Biodegradable resin composition, method for producing the same and molding

A poly(3-hydroxybutyrate) resin composition with specific glycerin fatty acid esters addresses the antistatic shortcomings of biodegradable resins, ensuring rapid and sustained antistatic performance and mechanical strength in molded products.

JP2024145936APending Publication Date: 2024-10-15KANEKA CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023058553
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing biodegradable poly(3-hydroxybutyrate)-based resins suffer from insufficient antistatic properties immediately after molding, leading to issues like dust and metal scum adhesion, which can compromise the quality and safety of food contact products such as straws and cutlery.

Method used

A resin composition comprising a poly(3-hydroxybutyrate) resin component and two distinct glycerin fatty acid ester antistatic agents, with specific carbon chain lengths, is formulated and processed under controlled temperature and cooling conditions to ensure rapid and sustained antistatic performance without compromising mechanical strength.

Benefits of technology

The resin composition achieves excellent antistatic properties immediately after molding, enhancing the production efficiency and quality of molded articles by preventing foreign matter adhesion, while maintaining mechanical integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145936000001
    Figure 2024145936000001
Patent Text Reader

Abstract

To provide a resin composition which is suitably usable for manufacturing a molding that has excellent anti-static properties immediately after molding, and also has excellent mechanical strength, and contains a poly(3-hydroxybutyrate)-based resin component and an anti-static agent.SOLUTION: A resin composition contains a poly(3-hydroxybutyrate)-based resin component (A), and a first anti-static agent component (B1) and a second anti-static agent component (B2) which are different from each other as anti-static components, wherein 0.1 pt.wt. or more and less than 5 pts.wt. of the first anti-static agent component (B1) and 0.1 pt.wt. or more and less than 10 pts.wt. of the second anti-static agent component (B2) are contained with respect to 100 pts.wt. of the poly(3-hydroxybutyrate)-based resin component (A).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition containing a poly(3-hydroxybutyrate) resin and an antistatic agent, a production method thereof, and a molded article thereof. [Background technology]

[0002] In recent years, environmental issues caused by waste plastics have been attracting attention. In particular, marine pollution caused by waste plastics is serious, and there are hopes for the widespread use of biodegradable resins that decompose in the natural environment.

[0003] Various types of such biodegradable resins are known, but among them, poly(3-hydroxybutyrate) resins, in particular a copolymer of 3-hydroxybutyrate (hereinafter sometimes referred to as "3HB") and 3-hydroxyhexanoate (hereinafter sometimes referred to as "3HH") (hereinafter sometimes referred to as "PHBH"), are thermoplastic polyesters that are produced and accumulated as energy storage substances within the cells of many microbial species, and are a material that can biodegrade not only in soil but also in seawater, and therefore have attracted attention as a material that can solve the above problems.

[0004] Since PHBH is a material in which the copolymerization ratio of 3-hydroxybutyrate and 3-hydroxyhexanoate and the weight-average molecular weight can be controlled relatively easily, its tensile properties, bending properties, etc. can be easily adjusted to suit the intended application and shape. Taking advantage of this feature, it has been deployed in many food contact applications in recent years, such as cutlery and straws.

[0005] On the other hand, PHBH is easily charged with static electricity, and charging during the transportation process of the molded body and the secondary processing process of the molded body often becomes a problem. Excessive charging can attract dust, dirt, metal shavings, etc. during the process, increasing the risk of foreign matter being mixed into packages such as cutlery and straws. Patent Document 1 discloses a resin composition that is difficult to charge, in which a specific aliphatic polyester resin antistatic agent is kneaded into a poly(3-hydroxybutyrate) resin or a polybutylene succinate resin to reduce the surface resistivity, and a technology for using the resin composition. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2021-50286 A Summary of the Invention [Problem to be solved by the invention]

[0007] It is believed that the molded article containing the resin composition of Patent Document 1 exhibits antistatic properties due to bleeding out of the antistatic agent onto the surface of the molded article, etc., and the antistatic properties may not be sufficiently exhibited for several days immediately after molding, leaving room for improvement. From the viewpoint of preventing adhesion of foreign matter to the molded article during the manufacturing process of food contact articles such as straws and cutlery and the product packaging process, there has been a demand for the molded article to have sufficient antistatic properties for several days immediately after molding.

[0008] In view of the above-mentioned current situation, the present invention aims to provide a resin composition containing a poly(3-hydroxybutyrate)-based resin component and an antistatic agent, which has excellent antistatic properties even immediately after molding and can be suitably used for producing molded articles that are also excellent in mechanical strength. [Means for solving the problem]

[0009] As a result of intensive research aimed at solving the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by a resin composition containing a poly(3-hydroxybutyrate)-based resin component (A) and at least two different antistatic agent components, which are glycerin-based fatty acid esters, in specific amounts, and have thus completed the present invention.

