Martensitic stainless steel and method of producing the same
By optimizing martensite and ferrite phases in martensitic stainless steel through controlled heat treatment and phase generation, the steel achieves a balanced strength and workability, addressing weldability issues and maintaining low cost.
Patent Information
- Application Number
- JP2023059096
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Martensitic stainless steel exhibits poor weldability due to high sensitivity to cold cracking, necessitating preheating, and heat treatment to minimize C and N content, which compromises strength and workability.
Optimizing the contents of martensite and ferrite phases in martensitic stainless steel by controlling the KAM value through EBSD, generating δ ferrite during heating before hot rolling, and heat treating within specific temperature ranges to balance yield strength and elongation.
Achieves martensitic stainless steel with a yield strength of 400 MPa and elongation of 15% or more, maintaining low cost and improved workability while ensuring a balanced strength and ductility.
Smart Images

Figure 2024146293000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to martensitic stainless steel and a method for producing martensitic stainless steel. [Background technology]
[0002] Martensitic stainless steel is a Cr-based stainless steel that has a hard martensite phase that is formed by quenching from a high-temperature austenite phase state. Its hardness is used for blades, shafts, etc. SUS410 is known as a martensitic stainless steel, and since it contains less expensive elements such as Ni and Mo and has a relatively lower Cr content than other stainless steels, it is also a relatively inexpensive stainless steel with a reasonable level of corrosion resistance (for example, Patent Documents 1 to 3). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 49-53521 [Patent Document 2] JP 2011-190521 A [Patent Document 3] JP 2001-098348 A Summary of the Invention [Problem to be solved by the invention]
[0004] In general, martensitic stainless steels have poor weldability and are not used in welded structures. The reason is that they have a high so-called low-temperature cracking sensitivity, so they need to be preheated to 300 to 400°C before welding. To avoid this and enable welding using normal procedures, it is necessary to minimize the C and N contents, as described in Patent Document 1. Furthermore, when processing general martensitic stainless steel, heat treatment at about 800°C for several tens of minutes to several hours can cause the C and N in the steel to precipitate as carbonitrides and soften the steel, but this is not possible with ultra-low C, N steel such as that described in Patent Document 1.
[0005] Therefore, the present invention aims to provide a martensitic stainless steel material that achieves the objective of improving workability (elongation) while maintaining the low cost that is an advantage of martensitic stainless steel and ensuring a certain level of strength (0.2% yield strength). [Means for solving the problem]
[0006] In order to achieve the above object, the inventors investigated conditions for improving the workability (elongation) while ensuring a certain level of strength (0.2% proof stress (hereinafter simply referred to as proof stress)) of martensitic stainless steel, and obtained the following findings.
[0007] (a) In martensitic stainless steel, it is believed that the martensite phase in the steel contributes to strength (proof stress), and the ferrite phase in the steel contributes to elongation. Therefore, the inventors conceived and proceeded with development by optimizing the contents of martensite and ferrite phases in the steel in order to obtain martensitic stainless steel with a good balance between proof stress and elongation. We investigated the evaluation of the martensite and ferrite phase contents in steel and found that it can be evaluated using the KAM (Kernel Average Misorientation) value obtained by EBSD (Electron Backscatter Diffraction). In other words, by evaluating the internal strain in the crystal grains that occurs during martensitic transformation, it becomes a comprehensive index of the balance between the martensite and ferrite phases, and it was found that there is a correlation with the yield strength and elongation. In other words, there is a strong correlation between the area fraction of the region where the KAM value is 1.0 or less and the yield strength and elongation, and as the area fraction of the KAM value of 1.0 or less increases, the yield strength decreases and the elongation increases. Therefore, it was found that there exists a range of the area fraction of the KAM value of 1.0 or less that provides a good balance between yield strength and elongation.
[0008] (b) Since having a certain amount of ferrite phase is effective in ensuring a balance between yield strength and elongation, we investigated ways to ensure the ferrite phase. As a result, we found that elongation is improved if δ ferrite remains in the heating before hot rolling. This is thought to be because the δ ferrite formed in the heating before hot rolling remains as ferrite phase even after cooling, and becomes the starting point for the martensite phase to turn into ferrite during the heat treatment described below, ensuring elongation. This led us to think of using a composition system in which δ ferrite is formed in the heating before hot rolling.
[0009] (c) In addition, the relationship between the heat treatment (annealing) temperature and elongation of martensitic stainless steel was investigated. As a result, it was found that if the heat treatment is performed at a temperature above 720°C, the martensite transforms into ferrite and becomes soft. However, this temperature range is also the Ac1 point (the temperature at which the austenite phase begins to form) of martensitic stainless steel, and if the heat treatment temperature is too high, a large amount of austenite precipitates and becomes martensite when cooled, resulting in high strength and low ductility. As a result of the investigation, it was found that the inhibition of softening can be minimized by adjusting the steel composition to set the Ac1 point between 720 and 750°C. It was also confirmed that at this time, it is possible to ensure a certain level of yield strength (400 MPa).
