittance and haze of the cured product formed on the evaluation substrate were measured at light wavelengths of 450 to 750 nm using a Hazemeter NDH7000II (manufactured by Nippon Denshoku Industries Co., Ltd.) The obtained values of haze and total light transmittance are shown in Tables 3 and 4.
[0086] <Method of manufacturing light-emitting element substrate> Red light-emitting elements, green light-emitting elements, and blue light-emitting elements were prepared, each having a length of 200 μm, a width of 100 μm, a height of 75 μm, and a bump height of 30 μm. Next, the red light-emitting elements, green light-emitting elements, and blue light-emitting elements were arranged in this order horizontally at a pitch of 150 μm on a FR-4 substrate that had been previously wired, to prepare a set of light-emitting element substrates. Next, the elements were combined in a grid of 10 sets vertically and 10 sets horizontally at a pitch of 1 mm to prepare a substrate on which light-emitting elements were mounted as an evaluation substrate, i.e., a light-emitting element substrate.
[0087] <Method for producing a light-emitting element substrate covered with a covering layer made of the laminated structure of Example 1> The film C of the laminated structure of Example 1 was peeled off, and the second thermosetting resin layer side was attached to the light emitting element substrate using a vacuum laminator MVLP-500 (manufactured by Meiki Seisakusho). As a result, a laminated structure having the second thermosetting resin layer and the first thermosetting resin layer in this order was obtained on the light emitting element substrate. The conditions of the vacuum laminator were a lamination temperature of 50 to 80°C and a pressure of 0.3 MPa. Next, the laminated structure was heated at 100°C for 30 minutes in a hot air circulation drying oven, and further heated at 150°C for 60 minutes to harden the first thermosetting resin layer and the second thermosetting resin layer. After that, the film A was peeled off, and a light emitting element substrate in which the light emitting element was covered with a covering layer including the second resin cured material layer and the first resin cured material layer was produced. The reason for heating at 100°C for 30 minutes is that if a large amount of organic solvent remains in the second thermosetting resin layer and the first thermosetting resin layer, there is a risk of foaming when the resin is cured by heating at 150°C for 60 minutes. Heating at 100°C for 30 minutes is not a necessary condition.
[0088] <Methods for Producing Light-Emitting Element Substrates Covered with Covering Layers Made of Laminated Structures of Examples 2 to 10 and Comparative Examples 1 to 6> Light-emitting element substrates were produced in the same manner as in Example 1, except that the laminated structures of Examples 2 to 10 and Comparative Examples 1 to 6 were used.
[0089] <Difference in color when viewed from the front and at a 45° angle when illuminated> All the light emitting elements on the light emitting element substrate covered with the coating layer were turned on, and the difference in the emission color was visually observed from the front of the substrate and from a 45° oblique direction. ◎: 10 out of 10 people answered that there was no difference. ○: 5 to 9 out of 10 people answered that there was no difference. ×: Fewer than 4 out of 10 people answered that there was no difference.
[0090] <Blackness when the light is off> Using the light-emitting element substrate used in the evaluation of the color difference described above, the blackness when turned off was observed from the front of the substrate. ◎: 10 out of 10 people answered that it was black. ○: 5 to 9 out of 10 people answered that it was black. ×: Fewer than 4 in 10 people answered that it was black.
[0091] <Concealment of light-emitting element when turned off> Using the light emitting element substrate used in the evaluation of the color difference described above, the difficulty in seeing the light emitting element when it was turned off was observed from the front of the substrate. ◎: 10 out of 10 people answered that it was difficult to see. ○: 5 to 9 out of 10 people answered that it was difficult to see. ×: Fewer than 4 in 10 people answered that it was difficult to see.
