Manufacturing method of optical fiber preform and manufacturing method of optical fiber

The described method efficiently adds alkali metals to optical fibers by diffusing them into silica glass tubes, minimizing impurities and reducing transmission loss, thus improving fiber performance.

JP2024146061AInactive Publication Date: 2024-10-15FURUKAWA ELECTRIC CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023058763
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for adding alkali metals to optical fibers face challenges such as volatilization, incorporation of impurities, poor addition efficiency, and process complexity, leading to increased transmission loss and fiber breakage.

Method used

A method involving the preparation of a silica glass tube, filling it with a powder containing an alkali metal or alkaline earth metal component, diffusing the metal into the tube through heat treatment, and removing excess powder to form a cladding portion, ensuring efficient and impurity-minimized alkali metal addition.

Benefits of technology

This method allows for sufficient alkali metal or alkaline earth metal addition with minimal impurities, reducing optical fiber breakage and transmission loss, thereby enhancing the performance of optical fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146061000001_ABST
    Figure 2024146061000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method of an optical fiber preform capable of easily efficiently and sufficiently adding an alkali metal or an alkali earth metal with less impurity, and a manufacturing method of an optical fiber using the same.SOLUTION: A manufacturing method of an optical fiber preform includes: a first preparation step of preparing a silica glass tube; a second preparation step of preparing a powder containing an alkali metal component or an alkali earth metal component and a silica powder; a filling step of filling the powder into the silica glass tube; a diffusion step of diffusing an alkali metal or an alkali earth metal from the powder into the silica glass tube by heat treatment; a removal step of removing the powder not stuck to the silica glass tube from the silica glass tube to which the alkali metal or the alkali earth metal is diffused therein; and a clad part formation step of forming a clad part so as to surround an outer periphery of the silica glass tube to which the alkali metal or the alkali earth metal is diffused therein.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing an optical fiber preform and a method for manufacturing an optical fiber. [Background technology]

[0002] With the practical application of digital coherent transmission technology, optical fiber transmission lines are becoming faster and larger in capacity. This has led to a demand for a high SNR (signal-to-noise ratio) in transmission systems, and a demand for lower transmission loss characteristics in the optical fibers that make up the transmission lines in optical transmission systems.

[0003] In order to reduce the transmission loss of optical fibers, it is effective to reduce Rayleigh scattering that occurs in the optical fiber. Rayleigh scattering is caused by fluctuations in the dielectric constant of glass, and is caused by two factors: composition fluctuations and density fluctuations. Density fluctuations depend on the temperature (fictive temperature) at which the glass solidifies from a supercooled liquid state. It is known that adding an alkali metal to the core of an optical fiber significantly lowers the fictive temperature, thereby reducing Rayleigh scattering loss (see Patent Document 1). The effect of lowering the fictive temperature can also be obtained by using an alkaline earth metal instead of an alkali metal.

[0004] As a method for doping an alkali metal into the core of an optical fiber made of silica glass, the following methods have been proposed.

[0005] For example, a method has been proposed in which alkali metal-doped silica core soot is synthesized by the VAD (vapor phase axial deposition) method or the OVD (outside vapor deposition) method, and the core soot is dehydrated and vitrified to produce an alkali metal-doped core preform (Patent Document 2). In addition, a method has been proposed in which alkali metal vapor is introduced into a quartz core tube containing silica core soot, and the alkali metal is allowed to penetrate and be doped into the silica core soot (Patent Document 3), and a method has been proposed in which the alkali metal is doped by diffusion from the outer surface of a silica core preform placed in the core tube (Patent Document 4).

[0006] Also, a method has been proposed in which an alkali metal is diffused and doped from the inside of a quartz tube that is a silica core base material by the MCVD (modified chemical vapor deposition) method (Patent Document 5). Also, a method has been proposed in which a core rod having a core part and a glass part adjacent to the core part over its periphery is placed inside a glass pipe, and glass particles containing an alkali metal are filled in the gap between the core rod and the glass pipe to dope an alkali metal into the core part (Patent Document 6). Also, a method has been proposed in which a silica glass body that will be at least a part of the core part is formed around an alkali metal-doped silica glass body to which an alkali metal has been added, and an alkali metal is diffused from the alkali metal-doped silica glass body into the silica glass body by heat treatment (Patent Document 7). [Prior art documents] [Patent documents]

[0007] [Patent Document 1] U.S. Pat. No. 5,146,534 [Patent Document 2] US Patent Publication No. 2004 / 0206127 [Patent Document 3] JP 2013-199399 A [Patent Document 4] US Patent Publication No. 2005 / 0129376 [Patent Document 5] JP 2012-162409 A [Patent Document 6] Patent No. 6719505 [Patent Document 7] Patent No. 5995923 Summary of the Invention [Problem to be solved by the invention]

[0008] However, all of the known methods for adding alkali metals have room for improvement. For example, in the method of Patent Document 2, the alkali metals taken into the silica soot are easily chlorinated and volatilized by the chlorine-based gas flowed in the subsequent dehydration process, so it may be difficult to leave the alkali metals at a desired concentration in the core. In addition, in the method of Patent Document 3, impurities such as transition metals contained in the alkali metal raw material may be added together with the alkali metals, and if a dehydration purification process using chlorine is performed to remove the impurities, the alkali metals may volatilize and the desired alkali metal concentration may not be obtained. In addition, in the method of Patent Document 4, most of the alkali metals used are discharged outside the furnace, so the doping efficiency is considered to be poor. In addition, in the method of Patent Document 6, impurities such as transition metals contained in the glass particles containing alkali metals are likely to be mixed in, and in the optical fiber manufactured thereafter, the impurities may cause breakage of the optical fiber or an increase in transmission loss. In addition, in the method of Patent Document 7, cracks may easily occur during the cooling process after the alkali diffusion process due to the large difference in softening temperature between the alkali metal-doped silica glass body and the silica glass body. In addition, since the alkali metal-doped silica glass body and the silica glass body are integrated by welding, the alkali metal-doped silica glass body must be removed by drilling, which makes the process complicated.

