R-t-b based permanent magnet
The R-T-B permanent magnet with a core-shell structure and controlled Tb distribution addresses the limitations of Br, Hcj, and Hk/Hcj by enhancing magnetic anisotropy and reducing property variations, achieving superior magnetic performance.
Patent Information
- Application Number
- JP2023200937
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2023-11-28
- Publication Date
- 2024-10-15
AI Technical Summary
Existing R-T-B permanent magnets face challenges in achieving high residual magnetic flux density (Br), coercive force (Hcj), and squareness ratio (Hk/Hcj), particularly due to limitations in the distribution and concentration of Tb in the grain boundary phase.
The R-T-B permanent magnet is designed with a core-shell structure, where the shell contains Tb with a thickness of 70 nm or more and a maximum concentration of 1.7 at% or more, and the Tb concentration gradually increases from the core to the grain boundary phase, with a ratio of 1.0≦[Tb b ]/[Tb s ]≦1.5, and includes Fe and Co in the grain boundary phase.
This design enhances Br, Hcj, and Hk/Hcj by promoting magnetic anisotropy and reducing magnetic property variations, resulting in improved magnetic performance with a high Tb concentration in the shell and controlled diffusion processes.
Smart Images

Figure 2024146728000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an RTB-based permanent magnet. [Background technology]
[0002] Patent Document 1 describes an invention related to a method for producing a rare earth permanent magnet material. It states that a rare earth permanent magnet material with high residual magnetic flux density Br and coercive force Hcj can be provided by supplying a compound of a rare earth element (especially Dy and / or Tb) to the surface of a sintered magnet body and then performing a heat treatment. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2006 / 043348 Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to obtain an RTB permanent magnet having a high residual magnetic flux density Br, coercive force Hcj, and squareness ratio Hk / Hcj. [Means for solving the problem]
[0005] In order to achieve the above object, the present invention provides an RTB permanent magnet having a main phase consisting of a core and a shell, and a grain boundary phase adjacent to the main phase, the shell contains Tb, The shell has a thickness of 70 nm or more, The maximum Tb concentration in the shell is 1.7 at % or more.
[0006] The Tb concentration in the shell may increase gradually from the vicinity of the core to the vicinity of the grain boundary phase.
[0007] When measurement points of Tb concentration are set at 10 nm intervals from the core toward the grain boundary phase inside the shell, the measurement points closer to the grain boundary phase may have a higher Tb concentration, and the differences in Tb concentration between adjacent measurement points may all be 0.01 at % or more and 0.50 at % or less.
[0008] The maximum Tb concentration in the shell is [Tb s ], the maximum Tb concentration in the grain boundary phase is [Tb b ] as 1.0≦[Tb b ] / [Tb s ]≦1.5.
[0009] The Tb content may be 0.6 mass % or more and 2.1 mass % or less.
[0010] The transition metal element may include Fe, or Fe and Co.
[0011] The grain boundary phase may contain one or more selected from Fe and Co, and the minimum value of the total concentration of Fe and Co in the grain boundary phase may be 65.0 at % or less.
[0012] The squareness ratio Hk / Hcj may be 97.0% or more. [Brief description of the drawings]
[0013] [Figure 1] FIG. 2 is a schematic diagram showing the positional relationship between the main phase and the grain boundary phase and the line segment AB. [Diagram 2] 1 is a graph showing the change in concentration of Tb along line segment AB. [Diagram 3] 1 is a graph showing the change in Cu concentration along line segment AB. [Figure 4] 1 is a graph showing the change in the total concentration of Fe and Co, and the change in the concentration of Nd along line segment AB. [Diagram 5] FIG. 2 is a schematic diagram showing a magnet shape of an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, the present invention will be described based on specific embodiments.
[0015] <R-T-B-based permanent magnet> The R-T-B-based permanent magnet according to this embodiment has main phase particles including crystal particles having an R2T 14 B-type crystal structure. Further, it has grain boundaries formed by two or more adjacent main phase particles.
[0016] R-T-B-based permanent magnet and R2T 14 In the R2T
[0017] R-T-B-based permanent magnet and R2T 14 B-type crystal structure, R represents a rare earth element, T represents a transition metal element, and B represents boron. The rare earth element included as R may be Sc, Y, and lanthanoids. The transition metal element included as T does not include a rare earth element. The transition metal element included as T may be an iron group element. The iron group element included as T may be one or more selected from Fe and Co. The iron group element included as T may be Fe, or Fe and Co. A part of the boron included as B may be substituted with carbon.
[0018] In this embodiment, rare earth elements are classified into heavy rare earth elements and light rare earth elements. Heavy rare earth elements refer to Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu. Light rare earth elements refer to rare earth elements other than heavy rare earth elements. Iron group elements refer to Fe, Co, and Ni.
[0019] Hereinafter, the magnet composition of the R-T-B-based permanent magnet according to this embodiment will be shown. Note that there is no particular limitation on the measurement method of the R-T-B-based permanent magnet. For example, XRF can be used.
[0020] There is no particular limit to the content of rare earth elements in the RTB permanent magnet. It may be 25.0 mass% or more and 35.0 mass% or less, 29.0 mass% or more and 33.0 mass% or less, or 30.0 mass% or more and 32.0 mass% or less. When the R content is 25.0 mass% or more, the crystals contained in the main phase of the RTB permanent magnet, i.e., R2T 14 The formation of crystals having a B-type crystal structure is facilitated. In addition, the precipitation of α-Fe and other elements with soft magnetic properties is suppressed, making it easier to suppress the deterioration of magnetic properties. When the R content is 35.0 mass% or less, the Br of the RTB permanent magnet tends to improve.
