Silicon-carbon composite material and preparation method thereof, electrochemical device, and electronic device
A two-step chemical vapor deposition process for silicon-carbon composites addresses the complexity and stability issues in conventional methods, achieving high mass specific capacity and cycling stability by uniformly distributing silicon and carbon, suitable for large-scale industrial production.
Patent Information
- Application Number
- JP2023207079
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2023-12-07
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional methods for preparing silicon-carbon composites face challenges such as complex preparation processes, poor quality stability, and poor cycle stability, making them unsuitable for large-scale industrial production, and the materials exhibit issues like silicon aggregation, low electron mobility, and high volumetric expansion during lithiation.
A silicon-carbon composite material is prepared through a two-step chemical vapor deposition process, where silicon and carbon are co-deposited onto a carbon substrate, followed by a carbon coating, resulting in a structure with uniformly distributed silicon and carbon nanoparticles, controlled porosity, and optional silicon carbide inclusion, which enhances material strength and stability.
The method simplifies the preparation process, reduces volume expansion, improves cycling stability, and enhances electrochemical performance by uniformly distributing silicon and carbon, allowing for high mass specific capacity and suitability for large-scale industrial production.
Smart Images

Figure 2024146729000001
Abstract
Description
[Technical field]
[0001] The present invention relates to the technical field of secondary batteries, in particular to silicon-carbon composite materials and their preparation methods, electrochemical devices, and electronic devices. [Background technology]
[0002] Energy-saving and new energy vehicles are one of the top ten sectors of China Made 2025, and in order to accelerate the growth and development of energy-saving and new energy vehicles, pure electric drive has become the main strategic orientation for the development of new energy vehicles and the transformation of the automobile industry. The relevant technical indicators clearly require that the energy density of the battery cell must be more than 300Wh / kg, the cycle life must be more than 1500 times, and the specific capacity of the related negative electrode material must reach 600mAh / g. At present, the negative electrode material used for most commercially available power lithium-ion batteries is still graphite. However, the energy density of graphite has been developed to approach the theoretical level (372mAh / g), and graphite can no longer meet the requirements of the development of recent power lithium-ion batteries. Silicon provides the highest lithium storage capacity (4200mAh / g) as a negative electrode material for lithium-ion batteries. During the charge and discharge process, the possibility of lithium plating is low, and silicon has the advantages of high safety performance, but silicon also has some disadvantages. The volume expansion of silicon during the lithiation process is as high as 400%, which leads to shattering, disintegration, and poor cycle life of the material. Silicon has a low electron mobility (1350 cm 2 V -1 S -1 ) and low thermal conductivity (148m -1 K -1), leading to poor rate performance and poor material stability. Through nanoization of silicon material and modification of carbon coating, the performance of batteries with silicon as anode material can be effectively improved. Combining the advantages and disadvantages of traditional graphite and silicon as lithium-ion battery materials, nano-sized silicon can be used in combination with graphite material and modified through carbon coating to improve the electrochemical performance of graphite as anode material.
[0003] At present, some commonly used methods to prepare silicon-carbon composites include high-energy ball milling, chemical vapor deposition, sol-gel method, and high-temperature pyrolysis. Among these methods, high-energy ball milling and chemical vapor deposition are more suitable for industrial production. The ball milling method is simple and has low preparation costs. However, it is difficult for the particle size of silicon to reach the nanometer level in the ball milling process, and it is also difficult to disperse silicon in graphite powder, which makes it easy to generate homogeneous agglomeration (agglomeration of silicon and silicon or agglomeration of graphite and graphite). The uneven distribution of silicon and the large size of silicon affect the cycle safety of the battery. In the chemical vapor deposition method, a silicon source or a carbon source is used to deposit a nanometer layer on an existing substrate to prepare silicon-carbon composites. The most common silicon source is silane. Some studies have used chemical vapor deposition to deposit silicon nanowire arrays on copper foil. The resulting material retains a capacity of 3500 mAh / g after 20 cycles at a current density of 0.2 A / g, which is close to the theoretical capacity.
[0004] Although chemical vapor deposition has a high prospect for industrialization, it also has some disadvantages, such as complicated preparation steps, poor quality stability of product preparation, and poor cycle stability of the finished material. When silicon-carbon composite materials are prepared by traditional chemical vapor deposition, pure carbon or silicon substrates are generally used as substrates, and silicon or carbon is deposited on the surface to mix the two phases. Such methods bring about the following problems: 1. The preparation process is cumbersome, and in most cases, the deposition needs to be carried out repeatedly by using multiple devices to complete the material preparation. In addition, the quality stability of the finished product is poor, which is not suitable for large-scale industrial production. 2. The two phases of carbon and silicon in the finished product material are not firmly bonded, and the cycle stability is poor. Summary of the Invention [Problem to be solved by the invention]
[0005] In view of the above-mentioned shortcomings in the related art, the present invention aims to provide a silicon-carbon composite material exhibiting high overall performance (e.g., high mass-specific capacity and high cycle stability) for the negative electrode of an electrochemical energy storage device such as a lithium-ion battery, in order to solve the problems of the complicated preparation process, poor quality stability during product preparation, poor cycle stability of the finished product material, and other problems in the conventional chemical vapor deposition method used in the related art, and to provide a silicon-carbon composite material, a preparation method thereof, an electrochemical device, and an electronic device. [Means for solving the problem]
[0006] To achieve the above and other corresponding objects, a first aspect of the present invention provides a silicon-carbon composite material comprising an inner core and a carbon coating layer covering the inner core, the inner core comprising a carbon substrate and nanoparticles attached to a surface of the carbon substrate and / or within the carbon substrate, the nanoparticles comprising silicon and silicon carbide.
