Secondary battery, and manufacturing method thereof
A protective layer composed of Li, P, and O in secondary batteries mitigates resistance issues by preventing reactions between metallic lithium and sulfide electrolytes, enhancing conductivity and stability.
Patent Information
- Application Number
- JP2023058624
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Secondary batteries with deposited metal lithium negative electrodes face increased resistance during charging and discharging due to reactions between metallic lithium and sulfide solid electrolytes.
Incorporating a protective layer containing Li, P, and O between the solid electrolyte layer and the negative electrode current collector, which suppresses reactions and maintains lithium ion conductivity.
The protective layer reduces resistance and enhances the stability of the battery by preventing the reductive decomposition of the sulfide solid electrolyte, thereby improving the battery's performance and longevity.
Smart Images

Figure 2024145979000001_ABST
Abstract
Description
[Technical field]
[0001] The present application discloses a secondary battery and a method for manufacturing the same. [Background technology]
[0002] Patent Document 1 discloses an all-solid-state battery including a positive electrode, a solid electrolyte layer, a negative electrode current collector, and a Li-Mg alloy that is deposited between the solid electrolyte layer and the negative electrode current collector upon charging. Patent Document 2 discloses an all-solid-state lithium secondary battery including a positive electrode, a solid electrolyte layer, a negative electrode, and a predetermined metal layer formed between the solid electrolyte layer and the negative electrode. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-184513 A [Patent Document 2] International Publication No. 2013 / 141241 Summary of the Invention [Problem to be solved by the invention]
[0004] Secondary batteries equipped with a deposition-type metallic lithium negative electrode have room for improvement in terms of resistance after charging and discharging. [Means for solving the problem]
[0005] The present application discloses the following aspects as means for solving the above problems. <Aspect 1> A secondary battery comprising: a positive electrode; a solid electrolyte layer; a protective layer; a negative electrode current collector; and metallic lithium that is deposited between the solid electrolyte layer and the negative electrode current collector upon charging; the solid electrolyte layer includes a sulfide solid electrolyte, the protective layer is present between the solid electrolyte layer and the negative electrode current collector, The protective layer contains Li, P and O as constituent elements. Secondary battery. <Aspect 2> The secondary battery of aspect 1, The protective layer contains Li, P, O, and N as constituent elements. Secondary battery. <Aspect 3> The secondary battery according to aspect 1 or 2, The protective layer is -7 Lithium ion conductivity of over S / cm. Secondary battery. <Aspect 4> The secondary battery according to any one of aspects 1 to 3, the negative electrode current collector has a metal foil and an Mg-containing layer provided on a surface of the metal foil, The Mg-containing layer is present between the protective layer and the metal foil. Secondary battery. <Aspect 5> A method for manufacturing a secondary battery, comprising: Coating one or both surfaces of the negative electrode current collector and the solid electrolyte layer with a protective layer to obtain a coating; Obtaining a laminate having a positive electrode, a solid electrolyte layer, a protective layer, and a negative electrode current collector in this order using the coating; and and charging the laminate to deposit metallic lithium between the solid electrolyte layer and the negative electrode current collector. the solid electrolyte layer includes a sulfide solid electrolyte, The protective layer contains Li, P and O. Manufacturing method. Effect of the Invention
[0006] The secondary battery of the present disclosure includes a precipitated metallic lithium negative electrode and has low resistance. [Brief description of the drawings]
[0007] [Figure 1] 1 shows a schematic configuration of a secondary battery 100 after charging or discharging. [Diagram 2]1 shows an example of a flow of a manufacturing method for the secondary battery 100. [Diagram 3] 1 shows an SEM secondary electron image and EDX mapping of the LiPON film surface of a LiPON-coated Mg vapor-deposited current collector. [Figure 4] 3 shows the charge / discharge curves of the evaluation cell. [Diagram 5] The results of evaluating the cell impedance after the first charge are shown. [Figure 6] 4 shows the evaluation results of cell impedance after the initial charge / discharge. [Figure 7] This shows the change in cell 1s resistance over time when a 60°C storage test was performed in an open circuit after charging to an upper cutoff potential of 4.2V. [Figure 8] This shows a cross-sectional SEM secondary electron image and EDX mapping of the LiPON-coated Mg negative electrode-solid electrolyte layer interface after charging at 60° C. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] 1. Secondary battery Hereinafter, a secondary battery according to an embodiment will be described with reference to the drawings, but the technology of the present disclosure is not limited to the following embodiment. FIG. 1 shows a configuration of a secondary battery 100 according to an embodiment. As shown in FIG. 1, the secondary battery 100 includes a positive electrode 10, a solid electrolyte layer 20, a protective layer 30, an anode current collector 41, and metallic lithium 42 that is deposited between the solid electrolyte layer 20 and the anode current collector 41 by charging. The solid electrolyte layer 20 includes a sulfide solid electrolyte. The protective layer 30 exists between the solid electrolyte layer 20 and the anode current collector 41. The protective layer 30 includes Li, P, and O as constituent elements.
