Powder for powder metallurgy

A Si-containing copper-based powder with a sintering aid effectively removes oxide films, enabling sintering in normal atmospheres, thus overcoming sintering inhibition and producing high-quality sintered bodies with enhanced mechanical properties and cost-effectiveness.

JP2024145329APending Publication Date: 2024-10-15FUKUDA METAL FOIL & POWDER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023057627
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing powder metallurgy methods face sintering inhibition due to SiO2 oxide films, which require low oxygen partial pressure and dew point conditions, limiting the use of Si-containing metal powders and alloy types, and result in low sintered density at moderate pressures.

Method used

A Si-containing copper-based powder with a specific Si content and a sintering aid powder, such as an inorganic fluorine compound, that chemically removes the oxide film, allowing sintering in normal atmospheres without lowering oxygen partial pressure or dew point, and includes phosphorus to enhance mechanical properties.

Benefits of technology

The solution enables sintering without inhibitions, producing sintered bodies with excellent formability and mechanical properties, while maintaining flexibility in powder form and alloy type, reducing manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145329000001
    Figure 2024145329000001
  • Figure 2024145329000002
    Figure 2024145329000002
Patent Text Reader

Abstract

To provide a powder for powder metallurgy containing a Si-contained copper-based powder, which powder for powder metallurgy is less apt to cause an impediment to sintering even if sintered in an ordinary sintering atmosphere without lowering oxygen partial pressure or dew points, allowed to produce a sintered body excellent in formability or mechanical properties and moreover is not limitative in the form of powder or type of alloy.SOLUTION: A powder for powder metallurgy comprises: an Si-contained copper-based powder that is an alloy powder or powder mixture containing Si by 0.1-5.0 wt.% and a metal element having higher standard formation Gibbs energy of oxide in a temperature region of 750°C-1000°C than SiO2 by 30 wt.% or less, with the remainder of Cu and 0.5 wt.% or less of inevitable impurity elements; and a sinter-aid powder that is a powder consisting of an inorganic fluorine compound (AFn, where A is any element) and becoming negative in standard reaction Gibbs energy ΔGr of reaction represented by the following (reaction formula 1) in the above temperature region by 0.01-1.0 wt.%. (reaction formula 1) SiO2+(4 / n)AFn→SiF4+(2 / n)A2On.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a powder for powder metallurgy. More specifically, the powder for powder metallurgy is unlikely to cause sintering inhibition even when sintered in a normal sintering atmosphere without lowering the oxygen partial pressure or dew point, can produce a sintered body with excellent moldability and mechanical properties, and is not limited in powder form or alloy type. [Background technology]

[0002] Powder metallurgy is a method for manufacturing metal parts by compressing metal powder in a mold and sintering it at a temperature below the melting point of the metal.

[0003] With powder metallurgy, all that is required is a mold to form metal parts into a near-net shape, making it suitable for mass production of high-precision parts. Since there are fewer cutting processes, the powder metallurgy method is also economical and environmentally friendly.

[0004] In addition, because it is made from powder, it is also suitable for producing porous materials such as filters, and for producing composite materials with which there is no inherent affinity, such as cemented carbide and sliding materials.

[0005] In powder metallurgy, to eliminate the sintering inhibition caused by the formation of an oxide film on the powder surface, the oxide film is generally reduced and removed in an atmosphere containing reducing hydrogen before sintering.

[0006] However, when the standard reaction Gibbs energy of the reduction reaction between the oxide film and hydrogen is positive, the oxide film cannot be reduced or removed by hydrogen, resulting in the problem of sintering being hindered even when sintering in a hydrogen atmosphere.

[0007] Si is a commonly used element because it forms hard intermetallic compounds with Cr, Mn, Fe, Co, and Ni, contributing to strength and wear resistance.

[0008] However, silicon is an element that inhibits sintering. At 750°C to 1000°C, the Gibbs energy of the reaction SiO2+2H2→Si+2H2O is positive, while the Gibbs energy of the reaction Si+O2→SiO2 is negative. This means that the SiO2 oxide film cannot be reduced or removed by hydrogen, but reacts with oxygen and moisture in the sintering atmosphere to easily form a SiO2 oxide film.

[0009] Therefore, when sintering the Si-containing metal powder, it is necessary to carry out sintering by sufficiently lowering the oxygen partial pressure and water vapor pressure, for example by vacuum sintering.

