Ceramic electronic component and method of manufacturing ceramic electronic component
The ceramic electronic component addresses color variation issues by using a controlled concentration gradient of subcomponents in the side margin and cover layer, ensuring electrical characteristics are maintained and visual defects are minimized.
Patent Information
- Application Number
- JP2023059323
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Ceramic electronic components like multilayer ceramic capacitors face issues where the sintered state variation due to dielectric composition causes color differences between the side and cover portions, leading to potential defects in visual inspection, and adding silica to adjust color adversely affects electrical characteristics.
The ceramic electronic component includes a laminated structure with specific subcomponents like Si, Mn, Cu, Fe, V, Ni, B, Mg, Ho, Dy, Er, Tm, Yb, Gd, Li, Co, Sm, and Y in the side margin and cover layer, with a controlled concentration gradient to adjust color while minimizing diffusion into the capacitive part, ensuring electrical characteristics.
This approach allows for color adjustment of the exterior while maintaining electrical performance by localizing the subcomponents' concentration near the surface and preventing diffusion into the capacitive part, thus enhancing visual inspection and reducing defects.
Smart Images

Figure 2024146432000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a ceramic electronic component and a method for manufacturing a ceramic electronic component. [Background technology]
[0002] 2. Description of the Related Art In high-frequency communication systems, such as mobile phones, highly reliable ceramic electronic components, such as multilayer ceramic capacitors, are used to impart additional functionality (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-35788 A Summary of the Invention [Problem to be solved by the invention]
[0004] Ceramic electronic components such as multilayer ceramic capacitors can be manufactured by sintering powder materials. In this process, the sintering state varies greatly depending on the composition of the dielectric, resulting in differences in color between the sides and cover. In such cases, the product may be judged defective through visual inspection. To address this issue, it is possible to add secondary components such as silica to adjust the color. However, if the secondary components diffuse into the capacitance section, this can have a negative effect on electrical properties such as capacitance.
[0005] The present invention has been made in consideration of the above-mentioned problems, and has an object to provide a ceramic electronic component that can adjust the color of the appearance while ensuring electrical characteristics, and a manufacturing method thereof. [Means for solving the problem]
[0006] A ceramic electronic component according to the present invention comprises a laminated chip including a laminated portion in which a plurality of dielectric layers and a plurality of internal electrode layers are stacked, the plurality of internal electrode layers being alternately drawn out to two opposing end faces of the laminated chip, the laminated chip having a side margin outside a capacitive section which is a region where the plurality of dielectric layers and the plurality of internal electrode layers face each other in a third direction perpendicular to a first direction in which the plurality of internal electrode layers face each other and a second direction in which the two end faces face each other, the laminated chip having a cover layer mainly composed of ceramic on the upper and lower surfaces of the capacitive section in the first direction, the side margin and the cover layer having a high concentration portion having a higher concentration of at least one of the auxiliary components selected from Si, Mn, Cu, Fe, V, Ni, B, Mg, Ho, Dy, Er, Tm, Yb, Gd, Li, Co, Sm, and Y on a side closer to the outer surface than on a side closer to the capacitive section.
[0007] In the ceramic electronic component, the high concentration portion may be a region from an inflection point of the concentration of the minor component to the outer surface, and the inflection point may be a point that satisfies dD / dd≧35 when an EPMA line spectrum from the capacitive portion to the outer surface is obtained, the normalized intensity (D(%)) being normalized by setting the intensity to intensity / maximum intensity×100, and the distance from the capacitive portion to the outer surface being d (μm).
[0008] In the ceramic electronic component, the inflection point may be present in a range of 5.2% to 76% from the outer surface with respect to a thickness of the thinner of the side margin and the cover layer.
[0009] In the ceramic electronic component, the concentration of the minor component in the high concentration portion may be not less than 2.5 at % and not more than 9.0 at %.
[0010] In the side margin and the cover layer of the ceramic electronic component, a concentration of the minor component in a region inside the high concentration portion may be 2.0 at % or more and 6.0 at % or less.
[0011] In the high concentration portion of the ceramic electronic component, the minor component may be present in the form of a simple substance, an oxide crystal, or a glass.
[0012] In the ceramic electronic component, a ratio of a thickness of the high concentration portion of the cover layer to a thickness of the high concentration portion of the side margin may be 0.75 or greater and 1.26 or less.
[0013] Another ceramic electronic component according to the present invention comprises a laminated chip including a laminated portion in which a plurality of dielectric layers and a plurality of internal electrode layers are laminated, the plurality of internal electrode layers being alternately drawn out to two opposing end faces of the laminated chip, the laminated chip having a side margin outside a capacitive section which is a region where the plurality of dielectric layers and the plurality of internal electrode layers face each other in a third direction perpendicular to a first direction in which the plurality of internal electrode layers face each other and a second direction in which the two end faces face each other, the laminated chip having a side margin outside the capacitive section which is a region where the plurality of dielectric layers and the plurality of internal electrode layers face each other in a third direction perpendicular to the first direction in which the plurality of internal electrode layers face each other and the second direction in which the two end faces face each other, The upper and lower surfaces in the first direction are provided with cover layers mainly composed of ceramic, and the side margin and the cover layer have high concentration portions having a higher concentration of at least one of the minor components Si, Mn, Cu, Fe, V, Ni, B, Mg, Ho, Dy, Er, Tm, Yb, Gd, Li, Co, Sm, and Y on the side closer to the outer surface than on the side closer to the capacitance portion, and the high concentration portions are in the range of 5.2% to 76% from the outer surface with respect to the thickness of the thinner of the side margin and the cover layer.
[0014] A manufacturing method for a ceramic electronic component according to the present invention includes the steps of forming an internal electrode pattern on a dielectric green sheet, forming a dielectric pattern around the internal electrode pattern, stacking the dielectric green sheets on which the internal electrode pattern and the dielectric pattern are formed in a first direction so that the ends of the internal electrode patterns are shifted alternately in a second direction to obtain a laminate, impregnating or adhering at least one of the auxiliary components selected from Si, Mn, Cu, Fe, V, Ni, B, Mg, Ho, Dy, Er, Tm, Yb, Gd, Li, Co, Sm, and Y to both ends of the laminate in a third direction perpendicular to the first direction and the second direction, and firing the laminate.