[0009] 1.1 Positive electrode The positive electrode 10 includes at least a positive electrode active material. When the secondary battery 100 is charged, lithium ions released from the positive electrode active material reach between the solid electrolyte layer 20 and the negative electrode current collector 41 through the solid electrolyte layer 20, receive electrons, and are precipitated as metallic lithium 42. When the battery is discharged, the metallic lithium 42 between the solid electrolyte layer 20 and the negative electrode current collector 41 is dissolved (ionized) and returned to the positive electrode 10. The form of the positive electrode 10 may be any form known as a positive electrode for a secondary battery. For example, as shown in FIG. 1, the positive electrode 10 may include a positive electrode current collector 11 and a positive electrode active material layer 12.
[0010] The positive electrode collector 11 may be any material capable of functioning as a positive electrode collector of a secondary battery. The positive electrode collector 11 may be a metal foil or a metal mesh. In particular, a metal foil is excellent in terms of ease of handling. The positive electrode collector 11 may be made of a plurality of metal foils. Examples of metals constituting the positive electrode collector 11 include Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, and stainless steel. In particular, the positive electrode collector 11 may contain Al from the viewpoint of ensuring oxidation resistance. The positive electrode collector 11 may have some kind of coating layer on its surface for the purpose of adjusting resistance, etc. In addition, when the positive electrode collector 11 is made of a plurality of metal foils, some kind of layer may be present between the plurality of metal foils. The thickness of the positive electrode collector 11 is not particularly limited. For example, it may be 0.1 μm or more or 1 μm or more, and may be 1 mm or less or 100 μm or less.
[0011] The positive electrode active material layer 12 includes a positive electrode active material, and may further include an electrolyte, a conductive assistant, a binder, and the like. The contents of the positive electrode active material, the electrolyte, the conductive assistant, the binder, and the like in the positive electrode active material layer 12 may be appropriately determined according to the intended battery performance. The shape of the positive electrode active material layer 12 is not particularly limited, and may be, for example, a sheet shape having a substantially flat surface. The thickness of the positive electrode active material layer 12 may be appropriately determined according to the intended battery performance.
[0012] The positive electrode active material may be any known positive electrode active material for secondary batteries that can supply lithium to the negative electrode side during charging. For example, various lithium-containing oxides such as lithium cobalt oxide, lithium nickel oxide, lithium manganate, lithium nickel cobalt manganate, lithium nickel cobalt aluminum oxide, and spinel-based lithium compounds can be used as the positive electrode active material. Alternatively, a material in which lithium is absorbed into sulfur can be used as the positive electrode active material. In particular, when the positive electrode 10 contains a lithium-containing oxide as the positive electrode active material, lithium ions can be appropriately supplied from the positive electrode active material to the negative electrode side during charging, and the expansion and contraction of the positive electrode active material during charging and discharging is small, making it easy to obtain high performance. Only one type of positive electrode active material may be used alone, or two or more types may be used in combination. The positive electrode active material may be, for example, particulate, and its size is not particularly limited. The surface of the positive electrode active material may be covered with an ion-conductive oxide. This makes it easier to suppress reactions between the positive electrode active material and other battery materials (for example, the sulfide solid electrolyte described below). The ion-conductive oxide that coats the surface of the positive electrode active material is, for example, Li 3 BO 3 , LiBO 2 , Li 2 CO 3 , LiAlO 2 , Li 4 SiO 4 , Li 2 SiO 3 , Li 3 PO 4 , Li 2 SO 4 , Li 2 TiO 3 , Li 4 Ti 5 O 12 , Li 2 Ti 2 O 5 , Li 2 ZrO 3 , LiNbO 3 , Li 2 MoO 4 , Li 2 WO 4The coverage (area ratio) of the ion conductive oxide with respect to the surface of the positive electrode active material may be, for example, 70% or more, 80% or more, or 90% or more. The thickness of the ion conductive oxide layer may be, for example, 0.1 nm or more or 1 nm or more, and may be 100 nm or less, or 20 nm or less.
[0013] The electrolyte that can be included in the positive electrode active material layer 12 may be a solid electrolyte, a liquid electrolyte (electrolytic solution), or a combination of these. In particular, when the positive electrode active material layer 12 includes a solid electrolyte, the technology of the present disclosure can be expected to have a higher effect. The solid electrolyte may be any known solid electrolyte for secondary batteries. The solid electrolyte may be an inorganic solid electrolyte or an organic polymer electrolyte. In particular, the inorganic solid electrolyte has excellent ion conductivity and heat resistance. Examples of the inorganic solid electrolyte include oxide solid electrolytes and sulfide solid electrolytes. Among the inorganic solid electrolytes, sulfide solid electrolytes, and among them, sulfide solid electrolytes containing at least Li, S, and P as constituent elements, have high performance. Details of the sulfide solid electrolyte will be described later. The solid electrolyte may be amorphous or crystalline. The solid electrolyte may be particulate. Only one type of solid electrolyte may be used alone, or two or more types may be used in combination.
