Wiring board and method for manufacturing wiring board
By positioning the via's minimum diameter away from the bottom and applying controlled laser and desmear processes, the stress-induced reliability issues in multilayer wiring boards are mitigated, enhancing the board's durability.
Patent Information
- Application Number
- JP2023059131
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
The difference in thermal expansion coefficients between the dielectric layer and electrodes in capacitors within multilayer wiring boards leads to stress strain, affecting the reliability of vias and reducing the overall board reliability.
The via is designed with a minimum diameter portion located away from the via bottom portion, and specific ratios and dimensions are maintained to minimize stress concentration, with controlled laser processing and desmear treatments to enhance via integrity.
This design effectively reduces stress concentration at the via bottom portion, preventing conductor breakage and improving the reliability of the wiring board under thermal stress.
Smart Images

Figure 2024146315000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a wiring board having a capacitor and to a method of manufacturing the wiring board. [Background technology]
[0002] In recent years, multilayer wiring boards using glass materials as a core substrate are often used as interposers. In multilayer wiring boards, a capacitor with a MIM (Metal-Insulator-Metal) structure in which a dielectric layer is sandwiched between a lower electrode and an upper electrode may be formed inside the board as part of a passive circuit. The lower electrode, dielectric layer, and upper electrode are each composed of a first conductive layer, an insulating layer, and a second conductive layer, respectively. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2019 / 244382 Summary of the Invention [Problem to be solved by the invention]
[0004] In the above-mentioned capacitor, stress distortion may occur due to the difference in thermal expansion coefficient between the dielectric layer and each electrode. This stress distortion also affects the vias arranged on the capacitor, and becomes a factor in reducing the reliability of the wiring board.
[0005] An object of the present invention is to provide a technique for improving the reliability of a wiring board having a capacitor. [Means for solving the problem]
[0006] According to one aspect of the present invention, there is provided a wiring board having a capacitor including a lower electrode, a dielectric layer arranged above the lower electrode, and an upper electrode arranged above the dielectric layer, and a via whose via bottom portion is arranged on the upper electrode, wherein the via is formed such that a smallest part of the via diameter is located at a position away from the via bottom portion.
[0007] According to another aspect of the present invention, there is provided a wiring board, in which the via is formed such that, when the height from the via bottom to the via top is H and the height from the via bottom to the part of the via with the smallest diameter is h1, "h1 / H" is within the range of 0.03 to 0.6.
[0008] According to yet another aspect of the present invention, there is provided a wiring board, wherein the via is formed such that, when the diameter of the via bottom portion is db and the diameter of the smallest portion of the via diameter is d0, "db / d0" is within the range of 1.05 to 2.0.
[0009] According to yet another aspect of the present invention, there is provided a wiring board, in which the capacitor is formed on a substrate made of a glass material.
[0010] According to yet another aspect of the present invention, there is provided a wiring board, wherein the via is a filled via.
[0011] According to another aspect of the present invention, there is provided a method for manufacturing a wiring board, which manufactures a wiring board having a capacitor including a lower electrode, a dielectric layer arranged above the lower electrode, and an upper electrode arranged above the dielectric layer, and a via whose via bottom portion is arranged on the capacitor, the method including the steps of: forming an insulating resin layer on a conductive layer that becomes the upper electrode; and forming a via hole by drilling a through hole in a region of the insulating resin layer where the via is to be formed, wherein the step of forming the via hole includes forming the via hole such that a portion of the via with a minimum diameter is located away from the via bottom portion.
[0012] According to another aspect of the present invention, there is provided a method for manufacturing a wiring board, in which the step of forming the via hole includes a laser treatment for processing the through hole by irradiating the through hole with laser light, and a desmear treatment for removing a residue of an insulating resin generated by the laser treatment, and the laser treatment and the desmear treatment process the through hole such that a via diameter at a via bottom portion is larger than a portion of the via with a minimum via diameter.
[0013] According to yet another aspect of the present invention, there is provided a method for manufacturing a wiring board, in which laser processing conditions are adjusted in the laser processing so that an opening on the via bottom side is larger than an opening at a part of the via where the via diameter is smallest. Effect of the Invention
[0014] According to the present invention, a technique for improving the reliability of a wiring board having a capacitor is provided. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a wiring board according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing a part of a manufacturing process for the wiring board according to the embodiment of the present invention. [Diagram 3] FIG. 3 is a cross-sectional view showing a part of a manufacturing process for the wiring board according to the embodiment of the present invention. [Figure 4] FIG. 4 is a cross-sectional view showing a part of a manufacturing process for a wiring board according to an embodiment of the present invention. [Diagram 5] FIG. 5 is a cross-sectional view showing a part of a manufacturing process for a wiring board according to an embodiment of the present invention. [Figure 6] FIG. 6 is a cross-sectional view showing a part of a manufacturing process for a wiring board according to an embodiment of the present invention. [Figure 7] FIG. 7 is a cross-sectional view showing a part of a manufacturing process for a wiring board according to an embodiment of the present invention. [Figure 8] FIG. 8 is a cross-sectional view showing a part of a manufacturing process for a wiring board according to an embodiment of the present invention. [Figure 9] FIG. 9 is a cross-sectional view showing a part of a manufacturing process for a wiring board according to an embodiment of the present invention. [Figure 10] FIG. 10 is a cross-sectional view showing a part of a manufacturing process for a wiring board according to an embodiment of the present invention. [Figure 11] FIG. 11 is a cross-sectional view showing a part of a manufacturing process for a wiring board according to an embodiment of the present invention. [Figure 12] FIG. 12 is a cross-sectional view showing a part of a manufacturing process for a wiring board according to an embodiment of the present invention. [Figure 13] FIG. 13 is a cross-sectional view showing a part of a manufacturing process for a wiring board according to an embodiment of the present invention. [Figure 14] FIG. 14 is a cross-sectional view that diagrammatically illustrates a cross-sectional shape in the vicinity of the via 15 shown in FIG. [Figure 15] FIG. 15 is a cross-sectional view showing the cross-sectional shape of the vicinity of a via 15' in a portion other than the capacitor 10 in the wiring in the same layer as that shown in FIG. 12. In FIG. [Figure 16] FIG. 16 is a cross-sectional view showing the cross-sectional shape of the via hole 15H after the laser treatment and the cross-sectional shape of the via hole 15H after the desmear treatment in comparison with a conventional example, examples 1 and 2 of this embodiment. [Figure 17] FIG. 17 is a cross-sectional view showing various configurations of via cross-sectional shapes according to embodiments of the present invention. [Figure 18] FIG. 18 is a cross-sectional view showing various forms of cross-sectional shapes of vias according to the prior art. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, embodiments of the present invention will be described with reference to the drawings. The embodiments described below are more specific embodiments of any of the above aspects. The following items can be incorporated into each of the above aspects alone or in combination.