[0009] The present invention has been made in view of the above, and an object of the present invention is to provide a method for manufacturing an optical fiber preform capable of easily and efficiently doping an alkali metal or alkaline earth metal sufficiently with few impurities, and a method for manufacturing an optical fiber using the same. [Means for solving the problem]

[0010] In order to solve the above-mentioned problems and achieve the object, one aspect of the present invention is a method for manufacturing an optical fiber preform, comprising: a first preparation step of preparing a silica glass tube; a second preparation step of preparing a powder containing an alkali metal component or an alkaline earth metal component and silica powder; a filling step of filling the powder into the silica glass tube; a diffusion step of diffusing the alkali metal or alkaline earth metal from the powder into the interior of the silica glass tube by heat treatment; a removal step of removing the powder that is not adhered to the silica glass tube from the silica glass tube into which the alkali metal or alkaline earth metal has been diffused; and a cladding formation step of forming a cladding to surround the outer periphery of the silica glass tube into which the alkali metal or alkaline earth metal has been diffused.

[0011] The method for manufacturing the optical fiber preform may include a collapsing step for collapsing the silica glass tube after the diffusion step and before the cladding forming step, and in the cladding forming step, the alkali metal or alkaline earth metal may be diffused into the interior and the cladding formed so as to surround the outer periphery of the collapsible silica glass tube.

[0012] In the first preparation step, the silica glass tube doped with chlorine may be prepared.

[0013] One aspect of the present invention is a method for manufacturing an optical fiber preform, comprising: a first preparation step of preparing a silica glass tube; a second preparation step of preparing a powder containing an alkali metal component or an alkaline earth metal component and silica powder; a third preparation step of preparing a silica glass rod; an insertion step of inserting the silica glass rod into the silica glass tube; a filling step of filling the gap between the silica glass tube and the silica glass rod with the powder; a diffusion step of diffusing an alkali metal or alkaline earth metal from the powder into the interior of the silica glass rod by heat treatment; a removal step of removing the powder that is not adhered to the silica glass rod from the silica glass rod having the alkali metal diffused therein; and a cladding formation step of forming a cladding to surround the outer periphery of the silica glass rod having the alkali metal or alkaline earth metal diffused therein.

[0014] In the third preparation step, the silica glass rod doped with chlorine may be prepared.

[0015] One aspect of the present invention is a method for manufacturing an optical fiber preform, comprising: a first preparation step of preparing a silica glass tube; a second preparation step of preparing a powder containing an alkali metal component or an alkaline earth metal component and silica powder; a third preparation step of preparing a silica glass rod; a filling step of filling the powder into the silica glass tube; a diffusion step of diffusing an alkali metal or alkaline earth metal from the powder into the interior of the silica glass tube by heat treatment; a removal step of removing the powder that is not adhered to the silica glass tube from the silica glass tube into which the alkali metal or alkaline earth metal has been diffused; a jacketing step of jacketing the silica glass tube around the silica glass rod; and a cladding formation step of forming a cladding to surround the outer periphery of the jacketed silica glass tube.

[0016] In the first preparation step, the silica glass tube doped with chlorine may be prepared, and in the third preparation step, the silica glass rod doped with chlorine may be prepared.

[0017] The method for producing the optical fiber preform may further include, after the removing step, a second removing step of removing the powder adhered to the silica glass tube or the silica glass rod.

[0018] The alkali metal component is contained as at least one type of alkali metal compound selected from the group consisting of alkali metal silicate, alkali metal carbonate, alkali metal halide, alkali metal nitrate, alkali metal sulfate, and alkali metal hydroxide, and the alkaline earth metal component may be contained as at least one type of alkaline earth metal compound selected from the group consisting of alkaline earth metal silicate, alkaline earth metal carbonate, alkaline earth metal halide, alkaline earth metal nitrate, alkaline earth metal sulfate, and alkaline earth metal hydroxide.

[0019] In the diffusion step, the heat treatment may be performed under conditions that do not significantly promote sintering of the silica powder.

[0020] One aspect of the present invention is a method for manufacturing an optical fiber, comprising drawing an optical fiber preform manufactured by the method for manufacturing an optical fiber preform. Effect of the Invention

[0021] According to the present invention, it is possible to realize a method for manufacturing an optical fiber preform capable of doping an alkali metal or alkaline earth metal sufficiently with a small amount of impurities by a simple method, and a method for manufacturing an optical fiber using the same. [Brief description of the drawings]