[0007] Silicon-carbon composites meet the following requirements: R=[m×P / 2.21] / [1-m×n / 2.25]×100% Here, R is 20% to 80%. R is the accessible porosity in the silicon-carbon composite and m is the accessible porosity in g / cm in the silicon-carbon composite. 3 where n is the true density in wt%, n is the mass percentage of elemental carbon in the silicon-carbon composite in wt%, and P is the mass percentage of elemental silicon in the silicon-carbon composite in wt%.
[0008] Furthermore, the porosity (R) of the silicon-carbon composite material is 30% to 50%.
[0009] Furthermore, the mass percentage of carbon element in the silicon-carbon composite material is 35 wt% to 90 wt%, and preferably 40 wt% to 70 wt%.
[0010] Furthermore, the mass percentage of silicon element in the silicon-carbon composite material is 10 wt% to 65 wt%, and preferably 30 wt% to 50 wt%.
[0011] Furthermore, in the silicon-carbon composite material, the mass percentage of silicon carbide is 0 wt% to 20 wt%, and preferably 1 wt% to 20 wt%.
[0012] Furthermore, the specific surface area of the carbon substrate is 1 cm 2 / g~200cm 2 / g, and the porosity of the carbon substrate is 1% to 50%.
[0013] Further, the carbon substrate is selected from at least one of artificial graphite, natural graphite, expanded graphite, flake graphite, multi-layer graphene, hard carbon, soft carbon, mesocarbon microspheres, multi-layer graphene, porous carbon, and hollow carbon microspheres.
[0014] A second aspect of the present invention provides a method for preparing a silicon-carbon composite material, comprising the steps of:
[0015] In the carbon-silicon codeposition step, carbon and silicon are codeposited on the carbon substrate by first chemical vapor deposition using a gaseous carbon source and a gaseous silicon source to obtain an intermediate.
[0016] In the carbon coating step, a carbon coating layer is formed on the surface of the intermediate body by a second chemical vapor deposition using a carbon source to obtain a silicon-carbon composite material.
[0017] The silicon-carbon composite material includes an inner core and a carbon coating layer covering the inner core. The inner core includes a carbon substrate and nanoparticles attached to the surface of the carbon substrate and / or within the carbon substrate, the nanoparticles including silicon and silicon carbide.
[0018] Silicon-carbon composites meet the following requirements: R=[m×P / 2.21] / [1-m×n / 2.25]×100% Here, R is 20% to 80%. R is the porosity in the silicon-carbon composite and m is g / cm in the silicon-carbon composite 3 where n is the true density in wt%, n is the mass percentage of elemental carbon in the silicon-carbon composite in wt%, and P is the mass percentage of elemental silicon in the silicon-carbon composite in wt%.
[0019] Further, the silicon source is selected from at least one of monosilane (SiH4), disilane, tetrachlorosilane, dimethyldichlorosilane, trimethyldichlorosilane, tetramethylsilane, trichlorosilane, tetrachlorosilane, methylsilicate, and ethylsilicate.
[0020] Further, the carbon source is selected from at least one of methane, ethane, acetylene, propane, and propylene.
[0021] Further, the carbon substrate is selected from at least one of artificial graphite, natural graphite, expanded graphite, flake graphite, multi-layer graphene, hard carbon, soft carbon, mesocarbon microspheres, multi-layer graphene, porous carbon, and hollow carbon microspheres.
[0022] Furthermore, the reaction temperature of the first chemical vapor deposition and the second chemical vapor deposition is 400°C to 1000°C.
[0023] Furthermore, when the intermediate is prepared, the deposition time of the first chemical vapor deposition is 2 hours to 16 hours, preferably 4 hours to 16 hours, and more preferably 8 hours to 16 hours.
[0024] Furthermore, when a carbon coating layer is prepared, the deposition time of the second chemical vapor deposition is 0.5 hours to 2 hours, preferably 1 hour to 2 hours.
[0025] A third aspect of the present invention provides an electrochemical device including a negative electrode sheet. The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer provided on the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material. The negative electrode active material includes a silicon-carbon composite material according to the first aspect and / or a silicon-carbon composite material obtained by the method according to the second aspect.
[0026] A fourth aspect of the present invention provides an electronic device comprising an electrochemical device according to the third aspect of the present invention. Effect of the Invention
[0027] As described above, the silicon-carbon composite material, its preparation method, electrochemical device, and electronic device exhibit the following beneficial effects:
[0028] The silicon-carbon composite material provided by the present invention is a carbon-coated silicon-carbon composite material, in which silicon and carbon nanoparticles are uniformly distributed on the carbon substrate and constrain each other. In this way, the adverse effects caused by the volume expansion after the lithiation of silicon can be greatly reduced, and the cycling stability of the material can be improved. By increasing the porosity in the silicon-carbon structure, the deintercalation and intercalation of lithium during the charging and discharging process can be reduced, and the electrochemical performance of the battery is improved. Furthermore, the strength of the material particles can be increased by including an appropriate amount of silicon carbide in the silicon-carbon composite structure, and the cycling characteristics of the battery using this material as the negative electrode active material are greatly improved.
[0029] In the method for preparing silicon-carbon composite material provided by the present invention, gaseous silicon and carbon sources are selected for chemical vapor co-deposition. Compared with the multi-step deposition method of preparing silicon and carbon on a substrate, in this method, the processing steps are effectively reduced, the processing flow time is shortened, and the production efficiency is greatly improved. Furthermore, the preparation cost is reduced and mass production is easily achieved. In addition, the CVD method adopted by the present invention can effectively control the generation of silicon carbide phase during the deposition process, allowing nanoscale silicon and carbon to be uniformly distributed on the carbon substrate and restrict each other. In this way, the adverse effect caused by the volume expansion after the lithiation of silicon can be greatly reduced and the cycle stability of the material can be improved. When the silicon and carbon contents of the finished material are close, the silicon-carbon composite material prepared by co-deposition exhibits good cycle stability.
