Hydraulic composition, and mortar and ready mixed-concrete containing the same
A hydraulic composition with Portland cement and fine bamboo charcoal powder addresses lead elution and CO2 emissions by utilizing bamboo charcoal, achieving environmental sustainability and pollution reduction.
Patent Information
- Application Number
- JP2023059555
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Cement-based materials used in water environments elute harmful substances like lead, contributing to environmental pollution, and their production emits significant carbon dioxide, while the decline in bamboo usage leads to ecological issues.
A hydraulic composition comprising ordinary Portland cement and fine bamboo charcoal powder, with a ratio of 10 to 70 parts by mass of bamboo charcoal per 100 parts of cement, suppresses lead elution and traps carbon, reducing CO2 emissions.
The composition effectively reduces lead elution into water and contributes to carbon dioxide reduction by utilizing bamboo charcoal, enhancing environmental sustainability.
Smart Images

Figure 2024146572000003 
Figure 2024146572000004 
Figure 2024146572000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a hydraulic composition containing ordinary Portland cement and bamboo charcoal fine powder, and to a mortar and concrete containing the hydraulic composition. [Background technology]
[0002] In response to the deterioration of the water environment in rivers, lakes, and oceans, various direct and indirect water purification and water environment restoration technologies have been developed in recent years. Many of these technologies emphasize the social demand for the recycling of industrial by-products, and aim to directly improve bottom sediment by using solidified dredged soil (sludge) as a sand-capping material, or indirectly purify water and restore ecosystems by regenerating seaweed beds by sinking blocks made of cement-based materials. Among these, cement, an inorganic binding material, is easy to handle and is convenient for manufacturing granular bodies of any size, and can maintain chemical stability for a long period of time after hardening.
[0003] However, when cement-based materials are used in an aqueous environment, care must be taken to prevent the elution of various harmful substances, including heavy metals. It has been reported that when heavy metal elution tests are conducted on ordinary Portland cement in accordance with Environmental Notification No. 46, lead often shows values that exceed environmental standards, and it has been pointed out that lead is a component that is relatively easily eluted into water. (Non-Patent Document 1) [Prior art documents] [Non-patent literature]
[0004] [Non-Patent Document 1] Japan Society of Civil Engineers, Committee on Concrete, Subcommittee on Research and Study on Leaching of Trace Elements, Current Situation and Issues on Leaching of Trace Elements from Concrete, May 30, 2003 issue, page 26, left column Summary of the Invention [Problem to be solved by the invention]
[0005] From Non-Patent Document 1, it is an object of the present invention to provide a hydraulic composition that suppresses the elution of lead into water.
[0006] On the other hand, while there is a demand to reduce greenhouse gas emissions, a large amount of carbon dioxide is emitted during the production of cement-based materials, and there is a demand to reduce carbon dioxide emissions by reducing the amount of cement used, etc.
[0007] On the other hand, the recent decline in bamboo use and the devastation of forests due to the decline of forestry have led to serious problems such as landslides and a decline in biodiversity, which is called "bamboo damage." Increasing bamboo use will help combat this problem, so it is necessary to find new ways to use bamboo. [Means for solving the problem]
[0008] The present inventors have conducted extensive research to solve the above problems, and as a result have discovered that the use of fine bamboo charcoal powder makes it possible to obtain a hydraulic composition that inhibits the elution of lead contained in ordinary Portland cement into water, thereby completing the present invention.
[0009] That is, the first invention is a hydraulic composition containing ordinary Portland cement and bamboo charcoal fine powder, in which the ratio of the bamboo charcoal fine powder to 100 parts by mass of the ordinary Portland cement is 10 parts by mass or more and 70 parts by mass or less.
[0010] A second aspect of the present invention is a mortar comprising the above hydraulic composition, fine aggregate and water.
[0011] A third aspect of the present invention is a ready-mix concrete comprising the above hydraulic composition, fine aggregate, coarse aggregate, water and a chemical admixture. Effect of the Invention
[0012] According to the present invention, by using fine powder of bamboo charcoal, a hydraulic composition that suppresses the elution of lead contained in ordinary Portland cement into water can be obtained. Furthermore, by utilizing bamboo charcoal, bamboo materials can be effectively utilized, and carbon contained in bamboo charcoal can be trapped in concrete structures, etc., and carbon can be stored without being released into the atmosphere, which contributes to reducing CO2 emissions. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 shows the relationship between the addition rate of bamboo charcoal fine powder and the amount of lead eluted. [Diagram 2] Figure 2 shows the relationship between the bamboo charcoal addition rate and the 28-day mortar compressive strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] An embodiment of the present invention will be described.
