Phosphor and light-emitting device

The use of crystal particles with controlled size and density in the phosphor suppresses fluorescence leakage and enhances light uniformity, ensuring efficient conversion of blue laser light to white light with improved mechanical strength.

JP2024145860AInactive Publication Date: 2024-10-15TDK CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023058403
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional phosphors used in laser illumination exhibit fluorescence leakage from the side surfaces, leading to ring-shaped fluorescence around the projected light and insufficient mixing of excitation and fluorescence, which affects the quality and uniformity of the emitted light.

Method used

A phosphor composed of crystal particles with a specific D50 size range (10 to 100 μm) and controlled density (3.73 to 4.10 g/cm³) is used, featuring voids between the particles to reflect light perpendicularly, suppressing lateral fluorescence propagation and enhancing mechanical strength.

Benefits of technology

The solution effectively suppresses fluorescence leakage from the side surfaces, improves light uniformity, and maintains high luminescence intensity, resulting in efficient conversion of blue laser light to white light with reduced color unevenness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145860000001_ABST
    Figure 2024145860000001_ABST
Patent Text Reader

Abstract

To provide a phosphor that prevents the leakage of fluorescent light near the side areas of the phosphor.SOLUTION: A phosphor includes crystal particles expressing fluorescent properties, the crystal particle having a D50 of 10-100 μm.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a phosphor and a light-emitting device having the phosphor. [Background technology]

[0002] A part of the blue light, which is the excitation light, is absorbed by the phosphor and undergoes wavelength conversion, resulting in the emission of fluorescence. The fluorescence and the blue light are mixed together, causing the phosphor to emit white light.

[0003] As described in Patent Document 1, yttrium aluminum garnet (abbreviation: YAG, basic chemical composition: Y 3 Al 5 O 12 ) with trivalent cerium (Ce 3+ ) was introduced 3 Al 5 O 12 :Ce 3+ is a phosphor that is used as a phosphor that emits white light using blue light as excitation light.

[0004] Y 3 Al 5 O 12 :Ce 3+ Since single crystal and transparent ceramic phosphors have good thermal conductivity and are resistant to thermal quenching even when strong laser light is incident on them, they are being considered as light sources for spot irradiation using blue laser light as excitation light.

[0005] However, with laser illumination that uses blue laser light as the excitation light, the fluorescence propagates laterally and may be emitted from near the side of the plate-shaped phosphor. For this reason, with laser illumination, the fluorescence emitted from near the side of the phosphor may be concentrated, and a fluorescent ring may be observed around the outer periphery of the projected light.

[0006] In particular, Y 3 Al 5 O 12 :Ce 3+ Single crystal plates and dense Y-type 3 Al 5 O 12 :Ce3+ In elements such as transparent ceramics, the fluorescence tends to propagate horizontally (parallel to the incident surface), so the fluorescence tends to leak out from near the side of the phosphor. For this reason, when such elements are used as phosphors for laser lighting, the excitation light and the fluorescence do not mix sufficiently, and the phenomenon of a fluorescent ring appearing around the outer periphery of the projected light tends to be particularly observed. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] International Publication No. 2021 / 029364 Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present invention is to provide a phosphor capable of suppressing leakage of fluorescence from the vicinity of the side surface of the phosphor. [Means for solving the problem]

[0009] In order to achieve the above object, the phosphor according to the present invention comprises: A phosphor having crystal particles that exhibit fluorescent properties, The crystal grains of the phosphor have a D50 of 10 to 100 μm.

[0010] The phosphor according to the present invention can suppress leakage of fluorescence from the vicinity of the side surface of the phosphor for the following reasons.

[0011] Since the difference in refractive index between the crystal grains and air is large, light is reflected at the interface between the crystal grains and the voids. Therefore, the phosphor according to the present invention has crystal grains with a predetermined D50, so that light is appropriately reflected at the interface between the crystal grains and the voids, the propagation of light toward the side of the phosphor is suppressed, and the light tends to be projected in a direction perpendicular to the incident surface of the phosphor. As a result, it is possible to suppress the leakage of fluorescence from near the side of the phosphor, and to suppress the appearance of ring-shaped fluorescence appearing in the projected light. In other words, in the present invention, the frequency of light reflection at the interface between the crystal grains of the phosphor and the voids is increased, so that it is possible to suppress the leakage of fluorescence from near the side of the phosphor.

[0012] Preferably, the crystal grains are cerium doped Y 3 Al 5 O 12 It is.

[0013] The refractive index of air is 1. Meanwhile, the refractive index of YAG is 1.83 (wavelength 440 nm). Because there is a large difference in the refractive index between YAG and air, 8 to 9% of light is reflected at the interface between the crystal particles and the voids. As a result, more light is reflected at the interface between the crystal particles and the voids, so the propagation of light toward the side of the phosphor is more suppressed, and the light tends to be projected more perpendicularly to the incident surface of the phosphor. As a result, it is possible to further suppress the leakage of fluorescence from near the side of the phosphor.

[0014] Preferably, the density of the phosphor is 3.73 to 4.10 g / cm 3 It is.

