Film, package, and package with content

The film design with a rupture part and thermal printing section on opposite sides prevents water vapor from obscuring the print, maintaining readability and safety in microwave-heated packages.

JP2024146368APending Publication Date: 2024-10-15DAIWA CAN
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023059217
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

When a package is heated in a microwave oven, the internal pressure increases, causing water vapor to be ejected through a ruptured film, which can adhere to a thermal printing section and obscure the print.

Method used

A film with a rupture part and a thermal printing part on opposite symmetrical regions, ensuring the rupture part is positioned away from the thermal printing section to prevent water vapor adherence.

Benefits of technology

Prevents the thermal printing section from being colored by water vapor, maintaining print identifiability and ensuring safe handling after heating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146368000001_ABST
    Figure 2024146368000001_ABST
Patent Text Reader

Abstract

To provide a film which can prevent entry of a thermo-sensitive paint into the interior and can inhibit deterioration of discriminability of a thermal printing part, and to provide a package and a package with a content.SOLUTION: A film is used for a lid which is heat-sealed to a container body of a package which is heated by a microwave and includes: a breaking part which is provided at one of two areas being symmetric with respect to a center of an inner area of a seal part to be heat-sealed and which is broken by increase of an inner pressure; and a thermal printing part provided at the other area of the two areas and including a thermo-sensitive paint.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a film, a package, and a package containing a content, which release water vapor generated when the packaged content is heated in a microwave oven to the outside. [Background technology]

[0002] There have been known packages that contain contents and heat the contents in a microwave oven in a sealed state. However, when the contents are heated in a microwave oven, the internal pressure of such packages increases. For this reason, there are also known packages that are equipped with a means for automatically releasing water vapor and reducing the internal pressure during microwave heating.

[0003] For example, Patent Document 1 discloses a cup container and film that can release water vapor when heated in a microwave oven by providing a break section with non-oriented sections arranged opposite each other across an oriented section of a crystalline stretch-oriented film.

[0004] Furthermore, for example, Patent Document 2 discloses a cup container and a film that perform steaming without releasing excessive water vapor.

[0005] Also known is a technique for welding these films to a part of a flanged cup container or a pouch container. Also, as a packaging material, it has been considered to provide a thermal print part on the film that is printed by heat. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2019-64642 A [Patent Document 2] JP 2017-74965 A Summary of the Invention [Problem to be solved by the invention]

[0007] It is also possible to provide the above-mentioned packaging body with a thermally printed portion that is printed by heat. However, if the film breaks at the break portion and water vapor is emitted from the break portion and adheres to the thermally printed portion, the heat-sensitive layer may become colored, which may hinder the identification of the print on the thermally printed portion.

[0008] Therefore, an object of the present invention is to provide a film, a packaging material, and a packaging material containing contents that can suppress a decrease in the distinctiveness of a thermally printed portion. [Means for solving the problem]

[0009] According to one aspect of the present invention, the film is used for a lid that is heat-sealed to a container body of a packaging material to be heated in a microwave oven, and includes a breaking portion that is provided in one of two regions symmetrical about the center of the inner region of the heat-sealed seal portion and breaks due to an increase in internal pressure, and a thermal printed portion containing heat-sensitive paint that is provided in the other of the two regions. Effect of the Invention

[0010] According to the present invention, it is possible to provide a film, a package, and a package containing contents, which can suppress a decrease in the distinguishability of a thermally printed portion. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a perspective view showing a configuration of a packaging body according to an embodiment of the present invention. [Diagram 2] FIG. [Diagram 3] FIG. 3 is a cross-sectional view showing a schematic configuration of the packaging body. [Figure 4] FIG. 4 is a plan view showing a main configuration of a lid used in the packaging body. [Diagram 5] FIG. [Figure 6] FIG. 4 is an explanatory diagram showing an example of the configuration of the packaging body. [Figure 7] FIG. 4 is an explanatory diagram showing an example of the configuration of the packaging body. [Figure 8] FIG. 4 is an explanatory diagram showing an example of the configuration of the packaging body. [Figure 9] FIG. 4 is an explanatory diagram showing an example of the configuration of the packaging body. [Figure 10] FIG. 11 is an explanatory diagram showing another example of the configuration of the packaging body. [Figure 11] FIG. 4 is a cross-sectional view showing a schematic configuration of a lid of a packaging body of a comparative example. [Figure 12] FIG. 4 is an explanatory diagram showing an example of an evaluation test using the same packaging body. [Figure 13] FIG. [Figure 14] FIG. 11 is an explanatory diagram showing the results of the evaluation test using photographs of the working samples used in the evaluation test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] A packaging body 1 according to a first embodiment of the present invention will be described with reference to FIGS. FIG. 1 is a perspective view showing the configuration of a packaging body 1 according to an embodiment of the present invention, and FIG. 2 is a plan view showing the configuration of the packaging body 1. FIG. 3 is a cross-sectional view showing a schematic configuration of the packaging body 1. FIG. 4 is a plan view showing the configuration of the orientation relaxation portion 21a and the steam port 21c (breaking portion 13) of the lid 11 used in the packaging body 1. FIG. 5 is an explanatory diagram showing the configuration of the main portion from the orientation relaxation portion 21a and the steam port 21c of the lid 11. FIG. 6 is an explanatory diagram showing an example of an area E1 where the thermal printed portion 31 of the packaging body 1 is arranged, as an arrangement configuration of the breaking portion 13 and the thermal printed portion 31 of the packaging body 1, and FIG. 7 is an explanatory diagram showing an example of an area E2 where the thermal printed portion 31 of the packaging body 1 is arranged, as another example. Fig. 8 is an explanatory diagram showing an example of the region F1 where the break portion 13 of the packaging body 1 is arranged and the region F2 where the thermal printed portion 31 is arranged in a plan view, and Fig. 9 is an explanatory diagram showing an example of the region F1 where the break portion 13 of the packaging body 1 is arranged and the region F2 where the thermal printed portion 31 is arranged in a side view. Fig. 10 is an explanatory diagram showing an example of the region F1 where the break portion 13 of the packaging body 1 is arranged and the region F2 where the thermal printed portion 31 is arranged in a plan view, as another example. Fig. 11 is a cross-sectional view showing a schematic configuration of a lid 110 of a packaging body of a comparative example.