[0014] Examples of the conductive assistant that may be included in the positive electrode active material layer 12 include carbon materials such as vapor grown carbon fiber (VGCF), acetylene black (AB), ketjen black (KB), carbon nanotubes (CNT), and carbon nanofibers (CNF); and metal materials such as nickel, aluminum, and stainless steel. The conductive assistant may be, for example, particulate or fibrous, and the size is not particularly limited. Only one type of conductive assistant may be used alone, or two or more types may be used in combination.
[0015] Examples of binders that can be included in the positive electrode active material layer 12 include butadiene rubber (BR)-based binders, butylene rubber (IIR)-based binders, acrylate butadiene rubber (ABR)-based binders, styrene butadiene rubber (SBR)-based binders, polyvinylidene fluoride (PVdF)-based binders, polytetrafluoroethylene (PTFE)-based binders, polyimide (PI)-based binders, polyacrylic acid-based binders, etc. Only one type of binder may be used alone, or two or more types may be used in combination.
[0016] 1.2 Solid electrolyte layer The solid electrolyte layer 20 includes at least a sulfide solid electrolyte. The sulfide solid electrolyte included in the solid electrolyte layer 20 may be the same or different from the sulfide solid electrolyte that may be included in the positive electrode active material layer 12. The solid electrolyte layer 20 may include other electrolytes together with the sulfide solid electrolyte. The other electrolytes may be solid electrolytes or electrolyte solutions. The solid electrolyte layer 20 may further include a binder, various additives, and the like. The binder that may be included in the solid electrolyte layer 20 may be the same or different from the binder that may be included in the positive electrode active material layer 12. In the solid electrolyte layer 20, each of the electrolyte and the binder may be used alone, or two or more types may be used in combination. The solid electrolyte layer 20 may be entirely formed of a solid, or may include a solid electrolyte and a liquid. The content of the solid electrolyte and the binder in the solid electrolyte layer 20 is not particularly limited. For example, the solid electrolyte content may be 50 mass% or more, 60 mass% or more, or 70 mass% or more, or 100 mass% or less, or 90 mass% or less, where the entire solid electrolyte layer 20 (total solid content) is taken as 100 mass%. The thickness of the solid electrolyte layer 20 is not particularly limited, and may be, for example, 0.1 μm or more, or 1 μm or more, and 2 mm or less, or 1 mm or less.
[0017] The sulfide solid electrolyte may be a glass-based sulfide solid electrolyte (sulfide glass), a glass ceramic-based sulfide solid electrolyte, or a crystalline sulfide solid electrolyte. When the sulfide solid electrolyte has a crystalline phase, examples of the crystalline phase include a Thio-LISICON-type crystalline phase, a LGPS-type crystalline phase, and an Argyrodite-type crystalline phase. The sulfide solid electrolyte may contain, for example, a Li element, an X element (X is at least one of P, As, Sb, Si, Ge, Sn, B, Al, Ga, and In), and an S element. The sulfide solid electrolyte may further contain at least one of an O element and a halogen element. The sulfide solid electrolyte may contain an S element as a main component of an anion element. The sulfide solid electrolyte may contain, for example, Li 2 SP 2 S 5 , Li 2 SP 2 S 5 - LiI, Li 2 SP 2 S 5 -GeS 2 , Li 2 SP 2 S 5 -Li 2 O, Li 2 SP 2 S 5 -Li 2 O-LiI, Li 2 SP 2 S 5 -LiI-LiBr, Li 2 S-SiS 2 , Li 2 S-SiS 2 - LiI, Li 2 S-SiS 2 -LiBr, Li 2 S-SiS 2 -LiCl, Li 2 S-SiS 2 -B 2 S 3 - LiI, Li 2 S-SiS 2 -P 2 S 5 - LiI, Li 2 S.B.2 S 3 、 Li 2 S-P 2 S 5 -ZmSn (where m and n are positive numbers. Z is any one of Ge, Zn, Ga.), Li 2 S-GeS 2 、 Li 2 S-SiS 2 -Li 3 PO 4 、 Li 2 S-SiS 2 -Li x MO y (where x and y are positive numbers. M is any one of P, Si, Ge, B, Al, Ga, In.) may be at least one selected therefrom. The composition of the sulfide solid electrolyte is not particularly limited. For example, xLi 2 S·(100 - x)P 2 S 5 (70 ≤ x ≤ 80), yLiI·zLiBr·(100 - y - z)(xLi 2 S·(1 - x)P 2 S 5 )(0.7 ≤ x ≤ 0.8, 0 ≤ y ≤ 30, 0 ≤ z ≤ 30), etc. may be mentioned. Alternatively, the sulfide solid electrolyte may have a composition represented by the general formula: Li 4-x Ge 1-x P x S 4 (0 < x < 1). In the above general formula, at least a part of Ge may be substituted with at least one of Sb, Si, Sn, B, Al, Ga, In, Ti, Zr, V, and Nb. In the above general formula, at least a part of P may be substituted with at least one of Sb, Si, Sn, B, Al, Ga, In, Ti, Zr, V, and Nb. In the above general formula, a part of Li may be substituted with at least one of Na, K, Mg, Ca, and Zn. In the above general formula, a part of S may be substituted with a halogen (at least one of F, Cl, Br, and I). Alternatively, the sulfide solid electrolyte is Li 7-a PS 6-a X a(X is at least one of Cl, Br, and I, and a is a number of 0 or more and 2 or less). a may be 0 or more than 0. In the latter case, a may be 0.1 or more, 0.5 or more, or 1 or more. Also, a may be 1.8 or less, or 1.5 or less.