[0010] That is, the present invention relates to a poly(3-hydroxybutyrate)-based resin component (A), A resin composition comprising a first antistatic agent component (B1) and a second antistatic agent component (B2), the first antistatic agent component (B1) and the second antistatic agent component (B2) are different from each other, the first antistatic agent component (B1) is a fatty acid ester selected from the group of fatty acid esters consisting of monoglycerol fatty acid esters, diglycerol fatty acid esters, and polyglycerol fatty acid esters, and includes at least one fatty acid ester having a saturated fatty acid residue with a carbon number of 14, 16, 18, 20, or 22; the second antistatic agent component (B2) is a fatty acid ester selected from the group of fatty acid esters consisting of monoglycerol fatty acid esters, diglycerol fatty acid esters, and polyglycerol fatty acid esters, and includes at least one fatty acid ester having a saturated fatty acid residue with 6, 8, 10, or 12 carbon atoms; For 100 parts by weight of the poly(3-hydroxybutyrate)-based resin component (A), The first antistatic agent component (B1) is 0.1 parts by weight or more and less than 5 parts by weight, The present invention relates to a resin composition comprising 0.1 parts by weight or more and less than 10 parts by weight of the second antistatic agent component (B2).

[0011] The present invention also relates to a molded article comprising the above-mentioned resin composition.

[0012] The present invention also provides a method for producing a poly(3-hydroxybutyrate)-based resin component (A), the first antistatic agent component (B1), and the second antistatic agent component (B2), comprising: a step (first step) of feeding a resin mixture containing the poly(3-hydroxybutyrate)-based resin component (A), the first antistatic agent component (B1), and the second antistatic agent component (B2) into an extruder equipped with a die at its tip, and melt-extruding the mixture so that the temperature of the mixture at the die outlet is 150° C. or higher and lower than 175° C.; The present invention also relates to a method for producing the resin composition, which sequentially includes a step (second step) of cooling the mixture discharged from the die outlet at a temperature of 30°C or higher and lower than 90°C for a cooling time of 5 seconds or higher and lower than 20 seconds. Effect of the Invention

[0013] According to the present invention, there is provided a resin composition containing a poly(3-hydroxybutyrate)-based resin component and an antistatic agent, which has excellent antistatic properties even immediately after molding and can be suitably used for producing a molded article having excellent mechanical strength. The resin composition of the present invention makes it possible to improve the production efficiency and quality of molded articles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, an embodiment of the present invention will be described, however, the present invention is not limited to the following embodiment. [Resin composition] The resin composition according to this embodiment contains a poly(3-hydroxybutyrate)-based resin component (A) described below, a first antistatic agent component (B1) and a second antistatic agent component (B2) which are different from each other and are selected from the group consisting of monoglycerin fatty acid esters, diglycerin fatty acid esters, and polyglycerin fatty acid esters, and may contain other additives within the scope of not impairing the effects of the present invention.

[0015] [Poly(3-hydroxybutyrate) resin component (A)] As the poly(3-hydroxybutyrate)-based resin component (A) according to this embodiment, a poly(3-hydroxybutyrate)-based resin (hereinafter sometimes referred to as P3HB) is a polymer having a 3-hydroxybutyrate unit, and specifically, it is preferable that the poly(3-hydroxybutyrate)-based resin is a polymer having a unit represented by the following general formula (1). [-CHCH3-CH2-CO-O-] (1) The poly(3-hydroxybutyrate)-based resin is preferably a poly(3-hydroxybutyrate)-based resin produced from a microorganism, in which all 3-hydroxybutyrate units are contained as (R)-3-hydroxybutyrate units.

[0016] The poly(3-hydroxybutyrate) resin preferably contains 3-hydroxybutyrate units (particularly units represented by general formula (1)) in an amount of 50 mol % or more, more preferably 60 mol % or more, and even more preferably 70 mol % or more of the total structural units. The poly(3-hydroxybutyrate) resin may contain only 3-hydroxybutyrate units as structural units of the polymer, or may contain 3-hydroxybutyrate units and one or more types of 3-hydroxyalkanoate units other than the 3-hydroxybutyrate units or other units (e.g., 4-hydroxyalkanoate units, etc.).

[0017] In the poly(3-hydroxybutyrate)-based resin component (A) according to the present embodiment, it is preferable that all of the 3-hydroxybutyrate units are (R)-3-hydroxybutyrate units. Also, it is preferable that the poly(3-hydroxyalkanoate)-based resin is a copolymer of 3-hydroxybutyrate units and other hydroxyalkanoate units.

