Manufacturing method of electrode material
By fixing electronically conductive oxides to the surfaces of mesoporous carbon within the electrode material, the method addresses carbon corrosion and agglomeration issues, resulting in improved durability and conductivity for polymer electrolyte fuel cells.
Patent Information
- Application Number
- JP2023057013
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Existing electrode materials for polymer electrolyte fuel cells (PEFC) face issues with carbon corrosion and agglomeration of platinum catalyst particles due to carbon dioxide formation, leading to decreased performance and durability, especially under varying operational conditions.
A method for producing an electrode material that involves fixing electronically conductive oxides, primarily tin oxide, to the inner and outer surfaces of mesoporous carbon using anhydrous alcohol and controlled hydrolysis, followed by heat treatment, to create a porous composite carrier that supports electrode catalyst particles.
The method enhances the durability of the electrode material against carbon corrosion and maintains excellent electronic conductivity, ensuring stable performance even under start-stop cycles and varying load conditions.
Smart Images

Figure 2024144863000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an electrode material suitable for use in a fuel cell electrode. [Background technology]
[0002] Fuel cell vehicles (FCVs) that use polymer electrolyte fuel cells (PEFCs) as their power source are already commercially available, and their use is expected to expand to trucks, buses, ships, and other vehicles in the future. PEFCs generally have a structure in which a membrane electrode assembly (MEA), in which a pair of electrodes are arranged on both sides of a solid polymer electrolyte membrane, is sandwiched between separators with gas flow paths. Fuel cell electrodes (particularly PEFC electrodes) generally consist of an electrode catalyst layer made of an electrode material with electrocatalytic activity and a polymer electrolyte, and a gas diffusion layer that combines gas permeability and electronic conductivity.
[0003] Currently, the most widely used electrode material for PEFCs is one in which electrode catalyst particles (typically Pt or Pt alloy particles) are dispersed and supported on a carbon-based support.
[0004] On the other hand, since the electrolyte membrane of a PEFC is acidic (pH = 0 to 3), the electrode material of the PEFC is used in an acidic atmosphere. Also, the cell voltage during normal operation is 0.4 to 1.0 V, but it is known that the cell voltage rises to 1.5 V during start-up and shutdown. The state of the cathode and anode under such PEFC operating conditions is as follows: In the cathode, the carbon-based material, which acts as a carrier, is converted into carbon dioxide (CO 2 ) at the cathode. Therefore, at the cathode, the carbon support is electrochemically oxidized to CO 2This causes a reaction that breaks down the carbon into carbon and results in corrosion of the carbon support (carbon corrosion), which causes the Pt particles, which are the catalytically active component, to aggregate and fall off, resulting in a decrease in fuel cell performance. Also, when there is a shortage of fuel gas not only in the cathode but also in the anode, such as at the beginning of operation, a voltage drop or concentration polarization occurs in that area, resulting in a localized potential that is opposite to normal, which can cause an electrochemical oxidative decomposition reaction of carbon.
[0005] To address the above-mentioned problem of corrosion of the carbon support, we developed an electronically conductive oxide (SnO 2 , TiO 2 Electrode materials using metal oxides have been reported (Patent Documents 1 and 2). Such electrode materials have excellent durability due to the metal oxide.
[0006] Furthermore, in recent years, electrode materials that use mesoporous carbon as the skeleton of a catalyst support and support Pt fine particles in the pores (mesopores) of the mesoporous carbon have attracted attention (e.g., Patent Documents 3 and 4). Mesoporous carbon has excellent electrical conductivity, good gas diffusion properties, and a large surface area, so that when it is used as a support for an electrode catalyst in a polymer electrolyte fuel cell, an electrode with excellent power generation performance can be obtained.
[0007] The methods for supporting (fixing) electronic conductive oxides described in Patent Documents 1 and 2 involve dropping ammonia water or pure water onto a precursor dissolved in an organic solvent to obtain an electronic conductive oxide, but these methods have a fast reaction rate that is difficult to control, resulting in large primary particle sizes of the generated electronic conductive oxides (10 nm or more), and the primary particles end up being supported (fixed) in an aggregated state on the carbon support. For this reason, even if one were to apply these methods for supporting (fixing) electronic conductive oxides to mesoporous carbon, it was thought to be extremely difficult to uniformly support (fix) electronic conductive oxides within the mesopores of mesoporous carbon.
[0008] Meanwhile, in Patent Document 5, the present inventors have reported a method for producing an electrode material for a fuel cell, which includes the steps of mixing mesoporous carbon and an alkoxide compound of an electronically conductive oxide precursor in a non-aqueous organic solvent until the mixture is homogeneous, then distilling off the solvent and drying the mixture to obtain a dried product, which is then hydrolyzed with water vapor to decompose the electronically conductive oxide precursor, and then heat-treated to adhere the electronically conductive oxide to the surface of the mesoporous carbon. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Patent No. 5322110 [Patent Document 2] Patent No. 6598159 [Patent Document 3] Patent No. 6969996 [Patent Document 4] Patent No. 6931808 [Patent Document 5] Patent application No. 2022-141541 Summary of the Invention [Problem to be solved by the invention]
[0010] The method disclosed in Patent Document 5 in which an electronically conductive oxide precursor is introduced into the pores of mesoporous carbon and then water vapor is introduced to perform hydrolysis can reliably form an electronically conductive oxide inside the pores of mesoporous carbon, but there is room for improvement in terms of productivity.
[0011] Under these circumstances, an object of the present invention is to provide a method for producing an electrode material that can adhere an electronically conductive oxide to the outer and inner pore surfaces of mesoporous carbon without hydrolysis using water vapor, and that has both excellent durability against carbon corrosion and the excellent electronic conductivity inherent to mesoporous carbon. [Means for solving the problem]
[0012] As a result of intensive research aimed at solving the above problems, the present inventors discovered that the following invention meets the above object, and thus completed the present invention.