[0015] Another method for manufacturing a ceramic electronic component according to the present invention includes the steps of forming an internal electrode pattern on a dielectric green sheet, stacking the dielectric green sheets on which the internal electrode pattern is formed in a first direction so that the ends of the internal electrode patterns are shifted alternately in a second direction to obtain a laminate, forming side margin sheets containing ceramic powder on both ends of the laminate in a third direction perpendicular to the first and second directions, impregnating or adhering at least one of the accessory components selected from the group consisting of Si, Mn, Cu, Fe, V, Ni, B, Mg, Ho, Dy, Er, Tm, Yb, Gd, Li, Co, Sm, and Y, to the surface of the side margin sheet, and firing the laminate.
[0016] In the above method for producing a ceramic electronic component, the laminate may be fired at a temperature increase rate of 1000° C. / h or more. Effect of the Invention
[0017] According to the present invention, it is possible to provide a ceramic electronic component that can adjust the color of the appearance while ensuring electrical characteristics, and a method for manufacturing the same. [Brief description of the drawings]
[0018] [Figure 1]FIG. 2 is a partial cross-sectional perspective view of a multilayer ceramic capacitor. [Diagram 2] 2 is a cross-sectional view taken along line AA in FIG. 1. [Diagram 3] FIG. 2 is a cross-sectional view taken along line BB in FIG. [Figure 4] FIG. 4 is an enlarged cross-sectional view of the vicinity of an external electrode. [Diagram 5] FIG. 13 is a diagram illustrating a high-concentration portion. [Figure 6] FIG. 1 is a diagram for explaining EPMA line analysis. [Figure 7] FIG. 13 is a diagram illustrating an example of a graph before and after smoothing. [Figure 8] FIG. 13 is a diagram illustrating a normalized concentration. [Figure 9] FIG. 13 is a diagram illustrating the point where dD / dd=35 and an inflection point. [Figure 10] 1A to 1C are diagrams illustrating a flow of a method for manufacturing a multilayer ceramic capacitor. [Figure 11] 4(a) and 4(b) are diagrams illustrating an internal electrode forming step. [Figure 12] FIG. 1 is a diagram illustrating a lamination process. [Figure 13] 13 is a diagram illustrating an example in which a side margin portion is retrofitted. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, an embodiment will be described with reference to the drawings.
[0020] (Embodiment) FIG. 1 is a partial cross-sectional perspective view of a multilayer ceramic capacitor 100 according to an embodiment. FIG. 2 is a cross-sectional view taken along line AA in FIG. 1. FIG. 3 is a cross-sectional view taken along line BB in FIG. 1. As illustrated in FIGS. 1 to 3, the multilayer ceramic capacitor 100 includes a laminated chip 10 having a substantially rectangular parallelepiped shape, and external electrodes 20a, 20b provided on any two opposing end faces of the laminated chip 10. Of the four faces of the laminated chip 10 other than the two end faces, the two faces other than the top and bottom faces in the stacking direction are referred to as side faces. The external electrodes 20a, 20b extend on the top, bottom and two side faces in the stacking direction of the laminated chip 10. However, the external electrodes 20a, 20b are spaced apart from each other.
[0021] 1 to 3, the Z-axis direction (first direction) is the stacking direction, and is the direction in which the internal electrode layers 12 face each other. The X-axis direction (second direction) is the length direction of the laminated chip 10, and is the direction in which the two end faces of the laminated chip 10 face each other, and is the direction in which the external electrodes 20a and 20b face each other. The Y-axis direction (third direction) is the width direction of the internal electrode layers 12, and is the direction in which the two side faces other than the two end faces of the four side faces of the laminated chip 10 face each other. The X-axis direction, Y-axis direction, and Z-axis direction are mutually perpendicular.
[0022] The laminated chip 10 has a configuration in which dielectric layers 11 containing a ceramic material that functions as a dielectric and internal electrode layers 12 are alternately laminated. The edges of the internal electrode layers 12 are alternately drawn to the end face on which the external electrode 20a of the laminated chip 10 is provided and the end face on which the external electrode 20b is provided. As a result, each internal electrode layer 12 is alternately conductive to the external electrode 20a and the external electrode 20b. As a result, the laminated ceramic capacitor 100 has a configuration in which a plurality of dielectric layers 11 are laminated via the internal electrode layers 12. In addition, in the lamination of the dielectric layers 11 and the internal electrode layers 12, the internal electrode layers 12 are arranged on both outermost layers in the lamination direction, and the internal electrode layers 12 of the outermost layers are covered by the cover layers 13. The cover layers 13 are mainly composed of a ceramic material. For example, the cover layers 13 may have the same composition as the dielectric layers 11 or may have a different composition.
[0023] The size of the multilayer ceramic capacitor 100 is, for example, 0.25 mm in length, 0.125 mm in width, and 0.125 mm in height, or 0.4 mm in length, 0.2 mm in width, and 0.2 mm in height, or 0.6 mm in length, 0.3 mm in width, and 0.3 mm in height, or 1.0 mm in length, 0.5 mm in width, and 0.5 mm in height, or 3.2 mm in length, 1.6 mm in width, and 1.6 mm in height, or 4.5 mm in length, 3.2 mm in width, and 2.5 mm in height, but is not limited to these sizes.
[0024] The internal electrode layers 12 are mainly composed of base metals such as nickel (Ni), copper (Cu), and tin (Sn), or alloys thereof. The main components of the internal electrode layers 12 may be precious metals such as platinum (Pt), palladium (Pd), silver (Ag), and gold (Au), or alloys containing these metals. The internal electrode layers 12 may contain ceramic particles such as co-materials. The average thickness of each of the internal electrode layers 12 in the Z-axis direction is, for example, 0.5 μm or less, and preferably 0.4 μm or less. The average thickness of each of the internal electrode layers 12 can be measured by observing the cross section of the multilayer ceramic capacitor 100 with a SEM (scanning electron microscope), measuring the thickness at 10 points for each of the 10 different internal electrode layers 12, and deriving the average value of all the measurement points.
