Electronic component and manufacturing method for electronic component

By manipulating dielectric grain sizes and incorporating side margins in the laminate structure, the peeling issue between internal electrode and dielectric layers is mitigated, improving the reliability of laminated ceramic capacitors.

JP2024146066AInactive Publication Date: 2024-10-15MURATA MFG CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023058771
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The peeling between internal electrode layers and dielectric layers in laminated ceramic capacitors is a common issue, particularly during the process of dividing the laminate into individual pieces or forming side margins, due to the differing physical properties of these components.

Method used

The electronic component design includes a laminate structure with internal electrode layers and dielectric layers, where the average grain size of dielectric grains in specific portions is manipulated to enhance adhesion, and side margins are formed to cover the laminate sides, with external electrodes connected to the internal layers, ensuring electrical connectivity.

Benefits of technology

This design significantly reduces the likelihood of peeling between the internal electrode and dielectric layers, enhancing the reliability and stability of the electronic component.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146066000001_ABST
    Figure 2024146066000001_ABST
Patent Text Reader

Abstract

To provide an electronic component in which the separation between an internal electrode layer and a dielectric layer is suppressed.SOLUTION: An electronic component includes: an element assembly including a multilayer body with a rectangular parallelepiped shape having main surfaces facing each other in a thickness direction, side surfaces facing each other in a width direction orthogonal to the thickness direction, and end surfaces facing each other in a length direction orthogonal to the thickness direction and the width direction, in which internal electrode layers 10 and dielectric layers 20 are alternately stacked in the thickness direction, and a side margin that covers both side surfaces of the multilayer body in the width direction; and an external electrode covering both end surfaces of the element assembly in the length direction and electrically connected to the internal electrode layer. The multilayer body includes a first part 301 existing at an end part of the multilayer body in the width direction in a part held between the internal electrode layers in the thickness direction, and a second part 302 existing in the center of the multilayer body in the width direction in the part held between the internal electrode layers in the thickness direction. The average particle diameter of dielectric grains 31 in the first part is larger than that of dielectric grains included in the second part.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electronic component and a method for manufacturing an electronic component. [Background technology]

[0002] 2. Description of the Related Art Electronic components such as ceramic capacitors that include a laminate in which internal electrode layers and dielectric layers are laminated may be provided with a protective portion for protecting the periphery of the internal electrode layers.

[0003] For example, Patent Document 1 discloses a method for manufacturing a multilayer ceramic capacitor in which a laminate in which internal electrodes and dielectric layers are laminated is prepared, side margins serving as protective sections are provided on the sides of the laminate, and then external electrodes are formed on the end faces. Patent Document 1 also discloses a method for manufacturing a laminate in which sheets serving as large-area internal electrodes and large-area dielectric layers are laminated, and then the sheets are diced to manufacture a large number of laminates at once. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2020-188086 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, because the internal electrodes and the dielectric layers constituting the laminate have different physical properties, there was a problem that the internal electrodes and the dielectric layers were prone to peeling off from each other, particularly when the laminate was divided into individual pieces or when the side margins were formed.

[0006] The present invention has been made to solve the above problems, and has an object to provide an electronic component in which peeling is less likely to occur between the internal electrode layers and the dielectric layers. [Means for solving the problem]

[0007] The electronic component of the present invention is an electronic component comprising: a rectangular laminate having main surfaces facing in a thickness direction, side surfaces facing in a width direction perpendicular to the thickness direction, and end surfaces facing in a length direction perpendicular to the thickness direction and the width direction, the laminate being formed by stacking internal electrode layers and dielectric layers in the thickness direction; and side margins covering both side surfaces in the width direction of the laminate; and external electrodes covering both end faces in the length direction of the element body and electrically connected to the internal electrode layers, wherein the laminate has a first portion located at an end of the laminate in the width direction among portions sandwiched between the internal electrode layers in the thickness direction, and a second portion located in the center of the laminate in the width direction among portions sandwiched between the internal electrode layers in the thickness direction, and the average grain size of dielectric grains contained in the first portion is larger than the average grain size of dielectric grains contained in the second portion.

[0008] The method for manufacturing an electronic component of the present invention includes a laminate precursor preparation step of preparing a rectangular parallelepiped laminate precursor having main surfaces facing in a thickness direction, side surfaces facing in a width direction perpendicular to the thickness direction, and end surfaces facing in a length direction perpendicular to the thickness direction and the width direction, in which a conductive paste layer serving as an internal electrode layer and a dielectric ceramic layer serving as a dielectric layer are stacked in the thickness direction, and the conductive paste layer is exposed on the side surface and the end surface; a side heating step of heating the side surface of the laminate precursor to remove the conductive paste layer exposed on the side surface of the laminate precursor and to cause grain growth of dielectric grains included in the dielectric ceramic layer adjacent to the conductive paste layer exposed on the side surface of the laminate precursor; a side margin forming step of forming side margins on both side surfaces in the width direction of the heated laminate; a firing step of firing the laminate precursor with the side margins formed thereon to obtain an element; and an external electrode forming step of forming external electrodes that cover both end surfaces in the length direction of the element and are electrically connected to the internal electrode layers. Effect of the Invention

[0009] According to the present invention, it is possible to provide an electronic component in which peeling is unlikely to occur between the internal electrode layer and the dielectric layer. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a perspective view that illustrates an example of an electronic component of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view of the electronic component shown in FIG. 1 taken along line AA. [Diagram 3] 3 is a cross-sectional view of the electronic component shown in FIG. 1 taken along line BB. [Figure 4] FIG. 4 is a partially enlarged view of the laminate in FIG. [Diagram 5] FIG. 5 is a diagram showing a schematic diagram of a difference in grain size of dielectric grains in a further enlarged partial view of the laminate shown in FIG. [Figure 6] FIG. 6 is a partial cross-sectional view of the WT surface of a laminate, illustrating typically differences in the particle size of dielectric grains in another example of an electronic component of the present invention. [Figure 7] FIG. 7 is a partial cross-sectional view of the WT surface of a laminate, illustrating typically differences in the particle size of dielectric grains in still another example of an electronic component of the present invention. [Figure 8] FIG. 8 is a partial cross-sectional view of the WT surface, which diagrammatically illustrates the state of dielectric grains in the laminate precursor before the side heating step is performed. [Figure 9] FIG. 9 is a partial cross-sectional view of the WT surface, which diagrammatically illustrates the state of dielectric grains in the laminate precursor after the side heating step has been carried out. [Figure 10] FIG. 10 is a perspective view illustrating an example of a side margin forming step. [Figure 11] FIG. 11 is a perspective view that illustrates an example of an element body prepared by a firing step. [Figure 12] FIG. 12 is a perspective view illustrating an example of the external electrode forming step. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The electronic component and the manufacturing method of the electronic component of the present invention will be described below. However, the present invention is not limited to the following configurations, and can be appropriately modified and applied within the scope of the present invention. Note that the present invention also includes a combination of two or more of the individual preferable configurations of the present invention described below.

[0012] In this specification, terms indicating the relationship between elements (e.g., "opposite," "orthogonal," etc.) and terms indicating the shape of an element (e.g., "rectangular prism") are not intended to be used in a strict sense, but are intended to include a substantially equal range, for example, a difference of a few percent.

[0013] The drawings shown below are schematic diagrams, and the dimensions, aspect ratios, and other scales may differ from those of the actual products.