[0022] [Figure 1] FIG. 1 is a flow diagram of a method for producing an optical fiber preform according to the first embodiment. [Diagram 2] FIG. 2 is an explanatory diagram of a method for producing the optical fiber preform according to the first embodiment. [Diagram 3] FIG. 3 is an explanatory diagram of a method for producing the optical fiber preform according to the first embodiment. [Figure 4]FIG. 4 is an explanatory diagram of a method for producing the optical fiber preform according to the first embodiment. [Diagram 5] FIG. 5 is an explanatory diagram of a method for producing the optical fiber preform according to the first embodiment. [Figure 6] FIG. 6 is an explanatory diagram of a method for producing the optical fiber preform according to the first embodiment. [Figure 7] FIG. 7 is a flow diagram of a method for producing an optical fiber preform according to the second embodiment. [Figure 8] FIG. 8 is an explanatory diagram of a method for producing an optical fiber preform according to the second embodiment. [Figure 9] FIG. 9 is an explanatory diagram of a method for producing an optical fiber preform according to the second embodiment. [Figure 10] FIG. 10 is an explanatory diagram of a method for producing an optical fiber preform according to the second embodiment. [Figure 11] FIG. 11 is an explanatory diagram of a method for producing an optical fiber preform according to the second embodiment. [Figure 12] FIG. 12 is an explanatory diagram of a method for producing an optical fiber preform according to the second embodiment. [Figure 13] FIG. 13 is a flow diagram of a method for producing an optical fiber preform according to the third embodiment. [Figure 14] FIG. 14 is an explanatory diagram of a method for producing an optical fiber preform according to the third embodiment. [Figure 15] FIG. 15 is an explanatory diagram of a method for producing an optical fiber preform according to the third embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. Note that the present invention is not limited to the embodiment described below. In addition, in each drawing, the same or corresponding components are appropriately assigned the same reference numerals. In addition, in this specification, terms that are not particularly defined shall follow the definitions and measurement methods in G.650.1 and G.650.2 of the International Telecommunications Union (ITU).

[0024] (Embodiment 1) FIG. 1 is a flow diagram of a method for manufacturing an optical fiber preform according to the first embodiment. In this manufacturing method, first, in step S101, a silica glass tube is prepared (first preparation step). Then, in step S102, a powder containing an alkali metal component or an alkaline earth metal component and silica powder is prepared (second preparation step). Then, in step S103, the powder is filled into the silica glass tube (filling step). Then, in step S104, the alkali metal or alkaline earth metal is diffused from the powder into the inside of the silica glass tube by heat treatment (diffusion step). Then, in step S105, the powder that is not fixed to the silica glass tube is removed from the silica glass tube into which the alkali metal or alkaline earth metal has been diffused (removal step). Then, in step S106, the silica glass tube is collapsed and collapsed (collapse step). Next, in step S107, an alkali metal or an alkaline earth metal is diffused into the inside of the silica glass tube, and a cladding portion is formed so as to surround the outer periphery of the solidified silica glass tube (cladding portion forming step).

[0025] A specific description will be given below. In the first preparation step, a hole is drilled in the center of a high-purity silica glass rod produced by, for example, the VAD method to prepare a silica glass tube 110 as shown in FIG. 2. Chlorine may be added when the silica glass rod is produced. Chlorine is added, for example, to lower the fictive temperature of the glass. The amount of chlorine added is not particularly limited, but is, for example, 8000 ppmwt. Also, when the silica glass rod is produced, dopants such as fluorine, phosphorus, germanium, and aluminum may be co-added as necessary. Also, the silica glass tube may be prepared by using the OVD method, the MCVD method, or the PCVD (Plasma CVD) method.

[0026] In the second preparation step, the alkali metal is one or more appropriately selected from lithium (Li), sodium (Na), potassium (K), rubidium (Rb), and cesium (Cs). The alkaline earth metal is one or more appropriately selected from beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), and barium (Ba). The alkali metal or alkaline earth metal may be contained as at least one alkali metal compound or alkaline earth metal compound of silicate, carbonate, halide, nitrate, sulfate, and hydroxide. The silica powder is preferably high purity, but is not particularly limited. The size of the silica powder is, for example, an average particle size of 0.1 to 200 μm, but is not particularly limited. The powder containing the alkali metal component or alkaline earth metal component and the silica powder can be prepared, for example, by thoroughly mixing and dispersing the powder of the alkali metal compound and the silica powder.

[0027] In the filling step, powder 120 is filled into the space inside the inner circumferential surface 111 of the silica glass tube 110 as shown in Fig. 3. At this time, it is preferable to fill the powder 120 so that it has a certain level of bulk density in order to sufficiently diffuse the alkali metal or alkaline earth metal inside the silica glass tube in the diffusion step. For this reason, it is preferable to set the size of the silica powder so that it has a certain level of bulk density when filled into the silica glass tube.

[0028] In the diffusion step, for example, an electric furnace is used to maintain a predetermined temperature for a predetermined time, thereby diffusing the alkali metal or alkaline earth metal into the silica glass tube 110. At this time, the powder may contain impurities such as transition metals (iron, etc.) and hydroxyl groups, but the diffusion coefficients of these impurities in silica glass are much smaller than the diffusion coefficients of the alkali metals or alkaline earth metals in silica glass. Therefore, the alkali metals or alkaline earth metals are selectively diffused into the silica glass tube 110.

[0029] In the diffusion step, the heat treatment may be performed using a flame such as an oxyhydrogen flame instead of an electric furnace.

[0030] In the removal step, the silica glass tube is tilted or held vertically to remove the powder. The silica glass tube may also be vibrated or sprayed with inert gas to remove the powder. All of these removal methods are extremely easy to implement. The powder may contain impurities, which are easily removed from the silica glass tube. This results in the silica glass tube 130 with the alkali metal diffused therein, as shown in FIG. 4.

[0031] In the diffusion step, if the heat treatment is performed under conditions that do not significantly promote sintering of the silica powder, the powder is suppressed or prevented from adhering to the silica glass tube, and impurities can be more easily and reliably removed from the silica glass tube. The conditions that do not significantly promote sintering of the silica powder include, for example, a heat treatment temperature that is lower than the glass transition point of the silica powder.

[0032] However, even if the powder adheres to the silica glass tube in the diffusion process, it may remain adhered as long as it does not affect the characteristics of the optical fiber when it is manufactured later. Furthermore, if a second removal process is performed after the removal process to remove the powder adhered to the silica glass tube, impurities can be more reliably removed from the silica glass tube. The second removal process can be performed, for example, by grinding the inner surface of the silica glass tube or by physically or chemically polishing it.