[0030] In summary, the present invention provides a silicon-carbon composite material that exhibits high overall performance (e.g., high mass-specific capacity and high cycle stability) of the negative electrode of an electrochemical energy storage device such as a lithium-ion battery. The present invention further provides a method for preparing a silicon-carbon composite material that requires a low-cost and simple preparation process, and the problems of poor quality stability during product preparation and poor cycle stability of the finished product material are solved. This preparation method is suitable for large-scale industrial production. The silicon-carbon composite material provided by the present invention can be used as a negative electrode active material applied to a negative electrode active material layer, and can be made into a negative electrode sheet, which can be assembled with a positive electrode sheet, a separator, an electrolyte, and a positive electrode sheet to form an electrochemical device such as a lithium-ion battery, and the electrical performance is greatly improved. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0031] The implementation of the present invention is shown below by a specific embodiment. Those skilled in the art can easily understand the advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied by other different specific implementation methods. The details of this specification can be modified or changed based on different perspectives and applications without departing from the spirit of the present invention.
[0032] One embodiment of the present invention provides a silicon-carbon composite material comprising an inner core and a carbon coating layer covering the inner core, the inner core comprising a carbon substrate and nanoparticles uniformly deposited on a surface of the carbon substrate and / or within the carbon substrate, the nanoparticles comprising silicon and silicon carbide.
[0033] Silicon-carbon composites meet the following requirements: R=[m×P / 2.21] / [1-m×n / 2.25]×100% Here, R is 20% to 80%, and preferably 30% to 50%. R is the porosity in the silicon-carbon composite and m is g / cm in the silicon-carbon composite 3where n is the true density in wt%, n is the mass percentage of elemental carbon in the silicon-carbon composite in wt%, and P is the mass percentage of elemental silicon in the silicon-carbon composite in wt%.
[0034] In this embodiment, the silicon and carbon nanoparticles in the silicon-carbon composite material are uniformly distributed on the carbon substrate to restrict each other. In this way, the adverse effects caused by the volume expansion after the lithiation of silicon can be greatly reduced, and the cycling stability of the material can be improved. By increasing the porosity in the silicon-carbon structure, the deintercalation and intercalation of lithium during the charging and discharging process can be reduced, and the electrochemical performance of the battery is improved. In addition, the strength of the material particles can be increased by including an appropriate amount of silicon carbide in the silicon-carbon composite structure, and the cycling characteristics of the battery using this material as the negative electrode active material are greatly improved.
[0035] In some embodiments, the mass percentage of carbon element in the silicon-carbon composite material is 35 wt% to 90 wt%, preferably 40 wt% to 70 wt%, the mass percentage of silicon element is 10 wt% to 65 wt%, preferably 30 wt% to 50 wt%, and the mass percentage of silicon carbide in the silicon-carbon composite material is 0 wt% to 20 wt%, preferably 1 wt% to 20 wt%, more preferably 1 wt% to 10 wt%.
[0036] In some embodiments, the specific surface area of the carbon substrate is less than 1 cm 2 / g~200cm 2 / g, and the porosity of the carbon substrate is 1% to 50%.
[0037] In some embodiments, the carbon substrate is selected from at least one of synthetic graphite, natural graphite, expanded graphite, flake graphite, multi-layer graphene, hard carbon, soft carbon, mesocarbon microspheres, multi-layer graphene, porous carbon, and hollow carbon microspheres.
[0038] In some embodiments, the silicon material is Si and SiOx and the silicon material is nanoscale. The particle size of the silicon material is preferably 2 nm to 20 nm. The silicon material is rod-shaped and / or granular, including but not limited to spherical, quasi-spherical, or acicular particles.
[0039] One embodiment of the present invention provides a method for preparing a silicon-carbon composite material, which includes the following steps:
[0040] In the carbon-silicon codeposition step, carbon and silicon are codeposited on the carbon substrate by first chemical vapor deposition using a gaseous carbon source and a gaseous silicon source to obtain an intermediate.
[0041] In the carbon coating step, a carbon coating layer is formed on the surface of the intermediate body by a second chemical vapor deposition using a carbon source to obtain a silicon-carbon composite material.
[0042] The silicon-carbon composite material includes an inner core and a carbon coating layer covering the inner core. The inner core includes a carbon substrate and nanoparticles attached to the surface of the carbon substrate and / or within the carbon substrate, the nanoparticles including silicon and silicon carbide.
[0043] Silicon-carbon composites meet the following requirements: R=[m×P / 2.21] / [1-m×n / 2.25]×100% Here, R is 20% to 80%, and preferably 30% to 50%. R is the porosity in the silicon-carbon composite and m is g / cm in the silicon-carbon composite 3 where n is the true density in wt%, n is the mass percentage of elemental carbon in the silicon-carbon composite in wt%, and P is the mass percentage of elemental silicon in the silicon-carbon composite in wt%.
[0044] In this embodiment, gaseous silicon and carbon sources are selected for chemical vapor co-deposition. Compared with the multi-step deposition method of preparing silicon and carbon on a substrate, in this method, the processing steps are effectively reduced to shorten the processing flow time, and the production efficiency is greatly improved. Furthermore, the preparation cost is reduced and mass production is easier to achieve. Furthermore, the CVD method adopted by this embodiment can effectively control the generation of silicon carbide phase during the deposition process, allowing nanoscale silicon and carbon to be uniformly distributed on the carbon substrate and restrict each other. In this way, the adverse effects caused by the volume expansion after the lithiation of silicon can be greatly reduced and the cycle stability of the material can be improved. Furthermore, by increasing the porosity of the silicon-carbon structure, the deintercalation and intercalation of lithium during the charge-discharge process can be reduced, and the electrochemical performance of the battery can be improved.
