Polarizing film, polarizing plate, and method for manufacturing polarizing film
A dichroic organic dye-based polarizing film with a non-polarized portion formed by laser decoloration addresses recoloring issues and maintains stable light transmittance, enhancing the performance of image display devices.
Patent Information
- Application Number
- JP2023059132
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing polarizing films used in image display devices face issues with recoloring of non-polarized portions over time and maintain poor light transmittance stability, especially under moist heat conditions.
A polarizing film composed of a resin film containing a dichroic organic dye, with a non-polarizing portion having specific absorbance and haze values, is manufactured using a solid-state pulse laser to form a non-polarized area, ensuring stable light transmittance and resistance to recoloring.
The solution effectively suppresses recoloring and maintains excellent light transmittance in the non-polarized portion, even under moist heat conditions, with improved durability and optical properties.
Smart Images

Figure 2024146316000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a polarizing film, a polarizing plate, and a method for producing a polarizing film. [Background technology]
[0002] In recent years, image display devices, such as liquid crystal display devices and electroluminescence (EL) display devices (e.g., organic EL display devices, inorganic EL display devices), have rapidly become widespread. In such image display devices, a polarizing film containing iodine is typically used. In addition, in order to accommodate the diversification of shapes and high functionality of image display devices, a polarizing film having partial polarization performance is required. As a method for producing such a polarizing film, a technique is known in which a part of the polarizing film is irradiated with laser light containing light with a wavelength of at least 1500 nm or less to bleach the film and form a non-polarizing part (e.g., Patent Document 1). However, in the non-polarizing part of the polarizing film produced by such a method, although it is bleached immediately after irradiation with the laser light, there is a risk that the non-polarizing part will recolor over time. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2014-81482 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention has been made to solve the above-mentioned problems in the conventional art, and its main object is to provide a polarizing film, a polarizing plate, and a method for manufacturing a polarizing film that can suppress color recovery in the non-polarized part and maintain excellent light transmittance in the non-polarized part. [Means for solving the problem]
[0005] [1] A polarizing film according to an embodiment of the present invention is made of a resin film containing a dichroic organic dye. The polarizing film has a non-polarizing portion. The non-polarizing portion has an absorbance of 0.001 to 3.0 for light having wavelengths of 470 nm, 560 nm, and 700 nm. [2] In the polarizing film according to the above [1], the resin film may contain a polyvinyl alcohol resin. The dichroic organic dye may contain at least one selected from an azo dye represented by the following formula (1), a salt of the azo dye, a chelate of the azo dye, or a mixture thereof: [ka] (In formula (1), X and Z each represent an atomic group shown in the following (2) to (13); Y represents an atomic group shown in the following (14) to (29); and m represents an integer of 0 to 6.) [ka] (In the formulas (2) to (13), A represents H, OH, OR1, SO3H, NH2, NR2, NO2, COOH, COOR, NHCOR, or a hydrocarbon group having 1 to 12 carbon atoms which may have a linear structure, branched structure, cyclic structure, double bond, or triple bond; R represents a hydrocarbon group having 1 to 12 carbon atoms which may have a linear structure, branched structure, cyclic structure, double bond, or triple bond; n represents an integer of 0 to 5; o represents an integer of 0 to 4; p represents an integer of 0 to 3; q represents an integer of 0 to 2; and r represents 0 or 1.) [ka] (In formulas (14) to (29), A represents H, OH, OR1, SO3H, NH2, NR2, NO2, COOH, COOR, NHCOR, or a hydrocarbon group having 1 to 12 carbon atoms which may contain a branched structure, a cyclic structure, a double bond, or a triple bond; R, n, o, p, q, and r are the same as those in formulas (2) to (13) above). [3] In the polarizing film according to [1] or [2] above, the content of the dichroic organic dye in the non-polarizing portion may be 3.0% by mass or less, when the content of the dichroic organic dye in the polarizing film excluding the non-polarizing portion is taken as 100% by mass. [4] In the polarizing film according to any one of the above [1] to [3], the haze value in the non-polarizing portion may be 5.0% or less. [5] The polarizing film according to any one of [1] to [4] above may have an absolute change in the single-phase hue L value of the Lab color system in the non-polarized portion of 4.0 or less, and an absolute change in the single-phase hue a value of the Lab color system in the non-polarized portion of 2.0 or less, before and after a moist heat test in which the polarizing film is left to stand for 8 hours in an environment of 85°C and 85% RH (relative humidity). [6] A polarizing plate according to another aspect of the present invention includes the polarizing film according to any one of the above [1] to [5], and a protective layer provided on at least one surface of the polarizing film. [7] A method for producing a polarizing film according to still another aspect of the present invention includes the steps of dyeing a resin film with a dichroic organic dye; stretching the resin film dyed with the dichroic organic dye; and irradiating laser light from a solid-state pulse laser to a part of the stretched resin film to decolorize it, thereby forming a non-polarizing portion. [8] In the method for producing a polarizing film described in [7] above, the laser light may have a wavelength of 500 nm to 550 nm. The solid-state pulse laser may have an output of 0.5 W to 100 W. Effect of the Invention
[0006] According to the embodiments of the present invention, it is possible to realize a polarizing film and a polarizing plate that can suppress color recovery in the non-polarizing portion and maintain excellent light transmittance in the non-polarizing portion. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a schematic cross-sectional view of a polarizing plate including a polarizing film according to one embodiment of the present invention. [Diagram 2]FIG. 2 is a schematic cross-sectional view of an optical laminate including the polarizing plate of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Representative embodiments of the present invention will be described below, but the present invention is not limited to these embodiments. In addition, in order to clarify the description, the width, thickness, shape, etc. of each part may be shown in a schematic manner compared to the embodiment, but these are merely examples and do not limit the interpretation of the present invention.
[0009] (Definition of terms and symbols) The definitions of terms and symbols used in this specification are as follows. (1) Refractive index (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the direction perpendicular to the slow axis in the plane (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-plane phase difference (Re) "Re(λ)" is the in-plane retardation measured with light of wavelength λ nm at 23° C. For example, "Re(550)" is the in-plane retardation measured with light of wavelength 550 nm at 23° C. Re(λ) is calculated by the formula: Re(λ)=(nx-ny)×d, where d(nm) is the thickness of the layer (film). (3)Angle When angles are referred to herein, the angles include both clockwise and counterclockwise angles relative to a reference direction, so for example, "45°" means ±45°. (4) Substantially parallel or perpendicular The expressions "substantially orthogonal" and "approximately orthogonal" include the case where the angle between two directions is 90°±10°, preferably 90°±7°, and more preferably 90°±5°. The expressions "substantially parallel" and "approximately parallel" include the case where the angle between two directions is 0°±10°, preferably 0°±7°, and more preferably 0°±5°. Furthermore, when the term "orthogonal" or "parallel" is used herein, it is intended to include the substantially orthogonal or substantially parallel state.
