Method of improving fatigue strength of weld part

Hammer peening with periodic treatments on the base metal near the weld toe addresses the challenge of maintaining compressive residual stress in thick-walled welded structures, enhancing fatigue life by forming linear impact marks and adjusting impact parameters to improve fatigue strength.

JP2024146759AActive Publication Date: 2024-10-15JFE STEEL CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024017598
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-02-08
Publication Date
2024-10-15
Estimated Expiration
2044-02-08

AI Technical Summary

Technical Problem

Existing methods for improving fatigue strength in thick-walled welded structures, such as those used in offshore wind power generation, are ineffective in maintaining compressive residual stress under long-term external forces, leading to potential fatigue crack initiation and propagation.

Method used

A method involving hammer peening treatment is applied to form linear impact marks on the base metal near the weld toe, with subsequent treatments at predetermined intervals to maintain compressive residual stress, using a chipper with specific tip dimensions and striking parameters, to enhance fatigue life.

Benefits of technology

The method effectively maintains compressive residual stress on the base metal near the weld toe, improving fatigue strength and extending the life of welded structures under constant external forces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146759000001_ABST
    Figure 2024146759000001_ABST
Patent Text Reader

Abstract

To provide a method of improving the fatigue strength of a weld part which can improve the fatigue life of a weld part in a large sized weld structure, such as a floating type offshore wind power generation facility.SOLUTION: A method of improving the fatigue strength of a weld part 1 includes: forming a linear striking mark 41 extending in a weld bead extension direction 2, in a base material part 3 adjacent to a weld stop end 1a of the weld part, with hammer peening processing; and forming a similar linear striking mark 42 in the base material part adjacent to the weld stop end after a predetermined period.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for improving the fatigue strength of a welded portion, particularly a welded portion in a large welded structure, by using a hammer peening treatment to improve the fatigue life of the welded portion. [Background technology]

[0002] In recent years, offshore wind power generation has been attracting attention from the perspective of preventing global warming. Also, in order to reduce power generation costs and increase power generation efficiency, the size of wind power generation facilities is increasing, and the thickness of the steel plates used in welds is also tending to become thicker, at 30 mm or more.

[0003] Generally, fatigue cracks in welded joints occur in the plate thickness direction from stress concentration points such as the weld toe. In particular, in large welded structures such as offshore wind power generation facilities, which use thick materials, the distribution of compressive residual stress in the plate thickness direction is considered to be important for suppressing the initiation and propagation of fatigue cracks.

[0004] On the other hand, as welded structures become larger, the strength of the materials used is being increased in order to reduce the weight. As the strength of materials increases, the fatigue strength of the base material increases, but there is a concern that the fatigue strength of the welds may decrease. Therefore, various methods have been proposed to improve the fatigue properties of the welds.

[0005] For example, Patent Document 1 proposes a peening method for improving the fatigue performance of welds in structures that are subjected to repeated loads. In this method, an impact tool with a flat tip is moved up and down at a frequency of 100 Hz or less while moving continuously along the weld bead to form a continuous band-like impact mark on the base material near the weld toe. In this method, the distance between the impact mark and the toe is adjusted so as not to strike the weld toe. Preferably, the impact mark is formed by two or more successive strikes or four or more successive strikes. According to the technology of Patent Document 1, a compressive residual stress of 50% or more of the yield stress of the base material at the maximum value can be imparted to the surface layer near the weld toe, and since no notch is formed at the weld toe compared to conventional peening, fatigue strength can be significantly improved.

[0006] Furthermore, Patent Document 2 proposes a fatigue reinforcement method for a girder structure with flange gussets. In this technology, ultrasonic impact treatment is applied to the flange side toes of the welds at the ends of the flange gussets in an area of ​​at least 1t (t: gusset plate thickness) from the end of the flange gusset to the top and bottom. The technology described in Patent Document 2 is said to improve the toe shape, suppress stress concentration, and improve the fatigue performance of the girder structure with flange gussets.

[0007] Also, Patent Document 3 proposes a method for managing the useful life of a group of metal parts that are subject to fatigue-related failure, mainly targeting parts such as gas turbines and jet engines. In this technique, the compressive residual stress of the surface of a selected metal part in a high stress concentration area is measured by X-ray diffraction technology. If the measured value exceeds a predetermined value, the metal part is returned to a state of use. If the measured value is equal to or less than the predetermined value, the metal part is permanently removed from a state of use or is reworked to increase the compressive residual stress to above the predetermined value and returned to a state of use. Then, this process is repeated periodically, preferably for each part. According to this method for managing a group of metal parts, the useful life of the parts can be safely and effectively extended. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Patent No. 4895407 [Patent Document 2] JP 2004-167516 A [Patent Document 3] Special Publication No. 10-503839 Summary of the Invention [Problem to be solved by the invention]

[0009] However, it remains unclear whether the technology of Patent Document 1 is effective in improving the fatigue strength of welds that join steel materials with a plate thickness of 30 mm or more.