[0015] The density of a YAG single crystal is 4.55g / cm 3 Therefore, the density is 3.73 to 4.10 g / cm 3 In this phosphor, 9.9 to 18.0% by volume of voids are present between the crystal grains. When voids are present in the phosphor within the above range, leakage of fluorescence from near the side surfaces of the phosphor can be further suppressed.

[0016] Density 4.10g / cm 3 In the following cases, the density is 4.10 g / cm3 Compared to when the temperature is above 100°C, the formation of a chain of crystal grains in close contact with each other is suppressed, and a moderate amount of voids are formed. This makes it difficult for the fluorescence to propagate laterally through the crystal grains, and it is possible to suppress the leakage of fluorescence from near the sides of the phosphor.

[0017] Density 3.73g / cm 3 If it is more than 3.73g / cm 3 Since the mechanical strength is higher than when the thickness is lower than 100 nm, it is possible to prevent crystal grains from falling off when the phosphor is processed.

[0018] Preferably, the crystalline particles are single crystals.

[0019] This makes it possible to improve the thermal conductivity, and as a result, the temperature quenching resistance characteristics can be improved.

[0020] Preferably, the crystalline particles have the formula Y 3-a Ce a Al 5 O 12 (a is 0.0075 to 0.060).

[0021] By using YAG single crystal particles doped with a high concentration of Ce, with a value of a ranging from 0.0075 to 0.060, it is possible to convert strong blue laser light into white light.

[0022] A method for producing a phosphor according to the present invention includes the steps of: pulverizing a single crystal exhibiting fluorescent properties to obtain crystal particles; and firing the crystal particles at a temperature of 1650 to 1800° C. in an inert gas atmosphere.

[0023] When the firing temperature of the crystal particles in an inert gas atmosphere is 1650°C or higher, the crystal particles are less likely to fall off during processing, and the mechanical strength is higher than when the firing temperature in an inert gas atmosphere is less than 1650°C.

[0024] In addition, when the firing temperature of the crystal particles in the inert gas atmosphere is 1800°C or less, the density is 4.10 g / cm3, compared with the case where the firing temperature of the crystal particles in the inert gas atmosphere is more than 1800°C. 2 Since it is easy to achieve the above, leakage of fluorescence from the vicinity of the side surface of the phosphor can be suppressed.

[0025] That is, by setting the firing temperature in the inert gas atmosphere firing of the crystal particles to 1650 to 1800° C., leakage of light from near the side surfaces of the phosphor can be suppressed, and appropriate mechanical strength can be maintained.

[0026] The light emitting device according to the present invention comprises a blue light emitting element and the phosphor.

[0027] The phosphor of the present invention can suppress leakage of fluorescence from near the sides of the phosphor, and therefore the light emitting device of the present invention can obtain a light source that suppresses color unevenness and is capable of spot projecting white light with high luminous intensity.

[0028] Furthermore, the phosphor can prevent fluorescence from propagating laterally, so that even if a blue laser, which generally tends to cause fluorescence to propagate laterally, is used as a blue light-emitting element, the lateral propagation of fluorescence can be sufficiently suppressed. [Brief description of the drawings]

[0029] [Figure 1] FIG. 1 is a schematic cross-sectional view of a light emitting device according to one embodiment of the present invention. [Diagram 2] FIG. 2 is an enlarged view of part II in FIG. [Diagram 3] FIG. 3 is a backscattered electron image of the surface of a phosphor according to one embodiment of the present invention. [Figure 4] FIG. 4 is a diagram of an apparatus for producing a single crystal that is a material for a phosphor according to one embodiment of the present invention. [Diagram 5] FIG. 5 is a schematic cross-sectional view of a conventional light emitting device. [Figure 6]FIG. 6 is a schematic cross-sectional view of a light emitting device according to another embodiment of the present invention. [Figure 7] FIG. 7 is a diagram of a device for measuring the light quantity ratio. [Figure 8] FIG. 8 is a graph showing the relative emission intensity at each position on a line segment passing through approximately the center of the emission spot diameter. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] [ First embodiment ] < Light-emitting device > As shown in FIG. 1, the light emitting device 2 according to this embodiment is a reflective type light emitting device 2 and includes a phosphor 4 and a blue light emitting element 6. The light emitting device 2 is of a reflective type.

[0031] The reflection-type light-emitting device 2 has the advantage that high brightness can be easily obtained since the reflection surface 44 side can be effectively used for heat dissipation.

[0032] < Blue light emitting element > 1, the blue light emitting element 6 emits blue light LB, which is excitation light for exciting the fluorescent component of the phosphor 4. The blue light LB from the blue light emitting element 6 usually has a peak wavelength of 425 nm to 500 nm. A part of the blue light LB that enters the phosphor 4 from the incident surface 42 is absorbed by the phosphor 4 and undergoes wavelength conversion, resulting in the emission of fluorescence.