[0013] That is, the present invention relates to the following inventions. <1> A method for producing an electrode material comprising: a porous composite support made of mesoporous carbon and an electronically conductive oxide mainly composed of tin oxide adhered to the inner and outer pore surfaces of the mesoporous carbon; and electrode catalyst particles supported on the porous composite support, the method comprising the following steps (1) to (4): Step (1): A step of contacting mesoporous carbon with anhydrous alcohol to obtain a dispersion containing mesoporous carbon having anhydrous alcohol introduced into the pores. Step (2): A step of mixing the dispersion containing the mesoporous carbon into which the anhydrous alcohol has been introduced obtained in step (1), a tin alkoxide solution containing a tin alkoxide of the electronically conductive oxide, and a water / alcohol solvent to obtain a mixed solution, and then distilling off the solvent from the mixed solution to obtain a dried product in which a hydrolyzate of the tin alkoxide is fixed to the inner and outer pore surfaces of the mesoporous carbon. Step (3): A step of heat-treating the dried product obtained in step (2) to obtain a porous composite carrier in which an electronically conductive oxide is adhered to the inner and outer pore surfaces of the mesoporous carbon. Step (4): A step of mixing the porous composite support obtained in step (3) and the solution containing the electrode catalyst precursor until homogeneous, and then evaporating the solvent to obtain a dried product, and heat-treating the dried product in an inert gas atmosphere. <2> In step (1), the absolute alcohol is one or more selected from the group consisting of methanol, ethanol, n-propanol, and isopropanol. <1> A method for producing the electrode material according to claim 1. <3> In step (2), a dried product is obtained in which a hydrolyzate of tin alkoxide is fixed to the inner and outer pore surfaces of the mesoporous carbon, and then the dried product is dispersed in a niobium alkoxide solution, and the solvent is then distilled off to obtain a dried product. <1> or <2> A method for producing the electrode material according to claim 1. <4> In step (2), the proportion of water in the mixed solution is 0.1% by volume or more and 10% by volume or less in a total of 100% by volume of water and alcohol (including the absolute alcohol content in the dispersion liquid). <1> from <3> 13. A method for producing the electrode material according to any one of claims 1 to 12. <5> In step (3), the heat treatment temperature is 350° C. or more and 650° C. or less. <1> from <4> 13. A method for producing the electrode material according to any one of claims 1 to 12. <6> In step (4), the electrode catalyst precursor is a noble metal acetylacetonate. <1> from <5> 13. A method for producing the electrode material according to any one of claims 1 to 12. Effect of the Invention
[0014] According to the present invention, there is provided a method for producing an electrode material having both excellent durability against carbon corrosion and excellent electronic conductivity due to mesoporous carbon. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1(a) is a conceptual schematic diagram of an electrode material according to the present invention, FIG. 1(b) is an enlarged schematic diagram of the vicinity of pores (electronically conductive oxide is dispersed and fixed), and FIG. 1(c) is an enlarged schematic diagram of the vicinity of pores (electronically conductive oxide is continuously fixed (coated)). [Diagram 2] 1 is a flowchart showing a procedure for producing an electrode material (without supporting an electrode catalyst) in an experimental example. [Diagram 3] 1 shows an XRD profile of an electrode material (without supporting an electrode catalyst) of an experimental example. [Figure 4] 1 shows the microstructural observation results of the electrode material of Experimental Example A3 (electrode catalyst not supported, 600° C.), where (a) is an SEM image and (b) is a TEM image. [Diagram 5] 1 shows the microstructure observation results (SEM image) of the electrode material of Experimental Example A4 (electrode catalyst not supported, 700° C.). [Figure 6] This is a selected-area electron diffraction pattern of the electrode material of the experimental example (electrode catalyst not supported, 400°C, 500°C, 600°C). [Figure 7]1 shows STEM / EDS mapping images of the electrode materials (electrode catalyst unsupported, SnO2 adhesion rate 20 to 75 wt%) of Experimental Examples A3, and A5 to A7. [Figure 8] FIG. 1 shows STEM images (right figures (a) to (c)) of the electrode material of Experimental Example A6 (electrode catalyst not supported, SnO2 adhesion rate 40 wt%) and a schematic diagram (left figure) of the arrangement of tin oxide particles inside mesopores. [Figure 9] 1 is a flow chart showing a procedure for supporting an electrode catalyst by an acetylacetonate method. [Figure 10] This is STEM / EDS of the electrode material (Pt / Sn0.98Nb0.02O2 / MC) of Experimental Example A3. [Figure 11] FIG. 13 is a diagram showing conditions of a start-stop cycle test. [Figure 12] FIG. 1 is a diagram showing changes in electrochemically effective surface area (ECSA) of the electrode material of the embodiment (SnO2 adhesion rate: 20 to 75 wt%) and the electrode material of the comparative example (SnO2 adhesion rate: 0 wt%) in a start-stop cycle test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the following examples, and can be modified as desired without departing from the gist of the present invention. In this specification, the word "to" is used as an expression including the numerical values or physical quantities before and after it.
[0017] The present invention relates to a method for producing an electrode material including a porous composite support made of mesoporous carbon and an electronically conductive oxide mainly composed of tin oxide adhered to the inner and outer pore surfaces of the mesoporous carbon, and electrode catalyst particles supported on the porous composite support, the method comprising the following steps (1) to (4) (hereinafter referred to as the "method for producing the electrode material of the present invention" or simply the "method for producing the electrode material of the present invention").
[0018] Step (1): A step of contacting mesoporous carbon with anhydrous alcohol to obtain a dispersion containing mesoporous carbon having anhydrous alcohol introduced into the pores. Step (2): A step of mixing the dispersion containing the mesoporous carbon into which the anhydrous alcohol has been introduced obtained in step (1), a tin alkoxide solution containing a tin alkoxide of the electronically conductive oxide, and a water / alcohol solvent to obtain a mixed solution, and then distilling off the solvent from the mixed solution to obtain a dried product in which a hydrolyzate of the tin alkoxide is fixed to the inner and outer pore surfaces of the mesoporous carbon. Step (3): A step of heat-treating the dried product obtained in step (2) to obtain a porous composite carrier in which an electronically conductive oxide is adhered to the inner and outer pore surfaces of the mesoporous carbon. Step (4): A step of mixing the porous composite support obtained in step (3) and the solution containing the electrode catalyst precursor until homogeneous, and then evaporating the solvent to obtain a dried product, and heat-treating the dried product in an inert gas atmosphere.
[0019] In the electrode material produced by the production method of the present invention (hereinafter, sometimes referred to as "the electrode material of the present invention"), an electronically conductive oxide mainly composed of tin oxide is fixed to all or part of the inner and outer surfaces of the pores in the mesoporous carbon, and the electrode catalyst particles have a structure supported by the electronically conductive oxide. In other words, the electrode catalyst particles are supported by the mesoporous carbon via the electronically conductive oxide.
[0020] In the following description, the tin alkoxide (and other alkoxides containing an element that serves as a dopant) that serves as the raw material for the electronically conductive oxide mainly composed of tin oxide may be referred to as the "raw material alkoxide".
[0021] In addition, in this specification, "fixed" means that the alkoxide hydrolysate (electronically conductive oxide precursor) or the electronically conductive oxide is fixed to the inner and outer pore surfaces of the mesoporous carbon, which is the support skeleton, to an extent that it does not easily detach (peel off).
[0022] Although the details will be described later, one of the features of the method for producing an electrode material of the present invention is that an absolute alcohol is introduced into the pores of the mesoporous carbon in step (1). Mesoporous carbon is a porous carbon having pores in the mesopore region (2 to 50 nm). When fixing a hydrolysate of a raw material alkoxide (electronically conductive oxide precursor) to the surface of mesoporous carbon, it is difficult to introduce the raw material alkoxide, which is a precursor compound of an electronically conductive oxide, and water for hydrolysis of the raw material alkoxide into the pores of untreated mesoporous carbon. As a result, with untreated mesoporous carbon, a problem arises in that most of the hydrolysate of the raw material alkoxide is fixed to the outer surface of the pores. In response to this problem, in the manufacturing method of the present invention, an anhydrous alcohol, which is an amphipathic solvent, is introduced into the pores of the mesoporous carbon, so that in step (2), the raw alkoxide and the water / alcohol solvent are easily introduced into the pores of the mesoporous carbon. When the solvent is distilled off in this state, the alcohol component is preferentially distilled off, resulting in a relatively high concentration of water, which advances the hydrolysis reaction of the raw alkoxide, and the hydrolysate of the raw alkoxide (electron-conductive oxide precursor) can be fixed not only to the outer surface of the pores of the mesoporous carbon but also to the inner surface of the pores. Therefore, by heat-treating the dried product obtained in step (2), a porous composite support in which an electron-conductive oxide is fixed to the inner and outer surfaces of the pores of the mesoporous carbon can be obtained (step (3)). The obtained porous composite support and a solution containing an electrode catalyst precursor are mixed until homogeneous, and then the solvent is distilled off to obtain a dried product, which is then heat-treated in an inert gas atmosphere, to obtain the desired electrode material in which electrode catalyst particles are supported on the porous composite support (step (4)).