[0033] Furthermore, impurities may diffuse into the silica glass tube during the diffusion process, and in this case too, it is preferable to polish the inner circumferential surface of the silica glass tube by a small thickness.

[0034] In the collapsing process, the silica glass tube is heated to collapse and the holes are closed. This causes the silica glass tube 130 to be collapsed into a rod shape, and a silica glass rod 140 shown in Fig. 5 is obtained. The silica glass rod 140 is an example of a collapsed silica glass tube.

[0035] In the cladding forming step, the OVD method is used to form the cladding 150 so as to surround the outer periphery of the silica glass rod 140 as shown in Fig. 6. This results in an optical fiber preform 100 having the silica glass rod 140 doped with an alkali metal or alkaline earth metal as its core. Fluorine may be added to the cladding 150. The method of forming the cladding 150 is not limited to the OVD method, and the cladding 150 may be formed by jacketing the silica glass rod 140 with a silica glass tube doped with fluorine, for example.

[0036] Moreover, by drawing the optical fiber preform 100 manufactured as described above by a known method, an optical fiber having an alkali metal or alkaline earth metal added to the core portion can be manufactured.

[0037] According to the method for manufacturing an optical fiber preform and an optical fiber according to the first embodiment described above, an alkali metal or an alkaline earth metal can be sufficiently doped with few impurities into an optical fiber preform and an optical fiber by a simple method.

[0038] In particular, by allowing the addition of small amounts of alkali metals or alkaline earth metals as impurities, breakage of the optical fiber and increases in transmission loss caused by impurities can be significantly suppressed.

[0039] In addition, by using a powder containing an alkali metal component or an alkaline earth metal component and silica powder, the alkali metal source or the alkaline earth metal source can be easily prepared, and the process of removing the alkali metal source after addition is also simplified.

[0040] (Examples 1-1 to 1-9, Comparative Examples 1 and 2) The optical fiber preforms of Examples 1-1 to 1-9 were manufactured by the manufacturing method according to the first embodiment, and optical fibers were further manufactured. In Examples 1-1 to 1-9, a silica glass tube with an inner diameter of 12 mm and an outer diameter of 30 mm was prepared using a silica glass rod with 8000 ppmwt of chlorine added, which was manufactured by the VAD method. In addition, a powder containing an alkali metal component or an alkaline earth metal component and silica powder was prepared by mixing and dispersing silica powder and potassium carbonate (K2CO3). The concentration of potassium carbonate in the powder was 0.7 wt%.

[0041] In Example 1-1, the average particle size of the silica powder was 200 μm. The heat treatment temperature in the diffusion step was 1,100° C., and the heat treatment was performed at 1,100° C. for 24 hours. The heat treatment conditions correspond to conditions under which sintering of the silica powder does not proceed. However, after the removal step, the inner circumferential surface of the silica glass tube was polished. The inner diameter of the silica glass tube after polishing was 12.3 mm. The outer diameter of the silica glass rod after the solidification step (after collapse) was 27.0 mm.

[0042] In Example 1-1, the peak concentration of potassium in the silica glass rod after collapse was chemically analyzed and found to be 0.08 wt%. In addition, the concentrations of other impurities (iron, nickel, chromium, aluminum, and hydroxyl groups) were below the detection limit. Furthermore, the transmission loss of the manufactured optical fiber at a wavelength of 1550 nm was an extremely low value of 0.155 dB / km.

[0043] In Example 1-2, the average particle size of the silica powder was 200 μm. The heat treatment temperature in the diffusion step was 1,200° C., and the heat treatment was performed at 1,200° C. for 24 hours. This heat treatment condition corresponds to a condition under which the sintering of the silica powder does not progress significantly. However, since the heat treatment temperature is higher than in Example 1-1, there is a possibility that the sintering of the silica powder has slightly occurred, so after the removal step, the inner surface of the silica glass tube was polished more than in Example 1-1. The inner diameter of the silica glass tube after polishing was 12.5 mm. The outer diameter of the silica glass rod after the solidification step (after collapse) was 26.9 mm.

[0044] In Example 1-2, the peak concentration of potassium in the silica glass rod after collapse was chemically analyzed and found to be 0.10 wt%. The concentrations of other impurities were below the detection limit. Furthermore, the transmission loss of the manufactured optical fiber at a wavelength of 1550 nm was an extremely low value of 0.155 dB / km.

[0045] In Example 1-3, the average particle size of the silica powder was 200 μm. The heat treatment temperature in the diffusion step was 1,300° C., and the heat treatment was performed at 1,300° C. for 24 hours. This heat treatment condition corresponds to a condition under which the sintering of the silica powder does not progress significantly. However, since the heat treatment temperature is higher than in Example 1-2, there is a possibility that the sintering of the silica powder has further occurred, so after the removal step, the inner surface of the silica glass tube was polished more than in Example 1-2. After the removal step, the inner surface of the silica glass tube was polished. The inner diameter of the silica glass tube after polishing was 12.6 mm. The outer diameter of the silica glass rod after the solidification step (after collapse) was 26.8 mm.

[0046] In Example 1-3, the peak concentration of potassium in the silica glass rod after collapse was chemically analyzed and found to be 0.11 wt%. The concentrations of other impurities were below the detection limit. Furthermore, the transmission loss of the manufactured optical fiber at a wavelength of 1550 nm was an extremely low value of 0.156 dB / km.