[0018] Specific examples of poly(3-hydroxybutyrate)-based resins include poly(3-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxypropionate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (abbreviation: P3HB3HV), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (abbreviation: P3HB3HH), Examples of such poly(3-hydroxybutyrate-co-3-hydroxyheptanoate), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate), poly(3-hydroxybutyrate-co-3-hydroxynonanoate), poly(3-hydroxybutyrate-co-3-hydroxydecanoate), poly(3-hydroxybutyrate-co-3-hydroxyundecanoate), poly(3-hydroxybutyrate-co-4-hydroxybutyrate) (abbreviation: P3HB4HB), and the like.In particular, from the viewpoint of achieving both processability into molded articles and physical properties of the obtained molded articles, poly(3-hydroxybutyrate) (PHB), poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHB3HV), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (PHB3HH), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-co-3-hydroxyhexanoate) (PHB3HV3HH), poly(3-hydroxybutyrate-co-4-hydroxybutyrate) (PHB4HB), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate) (PHB3HO), poly(3-hydroxybutyrate-co-3-hydroxyoctadecanoate) (PHB3 Preferably usable are poly(3-hydroxybutyrate-co-3-hydroxydecanoate) (PHB3HD), and in particular, poly(3-hydroxybutyrate-co-3-hydroxyvalerate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-4-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate) and poly(3-hydroxybutyrate-co-3-hydroxydecanoate), with PHB3HH being the most preferred due to ease of industrial production.

[0019] In addition, the poly(3-hydroxybutyrate)-based resin component (A) may contain one or more biodegradable resins other than P3HB, such as aliphatic polyester-based resins such as polycaprolactone, polybutylene succinate adipate, polybutylene succinate, and polylactic acid, and aliphatic aromatic polyester-based resins such as polybutylene adipate terephthalate and polybutylene azelate terephthalate, as long as the effects of the present invention are not impaired.

[0020] In addition, the poly(3-hydroxybutyrate)-based resin component (A) may contain one or more of other additives that are usually added to resin materials, such as inorganic fillers, colorants such as pigments and dyes, odor absorbers such as activated carbon and zeolite, fragrances such as vanillin and dextrin, plasticizers, antioxidants, weather resistance improvers, ultraviolet absorbers, crystal nucleating agents, lubricants, release agents, water repellents, antibacterial agents, sliding property improvers, and other secondary additives, within the scope of not impairing the effects of the present invention. However, these are optional components, and the poly(3-hydroxybutyrate)-based resin component (A) may not contain these components, as well as the poly(3-hydroxybutyrate)-based resin component (A). As optional components, lubricants and inorganic fillers are preferably used from the viewpoint of further improving the molding stability of the poly(3-hydroxybutyrate)-based resin component (A).

[0021] Examples of the lubricant include saturated or unsaturated fatty acid amides such as lauric acid amide, myristic acid amide, palmitic acid amide, stearic acid amide, behenic acid amide, oleic acid amide, and erucic acid amide; alkylene fatty acid amides such as methylene bisstearic acid amide and methylene bisstearic acid amide; and aliphatic amide compounds, such as pentaerythritol.

[0022] The amount of the lubricant in the poly(3-hydroxybutyrate)-based resin component (A) is preferably 0.1 to 2 parts by weight, more preferably 0.2 to 1 part by weight, based on 100 parts by weight of the poly(3-hydroxybutyrate)-based resin component (A). By making the amount 0.1 part by weight or more, it is possible to obtain an effect of improving the releasability by adding the lubricant. On the other hand, if the amount exceeds 2 parts by weight, the lubricant bleeds out during compression and adheres to the compression surface of the cooling roll, etc., which makes it difficult to perform continuous processing for a long time.

[0023] Examples of the inorganic filler include talc, calcium carbonate, mica, silica, clay, kaolin, titanium oxide, alumina, and zeolite, each having an average particle size of 0.5 μm or more.

[0024] The amount of inorganic filler in the poly(3-hydroxybutyrate)-based resin component (A) is preferably 0.5 to 5 parts by weight, more preferably 1 to 3 parts by weight, based on 100 parts by weight of the poly(3-hydroxybutyrate)-based resin component (A). By making the amount 0.5 parts by weight or more, it is possible to obtain an effect of improving the releasability by adding the inorganic filler. On the other hand, if the amount exceeds 5 parts by weight, the molded article may be easily cracked.

[0025] Among poly(3-hydroxybutyrate) resins, PHBH in particular is an especially useful plastic industrially because its melting point and crystallinity can be altered by changing the composition ratio of the repeating units, and as a result, its physical properties such as Young's modulus and heat resistance can be easily adjusted, and it is also possible to impart physical properties between those of polypropylene and polyethylene.

[0026] A specific method for producing PHBH is described in, for example, International Publication No. 2010 / 013483. Commercially available PHBH products include Kaneka Biodegradable Polymer Green Planet (registered trademark) manufactured by Kaneka Corporation.