[0014] The electronic component of the present invention is an electronic component comprising: a rectangular laminate having main surfaces facing in a thickness direction, side surfaces facing in a width direction perpendicular to the thickness direction, and end surfaces facing in a length direction perpendicular to the thickness direction and the width direction, the laminate being formed by stacking internal electrode layers and dielectric layers in the thickness direction; and side margins covering both side surfaces in the width direction of the laminate; and external electrodes covering both end faces in the length direction of the element body and electrically connected to the internal electrode layers, wherein the laminate has a first portion located at an end of the laminate in the width direction among portions sandwiched between the internal electrode layers in the thickness direction, and a second portion located in the center of the laminate in the width direction among portions sandwiched between the internal electrode layers in the thickness direction, and the average grain size of dielectric grains contained in the first portion is larger than the average grain size of dielectric grains contained in the second portion.

[0015] FIG. 1 is a perspective view that illustrates an example of an electronic component of the present invention.

[0016] The electronic component 1 shown in FIG. 1 comprises a rectangular parallelepiped base body 50 having a first main surface 50a and a second main surface 50b which are main surfaces facing in the thickness direction (the direction indicated by arrow T in FIG. 1), a first side surface 50c and a second side surface 50d which are side surfaces facing in a width direction (the direction indicated by arrow W in FIG. 1) perpendicular to the thickness direction, and a first end surface 50e and a second end surface 50f which are end surfaces facing in a length direction (the direction indicated by arrow L in FIG. 1) perpendicular to the thickness direction and the width direction, and a first external electrode 70e and a second external electrode 70f which cover the first end surface 50e and the second end surface 50f of the base body 50, respectively.

[0017] The first external electrode 70e extends from the first end face 50e and wraps around to cover the first main face 50a, the second main face 50b, the first side face 50c, and parts of the second side face 50d in addition to the first end face 50e of the element body. The second external electrode 70f extends from the second end face 50f and wraps around to cover the first main face 50a, the second main face 50b, the first side face 50c, and parts of the second side face 50d in addition to the second end face 50f of the element body. The first external electrode 70e and the second external electrode 70f cover parts of the surfaces of the first main surface 50a, the second main surface 50b, the first side surface 50c, and the second side surface 50d, respectively, but are not in contact with each other.

[0018] FIG. 2 is a cross-sectional view of the electronic component shown in FIG. 1 taken along line AA. The cross-sectional view shown in FIG. 2 is a cross-section parallel to the width direction (W) and thickness direction (T) of the electronic component 1 shown in FIG. 1, and therefore this cross-section is also referred to as a WT cross-section.

[0019] As shown in FIG. 2, the element body 50 has a laminate 30, and a first side margin 40c and a second side margin 40d that cover the first side surface 30c and the second side surface 30d, which are the sides of the laminate 30 in the width direction, respectively.

[0020] The laminate 30 is formed by laminating internal electrode layers 10 and dielectric layers 20 in the thickness direction. The internal electrode layers 10 are exposed on a first side surface 30c and a second side surface 30d of the multilayer body 30, respectively.

[0021] The dielectric layer 20 includes an intermediate dielectric layer 21, an upper dielectric layer 22, and a lower dielectric layer . The intermediate dielectric layer 21 is the portion of the dielectric layer 20 that is sandwiched between two internal electrode layers 10. The upper dielectric layer 22 is a dielectric layer 20 that is adjacent to one of the internal electrode layers 10 and is located on the side of the first main surface 30a of the laminate 30. The lower dielectric layer 23 is adjacent to one of the internal electrode layers 10 and is a dielectric layer 20 located on the second main surface 30b side of the laminate 30.

[0022] In the electronic component 1 shown in FIG. 2, the internal electrode layers 10 are exposed on the first side surface 30c and the second side surface 30d of the laminate 30, but in the electronic component of the present invention, the internal electrode layers do not have to be exposed on the first side surface and the second side surface of the laminate.

[0023] The first side margin 40c covers the entire first side surface 30c of the laminate 30. That is, among the dielectric layers 20 constituting the laminate 30, the side surfaces of the upper dielectric layer 22 and the lower dielectric layer 23 on the first side surface 30c side are also covered by the first side margin 40c. Similarly, the side surfaces of the upper dielectric layer 22 and the lower dielectric layer 23 on the second side surface 30d side are also covered by the second side margin 40d.

[0024] The boundaries between the laminate 30 and the first side margin 40c, and between the laminate 30 and the second side margin 40d can be determined from the formation of an interface and differences in grain size when the WT cross section of the electronic component is observed with a scanning electron microscope (SEM).

[0025] 3 is a cross-sectional view of the electronic component shown in FIG. 1 taken along line BB. The cross-sectional view shown in FIG. 3 is a cross-section parallel to the length direction (L) and thickness direction (T) of the electronic component 1, and therefore this cross-section is also referred to as an LT cross-section.

[0026] As shown in FIG. 3, the internal electrode layer 10 has a first internal electrode layer 10e exposed to a first end face 50e of the element body 50 and electrically connected to a first external electrode 70e, and a second internal electrode layer 10f exposed to a second end face 50f of the element body 50 and electrically connected to a second external electrode 70f.

[0027] The first end face 30e and a side margin (not shown) of the laminate 30 are exposed at the first end face 50e of the element body 50. Therefore, the portion of the first end face 50e of the element body 50 where the laminate 30 is exposed also serves as the first end face 30e of the laminate 30. Therefore, it can be said that the first internal electrode layer 10e is exposed at the first end face 30e of the multilayer body 30. Also, it can be said that the first external electrode 70e covers the first end face 30e of the multilayer body 30.

[0028] The second end face 30f and a side margin (not shown) of the laminate 30 are exposed at the second end face 50f of the element body 50. Therefore, the portion of the second end face 50f of the element body 50 where the laminate 30 is exposed also constitutes the second end face 30f of the laminate 30. Therefore, it can be said that the second internal electrode layer 10f is exposed at the second end face 30f of the multilayer body 30. Also, it can be said that the second external electrode 70f covers the second end face 30f of the multilayer body 30.

[0029] Of the internal electrode layers 10, the regions that face each other via the intermediate dielectric layer 21 are also referred to as opposing electrode portions, and the regions other than the opposing electrode portions are also referred to as extraction electrode portions. The distance in the longitudinal direction from the end of the first internal electrode layer 10e on the second end face 50f side to the second end face 50f of the element body 50, and the distance from the end of the second internal electrode layer 10f on the first end face 50e side to the first end face 50e of the element body 50 are also referred to as the L gap.

[0030] Hereinafter, preferred embodiments of each configuration of the electronic component of the present invention will be described.

[0031] [Dielectric layer] The dielectric layer includes a dielectric ceramic. Examples of dielectric ceramics include barium titanate (BaTiO3), calcium titanate (CaTiO3), strontium titanate (SrTiO3), magnesium titanate (MgTiO3), calcium zirconate (CaZrO3), calcium zirconate titanate [Ca(Zr,Ti)O3], barium zirconate (BaZrO3), and titanium oxide (TiO2). Furthermore, Mn compounds, Fe compounds, Cr compounds, Co compounds, Ni compounds, etc. may be added to these components. In addition to the above components, Ho, Dy, Tb, etc. may also be contained.

[0032] The dielectric layer is mainly composed of particles of dielectric ceramics (dielectric grains).

[0033] The dielectric grains may have a core-shell structure. The larger the particle size of the dielectric grains, the thicker the shell portion of the core-shell structure may be. A thicker shell portion improves reliability.

[0034] The thickness of the intermediate dielectric layer, the upper dielectric layer and the lower dielectric layer may differ. Of the dielectric layers, the region sandwiched between two internal electrode layers is the intermediate dielectric layer. Among the dielectric layers, the dielectric layer adjacent to one of the internal electrode layers and disposed closest to the first main surface of the laminate is the upper dielectric layer, and the dielectric layer adjacent to one of the internal electrode layers and disposed closest to the second main surface of the laminate is the lower dielectric layer.