[0023] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the drawings.
[0024] FIG. 1(a) is a schematic diagram showing a typical structure of an electrode material of the present invention, and FIG. 1(b) is an enlarged schematic diagram of the vicinity of a pore.
[0025] As shown in FIG. 1(a), an electrode material 1 according to the present invention is composed of a porous composite support made of mesoporous carbon 2, which is a support skeleton, and particulate electronically conductive oxide 3a fixed to the mesoporous carbon 2 (pore inner surfaces 2a and outer surfaces 2b), and electrode catalyst particles 3b supported on the electronically conductive oxide 3a.
[0026] The mesoporous carbon 2 which is the support skeleton of the electrode material 1 (hereinafter, may be referred to as "mesoporous carbon according to the present invention") is a porous carbon having a large number of pores in the mesopore region.
[0027] In this specification, the term "pore" includes, for example, pores having a diameter of 150 nm or less (particularly, pores having a diameter of 100 nm or less). "Mesopore region pores" refers to pores having a diameter of 2 nm to 50 nm. In addition, in this specification, "micropore region pores" refers to pores having a diameter of less than 2 nm, and "macropore region pores" refers to pores having a diameter of more than 50 nm and not more than 150 nm.
[0028] Porous carbon having pores in the mesopore region (2 to 50 nm) can be used as the mesoporous carbon 2, and preferably has a pore diameter of 3 nm to 40 nm. If the pore diameter is within this range, even if an electronic conductive oxide or an electrode catalyst is fixed (supported) on the inner wall of the pore, the diffusion of the substance into the pore is not significantly hindered and proceeds smoothly.
[0029] Furthermore, when the electrode material of the present invention is used to prepare an electrode for a fuel cell, the electrode material of the present invention is mixed with a proton-conductive electrolyte material (ionomer). Since the proton-conductive electrolyte material (ionomer) has a size of several tens of nanometers, it cannot penetrate into mesopores having a small pore diameter. This makes it possible to suppress poisoning of the electrode catalyst metal supported in the pores of the mesoporous carbon via the electronically conductive oxide, which is caused by the ionomer.
[0030] The mesoporous carbon according to the present invention may contain regions (micropore region, macropores) other than the mesopore region (2 nm to 50 nm) pores, but it is preferable that the proportion of pores in the mesopore region is high.
[0031] The pore structure (pore diameter, shape, etc.) of mesoporous carbon can be confirmed by observation with an electron microscope, such as a field emission scanning electron microscope (FESEM) or a scanning transmission electron microscope (STEM).
[0032] The pores in the mesopore region of the mesoporous carbon 2 preferably have a three-dimensional network structure, including not only individual pores independent of other pores, but also interconnected pores in which some or all of the pores in the mesopore region are interconnected with the pores in adjacent mesopore regions. The presence of interconnected pores promotes the diffusion of substances inside the pores of the mesoporous carbon.
[0033] The size and shape of the electrode material depend on the size and shape of the mesoporous carbon that is its framework material. The size and shape of the mesoporous carbon are determined so that the electrode material can be in continuous contact when the fuel cell electrode is formed, and a space can be formed that allows smooth diffusion of gases such as hydrogen and oxygen and smooth discharge of water (steam) within the fuel cell electrode.
[0034] The mesoporous carbon used in the electrode material of the present invention may be appropriately synthesized or may be a commercially available product, such as the CNovel series (designed mesopore diameter: 5 to 150 nm) manufactured by Toyo Tanso Co., Ltd., which is a mesoporous carbon using MgO as a template.
[0035] (Electron-conducting oxide) 1, in the electrode material 1 of this embodiment, the electronic conductive oxide 3a is fixed to the inner surfaces 2a of the pores in the mesopore region of the mesoporous carbon 2. In the electrode material 1 of this embodiment, the electronic conductive oxide 3a is also fixed to the outer surface of the mesoporous carbon 2.
[0036] The amount of the electronically conductive oxide adhered varies depending on the physical properties of the electronically conductive oxide, such as particle size (film thickness in the case of a thin film) and surface area, and the manufacturing method of the electronically conductive oxide, and is therefore appropriately determined within a range in which a sufficient amount of electrode catalyst particles can be supported. For example, the amount is 10% by weight or more and 80% by weight or less, when the total of the electronically conductive oxide and the mesoporous carbon is 100% by weight.
[0037] The size of the electronically conductive oxide in the pores is determined within a range that does not block the pores of the mesoporous carbon 2 and does not inhibit the transfer of substances such as gas. Although it depends on the pore size of the mesoporous carbon 2, the size of the electronically conductive oxide adhered to the inner surfaces of the pores is preferably a particle size of 0.5 nm or more and 3 nm or less.
[0038] The electronically conductive oxide 3a on the outer surface does not substantially contribute to blocking of the mesopores and may be larger than the electronically conductive oxide in the pores, but in order to reduce electrical resistance, it is preferable that the particle size is small within a range in which the electrode catalyst particles 3b can be dispersed and supported. When an electronically conductive oxide is present on the outer surface, its size is preferably 0.5 nm or more and 10 nm or less.
[0039] The "average particle size of the particulate electronically conductive oxide" can be obtained by averaging the particle sizes of any (20) particulate electronically conductive oxide particles examined from an electron microscope image.
[0040] 1(a) and 1(b), the electronic conductive oxide 3a is a particulate electronic conductive oxide dispersed and fixed to the mesoporous carbon 2, but is not limited thereto, and it is sufficient that the electronic conductive oxide 3a is fixed to the mesoporous carbon 2. For example, as shown in FIG. 1(c), the electronic conductive oxide 3a may be fixed so as to continuously cover the surface (particularly the inner surface of the pores) of the mesoporous carbon 2 without being dispersed. That is, in the electrode material of the present invention, the form of the fixed electronic conductive oxide may be any form such as particulate, island, thin film, etc., as long as it does not impair the object of the present invention.
[0041] The electronically conductive oxide constituting the electronically conductive oxide 3a is an electronically conductive oxide mainly composed of tin oxide. In the present invention, the term "electronically conductive oxide mainly composed of tin oxide" means (A) an oxide composed only of a base oxide, and (B) an oxide doped with another element, which contains 80 mol % or more of the base oxide. Since electronically conductive oxides mainly composed of tin oxide have both sufficient durability and electronic conductivity under the cathode conditions of fuel cells (particularly solid polymer fuel cells), the electrode material of the present invention is preferably used as a cathode for fuel cells.