[0017] The embodiments described below are merely examples of configurations for embodying the technical idea of the present invention, and the technical idea of the present invention is not limited by the materials, shapes, structures, etc. of the components described below. Various modifications can be made to the technical idea of the present invention within the technical scope defined by the claims.
[0018] In addition, elements having the same or similar functions are given the same reference numerals in the drawings referred to below, and duplicated explanations are omitted. In addition, the drawings are schematic, and the relationship between dimensions in one direction and dimensions in another direction, the relationship between the dimensions of one member and the dimensions of another member, etc. may differ from the actual ones.
[0019] In the following, the terms "upper" and "lower" are used to indicate positions in the thickness direction of a layer, and correspond to the upper side (positive direction of the Z axis) and the lower side (negative direction of the Z axis) in a cross-sectional view, respectively. The terms "upper surface" and "lower surface" mean the upper and lower main surfaces, respectively, of the two main surfaces of a layer whose cross section is drawn so that the thickness direction is the vertical direction. The term "horizontal direction" means a direction perpendicular to the Z axis in a cross-sectional view (e.g., the positive or negative direction of the X axis, the positive or negative direction of the Y axis, etc.). The term "planar view" means the shape of a surface or layer when viewed from above, that is, from the positive direction to the negative direction of the Z axis.
[0020] <1> Basic structure First, with reference to FIG. 1, a basic structure of a wiring board according to an embodiment of the present invention will be described.
[0021] FIG. 1 is a cross-sectional view showing an example of a wiring board according to an embodiment of the present invention.
[0022] The wiring board 100 shown in Fig. 1 is a multilayer wiring board, and is a glass core wiring board including a glass substrate as a core substrate. The wiring board 100 is connected to, for example, a printed wiring board or a silicon chip (not shown). In the example of Fig. 1, the wiring board 1 is a wiring board used as an interposer, that is, a glass interposer.
[0023] As shown in FIG. 1, wiring board 100 has a substrate 1 having an insulating surface, an adhesion layer 2 arranged on substrate 1, a first seed layer 3 arranged on adhesion layer 2 (above substrate 1), a first conductive layer 4 arranged on first seed layer 3, a lower adhesion layer 5 arranged on first conductive layer 4, an insulating layer 6 arranged on lower adhesion layer 5 (above first conductive layer 4), an upper adhesion layer 7 arranged on insulating layer 6, a second seed layer 8 arranged on upper adhesion layer 7 (above insulating layer 6), a second conductive layer 9 arranged on second seed layer 8, an insulating resin layer 12 that protects the conductive layers, and a third seed layer 13 and a third conductive layer 14 arranged above second conductive layer 9.
[0024] In such a wiring board 100, the first conductive layer 4 becomes a lower electrode in the MIM structure, the insulating layer 6 becomes a dielectric layer in the MIM structure, and the second conductive layer 9 becomes an upper electrode in the MIM structure, and at least these constitute a capacitor with an MIM structure (MIM capacitor) 10.
[0025] In addition, on the capacitor 10, there is a via 15 that leads to the third conductive layer 14. The via 15 is formed as a filled via. The via 15 provides electrical continuity between the second conductive layer 9 and the third conductive layer 14 in the capacitor 10.
[0026] <2> Explanation of each element Hereinafter, the materials, shapes, etc. of each element constituting wiring board 100 will be described in detail.
[0027] <2.1> Substrate It is desirable to use transparent glass having optical transparency as the material for the substrate 1. By using glass with a thickness and linear expansion coefficient within a certain range, it is possible to improve the ease of the process for forming the through holes in the substrate 1, the handling properties during manufacturing, and the stability when stress and strain occur.
[0028] There are no particular limitations on the glass material, components, or blending ratio of each component contained in the glass, or the method for producing the glass.
[0029] For example, the glass material may be non-alkali glass, alkali glass, borosilicate glass, quartz glass, sapphire glass, photosensitive glass, etc., but any glass material containing silicate as a main component may be used. Furthermore, other so-called glass materials may be used. However, when a semiconductor is mounted on the substrate 1 of this embodiment, it is preferable to use non-alkali glass.
[0030] Examples of the glass manufacturing method include a float method, a down-draw method, a fusion method, an up-draw method, and a roll-out method, and any of these methods may be used.
[0031] The thickness of the substrate 1 is preferably 1 mm or less, but taking into consideration the ease of the process for forming through holes in the glass and handling during production, the thickness is more preferably 0.1 mm or more and 0.8 mm or less.
[0032] The linear expansion coefficient of the glass is preferably -1 ppm / K or more and 15.0 ppm / K or less. The reason is that if it is -1 ppm / K or less, it is difficult to select the glass material itself and it cannot be manufactured at low cost, while if it is 15.0 ppm / K or more, the difference in thermal expansion coefficient with other layers is large and reliability is reduced. In addition, when a silicon chip is mounted on the substrate 1, the connection reliability with the silicon chip is reduced. The linear expansion coefficient of the glass is more preferably 0.5 ppm / K or more and 8.0 ppm / K or less, and even more preferably 1.0 ppm / K or more and 4.0 ppm / K or less.
[0033] The substrate 1 may have a functional film such as an anti-reflection film or an IR cut filter formed thereon in advance. In addition, the substrate may have functions such as strength imparting, anti-static, coloring, and texture control. Examples of such functional films include, but are not limited to, a hard coat film for strength imparting, an anti-static film for anti-static imparting, an optical filter film for coloring, and an anti-glare or light scattering film for texture control. Film formation techniques such as vapor deposition, sputtering, and wet methods are used to form these functional films.