[0035] The thickness of each intermediate dielectric layer is preferably 0.3 μm or more and 0.45 μm or less. The thicknesses of the upper and lower dielectric layers are preferably 10 μm or more and 30 μm or less, respectively.

[0036] The thickness of the dielectric layer is measured by the following method. First, the WT cross section of the laminate is exposed by polishing, and after polishing, the surface is observed with a scanning electron microscope. Five lines are assumed to divide the laminate into six equal parts in the width direction, and the average thickness of the dielectric layer on each line is taken as the thickness of the dielectric layer.

[0037] The number of dielectric layers is not particularly limited, but is preferably 100 layers or more and 600 layers or less. The number of upper and lower dielectric layers is also included in the number of dielectric layers.

[0038] [Internal electrode layer] Examples of conductive materials constituting the internal electrode layers include Ni, Cu, Ag, Pd, Au, and alloys of these.

[0039] The thickness of each internal electrode layer is preferably 0.3 μm or more and 0.45 μm or less, and more preferably 0.3 μm or more and 0.38 μm or less.

[0040] The number of the internal electrode layers is preferably 100 or more and 600 or less.

[0041] The thickness of the internal electrode layer is measured by the following method. First, the WT cross section of the laminate is exposed by polishing, and after polishing, the surface is observed with a scanning electron microscope. Five lines are assumed to divide the laminate into six equal parts in the width direction, and the average thickness of the internal electrode layer on each line is taken as the thickness of the internal electrode layer.

[0042] The projected area of ​​the internal electrode layers in the lamination direction is preferably 80% or more and 95% or less of the projected area of ​​the dielectric layers in the lamination direction.

[0043] The internal electrode layers may contain dielectric ceramics having the same composition as the dielectric ceramics contained in the dielectric layers.

[0044] The surface layer of the internal electrode layer may contain Sn as a solid solution. When Sn is dissolved in the surface layer of the internal electrode layer, reliability is improved.

[0045] It is preferable that the internal electrode layer has a first internal electrode layer that is exposed at a first end face of the laminate but not exposed at a second end face of the laminate, and a second internal electrode layer that is exposed at the second end face of the laminate but not exposed at the first end face of the laminate. The first internal electrode layer is exposed at a first end face of the laminate and is electrically connected to the first external electrode. The second internal electrode layer is exposed at a second end face of the laminate and is electrically connected to the second external electrode.

[0046] The first internal electrode layer and the second internal electrode layer have opposing electrode portions which are portions opposing each other in the thickness direction, and lead electrode portions which extend from the opposing electrode portions to the first end face or the second end face of the laminate. The first internal electrode layer and the second internal electrode layer face each other via the dielectric layer, so that the electronic component functions as a capacitor.

[0047] The distance from the end of the first internal electrode layer on the second end face side to the second end face, and the distance from the end of the second internal electrode layer on the first end face side to the first end face are also referred to as L gaps. The L gap is preferably 5 μm or more and 30 μm or less.

[0048] It is preferable that the ends of the internal electrode layers in the width direction are aligned. Specifically, it is preferable that the positions of the widthwise ends of the internal electrode layers are within 1 μm in the width direction. For example, when looking at the positions of the ends of the internal electrode layers constituting the laminate on the first side surface side of the laminate, it is preferable that the position of the end of the outermost internal electrode layer and the position of the end of the innermost internal electrode layer are within 1 μm in the width direction. Similarly, when looking at the position of the end portion on the second side surface of the laminate, it is preferable that the position of the end portion of the internal electrode layer arranged on the outermost side and the position of the end portion of the internal electrode layer arranged on the innermost side are within 1 μm in the width direction.

[0049] In the electronic component of the present invention, the average grain size of the dielectric grains contained in the first portion is larger than the average grain size of the dielectric grains contained in the second portion.

[0050] The laminate has a first portion and a second portion. The first portion is a portion located at an end in the width direction among the portions sandwiched between the internal electrode layers of the laminate. The second portion is a portion located at the center in the width direction among the portions sandwiched between the internal electrode layers of the laminate.

[0051] The first portion is preferably a portion sandwiched between the internal electrode layers of the laminate, the portion extending from one end of the laminate in the width direction (first side surface of the laminate) to 1 μm toward the other end of the laminate in the width direction (second side surface of the laminate) and the portion extending from the other end of the laminate in the width direction (second side surface of the laminate) to 1 μm toward one end of the laminate in the width direction (first side surface of the laminate).The second portion is preferably a portion sandwiched between the internal electrode layers of the laminate other than the first portion. That is, when the laminate is viewed in a WT cross section, among the portions sandwiched between the internal electrode layers, a region extending from the side surface of the laminate to 1 μm in the width direction is the first portion, and the remaining portion is the second portion.

[0052] FIG. 4 is a partially enlarged view of the laminate in FIG. As shown in FIG. 4, the laminate 30 has a first portion 301 and a second portion 302 .

[0053] The first portion 301 is a portion sandwiched between two internal electrode layers 10 and located at an end of the laminate 30 in the width direction. The second portion 302 is a portion sandwiched between two internal electrode layers 10 and located in the center of the laminate 30 in the width direction.

[0054] The length of the first portion 301 in the width direction is 1 μm. That is, of the portion sandwiched between the internal electrode layers 10, the first portion 301 corresponds to a 1 μm region extending from the first side surface 30c of the laminate 30 to the second side surface 30d, and a 1 μm region extending from the second side surface 30d to the first side surface 30c.

[0055] Of the portions of the laminate 30 sandwiched between the internal electrode layers 10 , the portions other than the first portion 301 are the second portion 302 .

[0056] Fig. 5 is a diagram showing a schematic diagram of differences in particle size of dielectric grains in a further enlarged partial view of the laminate shown in Fig. 4. The dielectric particles constituting the dielectric layer are also called dielectric grains. 5, the average grain size of the dielectric grains 31 included in the first portion 301 is larger than the average grain size of the dielectric grains 32 included in the second portion 302. Therefore, the dielectric grains 31a included in the first portion 301 are embedded in the internal electrode layer 10, and the adhesion between the dielectric layer 20 and the internal electrode layer 10 is improved by the anchor effect, and peeling can be prevented.

[0057] Of the dielectric grains included in the first portion, the dielectric grains exposed on the side surface of the laminate and the dielectric grains disposed inside thereof may have different grain sizes. 5, the average grain size of the dielectric grains exposed on the first side surface 30c or the second side surface 30d of the laminate 30 among the dielectric grains included in the first portion 301 is larger than the average grain size of the dielectric grains not exposed on the side surface of the laminate among the dielectric grains included in the first portion 301. Note that the dielectric grains exposed on the side surface of the laminate may have a core-shell structure by reacting with the surrounding additive material when heated.

[0058] The average grain size of the dielectric grains contained in the second portion is preferably 10 nm or more and less than 200 nm.

[0059] The average grain size of the dielectric grains contained in the first portion is preferably 200 nm or more and 1000 nm or less.