[0027] The ratio of 3-hydroxyhexanoate (3HH) in the PHBH is not particularly limited, but the ratio of 3HH is preferably 2 mol% or more and less than 25 mol%, and more preferably 3 mol% or more and 15 mol% or less. When the ratio of 3HH in the PHBH contained in the poly(3-hydroxybutyrate)-based resin component (A) is 2 mol% or more, the melting point does not become too high and the difference between the decomposition temperature and the processing temperature can be set large, so that stable extrusion processing is possible. In addition, PHBH having a ratio of 3HH of less than 25 mol% does not have a too slow crystallization rate, and it is relatively easy to manufacture a pellet-shaped compound containing PHBH. The ratio of 3HH is the monomer ratio of 3HH to all monomers constituting PHBH, and can be determined by a method known to those skilled in the art, for example, the method described in paragraph

[0047] of International Publication WO 2013 / 147139 or by NMR measurement. In addition, when multiple PHBHs are contained, it is the ratio to the total amount of constituent monomers contained in all components of PHBH.

[0028] The weight average molecular weight (hereinafter sometimes referred to as Mw) of the entire poly(3-hydroxybutyrate)-based resin component (A) according to this embodiment is preferably 100,000 or more and less than 750,000, more preferably 200,000 or more and less than 650,000, and even more preferably 250,000 or more and less than 550,000, from the viewpoint of achieving both an appropriate crystallization rate and mechanical strength. If the weight average molecular weight is less than 100,000, there is a possibility that the amount of elution during heating will increase, and not only may the container be unusable as a food container, but the contribution of decomposition products during extrusion processing may become large, and extrusion processability may become unstable. If the weight average molecular weight exceeds 750,000, the melt viscosity will increase, and there is a possibility that problems will occur in appearance, such as the surface of the extruded molded product becoming rough. In this application, the weight average molecular weight of PHBH can be determined as the molecular weight converted into polystyrene by gel permeation chromatography (GPC) (Shodex GPC-101 manufactured by Showa Denko K.K.) using polystyrene gel (Shodex K-804 manufactured by Showa Denko K.K.) as a column and chloroform as a mobile phase.

[0029] In this embodiment, a mixture of multiple types of PHBH having different weight average molecular weights can be used for the poly(3-hydroxybutyrate) resin component (A).

[0030] In addition, when a mixture of multiple types of PHBH is used, or when other resin components are mixed, the weight average molecular weight of the poly(3-hydroxybutyrate)-based resin component (A) refers to the weight average molecular weight of the entire poly(3-hydroxybutyrate)-based resin component (A).

[0031] [First antistatic agent component (B1)] The first antistatic agent component (B1) according to this embodiment desirably contains at least one type of material exhibiting good dispersibility and compatibility with the poly(3-hydroxybutyrate)-based resin component (A) during melt processing, and contains at least one type of fatty acid ester having a saturated fatty acid residue with a carbon number of 14, 16, 18, or 20 selected from the group of fatty acid esters consisting of monoglycerin fatty acid esters, diglycerin fatty acid esters, and polyglycerin fatty acid esters, which tends to exhibit high antistatic properties while suppressing the influence on mechanical properties such as the tensile modulus of elasticity of the resulting molded article. The fatty acid esters can be used alone, or two or more types of resins can be mixed in any ratio as necessary.

[0032] In the resin composition according to the present embodiment, the content of the first antistatic agent (B1) is 0.1 parts by weight or more and less than 5 parts by weight, preferably 0.3 parts by weight or more and less than 4 parts by weight, and more preferably 0.5 parts by weight or more and less than 3 parts by weight, relative to 100 parts by weight of the poly(3-hydroxybutyrate)-based resin component (A) in terms of excellent electrostatic chargeability and mechanical properties of the resulting molded article. If it is 0.1 parts by weight or less, the antistatic effect is not fully exhibited, and if it is 5 parts by weight or more, the molded article may be excessively plasticized, resulting in insufficient mechanical strength of the molded article, or the antistatic agent component that bleeds out on the surface of the molded article may crystallize over a long period of time, resulting in loss of antistatic properties.

[0033] [Second antistatic agent component (B2)] The second antistatic agent component (B2) according to this embodiment preferably contains at least one type of material that has a minimum level of dispersibility and compatibility with the poly(3-hydroxybutyrate)-based resin component (A) during melt processing, and in addition, quickly bleeds out with the crystallization of the poly(3-hydroxybutyrate)-based resin component (A), specifically, it contains at least one type of fatty acid ester having a saturated fatty acid residue with a carbon number of 6, 8, 10, or 12 selected from the group of aliphatic esters consisting of monoglycerin fatty acid esters, diglycerin fatty acid esters, and polyglycerin fatty acid esters, and this tends to enable the antistatic property to be exhibited immediately after molding (excellent immediate effect). These resins can be used alone, or two or more types can be mixed in any ratio as necessary.