[0034] <2.2> First seed layer The first seed layer 3 has a copper layer or other metal layer (seed metal layer). The seed metal layer acts as a power supply layer for electrolytic plating in the formation of wiring in the semi-additive process. The first seed layer 3 is formed by, for example, a sputtering method or a CVD method, and is made of, for example, Cu, Ni, Al, Ti, Cr, Mo, W, Ta, Au, Ir, Ru, Pd, Pt, AlSi, AlSiCu, AlCu, NiFe, ITO, IZO, AZO, ZnO, PZT, TiN, Cu3N4, or a Cu alloy alone or in combination. An electroless plating layer (a layer such as electroless copper plating or electroless nickel plating) may be formed above the first seed layer 3.
[0035] <2.3> Adhesion layer Before forming a seed layer above the substrate 1 or the insulating layer 6, it is desirable to form an adhesion layer of titanium deposited by a sputtering method on the lower surface or upper surface of the substrate 1 or the insulating layer 6, taking into consideration electrical properties, ease of manufacture, and cost. In this embodiment, the adhesion layers include the adhesion layer 2 formed on the upper surface of the substrate 1, the lower adhesion layer 5 formed on the lower surface of the insulating layer 6, and the upper adhesion layer 7 formed on the upper surface of the insulating layer 6. The adhesion layer 2 has a function of improving adhesion between the substrate 1 and the first seed layer 3, the lower adhesion layer 5 has a function of improving adhesion between the first conductive layer 4 and the insulating layer 6, and the upper adhesion layer 7 has a function of improving adhesion between the insulating layer 6 and the second seed layer 8.
[0036] The material of the lower adhesion layer 5 and the upper adhesion layer 7 is, for example, Ti. Other than this, for example, Cu, Ni, Al, Cr, Mo, W, Ta, Au, Ir, Ru, Pd, Pt, AlSi, AlSiCu, AlCu, NiFe, Cu alloys alone or in combination may be used. Ti is excellent in terms of adhesion, electrical conductivity, ease of manufacture, and cost.
[0037] The thickness of the lower adhesion layer 5 and the upper adhesion layer 7 is preferably, for example, 10 nm or more and 1 μm or less. If it is less than 10 nm, there is a risk that the adhesion strength will be insufficient. If it exceeds 1 μm, not only will the film formation time be too long in the manufacturing process described below, resulting in a lack of mass productivity, but the process of removing unnecessary parts may take even more time. The thickness of the lower adhesion layer 5 and the upper adhesion layer 7 is more preferably 10 nm or more and 500 nm or less.
[0038] The lower adhesion layer 5 and the upper adhesion layer 7 may have different thicknesses, but it is preferable that they have the same thickness in order to simplify the structure. If the adhesion between the first conductive layer 4 and the insulating layer 6 is sufficient, the lower adhesion layer 5 may be omitted. If the adhesion between the insulating layer 6 and the second seed layer 8 is sufficient, the upper adhesion layer 7 may be omitted.
[0039] <2.4> Wiring The adhesion layer 2, the first seed layer 3, and the first conductive layer 4 formed on the substrate 1 can be used as wiring for forming a circuit in the region on the substrate 1 other than where the capacitor 10 is formed. For example, the adhesion layer 2 is made of titanium, and the first seed layer 3 is made of copper. To be used as wiring for forming a circuit, the total thickness of titanium and copper is desirably 5 μm or less, which is advantageous for forming fine wiring by the semi-additive method. If it is thicker than 5 μm, it is difficult to form fine wiring with a pitch of 30 μm or less.
[0040] Considering that the first conductive layer 4 will be used as wiring for forming a circuit in addition to being the lower electrode of the capacitor 10, it is preferable that the first conductive layer 4 be electrolytic copper plating, which is simple, inexpensive, and has good electrical conductivity. However, in addition to electrolytic copper plating, electrolytic nickel plating, electrolytic chromium plating, electrolytic Pd plating, electrolytic gold plating, electrolytic rhodium plating, electrolytic iridium plating, etc. may also be used.
[0041] <2.5> Insulating layer Insulating layer 6, which becomes the dielectric layer of capacitor 10, can be selected from alumina, silica, silicon nitride, tantalum oxide, titanium oxide, calcium titanate, barium titanate, and strontium titanate in terms of insulation properties and relative dielectric constant.
[0042] The thickness of the insulating layer 6 is preferably 10 nm or more and 5 μm or less. If the thickness of the insulating layer 6 is 10 nm or less, the insulating properties cannot be maintained and the function of the capacitor 10 is not exhibited. If the thickness of the insulating layer 6 is 5 μm or more, not only is it difficult to mass-produce the insulating layer 6 because the deposition time is too long, but the process of removing unnecessary portions takes even more time. The thickness is more preferably 50 nm or more and 1 μm or less.
[0043] <2.6> Second seed layer The second seed layer 8 is a power supply layer for forming the second conductive layer 9 by a semi-additive method. For example, Cu, Ni, Al, Ti, Cr, Mo, W, Ta, Au, Ir, Ru, Pd, Pt, AlSi, AlSiCu, AlCu, NiFe, or a Cu alloy alone or in combination is used for the second seed layer 8. Copper is preferable for easy subsequent etching removal.
[0044] The thickness of the second seed layer 8 is preferably 50 nm or more and 5 μm or less. If the thickness of the second seed layer 8 is less than 50 nm, electrical conductivity failure may occur in the subsequent electrolytic plating process. If the thickness of the second seed layer 8 exceeds 5 μm, it takes a long time to remove it by etching. The thickness of the second seed layer 8 is more preferably 100 nm or more and 500 nm or less.
[0045] <2.7> Second conductive layer The second conductive layer 9, which becomes the upper electrode of the capacitor 10, is an electrolytic plating layer. The second conductive layer 9 is preferably made of electrolytic copper plating, which is simple, inexpensive, and has good electrical conductivity. However, in addition to electrolytic copper plating, electrolytic nickel plating, electrolytic chromium plating, electrolytic Pd plating, electrolytic gold plating, electrolytic rhodium plating, electrolytic iridium plating, etc. may also be used.
[0046] The thickness of the second conductive layer 9 (thickness of electrolytic copper plating) is preferably 3 μm or more and 30 μm or less. If it is less than 3 μm, there is a risk that the circuit will disappear depending on the etching process after the formation of the second conductive layer 9. Furthermore, the connection reliability and electrical conductivity of the circuit may decrease. If the thickness of the electrolytic copper plating exceeds 30 μm, it is necessary to form a resist layer with a thickness of 30 μm or more, which increases the manufacturing cost. Furthermore, since the resist resolution decreases, it becomes difficult to form fine wiring with a pitch of 30 μm or less. It is more preferable that the thickness is 5 μm or more and 25 μm or less. Further preferably, it is 7 μm or more and 20 μm or less.