[0047] In Example 1-4, the average particle size of the silica powder was 10 μm. Compared with Examples 1-1 to 1-3, the average particle size of the silica powder was small and the flowability was low, so the bulk density was difficult to increase in the filling process. Therefore, pressure was applied in one axial direction during filling to increase the bulk density while filling. In addition, the heat treatment temperature in the diffusion process was set to 1,100°C, and heat treatment was performed at 1,100°C for 24 hours. This heat treatment condition corresponds to a condition in which sintering of the silica powder does not progress. However, after the removal process, the inner circumferential surface of the silica glass tube was polished. The inner diameter of the silica glass tube after polishing was 12.3 mm. In addition, the outer diameter of the silica glass rod after the solidification process (after collapse) was 27.0 mm.

[0048] In Example 1-4, the peak concentration of potassium in the silica glass rod after collapse was chemically analyzed and found to be 0.065wt%. The concentrations of other impurities were below the detection limit. Furthermore, the transmission loss of the manufactured optical fiber at a wavelength of 1550nm was an extremely low value of 0.157dB / km.

[0049] In addition, when comparing Examples 1-1 to 1-3 with Example 1-4, it was found that an average particle size of the silica powder of 200 μm is more preferable than that of 10 μm in terms of increasing the concentration of potassium added and reducing the transmission loss.

[0050] In Example 1-5, the average particle size of the silica powder was 0.1 μm. Since the average particle size of the silica powder was smaller than those in Examples 1-1 to 1-3, potassium carbonate, silica powder, and water were mixed and stirred in a pot mill to prepare a slurry, which was then spray-dried at 150° C. and granulated. The slurry was then classified into particles having a particle size of 50 μm to 150 μm for use. The heat treatment temperature in the diffusion step was set to 1,100° C., and the heat treatment was performed at 1,100° C. for 24 hours. The heat treatment conditions correspond to conditions under which sintering of the silica powder does not proceed. However, after the removal step, the inner circumferential surface of the silica glass tube was polished. The inner diameter of the silica glass tube after polishing was 12.3 mm. The outer diameter of the silica glass rod after the solidification step (after collapse) was 27.0 mm.

[0051] In Examples 1-5, the peak concentration of potassium in the silica glass rod after collapse was chemically analyzed and found to be 0.06 wt%. The concentrations of other impurities were below the detection limit. Furthermore, the transmission loss of the manufactured optical fiber at a wavelength of 1550 nm was an extremely low value of 0.156 dB / km.

[0052] The granulation method is not limited to the above-mentioned method. For example, the slurry may be poured into a tray or the like, dried, and then crushed in a crusher or the like to easily form granules.

[0053] In Examples 1-6, the average particle size of the silica powder was 200 μm. The heat treatment temperature in the diffusion step was 1,050° C., and the heat treatment was performed at 1,050° C. for 24 hours. The heat treatment conditions correspond to conditions under which sintering of the silica powder does not proceed. However, after the removal step, the inner circumferential surface of the silica glass tube was polished. The inner diameter of the silica glass tube after polishing was 12.3 mm. The outer diameter of the silica glass rod after the solidification step (after collapse) was 27.0 mm.

[0054] In Examples 1-6, the peak concentration of potassium in the silica glass rod after collapse was chemically analyzed and found to be 0.07 wt%. The concentrations of other impurities were below the detection limit. Furthermore, the transmission loss of the manufactured optical fiber at a wavelength of 1550 nm was an extremely low value of 0.155 dB / km.

[0055] In Examples 1-7, the average particle size of the silica powder was 200 μm. The heat treatment temperature in the diffusion step was 1,000° C., and the heat treatment was performed at 1,000° C. for 24 hours. The heat treatment conditions correspond to conditions under which sintering of the silica powder does not proceed. However, after the removal step, the inner circumferential surface of the silica glass tube was polished. The inner diameter of the silica glass tube after polishing was 12.3 mm. The outer diameter of the silica glass rod after the solidification step (after collapse) was 27.0 mm.

[0056] In Examples 1-7, the peak concentration of potassium in the silica glass rod after collapse was chemically analyzed and found to be 0.06 wt%. The concentrations of other impurities were below the detection limit. Furthermore, the transmission loss of the manufactured optical fiber at a wavelength of 1550 nm was an extremely low value of 0.156 dB / km.

[0057] In Examples 1-8, the average particle size of the silica powder was 200 μm. The heat treatment temperature in the diffusion step was 900° C., and the heat treatment was performed at 900° C. for 24 hours. The heat treatment conditions correspond to conditions under which sintering of the silica powder does not proceed. However, after the removal step, the inner circumferential surface of the silica glass tube was polished. The inner diameter of the silica glass tube after polishing was 12.2 mm. The outer diameter of the silica glass rod after the solidification step (after collapse) was 27.0 mm.

[0058] In Example 1-8, the peak concentration of potassium in the silica glass rod after collapse was chemically analyzed and found to be 0.04 wt%. The concentrations of other impurities were below the detection limit. Furthermore, the transmission loss of the manufactured optical fiber at a wavelength of 1550 nm was an extremely low value of 0.158 dB / km.

[0059] Comparing Examples 1-1 to 1-3 and 1-6 to 1-8, it was confirmed that when the heat treatment temperature was in the range of 1000°C to 1300°C, approximately the same transmission loss could be achieved.

[0060] In Examples 1-9, the average particle size of the silica powder was 200 μm. The heat treatment temperature in the diffusion step was 1,400° C., and the heat treatment was performed at 1,400° C. for 24 hours. The heat treatment conditions correspond to conditions under which the sintering of the silica powder progresses relatively. Therefore, after the removal step, the inner circumferential surface of the silica glass tube was polished relatively thickly. The inner diameter of the silica glass tube after polishing was 12.7 mm. The outer diameter of the silica glass rod after the solidification step (after collapse) was 26.8 mm.