[0045] In another embodiment of the present invention, a method for preparing a silicon-carbon composite material includes the following steps.
[0046] a) A carbon substrate is placed in a deposition chamber, and the reaction chamber is filled with an inert gas by introducing an inert gas to evacuate the original air, and the temperature is raised to the reaction temperature.
[0047] b) feeding a gaseous silicon source, a gaseous carbon source, and a protective atmosphere gas into the vacuum reaction chamber formed in step a) to perform a first chemical vapor deposition to codeposit carbon and silicon onto the carbon substrate to obtain an intermediate;
[0048] c) After the codeposition is completed, the gaseous silicon source is shut off and the gaseous carbon source and the protective atmosphere gas are continuously flowed in, so that a stable carbon coating layer is formed on the surface of the intermediate obtained in step b) to obtain a silicon-carbon composite material.
[0049] d) After the deposition is completed, other gas sources are shut off, an inert gas is introduced, and the resulting silicon-carbon composite material is removed after cooling to room temperature.
[0050] In some embodiments, the silicon source is selected from at least one of monosilane (SiH4), disilane, tetrachlorosilane, dimethyldichlorosilane, trimethyldichlorosilane, tetramethylsilane, trichlorosilane, tetrachlorosilane, methylsilicate, and ethylsilicate.
[0051] In some embodiments, the carbon source is selected from at least one of methane, ethane, acetylene, propane, and propylene.
[0052] In some embodiments, the carbon substrate is selected from at least one of synthetic graphite, natural graphite, expanded graphite, flake graphite, multi-layer graphene, hard carbon, soft carbon, mesocarbon microspheres, multi-layer graphene, porous carbon, and hollow carbon microspheres.
[0053] In some embodiments, the reaction temperature of the first chemical vapor deposition and the second chemical vapor deposition is 400°C to 1000°C, preferably 500°C to 1000°C, more preferably 500°C to 800°C, and may be, for example, 500°C, 510°C, 520°C, 530°C, 550°C, 580°C, 600°C, 620°C, 650°C, 680°C, or 700°C.
[0054] In some embodiments, when the intermediate is prepared, the deposition time of the first chemical vapor deposition is 2 hours to 16 hours, preferably 4 hours to 16 hours, more preferably 8 hours to 16 hours. During the decomposition process of the silicon source and the carbon source, they are likely to react and form silicon carbide. By controlling the deposition time, the deposition rate of each product phase can be effectively controlled. With the increase of the deposition time, the content of silicon and silicon carbide in the obtained composite material increases.
[0055] In some embodiments, when a carbon coating layer is prepared, the deposition time of the second chemical vapor deposition is 0.5 hours to 2 hours, preferably 1 hour to 2 hours.
[0056] In some embodiments, when the intermediate is prepared, the flow rate ratio of the silicon source gas, the carbon source gas and the protective atmosphere gas is 2:(1-4):(1-4), and the total flow rate is 1L-5L per minute.
[0057] In some embodiments, the first chemical vapor deposition reaction and the second chemical vapor deposition reaction are carried out under slightly positive, normal, or negative pressure.
[0058] In some embodiments, the protective atmosphere gas for the first chemical vapor deposition and the second chemical vapor deposition includes hydrogen and an inert gas. The proportion of hydrogen in the protective atmosphere gas is preferably 80% or more. The inert gas is selected from at least one of nitrogen, helium, argon, and neon. During the decomposition process of the silicon source and the carbon source, they are likely to react to form silicon carbide. By controlling the proportion of the reducing gas hydrogen in the protective atmosphere gas, the deposition rate of each production phase can be effectively controlled, the proportion of the reducing gas hydrogen in the protective atmosphere gas can be increased, and the content of silicon carbide in the resulting composite material can be reduced.
[0059] In some embodiments, the first chemical vapor deposition and the second chemical vapor deposition are performed in a chemical vapor deposition furnace, and the chemical vapor deposition furnace is selected from the group consisting of a tubular furnace, a rotary furnace, and a fluidized bed.
[0060] It should be noted that the silicon-carbon composite material described in the above embodiment may be obtained by the method described in the above embodiment, but the present invention is not limited thereto.
[0061] One embodiment of the present invention provides a negative electrode sheet. The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer provided on the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material. The negative electrode active material includes a silicon-carbon composite material according to the above embodiment and / or a silicon-carbon composite material prepared by the method according to the above embodiment.
[0062] In some embodiments, the negative electrode active material comprises 24% to 45% by mass of the silicon-carbon composite material.
[0063] One embodiment of the present invention provides an electrochemical device including the negative electrode sheet described in the above embodiment, a positive electrode sheet, a separator, and an electrolyte.
[0064] The electrochemical device of this embodiment of the present invention is any electrochemical device, such as, but not limited to, a lithium ion battery or a sodium ion battery.
[0065] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer provided on the positive electrode current collector. The positive electrode active material layer includes a positive electrode active material.
[0066] The positive electrode active material is generally a lithium-containing composite oxide, specific examples of which include LiMnO2, LiFeO2, LiMn2O4, Li2FeSiO4, and LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi5CO2Mn3O2, Li z Ni (1-x-y) Co x M y O2 (wherein 0.01≦x≦0.20, 0≦y≦0.20, 0.97≦z≦1.20, and M represents an element selected from at least one of Mn, V, Mg, Mo, Nb, and Al), LiFePO4, and Li z CO (1-x) M x O2 (wherein 0≦x≦0.1, 0.97≦z≦1.20, and M represents an element selected from at least one of Mn, Ni, V, Mg, Mo, Nb, and Al).