[0092] [Table 1]
[0093] *1: Hydrogenated bisphenol A epoxy resin, epoxy resin with an alicyclic skeleton (manufactured by Mitsubishi Chemical Corporation) *2: Hydrogenated bisphenol A epoxy resin, epoxy resin with alicyclic structure (manufactured by Nippon Steel Chemical & Material Co., Ltd.) *3: Phenol novolac epoxy resin (DIC) *4: Phenoxy resin (manufactured by Mitsubishi Chemical Corporation) (mixed solvent of cyclohexanone and methyl ethyl ketone, solid content 30% by mass) *5: Dicyandiamide (Mitsubishi Chemical) *6: 2-Ethyl-4-methylimidazole (manufactured by Shikoku Chemical Industry Co., Ltd.) *7: Carbon black, black colorant (manufactured by Mitsubishi Chemical Corporation) *8: Titanium black, black colorant (manufactured by Ako Kasei Co., Ltd.) *9: Silica (manufactured by Admatechs) (average particle size: 0.5 μm)
[0094] [Table 2]
[0095] [Table 3]
[0096] [Table 4]
[0097] From the results shown in Tables 3 and 4, it can be seen that the laminated structures of Examples 1 to 10 can form a coating layer that improves the color change when the light-emitting element is emitting light when viewed from the front and from a 45° diagonal direction, and improves the concealment of the light-emitting element when it is turned off. Furthermore, from the results shown in Tables 3 and 4, it can be seen that the laminated structures of Examples 1 to 10 can form a coating layer that is excellent in blackness when the light-emitting element is turned off. In contrast, the laminated structures of Comparative Examples 1 to 6 could not improve the color change when the light-emitting element is emitting light when viewed from the front and from a 45° diagonal direction. Furthermore, the laminated structures of Comparative Examples 1 to 3 could not improve the blackness when it is turned off. Furthermore, the laminated structures of Comparative Examples 1 and 6 could not improve the concealment of the light-emitting element when it is turned off. [Explanation of symbols]
[0098] 1. Laminated structure of the present invention 3. Light-emitting device substrate of the present invention 10 First thermosetting resin layer 11: First cured resin layer formed by curing the first thermosetting resin layer 20 Second thermosetting resin layer 21: A second resin cured layer formed by curing the second thermosetting resin layer 30 Red light emitting element 31 Green light emitting element 32 Blue light emitting element 40 Substrate
Claims
1. A laminated structure having a first thermosetting resin layer and a second thermosetting resin layer, the first thermosetting resin layer has a haze of 12% or more at a light wavelength of 450 to 750 nm after heat treatment at 150° C. for 60 minutes; The laminated structure, wherein the second thermosetting resin layer contains an inorganic filler.
2. A laminated structure having a first thermosetting resin layer and a second thermosetting resin layer, the first thermosetting resin layer contains at least one of carbon black and titanium black, an epoxy resin having an alicyclic skeleton, and a thermoplastic resin; In the case where the first thermosetting resin layer contains the carbon black, the content of the carbon black in the first thermosetting resin layer is 0.07 mass% or less based on the total solid content, When the first thermosetting resin layer contains the titanium black, the content of the titanium black in the first thermosetting resin layer is 0.70 mass% or more based on the total solid content, The laminated structure, wherein the second thermosetting resin layer contains an inorganic filler.
3. 3. The laminate structure according to claim 1, which is used to form a coating layer for a light emitting element in a light emitting element substrate for an image display device.
4. 3. The laminate structure according to claim 1, wherein the first thermosetting resin layer has a total light transmittance of 30 to 80% at a light wavelength of 450 to 750 nm after heat treatment at 150° C. for 60 minutes.
5. 3. The laminate structure according to claim 1, wherein the second thermosetting resin layer contains 1 to 20 mass % of an inorganic filler based on the total solid content of the second thermosetting resin layer.
6. 3. The laminated structure according to claim 1, wherein the inorganic filler is silica.
7. 2. The laminate structure according to claim 1, wherein the first thermosetting resin layer contains a black colorant.
8. 3. A laminate structure according to claim 1, wherein at least one surface of the laminate structure is supported or protected by a film.
9. 3. A cured product, which is obtained by curing the first thermosetting resin layer and the second thermosetting resin layer constituting the laminate structure according to claim 1 or 2.
10. A light emitting element substrate for an image display device, comprising a light emitting element covered with a covering layer comprising the cured product according to claim 9.
11. A light emitting element substrate for an image display device, in which a light emitting element is covered with a covering layer including a first cured resin layer and a second cured resin layer, the second cured resin layer and the first cured resin layer are laminated in this order from the light emitting element side, The first cured resin layer has a haze of 12% or more at a light wavelength of 450 to 750 nm, and the second cured resin layer contains an inorganic filler.
Citation Information
Patent Citations
Colorless or lowly colored epoxy resin composition, and molded article and transparent sealing material both made by using the composition
JP1996283385A
Composition for transparent sealing material
JP2011042762A
Sealing material composition, dry film, cured product and sealing structure
JP2021161413A