[0061] In Example 1-9, the peak concentration of potassium in the silica glass rod after collapse was chemically analyzed and found to be 0.14 wt%. The concentrations of other impurities were below the detection limit. Furthermore, the transmission loss of the manufactured optical fiber at a wavelength of 1550 nm was an extremely low value of 0.158 dB / km.

[0062] In contrast, in Comparative Example 1, the average particle size of the silica powder was 200 μm. The heat treatment temperature in the diffusion step was 800° C., and the heat treatment was performed at 800° C. for 24 hours. The heat treatment conditions correspond to conditions under which sintering of the silica powder does not proceed. However, after the removal step, the inner circumferential surface of the silica glass tube was polished. The inner diameter of the silica glass tube after polishing was 12.2 mm. The outer diameter of the silica glass rod after the collapsing step (after collapse) was 27.0 mm.

[0063] In Comparative Example 1, the peak concentration of potassium in the silica glass rod after collapse was chemically analyzed, and was found to be below the detection limit. The concentrations of other impurities were also below the detection limit. Furthermore, the transmission loss of the manufactured optical fiber at a wavelength of 1550 nm was a low value of 0.167 dB / km, but was higher than the values ​​in the other Examples.

[0064] In Comparative Example 2, a silica glass rod doped with 10000 ppmwt chlorine was prepared by the VAD method. A cladding part doped with fluorine was formed on this silica glass rod by the OVD method to obtain an optical fiber preform. The optical fiber produced from this optical fiber preform had a relatively high transmission loss of 0.170 dB / km at a wavelength of 1550 nm.

[0065] (Embodiment 2) FIG. 7 is a flow diagram of a method for manufacturing an optical fiber preform according to the second embodiment. In this manufacturing method, first, in step S201, a silica glass rod and a silica glass tube are prepared (first and third preparation steps). Then, in step S202, a powder containing an alkali metal component or an alkaline earth metal component and silica powder is prepared (second preparation step). Then, in step S203, the silica glass rod is inserted into the silica glass tube (insertion step). Then, in step S204, the powder is filled into the gap between the silica glass tube and the silica glass rod (filling step). Then, in step S205, the alkali metal or alkaline earth metal is diffused from the powder into the inside of the silica glass rod by heat treatment (diffusion step). Then, in step S206, the powder that is not fixed to the silica glass rod is removed from the silica glass rod into which the alkali metal has been diffused (removal step). Next, in step S207, a cladding portion is formed so as to surround the outer periphery of the silica glass rod having the alkali metal or alkaline earth metal diffused therein (cladding portion forming step).

[0066] A detailed description will be given below. In the first preparation step, as in the first embodiment, a hole is drilled in the center of a high-purity silica glass rod produced by, for example, the VAD method to prepare a silica glass tube 210 as shown in Fig. 8. However, the silica glass rod does not necessarily have to be of high purity, and dopants such as chlorine, fluorine, phosphorus, germanium, and aluminum do not have to be added. The silica glass tube 210 may be, for example, a commercially available silica glass tube that is not of high purity.

[0067] In the third preparation step, a high-purity silica glass rod 220 is prepared by the VAD method, as shown in FIG. 8. Chlorine may be added when the silica glass rod is prepared. The amount of chlorine added is not particularly limited, but is, for example, 8000 ppmwt. Dopants such as fluorine, phosphorus, germanium, and aluminum may be added as necessary when the silica glass rod is prepared. The silica glass rod may be prepared by the OVD method, the MCVD method, or the PCVD method.

[0068] The second preparation step is similar to that in the first embodiment, and therefore a description thereof will be omitted.

[0069] In the insertion step, as shown in FIG.

[0070] 10, the powder 120 is filled into the gap G between the silica glass tube 210 and the silica glass rod 220. At this time, similarly to the case of the first embodiment, it is preferable to fill the powder 120 so as to obtain a desired bulk density.

[0071] In the diffusion step, for example, an electric furnace is used to maintain a predetermined temperature for a predetermined time, thereby diffusing the alkali metal or alkaline earth metal into the inside of the silica glass rod 220. At this time, the alkali metal or alkaline earth metal is selectively diffused into the inside of the silica glass rod 220, similarly to the case of the first embodiment.

[0072] In the removal step, the powder may be removed by vibrating the silica glass rod or spraying an inert gas onto it, as in the case of embodiment 1. This results in a silica glass rod 230 having an alkali metal diffused therein, as shown in FIG.

[0073] In the diffusion step, similarly to the first embodiment, the heat treatment may be performed under conditions in which sintering of the silica powder does not progress significantly.

[0074] Moreover, similarly to the first embodiment, after the removing step, a second removing step may be carried out to remove the powder adhering to the silica glass rod.

[0075] Furthermore, since impurities may diffuse into the silica glass rod during the diffusion process, the outer circumferential surface of the silica glass rod may be polished to a small thickness.

[0076] In the cladding formation step, similarly to the first embodiment, the cladding 240 is formed so as to surround the outer periphery of the silica glass rod 230 as shown in Fig. 12. This results in an optical fiber preform 200 having the silica glass rod 230 doped with an alkali metal or alkaline earth metal as its core.

[0077] Moreover, by drawing the optical fiber preform 200 manufactured as described above by a known method, an optical fiber having an alkali metal or alkaline earth metal added to the core portion can be manufactured.

[0078] According to the manufacturing method of the optical fiber preform and the manufacturing method of the optical fiber of the embodiment 2 described above, similarly to the case of the embodiment 1, an alkali metal or an alkaline earth metal can be sufficiently doped with few impurities in the optical fiber preform and the optical fiber by a simple method.