[0034] In the resin composition according to the present embodiment, the content of the second antistatic agent (B2) is 0.1 parts by weight or more and less than 10 parts by weight, preferably 0.5 parts by weight or more and less than 7 parts by weight, and more preferably 1 part by weight or more and less than 5 parts by weight, relative to 100 parts by weight of the poly(3-hydroxybutyrate)-based resin component (A) in terms of excellent electrostatic properties and rapid action of the resulting molded article. If it is 0.1 parts by weight or less, not only is the antistatic effect not fully exhibited, but bleeding out from the resin composition is slow, and rapid action may be poor. If it is 10 parts by weight or more, the molded article may be excessively plasticized, resulting in insufficient mechanical strength of the molded article.

[0035] In this embodiment, the value (B1 / B2) obtained by dividing the content of the first antistatic agent component (B1) by the content of the second antistatic agent component (B2) is preferably 0.1 or more and less than 5.0, more preferably 0.2 or more and less than 3.0, and even more preferably 0.3 or more and less than 1.0. By being within this range, it is possible to quickly develop sufficient antistatic properties after molding without excessively decreasing the tensile modulus of the molded article. [Method for producing resin composition] The resin composition according to the present embodiment can be produced by melt-kneading each component by a general method, for example, by feeding each component into an extruder equipped with a die at the tip and melt-kneading the resin mixture containing each component, and may be cooled and pelletized after melt-kneading. That is, the resin composition can be produced by a method that sequentially includes a step of feeding a mixture of resins containing the poly(3-hydroxybutyrate)-based resin component and the second antistatic agent component into an extruder equipped with a die at the tip and melt-extruding the mixture (first step), and a step of cooling the mixture discharged from the die outlet (second step). The following is a detailed description.

[0036] First, poly(3-hydroxybutyrate)-based resin component (A), first antistatic agent component (B1), second antistatic agent component (B2), and any additives as necessary are added, and melt-kneaded using an extruder, kneader, Banbury mixer, roll, or the like to prepare a resin composition. The resin composition may be extruded into a strand shape and then cut to obtain pellets having a particle shape such as a cylindrical shape, an elliptical cylindrical shape, a spherical shape, a cubic shape, or a rectangular parallelepiped shape. The prepared pellets are desirably thoroughly dried at 40 to 80°C to remove moisture, and then subjected to the next molding.

[0037] The temperature at which the melt kneading is carried out cannot be generally defined because it depends on the melting point, melt viscosity, etc. of the resin used, but the temperature of the resin mixture at the die outlet of the melt kneaded product is preferably 150° C. to 175° C., more preferably 155° C. to 170° C., even more preferably 158° C. to 167° C., and particularly preferably 160° C. to 165° C. If the resin temperature of the melt kneaded product is less than 150° C., the poly(3-hydroxybutyrate)-based resin component (A) may not melt, and if it exceeds 175° C., the poly(3-hydroxybutyrate)-based resin component (A) may be thermally decomposed.

[0038] In order to promote solidification, the resin composition discharged from the die outlet is preferably cooled at a temperature of 30° C. or more and less than 90° C. for a cooling time of 5 seconds or more and less than 20 seconds.

[0039] That is, in the method for producing a resin composition according to this embodiment, the method includes a step (first step) of feeding a resin mixture containing the poly(3-hydroxybutyrate)-based resin component (A), the first antistatic agent component (B1), and the second antistatic agent component (B2) into an extruder equipped with a die at its tip, and melt-extruding the mixture so that the temperature of the mixture at the die outlet is 150° C. or higher and lower than 175° C.; and a step (second step) of cooling the mixture discharged from the die outlet at a temperature of 30° C. or more and less than 90° C. for a cooling time of 5 seconds or more and less than 20 seconds. [Molded body] The resin composition according to the present embodiment can be used to produce a molded product by various molding methods such as extrusion molding, injection molding, calendar molding, etc. Also, a laminate can be produced by extrusion lamination, thermal lamination, coating, etc. on a substrate such as paper. [Resin tube] The thickness of the resin tube according to the present embodiment is preferably 0.01 mm to 0.6 mm, more preferably 0.05 mm to 0.5 mm, and even more preferably 0.1 mm to 0.4 mm, because it is not crushed by suction when drinking a beverage as a straw, has moderate flexibility, is unlikely to break, is unlikely to cause injury when poking a fingertip, and is rapidly biodegradable even in seawater. The outer diameter of the resin tube is not particularly limited, but is preferably 2 to 10 mm, more preferably 4 to 8 mm, and even more preferably 5 to 7 mm, from the viewpoint of ease of use when drinking a beverage as a straw. The cross-sectional shape of the biodegradable resin tube is approximately circular, but from the viewpoint of usability as a straw or pipe, the closer to a perfect circle the more preferable. Therefore, the flatness of the cross-sectional shape of the resin tube [100 x (maximum outer diameter - minimum outer diameter) / maximum outer diameter] is preferably 10% or less, more preferably 8% or less, even more preferably 5% or less, and even more preferably 3% or less. A flatness of 0% means that the cross-sectional shape is a perfect circle.