[0033] Incidentally, the incident surface 42 of the phosphor 4 is the surface of the phosphor 4 facing the blue light emitting element 6, and in this embodiment, the incident surface 42 is also the exit surface. The reflective surface 44 of the phosphor 4 is the surface on the opposite side of the phosphor 4 from the blue light emitting element 6 side, and faces the incident surface 42. In other words, the incident surface 42 and the reflective surface 44 are substantially parallel. Incidentally, "substantially parallel" means that they may have some portions that are not parallel.

[0034] 2, blue light LB is incident on incident surface 42, and fluorescence LF is emitted in all directions starting from the irradiation position of the blue light LB. A portion of the blue light LB that has not been wavelength-converted undergoes surface scattering at the irradiation position of the blue light LB, and the blue light LB is emitted in all directions starting from the irradiation position of the blue light LB (Lambertian light distribution). The fluorescence LF and blue light LB emitted from the exit surface (incident surface) 42 toward the outside of the phosphor 4 are mixed together to emit white light LW.

[0035] The blue light-emitting element 6 is not particularly limited as long as it can emit blue light LB that can be mixed with the fluorescence LF to emit white light LW and can also be wavelength-converted to the fluorescence LF by the phosphor 4, but examples of the blue light-emitting element 6 include a blue light-emitting diode (blue LED) or a blue semiconductor laser (blue LD).

[0036] < Phosphor > The shape of the phosphor 4 according to this embodiment is not particularly limited, and may be, for example, a disk, a flat plate, or a rectangular column, and has a pair of opposing surfaces that function as an incident surface 42 or a reflecting surface 44 .

[0037] The size of phosphor 4 is not particularly limited. For example, if phosphor 4 has a flat plate shape, the width direction (X0) is 1 to 10 mm, the depth direction is 1 to 10 mm, and the thickness direction (Y0) is 0.03 to 1 mm.

[0038] Figure 3 is a backscattered electron image of the surface of phosphor 4. The white parts in Figure 3 are crystal particles 4a, and the black parts are voids 4b. Phosphor 4 has voids 4b and crystal particles 4a that exhibit fluorescent properties. The multiple crystal particles 4a that make up phosphor 4 are fused and joined to each other.

[0039] The crystal grains 4a have a D50 of 10 to 100 μm, and preferably 40 to 80 μm.

[0040] Here, D50 is the particle size of particles having a cumulative frequency of 50%, counting from the smallest particle size.

[0041] The density of the phosphor 4 is preferably 3.73 to 4.10 g / cm 3 and more preferably 3.78 to 3.96 g / cm 3 The method for adjusting the density is not particularly limited, but examples thereof include adjusting the D50 of the crystal particles 4a and adjusting the firing temperature in the inert gas atmosphere firing described below. When the firing temperature in the inert gas atmosphere firing is increased, the density tends to increase.

[0042] The volume ratio of the voids 4b formed between the crystal grains 4a of the phosphor 4 to the volume of the phosphor 4 is preferably 9.9 to 18.0% by volume, and more preferably 13.0 to 17.0% by volume.

[0043] The crystalline state of the crystal particles 4a is not particularly limited, and may be a single crystal or a transparent ceramic, but is preferably a single crystal.

[0044] The composition of the crystal grains 4a is not particularly limited, but preferably, the main component is A. x B y O z where x is 2.7 to 3.3, y is 4.7 to 5.3, and z is 11.7 to 12.3. Here, the "main component" refers to a component that does not contain an activator, which will be described later.

[0045] Moreover, the element A is preferably at least one selected from the group consisting of yttrium (Y), gadolinium (Gd), terbium (Tb), ytterbium (Yb) and lutetium (Lu), and the element A is more preferably Y.

[0046] The element B is preferably at least one selected from the group consisting of aluminum (Al), gallium (Ga) and scandium (Sc), and the element B is more preferably Al.

[0047] The activator is preferably at least one selected from the group consisting of lanthanide elements and actinide elements, and more preferably at least one selected from the group consisting of cerium (Ce), neodymium (Nd) and gadolinium (Gd).

[0048] When the total content of the main component element A and the activator element is taken as 100 parts by mol, the content of the activator element is preferably 0.25 to 2.0 parts by mol.

[0049] The crystal particle 4a according to this embodiment is represented by the chemical formula Y 3-a Ce a Al 5 O 12 It is preferable that the composition is as follows: Here, a is preferably 0.0075 to 0.060, and more preferably 0.015 to 0.045.

[0050] Since the blue laser light LB is concentrated locally, with conventional phosphors, the amount of fluorescent light LF may be insufficient, causing the projected light to become bluish white light.

[0051] In contrast, when a is 0.0075 or more, even if strong blue laser light LB of, for example, 1 W or more is used as excitation light, the amount of fluorescent light LF is not insufficient, and the projected light can be turned into white light LW.

[0052] In addition, by setting a to 0.060 or less, concentration quenching can be prevented, the fluorescent light LF can be easily emitted, and the projected light can be made into white light. In other words, the projected light can be prevented from becoming bluish white light.

[0053] In summary, by using phosphor 4 in which crystal particles 4a to which a high concentration of activator, with a being 0.0075 to 0.060, is added, it becomes easier to convert strong blue laser light into white light.