[0079] Example 2 An optical fiber preform of Example 2 was manufactured by the manufacturing method according to the second embodiment, and an optical fiber was further manufactured. In Example 2, a silica glass rod was prepared by the VAD method and doped with 8000 ppmwt of chlorine. The outer diameter of the silica glass rod was 15 mm. A commercially available silica glass tube with an inner diameter of 35 mm and an outer diameter of 45 mm was also prepared. A powder containing an alkali metal component or an alkaline earth metal component and silica powder was prepared by mixing and dispersing silica powder with an average particle size of 200 μm and potassium carbonate. The concentration of potassium carbonate in the powder was 0.7 wt%.

[0080] The heat treatment temperature in the diffusion process was set to 1,100°C, and the heat treatment was performed at 1,100°C for 24 hours. The heat treatment conditions corresponded to conditions under which sintering of the silica powder did not proceed. However, after the removal process, the outer surface of the silica glass rod was polished. The outer diameter of the silica glass rod after polishing was 14.7 mm. In addition, the outer diameter of the silica glass tube (core rod) after jacketing and collapsing was 29.0 mm.

[0081] In Example 3, the peak concentration of potassium in the silica glass rod was chemically analyzed and found to be 0.09 wt%. The concentrations of other impurities were below the detection limit. Furthermore, the transmission loss of the manufactured optical fiber at a wavelength of 1550 nm was an extremely low value of 0.156 dB / km.

[0082] (Embodiment 3) FIG. 13 is a flow diagram of a method for manufacturing an optical fiber preform according to the third embodiment. In this manufacturing method, first, in step S301, a silica glass rod and a silica glass tube are prepared (first preparation step, third preparation step). Then, in step S302, a powder containing an alkali metal component or an alkaline earth metal component and silica powder is prepared (second preparation step). Then, in step S303, the powder is filled into the silica glass tube (filling step). Then, in step S304, the alkali metal or alkaline earth metal is diffused from the powder into the inside of the silica glass tube by heat treatment (diffusion step). Then, in step S305, the powder that is not fixed to the silica glass tube is removed from the silica glass tube into which the alkali metal has been diffused (removal step). Then, in step S306, the silica glass tube is jacketed around the silica glass rod (jacket step). Then, in step S307, a cladding portion is formed so as to surround the outer periphery of the jacketed silica glass tube (cladding portion forming step).

[0083] A detailed description will be given below. In the first preparation step, as in the first embodiment, a silica glass tube is prepared by drilling a hole in the center of a high-purity silica glass rod produced by, for example, the VAD method. Chlorine may be added when the silica glass tube is produced. Also, dopants such as fluorine, phosphorus, germanium, and aluminum may be co-added as necessary when the silica glass tube is produced.

[0084] In the third preparation step, a high-purity silica glass rod is prepared, for example, by the VAD method, as in the second embodiment. Chlorine may be added when the silica glass rod is prepared. Dopants such as fluorine, phosphorus, germanium, and aluminum may be added when the silica glass rod is prepared, if necessary.

[0085] The second preparation step is similar to that in the first and second embodiments, and therefore a description thereof will be omitted.

[0086] The filling step, the diffusion step, and the removal step are the same as those in the first embodiment, and therefore the description thereof will be omitted. In addition, a second removal step may be performed after the removal step, or the inner circumferential surface of the silica glass tube may be polished to a small thickness.

[0087] 14, in the jacketing process, the silica glass tube 310 is jacketed around the silica glass rod 320 and integrated by heating to form a core glass rod 330. The gap between the silica glass tube 310 and the silica glass rod 320 is blocked by the collapse of the silica glass tube 310.

[0088] In the cladding formation step, as in the first and second embodiments, the cladding 340 is formed to surround the outer periphery of the core glass rod 330 as shown in Fig. 15. This results in an optical fiber preform 300 having the core glass rod 330 doped with an alkali metal or alkaline earth metal as its core portion.

[0089] Moreover, by drawing the optical fiber preform 300 manufactured as described above by a known method, an optical fiber having an alkali metal or alkaline earth metal added to the core portion can be manufactured.

[0090] According to the manufacturing method of the optical fiber preform and the manufacturing method of the optical fiber of the embodiment 3 described above, similarly to the cases of the embodiments 1 and 2, an alkali metal or an alkaline earth metal can be sufficiently doped with few impurities in the optical fiber preform and the optical fiber by a simple method.

[0091] Example 3 The optical fiber preform of Example 3 was manufactured by the manufacturing method according to the third embodiment, and further, an optical fiber was manufactured. In Example 3, a silica glass rod to which 8000 ppmwt of chlorine was added and a silica glass tube to which 2000 ppmwt of chlorine and 1.1 wt% of fluorine were added, both manufactured by the VAD method, were prepared. The outer diameter of the silica glass rod was 10.5 mm. The inner diameter of the silica glass tube was 12 mm and the outer diameter was 30 mm. In addition, a powder containing an alkali metal component or an alkaline earth metal component and silica powder was prepared by mixing and dispersing silica powder having an average particle size of 200 μm and potassium carbonate. The concentration of potassium carbonate in the powder was 0.7 wt%.

[0092] The heat treatment temperature in the diffusion step was 1,100°C, and the heat treatment was performed at 1,100°C for 24 hours. The heat treatment conditions corresponded to conditions under which sintering of the silica powder did not proceed. However, after the removal step, the inner surface of the silica glass tube was polished. The inner diameter of the silica glass tube after polishing was 12.3 mm. In addition, the outer diameter of the silica glass tube (core glass rod) after jacketing and collapsing was 29.0 mm.

[0093] In Example 3, the peak concentration of potassium in the core glass rod was 0.08 wt% by chemical analysis. The concentrations of other impurities were below the detection limit. Furthermore, the transmission loss of the manufactured optical fiber at a wavelength of 1550 nm was an extremely low value of 0.155 dB / km.