[0040] The length of the resin tube is not particularly limited, but when the resin tube is used as a straw, the length of the resin tube is preferably 50 to 350 mm, more preferably 70 to 300 mm, and even more preferably 90 to 270 mm, from the viewpoint of ease of use when using the tube as a straw to drink a beverage. When the resin tube is used as a straw, it may be a tube that has not been subjected to secondary processing, or a tube that has been subjected to secondary processing such as the formation of a stopper portion or a bellows portion. The resin tube according to the present embodiment can be manufactured by a known method, for example, by melting a blend of the resin composition according to the present embodiment and any additives in an extruder, extruding it from an annular die connected to the outlet of the extruder, and pouring it into water to solidify it into a tubular shape.

[0041] The following items enumerate preferred aspects of the present disclosure, but the present invention is not limited to the following items. [Item 1] Poly(3-hydroxybutyrate)-based resin component (A), A resin composition comprising a first antistatic agent component (B1) and a second antistatic agent component (B2), the first antistatic agent component (B1) and the second antistatic agent component (B2) are different from each other, the first antistatic agent component (B1) is a fatty acid ester selected from the group of fatty acid esters consisting of monoglycerol fatty acid esters, diglycerol fatty acid esters, and polyglycerol fatty acid esters, and includes at least one fatty acid ester having a saturated fatty acid residue with a carbon number of 14, 16, 18, 20, or 22; the second antistatic agent component (B2) is a fatty acid ester selected from the group of fatty acid esters consisting of monoglycerol fatty acid esters, diglycerol fatty acid esters, and polyglycerol fatty acid esters, and includes at least one fatty acid ester having a saturated fatty acid residue with 6, 8, 10, or 12 carbon atoms; For 100 parts by weight of the poly(3-hydroxybutyrate)-based resin component (A), The first antistatic agent component (B1) is 0.1 parts by weight or more and less than 5 parts by weight, A resin composition comprising 0.1 parts by weight or more and less than 10 parts by weight of the second antistatic agent component (B2). [Item 2] 2. The resin composition according to item 1, wherein a value (B1 / B2) obtained by dividing the content of the first antistatic agent component (B1) by the content of the second antistatic agent component (B2) is 0.1 or more and less than 5.0. [Item 3] 3. The resin composition according to item 1 or 2, wherein the poly(3-hydroxybutyrate)-based resin component (A) comprises a poly(3-hydroxybutyrate)-based copolymer containing 3-hydroxybutyrate units and other hydroxyalkanoate units. [Item 4] Item 4. The resin composition according to item 3, wherein the poly(3-hydroxybutyrate)-based copolymer is at least one selected from the group consisting of poly(3-hydroxybutyrate-co-3-hydroxyvalerate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-4-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate) and poly(3-hydroxybutyrate-co-3-hydroxydecanoate). [Item 5] 4. The resin composition according to item 3, which simultaneously satisfies the following requirements (a) and (b): (a) The poly(3-hydroxybutyrate)-based resin component (A) contains poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) containing 3 mol % or more and less than 15 mol % of 3-hydroxyhexanoate units as other hydroxyalkanoate units. (b) the weight average molecular weight of the entire poly(3-hydroxybutyrate)-based resin component (A) is 250,000 or more and less than 550,000; [Item 6] A molded article comprising the resin composition according to any one of items 1 to 5. [Item 7] 7. The molded article according to item 6, which is a resin tube. [Item 8] a step (first step) of feeding a resin mixture containing the poly(3-hydroxybutyrate)-based resin component (A), the first antistatic agent component (B1), and the second antistatic agent component (B2) into an extruder equipped with a die at its tip, and melt-extruding the mixture so that the temperature of the mixture at the die outlet is 150° C. or higher and lower than 175° C.; and a step (a second step) of cooling the mixture discharged from the die outlet at a temperature of 30° C. or higher and lower than 90° C. for a cooling time of 5 seconds or higher and lower than 20 seconds. EXAMPLES

[0042] The present invention will be specifically described below with reference to examples, but the technical scope of the present invention is not limited to these examples.