[0010] A. Overview of polarizing film FIG. 1 is a schematic cross-sectional view of a polarizing plate including a polarizing film according to one embodiment of the present invention. The polarizing film 11 is composed of a resin film containing a dichroic organic dye. The polarizing film 11 has a non-polarizing section 15. The absorbance of the non-polarizing section 15 for each of the light having wavelengths of 470 nm, 560 nm, and 700 nm is 3.0 or less, preferably 1.0 or less, more preferably 0.5 or less, and even more preferably 0.2 or less. On the other hand, the absorbance of the non-polarizing section 15 for the above-mentioned light is, for example, 0.001 or more, preferably 0.01 or more. The absorbance of the non-polarizing section is measured, for example, in accordance with JIS K 0115. Although the details will be described later, the non-polarized portion is a decolorized portion decolorized by irradiation of laser light by a solid pulse laser. Therefore, the absorbance of the non-polarized portion of the polarizing film can be adjusted to the above range, and excellent light transmittance can be imparted to the non-polarized portion. In addition, the polarizing film is composed of a resin film containing a dichroic organic dye. That is, the polarizing film is dyed with a dichroic organic dye different from iodine. Therefore, excellent polarization characteristics (optical characteristics; single transmittance and / or polarization degree) can be imparted to the polarizing film except for the non-polarized portion, and color recovery of the non-polarized portion can be stably suppressed. In addition, even if the polarizing film is exposed to a humid and hot environment (typically 80°C and 80 RH% or more), changes in hue can be sufficiently suppressed, and excellent light transmittance of the non-polarized portion can be maintained.
[0011] The arrangement, shape and size of the non-polarizing portion 15 can be arbitrarily and appropriately set depending on the application of the polarizing film 11 . The content of the dichroic organic dye in the non-polarizing section 15 is, for example, 10.0% by mass or less, preferably 3.0% by mass or less, and more preferably 1.5% by mass or less, when the content of the dichroic organic dye in the polarizing film 11 excluding the non-polarizing section 15 is taken as 100% by mass. On the other hand, the lower limit of the content of the dichroic organic dye in the non-polarizing section 15 is typically 0% by mass. When the content of the dichroic organic dye in the non-polarizing portion is within this range, the light transmittance in the non-polarizing portion can be stably improved.
[0012] The haze value in the non-polarizing section 15 is, for example, 30.0% or less, preferably 10.0% or less, more preferably 5.0% or less, even more preferably 3.0% or less, still more preferably 2.0% or less, and particularly preferably 0.9% or less. Meanwhile, the lower limit of the haze value in the non-polarizing section 15 is, for example, 0%. If the haze value in the non-polarizing section is in such a range, the light transmittance in the non-polarizing section can be further improved.
[0013] The polarizing film 11 (excluding the non-polarizing portion 15) has a single transmittance Ts for light with wavelengths of 380 nm to 780 nm of, for example, 38.0% or more, preferably 40.0% or more, and more preferably 40.5% or more. The polarizing film 11 has a polarization degree P of, for example, 97.5% or more, preferably 98.0% or more, more preferably 98.5% or more, and even more preferably 99.0% or more. The single transmittance Ts of the non-polarized portion 15 for light with wavelengths of 380 nm to 780 nm is, for example, 70.0% or more, preferably 85.0% or more, and more preferably 90.0% or more. The polarization degree P of the non-polarized portion 15 is, for example, 70.0% or less, preferably 25.0% or less, more preferably 3.0% or less, even more preferably 2.0% or less, and particularly preferably 0.9% or less. The single transmittance Ts can be calculated as a Y value corrected for visibility by measuring with a 2-degree visual field (C light source) according to JIS Z8701, for example.
[0014] The absolute value of the amount of change in the single-phase hue L value of the Lab color system of the non-polarizing section 15 before and after a moist heat test in which the polarizing film 11 is left standing for 8 hours in an environment of 85°C and 85% RH (relative humidity) is, for example, 10.0 or less, preferably 6.00 or less, more preferably 4.0 or less, and even more preferably 0.10 or less. Meanwhile, the lower limit of the absolute value of the amount of change in the single-phase hue L value of the Lab color system of the non-polarizing section 15 before and after the moist heat test is typically 0.10. The single-phase hue L value of the Lab color system is measured, for example, by any appropriate spectrophotometer (typically, the product name "LPF-200" manufactured by Otsuka Electronics Co., Ltd.). The absolute value of the change in the single-phase hue a value of the Lab color system of the non-polarized section 15 before and after the above-mentioned moist heat test is, for example, 5.0 or less, preferably 3.0 or less, more preferably 2.0 or less, and even more preferably 1.0 or less. Meanwhile, the lower limit of the absolute value of the change in the single-phase hue a value of the Lab color system of the non-polarized section 15 before and after the above-mentioned moist heat test is typically 0.10. The single-phase hue a value of the Lab color system is measured, for example, by any appropriate spectrophotometer (typically, the product name "LPF-200", manufactured by Otsuka Electronics Co., Ltd.). In the polarizing film described above, the absolute value of the change in the single-phase hue L value and / or the single-phase hue a value of the Lab color system of the non-polarizing part before and after the moist heat test can be within this range, and the change in hue (recoloration) of the non-polarizing part in a moist and hot environment is sufficiently suppressed.
[0015] The thickness of the polarizing film 11 is, for example, 80 μm or less, preferably 30 μm or less, more preferably 15 μm or less, and further preferably 13 μm or less. On the other hand, the thickness of the polarizing film 11 is, for example, 1 μm or more, and preferably 3 μm or more.
[0016] The resin film and the dichroic organic dye will be described in detail below.
[0017] B. Details of the resin film Any resin applicable to a polarizing film may be used as the material of the resin film. In one embodiment, the resin film contains a polyvinyl alcohol-based resin (hereinafter, referred to as a PVA-based resin). Examples of PVA resins include polyvinyl alcohol, acetal-modified polyvinyl alcohol, acetoacetyl-modified polyvinyl alcohol, and ethylene-vinyl alcohol copolymers. These PVA resins may be used alone, or two or more PVA resins having different types of modification, modification rates, polymerization degrees, and saponification degrees may be used in combination.
