Silicon-carbon composite material, preparation method thereof, electrochemical device and electronic apparatus

A non-metallic doped silicon-carbon composite material addresses manufacturing complexities and safety issues, enhancing cycle stability and conductivity for lithium ion batteries.

JP2024146735AInactive Publication Date: 2024-10-15AESC JAPAN LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023215325
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2023-12-20
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Current silicon-carbon composite materials for lithium batteries face challenges in achieving high performance due to complex manufacturing processes, agglomeration issues, and the need for metal catalysts, which affect cycle stability and safety.

Method used

A silicon-carbon composite material is developed with a non-metallic element doped carbon substrate, forming covalent bonds to enhance active sites and conductivity, avoiding metal catalysts and improving manufacturing efficiency.

Benefits of technology

The optimized silicon-carbon composite material exhibits improved cycle stability, conductivity, and safety, suitable for large-scale production and high-performance lithium ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146735000001
    Figure 2024146735000001
Patent Text Reader

Abstract

To provide a silicon-carbon composite material, a preparation method thereof, an electrochemical device, and an electronic apparatus, so as to improve the performance of the silicon-carbon composite material through nonmetal doping optimization and solve the problems of insufficient active sites on the carbon substrate and insufficient adsorption capacity of silicon during the vapor deposition process.SOLUTION: The silicon-carbon composite material includes a carbon substrate, a silicon material attached to a surface of the carbon substrate and / or an inner portion of the carbon substrate, and a nonmetal element doped on the carbon substrate. Covalent bond energy formed by the nonmetal element and a carbon element is 180 eV≤E1≤700 eV or 130 eV≤E2≤210 eV.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the technical field of secondary batteries, and in particular to a silicon-carbon composite material, its manufacturing method, an electrochemical device and an electronic device. [Background technology]

[0002] At present, the commercialization of lithium battery anodes is mainly based on artificial / natural graphite, but is approaching the theoretical specific capacity limit (372mAh / g). The theoretical specific capacity of silicon is as high as 4200mAh / g, which is more than 10 times that of currently available graphite-based anode materials, so the hidden danger of lithium precipitation may not occur. Silicon is safer than graphite anode materials, and moreover, it has abundant silicon reserves and low cost, so it is the most promising anode material for next-generation lithium batteries. However, silicon materials react with lithium alloys during charging and discharging, which causes a significant impact on the volume (expansion rate can reach 300%). The expansion effect causes repeated destruction and formation of SEI film on the anode surface, which eventually leads to a decrease in cycle performance and coulombic efficiency, so silicon materials need to be modified before application. The modification of silicon anode materials mainly includes nanoization, carbon coating, and other technical contents to form silicon-carbon composites that improve cycle performance. Nanoization of silicon contributes to stress relief. When the particle diameter is smaller than 150 nm, the volume effect is weak, and the nanosilicon expands during the charge and discharge process but is not easily broken, so the cycle performance is improved. Nanosilicon mainly includes nanoparticles, nanowires and nanosheets, so nanosilicon can be used to improve the structural stability of the material, buffer the volume expansion of the material, and increase the active interface of the material. Carbon coating can be used to improve the conductivity of silicon particles, improve the rate performance, and prevent the aggregation of nanosilicon. Complete carbon coating can reduce the direct contact between the silicon material and the electrolyte, inhibit the excessive growth of the SEI film, stabilize the interface, and improve the Coulombic efficiency.

[0003] The manufacturing process of silicon-carbon composite materials is complicated, and there is no standardized process. The technical difficulties mainly lie in the nanoization of silicon materials and the blending and preparation process with carbon materials. At present, the commonly used manufacturing methods mainly include chemical vapor deposition, mechanical ball milling method, sol-gel process, high-temperature pyrolysis method, etc., and the former two are suitable for industrial production. The mechanical ball milling method uses a sand mill to grind silicon powder with a particle size of microns into nano-silicon slurry, which is mixed with graphite and dried to produce silicon-carbon composite materials. However, the grinding time of nano-silicon in this process is long, the energy consumption is high, the aggregation of nano-silicon particles is serious, and the process path is long. The silicon-carbon composite materials prepared by chemical vapor deposition have components that are closely bonded and have strong binding force, so the active material is not easily dropped off during charging and discharging. They have good cycle stability and are not easily aggregated. However, the method for producing silicon-carbon composite materials by chemical vapor deposition disclosed in the prior art uses a static deposition method, which is prone to aggregation of particulate materials and uneven coating, which may affect the performance of the material. Furthermore, when using chemical vapor deposition to produce silicon materials in the related art, some silicon sources such as dichlorodimethylsilane need to introduce a metal catalyst to properly prepare and adjust the morphology of the silicon material. However, the metal catalyst is difficult to completely remove by conventional methods, which may affect the performance and safety of the battery.

[0004] Although currently available silicon-carbon composite materials can improve the electrical conductivity and cycle properties of silicon materials to some extent, they still have difficulty in meeting the increasing demands for battery performance in various fields. Therefore, there is still a need to improve the materials in terms of material composition and process to better meet the demands of anode materials for high-performance lithium-ion batteries. Summary of the Invention [Problem to be solved by the invention]

[0005] In view of the above-mentioned shortcomings of the prior art, the present invention aims to provide a silicon-carbon composite material and its manufacturing method, an electrochemical device and an electronic device, in order to improve the performance of the silicon-carbon composite material by optimizing non-metallic doping, and to solve the problems of the lack of active sites on the carbon substrate and the lack of adsorption ability of silicon during the deposition process. [Means for solving the problem]

[0006] To achieve the above and other related objectives, a first aspect of the present invention provides a silicon-carbon composite material comprising a carbon substrate, a silicon material attached to a surface of the carbon substrate and / or within the carbon substrate, and a non-metallic element doped on the carbon substrate, wherein the non-metallic element and the carbon element form a covalent bond.