[0042] As an element, tin (Sn) forms the oxide SnO under PEFC cathode conditions. 2 is thermodynamically stable and does not undergo oxidative decomposition. In addition, tin oxide has sufficient electronic conductivity and serves as a support capable of supporting electrode catalyst particles (particularly precious metal particles) in a highly dispersed state. The cathode conditions of a PEFC refer to the conditions at the cathode during normal operation of the PEFC, and refer to conditions where the temperature is from room temperature to about 150° C. and a gas containing oxygen, such as air, is supplied (oxidizing atmosphere).
[0043] Among oxides mainly composed of tin oxide, niobium-doped tin oxide doped with 0.1 to 20 mol % of niobium (Nb) is particularly preferred, since it allows the formation of a fuel cell electrode having superior electrode performance.
[0044] When the fuel cell electrode of the present invention is used as an anode, an oxide mainly composed of tin oxide is not preferred because it is reduced to metallic Sn under the anode conditions of the PEFC.
[0045] (electrode catalyst particles) The electrode catalyst particles 3b are selectively dispersed and supported on the electronically conductive oxide 3a. Here, "selectively dispersed and supported on the electronically conductive oxide" means that 80% or more, preferably 90% or more, and more preferably 95% or more (including 100%) of all the electrode catalyst particles (number) are supported on the electronically conductive oxide. The proportion of the electrode catalyst particles supported on the electronically conductive oxide can be evaluated by selecting any electrode catalyst particles (100 or more) observed under an electron microscope from the electrode material to be evaluated, and counting the number of those supported on the electronically conductive oxide and the number of those supported on the mesoporous carbon.
[0046] The electrode catalyst particles 3b may be either a precious metal catalyst or a non-precious metal catalyst as long as it has electrochemical catalytic activity for the reduction of oxygen (and the oxidation of hydrogen), but is preferably selected from precious metals such as Pt, Ru, Ir, Pd, Rh, Os, Au, Ag, and alloys containing these precious metals. The term "alloy containing a precious metal" includes "alloys consisting of only the above-mentioned precious metals" and "alloys consisting of the above-mentioned precious metals and other metals and containing 10 mass % or more of the above-mentioned precious metals". The "other metals" to be alloyed with the precious metal are not particularly limited, but suitable examples include Co, Ni, W, Ta, Nb, and Sn, and one or more of these may be used. Two or more of the above-mentioned precious metals and alloys containing the precious metals in a phase-separated state may also be used. In this specification, the above-mentioned precious metals and alloys containing these precious metals may be referred to as "electrode catalyst metals" hereinafter.
[0047] Among the electrode catalyst metals, Pt and alloys containing Pt are particularly suitable for use because they have high electrochemical catalytic activity for the reduction of oxygen (and the oxidation of hydrogen) in the temperature range around 80°C, which is the operating temperature of solid polymer electrolyte fuel cells.
[0048] The shape of the electrode catalyst particles 3b is not particularly limited, and may be the same as that of known electrode catalyst particles. Specific shapes include a sphere, an ellipse, a polyhedron, a core-shell structure, etc. The structure of the electrode catalyst particles 3b is not limited to a crystal, and may be amorphous or a mixture of a crystal and an amorphous structure.
[0049] The smaller the size of the electrode catalyst particles 3b, the greater the effective surface area for the electrochemical reaction to proceed, and therefore the higher the electrochemical catalytic activity tends to be. However, if the size is too small, the electrochemical reaction activity decreases. Therefore, the size of the electrode catalyst particles 3b is preferably 0.5 to 4 nm in average particle diameter.
[0050] In the present invention, the "average particle size of electrode catalyst particles" can be obtained by averaging the particle sizes of electrode catalyst particles (20 particles) examined from an electron microscope image. When calculating the average particle size from an electron microscope image, if the shape of the fine particles is other than spherical, the length in the direction showing the maximum length of the particle is taken as the particle size.
[0051] The amount of electrode catalyst particles supported is appropriately determined taking into consideration the type of catalyst, the size (thickness) of the electronic conductive oxide carrier, etc. If the amount of catalyst supported is too small, the electrode performance will be insufficient, and if it is too large, the electrode catalyst particles may aggregate and performance may decrease.
[0052] When the amount of electrode catalyst particles supported is preferably 0.1 to 60 mass%, and more preferably 0.5 to 20 mass%, relative to the total weight of the electrode material, excellent catalytic activity per unit mass can be obtained, and a desired electrode reaction activity can be obtained according to the supported amount.
[0053] The amount of the electrode catalyst particles supported is usually 3 to 40 mass % relative to the electronic conductive oxide. Within this range, excellent catalytic activity per unit mass can be obtained, and a desired electrochemical catalytic activity according to the supported amount can be obtained. If the amount of the electrode catalyst particles loaded is less than 3 mass%, the electrode reaction activity is insufficient, and if the amount of the electrode catalyst particles loaded is more than 40 mass%, the electrode catalyst particles are likely to aggregate, resulting in a problem of a decrease in the effective surface area for the electrochemical reaction of oxygen and hydrogen. The amount of the electrode catalyst particles loaded can be examined, for example, by inductively coupled plasma emission spectrometry (ICP).
[0054] As described above, the method for producing an electrode material of the present invention includes steps (1) to (4). Each step will be described in detail below.
[0055] <Process (1)> Step (1) is a step of contacting mesoporous carbon with anhydrous alcohol to obtain a dispersion containing mesoporous carbon having anhydrous alcohol introduced into the pores.
[0056] Since absolute alcohol is an amphipathic solvent (dispersion medium), it is possible to introduce absolute alcohol into the pores by contacting it with mesoporous carbon (hydrophobic).
[0057] In the present invention, absolute alcohol means alcohol having a purity of 99.5% by volume or more, more preferably 99.7% by volume or more, and particularly preferably 99.8% by volume or more. The alcohol may be any alcohol that has high permeability into the pores of the mesoporous carbon, specifically, one or more selected from methanol, ethanol, n-propanol, and isopropanol, with ethanol being preferred.
[0058] The method for contacting the mesoporous carbon with the absolute alcohol is not limited as long as it does not impair the object of the present invention, but a typical method includes immersing the mesoporous carbon in the absolute alcohol and stirring it.
[0059] The amount of absolute alcohol relative to the mesoporous carbon may be any amount as long as it is capable of sufficiently filling the pores of the mesoporous carbon. The dispersion liquid containing the mesoporous carbon is subjected to the next step (step (2)), and the absolute alcohol that is the solvent (dispersion medium) in step (1) becomes part of the solvent of the mixed solution in step (2).
[0060] <Process (2)> Step (2) is a step of mixing the dispersion containing the mesoporous carbon into which the anhydrous alcohol has been introduced obtained in step (1), a tin alkoxide solution containing a tin alkoxide of an electronically conductive oxide, and a water / alcohol solvent to obtain a mixed solution, and then distilling off the solvent from the mixed solution to obtain a dried product in which a hydrolysate of the tin alkoxide is fixed to the inner and outer pore surfaces of the mesoporous carbon.