[0054] The YAG:Ce, LuAG:Ce and GAGG:Ce constituting the crystal particle 4a have the same garnet composition and have very close refractive indices. Specifically, the refractive index of YAG:Ce is 1.82, the refractive index of LuAG:Ce is 1.84, and the refractive index of GAGG:Ce is 1.90. Therefore, when YAG:Ce, LuAG:Ce or GAGG:Ce is used as the material of the crystal particle 4a according to this embodiment, it is considered that the same behavior is exhibited and the same effect is obtained.

[0055] The concentration of each component in the crystal particles 4a can be measured by laser ablation inductively coupled plasma mass spectrometry (LA-ICP-MS), an electron probe microanalyzer (EPMA), an energy dispersive spectrometer (EDX), or the like.

[0056] < Phosphor manufacturing method > The phosphor 4 according to this embodiment is not particularly limited, but can be obtained, for example, by the following method. First, a single crystal is obtained, and the single crystal is pulverized to obtain a pulverized material. Next, the pulverized material is molded to obtain a molded body, and the molded body is fired to obtain a fired body. Thereafter, the fired body is polished and cut to obtain the phosphor 4 according to this embodiment (resintered phosphor 4). Specifically, the method is as follows.

[0057] The method for obtaining a single crystal is not particularly limited, and it can be obtained by, for example, the micro-pulling down method (μ-PD method), the Czochralski method (CZ method), the Bridgman method, or the Edge-defined Film-fed Growth method (EFG method).

[0058] The μ-PD method makes it easier to increase the concentration of the activator in the single crystal compared to the conventional CZ method, and therefore makes it easier to make the projected light white. In addition, the μ-PD method can ease the concentration distribution of the activator, making it difficult for concentration quenching to occur, and therefore makes it easier to make the projected light white. For this reason, it is preferable to obtain the phosphor 4 according to this embodiment using a single crystal produced by the μ-PD method.

[0059] 4 shows a schematic cross-sectional view of a single crystal manufacturing apparatus 22 using the μ-PD method. The μ-PD method is a melting and solidification method in which a crucible 24 containing a sample is heated directly or indirectly to obtain a melt of the target substance in the crucible 24, a seed crystal 34 placed below the crucible 24 is brought into contact with the opening at the bottom end of the crucible 24, and a solid-liquid interface is formed there while the seed crystal 34 is pulled down, thereby growing a single crystal.

[0060] 4, single crystal production apparatus 22 for producing phosphor 4 according to this embodiment includes crucible 24 installed with its opening facing downward and refractory furnace 26 surrounding it. Refractory furnace 26 is further covered with quartz tube 28, and induction heating coil 30 for heating crucible 24 is installed near the center of quartz tube 28 in the vertical direction.

[0061] A seed crystal 34 held by a seed crystal holding jig 32 is placed at the opening of the crucible 24. An after-heater 36 is placed near the opening of the crucible 4 to prevent rapid cooling.

[0062] The seed crystal 34 is a rod-shaped single crystal. The seed crystal 34 is the above-mentioned A x B y O z A single crystal having the composition is preferred.

[0063] Next, a method for producing the phosphor 4 according to this embodiment will be specifically described.

[0064] First, the raw materials for the single crystal, element A, element B, and an activator, are placed in the crucible 24 in the refractory furnace 26, and the inside of the furnace is heated with H 2 +N 2 , N 2 Alternatively, it is replaced with a gas such as argon (Ar).

[0065] Next, inert gas is pumped at 10 to 100 cm 3 1 / min, the crucible 24 is heated by an induction heating coil (high frequency coil for heating) 30 to melt the raw materials and obtain a molten liquid.

[0066] When the raw material is sufficiently melted, a seed crystal 34 is gradually brought closer from the bottom of the crucible until it comes into contact with the opening at the bottom of the crucible 24. When the melt comes out of the opening at the bottom of the crucible 24, the seed crystal 34 is lowered to start crystal growth. The speed at which the seed crystal 34 is lowered here is called the growth speed.

[0067] The growth rate and temperature can be controlled manually while observing the state of the solid-liquid interface with a CCD camera or a thermo camera.

[0068] The temperature gradient can be selected in the range of 10 to 100° C. / mm by moving the induction heating coil 30. The single crystal growth speed can also be selected in the range of 0.01 to 0.20 mm / min.

[0069] The seed crystal 34 is lowered until the melt in the crucible 24 stops flowing out, and after the seed crystal 34 is separated from the crucible 24, the single crystal is cooled so as not to crack. The cooling rate of the single crystal varies depending on the growth rate and can be selected, for example, within the range of 70 to 300°C / hour.

[0070] In this way, the activator-doped A x B y O z Obtain a single crystal (phosphor).

[0071] The resulting single crystal is then pulverized to obtain a pulverized product. The pulverized product is then classified, for example, using a metal mesh. The mesh size can be adjusted by changing the mesh size used. The pulverized product that does not pass through the mesh is pulverized again and classified.

[0072] The classified pulverized material is hydraulically pressed into a die, and then molded by cold isostatic pressing (CIP) to obtain a green body.

