Bending method, metal mold for bending and bent article
The described bending method for high-yield strength metal plates uses a punch with a protrusion and divided dies to achieve precise, damage-free bending with reduced springback, ensuring high dimensional accuracy and structural integrity for building materials.
Patent Information
- Application Number
- JP2023058122
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Bending high-yield strength metal plates for building materials results in low dimensional accuracy, mold damage, and springback issues, while conventional methods fail to maintain aesthetic quality and structural integrity.
A bending method using a punch with a protrusion and a die composed of divided dies with a V-shaped groove, where the punch and die recesses apply controlled deformation to high-yield strength metal plates, ensuring precise bending with reduced springback and mold damage.
The method achieves high dimensional accuracy, prevents mold damage, and produces bent products with sufficient strength and aesthetic appeal, suitable for exterior and interior building materials.
Smart Images

Figure 2024145671000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a bending method, a bending die, and a bent product. [Background technology]
[0002] Exterior and interior building materials include components used in easily visible locations such as window frames and curtain walls. These components require precise dimensions without distortion, small diameters at bent parts, and sharp bend ridges, and are required to have design and aesthetic appeal. In recent years, there has been a trend to use metal materials with high yield strength of 300 MPa or more for these components in order to ensure their strength as structural members.
[0003] When high-strength metal plate material is bent, the dimensional accuracy after bending may be reduced. If the processing conditions are made strict in order to improve the dimensional accuracy, cracks may occur in the bent portion. In addition, if the processing conditions are made strict, scratches or scoring marks may occur, which may impair the design. This is particularly problematic when the material is applied to building materials where aesthetics are important.
[0004] Furthermore, when bending is repeatedly performed on a high strength metal plate, there is a risk that the die used in the bending process may be damaged.
[0005] Patent Document 1 describes a grooved austenitic stainless steel sheet that makes it possible to provide a grooved steel sheet material that can form sharp ridgelines with excellent design by bending. However, Patent Document 1 requires the provision of a V-groove on the steel sheet surface, which is disadvantageous in terms of cost. In addition, the provision of a V-groove on the steel sheet surface reduces the thickness of the steel sheet, which reduces the wall thickness at the bent part of the bent product after bending, which may result in insufficient strength.
[0006] Patent Document 2 describes a press processing method in which, when bending a metal plate using a bending device consisting of a punch and a die, a recess having a depth of 20% or less of the metal plate thickness is formed on at least a part of the convex side of the bent metal plate in the final step of the forming stroke. However, the processed product manufactured by the press processing method described in Patent Document 2 may be unsightly because a recess is formed on the convex side, making it difficult to use it as a material for exterior or interior building materials. In addition, Patent Document 2 assumes that the material is a soft aluminum alloy plate, so there is a risk that it cannot be applied to bending metal plate materials having high strength.
[0007] Patent Document 3 describes a method of bending a workpiece having a thickness of t at a desired angle using a bending die that is made of a die and a punch, with the vicinity of the portion of the die and punch where the workpiece is to be bent being higher than the other die surfaces by a height of at most 10% of the thickness t, and with the apex corner of the die being rounded with a radius of approximately t. However, with the bending method described in Patent Document 3, it is difficult to suppress springback after bending. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2008-169423 A [Patent Document 2] Patent No. 3633012 [Patent Document 3] Special Publication No. 47-25266 Summary of the Invention [Problem to be solved by the invention]
[0009] The present invention has been made in consideration of the above-mentioned circumstances, and an object of the present invention is to provide a bending method, a bending die, and a bent product that can stably produce bent products with high dimensional accuracy while preventing damage to the die, can suppress springback, and is free of the risk of insufficient strength in the bent portion. [Means for solving the problem]
[0010] In order to solve the above problems, the present invention employs the following configuration. [1] A placement step of placing a blank made of a metal plate between a punch and a die; a forming step of bending the blank by bringing the punch and the die closer to each other, The material is a metal plate material having a 0.2% proof stress of 300 MPa or more, a yield ratio of 0.90 or less, and a plate thickness of 6.0 mm or less, the punch comprises a pair of punch die surfaces approaching each other toward a tip of the punch, and a protrusion provided at the tip of the punch, the tip surface of the protrusion is a convex curved surface having a radius of curvature corresponding to a length of 30% to 50% of the thickness of the material, and the length of the protrusion is a length corresponding to 30% to 100% of the thickness of the material, the die is composed of a first split die having a first inclined surface relative to one of the punch die faces and a first divided concave curved surface located on a lower end side of the first inclined surface, and a second split die having a second inclined surface relative to the other punch die face and a second divided concave curved surface located on a lower end side of the second inclined surface, Furthermore, when the first divided die and the second divided die are integrated, a V-groove-shaped die recess is formed with respect to the pair of punch mold surfaces by the first inclined surface and the second inclined surface, and the first divided concave curved surface and the second divided concave curved surface are continuous with each other to form a concave curved surface at the bottom of the die recess, the concave curved surface having a radius of curvature corresponding to a length of 50% or less of the thickness of the metal plate material, The forming process includes a first step of bending and deforming the blank while moving the punch toward a bottom dead center where the bending angle of the blank during processing is in the range of (target forming angle -8)° to (target forming angle +2)°, while keeping the first and second divided dies spaced apart from each other by an interval corresponding to a length of 30% to 50% of the thickness of the blank. and a second step of, after the punch reaches the bottom dead center, bringing the first and second split dies close together until they are integrated to form the die recess, thereby pressing the pair of punch type surfaces and the protrusion of the punch, and the die recess and the concave curved surface of the die, respectively, against the material. [2] A die for bending a material made of a metal plate having a 0.2% proof stress of 300 MPa or more, a yield ratio of 0.90 or less, and a plate thickness of 6.0 mm or less, A punch including a pair of punch die faces approaching each other toward a tip of the punch and a protrusion provided at the tip of the punch; A die block having a V-groove-shaped die recess corresponding to the pair of punch faces, The tip surface of the protrusion is a convex curved surface having a radius of curvature corresponding to a length of 30% to 50% of the plate thickness of the material, and the length of the protrusion is a length corresponding to 30% to 100% of the plate thickness of the material, The bottom of the die recess is provided with a concave curved surface having a radius of curvature corresponding to a length of 50% or less of the plate thickness of the material, The die includes: a first split die having a first inclined surface relative to one of the punch die faces and a first divided concave curved surface located on a lower end side of the first inclined surface, and a second split die having a second inclined surface relative to the other of the punch die faces and a second divided concave curved surface located on a lower end side of the second inclined surface, Furthermore, when the first divided die and the second divided die are integrated, the die recess is formed by the first inclined surface and the second inclined surface, and the first divided concave curved surface and the second divided concave curved surface are continuous to form the concave curved surface of the die recess.This is a mold for bending. [3] A plate part made of a metal plate material having a 0.2% proof stress of 300 MPa or more, a yield ratio of 0.90 or less, and a plate thickness of 6.0 mm or less; and a bending part provided on the plate part; The radius of curvature of the convex curved surface on the outer side of the bent portion is a radius of a length equivalent to the plate thickness of the plate portion, The minimum thickness of the bent portion is 0.75 times or more the plate thickness t of the plate portion, A recess is provided on the inner side of the bent portion along the longitudinal direction of the bent portion, The recess has a depth equivalent to 30 to 100% of the thickness of the plate material portion, and has a concave curved surface at its bottom with a radius of curvature equivalent to 30 to 50% of the thickness of the plate material portion. [4] Vickers hardness HV m Vickers hardness HV r Ratio (HV r / HV m ) is in the range of 1.50 or more and 1.90 or less. [5] The metal plate has a 0.2% yield strength of 450 MPa or more, a yield ratio of 0.50 to 0.90, and a chemical composition of the metal plate in mass percent: C: 0.050% or less, Si: 2.00% or less, Mn: 1.00-8.00%, P: 0.050% or less, S: 0.0500% or less, Ni: 0.10-6.00%, Cr: 17.00~25.00%, Mo: 0.10-2.50%, Cu: 0.10-3.00%, N: Contains 0.080 to 0.300% The bent product according to [3] or [4], wherein the remainder is a ferritic-austenitic duplex stainless steel plate consisting of Fe and impurities. [6] The bent product according to [5], wherein the metal plate further contains, in mass %, one or more of the following group A, group B or group C in place of a portion of Fe: (Group A) One or more of the following: Sn: 0.01 to 1.00% or less, W: 0.01 to 1.00%, V: 0.01 to 1.00%. (Group B) One or more of the following: Ca: 0.0050% or less, Mg: 0.0050% or less, Al: 0.50% or less, rare earth elements: 0.50% or less. (Group C) Nb: 0.100% or less Effect of the Invention
[0011] According to the bending method of the present invention, when bending a material using a punch and a die, a punch having a protrusion at its tip, and first and second split dies which, when integrated, form a die having a V-groove-shaped die recess and a concave curved bottom are used, and the material is bent and deformed while the first and second split dies are kept apart and the punch approaches bottom dead center, and then, after the punch reaches bottom dead center, the first and second split dies are integrated to press the punch surface and protrusion, and the die recess and concave curved surface against the material, respectively, allowing material to flow to the bottom of the die recess and preventing damage to the die. Furthermore, the radius of curvature of the concave surface at the bottom of the die recess is set to a length equivalent to 50% or less of the thickness of the material, and the length of the protrusion is set to a length equivalent to 100% or less of the thickness of the material, so that the radius of curvature of the convex surface on the outside of the bend of the bending portion is small. Furthermore, by using a punch having a protrusion, the distribution of residual stress in the bent portion is made different from the distribution of residual stress in the bent portion when die bending is performed using a punch without a protrusion. In conventional die bending, it is believed that springback occurs due to tensile residual stress on the outside of the bend and compressive residual stress on the inside of the bend, but in the present invention, the residual stress distribution in the bent portion changes compared to the conventional method, thereby reducing springback after die bending. Therefore, according to the present invention, it is possible to stably manufacture bent products with high dimensional accuracy while preventing damage to the die, using a metal plate material that satisfies the following requirements: 0.2% proof stress of 300 MPa or more, a yield ratio of 0.90 or less, and a plate thickness of 6.0 mm or less. That is, according to the processing method of the present invention, it is possible to manufacture a bent product with a small radius of curvature of the convex curved surface on the outside of the bent portion, a sharp shape, and small springback after die bending, while preventing damage to the die.