[0025] The dielectric layer 11 has a main phase made of a ceramic material having a perovskite structure represented by the general formula ABO3. 3-α For example, the ceramic material includes barium titanate (BaTiO3), calcium zirconate (CaZrO3), calcium titanate (CaTiO3), strontium titanate (SrTiO3), magnesium titanate (MgTiO3), BaTiO3, which forms a perovskite structure, 1-x-y Ca x Sr y Ti 1-z Zr z O3 (0≦x≦1, 0≦y≦1, 0≦z≦1), etc. 1-x-y Cax Sr y Ti 1-z Zr z O3 is barium strontium titanate, barium calcium titanate, barium zirconate, barium titanate zirconate, calcium titanate zirconate, barium calcium titanate zirconate, etc. For example, the dielectric layer 11 contains 90 at% or more of the main component ceramic. The average thickness per layer of the dielectric layer 11 in the Z-axis direction is, for example, 1.0 μm or less, and preferably 0.8 μm or less. The average thickness per layer of the internal electrode layer 12 in the Z-axis direction can be measured by observing the cross section of the multilayer ceramic capacitor 100 with a SEM (scanning electron microscope), measuring the thickness at 10 points for each of 10 different dielectric layers 11, and deriving the average value of all the measurement points.
[0026] An additive may be added to the dielectric layer 11. Examples of the additive to the dielectric layer 11 include oxides of zirconium (Zr), hafnium (Hf), magnesium (Mg), manganese (Mn), molybdenum (Mo), vanadium (V), chromium (Cr), and rare earth elements (yttrium (Y), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), and ytterbium (Yb)), or oxides containing cobalt (Co), nickel (Ni), lithium (Li), boron (B), sodium (Na), potassium (K), or silicon (Si), or glasses containing cobalt, nickel, lithium, boron, sodium, potassium, or silicon.
[0027] 2, a region where the internal electrode layer 12 connected to the external electrode 20a and the internal electrode layer 12 connected to the external electrode 20b face each other is a region that generates capacitance in the multilayer ceramic capacitor 100. Therefore, the region that generates capacitance is referred to as a capacitive portion 14. In other words, the capacitive portion 14 is a region where adjacent internal electrode layers 12 connected to different external electrodes face each other.
[0028] The region where the internal electrode layers 12 connected to the external electrode 20a face each other without an internal electrode layer 12 connected to the external electrode 20b being interposed therebetween is referred to as the end margin 15. The region where the internal electrode layers 12 connected to the external electrode 20b face each other without an internal electrode layer 12 connected to the external electrode 20a being interposed therebetween is also the end margin 15. In other words, the end margin 15 is a region where the internal electrode layers 12 connected to the same external electrode face each other without an internal electrode layer 12 connected to a different external electrode being interposed therebetween. The end margin 15 is a region that does not generate capacitance.
[0029] 3, in the laminated chip 10, the side margin 16 is a region provided so as to cover the ends (ends in the Y-axis direction) of two side surfaces of the dielectric layer 11 and the internal electrode layer 12. In other words, the side margin 16 is a region provided outside the capacitive section 14 in the Y-axis direction. The side margin 16 is also a region that does not generate capacitance.
[0030] FIG. 4 is an enlarged cross-sectional view of the vicinity of the external electrode 20a. Hatching is omitted in FIG. 4. As illustrated in FIG. 4, a plating layer 22 may be provided on the outer surface of the external electrode 20a with the external electrode 20a as a base layer. The external electrode 20a is mainly composed of Cu. The external electrode 20a may contain a glass component. The plating layer 22 is mainly composed of a metal such as Cu, Ni, aluminum (Al), zinc (Zn), Sn, or an alloy of two or more of these metals. The plating layer 22 may be a plating layer of a single metal component, or may be a plurality of plating layers of different metal components. For example, the plating layer 22 has a structure in which a first plating layer 23, a second plating layer 24, and a third plating layer 25 are formed in this order from the external electrode 20a side. The first plating layer 23 is, for example, a Cu plating layer. The second plating layer 24 is, for example, a Ni plating layer. The third plating layer 25 is, for example, a Sn plating layer. Although FIG. 4 illustrates the external electrode 20a as an example, the plating layer 22 may be provided on the outer surface of the external electrode 20b as well.
[0031] Multilayer ceramic capacitors can be manufactured by simultaneously firing the powder materials for the dielectric layers and the internal electrode layers. For example, in order to prevent the internal electrode layers from being broken, firing may be performed at a high heating rate of 1000°C / h or more. In this case, the sintering state varies greatly depending on the composition of the dielectric, so that a difference in color occurs between the cover layer and the side margin. If a multilayer ceramic capacitor with a difference in color is inspected, it may be judged as defective. Therefore, in order to adjust the color of the side margin, it is possible to add a large amount of secondary components such as silica in advance to adjust the color. However, in this case, the added secondary components diffuse into the capacitance part during the firing process, adversely affecting electrical properties such as capacitance.
[0032] In contrast, the multilayer ceramic capacitor 100 according to this embodiment has a configuration that allows the color of the appearance to be adjusted while ensuring electrical characteristics, as will be described in detail below.
[0033] In this embodiment, the side margin 16 and the cover layer 13 contain a subcomponent (hereinafter, a color-adjusting component) for adjusting the color. As the color-adjusting component, at least one of silicon (Si), manganese (Mn), copper (Cu), iron (Fe), vanadium (V), nickel (Ni), boron (B), magnesium (Mg), holmium (Ho), dysprosium (Dy), erbium (Er), thulium (Tm), ytterbium (Yb), gadolinium (Gd), lithium (Li), cobalt (Co), samarium (Sm), and yttrium (Y) can be used. By containing the color-adjusting component in the side margin 16 and the cover layer 13, the color of the outer surface of the side margin 16 and the cover layer 13 can be adjusted. For example, the solid solution state of the additive changes, becoming whitish. As a result, when the multilayer ceramic capacitor 100 according to this embodiment is subjected to an appearance inspection, it is more likely to pass.