[0067] Generally, materials such as conductive agents and binders are added to the active materials. According to different requirements, the amount of the materials added may be adjusted within 1% to 50% of the total mass of the positive electrode active material, and within 55% to 76% of the total mass of the negative electrode active material.
[0068] The conductive agent is a reagent used to ensure that the electrode has good charge and discharge performance. The conductive agent may be, for example, graphite materials such as natural graphite and artificial graphite, carbon black materials such as conductive carbon black (Super P), acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black, conductive fibers such as carbon fibers and metal fibers, metal powders such as fluorocarbon powder, aluminum powder, and nickel powder, conductive whiskers such as metal powder, zinc oxide, and potassium titanate, and conductive metal oxides such as titanium dioxide or polyphenylene derivatives.
[0069] The binder is a component that promotes bonding between the active material and the conductive agent and promotes bonding between the active material and the current collector. The binder may generally be selected from polyvinylidene fluoride, polyvinyl alcohol, polyacrylic acid (PAA), carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene propylene diene terpolymer (EPDM), sulfonated EPDM, styrene butadiene rubber, styrene acrylic rubber, fluororubber, and various copolymers.
[0070] The current collector as a substrate for carrying the electrode active material is usually a metal foil having a thickness of 3 microns to 500 microns. There is no particular limitation on the material of the current collector as long as it has high conductivity and does not cause a chemical reaction in the secondary battery system. For example, the material may be a foil material obtained by surface-treating nickel, titanium, aluminum, silver, stainless steel, carbon, etc. The current collector usually has a smooth surface, but fine lines may be formed on the surface to improve the adhesion between the positive electrode active material and the current collector. In addition, the current collector may adopt one or a combination of various forms such as a film, a mesh, a porous material, a foam, and a nonwoven fabric.
[0071] The separator is placed between the positive electrode sheet and the negative electrode sheet, and is usually an insulating film having high ion permeability and high mechanical strength. The separator typically has a thickness of 9 μm to 18 μm, a pore size of 5 μm to 300 μm, an air permeability of 180 s / 100 mL to 380 s / 100 mL, and a porosity of 30% to 50%. As the separator, a sheet or nonwoven fabric made of an olefin polymer such as polypropylene, which is chemically resistant and hydrophobic, and glass fiber or polyethylene is used.
[0072] The electrolyte used in the lithium ion battery usually contains a non-aqueous solvent, a lithium salt, and an additive.
[0073] Here, the non-aqueous solvent may be a conventional non-aqueous solvent in the technical field, preferably an ester-based solvent, more preferably a carbonate-based solvent.Specifically, the carbonate-based solvent may be selected from at least one of ethylene carbonate, dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC).
[0074] Lithium salts include LiPF6, LiBF4, LiN(SO2F)2 (abbreviated as LiFSI), LiClO4, LiAsF6, LiB(C2O4)2 (abbreviated as LiBOB), LiBF2(C2O4) (abbreviated as LiDFOB), LiN(SO2R F )2, and LiN(SO2F)(SO2R F The content of the lithium salt in the electrolyte is preferably 5% to 20%.
[0075] The additive may be selected from at least one of vinylene carbonate (VC), fluoroethylene carbonate (FEC), vinylethylene carbonate (VEC), vinyl sulfate (DTD), vinylene sulfate, 1,3-propane sultone (PS), propene sultone, 1,4-butane sultone. A typical amount of additive used in the electrolyte is 1% to 4%, e.g., 2%, of the electrolyte.
[0076] In some embodiments, the negative electrode active material includes a silicon-carbon composite material, graphite, conductive carbon black, and a binder. The negative electrode active material preferably includes 1.6% to 45% of the silicon-carbon composite material, 40% to 88.2% of the graphite, 2% to 8% of the conductive carbon black, and 2% to 18% of the binder. More preferably, the negative electrode active material includes, by mass percentage, 24% to 45% of the silicon-carbon composite material, 40% to 63% of the graphite, 2% to 8% of the conductive carbon black, and 2% to 18% of the binder.
[0077] In some embodiments, the method for preparing the negative electrode sheet described in the above embodiments includes the following steps.
[0078] To prepare the mixed negative electrode active material powder, the silicon-carbon composite material and graphite are mixed at a mass ratio of (2-50):(98-50) by stirring at high speed. Then, the mixed negative electrode active material powder, conductive carbon black and binder are mixed at a mass ratio of (80-90):(2-8):(2-18) by stirring in a suitable amount of deionized water to form a uniform negative electrode slurry. The negative electrode slurry is coated on the surface of the negative electrode current collector copper foil, and a negative electrode sheet is obtained after drying and cold pressing.
[0079] It should be noted that the above-mentioned embodiments of the present invention do not describe in detail other processing conditions and parameters in the preparation method of the negative electrode sheet. Those skilled in the art can prepare the negative electrode sheet according to the method described in the above-mentioned embodiments by combining common or conventional technical means and general knowledge in the technical field.
[0080] One embodiment of the present invention provides an electronic device including the electrochemical device described in the above embodiments.
[0081] The electronic device of this embodiment of the present invention can be any electronic device, such as but not limited to notebook computers, pen-based computers, mobile computers, e-book players, mobile phones, portable fax machines, portable copiers, portable printers, stereo headphones, video cassette recorders, liquid crystal display televisions, portable vacuum cleaners, portable CD players, mini discs, transceivers, electronic notepads, calculators, memory cards, portable recorders, radios, backup power supplies, motors, cars, motorcycles, power-assisted bicycles, bicycles, lighting fixtures, toys, game consoles, watches, electric tools, flash lamps, cameras, large household batteries, or lithium ion capacitors. It should be noted that the electrochemical device provided by the present invention can be applied not only to the above electronic devices, but also to energy storage power plants, marine transports, and air transports. Air transports include air transports in the atmosphere and air transports outside the atmosphere.