[0060] The average grain size of the dielectric grains (dielectric particles) can be measured using a scanning electron microscope (SEM). Specifically, an enlarged image of the intermediate dielectric layer near the center of the laminate in the thickness direction in the WT cross section of the laminate is captured using the SEM. In the captured image of the intermediate dielectric layer, the intermediate dielectric layer is divided into a first part and a second part, 20 dielectric grains are randomly selected from each of the first part and the second part, and the average value of the circle equivalent diameter calculated from the area of ​​each dielectric grain is set as the average grain size of the dielectric grains in that part. The field of view of the SEM when calculating the area of ​​the dielectric grains is 15 μm × 15 μm. However, dielectric grains that are incompletely included in the field of view (parts are not displayed) are not included in the grain size calculation.

[0061] When a dielectric grain is disposed across the first portion and the second portion, the dielectric grain is defined as a dielectric grain included in both the first portion and the second portion. However, when calculating the average grain size of the dielectric grains contained in the first portion and the average grain size of the dielectric grains contained in the second portion, the dielectric grains contained in both the first portion and the second portion are not included in the grain size calculation.

[0062] The dielectric grains included in the first portion may be necked together. When the dielectric grains in the first portion are necked together, the apparent average particle size of the dielectric grains increases and the dielectric grains are more strongly embedded in the internal electrode layers, improving the adhesion between the internal electrode layers and the dielectric layers, and making it possible to more effectively prevent peeling of the internal electrode layers. Furthermore, the dielectric grains included in the two first portions opposed to each other via the internal electrode layer may be necked together, in which case the necked dielectric grains penetrate the internal electrode layer.

[0063] The average grain size of the dielectric grains contained in the first portion is preferably not less than two times and not more than ten times the average grain size of the dielectric grains contained in the second portion.

[0064] The average grain size of the dielectric grains contained in the first portion is preferably larger than the thickness of the internal electrode layer. If the average grain size of the dielectric grains contained in the first portion is larger than the thickness of the internal electrode layer, the dielectric grains contained in the first portion tend to sink into the internal electrode layer.

[0065] The stack further includes a third portion. The third portion is a portion located at an end in the width direction of the laminate among the portions sandwiched between the dielectric layers in the thickness direction.

[0066] At least a part of the widthwise end portion of the internal electrode layer is preferably covered with the dielectric grains included in the third portion.

[0067] Fig. 6 is a partial cross-sectional view of the WT surface of a laminate, which shows a schematic diagram of the difference in grain size of the dielectric grains in another example of the electronic component of the present invention. Fig. 6 also shows an example in which the dielectric grains included in the third part of the laminate cover a part of the end of the internal electrode layer in the width direction.

[0068] The laminate 30 shown in FIG. 6 has a third portion 303 at an end in the width direction of the portion sandwiched between the intermediate dielectric layers 21. The length of the third portion 303 in the width direction is 1 μm. That is, among the portions sandwiched between the dielectric layers 20, the third portion 303 corresponds to a 1 μm region extending from the first side surface 30c of the laminate 30 toward the second side surface 30d, and a 1 μm region extending from the second side surface 30d toward the first side surface 30c.

[0069] As shown in FIG. 6, a part of the end face in the width direction of the internal electrode layer 10 is covered with the dielectric grains 33 included in the third portion 303. In FIG. 6, the portions of the widthwise ends of the internal electrode layers 10 that are covered with the dielectric grains 33 included in the third portion 303 are indicated by dashed lines.

[0070] By covering at least a part of the widthwise end portion of the internal electrode layer with the dielectric grains contained in the third portion, the effect of suppressing peeling of the internal electrode layer is enhanced.

[0071] The average grain size of the dielectric grains contained in the third portion is preferably larger than the average grain size of the dielectric grains contained in the second portion. In the laminate 30 shown in FIG. 6, the average grain size of the dielectric grains 33 contained in the third portion 303 is larger than the average grain size of the dielectric grains 32 contained in the second portion 302.

[0072] The average grain size of the dielectric grains contained in the third portion is preferably 200 nm or more and 1000 nm or less.

[0073] The average grain size of the dielectric grains contained in the third portion is preferably not less than two times and not more than ten times the average grain size of the dielectric grains contained in the second portion.

[0074] The dielectric grains included in the third portion may be necked together. Furthermore, the dielectric grains included in the first portion and the dielectric grains included in the third portion may be necked.

[0075] The average grain size of the dielectric grains contained in the third portion is preferably larger than the thickness of the internal electrode layer. When the average grain size of the dielectric grains contained in the third portion is larger than the thickness of the internal electrode layer, the entire end face of the internal electrode layer is easily covered by the third portion.

[0076] It is preferable that the entire ends of the internal electrode layers are covered with the dielectric grains contained in the third portion. When the entire ends of the internal electrode layers are covered with the dielectric grains contained in the third portion, peeling of the internal electrode layers can be particularly suppressed.

[0077] Fig. 7 is a partial cross-sectional view of the WT surface of a laminate, which shows a schematic diagram of the difference in grain size of the dielectric grains in yet another example of the electronic component of the present invention. Fig. 7 also shows an example in which the entire end of the width direction of the internal electrode layer is covered with the dielectric grains contained in the third part of the laminate.

[0078] The laminate 30 shown in FIG. 7 has a third portion 303 at an end in the width direction of the portion sandwiched between the dielectric layers 20. The entire widthwise end portions of the internal electrode layers 10 constituting the laminate 30 are covered with the dielectric grains 33 included in the third portion 303 . In FIG. 7, the portions of the widthwise ends of the internal electrode layers 10 that are covered with the dielectric grains 33 included in the third portion 303 are indicated by dashed lines. The average grain size of the dielectric grains 33 contained in the third portion 303 is larger than the average grain size of the dielectric grains 32 contained in the second portion 302 .

[0079] The average grain size of the dielectric grains contained in the third portion can be determined in the same manner as the average grain size of the dielectric grains contained in the first portion and the average grain size of the dielectric grains contained in the second portion. However, for a dielectric grain included in both the first and third portions, the belonging to the first or third portion is determined based on the center of gravity obtained from the outer shape of the dielectric grain. That is, when determining the particle size of the dielectric grain, the dielectric grain whose center of gravity is included in the first portion is treated as the dielectric grain included in the first portion, and the dielectric grain whose center of gravity is included in the third portion is treated as the dielectric grain included in the third portion. In addition, when the center of gravity of the dielectric grain cannot be easily obtained, the following method is used to determine whether the dielectric grain belongs to the first portion or the third portion. In this case, the grain in contact with the boundary with the side margin may be treated as the dielectric grain included in the third portion, and the dielectric grain included in the portion sandwiched between the end of the internal electrode layer in the width direction and the end of the laminate may be treated as the dielectric grain included in the first portion.

[0080] [Side Margin] Next, the side margins formed on the side surfaces of the laminate will be described. The sides of the laminate are each covered with a side margin. The side margin disposed on the first side surface of the laminate is the first side margin. The side margin disposed on the second side surface of the laminate is the second side margin.

[0081] The material constituting the side margin can be preferably the same as the material constituting the dielectric layer described above. Note that the material constituting the dielectric layer and the material constituting the side margin may be different from each other, but it is preferable that they are the same. The boundary between the side margin and the laminate can be easily confirmed, and therefore, even if the material constituting the side margin is the same as that of the dielectric layer, the dielectric grains constituting the side margin and the dielectric grains constituting the dielectric layer may be clearly distinguishable in some cases.

[0082] The thickness of the side margin is not particularly limited, but is preferably 10 μm or more and 30 μm or less.

[0083] Each side margin may be one layer or two or more layers. The number of layers in the side margin can be determined by observing with a scanning electron microscope (SEM) based on the difference in particle size of the particles that make up the side margin and the presence or absence of a boundary line (interface).

[0084] The sum of the thicknesses of the first side margin and the second side margin and the sum of the dimensions of the laminate in the width direction constitutes the length of the element in the width direction.