[0034] The color-adjusting component may be present in the form of a simple element or in the form of an oxide in the side margin 16 and the cover layer 13. For example, the color-adjusting component may be present in the form of an oxide crystal or in the form of glass.
[0035] As illustrated in FIG. 5, the side margin 16 and the cover layer 13 have a high-concentration portion 30 having a higher concentration of the color-adjusting component on the side closer to the outer surface than on the side closer to the capacitance portion 14. This allows the color of the outer surface of the side margin 16 and the cover layer 13 to be adjusted. Meanwhile, in the side margin 16 and the cover layer 13, the concentration of the color-adjusting component on the capacitance portion 14 side is low, so that the diffusion of the color-adjusting component to the capacitance portion 14 is suppressed. This allows the deterioration of the electrical characteristics of the multilayer ceramic capacitor 100 to be suppressed. The region on the capacitance portion 14 side of the high-concentration portion 30 is referred to as the low-concentration portion 40. Hatching is omitted in FIG. 5.
[0036] As described above, the multilayer ceramic capacitor 100 in accordance with this embodiment can adjust the color of its appearance while ensuring its electrical characteristics.
[0037] For example, when an EPMA (Electron Probe Micro Analyzer) line spectrum is obtained for the concentration of the color adjusting component in the thickness direction of the side margin 16 and the cover layer 13, an inflection point appears in the concentration change of the color adjusting component. Whether or not an inflection point appears in the concentration change of the color density adjusting component can be confirmed by the following procedure. Note that the thickness direction of the side margin 16 is the Y-axis direction, and the thickness direction of the cover layer 13 is the Z-axis direction.
[0038] First, as illustrated in FIG. 6, EPMA line analysis is performed in the thickness direction of the side margin 16 and the cover layer 13 at a predetermined sampling period. Each circle in FIG. 6 indicates a sampling point. In the example of FIG. 6, the sampling interval is 0.25 μm as an example. Next, for each sampling point, the average intensity value is calculated within a range of 0.5 μm before and after. This calculated average intensity value is used as the intensity value at each sampling point. By calculating and smoothing the moving average in this way, it is possible to measure the intensity change while suppressing the effects of noise.
[0039] In Fig. 7, a graph before smoothing and a graph after smoothing are shown side by side. The horizontal axis in Fig. 7 represents the distance d (μm). As an example, "0" on the horizontal axis in Fig. 7 indicates the boundary between the side margin 16 and the capacitive section 14. In Fig. 7, the more to the right on the horizontal axis, the further in the thickness direction of the side margin 16 it progresses, and reaches the outer surface of the side margin 16. As shown in the graph in Fig. 7, in the side margin 16, the concentration of the color adjusting component is higher on the outer surface than on the capacitive section 14 side.
[0040] Next, the graph of the measured intensity change is normalized. The intensity measured at each sampling point is set to intensity / maximum intensity×100 to obtain the normalized intensity (D(%)). This normalization makes it possible to confirm the inflection point even if there is variation in the absolute value of the concentration value. FIG. 8 is a diagram illustrating the normalized concentration.
[0041] Next, the graph of the normalized intensity D (%) is differentiated by the distance d (μm) to calculate dD / dd. The point where dD / dd becomes 35 is defined as the inflection point. FIG. 9 illustrates the point where dD / dd=35 and the inflection point. In the multilayer ceramic capacitor 100 according to this embodiment, the inflection point appears in the change in concentration of the color adjusting component in the cover layer 13 and the side margin 16. This confirms that the concentration of the color adjusting component is kept low in the region close to the capacitance section 14 in the side margin 16 and the cover layer 13, and the concentration of the color adjusting component is locally high in the high concentration portion 30 close to the outer surface. Note that when two or more kinds of color adjusting components are added, the concentration of the color adjusting component refers to the concentration when focusing on any one of them.
[0042] For example, the region from the inflection point to the outer surface in the thickness direction of the side margin 16 and the cover layer 13 can be defined as the high concentration portion 30 .
[0043] If the inflection point is close to the outer surface of the side margin 16 and the cover layer 13, the amount of the color adjusting component will be small, and there is a risk that the color of the side margin 16 and the cover layer 13 cannot be sufficiently adjusted. Therefore, it is preferable that the inflection point is away from the outer surface. In this embodiment, in the thickness direction of the side margin 16 and the cover layer 13, the inflection point is preferably 5.2% or more away from the outer surface with respect to the thinner thickness of the side margin 16 or the cover layer 13, more preferably 18% or more away, and even more preferably 30% or more away.
[0044] On the other hand, if the inflection point is close to the capacitive section 14, there is a risk that the color adjusting component will diffuse into the capacitive section 14. Therefore, it is preferable that the inflection point is away from the capacitive section 14. In this embodiment, in the thickness direction of the side margin 16 and the cover layer 13, the inflection point is preferably located 76% or less away from the outer surface with respect to the thickness of the thinner of the side margin 16 and the cover layer 13, more preferably 67% or less away, and even more preferably 61% or less away.
[0045] If the concentration of the color adjusting component in the high concentration portion 30 is low, the color of the side margin 16 and the cover layer 13 may not be adjusted sufficiently. Therefore, it is preferable to set a lower limit for the concentration of the color adjusting component in the high concentration portion 30. In this embodiment, the concentration of the color adjusting component in the high concentration portion 30 is preferably 2.5 at% or more, more preferably 2.75 at% or more, and even more preferably 3.0 at% or more. The concentration of the color adjusting component here refers to the concentration when the B site (e.g., Ti) of the main component ceramic having a perovskite structure contained in the side margin 16 and the cover layer 13 is 100 at%. The concentration of the color adjusting component in the high concentration portion 30 can be measured, for example, by LA-ICP-MS.