[0061] As described above, water does not easily penetrate into the pores of untreated mesoporous carbon. However, in the production method of the present invention, mesoporous carbon having an amphipathic anhydrous alcohol introduced into the pores is used in step (1), and a dispersion containing this mesoporous carbon is mixed with a tin alkoxide solution and a water / alcohol solvent (a mixed solvent of water and alcohol), making it possible to introduce tin alkoxide (hydrophobic) and water (hydrophilic) into the pores of the mesoporous carbon together with the alcohol solvent.
[0062] The ratio of water to alcohol in the mixed solvent is appropriately determined within a range that does not impair the object of the present invention. In order to reliably produce a hydrolysate in the pores of the mesoporous carbon, the ratio of water in the mixed solution in step (2) is 0.1 vol% to 10 vol% (preferably 0.5 vol% to 5 vol%) in a total of 100 vol% of water and alcohol. If the proportion of water in the solvent is too high, the hydrolysis reaction will proceed rapidly in the liquid, the hydrolyzate produced will be more likely to aggregate, and the proportion of tin alkoxide that reacts within the pores of the mesoporous carbon will decrease, tending to reduce the amount of hydrolyzate produced within the pores. The amount of alcohol in the mixed solution is the sum of the amount of alcohol added as the water / alcohol solvent in step (2) and the amount of absolute alcohol used as the solvent (dispersion medium) in step (1).
[0063] Although it is not entirely clear why the above water concentration is appropriate in step (2), it is speculated as follows. Since tin alkoxide is an alkoxide that is relatively low in reactivity with water, the hydrolysis reaction does not proceed easily when the concentration of water in the mixed solution is low. Therefore, if the ratio of water in the mixed solution is within the above range, the hydrolysis reaction in the liquid does not proceed substantially, and the tin alkoxide and water are introduced into the pores of the mesoporous carbon without reacting. If the solvent is distilled off in this state, the alcohol is preferentially removed, so the concentrations of the tin alkoxide and water become relatively large. As a result, the hydrolysis reaction of the tin alkoxide proceeds (both inside and outside the pores of the mesoporous carbon), and the mesoporous carbon can be dried in a state in which the hydrolyzate of the tin alkoxide is retained on the surface (the inner and outer surfaces of the pores).
[0064] The alcohol in the water / alcohol solvent used in step (2) may be at least one selected from methanol, ethanol, n-propanol, and isopropanol, but is preferably the same as the absolute alcohol used in step (1). That is, when absolute ethanol is used in step (1), it is preferable to use ethanol in step (2).
[0065] As the tin alkoxide, tin methoxide, tin ethoxide, tin propoxide, tin butoxide, tin methoxyethoxide, and tin ethoxyethoxide can be used. Among these, tin ethoxide is preferred.
[0066] For example, when the target electronic conductive oxide is a Sn oxide containing niobium oxide, niobium alkoxide may be used together with the above-mentioned tin alkoxide. As the niobium alkoxide, niobium methoxide, niobium ethoxide, niobium propoxide, niobium butoxide, niobium methoxyethoxide, and niobium ethoxyethoxide may be used. Among these, niobium ethoxide is preferable.
[0067] When the target electronically conductive oxide is a Sn oxide containing niobium oxide, as shown in the examples, a method is preferable in which, as described above, a dried product in which a hydrolyzate of tin alkoxide is fixed to the inner and outer pore surfaces of mesoporous carbon is obtained, the obtained dried product is dispersed in a niobium alkoxide solution, and the solvent is then distilled off to obtain a dried product. The solvent in the niobium alkoxide solution is preferably the same as that of the mixed solution containing tin alkoxide. That is, when the solvent of the mixed solution containing tin alkoxide is ethanol, the solvent of the niobium alkoxide solution is also preferably ethanol.
[0068] The amount and concentration of mesoporous carbon may be appropriately determined within a range that allows sufficient fixation of the generated hydrolysate, for example, 10% by weight to 80% by weight based on the final electronically conductive oxide derived from the raw material alkoxide, where the total of the electronically conductive oxide and mesoporous carbon is 100% by weight.
[0069] The non-aqueous organic solvent for the raw material alkoxide solution may be any organic solvent that does not react with the raw material alkoxide, and examples of such organic solvents include acetone, acetylacetone, toluene, xylene, and kerosene.
[0070] The method for distilling off the solvent and drying the mixture may be any method as long as it does not impair the object of the present invention, but distilling off the solvent under reduced pressure is preferred. A specific example of this is a method for drying the mixture under reduced pressure using a vacuum device such as a rotary evaporator.
[0071] <Process (3)> The step (3) is a step of heat-treating the dried product obtained in the step (2) to obtain a porous composite support in which an electronically conductive oxide is adhered to the inner and outer pore surfaces of the mesoporous carbon.
[0072] As described above, the dried material obtained in step (2) retains the hydrolyzate produced by hydrolysis on the surface of the mesoporous carbon (the inner and outer surfaces of the pores). The hydrolyzate is a hydroxide or non-stoichiometric oxide that has low crystallinity and poor adhesion to the mesoporous carbon carrier, but heat treatment improves the crystallinity of the electronically conductive oxide, allowing it to adhere (fix) strongly to the mesoporous carbon.
[0073] The atmosphere during the heat treatment may be any atmosphere that converts the hydrolysate of the alkoxide compound into an oxide and does not affect the electronically conductive oxide or the carbon carrier, and is usually an inert gas atmosphere such as nitrogen, helium, or argon.
[0074] The heat treatment temperature may be any temperature at which the crystallinity of the electronically conductive oxide is improved, and is 350° C. or higher, preferably 500° C. or higher, and more preferably 550° C. or higher. Furthermore, since tin oxide, which is the main component of the electronically conductive oxide, becomes metallic tin when the temperature approaches 700° C., the upper limit temperature is 650° C. or lower, and preferably 630° C. or lower.
[0075] The heat treatment time may be set so as to increase the crystallinity without causing aggregation, and is usually about 20 minutes to 3 hours, although it depends on the heat treatment temperature.
[0076] <Process (4)> Step (4) is a step of mixing the porous composite support obtained in step (3) (mesoporous carbon having an electronically conductive oxide adhered to the inner and outer pore surfaces) with a solution containing an electrode catalyst precursor until the mixture is homogeneous, and then distilling off the solvent to obtain a dried product, which is then heat-treated in an inert gas atmosphere.
[0077] In step (3), a dried product is obtained in which the electrode catalyst particle precursor is supported on the electronic conductive oxide in the porous composite support (mesoporous carbon with an electronic conductive oxide fixed to the surface). The electrode catalyst particles supported on the porous composite support contained in the obtained dried product may contain non-stoichiometric metal oxides and have low activity as is, so the electrochemical catalytic action of the metal that becomes the electrode catalyst is activated by heat treatment in an inert atmosphere such as nitrogen or argon, or in a reducing atmosphere containing hydrogen.
[0078] The electrode catalyst precursor in step (3) is not limited as long as it does not impair the object of the present invention. However, depending on the electrode catalyst precursor, the object of the present invention may not be achieved in terms of the particle size or dispersibility of the electrode metal particles.