[0013] The packaging body 1 is a packaging container for packaging a content 100, which is configured by bonding two or more members by a means such as heat fusion (welding). The packaging body 1 is a content-containing packaging body in which the content 100 is accommodated and sealed. The packaging body 1 is a container for microwave heating that accommodates the content so that it can be heated in a microwave oven. The packaging body 1 is, for example, a container in which a film is welded as a lid 11 to a container body 10 such as a cup container or a tray container. In this embodiment, the packaging body 1 is a tray container formed by heat-welding two members, a tray container and a lid, and hereinafter, the packaging body 1 will be described as the tray container 1 and the container body 10 as the tray body 10.

[0014] The tray container 1 is a packaging container that is filled with and packaged with the contents 100. The tray container 1 is a container for microwave heating that accommodates the contents 100 so that the contents 100 can be heated in a microwave oven. As shown in Fig. 1, in this embodiment, the tray container 1 includes a rectangular cylindrical tray body 10 with a bottom, and a lid 11 that seals the tray body 10.

[0015] 1 to 3, the tray body 10 is made of a resin material, a paper material, or a composite material thereof. The tray body 10 includes a bottomed rectangular tubular body 10a and a flange 10b formed on the outer periphery of the opening of the body 10a. The tray body 10 may have a plurality of ribs that connect the outer periphery of the body 10a to the underside of the flange 10b.

[0016] The body 10a is in the form of a rectangular cylindrical tray, but may be in the form of a polygonal cylinder other than a rectangle, a cylinder, or a cup. The body 10a is formed to have a volume capable of accommodating a desired amount of contents 100 therein.

[0017] The flange 10b is formed in an annular flat plate shape extending in a direction perpendicular to the axial direction of the tray body 10 along the opening shape of the tray body 10. The flange 10b may be configured to be formed in an annular flat plate shape inclined in a direction perpendicular to the axial direction of the tray body 10 along the opening shape of the tray body 10. The flange 10b may be formed in an annular flat plate shape and have an annular protrusion protruding upward from the upper surface to seal the lid 11.

[0018] 1 to 4, the lid 11 is a laminated film having a base layer 21 on the outer surface side. The lid 11 is fixed by a seal portion 30 formed by heat sealing to the flange 10b of the tray body 10. The lid 11 may have a tab that can be pinched when peeling it off from the fixed flange 10b. The lid 11 also has a breakable portion 13 that forms a steam vent 21c through which steam can be discharged by breaking when the internal pressure of the tray container 1 increases, and a printed portion 14 that displays information on the contents, product, etc.

[0019] Here, the contents 100 refer to food to be cooked in a microwave oven, hand towels to be heated in a microwave oven, and other items that contain moisture to be heated in a microwave oven. The information on the contents and goods (products) displayed by the printing unit 14 may include at least any of the following: various indications on the contents such as the names of raw materials, the place of origin of raw materials, allergies and additives, nutritional components, and content volume; information on the product such as a barcode, product name, price, manufacturer's unique code, recycle mark, and care mark; and information on product identification such as the name of the sales / manufacturing company, design, and mark.

[0020] The outer shape of the lid 11 is formed to be the same as the outer peripheral shape of the flange 10b or to be substantially the same shape but slightly larger than the outer peripheral shape of the flange 10b. Also, the tab may be formed, for example, substantially triangular or semicircular so as to protrude outward so as to be pinched by fingers.

[0021] The lid (film) 11 includes, from the outer surface side of the tray container 1 when the tray container 1 is formed, a base material layer 21 which is an oriented film, an adhesive layer 22, a sealant layer 23 which is a sealant film, and an anti-fogging layer 24. The lid 11 also has a printed portion 14 on which product information is provided on the outer surface of the base material layer 21 or between the base material layer 21 and the sealant layer 23. The layer structure of the lid 11 is not limited to this, and may be two or more layers, with at least one layer having the base material layer 21 and a portion having a break portion 13 and a printed portion 14.

[0022] The base material layer 21 includes an orientation relaxation portion 21a formed by heating a portion of the base material layer 21 to a predetermined temperature or higher near the melting point through explosion-proof processing. The orientation relaxation portion 21a constitutes a part of the breaking portion 13. The orientation relaxation portion 21a can be formed into various shapes depending on the configuration of the breaking portion 13.