[0015] <Hydraulic composition> The hydraulic composition of the present invention is characterized in that it contains 10 to 70 parts by mass of bamboo charcoal fine powder per 100 parts by mass of ordinary Portland cement. The hydraulic composition may contain blast furnace slag as specified in JIS R 5211 "blast furnace cement", JIS R 5212 "siliceous admixture", fly ash as specified in JIS A 6201 "fly ash for concrete", and limestone fine powder having a quality of 90% by mass or more of calcium carbonate and 1% by mass or less of aluminum oxide as a minor mixed component of 5 parts by mass or less per 100 parts by mass of the hydraulic composition.
[0016] As the ordinary Portland cement used in the hydraulic composition of the present invention, any ordinary Portland cement available on the market can be used without any restrictions.
[0017] As the bamboo charcoal fine powder used in the hydraulic composition of the present invention, commercially available bamboo charcoal fine powder can be used without any particular restrictions. The higher the carbonization temperature, the higher the electrical conductivity, which in turn increases the ability to adsorb harmful substances, and the higher the carbon content, which increases the effect of reducing carbon dioxide. Therefore, it is preferable to use charcoal produced at a high temperature of 800°C or higher.
[0018] The mixing ratio of the above materials is 10 parts by mass or more and 70 parts by mass or less of bamboo charcoal fine powder per 100 parts by mass of ordinary Portland cement.
[0019] If the amount of bamboo charcoal fine powder is 10 parts by mass or less, the effect of inhibiting the elution of lead is poor, and if it is 70 parts by mass or more, it is difficult to obtain sufficient strength. The ratio of bamboo charcoal fine powder is preferably 20 parts by mass or more because the effect of inhibiting the elution of lead is sufficient. If it is 20 parts by mass or more, the amount of lead eluted into water will be below the environmental standard. The upper limit of the ratio of bamboo charcoal fine powder may be set within the range of 10 parts by mass or more and 70 parts by mass or less according to the design standard strength of the hydraulic composition.
[0020] From the perspective of reducing carbon dioxide emissions, it is preferable to increase the amount of bamboo charcoal powder used.
[0021] The hydraulic composition of the present invention can be manufactured by mixing ordinary Portland cement and bamboo charcoal fine powder. The hydraulic composition of the present invention can achieve the required design standard strength by adjusting the ratio of bamboo charcoal fine powder, and can be used for many purposes such as concrete structures. When used as a ground improvement material that does not require strength compared to structural concrete, the ratio of bamboo charcoal fine powder can be increased.
[0022] <Mortar> The mortar of the present invention contains the above hydraulic composition as a cement-based binder, fine aggregate, and water.
[0023] The fine aggregate used in the mortar of the present invention can be any known fine aggregate used in the production of general mortar or concrete, such as fine aggregates such as crushed sand and pit sand, lightweight aggregates, slag aggregates specified in JIS A 5011, size-adjusted crushed stone, seed stones used in paving materials and building materials, etc., that do not affect the quality of the mortar. Note that fine aggregate is an aggregate that passes entirely through a sieve with 10 mm openings, 85 parts by weight through a sieve with 5 mm openings, and 80 parts by weight or more remaining on a sieve with 150 μm openings.
[0024] In the mortar of the present invention, the fine aggregate may be used alone or in a mixture of two or more kinds.
[0025] The water used in the mortar of the present invention may be any known water used in the production of general mortar or concrete, without any particular limitation. Specifically, industrial water, tap water, etc.
[0026] In the mortar of the present invention, in addition to the above-mentioned hydraulic composition, fine aggregate and water, polymers for admixture with cement and known admixtures generally used in the preparation of concrete, such as air-entraining water reducing agents, high-performance water reducing agents, high-performance air-entraining water reducing agents, air content regulators, setting accelerators and the like, may be added within a range that does not impair the effects of the present invention.
[0027] In the mortar of the present invention, the amount of fine aggregate used is not particularly limited, but is generally 1 to 5.5 times the amount of cement-based binder material.
[0028] The water-cement ratio (weight ratio of water to cement) is not particularly limited as long as it is within the range used in general mortar, and is usually 25% or more and 100% or less.
[0029] In the mortar of the present invention, as a method for producing the mortar by kneading the hydraulic composition, fine aggregate, water and materials used as necessary, a usual method carried out in a ready-mix concrete factory or on-site can be adopted without any particular limitation.