[0073] The obtained molded body is first subjected to inert gas atmosphere firing in an inert gas atmosphere, and then subjected to air firing in air to obtain a fired body. The fired body is cut to a predetermined size to obtain the phosphor 4 according to this embodiment.

[0074] The firing furnace used for firing in an inert gas atmosphere is not particularly limited, but for example, a carbon furnace can be used.

[0075] The conditions for the inert gas atmosphere firing are not particularly limited, but may be, for example, as follows.

[0076] Firing temperature: 1650~1800℃ Firing atmosphere: Ar Baking time: 1 to 10 hours

[0077] The firing furnace used for firing in air is not particularly limited, but for example, an electric furnace can be used.

[0078] The conditions for the calcination in air are not particularly limited, but may be, for example, as follows.

[0079] Firing temperature: 1400~1700℃ Atmosphere: Air

[0080] The surface of the obtained fired body corresponding to the incident surface 42 and the surface corresponding to the reflecting surface 44 are polished, and then cut to a predetermined size to obtain the phosphor 4 according to this embodiment.

[0081] Conventional single crystal phosphors and transparent ceramic phosphors have a dense structure without voids. The transparent ceramic phosphor is a phosphor obtained by firing raw oxide powder.

[0082] For this reason, in the case of a single crystal phosphor or a transparent ceramic phosphor, the fluorescence LF radiated toward the phosphor 4 side by the Lambertian light distribution becomes an internal waveguiding that repeats total reflection at the reflecting surface 44 and the incident surface 42, as shown in Fig. 5. As a result, the fluorescence LF may be emitted toward the outside of the phosphor 4 from the incident surface 42, the reflecting surface 44, or the side surface 46 at a position away from the irradiation position. In other words, the fluorescence LF may leak from near the side surface 46 of the phosphor 4.

[0083] When the fluorescent light LF is emitted from a position away from the irradiation position, it can cause the diameter of the light emission spot to increase, or a ring-shaped fluorescent light (yellow ring) can appear, causing color unevenness or reduced brightness.

[0084] Furthermore, since conventional phosphor 4 has a dense structure with substantially no voids, when the angle of incidence of the fluorescence LF approaches the critical angle and the refraction angle of the fluorescence LF approaches 90 degrees, the fluorescence LF travels straight and parallel to the surface of phosphor 4, making it difficult to extract the fluorescence LF from phosphor 4.

[0085] In contrast, according to the phosphor 4 of this embodiment, it is possible to suppress the leakage of the fluorescence LF from the vicinity of the side surface 46 of the phosphor 4. The reasons for this are considered to be as follows. The phosphor 4 of this embodiment is composed of crystal particles 4a having a predetermined average particle size. Since the difference in refractive index between the crystal particles 4a and air is large, light is reflected at the interface between the crystal particles 4a and the voids. Therefore, in the phosphor 4 of this embodiment, light is appropriately reflected at the interface between the crystal particles 4a and the voids 4b. In other words, in this embodiment, the frequency of light reflection on the surface or inside of the phosphor 4 can be increased. Therefore, the propagation of the fluorescence LF toward the side surface 46 of the phosphor 4 due to the internal waveguiding is suppressed, and the propagation of the fluorescence LF toward the side surface 46 due to the refraction angle being approximately 90 degrees is suppressed.

[0086] This tends to project the light in a direction perpendicular to the incident surface 42 of the phosphor 4. As a result, it is possible to suppress leakage of the fluorescence LF from the vicinity of the side surface 46 of the phosphor 4, and to suppress the appearance of ring-shaped fluorescence LF in the projected light, and in addition, it is possible to narrow the emission spot diameter of the fluorescence LF and increase the efficiency of extracting light from the exit surface 42 side, thereby increasing the brightness.

[0087] In addition, in conventional single crystal phosphors or transparent ceramic phosphors, not only the fluorescent light LF but also the blue light LB may propagate toward the side surface 46 of the phosphor 4 due to the internal waveguiding and the propagation toward the side surface 46 due to the refraction angle being approximately 90 degrees. In contrast, according to the present embodiment, the blue light LB is also appropriately reflected at the interface between the crystal grains 4a and the voids 4b, so that the propagation of the blue light LB toward the side surface 46 of the phosphor 4 due to the internal waveguiding and the propagation toward the side surface 46 due to the refraction angle being approximately 90 degrees can be suppressed. As a result, the deterioration of the structure disposed outside the side surface 46 of the phosphor 4 due to the blue light LB can be suppressed.

[0088] Furthermore, since the crystal particles 4a of the phosphor 4 according to this embodiment are single crystals, the phosphor 4 according to this embodiment has higher crystallinity than a transparent ceramic phosphor, resulting in better thermal conductivity.

[0089] Furthermore, in transparent ceramic phosphors, a layer of a different material from the particles may be formed between the particles, and the layer of the different material may reduce thermal conductivity. On the other hand, in the phosphor 4 according to this embodiment, a layer of a different material is not substantially formed, and therefore the thermal conductivity can be improved.

[0090] The phosphor 4 according to this embodiment has good thermal conductivity and therefore good temperature quenching resistance.