[0010] Based on the above findings, it was discovered that by generating δ-ferrite in the heating before hot rolling, controlling the amount of ferrite and martensite to be appropriate, and then performing heat treatment (annealing) in an appropriate temperature range in the reheating heat treatment after hot rolling, it is possible to obtain a martensitic stainless steel material with improved elongation while maintaining a certain level of strength (yield strength). The present invention was made based on these findings, and the gist of the invention is as follows.
[0011] [1] In mass%, C: 0.030% or less Si: 1.00% or less Mn: 0.50-2.00%, P: 0.050% or less, S: 0.003% or less, Cr: 10.5-12.5%, Ni: 0.30-1.50%, N: 0.0200% or less, Cu: 1.00% or less, Al: 0.050% or less C+N≦0.040%, the balance being Fe and impurities, A martensitic stainless steel material characterized in that the area ratio in the center of the cross section where the KAM (Kernel Average Misorientation) value is 1.0 or less as measured by EBSD (Electron Backscatter Diffraction) is 30 to 75%. [2] The martensitic stainless steel material further comprises, in mass %, Mo: 1.00% or less W: 0.50% or less, V: 0.30% or less, Sn: 0.100% or less, Ca: 0.0050% or less, Mg: 0.0050% or less, REM: 0.050% or less, Ti: 0.020% or less, Nb: 0.05% or less, B: 0.0050% or less, The martensitic stainless steel material according to claim 1, which contains one or more of the following: [3] The martensitic stainless steel material The formation temperature of δ ferrite is 1140°C or more and 1190°C or less, The austenite formation temperature during heating is 720°C or higher and 750°C or lower. The martensitic stainless steel material according to [1] or [2]. [4] The temperature at which the δ ferrite is generated is Tδ calculated by the following formula 1: The austenite formation temperature during heating is Ac1, which is calculated by the following formula 2. The martensitic stainless steel material according to [3]. Tδ(℃)=930C+1065N+62Ni+47Cu+22Mn-56Cr-6Si-91Mo+1723 ...Formula 1 Ac1(℃)=-50C―48N―79Ni-106Cu-79Mn+6.5Cr+15Si+21Mo+824 ...Formula 2 In the formulas 1 and 2, the element symbols indicate the content (mass%) of each element, and 0 is substituted when the element is not contained. [5] The martensitic stainless steel material according to any one of the above [1] to [4], having a 0.2% yield strength of 400 MPa or more and a fracture elongation of 15% or more. [6] A method for producing a martensitic stainless steel material according to any one of the above [1] to [5], comprising the steps of: heating a steel material containing the components according to the above [1] or [2] to a temperature between Tδ (°C) and Tδ + 50 (°C), where Tδ (°C) is the temperature at which δ ferrite is formed, and then hot working the steel material; heating the resulting steel material to a temperature within a range of 720°C to 800°C, holding the steel material within the temperature range for 5 to 30 minutes, and then cooling the steel material. [7] A method for producing a martensitic stainless steel material as described in any one of the items [1] to [5], comprising the steps of: heating a steel material containing the components as described in [3] to a temperature of Tδ (°C) or more and Tδ + 50 (°C) or less, where Tδ (°C) is the formation temperature of δ ferrite; hot working the steel material; heating the resulting steel material to a temperature in the range of 720°C or more and 800°C or less; holding the steel material within the temperature range for 5 to 30 minutes; and then cooling the steel material. [8] A method for producing a martensitic stainless steel material as described in any one of [1] to [5] above, comprising the steps of: heating a steel material containing the components as described in [4] to a temperature of Tδ (°C) or more and Tδ + 50 (°C) or less, where Tδ (°C) is the formation temperature of δ ferrite; hot working the steel material; heating the resulting steel material to a temperature in the range of 720°C or more and 800°C or less; holding the steel material within the temperature range for 5 to 30 minutes; and then cooling the steel material. [9] The method for producing a martensitic stainless steel material according to [6], wherein Tδ (°C) is calculated by the following formula 1: Tδ(℃)=930C+1065N+62Ni+47Cu+22Mn-56Cr-6Si-91Mo+1723 ...Formula 1 Here, the element symbols in formula 1 indicate the content (mass%) of each element, and 0 is substituted when the element is not contained.
[10] The method for producing a martensitic stainless steel material according to the above [7] or [8], wherein Tδ (°C) is Tδ (°C) calculated by the following formula 1: Tδ(℃)=930C+1065N+62Ni+47Cu+22Mn-56Cr-6Si-91Mo+1723 ...Formula 1 Here, the element symbols in formula 1 indicate the content (mass%) of each element, and 0 is substituted when the element is not contained. Effect of the Invention
[0012] According to the present invention, it is possible to obtain a martensitic stainless steel having a well-balanced strength and workability, that is, a strength (0.2% proof stress) of 400 MPa or more and an elongation (workability) of 15% or more. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a graph showing the relationship between the heat treatment temperature and the proof stress and elongation of 0.7%Ni-11.7Cr steel. [Diagram 2]FIG. 2 is a graph showing the relationship between the area ratio where the KAM value is 1.0 or less and the 0.2% proof stress and breaking elongation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The following description is based on one embodiment of the martensitic stainless steel material according to the present invention. The present invention is not limited to the embodiment introduced here. In this specification, one embodiment of the present invention may be simply referred to as "the present invention". In addition, the martensitic stainless steel material according to the present invention is not particularly limited in shape, such as plate, bar, wire, or tube, as long as it is made of the martensitic stainless steel described below.