[0085] [External electrode] Next, the external electrodes formed on the end faces of the element body will be described. An element body with external electrodes formed on its end faces is an electronic component.

[0086] The external electrodes are provided so as to cover a first end face and a second end face, which are end faces in the longitudinal direction of an element body constituting an electronic component. The external electrode covering the first end face of the element body is the first external electrode, and the external electrode covering the second end face of the element body is the second external electrode.

[0087] The first external electrode is electrically connected to the first internal electrode layer exposed at the first end face of the laminate. The second external electrode is electrically connected to the second internal electrode layer exposed at the second end face of the laminate.

[0088] The external electrodes preferably include an underlying electrode layer and a plating layer disposed on the underlying electrode layer.

[0089] The base electrode layer preferably includes at least one layer selected from a baked layer, a resin layer, and a thin film layer.

[0090] The baked layer is formed by applying a conductive paste containing glass and metal to the element body and baking it. The conductive paste may be baked simultaneously with the firing of the internal electrodes, or may be baked after the firing of the internal electrodes.

[0091] When the conductive paste is baked simultaneously with the firing of the internal electrode layers, it is preferable that the common material contains the same dielectric ceramic as the dielectric ceramic constituting the laminate in an amount of about 30% by weight or more and less than 40% by weight. The fired layer, which is fired simultaneously with the firing of the internal electrodes, contains glass.

[0092] The glass contained in the baking layer may be, for example, a boric acid-based glass. Examples of metals contained in the baked layer include Ni, Cu, Ag, Pd, Au, and alloys thereof.

[0093] The baking layer may be a multi-layer.

[0094] The resin layer may contain conductive particles and a thermosetting resin.

[0095] Examples of the conductive particles constituting the resin layer include particles containing Ni, Cu, Ag, Pd, Au, and alloys thereof.

[0096] The thermosetting resin constituting the resin layer includes an epoxy resin and the like.

[0097] The resin layer may be formed directly on the end face of the element body. When a resin layer is provided, the above-mentioned baked layer is not necessary, and the resin layer may be provided directly on the end face of the element body.

[0098] The resin layer may be a multi-layered layer.

[0099] The thin film layer is a layer of metal particles deposited to a thickness of 1 μm or less, formed by a thin film formation method such as sputtering or vapor deposition.

[0100] Examples of metal particles that form the thin film layer include particles containing Ni, Cu, Ag, Pd, Au, and alloys thereof.

[0101] The plating layer is a layer formed by subjecting the surface of the base electrode layer to a plating treatment. The plating layer may be formed by electrolytic plating or electroless plating.

[0102] Examples of conductive materials constituting the plating layer include Ni, Sn, Cu, Ag, Pd, Au, and alloys thereof.

[0103] The plating layer may be a multi-layer structure, for example, a two-layer structure of a Ni plating layer and a Sn plating layer formed on the surface of the Ni plating layer. The Ni plating layer can prevent the underlying electrode layer from being eroded by solder when electronic components are mounted. The Sn plating layer improves the wettability of the solder when mounting electronic components, thereby improving mountability.

[0104] The length (L dimension) of the electronic component in the longitudinal direction is preferably 0.1 mm or more and 1.0 mm or less. The width and height dimensions (W dimension and T dimension) of the electronic component are preferably 0.05 mm or more and 0.5 mm or less, respectively. The L, W and T dimensions of an electronic component include not only the element body but also the external electrodes.

[0105] [Electronic component manufacturing method] The method for manufacturing an electronic component of the present invention includes a laminate precursor preparation step of preparing a rectangular parallelepiped laminate precursor having main surfaces facing in a thickness direction, side surfaces facing in a width direction perpendicular to the thickness direction, and end surfaces facing in a length direction perpendicular to the thickness direction and the width direction, in which a conductive paste layer serving as an internal electrode layer and a dielectric ceramic layer serving as a dielectric layer are stacked in the thickness direction, and the conductive paste is exposed on the side surfaces and the end surfaces; a side heating step of heating the side surfaces of the laminate precursor to remove the conductive paste layer exposed on the side surfaces of the laminate precursor and to cause grain growth of dielectric grains included in the dielectric ceramic layer adjacent to the conductive paste layer exposed on the side surfaces of the laminate precursor; a side margin forming step of forming side margins on both side surfaces in the width direction of the heated laminate precursor; a firing step of firing the laminate precursor with the side margins formed thereon to obtain an element; and an external electrode forming step of forming external electrodes that cover both end faces in the length direction of the element and are electrically connected to the internal electrode layers.

[0106] [Laminate precursor preparation process] In the laminate precursor preparation step, a laminate precursor is prepared. The laminate precursor preparation step can use a known method for producing a rectangular parallelepiped laminate precursor in which conductive paste layers that will become internal electrode layers and dielectric ceramic layers that will become dielectric layers are laminated.

[0107] For example, a ceramic sheet laminate can be obtained by preparing a first ceramic green sheet having a conductive paste applied onto a dielectric sheet to form a first internal electrode layer, and a second ceramic green sheet having a conductive paste applied onto a dielectric sheet to form a second internal electrode layer, and stacking them so that the lead-out directions of the first internal electrode layer and the second internal electrode layer are different from each other.

[0108] The dielectric sheet can be formed, for example, from a ceramic slurry containing a dielectric ceramic.

[0109] A conductive paste that will become the internal electrode layers can be printed in a predetermined pattern on the surface of the dielectric sheet to obtain the first ceramic green sheet and the second ceramic green sheet.

[0110] The first and second ceramic green sheets do not necessarily need to be alternately laminated, and a dielectric sheet not coated with a conductive paste may be laminated between the first and second ceramic green sheets as necessary, which allows the distance between the first and second internal electrode layers to be adjusted.

[0111] In addition, when stacking the first ceramic green sheet and the second ceramic green sheet, an upper dielectric layer and a lower dielectric layer can be formed among the dielectric layers by stacking dielectric sheets on the bottom and top layers that are not coated with conductive paste.

[0112] The ceramic sheet laminate may be a large unsingulated sheet or a single laminate. When the ceramic sheet laminate is a large sheet that has not been divided into individual pieces, it may be cut into individual pieces.

[0113] The obtained ceramic sheet laminate, or a piece cut from the laminate, serves as a laminate precursor.

[0114] [Side heating process] In the side surface heating step, the side surface of the laminate precursor is heated.

[0115] Fig. 8 is a partial cross-sectional view of the WT surface, which shows a schematic view of the dielectric grains in the laminate precursor before and after the side heating step is performed. Fig. 9 is a partial cross-sectional view of the WT surface, which shows a schematic view of the dielectric grains in the laminate precursor after the side heating step is performed. As shown in FIG. 8, before the side heating step is carried out, the laminate precursor 130 is formed by laminating conductive paste layers 110 which will become internal electrode layers and dielectric ceramic layers 120 which will become dielectric layers.

[0116] The laminate precursor 130 has a first portion and a second portion. However, the first portion 1301 and the second portion 1302 of the laminate precursor 130 correspond to the first portion 301 and the second portion 302 of the laminate 30. That is, the positions of the first portion 301 and the second portion 302 when the laminate 30 is formed by the firing process described below are the same as the positions of the first portion 1301 and the second portion 1302 in the laminate precursor 130 before the firing process is performed.

[0117] The first portion 1301 is a portion of the laminate precursor 130 that is sandwiched between the conductive paste layers 110 and that is located at an end in the width direction. The second portion 1302 is a portion of the laminate precursor 130 that is sandwiched between the conductive paste layers 110 and that is located in the center in the width direction.