[0018] A typical PVA-based resin contains polyvinyl alcohol, which is obtained by saponifying polyvinyl acetate. The content of polyvinyl alcohol in the PVA-based resin is, for example, 80% by mass to 100% by mass, and preferably 88% by mass to 95% by mass.
[0019] The PVA-based resin may contain, in addition to polyvinyl alcohol, acetoacetyl-modified polyvinyl alcohol. The content of acetoacetyl-modified polyvinyl alcohol in the PVA-based resin is, for example, 5% by mass to 20% by mass, and preferably 8% by mass to 12% by mass.
[0020] The saponification degree of the PVA resin is usually 85 mol% to 100 mol%, preferably 95.0 mol% to 99.95 mol%, more preferably 99.0 mol% to 99.93 mol%, and further preferably 99.0 mol% to 99.5 mol%. The saponification degree is measured, for example, in accordance with JIS K 6726-1994. By using a PVA resin having such a saponification degree, a thin polarizing film having excellent durability can be realized.
[0021] The average degree of polymerization of the PVA resin can be appropriately selected depending on the purpose. The average degree of polymerization is, for example, 1000 or more, preferably 1500 or more, more preferably 2000 or more, and even more preferably 3000 or more. On the other hand, the average degree of polymerization is, for example, 10000 or less, preferably 6000 or less, and even more preferably 4300 or less. The average degree of polymerization is measured, for example, in accordance with JIS K 6726-1994.
[0022] C. Details of dichroic organic dyes Any appropriate dye may be used as the dichroic organic dye, and examples of the dichroic organic dye include acid dyes, direct dyes, basic dyes, salt-forming dyes, oil-soluble dyes, disperse dyes, reactive dyes, mordant dyes, vat dyes, sulfur dyes, derivatives thereof, and lake dyes thereof.
[0023] Dichroic organic dyes can also be classified based on their chemical structure. Examples of dichroic organic dyes include azo dyes, disazo dyes, azomethine dyes (such as indoaniline dyes and indophenol dyes), dipyrromethene dyes, quinone dyes (such as benzoquinone dyes, naphthoquinone dyes, anthraquinone dyes, and anthrapyridone dyes), carbonium dyes (such as diphenylmethane dyes, triphenylmethane dyes, xanthene dyes, and acridine dyes), quinoneimine dyes (such as oxazine dyes and thiazine dyes), and quinoneimine dyes (such as oxazine dyes and thiazine dyes). based dyes, etc.), azine based dyes, polymethine based dyes (oxonol based dyes, merocyanine based dyes, arylidene based dyes, styryl based dyes, cyanine based dyes, squarylium based dyes, croconium based dyes, etc.), quinophthalone based dyes, phthalocyanine based dyes, subphthalocyanine based dyes, perinone based dyes, indigo based dyes, thioindigo based dyes, quinoline based dyes, nitro based dyes, nitroso based dyes, rhodamine based dyes, and metal complex based dyes thereof. These dichroic organic dyes may be used alone or in combination.
[0024] Of these dichroic organic dyes, preferred are direct dyes, and more preferred are azo dyes. When the dichroic organic dye is an azo dye, color recovery in the non-polarized portion can be more stably suppressed. In one embodiment, the dichroic organic dye includes at least one selected from an azo dye represented by the following formula (1), a salt of the azo dye, a chelate of the azo dye, or a mixture thereof: [ka] (In formula (1), X and Z each represent an atomic group shown in the following (2) to (13); Y represents an atomic group shown in the following (14) to (29); and m represents an integer of 0 to 6.) In the above formula (1), X and Z may be the same or different from each other. When m is 2 to 6, multiple Y's may be the same or different from each other.
[0025] [ka] (In the formulas (2) to (13), A represents H, OH, OR1, SO3H, NH2, NR2, NO2, COOH, COOR, NHCOR, or a hydrocarbon group having 1 to 12 carbon atoms which may have a linear structure, branched structure, cyclic structure, double bond, or triple bond; R represents a hydrocarbon group having 1 to 12 carbon atoms which may have a linear structure, branched structure, cyclic structure, double bond, or triple bond; n represents an integer of 0 to 5; o represents an integer of 0 to 4; p represents an integer of 0 to 3; q represents an integer of 0 to 2; and r represents 0 or 1.)
[0026] [ka] (In formulas (14) to (29), A represents H, OH, OR1, SO3H, NH2, NR2, NO2, COOH, COOR, NHCOR, or a hydrocarbon group having 1 to 12 carbon atoms which may contain a branched structure, a cyclic structure, a double bond, or a triple bond; R, n, o, p, q, and r are the same as those in formulas (2) to (13) above).
[0027] Of the atomic groups represented by the above formulas (2) to (13) (i.e., X and Z in the above formula (1)), preferred examples include the atomic groups represented by the above formulas (2), (7), (8) and (13). Of the atomic groups represented by the formulae (14) to (29) (i.e., Y in the formula (1)), preferred are the atomic groups represented by the formulae (14), (22), (24), (28), and (29). In the atomic group represented by the above formulae (2) to (13), when a plurality of As are contained, the plurality of As may be the same or different from each other. In the atomic group represented by the above formulae (14) to (29), when a plurality of B's are contained, the plurality of B's may be the same or different. In the atomic group represented by the above formulae (2) to (29), when a plurality of Rs are contained, the plurality of Rs may be the same or different.
[0028] Examples of salts of azo dyes include ammonium salts, alkaline earth metal salts, transition metal salts, and poor metal salts. Examples of the chelate of an azo dye include a chelate of a metal element and a hydroxyl-containing azo dye, a chelate of an alkoxy-containing azo dye, and a chelate of a carboxyl-containing azo dye.
[0029] Of these azo dyes, Direct Red 80, Direct Red 81, Direct Blue 2, Direct Yellow 8, and Direct Violet 9 are preferable.
[0030] D. Polarizing plate As shown in Fig. 1, the polarizing films described in the above items A to C can be suitably applied to a polarizing plate. A polarizing plate including the above polarizing film can suppress color recovery in the non-polarized part, like a polarizing film, and can stably maintain excellent light transmittance in the non-polarized part. The polarizing plate 10 in the illustrated example includes the above-mentioned polarizing film 11 and a protective layer 12 provided on at least one surface of the polarizing film 11. In the illustrated example, the protective layer 12 is provided only on one surface of the polarizing film 11. Although not shown, a protective layer may be provided on both surfaces of the polarizing film 11. The protective layer may be attached to the polarizing film via a pressure-sensitive adhesive layer or an adhesive layer.