[0007] Silicon-carbon composites satisfy the following relationship: E1 = [910.4ln(t1)-1997.7] ± 10 (I), and E2=[503.1ln(t2)-1586]±10 (II). E1 ranges from 180 eV to 700 eV, E2 ranges from 130 eV to 210 eV, In the formula, E1 and E2 are the covalent bond energies formed by the nonmetallic elements and the carbon element in the silicon-carbon composite, and t1 and t2 are the relative atomic weights of the nonmetallic elements.

[0008] Further, the nonmetallic element is selected from at least one of B, N, F, Cl, S, and P.

[0009] Furthermore, the covalent bond formed by the nonmetallic element and the carbon element is selected from at least one of a B-C bond, an N-C bond, an F-C bond, a Cl-C bond, an S-C bond, and a P-C bond. The bond energy range of the B-C bond is 188±10 eV, the bond energy range of the N-C bond is 400±10 eV, the bond energy range of the F-C bond is 685±10 eV, the bond energy range of the Cl-C bond is 200±10 eV, the bond energy range of the S-C bond is 168±10 eV, and the bond energy range of the P-C bond is 134±10 eV.

[0010] Furthermore, the mass percentage of the nonmetallic elements in the silicon-carbon composite material is 0.001% to 5% by weight, and preferably 0.001% to 2% by weight.

[0011] Furthermore, the mass percentage of silicon element in the silicon-carbon composite material is 10% by weight to 65% by weight, and preferably 20% by weight to 65% by weight.

[0012] Furthermore, in the silicon-carbon composite material, the mass percentage of carbon element is 35% by weight to 90% by weight, and preferably 40% by weight to 80% by weight.

[0013] Furthermore, the ID / IG ratio of the silicon-carbon composite material is 0.4-2, and preferably 0.4-1.

[0014] Furthermore, the silicon-carbon composite material satisfies the following relationship: R=[m×P / 2.21] / [1- m×n / 2.25]×100%, R is 20% to 70%. where R is the available porosity and m is the g / cm in the silicon-carbon composite. 3 where n is the true density in units, and n and P are the mass percentages in weight percent of elemental carbon and elemental silicon in the carbon coated silicon, respectively.

[0015] Furthermore, the available porosity (R) of silicon-carbon composites is between 30% and 60%.

[0016] Furthermore, the silicon-carbon composite material includes an inner core and a carbon coating layer covering the inner core, the inner core including a carbon substrate, a silicon material attached to the surface of the carbon substrate and / or inside the carbon substrate, and a non-metallic element doped into the carbon substrate, wherein the non-metallic element and the carbon element form a covalent bond.

[0017] A second aspect of the present invention provides a method for producing a silicon-carbon composite material, comprising the steps of:

[0018] In the high-temperature heat treatment step, the carbon source, the inorganic non-metal source and the pore-forming agent are mixed uniformly, and then the non-metal doped carbon-based material is obtained by high-temperature heat treatment.

[0019] In the chemical vapor deposition step, a silicon source is reacted with a non-metal doped carbon-based material via chemical vapor deposition to obtain a silicon-carbon composite material.

[0020] The silicon-carbon composite material includes a carbon substrate, a silicon material attached to the surface of the carbon substrate and / or inside the carbon substrate, and a non-metallic element doped on the carbon substrate, the non-metallic element and the carbon element forming a covalent bond.

[0021] Silicon-carbon composites satisfy the following relationship: E1 = [910.4ln(t1)-1997.7] ± 10 (I), and E2=[503.1ln(t2)-1586]±10 (II). E1 ranges from 180 eV to 700 eV, E2 ranges from 130 eV to 210 eV, In the formula, E1 and E2 are the covalent bond energies formed by the nonmetallic elements and the carbon element in the silicon-carbon composite, and t1 and t2 are the relative atomic weights of the nonmetallic elements.

[0022] Additionally, the carbon source is selected from at least one of glucose, sucrose, maltose, chitosan, and soluble starch.

[0023] Further, the inorganic non-metal source is selected from at least one of a boron source, a nitrogen source, a fluorine source, a chlorine source, a sulfur source, and a phosphorus source.

[0024] Further, the silicon source is selected from at least one of monosilane (SiH4), disilane (H6Si2), dimethyldichlorosilane, trichloromethylsilane, tetramethylsilane, trichlorosilane, tetrachlorosilane, methylsilicate, and ethylsilicate.

[0025] Furthermore, the method for producing the silicon-carbon composite material further comprises the steps of: applying a carbon coating to the silicon-carbon composite material.

[0026] Furthermore, the time for chemical vapor deposition is 1 hour to 12 hours, preferably 2 hours to 12 hours, and more preferably 3 hours to 12 hours.

[0027] Furthermore, the mass ratio of the carbon source to the inorganic non-metallic source is (80-99):(1-40), and preferably (80-90):(10-20).

[0028] A third aspect of the present invention provides an electrochemical device including a negative electrode sheet. The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material. The negative electrode active material includes the silicon-carbon composite material according to the first aspect and / or the silicon-carbon composite material obtained by the method according to the second aspect.

[0029] A fourth aspect of the present invention provides an electronic device comprising the electrochemical device according to the third aspect of the present invention. Effect of the Invention

[0030] As described above, the silicon-carbon composite material and its manufacturing method, electrochemical device, and electronic device of the present invention provide the following beneficial effects.

[0031] 1. In the present invention, taking into account the lack of active sites on the carbon substrate and the lack of adsorption ability of silicon during the deposition process, the growth of silicon particles is catalyzed by increasing the active sites of the carbon substrate during the chemical vapor deposition process through in-situ doping of nonmetallic elements. Thus, the optimization of the carbon component in the silicon-carbon composite material is improved, and the performance of the silicon-carbon composite material is improved. In addition, the introduction of a large number of active sites can act as a catalyst, so that the introduction of metal catalysts is avoided, and the safety and performance of the battery are ensured. In addition, compared with the chemical vapor deposition process without nonmetallic element doping, the presence of active sites can improve the utilization rate of silicon source in the deposition process and reduce the cost.