[0047] <2.8> Insulating resin layer The insulating resin layer 12 is mainly made of a thermosetting resin filled with a filler. It is a material containing at least one of epoxy resin, polyimide resin, and polyamide resin, and containing fillers such as silica, titanium oxide, and urethane, and is preferably a liquid or film-like material. In the case of liquid resin, it can be formed by spin coating, and in the case of film-like resin, it can be formed by heating and pressing under vacuum using a vacuum laminator. The material of the insulating resin layer 12 can be appropriately selected according to the needs.
[0048] <2.9> Third seed layer The third seed layer 13 is formed using the same material as the second seed layer 8.
[0049] <2.10> Third conductive layer The third conductive layer 14 is formed using the same material as the second conductive layer 9.
[0050] <3> Wiring board manufacturing process 2 to 12 are cross-sectional views showing an example of a manufacturing process for wiring board 100. Fig. 13 is a cross-sectional view showing an example of wiring board 100 formed as a multilayer wiring board through the manufacturing processes shown in Figs. 2 to 12.
[0051] An example of a method for manufacturing the wiring board 100 will now be described with reference to FIGS.
[0052] <3.1>Process 1 First, a substrate 1 having a through hole penetrating from the upper surface to the lower surface of the substrate 1 is prepared, although this is not shown in Figs. 2 to 12. When the wiring substrate 100 is completed as a multilayer wiring substrate, the through hole 16 of the substrate 1 is filled with an insulating resin layer 12, as shown in Fig. 13. The cross-sectional shape and diameter of the through hole may be, for example, a shape in which the diameter at the center is narrower than the top and bottom diameters of the through hole, or a shape in which the bottom diameter is smaller than the top diameter. Furthermore, the through hole may be a shape in which the diameter at the center is wider than the top and bottom diameters.
[0053] <3.2> Process 2 Next, as shown in Fig. 2, an adhesion layer 2 and a first seed layer 3 are formed on the surface of the substrate 1, and are also formed on the inner surfaces of the through holes of the substrate 1, although not shown in Figs. 2 to 12. When the wiring substrate 100 is completed as a multilayer wiring substrate, the adhesion layer 2 and the first seed layer 3 are formed on the upper and lower surfaces of the substrate 1 and on the inner surfaces of the through holes, as shown in Fig. 13. The adhesion layer 2 and the first seed layer 3 act as a power supply layer for electrolytic plating in the wiring formation process in the semi-additive process.
[0054] In the process of forming the adhesion layer 2 and the first seed layer 3, it is desirable to form a titanium layer as the adhesion layer 2 on the substrate 1 by a sputtering method, then form a copper layer as the first seed layer 3 by a sputtering method, and then additionally form a metal layer by electroless plating.
[0055] If the titanium layer or copper layer is formed only by sputtering, the metal film may not be uniformly formed on the inner wall of the through hole. For this reason, it is desirable to reinforce the metal layer by electroless plating. Examples of electroless plating layers include electroless copper plating and electroless nickel plating, but electroless nickel plating is desirable because of its good adhesion to glass, titanium layer, and copper layer.
[0056] If the nickel plating layer is too thick, it may be difficult to form fine wiring. Also, the adhesion may decrease due to an increase in film stress. Therefore, the thickness of the electroless nickel plating is preferably 1 μm or less. Also, it is more preferably 0.5 μm or less, and further preferably 0.3 μm or less.
[0057] Furthermore, the electroless nickel plating film may contain phosphorus, which is a co-deposit derived from the reducing agent, and sulfur, lead, bismuth, and the like, which are contained in the electroless nickel plating solution.
[0058] Through the above steps, a substrate is obtained in which a seed metal layer is formed on a glass substrate having through holes formed thereon.
[0059] <3.3>Process 3 2, a pattern is formed using a resist 11 above the first seed layer 3. In the process of forming a pattern using the resist 11, first, a layer of the resist 11 is formed over the entire surface of the first seed layer 3. Examples of resists that can be used include negative dry film resists, negative liquid resists, and positive liquid resists, but negative photoresists are preferable because the resist layer can be easily formed and is inexpensive.
[0060] <3.4>Process 4 Next, a pattern for forming a desired conductor circuit layer is formed on the photoresist layer by photolithography. That is, the pattern of the resist 11 is aligned so that the portion where the conductor circuit layer is to be formed is exposed, and patterning is achieved by exposure and development. The thickness of the resist layer depends on the thickness of the conductor circuit layer, but is preferably 5 μm or more and 25 μm or less. If it is thinner than 5 μm, the electrolytic plating layer that becomes the conductor circuit layer cannot be thickened to 5 μm or more, and the connection reliability of the circuit may decrease. If it is thicker than 25 μm, it becomes difficult to form fine wiring with a pitch of 30 μm or less. This results in a substrate on which a photoresist pattern is formed.
[0061] <3.5>Process 5 Next, as shown in FIG. 3, power is supplied to the first seed layer 3 and it is immersed in a plating solution to form an electrolytic plating layer, which is the first conductive layer 4, which will later become a conductor circuit layer, on the upper surface of the first seed layer 3 on which the photoresist pattern is not formed.
[0062] <3.6>Process 6 Next, the photoresist pattern that is no longer necessary is removed to expose the first conductive layer 4 and the first seed layer 3, as shown in Fig. 4. The method for removing the resist 11 is not limited to any particular method, but it can be peeled off and removed, for example, with an alkaline aqueous solution.
[0063] <3.7>Process 7 5, a lower adhesive layer 5, an insulating layer 6, an upper adhesive layer 7, and a second seed layer 8 are sequentially deposited over the entire surface of the first conductive layer 4 that will become the lower electrode. Methods for forming these layers include, but are not limited to, vacuum deposition, sputtering, ion plating, MBE, laser ablation, and CVD.
[0064] The lower adhesion layer 5 below the insulating layer 6 has the function of improving the adhesion between the insulating layer 6 and the first conductive layer 4. However, if the adhesion between the insulating layer 6 and the first conductive layer 4 is sufficient, the lower adhesion layer 5 may be omitted.