[0010] Sintering of Si-containing metal powder depends on the composition and powder form (alloy powder, mixed powder), but sufficient sintering is possible if the dew point temperature is -50℃ to -40℃.

[0011] However, in the production of general-purpose sintered bodies, the dew point temperature during sintering is often set to −20° C. to 0° C. from the viewpoint of production costs, which causes a problem of sintering inhibition in the sintering of Si-containing metal powder.

[0012] Therefore, there is a need to develop a powder for powder metallurgy that can chemically remove the silicon oxide film, regardless of the powder form or alloy type, and that can suppress sintering inhibition even in normal sintering atmospheres that do not lower the oxygen partial pressure or dew point. [Patent Document 1] Patent No. 7143899 [Patent Document 2] Patent No. 6315241 [Patent Document 3] JP 2022-74433 A Summary of the Invention [Problem to be solved by the invention]

[0013] Patent Document 1 describes a copper-based sintered body that exhibits high electrical conductivity and strength by dissolving Ni and Si in Cu and then subjecting the resulting material to aging treatment to cause the precipitation of fine Ni2Si.

[0014] Patent Document 2 describes a copper-based sintered body in which coarse Ni2Si particles of about 2 μm are precipitated in the structure to improve wear resistance.

[0015] However, the inventions described in Patent Documents 1 and 2 are both intended for valve guides, and although the high molding pressure (500 MPa) for a copper-based material is used to improve the adhesion between powder particles and increase the sintered density, this does not fundamentally improve the sintering inhibition caused by the Si oxide film, and there is a problem that the sintered density becomes extremely low at molding pressures of 100 MPa to 400 MPa.

[0016] Patent Document 3 describes that a method using a mixture of Cu-Si powder and Ni powder can provide excellent sinterability even at a low molding pressure.

[0017] However, the invention described in Patent Document 3 has a problem in that the powder form and alloy type are limited, and other mixed powders and alloy powders cannot be used.

[0018] The inventors of the present invention set out to solve the above-mentioned problems as a technical task, and as a result of numerous trials and evaluations, have discovered a powder for powder metallurgy containing a Si-containing copper-based powder and a sintering aid powder, the Si-containing copper-based powder being an alloy powder or mixed powder containing 0.1 wt % or more and 5.0 wt % or less of Si, 30 wt % or less of a metal element whose standard Gibbs energy of oxide formation in the temperature range of 750°C or more and 1000°C or less is higher than that of SiO2, and the balance being Cu and 0.5 wt % or less of unavoidable impurity elements, and the sintering aid powder being a binary inorganic fluorine compound (AF n (where A is any element) and (Reaction formula 1) SiO2 + (4 / n)AF in the above temperature range. n →SiF4+(2 / n)A2O n Standard reaction Gibbs energy ΔG rThe present invention has achieved the above technical objective by obtaining the knowledge that, as long as the powder for powder metallurgy contains 0.01% by weight or more and 1.0% by weight or less of the sintering aid powder, sintering inhibition is unlikely to occur even when sintering is performed in a normal sintering atmosphere without lowering the oxygen partial pressure or the dew point, a sintered body having excellent moldability and mechanical properties can be produced, and further, a powder for powder metallurgy is capable of producing a sintered body having no limitations on the powder form or alloy type. [Means for solving the problem]

[0019] The above technical problems can be solved by the present invention as follows.

[0020] The present invention relates to a powder for powder metallurgy containing a Si-containing copper-based powder and a sintering aid powder, the Si-containing copper-based powder being an alloy powder or a mixed powder containing 0.1% by weight or more and 5.0% by weight or less of Si, 30% by weight or less of a metal element whose standard Gibbs energy of oxide formation in the temperature range of 750°C or more and 1000°C or less is higher than that of SiO2, and the balance being Cu and 0.5% by weight or less of unavoidable impurity elements, and the sintering aid powder is a binary inorganic fluorine compound (AF n where A is any element, and the standard reaction Gibbs energy ΔG of the reaction represented by the following (Reaction Scheme 1) in the above temperature range is r is negative, and the powder for powder metallurgy contains 0.01% by weight or more and 1.0% by weight or less of the sintering additive powder. (Reaction formula 1) SiO2 + (4 / n) AF n →SiF4+(2 / n)A2O n

[0021] The present invention also relates to the powder for powder metallurgy, which contains a phosphorus-containing alloy powder and has a total phosphorus content of 0.1% by weight or more and 0.5% by weight or less.