[0032] 2. In the present invention, the non-metallic elements introduced by doping gradually diffuse into the carbon substrate during high-temperature sintering and replace some of the carbon atoms, thus forming substitutional doping. In this way, the concentration of carriers (holes) in the carbon material is effectively increased, so that the inherent conductivity of the carbon material is improved and the effect of powder conductivity is further enhanced. The carbon layer obtains high powder conductivity, while at the same time limiting the volume expansion effect of the silicon material, allowing the high capacity of the silicon-based material to be fully utilized.

[0033] 3. The method for producing silicon-carbon composite material in the present invention has a simple process and easy operation, and the method is suitable for large-scale and industrial production. The silicon-carbon composite material provided by the present invention is used as the negative active material coated on the negative active material layer to form a negative electrode sheet, which is then packaged with a positive electrode sheet, a separator, an electrolyte, and other components to form an electrochemical device such as a lithium ion battery, thus greatly improving the electrical performance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0034] The implementation method of the present invention will be described below through a specific embodiment. Those skilled in the art can easily understand other advantages and effects of the present invention from the disclosure of this specification. The present invention can also be implemented or applied through other different specific implementation methods. The details of this specification can also be modified or changed based on different perspectives and applications without departing from the spirit of the present invention.

[0035] One embodiment of the present invention provides a silicon-carbon composite material comprising a carbon substrate, a silicon material attached to a surface of the carbon substrate and / or within the carbon substrate, and a non-metallic element doped on the carbon substrate, wherein the non-metallic element and the carbon element form a covalent bond.

[0036] Silicon-carbon composites satisfy the following relationship: E1 = [910.4ln(t1)-1997.7] ± 10 (I), and E2=[503.1ln(t2)-1586]±10 (II). E1 ranges from 180 eV to 700 eV, E2 ranges from 130 eV to 210 eV, In the formula, E1 and E2 are the covalent bond energies formed by the nonmetallic elements and the carbon element in the silicon-carbon composite, and t1 and t2 are the relative atomic weights of the nonmetallic elements.

[0037] In some embodiments, the non-metallic element is selected from at least one of B, N, F, Cl, S, and P.

[0038] In some embodiments, the covalent bond formed by the nonmetallic element and the carbon element is selected from at least one of a B-C bond, an N-C bond, an F-C bond, a Cl-C bond, an S-C bond, and a P-C bond. The bond energy range of the B-C bond is 188±10 eV, the bond energy range of the N-C bond is 400±10 eV, the bond energy range of the F-C bond is 685±10 eV, the bond energy range of the Cl-C bond is 200±10 eV, the bond energy range of the S-C bond is 168±10 eV, and the bond energy range of the P-C bond is 134±10 eV.

[0039] In the above embodiment, taking into consideration the lack of active sites on the carbon substrate in the deposition process and the lack of adsorption ability of silicon during the deposition process, the growth of silicon particles is catalyzed by increasing the active sites of the carbon substrate during the chemical vapor deposition process through in situ doping of nonmetallic elements. Thus, the optimization of the carbon component in the silicon-carbon composite material is improved, and the performance of the silicon-carbon composite material is improved. In addition, the introduction of a large number of active sites can act as a catalyst, so that the introduction of metal catalysts is avoided, ensuring the safety and performance of the battery. Furthermore, compared with the chemical vapor deposition process without nonmetallic element doping, the presence of active sites can improve the availability of silicon source in the deposition process and reduce the cost. In some embodiments, the mass percentage of nonmetallic elements in the silicon-carbon composite material is 0.001 wt% to 5 wt%, preferably 0.001 wt% to 2 wt%.

[0040] In some embodiments, the mass percentage of elemental silicon in the silicon-carbon composite material is between 10% and 65% by weight, preferably between 20% and 65% by weight.

[0041] In some embodiments, the mass percentage of elemental carbon in the silicon-carbon composite material is between 35% and 90% by weight, preferably between 40% and 80% by weight.

[0042] In some embodiments, the ID / IG ratio of the silicon-carbon composite is between 0.4 and 2, preferably between 0.4 and 1.

[0043] In some embodiments, the silicon-carbon composite material satisfies the following relationship: R=[m×P / 2.21] / [1- m×n / 2.25]×100%, R is 20% to 70%, and preferably 30% to 60%. where R is the available porosity and m is the g / cm in the silicon-carbon composite. 3 where n is the true density in units, and n and P are the mass percentages in weight percent of elemental carbon and elemental silicon in the carbon coated silicon, respectively.

[0044] In some embodiments, the carbon substrate is selected from at least one of artificial graphite, natural graphite, expanded graphite, flake graphite, multi-layer graphene, hard carbon, soft carbon, mesocarbon microspheres, porous carbon, and hollow carbon microspheres.

[0045] In some embodiments, the silicon materials are Si and SiO x and the silicon material is nanoscale. The grain size of the silicon material is preferably 2 nm to 20 nm. The silicon material may be rod-shaped and / or particulate, including but not limited to spherical, quasi-spherical, or needle-shaped particles. In another embodiment of the present invention, the silicon-carbon composite material comprises an inner core and a carbon coating layer covering the inner core, the inner core comprising a silicon material attached to a carbon substrate, a surface of the carbon substrate, and / or inside the carbon substrate, and a non-metallic element doped on the carbon substrate. The non-metallic element and the carbon element form a covalent bond.

[0046] One embodiment of the present invention provides a method for producing a silicon-carbon composite material, comprising the following steps.

[0047] In the high-temperature heat treatment step, the carbon source, the inorganic non-metal source and the pore-forming agent are mixed uniformly, and then the non-metal doped carbon-based material is obtained by high-temperature heat treatment.

[0048] In the chemical vapor deposition step, a silicon source reacts with a non-metal doped carbon-based material via chemical vapor deposition to obtain a silicon-carbon composite material.