[0031] The protective layer is formed of any suitable film that can be used as a protective layer for a polarizing film. Specific examples of materials that are the main components of the film include cellulose-based resins such as triacetyl cellulose (TAC), polyester-based resins such as polyethylene terephthalate (PET), polyvinyl alcohol-based resins, polycarbonates-based resins, polyamides-based resins, polyimides-based resins, polyethersulfone-based resins, polysulfone-based resins, polystyrene-based resins, polynorbornene-based resins, polyolefin-based resins, cycloolefin (COP)-based resins, (meth)acrylic-based resins, and transparent resins such as acetate-based resins. In addition, examples of the resins include thermosetting resins or ultraviolet-curing resins such as (meth)acrylic-based resins, urethane-based resins, (meth)acrylic urethane-based resins, epoxy-based resins, and silicone-based resins. In addition, examples of the resins include glassy polymers such as siloxane-based polymers. In addition, the polymer films described in JP-A-2001-343529 (WO01 / 37007) can also be used. Note that "(meth)acrylic-based resins" refers to acrylic-based resins and / or methacrylic-based resins. Among the materials for the protective layer, a material having no polyaromatic ring is preferable, a material having no aromatic ring as a main component is more preferable, and a transparent material not having PET is even more preferable. When the protective layer is made of a material having no aromatic ring, even if the polarizing plate is subjected to a bleaching process described later, the damage to the protective layer caused by the laser light can be suppressed, and the occurrence of scorching on the protective layer can be suppressed.
[0032] The thickness of the protective layer is, for example, 5 mm or less, preferably 1 mm or less, more preferably 500 μm or less, further preferably 150 μm or less, particularly preferably 40 μm or less, whereas the thickness of the protective layer is, for example, 1 μm or more, preferably 5 μm or more.
[0033] A surface treatment layer may be provided on the surface of the protective layer (the surface opposite to the polarizing film). Examples of the surface treatment layer include a hard coat treatment layer, an anti-reflection treatment layer, an anti-sticking treatment layer, and an anti-glare treatment layer. The thickness of the surface treatment layer may be set arbitrarily and appropriately. The thickness of the surface treatment layer is, for example, 1 μm or more and 10 μm or less.
[0034] E. Optical laminate The polarizing films described above in items A to C and the polarizing plate described above in item D can be applied to an optical laminate. The optical laminate including the polarizing film described above can suppress color recovery in the non-polarized part, like the polarizing film, and can stably maintain excellent light transmittance in the non-polarized part. The optical laminate 100 in the illustrated example comprises the above-mentioned polarizing plate 10; a retardation film 20 attached to the polarizing plate 10 via an adhesive layer 30; and an adhesive layer 40 located on the opposite side of the retardation film 20 from the polarizing plate 10.
[0035] The retardation film 20 typically has an in-plane retardation. The refractive index characteristics of the retardation film 20 preferably satisfy the relationship of nx>ny≧nz. In one embodiment, the retardation film 20 functions as a λ / 4 plate. When the retardation film 20 functions as a λ / 4 plate, the in-plane retardation Re(550) of the retardation film 20 is, for example, 100 nm to 180 nm, and preferably 135 nm to 155 nm. The retardation film 20 may be composed of one layer or two or more layers. The retardation film is typically composed of a stretched film of a polyester carbonate-based resin film.
[0036] The angle between the absorption axis direction of the polarizing film 11 and the slow axis direction of the retardation film 20 is typically 40° to 50°, preferably 42° to 48°, more preferably 44° to 46°, and particularly preferably 45°. Such an angle allows the optical laminate to function as a circular polarizing plate.
[0037] Each of the pressure-sensitive adhesive layer 30 and the pressure-sensitive adhesive layer 40 is typically made of a (meth)acrylic pressure-sensitive adhesive. The thickness of each of the pressure-sensitive adhesive layer 30 and the pressure-sensitive adhesive layer 40 is, for example, 3.5 μm or more and 35 μm or less.
[0038] F. Manufacturing method of polarizing film Next, one embodiment of a method for producing a polarizing film will be described. One embodiment of the method for producing a polarizing film includes a dyeing step of dyeing the above-mentioned resin film with the above-mentioned dichroic organic dye; a stretching step of stretching the resin film dyed with the dichroic organic dye; and a bleaching step of irradiating a part of the stretched resin film with laser light from a solid pulse laser to bleach the part and form a non-polarizing part. The above-mentioned method for producing a polarizing film may further include a swelling step and / or a washing step. In the swelling step, typically, the resin film before the dyeing step is immersed in a swelling bath (swelling liquid). In the washing step, typically, the resin film is immersed in a washing bath after the stretching step and before the bleaching step. In the following, a detailed description will be given of the case where the resin film is the above-mentioned PVA-based resin film.
[0039] F-1. PVA resin film The PVA resin film before the above-mentioned steps are carried out is referred to as a raw film. The raw film may be a single-layer resin film, or may be laminated on a thermoplastic resin substrate.
[0040] Specific examples of single-layer resin films include hydrophilic polymer films such as PVA-based films, partially formalized PVA-based films, and partially saponified ethylene-vinyl acetate copolymer films, as well as polyene-based oriented films such as dehydrated PVA and dehydrochlorinated polyvinyl chloride. When the raw film is a single-layer resin film, its thickness is, for example, 20 μm to 65 μm, and preferably 30 μm to 60 μm.
[0041] When the raw film is laminated to a thermoplastic resin substrate, the raw film may be a PVA-based resin film supported on the resin substrate, or a PVA-based resin layer formed by coating on the resin substrate.
[0042] When the raw film is a PVA-based resin layer formed by coating on a resin substrate, a coating liquid containing a PVA-based resin is applied onto a long-sized resin substrate by any appropriate method, and if necessary, dried at, for example, 50°C or higher to produce a laminate comprising a PVA-based resin layer and a resin substrate.