[0021] There is no particular limit to the content of the heavy rare earth element. For example, it may be 0.1 mass% or more and 5.0 mass% or less, or 0.6 mass% or more and 2.1 mass% or less. There is no particular limit to the type of heavy rare earth element, but the RTB permanent magnet according to this embodiment contains at least Tb. It may or may not contain heavy rare earth elements other than Tb. When a heavy rare earth element other than Tb is contained, it may contain, for example, Dy.
[0022] There is no particular limit to the Tb content. For example, it may be 0.1% by mass or more and 5.0% by mass or less, or 0.6% by mass or more and 2.1% by mass or less. When Tb is high, Br tends to decrease. When Tb is low, Hcj tends to decrease.
[0023] The total content of heavy rare earth elements other than Tb may be 0% by mass or more and 0.1% by mass or less. When the total content of heavy rare earth elements other than Tb is 0.1% by mass or less, Br tends to be improved.
[0024] There is no particular limit to the content of the light rare earth element. In addition, there is no particular limit to the type of the light rare earth element. For example, it may be one or more elements selected from Nd and Pr, or it may be Nd.
[0025] The total content of light rare earth elements other than Nd may be 0% by mass or more and 7.0% by mass or less, or 0% by mass or more and 0.1% by mass or less. The total content of light rare earth elements other than Nd and Pr may be 0% by mass or more and 0.1% by mass or less.
[0026] There is no particular limit to the boron content in the RTB permanent magnet. It may be 0.50 mass% or more and 1.50 mass% or less, or 0.85 mass% or more and 1.05 mass% or less. When the boron content is 0.50 mass% or more, Hcj tends to improve. Also, when the boron content is 1.50 mass% or less, Br tends to improve.
[0027] There is no particular limit to the carbon content in the RTB permanent magnet, and it may be, for example, between 0% and 0.10% by mass.
[0028] There is no particular limit to the Co content in the RTB permanent magnet. It may be 0% by mass or more and 4.00% by mass or less, 0% by mass or more and 0.50% by mass or less, or 0% by mass or more and 0.30% by mass or less. The higher the Co content, the higher the raw material cost tends to be. The lower the Co content, the lower the corrosion resistance tends to be.
[0029] The RTB permanent magnet according to this embodiment may contain Ga, Cu, Al and / or Zr as metal elements other than the above elements. There are no particular limitations on the content of each element.
[0030] The Ga content in the RTB permanent magnet may be from 0 mass % to 0.15 mass %, or from 0 mass % to 0.10 mass %.
[0031] The Cu content in the RTB permanent magnet may be from 0 mass % to 0.50 mass %, from 0 mass % to 0.20 mass %, or more than 0 mass % to 0.05 mass %.
[0032] The Al content in the RTB permanent magnet may be from 0% to 0.40% by mass, or from 0.25% to 0.40% by mass.
[0033] The Zr content in the RTB permanent magnet may be from 0% to 0.50% by mass, or from 0% to 0.20% by mass.
[0034] The RTB permanent magnet may contain oxygen and nitrogen in addition to the above elements.
[0035] The oxygen content in the RTB permanent magnet may be 0% by mass or more and 0.10% by mass or less.The nitrogen content in the RTB permanent magnet may be 0% by mass or more and 0.10% by mass or less.
[0036] The Fe content in the RTB permanent magnet may be the substantial remainder of the RTB permanent magnet. Specifically, the total content of other elements, i.e., elements other than rare earth elements, Fe, Co, B, C, Ga, Cu, Al, Zr, O, and N, may be 1.0 mass% or less.
[0037] Other types of elements include inevitable impurities such as Mn, Ca, Cl, S, and F.
[0038] As shown in Fig. 1, the RTB permanent magnet according to this embodiment has a main phase 11 consisting of a core and a shell, and a grain boundary phase 13 adjacent to the main phase 11. The shell contains Tb. The grain boundary phase 13 contains one or more elements selected from Fe and Co. The shell has a thickness of 70 nm or more. Furthermore, the maximum Tb concentration in the shell is 1.7 at% or more.
[0039] The minimum value of the total concentration of Fe and Co in the grain boundary phase 13 may be 65.0 at% or less. The maximum value of the total concentration of the light rare earth elements in the grain boundary phase 13 may be 25.0 at% or more.
[0040] The grain boundary phase 13 may contain a transition metal element other than Fe and Co. For example, it may contain Cu, Zr, Mn, Ni, etc. The ratio of the total concentration of Fe and Co to the total concentration of the transition metal elements contained in the grain boundary phase 13 may be 90% or more on an atomic number basis.
[0041] The RTB permanent magnet according to this embodiment has the above-mentioned characteristics, and therefore can achieve high Br, Hcj and Hk / Hcj with a relatively small amount of heavy rare earth element used.
[0042] The Tb concentration in the shell may gradually increase from the vicinity of the core toward the vicinity of the grain boundary phase 13 .
[0043] The maximum Tb concentration in the shell is [Tb s ](at%), and the maximum Tb concentration in the grain boundary phase 13 is [Tb b ](at%), 1.0≦[Tb b ] / [Tb s ]≦1.5.
[0044] There is no particular restriction on the Tb concentration in the core. For example, it may be 0 at% or more and 2.0 at% or less. It is preferably 0.3 at% or more and 1.0 at% or less. When the core contains 0.3 at% or more and 1.0 at% or less of Tb, dissolution of the main phase 11 is suppressed in the high-temperature atmospheric pressure diffusion step described below. Since dissolution of the main phase 11 is suppressed, the shell of the main phase 11 does not become too thick, and the maximum Tb concentration in the shell of the main phase 11 [Tb s The maximum Tb concentration in the shell of the main phase 11 [Tb s ] is high, the Hcj of the RTB permanent magnet tends to be high.