[0049] The silicon-carbon composite material includes a carbon substrate, a silicon material attached to the surface of the carbon substrate and / or inside the carbon substrate, and a non-metallic element doped on the carbon substrate, the non-metallic element and the carbon element forming a covalent bond.

[0050] Silicon-carbon composite materials satisfy the following relationship: E1 = [910.4ln(t1)-1997.7] ± 10 (I), and E2=[503.1ln(t2)-1586]±10 (II). The range of E1 is from 180 eV to 700 eV, and the range of E2 is from 130 eV to 210 eV. In the formula, E1 and E2 are the covalent bond energies formed by the nonmetallic elements and the carbon element in the silicon-carbon composite, and t1 and t2 are the relative atomic weights of the nonmetallic elements.

[0051] In some embodiments, a method for preparing a non-metal doped carbon-based material comprises the following steps.

[0052] The carbon source, inorganic non-metal source and pore-forming agent are added to a solvent, the solvent is stirred uniformly, and then the solvent is removed. The resulting solid is pulverized into a powder, and the carbon source, inorganic non-metal source and pore-forming agent are uniformly mixed in the resulting powder. The resulting powder is heat-treated at high temperature to obtain a non-metal-doped carbon-based material.

[0053] In some embodiments, the carbon source, inorganic non-metal source, and pore-forming agent are water-soluble compounds and the solvent is selected from water. A method for producing a non-metal doped carbon-based material includes the following steps.

[0054] The carbon source, inorganic non-metal source, and pore-forming agent are added to water and stirred until completely dissolved to form a homogeneous and stable solution. The solution is reheated to recrystallize, and the resulting solid is ground into a powder, and the carbon source, inorganic non-metal source, and pore-forming agent in the resulting powder are uniformly mixed. The resulting powder is subjected to high-temperature heat treatment. After high-temperature heat treatment, the product is cooled, ground, sieved, and stirred with water until the recrystallized salt is dissolved, and then the product is filtered, washed, and finally dried to obtain a non-metal-doped carbon-based material.

[0055] In some embodiments, the heating temperature is 90° C. to 110° C., and the heating time is 10 hours to 24 hours.

[0056] In some embodiments, the carbon source is selected from at least one of glucose, sucrose, maltose, chitosan, and soluble starch. The inorganic non-metal source is selected from at least one of boron source, nitrogen source, fluorine source, chlorine source, sulfur source, and phosphorus source. Preferably, the boron source is selected from at least one of titanium boride, boron nitride, boron trichloride, boric acid, diboron trioxide, sodium tetraphenylborate, sodium borohydride, and sodium borate. The nitrogen source is selected from at least one of aqueous ammonia, urea, and ammonium sulfate. The fluorine source is selected from at least one of hydrofluoric acid, sodium fluoride, and potassium fluoride. The chlorine source is selected from at least one of hydrochloric acid, sodium chloride, potassium chloride, and calcium chloride. The sulfur source is selected from at least one of sulfuric acid, sodium sulfide, thiourea, and thioacetamide. The phosphorus source is selected from at least one of sodium dihydrogen phosphate, potassium dihydrogen phosphate, monoammonium phosphate, and ammonium dihydrogen phosphate. The silicon source is selected from at least one of monosilane (SiH4), disilane (H6Si2), dimethyldichlorosilane, trichloromethylsilane, tetramethylsilane, trichlorosilane, tetrachlorosilane, methylsilicate, and ethylsilicate.

[0057] In another embodiment of the present invention, the method for producing a silicon-carbon composite further comprises providing a carbon coating on the silicon-carbon composite.

[0058] In some embodiments, the firing temperature during the high-temperature heat treatment is 500° C. to 1000° C., and the firing time is 1 hour to 5 hours.

[0059] In some embodiments, the chemical vapor deposition time is between 1 hour and 12 hours, preferably between 2 hours and 12 hours, and more preferably between 3 hours and 12 hours. Longer chemical vapor deposition times can result in increased silicon content.

[0060] In some embodiments, the mass ratio of the carbon source to the inorganic nonmetallic source is (80-99):(1-40), preferably (80-90):(10-20). By changing the ratio of the carbon source to the inorganic nonmetallic source, the doping amount of the inorganic nonmetallic can be effectively increased, and the deposition efficiency of silicon can be further improved by increasing the doping amount of the inorganic nonmetallic. Under the same conditions, the silicon content of the composite material increases as the inorganic nonmetallic content in the material increases, and the ID / IG value of the material increases accordingly. This suggests that the degree of disorder of the carbon material increases, the electrical conductivity increases, and the direct current resistance (DCR) of the battery decreases.

[0061] The silicon-carbon composite material described in the above embodiment can be obtained by the method described in the above embodiment, but the present invention is not limited to this.

[0062] One embodiment of the present invention provides a negative electrode sheet. The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material. The negative electrode active material includes a silicon-carbon composite material according to the above-described embodiment and / or a silicon-carbon composite material produced and obtained by the method according to the above-described embodiment. In some embodiments, the negative electrode active material includes 24% to 45% by mass of the silicon-carbon composite material.

[0063] One embodiment of the present invention provides an electrochemical device including the negative electrode sheet described in the above embodiment, a positive electrode sheet, a separator, and an electrolyte.

[0064] The electrochemical device in embodiments of the present invention may be any electrochemical device, such as, but not limited to, a lithium ion battery or a sodium ion battery.

[0065] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector. The positive electrode active material layer includes a positive electrode active material.

[0066] The positive electrode active material generally includes lithium-containing composite oxides, specifically LiMnO2, LiFeO2, LiMn2O4, Li2FeSiO4, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi5CO2Mn3O2, Li z Ni (1-x-y) Co x M y O2 (wherein 0.01≦x≦0.20, 0≦y≦0.20, 0.97≦z≦1.20, and M represents at least one element selected from Mn, V, Mg, Mo, Nb, and Al), LiFePO4, Li z CO (1-x) M x O2 (wherein 0≦x≦0.1, 0.97≦z≦1.20, and M represents at least one element selected from the group including Mn, Ni, V, Mg, Mo, Nb, and Al).