[0043] Any suitable material may be used as the constituent material of the resin substrate. A typical constituent material of the resin substrate is an amorphous (not crystallized) polyethylene terephthalate resin, preferably an amorphous (hard to crystallize) polyethylene terephthalate resin. Specific examples of the amorphous polyethylene terephthalate resin include copolymers further containing isophthalic acid as a dicarboxylic acid and copolymers further containing cyclohexane dimethanol as a glycol. Among the resin substrates, an amorphous isophthalic copolymerized polyethylene terephthalate film resin substrate is preferably used. The thickness of the resin substrate before stretching is, for example, 20 μm to 300 μm, and preferably 50 μm to 200 μm. The surface of the resin substrate may be subjected to any suitable surface treatment (e.g., corona treatment) or may have an easy-adhesion layer formed thereon, which can improve the adhesion between the resin substrate and the PVA-based resin layer.
[0044] The coating liquid is typically a solution in which the above-mentioned PVA-based resin is dissolved in a solvent. The content of the PVA resin in the coating liquid is, for example, 3 to 20 parts by mass with respect to 100 parts by mass of the solvent. With such a resin concentration, a uniform coating film that adheres closely to the resin substrate can be formed.
[0045] Examples of the solvent include water, dimethylsulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, various glycols, polyhydric alcohols such as trimethylolpropane, and amines such as ethylenediamine and diethylenetriamine. These may be used alone or in combination. Of the solvents, water is preferred. The coating liquid may contain additives. Examples of additives include plasticizers and surfactants. Examples of plasticizers include polyhydric alcohols such as ethylene glycol and glycerin. Examples of surfactants include nonionic surfactants.
[0046] The thickness of the PVA-based resin layer formed from such a coating liquid before stretching is, for example, 3 μm or more, preferably 5 μm or more, and for example, 40 μm or less, preferably 30 μm or less.
[0047] Moreover, the laminate comprising the PVA-based resin layer and the resin substrate is preferably previously subjected to an auxiliary stretching step and stretched in the air in the longitudinal direction. The stretching temperature in the auxiliary stretching step is typically equal to or higher than the glass transition temperature (Tg) of the PVA resin, for example, equal to or higher than 95° C., and preferably equal to or higher than 120° C. The stretching temperature in the auxiliary stretching step is typically equal to or lower than 150° C. The stretching ratio of the laminate in the auxiliary stretching step is, for example, 2.1 times or more, and preferably 2.3 times or more. On the other hand, the upper limit of the stretching ratio of the laminate in the auxiliary stretching step is typically 4 times. The air-stretching method in the auxiliary stretching step may be fixed-end stretching (e.g., a method of stretching using a tenter stretching machine) or free-end stretching (e.g., a method of uniaxially stretching the laminate by passing it between rolls having different peripheral speeds).
[0048] F-2. Swelling process (insolubilization process) The above-mentioned raw film (either a raw film alone or a raw film included in a laminate) is, if necessary, subjected to the above-mentioned swelling step (insolubilization step) before the dyeing step. In the swelling step, typically, the raw film is immersed in a swelling liquid (swelling bath). The swelling liquid may be pure water or an aqueous solution of boric acid. When the swelling liquid is an aqueous solution of boric acid (i.e., an insolubilizing liquid), the content of boric acid in the insolubilizing liquid is, for example, 1 part by mass to 10 parts by mass with respect to 100 parts by mass of water. The temperature of the swelling bath is, for example, 10° C. to 60° C., and preferably 20° C. to 50° C. The immersion time in the swelling step is, for example, 10 seconds to 200 seconds, and preferably 20 seconds to 60 seconds.
[0049] F-3. Dyeing process In the dyeing process, the PVA-based resin film is dyed with a dyeing solution containing the dichroic organic dye. Specifically, the dyeing solution is brought into contact with the PVA-based resin film to adsorb the dichroic organic dye. The content of the dichroic organic dye in the dye solution can be arbitrarily and appropriately set depending on the dyeing temperature, time, pH, type of dichroic organic dye, and stretching ratio. The content of the dichroic organic dye in the dye solution is, for example, 0.01% by mass to 30.0% by mass, and preferably 0.10% by mass to 10.0% by mass.
[0050] In one embodiment, in the dyeing step, the PVA-based resin film is immersed in the dye bath. The temperature of the dye bath is, for example, 10° C. to 80° C., and preferably 20° C. to 60° C. The immersion time (dyeing time) in the dyeing step is, for example, 5 seconds to 300 seconds, and preferably 10 seconds to 60 seconds. The method of adsorbing the dye in the dyeing step is not limited to the above-mentioned immersion. For example, the dyeing solution may be applied to the PVA-based resin film, or the dyeing solution may be sprayed onto the PVA-based resin film.
[0051] F-4. Stretching process In one embodiment, in the stretching step, the PVA-based resin film after the dyeing step is stretched in the longitudinal direction in a boric acid aqueous solution as a stretching bath. Stretching the PVA-based resin film in the boric acid aqueous solution can prevent the PVA-based resin film from dissolving in the boric acid aqueous solution. The stretching ratio in the stretching step varies depending on whether or not an auxiliary stretching step is performed on the raw film. When the auxiliary stretching step is not performed on the raw film (i.e., when the raw film is a single-layer resin film or a resin film supported on a resin substrate), the stretching ratio in the stretching step is, for example, 4.5 to 7 times, and preferably 5.0 to 6.5 times or less. When the auxiliary stretching step is performed on the raw film (i.e., when the raw film is a PVA-based resin layer formed by coating on a resin substrate), the stretching ratio in the stretching step is, for example, 1.5 to 4.0 times or less, and preferably 1.5 to 3.0 times or less. The product of the stretching ratio in the auxiliary stretching step and the stretching ratio in the stretching step is, for example, 4.5 to 7.0 times, and preferably 5.0 to 6.5 times. By stretching at the above-mentioned stretching ratio, the polarizing film can be imparted with extremely excellent polarizing properties.
[0052] The content of boric acid in the drawing liquid (aqueous boric acid solution) is, for example, 0.5 parts by mass to 5.0 parts by mass, and preferably 0.7 parts by mass to 3.0 parts by mass, relative to 100 parts by mass of water. The temperature of the stretching bath is, for example, 40° C. to 85° C., and preferably 50° C. to 65° C. If the temperature of the stretching bath is equal to or lower than the upper limit, the PVA resin can be stably prevented from dissolving in the stretching bath even if the concentration of boric acid in the stretching bath is equal to or lower than the upper limit. The immersion time in the stretching step is, for example, 15 seconds or more and 300 seconds or less.