[0045] Hereinafter, a method for distinguishing between the core, shell, and grain boundary phase 13 in the RTB permanent magnet according to this embodiment, and a method for measuring various parameters will be described. In the following explanation, it is assumed that the grain boundary phase 13 contains one or more transition metal elements other than rare earth elements selected from Fe and Co, and contains only Tb and Nd as rare earth elements.
[0046] First, a measurement range is set for the RTB permanent magnet. The method for setting the measurement range will be described later. The RTB permanent magnet is cut at a position that includes the set measurement range to obtain a cross section.
[0047] In the obtained cross section, a three-dimensional atom probe (3DAP) is used to select the main phase 11 and the grain boundary phase 13 adjacent to the main phase 11 included in the measurement range.
[0048] Next, as shown in Fig. 1, a line segment AB is set which passes through two main phases 11 and a grain boundary phase 13 existing between the two main phases 11 and is approximately perpendicular to the boundary line between the main phases 11 and the grain boundary phase 13. Note that Fig. 1 is a schematic diagram for explaining a method for setting the line segment AB, and the length of the actual line segment AB does not necessarily match the length of the line segment AB shown in Fig. 1.
[0049] Next, the Tb concentration is analyzed along the line segment AB. An example of the results is shown in Figure 2. In Figure 2, the horizontal axis indicates the distance from point A, and the vertical axis indicates the Tb concentration.
[0050] At the same time, an element (Cu in FIG. 3) that is relatively unlikely to be contained in the main phase 11, particularly the shell, and relatively likely to be contained in the grain boundary phase 13 is selected, and the concentration of that element is analyzed linearly along the line segment AB. An example of the results is shown in FIG. 3. As in FIG. 2, the horizontal axis in FIG. 3 also shows the distance from point A, and the vertical axis shows the concentration of the element. Furthermore, the Fe concentration, Co concentration, and the concentration of the light rare earth element (Nd concentration) are analyzed linearly along the line segment AB. An example of the results is shown in FIG. 4. FIG. 4 shows the concentrations of each element in the grain boundary phase 13 and its vicinity.
[0051] The boundary between the shell and the grain boundary phase 13 may be determined visually from Fig. 3. From Fig. 3, the Cu concentration drops sharply from the grain boundary phase 13 toward the shell. The position where the Cu concentration becomes roughly constant is determined as the boundary between the shell and the grain boundary phase 13. The position of the boundary determined from Fig. 3 is shown by a dashed line in Fig. 3. The position of the boundary in Fig. 2 is the same as that in Fig. 3.
[0052] In FIG. 3, the boundary between the shell and the grain boundary phase 13 is determined from the change in Cu concentration, but the boundary between the shell and the grain boundary phase 13 may be determined using an element other than Cu, or the boundary between the shell and the grain boundary phase 13 may be determined by observing factors other than the change in concentration of each element.
[0053] As can be seen from FIG. 2, the Tb concentration decreases from the boundary between the shell and the grain boundary phase 13 toward the inside of the main phase, and becomes roughly constant at a location sufficiently away from the boundary. The location where the Tb concentration is roughly constant is the core. The location where the Tb concentration decreases from the boundary toward the main phase is the shell. Whether or not the Tb concentration in the shell gradually increases from the vicinity of the core toward the vicinity of the grain boundary phase 13 is determined visually from the measurement results of the Tb concentration. In FIG. 2, the Tb concentration in the shell gradually increases from the vicinity of the core toward the vicinity of the grain boundary phase 13. The boundary between the core and the shell is determined visually from FIG. 2.
[0054] The boundary between the shell and the grain boundary phase 13 may be determined so that the Cu concentration in the grain boundary phase 13 is always 0.15 at % or more, and the Cu concentration in the portion of the shell in contact with the grain boundary phase 13 is less than 0.15 at %.
[0055] The inside of the core may be a portion that is included in the core and is 100 nm or more away from the boundary between the core and the shell. The Tb concentration inside the core before the diffusion treatment described below is approximately equal to the Tb concentration in the base material before the diffusion treatment. Since it is difficult to diffuse Tb to the inside of the core by the diffusion treatment step, the Tb concentration inside the core after the diffusion treatment is also approximately equal to the Tb concentration in the base material before the diffusion treatment. The Tb concentration inside the core is approximately constant. The Tb concentration inside the core can be measured by a method such as 3DAP or EPMA. The boundary between the core and the shell may be determined so that the shell is the portion where the Tb concentration is increased by 0.10 at % or more from the Tb concentration inside the core.
[0056] The inside of the shell may be a portion that is included in the shell and is at a distance of 1.0 nm or more from the grain boundary phase 13 that contacts the shell. The Cu concentration is approximately constant inside the shell.
[0057] When measuring points of Tb concentration are set at 10 nm intervals from the core toward the grain boundary phase 13 inside the shell, the measuring points closer to the grain boundary phase 13 may have a higher Tb concentration. Furthermore, the difference in Tb concentration between adjacent measuring points may all be 0.01 at% or more and 0.50 at% or less. When the measuring points closer to the grain boundary phase 13 have a higher Tb concentration and the difference in Tb concentration between adjacent measuring points are all 0.01 at% or more and 0.50 at% or less, the Tb concentration in the shell may gradually increase from the vicinity of the core toward the vicinity of the grain boundary phase 13.