[0065] In this embodiment, after the formation of the first conductive layer 4, the lower adhesive layer 5, the insulating layer 6, the upper adhesive layer 7, and the second seed layer 8 are formed without etching the first seed layer 3. Therefore, when forming the second seed layer 8, it is possible to suppress abnormalities in the adhesion of the second seed layer 8. As a result, the second conductive layer can also be formed stably.
[0066] The second seed layer 8 functions as a power supply layer for forming the second conductive layer 9 by a semi-additive method.
[0067] <3.8>Process 8 6, a pattern of resist 11 is formed on the upper surface of second seed layer 8 in an area other than the area where second conductive layer 9 is to be formed. The pattern of resist 11 can be formed in the same manner as the photoresist pattern described above. In this case, the opening area of the pattern of resist 11 is formed so as to be contained inside the area of first conductive layer 4 that will become the lower electrode, and is also formed so as to be contained inside first conductive layer 4 in plan view in the stacking direction, except for the portion of the connection line to the outside of capacitor 10.
[0068] <3.9>Process 9 Subsequently, power is supplied to the second seed layer 8, and a second conductive layer 9 that will become the upper electrode is formed by electrolytic plating.
[0069] <3.10>Process 10 Subsequently, the pattern of the resist 11 is removed as shown in Fig. 7. The photoresist pattern can be removed by peeling off with an alkaline aqueous solution.
[0070] <3.11>Process 11 Next, the second seed layer 8, the upper adhesion layer 7, the insulating layer 6, and the lower adhesion layer 5 are removed by etching. At this time, unnecessary portions of the second seed layer 8 and the upper adhesion layer 7 may be removed using the second conductive layer 9 as a mask. In this way, the area of the insulating layer on the outer surface of the MIM capacitor device is increased, and current leakage from the side surface between the upper electrode and the lower electrode can be suppressed.
[0071] <3.12>Process 12 8, the pattern of resist 11 is again formed so as to surround the first conductive layer 4. That is, the pattern of resist 11 is formed so as to become an etching mask having a width b larger than the width a of the first conductive layer 4 in at least one lateral direction (for example, the positive or negative direction of the X-axis).
[0072] That is, the width of the etching mask, which is wider than the first conductive layer 4, corresponds to the width of the first seed layer 3. In this case, the non-opening regions of the photoresist pattern are formed so as to be outside the region of the first conductive layer 4, and are also formed so as to be outside the region of the first conductive layer 4 in plan view in the stacking direction, except for the portion of the connection line to the outside of the capacitor 10.
[0073] <3.13>Process 13 Subsequently, the exposed portions of the first seed layer 3 are removed.
[0074] The electroless Ni layer, copper layer, and titanium layer can be sequentially removed by chemical etching. The type of etching solution is appropriately selected depending on the type of metal to be removed, and the removal method is not limited to the method described in this embodiment.
[0075] <3.14>Process 14 Subsequently, the pattern of resist 11 is removed to obtain a wiring board on which a capacitor is formed, as shown in Fig. 9. The photoresist pattern can be removed and peeled off with an alkaline aqueous solution.
[0076] <3.15>Process 15 Thereafter, as shown in Fig. 10, an insulating resin layer 12 is formed on the wiring board formed in step 14. The insulating resin layer 12 can be formed by using a method such as vacuum lamination or roll lamination. After lamination of the insulating resin layer 12, the insulating resin layer 12 may be semi-cured by heating or UV irradiation. Furthermore, in order to improve resistance in a reliability test, full curing may be performed in a final step after forming vias or the like, which will be described later.
[0077] <3.16>Process 16 11, in order to form a via that provides electrical connection between the capacitor and the upper wiring, a via hole 15H is formed in the region of portion X. Specifically, the via hole 15H is formed by opening a through hole in the region of the insulating resin layer 12 where the via is to be formed.
[0078] To form the via hole 15H, a laser process is performed in which the through hole is processed by irradiating the through hole with a laser beam. For the laser process, it is preferable to use a pulsed laser such as a carbon dioxide gas laser or a UV-YAG laser, and a laser with a pulse width on the order of μs is suitable. The shape of the via hole 15H may be adjusted by adjusting the wavelength, output, pulse width, number of shots, spot diameter, etc. of the laser. The details of the laser process will be described later.
[0079] <3.17>Process 17 Next, a desmear process is performed to remove the insulating resin residue generated by the laser process. The desmear process may be a wet process using permanganic acid or a dry process using plasma. The details of the desmear process will be described later.
[0080] <3.18>Process 18 Thereafter, as shown in Fig. 12, a third seed layer 13 is formed. The above-mentioned layers can be formed by a method such as, but not limited to, a vacuum deposition method, a sputtering method, an ion plating method, an MBE method, a laser ablation method, and a CVD method. To improve the adhesion of the third seed layer 13, an adhesion layer can be added.
[0081] Furthermore, using the third seed layer 13 as a power supply layer, a third conductive layer 14 including vias 15 is formed by a semi-additive method or the like. The procedure is as follows: a desired pattern is formed using resist 11, and then the third conductive layer 14 is formed in places other than the resist 11 using an electrolytic plating layer.
[0082] <3.19>Process 19 Thereafter, as shown in Fig. 13, laminated conductor circuit layers and insulating resin layers 12 are repeatedly formed to form a multilayer wiring board, forming wiring board 100. The conductor circuits and laminated structure on the wiring board can be formed using a semi-additive method or a subtractive method.
[0083] In the multilayer wiring board, not only are there capacitors 10 and vias 15 formed through steps 1 to 18, but there are also vias 15' and the like that are disposed in places where there are no capacitors 10. This will be described later.
[0084] After forming the multilayer wiring board, external connection terminals may be formed, and solder balls may be formed on the external connection terminals. The multilayer wiring board may have laminated conductor circuit layers, external connection terminals, and solder balls on only one side, or the same on both sides. Semiconductor chips and chip components may also be mounted.
[0085] <4> Via shape and dimensions Fig. 14 is a cross-sectional view that shows a schematic cross-sectional shape in the vicinity of via 15 shown in Fig. 12. In Fig. 14, in order to make it easier to understand the stress caused by the difference in linear expansion coefficient between the conductor and the insulating resin, the third seed layer 13 and the third conductive layer 14 are collectively represented as the third conductive layer 14.