[0012] The bending die of the present invention comprises a punch having a protrusion at its tip, and a die having a V-groove-shaped die recess with a concave bottom, and the tip surface of the protrusion is a convex surface with a radius of curvature equivalent to a length of 30% to 50% of the thickness of the material, and the length of the protrusion is a length equivalent to 100% or less of the thickness of the material. Therefore, by using this die as a die for bending a material made of a metal plate satisfying the following requirements: 0.2% proof stress of 300 MPa or more, a yield ratio of 0.90 or less, and a thickness of 6.0 mm or less, bent products with high dimensional accuracy can be stably produced.
[0013] In addition, according to the bending mold of the present invention, the die is composed of a first split die and a second split die, and when the first split die and the second split die are integrated, a die recess is formed and a concave curved surface of the die recess is formed, thereby preventing damage to the die.
[0014] According to the bent product of the present invention, the radius of curvature of the convex curved surface on the outside of the bent portion is a radius of a length equivalent to or less than the plate thickness of the plate portion, and a recess with a depth equivalent to 30 to 100% of the plate thickness of the plate portion is provided on the inside of the bent portion, and a concave curved surface is provided at the bottom of the recess, so that the radius of curvature of the convex curved surface on the outside of the bent portion is small and a sharp shape can be obtained. Also, since the minimum thickness of the bent portion is 0.75 times or more the plate thickness of the plate portion, the strength of the bent portion can be made sufficient.
[0015] In addition, the bent product of the present invention has a recess along the longitudinal direction of the bent portion, and a concave curved surface is provided inside the recess. This recess is an indentation formed by the protruding portion of the punch during die bending. By providing such an indentation, the bent portion of the bent product is in a state in which compressive residual stress is imparted in the thickness direction of the bent portion. Therefore, according to the present invention, springback caused by the relationship between the conventional compressive residual stress and the tensile residual stress is reduced, and the springback can be reduced. In addition, since the inner surface of the recess is a concave curved surface, the occurrence of cracks originating from the recess can also be prevented.
[0016] In addition, according to the bent product of the present invention, the Vickers hardness HV m Vickers hardness HV in the bent part r Ratio (HV r / HV m ) is in the range of 1.50 to 1.90, and the Vickers hardness of the bent portion is high. Therefore, even though the thickness of the bent portion is smaller than the plate thickness of the plate portion by providing a recess in the bent portion, sufficient strength can be imparted to the bent portion. [Brief description of the drawings]
[0017] [Figure 1A] FIG. 1A is a schematic diagram showing a bending mold according to an embodiment of the present invention, illustrating a state in which the die is integrated. [Figure 1B] FIG. 1B is a schematic diagram showing a bending die according to an embodiment of the present invention, illustrating a state in which the die is divided. [Figure 1C] FIG. 1C is a schematic diagram illustrating the length of a protrusion in a mold according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram illustrating a bending method according to an embodiment of the present invention, showing an arrangement step. [Diagram 3] FIG. 3 is a schematic diagram for explaining the bending method according to the embodiment of the present invention, showing the first step of the forming process. [Figure 4]FIG. 4 is a schematic diagram illustrating the bending method according to the embodiment of the present invention, showing a second step of the forming process. [Diagram 5] FIG. 5 is a schematic cross-sectional view of a bent product according to an embodiment of the present invention. [Figure 6] FIG. 6 is a schematic diagram illustrating a conventional bending method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, a bending method, a bending die (hereinafter sometimes referred to as a die), and a bent product according to embodiments of the present invention will be described.
[0019] The outline of this embodiment is as follows. The bending method of this embodiment includes a placement step of placing a blank 3 made of a metal plate between a punch 1 and a die 2 as shown in Fig. 2, and a forming step of bending the blank 3 by bringing the punch 1 and the die 2 close to each other as shown in Fig. 3 and Fig. 4. The blank 3 is a metal plate satisfying the following requirements: 0.2% proof stress of 300 MPa or more, a yield ratio of 0.90 or less, and a plate thickness t of 6.0 mm or less.
[0020] As shown in FIG. 1A and FIG. 1B, the punch 1 has a pair of punch die faces 1b and a protrusion 1c provided on the punch tip 1a. The tip face 1e of the protrusion 1c is a convex curved surface, and the length H of the protrusion 1c is a predetermined length. Also, as shown in FIG. 1A and FIG. 1B, the die 2 is composed of a first divided die 2A and a second divided die 2B. The first divided die 2A and the second divided die 2B can be separated from each other as shown in FIG. 1B, or can be integrated as shown in FIG. 1A. When the first divided die 2A and the second divided die 2B are integrated, a V-groove-shaped die recess 2a is formed with respect to the pair of punch die faces 1b as shown in FIG. 1A. Also, a concave curved surface 2b with a predetermined radius of curvature Rd is provided on the bottom 2d of the die recess 2a.
[0021] In the forming process, as shown in Fig. 3, the punch 1 is moved toward the bottom dead center while the first and second divided dies 2A and 2B are kept apart, and then, after the punch 1 reaches the bottom dead center, the first and second divided dies 2A and 2B are integrated together, as shown in Fig. 4. This results in a bent product 4 having a sharply shaped bent portion 4b with a small radius of curvature Rout of the convex curved surface 4c on the outer side of the bent portion, as shown in Fig. 5. The present embodiment will be described below in order.
[0022] (material) The raw material 3 according to this embodiment is a metal plate material that satisfies the following requirements: 0.2% proof stress of 300 MPa or more, a yield ratio of 0.90 or less, and a plate thickness t of 6.0 mm or less. The reasons for limiting the metal plate material suitable for the raw material 3 will be described below.
[0023] <0.2% yield strength> The 0.2% yield strength of the metal plate material according to this embodiment is 300 MPa or more. This ensures sufficient strength when the metal plate material according to this embodiment is used as a material for exterior building materials or interior building materials. If the 0.2% yield strength is less than 300 MPa, the strength is insufficient. The 0.2% yield strength may be 450 MPa or more.
[0024] <Yield ratio> The yield ratio of the metal plate material according to this embodiment is set to 0.90 or less. This makes it possible to suppress cracks in the bent portion, particularly on the outer surface of the bent portion, during bending. If the yield ratio exceeds 0.90, cracks will occur on the outer surface of the bent portion during bending, making it impossible to provide a bent product with excellent appearance. The ratio of yield strength (YS) to tensile strength (TS) is called the yield ratio (YS / TS), and here, the 0.2% proof stress is defined as the yield strength (YS). The yield ratio may be 0.50 or more.
