Water-based coating material composition and method for manufacturing coating film
A water-based paint composition using core-shell and single-layer acrylic resin emulsions with specific glass transition temperatures and additives achieves a dry, corrosion-resistant, and blocking-resistant coating film at room temperature, addressing the limitations of conventional paints.
Patent Information
- Application Number
- JP2023058420
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Conventional water-based paint compositions form films that are not sufficiently dry to the touch at room temperature, lacking good appearance, corrosion resistance, and blocking resistance, especially when applied in one coat.
A water-based paint composition containing a combination of core-shell and single-layer acrylic resin emulsions with specific glass transition temperatures, anti-rust pigments, and resin beads, applied after preheating to 60-110°C, to form a coating film with improved dryness, appearance, corrosion resistance, and blocking resistance.
The composition achieves a coating film that is dry to the touch within minutes at room temperature, with excellent appearance, corrosion resistance, and blocking resistance, meeting industry standards like JIS K 5674.
Smart Images

Figure 2024145872000001 
Figure 2024145872000002 
Figure 2024145872000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an aqueous coating composition and a method for producing a coating film. [Background technology]
[0002] 2. Description of the Related Art In various fields, such as building exteriors, building materials, bridges, ships, vehicles, industrial machinery, construction machinery, and automobiles, coating films are formed on the surfaces of the substrates using coating compositions in order to protect and beautify the substrates.
[0003] In recent years, as environmental problems have become more serious, there has been a demand for reducing the environmental load in the paint field, and various studies have been conducted. One of the important issues in the paint field is the reduction of the amount of organic solvent used. From this perspective, water-based paints are used as paints with reduced organic solvents, and their use is expanding in various fields. Among these, steel materials are used for building materials, civil engineering materials, and machine applications, and coating films with good corrosion resistance are required to withstand long-term use in outdoor environments.
[0004] In a manufacturing line for light-gauge steel among steel materials, a process is generally carried out in which the formed steel material is degreased, the steel material is preheated at a temperature of about 60 to 110° C., and the preheated steel material is airless-painted with an aqueous coating composition. The coated steel material is then bundled, stacked, and transported.
[0005] Since the above series of steps is carried out in a short time of about 5 minutes, the aqueous paint composition is required to dry quickly, and the resulting coating film is required to have a good finished appearance, blocking resistance, crack resistance, etc. In particular, to satisfy the standard of JIS K 5674 (lead-chromium-free rust-preventive paint), a film thickness of 30 μm or more is required, and blocking resistance and crack resistance are significant issues. In addition, in the case of industrial products, low cost is extremely important for expanding the market for the product.
[0006] Patent Document 1 describes an aqueous paint that contains an acrylic resin emulsion and an acrylic resin dispersion having a glass transition temperature (Tg) of 28 to 50°C in a solid content of 1 to 5 mass%, contains a film-forming auxiliary in an amount of 1 to 5 mass%, and has a minimum film-forming temperature of 25 to 45°C. Patent Document 2 describes an aqueous coating composition that contains urethane resin particles having a weight-average molecular weight of 100,000 to 5,000,000 and a glass transition temperature of 30 to 100°C and acrylic resin particles having a glass transition temperature of -20 to 30°C, in which the solid content of the urethane resin particles and the acrylic resin particles relative to the total solid content is 40 to 80 mass% for the urethane resin particles and 20 to 60 mass% for the acrylic resin particles. Patent Document 3 describes a resin composition for aqueous paints that contains a binder composed of two types of heterogeneous emulsion particles, and describes that in one of the heterogeneous emulsion particles, the emulsion polymer that forms the outermost phase has a glass transition temperature of -50 to 10°C and the emulsion polymer that forms at least one phase inside the outermost phase has a glass transition temperature of 30 to 110°C, and that in the other, the emulsion polymer that forms the outermost phase has a glass transition temperature of 60 to 80°C and the emulsion polymer that forms at least one phase inside the outermost phase has a glass transition temperature of -50 to 0°C. Patent Document 4 describes an emulsion paint for bitumen-based vibration-damping sheets, the main component of which is a synthetic resin emulsion containing a styrene / acrylic copolymer synthetic resin emulsion with a minimum film-forming temperature of 80 to 100°C and an acrylic ester copolymer synthetic resin emulsion with a minimum film-forming temperature of 20°C or less in a mass ratio of 2 to 4:8 to 6. Patent Document 5 describes an aqueous resin dispersion comprising a high-Tg resin component having a glass transition temperature (Tg) of 50°C or higher, which is obtained by polymerizing two or more types of polymerizable monomers having different glass transition temperatures (Tg), and a low-Tg resin component having a glass transition temperature of 40°C or lower, and further describes that the minimum film formation temperature (MFT) of the aqueous resin dispersion is 10°C or higher lower than the glass transition temperature (Tg) of the entire aqueous resin dispersion. Patent Document 6 describes that in a coating composition containing water, an organic solvent, a pigment, and a resin, the pigment volume concentration (PVC) is within the range of 0.1 to 35%, and the resin has at least one loss tangent (tan δ) peak that is within the range of 45°C to 180°C. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2020-002330 A [Patent Document 2] JP 2020-002327 A [Patent Document 3] JP 2003-128981 A [Patent Document 4] Japanese Patent Application Publication No. 09-087572 [Patent Document 5] JP 2008-063567 A [Patent Document 6] JP 2022-154462 A Summary of the Invention [Problem to be solved by the invention]
[0008] However, conventionally known aqueous coating compositions, when used to form a coating film in a single application and then dried at room temperature, were not fully satisfactory in terms of touch dryness, appearance, corrosion resistance, or blocking resistance of the resulting coating film.
[0009] The present disclosure aims to provide an aqueous coating composition which forms a coating film in a single application, has good tactile dryness even when dried at room temperature, and provides a coating film with good appearance, corrosion resistance, and blocking resistance. [Means for solving the problem]
[0010] [1] The coating composition includes a film-forming resin (A), an anti-rust pigment (B) and resin beads (C), the coating film-forming resin (A) comprises an acrylic resin emulsion (A1) and an acrylic resin emulsion (A2); The acrylic resin emulsion (A1) contains a core-shell type acrylic resin emulsion having a core portion and a shell portion, The acrylic resin emulsion (A2) contains a single-layer type acrylic resin emulsion, the glass transition temperature of the entire acrylic resin of the acrylic resin emulsion (A1) is 30° C. or higher and 50° C. or lower; the glass transition temperature of the entire acrylic resin of the acrylic resin emulsion (A2) is -20°C or higher and 0°C or lower; Water-based paint composition. [2] The aqueous coating composition according to [1], wherein the glass transition temperature of the shell part of the core-shell type acrylic resin emulsion is higher than the glass transition temperature of the core part of the core-shell type acrylic resin emulsion. [3] The aqueous coating composition according to [1] or [2], wherein the ratio of the solid content of the acrylic resin emulsion (A1) to the solid content of the acrylic resin emulsion (A2) is 90:10 to 50:50. [4] The aqueous coating composition according to any one of [1] to [3], wherein the content of the anti-rust pigment (B) is 1 part by mass or more and 50 parts by mass or less per 100 parts by mass of the solid content of the coating film-forming resin (A). [5] The aqueous coating composition according to any one of [1] to [4], wherein the resin beads (C) have an average particle size of 1 μm or more. [6] The aqueous coating composition according to any one of [1] to [5], wherein the content of the resin beads (C) is 1 part by mass or more and 30 parts by mass or less per 100 parts by mass of the solid content of the coating film-forming resin (A). [7] The aqueous coating composition according to any one of [1] to [6], further comprising a film-forming auxiliary (D), the content of which is from 1 to 40 parts by mass per 100 parts by mass of the solid content of the coating film-forming resin (A). [8] Preheat the workpiece to between 60℃ and 110℃. applying the aqueous coating composition according to any one of [1] to [7] to the surface of the substrate after the preheating, to form a coating film. Effect of the Invention
[0011] The aqueous coating composition of the present disclosure forms a coating film in a single application, and even when dried at room temperature, the coating film has good dryness to the touch, and the appearance, corrosion resistance, and blocking resistance of the resulting coating film are good. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The aqueous coating composition of the present disclosure comprises: The coating composition includes a film-forming resin (A), an anti-rust pigment (B) and resin beads (C), the coating film-forming resin (A) comprises an acrylic resin emulsion (A1) and an acrylic resin emulsion (A2); The acrylic resin emulsion (A1) contains a core-shell type acrylic resin emulsion having a core portion and a shell portion, The acrylic resin emulsion (A2) contains a single-layer type acrylic resin emulsion, the glass transition temperature of the entire acrylic resin of the acrylic resin emulsion (A1) is 30° C. or higher and 50° C. or lower; The glass transition temperature of the entire acrylic resin of the acrylic resin emulsion (A2) is -20°C or higher and 0°C or lower.