[0023] The substrate layer 21 is a crystalline stretch-oriented film whose molecules are oriented by biaxial stretching. The substrate layer 21 is composed of a general-purpose biaxially stretched film such as a biaxially stretched PET film, a biaxially stretched nylon film, or a biaxially stretched PP film, or a composite film thereof. Other suitable examples of the substrate layer 21 include biaxially stretched films having barrier properties such as a biaxially stretched PVA film or a biaxially stretched EVOH film, and co-extruded biaxially stretched films having barrier resins such as PET / NY, PP / EVOH / PP, NY / EVOH / NY, or NY / MXD-NY / NY in the intermediate layer. In addition, a film in which a general-purpose biaxially stretched film is coated with a barrier resin of a PVA system, PVDC, or PAA system, or a hybrid coat film in which an inorganic substance is dispersed in the barrier resin described above can also be suitably used for the substrate layer 21. The thickness of the substrate layer 21 is preferably 12 μm or more and 50 μm or less.

[0024] This is because if the thickness of the base material layer 21 is less than 12 μm, the physical strength of the tray container 1 may decrease, and film formation is technically difficult, resulting in increased costs. Also, if the thickness of the base material layer 21 exceeds 50 μm, the lid 11 including the base material layer 21 becomes difficult to extend. However, the thickness of the base material layer 21 is not limited as long as the breaking portion 13 is broken due to the shape of the orientation relaxation portion 21a or the like.

[0025] The orientation relaxation portion 21a is formed by heating the base material layer 21 to a predetermined temperature or higher near the melting point to relax the orientation or to eliminate the orientation. That is, the base material layer 21 of the lid 11 has the orientation relaxation portion 21a heated to a predetermined temperature or higher near the melting point in a part of the orientation portion 21b having the orientation that is not heated to a predetermined temperature or higher near the melting point. Note that the predetermined temperature near the melting point differs depending on the base material layer 21, but is at least a temperature at which the orientation is relaxed and the tensile modulus and breaking elongation of the orientation relaxation portion 21a and the orientation portion 21b can have a desired relationship. That is, the orientation relaxation portion 21a is formed by amorphizing a part of the base material layer 21.

[0026] The method of heating the base layer 21 for forming the orientation relaxing portions 21a in the base layer 21 preferably uses laser beam heating, hot plate heating, impulse heating, near infrared heating, or the like.

[0027] For example, laser beam heating and near-infrared heating have the advantage of being able to heat the base layer 21 without contact, but laser beam heating is preferred because it is possible to locally heat the base layer 21. In addition, when the base layer 21 used has poor laser beam absorption and it is difficult to form the orientation relaxation portion 21a, a laser beam absorbing material that improves the laser beam absorption of the base layer 21 may be blended in advance into the material of the base layer 21, or the base layer 21 may be coated with a laser beam absorbing material.

[0028] As for the type of laser light, it is preferable to use a carbon dioxide gas laser, which has relatively high absorption properties for many of the resin materials used in the base layer 21. The laser light absorbing material can be appropriately selected depending on the type of laser light. These heating methods can be appropriately selected depending on the material of the base layer 21 to be used, etc.

[0029] In the case of hot plate heating or impulse heating, it is preferable to perform a treatment such as Teflon (registered trademark) surface treatment on the pressing head portion so that the pressing head portion is not contaminated with a part of the molten resin of the base material layer 21 or the resin of the sealant layer 23. For example, in the case of hot plate heating, the pressing head (hot plate) that is set to a temperature equal to or higher than a predetermined temperature near the melting point of the base material layer 21 is pressed against the base material layer 21 to melt and heat it, thereby forming the orientation relaxation portion 21a.

[0030] Moreover, whether or not the orientation relaxation portion 21a is properly formed can be determined by inspecting the formed base material layer 21. As the inspection method, X-ray diffraction, FT-IR (Fourier transform infrared spectroscopy), DSC (differential scanning calorimetry), or other crystallinity measurement, an orientation viewer using a polarizing plate, or the like can be used.

[0031] In such a base layer 21, for example, the breaking elongation of the orientation portion 21b is set to 200% or less, and the breaking elongation of the orientation relaxed portion 21a is set to 300% or more.

[0032] The adhesive layer 22 can be appropriately selected from general dry lamination adhesives for food applications. However, since the tray container 1 is used for heating in a microwave oven, it is preferable that the adhesive layer 22 has heat resistance. The thickness of the adhesive layer 22 is preferably 2 μm to 5 μm from the viewpoints of performance and economy.

[0033] The sealant layer 23 is composed of, for example, an unstretched low density polyethylene (LDPE) film, an unstretched linear low density polyethylene (LLDPE) film, an unstretched polypropylene (PP) film, an unstretched polyethylene terephthalate film, etc. The thickness of the sealant layer 23 is preferably 10 μm or more and 100 μm or less. The thickness of the sealant layer 23 is more preferably 20 μm or more and 60 μm or less.

[0034] This is because if the thickness of the sealant layer 23 is less than 10 μm, the practical strength of the package 1 may be insufficient, and the seal portion 30 may be easily broken by vibration during transportation or the impact of being dropped. Also, if the thickness of the sealant layer 23 exceeds 100 μm, it becomes difficult to stretch, which may cause problems with the reliability of steam release.

[0035] The anti-fogging layer 24 is formed so as to be capable of preventing fogging on the inner surface of the lid 11. For example, the anti-fogging layer 24 is formed of a material having hygroscopic properties. The anti-fogging layer 24 is preferably 10 μm or less, for example. The lid 11 may be configured such that an anti-fogging material is kneaded into the sealant layer 23 without having the anti-fogging layer 24. In addition, in the case of a product in which fogging on the inner surface of the lid 11 due to temperature and humidity is acceptable, the lid 11 does not need to have anti-fogging properties.