[0046] On the other hand, if the concentration of the color adjusting component in the high concentration portion 30 is high, necking, in which the stacked chips stick to each other, may occur when firing the multiple stacked chips. Therefore, it is preferable to set an upper limit on the concentration of the color adjusting component in the high concentration portion 30. In this embodiment, the concentration of the color adjusting component in the high concentration portion 30 is preferably 9.0 at% or less, more preferably 8.5 at% or less, and even more preferably 8.0 at% or less.
[0047] If the concentration of the color adjusting component in the low-density portion 40 is high, there is a risk that the color adjusting component will diffuse into the capacitance portion 14. Therefore, it is preferable to set an upper limit on the concentration of the color adjusting component in the low-density portion 40. In this embodiment, the concentration of the color adjusting component in the low-density portion 40 is preferably 6.0 at % or less, more preferably 5.5 at % or less, and even more preferably 5.0 at % or less.
[0048] On the other hand, if the concentration of the color adjusting component in the low-density portion 40 is low, Si present in the capacitance portion 14 may diffuse into the cover layer 13 and the side margin 16, which may cause a change in characteristics. Therefore, it is preferable to set a lower limit for the concentration of the color adjusting component in the low-density portion 40. In this embodiment, the concentration of the color adjusting component in the low-density portion 40 is preferably 2.0 at% or more, more preferably 2.25 at% or more, and even more preferably 2.5 at% or more.
[0049] If the difference in thickness between the high concentration portion 30 in the side margin 16 and the high concentration portion 30 in the cover layer 13 is large, there is a risk of a large difference in color. Therefore, it is preferable that the difference in thickness between the high concentration portion 30 in the side margin 16 and the high concentration portion 30 in the cover layer 13 is small. In this embodiment, the ratio of the thickness of the high concentration portion 30 in the cover layer 13 to the thickness of the high concentration portion 30 in the side margin 16 is preferably 0.75 or more and 1.26 or less.
[0050] Next, a description will be given of a method for manufacturing the multilayer ceramic capacitor 100. FIG 10 is a diagram illustrating a flow of the method for manufacturing the multilayer ceramic capacitor 100.
[0051] (Raw powder production process) First, a dielectric material for forming the dielectric layer 11 is prepared. The A-site elements and B-site elements contained in the dielectric layer 11 are usually contained in the dielectric layer 11 in the form of a sintered body of ABO3 particles. For example, barium titanate is a tetragonal compound having a perovskite structure and exhibits a high dielectric constant. This barium titanate can generally be obtained by reacting a titanium raw material such as titanium dioxide with a barium raw material such as barium carbonate to synthesize barium titanate.
[0052] A predetermined additive compound is added to the obtained ceramic powder according to the purpose. Examples of the additive compound include oxides of zirconium, hafnium, magnesium, manganese, molybdenum, vanadium, chromium, rare earth elements (yttrium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, and ytterbium), oxides containing cobalt, nickel, lithium, boron, sodium, potassium, or silicon, or glasses containing cobalt, nickel, lithium, boron, sodium, potassium, or silicon.
[0053] For example, a compound containing an additive compound is wet-mixed with a ceramic raw material powder, and then dried and pulverized to prepare a ceramic material. For example, the ceramic material obtained as described above may be pulverized as necessary to adjust the particle size, or may be combined with a classification process to adjust the particle size. Through the above steps, a dielectric material is obtained.
[0054] (Coating process) Next, a binder such as polyvinyl butyral (PVB) resin, an organic solvent such as ethanol or toluene, and a plasticizer are added to the obtained raw material powder and wet mixed. The obtained slurry is used to coat a dielectric green sheet 51 on a substrate by, for example, a die coater method or a doctor blade method, and then dried. The substrate is, for example, a polyethylene terephthalate (PET) film. Figures illustrating the coating process are omitted.
[0055] (Internal electrode formation process) 11(a), a metal conductive paste for forming an internal electrode containing an organic binder is printed on the surface of the dielectric green sheet 51 by screen printing, gravure printing, or the like to arrange an internal electrode pattern 52 for the internal electrode layer. In addition to nickel, ceramic particles are added to the metal conductive paste as a co-material. The main component of the ceramic particles is not particularly limited, but is preferably the same as the main component ceramic of the dielectric layer 11.
[0056] Next, a binder such as an ethyl cellulose-based binder and an organic solvent such as a terpineol-based binder are added to the dielectric pattern material obtained in the raw powder preparation process, and the mixture is kneaded in a roll mill to obtain a dielectric pattern paste for the reverse pattern layer. As illustrated in Fig. 11(a), a dielectric pattern paste is printed on a peripheral area of a dielectric green sheet 51 where an internal electrode pattern 52 is not printed, thereby disposing a dielectric pattern 53 and filling in the step with the internal electrode pattern 52. The dielectric green sheet 51 on which the internal electrode pattern 52 and the dielectric pattern 53 are printed is referred to as a lamination unit.
[0057] 11(b), the lamination units are laminated so that the internal electrode layers 12 and the dielectric layers 11 are alternately arranged, and the edges of the internal electrode layers 12 are alternately exposed at both end faces in the length direction of the dielectric layers 11 and alternately drawn out to a pair of external electrodes 20a, 20b having different polarities. For example, the number of layers of the internal electrode pattern 52 is set to 100 to 500.
[0058] (Crimping process) 12, a predetermined number of cover sheets 54 (for example, 2 to 10 layers) are laminated on the top and bottom of a laminate in which the laminate units are laminated, and are thermocompression bonded. The cover sheets 54 are also green sheets containing ceramic powder.
[0059] (Chipping process) The resulting ceramic laminate is cut into chips of a predetermined size.
[0060] The side margin portion may be attached or applied to the side surface of the laminated portion. Specifically, as illustrated in Fig. 13, ceramic green sheets 51 and internal electrode patterns 52 having the same width as the ceramic green sheets 51 are alternately laminated to obtain the laminated portion. Next, a sheet formed of a dielectric pattern paste may be attached as a side margin portion 55 to the side surface of the laminated portion.