[0013] The aqueous coating composition of the present disclosure forms a coating film in a single application, and even when dried at room temperature, the coating film has good dryness to the touch, and the appearance, corrosion resistance, and blocking resistance of the resulting coating film are good.
[0014] Although the present disclosure should not be interpreted as being limited to a particular theory, the reason why the aqueous coating composition of the present disclosure exhibits such an effect is considered to be as follows. That is, the aqueous coating composition of the present disclosure contains two types of acrylic resin emulsions as a coating film-forming resin, one of the acrylic resin emulsions (A1) contains a core-shell type acrylic resin emulsion, and the glass transition temperature of the entire acrylic resin of the acrylic resin emulsion (A1) is 30°C or higher and 50°C or lower. This allows the aqueous coating composition to have good film-forming properties when applied, and the blocking resistance of the resulting coating film can be good. In addition, the glass transition temperature of the entire acrylic resin of the other acrylic resin emulsion (A2) is -20°C or higher and 0°C or lower. Therefore, it is considered that the touch dryness is good and the film-forming properties can be good even when the aqueous coating composition is applied once to form a coating film and dried at room temperature. Furthermore, since the aqueous coating composition of the present disclosure contains both the acrylic resin emulsion (A1) and the acrylic resin emulsion (A2), even if it contains an anti-rust pigment and resin beads, it can suppress cracks in the resulting coating film and has a good appearance. Therefore, it is considered that the resin beads can exhibit the effect of improving blocking resistance, and the anti-rust pigment can exhibit the effect of improving corrosion resistance. As a result, it is considered that an aqueous coating composition can be provided that has good tactile dryness even when a coating film is formed by one coating and dried at room temperature, and the resulting coating film has good appearance, corrosion resistance, and blocking resistance.
[0015] (A) Film-forming resin The coating film-forming resin (A) contains an acrylic resin emulsion (A1) and an acrylic resin emulsion (A2) from the viewpoint of obtaining a coating film excellent in touch dryness, coating film appearance and corrosion resistance, which will be described later. The acrylic resin emulsion (A1) and the acrylic resin emulsion (A2) are also advantageous from the viewpoint of cost.
[0016] Acrylic resin emulsion (A1) The acrylic resin emulsion (A1) is an aqueous dispersion containing an acrylic resin, and more specifically, refers to an acrylic resin dispersed in a medium in the form of particles. The acrylic resin may be, for example, a polymer of a monomer mixture containing an ethylenic monomer.
[0017] Examples of the ethylenic monomer that can be used include hydroxyl group-containing monomers; ε-caprolactone-modified (meth)acrylic monomers; esters of polyhydric alcohols such as ethylene glycol and propylene glycol with (meth)acrylic acid; ε-caprolactone-modified esters of polyhydric alcohols such as ethylene glycol and propylene glycol with (meth)acrylic acid; and mixtures of carboxyl group-containing monomers and other monomers.
[0018] Examples of the hydroxyl group-containing monomer include hydroxyalkyl group-containing monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2,3-dihydroxybutyl (meth)acrylate, and hydroxymethylcyclohexyl (meth)acrylate; and monomers obtained by modifying the hydroxyalkyl group-containing monomers with ε-caprolactone. Specific examples of the ε-caprolactone-modified (meth)acrylic monomers include PLACCEL FA-1, PLACCEL FA-2, PLACCEL FA-3, PLACCEL FA-4, PLACCEL FA-5, PLACCEL FM-1, PLACCEL FM-2, PLACCEL FM-3, PLACCEL FM-4, and PLACCEL FM-5, all of which are manufactured by Daicel Corporation. In the present disclosure, (meth)acrylic acid means acrylic acid and methacrylic acid.
[0019] Examples of the carboxyl group-containing monomer include carboxylic acid monomers such as (meth)acrylic acid, 2-ethylpropenoic acid, crotonic acid, maleic acid, fumaric acid, and itaconic acid, and dicarboxylic acid monoester monomers thereof. Preferred carboxyl group-containing monomers are acrylic acid and methacrylic acid. These may be used alone or in combination of two or more.
[0020] Examples of other ethylenic monomers include styrene-based monomers such as styrene, α-methylstyrene, and vinyltoluene; (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-, i-, and t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and lauryl (meth)acrylate; amino group-containing monomers such as aminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, and butylaminoethyl (meth)acrylate; ethyl maleate, maleic acid, and the like. dicarboxylic acid monoester monomers such as butyl itaconate, ethyl itaconate, and butyl itaconate; alicyclic group-containing monomers such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, cyclooctyl (meth)acrylate, cyclodecyl (meth)acrylate, cyclododecyl (meth)acrylate, isobornyl (meth)acrylate, tricyclodecanyl (meth)acrylate, and adamantyl (meth)acrylate; aminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, aminoalkyl (meth)acrylamide monomers such as aminoethyl (meth)acrylamide, dimethylaminomethyl (meth)acrylamide, and methylaminopropyl (meth)acrylamide; other N-substituted (meth)acrylamide monomers such as acrylamide and methacrylamide; vinyl cyanide monomers such as (meth)acrylonitrile and α-chloroacrylonitrile; saturated aliphatic carboxylic acid vinyl ester monomers such as vinyl acetate and vinyl propionate; (meth)acrylamide, N-hydroxy (meth)acrylamide, methoxybutyl (meth)acrylamide, N-alkoxy (meth)acrylamide, N-alkylol (meth)acrylamide (e.g., N-methylol (meth)acrylamide, etc.), and diacetone (meth)acrylamide (meth)acrylamide (meth)acrylamide; amino group-containing (meth)acrylamide monomers such as aminoethyl (meth)acrylamide, dimethylaminomethyl (meth)acrylamide, and methylaminopropyl (meth)acrylamide;Examples of the monomers include glycidyl-containing monomers such as glycidyl (meth)acrylate; vinyl cyanide monomers such as (meth)acrylonitrile and α-chloroacrylonitrile; alkoxysilyl-containing monomers such as trimethoxysilylpropyl (meth)acrylate and triethoxysilylpropyl (meth)acrylate; and bifunctional monomers such as divinylbenzene and ethylene glycol (meth)acrylate. The ethylenic monomer may be used alone or in combination of two or more kinds.
[0021] The glass transition temperature of the entire acrylic resin in the acrylic resin water dispersion (A1) is preferably from 30° C. to 50° C., more preferably from 35° C. to 45° C. When the glass transition temperature of the acrylic resin is within the above range, the appearance and blocking resistance of the resulting coating film are good. In the present disclosure, the term "the entire acrylic resin in the acrylic resin water dispersion" refers to the entire acrylic resin contained in the acrylic resin water dispersion.
[0022] In the present disclosure, the glass transition temperature (Tg) of the acrylic resin (polymer) in the acrylic resin emulsion can be calculated as the reciprocal of the sum of the quotients obtained by dividing the mass fraction of each monomer constituting the acrylic resin (polymer) by the Tg (expressed in K: Kelvin) value of a homopolymer derived from each monomer.