[0018] 1.3 Protective layer As shown in FIG. 1, the protective layer 30 is present between the solid electrolyte layer 20 and the negative electrode current collector 41. According to the findings of the present inventor, in a conventional secondary battery, when the deposition and dissolution of metallic lithium is repeated between the solid electrolyte layer and the negative electrode current collector, the metallic lithium reacts with the sulfide solid electrolyte contained in the solid electrolyte layer, and the sulfide solid electrolyte is reduced and decomposed, and the resistance is likely to increase. In contrast, in the secondary battery 100 of the present disclosure, the protective layer 30 is present between the solid electrolyte layer 20 and the negative electrode current collector 41, so that direct contact between the solid electrolyte layer 20 and the metallic lithium 42 is suppressed when the metallic lithium 42 is deposited, and the reaction between the sulfide solid electrolyte contained in the solid electrolyte layer 20 and the metallic lithium 42 is likely to be suppressed. In addition, the protective layer 30 contains the following constituent elements, so that lithium ion conductivity is ensured in the protective layer 30. As a result, according to the secondary battery 100, it is possible to suppress an increase in resistance after charging and discharging.
[0019] The protective layer 30 contains Li, P, and O as constituent elements. The protective layer 30 may contain Li, P, O, and N as constituent elements. The protective layer 30 containing Li, P, and O as constituent elements has excellent lithium ion conductivity. The protective layer 30 is, for example, 10 -7The protective layer 30 may have a lithium ion conductivity of more than 10 ...
[0020] The protective layer 30 may cover, for example, at least a part of the surface of the solid electrolyte layer 20 on the negative electrode collector 41 side (for example, 50 area% to 100 area%, 75 area% to 100 area%, or 90 area% to 100 area% of the surface of the solid electrolyte layer 20), or may cover at least a part of the surface of the negative electrode collector 41 on the solid electrolyte layer 20 side (for example, 50 area% to 100 area%, 75 area% to 100 area%, or 90 area% to 100 area% of the surface of the negative electrode collector 41). In either case, metallic lithium 42 may be precipitated between the protective layer 30 and the negative electrode collector 41 during charging. The thickness of the protective layer 30 is not particularly limited, and may be, for example, 5 nm to 500 μm, 10 nm to 50 μm, or 50 nm to 1 μm. The secondary battery 100 may include only one protective layer 30, or may include two or more protective layers 30.
[0021] 1.4 Negative electrode current collector The negative electrode current collector 41 may be any material capable of functioning as a negative electrode current collector for a secondary battery. The negative electrode current collector 41 may be a metal foil or a metal mesh, or may be a carbon sheet. In particular, a metal foil is excellent in terms of ease of handling. The negative electrode current collector 41 may be made of a plurality of metal foils or sheets. Examples of metals constituting the negative electrode current collector 41 include Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, stainless steel, and the like. In particular, from the viewpoint of ensuring reduction resistance and being difficult to alloy with lithium, the negative electrode current collector 41 may be one containing at least one metal selected from Cu, Ni, and stainless steel, and particularly one containing at least one metal of Ni and stainless steel. The negative electrode current collector 41 may have some kind of coating layer on its surface. In addition, when the negative electrode current collector 41 is made of a plurality of metal foils, some kind of layer may be present between the plurality of metal foils. The thickness of the negative electrode current collector 41 is not particularly limited. For example, it may be 0.1 μm or more, or 1 μm or more, and may be 1 mm or less, or 100 μm or less.