[0058] When 3DAP is used to measure the Tb concentration, the Tb concentration may be measured by setting provisional measurement points at 1 nm intervals. The average position of 10 consecutive provisional measurement points may be set as the position of the measurement point, and the average Tb concentration of the 10 consecutive provisional measurement points may be set as the Tb concentration of the measurement point. When the position of the measurement point is set by the above method and the Tb concentration of the measurement point is measured, the influence of measurement noise is easily reduced, and an error is less likely to occur in the difference in Tb concentration between adjacent measurement points.
[0059] When determining the boundary between the shell and the grain boundary phase 13 using an element other than Cu (an element that is relatively likely to be included in the grain boundary phase 13), Cu may be replaced with an element other than Cu (an element that is relatively likely to be included in the grain boundary phase 13) in the above-mentioned method for determining each boundary.
[0060] From the determined boundaries between the grain boundary phase 13 and the shell, and between the shell and the core, the thickness of the shell in the main phase 11, the Tb concentration in the core, the minimum value of the total concentration of Fe and Co in the grain boundary phase 13, the maximum value of the Nd concentration in the grain boundary phase 13, [Tb s ] and [Tb b ] can be determined. Then, [Tb b ] / [Tb s ] can be calculated.
[0061] A method for setting the measurement range will be described below. The measurement range may be in any part of the RTB permanent magnet. The measurement range may also be in a part away from the surface of the RTB permanent magnet. For example, it may be a part that is 500 μm or more away from the surface of the RTB permanent magnet.
[0062] There are no particular limitations on the content of the main phase 11 having the above configuration in the RTB permanent magnet.
[0063] For example, the content of main phases 11 having the above configuration may be 80% or more by number with respect to the main phases 11 contained in the RTB permanent magnet.
[0064] For example, the content of main phases 11 having the above configuration may be 65% or more by number relative to main phases 11 contained in a portion 500 μm or more away from the surface of the RTB permanent magnet.
[0065] For example, a line segment may be drawn from the center of gravity of the surface of the R-T-B-based permanent magnet to the center of gravity of the R-T-B-based permanent magnet, and several measurement points may be set at equal intervals on the line segment to check whether the main phase 11 at each measurement point has the above configuration. The content ratio of the main phase 11 having the above configuration at each measurement point may be 80% or more based on the number.
[0066] For example, with respect to the main phase 11 contained in the central portion of the R-T-B-based permanent magnet, that is, the portion that is similar in shape to the R-T-B-based permanent magnet, has the same center of gravity position, and has a volume of about 10%, for example, 5% or more and 15% or less, the content ratio of the main phase 11 having the above configuration may be 55% or more based on the number.
[0067] <Manufacturing Method of R-T-B-Based Permanent Magnet> Hereinafter, the manufacturing method of the R-T-B-based permanent magnet will be described in detail. For matters not specifically mentioned, known methods may be used.
[0068] [Preparation Step of Raw Material Powder] The raw material powder can be produced by a known method. In this embodiment, an R-T-B-based permanent magnet is manufactured by a single alloy method using one type of raw material alloy mainly composed of the R2T 14 B phase, but it may also be manufactured by a two alloy method using two types of raw material alloys.
[0069] First, raw material metals corresponding to the composition of the raw material alloy according to this embodiment are prepared, and the raw material alloy corresponding to this embodiment is produced from the raw material metals. There is no particular limitation on the method for producing the raw material alloy. For example, the raw material alloy can be produced by the strip casting method.
[0070] The larger the amount of Tb in the raw material alloy (in the case of using the two alloy method, mainly the raw material alloy that becomes the main phase), the less likely the Tb concentration in the grain boundary phase will be higher than the Tb concentration in the main phase in the grain boundary diffusion described later.
[0071] When the amount of Tb in the raw material alloy is large, the dissolution of the main phase by the diffusion material is suppressed, and the diffusion of Tb from the grain boundary phase to the main phase is suppressed.
[0072] The diffusion material suppresses dissolution of the main phase, which in turn suppresses excessive dissolution of the main phase near the diffusion surface. By suppressing excessive dissolution of the main phase near the diffusion surface, Tb can be diffused to the center of the magnet.
[0073] The diffusion of Tb from the grain boundary phase to the main phase is suppressed, and [Tb b ] / [Tb s ] tends to become smaller.
[0074] After the raw alloy is prepared, the prepared raw alloy is pulverized (pulverization step). The pulverization step may be performed in two stages or in one stage. There is no particular limitation on the pulverization method. For example, it is performed by a method using various pulverizers. For example, the pulverization step may be performed in two stages, a coarse pulverization step and a fine pulverization step, and the coarse pulverization step may be performed by, for example, hydrogen pulverization. Specifically, after hydrogen is absorbed into the raw alloy at room temperature, dehydrogenation may be performed in an Ar gas atmosphere at 400°C to 650°C for 0.5 hours to 2 hours. In addition, the fine pulverization step may be performed by adding a lubricant such as oleic acid amide or zinc stearate as a pulverization aid to the powder after the coarse pulverization, for example, using a jet mill, a wet attritor, or the like. There is no particular limitation on the particle size of the obtained finely pulverized powder (raw powder). For example, fine pulverization may be performed so that the particle size (D50) of the finely pulverized powder (raw powder) is 1 μm to 10 μm. Incidentally, from the hydrogen absorption pulverization to the sintering step described later, a low-oxygen atmosphere with an oxygen concentration of less than 200 ppm may be used all the time.
[0075] [Molding process] In the molding process, the finely pulverized powder (raw material powder) obtained in the pulverization process is molded into a predetermined shape. Although there is no particular limitation on the molding method, in this embodiment, the finely pulverized powder (raw material powder) is filled into a die and pressurized in a magnetic field.