[0025] <Thickness> The sheet thickness t of the metal sheet material according to this embodiment is 6.0 mm or less, preferably 4.0 mm or less. The lower limit of the sheet thickness t may be 0.5 mm or more, or may be 1 mm or more. By setting the sheet thickness t to 6.0 mm or less, the springback of the bent product after bending can be reduced.
[0026] The metal plate material according to the present embodiment is preferably a ferritic-austenitic duplex stainless steel plate (hereinafter, referred to as a duplex stainless steel plate). The duplex stainless steel plate has sufficient strength, is less expensive than an austenitic stainless steel plate, and has better corrosion resistance than a ferritic stainless steel plate.
[0027] However, because stainless steel has a higher yield strength than austenitic stainless steel and ferritic stainless steel, bending the material may result in poor dimensional accuracy. If the processing conditions are made strict in order to improve dimensional accuracy, cracks may occur in the bent portion. In addition, if the processing conditions are made strict, scratches or scoring may occur, which may impair the design and aesthetics of the material.
[0028] Furthermore, because the material itself is hard, a large forming pressure must be applied, which causes a large stress concentration on the punch and die, which may damage the die. For this reason, it has been difficult to apply duplex stainless steel sheets to exterior and interior building materials that require bending in places that are easily visible.
[0029] However, by applying the present invention, bending can be performed without causing such problems, in particular without damaging the mold, and a bent product with excellent design and aesthetic appeal can be provided.
[0030] Furthermore, when the metal plate material is a duplex stainless steel plate, it may be a steel plate having a 0.2% proof stress of 450 MPa or more, a yield ratio of 0.50 to 0.90, and a plate thickness t of 6.0 mm or less.
[0031] (Mold) Next, a metal bending die for use in manufacturing the bent product of this embodiment will be described with reference to FIGS. 1A to 1C. The die K according to this embodiment is a die for so-called die bending. That is, the die K according to this embodiment is used as a die for a processing method in which the die K (punch 1 and die 2) is pressed against the top and bottom of the material 3 with both ends 3a of the material 3 as free ends to bend the material 3. The die K according to this embodiment will be described below.
[0032] The mold K according to this embodiment is composed of a punch 1 and a die 2. The die 2 is composed of a first split die 2A and a second split die 2B.
[0033] As shown in Fig. 1, the punch 1 has a pair of punch die surfaces 1b that are inclined so as to approach each other toward the punch tip 1a, and a protrusion 1c provided on the punch tip 1a. The pair of punch die surfaces 1b have a relative angle θp in the range of, for example, 80 to 100°, preferably 85 to 95°, more preferably 88 to 92°, and even more preferably 90°. The pair of punch die surfaces 1b form the outer shape of the punch 1, and are inclined so as to approach each other toward the punch tip 1a. The punch tip 1a has a protrusion 1c.
[0034] The protrusion 1c protrudes from the punch tip 1a toward the die 2. As shown in Figures 1A and 1C, the protrusion 1c has a side wall surface 1d in contact with the punch die surface 1b and a tip surface 1e in contact with the side wall surface 1d. The side wall surface 1d is flat, and the tip surface 1e is a convex curved surface.
[0035] The tip surface 1e of the protrusion 1c is a convex curved surface with a curvature radius Rp. The curvature radius Rp of the tip surface 1e is a radius equivalent to a length of 30% to 50% of the thickness t of the material 3, that is, a length of 0.30t to 0.50t. By setting the curvature radius Rp to a radius equivalent to a length of 30% (0.30t) or more of the thickness t of the material 3, sufficient compressive stress can be applied to the bent portion 4b, as described below, and the springback of the bent product 4 can be reduced. In addition, by setting the curvature radius Rp to a radius equivalent to a length of 50% (0.50t) or less of the thickness t of the material 3, the curvature radius Rout of the convex curved surface 4c on the outer side of the bent portion 4b after bending can be reduced. In addition, by setting the tip surface 1e to a convex curved surface, cracking of the bent portion 4b of the bent product 4 can be prevented.
[0036] The length H of the protrusion 1c is set to a length equivalent to 30% or more and 100% or less of the sheet thickness t of the material 3, that is, a length equivalent to 0.30t to 1.00t. As shown in FIG. 1A and FIG. 1C, the length H of the protrusion 1c is the length in the protruding direction of the protrusion 1c, and is the length from the boundary position between the side wall surface 1d and the punch die surface 1b to the tip surface 1e. By setting the length H of the protrusion 1c to a length equivalent to 30% (0.30t) or more of the sheet thickness t of the material 3, the material flow to the bottom of the die recess 2a is promoted, and the curvature radius Rout of the convex curved surface 4c on the outer side of the bent portion 4b after bending can be reduced. In addition, a sufficient compressive stress can be applied to the bent portion 4b, and the springback of the bent product can be suppressed. Furthermore, by setting the length H of the protrusion 1c to a length equivalent to 100% (1.00t) or less of the plate thickness t of the raw material 3, the radius of curvature Rout of the convex curved surface 4c on the outer side of the bent portion 4b after bending can be reduced.
[0037] Length H of protrusion 1c is defined as the length from the boundary between side wall surface 1d and punch die surface 1b to tip surface 1e, but if the boundary between side wall surface 1d and punch die surface 1b is unclear, length H of protrusion 1c may be determined as follows. That is, as shown in Fig. 1C, the position of intersection X between an extension of the contour of punch die surface 1b and an extension of the contour of side wall surface 1d is identified, and an imaginary horizontal line M is drawn from intersection X in the direction of width W of protrusion 1c. Then, the distance between horizontal line M and the tip of protrusion 1c (the apex of the convex curved surface) is defined as length H of protrusion 1c.
[0038] In addition, it is preferable that the distance between the side wall surfaces 1d of the protrusions 1c, i.e., the width W of the protrusions 1c, is a length equivalent to 50% to 150% (0.50t to 1.50t) of the plate thickness t of the material 3. This can prevent damage to the protrusions 1c.
[0039] A concave curved surface 1g may be provided at the boundary between the pair of punch die surfaces 1b and the protrusion 1c. The radius of curvature Rj of the concave curved surface 1g is preferably set to a radius of curvature equivalent to a length equal to or less than 150% (1.50t) of the plate thickness t of the material 3. The provision of the concave curved surface 1g can prevent damage to the protrusion 1c.
[0040] Next, the die 2 will be described. The die 2 is composed of a first divided die 2A and a second divided die 2B. The first divided die 2A and the second divided die 2B can be integrated as shown in Fig. 1A, or can be separated from each other as shown in Fig. 1B.
[0041] The first split die 2A is composed of a split block 12A. On the upper side of the split block 12A, a first inclined surface 12a facing one punch die surface 1b of the punch 1 and a first split concave curved surface 12b on the lower end side of the first inclined surface 12a are provided. The first inclined surface 12a and the first split concave curved surface 12b are adjacent to each other. In addition, a first split surface 12e is provided on the side of the split block 12A. The first split surface 12e is adjacent to the first split concave curved surface 12b.
[0042] The second split die 2B is composed of a split block 12B. On the upper side of the split block 12B, a second inclined surface 12c facing the other punch die surface 1b of the punch 1 and a second split concave curved surface 12d at the lower end side of the second inclined surface 12c are provided. The second inclined surface 12c and the second split concave curved surface 12d are adjacent to each other. In addition, a second split surface 12f is provided on the side of the split block 12B. The second split surface 12f is adjacent to the second split concave curved surface 12d.
[0043] As shown in FIG. 1A, the first divided die 2A and the second divided die 2B can be integrated to form the die 2 by the first divided surface 12e of the first divided die 2A and the second divided surface 12f of the second divided die 2B being in contact with each other. When the first divided die 2A and the second divided die 2B are integrated, the divided block 12A and the divided block 12B form the die block 2C. When the first divided die 2A and the second divided die 2B are integrated, the die recess 2a is formed by the first inclined surface 12a and the second inclined surface 12c, and the first divided concave curved surface 12b and the second divided concave curved surface 12d are continuous to form the concave curved surface 2b at the bottom of the die recess 2a.