[0036] The break portion 13 is formed by the oriented portion 21b at a portion disposed between the opposing orientation relaxation portions 21a. That is, the break portion 13 is provided in a portion of the lid 11, extends in a linear shape such as a straight line or a curve, and is constituted by a single orientation relaxation portion 21a that is disposed in a shape in which two portions of the break portion 13 face each other with a predetermined interval therebetween, or by a plurality of orientation relaxation portions 21a that are disposed opposite each other, so that the break portion 13 is constituted by the orientation relaxation portions 21b that are disposed opposite each other, with the orientation relaxation portions 21b that are not heated to a predetermined temperature or higher near the melting point of the base layer 21, in other words, with the orientation portions 21b of the base layer 21 that have orientation interposed therebetween. As a specific example, the orientation relaxation portion 21a has a short side and a long side, and one or more orientation relaxation portions 21a are provided.

[0037] When one orientation relaxation portion 21a is provided, the orientation relaxation portion 21a faces its own short sides with a predetermined gap therebetween, or its own short side and long side face each other with a predetermined gap therebetween. The shape of one orientation relaxation portion 21a may be a partially cut-out circular ring or polygonal ring, or the like.

[0038] When two orientation relaxation sections 21a are provided, the short sides or long sides of the two orientation relaxation sections 21a face each other with a predetermined gap between them, or the short side of one orientation relaxation section 21a faces the long side of the other orientation relaxation section 21a with a predetermined gap between them. The two orientation relaxation sections 21a may be, for example, linearly configured, with the short sides facing each other so as to intersect linearly or at a predetermined angle, or with the short sides facing each other in a T-shape. The two orientation relaxation sections 21a may also be wavy or otherwise configured in addition to being linear.

[0039] When three or more orientation relaxation parts 21a are provided, any two orientation relaxation parts 21a or three or more orientation relaxation parts 21a face each other with their short sides or their short sides and long sides facing each other with a predetermined interval. When multiple orientation relaxation parts 21a are provided in the breaking part 13, it is preferable that the orientation relaxation parts 21a have the same size and shape, but they may have different sizes and shapes as long as the breaking part 13 is configured to break. As for three or more orientation relaxation parts 21a, as shown in FIG. 2, a configuration in which the longitudinal direction is aligned in one direction or a configuration in which the orientation relaxation parts 21a are aligned in the circumferential direction around the breaking part 13 may be considered.

[0040] Such a broken portion 13 is formed by one or more orientation relaxation portions 21a, which are amorphized by heating the base layer 21, being spaced apart by a predetermined distance from each other and sandwiching an orientation portion 21b having the orientation of the base layer 21. Here, the predetermined distance can be set appropriately as long as the breaking portion 13 can break and form a steam port 21c when heated in a microwave oven, but is preferably less than 5 mm. In addition, the long side and the short side are not limited to being linear, and may be curved. That is, the breaking portion 13 is configured in a shape in which the orientation relaxation portion 21a extends in any direction, and one end of one orientation relaxation portion 21a faces another portion of the same orientation relaxation portion 21a or a part of another orientation relaxation portion 21a at a predetermined distance. Note that, as long as the breaking portion 13 can break and form a steam port 21c, a part of the orientation portion 21b sandwiched between the opposing orientation relaxation portions 21a may be orientation-relaxed.

[0041] 1 to 10, the break portion 13 has three orientation relaxing portions 21a. The three orientation relaxing portions 21a are linearly arranged at predetermined intervals.

[0042] In consideration of manufacturing costs, the orientation relaxation section 21a is preferably formed in a rectangular shape that is long in one direction and has short sides that face each other, as shown in Fig. 2. The orientation relaxation section 21a shown in Fig. 2 has a short side length of 0.5 to 10 mm and a long side length of 3 to 100 mm, and the length of the short side is preferably set to a range shorter than the length of the long side, and is appropriately selected depending on the size of the tray container 1 and the configuration of the lid 11. The distance between the opposing short sides of the two orientation relaxation sections 21a is set to less than 5 mm, and more preferably to 0.5 to 3.0 mm, and is appropriately selected depending on the size of the tray container 1 and the configuration of the lid 11.

[0043] This is because, if the dimensions of the orientation relaxation portions 21a are less than this range, the range of extension is too narrow and steam release may not be performed well, and if the dimensions exceed this range, the strength of the lid 11 and the gas barrier properties may be significantly reduced. Also, if the distance between the opposing short sides of the two orientation relaxation portions 21a is less than this range, the tips of the opposing orientation relaxation portions 21a may become integrated with each other, and the steam port 21c may not be formed at the rupture portion 13, resulting in rupture. Also, if the distance between the opposing short sides of the two orientation relaxation portions 21a exceeds this range, the region between the opposing short sides of the two orientation relaxation portions 21a cannot extend, so the rupture portion 13 does not rupture, and the tray container 1 may not be able to form the steam port 21c and may rupture.

[0044] The printing unit 14 has at least a thermal printing unit 31. In this embodiment, the printing unit 14 has the thermal printing unit 31 and a normal printing unit 32.