[0082] It should be noted that in the above embodiments of the present invention, the methods and steps of assembling the lithium ion battery are not described in detail. Those skilled in the art can assemble the positive electrode sheet, the negative electrode sheet, the electrolyte and the separator to form a lithium ion battery based on common or existing technical means and general knowledge in the technical field.
[0083] In order to illustrate the present invention in detail, specific examples are provided below. It should be understood that the following examples are only used to illustrate the present invention and should not be considered as limiting the protection scope of the present invention. Any minor improvements and adjustments made by those skilled in the art based on the above content of the present invention all belong to the protection scope of the present invention. The specific process parameters, etc. in the following examples are merely examples of suitable ranges. That is, those skilled in the art can select within the appropriate range through the description herein and are not limited to the specific numerical values exemplified below.
[0084] Example 1
[0085] Silicon-carbon composite materials were prepared through the following specific preparation process.
[0086] a) 500 g of carbon substrate was placed in a deposition chamber, and the reaction chamber was filled with inert gas by introducing inert gas to evacuate the original air, and the temperature was raised to the reaction temperature of 500°C.
[0087] b) To carry out the first chemical vapor deposition, monosilane, ethylene, and protective atmosphere gas (Ar:H2=80%:20%) were delivered to the vacuum reaction chamber formed in step a) at a flow rate of 1:1:3 and a total flow rate of 5 L per minute. The deposition time was 4 hours, whereby carbon and silicon were co-deposited on the carbon substrate to obtain an intermediate.
[0088] c) After the codeposition was completed, the monosilane gas was shut off and the carbon source gas and protective atmosphere gas were continuously flowed for deposition for 1 hour, whereby a stable carbon coating layer was formed on the surface of the intermediate obtained in step b), and a silicon-carbon composite material was obtained.
[0089] d) After the deposition was completed, other gas sources were shut off, an inert gas was introduced, and the resulting silicon-carbon composite material was removed after cooling to room temperature.
[0090] Example 2
[0091] In this example, a silicon-carbon composite material was prepared, and the preparation process was essentially the same as that in Example 1, except that the deposition time in step b) was 2 hours.
[0092] Example 3
[0093] In this example, a silicon-carbon composite material was prepared, and the preparation process was essentially the same as that in Example 1, except that the deposition time in step b) was 16 hours.
[0094] Example 4
[0095] In this example, a silicon-carbon composite material was prepared, and the preparation process was essentially the same as that of Example 1, except that the protective atmosphere gas in step b) was Ar:H2=50%:50%.
[0096] Example 5
[0097] In this example, a silicon-carbon composite material was prepared, and the preparation process was essentially the same as that of Example 1, except that the protective atmosphere gas in step b) was Ar:H2=10%:90%.
[0098] Example 6
[0099] In this example, a silicon-carbon composite material was prepared, and the preparation process was essentially the same as that in Example 5, except that the deposition time in step b) was 8 hours.
[0100] Example 7
[0101] In this example, a silicon-carbon composite material was prepared, and the preparation process was essentially the same as that of Example 5, except that the protective atmosphere gas in step b) was Ar:H2=2%:98%.
[0102] Example 8
[0103] In this example, a silicon-carbon composite material was prepared, and the preparation process was essentially the same as that of Example 1, except that only a gaseous silicon source was introduced in step b).
[0104] Example 9
[0105] In this example, a silicon-carbon composite material was prepared, and the preparation process was essentially the same as that of Example 1, except that the protective atmosphere gas in step b) was Ar:H2=2%:98%, and the deposition time was 5 hours.
[0106] Comparative Example 1
[0107] In this comparative example, a carbon-coated silicon-carbon composite material was prepared, and the preparation process was essentially the same as that of Example 1, except that step c) was omitted.
[0108] Example 10
[0109] In this example, a lithium ion battery was fabricated by using the silicon-carbon composite materials in Examples 1 to 9 based on the following specific method.
[0110] 1. Preparation of Positive Electrode Sheet
[0111] Ternary material LiNi 0.8 Co 0.1 Mn 0.1The mixed positive electrode active material powder was prepared by stirring and mixing with O2 at high speed. To prepare the conductive slurry, conductive carbon black (Super P), conductive carbon tubes (CNT), nitrogen methylpyrrolidone solvent (NMP), and polyvinylidene fluoride (PVDF) were dispersed and stirred at high speed for 2 hours in a mass ratio of 1:0.5:40:1. To prepare the positive electrode slurry with a specific viscosity, the mixed active material powder was mixed with the conductive slurry by stirring and mixing at high speed. The prepared slurry was uniformly coated on aluminum foil with a scraper, and then placed in a blower drying oven to dry at 120 °C for 20 minutes. Finally, the dried electrode sheet was rolled and cut to prepare the positive electrode sheet.
[0112] 2. Preparation of the negative electrode sheet
[0113] To prepare the mixed negative electrode active material powder, the prepared silicon-based material and graphite with a D50 of 10 μm were mixed at a mass ratio of 40:60 by stirring at high speed. Then, the mixed negative electrode active material powder material, Super P, and PAA (polyacrylic acid) were mixed at a mass ratio of 85:5:10 in an appropriate amount of deionized water by stirring thoroughly to form a uniform negative electrode slurry. The negative electrode slurry was coated on the surface of the negative electrode current collector copper foil, and a negative electrode sheet was obtained after drying and cold pressing.
[0114] 3. Electrolyte Preparation
[0115] The organic solvent was a mixture of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC), with a volume ratio of EC, EMC, and DEC of 20:20:60. In an argon atmosphere glove box with a moisture content of less than 10 ppm, completely dried lithium ion salt (LiPF6) was dissolved in the above organic solvent and mixed uniformly to obtain an electrolyte solution, with a LiPF6 concentration of 1 mol / L.