[0067] A conductive agent, a binder, etc. are usually added to the active material. If necessary, the amount of these substances added can be adjusted within a range of 1% to 50% of the total mass of the positive electrode active material, and can be adjusted within a range of 55% to 76% of the total mass of the negative electrode active material.

[0068] The conductive agent is a reagent used to improve the charge and discharge performance of the electrode. Examples of the conductive agent include graphite materials such as natural graphite and artificial graphite, carbon black materials such as conductive carbon black (Super P), acetylene black, ketjen black, channel black, furnace black, and lamp black, conductive fibers such as carbon fibers and metal fibers, metal powders such as carbon fluoride powder, aluminum powder, and nickel powder, conductive whiskers such as zinc oxide and potassium titanate, and conductive metal oxides such as titanium dioxide and polyphenylene derivatives.

[0069] The binder is a component that promotes the bonding between the active material and the conductive agent, and promotes the bonding between the active material and the current collector. The binder may generally be selected from polyvinylidene fluoride, polyvinyl alcohol, polyacrylic acid (PAA), carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, styrene-acrylic rubber, fluororubber, various copolymers, etc.

[0070] The current collector is a substrate that supports the electrode active material, and is usually a metal foil having a thickness of 3 microns to 500 microns. The material of the current collector is not particularly limited as long as it is highly conductive and does not cause a chemical reaction in the secondary battery system. For example, the material may be a foil material obtained by surface treatment of nickel, titanium, aluminum, nickel, silver, stainless steel, carbon, etc. The surface of the current collector is usually smooth, but fine lines may be formed on the surface to improve the adhesion between the positive electrode active material and the current collector. In addition to foil, the current collector may be in various forms such as film, mesh, porous, foam, nonwoven fabric, etc., either alone or in combination.

[0071] The separator is disposed between the positive electrode sheet and the negative electrode sheet, and is usually an insulating film with high ion permeability and high mechanical strength. The separator usually has a thickness of 9 μm to 18 μm, a pore size of 5 μm to 300 μm, an air permeability of 180 sec / 100 mL to 380 sec / 100 mL, and a porosity of 30% to 50%. As the separator, a sheet or nonwoven fabric made of an olefin polymer such as polypropylene or glass fiber, which has chemical resistance and hydrophobicity, or polyethylene, is used.

[0072] The electrolyte used in lithium-ion batteries usually contains a non-aqueous solvent, a lithium salt, and an additive.

[0073] Here, the non-aqueous solvent may be a conventional non-aqueous solvent in the art, preferably an ester solvent, more preferably a carbonate solvent. Specifically, the carbonate solvent may be selected from at least one of ethylene carbonate, dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC).

[0074] Lithium salts include LiPF6, LiBF4, LiN(SO2F)2 (abbreviated as LiFSI), LiClO4, LiAsF6, LiB(C2O4)2 (abbreviated as LiBOB), LiBF2(C2O4) (abbreviated as LiDFOB), LiN(SO2R F )2 and LiN(SO2F)(SO2R F The content of the lithium salt in the electrolyte is preferably 5% to 20%.

[0075] The additive is selected from at least one of vinylene carbonate (VC), fluoroethylene carbonate (FEC), vinyl ethylene carbonate (VEC), vinyl sulfate (DTD), vinylene sulfate, 1,3-propane sultone (PS), propene sultone, and 1,4-butane sultone. A typical amount of additive used in the electrolyte is 1% to 4% of the electrolyte, such as 2%.

[0076] In some embodiments, the negative electrode active material includes a silicon-carbon composite, graphite, conductive carbon black, and a binder. The negative electrode active material preferably includes 1.6% to 45% silicon-carbon composite, 40% to 88.2% graphite, 2% to 8% conductive carbon black, and 2% to 18% binder. More preferably, the negative electrode active material includes, by mass percentage, 24% to 45% silicon-carbon composite, 40% to 63% graphite, 2% to 8% conductive carbon black, and 2% to 18% binder.

[0077] In some embodiments, the method for producing the negative electrode sheet described in the above embodiments includes the following steps.

[0078] A silicon-carbon composite material and graphite are mixed at high speed in a mass ratio of (2-50):(98-50) to prepare a mixed negative electrode active material powder. Next, the mixed negative electrode active material powder is thoroughly mixed with conductive carbon black and a binder in an appropriate amount of deionized water in a mass ratio of (80-90):(2-8):(2-18) to form a uniform negative electrode slurry. This negative electrode slurry is applied to the surface of a negative electrode current collector copper foil, dried, and cold pressed to obtain a negative electrode sheet.

[0079] It should be noted that in the above-mentioned embodiments of the present invention, details of other process conditions and parameters in the manufacturing process of the negative electrode sheet are not described in detail. A person skilled in the art can prepare the negative electrode sheet according to the method described in the above-mentioned embodiments in combination with general or conventional technical means and ordinary knowledge in the art.

[0080] An embodiment of the present invention provides an electronic device including the electrochemical device described in the above embodiment.

[0081] The electronic device of this embodiment of the present invention is any electronic device such as, but not limited to, a notebook computer, a pen-input computer, a mobile computer, an electronic book player, a mobile phone, a portable fax machine, a portable copier, a portable printer, a stereo headphone, a video deck, a liquid crystal television, a portable cleaner, a portable CD player, a mini disk, a transceiver, an electronic memo pad, a calculator, a memory card, a portable recorder, a radio, a backup power source, a motor, an automobile, a motorcycle, an electrically assisted bicycle, a bicycle, a lighting device, a toy, a game machine, a clock, an electric tool, a flash lamp, a camera, a large household storage battery, and a lithium ion capacitor. It should be noted that the electrochemical device provided by the present invention is not only applicable to the above electronic devices, but also to energy storage power plants, marine transport ships, and air transport facilities. Airlines include airlines within the atmosphere and airlines outside the atmosphere.