[0053] F-5. Cleaning process In the washing step, the PVA-based resin film after the stretching step is typically immersed in a washing bath, which is typically water. The temperature of the cleaning bath is, for example, 0° C. to 40° C., and preferably 10° C. to 30° C. The immersion time in the cleaning step is, for example, 5 seconds to 200 seconds, and preferably 10 seconds to 60 seconds.
[0054] F-6. Drying shrinkage process The PVA-based resin film after the washing step is preferably subjected to a drying and shrinking step before the decolorizing step. In the drying and shrinking step, typically, the PVA-based resin film is heated while being transported in the longitudinal direction. The drying and shrinking step is carried out by a heating and drying section. The heating and drying section may be a zone heating type in which the entire inside of the heating and drying section is heated, or may be a heating roll drying type in which the transport roll is heated. The heating and drying section preferably uses both of these. The inner temperature of the heating and drying section is, for example, 70°C to 120°C, and preferably 80°C to 100°C. The surface temperature of the heating roll is, for example, 60°C to 100°C, and preferably 70°C to 80°C. By drying using a heated roll, it is possible to efficiently suppress the heat curl of the PVA-based resin film (laminate), and efficiently produce a polarizing film with excellent appearance. In addition, in the drying shrinkage step, the PVA-based resin film shrinks in the width direction perpendicular to the longitudinal direction. The shrinkage rate in the width direction of the PVA-based resin film in the drying shrinkage step is, for example, 2% or more, preferably 4% or more. If the shrinkage rate in the width direction is equal to or more than such a lower limit, the orientation of the PVA and the PVA / each dichroic organic dye can be improved, and the polarization properties of the polarizing film (excluding the non-polarizing portion) can be improved. The shrinkage rate of the PVA-based resin film in the width direction is typically 10% or less, preferably 8% or less, and more preferably 6% or less. If the shrinkage rate in the width direction is equal to or less than the upper limit, the occurrence of defects in appearance such as wrinkles in the polarizing film can be suppressed. In this manner, the polarizing film 11 before the formation of the non-polarizing portions 15 is prepared.
[0055] F-7. Decolorization process In the bleaching step, any appropriate portion of the polarizing film 11 is irradiated with laser light from a solid-state pulse laser. In the bleaching step, the target of irradiation with the laser light may be only the polarizing film 11, may be a polarizing plate 10 including the polarizing film 11, or may be an optical laminate 100 including the polarizing plate 10. In other words, the polarizing film 11 may be subjected to the bleaching step after being provided with the above-mentioned layers and / or films (e.g., a protective layer, a retardation layer, a pressure-sensitive adhesive layer). When the polarizing plate 10 or the optical laminate 100 is subjected to the bleaching step, the polarizing film 11 is irradiated with laser light from the viewing side (the side opposite to the protective layer 12 in the illustrated example). In one embodiment, the laser light is moved at a predetermined processing speed to irradiate the entire area of the polarizing film 11 where the non-polarizing portion is to be formed. In this way, by irradiating the above-mentioned irradiation target with laser light from a solid-state pulse laser, a non-polarized portion having excellent light transmittance can be formed. In addition, by adjusting the irradiation conditions of the laser light, the color tone of the non-polarized portion formed can be suitably adjusted.
[0056] Examples of the solid-state pulse laser include a YAG laser and a YVO4 laser, and a YAG laser is preferable. The output of the solid-state pulse laser is, for example, 0.5W to 100W, and preferably 3.0W to 10.0W. If the output of the solid-state pulsed laser is within this range, the haze in the non-polarized portion can be stably reduced. The attenuation of the solid-state pulse laser is, for example, 20% to 80%, and preferably 30% to 50%.
[0057] The pulse width of the laser light is, for example, 1.0 ps to 100 ps, and preferably 3.0 ps to 15.0 ps. The wavelength of the laser light is, for example, 300 nm or more, preferably 355 nm or more, more preferably 500 nm or more. On the other hand, the wavelength of the laser light is, for example, 1070 nm or less, preferably 550 nm or less. If the wavelength of the laser light is in such a range, a part of the polarizing film can be smoothly decolorized, and the resin material (typically a PVA-based resin) contained in the polarizing film can be prevented from being damaged by the laser light. As a result, the haze of the non-polarized part can be reduced.
[0058] The frequency of the laser light is, for example, 5.0 kHz to 200 kHz, preferably 8.0 kHz to 30 kHz, more preferably 10 kHz to 20 kHz, and particularly preferably 10 kHz to 15 kHz. The pulse energy of the laser light is, for example, 8 μJ to 40 μJ, preferably 8 μJ to 35 μJ, more preferably 8 μJ to 30 μJ, still more preferably 10 μJ to 30 μJ, and particularly preferably 20 μJ to 30 μJ. If the frequency and / or pulse energy of the laser light is within such range, the haze in the non-polarized portion can be reduced more stably.
[0059] In one embodiment, the pulse energy of the laser beam and the frequency of the laser beam satisfy the following formula (I). y=0.0524x 2 -2.7475x+48.325···(I) (In formula (I), y represents the frequency (KHz) of the laser light, and x represents the pulse energy (μJ) of the laser light.) When the pulse energy of the laser beam and the frequency of the laser beam satisfy the above formula (I), excellent absorbance can be imparted to the non-polarized portion, and haze in the non-polarized portion can be significantly reduced.
[0060] The processing speed of the laser light is, for example, 0.1 cm / s to 100.0 cm / s, preferably 1.0 cm / s to 50.0 cm / s, and more preferably 2.5 cm / s to 9.0 cm / s. The ratio of the frequency of the laser light to the processing speed of the laser light (frequency / processing speed) is, for example, 3-16, and preferably 4-8.
[0061] The laser light preferably contains polarized light that is approximately parallel to the absorption axis of the polarizing film 11. When the laser light contains such polarized light, a part of the polarizing film can be decolorized more smoothly, and a non-polarized portion can be efficiently formed.
[0062] When the bleaching step is carried out under such conditions, a non-polarized portion having an absorbance in the above range can be smoothly formed, and damage to the polarizing film itself can be suppressed. Therefore, the haze in the non-polarized portion can be reduced. Thus, a non-polarized portion having excellent light transmittance and reduced haze can be stably realized. In this manner, a polarizing film having a non-polarizing portion is manufactured. When a polarizing plate is subjected to the bleaching step, a polarizing plate having a non-polarizing portion is manufactured, and when an optical laminate is subjected to the bleaching step, an optical laminate having a non-polarizing portion is manufactured. EXAMPLES
[0063] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring the various properties are as follows.