[0045] The thermal print part 31 is formed, for example, on the outer surface of the base layer 21 of the lid 11. The thermal print part 31 is provided in one or more regions of the lid 11. The thermal print part 31 includes a thermosensitive layer 41 and a protective layer 42 that covers the thermosensitive layer 41. The thermal print part 31 is formed so that it can be printed in black when the thermosensitive layer 41 is heated. The thermosensitive layer 41 includes a thermosensitive paint. The thermosensitive layer 41 is formed by applying the thermosensitive paint to a predetermined region of the outer surface of the base layer 21. The protective layer 42 protects the thermosensitive layer 41. In addition, the protective layer 42 is colored so that it can improve the visibility of the print on the thermosensitive layer 41 and the visibility of the black print, and has transparency that allows the inside of the package 1 to be visible. For example, the protective layer 42 is formed in a translucent white color. The protective layer 42 may be formed colorless and transparent, and the region of the base material layer 21 where the thermal printed portion 31 is provided may be formed colored and semi-transparent to improve the visibility of the printing on the thermosensitive layer 41. The thermal printed portion 31 is formed on the lid 11, separated from the breaking portion 13 and the sealing portion 30. For example, the thermal printed portion 31 has ingredients and a barcode printed thereon.

[0046] The normal printed portion 32 is formed, for example, on the inner surface of the base material layer 21 of the lid 11 facing the sealant layer 23, and is covered with the adhesive layer 22. The normal printed portion 32 is provided in one or more areas of the lid 11. For example, the normal printed portion 32 is printed with paint. The normal printed portion 32 is, for example, multi-color printed. Hereinafter, the normal printed portion 32 is, for example, gravure printed. Hereinafter, the normal printed portion 32 will be described as the gravure printed portion 32. The gravure printed portion 32 is formed on the lid 11, separated from the breaking portion 13. For example, the product name, sales company, price, recycle mark, care mark, etc. are printed on the gravure printed portion 32.

[0047] The seal portion 30 formed by heat-sealing the lid 11 to the flange 10b is formed in a ring shape along the flange 10b. The width of the seal portion 30 is the same as or smaller than the width of the flange 10b. The seal strength of the seal portion 30 to the flange 10b of the lid 11 is higher than the opening strength at which the breaking portion 13 breaks due to an increase in the internal pressure of the tray container 1. Here, the seal strength and opening strength are, for example, strengths after heating when the internal pressure increases and the lid 11 expands, i.e., when the contents are heated in a microwave oven.

[0048] Next, the configurations of the breakage portion 13, the print portion 14, and the seal portion 30 of the package 1 will be described with reference to Figs. 5 to 10. In the example of Fig. 5, the orientation relaxation portion 21a constituting the breakage portion 13 of the lid 11 is laser processed to form three orientation relaxation portions 21a, and two breakage portions 13 (steam ports 21c) are formed between adjacent orientation relaxation portions 21a. In addition, an example will be described in which the width W1 of the laser processed portion (orientation relaxation portion 21a) is 1 mm, and the length L1 from the end of the orientation relaxation portion 21a provided at one end side in the longitudinal direction to the end of the orientation relaxation portion 21a provided at the other end side among the three orientation relaxation portions 21a is 47 mm. In Fig. 5, the varnish avoidance of the laser processing, that is, the region G of the laser processed portion (orientation relaxation portion 21a) misaligned in the laser processing is shown by a two-dot chain line. In addition, in the fracture portion 13 having a width W1=1 mm and a length L1=47 mm, the width W2 of the laser processing varnish avoidance (shift range G) is 6 mm, and the length L2 of the laser processing varnish avoidance is 57 mm.

[0049] The breaking portion 13 is disposed at a position offset from at least the thermosensitive layer 41 of the thermal printed portion 31 of the lid 11. Preferably, the breaking portion 13 is disposed at a position offset from the thermosensitive layer 41 and the protective layer 42 of the thermal printed portion 31 of the lid 11. Also, for example, the breaking portion 13 is disposed at a position offset from the gravure printed portion 32.

[0050] 5, the break portion 13 is spaced from the thermal printed portion 31 by a distance equal to or greater than the radius R1 of the circle C1 when the break portion 13 is centered at the location where the steam port 21c is formed (the break portion 13). Here, the radius R1 of the circle C1 is, for example, 15 mm.

[0051] More preferably, as shown by a circle C2 indicated by a two-dot chain line in Fig. 5, the breaking portion 13 is spaced from the thermal printed portion 31 by a distance equal to or greater than the radius R2 of the circle C2 when the center is the portion where the steam port 21c is formed. Here, the radius R2 of the circle C2 is, for example, 40 mm.

[0052] This is because the water vapor ejected from the steam port 21c is likely to adhere within a radius of 15 mm from the steam port 21c, causing stains (black coloring) on ​​the thermal printed portion 31 and making it difficult to distinguish the print. Also, the water vapor ejected from the steam port 21c may adhere even within a radius of less than 40 mm from the steam port 21c.

[0053] The circles C1 and C2 were determined using the following package 1. A 143 mm square deli tray was used as the tray body 10, and a cover 11 was used with a protective layer 42 (1.2 g / m2) / thermosensitive layer 41 (3.7 g / m2) / HBN (base layer 21) (15 μm) / adhesive layer 22 / TE-100 (sealant layer 23) (30 μm). The sealing conditions of the seal part 30 of the tray body 10 and the cover 11 were 165°C x 0.4 MPa x 2 seconds, and an AL mask was used for insulation. The contents 100 contained 100 g of water. The circles C1 and C2 were determined based on the scattering state of water vapor 200 when such a package 1 (package containing contents) was heated in a 600 W microwave oven for 2 minutes.