[0044] That is, as shown in FIG. 1A, the die 2, which is formed by integrating the first divided die 2A and the second divided die 2B, is provided with a die block 2C consisting of a divided block 12A and a divided block 12B. By integrating the first divided die 2A and the second divided die 2B, a die recess 2a is provided in the die block 2C. The die recess 2a is provided on the upper surface 2m of the die block 2C. The cross-sectional shape of the die recess 2a is a V-shaped groove shape with respect to the pair of punch die surfaces 1b of the punch 1. That is, the die recess 2a is defined by a pair of die die surfaces 2c corresponding to the pair of punch die surfaces 1b and a concave curved surface 2b provided on the bottom 2d of the die recess 2a. The pair of die die surfaces 2c are formed by a first inclined surface 12a and a second inclined surface 12c, and the concave curved surface 2b is formed by a first divided concave curved surface 12b and a second divided concave curved surface 12d.
[0045] The pair of die mold surfaces 2c are inclined so as to approach each other toward the bottom 2d of the die recess 2a. The concave curved surface 2b is located between the pair of die mold surfaces 2c. The pair of die mold surfaces 2c and the concave curved surface 2b are in contact with each other.
[0046] The radius of curvature Rd of the concave curved surface 2b of the die recess 2a is set to a radius equivalent to a length of 50% or less of the thickness t of the material 3, that is, a length of 0.50t or less. By setting the radius of curvature Rd to a radius of 50% (0.50t) or less of the thickness t of the material 3, a space in which the material can flow is secured at the bottom 2d of the die recess 2a, and the radius of curvature Rout of the convex curved surface 4c on the outer side of the bent portion 4b after bending can be reduced. In addition, a compressive stress of an appropriate magnitude that does not cause spring-go can be applied to the bent portion 4b, and springback can be suppressed. The lower limit of the radius of curvature Rd of the concave curved surface 2b does not need to be particularly limited, but it may be a radius equivalent to a length of 20% or more of the thickness t of the material 3, that is, a length of 0.20t or more.
[0047] Next, the bending method of this embodiment will be described with reference to Fig. 2 to Fig. 4. In the bending method of this embodiment, a bent portion 4b is formed in the material 3 by performing die bending on the material 3 using a punch 1 and a die 2. The punch 1 and die 2 used in the bending are as shown in Fig. 1A and Fig. 1B. The bending method of this embodiment includes a placement step and a forming step.
[0048] (Placement process) In the placement step, as shown in FIG. 2, the first and second split dies 2A and 2B constituting the die 2 are separated from each other, the material 3 is placed on the upper surfaces 2m of the first and second split dies 2A and 2B, and the punch 1 is placed above the material 3. The material 3 is placed so that its upper surface 3b faces the punch 1 and its lower surface 3c contacts the upper surfaces 2m of the first and second split dies 2A and 2B. In this manner, the material 3 is placed between the punch 1 and the die 2. Both ends 3a of the material 3 are free ends and are not constrained. The punch 1, the first and second split dies 2A and 2B are attached to a press molding machine (not shown).
[0049] (molding process) Next, in the molding process, the press molding machine is operated to sequentially perform a first step of moving the punch 1 toward the bottom dead center, and a second step of moving the first split die 2A and the second split die 2B toward each other and integrating them after the punch 1 reaches the bottom dead center, thereby performing die bending processing on the material 3.
[0050] In the first step, as shown in Fig. 3, while the first divided die 2A and the second divided die 2B are kept apart, the punch 1 and the die 2 (the first divided die 2A and the second divided die 2B) are brought relatively close to each other in order to bring the punch 1 closer to the bottom dead center, and the protrusion 1c of the punch 1 is pressed against the upper surface 3b of the material 3. The material 3 against which the protrusion 1c is pressed is pushed downward by the punch 1. As a result, bending deformation (plastic deformation) of the material 3 begins at the point where the protrusion 1c is in contact.
[0051] In addition, when the first divided die 2A and the second divided die 2B are separated, it is preferable that the distance z between the first divided surface 12e and the second divided surface 12f is a distance equivalent to a length of 30% to 50% (0.30t to 0.50t) of the thickness t of the material 3. If the distance z between the first divided surface 12e and the second divided surface 12f is shorter than the length equivalent to 30% of the thickness t of the material, stress caused by the protrusion 1c being pressed down through the material 3 is concentrated on the first divided concave curved surface 12b and the second divided concave curved surface 12d of the first divided die 2A and the second divided die 2B, making the first divided die 2A and the second divided die 2B more likely to be damaged. On the other hand, if the distance z between the first divided surface 12e and the second divided surface 12f is longer than the length equivalent to 50% of the thickness t of the material, the bending angle of the bent product cannot be set to the target angle.
[0052] When the punch 1 is pressed further down, the material 3 undergoes bending deformation (plastic deformation) and the lower surface 3c of the material comes into contact with the first inclined surface 12a of the first separate die 2A and the second inclined surface 12c of the second separate die 2B. Meanwhile, the lower surface 3c of the material 3 moves away from the upper surfaces 2m of the first separate die 2A and the second separate die 2B. The upper surface 3b of the material 3 is in contact only with the protrusion 1c, and is not in contact with the punch die surface 1b.
[0053] The bottom dead center of the punch 1 is a position where the bending angle of the blank 3 during processing is in the range of (target forming angle -8)° to (target forming angle +2)°. Here, the target forming angle means a target value of the bending angle θ of the bent product 4, but may be the relative angle θp of the punch die surface 1b of the punch 1. If the position where the bending angle of the blank 3 exceeds (target forming angle +2)° is set as the bottom dead center of the punch 1, the pushing amount of the punch 1 will be insufficient, resulting in a defective shape, which is not preferable. Also, if the position where the bending angle of the blank 3 is less than (target forming angle -8)° is set as the bottom dead center of the punch 1, the pushing amount of the punch 1 will be excessive, making it difficult for the material flow described below to occur, which is not preferable. Also, from the viewpoint of suppressing springback and spring-go after bending, a more preferable bottom dead center of the punch 1 is a position where the bending angle of the blank 3 during processing is in the range of (target forming angle -4)° to (target forming angle)°.
[0054] Next, in the second step, after the punch 1 reaches the bottom dead center, as shown in FIG. 4, the first divided die 2A and the second divided die 2B are brought close to each other, and the first divided surface 12e and the second divided surface 12f are brought into contact with each other. In this way, the first divided die 2A and the second divided die 2B are brought close to each other until they are integrated. The first divided die 2A and the second divided die 2B are integrated to form the die 2, and the die recess 2a is formed, and the concave curved surface 2b is formed at the bottom 2d of the die recess 2a. Then, the pair of punch die surfaces 1b and protrusions 1c of the punch 1 and the die recess 2a and concave curved surface 2b of the die are pressed against the material 3, respectively. As a result, the bent portion 4b is formed in the material 3.
[0055] Since the punch 1 remains stationary after reaching the bottom dead center, the blank 3 located near the protrusion 1c is pressed against the side wall surface 1d of the protrusion 1c from both sides of the protrusion 1c as the first and second divided dies 2A and 2B approach each other. The blank 3 pressed against the side wall surface 1d of the protrusion 1c is subjected to a process similar to forging. As a result, material flow occurs in the bent portion 4b, and material flow occurs between the lower surface 3c of the blank 3 and the concave curved surface 2b of the die 2. As a result, the convex curved surface 4c on the outer side of the bent portion 4b is formed by the concave curved surface 2b of the die 2, and the radius of curvature Rout becomes smaller. As a result of the above, a bent product 4 having a bent portion 4b as shown in FIG. 5 is manufactured.
[0056] FIG. 6 shows a cross-sectional schematic diagram of a case where a punch 111 without a protrusion and a die 102 without a division are used for comparison. When the blank 3 is bent using the punch 111 without a protrusion, the punch 111 and the die 102 are moved relatively close to each other until the punch surface 111b and the die surface 102c are in close contact with the upper surface 3b and the lower surface 3c of the blank 3, respectively, as shown in FIG. 6. However, since the punch 111 does not have a protrusion, no material flow occurs in the bent portion 14b, and the bending process ends with a gap S1 remaining between the lower surface 3c of the blank 3 and the concave curved surface 102b of the die 102. For this reason, the bent product manufactured using the punch 111 without a protrusion cannot reduce the radius of curvature Rout of the convex curved surface 14c on the outer side of the bent portion 14b. In addition, since no compressive residual stress is imparted in the thickness direction of the bent portion 14b, it is difficult to suppress springback. In the case of Figure 6, in order to suppress springback, it is effective to press the material 3 with a large force at the bottom dead center (perform a final press). However, in that case, the load on the die 102 becomes large, and the undivided die 102 may be damaged.