[0023] More specifically, in the present disclosure, the glass transition temperature (Tg) of the acrylic resin in the acrylic resin emulsion can be calculated by the Fox formula (TGFox; Bull. Am. Phys. Soc., 1(3), 123(1956)).
[0024] For example, when the fine particles are polymers of a plurality of acrylic monomers, the polymers are represented by the following general formula: 1 / Tg=w1 / Tg1+w2 / Tg2+···+w n / Tg n The Tg represented by the following formula is defined as the Tg of the fine particles. Tg a : Glass transition temperature of homopolymer of monomer A (K), W a : Mass fraction of monomer A Tg b : Glass transition temperature of homopolymer of monomer B (K), W b : Mass fraction of monomer B Tg n : Glass transition temperature of homopolymer of monomer N (K), W n : Mass fraction of monomer N (W a +W b +···+W n =1)
[0025] The acid value of the entire acrylic resin in the acrylic resin emulsion (A1) is preferably from 10 mgKOH / g to 150 mgKOH / g, more preferably from 10 mgKOH / g to 120 mgKOH / g. The acid value of the acrylic resin in the above range has the advantage that the appearance and corrosion resistance of the resulting coating film are improved. In the present disclosure, the acid value and the hydroxyl value are both expressed as solid content equivalent values, and are values measured by a method in accordance with JIS K 0070.
[0026] The weight average molecular weight of the acrylic resin in the acrylic resin emulsion (A1) may be preferably more than 50,000 and not more than 10,000,000, more preferably more than 100,000 and not more than 2,000,000. When the weight average molecular weight of the acrylic resin is within the above range, the strength of the resulting coating film may be good. In this disclosure, the weight average molecular weight is a polystyrene equivalent value measured by gel permeation chromatography.
[0027] The average particle size of the acrylic resin in the acrylic resin emulsion (A1) may be preferably 50 nm or more and 200 nm or less, more preferably 75 nm or more and 180 nm or less, and even more preferably 80 nm or more and 150 nm or less. The average particle size of the acrylic resin within the above range has the advantage that the appearance and corrosion resistance of the resulting coating film are improved. In the present disclosure, the average particle size is an average particle size determined by dynamic light scattering, and specifically, can be measured using an electrophoretic light scattering photometer ELSZ series (manufactured by Otsuka Electronics Co., Ltd.) or the like.
[0028] The solubility parameter (SP value) of the entire acrylic resin of the acrylic resin emulsion (A1) is preferably 9.5 or more and 10.9 or less, more preferably 9.8 or more and 10.7 or less, and even more preferably 10.0 or more and 10.7 or less. When the SP value of the acrylic resin is within the above range, there is an advantage that the appearance of the obtained coating film is improved. In this disclosure, the unit of the solubility parameter (SP value) is [(cal / cm 3 ) 1 / 2 ].
[0029] The SP value is an abbreviation for solubility parameter, and is a measure of solubility. The larger the SP value, the higher the polarity, and conversely, the smaller the SP value, the lower the polarity.
[0030] The SP value can be measured by the following method [Reference: SUH, CLARKE, JPSA-1, 5, 1671-1681 (1967)]. The sample used is 0.5 g of monomer weighed into a 100 mL beaker, 10 mL of acetone added using a volumetric pipette, and dissolved using a magnetic stirrer. A poor solvent is dripped onto this sample using a 50 mL burette at a measurement temperature of 20°C, and the point at which turbidity occurs is regarded as the amount of dripped solution. Ion-exchanged water is used as the high SP poor solvent, and n-hexane is used as the low SP poor solvent, and the turbidity point is measured for each poor solvent. SP value of monomer δ[(cal / cm 3 ) 1 / 2 ] is given by the following formula: δ = (Vml 1 / 2 δml+Vmh 1 / 2 δmh) / (Vml 1 / 2 +Vmh 1 / 2 ) Vm = V1V2 / (φ1V2+φ2V1) δm = φ1δ1 + φ2δ2 V i : Molar volume of the solvent (mL / mol) φ i : Volume fraction of each solvent at the clouding point δ i : SP value of the solvent ml: Low SP poor solvent mixed system mh: High SP poor solvent mixed system
[0031] When the acrylic resin emulsion (A1) contains two or more kinds of acrylic resins, the SP value of the entire acrylic resin in the acrylic resin water dispersion (A1) can be determined by using the SP values of each monomer and calculating an average value based on the solid content mass ratio in the acrylic resin water dispersion (A1) components. In the present disclosure, the solid content of the resin can be determined by measuring the heating residue (the mass of the residue after heating at 105° C. for 180 minutes) in accordance with JIS K 5601-1-2 (2008).
[0032] The acrylic resin emulsion (A1) contains a core-shell type acrylic resin emulsion. The core-shell type acrylic resin emulsion is an acrylic resin emulsion in the form of particles, which has a core part inside the particle and a shell part covering at least a part of the core part.
[0033] The glass transition temperature of the shell part of the core-shell type acrylic resin emulsion (hereinafter, simply referred to as the "shell part") is preferably higher than the glass transition temperature of the core part of the core-shell type acrylic resin emulsion (hereinafter, simply referred to as the "core part"), which has the advantage that the blocking resistance of the resulting coating film can be improved.
[0034] The glass transition temperature (Tgc) of the core portion may be preferably 80° C. or lower, more preferably 30° C. or lower, still more preferably 0° C. or higher and 30° C. or lower, and even more preferably 5° C. or higher and 30° C. or lower. When the glass transition temperature of the core portion is within this range, the film-forming properties are good, and the appearance of the resulting coating film can be improved.
[0035] The glass transition temperature (Tgs) of the shell portion may be preferably 10° C. or higher, more preferably 60° C. or higher, even more preferably 60° C. or higher and 150° C. or lower, and even more preferably 60° C. or higher and 100° C. or lower. When the glass transition temperature of the shell portion is in this range, the blocking resistance of the resulting coating film may be better.
[0036] The difference (Tgs-Tgc) between the glass transition temperature (Tgs) of the shell portion and the glass transition temperature (Tgc) of the core portion may be preferably -60° C. or more, more preferably 40° C. or more, even more preferably 40° C. or more and 130° C. or less, still more preferably 45° C. or more and 70° C. or less, and even more preferably 50° C. or more and 60° C. or less. When the difference (Tgs-Tgc) is within this range, the appearance and blocking resistance of the resulting coating film may be better.
[0037] The glass transition temperature of the entire acrylic resin in the core-shell type acrylic resin emulsion can be calculated as the reciprocal of the sum of the quotients obtained by dividing the mass fractions of the core and shell constituting the acrylic resin in the core-shell type acrylic resin emulsion by the Tg (K: expressed in Kelvin) values of the core and shell, respectively.
[0038] The solid content of the core-shell acrylic resin emulsion is preferably 80% by mass or more and 100% by mass or less, more preferably 90% by mass or more and 100% by mass or less, and even more preferably 95% by mass or more and 100% by mass or less, based on 100% by mass of the total solid content of the acrylic resin emulsion (A1).
[0039] The acrylic resin emulsion (A1) can be prepared by polymerizing a monomer mixture containing the ethylenic monomer in an aqueous medium. The polymerization reaction is preferably carried out by emulsion polymerization, specifically, by batch polymerization, monomer dropwise polymerization, emulsion monomer dropwise polymerization, or the like.
[0040] The emulsion polymerization can be carried out by heating the monomer mixture in an aqueous liquid in the presence of a radical polymerization initiator and an emulsifier while stirring. The reaction temperature is preferably about 30 to 100°C, and the reaction time is preferably about 1 to 10 hours. The reaction temperature can be adjusted, for example, by adding the monomer mixture or the monomer pre-emulsion all at once or gradually dropping it into a reaction vessel containing water and an emulsifier.