[0010] In addition, in the technology of Patent Document 2, in order to perform ultrasonic impact treatment to strike the weld surface of the flange gusset, it is necessary to use a special tool and ultrasonically vibrate the tip of the tool with an amplitude of 20 to 60 μm and a frequency of 15 to 60 kHz, which is disadvantageous in terms of construction costs.

[0011] In addition, the technology of Patent Document 3 targets machine parts and measures the compressive residual stress on the surface of the parts by X-ray diffraction technology, which makes it difficult to apply to large welded structures such as offshore wind power generation facilities.

[0012] Furthermore, in the field of offshore wind power generation, floating wind power generation equipment has been considered recently due to its ease of installation. Floating offshore wind power generation equipment is constantly subjected to external forces from waves. As a result, there is a concern that the absolute value of the compressive residual stress introduced around the weld toe will fall below the level that can prevent the initiation and propagation of fatigue cracks due to the long-term action of the external forces, and the intended fatigue strength improvement effect will be lost.

[0013] However, none of Patent Documents 1 to 3 takes into consideration measures against the decrease in compressive residual stress caused by the action of an external force for a long period of time.

[0014] The present invention aims to provide a method for improving the fatigue strength of a welded portion that advantageously solves the problems of the conventional technology and can improve the fatigue life of the welded portion in a large welded structure such as a floating offshore wind power generation facility. [Means for solving the problem]

[0015] In order to achieve the above object, the present inventors have conducted extensive research into a method for maintaining, for a long period of time, the fatigue strength improving effect of compressive residual stress introduced by hammer peening under the above conditions before use in a welded structure in an environment where an external force is constantly acting, such as the above floating offshore wind power generation facility. As a result, the following new findings have been obtained. (a) It is important to perform hammer peening again after a specified period of time has passed since the start of service. (a) The impact position for the hammer peening process must be the base metal part in the vicinity of the weld toe. (c) This makes it possible to maintain the compressive residual stress at an appropriate level (-400 to -200 MPa) on the surface of the base material in the vicinity of the weld toe (hereinafter simply referred to as "toe").

[0016] The present invention was completed based on these findings and further investigations. [1] A method for improving the fatigue strength of a welded part, comprising the steps of: forming linear impact marks in the extending direction of the weld bead by hammer peening on a base metal part in the vicinity of a weld toe of the welded part; and then forming similar linear impact marks again in the base metal part in the vicinity of the weld toe after a predetermined period of time. [2] The method for improving fatigue strength of a welded joint according to [1] above, characterized in that the specified period is 3 years or less. [3] The method for improving fatigue strength of a welded joint according to [1] above, characterized in that the specified period is 0.5 years or more and 3 years or less. [4] The method for improving fatigue strength of a welded portion according to any one of the above [1] to [3], characterized in that the distance between the impact mark and the weld toe is within 1.0 mm. [5] In any one of the above [1] to [4], the maximum depth of the impact mark (D P ) and width (W P ) product (D P ×W P ) is 3.0 to 5.0 mm 2 1. A method for improving fatigue strength of a welded portion, comprising: [6] The method for improving fatigue strength of a weld in any one of the above [1] to [5], characterized in that the weld is a weld that joins a tower and a base of a floating offshore wind power generation facility. [7] The method for improving fatigue strength of a welded joint according to any one of the above [1] to [6], wherein the base material is a steel material having a plate thickness of 30 mm or more. Effect of the Invention

[0017] According to the present invention, compressive residual stress can be maintained on the surface of the base material near the toe of a weld in a welded structure that is subjected to external forces such as waves, and the fatigue strength of the weld can be improved over the long term. [Brief description of the drawings]

[0018] [Figure 1] 1A and 1B are explanatory views showing a schematic diagram of an example of an embodiment of the present invention, in which (a) shows a state after a first hammer peening treatment and (b) shows a state after a second hammer peening treatment. [Diagram 2] 1(b), and (b) is a partially enlarged view of FIG. 2(a). [Diagram 3] 1A, 1B, and 1C are schematic diagrams showing an example of a shape of a chipper, in which FIG. 1A is a perspective view, FIG. 1B is an XZ cross-sectional view, and FIG. [Figure 4] FIG. 2 is an explanatory diagram showing a schematic diagram of a fillet welded joint in an embodiment. [Diagram 5] FIG. 2 is an explanatory diagram illustrating a fatigue test method in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The present invention relates to a method for improving the fatigue strength of a welded part subjected to repeated loads by performing hammer peening again after a predetermined period of time. An example of the embodiment is shown in Fig. 1. Fig. 1 shows a welded part 1 of a fillet welded joint formed by joining a horizontal member 3a and a vertical member 3b as a base material part 3 by fillet welding, but the subject of the present invention is not limited to the welded part of a fillet welded joint, and may also be a welded part of a butt welded joint (not shown).