[0057] Next, the bent product 4 according to this embodiment will be described. Fig. 5 shows a schematic cross-sectional view of the bent product of this embodiment.
[0058] The bent product 4 according to this embodiment includes a plate part 4a made of a metal plate having a 0.2% proof stress of 300 MPa or more, a yield ratio of 0.90 or less, and a plate thickness t of 6.0 mm or less, and a bent part 4b provided on the plate part 4a. A convex curved surface 4c is provided on the bent outer side of the bent part 4b, and a recess 4d of depth D is provided on the bent inner side.
[0059] The bending angle θ of the bent portion 4b is in the range of 85° to 95°, more preferably in the range of 88° to 92°, and further preferably 90°. This means that when the target bending angle θ is 90°, the bending angle θ of the bent portion 4b is within the range of ±5° or ±2°. By setting the bending angle θ within the above range, the variation in the bending angle θ is reduced, and a sharp ridgeline is formed over the entire length of the outer side of the bend of the bent portion 4b.
[0060] The radius of curvature Rout of the convex surface 4c on the outside of the bend is set to a radius of a length equal to or less than the plate thickness of the plate portion 4a. By setting the radius of curvature Rout of the convex surface 4e on the outside of the bend to be equal to or less than the plate thickness t of the plate portion 4a, the appearance of the outside of the bend of the bent portion 4b becomes angular and sharp, making it suitable for use as an exterior and interior building material.
[0061] A recess 4d having a depth D is provided on the inside of the bent portion 4b. This recess 4d is an impression formed when the protrusion 1c of the punch 1 is brought into close contact with the material in the final stage of the forming process. The recess 4d has a concave curved surface 4e formed by the tip surface 1e of the protrusion 1c. Since the inside of the recess 4d is the concave curved surface 4e, the occurrence of cracks originating from the recess 4d is prevented.
[0062] The depth D of the recess 4d provided on the inner side of the bent portion 4b is set to a depth equivalent to 30 to 100% (0.30t to 1.00t) of the thickness t of the plate material portion 4a. Furthermore, the recess 4d is provided at its bottom with a concave curved surface 4e having a radius of curvature Rq equivalent to 30 to 50% (0.30t to 0.50t) of the thickness t of the plate material portion 4a. By setting the depth D of the recess and the radius of curvature Rq of the concave curved surface 4e within the above range, it is possible to reduce the radius of curvature Rout of the convex curved surface 4c on the outer side of the bend, and also to prevent the occurrence of cracks. As shown in FIG. 5, the depth D of the recess 4d is the length in the depth direction of the recess 4d, and is the length from the position corresponding to the boundary between the side wall surface 1d and the punch die surface 1b of the punch 1 to the groove bottom of the recess 4d (the apex of the concave curved surface 4e) corresponding to the tip of the protrusion 1c of the punch (the apex of the convex curved surface). The depth D of the recess 4d can be determined in the same manner as the method for measuring the length H of the protrusion 1c of the punch.
[0063] In addition, by providing a recess 4d on the inner side of the bend of the bent portion 4b, the thickness of the bent portion 4b becomes smaller than the plate thickness t of the plate portion 4a, but the minimum thickness of the bent portion 4b needs to be 0.75 times (0.75t) or more the plate thickness t of the plate portion 4a, thereby making it possible to ensure sufficient strength of the bent portion 4b.
[0064] In addition, the Vickers hardness HV m Vickers hardness HV at bent portion 4b r Ratio (HV r / HV m ) is preferably in the range of 1.50 or more and 1.90 or less. In addition to the work hardening caused by the plastic deformation of the raw material 3, the bent portion 4b according to this embodiment is also work hardened due to the residual stress applied in the thickness direction by the protrusion 1c during the forming process. Therefore, the hardness of the bent portion 4b of the bent part 4 according to this embodiment is higher than the hardness of the plate portion 4a, and the strength of the bent portion 4b is increased. On the other hand, if the hardness of the bent portion 4b becomes too high, cracks are more likely to occur in the bent portion 4b. Therefore, the Vickers hardness HV m Vickers hardness HV at bent portion 4b rRatio (HV r / HV m ) is preferably in the range of 1.50 to 1.90.
[0065] Vickers hardness HV of plate part 4a m and the Vickers hardness HV of the bent portion 4b r are measured as follows:
[0066] Vickers hardness HV of plate part 4a m As shown in FIG. 5, a virtual line L1 connecting the inner and outer surfaces of the bent part is set along the thickness direction of the plate part 4a at a position t mm from the plate end of the bent product, and the Vickers hardness HV is measured at at least three points on this virtual line L1. The average of these measured values is defined as the Vickers hardness HV of the plate part 4a. m Here, t is the plate thickness 4a of the plate part.
[0067] Vickers hardness HV of bent section 4b r As shown in FIG. 5, in the minimum thickness portion of the bent portion 4b, an imaginary line L2 connecting the inner surface and the outer surface of the bent portion is set along the thickness direction of the plate portion 4a, and the Vickers hardness HV is measured at least at three points on this imaginary line L2. The average of these measured values is defined as the Vickers hardness HV at the bent portion 4b. r Let us assume that.
[0068] The interval between the measurement positions on the imaginary lines L1 and L2 is, for example, 100 μm.
[0069] It is advisable to use a micro Vickers hardness tester to measure the Vickers hardness HV. The Vickers hardness HV is measured in accordance with the micro Vickers hardness test in JIS Z 2244:2009. The test force (F) is 0.098N (HV0.01).
[0070] The material for the bent product 4 is preferably a ferritic-austenitic duplex stainless steel sheet having a 0.2% proof stress of 300 MPa or more, preferably 450 MPa or more, a yield ratio of 0.90 or less, preferably 0.50 to 0.90, and a sheet thickness t of 6.0 mm or less.
[0071] An example of such a stainless steel sheet is a ferritic-austenitic duplex stainless steel sheet having a chemical composition, in mass%, of C: 0.050% or less, Si: 2.00% or less, Mn: 1.00 to 8.00%, P: 0.050% or less, S: 0.0500% or less, Ni: 0.10 to 6.00%, Cr: 17.00 to 25.00%, Mo: 0.10 to 2.50%, Cu: 0.10 to 3.00%, N: 0.080 to 0.300%, with the balance being Fe and impurities.
[0072] Moreover, the above stainless steel sheet may further contain, in mass %, one or more of Sn: 0.01 to 1.00%, W: 0.01 to 1.00%, and V: 0.01 to 1.00%, instead of a portion of Fe. Furthermore, the above stainless steel sheet may contain, in place of a portion of Fe, one or more of the following, by mass%, Ca: 0.0050% or less, Mg: 0.0050% or less, Al: 0.50% or less, and rare earth elements: 0.50% or less. Furthermore, the above stainless steel sheet may further contain, in mass %, Nb: 0.100% or less in place of a portion of Fe.
[0073] In order to ensure the corrosion resistance of the steel sheet, the C content may be 0.050% or less, preferably 0.040% or less. On the other hand, since C is an element that forms austenite that constitutes a dual-phase structure, the C content may be preferably 0.005% or more, more preferably 0.010% or more.
[0074] For deoxidation, the Si content is preferably 0.01% or more, more preferably 0.10% or more, and even more preferably 0.30% or more. Since the Si content exceeding 2.00% promotes the precipitation of the σ phase, the Si content is preferably 2.00% or less, and more preferably 0.60% or less.
[0075] Mn is a deoxidizing agent and an austenite stabilizing element for forming a dual-phase structure, and should be contained in an amount of 1.00% or more, preferably 1.30% or more, and more preferably 2.00% or more. On the other hand, if the Mn content exceeds 8.00%, the corrosion resistance deteriorates, so the Mn content should be 8.00% or less, preferably 5.00% or less, and more preferably 4.00% or less.
[0076] Since P deteriorates hot workability and toughness, the P content is limited to 0.050% or less, and preferably 0.035% or less. On the other hand, since an excessive reduction in the P content increases refining costs, it may be set to 0.005% or more.
[0077] Since S deteriorates hot workability, toughness, and corrosion resistance, the S content is limited to 0.0500% or less, preferably 0.0100% or less, and more preferably 0.0040% or less. On the other hand, if the S content is excessively reduced, the raw material cost and refining cost will increase, so it may be set to 0.0003% or more.