[0043] [Raw materials used] The following raw materials were used in each of the Examples and Comparative Examples. (Poly(3-hydroxybutyrate)-based resin component (A)) The PHBH powder used in the poly(3-hydroxybutyrate) resin component (A) used in the examples and comparative examples was produced in accordance with the method described in International Publication WO2019-142845. The specific formulation is shown below. PHBH powder 1: Low-crystalline PHBH powder with a weight-average molecular weight of 400,000 and a ratio of 3HH to the total of 3HB and 3HH in PHBH of 9 mol%. PHBH powder 2: Low-crystalline PHBH powder with a weight-average molecular weight of 300,000 and a ratio of 3HH to the total of 3HB and 3HH in PHBH of 9 mol%. PHBH powder 3: Highly crystalline PHBH powder with a weight-average molecular weight of 500,000 and a ratio of 3HH to the total of 3HB and 3HH in PHBH of 9 mol%. PHBH powder 4: Highly crystalline PHBH powder with a weight-average molecular weight of 400,000 and a ratio of 3HH to the total of 3HB and 3HH in PHBH of 4 mol%. (Antistatic agent) Rikemal S-100 (glycerin monostearate): manufactured by Riken Vitamin Co., Ltd.; contains saturated fatty acid residues with 18 carbon atoms as the main component Rikemal B-100 (glycerin monobehenate): manufactured by Riken Vitamin Co., Ltd.; contains saturated fatty acid residues with 22 carbon atoms as the main component Poem DS-100A (Diglycerol Monostearate): Manufactured by Riken Vitamin Co., Ltd.; Contains saturated fatty acid residues with 18 carbon atoms as the main component Biosizer: manufactured by Riken Vitamin Co., Ltd.; contains saturated fatty acid residues with 12 carbon atoms as the main component Poem M-100 (glycerin monocaprylate): manufactured by Riken Vitamin Co., Ltd.; contains saturated fatty acid residues with 8 carbon atoms as the main component Poem M-200 (glycerin monocaprate): manufactured by Riken Vitamin Co., Ltd.; contains saturated fatty acid residues with 10 carbon atoms as the main component Example 1 [Preparation of strands of resin composition] PHBH powder 1 (100 parts by weight) was dry-blended with behenic acid amide (0.5 parts by weight) as a crystal nucleating agent and lubricant, Rikemal S100 (1.0 parts by weight) as the first antistatic agent (B1), and Biocizer (3.0 parts by weight) as the second antistatic agent (B2), and melt-kneaded and extruded into strands using a twin-screw extruder so that the die outlet resin temperature immediately after leaving the extruder was 168°C, and pellets were obtained by cooling with water at 40°C, solidifying, and cutting. At this time, the time for cooling with water (cooling time) was adjusted to 15 seconds.

[0044] The antistatic effect and tensile modulus of elasticity of the obtained strands (or pellets) were measured, and the results are shown in Table 1. The evaluation was performed by the following methods.

[0045] (Evaluation of antistatic properties) This evaluation was carried out immediately after the strand obtained above was aged in a constant temperature and humidity environment of 23° C. and 50% humidity for 1 day after production.

[0046] Cylindrical strands cut to a length of 250 mm and a cross-sectional diameter of 3 to 5 mm were laid out tightly in a SUS304 container with a length of 300 mm and a width of 200 mm. A smaller container made of the same material as the above container was placed on top of the strands, and the strands were rubbed together along the length of the strands for 30 seconds to generate static electricity on the surface, charging the strands. The amount of charge on the surface of the biodegradable resin strands was measured using a digital static electricity detector (model number: EG-1) manufactured by Sanhayato Co., Ltd.

[0047] <Evaluation criteria> ◎: Less than 0.1 kV ○: 0.1 kV or more and less than 0.5 kV △: 0.6kV or more and less than 2.0kV ×: 2.0kV or more If the above evaluation result is ⊚, ◯, or Δ, it indicates that the antistatic property is rapid and sufficient. (Evaluation of tensile modulus) This evaluation was carried out immediately after the strand obtained above was aged in a constant temperature and humidity environment of 23° C. and 50% humidity for 7 days after production.

[0048] The tensile tester used was a Shimadzu Autograph EZ-LX (Shimadzu Corporation), and the sample was set so that the distance between the grippers was 80 mm. The sample was then pulled at a tensile speed of 200 mm / min until it broke. The tensile modulus was calculated in the elastic deformation region of strain between 1.0% and 5.0% from the obtained stress-strain curve.

[0049] <Evaluation criteria> ◎: 1600MPa or more ○: 1400MPa or more and less than 1600MPa △: 1200MPa or more and less than 1400MPa ×: Less than 1200MPa If the above evaluation result is ⊚, ◯, or Δ, the sample has a sufficient tensile modulus and is excellent in mechanical strength. [Making resin tubes] The strand obtained by the above method was used to prepare a resin tube by the following method.

[0050] The cylinder temperature and die temperature of a φ50 mm single screw extruder connected to an annular die (outer diameter 15 mm, inner diameter 13.5 mm) were set to 150°C, and the strand pellets were added and extruded into a tube. The extruded tube was passed through 40°C water located 100 mm away from the annular die and taken up by a take-up machine at a speed of 60 m / min, yielding a resin tube with an outer diameter of 6 mm, a wall thickness of 0.2 mm, and a length of 200 mm. (Adhesion of foreign matter to resin tubes) The obtained resin tube was left to stand at room temperature and normal pressure for one day, and then the outer surface of the resin tube was wiped with cotton gauze. At that time, the number of foreign matter with a long side of 0.5 mm or more among the foreign matter wiped off with the gauze was counted, and the adhesion of the foreign matter was evaluated according to the following evaluation criteria, and the results are shown in Table 1. <Evaluation criteria> ◎:0 pieces 〇:1 piece △:2~3 pieces ×: 4 or more If the above evaluation result is ⊚, ◯, or Δ, it indicates that the antistatic property is rapid and sufficient.