[0015] [Yield strength and elongation of martensitic stainless steel] The martensitic stainless steel according to the present invention has a balance between strength and workability, with a yield strength (strength) of 400 MPa or more and an elongation (workability) of 15% or more at break. This strength property is equivalent to the strength and elongation levels of duplex stainless steel, which is recognized as a high-strength material and is widely processed.
[0016] First, the relationship between the heating temperature and elongation of martensitic stainless steel was investigated. As a result, it was thought that increasing the heat treatment temperature would decrease the yield strength and increase the elongation, but as shown in Figure 1, when the heat treatment temperature was set to a temperature several tens of degrees higher than the Ac1 point temperature (about 730°C for the steel in Figure 1), it was found that the yield strength increased and the elongation decreased. This is because when the Ac1 point is exceeded, the ferrite phase in the steel transforms into the austenite phase, and when it is cooled, it becomes martensite. It is thought that the yield strength does not increase until a temperature slightly higher than the Ac1 point due to the balance between the formation of new martensite phase and the softening of the old martensite phase. However, it was confirmed that even if the yield strength decreases under the temperature condition that causes the softest, it is possible to secure a certain yield strength (400 MPa). Therefore, it was confirmed that the desired strength characteristics can be obtained by holding at a temperature of around 750°C, slightly higher than the Ac1 point, and then cooling.
[0017] Next, assuming that the material would be heat-treated up to the Ac1 point (near 750°C), the effects of the composition on yield strength and elongation, particularly that of Cr, an important element for obtaining the corrosion resistance of stainless steel, were investigated. As a result, it was confirmed that elongation improves with an increase in Cr content, and that if Cr exceeds 10%, elongation of 15% or more can be ensured. On the other hand, it was confirmed that if Cr exceeds 12.5%, the yield strength may fall below 400 MPa. Based on these findings, it was predicted that a balance between elongation and yield strength could be achieved by designing the composition around a Cr content of 11.5%, and so the composition was tuned.
[0018] [Components of martensitic stainless steel] An example of an embodiment of the present invention will be described below. Unless otherwise specified, "%" regarding the content of an element means mass%. Furthermore, when no lower limit is specified, it includes the case where no element is contained (0%). Furthermore, when an element symbol is used in a formula, the element symbol indicates the content (mass%) of each element, and when no element is contained, 0 (%) is substituted.
[0019] C: 0.030% or less C has the effect of improving strength, but at the same time increases susceptibility to weld cracking. For this reason, it is preferable to reduce C as much as possible, to 0.030% or less. The upper limit of the C content can preferably be 0.028%, 0.026%, 0.024%, 0.022%, 0.020%, or 0.018%. On the other hand, the lower limit of the C content is not particularly limited and may not be included (0%). However, since an excessive reduction in the C content leads to an extreme increase in costs, the lower limit may be set to 0.001%, and preferably to 0.002%, 0.003%, 0.004%, or 0.005%.
[0020] Si: 1.00% or less Silicon has a deoxidizing effect during refining and is also useful for suppressing the formation of oxide scale during heat treatment, but too much silicon leads to an increase in Ac1 temperature and a decrease in toughness, so the silicon content is set to 1.00% or less. The upper limit of the silicon content is preferably 0.90%, 0.80%, 0.70%, 0.60%, 0.55%, 0.50%, 0.45%, or 0.40%. On the other hand, the lower limit of the Si content is not particularly limited and may be absent (0%). However, since Si is also a deoxidizing element in the refining process, the lower limit of the Si content may be 0.01%, and preferably may be 0.03%, 0.05%, 0.08%, 0.10%, 0.13%, 0.15%, 0.17%, or 0.18%.
[0021] Mn: 0.50-2.00% Mn has a deoxidizing effect during refining and also has the effect of lowering the Ac1 point. To reliably obtain this effect, the Mn content is set to 0.50% or more. From the viewpoint of obtaining the deoxidizing effect, the lower limit of the Mn content can be 0.55%, 0.60%, 0.65%, or 0.70%. On the other hand, since excessive Mn reduces corrosion resistance and promotes the formation of oxide scale, the Mn content is set to 2.00% or less. Taking into consideration the reduction in corrosion resistance caused by MnS and other granular substances, the upper limit of the Mn content can be 1.90%, 1.80%, 1.70%, 1.60%, or 1.50%.
[0022] P:0.050% or less P is an element contained as an impurity in the main raw materials such as molten iron and ferrochrome. Since P is an element that is the main cause of the decrease in hot ductility, it is better to reduce its content as much as possible. From this viewpoint, the P content should be 0.050% or less. Preferably, the upper limit of the P content should be 0.045%, 0.040%, 0.035%, or 0.030%. However, an excessive reduction leads to an extreme increase in costs, so the lower limit of the P content is preferably 0.001%, 0.005%, or 0.010%.