[0078] When Ni is contained in the coating of the steel sheet, it has the effect of suppressing the occurrence of pitting corrosion when the Fe concentration of the coating is high, and the effect of suppressing the progression of corrosion when corrosion occurs. On the other hand, if the Ni content is excessive, the Cr content of the coating is too low, and sufficient corrosion resistance cannot be obtained. Therefore, it is preferable to set the Ni content in the range of 0.10 to 6.00%. The lower limit of the Ni content is preferably 0.30% or more, 0.50% or more, or may be 1.00% or more. The upper limit of the Ni content is preferably 5.50% or less, 4.00% or less, or 3.00% or less.
[0079] In order to impart sufficient corrosion resistance to the steel, the Cr content is preferably in the range of 17.00 to 25.00%. The lower limit of the Cr content is preferably 17.50% or more, more preferably 20.00% or more, and further preferably 21.00% or more. The upper limit of the Cr content is preferably 24.00% or less, and more preferably 22.00% or less.
[0080] Mo is an element that improves corrosion resistance, and is effective when contained at 0.10% or more. Mo may be contained up to 2.50%, but if the Mo content exceeds 2.50%, σ phase is likely to precipitate during hot working. Therefore, the lower limit of the Mo content is 0.10% or more, preferably 0.20% or more, and more preferably 0.30% or more. The upper limit of the Mo content is 2.50% or less, preferably 2.00% or less, and more preferably 1.50% or less.
[0081] When 0.10% or more of Cu is contained, the effect of suppressing the progress of corrosion when corrosion occurs is obtained. Cu may be contained in an amount of 3.00% or less. Furthermore, when the Cu amount exceeds 3.00%, cracks may easily occur during casting. Therefore, the lower limit of the Cu amount is 0.10% or more, preferably 0.30% or more, and more preferably 0.50% or more. The upper limit of the Cu amount is 3.00% or less, preferably 2.50% or less, and more preferably 2.00% or less.
[0082] N is an element that significantly improves corrosion resistance and increases the amount of austenite phase, and is preferably contained at 0.080% or more as an austenite stabilizing element. The lower limit of the N content is preferably 0.120% or more, and more preferably 0.150% or more. On the other hand, if the N content is excessive, nitrides are formed in the steel, which reduces the corrosion resistance and toughness, so the upper limit of the N content should be 0.300% or less. The upper limit of the N content is preferably 0.250% or less.
[0083] Furthermore, when a small amount of Sn is contained, the corrosion resistance is improved. Therefore, Sn is an element useful for improving the corrosion resistance, and may be contained within a range that does not impair the low cost. If the Sn content is less than 0.001%, the effect of improving the corrosion resistance is not realized, and if the Sn content exceeds 1.00%, the cost increase becomes apparent and the workability is also reduced, so the appropriate range of the Sn content is 0.001 to 1.00%. The lower limit of the Sn content is preferably 0.01% or more, and the upper limit of the Sn content is preferably 0.50% or less. Note that Sn is an optional element and may not be contained. In other words, the Sn content may be 0%.
[0084] V and W may be contained as necessary to improve corrosion resistance, particularly crevice corrosion resistance. However, excessive inclusion of V or W reduces workability and saturates the effect of improving corrosion resistance, so the lower limit of each of the amounts of V and W is set to 0.01% or more, and the upper limit of each of the amounts of V and W is set to 1.00% or less. The lower limit of each of the amounts of V and W is preferably 0.04% or more, and the upper limit of each of the amounts of V and W is preferably 0.50% or less. Note that V and W are optional elements and may not be contained. In other words, the V amount and the W amount may each be 0%.
[0085] Ca, Mg, and REM are elements that improve hot workability, and for that purpose, one or more of Ca, Mg, and REM may be contained. Since the effects of Ca and Mg are manifested at an amount of 0.0002% or more, the lower limit of each of the amounts of Ca and Mg is set to 0.0002% or more. In the case of REM, the lower limit is set to 0.001% or more. Note that Ca, Mg, and REM are optional elements and do not need to be contained. In other words, the amount of Ca, the amount of Mg, and the amount of REM may each be 0%.
[0086] However, since excessive content of either element adversely reduces hot workability, it is preferable to set the upper and lower limits of their contents as follows: the amounts of Ca and Mg are each 0.0002-0.0050%, and the amount of REM is 0.001-0.50%.
[0087] The lower limit of each of the Ca and Mg contents is preferably 0.0005% or more. The upper limit of each of the Ca and Mg contents is preferably 0.0025% or less. The lower limit of the REM content is preferably 0.005% or more, and the upper limit of the REM content is preferably 0.30% or less.
[0088] Here, rare earth elements (REM) refer to the two elements scandium (Sc) and yttrium (Y) and the 15 elements (lanthanoids) from lanthanum (La) to lutetium (Lu) according to the general definition. They may be contained alone or as a mixture. The amount of REM is the total amount of these elements.
[0089] Al is useful as a deoxidizing element, but should not be contained in large amounts because it deteriorates workability. It is preferable to limit the upper limit of the Al content to 0.50% or less. The preferred range of the Al content is 0.30% or less. The lower limit of the Al content is 0.01% or more. Note that Al is an optional element and does not need to be contained. In other words, the Al content may be 0%.
[0090] Nb has a strong affinity with N and forms nitrides preferentially over chromium, thereby suppressing the decrease in the amount of chromium in the material and improving corrosion resistance. For this reason, it may be contained as necessary. However, if Nb is contained in excess, toughness will decrease, so the Nb content is set to 0.100% or less, and may be 0.060% or less. On the other hand, in order to obtain the above effect, the Nb content is preferably 0.005% or more, more preferably 0.010% or more, and more preferably 0.020% or more. Note that Nb is an optional element and may not be contained. In other words, the Nb content may be 0%.
[0091] The balance other than the above-mentioned elements is Fe and impurities. In addition to the above-mentioned elements, other elements may be contained within a range that does not impair the effects of this embodiment.
[0092] The bent product 4 of this embodiment as described above can be suitably used as a material for exterior and interior building materials.
[0093] As described above, according to the bending method of this embodiment, when bending the material 3 using the punch 1 and die 2, the punch 1 has a protrusion 1c on the punch tip 1a, and the first and second divided dies 2A and 2B form the die 2 having a V-groove-shaped die recess 2a and its bottom 2d as a concave curved surface 2b when integrated, and while keeping the first and second divided dies 2A and 2B apart, the punch 1 is moved toward the bottom dead center to bend and deform the material 3, and then, after the punch 1 reaches the bottom dead center, the first and second divided dies 2A and 2B are integrated to press the punch surface 1b and the protrusion 1c, and the die recess 2a and the concave curved surface 2b against the material 3, respectively, so that material flows up to the bottom 2d of the die recess 2a and damage to the die 2 is prevented. Furthermore, the radius of curvature Rd of the concave surface 2b of the bottom 2d of the die recess 2a is set to a length equivalent to 50% or less of the sheet thickness t of the material 3, and the length H of the protrusion 1c is set to a length equivalent to 100% or less of the sheet thickness t of the material, so that the radius of curvature Rout of the convex surface 4c on the outer side of the bend of the bending portion 4b is small. Furthermore, by using the punch 1 having the protrusion 1c, the distribution state of the residual stress in the bent portion 4b can be made different from the distribution state of the residual stress in the bent portion when die bending is performed using a punch without the protrusion 1c. That is, in conventional die bending, it is believed that springback occurs due to tensile residual stress on the outside of the bend and compressive residual stress on the inside of the bend, but in this embodiment, the residual stress distribution in the bent portion 4b changes compared to the conventional method, so that the springback after die bending is reduced. Therefore, according to the present invention, by using a metal plate material 3 that satisfies the requirements of a 0.2% proof stress of 300 MPa or more, a yield ratio of 0.90 or less, and a plate thickness of 6.0 mm or less, it is possible to stably manufacture a bent product 4 with high dimensional accuracy while preventing damage to the die 2. That is, according to the bending method of this embodiment, it is possible to manufacture a bent product 4 in which the convex curved surface 4c on the outer side of the bent portion has a small radius of curvature Rout and a sharp shape, and in which the springback after die bending is small, while preventing damage to the die 2.
[0094] The bending die K of this embodiment includes a punch 1 having a protrusion 1c at its punch tip 1a, and a die 2 having a V-groove-shaped die recess 2a with a bottom 2d formed as a concave curved surface 2b, and the tip surface of the protrusion 1c is a convex curved surface 1e with a radius of curvature Rp corresponding to a length that is 30% or more and 50% or less of the plate thickness of the material 3. Furthermore, the length H of the protrusion 1c is a length that is 100% or less of the plate thickness t of the material 3. Therefore, by using this die K as a die when bending a material 3 made of a metal plate material that satisfies the requirements of a 0.2% proof stress of 300 MPa or more, a yield ratio of 0.90 or less, and a plate thickness of 6.0 mm or less, a bent product 4 with high dimensional accuracy can be stably manufactured.