[0022] As shown in FIG. 1, the negative electrode current collector 41 may have a metal foil 41a and an Mg-containing layer 41b provided on the surface of the metal foil 41a, and the Mg-containing layer 41b may be present between the protective layer 30 and the metal foil 41a. It is believed that the negative electrode current collector 41 has the Mg-containing layer 41b, which promotes the diffusion of Li on the surface of the negative electrode current collector 41, increases the affinity of the metallic lithium 42 to the negative electrode current collector 41, suppresses voids between the negative electrode current collector 41 and the metallic lithium 42, and causes the metallic lithium 42 to deposit more uniformly on the surface of the negative electrode current collector 41. The Mg-containing layer 41b may be a layer in which the molar ratio of Mg is the highest among all of its constituent elements. The molar ratio of Mg in the entire Mg-containing layer 41b may be, for example, 50 mol% or more and 100 mol% or less, or 70 mol% or more, 80 mol% or more, or 90 mol% or more. The Mg-containing layer 41b may be, for example, either a metal thin film (e.g., a vapor deposition film) containing Mg or a layer containing Mg particles. The metal thin film containing Mg may be made of Mg or an Mg alloy. The Mg particles may be particles of simple Mg or may be particles containing Mg and an element other than Mg. Examples of elements other than Mg include various metal elements, semimetal elements, and nonmetal elements. For example, the Mg particles may be alloy particles (Mg alloy particles) containing Mg and a metal other than Mg. The Mg alloy particles may be an alloy containing Mg as a main component (an alloy in which 50 mol % or more of all constituent elements is Mg). The Mg alloy particles may contain at least one of Li, Au, Al, and Ni as the metal M other than Mg. The Mg alloy particles may or may not contain Li. The Mg alloy particles may contain a β single-phase alloy of Li and Mg. Alternatively, the Mg particles may be oxide particles (Mg oxide particles) containing Mg and O. The Mg particles may be primary particles, or secondary particles formed by agglomeration of primary particles. The average particle size (D50) of the Mg particles may be, for example, 10 nm or more and 100 μm or less.The thickness of the Mg-containing layer 41b may be, for example, 10 nm or more and 100 μm or less, 50 nm or more or 100 nm or more, or 50 μm or less, 10 μm or less, or 5 μm or less. The Mg-containing layer 41b may be formed, for example, on the surface of the metal foil 41a constituting the negative electrode current collector 41. Alternatively, the Mg-containing layer 41b may be formed by pressing Mg particles on the surface of the negative electrode current collector 41. Examples of methods for forming the Mg-containing layer 41b on the surface of the metal foil 41a include PVD methods such as vapor deposition and sputtering; plating methods such as electrolytic plating and electroless plating; and coating methods using a slurry.
[0023] 1.5 Metallic lithium as a negative electrode active material The secondary battery 100 includes a lithium deposition type negative electrode. Specifically, as shown in Fig. 1, metallic lithium 42 is deposited between the solid electrolyte layer 20 and the negative electrode current collector 41 (particularly, between the protective layer 30 and the negative electrode current collector 41) upon charging. The metallic lithium 42 deposited between the solid electrolyte layer 20 and the negative electrode current collector 41 dissolves (ionizes) upon discharging and is returned to the positive electrode 10. In the present application, the term "metallic lithium" is a concept that includes not only elemental lithium but also lithium alloys. The lithium alloy may be at least one selected from Li-Au, Li-Mg, Li-Sn, Li-Al, Li-B, Li-C, Li-Ca, Li-Ga, Li-Ge, Li-As, Li-Se, Li-Ru, Li-Rh, Li-Pd, Li-Ag, Li-Cd, Li-In, Li-Sb, Li-Ir, Li-Pt, Li-Hg, Li-Pb, Li-Bi, Li-Zn, Li-Tl, Li-Te, and Li-At. The amount of metallic lithium 42 precipitated between the solid electrolyte layer 20 and the negative electrode current collector 41 is not particularly limited, and may be appropriately adjusted according to the intended battery performance.
[0024] 1.6 Other configurations The secondary battery 100 may have other configurations in addition to the above configurations. For example, the secondary battery 100 may have tabs or terminals connected to each of the above configurations, may have an exterior body that houses each of the above configurations, may have each of the above configurations sealed with resin, or may have a restraining member for restraining each of the above configurations in the thickness direction.
[0025] 2. Manufacturing method of secondary batteries The secondary battery 100 of the present disclosure can be manufactured, for example, as follows. That is, as shown in FIG. 2, a manufacturing method of the secondary battery 100 according to one embodiment may include: coating one or both surfaces of the negative electrode current collector 41 and the solid electrolyte layer 20 with a protective layer 30 to obtain a coating 50; using the coating 50 to obtain a laminate 60 having the positive electrode 10, the solid electrolyte layer 20, the protective layer 30, and the negative electrode current collector 41 in this order; and charging the laminate 60 to deposit metallic lithium 42 between the solid electrolyte layer 20 and the negative electrode current collector 41. Here, the solid electrolyte layer 20 includes a sulfide solid electrolyte, and the protective layer 30 includes Li, P, and O.