[0054] For this reason, as shown in area D indicated by the dotted line in Figures 5 to 7, the thermal printing portion 31 is not provided in the area of ​​96 mm x 80 mm centered on the breaking portion 13, but is provided at a position outside of area D.

[0055] As a preferred example, as shown in Fig. 8 and Fig. 9, of two symmetrical regions F1 and F2 that are line-symmetrical with respect to a center line S that passes through the center of the inner region of the seal portion 30 of the lid 11 (the center of the tray body 10 in a plan view), it is preferable to provide at least a portion of the break portion 13 where the steam port 21c is formed in one symmetrical region F1, and provide at least the heat-sensitive layer 41 of the thermal printed portion 31 in the other symmetrical region F2. More specifically, as shown in Fig. 8 and Fig. 9, of two symmetrical regions F1 and F2 that are line-symmetrical with respect to a center line S that passes through the center of the tray body 10, it is more preferable to provide the break portion 13 in one symmetrical region F1, and provide the heat-sensitive layer 41 and the protective layer 42 of the thermal printed portion 31 in the other symmetrical region F2. That is, it is preferable that the break portion 13 is provided in the region F1, and the thermal printed portion 31 is provided in the region E2 and in the symmetrical region F2.

[0056] The gravure printing unit 32 may be provided in either one of the two symmetrical areas F1 and F2.

[0057] Here, the center line S may be a center line S1 passing through the center of the region inside the seal portion 30 of the lid 11 in a plan view and the center of two predetermined sides of the flange 10b, as shown in Figs. 8 and 9, as long as it is on the center of the region inside the seal portion 30 of the lid 11 in a plan view (the center of the tray body 10). Also, the center line S may be a center line S2 passing through the center of the region inside the seal portion 30 of the lid 11 in a plan view and two corners of the flange 10b, as shown in Fig. 10. Also, the two symmetrical regions F1 and F2 are not limited to symmetrical regions with respect to the center line S, but may be symmetrical regions with point symmetry about the center of the tray body 10. Also, when the tray body 10 is not a square rectangular cylinder, but a circular, rectangular, polygonal or irregular cylinder, it is not necessarily limited to linearly symmetrical regions.

[0058] That is, the lid 11 is provided with a breaking portion 13 and a thermal printed portion 31 in each of two regions F1, F2 on either side of the center of the tray body 10 within the sealing portion 30, and the thermal printed portion 31 is preferably formed in an area that is a predetermined distance from the breaking portion 13 of the lid 11, preferably 15 mm or more, more preferably 40 mm or more, and even more preferably 50 mm or more away from the portion where the steam port 21c is formed. Also, it is sufficient that the breaking portion 13 and the thermal printed portion 31 are provided in a part of each of the regions F1, F2.

[0059] With the packaging body 1 configured in this manner, the lid 11 is such that the location of the steam vent 21c formed in the breaking portion 13 is offset from the thermal printed portion 31, so that when the breaking portion 13 breaks and is formed from the steam vent 21c, discoloration of the thermal printed portion 31 due to water vapor ejected from the steam vent 21c can be prevented.

[0060] Moreover, the heat-sensitive paint used in the heat-sensitive layer 41 of the thermal print section 31 is generally a water-based paint, and there is a possibility that the paint will dissolve due to the water vapor 200. As in the lid 110 of the comparative example shown in Fig. 11, when the steam port 21c (breaking portion 13) is disposed at a position facing the heat-sensitive layer 41 in the thickness direction of the film, there is a risk that the water vapor 200 ejected to the outside from the steam port 21c will come into contact with the heat-sensitive layer 41. When the water vapor 200 comes into contact with the heat-sensitive paint of the heat-sensitive layer 41, the heat-sensitive paint of the heat-sensitive layer 41 will melt due to the water vapor 200, and there is a risk that water droplets generated by the water vapor 200 that has dissolved the heat-sensitive paint will enter the package 1 via the steam port 21c. However, in the lid 11 of the present embodiment, the steam vent 21c generated at the rupture portion 13 is positioned away from at least the heat-sensitive layer 41 of the thermal print portion 31, thereby preventing direct contact between the paint on the heat-sensitive layer 41 and the steam.

[0061] Furthermore, by setting the distance from the steam vent 21c to the thermal printed part 31 to 15 mm or more, preferably 40 mm or more, and more preferably 50 mm or more, it is possible to suppress discoloration of the thermal printed part 31 caused by water droplets contained in the steam ejected from the steam vent 21c adhering to the thermal printed part 31. Therefore, it is possible to prevent impairment of the identity of the information displayed on the thermal printed part 31 even after heating.

[0062] Furthermore, by positioning the gravure printed portion 32 away from the portion of the rupture portion 13 where the steam port 21c is formed, paint chips from the gravure printed portion 32 can be prevented from entering the package 1 through the steam port 21c.

[0063] Furthermore, by providing the breaking portion 13 and the thermal print portion 31 in two regions F1 and F2 on either side of the center line in the region within the seal portion 30 of the lid 11, the breaking portion 13 is disposed in the region F1 on one side of the lid 11. Therefore, even if the breaking portion 13 breaks and steam 200 jets out from the steam port 21c as shown in Figures 8 to 10, the steam 200 can be prevented from adhering to the region F2 opposite the region F1 where the breaking portion 13 is provided. Furthermore, as shown in Figure 9, since the breaking portion 13 is provided at a position shifted from the center that is the highest when the lid 11 expands, the steam 200 jetting out from the steam port 21c created by the breaking of the breaking portion 13 will be directed outward.