[0023] S: 0.0030% or less S is an element that forms sulfide-based inclusions and deteriorates the general corrosion resistance (general corrosion and pitting corrosion) of steel materials, and also reduces hot ductility and increases the edge cracking sensitivity of hot-rolled steel sheets, so its content is preferably as low as possible. In addition, when S and P coexist, it may particularly reduce hot ductility and increase cracking sensitivity, so S is particularly limited and the S content is set to 0.0030% or less. From these points of view, it is better to have as low an S content as possible, so its upper limit is preferably 0.0020% or 0.0010%. On the other hand, the lower the S content, the better the hot workability and corrosion resistance, but reducing S increases the desulfurization load and increases the manufacturing cost, so the lower limit of the content may be 0.0001%, and preferably 0.0003%.
[0024] Cr: 10.50~12.50% Cr provides corrosion resistance to martensitic stainless steels and increases the ferrite phase to improve workability. Therefore, the Cr content is set to 10.50% or more. The lower limit of the Cr content is preferably 10.60%, 10.70%, 10.80%, 10.90%, 11.00%, 11.10%, 11.20%, 11.30%, or 11.40%. On the other hand, if the Cr content is too high, the yield strength decreases, so the Cr content is set to 12.50% or less. The upper limit of the Cr content can preferably be 12.40, 12.30, 12.20, 12.10, or 12.00%.
[0025] Ni: 0.30~1.50% Ni not only improves toughness, but also inhibits the progression of pitting corrosion and is effective in corrosion resistance. From this viewpoint, the Ni content is set to 0.30% or more. To ensure these effects, the lower limit of the Ni content can be set to 0.35% or 0.40%. On the other hand, if it is contained in a large amount, it lowers the Ac1 point. Furthermore, from the viewpoint of alloy cost, it is preferable to have a small Ni content, so the Ni content is set to 1.50% or less. The upper limit of the Ni content can be 1.40%, 1.30%, 1.20%, 1.10%, 1.00%, 0.90%, or 0.80%.
[0026] N: 0.0200% or less N not only increases the formation temperature of δ-ferrite, but also increases weld crack susceptibility like C, so it is preferable to reduce it as much as possible, and the N content is set to 0.0200% or less. The upper limit of the N content can preferably be 0.0180%, 0.0160%, 0.0150%, 0.0140%, 0.0130%, 0.0120%, 0.0110%, or 0.0100%. On the other hand, the lower limit of the N content is not particularly limited and may not be included (0%). However, since an excessive reduction in the N content leads to an extreme increase in costs, the lower limit may be set at 0.0010%, and preferably, the value may be 0.0030% or 0.0050%.
[0027] Cu: 1.00% or less Cu may be contained since it has the effect of improving corrosion resistance and controlling the Ac1 point. However, excessive Cu content leads to a decrease in hot workability and an increase in raw material costs, so the Cu content is set to 1.00% or less. The upper limit of the Cu content can preferably be 0.90%, 0.80%, 0.70%, 0.60%, or 0.50%. Since Cu may not be contained, the lower limit of the Cu content is 0%, but since removing Cu is costly, the lower limit of the Cu content may be 0.01%, and preferably 0.10% or 0.20%.
[0028] Al: 0.050% or less Al is a deoxidizing element and improves oxidation resistance, so it may be contained. On the other hand, excessive Al content tends to form large oxide-based inclusions, impairing toughness. For this reason, the Al content is set to 0.050% or less. It can preferably be 0.040% or 0.030%. Since Al is not necessary, the lower limit of its content is 0%, but since removing Al is costly, the lower limit of the Al content may be 0.001%. Preferably, it can be 0.005% or 0.010%. Here, the Al content is the T.Al (total Al) content.
[0029] C+N≦0.040% Carbon (C) has the effect of increasing the strength of steel when combined with nitrogen (N), but it also increases susceptibility to weld cracking. In order to prevent weld cracking even without preheating, the total amount of C and N (C+N) is limited to 0.040% or less. The upper limit of the total amount of C and N (C+N) can preferably be 0.039%, 0.038%, 0.037%, 0.036%, 0.035%, 0.034%, 0.033%, 0.032%, 0.031%, 0.030%, 0.029%, 0.028%, 0.027%, 0.026%, or 0.025%.
[0030] In one embodiment of the present invention, the balance is Fe and impurities in addition to the above elements. Here, the impurities refer to elements that are inevitably and unintentionally mixed in raw materials such as ores and scraps during the industrial production of steel, and are permissible within a range that does not adversely affect the present invention.
[0031] Furthermore, in addition to these elements, the stainless steel of this embodiment may contain one or more of Mo, W, V, Sn, Ca, and REM in place of a portion of Fe. These elements do not have to be contained, but by containing them, further effects can be obtained. These elements will be described below.