[0095] In addition, according to the bending mold K of this embodiment, the die 2 is composed of a first split die 2A and a second split die 2B, and when the first split die 2A and the second split die 2B are integrated, a die recess 2a is formed and a concave curved surface 2b of the die recess 2a is formed, thereby preventing damage to the die 2.
[0096] According to the bent product of this embodiment, the radius of curvature Rout of the convex curved surface 4c on the outside of the bend of the bent portion 4b is a radius of a length equivalent to or less than the plate thickness t of the plate material portion 4a, and a recess 4d with a depth D equivalent to 30 to 100% of the plate thickness t of the plate material portion 4a is provided on the inside of the bend of the bent portion 4b, and a concave curved surface 4e with a radius of curvature Rq is provided at the bottom of the recess 4d, so that the radius of curvature Rout of the convex curved surface 4c on the outside of the bent portion can be made small and sharp. In addition, the minimum thickness tm of the bent portion 4b is 0.75 times or more the plate thickness t of the plate material portion 4a, so that the strength of the bent portion 4b can be made sufficient.
[0097] In addition, the bent product 4 of this embodiment has a recess 4d along the longitudinal direction of the bent portion 4b, and a concave curved surface 4e with a curvature radius Rq is provided inside the recess 4d. The recess 4d is an indentation formed by the protrusion 1c of the punch 1 during die bending. By providing such an indentation, the bent portion 4b of the bent product 4 is in a state in which compressive residual stress is imparted in the thickness direction of the bent portion 4b. Therefore, according to this embodiment, the springback caused by the relationship between the conventional compressive residual stress and the tensile residual stress is reduced, and the springback can be reduced. In addition, since the inner surface of the recess 4d is the concave curved surface 4e, the occurrence of cracks originating from the recess 4d can also be prevented.
[0098] In addition, according to the bent product 4 of this embodiment, the Vickers hardness HV m Vickers hardness HV at bent portion 4b r Ratio (HV r / HV m ) is in the range of 1.50 to 1.90, and the Vickers hardness of the bent portion 4b is high. Therefore, even though the thickness of the bent portion 4b is smaller than the plate thickness t of the plate portion 4a by providing the recess 4d in the bent portion 4b, sufficient strength can be imparted to the bent portion 4b.
[0099] Furthermore, by using stainless steel having the above-mentioned chemical composition as the material for the bent product 4, the bent product 4 of this embodiment has excellent strength and corrosion resistance and can be suitably used as an exterior building material and an interior building material. EXAMPLES
[0100] A ferritic-austenitic duplex stainless steel sheet was prepared with the chemical composition shown in Table 1 and the thickness t shown in Table 2A. The mechanical properties of the ferritic-austenitic duplex stainless steel sheet were as shown in Table 1. A metal plate material consisting of a ferritic-austenitic duplex stainless steel sheet was cut into a size of 100 mm in length and 30 mm in width to prepare the material. In Table 1, YS means yield strength, TS means tensile strength, T.El means total elongation, and 0.2 proof stress is shown as yield strength (YS).
[0101] In addition, a die having a punch and a die as shown in Fig. 1A and Fig. 1B was prepared. The punch used had a protrusion having a convex curved surface and a side wall surface connected to the convex curved surface. The relative angle θp of the punch type surface of the punch was 90°, and the target forming angle was 90°. The width of the punch was 80 mm, and the length (length in the depth direction in Fig. 1A and Fig. 1B) was 60 mm. The width of the die recess was 80 mm, and the length (length in the depth direction in Fig. 1) was 60 mm. The die used was composed of a first divided die and a second divided die.
[0102] Then, the punch, the first divided die, and the second divided die were attached to a press molding machine, and the material was placed between the punch, the first divided die, and the second divided die as shown in FIG. 2. At that time, the material was placed so that the length direction of the material coincided with the depth direction of FIG. 2. In addition, the width direction center of the material was aligned with the center of the die. Then, the press molding machine was operated, and as shown in FIG. 3 and FIG. 4, a first step of moving the punch toward the bottom dead center and a second step of moving the first divided die and the second divided die toward each other and integrating them after the punch reaches the bottom dead center were sequentially performed to perform V-bending on the material to form a bent portion. In this way, a bent product having a bent portion was manufactured. The number of metal plate materials was 1000, and the presence or absence of breakage or deformation of the punch and die was evaluated when V-bending was performed on 1000 metal materials using one die. The bottom dead center of the punch was set so that the bending angle of the material was in the range of -10° to +4° with respect to the target forming angle (90°).
[0103] The bending angle θ at the bent part was measured for the obtained bent product. The bending angle θ was measured by setting four measurement points at 1 cm intervals along the longitudinal direction of the bent part, and the bending angle θ at each measurement point was measured on the inside of the bent part. The average value of the bending angle θ at the four measurement points was then calculated. Δθ (= θ-θp) was calculated from the average value of the obtained bending angle θ and the relative angle θp (= 90 °) of the punch mold surface. Δθ is the angle change amount of the bent product with respect to the bending punch, and it indicates that springback has occurred when Δθ > 0, and spring-go has occurred when Δθ < 0. Since it is desirable that the absolute value of Δθ is small from the viewpoint of shape freezing, the range in which Δθ is -1.5 / t or more and 1.5 / t or less was passed. More specifically, when Δθ is 0 or more and 1.5 / t or less, the springback was evaluated as good, and when Δθ is less than 0 and -1.5 / t or more, the spring-go was evaluated as good. In addition, since the likelihood of springback or spring-go occurring and the absolute value of the angle change Δθ of the bent product relative to the bending punch vary depending on the plate thickness t, the plate thickness t is taken into consideration and a pass range of Δθ is set to be between -1.5 / t and 1.5 / t. The results are shown in Table 2.
[0104] As shown in Tables 2A to 2C, all of the invention examples A1 to A13 were subjected to die bending under conditions that satisfied the range of the invention. The target forming angle was 90°, and the bottom dead center of the punch was set at a position where the bending angle of the material during processing was in the range of (target forming angle -8)° to (target forming angle +2)°, i.e., 82° to 92°. As a result, the obtained bent product had a curvature radius of the convex curved surface on the outside of the bent part (outside diameter Rout in Table 2C) that was less than the thickness t of the sheet material part, a minimum thickness of the bent part (tm in Table 2C) that was 0.75 times or more the thickness t of the sheet material part, a curvature radius Rq of the concave curved surface of the recess and a depth D of the recess that satisfied the range of the invention, and an angle change amount of the bent product with respect to the bending punch (Δθ in Table 2) that was greater than or equal to -1.5 / t and less than or equal to 1.5 / t. Therefore, the bent products of the invention samples A1 to A13 were suppressed in springback and spring-go, and there was no risk of insufficient strength in the bent portion, and the shape of the outside of the bent portion was also sharp. In the invention samples A2, A5, and A10, the bottom dead center of the punch was set at a position where the bending angle of the material during processing was in the range of (target forming angle -3)° to (target forming angle)°, that is, in the range of 87° to 90°. As a result, the angle change amount (Δθ in Table 2) of the bent products was smaller in the invention samples A2, A5, and A10 compared to A1, A4, and A9, respectively. In other words, in the invention samples A2, A5, and A10, the springback after die bending was smaller and the dimensional accuracy was more stable.
[0105] In addition, in all of the invention samples A1 to A13, the Vickers hardness HV m Vickers hardness HV in the bent part r Ratio (HV r / HV m ) is now in the range of 1.50 to 1.90.
[0106] On the other hand, as shown in Tables 2A to 2C, in Comparative Example B1, the radius of curvature of the tip surface of the protrusion of the punch (punch diameter Rp in Table 2A) was more than 50% of the plate thickness of the material, so the radius of curvature on the outside of the bent portion (outer diameter Rout in Table 2C) exceeded the plate thickness, and a sharp shape was not obtained.
[0107] In Comparative Example B2, the radius of curvature Rp of the tip surface of the protrusion of the punch was less than 30% of the sheet thickness of the material, so that the compressive force of the bent portion was small and the springback was large.