[0064] Therefore, in the region F2, the thermal print portion 31 can be prevented from being colored by the steam 200. In addition, in the region F2 where the rupture portion 13 is not provided, the steam 200 emitted from the steam port 21c can be prevented from coming into contact with the region F2. Therefore, when carrying the tray container 1 after cooking, the tray container 1 can be safely carried by grasping the flange 10b adjacent to the region F2. For example, the packaging body 1 can be provided with an area on the flange 10b for a handle that can be held after heating, and by providing this handle at least in the region F2, the packaging body 1 after heating can be more safely held.

[0065] Next, an evaluation test of the packaging body 1 according to this embodiment and the results of the evaluation test will be described with reference to Fig. 12 to Fig. 14. Fig. 12 is an explanatory diagram showing an example of Examples 1 to 3 of the packaging body 1 used in the evaluation test, Fig. 13 is an explanatory diagram showing the results of the evaluation test, and Fig. 14 is an explanatory diagram showing the evaluation test results using photographs of working samples used in the evaluation test.

[0066] [Evaluation test] As an evaluation test, samples were prepared for each of the packages 1 of Examples 1 to 3 below, with the rupture portion 13 positioned at two different locations, and heated at 600 W for 2 minutes and at 1600 W for 1 minute, and the maximum distance from the steam port 21c of the colored stain and the maximum distance of the circular mark caused by the steam 200 sprayed from the steam port 21c resulting from the rupture of the rupture portion 13 were measured. A Sharp RE-TS3 was used as the 600 W microwave oven, and a National NE-1800 was used as the 1600 W microwave oven.

[0067] [Package of Example 1] The packaging body 1 of Example 1 uses a square tray body 10 with a flange made of a microwaveable resin and having a side of 143 mm, and a lid body 11 formed of a protective layer 42 (1.2 g / m2) / thermosensitive layer 41 (3.7 g / m2) / HBN (base material layer 21) (15 μm) / adhesive layer 22 / TE-100 (sealant layer 23) (30 μm). For the thermosensitive layer, a non-phenolic thermosensitive paint manufactured by Nippon Paper Industries Co., Ltd. that starts to develop color at 100°C or higher was used. The sealing conditions of the seal part 30 of the tray body 10 and the lid body 11 were 165°C x 0.4 MPa x 2 seconds, and an AL mask was used for insulation to eliminate the effect of coloring due to radiant heat from the seal head. The distance (seal inner length) from the innermost side (seal edge inner side) of one side of the seal part 30 to the inner side of the seal edge of the opposite side was 130 mm. In addition, 100 g of water was contained in the package 1 as the contents 100. The orientation relaxation portion 21a constituting the breaking portion 13 of the lid 11 was processed by laser processing to form three orientation relaxation portions 21a. The three orientation relaxation portions 21a were formed in a direction substantially parallel to a predetermined side of the seal portion. The width of the laser processed portion (orientation relaxation portion 21a) was 1 mm, and the length L1 from the end of one orientation relaxation portion of the breaking portion to the end of the orientation relaxation portion provided on the other end side was 47 mm. In addition, the position of the breaking portion 13 in the opposing direction (hereinafter, the first direction) of one pair of two sides of the tray main body 10 facing each other was formed to be approximately the center of the lid 11.

[0068] In addition, as the packaging body 1 of Example 1, as shown in Figure 12, two samples were created, each of which had the breaking portion 13 positioned at a position (approximately 43 mm) shifted from one side of the lid body 11 that is approximately parallel to the breaking portion 13 toward the central position in a second direction (the opposing direction of the other pair of opposing sides of the tray body 10) perpendicular to the first direction by approximately 1 / 3 of the inner length of the seal (hereinafter referred to as the "1 / 3 position") and one of which had the breaking portion 13 positioned at a position (approximately 32 mm) shifted from one side of the lid body 11 that is approximately parallel to the breaking portion 13 toward the central position by approximately 1 / 4 of the inner length of the seal (hereinafter referred to as the "1 / 4 position").

[0069] [Package of Example 2] The package 1 of Example 2 uses a rectangular tray body 10 with a long side of 148 mm and a short side of 98 mm, made of a resin flange and heatable in a microwave oven, and the lid body 11 is made of the same material as the lid body 11 of Example 1. The lid body 11 is formed with a breaking portion 13 having the same shape as the breaking portion 13 of Example 1. The inner seal length in the long side direction (second direction) of the tray body 10 and the lid body 11 is 135 mm. The breaking portion 13 is formed to extend approximately parallel to the short side. As the packaging body 1 of Example 2, two samples were created, one in which the position of the breaking portion 13 was shifted from the short side toward the central position by approximately 1 / 3 of the inner length of the seal in the second direction (longitudinal direction) (1 / 3 position, approximately 45 mm position), and the other in which the position was shifted from the short side toward the central position by approximately 1 / 4 of the inner length of the seal in the second direction (longitudinal direction) (1 / 4 position, approximately 33.8 mm position), as shown in Figure 12.