[0032] Mo: 1.000% or less Mo may be added because it is effective in improving the corrosion resistance of martensite structures containing δ-ferrite. However, Mo is a stabilizing element for the ferrite phase, and excessive addition of Mo increases the amount of ferrite phase in the HAZ, as with Cr. Furthermore, Mo is an expensive element, so the Mo content is set to 1.000% or less. The upper limit of the Mo content can preferably be 0.900%, 0.800%, 0.700%, 0.600%, 0.500%, 0.450%, 0.400%, 0.350%, 0.300%, 0.250%, 0.200%, 0.150%, or 0.100%. The lower limit of the Mo content is not particularly limited, but since removing Mo is costly, the lower limit may preferably be 0.005% or 0.010%.
[0033] W: 0.50% or less W, like Mo, is an element that improves the corrosion resistance of stainless steel and may be contained. However, since it is an expensive element, it is preferable to keep the content at 0.50% or less, and preferably at 0.40% or less or 0.30% or less. When W is contained, it is preferable to contain 0.01% or more in order to obtain the effect more reliably, preferably 0.05% or more, and more preferably 0.10% or more.
[0034] V: 0.30% or less V may be contained since it forms fine carbonitrides and is effective in improving the wear resistance as well as the corrosion resistance. However, excessive V content may cause the precipitates to become coarse, resulting in a decrease in toughness, so the upper limit of the V content is 0.30%, preferably 0.20% or 0.10%. The lower limit of the V content is not particularly limited, but considering the production cost and manufacturability, it is preferably 0.01%, 0.03%, 0.05%, or 0.07%.
[0035] Sn: 0.100% or less Sn is an effective element for improving corrosion resistance, but excessive addition promotes edge cracking during hot rolling. Therefore, the upper limit of the Sn content is 0.100%, preferably 0.090%, 0.080%, 0.070%, 0.060%, or 0.050%. The lower limit of the Sn content is not particularly limited, but from the viewpoint of reliably obtaining the effect, it is preferably 0.001%, preferably 0.002%, 0.005%, 0.010%, 0.015%, or 0.020%.
[0036] Ca:0.0050% or less Mg: 0.0050% or less Ca and Mg may be added to adjust the composition at the steelmaking stage, and may be included since they act as strong deoxidizers, promoting deoxidation and improving hot ductility. However, there is a concern that they may reduce corrosion resistance, so the Ca and Mg contents are set to 0.0050% or less. The upper limits of the Ca and Mg contents can preferably be 0.0030% and 0.0020%, respectively. There is no particular lower limit for the Ca or Mg content, but from the standpoint of ensuring the desired effect, the lower limit should be 0.0001%, preferably 0.0002%, 0.0003%, 0.0004%, or 0.0005%, respectively.
[0037] REM: 0.050% or less The inclusion of an appropriate amount of REM can significantly improve hot ductility, similar to the inclusion of Ca. To obtain this effect, the lower limit of the REM content should be set to 0.001%, 0.002%, 0.003%, 0.004%, or 0.005%. On the other hand, excessive addition of REM is undesirable because it tends to form large REM oxides, which can cause nozzle clogging during casting. The upper limit of the REM content should be set at 0.050% or 0.030%. REM is usually added in the form of a complex misch metal, but the addition of single elements such as La, Ce, Pr, and Nd also has the same effect. Here, REM (rare earth elements) refers to the two elements scandium (Sc) and yttrium (Y) and the 15 elements (lanthanoids) from lanthanum (La) to lutetium (Lu), as generally defined. These REM elements may be contained alone or in combination. If multiple REM elements are contained, the total amount should be within the above lower and upper limits.
[0038] Ti: 0.020% or less Nb: 0.05% or less B: 0.0050% or less Ti and Nb have the effect of improving corrosion resistance, and B has the effect of improving hot ductility, so Ti: 0.020% or less, Nb: 0.05% or less, and B: 0.0050% or less may be contained. Although it is not necessary to contain each of the elements Ti, Nb, and B, there is no need to remove them excessively. Therefore, the lower limit of the content of each of these elements is not particularly limited, but it may be Ti: 0.001%, Nb: 0.01%, and B: 0.0001%.
[0039] It is also preferable to reduce the amount of Zn, Pb, Bi, Se, Sb, Ga, Ta, Mg, Zr, etc. as much as possible. On the other hand, these elements may contain one or more of the following amounts as necessary to solve the problems of the present invention: Zn: 50 ppm or less, Pb: 10 ppm or less, Bi: 30 ppm or less, Se: 100 ppm or less, Sb: 100 ppm or less, Ga: 50 ppm or less, Ta: 500 ppm or less, Mg: 100 ppm or less, and Zr: 120 ppm or less.
[0040] [Area ratio with KAM value ≦ 1.0] The KAM (Kernel Average Misorientation) value is an index that can be measured by EBSD (Electron Backscatter Diffraction) and is obtained from the average value of the misorientation between a measurement point of interest in an image obtained by EBSD and adjacent measurement points. The KAM value represents the plastic strain gradient in a micro-region, and can evaluate damage to the ferrite matrix and strain distribution within crystal grains. The inventors therefore considered that the KAM value could be an index that represents the strain distribution within crystal grains that occurs during martensitic transformation. Thus, they investigated the relationship between the area ratio of the region in which the KAM value is 1.0 or less (region considered to have little strain) in martensitic stainless steel and the yield strength and fracture elongation, and found that there is a very good correlation. Thus, they found that the area ratio of the region in which the KAM value is 1.0 or less can be used as a comprehensive index from the viewpoint of the structure of martensitic stainless steel.