[0091] [ Second embodiment ] The light emitting device according to this embodiment is similar to the light emitting device 2 of the first embodiment, except as described below.

[0092] As shown in FIG. 6, a light emitting device 2a according to this embodiment is of a transmissive type.

[0093] In this embodiment, the emission surface 48 of the phosphor 4 is the surface of the phosphor 4 opposite to the blue light emitting element 6 side, and faces the incidence surface 42. In other words, the incidence surface 42 and the emission surface 48 are substantially parallel. Note that "substantially parallel" means that they may have some portions that are not parallel.

[0094] Blue light LB is incident on the incident surface 42, and the fluorescent light LF emitted from the exit surface 48 toward the outside of the phosphor 4 and the blue light LB are mixed together to emit white light LW.

[0095] The present invention is not limited to the above-described embodiment, and various modifications can be made within the scope of the present invention. EXAMPLES

[0096] The present invention will be described in more detail below by way of examples of the present invention, but the present invention is not limited to these examples.

[0097] < Examples 1 to 8 > Single crystals were obtained by the μ-PD method. 2 O 3 , Al 2 O 3 , CEO 2 YO was then placed in an Ir crucible 24 with an inner diameter of 16 mm. 1.5 , AlO 1.5 and CeO 2 Y is adjusted to have the composition ratio shown in Table 1. 2 O 3 , Al 2 O 3 and CeO 2 2g was added.

[0098] The crucible 24 used had a shape in which the melt leakage port was located in the center.

[0099] The crucible 24 containing the starting materials was placed in a refractory furnace 26. The atmosphere in the refractory furnace 26 was kept at 3% H 2 N added 2 and then, while maintaining normal pressure, 3 The gas flow was performed at a flow rate of 1 / min.

[0100] Thereafter, heating of the crucible 24 was started and gradually heated over one hour until the temperature reached the melting point of the YAG single crystal.

[0101] A YAG single crystal was used as the seed crystal 34, and the tip of the seed crystal 34 was brought into contact with the opening at the bottom of the crucible 24. After confirming that the melt had come out of the opening, crystal growth was started while lowering the seed crystal 34. At this time, the growth speed was changed within the range of 0.01 to 0.20 mm / min for each sample to grow the crystal.

[0102] During crystal growth, an after-heater 36 was installed below the crucible 24 in order to prevent rapid cooling.

[0103] The cooling rate of the crystal varies depending on the growth rate, and in this example was adjusted to be 70 to 300° C. / hour.

[0104] As a result of growing a single crystal, a columnar Y with a size of 5×5 mm and a length of 65 mm was obtained. 3 Al 5 O 12 :Ce 3+ A single crystal (phosphor) was obtained.

[0105] In addition, the crystal peaks of phosphor 4 were confirmed by X-ray diffraction (XRD) using a fully automated multipurpose X-ray diffraction device SmartLab (manufactured by Rigaku Corporation), and if no heterophase components were contained and a (100) diffraction spot was confirmed with three-fold rotational symmetry by pole measurement at (100), it was determined to be a single crystal. As a result, it was confirmed that single crystals were generated in Examples 1 to 8.

[0106] The obtained single crystal was crushed with a mortar and pestle to obtain a crushed product, which was then classified using a metal mesh with the openings shown in Table 1. The crushed product that did not pass through the mesh was crushed again and classified.

[0107] The classified pulverized material was hydraulically pressed into a mold and then molded by the CIP method to obtain a 10 mm diameter × 10 mm thick molded body.

[0108] The obtained molded body was first sintered in an inert gas atmosphere, and then sintered in air to obtain a sintered body.

[0109] The firing in an inert gas atmosphere was carried out using a carbon furnace under the following conditions. Firing temperature: See Table 1 Firing atmosphere: Ar Baking time: 4 hours

[0110] The calcination in air was carried out using an electric furnace under the following conditions. Firing temperature: 1500℃ Firing atmosphere: in air

[0111] The surfaces corresponding to the incident surface 42 and the reflecting surface 44 of the obtained fired body were polished so that the thickness was 0.5 mm, and the fired body was then cut into 5.0 mm squares with a dicer to produce phosphor 4 having a shape of 5.0 x 5.0 x 0.5 mm.

[0112] ( Average particle size ) The polished surface of phosphor 4 was observed with a field emission scanning electron microscope SU8200 (manufactured by Hitachi High-Technologies Corporation), and the average particle size (median diameter: D50) was obtained from the SEM image. The measurement mode was backscattered electron (BSE) imaging, the magnification was 400 times, and the number of particles measured for averaging was 500. The results are shown in Table 1.