[0070] [Example 3] The package 1 of Example 3 used a circular microwaveable resin cup container with a flange, a so-called round cup with an opening diameter of 115 mm, as the tray body 11. The lid 11 was made of the same material as the lids 11 of Examples 1 and 2. The lid 11 had a breaking portion 13 formed in the same shape as the breaking portion 13 of Examples 1 and 2. The inner radial seal length of the tray body 10 and the lid 11 was 85 mm. The breaking portion 13 was formed to extend approximately parallel to the radial direction. As the packaging body 1 of Example 3, two samples were created, one in which the position of the breaking portion 13 was shifted radially from a point on the inner circumference of the opening toward the central position by approximately 1 / 3 of the inner length of the seal (1 / 3 position, approximately 28 mm position), and the other in which the position was shifted from a point on the inner circumference of the opening toward the central position by approximately 1 / 4 of the inner length of the seal from the short side (1 / 4 position, approximately 21 mm position), as shown in Figure 12.

[0071] [Evaluation test results] As shown in Fig. 13, the maximum distance from the steam port 21c of the colored stain caused by the steam 200 injected from the steam port 21c was the largest when the sample in Example 1 having the broken portion 13 at the 1 / 4 position was heated in a 1600 W microwave oven, and the distance from the steam port 21c was 15 mm. The maximum distance of the circular mark was 40 mm when the sample in Example 1 having the broken portion at the 1 / 4 position was heated in a 1600 W microwave oven. Fig. 14 shows examples of the scattering of the injected steam 200, the coloring of the thermosensitive layer 41 caused by the steam 200, and the circular mark that were generated in the sample.

[0072] Therefore, by providing the heat-sensitive layer 41 of the thermal printed portion 31 at a position 15 mm or more away from the steam vent 21c (rupture portion 13), it is possible to prevent the occurrence of food stains caused by water vapor ejected from the steam vent 21c or water droplets generated by the water vapor. This makes it possible for the package 1 to prevent the heat-sensitive layer 41 of the thermal printed portion 31 from becoming discolored and hindering the identification of the characters and other printing printed on the thermal printed portion 31. Also, by providing the heat-sensitive layer 41 at a position 40 mm or more away from the steam vent 21c, it is possible to prevent the coloring of the heat-sensitive layer due to a circular mark from hindering the identification of the printing on the thermal printed portion 31.

[0073] As described above, the packaging body 1 according to one embodiment of the present invention can prevent the heat-sensitive paint from entering the contents and can suppress discoloration of the thermal printed portion 31 due to the water vapor 200 sprayed from the steam port 21c of the rupture portion 13.

[0074] The present invention is not limited to the above-mentioned embodiment. For example, in the above-mentioned example, the package 1 has the thermal printed part 31 and the gravure printed part 32 as the normal printed part 32 as the printed part 14, but the package 1 may have only the thermal printed part 31, and the normal printed part 32 may be printed by a method other than gravure printing. The normal printed part 32 may be provided on the outer surface of the base layer 21, instead of on the surface of the base layer 21 facing the sealant layer 23.

[0075] The thermal printed section 31 and the normal printed section 32 may be provided on the same main surface of the base material layer 21 or on different main surfaces of the base material layer 21 in regions that overlap in the surface direction of the lid 11. That is, the lid 11 may be configured so that the normal printed section 32 is provided overlapping a portion of the thermal printed section 31, or the thermal printed section 31 is provided overlapping a portion of the normal printed section 32.

[0076] That is, the present invention is not limited to the above-mentioned embodiment, and various modifications can be made in the implementation stage without departing from the gist of the invention. In addition, the embodiments may be implemented in appropriate combination, and in that case, the combined effect can be obtained. Furthermore, the above-mentioned embodiment includes various inventions, and various inventions can be extracted by combinations selected from the multiple components disclosed. For example, if the problem can be solved and the effect can be obtained even if some components are deleted from all the components shown in the embodiment, the configuration from which the components are deleted can be extracted as an invention. [Explanation of symbols]

[0077] DESCRIPTION OF THE PREFERRED EMBODIMENTS 1...packaging body (tray container), 10...tray body (container body), 10a...body portion, 10b...flange, 11...lid (film), 13...breaking portion, 14...printed portion, 21...base material layer, 21a...orientation relaxation portion, 21b...orientation portion, 21c...steam vent, 22...adhesive layer, 23...sealant layer, 24...anti-fogging layer, 30...sealing portion, 31...thermal printing portion, 32...gravure printing portion (normal printing portion), 41...thermosensitive layer, 42...protective layer, 100...contents, 200...water vapor.

Claims

1. A film used for a lid that is heat-sealed to a container body of a package that is heated by a microwave oven, a breaking portion provided in one of two regions symmetrical with respect to the center of the inner region of the heat-sealed seal portion, the breaking portion breaking due to an increase in internal pressure; a thermal printing portion including a heat-sensitive paint, the thermal printing portion being provided in the other of the two regions; A film comprising:

2. A molecularly oriented substrate layer is included, The film according to claim 1 , wherein the break portion is formed by one or more orientation relaxation portions formed in the base layer facing each other with a predetermined gap therebetween.

3. The film of claim 1 , further comprising a gravure printing section offset from the breaks.

4. the thermal printing unit has a heat-sensitive layer including the heat-sensitive paint, The film of claim 1 , wherein the heat sensitive layer is spaced at a radius of 15 mm or more from the center of the break.

5. The film of claim 4 , wherein the heat-sensitive layer is spaced from the center of the break by a radius of 40 mm or more.

6. A lid formed from the film according to any one of claims 1 to 5; a container body having a flange to which the lid is heat-sealed; A packaging body comprising:

7. A packaging body according to claim 6; Contents contained in the package; and A package containing a content.

Citation Information

Patent Citations

  • Laminated film and packaging container

    JP2017074965A

  • Package and film

    JP2019064642A