[0076] The pressure during molding is preferably 30 MPa or more and 300 MPa or less. The magnetic field applied is preferably 950 kA / m or more and 1600 kA / m or less. The magnetic field applied is not limited to a static magnetic field, but can also be a pulsed magnetic field. A static magnetic field and a pulsed magnetic field can also be used in combination. The shape of the molded body obtained by molding the finely pulverized powder (raw material powder) is not particularly limited, and can be any shape such as a rectangular parallelepiped, a plate, a column, etc., depending on the shape of the desired RTB-based permanent magnet.
[0077] [Sintering process] The sintering process is a process in which the molded body is sintered in a vacuum or in an inert gas atmosphere to obtain a sintered body. The sintering temperature needs to be adjusted depending on various conditions such as the composition, the crushing method, the particle size and particle size distribution, etc., but the molded body is sintered, for example, by heating it in a vacuum or in the presence of an inert gas at 1000°C to 1200°C for 1 hour to 10 hours. This produces a high-density sintered body (permanent magnet).
[0078] [Aging treatment process] The aging treatment step is performed by heating the sintered body (permanent magnet) after the sintering step in a vacuum or in an inert gas atmosphere at a temperature lower than the sintering temperature. There are no particular limitations on the temperature and time of the aging treatment, but it can be performed, for example, at 450°C to 900°C for 0.2 hours to 3 hours. This aging treatment step may be omitted.
[0079] The aging treatment process may be performed in one stage or two stages. When performing the aging treatment in two stages, for example, the first stage may be performed at 700°C to 900°C for 0.2 hours to 3 hours, and the second stage may be performed at 450°C to 700°C for 0.2 hours to 3 hours. The first and second stages may be performed consecutively, or the first stage may be cooled to near room temperature and then reheated before performing the second stage.
[0080] [Processing process (before grain boundary diffusion)] If necessary, a step of processing the sintered body according to the present embodiment into a desired shape may be included. Examples of the processing method include shaping such as cutting and grinding, and chamfering such as barrel polishing.
[0081] [Diffusion process] In this embodiment, the method further includes a diffusion process step for diffusing Tb. The diffusion process can be performed by attaching a compound containing Tb or the like to the surface of the sintered body and then performing a heat treatment. Any type of compound containing Tb can be used. For example, a hydride of Tb can be used. Any method can be used to attach the compound containing Tb. For example, the compound can be attached by applying a slurry containing Tb. The thickness of the shell and the Tb concentration in the shell can be controlled by controlling the amount of the slurry applied and the concentration of Tb contained in the slurry. The Tb concentration in the core does not substantially change before and after the grain boundary diffusion process.
[0082] There is no particular limitation on the method for attaching Tb, and examples of the method include deposition, sputtering, electrodeposition, spray coating, brush coating, jet dispenser, nozzle, screen printing, squeegee printing, and sheet construction.
[0083] When applying the slurry, the Tb-containing compound is preferably in the form of particles, and the average particle size is preferably from 100 nm to 50 μm, and more preferably from 1 μm to 30 μm.
[0084] The solvent used for the slurry is preferably one that can disperse the Tb-containing compound uniformly without dissolving it, such as alcohol, aldehyde, ketone, etc., and among these, ethanol is preferred.
[0085] The content of the compound containing Tb in the slurry is not particularly limited. For example, it may be 50% by mass or more and 90% by mass or less. The slurry may further contain components other than Tb as necessary. For example, a dispersant for preventing aggregation of Tb particles may be included.
[0086] By subjecting the sintered body to the above-mentioned diffusion treatment step, Tb is diffused to the grain boundaries throughout the sintered body, forming a shell with a high Tb concentration in the main phase, and a main phase consisting of a core and a shell is obtained.
[0087] In this embodiment, the diffusion process is performed in a plurality of stages. Specifically, the diffusion process is performed by repeating a diffusion process in a low-temperature reduced pressure atmosphere and a diffusion process in a high-temperature atmospheric pressure atmosphere. First, the temperature in the atmosphere is increased from room temperature to the diffusion process temperature in the low-temperature reduced pressure atmosphere. At the same time, the pressure in the atmosphere is reduced from atmospheric pressure to the diffusion process pressure in the low-temperature reduced pressure atmosphere. Next, the low-temperature reduced pressure atmosphere is maintained for a predetermined holding time.
[0088] The diffusion treatment temperature in the low-temperature reduced pressure atmosphere may be, for example, 500° C. or more and 700° C. or less. The diffusion treatment pressure in the low-temperature reduced pressure atmosphere may be, for example, 0.1 kPa or more and 20 kPa or less. There is no particular limit to the retention time in the low-temperature reduced pressure atmosphere. For example, it may be 3 hours or more and 9 hours or less.
[0089] Next, the temperature in the atmosphere is increased from the diffusion treatment temperature in the low-temperature reduced pressure atmosphere to the diffusion treatment temperature in the high-temperature atmospheric pressure atmosphere. At the same time, the pressure in the atmosphere is increased from the diffusion treatment pressure in the low-temperature reduced pressure atmosphere to the diffusion treatment pressure in the high-temperature atmospheric pressure atmosphere. Next, the high-temperature atmospheric pressure atmosphere is maintained for a predetermined holding time.
[0090] The diffusion treatment temperature in the high-temperature atmospheric pressure atmosphere may be, for example, 750° C. or more and 1000° C. or less. The diffusion treatment pressure in the high-temperature atmospheric pressure atmosphere may be, for example, 80 kPa or more and 120 kPa or less. There is no particular limit to the retention time in the high-temperature atmospheric pressure atmosphere. For example, it may be 3 hours or more and 9 hours or less.