[0116] 4. Preparation of Separator
[0117] A 12 μm thick polypropylene separator was chosen.
[0118] 5. Battery Preparation
[0119] The positive electrode sheet, separator, and negative electrode sheet prepared above were stacked in order, with the separator placed between the positive electrode sheet and the negative electrode sheet for insulation. Then, it was covered with an aluminum-plastic film, transferred to a vacuum oven at 120°C for drying, and sealed after injecting 3.0g / Ah of electrolyte. After standing, hot pressing, cold pressing, molding, fixing, screening, and other processes, a pouch battery (i.e., a lithium-ion battery) with a capacity of 1Ah was finally obtained.
[0120] The silicon-carbon composite materials in Examples 1 to 9 were subjected to a thermogravimetric analysis test based on the following specific method.
[0121] A 5 mg sample was placed in the sample chamber and heated to 1400° C. at a rate of 10° C. per minute in an air atmosphere, and the mass change with temperature was collected.
[0122] The electrical properties of the lithium ion battery assembled in Example 10 were tested according to the following specific method.
[0123] The assembled lithium-ion battery was charged to 4.2V at a constant current of 1C, charged to 0.05C at a low voltage of 4.2V, left for 10 minutes, discharged to 2.8V at a constant current of 1C, and then left for 10 minutes. This was considered as one cycle of charge and discharge, and the discharge capacity of this cycle was recorded. The charge and discharge process was repeated 100 times, and the discharge capacity of each cycle was recorded.
[0124] Cycle capacity retention rate (%) = discharge capacity at 100th cycle / discharge capacity at 1st cycle × 100%.
[0125] Mass energy density of battery (Wh / kg) = first discharge energy / battery mass.
[0126] The DCR of the lithium ion battery assembled in Example 10 was tested according to the following specific method.
[0127] The assembled lithium-ion battery was charged to 50% SOC and discharged at a rate of 4C for 30 seconds, and the initial discharge voltage was recorded as V1. After discharging for 30 seconds, the voltage was V2, the current was I, and the DCR was calculated based on the following formula: DCR=(V1-V2) / I.
[0128] The silicon-carbon composite materials in Examples 1 to 9 and Comparative Example 1 were analyzed and tested by inductively coupled plasma optical emission spectroscopy (ICP-OES) to obtain the contents of silicon, carbon, and silicon carbide, and the porosity (R) was calculated according to the formula. The results are shown in Table 1.
[0129] [Table 1]
[0130] As can be seen in Table 1, comparing Example 2 with Examples 1 and 3, it can be seen that the longer the deposition time in step b), the higher the silicon and silicon carbide content.
[0131] Comparing Example 1 with Examples 4, 5, 6 and 7, it can be seen that increasing the proportion of reducing gas hydrogen in the protective atmosphere gas can effectively control the silicon carbide content in the material.
[0132] Comparing Example 1 with Examples 2, 3, 4, 5, 6, 7, and 8, it can be seen that the direct current resistance (DCR) of the lithium ion battery is negatively correlated with the porosity of the silicon-carbon composite material.
[0133] Comparing Example 1 with Example 8, it can be seen that after codeposition, the produced silicon carbide phase can significantly improve the cycle performance of lithium ion batteries using the negative electrode material.
[0134] Comparing Example 8 with the examples, it can be seen that when the silicon and carbon contents of the finished material are close, the silicon-carbon composite materials prepared by codeposition exhibit favorable cycling stability.
[0135] Comparing Example 1 with Comparative Example 1, it can be seen that the surface carbon coating provided by step c) is beneficial to improving the cycle performance of the silicon-carbon composite material.
[0136] In view of the above, through the embodiment of the present invention, it is found that co-deposition can improve the problem of two-phase interface, and under the premise that the nanoscale is guaranteed, silicon and carbon accompany two phases in the deposition process. Carbon can buffer the volume expansion of silicon during the charge and discharge process, and improve the cycle performance of the material. In addition, during the decomposition process of the silicon source and the carbon source, they are prone to react and form silicon carbide. By controlling the component ratio of the protective atmosphere gas and the deposition time, the deposition rate of each generated phase, especially the content of silicon carbide, can be effectively controlled. By increasing the porosity in the silicon-carbon structure, the deintercalation and intercalation of lithium during the charge and discharge process can be reduced, and the electrochemical performance of the lithium-ion battery is improved. [Industrial Applicability]
[0137] Furthermore, the silicon-carbon composite material of the present invention, its preparation method, electrochemical device, and electronic device including the same can be used in the electronics field, and thus has high industrial applicability.
[0138] The above-described embodiments are illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Those skilled in the art may modify or change the above-described embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or changes made by those skilled in the art without departing from the spirit and technical ideas disclosed in the present invention are also intended to be encompassed in the scope of the claims of the present invention.
Claims
1. An inner core, a carbon coating layer covering the inner core; Including, the inner core comprises a carbon substrate and nanoparticles attached to a surface of the carbon substrate and / or to an interior of the carbon substrate, the nanoparticles comprising silicon and silicon carbide; R=[m×P / 2.21] / [1-m×n / 2.25]×100% Fulfilling the relationship of where R is between 30% and 70%; R is the porosity in the silicon-carbon composite and m is g / cm in the silicon-carbon composite. 3 where n is the true density in wt%, n is the mass percentage of elemental carbon in the silicon-carbon composite in wt%, and P is the mass percentage of elemental silicon in the silicon-carbon composite in wt%, Silicon-carbon composites.