[0094] The following Tables 1 and 2 show the production conditions and results of Examples 1-1 to 1-9, Examples 2 and 3, and Comparative Example 1.

[0095] [Table 1]

[0096] [Table 2]

[0097] In the above embodiment 1, a collapsing process for collapsing the silica glass tube is carried out after the diffusion process and before the cladding formation process. However, if the diameter of the hole in the silica glass tube is small, the collapsing process may be carried out in the process of drawing the optical fiber.

[0098] In the powder containing an alkali metal component or an alkaline earth metal component and silica powder, the alkali metal component or the alkaline earth metal component may be contained as a component of the silica powder.

[0099] Furthermore, the present invention is not limited to the above-mentioned embodiment. The present invention also includes a configuration in which the above-mentioned components are appropriately combined. Further effects and modifications can be easily derived by those skilled in the art. Therefore, the broader aspects of the present invention are not limited to the above-mentioned embodiment, and various modifications are possible. [Explanation of symbols]

[0100] 100, 200, 300: Optical fiber base material 110, 130, 210, 310: Silica glass tube 111: Inner surface 120: Powder 140, 220, 230, 320: Silica glass rod 150, 240, 340: Clad section 330: Core glass rod G: Gap

Claims

1. A first preparation step of preparing a silica glass tube; A second preparation step of preparing a powder containing an alkali metal component or an alkaline earth metal component and a silica powder; a filling step of filling the silica glass tube with the powder; a diffusion step of diffusing an alkali metal or an alkaline earth metal from the powder into the inside of the silica glass tube by heat treatment; a removing step of removing the powder not adhering to the silica glass tube from the silica glass tube having the alkali metal or alkaline earth metal diffused therein; a cladding forming step of forming a cladding around the outer periphery of the silica glass tube having the alkali metal or alkaline earth metal diffused therein; Equipped A method for manufacturing an optical fiber preform.

2. a collapsing step of collapsing the silica glass tube after the diffusion step and before the cladding portion forming step, In the cladding portion forming step, the alkali metal or alkaline earth metal is diffused into the inside of the silica glass tube, and the cladding portion is formed so as to surround the outer periphery of the solidified silica glass tube. The method for producing the optical fiber preform according to claim 1 .

3. In the first preparation step, the silica glass tube to which chlorine is added is prepared. The method for producing the optical fiber preform according to claim 1 .

4. A first preparation step of preparing a silica glass tube; A second preparation step of preparing a powder containing an alkali metal component or an alkaline earth metal component and a silica powder; A third preparation step of preparing a silica glass rod; an inserting step of inserting the silica glass rod into the silica glass tube; a filling step of filling the powder into a gap between the silica glass tube and the silica glass rod; a diffusion step of diffusing an alkali metal or an alkaline earth metal from the powder into the inside of the silica glass rod by heat treatment; a removing step of removing the powder not adhering to the silica glass rod from the silica glass rod having the alkali metal diffused therein; a cladding forming step of forming a cladding around the outer periphery of the silica glass rod having the alkali metal or alkaline earth metal diffused therein; Equipped A method for manufacturing an optical fiber preform.

5. In the third preparation step, the silica glass rod doped with chlorine is prepared. The method for producing an optical fiber preform according to claim 4 .

6. A first preparation step of preparing a silica glass tube; A second preparation step of preparing a powder containing an alkali metal component or an alkaline earth metal component and a silica powder; A third preparation step of preparing a silica glass rod; a filling step of filling the powder into the silica glass tube; a diffusion step of diffusing an alkali metal or an alkaline earth metal from the powder into the inside of the silica glass tube by heat treatment; a removing step of removing the powder not adhering to the silica glass tube from the silica glass tube having the alkali metal or alkaline earth metal diffused therein; a jacketing step of jacketing the silica glass tube onto the silica glass rod; a cladding forming step of forming a cladding so as to surround the outer periphery of the jacketed silica glass tube; Equipped A method for manufacturing an optical fiber preform.

7. In the first preparation step, the silica glass tube doped with chlorine is prepared, and in the third preparation step, the silica glass rod doped with chlorine is prepared. The method for producing an optical fiber preform according to claim 6 .

8. The method further includes a second removal step of removing the powder adhered to the silica glass tube or the silica glass rod after the removal step. The method for producing the optical fiber preform according to any one of claims 1 to 7.

9. the alkali metal component is contained as at least one type of alkali metal compound selected from the group consisting of an alkali metal silicate, an alkali metal carbonate, an alkali metal halide, an alkali metal nitrate, an alkali metal sulfate, and an alkali metal hydroxide; The alkaline earth metal component is contained as at least one type of alkaline earth metal compound selected from the group consisting of alkaline earth metal silicate, alkaline earth metal carbonate, alkaline earth metal halide, alkaline earth metal nitrate, alkaline earth metal sulfate, and alkaline earth metal hydroxide. The method for producing the optical fiber preform according to any one of claims 1 to 7.

10. In the diffusion step, the heat treatment is performed under conditions in which sintering of the silica powder does not progress significantly. The method for producing the optical fiber preform according to any one of claims 1 to 7.

11. An optical fiber is manufactured by drawing an optical fiber preform manufactured by the method for manufacturing an optical fiber preform according to any one of claims 1 to 7. A method for manufacturing optical fiber.

Citation Information

Patent Citations

  • Production of aqueous dispersion

    JP1984095923A

  • Method for producing optical fiber preform

    JP2012162409A

  • Method for producing glass preform

    JP2013199399A

  • Optical fiber manufacturing method and optical fiber preform manufacturing method

    JP6719505B2

  • Method and apparatus for making soot

    US20040206127A1