[0041] As the radical polymerization initiator, a known initiator that is usually used in emulsion polymerization of acrylic resins can be used. Specifically, as a water-soluble free radical polymerization initiator, for example, persulfates such as potassium persulfate, sodium persulfate, and ammonium persulfate can be used in the form of an aqueous solution. In addition, so-called redox initiators in which an oxidizing agent such as potassium persulfate, sodium persulfate, ammonium persulfate, and hydrogen peroxide is combined with a reducing agent such as sodium hydrogen sulfite, sodium thiosulfate, Rongalite, and ascorbic acid can be used in the form of an aqueous solution.
[0042] The emulsifier may be an anionic or nonionic emulsifier selected from micellar compounds having a hydrocarbon group with 6 or more carbon atoms and a hydrophilic portion such as a carboxylate, a sulfonate, or a sulfate partial ester in the same molecule. Among these, anionic emulsifiers include alkali metal salts or ammonium salts of sulfuric acid half esters of alkylphenols or higher alcohols; alkali metal salts or ammonium salts of alkyl or aryl sulfonates; alkali metal salts or ammonium salts of sulfuric acid half esters of polyoxyethylene alkylphenyl ethers, polyoxyethylene alkyl ethers, or polyoxyethylene allyl ethers. Nonionic emulsifiers include polyoxyethylene alkylphenyl ethers, polyoxyethylene alkyl ethers, or polyoxyethylene allyl ethers. In addition to these general-purpose anionic and nonionic emulsifiers, various anionic and nonionic reactive emulsifiers having a radically polymerizable unsaturated double bond in the molecule, i.e., an acrylic, methacrylic, propenyl, allyl, allyl ether, maleic acid, or other group, can also be used alone or in combination of two or more types as appropriate.
[0043] During emulsion polymerization, the use of an auxiliary agent (chain transfer agent) for adjusting the molecular weight, such as a mercaptan compound or a lower alcohol, in combination is often preferable from the viewpoint of advancing the emulsion polymerization and from the viewpoint of promoting smooth and uniform formation of a coating film and improving adhesion to the substrate, and is carried out appropriately depending on the situation.
[0044] As the emulsion polymerization method, any emulsion polymerization method can be used, such as a conventional one-stage continuous uniform monomer dropping method, a core-shell polymerization method which is a multi-stage monomer feed method, or a power feed polymerization method in which the monomer composition fed during polymerization is continuously changed.
[0045] In the polymerization, the monomer mixture may be continuously, gradually, or stepwise fed. For example, a core-shell acrylic resin emulsion having a core and a shell can be prepared by feeding two or more kinds of monomer mixtures stepwise.
[0046] If necessary, a basic compound can be added to the obtained acrylic resin emulsion in order to neutralize a part or all of the acid groups present therein and maintain the stability of the acrylic resin emulsion. Examples of the basic compound that can be used include ammonia, various amines, and alkali metals.
[0047] The solid content of the acrylic resin emulsion (A1) is preferably 30% by mass or more and 99% by mass or less, more preferably 40% by mass or more and 90% by mass or less, and even more preferably 50% by mass or more and 80% by mass or less, based on 100 parts by mass of the solid content of the coating film-forming resin (A).
[0048] Acrylic resin emulsion (A2) The acrylic resin emulsion (A2) is an aqueous dispersion containing an acrylic resin, and more specifically, refers to an acrylic resin dispersed in a medium in the form of particles. The acrylic resin may be, for example, a polymer of a monomer mixture containing an ethylenic monomer.
[0049] The ethylenic monomer used in the acrylic resin emulsion (A2) may be any of the monomers exemplified as the ethylenic monomer used in the acrylic resin emulsion (A2). The acrylic resin emulsion (A2) can be produced by polymerizing such an ethylenic monomer in the same manner as in the acrylic resin emulsion (A1). The glass transition temperature of the entire acrylic resin in the acrylic resin water dispersion (A2) is preferably from −20° C. to 0° C., more preferably from −18° C. to −5° C. When the glass transition temperature of the acrylic resin is in the above range, the film-forming properties are further improved, and the appearance and tack-drying properties of the resulting coating film are good.
[0050] The acid value of the entire acrylic resin in the acrylic resin emulsion (A2) is preferably 5 mgKOH / g or more and 150 mgKOH / g or less, more preferably 5 mgKOH / g or more and 120 mgKOH / g or less. The acid value of the acrylic resin in the above range has the advantage that the appearance and corrosion resistance of the obtained coating film are improved.
[0051] The weight average molecular weight of the acrylic resin in the acrylic resin emulsion (A2) may be preferably more than 50,000 and not more than 10,000,000, more preferably more than 100,000 and not more than 2,000,000. When the weight average molecular weight of the acrylic resin is within the above range, the strength of the resulting coating film may be good.
[0052] The average particle size of the acrylic resin in the acrylic resin emulsion (A2) may be preferably 50 nm or more and 250 nm or less, more preferably 75 nm or more and 230 nm or less, and even more preferably 100 nm or more and 200 nm or less. The average particle size of the acrylic resin within the above range has the advantage that the appearance and corrosion resistance of the resulting coating film are improved.
[0053] The solubility parameter (SP value) of the entire acrylic resin of the acrylic resin emulsion (A2) is preferably 9.0 or more and 10.3 or less, more preferably 9.3 or more and 10.0 or less, and even more preferably 9.3 or more and 9.7 or less. When the SP value of the acrylic resin is within the above range, there is an advantage that the appearance of the obtained coating film is improved.
[0054] The acrylic resin emulsion (A2) contains a single-layer type acrylic resin emulsion, and is preferably a single-layer type acrylic emulsion, which has the advantages of improving the film-forming properties of the aqueous coating composition, as well as improving the tack-drying properties and the appearance of the resulting coating film.
[0055] The ratio of the solid content of the acrylic resin emulsion (A1) to the solid content of the acrylic resin emulsion (A2) ((A1):(A2)) is preferably 97:3 to 50:50, more preferably 90:10 to 50:50, even more preferably 80:20 to 50:50, and even more preferably 75:25 to 55:45. When the ratio ((A1):(A2)) is within this range, there is an advantage that the appearance, blocking resistance, and tack-drying properties of the resulting coating film become better.
[0056] In 100 parts by mass of the total amount of solid contents of the coating film-forming resin (A), the total content of solid contents of the acrylic resin emulsion (A1) and the acrylic resin emulsion (A2) may be preferably from 50% by mass to 100% by mass, more preferably from 60% by mass to 100% by mass, and even more preferably from 70% by mass to 100% by mass.
[0057] The coating film-forming resin (A) may contain a resin other than the acrylic resin emulsion (A1) and the acrylic resin emulsion (A2), such as a polyester resin emulsion, a urethane resin emulsion, a fluororesin emulsion, etc.
[0058] In the aqueous coating composition, the solid content of the coating film-forming resin (A) may be preferably from 40 to 90 mass%, more preferably from 45 to 80 mass%, and even more preferably from 50 to 75 mass%, based on 100 parts by mass of the total solid content of the aqueous coating composition.
[0059] (B) Anti-rust pigment The anti-rust pigment (B) is typically present in a coating film and can exert an effect of suppressing the occurrence of rust on a coated object. The inclusion of the anti-rust pigment (B) can improve the corrosion resistance of the resulting coating film. The anti-rust pigment (B) typically has one or more properties selected from the following: a property of containing a metal with a higher ionization tendency than the coated object and suppressing the occurrence of rust on the coated object; a property of forming a coating on the coated object to suppress contact between the coated object and substances that cause rust, thereby suppressing the occurrence of rust on the coated object; a property of releasing a basic substance, and the like.
[0060] Examples of such anti-rust pigments (B) include inorganic anti-rust pigments. Examples of the inorganic anti-rust pigments include phosphoric acid-based anti-rust pigments, zinc oxide-based anti-rust pigments, molybdenum-based anti-rust pigments, boric acid-based anti-rust pigments, silicic acid-based anti-rust pigments, vanadate-based anti-rust pigments, and tungstic acid-based anti-rust pigments. These anti-rust pigments may be used alone or in combination of two or more.