[0082] It should be noted that in the above embodiments of the present invention, the methods and steps of packaging the lithium ion battery are not described in detail. Those skilled in the art can package the positive electrode sheet, the negative electrode sheet, the electrolyte and the separator according to common or conventional technical means and general knowledge in the art to form a lithium ion battery.

[0083] The following specific examples are given to explain the present invention in detail. It should also be understood that the following examples are only used to specifically explain the present invention and should not be construed as limiting the scope of protection of the present invention. Any non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention all belong to the scope of protection of the present invention. The specific process parameters in the following examples are merely examples of suitable ranges. That is, those skilled in the art can select within a suitable range through the description of this specification, and are not limited to the specific numerical values ​​exemplified below.

[0084] Example 1

[0085] In this example, a silicon-carbon composite material was prepared. The specific fabrication process is as follows:

[0086] (a) Glucose (carbon source) and boric acid (boron source) were weighed out in a ratio of 98%:2%, and 10% of the total amount of sodium chloride was weighed out as a pore-forming agent based on the total amount of the carbon source and boron source. The pore-forming agent, carbon source, and boron source were dissolved in a beaker, and an appropriate amount of deionized water was added. The mixture was magnetically stirred for 1 hour to completely dissolve the mixture, resulting in a transparent, homogeneous, and stable solution.

[0087] (b) The above solution was transferred to a blower oven, heated to 105°C, and baked for 12 hours until completely dry. The recrystallized sample was then crushed and sieved.

[0088] (c) The thinned samples were transferred to a crucible and subjected to high-temperature heat treatment in a tube furnace. The basic parameters of the heat treatment were 5 °C min under argon protective atmosphere. -1 The temperature was raised to 650°C at a rate of 100 / sq.m. / min, held for 2 hours, and then allowed to cool naturally to room temperature under a protective atmosphere.

[0089] (d) The heat-treated sample was crushed, sieved, placed in a beaker, an appropriate amount of deionized water was added, and the mixture was thoroughly stirred until the recrystallized salt was dissolved, suction filtered, and washed several times with deionized water to remove sodium chloride in the solution. After washing, the sample was dried in a blower drying oven at 80°C for 24 hours, and a boron-doped porous carbon material was obtained after drying was completed.

[0090] (e) The sample obtained in the previous step was further subjected to silicon deposition by flowing silicon source gas into a reactor forming a vacuum environment and carrying out chemical vapor deposition for 3 hours, resulting in the deposition of nanosilicon particles on the carbon-based material.

[0091] (f) The sample obtained in the previous step was further coated with carbon by flowing carbon source gas into the corresponding reactor and chemical vapor deposition of carbon. The deposition time was 2 h, and as a result, the composite material was uniformly coated with a carbon layer.

[0092] Example 2

[0093] In this example, a silicon-carbon composite material was prepared, and the preparation process was basically similar to that of Example 1, except that the ratio of glucose (carbon source) to boric acid (boron source) in step (a) was 99%:1%.

[0094] Example 3

[0095] In this example, a silicon-carbon composite material was prepared, and the preparation process was basically the same as that in Example 1, except that the deposition time in step (e) was 6 hours.

[0096] Example 4

[0097] In this example, a silicon-carbon composite material was prepared by a preparation process that was essentially similar to that of Example 1, except that in step (a), the ratio of glucose (carbon source) to boric acid (boron source) was 80%:20%.

[0098] Example 5

[0099] In this example, a silicon-carbon composite material was prepared, and the preparation process was basically the same as that of Example 4, except that in step (a), the ratio of glucose (carbon source) to boric acid (boron source) was 80%:40%.

[0100] Example 6

[0101] In this example, a silicon-carbon composite material was prepared, and the preparation process was basically the same as that in Example 1, except that the carbon source was sucrose and the dopant source was hydrazine (N2H4).

[0102] Comparative Example 1

[0103] In this comparative example, a silicon-carbon composite material was prepared, the preparation process of which is basically similar to that of Example 1, except that in step (a), no boron source was added, and only the carbon source and the pore-forming agent were kept.

[0104] Comparative Example 2

[0105] In this comparative example, a silicon-carbon composite material was prepared, and the preparation process was basically the same as that of Example 1, except that in step (a), no boron source was added, only the carbon source and the pore former were kept, and nickel nitrate or nickel cobalt iron-containing salt was added as a catalyst during the process, and the amount of addition was 2%.

[0106] Example 7

[0107] In this example, lithium ion batteries were fabricated using the silicon-carbon composite materials of Examples 1 to 6 and the silicon-carbon composite materials of Comparative Examples 1 and 2, specifically by the following method.

[0108] 1. Preparation of Positive Electrode Sheet

[0109] Ternary material LiNi 0.8 Co 0.1 Mn 0.1O2 was mixed and stirred at high speed to prepare a mixed positive electrode active material powder material. Conductive carbon black (Super P), conductive carbon tubes (CNT), nitrogen methylpyrrolidone solvent (NMP), and polyvinylidene fluoride (PVDF) were dispersed and stirred at high speed for 2 hours in a mass ratio of 1:0.5:40:1 to prepare a conductive slurry. The mixed active material powder material was mixed and stirred at high speed with the conductive slurry to prepare a positive electrode slurry with a specific viscosity. The prepared slurry was uniformly applied onto aluminum foil using a scraper, placed in a blower drying oven, and dried at 120°C for 20 minutes. Finally, the dried electrode sheet was rolled and cut to prepare a positive electrode sheet.