[0061] (addition process) Next, the chipped ceramic laminate is chamfered by barrel polishing, and the binder is removed in an air or nitrogen atmosphere. After that, a color adjuster is added to the surface of the ceramic laminate by dipping. For example, when silica is used as the color adjuster, colloidal silica is impregnated. This dipping process allows the surface of the region corresponding to the side margin 16 and the cover layer 13 to be impregnated with a precursor of the color adjuster. The amount of the color adjuster precursor impregnated can be adjusted by changing the dipping time. The amount of the impregnation can also be adjusted by changing the solvent viscosity, the stirring time, the solution temperature, etc.
[0062] The color-adjusting agent may be added by a method other than dipping. For example, the color-adjusting agent may be attached to the chip surface by chemical vapor deposition (CVD) or the like, and then allowed to penetrate into the chip surface at high temperatures during the firing process.
[0063] (Firing process) The ceramic laminate thus obtained was subjected to a binder removal treatment in a N2 atmosphere, after which a metal paste for the external electrodes 20a, 20b was applied thereto by a dipping method. -12 MPa~10 -9 The mixture is fired for 5 minutes to 10 hours in a reducing atmosphere at 1160° C. to 1280° C. (for example, 1180° C. or higher and 1230° C. or lower) under a pressure of 200 MPa. The rate of temperature rise to the firing temperature is, for example, 1000° C. / h or higher.
[0064] (Reoxidation treatment process) In order to return oxygen to the barium titanate, which is the partially reduced main phase of the dielectric layer 11 fired in a reducing atmosphere, a heat treatment may be performed in a mixed gas of N2 and water vapor at about 1000°C or in the air at 500°C to 700°C, to a temperature that does not oxidize the internal electrode layer 12. This process is called a reoxidation treatment process.
[0065] (Plating process) Thereafter, the external electrodes 20a, 20b are plated with a metal coating of copper, nickel, tin, etc. Through the above steps, the multilayer ceramic capacitor 100 is completed.
[0066] According to the manufacturing method of this embodiment, the color adjusting component is impregnated or attached to the regions corresponding to the outer surfaces of the side margin 16 and the cover layer 13, and then fired, so that in the side margin 16 and the cover layer 13, a region with a high concentration of the color adjusting component is formed on the outer surfaces, and a region with a low concentration of the color adjusting component is formed on the side closer to the capacitance portion 14. For example, the high concentration portion 30 and the low concentration portion 40 described above can be formed.
[0067] In the above-described embodiments, a multilayer ceramic capacitor has been described as an example of a multilayer ceramic electronic component, but the present invention is not limited to this. For example, other multilayer ceramic electronic components such as a varistor or a thermistor may be used. EXAMPLES
[0068] The multilayer ceramic capacitor according to the above embodiment was fabricated and its characteristics were examined.
[0069] Example 1 An internal electrode pattern of Ni was printed on a dielectric green sheet. A dielectric pattern was printed around the internal electrode pattern. Multiple laminate units were laminated so that the internal electrode patterns were alternately shifted in the X-axis direction, and then pressure-bonded and cut to obtain a ceramic laminate.
[0070] The produced ceramic laminate was chamfered with a barrel and subjected to a binder removal treatment. In Example 1, Si was used as a color-adjusting component. The chip margin was impregnated with silica precursor by impregnating colloidal silica into the chip by dipping. The impregnated amount of silica precursor was adjusted by the dipping time. In Example 1, the dipping time was set to 5 seconds. The impregnation depth of the Si component was 1 μm. After dipping, a heat treatment was performed at 200° C. in a nitrogen atmosphere to remove excess organic solvent. The ceramic laminate to which the Si component was added was rapidly fired (heating rate: 1000° C. / h) in a N2-H2-wet atmosphere, and external electrodes were baked and plated to produce a multilayer ceramic capacitor.
[0071] After firing, the thickness of the cover layer was 17 μm. The thickness of the side margin was 13 μm. EPMA line analysis was performed on the side margin and cover layer to measure the concentration of the color adjusting component and detect the inflection point, and the region from the inflection point to the outer surface was defined as the high concentration part. The range of the high concentration part in the cover layer was 1.1 μm from the outer surface. This corresponds to 6.5% of the thickness of the cover layer. The range of the high concentration part in the side margin was 1.0 μm from the outer surface. This corresponds to 8.5% of the thickness of the side margin. The ratio of the thickness of the high concentration part in the cover layer to the thickness of the high concentration part in the side margin was 1.10.
[0072] Example 2 In Example 2, the dipping time was 5 seconds. The impregnation depth of the Si component was 1 μm. After firing, the thickness of the cover layer was 21 μm. The thickness of the side margin was 17 μm. The range of the high concentration part in the cover layer was 1.2 μm from the outer surface. This corresponds to 5.2% of the thickness of the cover layer. The range of the high concentration part in the side margin was 1.0 μm from the outer surface. This corresponds to 6.5% of the thickness of the side margin. The ratio of the thickness of the high concentration part in the cover layer / the thickness of the high concentration part in the side margin was 1.20. The other conditions were the same as in Example 1.
[0073] Example 3 In Example 3, the dipping time was 60 seconds. The impregnation depth of the Si component was 9 μm. After firing, the thickness of the cover layer was 17 μm. The thickness of the side margin was 13 μm. The range of the high concentration part in the cover layer was 9.1 μm from the outer surface. This corresponds to 49% of the thickness of the cover layer. The range of the high concentration part in the side margin was 7.5 μm from the outer surface. This corresponds to 65% of the thickness of the side margin. The ratio of the thickness of the high concentration part in the cover layer / the thickness of the high concentration part in the side margin was 1.21. The other conditions were the same as in Example 1.
[0074] Example 4 In Example 4, the dipping time was 60 seconds. The impregnation depth of the Si component was 9 μm. After firing, the thickness of the cover layer was 21 μm. The thickness of the side margin was 17 μm. The range of the high concentration part in the cover layer was 9.1 μm from the outer surface. This corresponds to 40% of the thickness of the cover layer. The range of the high concentration part in the side margin was 7.2 μm from the outer surface. This corresponds to 49% of the thickness of the side margin. The ratio of the thickness of the high concentration part in the cover layer / the thickness of the high concentration part in the side margin was 1.26. The other conditions were the same as in Example 1.