[0022] The present invention also relates to a method for producing the Si-containing copper-based powder having an apparent density of 4.0 g / cm. 3 or less, and at least 70% of the particle size distribution has a particle diameter of 106 μm or less.

[0023] The present invention also relates to the powder for powder metallurgy, which contains 3% by weight or less of a lubricant.

[0024] The present invention also relates to a sintered body obtained by sintering a compact of the above powder for powder metallurgy. Effect of the Invention

[0025] The powder for powder metallurgy of the present invention is a powder for powder metallurgy that is unlikely to suffer from sintering inhibition even when sintered in a normal sintering atmosphere in the same manner as with general copper-based powders, without lowering the oxygen partial pressure or dew point, because the SiO2 oxide film formed during sintering is removed by the inorganic fluorine compound sintering aid.

[0026] Furthermore, if a phosphorus-containing alloy powder is added, a sintered body having even better mechanical properties can be produced.

[0027] In addition, the apparent density of the Si-containing copper-based powder is 4.0 g / cm 3 If the particle size distribution is 106 μm or less and 70% or more of the particle size distribution has a particle size of 106 μm or less, the powder for powder metallurgy will have even better compactibility and sinterability.

[0028] Furthermore, if a lubricant is contained, the powder for powder metallurgy has excellent ejection properties from a die during compaction.

[0029] Furthermore, the powder for powder metallurgy according to the present invention is unlikely to cause sintering inhibition even when sintered in a normal sintering atmosphere, so that a sintered body having excellent mechanical properties can be produced while keeping production costs down. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] The powder for powder metallurgy in the present invention contains a Si-containing copper-based powder and a sintering aid powder.

[0031] (Si-containing copper-based powder) The Si-containing copper-based powder is an alloy powder or mixed powder containing Si and a metal element whose standard Gibbs energy of oxide formation in the temperature range of 750°C to 1000°C (hereinafter referred to as the "temperature range") is higher than that of SiO2, with the balance being Cu and unavoidable impurity elements.

[0032] The Si content in the Si-containing copper-based powder is 0.1% by weight to 5.0% by weight.

[0033] If the Si content is less than 0.1% by weight, the amount of SiO2 oxide film is small due to the small Si content, and sintering inhibition is suppressed, allowing sufficient sintering to be performed. On the other hand, if the Si content exceeds 5.0% by weight, there is a risk of sintering inhibition occurring in a normal sintering atmosphere.

[0034] The Si-containing copper-based powder also contains 30 wt % or less of a metal element whose standard Gibbs energy of oxide formation in the above temperature range is higher than that of SiO2.

[0035] The content of the metal element may be 0% by weight.

[0036] If a metal element having a lower standard Gibbs energy of oxide formation than SiO2 is contained in the above temperature range, an oxide film that is more stable than the SiO2 oxide film will be formed, and there is a risk that the effect of the sintering aid powder of the present invention will not be obtained.

[0037] Also, even if an element has a higher standard Gibbs energy of oxide formation than SiO2, if the content exceeds 30% by weight, there is a risk of sintering being inhibited.

[0038] Comparison of the standard Gibbs energies of formation can be performed by calculation from values ​​in a thermodynamic database, or by visual comparison of the standard Gibbs energies of formation illustrated by Ellingham diagrams.

[0039] Examples of metal elements having a higher standard Gibbs energy of oxide formation than SiO2 in the above temperature range include Mn, Co, Ni, Zn, and Sn.

[0040] The Si-containing copper-based powder may be in the form of an alloy powder or a mixed powder, and may be a powder produced by any production method.

[0041] The Si-containing copper-based powder has an apparent density of 4.0 g / cm 3 It is preferable that the particle size distribution is 106 μm or less, and that 70% or more of the particle size distribution has a particle size of 106 μm or less.

[0042] This is because it is possible to improve powder compactibility and sinterability.

[0043] Apparent density is 4.0g / cm 3 If the particle diameter exceeds 106 μm and / or less than 70% of the particle size distribution has a particle diameter of 106 μm or less, it becomes difficult to compact powder into complex shapes, and there is a risk that a sufficient sintered density will not be obtained.

[0044] In the Si-containing copper-based powder of the present invention, the remainder other than Si and the above-mentioned metal elements is Cu and unavoidable impurities.

[0045] The content of unavoidable impurities in the Si-containing copper-based powder is preferably 0.5% by weight or less.