[0086] On the other hand, Fig. 15 is a cross-sectional view showing the cross-sectional shape of the vicinity of a via 15' in a portion other than the capacitor 10 in the wiring in the same layer as that shown in Fig. 14, as shown in Fig. 12. Since there is no capacitor 10 below the via 15' shown in Fig. 15, the first conductive layer 4 serves as a pad portion.
[0087] 14, there is a capacitor 10 below the via 15 as described above, and there are a first conductive layer (lower electrode) 4, an insulating layer (dielectric layer) 6, and a second conductive layer (upper electrode) 9 to form an MIM section. Since there are two conductive layers (wiring layers), the total thickness of the conductive layers (the thickness of the first conductive layer 4 plus the thickness of the second conductive layer 9) is larger at the location where the capacitor 10 exists than at other locations, and the stress difference is larger than at other locations. This also affects the wiring with the via 15 arranged above the capacitor 10, and unless some countermeasure is taken, there is a possibility that the reliability of the wiring board 100 will decrease. This embodiment solves such a problem.
[0088] Generally, some vias have a diameter (via diameter) that changes depending on the position in the Z-axis direction from the bottom part (via bottom part) 15B to the top part (via top part) 15T, while others do not. If the via diameter does not change depending on the position in the Z-axis direction, the via is cylindrical and its vertical cross-sectional shape is rectangular. On the other hand, if the via diameter changes depending on the position in the Z-axis direction, there are various vertical cross-sectional shapes of the via, and the part where the via diameter is smallest (smallest via diameter part) 15M also varies. Figure 14 shows an example of such various vertical cross-sectional shapes.
[0089] 14, "H" represents the height (via height) from the via bottom 15B to the via top 15T, and "h1" represents the height (via minimum diameter height) from the via bottom 15B to the via minimum diameter 15M. "dt" represents the diameter (via top diameter) of the via top 15T, "db" represents the diameter (via bottom diameter) of the via bottom 15B, and "d0" represents the diameter (via minimum diameter) of the via minimum diameter 15M. "d1" represents the horizontal spread width (via spread width) of the via bottom 15B relative to the via minimum diameter 15M, specifically, half the difference between the via bottom diameter db and the via minimum diameter d0, and is calculated by "(db-d0) / 2".
[0090] The via 15 according to this embodiment is configured such that the minimum via diameter part 15M is located at a position away from the via bottom part 15B. The minimum via diameter part 15M is not located in the via bottom part 15B. In the example of FIG. 14, the minimum via diameter part 15M is located midway between the via bottom part 15B and the via top part 15T. However, this is not the only example, and the minimum via diameter part 15M may be located in the via top part 15T. That is, the minimum via diameter height h1 is set to a value exceeding zero, with the via height H as the upper limit.
[0091] Thus, in this embodiment, since the via 15 has the smallest via diameter part 15M separated from the via bottom part 15B, the via 15 is less affected by stress strain caused by differences in thermal expansion coefficients between layers in the capacitor 10, and disconnection between the via 15 and the second conductive layer (upper electrode) 9 at the via bottom part 15B is suppressed.
[0092] In a thermal shock test, it was confirmed that the via bottom portion 15B is the location most susceptible to stress due to the difference in linear expansion coefficient between the insulating resin layer 12 and the conductor of the via 15. If the minimum via diameter portion 15M is located at the via bottom portion 15B, more stress will be concentrated therein. According to this embodiment, such stress concentration is suppressed.
[0093] As a result of examining the desirable value of the via minimum diameter height h1, it was confirmed that h1 is preferably 1 μm or more, and more preferably 5 μm or more. In other words, it was confirmed that by setting h1 to 1 μm or more, stress concentration at the via bottom portion 15B can be suppressed.
[0094] Furthermore, a desirable value of the minimum diameter height ratio Hp (=h1 / H), which is the ratio of the minimum diameter height h1 of the via to the via height H, was verified, and it was confirmed that Hp is preferably set in the range of 0.03 to 0.6, and more preferably in the range of 0.06 to 0.4. If Hp is less than 0.03, the effect of separating the minimum diameter part 15M of the via from the via bottom part 15B is reduced, and the possibility of wire breakage increases. On the other hand, if Hp is more than 0.6, the laser processing conditions (output, pulse width, number of shots, spot diameter, etc.) during via hole formation become too strong, causing thermal damage to the wiring near the via bottom part 15B. By setting Hp in the range of 0.03 to 0.6, the occurrence of such problems can be suppressed.
[0095] In addition, as a result of examining the desirable value of the via spread width d1, it was confirmed that d1 is preferably 1 μm or more, and more preferably 5 μm or more. In other words, it was confirmed that the connection reliability of the via is improved by making the via bottom diameter db larger than the via minimum diameter d0 by a certain amount or more.
[0096] Furthermore, a desirable value of the via bottom ratio Br (=db / d0), which is the ratio of the via bottom diameter db to the via minimum diameter d0, was verified, and it was found that Br is preferably set in the range of 1.05 to 2.0, and more preferably in the range of 1.1 to 1.6. If Br is less than 1.05, the effect of increasing db is small, and the effect of suppressing stress concentration is reduced. On the other hand, if Br exceeds 2.0, the laser processing conditions (output, pulse width, number of shots, spot diameter, etc.) during via hole formation become too strong, causing thermal damage to the wiring near the via bottom portion 15B. By setting Br in the range of 1.05 to 2.0, the occurrence of such problems can be suppressed.
[0097] <5> Laser and desmear processing details The laser treatment shown in step 16 of <3.16> above and the desmear treatment shown in step 17 of <3.17> above will be described in detail.
[0098] <5.1> Laser treatment and desmear treatment conditions In the laser processing and desmear processing, the above-mentioned through hole is processed so that the via diameter of the via bottom part 15B is larger than that of the minimum via diameter part 15M. For this purpose, in the laser processing, it is desirable to irradiate the laser light while adjusting the laser processing conditions (e.g., output, pulse width, number of shots, spot diameter, etc.) so that the opening on the via bottom part 15B side is larger than the opening on the minimum via diameter part 15M. In this case, the laser processing conditions for the opening on the via bottom part 15B side are set stronger than the laser processing conditions for the opening on the minimum via diameter part 15M.
[0099] Furthermore, when enlarging the opening near the via bottom portion 15B, it is desirable to set the laser processing conditions (e.g., output, pulse width, number of shots, spot diameter, etc.) for that area stronger than the laser processing conditions for an area without the MIM portion.