[0079] As an electrode catalyst precursor capable of obtaining highly dispersed and small particle size electrode catalyst particles, an acetylacetonate compound of the electrode catalyst is suitable. After the acetylacetonate compound, which is the electrode catalyst precursor, is supported on a porous composite carrier, the electrode catalyst precursor is directly converted into electrode catalyst particles. In this method, the electrode catalyst precursor does not contain residual impurities, so that the catalytic activity is expected to be improved. In the acetylacetonate method, the electrode catalyst precursor is supported by dispersing the porous composite support in a solution in which the acetylacetonate compound of the electrode catalyst is dissolved in a suitable solvent such as dichloromethane, stirring the solution, and distilling off the solvent. This method can avoid the inclusion of impurities such as chlorine and sulfur, and can support highly dispersed electrode catalyst particles with a uniform nano-sized particle size distribution. In addition, since no strong oxidizing agent or reducing agent is used in the solution, there is an advantage in that deterioration of the electronically conductive oxide constituting the porous composite support and the mesoporous carbon that is the carbon support can be avoided.
[0080] The acetylacetonate compound of the electrode catalyst includes acetylacetonates of noble metals such as Pt, Ru, Ir, Pd, Rh, Os, Au, Ag, etc., and one or more of these can be used. The solvent may be any organic solvent capable of dispersing the noble metal acetylacetonate, and representative examples include dichloromethane and acetylacetone.
[0081] A method for supporting electrode catalyst fine particles using the acetylacetonate method is to place a conductive auxiliary material supporting an electronically conductive oxide and a precious metal acetylacetonate in a designated container, and while cooling with ice, stir with an ultrasonic stirrer until all of the solvent has evaporated.
[0082] The heat treatment conditions are appropriately selected depending on the type of electronically conductive oxide, metal or precursor to be the electrode catalyst. For example, in the case of an electronically conductive oxide such as tin oxide that is unstable in a reducing atmosphere, when the electrode catalyst is Pt or a Pt alloy, the heat treatment temperature is usually 180 to 400°C, preferably 200 to 250°C. If the temperature is too low, the activation of the metal to be the electrode catalyst becomes insufficient, and if the temperature is too high, the electrode catalyst particles aggregate, resulting in a problem of the effective reaction surface area becoming too small. Water vapor may be added to the atmosphere as necessary.
[0083] The present invention has been described above, but these are merely examples of the present invention, and various configurations other than those described above may also be adopted. The embodiments disclosed herein are illustrative in all respects and are not limiting. In particular, matters not expressly disclosed in this disclosure, such as operating conditions, various parameters, dimensions, weights, volumes, etc. of components, do not deviate from the scope of ordinary practice by a person skilled in the art, and values that can be easily assumed by a person skilled in the art can be adopted. EXAMPLES
[0084] The present invention will be described in more detail below with reference to examples, but the present invention is not limited thereto. In the following, mesoporous carbon may be abbreviated as "MC".
[0085] 1. Preparation of Electrode Materials As the electrode material of the embodiment, the following electrode material was produced.
[0086] The porous carbon, raw material alkoxide (electron-conductive oxide precursor), electrode catalyst precursor, and solvent used are as follows. <Porous carbon> As the porous carbon, the following mesoporous carbon (MC) (manufactured by Toyo Tanso Co., Ltd., "Porous Carbon CNovel MJ(4)010 (grade name)") was used. Design pore diameter: 10nm Specific surface area: 1100m 2 / g Total pore volume: 2.0mL / g Micropore volume: 0.4mL / g Particle size: 100 mesh pass (crushed before use) <Electron-conductive oxide precursor> As the Sn alkoxide, tin ethoxide (Sn(OC 2 H 5 ) 4 ) (Strem Chemicals INC), as Nb alkoxide, niobium ethoxide (Nb(OC 2 H 5 ) 5 ) (Sigma Aldrich) was used. <Electrode catalyst precursor> As an electrode catalyst precursor (precious metal precursor compound), Pt acetylacetonate (Pt(C 5 H 7 O 2 ) 2 In addition, Pt acetylacetonate is hereinafter referred to as Pt precursor (Pt(acac) 2 ) may be written. <Solvent (dispersion medium)> Absolute ethanol (Kishida Chemical Co., Ltd. Special grade ethanol (99.5))
[0087] As shown in the flowchart in FIG. 2, a porous composite support (sometimes referred to as "electrode material (electrode catalyst not supported)") was produced in which niobium-doped tin oxide was fixed to mesoporous carbon (MC).
[0088] <Experimental Example A1> Step (1): 183.7 mg of the above mesoporous carbon (MC) serving as a carrier framework was added to 50 mL of absolute ethanol, and the mixture was thoroughly mixed so that absolute ethanol was introduced into the MC pores. Step (2): The MC and tin ethoxide solution containing anhydrous ethanol (375 mg of tin ethoxide dissolved in 6 mL of acetylacetone) was added to a mixed solvent of ethanol and water and mixed thoroughly to obtain a mixed solution. The molar ratio of the contents of the mixed solution was tin ethoxide:water:MC=1.8:55.6:15.3, and the amount of solvent in the mixed solution was 100 mL (92 mL of ethanol (including the amount of anhydrous ethanol from step (1)), 2 mL of water, and 6 mL of acetylacetone). Step (3): The obtained mixed solution was reduced in pressure using a rotary evaporator equipped with a vacuum pump for reducing pressure, a control unit, and a rotation function, and the pressure was reduced while ultrasonically stirring to evaporate the solvent, thereby obtaining a dry powder in which tin ethoxide was uniformly adsorbed on the MC surface (inner and outer surfaces of the pores). Next, the obtained dry powder was dispersed again in ethanol, and 11.663 mg of niobium ethoxide dissolved in 203.4 μL of ethanol was added. The mixture was dried under reduced pressure until all the solvent evaporated, obtaining a dry powder in which tin ethoxide and niobium ethoxide were adsorbed on the MC surface (inner and outer surfaces of the pores). Step (4): The obtained dried powder is crushed and then heated at 400°C for 2 hours in N 2 The electrode material of Experimental Example A1 (electrode catalyst not supported, "Sn 0.98 Nb 0.02 O 2 / MC-400℃" was obtained. In the electrode material of Experimental Example A1, the oxide (Sn 0.98 Nb 0.02 O 2 ) 60wt% (feed amount).
[0089] <Experimental Example A2> The electrode material of Experimental Example A2 (electrode catalyst unsupported, "Sn 0.98 Nb 0.02 O 2 / MC-500℃" was obtained.
[0090] <Experimental Example A3> The electrode material of Experimental Example A3 (electrode catalyst unsupported, "Sn 0.98 Nb 0.02 O 2 / MC-600℃" was obtained.
[0091] <Experimental Example A4> The electrode material of Experimental Example A4 (electrode catalyst unsupported, "Sn 0.98 Nb 0.02 O 2 / MC-700℃" was obtained.
[0092] <Experimental Example A5> Oxide (Sn 0.98 Nb 0.02 O 2 % (charge amount) was changed to 20 wt % (charge amount) in the same manner as in Experimental Example A3 (60 wt % (charge amount)), to obtain an electrode material (electrode catalyst not supported) of Experimental Example A5.
[0093] <Experimental Example A6> Oxide (Sn 0.98 Nb 0.02 O 2 % (charged amount) was changed to 40 wt %. In the same manner as in Experimental Example A3, an electrode material (without supporting an electrode catalyst) of Experimental Example A6 was obtained.