[0026] 2.1 Covering In the manufacturing method according to the present embodiment, the surface of one or both of the negative electrode collector 41 and the solid electrolyte layer 20 is covered with the protective layer 30 to obtain the coating 50. The method of covering the surface of the negative electrode collector 41 and the solid electrolyte layer 20 with the protective layer 30 is not particularly limited. For example, the surface of the negative electrode collector 41 and the solid electrolyte layer 20 can be covered with the protective layer 30 by a coating method using a solution or a slurry. Alternatively, a transfer material in which a layer made of the protective layer 30 is formed on a base material may be obtained, and then the protective layer 30 may be transferred from the transfer material to the surface of the negative electrode collector 41 and the solid electrolyte layer 20. Alternatively, the protective layer 30 may be formed on the surface of the negative electrode collector 41 and the solid electrolyte layer 20 by sputtering or the like.
[0027] 2.2 Preparation of the laminate In the manufacturing method according to the present embodiment, the laminate 60 having the positive electrode 10, the solid electrolyte layer 20, the protective layer 30, and the negative electrode current collector 41 in this order is obtained using the above-mentioned coating 50. The laminate 60 can be easily obtained by, for example, forming and laminating each of the above-mentioned materials by coating, transferring, adhering, or pressing the materials. The laminate 60 includes at least one lamination unit of the above-mentioned positive electrode current collector 11, the positive electrode active material layer 12, the solid electrolyte layer 20, the protective layer 30, and the negative electrode current collector 41. In the laminate 60, a plurality of lamination units may be electrically connected to each other in series, may be connected in parallel, or may not be electrically connected. Before or after obtaining the laminate 60, pressure may be applied to each of the layers or the laminate 60 in the thickness direction (lamination direction). Each layer or the laminate 60 can be pressurized by a known means. The magnitude of pressure applied to each layer or laminate 60 in the stacking direction can be appropriately determined depending on the target battery performance. The pressure may be 100 MPa or more, 150 MPa or more, 200 MPa or more, 250 MPa or more, 300 MPa or more, or 350 MPa or more. The pressurizing time and pressurizing temperature of each layer or laminate 60 are not particularly limited.
[0028] 2.3 Charging In the manufacturing method according to the present embodiment, the laminate 60 is charged, and metallic lithium 42 is precipitated between the solid electrolyte layer 20 and the negative electrode current collector 41. By charging the laminate 60, lithium ions are conducted from the positive electrode active material contained in the positive electrode active material layer 12 to the negative electrode current collector 41 side through the solid electrolyte layer 20, and the lithium ions receive electrons between the solid electrolyte layer 20 and the negative electrode current collector 41, and are precipitated as metallic lithium 42. The laminate 60 may be charged by a method similar to that of a general battery. For example, charging is performed by connecting an external power source to the positive electrode current collector 11 and the negative electrode current collector 41.
[0029] 2.4 Other processes In addition to the above-mentioned steps, the manufacturing method according to this embodiment may include general steps for manufacturing a secondary battery, such as a step of housing the laminate 60 inside an exterior body and a step of connecting tabs to the laminate 60. EXAMPLES
[0030] As described above, one embodiment of the technology of the present disclosure has been described, but the technology of the present disclosure can be modified in various ways other than the above embodiment without departing from the gist of the technology. The technology of the present disclosure will be described in more detail below while showing examples, but the technology of the present disclosure is not limited to the following examples.
[0031] 1. Preparation of the Negative Electrode Current Collector Mg was evaporated onto the surface of the SUS foil to obtain a Mg-evaporated current collector. The thickness of the evaporated Mg film was 1.0 μm.
[0032] 2. Covering with a protective layer A LiPON film was formed as a protective layer on the Mg of the evaporated Mg current collector by sputtering to obtain a LiPON-coated evaporated Mg current collector. The LiPON film had a thickness of 100 nm.
[0033] 3. Preparation of Positive Electrode In the butyl butyrate solvent, the positive electrode active material (NCA): sulfide solid electrolyte (Li 2 SP 2 S 5 Each component was added so that the mass ratio of LiI-LiBr), binder (PVdF), and conductive additive (AB) was 84.7:13.4:0.6:1.27, and a positive electrode slurry was obtained. The positive electrode slurry was applied to an Al foil with a coating gap of 225 μm, pre-dried at 60°C, and then dried at 165°C for 1 hour to obtain a positive electrode. The weight of the composite material in the positive electrode was 18.7 mg / cm 2 , designed capacity is 3.0mAh / cm 2 It is.