[0100] The pulse width is preferably on the order of microseconds, depending on the material of the insulating resin layer 12. The laser spot diameter is preferably 10 to 100 μm. The number of shots is preferably several tens to a hundred.
[0101] In order to adjust the shape of the via hole 15H, the composition of the insulating resin layer 12, additives, fillers, etc. may be adjusted in advance. Also, the curing conditions of the insulating resin layer 12, such as the lamination temperature, curing temperature, curing time, etc. may be adjusted.
[0102] Since the heat transfer conditions during laser processing differ depending on the thickness and pattern width of the underlying conductive layer (wiring layer), the shape of the via hole 15H may be adjusted by adjusting these conditions in advance.
[0103] After the laser treatment, a desmear process is performed to remove the residue of the insulating resin generated by the laser processing, and the desmear process may be a wet process using permanganic acid or a dry process using plasma, as described above. For example, in the case of a wet process, the via shape may be adjusted by adjusting the composition, temperature, processing time, etc. of the desmear solution.
[0104] <5.2> Shape after laser processing, shape after desmear processing 16 shows the cross-sectional shape of the via hole 15H after the laser processing and the cross-sectional shape of the via hole 15H after the desmear processing, in comparison with the conventional example and examples 1 and 2 of this embodiment. The laser processing conditions (pulse width, number of shots, etc.) are different between examples 1 and 2. Detailed conditions in examples 1 and 2 will be described later.
[0105] 16(a) shows a cross-sectional shape according to a conventional example. To form a via hole 15H, a part of the insulating resin layer 12 on the second conductive layer (upper electrode) 9 in the MIM part is processed by laser processing. After that, the residue of the insulating resin is removed by desmearing. At that time, the cross-linking of the resin is broken by the laser processing, and the part which has become low molecular weight is also removed, and a via hole which is one size larger than that formed by the laser processing is formed.
[0106] 16(b) shows a cross-sectional shape of Example 1 of this embodiment. By performing laser processing using the method described in <5.1> above, the area in which the insulating resin is depolymerized is enlarged, particularly in the vicinity of the via bottom. When desmear processing is then performed, the area in the vicinity of the via bottom of the via hole 15H after desmear processing is enlarged compared to the conventional example, and the via bottom diameter is enlarged.
[0107] 16(c) shows a cross-sectional shape according to Example 2 of this embodiment. In Example 2, the laser processing and desmear processing are performed in the same manner as in Example 1, but by strengthening the laser processing conditions compared to Example 1, the region near the via bottom of the via hole 15H is expanded compared to Example 1, and the via bottom diameter is increased.
[0108] <6> Examples of via shapes 17(a) to (f) show various forms of the cross-sectional shape of the via 15 according to this embodiment.
[0109] 17(a) to (f), all of the vias 15 have h1 and d1 that exceed zero. That is, the minimum via diameter portion of each of the vias 15 is located away from the via bottom portion 15B, and the via bottom diameter is greater than the minimum via diameter. By forming the vias 15 in this manner, it is possible to suppress stress concentration at the via bottom portion 15B and prevent breakage of the conductor at the via bottom portion 15B.
[0110] On the other hand, FIGS. 18(a) to (e) show various cross-sectional shapes of vias 15 according to the prior art.
[0111] 18(a) to 18(e), none of the vias 15 have h1 or d1 that exceed zero. In each of the vias 15, the smallest via diameter is at the via bottom 15B, and the via bottom diameter is the smallest via diameter. If the vias 15 are formed in this way, stress is concentrated at the via bottom 15B, making the conductor at the via bottom 15B more likely to break.
[0112] <7> Example 1, Example 2, Comparative Example 1 Hereinafter, Example 1, Example 2, and Comparative Example 1 of this embodiment will be described.
[0113] <7.1> Example 1 Example 1 of this embodiment is shown below.
[0114] In Example 1, a wiring board having a capacitor 10 with a 1-2-1 structure shown in FIG. 13 was fabricated.
[0115] Specifically, a non-alkali glass having a thickness of 150 μm and a size of 320 mm×400 mm was used as the substrate, and the front and back surfaces were electrically connected by a TGV (through glass via). Ti was used for the adhesion layer 2, the lower adhesion layer 5, and the upper adhesion layer 7, and the film thickness was set to 40 nm. Cu was used for the first seed layer 3, the second seed layer 8, and the third seed layer 13, and the film thickness was set to 100 nm. Cu was used for the first conductive layer 4, the second conductive layer 9, and the third conductive layer 14, and the film thickness was set to 10 μm, 5 μm, and 10 μm, respectively. A sheet-shaped epoxy resin having a film thickness of 30 μm was used for the insulating resin layer 12. The sheet-shaped epoxy resin was laminated under the condition of 100° C., and cured at 180° C. for 1 hour as a pre-cure. Silicon nitride was used for the insulating resin layer 12, and the film thickness was set to 500 nm. The electrode area of the MIM part was 20,000 μm for the lower electrode, and 20,000 μm for the insulating resin layer. 2 The upper electrode is 10000 μm 2 It was decided.
[0116] For the via 15, the via hole 15H was formed with a UV-YAG laser, with a pulse width of 100 us and 60 shots, aiming for a via top diameter dt of 40 μm. After the via hole was formed by the laser treatment, a desmear treatment was performed with a permanganic acid-based desmear solution at 75° C. for 40 minutes, and then electroless Cu plating and electrolytic plating were performed to form the via 15, which is a filled via, in the via hole 15H. The via dimensions at that time were a via top diameter dt of 40 μm, a minimum diameter d0 of 32 μm, a via bottom diameter db of 36 μm, a via height H of 27 μm, and a via minimum diameter height h1 of 5 μm. In addition, after the wiring was formed, the insulating resin layer 12 was fully cured at 200° C. for 1 hour.
[0117] A temperature cycle test (TCT test) was performed on the fabricated wiring board under the conditions described below. In addition, when a piece from the same lot as that used in the TCT test was observed in cross section, the via 15 was basically shaped as shown in FIG. 16(b), with the minimum diameter portion located above the via bottom portion 15B.
[0118] <7.2> Example 2 Example 2 of this embodiment is shown below.
[0119] In Example 2, a sample was produced in the same manner as in Example 1, except that the laser processing conditions were changed in forming a via above the MIM portion.