[0118] As shown in FIG. 8, in the laminate precursor 130 before the side heating process, the average grain size of the dielectric grains 31 contained in the first portion 1301 is equal to the average grain size of the dielectric grains 32 contained in the second portion 1302.

[0119] In contrast, in the laminate precursor that has been subjected to the side heating step, the dielectric grains 31 contained in the first portion 1301 grow and the grain size increases, as shown in Fig. 9. On the other hand, the dielectric grains 32 contained in the second portion 1302 do not grow because they are not affected by the heating. As a result, the average grain size of the dielectric grains 31 contained in the first portion 1301 becomes larger than the average grain size of the dielectric grains 32 contained in the second portion 1302.

[0120] Although not shown in Figures 8 and 9, the laminate precursor has a third portion. The position of the third portion of the laminate precursor is the same as the position of the third portion of the laminate after firing.

[0121] In the side heating step, the side of the laminate precursor is preferably heated to a temperature of 1000°C or higher and lower than 1500°C, and more preferably heated to a temperature of 1000°C or higher and 1300°C or lower.

[0122] In the side surface heating step, the side surface of the laminate precursor is preferably heated at a temperature of 1000° C. or more and less than 1500° C. for a time of 100 μsec or more and 2000 μsec or less.

[0123] The method for heating the side surface of the laminate precursor is not particularly limited, but may be, for example, irradiation with a flashlight.

[0124] When the side surface of the laminate precursor is irradiated with a flashlight, the degree of heating can be adjusted by the voltage applied to the flashlight, the irradiation time, and the number of irradiations. Examples of the radiation source (light source) of the flashlight include xenon. The voltage applied to the flashlight is preferably 1500V or more and 2000V or less.

[0125] By heating the side surface of the laminate precursor in the side surface heating step, the dielectric grains contained in the first portion near the side surface of the laminate precursor grow, and the grain size of the dielectric grains becomes larger than that before heating. On the other hand, since the dielectric grains that are not in the vicinity of the side surfaces of the laminate precursor are not heated by the side surface heating step, the particle size of the dielectric grains remains the same as before the side surface heating step. Therefore, the average particle size of the dielectric grains contained in the dielectric layers arranged near the side surfaces of the laminate precursor is larger than the average particle size of the dielectric grains contained in the dielectric layers not arranged near the side surfaces of the laminate precursor.

[0126] The dielectric grains present in the vicinity of the side surface of the laminate precursor and included in the first portion of the laminate undergo grain growth by the side surface heating step. Therefore, the electronic component of the present invention can be obtained by carrying out the side heating step.

[0127] In the side surface heating step, both the first side surface and the second side surface of the laminate are heated. The first and second sides of the laminate may be heated simultaneously or separately.

[0128] When the first and second sides of the laminate are heated separately, the order of heating is not particularly limited, and the first side may be heated first and the second side may be heated later, or the second side may be heated first and the first side may be heated later.

[0129] When the first side and the second side are heated separately, for example, a method can be used in which a flat jig having multiple recesses on a metal surface is prepared, the laminate precursor is poured into the recesses with the surface to be heated facing upward, and the upper surface is heated. For example, by using the processing method for ceramic chip components described in JP 2020-144700 A, the laminate precursor can be inserted into the recess of the jig so that the surface to be heated faces upward.

[0130] In the side heating step, the dielectric grains on the side surfaces of the laminate precursor may grow, so that the grown dielectric grains cover at least a part of the side surfaces of the conductive paste layer. Alternatively, the grown dielectric grains may cover the entire side surfaces of the conductive paste layer.

[0131] In the side heating step, the surface of the laminate precursor is preferably heated until the average grain size of the grown dielectric grains reaches 200 nm or more and 1000 nm or less.

[0132] In the side heating step, a part of the conductive paste layer exposed on the side surface of the laminate precursor is removed. As a method for removing the part of the conductive paste layer, for example, a method for evaporating the conductive paste layer exposed on the side surface of the laminate precursor by heating can be mentioned.

[0133] In the laminate precursor obtained by cutting and dividing the ceramic sheet laminate, the conductive paste that becomes the internal electrodes may deform at the cut surface, and multiple conductive paste layers stacked in the thickness direction may come into contact with each other. By removing a part of the conductive paste layer by the above process, the cutting sagging can be removed, and short-circuiting of the internal electrode layers in the laminate after firing can be prevented.

[0134] [Side margin formation process] In the side margin forming step, a side margin is formed on each of both widthwise side surfaces of the heated laminate precursor. As the side margin forming step, a conventionally known method for forming a side margin can be used.

[0135] In the side margin forming process, for example, side margins can be formed on both widthwise sides of the laminate precursor by attaching a side margin forming sheet that will serve as the side margin to both widthwise sides of the laminate precursor.

[0136] The side margin forming sheet can be obtained, for example, by mixing raw material particles that make up the side margin with an organic binder and a solvent to prepare a side margin slurry, which is then coated on a flat plate and dried. The raw material particles constituting the side margins can be made of the same material as the dielectric grains constituting the dielectric sheet.

[0137] [Firing process] In the firing step, the laminate precursor with the side margins formed thereon is fired to obtain an element body. The firing conditions are not particularly limited, but for example, when the dielectric ceramic is barium titanate, firing may be performed at a temperature of 1000 to 1300° C. for several hours. The calcination can be carried out, for example, in a reducing atmosphere or in an atmosphere with a low oxygen partial pressure.

[0138] By firing, the conductive paste layers become internal electrode layers, the dielectric ceramic layers become dielectric layers, and the laminate precursor becomes a laminate, resulting in an element body having side margins formed on both side surfaces of the laminate.

[0139] Fig. 10 is a perspective view showing an example of a side margin forming step, and Fig. 11 is a perspective view showing an example of an element body prepared by a firing step. 10, in the side margin forming step, a side margin forming sheet 140 that becomes a side margin is attached to the first side surface 130c and the second side surface 130d of the laminate precursor 130. Next, the laminate precursor with the side margin formed therein is fired to obtain the element body 50 shown in FIG.

[0140] The element 50 has a rectangular shape having a first main surface 50a and a second main surface 50b facing each other in the thickness direction, a first side surface 50c and a second side surface 50d facing each other in the width direction, and a first end surface 50e and a second end surface 50f facing each other in the length direction.

[0141] The element may be subjected to a polishing process such as barrel rolling. By subjecting the element body to a polishing process such as barrel rolling, the corners and ridges of the element body can be rounded.

[0142] [External electrode formation process] In the external electrode formation step, external electrodes are formed to cover both end faces in the longitudinal direction of the element body and to be electrically connected to the internal electrode layers.

[0143] There are no particular limitations on the method for forming the external electrodes on the end faces of the element body, and any conventional method for forming external electrodes can be used.

[0144] In the external electrode forming step, for example, it is preferable to carry out a base electrode forming step of forming a base electrode on the end face of the element body, and a plating layer forming step of forming a plating layer on the surface of the base electrode.

[0145] FIG. 12 is a perspective view illustrating an example of the external electrode forming step. The electronic component 1 shown in FIG. 12 is obtained by forming a first external electrode 70e and a second external electrode 70f on the first end face 50e and the second end face 50f, respectively, of the element body 50 shown in FIG.

[0146] The first external electrode 70e is electrically connected to the first internal electrode layer 10e exposed at the first end face 50e of the element body 50. The first external electrode 70e may wrap around and cover not only the first end face 50e of the element body 50, but also parts of the first main face 50a, the second main face 50b, the first side face 50c, and the second side face 50d.