[0061] The phosphorus-based rust-preventive pigment may be a metal salt of an oxyacid of phosphorus. The metal may be one or more metals selected from Mg, Ca, Ba, Sr, Zn, or Al. The phosphorus oxyacid salt may be, for example, a phosphite, a phosphate, and / or a polyphosphate. Specific examples of phosphorus-based rust-preventive pigments include metal phosphites such as magnesium phosphite, calcium phosphite, barium phosphite, strontium phosphite, zinc phosphite, aluminum phosphite, calcium zinc phosphite, and potassium zinc phosphite. Examples of metal phosphates include magnesium phosphate, calcium phosphate, barium phosphate, strontium phosphate, zinc phosphate, aluminum phosphate, magnesium zinc phosphate, calcium zinc phosphate, potassium zinc phosphate, and potassium zinc phosphate. Examples of metal polyphosphates include aluminum pyrophosphate, calcium polyphosphate, magnesium polyphosphate, zinc polyphosphate, and aluminum polyphosphate. These compounds may be modified with silica or the like, if necessary.
[0062] Examples of the zinc oxide-based rust-preventive pigment include zinc oxide and modified zinc oxide, etc. Examples of the modified zinc oxide include zinc oxide modified with a metal salt such as a metal nitrite.
[0063] The molybdenum-based rust-preventive pigment may, for example, be a metal molybdate.The metal molybdate may, for example, be zinc molybdate, calcium molybdate, barium molybdate, aluminum molybdate, magnesium molybdate, strontium molybdate, calcium zinc molybdate, and potassium zinc molybdate.The phosphomolybdate may, for example, be zinc molybdate, calcium molybdate, barium molybdate, aluminum molybdate, magnesium molybdate, strontium molybdate, and potassium zinc molybdate.
[0064] The borate-based rust-preventive pigment may, for example, be a metal borate or a metal metaborate. The metal borate may, for example, be zinc borate, calcium borate, barium borate, aluminum borate, magnesium borate, strontium borate, zinc calcium borate, or zinc potassium borate. The metal metaborate may, for example, be barium metaborate.
[0065] Examples of the silicic acid-based rust-preventive pigment include metal borosilicates, such as silicic acid, zinc borosilicate, calcium borosilicate, barium borosilicate, aluminum borosilicate, magnesium borosilicate, strontium borosilicate, potassium zinc borosilicate, calcium strontium zinc borosilicate, zinc phosphosilicate, calcium phosphosilicate, barium phosphosilicate, aluminum phosphosilicate, magnesium phosphosilicate, strontium phosphosilicate, potassium zinc phosphosilicate, calcium zinc phosphosilicate, and calcium strontium zinc phosphosilicate.
[0066] The metal salt may be any of a normal salt, a basic salt, and a complex salt, and may be either hydrous or anhydrous.
[0067] In addition to the above, examples of inorganic rust-preventive pigments include vanadate-based rust-preventive pigments, tungstic acid-based rust-preventive pigments, etc. Other examples include cyanamide zinc calcium-based rust-preventive pigments, and modified silica-based rust-preventive pigments in which metal cations such as calcium, zinc, cobalt, lead, strontium, barium, etc. are bonded to porous silica particles.
[0068] The rust-preventive pigment (B) may be a commercially available product. Examples of commercially available products include phosphoric acid-based rust-preventive pigments such as LF Bosei PM-300C, LF Bosei PW-2 (manufactured by Kikuchi Color Co., Ltd.), and K-White #140W (manufactured by Teika Co., Ltd.), silicate-based rust-preventive pigments such as SHIELDEX CS-311 (manufactured by GRACE Co., Ltd.), molybdenum-based rust-preventive pigments such as LF Bosei M-PSN (manufactured by Kikuchi Color Co., Ltd.), and zinc oxide-based rust-preventive pigments such as zinc oxide type 2 (manufactured by Sakai Chemical Industry Co., Ltd.).
[0069] The rust-preventive pigment (B) may be used alone or in combination of two or more kinds. The rust-preventive pigment (B) preferably contains at least one selected from the group consisting of phosphoric acid-based rust-preventive pigments, zinc oxide-based rust-preventive pigments, and molybdenum-based rust-preventive pigments, and more preferably contains at least one selected from the group consisting of phosphoric acid-based rust-preventive pigments and zinc oxide-based rust-preventive pigments. The rust-preventive pigment (B) may also contain a silicate-based rust-preventive pigment.
[0070] The content of the rust-preventive pigment (B) in the aqueous coating composition is preferably 1 part by mass or more and 50 parts by mass or less, more preferably 5 parts by mass or more and 30 parts by mass or less, based on 100 parts by mass of the total solid content of the coating film-forming resin (A) contained in the aqueous coating composition. The content of the rust-preventive pigment (B) within the above range has the advantage that the corrosion prevention properties of the resulting coating film are good.
[0071] (C) Resin beads The resin beads (C) are fine resin particles. By including the resin beads (C), the blocking resistance of the resulting coating film can be improved.
[0072] Examples of the resin constituting the resin beads (C) include acrylic resin, urethane resin, polyester resin, polyamide resin, polystyrene resin, polyethylene resin, melamine resin, urea resin, fluororesin, polyacrylonitrile resin, etc., and from the viewpoint of hardness and cost, acrylic resin is preferable. In addition, the fine particle shape means a particulate shape, a spherical shape, or a hollow spherical shape. The resin beads are preferably spherical. The spherical shape is not limited to a perfect sphere, and may include a shape such as an approximately spherical shape.
[0073] The average particle size of the resin beads (C) is preferably 1 μm or more, more preferably 10 μm or more and 150 μm or less, even more preferably 20 μm or more and 100 μm or less, and even more preferably 40 μm or more and 80 μm or less.
[0074] In this specification, the average particle size of the resin beads (C) means the volume average particle size (D50), and can be measured using a laser Doppler type particle size analyzer (for example, Microtrac UPA150 manufactured by Nikkiso Co., Ltd.).
[0075] The resin beads (C) may be acrylic resin particles, and may be commercially available products. Examples of commercially available products include Ganz Pearl GM-0801, GM-4003 (manufactured by Aica Kogyo Co., Ltd.), Tuftic AM, AR750MXQ, AR750MLQ2 (manufactured by Nippon Exlan Kogyo Co., Ltd.), Techpolymer MBX-40, MBX-80 (manufactured by Sekisui Chemical Co., Ltd.), etc. Examples of urethane resin particles include ART PEARL C-80T, C-100T (manufactured by Negami Electric Industries Co., Ltd.), etc.
[0076] The content of the resin beads (C) in the aqueous coating composition is preferably 1 part by mass or more and 30 parts by mass or less, more preferably 5 parts by mass or more and 25 parts by mass or less, per 100 parts by mass of the total resin solids contained in the aqueous coating composition.
[0077] (D) Film-forming agent The aqueous coating composition of the present disclosure may contain a film-forming auxiliary (D) as necessary. By adding the film-forming auxiliary, when the water evaporates and the emulsion resin particles fuse to form a coating film, the flow of the coating film is improved, and as a result, the finished appearance of the coating film is improved.
[0078] The film-forming auxiliary (D) is not particularly limited, but may be at least one of alcohols such as benzyl alcohol; cellosolves such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, and ethylene glycol monobutyl ether; propylene glycol ethers such as propylene glycol monomethyl ether and propylene glycol monoethyl ether; carbitols such as diethylene glycol monoethyl ether and diethylene glycol monobutyl ether; triglycol ethers such as triethylene glycol monomethyl ether and tripropylene glycol monomethyl ether; ketones such as acetylacetone; amines such as triethylamine and diethanolamine; and 2,2,4-trimethylpentanediol-1,3-monoisobutyrate (trade name "Texanol", manufactured by Eastman Chemical Japan Co., Ltd.). Two or more types of film-forming auxiliary may be used in combination.