[0034] 4. Preparation of Solid Electrolyte Layer To butyl butyrate as a solvent, each component was added in a mass ratio of sulfide solid electrolyte (same as above):binder (same as above) = 92.6:7.4 to obtain a solid electrolyte slurry. The solid electrolyte slurry was applied onto a release film with a coating gap of 325 μm, pre-dried at room temperature for 3 hours, and then fully dried at 165°C for 1 hour. The dried coated film was punched out into two pieces with a diameter of 14.5 mm, and the coated surfaces were overlapped and pressed at 7 tons. After pressing, the release film was peeled off to obtain a solid electrolyte layer.
[0035] 5. Preparation of Evaluation Cell 5.1 Example The positive electrode was punched out to φ11.28 mm, and the LiPON-coated Mg vapor deposition current collector was punched out to φ14.5 mm. The solid electrolyte layer of φ14.5 mm was placed between the positive electrode and the LiPON-coated Mg vapor deposition current collector (negative electrode), and the positive electrode tab was made of Al, and the negative electrode tab was made of Ni, and the laminate film was vacuum sealed. The sealed cell was isostatically pressed at 392 MPa using CIP (cold isostatic pressing) to produce a laminate cell. The produced cell was constrained at 1 MPa using a constant pressure jig with a spring inserted so that the constraining pressure was constant regardless of the volume change of the cell, and an evaluation cell having a configuration of Al foil / NCA positive electrode composite layer / solid electrolyte layer / LiPON protective layer / Mg layer / SUS foil was obtained.
[0036] Separate from the above evaluation cell, a cell used to evaluate the reactivity between the negative electrode and the solid electrolyte layer was fabricated as follows: 100 mg of sulfide solid electrolyte was placed in a fixed-size cell and pressed at 1 t, after which a LiPON-coated Mg vapor-deposited current collector punched to φ11.28 mm was attached to the sulfide solid electrolyte layer and pressed at 6 t to obtain a laminate, which was then restrained at 2 N m.
[0037] 5.2 Comparative Example The procedure was the same as in Example 1, except that a Mg vapor-deposited current collector (without LiPON) was used instead of the LiPON-coated Mg vapor-deposited current collector.
[0038] 6. Electrochemical Measurements The cutoff voltage is in the range of 4.2V-3.0V, and the constant current (current density: 0.15mA / cm2 , equivalent to 0.05C) - constant voltage (cutoff current density: 0.03mA / cm 2 The restrained cells were initially charged and discharged at a current of 0.01 C (equivalent to 0.01 C) at 60° C. After standing for 1 hour in an open circuit at the upper and lower cutoff voltages, the cell impedances after the initial charge and charge / discharge at 60° C. were measured by the AC impedance method at an amplitude of 10 mV and a frequency range of 1 MHz to 10 mHz.
[0039] To evaluate the reactivity between the negative electrode and the solid electrolyte layer and to evaluate aging in the charged state, the above cells were fabricated and charged at a constant current (current density: 0.15 mA / cm 2 , equivalent to 0.05C) - constant voltage (cutoff current density: 0.03mA / cm 2 After charging at a current of 100 V (equivalent to 0.01 C) up to an upper cutoff voltage of 4.2 V, each battery was held in an open circuit at 60° C., and the cell impedance at 60° C. was measured by an AC impedance method at an amplitude of 10 mV and a frequency range of 1 MHz to 10 mHz.
[0040] 7. Evaluation by SEM-EDX The LiPON film surface of the LiPON-coated Mg vapor-deposited current collector and its cross section after the first charge were subjected to SEM observation and EDX mapping using secondary electron images at an applied voltage of 5 kV.
[0041] 8. Evaluation Results 8.1 SEM observation and EDX mapping Figure 3 shows an SEM secondary electron image and EDX mapping of the LiPON film surface of the LiPON-coated Mg vapor-deposited current collector. As is clear from the EDX mapping, a uniform distribution of P, O, and N was observed on the surface. This suggests that the LiPON film is uniformly coated on the surface of the Mg vapor-deposited film.
[0042] 7.2 Charge-discharge curve Figure 4 shows the current density at 60℃ and 0.15mA / cm 2The initial charge / discharge curves of the evaluation cell at (~C / 20) are shown. The charge capacity and discharge capacity were 214mAh / g·201mAh / g for the example and 205mAh / g·188mAh / g for the comparative example, based on the positive electrode active material. While no specific differences were observed in the behavior of the charge / discharge curves with or without a LiPON coating, an increase was observed in the discharge capacity in particular for the example with a LiPON coating. This shows that the reversibility of the charge / discharge cycle is improved by the LiPON coating.