[0110] 2. Preparation of negative electrode sheet

[0111] The prepared silicon-based material and graphite with a D50 of 10 μm were mixed at high speed in a mass ratio of 40:60 to prepare a negative electrode active material mixed powder material. Next, this mixed negative electrode active material powder material, Super P, and PAA (polyacrylic acid) were thoroughly mixed in a suitable amount of deionized water in a mass ratio of 85:5:10 to form a uniform negative electrode slurry. This negative electrode slurry was applied to the surface of the negative electrode current collector copper foil, dried, and cold pressed to obtain a negative electrode sheet.

[0112] 3. Preparation of the electrolyte

[0113] The organic solvent was a mixture of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC), with a volume ratio of EC, EMC, and DEC of 20:20:60. In a glove box with an argon atmosphere and a moisture content of less than 10 ppm, a sufficiently dried lithium salt (LiPF6) was dissolved in the organic solvent and mixed uniformly to obtain an electrolyte (LiPF6 concentration was 1 mol / L).

[0114] 4. Preparation of the separator

[0115] A polypropylene separator with a thickness of 12 μm was selected.

[0116] 5. Battery Preparation

[0117] The positive electrode sheet, separator, and negative electrode sheet prepared above were laminated in order so that the separator was placed between the positive electrode sheet and the negative electrode sheet to insulate them. Then, it was covered with an aluminum plastic film, transferred to a vacuum oven at 120°C to dry, and sealed after injecting 3.0g / Ah of electrolyte. After standing, hot pressing, cold pressing, molding, fixing, sorting, and other processes, a pouch-type battery (i.e., a lithium-ion battery) with a capacity of 1Ah was finally obtained.

[0118] Thermogravimetric tests were carried out on the silicon-carbon composite materials of Examples 1 to 6 and the silicon-carbon composite materials of Comparative Examples 1 and 2 according to the following method, specifically as follows.

[0119] A 5 mg sample was placed in the sample chamber and heated to 1400°C at a rate of 10°C / min in an air atmosphere, and the mass change curve with temperature was collected.

[0120] The electrical characteristics of the lithium ion battery implemented in Example 7 were tested according to the following method, specifically as follows.

[0121] The mounted lithium-ion battery was charged to 4.2V at a constant current of 1C, charged to 0.05C at a constant voltage of 4.2V and left for 10 minutes, then discharged to 2.8V at a constant current of 1C and left for 10 minutes. This was the charge-discharge cycle, and the discharge capacity of this cycle was recorded. The charge-discharge process was repeated 100 times, and the discharge capacity of each cycle was recorded.

[0122] Cycle capacity retention rate (%) = discharge capacity at 100th cycle / discharge capacity at 1st cycle × 100%.

[0123] Mass energy density of battery (Wh / kg) = first discharge energy / battery mass.

[0124] The DCR of the lithium ion battery implemented in Example 7 was tested according to the following method, specifically as follows.

[0125] The assembled lithium-ion battery was charged to 50% SOC and discharged at a rate of 4C for 30 seconds, and the initial discharge voltage was recorded as V1. The voltage after 30 seconds of discharge was V2, the current was I, and the DCR was calculated according to the following equation: DCR = ((V1-V2) / I.

[0126] Using inductively coupled plasma optical emission spectroscopy (ICP-OES), elemental analysis and testing of the silicon-carbon composite materials of Examples 1-9 and Comparative Example 1 were carried out to determine the contents of nonmetallic elements (B / N), silicon, and carbon. The available porosity (R) was calculated according to the formula, and ID / IG was calculated through Raman spectrometer analysis and testing. The results are shown in Table 1. [Table 1]

[0127] Comparing Example 2, Example 4, and Example 1, it can be seen that by changing the ratio of glucose (carbon source) and boric acid (boron source), the doping amount of boron can be effectively increased, and the increase in the doping amount of boron can further improve the deposition efficiency of silicon. Under the same conditions, as the boron content in the material increases, the silicon content of the material also increases, and the ID / IG value of the material also increases accordingly. This suggests that the degree of disorder of the carbon material increases, the conductivity increases, and the direct current resistance (DCR) of the battery decreases.

[0128] Comparing Example 3 with Example 1, it can be seen that increasing the deposition time increases the silicon content.

[0129] Comparing Example 1 and Comparative Example 1, it can be seen that the deposition efficiency of the material without boron doping is much lower than that of the doped material, and the battery cycle performance and DC resistance (DCR) of the doped material are better, suggesting that doping with nonmetallic elements can catalyze the growth of silicon particles and improve the performance of silicon-carbon composite materials and batteries made from the materials.

[0130] Comparing Example 1 and Comparative Example 2, it can be seen that the deposition efficiency of the boron-doped catalyst is close to that of the metal catalyst, but the battery cycle stability is better. This is due to the impact of metal foreign matter on the performance of the battery, while the metal has strong catalytic activity and large silicon particles, which results in damage to the expansion of the electrode material during cycling.

[0131] Comparing Example 1 and Example 6, it can be seen that the silicon content is higher in the silicon-carbon composite of Example 6. This suggests that the catalytic efficiency of nitrogen doping is higher than that of boron doping, and indicates that the selection of the type of nonmetallic element affects the increase of active sites on the carbon substrate, which affects the adsorption ability of silicon and the availability of silicon source during the deposition process. [Industrial Applicability]

[0132] Furthermore, the silicon-carbon composite material, the manufacturing method thereof, the electrochemical device, and the electronic device equipped with the same of the present invention can be used in the electronics field and have high industrial applicability.

[0133] The above-described embodiments are illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Those skilled in the art may modify or change the above-described embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or changes made by those skilled in the art without departing from the spirit and technical ideas disclosed in the present invention are still intended to be included in the scope of the claims of the present invention.