[0041] FIG. 2 shows the relationship between the KAM value and the yield strength and the elongation at break in the examples. As is clear from FIG. 2, as the KAM value increases, the yield strength decreases and the elongation at break increases. This means that the area ratio of the KAM value of 1.0 or less increases, which is thought to mean that the martensite region decreases and the ferrite phase region increases. In other words, it is thought to mean that the smaller the area ratio of KAM≦1.0, the more the martensite region, and the larger the area ratio of KAM≦1.0, the more the ferrite phase region. From FIG. 2, if the area ratio of KAM≦1.0 is 30% or more, the elongation is 15%. Preferably, the area ratio of KAM≦1.0 is 35% or more, or 40% or more. On the other hand, it can be seen that if the area ratio of KAM≦1.0 is 75% or less, the yield strength can be secured to 400MPa or more. Preferably, the area ratio of KAM≦1.0 is 70% or less, 65% or less, or 60% or less.
[0042] [Tδ(℃): δ ferrite formation temperature] From the viewpoint of securing a certain amount of ferrite phase, it is preferable to use a composition system in which δ ferrite is generated in heating before hot rolling. Usually, the heating temperature before hot rolling of martensitic stainless steel is about 1160°C to 1220°C, so it is preferable that the δ ferrite generation temperature (Tδ(°C)) is about 20°C lower than the heating temperature before hot rolling. That is, it is preferable that the δ ferrite generation temperature (Tδ(°C)) is 1140°C to 1200°C. If the δ ferrite generation temperature (Tδ(°C)) is too low, the ferrite phase region will eventually become excessive, leading to a decrease in yield strength and a decrease in hot ductility. Therefore, it is preferable that the δ ferrite generation temperature (Tδ(°C)) is 1140°C or higher, and further 1150°C or higher. On the other hand, if the δ ferrite generation temperature (Tδ(°C)) is too high, δ ferrite will not be generated, leading to a decrease in elongation. Therefore, the δ-ferrite formation temperature (Tδ(° C.)) is preferably 1200° C. or lower, further preferably 1190° C. or lower, 1180° C. or lower, or 1170° C. or lower.
[0043] The delta ferrite formation temperature (T delta (°C)) varies depending on the components of the martensitic stainless steel, and can be determined by actual measurement for each steel. It is preferable that the delta ferrite formation temperature determined by actual measurement is within the above temperature range. The δ-ferrite formation temperature can also be estimated from the contents of each component using the following formula 1. The δ-ferrite formation temperature (Tδ (° C.)) calculated from formula 1 may be set to fall within the above temperature range. Tδ(℃)=930C+1065N+62Ni+47Cu+22Mn-56Cr-6Si-91Mo+1723 ...Formula 1 In the formula 1, the element symbols indicate the content (mass%) of each element, and 0 is substituted if the element is not contained.
[0044] [Ac1 (℃): Austenite formation temperature when heated] From the viewpoint of improving elongation, as shown in FIG. 1, it was confirmed that the improvement of elongation reaches its peak when the material is heated to about 750°C, which is a temperature slightly higher than the Ac1 point temperature (about 730°C), and then heat-treated (annealed). On the other hand, it was confirmed that, although the yield strength decreases when the material is heated to the vicinity of the Ac1 point due to softening, it is possible to secure a certain yield strength (400MPa). Here, if the austenite formation temperature (Ac1 (°C)) during heating of martensitic stainless steel is too low, the martensite phase is formed at a heat treatment temperature of about 750°C, which is a temperature at which the strength reduction effect can be exerted, and the ferrite phase cannot be secured after cooling, so the elongation does not improve. On the other hand, if the austenite formation temperature (Ac1 (°C)) during heating is too high, the martensite formation does not progress due to the temperature retention after heat treatment, and as a result, the ferrite phase becomes excessive and the yield strength decreases. Therefore, it is preferable that the austenite formation temperature (Ac1 (°C)) during heating is 720°C or higher and 750°C or lower.
[0045] The austenite formation temperature during heating varies depending on the components of the martensitic stainless steel, and can be determined by actual measurement for each steel. It is preferable that the austenite formation temperature during heating determined by actual measurement is within the above temperature range. The austenite formation temperature during heating can also be estimated from the content of each component using the following formula 2. The austenite formation temperature during heating (Ac1 (° C.)) calculated using formula 2 may be set to fall within the above temperature range. Ac1(℃)=-50C―48N―79Ni-106Cu-79Mn+6.5Cr+15Si+21Mo+824 ...Formula 2 In the formula 2, the element symbols indicate the content (mass%) of each element, and 0 is substituted if the element is not contained.