2. (a) the porosity (R) of the silicon-carbon composite material is between 30% and 50%; (b) the mass percentage of carbon element in the silicon-carbon composite material is 35 wt % to 90 wt %; (c) the mass percentage of silicon in the silicon-carbon composite material is 10 wt % to 65 wt %; (d) In the silicon-carbon composite material, the mass percentage of silicon carbide is 0 wt % to 20 wt %, excluding 0. At least one of the following conditions (a) to (d) is satisfied: The silicon-carbon composite material of claim 1.
3. The specific surface area of the carbon substrate is 1 cm 2 / g to 200 cm 2 / g, and the porosity of the carbon substrate is 1% to 50%. The silicon-carbon composite material of claim 1.
4. The carbon substrate is selected from at least one of artificial graphite, natural graphite, expanded graphite, flake graphite, multi-layer graphene, hard carbon, soft carbon, mesocarbon microspheres, multi-layer graphene, porous carbon, and hollow carbon microspheres; The silicon-carbon composite material of claim 1.
5. 1. A method for preparing a silicon-carbon composite material comprising the steps of: a carbon-silicon codeposition step, in which carbon and silicon are codeposited on a carbon substrate by a first chemical vapor deposition using a gaseous carbon source and a gaseous silicon source to obtain an intermediate; a carbon coating step of forming a carbon coating layer on the surface of the intermediate body by a second chemical vapor deposition using a carbon source to obtain the silicon-carbon composite material; Including, The silicon-carbon composite material includes an inner core and the carbon coating layer covering the inner core, the inner core includes the carbon substrate and nanoparticles attached to a surface of the carbon substrate and / or inside the carbon substrate, the nanoparticles including silicon and silicon carbide, The silicon-carbon composite material comprises: R=[m×P / 2.21] / [1-m×n / 2.25]×100% Fulfilling the relationship of where R is between 20% and 80%; R is the porosity in the silicon-carbon composite and m is g / cm in the silicon-carbon composite. 3 where n is the true density in wt%, n is the mass percentage of elemental carbon in the silicon-carbon composite in wt%, and P is the mass percentage of elemental silicon in the silicon-carbon composite in wt%, A method for preparing a silicon-carbon composite material.
6. (1) The silicon source is monosilane (SiH 4 ), disilane, tetrachlorosilane, dimethyldichlorosilane, trimethyldichlorosilane, tetramethylsilane, trichlorosilane, tetrachlorosilane, methylsilicate, and ethylsilicate; (2) The carbon source is selected from at least one of methane, ethane, acetylene, propane, and propylene; (3) The carbon substrate is selected from at least one of artificial graphite, natural graphite, expanded graphite, flake graphite, multi-layer graphene, hard carbon, soft carbon, mesocarbon microspheres, multi-layer graphene, porous carbon, and hollow carbon microspheres; At least one of the following conditions (1) to (3) is satisfied: A method for preparing the silicon-carbon composite material of claim 5.
7. The reaction temperature of the first chemical vapor deposition and the second chemical vapor deposition is 400° C. to 1000° C.; A method for preparing the silicon-carbon composite material of claim 5.
8. When the intermediate is prepared, the deposition time of the first chemical vapor deposition is 2 hours to 16 hours; or when the carbon coating layer is prepared, the deposition time of the second chemical vapor deposition is 0.5 hours to 2 hours. A method for preparing the silicon-carbon composite material of claim 5.
9. An electrochemical device including a negative electrode sheet, The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer provided on the negative electrode current collector, the negative electrode active material layer includes a negative electrode active material, and the negative electrode active material includes the silicon-carbon composite material according to claim 1. Electrochemical devices.
10. The electrochemical device according to claim 9 , electronic equipment.
11. An electrochemical device including a negative electrode sheet, The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer provided on the negative electrode current collector, the negative electrode active material layer includes a negative electrode active material, and the negative electrode active material includes the silicon-carbon composite material according to claim 2. Electrochemical devices.
12. An electrochemical device including a negative electrode sheet, The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer provided on the negative electrode current collector, the negative electrode active material layer includes a negative electrode active material, and the negative electrode active material includes the silicon-carbon composite material according to claim 3. Electrochemical devices.
13. An electrochemical device including a negative electrode sheet, The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer provided on the negative electrode current collector, the negative electrode active material layer includes a negative electrode active material, and the negative electrode active material includes the silicon-carbon composite material according to claim 4. Electrochemical devices.
14. An electrochemical device including a negative electrode sheet, The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer provided on the negative electrode current collector, the negative electrode active material layer includes a negative electrode active material, and the negative electrode active material includes a silicon-carbon composite material obtained by the preparation method according to claim 5. Electrochemical devices.
15. An electrochemical device including a negative electrode sheet, The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer provided on the negative electrode current collector, the negative electrode active material layer includes a negative electrode active material, and the negative electrode active material includes a silicon-carbon composite material obtained by the preparation method according to claim 6. Electrochemical devices.
16. An electrochemical device including a negative electrode sheet, The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer provided on the negative electrode current collector, the negative electrode active material layer includes a negative electrode active material, and the negative electrode active material includes a silicon-carbon composite material obtained by the preparation method according to claim 7. Electrochemical devices.
17. An electrochemical device including a negative electrode sheet, The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer provided on the negative electrode current collector, the negative electrode active material layer includes a negative electrode active material, and the negative electrode active material includes a silicon-carbon composite material obtained by the preparation method according to claim 8. Electrochemical devices.
Citation Information
Patent Citations
Negative electrode material for lithium ion secondary battery and its manufacturing method, negative electrode for lithium ion secondary battery, and lithium-ion secondary battery
JP2008235247A
Nanosilicon carbon composite material and method for preparing the same
JP2015503185A
Interconnected Silicon Porous Structure For Anode Active Material
US20200161635A1
Silicon-carbon composite material and preparation method thereof
WO2020151093A1