[0046] When the amount of unavoidable impurities is 0.5% by weight or less, inhibition of sintering due to the unavoidable impurities is unlikely to occur.

[0047] (sintering aid powder) The sintering aid powder in the present invention is a binary inorganic fluorine compound (AF n (where A is any element), the standard reaction Gibbs energy ΔG of the reaction represented by the following (reaction formula 1) in the above temperature range is r is a negative powder. (Reaction formula 1) SiO2 + (4 / n) AF n →SiF4+(2 / n)A2O n

[0048] The standard Gibbs energy ΔG of the reaction represented by (Reaction Scheme 1) r Inorganic fluorine compounds AF with negative nIf this is the case, the reaction of (Reaction formula 1) will proceed spontaneously, and the SiO2 oxide film on the surface of the Si-containing copper-based powder will be formed by the inorganic fluorine compound AF n This is because, as with ordinary copper-based powders, the occurrence of sintering inhibition can be suppressed even if the powder is sintered in a normal sintering atmosphere.

[0049] Binary inorganic fluorine compound AF n is the standard reaction Gibbs energy ΔG r is negative, and the element A is not limited.

[0050] The sintering aid powder in the present invention has the above ΔG r It is sufficient to contain at least one inorganic fluorine compound with a negative ΔG r It may contain an inorganic fluorine compound that has a positive value.

[0051] The aforementioned ΔG r Examples of inorganic fluorine compounds with negative charge include CaF2 and AlF3.

[0052] The inorganic fluorine compound particles preferably have an average particle size of 50 μm or less.

[0053] If the average particle size exceeds 50 μm, the reactivity decreases and it is necessary to increase the amount added. However, this is because a large amount of unreacted inorganic fluorine compound particles will remain in the structure of the sintered body, which may result in a decrease in sinterability and a decrease in mechanical properties such as hardness and radial crushing strength of the sintered body.

[0054] The content of the sintering aid powder in the powder for powder metallurgy of the present invention is preferably 0.01% by weight to 1.0% by weight.

[0055] If the amount is less than 0.01% by weight, there may not be enough inorganic fluorine compound for the reaction, which may cause sintering inhibition, whereas if the amount is more than 1.0% by weight, the amount of inorganic fluorine compound that does not contribute to the reaction may increase, which may cause a deterioration in the mechanical properties of the sintered body.

[0056] The powder for powder metallurgy in the present invention may contain a phosphorus-containing alloy powder in order to further improve the sinterability.

[0057] This is because the phosphorus-containing alloy powder becomes liquid at the sintering temperature, and the sintering is accelerated by liquid phase sintering. Furthermore, phosphorus is dissolved in the structure, improving the mechanical properties of the sintered body.

[0058] The total phosphorus content of the powder for powder metallurgy in the present invention is preferably 0.1% by weight to 0.5% by weight.

[0059] If the content is less than 0.1% by weight, a sufficient effect of liquid phase sintering cannot be obtained, whereas if the content exceeds 0.5% by weight, the amount of liquid phase increases too much, which may cause dimensional distortion or coarsening of the sintered body structure, resulting in a decrease in radial crushing strength.

[0060] Examples of phosphorus-containing alloy powder include copper phosphorus, iron phosphorus, and nickel phosphorus.

[0061] The powder for powder metallurgy in the present invention may contain a molding lubricant such as a metal soap or wax in order to improve the ease of removal from a die during molding.

[0062] The content of the lubricant is preferably 0.1% by weight to 3% by weight, and more preferably 0.2% by weight to 1% by weight.

[0063] If the content is less than 0.1% by weight, sufficient effect cannot be obtained, whereas if the content exceeds 3% by weight, the mechanical properties of the sintered body may be significantly deteriorated and the inside of the sintering furnace may be contaminated by volatilized lubricant.

[0064] The powder for powder metallurgy in the present invention may contain, in addition to the compacting lubricant, a solid lubricant that does not react with the matrix and hard particles.

[0065] An example of the solid lubricant is graphite. EXAMPLES

[0066] Examples of the present invention will be described below, but the present invention is not limited to these.

[0067] The Gibbs energies of the examples and comparative examples were calculated using the thermodynamic database of "Thermochemical data of pure substances" written by Ihsan Barin.

[0068] In the examples, the Gibbs energies shown are all values ​​at 1200K (927°C), but in the temperature range of 750°C to 1000°C, there was no inversion of magnitude or positive / negative for any of the values.