[0091] The diffusion treatment in a low-temperature, reduced-pressure atmosphere that is performed first in the diffusion treatment process can promote dissolution of the grain boundaries and diffusion materials (such as compounds containing Tb) while suppressing dissolution of the main phase. Therefore, in the diffusion treatment in a low-temperature, reduced-pressure atmosphere that is performed first, Tb is less likely to diffuse into the main phase near the diffusion surface (the surface to which the compound containing Tb is attached) of the RTB permanent magnet. The difference in Tb concentration between the grain boundary phase near the diffusion surface of the RTB permanent magnet and the grain boundary phase inside the RTB permanent magnet becomes the driving force for Tb diffusion. Therefore, Tb is more likely to diffuse from the grain boundary phase near the diffusion surface of the RTB permanent magnet to the grain boundary phase inside the RTB permanent magnet.
[0092] In the diffusion treatment process, which is carried out next in a high-temperature, atmospheric-pressure atmosphere, dissolution of the main phase progresses, particularly in the portion adjacent to the grain boundary phase. The Tb that was diffused to the grain boundary phase throughout the RTB permanent magnet in the diffusion treatment in a low-temperature, reduced-pressure atmosphere diffuses into the main phase adjacent to the grain boundary phase. During the subsequent cooling, the dissolved main phase is redeposited on the surface of the undissolved main phase. The amount of Tb contained in the redeposited portion increases.
[0093] As a result, compared to the diffusion method of the conventional diffusion treatment process, it is easier to diffuse Tb into the RTB permanent magnet, especially into the magnet's interior. Then, inside the RTB permanent magnet, the shell contained in the main phase can be made thicker and the Tb concentration in the shell can be increased. Furthermore, it is easier to reduce the difference in Tb concentration in the main phase between the surface and the interior of the RTB permanent magnet. Therefore, an RTB permanent magnet with high Br, Hcj, and Hk / Hcj can be obtained.
[0094] In particular, it is believed that the reason why Hcj can be increased is that the high Tb concentration in the shell increases the magnetic anisotropy of the outer edge of the main phase, which is the starting point of magnetization reversal, and that the thick shell promotes magnetic decoupling between adjacent main phases.
[0095] In particular, the Hk / Hcj can be increased, especially to 97.0% or more, because this reduces the difference in the Tb concentration in the main phase between the interior and surface of the magnet, thereby reducing variation in the magnetic properties throughout the magnet.
[0096] Hereinafter, the diffusion treatment in the low-temperature reduced pressure atmosphere and the diffusion treatment in the high-temperature atmospheric pressure atmosphere may be repeated multiple times. When the diffusion treatment in the low-temperature reduced pressure atmosphere and the diffusion treatment in the high-temperature atmospheric pressure atmosphere are repeated multiple times, the diffusion treatment temperature, the diffusion treatment pressure, and / or the holding time may be appropriately changed depending on the number of repetitions. In addition, by repeating the diffusion treatment in the low-temperature reduced pressure atmosphere and the diffusion treatment in the high-temperature atmospheric pressure atmosphere multiple times, the Tb concentration in the shell of the main phase tends to gradually increase from the vicinity of the core of the main phase to the vicinity of the grain boundary phase adjacent to the main phase.
[0097] Furthermore, in the diffusion method of the conventional diffusion treatment process, the diffusion material dissolves the main phase near the magnet surface in the vicinity of the diffusion material. As a result, an excess of Tb remains near the magnet surface in the vicinity of the diffusion material. This in turn slows down the diffusion of Tb from the magnet surface in the vicinity of the diffusion material to the center of the magnet. As Tb is less likely to diffuse into the grain boundary phase in the center of the magnet, the diffusibility of Tb from the grain boundary phase in the center of the magnet to the main phase is further reduced. As a result, the grain boundary phase in the center of the magnet tends to contain more Tb than the main phase in the center of the magnet, and the [Tb b ] / [Tb s ] is likely to be higher than 1.5. Therefore, the coercive force and squareness ratio are likely to be lower than those of the RTB permanent magnet according to this embodiment.
[0098] Furthermore, an aging treatment step may be carried out after the heat treatment in the diffusion treatment step.
[0099] After the diffusion process, the surface to which Tb is attached (diffusion surface) may be polished to remove the residue. By diffusing Tb using the above method, the amount of Tb contained in the residue that is removed can be relatively reduced, and expensive Tb can be used efficiently to improve the magnetic properties of RTB permanent magnets.
[0100] Although the preferred embodiments of the RTB permanent magnet of the present invention have been described above, the RTB permanent magnet of the present invention is not limited to the above embodiments. The RTB permanent magnet of the present invention can be modified and combined in various ways without departing from the gist of the invention.
[0101] Furthermore, magnets obtained by cutting and dividing the RTB permanent magnet according to this embodiment can be used.
[0102] Specifically, the RTB permanent magnet according to this embodiment is suitable for use in motors, compressors, magnetic sensors, speakers, and the like.
[0103] Furthermore, the RTB permanent magnet according to this embodiment may be used alone, or two or more RTB permanent magnets may be bonded together as necessary. There are no particular limitations on the bonding method. For example, there is a method of mechanically bonding them or a method of bonding them with a resin mold.
[0104] By combining two or more RTB permanent magnets, it is possible to easily manufacture a large RTB permanent magnet. A magnet formed by combining two or more RTB permanent magnets is preferably used in applications requiring a particularly large RTB permanent magnet, such as IPM motors, wind power generators, and large motors. EXAMPLES
[0105] The present invention will be described below with reference to more detailed examples, but the present invention is not limited to these examples.
[0106] (Magnet manufacturing process before Tb diffusion) The raw metals prepared were Nd, Tb, electrolytic iron, and low carbon ferroboron alloy. In addition, Al, Cu, Co, and Zr were prepared either as pure metals or alloys with Fe.