[0094] <Experimental Example A7> Oxide (Sn 0.98 Nb 0.02 O 2 % (charged amount) was changed to 75 wt %. In the same manner as in Experimental Example A3, an electrode material (without electrode catalyst supported) of Experimental Example A7 was obtained.
[0095] 2. Evaluation of electrode materials (without electrode catalyst) The crystallinity of the electrode materials (not carrying an electrode catalyst) of Experimental Examples A1 to A4 was evaluated by X-ray diffraction, and the microstructure was evaluated by an electron microscope. FIG. 3 shows XRD profiles obtained at heat treatment temperatures of 600° C. (Experimental Example A3), 700° C. (Experimental Example A4), and no heat treatment as a reference. FIG. 4 shows FE-SEM and TEM images at a heat treatment temperature of 600°C (Example A3), FIG. 5 shows an FE-SEM image at a heat treatment temperature of 700°C (Example A4), and FIG. 6 shows selected-area electron diffraction images at heat treatment temperatures of 400°C (Example A1) and 500°C (Example A2).
[0096] As shown in Fig. 3, at a heat treatment temperature of 600°C (Example A3), SnO 2 The XRD signal indicating crystals was clearly confirmed. In FIG. 4, it was confirmed that fine particles were present in addition to MC. In addition, at heat treatment temperatures of 400°C (Experimental Example A1) and 500°C (Experimental Example A2), SnO 2 Although the XRD signal indicating crystals was not clear compared to the heat treatment temperature of 600° C. (not shown), the selected area electron diffraction shown in FIG. 6 indicates that SnO was also formed at heat treatment temperatures of 400° C. (Experimental Example A1) and 500° C. (Experimental Example A2). 2 The crystals are present, and increasing the heat treatment temperature results in SnO 2 It was confirmed that the crystallinity of the film was improved.
[0097] On the other hand, at a heat treatment temperature of 700°C (Experimental Example A4), it was confirmed that very large particles were generated outside the MC, as shown in Figure 5. Also, as shown in Figure 3, at a heat treatment temperature of 700°C (Experimental Example A4), SnO 2Since metallic Sn peaks were confirmed along with XRD signals indicating crystals, it was determined that the tin oxide reacted with carbon upon high-temperature heat treatment at 700°C, resulting in the reduction of the tin oxide and the disappearance of the carbon, causing the MC mesostructure to disappear and the aggregation of metallic tin to progress.
[0098] FIG. 7 shows the results of evaluation by STEM / EDS mapping for Experimental Example A3 and Experimental Examples A5 to A7, in which the amount of adhered oxide was changed at a heat treatment temperature of 600° C. In experimental examples A3 (20 wt%) and A5 (40 wt%), the Sn signals are separated, whereas in experimental examples A6 (60 wt%) and A7 (75 wt%) the Sn signals are in contact, which led to the conclusion that when tin oxide is highly loaded, the particles come into contact with each other. On the other hand, even when the amount of tin oxide loaded was increased, no significant aggregation was observed. From these results, it was concluded that the porous structure of the mesoporous carbon suppresses the grain growth of tin oxide and inhibits aggregation.
[0099] Next, using Experimental Example A6 (tin oxide adhesion rate 40 wt%), the results of observing the microstructure inside the mesopores in the MC are shown in FIG. The right side of Figure 8 shows images of the same area photographed with different STEM focuses: (a) the focus is on the front (near the mesopore surface), (b) the inside of the mesopore, and (c) the inside of the mesopore. Since the particles were present within a circle of about 10 nm, which is the pore size of MC, it was confirmed that tin oxide particles were supported inside the mesopores. In addition, since lattice fringes could be observed from different particles by changing the focus, it was confirmed that tin oxide exists in layers (see the image on the left in Figure 8), and that it was dispersed and supported deep inside the mesopores without agglomerating near the surface.
[0100] 3. Preparation of electrode material (Pt-supported) and evaluation of microstructure As shown in the flow chart of FIG. 9, the electrode materials (not carrying an electrode catalyst) of Experimental Example A3 and Experimental Examples A5 to A7 were loaded with Pt catalyst particles, which are electrode catalyst particles, by the platinum acetylacetonate method. 2The amount of Pt was adjusted so that the Pt content was 30 wt %. The electrode material of Experimental Example 1 (electrode catalyst not supported) consisting of MC with niobium-doped tin oxide attached and Pt precursor (Pt(acac) 2 ) was added, and acetone was further added to dissolve the mixture. Next, the mixture was rotated in a rotary evaporator under reduced pressure while applying ultrasonic waves in an ultrasonic cleaner until all the solvent had evaporated, obtaining a dry powder. The obtained dry powder was then dried in N 2 The electrode materials of Experimental Examples A3 and A5 to A7 (Pt / Sn 0.98 Nb 0.02 O 2 / MC").
[0101] <Comparative Example 1> As a comparative example, an electrode material (Pt / MC) of Comparative Example 1 was obtained in which Pt was supported on MC by a platinum acetylacetonate method.
[0102] (2) Electrode material (Pt-supported) Electrode material (Pt / Sn 0.98 Nb 0.02 O 2 As shown in Figure 10, in the electrode material of Experimental Example A3, Pt particles are Sn(Nb)O 2 It was confirmed that the Pt particles were dispersed and supported on the MC via the MC. Although not shown, the same was true for the electrode materials of Experimental Examples A5 to A7. It was confirmed that the Pt particles were directly supported on the MC in the electrode material of Comparative Example 1.
[0103] 4. Electrochemical evaluation (half cell) 4-1. Evaluation of cyclic voltammetry (CV) The electrode materials of Experimental Examples A3, A5 to A7 and Comparative Example 1 were evaluated by cyclic voltammetry (CV). The electrochemical surface area (ECSA) was calculated from the amount of hydrogen adsorption determined from CV. The ECSA corresponds to the effective surface area of Pt contained in the electrode material.
[0104] The fuel cell electrodes for evaluation were prepared in the following manner. First, a mixed solution of 19 mL of ultrapure water and 6 mL of 2-propanol was added to a sample bottle containing the electrode material powder, followed by the addition of 100 μL of 5% Nafion dispersion. The sample bottle was then immersed in ice water and ultrasonically stirred for 30 minutes to obtain an electrode material dispersion. The amount of electrode material powder was determined based on the amount of Pt per unit area on the electrode when 10 μL of the electrode material dispersion was dropped onto the electrode. -Pt ·cm -2 10 μL of the prepared electrode material dispersion was dropped onto the Au disk electrode using a micropipette and placed in an incubator and dried at 60° C. for about 15 minutes to form a Nafion membrane and fix the electrode material onto the Au electrode, thereby obtaining a fuel cell electrode (working electrode) for evaluation.