[0069] (Preparation of raw powder) All of the alloy powders used in the Si-containing copper-based powders were produced by the water atomization method.

[0070] The mixed powder used was a mixture of Cu powder produced by electrolysis, Si powder produced by pulverization, and Ni powder (manufactured by Vale). Except for certain comparative examples, the apparent density of each powder form was 4.0 g / cm. 3 The particles were prepared so that 70% or more of the particle size distribution had a particle diameter of 106 μm or less.

[0071] CaF2 and AlF3 (manufactured by Kanto Chemical Co., Ltd.) were used as sintering aid powders.

[0072] For CaF2, the standard Gibbs energy of reaction ΔG for SiO2+2CaF2→SiF4+2CaO is r is -141 kJ / mol, and for AlF3, the standard Gibbs energy of reaction ΔG r is -38.7 kJ / mol, and both ΔG r <0.

[0073] In addition to the Si-containing copper-based powder and sintering aid powder, 0.5 wt% zinc stearate was added as a lubricant to improve the die removal property during powder compaction, and these were mixed in a rocking mixer to prepare the raw material powder.

[0074] The composition of the raw material powders is shown in Tables 1 and 2.

[0075] In Comparative Examples 1, 2, 3, 5, 6, 7, 9, and 10, no sintering aid powder was added to the Si-containing alloy powder.

[0076] In Comparative Examples 4, 8, and 11, ΔG r As an example of an additive inorganic fluorine compound with a molecular weight of >0, MgF2 (manufactured by Kanto Chemical Co., Ltd.) was used.

[0077] For MgF2, the standard Gibbs energy of reaction ΔG for SiO2+2MgF2→SiF4+2MgO is r is 144 kJ / mol.

[0078] In Comparative Example 12, as an example of excess Si, 6.0 wt % of Si was contained in the Si-containing copper-based powder.

[0079] In Comparative Example 13, a Si-containing copper-based powder containing 2.0 wt % Al was used as an example of an added metal element having a lower standard Gibbs energy of oxide formation than SiO2 in the temperature range of 750°C to 1000°C.

[0080] The standard Gibbs energy of formation of Si + O2 → SiO2 at 1200 K is -696 kJ / mol, and the standard Gibbs energy of formation of 4 / 3Al + O2 → 2 / 3Al2O3 is -863 kJ / mol.

[0081] In Comparative Example 14, 34.5 wt % of Ni was contained in the Si-containing copper-based powder as an example of an excess content of an element of an oxide having a higher standard Gibbs energy of formation than SiO2 in the temperature range of 750°C to 1000°C.

[0082] In Example 18 and Comparative Example 15, 3.0 wt % and 7.0 wt % of Cu-8.0P were added as examples of the addition and excess of phosphorus-containing alloy powder, that is, 0.24 wt % and 0.56 wt % were added as the total phosphorus content.

[0083] In Comparative Examples 16 and 17, the apparent density was 4.0 g / cm 3We produced a Si-containing alloy powder in which particles with a particle size of 106 μm or less accounted for less than 70% of the particle size distribution.

[0084] The apparent density (AD) of the Si-containing alloy powder was determined in accordance with the measurement method specified in JIS Z 2504.

[0085] The particle size distribution of the Si-containing alloy powder was determined according to JIS Z 2510, and the ratio of particles having a particle size of 106 μm or less was calculated based on the particle size distribution value.

[0086] (Compression of raw powder) Approximately 6 g of raw powder was filled into a cylindrical mold with an inner diameter of 7 mm and an outer diameter of 14 mm, and the molding density was 6.50 g / cm at a molding pressure of 150 MPa to 180 MPa. 3 A powder compact having an outer diameter of 14 mm, an inner diameter of 7 mm, and a height of approximately 6 mm was produced.

[0087] Regarding moldability, the powder compact was visually inspected after being taken out, and a powder compact without any chipped corners was rated as good, ◯, and otherwise was rated as ×.

[0088] (Sintering of powder compacts) The green compacts which showed good moldability were sintered by holding them in a nitrogen atmosphere at a sintering temperature of 1000°C for 30 minutes.

[0089] Regarding sinterability, the molding density is 6.50g / cm 3 At this time, the sintering density was 7.15g / cm when sintered at a dew point of -10°C. 3 If the density increased by 10% or more from the original density, the result was evaluated as good, with a rating of ◯; otherwise, the result was evaluated as ×.