[0107] A raw alloy was prepared from the raw metals by strip casting so that the composition of the magnet before Tb diffusion, described below, would be the composition shown in Table 1. The Fe content is described as "bal." This indicates that the Fe content is essentially the remainder. In all examples and comparative examples, the content of elements other than those shown in Table 1 was 1 mass % or less. The thickness of the raw alloy was 0.2 mm to 0.6 mm.
[0108] Other elements that may be detected as unavoidable impurities other than those shown in Table 1 include H, Si, Ca, La, Ce, and Cr. Si is mainly mixed in from the ferroboron raw material and the crucible used when melting the alloy. Ca, La, and Ce are mixed in from the rare earth raw material. Cr may also be mixed in from electrolytic iron.
[0109] Next, hydrogen gas was flowed into the raw alloy at room temperature for 1 hour to absorb hydrogen. The atmosphere was then switched to Ar gas, and dehydrogenation was performed at 450°C for 1 hour, after which the raw alloy was hydrogen-pulverized. After cooling, the alloy was sieved to a powder with a particle size of 400μm or less.
[0110] Next, 0.1% by mass of a lubricant (oleic acid amide) was added as a grinding aid to the raw alloy powder after the hydrogen grinding, and then mixed.
[0111] Next, the mixture was finely pulverized in a nitrogen gas flow using a collision plate type jet mill to obtain fine powders (raw powders) with an average particle size of about 4 μm. The average particle size was the average particle size D50 measured by a laser diffraction type particle size distribution analyzer.
[0112] The resulting fine powder was compacted in a magnetic field to produce a compact. The magnetic field applied was a static magnetic field of 1200 kA / m. The pressure during compaction was 120 MPa. The magnetic field application direction and the pressure application direction were perpendicular to each other. When the density of the compacts was measured at this point, the density of all the compacts was 4.10 Mg / m 3 More than 4.25Mg / m 3 It was within the following range.
[0113] Next, the compact was sintered to obtain a pre-Tb-diffusion magnet. The sintering conditions were a temperature of 1060°C for 4 hours. The sintering atmosphere was a vacuum. The sintered density was 7.50 Mg / m 3 More than 7.55Mg / m 3 The results were within the following range. Thereafter, a first aging treatment was performed in an Ar atmosphere at atmospheric pressure at a first aging temperature T1 of 900°C for 1 hour, and a second aging treatment was performed at a second aging temperature T2 of 500°C for 1 hour.
[0114] The composition of the obtained pre-diffusion permanent magnet was evaluated by fluorescent X-ray analysis. The B content was evaluated by ICP. As a result, it was confirmed that the composition was substantially the same as that of the raw material alloy. The obtained pre-diffusion permanent magnet was then subjected to the following treatment.
[0115] Comparative Example 1 The pre-Tb-diffusion magnet obtained by the above process was machined into a rectangular parallelepiped as shown in Figure 5. W = 20 mm, H = 10 mm. D was set to a length such that the length of D in the final permanent magnet was 4 mm. The orientation direction was parallel to D. Then, a slurry of TbH2 particles (D50 = 5 μm) dispersed in ethanol was applied to two faces of the pre-Tb-diffusion magnet measuring 20 mm x 10 mm to adhere Tb. The total amount of adhered Tb relative to the mass of the pre-Tb-diffusion magnet was adjusted to the ratio shown in Table 1.
[0116] After the slurry was applied, the diffusion treatment pressure was set to atmospheric pressure (100 kPa), and heat treatment was performed at a diffusion treatment temperature of 850°C for a holding time of 24 hours while flowing Ar, thereby diffusing Tb into grain boundaries. Furthermore, aging treatment was performed at 500°C for 1 hour in an Ar atmosphere at atmospheric pressure.
[0117] Next, the two diffusion surfaces measuring 20 mm x 10 mm were each scraped off by 500 μm in the D direction to obtain permanent magnets (magnets after Tb diffusion) for each sample with dimensions of W = 20 mm, H = 10 mm, and D = 4 mm.
[0118] The Tb content in the resulting permanent magnet was measured using an X-ray fluorescence analyzer (XRF), and the results are shown in Table 1.
[0119] The magnetic properties (Br, Hcj, and Hk / Hcj) of the obtained permanent magnets were evaluated at RT (23°C) using a BH tracer. In this experimental example, Hcj of 2000kA / m or more was considered good, and 2300kA / m or more was considered even better. Hk / Hcj of 97.0% or more was considered good.
[0120] Furthermore, for the obtained RTB permanent magnet 1, a three-dimensional atomic distribution image was obtained using 3DAP for the main phase 11 at measurement point 3 located 2.0 mm inward in the D direction from the center of gravity of the 20 mm × 10 mm surface. It was then confirmed that the main phase 11 has a core and a shell. Next, using 3DAP, a line segment AB was set that passes through the main phase 11 and the grain boundary phase 13 adjacent to the main phase 11 as shown in Figure 1, and the Tb concentration, Cu concentration, Fe concentration, Co concentration, and Nd concentration on the line segment AB were linearly analyzed to create graphs similar to Figures 2 to 4. From the shape of the graph, it was visually possible to determine the Tb concentration in the core, the thickness of the shell, the minimum value of the total concentration of Fe and Co in the grain boundary phase, the maximum value of the Nd concentration in the grain boundary phase, [Tb s ] and [Tb b ] and [Tb b ] / [Tb s The results are shown in Table 1.
[0121] The dashed line in FIG. 2 corresponds to the grain boundary phase in Example 1, but not to that in Comparative Example 1. However, the grain boundary phase in Comparative Example 1 is located close to the position indicated by the dashed line. In addition, Comparative Example 1 does not contain Co. Therefore, the change in concentration of Fe+Co in Comparative Example 1 shown in FIG. 4 is the same as the change in concentration of Fe.