[0113] ( Composition analysis ) The composition of phosphor 4 was analyzed using a fluorescent X-ray analyzer ZSX100e (manufactured by Rigaku Corporation). 1.5, AlO 1.5 and CeO 2 The composition in terms of molar ratio (mol%) is shown in Table 1. 3-a Ce a Al 5 O 12 The value of a in the formula Y 2.9925 Ce 0.0075 Al 5.0000 O 12 It was confirmed that the composition was

[0114] ( Light amount ratio ) Blue laser light LB was incident on phosphor 4 from directly above, and the intensity of the light projected from phosphor 4 was measured by sensor 134 directly above phosphor 4. The position of sensor 134 was moved linearly from the center (central) of phosphor 4 to side surface 46 (periphery), and the ratio (light amount ratio) of "the amount of light measured near the periphery of phosphor 4" to "the amount of light measured near the center of phosphor 4" was calculated. The results are shown in Table 1. Here, "the amount of light measured near the periphery of phosphor 4" means "the amount of light leaking from near the side surface 46 of phosphor 4."

[0115] The light quantity of phosphor 4 was measured using the device shown in Fig. 7. Specifically, first, blue laser light LB emitted from blue laser light source 6 was reflected by dichroic mirror 132 and made to enter phosphor 4. Next, the blue laser light LB that entered phosphor 4 was converted to fluorescence LF. The fluorescence LF was reflected by mirror 131 installed inside phosphor 4 or on the outside of phosphor 4 on the reflection surface 44 side, and thus the fluorescence LF was emitted from the entrance surface 42 (exit surface) of phosphor LF toward dichroic mirror 132. Since dichroic mirror 132 transmits only the fluorescence LF and does not transmit the blue laser light LB, sensor 134 can detect only the fluorescence LF.

[0116] In Example 1, the light amount ratio was 0. That is, in Example 1, the position of the sensor 134 was moved linearly from the center (center) of the phosphor 4 to the side surface 46 (periphery) to measure the amount of light leaking from near the side surface 46 of the phosphor 4, but there was no light leakage. In other words, it was confirmed that in Example 1, the appearance of the ring-shaped fluorescence LF can be suppressed.

[0117] ( density ) The weight of Phosphor 4 was measured using a balance, and the volume was determined by Archimedes' method to calculate the specific gravity of Phosphor 4. The results are shown in Table 1.

[0118] ( Projected light color ) A blue laser beam with an output of 1 W was incident on the phosphor at an incident angle of 45°, and the temperature of the light projected perpendicularly from the laser beam projection surface of the phosphor was measured with a color temperature meter. In Example 1, the light was white light with a color temperature of 4000 K, and in Examples 2 to 8, the projected light was also white light.

[0119] ( Thermal Conductivity ) The thermal diffusivity and specific heat of phosphor 4 were measured using a xenon flash method thermal diffusivity measuring device TD-1 (manufactured by Advance Riko Co., Ltd.) under the following measurement conditions. Temperature (degC): Room temperature Pulse Width:Long Sensitivity: Low DAQ voltage:5 Sampling Period(ms):0.05 The thermal conductivity was calculated from the thermal diffusivity, specific heat, and density obtained above. The results are shown in Table 1.

[0120] [Table 1]

[0121] < Example 9 > In Example 9, phosphor 4 was produced and evaluated in the same manner as in Examples 1 to 8, except that the material composition was as shown in Table 1. The results are shown in Table 1. It was confirmed that a single crystal was also obtained by the μ-PD method in Example 9.

[0122] The composition of phosphor 4 of Example 9 was analyzed by fluorescent X-ray analysis, and found to be of the chemical formula Y 2.9950 Ce 0.0050 Al 5.0000 O 12 The composition was as follows.

[0123] The color of the projected light from Phosphor 4 in Example 9 was bluish white light, and white light was not obtained.

[0124] < Example 10 > In Example 10, phosphor 4 was produced and evaluated in the same manner as in Examples 1 to 8, except that the material composition was as shown in Table 1. The results are shown in Table 1. It was confirmed that a single crystal was also obtained in Example 10 by the μ-PD method.

[0125] The composition of phosphor 4 of Example 10 was analyzed by fluorescent X-ray analysis, and found to be of the chemical formula Y 2.9380 Ce 0.0620 Al 5.0000 O 12 The composition was as follows.

[0126] The color of the projected light from phosphor 4 in Example 10 was bluish white light, and white light was not obtained. This is thought to be because the concentration of Ce in Example 10 was too high, and the amount of fluorescence LF was reduced due to concentration quenching.

[0127] < Comparative Example 1 > In Comparative Example 1, a single crystal was produced and evaluated in the same manner as in Examples 1 to 8, except that the material composition was as shown in Table 1. The results are shown in Table 1. That is, in Comparative Example 1, only single crystal phosphor 4 was produced, and subsequent crushing, molding, and firing were not carried out.

[0128] In Comparative Example 1, the obtained columnar single crystal was cut with a wire saw to a thickness of 1 mm to obtain a single crystal plate of 5 mm square. The surface corresponding to the incident surface 42 and the surface corresponding to the reflecting surface 44 of the single crystal plate were polished so that the thickness of the single crystal plate was 0.5 mm, and a single crystal phosphor having a shape of 5.0 × 5.0 × 0.5 mm was produced.

[0129] The composition of phosphor 4 of Comparative Example 1 was analyzed by fluorescent X-ray analysis, and found to be of the chemical formula Y 2.9925 Ce 0.0075 Al 5.0000 O 12 The composition was as follows.