[0043] 7.3 Resistance Table 1, Figures 5 and 6 below show the cell impedance and cell 1s resistance after the first charge and the first charge / discharge. As shown in Table 1 and Figure 5, the cell impedance after the first charge showed almost the same behavior regardless of the presence or absence of LiPON coating, and almost no change was observed in the cell 1s resistance. This shows that the presence of LiPON coating does not adversely affect Li deposition during charging. On the other hand, as shown in Table 1 and Figure 6, for the cell impedance after the first charge / discharge, the semicircle due to the interface resistance was significantly reduced in the example compared to the comparative example, and the cell 1s resistance was reduced by 34%.
[0044] [Table 1]
[0045] As described above, by coating the negative electrode current collector with LiPON, it was confirmed that the reversible capacity during the first discharge increased and the cell resistance decreased at the same time. It is presumed that the LiPON coating suppressed the reductive decomposition of the sulfide solid electrolyte by the precipitated Li during charging and discharging, and maintained the interface between the solid electrolyte layer and the precipitated Li or the negative electrode current collector. In addition, it is presumed that the products at the LiPON and LiPON / precipitated Li interface have lithium conductivity, which is why the lithium conduction path was maintained even after charging and discharging.
[0046] The stability of the LiPON coating at 60°C was confirmed. As shown in Table 2 below, in a cell composed only of a solid electrolyte layer and a negative electrode, the cell 1s resistance was measured after a storage test at 60°C for 5 days, and no significant difference was observed between the comparative example and the example. From this, it was found that the LiPON coating does not cause an increase in resistance due to a spontaneous chemical reaction with Mg or the sulfide solid electrolyte. In addition, FIG. 7 shows the change in cell 1s resistance over time when a storage test was performed at 60°C in an open circuit after charging up to an upper cutoff potential of 4.2V. As shown in Table 2 and FIG. 7, the cell 1s resistance in the example at 60°C charging state was about 53% compared to that of the comparative example, and when comparing the increase in cell 1s resistance over time after the start of the storage test, both were proportional to the square root of time, and the slope was smaller in the example than in the comparative example. In other words, it can be seen that the LiPON coating suppresses both the absolute value and the rate of increase of the cell 1s resistance. Furthermore, FIG. 8 shows a cross-sectional SEM secondary electron image and EDX mapping of the interface between the LiPON-coated Mg vapor-deposited current collector and the solid electrolyte layer after charging at 60°C. As shown in FIG. 8, a layer of a different form exists between the current collector and the solid electrolyte layer, and P, O, and N are observed to be concentrated in this layer. In other words, it is inferred that LiPON exists at the interface between the current collector and the solid electrolyte layer even in the charged state. As described above, considering that the presence of the LiPON coat in the charged state does not contribute to an increase in resistance due to spontaneous chemical reactions, it is considered that the increase in interfacial resistance and cell resistance caused by the reduction and decomposition of the sulfide solid electrolyte by precipitated Li at the current collector-solid electrolyte layer interface during charging is suppressed by the LiPON coat functioning as a protective layer.
[0047] [Table 2] [Explanation of symbols]
[0048] 10: Positive electrode 11: Positive electrode current collector 12: Positive electrode active material layer 20: Solid electrolyte layer 30: Protective layer 41: Negative electrode current collector 42: Metallic lithium 50: Coating 60: Laminate 100: Secondary battery
Claims
1. A secondary battery comprising: a positive electrode; a solid electrolyte layer; a protective layer; a negative electrode current collector; and metallic lithium that is deposited between the solid electrolyte layer and the negative electrode current collector upon charging; the solid electrolyte layer includes a sulfide solid electrolyte, the protective layer is present between the solid electrolyte layer and the negative electrode current collector, The protective layer contains Li, P and O as constituent elements. Secondary battery.
2. 2. The secondary battery according to claim 1, The protective layer contains Li, P, O, and N as constituent elements. Secondary battery.
3. 2. The secondary battery according to claim 1, The protective layer is -7 S / cm or more of lithium ion conductivity; Secondary battery.
4. The secondary battery according to any one of claims 1 to 3, the negative electrode current collector has a metal foil and an Mg-containing layer provided on a surface of the metal foil, The Mg-containing layer is present between the protective layer and the metal foil. Secondary battery.
5. A method for manufacturing a secondary battery, comprising: Coating one or both surfaces of the negative electrode current collector and the solid electrolyte layer with a protective layer to obtain a coating; Obtaining a laminate having a positive electrode, a solid electrolyte layer, a protective layer, and a negative electrode current collector in this order using the coating; and and charging the laminate to deposit metallic lithium between the solid electrolyte layer and the negative electrode current collector. the solid electrolyte layer includes a sulfide solid electrolyte, The protective layer comprises Li, P and O; Manufacturing method.
Citation Information
Patent Citations
All-solid battery and method for manufacturing the same
JP2020184513A
Lithium secondary battery
JP2020524889A
Solid battery
JP2022010554A
Anode protection layer
JP2022540085A
Solid-state electrolyte layer, and all-solid-state lithium secondary battery
WO2013141241A1