[0075] Example 5 In Example 5, the dipping time was 120 seconds. The impregnation depth of the Si component was 12 μm. After firing, the thickness of the cover layer was 21 μm. The thickness of the side margin was 17 μm. The range of the high concentration part in the cover layer was 13.0 μm from the outer surface. This corresponds to 62% of the thickness of the cover layer. The range of the high concentration part in the side margin was 12.0 μm from the outer surface. This corresponds to 76% of the thickness of the side margin. The ratio of the thickness of the high concentration part in the cover layer / the thickness of the high concentration part in the side margin was 1.08. The other conditions were the same as in Example 1.
[0076] Example 6 In Example 6, B was used as a color-adjusting component instead of Si, and was attached to the surface of the chip margin by CVD without dipping. After firing, the thickness of the cover layer was 17 μm. The thickness of the side margin was 13 μm. The range of the high-concentration part in the cover layer was 5.0 μm from the outer surface. This corresponds to 30% of the thickness of the cover layer. The range of the high-concentration part in the side margin was 4.0 μm from the outer surface. This corresponds to 38% of the thickness of the side margin. The ratio of the thickness of the high-concentration part in the cover layer to the thickness of the high-concentration part in the side margin was 1.25. The other conditions were the same as in Example 1.
[0077] Example 7 In Example 7, Al was used as a color-adjusting component instead of Si, and was attached to the surface of the chip margin by CVD without dipping. After firing, the thickness of the cover layer was 17 μm. The thickness of the side margin was 13 μm. The range of the high-concentration part in the cover layer was 7.0 μm from the outer surface. This corresponds to 41% of the thickness of the cover layer. The range of the high-concentration part in the side margin was 6.0 μm from the outer surface. This corresponds to 54% of the thickness of the side margin. The ratio of the thickness of the high-concentration part in the cover layer to the thickness of the high-concentration part in the side margin was 1.17. The other conditions were the same as in Example 1.
[0078] Example 8 In Example 8, Ge was used as a color-adjusting component instead of Si, and was attached to the surface of the chip margin by CVD without dipping. After firing, the thickness of the cover layer was 17 μm. The thickness of the side margin was 13 μm. The range of the high-concentration part in the cover layer was 3.0 μm from the outer surface. This corresponds to 18% of the thickness of the cover layer. The range of the high-concentration part in the side margin was 4.0 μm from the outer surface. This corresponds to 23% of the thickness of the side margin. The ratio of the thickness of the high-concentration part in the cover layer to the thickness of the high-concentration part in the side margin was 0.75. The other conditions were the same as in Example 1.
[0079] Comparative Example 1 In Comparative Example 1, no color-adjusting component was added to the side margin and the cover layer. After firing, the cover layer had a thickness of 17 μm. The side margin had a thickness of 13 μm. The other conditions were the same as in Example 1.
[0080] Comparative Example 2 In Comparative Example 2, the dipping time was 600 seconds. The impregnation depth of the Si component was deeper than 17 μm. After firing, the thickness of the cover layer was 17 μm. The thickness of the side margin was 13 μm. The range of the high concentration part in the cover layer was wider than 17 μm from the outer surface. This is more than 100% of the thickness of the cover layer. The range of the high concentration part in the side margin was wider than 13 μm from the outer surface. This is more than 100% of the thickness of the side margin. The other conditions were the same as in Example 1.
[0081] Comparative Example 3 In Comparative Example 3, the dipping time was 300 seconds. The impregnation depth of the Si component was 15 μm. After firing, the thickness of the cover layer was 17 μm. The thickness of the side margin was 13 μm. The range of the high concentration part in the cover layer was 16 μm from the outer surface. This is more than 100% of the thickness of the cover layer. The range of the high concentration part in the side margin was 13 μm from the outer surface. This is more than 100% of the thickness of the side margin. The ratio of the thickness of the high concentration part in the cover layer / the thickness of the high concentration part in the side margin was 1.07. The other conditions were the same as in Example 1.
[0082] The conditions for Examples 1 to 8 and Comparative Examples 1 to 3 are shown in Table 1. [Table 1]
[0083] (Visual defect inspection) A visual defect inspection was carried out on 100 samples for each of Examples 1 to 8 and Comparative Examples 1 to 3. In the visual defect inspection, samples in which the color quantified by a grayscale or the like was outside a certain standard range were judged to be defective. The ratio of the number of samples judged to be defective was defined as the defective judgment rate. If the defective judgment rate was less than 5%, the visual defect judgment rate was judged to be good "◯". If the defective judgment rate was 5% or more and less than 10%, the visual defect judgment rate was judged to be somewhat good "△". If the defective judgment rate was 10% or more, the visual defect judgment rate was judged to be poor "X". The results are shown in Table 2.
[0084] In Comparative Example 1, the appearance defect inspection was judged to be poor "X". This is believed to be because no color-adjusting component was added to the side margin and cover layer. In contrast, in all of Examples 1 to 8, the appearance defect inspection was judged to be good "O". This is believed to be because Si was added to the side margin and cover layer as a color-adjusting component.
[0085] (Capacitance change rate) The capacitance was examined for each of Examples 1 to 8 and Comparative Examples 1 to 3. If the capacitance reduction rate was 5% or more relative to the capacitance of Example XX, the capacitance change rate was judged as poor "X", if the capacitance reduction rate was 3% or more and less than 5%, the capacitance change rate was judged as somewhat good "△", and if the capacitance reduction rate was less than 3%, the capacitance change rate was judged as good "◯". The results are shown in Table 2.