[0079] The content of the coalescence aid (D) is preferably 1 to 40 parts by mass, more preferably 4 to 30 parts by mass, and even more preferably 8 to 20 parts by mass, relative to 100 parts by mass of the total solid content of the aqueous coating composition. When the content of the coalescence aid (D) is within this range, the appearance of the resulting coating film can be improved.
[0080] (Other ingredients) In addition to the above components, the aqueous coating composition may contain other components as necessary depending on the purpose and use. Examples of other components include curing agents, extender pigments, coloring pigments, resin particles, curing catalysts, viscosity agents, pH adjusters, film-forming assistants, and additives that are commonly used in aqueous coating compositions (e.g., dispersion stabilizers, ultraviolet absorbers, light stabilizers, antioxidants, defoamers, surface conditioners, pinhole inhibitors, organic rust inhibitors, etc.). These components can be added appropriately in a manner that does not impair the various physical properties of the aqueous coating composition of the present disclosure.
[0081] Examples of the pigment include color pigments and extender pigments. Examples of the color pigment include inorganic color pigments and organic color pigments. Examples of the inorganic color pigment include titanium oxide, carbon black, iron oxide, and yellow iron oxide. Examples of the organic color pigment include phthalocyanine pigments such as phthalocyanine blue and phthalocyanine green; azo pigments such as azo red, azo yellow, and azo orange; quinacridone pigments such as quinacridone red, shinkasha red, and shinkasha magenta; perylene pigments such as perylene red and perylene maroon; carbazole violet, anthrapyridine, flavanthrone yellow, isoindoline yellow, industhrone blue, dibromoanzathrone red, anthraquinone red, and diketopyrrolopyrrole. Examples of the extender pigment include calcium carbonate, precipitated barium sulfate, clay, and talc.
[0082] When the color pigment is used, the pigment mass concentration of the color pigment relative to the resin solid content of the aqueous coating composition is preferably 5% by mass or more and 60% by mass or less.
[0083] When the extender pigment is used, the pigment mass concentration of the extender pigment relative to the resin solid content of the aqueous coating composition is preferably 0% by mass or more and 60% by mass or less, more preferably 0% by mass or more and 40% by mass or less. By keeping the amount of the extender pigment within this range, there is an advantage that the water resistance of the resulting coating film is improved.
[0084] (Method of preparing aqueous coating composition) The aqueous coating composition can be prepared by mixing the film-forming resin (A), the rust-preventive pigment (B), the resin beads (C) and other components as required by a method known to those skilled in the art. The aqueous coating composition can be prepared by a method commonly used by those skilled in the art. For example, a kneading and mixing means using a kneader or roll, or a dispersing and mixing means using a sand grind mill or disperser, or other methods commonly used by those skilled in the art can be used.
[0085] (subject to be coated) Examples of the substrate include metal substrates such as iron, zinc, tin, copper, titanium, tinplate, etc. These metal substrates may be plated with zinc, copper, chromium, etc., or may be surface-treated using a surface treatment agent such as chromate, zinc phosphate, or zirconium salt.
[0086] The aqueous coating composition of the present disclosure is suitable for coating metal substrates, particularly steel materials such as bar steel, steel plate, and steel pipe, as well as steel towers, steel poles, steel doors, and vehicle bodies. More specific examples of the steel materials include C-shaped steel such as lip groove steel, light groove steel, and deformed light groove steel, L-angles such as equal leg light angle steel and unequal leg light angle steel, lightweight steel such as square steel pipes and deck plates, cast iron pipes, and the like; and steel materials obtained by subjecting these steel materials to chemical conversion treatment such as phosphating and / or metal spraying treatment.
[0087] (Method of forming coating film) A coating film can be produced by applying the aqueous coating composition to the surface of an article to be coated and forming a coating film.
[0088] The method of applying the aqueous coating composition is not particularly limited, and examples thereof include commonly used coating methods such as immersion, brush, roller, roll coater, air spray, airless spray, curtain flow coater, roller curtain coater, and die coater. These can be appropriately selected depending on the type of building material, etc. The aqueous coating composition is preferably applied to a dry film thickness of 30 to 100 μm, and more preferably applied to a dry film thickness of 40 to 80 μm.
[0089] In the drying step, the coating film is dried, thereby forming a coating film. In one embodiment, the drying temperature may be 5 to 35° C., and the drying time may be 1 to 10 days. In another embodiment, the drying temperature may be, for example, 50 to 100° C., or further 60 to 80° C., and the drying time in this case may be 15 to 60 minutes.
[0090] In a preferred embodiment, the substrate may be preheated before coating. The preheating temperature may be such that the substrate temperature at the time of coating is 60 to 110° C. When such preheating is performed, for example, the method for producing a coating film may include preheating the substrate to a temperature of 60° C. or higher and 110° C. or lower, and applying the aqueous coating composition to the surface of the substrate after the preheating to form a coating film.
[0091] The heating method is not particularly limited, and may be performed using a heating furnace such as a gas furnace or an electric furnace. The heating temperature of the object to be coated is not particularly limited, and should be within a range that allows the object to be heated to the above temperature, taking into consideration the amount of heat stored due to the shape and thickness of the object to be coated and the interval from preheating to painting. In general, the heating temperature is set to about 10 to 30°C higher than the painting temperature, and preferably 90°C or higher. EXAMPLES
[0092] The present disclosure will be described more specifically with reference to the following examples, but the present disclosure is not limited thereto.
[0093] Manufacturing example (A1-1) Preparation example of acrylic resin emulsion (A1-1) 61.5 parts by mass of methyl methacrylate, 1.8 parts by mass of methacrylic acid, and 36.7 parts by mass of 2-ethylhexyl acrylate were mixed and stirred in a stainless steel container, and then 2.5 parts by mass of sulfosuccinic acid diester ammonium salt (Latemul S-180A, manufactured by Kao Corporation) as an emulsifier and 60.0 parts by mass of water were added, and the mixture was stirred at room temperature for 15 minutes using a homomixer to obtain a first pre-reaction emulsified mixture.
[0094] 60.0 parts by mass of water was placed in a reaction vessel equipped with a stirrer, a reflux condenser, a dropping funnel and a thermometer, and the temperature in the reaction vessel was raised to 80° C., after which 91.8 parts by mass of the first pre-reaction emulsification mixture and 5.5 parts by mass of a 1.5% by mass aqueous solution of ammonium persulfate as a reaction initiator were dropped simultaneously from separate dropping funnels over a period of 2 hours. After the dropping was completed, the temperature in the reaction vessel was maintained at 80° C. for 30 minutes to obtain an acrylic resin emulsion. In a separate container, 85.9 parts by mass of methyl methacrylate, 1.8 parts by mass of methacrylic acid, and 12.3 parts by mass of 2-ethylhexyl acrylate were mixed with stirring, and then 2.5 parts by mass of sulfosuccinic acid diester ammonium salt (Latemul S-180A, manufactured by Kao Corporation) as an emulsifier and 60.0 parts by mass of water were added, and the mixture was stirred at room temperature for 15 minutes using a homomixer to obtain a second pre-reaction emulsified mixture.
[0095] Into the vessel containing the previously obtained acrylic resin emulsion, 91.8 parts by mass of the second pre-reaction emulsification mixture and 5.5 parts by mass of a 1.5% by mass aqueous solution of ammonium persulfate as a reaction initiator were simultaneously dropped from separate dropping funnels over a period of 2 hours. After the dropping was completed, the temperature in the reaction vessel was maintained at 80°C for 1 hour, and then cooled to 30°C to obtain a core-shell type acrylic resin emulsion (A1-1) (solid content concentration: 45% by mass).