[0064] (1) Thickness measurement The thickness of the polarizing films obtained in the examples and comparative examples was measured using a film tester thickness measuring device (HKT-1202, manufactured by Fujiwork Co., Ltd.).
[0065] (2) Measurement of absorbance and calculation of residual dye amount The absorbance at 470 nm, 560 nm, and 700 nm of the polarizing films (excluding the non-polarizing portion) and the non-polarizing portion obtained in the examples and comparative examples were measured using a spectrophotometer (product name: U-4100, manufactured by Hitachi High-Technologies Corporation). The absorbance of the non-polarizing portion is shown in Table 1. The content of the dichroic material in the non-polarized portion (amount of remaining dye) was calculated using the following formula (II). The results are shown in Table 1. Amount of dye remaining (mass%) = (absorbance of non-polarized part / absorbance of other than non-polarized part) × content of dichroic substance in the part of polarizing film other than the non-polarized part (mass%) (II)
[0066] (3) Haze value measurement The haze values of the non-polarizing portions of the polarizing films obtained in the examples and comparative examples were measured using a haze meter (product name: HM-150, Murakami Color Research Laboratory) in accordance with JIS K7136. The results are shown in Table 1.
[0067] (4) Polarization measurement The single transmittance (Ts: initial transmittance), parallel transmittance (Tp) and crossed transmittance (Tc) of the non-polarized portion of the polarizing film obtained in the examples and comparative examples were measured using a spectrophotometer (product name: U-4100, manufactured by Hitachi High-Tech Corporation). Furthermore, the degree of polarization (P) of the non-polarized portion was calculated using the following formula (III). The results are shown in Table 1. Degree of polarization (P)(%)={(Tp-Tc) / (Tp+Tc)}1 / 2×100··(III) The above Ts, Tp and Tc are Y values measured using a 2-degree visual field (C light source) according to JIS Z8701 and corrected for visibility.
[0068] (5) Humidity and heat durability test The L and a values of the non-polarizing parts of the polarizing films obtained in the Examples and Comparative Examples were measured before and after a wet heat durability test (85°C, 85% RH, 8h) using a spectrophotometer (product name "LPF-200", manufactured by Otsuka Electronics Co., Ltd.). The difference between the value before the test and the value after the test was calculated as ΔL and Δa. The results are shown in Table 2. In addition, the single transmittance (Ts) and polarization degree (P) of the non-polarizing parts of the polarizing films obtained in the Examples and Comparative Examples before and after a wet heat durability test (85°C, 85% RH for 8 h) were measured and calculated in the same manner as above, and the differences obtained by subtracting the values before the test from the values after the test were calculated as ΔY and ΔP. The results are shown in Table 2.
[0069] <<Production Example 1>> <Retardation film> Into a batch polymerization apparatus consisting of two vertical reactors equipped with stirring blades and reflux condensers controlled at 100°C, 29.60 parts by mass (0.046 mol) of bis[9-(2-phenoxycarbonylethyl)fluoren-9-yl]methane, 29.21 parts by mass (0.200 mol) of isosorbide (ISB), 42.28 parts by mass (0.139 mol) of spiroglycol (SPG), 63.77 parts by mass (0.298 mol) of diphenyl carbonate (DPC), and 1.19 × 10 calcium acetate monohydrate as a catalyst were added. -2 Part of mass (6.78×10 -5mol) was charged. After the inside of the reactor was purged with nitrogen under reduced pressure, heating was performed with a heat medium, and stirring was started when the inside temperature reached 100 ° C. 40 minutes after the start of the temperature increase, the inside temperature was reached 220 ° C., and while controlling to maintain this temperature, the pressure was reduced and 90 minutes after reaching 220 ° C., the pressure was reduced to 13.3 kPa. Phenol vapor by-produced with the polymerization reaction was led to a reflux condenser at 100 ° C., a small amount of monomer components contained in the phenol vapor were returned to the reactor, and the uncondensed phenol vapor was led to a condenser at 45 ° C. and recovered. Nitrogen was introduced into the first reactor to restore the pressure to atmospheric pressure, and the oligomerized reaction liquid in the first reactor was transferred to the second reactor. Next, the temperature increase and pressure reduction in the second reactor were started, and the inside temperature was set to 240 ° C. and the pressure to 0.2 kPa in 50 minutes. Thereafter, polymerization was allowed to proceed until the specified stirring power was reached. When the predetermined power was reached, nitrogen was introduced into the reactor to restore pressure, and the produced polyester carbonate resin was extruded into water and the strands were cut to obtain pellets. The obtained polyester carbonate resin (pellets) was vacuum-dried at 80°C for 5 hours, and then a long resin film was produced using a film-forming device equipped with a single-screw extruder (manufactured by Toshiba Machine Co., Ltd., cylinder setting temperature: 250°C), a T-die (width 200 mm, setting temperature: 250°C), a chill roll (setting temperature: 120-130°C) and a winder. The obtained long resin film was stretched longitudinally at the free end at 140°C to obtain a retardation film (positive A plate) with a thickness of 40 μm. The refractive index characteristics of the retardation film showed the relationship of nx>ny=nz.
[0070] <<Examples 1 to 7 and Comparative Examples 1 to 3>> A polyvinyl alcohol film (PVA resin film, manufactured by Kuraray Co., Ltd.) having a thickness of 30 μm was immersed in a dye bath at a liquid temperature of 30° C. for 30 seconds to be dyed (dyeing step). The dye bath was prepared by dissolving the dichroic substance shown in Table 1 in water. The concentration of the dichroic substance in the dye bath was 1.0 mass %. Next, the PVA-based resin film after the dyeing process was immersed in a crosslinking bath (a boric acid aqueous solution obtained by mixing 5 parts by mass of boric acid with 100 parts by mass of water) at a liquid temperature of 60°C for 300 seconds, while being uniaxially stretched to a total stretching ratio of 6.0 times the original length, and crosslinked with boric acid (stretching process). Next, the PVA-based resin film after the above-mentioned stretching step was immersed in a washing bath (water) at a liquid temperature of 20° C. (washing treatment). After that, the PVA resin film after the above-mentioned washing process was dried in an oven at 60°C for 4 minutes to obtain a polarizing film with a thickness of 13 μm. Next, a (meth)acrylic film (manufactured by Toyo Kohan Co., Ltd., RV20, thickness 20 μm) was attached as a protective layer to both sides of the obtained polarizing film via an ultraviolet-curable adhesive layer (thickness 1 μm). In this way, a polarizing plate having a protective layer / polarizing film configuration was obtained.