[0120] Specifically, processing was performed with a UV-YAG laser, with a pulse width of 80 μm and the number of shots set to 120, aiming for a via top diameter dt of 40 μm. The via dimensions at that time were: via top diameter dt 41 μm, minimum diameter d0 35 μm, via bottom diameter db 43 μm, via height H 27 μm, and via minimum diameter height h1 7 μm.
[0121] As in Example 1, when a piece from the same lot as that submitted to the TCT test was observed in cross section, it was found that the via 15 basically had the shape shown in Figure 16(c), with the minimum diameter portion located above the via bottom portion 15B.
[0122] <7.3> Comparative Example 1 Comparative Example 1 of this embodiment is shown below.
[0123] In Comparative Example 1, a sample was produced in the same manner as in Example 1, except that the laser processing conditions were changed in forming a via above the MIM portion.
[0124] Specifically, processing was performed with a UV-YAG laser with 40 shots, aiming for a via top diameter dt of 40 μm. The via dimensions at that time were as follows: via top diameter dt was 40 μm, the via bottom diameter db was the minimum diameter d0 because the minimum part of the via diameter was at the via bottom, via bottom diameter db was 29 μm, via height H was 27 μm, and there was no minimum via diameter height h1.
[0125] As in Example 1, when a piece from the same lot as that used in the TCT test was examined for cross section, the via of capacitor 10 basically had the shape shown in FIG. 16(a), with the minimum diameter portion at the via bottom.
[0126] <7.4> Test conditions The TCT test is generally used as a standard for judging the connection reliability of through electrodes in multilayer wiring boards. In the TCT test, the multilayer wiring board is repeatedly exposed to high and low temperature environments, which generates stress in each layer of the multilayer wiring board due to differences in thermal expansion coefficients, making it possible to verify the tendency of wiring breakage due to stress, especially in vias.
[0127] Specifically, the capacitance of the MIM portion was measured in wiring passing through the MIM portion of the wiring substrate 100 shown in Fig. 13. Based on the change in the MIM capacitance before and after the TCT test, an open circuit (wiring breakage) in the wiring near the MIM (especially the via bottom portion) was verified.
[0128] The TCT test conditions were -55°C to 125°C, 500 cycles, and 500 pieces of each type. The wiring width was 140 μm, and the pad diameter was φ100 μm (vias other than the MIM part were formed on the above pads).
[0129] In the judgment, if the rate of change from the initial capacitance was within ±10, it was marked as OK, and if it exceeded 10%, it was marked as × (NG) (because the MIM capacitance changes significantly if an open circuit occurs in the via of the MIM section).
[0130] <7.5> Verification results The results of verification of Example 1, Example 2, and Comparative Example 1 are summarized in the table below.
[0131] [Table 1]
[0132] In particular, in Comparative Example 1, 23% of defects occurred after 500 cycles of TCT testing, whereas no defects occurred in Examples 1 and 2. From the above results, it was confirmed that the treatments performed in Examples 1 and 2 were effective in suppressing disconnection of vias 15 on capacitor 10 in thermal shock testing. From these verification results, it was found that a highly reliable wiring board 100 could be manufactured.
[0133] <8> summary As described above in detail, according to the embodiment, the via 15 has the minimum via diameter part 15M separated from the via bottom part 15B, so that the via 15 is less affected by the stress strain caused by the difference in thermal expansion coefficient between the layers in the capacitor 10, and disconnection between the via 15 and the second conductive layer (upper electrode) 9 at the via bottom part 15B is suppressed. Therefore, it is possible to improve the reliability of the wiring board 100 having the capacitor 10. [Explanation of symbols]
[0134] 1...substrate, 2...adhesion layer, 3...first seed layer, 4...first conductive layer (lower electrode), 5...lower adhesion layer, 6...insulating layer (dielectric layer), 7...upper adhesion layer, 8...second seed layer, 9...second conductive layer (upper electrode), 10...capacitor, 11...resist, 12...insulating resin layer, 13...third seed layer, 14...third conductive layer, 15...via, 15B...via bottom portion, 15T...via top portion, 15H...via hole, 15M...minimum via diameter portion, 16...through hole, dt...via top diameter, db...via bottom diameter, d0...minimum via diameter, d1...via spread width, H...via height, h1...minimum via diameter height.
Claims
1. A wiring substrate having a capacitor including a lower electrode, a dielectric layer disposed above the lower electrode, and an upper electrode disposed above the dielectric layer, and a via having a via bottom portion disposed on the upper electrode, The via is formed so that a portion of the via having a minimum diameter is located away from the via bottom.
2. The via is When the height from the via bottom portion to the via top portion is H and the height from the via bottom portion to the portion with the smallest via diameter is h1, the via is formed so that "h1 / H" is within a range of 0.03 to 0.
6. The wiring board according to claim 1 .
3. The via is When the diameter of the via bottom portion is db and the diameter of the minimum portion of the via diameter is d0, the via is formed so that "db / d0" is within a range of 1.05 to 2.
0. The wiring board according to claim 1 .
4. The capacitor is formed on a substrate made of a glass material. The wiring board according to claim 1 .
5. The via is a filled via. The wiring board according to claim 1 .
6. 1. A method for manufacturing a wiring board, the method comprising the steps of: manufacturing a wiring board having a capacitor including a lower electrode, a dielectric layer disposed above the lower electrode, and an upper electrode disposed above the dielectric layer; and a via having a via bottom portion disposed on the capacitor, the method comprising the steps of: forming an insulating resin layer on the conductive layer that will become the upper electrode; and forming a via hole by opening a through hole in a region of the insulating resin layer where the via is to be formed, A method for manufacturing a wiring substrate, wherein the step of forming the via hole includes forming the via hole such that a portion of the via having a minimum diameter is located away from a via bottom portion.
7. In the step of forming the via hole, performing a laser treatment for processing the through hole by irradiating the through hole with a laser beam, and a desmear treatment for removing a residue of an insulating resin generated by the laser treatment; In the laser treatment and the desmear treatment, the through hole is treated so that the via diameter at the via bottom portion is larger than the via diameter at a portion where the via diameter is minimum. The method for manufacturing a wiring board according to claim 6 .
8. In the laser processing, laser processing conditions are adjusted so that an opening on the via bottom side is larger than an opening at a portion where the via diameter is smallest. The method for manufacturing a wiring board according to claim 7 .
Citation Information
Patent Citations
Wiring substrate and semiconductor device
WO2019244382A1