[0108] In Comparative Example B3, the length of the protrusion of the punch (protrusion length H in Table 2A) was more than 100% of the sheet thickness of the material, the minimum thickness tm of the bent portion was small, and the strength and rigidity of the bent portion were reduced.
[0109] In Comparative Example B4, the length H of the punch projection was less than 30% of the sheet thickness of the material, so that the radius of curvature Rout of the outer bent portion exceeded the sheet thickness t, and a sharp shape could not be obtained. In addition, the springback was large.
[0110] In Comparative Example 5, an integrated die was used instead of a divided die, and the die and punch were damaged.
[0111] In comparative example B6, the radius of curvature of the bottom surface of the die recess of the die (die diameter Rd in Table 2A) exceeded 50% of the sheet thickness of the material, and therefore space for material flow was not secured, so that the radius of curvature Rout on the outside of the bent portion exceeded the sheet thickness t, and a sharp shape was not obtained.
[0112] In Comparative Example B7, the distance between the first and second separate die (initial die distance z in Table 2B) was too wide, so that the compression force in the bent portion was small and the springback was large. In Comparative Example B8, the distance z between the first and second separate dies was too narrow, so the punch was broken.
[0113] In Comparative Example B9, the bottom dead point of the punch (the angle θ of the workpiece when the die slide is opened in Table 2B) exceeded (target forming angle + 2)°, the amount of pressing of the punch was insufficient, and the material could not be formed at the desired angle, no material flow occurred, and a sharp shape could not be formed. In Comparative Example B10, the bottom dead center of the punch was less than (target forming angle-8)°, the punch thrust amount was excessive, and the die and punch were damaged, making forming difficult. In Comparative Example B11, since the yield strength (0.8% proof stress) of the material was less than 300 MPa, strain was concentrated in the bent portion, causing cracks.
[0114] In each test example, the width W of the protrusion was a length equivalent to 50% or more and 150% or less of the thickness of the material, and the radius of curvature Rj of the concave curved surface at the boundary between the punch die surface and the protrusion was a radius of curvature equivalent to a length not exceeding 150% of the thickness of the material.
[0115] [Table 1]
[0116] [Table 2A]
[0117] [Table 2B]
[0118] [Table 2C] [Explanation of symbols]
[0119] Reference Signs List 1... punch, 1a... punch tip, 1b... punch surface, 1c... protrusion, 1e... tip surface of protrusion, 2... die, 2A... first split die, 2B... second split die, 2C... die block, 2a... die recess, 2b... concave curved surface of die recess, 2d... bottom, 3... material, 4... bent product (bent product made of metal plate), 4a... plate portion, 4b... bent portion, 4c... bent outer side of bent portion of the die, 4d...concave portion of the bent portion, 4e...concave surface of the concave portion, 12a...first inclined surface, 12b...first divided concave surface, 12c...second inclined surface, 12d...second divided concave surface, D...depth of the concave portion, H...length of the protrusion, Rd...radius of curvature of the concave surface of the die, Rp...radius of curvature of the convex surface of the protrusion, Rq...radius of curvature of the concave surface of the concave portion, t...sheet thickness, z...distance between the first divided die and the second divided die.
Claims
1. a placement step of placing a blank made of a metal plate between the punch and the die; a forming step of bending the blank by bringing the punch and the die closer to each other, The material is a metal plate material satisfying the following requirements: 0.2% proof stress is 300 MPa or more, a yield ratio is 0.90 or less, and a plate thickness is 6.0 mm or less; the punch comprises a pair of punch die surfaces approaching each other toward a tip of the punch, and a protrusion provided at the tip of the punch, a tip surface of the protrusion is a convex curved surface having a radius of curvature corresponding to a length of 30% to 50% of a plate thickness of the material, and a length of the protrusion is a length corresponding to 30% to 100% of a plate thickness of the material, the die is composed of a first divided die having a first inclined surface relative to one of the punch die faces and a first divided concave curved surface located on a lower end side of the first inclined surface, and a second divided die having a second inclined surface relative to the other punch die face and a second divided concave curved surface located on a lower end side of the second inclined surface, Furthermore, when the first divided die and the second divided die are integrated, a V-groove-shaped die recess is formed with respect to the pair of punch mold surfaces by the first inclined surface and the second inclined surface, and the first divided concave curved surface and the second divided concave curved surface are continuous with each other to form a concave curved surface at the bottom of the die recess, the concave curved surface having a radius of curvature corresponding to a length of 50% or less of a thickness of the metal plate material, The forming process includes a first step of bending and deforming the material while moving the punch toward a bottom dead center where the bending angle of the material being processed is in the range of (target forming angle -8)° to (target forming angle +2)°, while keeping the first and second divided dies spaced apart from each other by an interval corresponding to a length of 30% to 50% of the thickness of the material; and a second step of, after the punch reaches the bottom dead center, bringing the first and second split dies close together until they are integrated to form the die recess, thereby pressing the pair of punch type surfaces and the protrusion of the punch, and the die recess and the concave curved surface of the die, respectively, against the material.
2. A die for bending a material made of a metal plate material having a 0.2% proof stress of 300 MPa or more, a yield ratio of 0.90 or less, and a plate thickness of 6.0 mm or less, A punch including a pair of punch die faces approaching each other toward a tip of the punch and a protrusion provided at the tip of the punch; A die including a die block having a V-groove-shaped die recess corresponding to the pair of punch faces, a tip surface of the protrusion is a convex curved surface having a radius of curvature corresponding to a length of 30% to 50% of the plate thickness of the material, and a length of the protrusion is a length corresponding to 30% to 100% of the plate thickness of the material, A bottom of the die recess is provided with a concave curved surface having a radius of curvature corresponding to a length of 50% or less of the plate thickness of the material, The die includes: a first split die having a first inclined surface relative to one of the punch die faces and a first divided concave curved surface located on a lower end side of the first inclined surface, and a second split die having a second inclined surface relative to the other punch die face and a second divided concave curved surface located on a lower end side of the second inclined surface, Furthermore, when the first divided die and the second divided die are integrated, the die recess is formed by the first inclined surface and the second inclined surface, and the first divided concave curved surface and the second divided concave curved surface are continuous to form the concave curved surface of the die recess, which is a mold for bending.
3. A plate portion made of a metal plate material satisfying the following requirements: 0.2% proof stress is 300 MPa or more, a yield ratio is 0.90 or less, and a plate thickness is 6.0 mm or less; and a bending portion provided on the plate portion, The radius of curvature of the convex curved surface on the outer side of the bent portion is a radius of a length equivalent to the plate thickness of the plate portion, The minimum thickness of the bent portion is 0.75 times or more the plate thickness t of the plate portion, A recess is provided on the inner side of the bent portion along the longitudinal direction of the bent portion, The recess has a depth equivalent to 30 to 100% of the thickness of the plate material portion, and a concave curved surface having a radius of curvature equivalent to 30 to 50% of the thickness of the plate material portion is provided at the bottom.
4. Vickers hardness HV m Vickers hardness HV at the bent portion r Ratio of (HV r / HV m 4. The bent product according to claim 3, wherein the ratio of the bending moment to the bending moment is in the range of 1.50 or more and 1.90 or less.
5. The metal plate material has a 0.2% yield strength of 450 MPa or more, a yield ratio of 0.50 to 0.90, and a chemical composition, in mass%, of: C: 0.050% or less, Si: 2.00% or less, Mn: 1.00-8.00%, P: 0.050% or less, S: 0.0500% or less, Ni: 0.10-6.00%, Cr: 17.00-25.00%, Mo: 0.10-2.50%, Cu: 0.10-3.00%, N: 0.080 to 0.300%; 5. The bent product according to claim 3 or 4, wherein the balance is a ferritic-austenitic duplex stainless steel sheet consisting of Fe and impurities.
6. The bent product according to claim 5 , wherein the metal plate further contains, in mass %, one or more of the following group A, group B, or group C in place of a portion of Fe: (Group A) One or more of Sn: 0.01 to 1.00% or less, W: 0.01 to 1.00%, V: 0.01 to 1.00%. (Group B) One or more of the following: Ca: 0.0050% or less, Mg: 0.0050% or less, Al: 0.50% or less, rare earth elements: 0.50% or less. (Group C) Nb: 0.100% or less
Citation Information
Patent Citations
Die for adjusting spring-back
JP1984178130A
Split die for bend-working
JP1999226646A
Mold
JP2004050265A
Metal plate bending method, metal mold for metal plate bending and bent article comprised of metal plate
JP2022182994A