[0046] [Manufacturing method] An embodiment of the method for producing a martensitic stainless steel according to the present invention will be described below. The method for producing a martensitic stainless steel according to the present invention is not limited to this embodiment. First, a slab having the above-described composition is produced. A conventional slab production method can be used for producing the slab. Generally, slabs can be obtained by subjecting molten steel, whose composition has been adjusted in an electric furnace or the like, to a continuous casting method or the like. Next, the obtained steel slab is heated and hot worked. At this time, when heating before hot working (heating before hot rolling), the steel slab should be heated so that its temperature is higher than the δ ferrite formation temperature (Tδ (°C)) explained above, preferably 10°C or more higher, more preferably 20°C or more higher than the δ ferrite formation temperature (Tδ (°C)). This forms δ ferrite in the steel slab, which remains as a ferrite phase even after cooling, and can contribute to improving the elongation of martensitic stainless steel.
[0047] Next, the heated steel slab is hot worked. The hot working method is not particularly limited. Conventional hot working methods, such as hot rolling and hot forging, can be applied. After the hot working, the steel is heat treated by holding at a temperature of 720°C or more and 800°C or less for 5 to 30 minutes. At temperatures below 720°C and for less than 5 minutes, the strength reduction effect due to the heat treatment is low, and at temperatures above 800°C, in the case of the composition system of the present invention, a new martensite phase is generated and the strength increases. There is no particular upper limit to the heat treatment time, but at 30 minutes or more, the improvement effect is saturated and the heat treatment time is not shortened. The lower limit of the heat treatment temperature is preferably 730°C or 740°C, and the upper limit is more preferably Ac1 point + 50°C or less, or 780°C or 770°C. This can improve the elongation of the martensitic stainless steel obtained after cooling.
[0048] For example, if the hot working is hot rolling, the material is heated to a temperature higher than the δ ferrite formation temperature (Tδ (℃)) before hot rolling, and then hot rolled and cooled according to the usual method. After that, it is recommended to heat the material to a temperature of 720℃ to 800℃, hold the material in that temperature range for 5 to 30 minutes, and then cool it.
[0049] [0.2% yield strength ≧ 400MPa, breaking elongation ≧ 15%] The martensitic stainless steel thus obtained can ensure a yield strength (0.2% yield strength) of 400 MPa or more and an elongation (elongation at break) of 15% or more. EXAMPLES
[0050] Examples of the present invention will be described below. Note that the present invention is not limited to the conditions used in the following examples. Steel with the composition shown in Table 1 was melted in an MgO crucible in a 50 kg vacuum induction furnace in the laboratory and cast into a flat slab (steel billet) with a thickness of approximately 100 mm. A hot rolling material was processed from the main part of the slab, heated to the slab heating temperature shown in Table 2, held for 1 to 2 hours, and hot rolled into a hot-rolled steel plate with a thickness of 15 mm. It was then heated to the heat treatment temperature shown in Table 2, held for 30 minutes, and water-cooled. From the steel plate thus obtained, multiple strip-shaped steel test pieces (at least 4 pieces) with a length of 200 mm and a width of 100 mm were prepared.
[0051] A KAM map was obtained by EBSD using one of the thickness direction cross sections of the test material as the observation surface, and the area ratio of the area with a KAM value of 1.0 or less was measured. The observation surface was measured in three arbitrary 0.1 mm2 areas in the center of the cross section of the test piece, and the area ratios obtained were arithmetically averaged to obtain the area ratio for the test piece. Since the surface of the steel plate is affected by processing such as rolling, it is desirable to select a part at least 0.1 mm (100 μm) away from the surface or edge of the steel plate. There is no particular limit to the measurement area, but it is desirable to have at least 0.1 mm2 or more, and the total observation area is desirable to be 0.3 mm2 or more. The area ratio of the area with a KAM value of 1·0 or less from the obtained KAM map can be obtained using the software attached to EBSD. When measurements are made at multiple locations, the measured values at each location can be arithmetically averaged, and the average value can be used as the area ratio of the steel material with a KAM value of 1.0 or less. The area ratios of the measured KAM values of 1.0 or less are shown in Table 2. A tensile test was performed in accordance with JIS on one of the obtained test pieces to determine the 0.2% yield strength and breaking elongation. The obtained 0.2% yield strength and breaking elongation are shown in Table 2. As mentioned above, the relationship between the area ratio of the region with a KAM value of 1·0 or less and the 0.2% yield strength and breaking elongation is shown in Figure 2.
[0052] In addition, other properties of martensitic stainless steel were evaluated, including hot workability, toughness, corrosion resistance, and weld cracking. For hot workability, specimens that did not have edge cracks at the width end during hot rolling were deemed to have passed. For toughness, a Charpy impact test (-20°C absorbed energy) was performed on one of the obtained test pieces in accordance with JIS Z 2242:2018, and specimens that had an absorbed energy value of 80J or more were deemed to have passed. For corrosion resistance, samples taken from the steel surface and polished to #600 were subjected to pitting potential measurement in accordance with JIS G 0577, and specimens that had an average value of 0VvsAg / AgCl or more were deemed to have passed. In Table 2, specimens that passed each evaluation are marked with "○" and those that failed are marked with "×".
[0053] As can be seen from Tables 1 and 2, it was confirmed that by satisfying the conditions stipulated in the present invention, a martensitic stainless steel having a good balance between 0.2% yield strength and fracture elongation can be obtained.