[0090] However, in order to confirm the change in sinterability due to the dew point, the dew point was changed to -50°C in Comparative Examples 1, 5, and 9.

[0091] The results are shown in Tables 1 and 2. The numerical values ​​in the column for the Si-containing copper-based powder indicate the composition values ​​of the Si-containing copper-based powder in terms of weight percent.

[0092] [Table 1]

[0093] [Table 2]

[0094] It was shown that all of the powders in Examples 1 to 19 had good moldability and sinterability.

[0095] Regarding Comparative Examples 1 to 10, in Comparative Examples 1, 5, and 9, some Si-containing copper-based powders exhibited good sinterability at a dew point of -50°C even without the addition of a sintering aid powder. However, as shown in Comparative Examples 2, 3, 6, 7, and 10, all of the Si-containing copper-based powders exhibited significantly reduced sinterability at a dew point of -10°C, and good sinterability was not obtained.

[0096] From Comparative Examples 4, 8, and 11, ΔG r The addition of MgF2, an inorganic fluorine compound with a sintering rate of >0, did not improve the sinterability.

[0097] From Comparative Example 12, it was found that the sinterability significantly decreased in the raw material powder having a Si content of more than 5.0 wt %.

[0098] From Comparative Example 13, in the temperature range of 750°C to 1000°C, the sinterability was significantly reduced in the raw material powder containing a metal element whose oxide has a lower standard Gibbs energy of formation than SiO2.

[0099] From Comparative Example 14, in the temperature range of 750°C to 1000°C, when the content of oxide elements having a standard Gibbs energy of formation higher than SiO2 exceeded 30.0 wt%, the sinterability significantly decreased.

[0100] As seen from Comparative Example 15, the sintered body obtained by adding more than 0.5 wt % of the total phosphorus content had tapered dimensional distortion to the extent that the dimensions could not be measured accurately, and good sinterability was not obtained.

[0101] From Comparative Examples 16 and 17, the apparent density was 4.0 g / cm 3 In the case of the Si-containing copper-based powder in which particles with a particle size of 106 μm or less accounted for less than 70% of the particle size distribution, corner chipping occurred and a suitable green compact could not be obtained.

[0102] A comparison between the Examples and Comparative Examples proves that the powder for powder metallurgy of the present invention is unlikely to cause sintering inhibition even in a normal sintering atmosphere, and makes it possible to produce a sintered body having excellent moldability and mechanical properties. [Industrial Applicability]

[0103] The present invention relates to a powder for powder metallurgy which is unlikely to cause sintering inhibition even when sintering is performed in a normal sintering atmosphere without lowering the oxygen partial pressure or dew point, can produce a sintered body which has excellent moldability and mechanical properties, and is not limited in terms of powder form or alloy type. Therefore, the present invention has high industrial applicability.

Claims

1. A powder for powder metallurgy containing a Si-containing copper-based powder and a sintering aid powder, the Si-containing copper-based powder containing 0.1% by weight or more and 5.0% by weight or less of Si and having a standard Gibbs energy of oxide formation in a temperature range of 750° C. or more and 1000° C. or less of SiO 2 The alloy powder or mixed powder contains 30% by weight or less of a metal element having a higher content than 100% by weight, and the balance is Cu and 0.5% by weight or less of an inevitable impurity element, and the sintering aid powder is a binary inorganic fluorine compound (AF n where A is any element, and the standard reaction Gibbs energy ΔG of the reaction represented by the following reaction formula 1 in the above temperature range is r is negative, and the powder for powder metallurgy contains 0.01% by weight or more and 1.0% by weight or less of the sintering additive powder. (Reaction formula 1) SiO 2 +(4 / n)AF n →SiF 4 + (2 / n) A 2 O n

2. 2. The powder for powder metallurgy according to claim 1, which contains a phosphorus-containing alloy powder and has a total phosphorus content of 0.1% by weight or more and 0.5% by weight or less.

3. The apparent density of the Si-containing copper-based powder is 4.0 g / cm 3 3. The powder for powder metallurgy according to claim 1, wherein the particle size distribution is 106 μm or less and 70% or more of the particles have a particle size of 106 μm or less.

4. 3. The powder for powder metallurgy according to claim 1, further comprising not more than 3% by weight of a lubricant.

5. 3. A sintered body obtained by sintering a green compact of the powder for powder metallurgy according to claim 1 or 2.