[0130] The light amount ratio was 0.47 in Comparative Example 1. In Comparative Example 1, it was confirmed that the fluorescent light LF propagated laterally and leaked from the vicinity of the side surface 46.

[0131] < Comparative Example 2 > In Comparative Example 2, Y was used as the starting material. 2 O 3 , Al 2 O 3 , CEO 2 Prepare the powder and 1.5 , AlO 1.5 and CeO 2 In the same manner as in Examples 1 to 8, except that the raw material powder was prepared by mixing the above in a ball mill so as to have the composition ratio shown in Table 1, the raw material powder was hydraulically pressed, and then molded by a CIP method to obtain a molded body of 10 mmΦ×10 mm thickness, the molded body was fired in an inert gas atmosphere and then fired in air to obtain a fired body, which was polished and cut to obtain phosphor 4, and phosphor 4 was evaluated. The results are shown in Table 1. That is, in Comparative Example 2, a ceramic phosphor was used.

[0132] The composition of phosphor 4 of Comparative Example 2 was analyzed by fluorescent X-ray analysis, and found to be of the chemical formula Y 2.9925 Ce 0.0075 Al 5.0000 O 12 It was confirmed that the composition was

[0133] The light amount ratio in Comparative Example 2 was 0.13, and light leakage from the side surfaces was observed.

[0134] < Comparative Example 3 > In Comparative Example 3, phosphor 4 was produced and evaluated in the same manner as in Examples 1 to 8, except that a mesh with the openings shown in Table 1 was used. The results are shown in Table 1.

[0135] The light amount ratio in Comparative Example 3 was 0.24, and light leakage from the side surfaces was observed.

[0136] < Comparative Example 4 > In Comparative Example 4, an attempt was made to produce phosphor 4 in the same manner as in Examples 1 to 8, except that a mesh with the openings shown in Table 1 was used. However, in Comparative Example 4, a molded body could not be produced by hydraulic die pressing. This is thought to be because the grain size of the pulverized material was too coarse, making it impossible to produce a molded body.

[0137] < Comparative Example 5 > In Comparative Example 5, phosphor 4 was produced and evaluated in the same manner as in Examples 1 to 8, except that the firing temperature in the inert gas atmosphere was set to 1820° C. The results are shown in Table 1.

[0138] The light amount ratio in Comparative Example 5 was 0.16, and light leakage from the side surfaces was observed.

[0139] < Comparative Example 6 > In Comparative Example 6, the firing temperature in the inert gas atmosphere firing was set to 1630°C, and other methods were used to produce phosphor 4 in the same manner as in Examples 1 to 8. However, in Comparative Example 6, when the fired phosphor 4 was polished, the crystal particles 4a fell off from the surface, and it was not possible to process it into phosphor 4. This is thought to be because the firing temperature in the inert gas atmosphere firing was too low, and therefore the crystal particles 4a were not sufficiently fused to each other.

[0140] 8 shows the relative emission intensity at each position on a line segment passing through approximately the center of the emission spot diameter for Example 1 and Comparative Example 2. The center of the emission spot diameter on the line segment is set as 0, and the horizontal axis (X) represents the length [μm] to each measurement point, while the vertical axis (Y) represents the emission intensity at each measurement point. The emission intensity is a relative value (%) when the peak value of the fluorescence intensity in Example 1 is set as 100%. Example 1 is shown by a solid line, and Comparative Example 2 is shown by a dashed line.

[0141] 8, it was confirmed that Example 1 had a higher emission intensity than Comparative Example 2. [Explanation of symbols]

[0142] 2. Light emitting device 4. Phosphor 4a…Crystalline particles 4b... void 42…Incidence plane 44… Reflective surface 46… Side 48… Exit surface 6... Blue light emitting element, blue laser light source 8…Reflection layer 22... Single crystal manufacturing equipment 24… Crucible 26… Refractory furnace 28…Quartz tube 30… Induction heating coil 32… Seed crystal holding jig 34… Seed crystal 36... After heater 131…Mirror 132…Dichroic mirror 134…CCD camera LB: Excitation light, blue light, blue laser light LF: Fluorescence LW…white light

Claims

1. A phosphor having crystal particles that exhibit fluorescent properties, The crystal grains of the phosphor have a D50 of 10 to 100 μm.

2. The crystal grains are Y doped with cerium. 3 A 5 O 12 The phosphor according to claim 1 ,

3. The density of the phosphor is 3.73 to 4.10 g / cm 3 The phosphor according to claim 1 ,

4. The phosphor according to claim 1 , wherein the crystal grains are single crystals.

5. The crystal particles are represented by the chemical formula Y 3-a C.E. a A 5 O 12 2. The phosphor according to claim 1, having a composition of (a is 0.0075 to 0.060).

6. A step of crushing the single crystal exhibiting fluorescent properties to obtain crystal particles; and firing the crystal particles at a temperature of 1650 to 1800° C. in an inert gas atmosphere.

7. A light emitting device comprising: a blue light emitting element; and the phosphor according to claim 1.

Citation Information

Patent Citations

  • Wavelength conversion member

    WO2021029364A1