[0096] Manufacturing Examples (A1-2) to (A1-5), (a1-1), and (a1-2) Film-forming resins (A1-2) to (A1-5), (a1-1) and (a1-2) were prepared in the same manner as above, except that the monomer type and amount were changed as shown in Table 1. Table 1 shows the characteristics of each film-forming resin, such as the glass transition temperature.
[0097] [Table 1]
[0098] Manufacturing example (A2-1) Preparation example of acrylic resin emulsion (A2-1) 34.0 parts by mass of methyl methacrylate, 1.0 part by mass of acrylic acid, 5.0 parts by mass of styrene, and 60.0 parts by mass of 2-ethylhexyl acrylate were mixed and stirred in a stainless steel container, and then 2.5 parts by mass of sulfosuccinic acid diester ammonium salt (Latemul S-180A, manufactured by Kao Corporation) as an emulsifier and 60.0 parts by mass of water were added, and the mixture was stirred at room temperature for 15 minutes using a homomixer to obtain a first pre-reaction emulsified mixture.
[0099] 30.0 parts by mass of water was placed in a reaction vessel equipped with a stirrer, a reflux condenser, a dropping funnel and a thermometer, and the temperature in the reaction vessel was raised to 80°C, after which 91.8 parts by mass of the first pre-reaction emulsification mixture and 5.5 parts by mass of a 1.5% by mass aqueous solution of ammonium persulfate as a reaction initiator were dropped simultaneously from separate dropping funnels over a period of 2 hours. After the dropping was completed, the temperature in the reaction vessel was maintained at 80°C for 30 minutes to obtain an acrylic resin emulsion (A2-1) (solid content concentration: 45% by mass).
[0100] Production example (A2-2), (A2-3), (a2-1)~(a2-3) Film-forming resins (A2-2), (A2-3), and (a2-1) to (a2-3) were prepared in the same manner as above, except that the monomer type and amount were changed as shown in Table 1. Table 2 shows the characteristics of each film-forming resin, such as the glass transition temperature.
[0101] [Table 2]
[0102] <Production example of pigment dispersion paste 1> 1.63 parts by mass of Disperbyk190 as a dispersant, 0.05 parts by mass of SN-477T as an antifoaming agent, 32.9 parts by mass of ion-exchanged water, 31.4 parts by mass of Ti-Pure R-706 as a pigment, and 33.8 parts by mass of LF Bousei PW-2 as an anti-rust pigment (B-1) were premixed, and then the mixture was dispersed at 1,600 rpm using an SG mill (dispersion medium: glass beads) until the maximum particle diameter of the pigment coarse particles became 5 μm, thereby obtaining pigment dispersion paste 1.
[0103] <Production example of pigment dispersion paste 2> 1.63 parts by mass of Disperbyk190 as a dispersant, 0.05 parts by mass of SN-477T as an antifoaming agent, 32.9 parts by mass of ion-exchanged water, 31.4 parts by mass of Ti-Pure R-706 as a pigment, 16.9 parts by mass of LF Bousei PW-2 as an anti-rust pigment (B-1), and 16.9 parts by mass of SHIELDEX CS-311 as an anti-rust pigment (B-2) were premixed, and then dispersed at 1,600 rpm using an SG mill (dispersion medium: glass beads) until the maximum particle diameter of the pigment coarse particles became 5 μm, thereby obtaining pigment dispersion paste 1.
[0104] <Production example of pigment dispersion paste 3> 1.63 parts by mass of Disperbyk190 as a dispersant, 0.05 parts by mass of SN-477T as an antifoaming agent, 32.9 parts by mass of ion-exchanged water, 31.4 parts by mass of Ti-Pure R-706 as a pigment, 16.9 parts by mass of LF Bowsei PW-2 as an anti-rust pigment (B-1), and 16.9 parts by mass of two types of zinc oxide as an anti-rust pigment (B-3) were premixed, and then dispersed at 1,600 rpm using an SG mill (dispersion medium: glass beads) until the maximum particle diameter of the pigment coarse particles became 5 μm, thereby obtaining pigment dispersion paste 1.
[0105] <Production example of pigment dispersion paste 4> 1.63 parts by mass of Disperbyk190 as a dispersant, 0.05 parts by mass of SN-477T as an antifoaming agent, 32.9 parts by mass of ion-exchanged water, and 64.7 parts by mass of Ti-Pure R-706 as a pigment were premixed, and then the mixture was dispersed at 1,600 rpm using an SG mill (dispersion medium: glass beads) until the maximum particle size of the coarse pigment particles became 5 μm, thereby obtaining pigment dispersion paste 1.
[0106] <Production example of pigment dispersion paste 5> 1.63 parts by mass of Disperbyk190 as a dispersant, 0.05 parts by mass of SN-477T as an antifoaming agent, 32.9 parts by mass of ion-exchanged water, 31.4 parts by mass of Ti-Pure R-706 as a pigment, and 7.7 parts by mass of LF Bousei PW-2 as an anti-rust pigment (B-1) were premixed, and then the mixture was dispersed at 1,600 rpm using an SG mill (dispersion medium: glass beads) until the maximum particle diameter of the pigment coarse particles became 5 μm, thereby obtaining pigment dispersion paste 1.
[0107] <Production example of pigment dispersion paste 6> 1.63 parts by mass of Disperbyk190 as a dispersant, 0.05 parts by mass of SN-477T as an antifoaming agent, 32.9 parts by mass of ion-exchanged water, 31.4 parts by mass of Ti-Pure R-706 as a pigment, and 61.3 parts by mass of LF Bousei PW-2 as an anti-rust pigment (B-1) were premixed, and then dispersed at 1,600 rpm using an SG mill (dispersion medium: glass beads) until the maximum particle diameter of the pigment coarse particles became 5 μm, thereby obtaining pigment dispersion paste 1.
[0108] (Example 1) Preparation of Water-Based Coating Composition 1 To 20.8 parts by mass of the pigment dispersion paste 1, 46.0 parts by mass of the acrylic resin water dispersion (A1-1), 25.0 parts by mass of the acrylic resin water dispersion (A2-1), 7.0 parts by mass of the resin beads (C-1) and 6.0 parts by mass of the film-forming auxiliary (D-1) were added, and the mixture was stirred and mixed with a disper to obtain an aqueous coating composition 1.
[0109] (Examples 2 to 23, Comparative Examples 1 to 7) Except for changing the type and amount of each component as shown in Tables 3 to 5, the coating compositions were prepared in the same manner as for the aqueous coating composition 1. The amount of the rust-preventive pigment (B) shown in Tables 3 to 5 indicates the amount of the rust-preventive pigment (B) contained in the pigment dispersion paste. In addition, in the examples in which (a) was used instead of the coating film-forming resin (A), the amount of (A) was read as the amount of (a). The amount of each component means the amount as it is, including volatile matters such as the solvent.
[0110] The components used in the preparation of the aqueous coating composition are as follows: (1) Materials used (B) Anti-corrosive pigments; (B-1) LF Bousei PW-2 (phosphate-based anti-rust pigment, manufactured by Kikuchi Color Co., Ltd.) (B-2) SHIELDEX CS-311 (silica-based anti-rust pigment, manufactured by GRACE) (B-3) Zinc oxide type 2 (zinc oxide-based anti-rust pigment, manufactured by Sakai Chemical Industry Co., Ltd.) (C) resin beads; (C-1) Tuftic AR750MXQ (acrylic resin beads, manufactured by Nippon Exlan Kogyo Co., Ltd.), particle size: 40 μm (C-2) Techpolymer MBX-80 (acrylic resin beads, manufactured by Sekisui Chemical Co., Ltd.), particle size: 80 μm (C-3) ART PEARL C-100T (urethane resin beads, manufactured by Negami Electric Industries), particle size: 50 μm (D) coalescents; (D-1) Benzyl alcohol (manufactured by LANXESS) (D-2) Diethylene glycol monobutyl ether (manufactured by Nippon Nyukazai) others; Color pigment: Ti-Pure R-706 (titanium dioxide, manufactured by DuPont) Dispersant: Disperbyk190 (manufactured by BYK-Chemie), active ingredient concentration: 40% by weight Defoamer: SN-477T (mineral oil-based defoamer, manufactured by San Nopco), active ingredient concentration: 100% by mass
[0111] Preparation of test plates The aqueous coating composition obtained in the Examples or Comparative Examples was diluted with water in an NK2 cup manufactured by Anest Iwata for 30 seconds (25°C), then air spray painted onto a JIS G 3141 (SPCC-SD) cold-rolled steel plate (0.8 x 70 x 150 mm) that had been degreased with a solvent and preheated to 60°C to a dry film thickness of 80 μm, and then cured at room temperature for 7 days to obtain a test plate.