[0122] (Examples 1 to 6) Examples 1 to 6 were carried out under the same conditions as Comparative Example 1, except that the diffusion step was a multi-stage diffusion. The diffusion steps of Examples 1 to 6 are described below.
[0123] After the slurry was applied, a diffusion treatment was performed in a low-temperature reduced pressure atmosphere. Specifically, a heat treatment was performed at a diffusion treatment temperature of 600°C for 6 hours while Ar was flowing under a diffusion treatment pressure of 1 kPa. Next, a diffusion treatment was performed in a high-temperature atmospheric pressure atmosphere. Specifically, the diffusion treatment pressure was increased to atmospheric pressure (100 kPa), the diffusion treatment temperature was increased to 850°C (870°C only in Example 5), and a heat treatment was performed at the holding temperature for 6 hours. Next, a diffusion treatment was performed in a low-temperature reduced pressure atmosphere. Specifically, a heat treatment was performed at a diffusion treatment pressure of 1 kPa, the diffusion treatment temperature was increased to 600°C for 6 hours while Ar was flowing. Next, a diffusion treatment was performed in a high-temperature atmospheric pressure atmosphere. Specifically, the diffusion treatment pressure was increased to atmospheric pressure (100 kPa), the diffusion treatment temperature was increased to 850°C (870°C only in Example 5), and a heat treatment was performed at the holding temperature for 6 hours. Furthermore, an aging treatment was performed at 500°C for 1 hour in an Ar atmosphere at atmospheric pressure. The results are shown in Table 1.
[0124] [Table 1]
[0125] From Table 1, in each embodiment in which the diffusion process was performed in multiple steps, the shell thickness was 70 nm or more, [Tb s ] was 1.7 at% or more, and the minimum value of the total concentration of Fe and Co in the grain boundary phase was 65.0 at% or less. As a result, each Example had good Hcj and Hk / Hcj. In contrast, Comparative Example 1, in which the magnet before Tb diffusion did not contain Tb and the diffusion process was not a multi-stage diffusion, had a shell thickness and [Tb s ] was too small, resulting in a decrease in Hcj and Hk / Hcj.
[0126] It was confirmed that the test results shown in Table 1 did not change even when the boundary between the shell and the grain boundary phase was determined so that the Cu concentration in the grain boundary phase was always 0.15 at% or more and the Cu concentration in the part of the shell that contacted the grain boundary phase was less than 0.15 at%, and the boundary between the core and shell was determined so that the part where the Tb concentration increased by 0.10 at% or more from the Tb concentration inside the core was the shell. In this case, the calculation was made under the assumption that the Tb concentration inside the core was equal to the Tb concentration of the magnet before Tb diffusion.
[0127] In all examples, it was confirmed that when measuring points of Tb concentration were set at 10 nm intervals from the core toward the grain boundary phase 13 inside the shell, the closer the measurement point was to the grain boundary phase 13, the higher the Tb concentration was, and the difference in Tb concentration between adjacent measurement points was all 0.01 at% or more and 0.50 at% or less. That is, it was confirmed that in all examples, the Tb concentration in the shell gradually increased from the vicinity of the core toward the vicinity of the grain boundary phase.
[0128] On the other hand, in Comparative Example 1, it was confirmed that when measuring points of Tb concentration were set at 10 nm intervals from the core toward the grain boundary phase 13 inside the shell, the difference in Tb concentration between adjacent measuring points was sometimes about 1 at %. That is, it was confirmed that in Comparative Example 1, the Tb concentration in the shell did not gradually increase from the vicinity of the core toward the vicinity of the grain boundary phase. [Explanation of symbols]
[0129] 1...RTB permanent magnet 3…Center of gravity 11…Main phase 13...Grain boundary phase
Claims
1. A main phase consisting of a core and a shell, and a grain boundary phase adjacent to the main phase, The shell contains Tb, The shell has a thickness of 70 nm or more, The RTB system permanent magnet has a maximum Tb concentration in the shell of 1.7 at % or more.
2. 2. The R-T-B system permanent magnet according to claim 1, wherein the Tb concentration in the shell gradually increases from the vicinity of the core toward the vicinity of the grain boundary phase.
3. 3. The R-T-B system permanent magnet according to claim 1 or 2, wherein when measurement points for Tb concentration are set at 10 nm intervals inside the shell from the core toward the grain boundary phase, the closer the measurement point is to the grain boundary phase, the higher the Tb concentration, and all differences in Tb concentration between adjacent measurement points are 0.01 at% or more and 0.50 at% or less.
4. The maximum Tb concentration in the shell is [Tb s ], the maximum value of the Tb concentration in the grain boundary phase is [Tb b ] as 1.0≦[Tb b ] / [Tb s 3. The RTB system permanent magnet according to claim 1, wherein:
5. 3. The R-T-B system permanent magnet according to claim 1, wherein the Tb content is from 0.6% by mass to 2.1% by mass.
6. 3. The R-T-B system permanent magnet according to claim 1, which contains Fe, or Fe and Co, as the transition metal element.
7. 3. The R-T-B system permanent magnet according to claim 1, wherein the grain boundary phase contains one or more elements selected from Fe and Co, and the minimum value of the total concentration of Fe and Co in the grain boundary phase is 65.0 at% or less.
8. 3. The RTB system permanent magnet according to claim 1, wherein the squareness ratio Hk / Hcj is 97.0% or more.
Citation Information
Patent Citations
Method for producing rare earth permanent magnet material
WO2006043348A1