[0147] The second external electrode 70f is electrically connected to the second internal electrode layer 10f exposed at the second end face 50f of the element body 50. The second external electrode 70f may wrap around and cover not only the second end face 50f of the element body 50, but also parts of the first principal face 50a, the second principal face 50b, the first side face 50c, and the second side face 50d. However, the first external electrode 70e and the second external electrode 70f are configured not to be in contact with each other.

[0148] However, the electronic component of the present invention can also be obtained by carrying out the external electrode formation step on a laminate precursor on which side margins have been formed before the firing step, and then firing the laminate precursor. In particular, when forming a firing layer as a base layer for an external electrode, a conductive paste containing glass and metal is applied to the first end face and the second end face of the laminate precursor on which side margins have been formed before undergoing the firing process, and then fired, thereby enabling the formation of the element body and the formation of the firing layer to be carried out simultaneously.

[0149] This specification describes the following:

[0150] The present disclosure (1) provides an element body including a rectangular parallelepiped laminate having main surfaces facing in a thickness direction, side surfaces facing in a width direction perpendicular to the thickness direction, and end surfaces facing in a length direction perpendicular to the thickness direction and the width direction, in which internal electrode layers and dielectric layers are laminated in the thickness direction, and side margins covering both side surfaces of the laminate in the width direction, an external electrode covering each of both end faces in the longitudinal direction of the element body and electrically connected to the internal electrode layer, the laminate has a first portion located at an end of the laminate in the width direction among portions sandwiched between the internal electrode layers in the thickness direction, and a second portion located at a center of the laminate in the width direction among portions sandwiched between the internal electrode layers in the thickness direction, The electronic component is characterized in that the average grain size of the dielectric grains contained in the first portion is larger than the average grain size of the dielectric grains contained in the second portion.

[0151] The present disclosure (2) is directed to a method for manufacturing a laminate comprising the steps of: forming a first insulating film having a first insulating layer and a second insulating layer; The electronic component according to the present disclosure (1), wherein at least a part of the end portion in the width direction of the internal electrode layer is covered by the dielectric grains included in the third portion.

[0152] The present disclosure (3) is the electronic component according to the present disclosure (2), wherein the average grain size of the dielectric grains included in the third portion is larger than the average grain size of the dielectric grains included in the second portion.

[0153] The present disclosure (4) is the electronic component according to the present disclosure (2) or (3), in which the entire ends of the internal electrode layers are covered by the dielectric grains included in the third portion.

[0154] The present disclosure (5) is the electronic component according to any one of the present disclosures (2) to (4), in which the average grain size of the dielectric grains contained in the third portion is larger than the thickness of the internal electrode layer.

[0155] The present disclosure (6) is the electronic component according to any one of the present disclosures (1) to (5), in which the average grain size of the dielectric grains contained in the first portion is not less than 200 nm and not more than 1000 nm.

[0156] The present disclosure (7) provides a laminate precursor preparation process for preparing a rectangular parallelepiped laminate precursor having main surfaces facing in a thickness direction, side surfaces facing in a width direction perpendicular to the thickness direction, and end surfaces facing in a length direction perpendicular to the thickness direction and the width direction, in which conductive paste layers to become internal electrode layers and dielectric ceramic layers to become dielectric layers are laminated in the thickness direction, and the conductive paste layers are exposed on the side surfaces and the end surfaces; a side heating step of heating the side surface of the laminate precursor to remove the conductive paste layer exposed on the side surface of the laminate precursor and to grow dielectric grains included in the dielectric ceramic layer adjacent to the conductive paste layer exposed on the side surface of the laminate precursor; a side margin forming step of forming side margins on both side surfaces in the width direction of the heated laminate precursor; a firing step of firing the laminate precursor having the side margins formed thereon to obtain a body; an external electrode forming step of forming external electrodes covering both end faces of the element body in the longitudinal direction and electrically connecting to the internal electrode layers; The method for producing an electronic component is characterized by comprising the steps of:

[0157] The present disclosure (8) is the method for producing an electronic component according to the present disclosure (7), wherein in the side heating step, a flashlight is irradiated onto a side surface of the laminate precursor.

[0158] The present disclosure (9) is the method for producing an electronic component according to the present disclosure (7) or (8), wherein in the side heating step, the side of the laminate precursor is heated to a temperature of 1000°C or higher and lower than 1500°C.

[0159] The present disclosure (10) is the method for producing an electronic component according to any one of the present disclosures (7) to (9), wherein the average grain size of the grown dielectric grains is 200 nm or more and 1000 nm or less.

[0160] The present disclosure (11) is a method for producing an electronic component according to any one of the present disclosures (7) to (10), wherein in the side heating process, the grown dielectric grains cover at least a portion of a side surface of the conductive paste layer.

[0161] The present disclosure (12) is a method for producing an electronic component according to any one of the present disclosures (7) to (10), wherein in the side heating process, the grown dielectric grains cover the entire side of the conductive paste layer. EXAMPLES

[0162] EXAMPLES Hereinafter, examples that more specifically disclose the present invention will be described, however, the present invention is not limited to these examples.

[0163] Example 1 [Laminate precursor preparation process] An organic binder, a plasticizer, and ethanol and toluene as dispersion media were added to BaTiO3 as a dielectric material, and the mixture was wet-mixed in a ball mill with PSZ balls to create a ceramic slurry for sheet molding. This ceramic slurry was formed into a sheet by a doctor blade method to obtain a rectangular ceramic green sheet A. Moreover, a ceramic green sheet B was obtained in the same manner.

[0164] A conductive paste containing Ni as a conductive component was printed on ceramic green sheet A, and a conductive paste layer for constituting an internal electrode layer was formed on the dielectric sheet to form a first ceramic green sheet and a second ceramic green sheet.

[0165] The first ceramic green sheet and the second ceramic green sheet on which the conductive paste layer was printed were stacked so that the sides on which the conductive paste layer was pulled out were staggered, and the top and bottom surfaces were sandwiched between six ceramic green sheets B, respectively, and pressed to separate the sheets into individual pieces to obtain a laminate precursor. The conductive paste layers that were to become internal electrode layers were exposed on both side surfaces of the obtained laminate precursor.

[0166] [Side heating process] A flashlight was irradiated onto one side of the obtained laminate precursor, and the side of the laminate precursor was heated. The side temperature of the laminate precursor during heating varies depending on the voltage of the flashlight. Here, the voltage of the flashlight was adjusted so that the side temperature of the laminate precursor was about 1000°C. Further, the other side surface of the unheated laminate precursor was also irradiated with a flashlight under the same conditions and heated.

[0167] [Side margin formation process] A ceramic green sheet was produced using the ceramic slurry prepared in the laminate precursor preparation step, and used as a sheet for forming a side margin. Side margin forming sheets were attached to both side surfaces of the laminate precursor whose side surfaces had been heated in the side heating step.

[0168] [Firing process] The laminate precursor with the side margin forming sheet attached was heated at 1300° C. for several hours in a reducing atmosphere to obtain an element.

[0169] [External electrode formation process] A slurry consisting of glass and metal particles was applied to the end faces of the obtained element body, which was then fired at 800 to 900°C for several hours to form baked electrodes. After that, a Ni / Sn plating layer was formed by plating, and an electronic component of Example 1 was obtained in which external electrodes were formed on the end faces of the element body. The internal electrode layers had an average thickness of 450 nm and contained 300 layers. The upper electrode layer, intermediate dielectric layer and lower electrode layer each had a thickness of 0.3 to 0.4 μm, and the total number of dielectric layers, including the upper electrode layers, intermediate electrode layers and lower dielectric layers, was 1000. The dimensions of the resulting electronic component, taking into account the external electrode layers and tolerances, were 0.5 mm thick, 0.5 mm high, and 1 mm long.