[0086] In Comparative Examples 2 and 3, the capacitance change rate was judged to be poor (×). This is believed to be because the high concentration portion of the color adjusting component was formed over the entire side margin and cover layer, causing the color adjusting component to diffuse into the capacitance portion. In contrast, in Examples 1 to 8, the capacitance change rate was judged to be somewhat good (△) or good (◯). This is believed to be because the high concentration portion of the color adjusting component was formed over the side margin and part of the cover layer, causing the concentration of the color adjusting component on the capacitance portion side to be low, suppressing the diffusion of the color adjusting component.
[0087] The reason why the capacitance change rate results were better in Examples 1 to 4 and 6 to 8 than in Example 5 is believed to be because an inflection point existed in the concentration of the color adjusting component within a range of 67% or less from the outer surface relative to the thinner of the side margin and cover layer. [Table 2]
[0088] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to such specific embodiments, and various modifications and variations are possible within the scope of the gist of the present invention described in the claims. [Explanation of symbols]
[0089] 10 Stacked Chip 11 Dielectric layer 12 Internal electrode layer 13 Cover Layer 14 Capacity part 15 End Margin 16 Side Margin 20a,20b external electrode 22 Plating layer 23 First plating layer 24 Second plating layer 25 3rd plating layer 51 Dielectric green sheet 52 Internal electrode pattern 53 Dielectric Pattern 54 Cover Sheet 55 Side margin 100 Multilayer ceramic capacitors
Claims
1. a laminated chip including a laminated portion in which a plurality of dielectric layers and a plurality of internal electrode layers are laminated; The plurality of internal electrode layers are alternately drawn out to two opposing end surfaces of the laminated chip, the laminated chip has a side margin on the outside of a capacitance section, which is a region where the plurality of dielectric layers and the plurality of internal electrode layers face each other, in a third direction perpendicular to a first direction in which the plurality of internal electrode layers face each other and a second direction in which the two end faces face each other; the laminated chip includes a cover layer mainly made of ceramic on an upper surface and a lower surface of the capacitance section in the first direction; A ceramic electronic component, wherein the side margin and the cover layer have a high concentration portion having a high concentration of at least one of the accessory components selected from the group consisting of Si, Mn, Cu, Fe, V, Ni, B, Mg, Ho, Dy, Er, Tm, Yb, Gd, Li, Co, Sm, and Y, on a side closer to the outer surface than on a side closer to the capacitive portion.
2. the high concentration portion is a region from an inflection point of the concentration of the subcomponent to the outer surface, 2. The ceramic electronic component according to claim 1, wherein the inflection point is a point that satisfies dD / dd≧35, where D (%) is a normalized intensity obtained by normalizing an intensity by dividing the intensity by a maximum intensity×100 when an EPMA line spectrum is obtained from the capacitance portion to the outer surface, and d (μm) is a distance from the capacitance portion to the outer surface.
3. 2. The ceramic electronic component according to claim 1, wherein the inflection point is present within a range of 5.2% to 76% from the outer surface with respect to a thickness of the thinner of the side margin and the cover layer.
4. 3. The ceramic electronic component according to claim 2, wherein the concentration of the minor component in the high concentration portion is 2.5 at % or more and 9.0 at % or less.
5. 3. The ceramic electronic component according to claim 2, wherein the concentration of the minor component in the side margin and in the cover layer in a region inside the high concentration portion is 2.0 at % or more and 6.0 at % or less.
6. The ceramic electronic component according to claim 1 , wherein the minor component is present in the high concentration portion in the form of an element, an oxide crystal, or glass.
7. 3. The ceramic electronic component according to claim 2, wherein a ratio of a thickness of the high concentration portion of the cover layer to a thickness of the high concentration portion of the side margin is equal to or greater than 0.75 and equal to or less than 1.
26.
8. a laminated chip including a laminated portion in which a plurality of dielectric layers and a plurality of internal electrode layers are laminated; The plurality of internal electrode layers are alternately drawn out to two opposing end surfaces of the laminated chip, the laminated chip has a side margin on the outside of a capacitance section, which is a region where the plurality of dielectric layers and the plurality of internal electrode layers face each other, in a third direction perpendicular to a first direction in which the plurality of internal electrode layers face each other and a second direction in which the two end faces face each other; the laminated chip includes a cover layer mainly made of ceramic on an upper surface and a lower surface of the capacitance section in the first direction; The side margin and the cover layer have a high concentration portion having a high concentration of at least one of the subcomponents selected from the group consisting of Si, Mn, Cu, Fe, V, Ni, B, Mg, Ho, Dy, Er, Tm, Yb, Gd, Li, Co, Sm, and Y, on a side closer to the outer surface than on a side closer to the capacitance portion, the high concentration portion is in a range of 5.2% to 76% of the thickness of the thinner of the side margin and the cover layer from the outer surface.
9. forming an internal electrode pattern on a dielectric green sheet; forming a dielectric pattern around the internal electrode pattern; a step of laminating the dielectric green sheets on which the internal electrode patterns and the dielectric patterns are formed in a first direction, and obtaining a laminate by displacing ends of the internal electrode patterns alternately in a second direction; A step of impregnating or depositing at least one or more of the auxiliary components selected from Si, Mn, Cu, Fe, V, Ni, B, Mg, Ho, Dy, Er, Tm, Yb, Gd, Li, Co, Sm, and Y on both ends of the laminate in a third direction perpendicular to the first direction and the second direction; and firing the laminate.
10. forming an internal electrode pattern on a dielectric green sheet; a step of laminating the dielectric green sheets on which the internal electrode patterns are formed in a first direction, and obtaining a laminate by displacing ends of the internal electrode patterns alternately in a second direction; forming side margin sheets containing ceramic powder on both ends of the laminate in a third direction perpendicular to the first direction and the second direction; A step of impregnating or depositing at least one of the following minor components on the surface of the side margin sheet: Si, Mn, Cu, Fe, V, Ni, B, Mg, Ho, Dy, Er, Tm, Yb, Gd, Li, Co, Sm, and Y; and firing the laminate.
11. 11. The method for producing a ceramic electronic component according to claim 9, wherein a temperature increase rate during firing of the laminate is set to 1000[deg.] C. / h or more.
Citation Information
Patent Citations
Electronic component
JP2020035788A