[0112] 1) Dry to the touch The aqueous coating composition obtained in the Examples or Comparative Examples was diluted with water in an NK2 cup manufactured by Anest Iwata for 30 seconds (25°C), and then painted using an 8MIL doctor blade onto a JIS G 3141 (SPCC-SD) cold-rolled steel plate (0.8 x 70 x 150 mm) that had been degreased with a solvent and preheated to 60°C. The time required for the coating film obtained by painting to reach a "touch-dry" state based on the JIS K 5600-1-1 standard under conditions of a temperature of 23 degrees and a humidity of 50% was measured and rated according to the following criteria. A score of △ or higher was considered a pass. ○: Dry to the touch within 90 seconds △: Dry to the touch in more than 90 seconds but less than 120 seconds ×: Dry to the touch for 120 seconds or more
[0113] 2) Crack resistance The appearance of the coating film of the test plates obtained in the Examples and Comparative Examples was visually observed and evaluated according to the following criteria. A score of △ or higher was considered to be a pass. ○: No abnormalities in appearance such as cracks were observed in the coating film. △: Cracks are observed in some parts of the coating ×: Cracks are observed over the entire surface of the coating
[0114] 3) Blocking resistance The test plates obtained in the examples and comparative examples were evaluated for blocking resistance using a blocking tester (manufactured by Kami Kiko Co., Ltd.) according to the following procedure. The painted surfaces of two test panels were placed one on top of the other, with the panel temperature at 50°C and the load at 3kg / cm 2The test was carried out for 10 minutes at 40° C., and when the test plate was removed, the appearance of the coating film was visually observed and rated according to the following criteria. A score of △ or higher was deemed to be a pass. ○: No change in the coating surface △: Damage to part of the coating is observed. ×: Damage is observed over the entire surface of the coating.
[0115] 4)Corrosion resistance A 10 cm long cross-cut was made with a cutter knife on the coating film of the test plate obtained in the examples and comparative examples so as to reach the substrate, and a salt spray test (SST) was carried out for 120 hours using a salt spray tester ST-11L (manufactured by Suga Test Instruments Co., Ltd.) according to the neutral salt spray resistance test method described in JIS K 5600-7-1 (JIS Z 2371). After the test, the corrosion resistance of the coating film was visually evaluated according to the following criteria based on the occurrence of rust and blisters from the cross-cut part. A score of △ or higher was considered to be a pass. ○: The maximum width of the rust or blister that occurred is less than 2 mm from the cross-cut part. △: The maximum width of the rust or blister that has occurred is 2mm or more but less than 3mm from the cross-cut area. ×: The maximum width of the rust or blister that occurred is 3 mm or more from the cross-cut part.
[0116] [Table 3]
[0117] [Table 4]
[0118] [Table 5]
[0119] Examples 1 to 23 are examples of the present disclosure, and even when a coating film was formed by a single application and dried at room temperature, the drying properties were good to the touch, and the appearance, corrosion resistance, and blocking resistance of the resulting coating film were good.
[0120] Comparative Example 1 is an example in which a material was used in which the glass transition temperature of the entire resin of the core-shell type acrylic resin emulsion, which is one of the coating film-forming resins, was less than 30°C, and the blocking resistance of the obtained coating film was not fully satisfactory. Comparative Example 2 is an example in which a material was used in which the glass transition temperature of the entire resin of the core-shell type acrylic resin emulsion, which is one of the coating film-forming resins, exceeded 50°C, and the crack resistance and corrosion resistance of the obtained coating film were not fully satisfactory. Comparative Example 3 is an example in which a material was used in which the glass transition temperature of the entire resin of the single-layer acrylic resin emulsion, which is one of the coating film-forming resins, was less than -20°C, and the blocking resistance and corrosion resistance of the obtained coating film were not fully satisfactory. Comparative Example 4 is an example in which a material was used in which the glass transition temperature of the entire resin of the single-layer acrylic resin emulsion, which is one of the coating film-forming resins, exceeded 0°C, and the crack resistance of the obtained coating film was not fully satisfactory. Comparative Example 5 is an example that did not contain the core-shell type acrylic resin emulsion (A1) as a coating film-forming resin, and the crack resistance and blocking resistance of the obtained coating film were not fully satisfactory. Comparative Example 6 is an example that does not contain the rust-preventive pigment (B), and the corrosion resistance of the resulting coating film was not fully satisfactory. Comparative Example 7 is an example that did not contain resin beads (C), and the blocking resistance of the obtained coating film was not fully satisfactory. [Industrial Applicability]
[0121] The aqueous coating composition of the present disclosure forms a coating film in a single application and has good tactile dryness even when dried at room temperature, and the resulting coating film has good appearance, corrosion resistance, and blocking resistance, and can be suitably used in a variety of fields, including architectural exteriors, building materials, bridges, ships, vehicles, industrial machinery, construction machinery, and automobiles.
Claims
1. The coating composition comprises a film-forming resin (A), an anti-rust pigment (B) and resin beads (C), the coating film-forming resin (A) comprises an acrylic resin emulsion (A1) and an acrylic resin emulsion (A2); The acrylic resin emulsion (A1) contains a core-shell type acrylic resin emulsion having a core portion and a shell portion, The acrylic resin emulsion (A2) contains a single-layer type acrylic resin emulsion, the glass transition temperature of the entire acrylic resin of the acrylic resin emulsion (A1) is 30° C. or higher and 50° C. or lower; the glass transition temperature of the entire acrylic resin of the acrylic resin emulsion (A2) is −20° C. or higher and 0° C. or lower; Water-based paint composition.
2. 2. The aqueous coating composition according to claim 1, wherein the glass transition temperature of the shell part of the core-shell type acrylic resin emulsion is higher than the glass transition temperature of the core part of the core-shell type acrylic resin emulsion.
3. 2. The aqueous coating composition according to claim 1, wherein the ratio of the solid content of said acrylic resin emulsion (A1) to the solid content of said acrylic resin emulsion (A2) is 90:10 to 50:
50.
4. 2. The aqueous coating composition according to claim 1, wherein the content of said anti-rust pigment (B) is 1 part by mass or more and 50 parts by mass or less per 100 parts by mass of the solid content of said coating film-forming resin (A).
5. 2. The aqueous coating composition according to claim 1, wherein the resin beads (C) have an average particle size of 1 μm or more.
6. 2. The aqueous coating composition according to claim 1, wherein the content of said resin beads (C) is from 1 part by mass to 30 parts by mass per 100 parts by mass of the solid content of said coating film-forming resin (A).
7. 2. The aqueous coating composition according to claim 1, further comprising a film-forming auxiliary (D), the content of which is 1 part by mass or more and 40 parts by mass or less per 100 parts by mass of the solid content of the coating film-forming resin (A).
8. Preheat the workpiece to 60°C or higher and 110°C or lower; and A method for producing a coating film, comprising: applying the aqueous coating composition according to any one of claims 1 to 7 to the surface of the substrate after the preheating, and forming a coating film.
Citation Information
Patent Citations
Resin composition for aqueous coating
JP2003128981A
Aqueous resin dispersion
JP2008063567A
Corrosion resistant layer for metal pipe
JP2020002330A
Coating composition
JP2022041147A