[0030] In the mortar of the present invention, the mixing device used for mixing the above-mentioned materials may be a mixer generally used for mixing mortar or concrete, such as a pan mixer, a forced twin-shaft mixer, a tilting mixer, a mortar mixer, or a hand mixer.
[0031] <Ready-mix concrete> The ready-mix concrete of the present invention contains the above hydraulic composition as a cement-based binder, fine aggregate, coarse aggregate, water, and admixtures.
[0032] The fine aggregate, water and admixtures used in the ready-mix concrete of the present invention are the same as those described above.
[0033] The coarse aggregate used in the ready-mix concrete of the present invention can be any known coarse aggregate used in the manufacture of general concrete, i.e., gravel collected from rivers, crushed stone produced by crushing rocks, etc. Coarse aggregate is one that has 85% or more of its weight remaining on a 5 mm sieve.
[0034] The above coarse aggregate and fine aggregate can be used alone or in a mixture of two or more kinds. In the ready-mix concrete of the present invention, the total amount of aggregate used is not particularly limited, but is generally 60 to 90 parts by mass of the total mass of the ready-mix concrete.
[0035] The fine aggregate and the coarse aggregate are usually mixed in a ratio of 35 to 70 parts by mass of fine aggregate and 30 to 65 parts by mass of coarse aggregate. The ratio is appropriately selected and determined depending on the physical properties required for the final concrete product, such as material separation resistance, pumpability, and compressive strength.
[0036] The water-cement ratio (weight ratio of water to cement) is not particularly limited as long as it is within the range used in general concrete, and is usually 25 parts by mass or more and 70 parts by mass.
[0037] In the ready-mix concrete of the present invention, as a method for producing ready-mix concrete by kneading the hydraulic composition, fine aggregate, coarse aggregate, water and admixtures, a conventional method carried out in ready-mix concrete factories or secondary concrete product factories can be used without any particular limitation.
[0038] In the ready-mix concrete of the present invention, the mixing device used to mix the above-mentioned materials can be a mixer generally used for mixing mortar or concrete. Specific examples include a pan mixer, a forced twin-shaft mixer, a tilting mixer, a mortar mixer, and a hand mixer. EXAMPLES
[0039] In order to explain the present invention more specifically, examples and comparative examples are given below, but the present invention is not limited to these examples.
[0040] 1.Materials used (a) Ordinary Portland cement As for the ordinary Portland cement, commercially available ordinary Portland cement was used.
[0041] (b) Fine bamboo charcoal powder Commercially available fine bamboo charcoal powder was used. The carbonization temperature was in the range of 800 to 900°C, and the particle size of the fine bamboo charcoal powder was 104 μm or less.
[0042] 2. Trace component elution test The trace elements measured were six items: cadmium, lead, hexavalent chromium, arsenic, selenium, fluorine, and boron, and the amount of eluted trace elements was measured according to the method stipulated in Environment Ministry Notification No. 77. Although Environment Ministry Notification No. 77 stipulates that the solid-liquid ratio of powder to solvent is 1:10, when converting the bamboo charcoal fine powder by internal ratio substitution, it is impossible to determine whether the decrease in the amount of trace elements is due to the insolubilization effect of bamboo charcoal or due to a decrease in the ratio of ordinary Portland cement, so an amount of hydraulic composition that results in a solid-liquid ratio of solvent to ordinary Portland cement of 1:10 was used as the sample.
[0043] (Reference example) The amount of trace components eluted from the bamboo charcoal fine powder was measured. The measurement results are shown in Table 1.
[0044] (Examples 1 to 3) Bamboo charcoal fine powder was added to ordinary Portland cement, and then mixed in a soil mixer to obtain a powdered hydraulic composition. The amount of trace components eluted from the obtained hydraulic composition was then measured.
[0045] The composition of the obtained hydraulic composition and the measurement results of the amount of eluted trace components are shown in Table 1.
[0046] Comparative Example 1 A hydraulic composition was prepared using only ordinary Portland cement but not containing fine bamboo charcoal powder, and the amount of eluted trace components was measured.
[0047] The composition of the obtained hydraulic composition and the measurement results of the amount of eluted trace components are shown in Table 1.
[0048] [Table 1]
[0049] No elution of trace components was observed from the bamboo charcoal fine powder used as a reference example.
[0050] In Example 1, in which 11.1 parts by mass of bamboo charcoal fine powder was added, the amount of lead elution was reduced by half compared to Comparative Example 1, and in Examples 2 and 3, in which 20.5 and 25.0 parts by mass of bamboo charcoal fine powder were added, respectively, the amount of lead elution was further reduced and was below the environmental standard. As for fluorine, the addition of bamboo charcoal fine powder did not have a reducing effect in Examples 1 to 3.