[0051] [Table 1]

[0052] (Examples 2 to 14, Comparative Examples 1 to 5) A strand and a resin tube were produced in the same manner as in Example 1, except that the blending or molding conditions (die outlet temperature, hot water passing time) were changed as shown in Table 1, and evaluations were carried out in the same manner as in Example 1. The results are summarized in Table 1.

[0053] <Result> From Table 1, it can be seen that in the examples, the antistatic effect was sufficiently exhibited even after several days from immediately after molding, and the obtained resin compositions had excellent mechanical strength in the resulting molded articles.

[0054] On the other hand, the comparative examples did not have sufficient antistatic properties immediately after molding and did not provide excellent mechanical strength for the molded article. Therefore, according to the present invention, by using a resin composition containing a poly(3-hydroxybutyrate)-based resin component (A) and at least two different antistatic agent components of glycerin-based fatty acid esters in specific ranges, it is possible to produce a molded article that has sufficient antistatic properties even immediately after molding and also has excellent mechanical strength.

Claims

1. Poly(3-hydroxybutyrate)-based resin component (A), A resin composition comprising a first antistatic agent component (B1) and a second antistatic agent component (B2), the first antistatic agent component (B1) and the second antistatic agent component (B2) are different from each other, the first antistatic agent component (B1) is a fatty acid ester selected from the group of fatty acid esters consisting of monoglycerol fatty acid esters, diglycerol fatty acid esters, and polyglycerol fatty acid esters, and includes at least one fatty acid ester having a saturated fatty acid residue with a carbon number of 14, 16, 18, 20, or 22; the second antistatic agent component (B2) is a fatty acid ester selected from the group of fatty acid esters consisting of monoglycerin fatty acid esters, diglycerin fatty acid esters, and polyglycerin fatty acid esters, and includes at least one fatty acid ester having a saturated fatty acid residue having 6, 8, 10, or 12 carbon atoms; For 100 parts by weight of the poly(3-hydroxybutyrate)-based resin component (A), The first antistatic agent component (B1) is 0.1 parts by weight or more and less than 5 parts by weight, A resin composition comprising 0.1 parts by weight or more and less than 10 parts by weight of the second antistatic agent component (B2).

2. 2. The resin composition according to claim 1, wherein a value (B1 / B2) obtained by dividing the content of the first antistatic agent component (B1) by the content of the second antistatic agent component (B2) is 0.1 or more and less than 5.

0.

3. The resin composition according to claim 1 or 2, wherein the poly(3-hydroxybutyrate)-based resin component (A) comprises a poly(3-hydroxybutyrate)-based copolymer containing 3-hydroxybutyrate units and other hydroxyalkanoate units.

4. The resin composition according to claim 3, wherein the poly(3-hydroxybutyrate)-based copolymer is at least one selected from the group consisting of poly(3-hydroxybutyrate-co-3-hydroxyvalerate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-4-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate) and poly(3-hydroxybutyrate-co-3-hydroxydecanoate).

5. The resin composition according to claim 3, which simultaneously satisfies the following requirements (a) and (b): (a) The poly(3-hydroxybutyrate)-based resin component (A) contains poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) containing 3 mol % or more and less than 15 mol % of 3-hydroxyhexanoate units as other hydroxyalkanoate units. (b) the weight average molecular weight of the entire poly(3-hydroxybutyrate)-based resin component (A) is 250,000 or more and less than 550,000;

6. A molded article comprising the resin composition according to claim 1 or 2.

7. The molded article according to claim 6, which is a resin tube.

8. a step (first step) of feeding a resin mixture containing the poly(3-hydroxybutyrate)-based resin component (A), the first antistatic agent component (B1), and the second antistatic agent component (B2) into an extruder equipped with a die at its tip, and melt-extruding the mixture so that the temperature of the mixture at the die outlet is 150° C. or higher and lower than 175° C.; 3. The method for producing a resin composition according to claim 1 or 2, further comprising the steps of: (a) cooling the mixture discharged from the die outlet at a temperature of 30° C. or more and less than 90° C. for a cooling time of 5 seconds or more and less than 20 seconds (a second step).

Citation Information

Patent Citations

  • Antistatic agent composition and saturated polyester resin composition

    JP2001146547A

  • Antistatic agent and antistatic resin composition

    JP2002047485A

  • Resin composition and use thereof