[0170] (Examples 2 to 5 and Comparative Examples 1 to 3) Electronic components according to Examples 2 to 5 and Comparative Examples 2 to 3 were manufactured using the same procedure as in Example 1, except that the voltage applied to the flashlight in the side heating process was adjusted to change the heating temperature of the side of the laminate during heating as shown in Table 1. Moreover, an electronic component according to Comparative Example 1 was manufactured in the same manner as in Example 1, except that the side heating step was not performed.

[0171] [Table 1]

[0172] [Measurement of the average particle size of the dielectric grains contained in the first and second parts] The electronic components according to each of the examples and comparative examples were cut approximately at the center in the length direction, polished, and the WT cross section was photographed by SEM to determine the average grain size of the dielectric grains in the first and second portions. The results are shown in Table 1.

[0173] [Reliability test] 500 electronic components according to each of the examples and comparative examples were used, and a voltage (25 V) lower than the dielectric breakdown voltage (65 V) but higher than the rated voltage (10 V) was applied, and then the insulation resistance value was measured. The number of samples whose measured insulation resistance value was lower than the specified value (45.5 MΩ) was counted. The results are shown in Table 1. When peeling occurs between the internal electrode layer and the dielectric layer, the insulation resistance value decreases, so it can be said that the more samples there are that have insulation resistance values ​​below the specified value, the more likely peeling is to occur between the internal electrode layer and the dielectric layer.

[0174] The results in Table 1 show that in Examples 1 to 5 in which the side surface of the laminate precursor was heated to a temperature of 1000° C. or higher and lower than 1500° C., interlayer peeling could be suppressed. Also, it was confirmed that the dielectric grains contained in the first portion grew in Examples 1 to 5. It is considered that the average grain size of the dielectric grains contained in the first portion became larger than the average grain size of the dielectric grains contained in the second portion by the side heating process, and therefore the adhesion between the internal electrode layer and the dielectric layer was increased at the end of the internal electrode layer in the width direction, and peeling was suppressed.

[0175] On the other hand, in Comparative Example 1 in which the side heating step was not performed and Comparative Example 2 in which the flashlight output was significantly reduced and the end face of the laminate precursor was heated at 400° C., peeling between layers could not be suppressed. This is presumably because the dielectric grains contained in the first portion were not sufficiently heated in the side heating step and did not grow.

[0176] In the electronic component according to Comparative Example 3, a part of the conductive paste layer was evaporated by the side heating process, and the electronic component did not function. In addition, it was impossible to measure the average grain size of the dielectric grains contained in the first portion. Therefore, an evaluation of peeling between layers was not performed. [Explanation of symbols]

[0177] 1. Electronic Components 10 Internal electrode layer 10e 1st internal electrode layer 10f 2nd internal electrode layer 20 Dielectric layer 21 Intermediate dielectric layer 22 Upper dielectric layer 23 Lower dielectric layer 30 Laminate 30a: First main surface of laminate 30b Second main surface of laminate 30c: first side of laminate 30d Layered second side 30e: first end surface of laminate 30f: second end surface of laminate 31, 31a Dielectric grains included in the first portion 32 Dielectric grains contained in the second part 33 Dielectric grains included in the third part 40 Side Margin 40c 1st side margin 40b Second Side Margin 50 Base 50a: First principal surface of element 50b: second main surface of the body 50c Body first side 50d Second side of the body 50e First end face of element 50f Second end face of element 70e 1st external electrode 70f 2nd external electrode 110 Conductive paste layer 120 Dielectric ceramic layer 130 Laminate precursor 130c: First side of laminate precursor 130d Second side of laminate precursor 140 Side margin forming sheet 301 First part of laminate 302 Second part of the laminate 303 Third part of laminate 1301 First part of laminate precursor 1302 Second part of laminate precursor

Claims

1. an element body including: a rectangular parallelepiped laminate having main surfaces facing in a thickness direction, side surfaces facing in a width direction perpendicular to the thickness direction, and end surfaces facing in a length direction perpendicular to the thickness direction and the width direction, in which internal electrode layers and dielectric layers are laminated in the thickness direction; and side margins covering both side surfaces of the laminate in the width direction; an external electrode covering each of both end faces in the longitudinal direction of the element body and electrically connected to the internal electrode layer, the laminate has a first portion located at an end of the laminate in the width direction among portions sandwiched between the internal electrode layers in the thickness direction, and a second portion located at a center of the laminate in the width direction among portions sandwiched between the internal electrode layers in the thickness direction, an average grain size of the dielectric grains contained in the first portion being larger than an average grain size of the dielectric grains contained in the second portion;

2. the laminate further has a third portion located at an end in the width direction of the portion sandwiched between the dielectric layers in the thickness direction, The electronic component according to claim 1 , wherein at least a portion of an end portion in the width direction of the internal electrode layer is covered by dielectric grains included in the third portion.

3. 3. The electronic component according to claim 2, wherein an average grain size of the dielectric grains contained in the third portion is larger than an average grain size of the dielectric grains contained in the second portion.

4. 4. The electronic component according to claim 2, wherein the entire ends of the internal electrode layers are covered with dielectric grains included in the third portion.

5. The electronic component according to claim 2 , wherein an average grain size of the dielectric grains contained in the third portion is larger than a thickness of the internal electrode layer.

6. 3. The electronic component according to claim 1, wherein an average grain size of the dielectric grains contained in the first portion is not less than 200 nm and not more than 1000 nm.

7. a laminate precursor preparation step of preparing a rectangular parallelepiped laminate precursor having main surfaces opposed in a thickness direction, side surfaces opposed in a width direction perpendicular to the thickness direction, and end surfaces opposed in a length direction perpendicular to the thickness direction and the width direction, in which conductive paste layers serving as internal electrode layers and dielectric ceramic layers serving as dielectric layers are laminated in the thickness direction, and the conductive paste layers are exposed on the side surfaces and the end surfaces; a side heating step of heating the side surface of the laminate precursor to remove the conductive paste layer exposed on the side surface of the laminate precursor and to grow dielectric grains included in the dielectric ceramic layer adjacent to the conductive paste layer exposed on the side surface of the laminate precursor; a side margin forming step of forming side margins on both side surfaces in the width direction of the heated laminate precursor; a firing step of firing the laminate precursor having the side margins formed thereon to obtain a body; an external electrode forming step of forming external electrodes covering both end faces of the element body in the longitudinal direction and electrically connecting the internal electrode layers; A method for manufacturing an electronic component, comprising:

8. The method for producing an electronic component according to claim 7 , wherein in the side heating step, a flashlight is irradiated onto the side surface of the laminate precursor.

9. The method for producing an electronic component according to claim 7 or 8, wherein in the side surface heating step, the side surface of the laminate precursor is heated to a temperature of 1000° C. or higher and lower than 1500° C.

10. 9. The method for producing an electronic component according to claim 7, wherein an average grain size of the grown dielectric grains is 200 nm or more and 1000 nm or less.

11. The method for producing an electronic component according to claim 7 or 8, wherein in the side surface heating step, at least a part of the side surface of the conductive paste layer is covered with the grown dielectric grains.

12. 9. The method for producing an electronic component according to claim 7, wherein in the side surface heating step, the grown dielectric grains cover the entire side surfaces of the conductive paste layer.

Citation Information

Patent Citations

  • Multilayer ceramic electronic component

    JP2020188086A