[0051] The results of the elution test of the hydraulic composition powder of Comparative Example 1 to which no fine bamboo charcoal powder was added showed that the amount of eluted lead exceeded the environmental standard, being 0.022 mg / L.
[0052] The relationship between the amount of eluted lead and the amount of added bamboo charcoal powder is shown in Figure 1. As the amount of added bamboo charcoal powder increases, the effect of suppressing elution of lead increases.
[0053] 3.Mortar strength test (1) Mortar Mixture Mortar was prepared by mixing water, hydraulic composition, and fine aggregate in the ratios shown in Table 2, and the compressive strength of the mortar was measured after 28 days. Tap water was used as the water, and standard sand was used as the fine aggregate. The measurement results of the mortar compressive strength after 28 days are also shown in Table 2.
[0054] (2) Mixing The mixing was carried out in accordance with JIS R 5201 (physical testing method for cement). The mixing method is described below.
[0055] A Hobart mixer was used for mixing. Ordinary Portland cement and bamboo charcoal powder were added to the mixing bowl, and the mixer was started at low speed. Thirty seconds after the mixer was started, standard sand was added at a steady speed over a period of 30 seconds. The mixture was then mixed at high speed for 30 seconds, followed by a 90-second pause. During the first 30 seconds of the pause, the mortar adhering to the mixing bowl and paddle was scraped off with a spoon. After the pause, the mixture was mixed again at high speed for 60 seconds.
[0056] (3) Molding The molding was performed in accordance with JIS R 5201 (physical testing method for cement). The molding method is explained below.
[0057] A 40 x 40 x 160 mm formwork was used. The mortar was immediately poured into the formwork after mixing. A table vibrator was used for pouring. The pouring method was as follows: The first layer of mortar was packed to about half the height of the formwork in 15 seconds from the start of vibration. After a 15-second interval, the remaining amount of mortar was packed in over the same 15 seconds as the first layer. Vibration was continued for a further 75 seconds. Finally, the excess was carefully scraped off so as not to damage the specimen, and the top surface was made smooth.
[0058] (4)Curing After molding, the mixture was covered with an iron plate for 24 hours from mixing to prevent evaporation of moisture and stored at 20°C. After 24 hours from mixing, the mixture was demolded and then cured in water at 20°C for a specified period of time.
[0059] (5) Compressive strength measurement The compressive strength was measured in accordance with JIS R 5201 (physical testing method for cement). The compressive strength of mortar aged 28 days was measured.
[0060] [Table 2]
[0061] Comparative Example 2 shows the results of measurements on a hydraulic composition using only ordinary Portland cement and not including bamboo charcoal fine powder. The compressive strength was 63.6 N / mm 2 In contrast, in Examples 4 and 5, which used the hydraulic compositions of Examples 1 and 3, in which bamboo charcoal was added to ordinary Portland cement, the strength was 50.7 N / mm 2 , and Example 5 is 43.1 N / mm 2 It was.
[0062] Figure 2 shows the relationship between the bamboo charcoal addition rate and the 28-day mortar compressive strength. As the bamboo charcoal addition rate increases, the 28-day mortar compressive strength decreases, demonstrating a correlation. Linear approximation was also performed to estimate the value of mortar compressive strength when the bamboo charcoal fine powder addition rate exceeds 25 parts by mass. As a result, it was predicted that the mortar would not harden when it exceeds 70 parts by mass. When used as a ground improvement material that does not require as much strength as structural concrete, the bamboo charcoal fine powder addition rate can be increased as long as it is within the range of 70 parts by mass or less.
Claims
1. A hydraulic composition comprising ordinary Portland cement and bamboo charcoal fine powder, characterized in that the ratio of the bamboo charcoal fine powder to 100 parts by mass of the ordinary Portland cement is within the range of 10 parts by mass to 70 parts by mass.
2. A mortar comprising the hydraulic composition according to claim 1, aggregate, and water.
3. A ready-mix concrete comprising the hydraulic composition of claim 1, aggregate, water and chemical admixtures.
Citation Information
Patent Citations
Carbon-containing concrete product
JP2000211960A
Concrete product containing porous charcoal
JP2001032402A
Shirasu concrete decorative material and its manufacturing method
JP2005007667A
Water-permeable block
JP2005145771A
Material for construction
JP2007197291A