[0054] [Table 1]
[0055] [Table 2] [Industrial Applicability]
[0056] The present invention can be used not only in the steel industry that produces stainless steel, but also in a wide range of industries that use martensitic stainless steel materials, such as the civil engineering and construction industry related to social infrastructure such as general buildings and bridges, the chemical industry, the machinery industry, and the automobile industry.
Claims
1. In mass percent, C: 0.030% or less Si: 1.00% or less Mn: 0.50-2.00%, P: 0.050% or less, S: 0.003% or less, Cr: 10.5-12.5%, Ni: 0.30 to 1.50%, N: 0.0200% or less, Cu: 1.00% or less, Al: 0.050% or less; C+N≦0.040%, The balance is Fe and impurities, A martensitic stainless steel material characterized in that the area ratio in which the KAM (Kernel Average Misorientation) value measured by EBSD (Electron Backscatter Diffraction) at the center of the cross section is 1.0 or less is 30 to 75%.
2. The martensitic stainless steel material further comprises, in mass %, Mo: 1.00% or less, W: 0.50% or less, V: 0.30% or less, Sn: 0.100% or less, Ca: 0.0050% or less, Mg: 0.0050% or less, REM: 0.050% or less, Ti: 0.020% or less, Nb: 0.05% or less, B: 0.0050% or less, 2. The martensitic stainless steel material according to claim 1, further comprising one or more of the following:
3. The martensitic stainless steel material The formation temperature of δ ferrite is 1140° C. or more and 1190° C. or less, The austenite formation temperature during heating is 720°C or higher and 750°C or lower. The martensitic stainless steel material according to claim 1 or 2.
4. The formation temperature of the δ ferrite is Tδ calculated by the following formula 1, The austenite formation temperature during heating is Ac1, which is calculated by the following formula 2: The martensitic stainless steel material according to claim 3. Tδ (℃)=930C+1065N+62Ni+47Cu+22Mn-56Cr-6Si-91Mo+1723 ...Formula 1 Ac1 (℃) = -50C-48N-79Ni-106Cu-79Mn+6.5Cr+15Si+21Mo+824 ...Formula 2 In the formulas 1 and 2, the element symbols indicate the content (mass%) of each element, and 0 is substituted when the element is not contained.
5. 3. The martensitic stainless steel material according to claim 1 or 2, having a 0.2% yield strength of 400 MPa or more and a fracture elongation of 15% or more.
6. A method for producing a martensitic stainless steel material according to claim 1 or 2, comprising the steps of: heating a steel material containing the components according to claim 1 or 2 to a temperature of Tδ (°C) or more and Tδ + 50 (°C) or less, where Tδ (°C) is the formation temperature of δ ferrite, and then hot working the steel material; heating the resulting steel material to a temperature in the range of 720°C or more and 800°C or less, holding the steel material within the temperature range for 5 to 30 minutes, and then cooling the steel material.
7. A method for producing a martensitic stainless steel material as described in claim 3, characterized in that a steel material containing the components as described in claim 3 is heated to a temperature of Tδ (°C) or more and Tδ + 50 (°C) or less, where Tδ (°C) is the formation temperature of δ ferrite, and then hot worked, and the resulting steel material is heated to a temperature in the range of 720°C or more and 800°C or less, held within the temperature range for 5 to 30 minutes, and then cooled.
8. A method for producing a martensitic stainless steel material as described in claim 4, characterized in that a steel material containing the components as described in claim 4 is heated to a temperature of Tδ (°C) or more and Tδ + 50 (°C) or less, where Tδ (°C) is the formation temperature of δ ferrite, and then hot worked, and the resulting steel material is heated to a temperature in the range of 720°C or more and 800°C or less, held within the temperature range for 5 to 30 minutes, and then cooled.
9. The method for producing a martensitic stainless steel material according to claim 6, wherein the Tδ (°C) is calculated by the following formula 1: Tδ (℃)=930C+1065N+62Ni+47Cu+22Mn-56Cr-6Si-91Mo+1723 ...Formula 1 Here, the element symbols in formula 1 indicate the content (mass%) of each element, and 0 is substituted when the element is not contained.
10. The method for producing a martensitic stainless steel material according to claim 7, wherein the Tδ (°C) is calculated by the following formula 1: Tδ (℃)=930C+1065N+62Ni+47Cu+22Mn-56Cr-6Si-91Mo+1723 ...Formula 1 Here, the element symbols in formula 1 indicate the content (mass%) of each element, and 0 is substituted when the element is not contained.
11. The method for producing a martensitic stainless steel material according to claim 8, wherein the Tδ (°C) is calculated by the following formula 1: Tδ (℃)=930C+1065N+62Ni+47Cu+22Mn-56Cr-6Si-91Mo+1723 ...Formula 1 Here, the element symbols in formula 1 indicate the content (mass%) of each element, and 0 is substituted when the element is not contained.
Citation Information
Patent Citations
JP1974053521A
High strength martensitic stainless steel oil well pipe
JP2001098348A
Martensitic stainless steel with excellent weld characteristics, and mertensitic stainless steel material
JP2011190521A