Claims

1. 1. A silicon-carbon composite material comprising: a carbon substrate; a silicon material attached to a surface of the carbon substrate and / or inside the carbon substrate; and a non-metallic element doped on the carbon substrate, The nonmetallic element and the carbon element form a covalent bond, The silicon-carbon composite material satisfies the following relationship: E 1 = [910.4ln(t 1 )-1997.7] ± 10 (I), and E 2 = [503.1 ln(t 2 ) - 1586] ± 10 (II) E 1 The range is 180 eV to 700 eV, and E 2 The range is 130 eV to 210 eV, In the formula, E 1 and E 2 is the covalent bond energy formed by the nonmetallic element and the carbon element in the silicon-carbon composite material, and t 1 and t 2 is the relative atomic weight of the nonmetallic element.

2. 2. The silicon-carbon composite material of claim 1, wherein the non-metallic element is selected from at least one of B, N, F, Cl, S, and P.

3. The silicon-carbon composite material according to claim 1, which satisfies at least one of the following conditions (a) to (e): (a) the mass percentage of the non-metallic element in the silicon-carbon composite material is 0.001% to 5% by weight; (b) the mass percentage of elemental silicon in the silicon-carbon composite material is 10% by weight to 65% by weight; (c) the mass percentage of the carbon element in the silicon-carbon composite material is 35% by weight to 90% by weight; (d) the silicon-carbon composite has an ID / IG ratio of 0.4 to 2; (e) the silicon-carbon composite satisfies the relationship: R=[m×P / 2.21] / [1−m×n / 2.25]×100%, where R is between 20% and 70%, where R is the available porosity and m is the mass fraction of available porosity in the silicon-carbon composite in g / cm 3 where n is the true density in units of mass percent, and p and P are the mass percentages in weight percent of the elemental carbon and silicon, respectively, in the silicon-carbon composite material.

4. 2. The silicon-carbon composite material of claim 1, comprising an inner core and a carbon coating layer covering the inner core, the inner core comprising the carbon substrate, the silicon material attached to the surface of the carbon substrate and / or the interior of the carbon substrate, and the nonmetallic element doped into the carbon substrate, the nonmetallic element and the carbon element forming the covalent bond.

5. a high-temperature heat treatment step of uniformly mixing a carbon source, an inorganic non-metal source, and a pore-forming agent, and then obtaining a non-metal doped carbon-based material through high-temperature heat treatment; a chemical vapor deposition step of reacting a silicon source with the non-metal doped carbon-based material via chemical vapor deposition to obtain the silicon-carbon composite material; 1. A method for producing a silicon-carbon composite material comprising: The silicon-carbon composite material includes a carbon substrate, a silicon material attached to a surface of the carbon substrate and / or inside the carbon substrate, and a nonmetallic element doped on the carbon substrate, the nonmetallic element and the carbon element forming a covalent bond; The method for producing the silicon-carbon composite material satisfies the following relationship: E 1 = [910.4ln(t 1 )-1997.7] ± 10 (I), and E 2 = [503.1 ln(t 2 ) - 1586] ± 10 (II), E 1 The range is 180 eV to 700 eV, and E 2 The range is 130 eV to 210 eV. In the formula, E 1 and E 2 is the covalent bond energy formed by the nonmetallic element and the carbon element in the silicon-carbon composite material, and t 1 and t 2 is the relative atomic weight of the nonmetallic element.

6. The method of claim 5 further comprising the step of carbon coating the silicon-carbon composite material.

7. The method for producing a silicon-carbon composite material according to claim 5, wherein the chemical vapor deposition is carried out for a period of 1 to 12 hours.

8. The method for producing a silicon-carbon composite material according to claim 5, wherein a mass ratio of the carbon source to the inorganic non-metallic source is (80-99):(1-40).

9. 13. An electrochemical device including a negative electrode sheet, the negative electrode sheet including a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, the negative electrode active material layer including a negative electrode active material, the negative electrode active material including the silicon-carbon composite material of claim 1.

10. An electronic device comprising the electrochemical device according to claim 9.

11. 3. An electrochemical device including a negative electrode sheet, the negative electrode sheet including a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, the negative electrode active material layer including a negative electrode active material, the negative electrode active material including the silicon-carbon composite material according to claim 2.

12. 4. An electrochemical device including a negative electrode sheet, the negative electrode sheet including a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, the negative electrode active material layer including a negative electrode active material, the negative electrode active material including the silicon-carbon composite material according to claim 3.

13. 5. An electrochemical device including a negative electrode sheet, the negative electrode sheet including a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, the negative electrode active material layer including a negative electrode active material, the negative electrode active material including the silicon-carbon composite material according to claim 4.

14. 6. An electrochemical device including a negative electrode sheet, the negative electrode sheet including a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, the negative electrode active material layer including a negative electrode active material, the negative electrode active material including a silicon-carbon composite material obtained by the method according to claim 5.

15. 7. An electrochemical device including a negative electrode sheet, the negative electrode sheet including a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, the negative electrode active material layer including a negative electrode active material, and the negative electrode active material including a silicon-carbon composite material obtained by the method according to claim 6.

16. 8. An electrochemical device including a negative electrode sheet, the negative electrode sheet including a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, the negative electrode active material layer including a negative electrode active material, the negative electrode active material including a silicon-carbon composite material obtained by the method according to claim 7.

17. 9. An electrochemical device including a negative electrode sheet, the negative electrode sheet including a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, the negative electrode active material layer including a negative electrode active material, the negative electrode active material including a silicon-carbon composite material obtained by the method according to claim 8.

Citation Information

Patent Citations

  • Research of surface-modified nitrogen-doped porous carbon-sulfur composite material in positive electrode of lithium-sulfur battery

    CN105938900A

  • Phosphate-doping silicon carbon negative electrode material for lithium ion battery and preparation method of phosphate-doping silicon carbon negative electrode material

    CN108172775A

  • High-compaction silicon-carbon composite negative electrode material as well as preparation and application thereof

    CN112028049A

  • Preparation method and application of nitrogen-and-sulfur-doped porous hollow carbon sphere

    CN112707382A

  • Silicon-carbon negative electrode material, electrochemical device and electronic device

    CN113066970A