[0105] The CV measurement conditions are as follows. Assuming that one atom of H is adsorbed per one atom of Pt, the CV is 210 μC / cm 2 This results in an electrical charge of Measurement: Three-electrode cell (working electrode: fuel cell electrode for evaluation, counter electrode: Pt, reference electrode: Ag / AgCl) Electrolyte: 0.1M HClO 4 (pH: approx. 1) Measurement potential range: 0.05 to 1.2 V (based on the reversible hydrogen electrode) Scan speed: 50 mV / s Amount of hydrogen adsorption: Calculated from the peak area showing hydrogen adsorption at 0.05 to 0.4 V Electrochemical surface area (ECSA): Calculated using the following formula ECSA=(hydrogen adsorption amount)[μC] / 210[μC / cm 2 ]
[0106] 4-2. Evaluation of ORR activity The electrode materials of Experimental Examples A3, A5 to A7 and Comparative Example 1 were evaluated for ORR activity. ORR activity was measured by linear sweep voltammetry (LSV) using the rotating disk electrode (RDE) method, and the activation-dominant current (i k) was used as an index. Mass activity = i k / mass of Pt on electrode Activation dominant current (i k ) is the current-potential curve obtained by rotating electrode measurement at any potential i -1 and ω -1 / 2 A Koutecky-Levich plot was created by plotting the above-mentioned line, and the intercept was determined by extrapolating the obtained line. As a specific procedure, first, 2 After bubbling at 50 mL / min for 30 min, RHE 1.20 V at 10 mV / s in the positive direction RHE The potential was scanned up to 1000 V, and the measurements were performed. 2 The gas was purged at 50 mL / min. RHE is the potential relative to the reversible hydrogen electrode (RHE).
[0107] Electrode materials for experimental examples A3, A5 to 7 (Pt / Sn 0.98 Nb 0.02 O 2 CV and LSV were performed for the Pt / MC and Comparative Example 1 (Pt / MC), and the electrochemical surface area (ECSA), mass activity (j m (0.9V RHE )), Specific activity(j s The results are summarized in Table 1.
[0108] [Table 1]
[0109] 4-3. Start-stop cycle test A start-stop cycle test was conducted for the electrode materials of Experimental Examples A3, A5 to 7 and Comparative Example 1 according to the method recommended by the Fuel Cell Commercialization Promotion Council of Japan (Proposal of the Goals, Research and Development Issues and Evaluation Methods of Polymer Electrolyte Fuel Cells, published in January 2011). The start-stop cycle test is a cycle test that promotes carbon corrosion, and specifically, the start-stop cycle test was conducted at 1.0 to 1.5 V as shown in FIG. RHE A square wave of this voltage is applied for 2 seconds per cycle, and the deterioration behavior of the electrode catalyst after the cycle test is evaluated as a change in ECSA.
[0110] FIG. 12 shows the ECSA changes (relative values) of the electrode materials of Experimental Examples A3, A5 to A7, and Comparative Example 1 in a start-stop cycle test (up to 60,000 cycles). As can be seen from FIG. 12, the electrode using the electrode material of Comparative Example 1 (Pt / MC, 0 wt%) showed a large decrease in ECSA immediately after the start-stop cycle test, reaching about 50% of the initial value at 10,000 cycles, and the test could not be continued until 20,000 cycles (ECSA maintenance rate was almost 0). In contrast, the electrode materials (Pt / Sn 0.9 Nb 0.1 O 2 In the case of electrodes using Cr-Cr / MC, the decrease in ECSA was gradual, and both could be tested up to 60,000 cycles. In particular, it was confirmed that in Experimental Example A3 (oxide adhesion rate, 60 wt%), approximately 30% of the initial value could be maintained, and in Experimental Example A7 (oxide adhesion rate, 75 wt%), approximately 55% of the initial value could be maintained. These results indicate that degradation can be suppressed by supporting Pt via an oxide rather than by directly contacting the MC. [Industrial Applicability]
[0111] The electrode material of the present invention can provide a fuel cell electrode having excellent electrocatalytic activity, electronic conductivity, gas diffusibility, and durability, and is promising as an electrode component of a polymer electrolyte fuel cell used in the automobile, electric power, gas, and home appliance industries. It is particularly expected to be used for fuel cell automobiles that are subject to large load fluctuations. [Explanation of symbols]
[0112] 1 Electrode material 2. Porous carbon (mesoporous carbon) 2a Pore inner surface 2b Outer surface 3a Electronically Conductive Oxides 3b Electrocatalyst particles P Pore (mesopore)
Claims
1. A method for producing an electrode material comprising: a porous composite support made of mesoporous carbon and an electronically conductive oxide mainly composed of tin oxide adhered to the inner and outer pore surfaces of the mesoporous carbon; and electrode catalyst particles supported on the porous composite support, the method comprising the following steps (1) to (4): Step (1): A step of contacting mesoporous carbon with anhydrous alcohol to obtain a dispersion containing mesoporous carbon having anhydrous alcohol introduced into the pores. Step (2): A step of mixing the dispersion containing the mesoporous carbon into which the anhydrous alcohol has been introduced obtained in step (1), a tin alkoxide solution containing a tin alkoxide of an electronically conductive oxide, and a water / alcohol solvent to obtain a mixed solution, and then distilling off the solvent from the mixed solution to obtain a dried product in which a hydrolyzate of the tin alkoxide is fixed to the inner and outer surfaces of the pores of the mesoporous carbon. Step (3): A step of heat-treating the dried product obtained in step (2) to obtain a porous composite carrier in which an electronic conductive oxide is adhered to the inner and outer pore surfaces of the mesoporous carbon. Step (4): A step of mixing the porous composite support obtained in step (3) and the solution containing the electrode catalyst precursor until homogeneous, and then distilling off the solvent to obtain a dried product, which is then heat-treated in an inert gas atmosphere.
2. 2. The method for producing an electrode material according to claim 1, wherein in step (1), the absolute alcohol is at least one selected from the group consisting of methanol, ethanol, n-propanol and isopropanol.
3. 2. The method for producing an electrode material according to claim 1, wherein in the step (2), after obtaining a dried product in which a hydrolysate of tin alkoxide is fixed to the inner and outer pore surfaces of the mesoporous carbon, the dried product obtained is dispersed in a niobium alkoxide solution, and then the solvent is distilled off to obtain a dried product.
4. 4. The method for producing an electrode material according to claim 1, wherein in step (2), the proportion of water in the mixed solution is 0.1 vol% or more and 10 vol% or less in a total of 100 vol% of water and alcohol (including the absolute alcohol content in the dispersion).
5. 2. The method for producing an electrode material according to claim 1, wherein in the step (3), the heat treatment temperature is 350° C. or higher and 650° C. or lower.
6. 2. The method for producing an electrode material according to claim 1, wherein in the step (4), the electrode catalyst precursor is a noble metal acetylacetonate.
Citation Information
Patent Citations
Electrode material and method of manufacturing the same
JP2023101475A
Fuel cell electrode material and its manufacturing method, as well as fuel cell electrode, membrane electrode assembly, and polymer electrolyte fuel cell
JP6598159B2
Electrode material for fuel cells, and electrodes for fuel cells, membrane electrode assemblies, and polymer electrolyte fuel cells using the same
JP7228942B1
Noble metal single atom or cluster-porous molybdenum carbide / carbon nanocomposite using dynamic arrangement of noble metal atoms, method for manufacturing same, catalyst for hydrogen evolution reaction or hydrogen oxidation reaction comprising same, and electrode comprising the catalyst
US20230378481A1
Plastic working method for improving toughness of allsi alloy
JP1978022110A