[0071] Next, the retardation film of Production Example 1 was attached to the surface of the polarizing film opposite to the protective layer via a (meth)acrylic adhesive layer (thickness: 5 μm). Then, a (meth)acrylic adhesive layer (thickness: 15 μm) was formed on the retardation film. As a result, an optical laminate having a structure of protective layer / polarizing film / (meth)acrylic pressure-sensitive adhesive layer / retardation film / (meth)acrylic pressure-sensitive adhesive layer was obtained.
[0072] Next, the obtained optical laminate was irradiated with green laser light from a solid-state pulse laser from the side of the polarizing film opposite to the protective layer under the conditions shown in Table 1. As a result, predetermined parts of the polarizing film were decolorized, and non-polarized parts were formed. In this manner, an optical laminate having a non-polarizing portion was obtained. The obtained optical laminate was subjected to the above-mentioned "(2) Measurement of absorbance and calculation of residual dye amount", "(3) Measurement of haze value", "(4) Measurement of polarization degree", and "(5) Humidity and heat durability test".
[0073] <<Comparative Example 4>> An optical laminate having a non-polarized portion was obtained in the same manner as in Example 1, except that the green laser light was changed to a UV laser light.
[0074] <<Comparative Example 5>> An optical laminate provided with a polarizing film including a non-polarizing portion was obtained in the same manner as in Example 1, except that the green laser light was changed to a CO2 laser light.
[0075] <<Comparative Example 6>> An optical laminate having a non-polarizing portion was obtained in the same manner as in Example 1, except that a 0.7% by mass iodine dyeing solution of iodine:potassium iodide (mass ratio = 1:7) was used as the dye bath, and the laser bleaching was changed to the following chemical bleaching. (chemical bleaching) A surface protective film having a through hole was attached to the surface of the polarizing film opposite to the protective layer to obtain a laminate having a configuration of protective layer / polarizing film / surface protective film. The laminate was then immersed in an aqueous NaOH solution (basic solution) to bring the polarizing film exposed from the through hole into contact with the basic solution. As a result, the portion of the polarizing film that was in contact with the basic solution was decolorized to form a non-polarizing portion. The surface protective film was then peeled off and removed from the polarizing film.
[0076] <<Comparative Example 7>> An optical laminate having a non-polarizing portion was obtained in the same manner as in Example 1, except that an iodine dyeing solution having a concentration of 0.7 mass % of iodine:potassium iodide (mass ratio = 1:7) was used as the dye bath.
[0077] [Table 1]
[0078] [Table 2]
[0079] [evaluation] As is clear from Tables 1 and 2, when a polarizing film contains a dichroic organic dye and is decolorized by irradiation with laser light under the above-mentioned conditions, it is possible to suppress recoloring and significantly reduce the absorbance of the non-polarized portion. It is also possible to reduce the absolute values of ΔL and Δa of the non-polarized portion before and after the moist heat test, and suppress recoloring of the non-polarized portion. [Industrial Applicability]
[0080] The polarizing film and polarizing plate of the present invention can be suitably used in image displays (typically, liquid crystal displays and organic EL displays). [Explanation of symbols]
[0081] 10 Polarizing plate 11 Polarizing film 12 Protective layer 100 Optical laminate
Claims
1. It is made of a resin film containing a dichroic organic dye, A polarizing film having a non-polarizing portion, the non-polarizing portion having an absorbance of 0.001 or more and 3.0 or less for light having wavelengths of 470 nm, 560 nm, and 700 nm, respectively.
2. The resin film contains a polyvinyl alcohol-based resin, 2. The polarizing film according to claim 1, wherein the dichroic organic dye comprises at least one selected from the group consisting of an azo dye represented by the following formula (1), a salt of the azo dye, a chelate of the azo dye, and a mixture thereof: [Formula 1] (In formula (1), X and Z each represent an atomic group shown in (2) to (13) below; Y represents an atomic group shown in (14) to (29) below; and m represents an integer of 0 to 6.) [Case 2] In the formulas (2) to (13), A is H, OH, OR 1 , S.O. 3 H, N.H. 2 , N.R. 2 , NO 2 , COOH, COOR, NHCOR, or a hydrocarbon group having 1 to 12 carbon atoms which may have a linear structure, a branched structure, a cyclic structure, a double bond, or a triple bond; R represents a hydrocarbon group having 1 to 12 carbon atoms which may have a linear structure, a branched structure, a cyclic structure, a double bond, or a triple bond; n represents an integer of 0 to 5; o represents an integer of 0 to 4; p represents an integer of 0 to 3; q represents an integer of 0 to 2; and r represents 0 or 1). [C3] (In formulas (14) to (29), A is H, OH, OR 1 , S.O. 3 H, N.H. 2 , N.R. 2 , NO 2, COOH, COOR, NHCOR, or a hydrocarbon group having 1 to 12 carbon atoms which may contain a branched structure, a cyclic structure, a double bond, or a triple bond; R, n, o, p, q, and r are the same as those in the above formulas (2) to (13).
3. 2. The polarizing film according to claim 1, wherein the content of the dichroic organic dye in the non-polarizing portion is 3.0% by mass or less, when the content of the dichroic organic dye in the polarizing film excluding the non-polarizing portion is taken as 100% by mass.
4. The polarizing film according to claim 1 , wherein the haze value in the non-polarizing portion is 5.0% or less.
5. 2. The polarizing film according to claim 1, wherein, before and after a moist heat test in which the polarizing film is left standing in an environment of 85° C. and 85% RH (relative humidity) for 8 hours, the absolute value of the change in single-phase hue L value of the Lab color system in the non-polarizing portion is 4.0 or less, or the absolute value of the change in single-phase hue a value of the Lab color system in the non-polarizing portion is 2.0 or less.
6. The polarizing film according to any one of claims 1 to 5, A polarizing plate comprising a protective layer provided on at least one surface of a polarizing film.
7. Dyeing the resin film with a dichroic organic dye; stretching the resin film dyed with the dichroic organic dye; and a step of irradiating a portion of the stretched resin film with laser light from a solid-state pulse laser to decolorize the portion, thereby forming a non-polarizing portion.
8. The wavelength of the laser light is 500 nm to 550 nm, 8. The method for producing a polarizing film according to claim 7, wherein the output of the solid-state pulsed laser is 0.5 W to 100 W.
Citation Information
Patent Citations
Polarizer and image display device
JP2014081482A