[0020] [Hammer peening treatment] In the hammer peening process (hereinafter also referred to as "HP process"), it is preferable to use, as an impact tool, a chipper having a tip shape shown in FIG. 3. The tip shape of the chipper is such that the chipper travel direction is the Y direction, the chipper length direction is the Z direction, and the chipper width direction is the X direction (FIG. 3(a)), the XZ cross section is a semicircle shape with a diameter a and a curvature radius r (FIG. 3(b)), and the YZ cross section is a trapezoid shape with a base b (FIG. 3(c)). The diameter a and the base b are both preferably 1.0 to 10.0 mm. More preferably, they are 5.0 to 9.5 mm. The curvature radius r is preferably 1.0 to 10.0 mm. If r is less than 1.0 mm, deformation that causes stress concentration may be formed at the toe 1a. On the other hand, if r exceeds 10.0 mm, the contact area with the base material 3 becomes excessively large, and compressive residual stress may not be introduced to a region within a depth of 3.0 mm from the surface of the base material 3 at the toe 1a.

[0021] The chipper is connected to an impact device (not shown), which is driven by air pressure, high-frequency current, ultrasonic waves, or the like. For example, a method is preferred in which the tip of the chipper is operated by air pressure to impact the aforementioned area. Here, the impact frequency is preferably a low frequency of 100 Hz or less, and more preferably 50 Hz or more and 100 Hz or less.

[0022] Furthermore, the inclination angle of the chipper's striking direction is permissible if it is about 80 to 100° with respect to the base material surface, but it is preferable to set it at a nearly perpendicular 90°, since this reduces variation in each treatment.

[0023] [Selection of a specified period] In the present invention, a structure is first welded, and then the welded joint of the welded structure is struck in the first HP treatment. Here, "after welding" refers to the time immediately after welding. "start of service" refers to the time when the welded structure is installed at the service site.

[0024] Then, after a certain period of time has passed since the start of service, the welded joint is subjected to a second HP treatment. The absolute value of the compressive residual stress introduced in the first HP treatment decreases due to the long-term action of external forces such as waves. However, the absolute value of the compressive residual stress can be increased by the second HP treatment, making it possible to improve the fatigue strength of the welded joint.

[0025] In the present invention, the predetermined period is preferably three years or less, the reason for which will be explained below.

[0026] In selecting the predetermined period, it is preferable to consider the period during which the absolute value of the compressive residual stress imparted by the first HP treatment is reduced by the action of repeated external forces. Therefore, it is preferable to select the predetermined period based on the SN curve obtained in a fatigue test of a welded joint having a target welded portion. In the case of a floating offshore wind power generation facility, the predetermined period can be associated with the number of repetitions (cycles) of a fatigue test of a fillet welded joint simulating a repeated stress load state due to waves. An example of this number of repetitions is 300,000 cycles at a stress amplitude of 200 MPa. This corresponds to 3 years in service of the floating offshore wind power generation facility. Therefore, it is preferable to set the predetermined period to less than this, that is, 3 years or less. In order to avoid economic disadvantages due to an unnecessary increase in the number of HP treatments, the predetermined period is more preferably 0.5 years or more and 3 years or less. Furthermore, it is even more preferable to set the predetermined period to 2 years or more and 3 years or less. Here, the predetermined periods of 0.5 years and 2 years correspond to 50,000 cycles and 200,000 cycles, respectively, in terms of the number of repetitions at a stress amplitude of 200 MPa.

[0027] [Strike position] In the first HP treatment, as shown in Fig. 1(a), linear impact marks 41 continuing in the weld bead extending direction 2 are formed in the base material 3 near the weld toe 1a of the weld 1. In the second HP treatment, after the predetermined period has elapsed, a similar linear impact mark 42 is again formed in the base material 3 near the weld toe 1a.

[0028] The vicinity of the weld toe, which is the impact position, will be explained using Figures 1 and 2(a). In this example, the toe related to the vicinity of the weld toe is the toe 1a on the horizontal member 3a side, but the same applies when the toe is the toe 1b on the vertical member 3b side.

[0029] The vicinity of the weld toe is a region (not shown) on the base metal 3 side where the distance L1 from the toe 1a is more than 0.0 mm and not more than 2.0 mm. The region where the distance from the toe 1a is 0.0 mm or less is excluded from the impact position because it may cause damage to the weld 1 due to impact. In addition, the region where the distance from the toe 1a is more than 2.0 mm is too far from the toe 1a, and even if this region is impacted, it is not possible to introduce compressive residual stress into the surface of the base metal 3 near the toe 1a. Therefore, the distances L1 and L2 between the impact marks 41 and 42 and the toe 1a shown in FIG. 2(a) are set to more than 0.0 mm and not more than 2.0 mm, and preferably more than 0.0 mm and not more than 1.0 mm. By setting the distances L1 and L2 to more than 0.0 mm and not more than 1.0 mm, the fatigue strength can be improved under more severe external force conditions.

[0030] In the present invention, the impact by the HP treatment may be repeated any number of times, from the second time, to the third time, the fourth time, etc. The impact position (not shown) for the third time and thereafter is the same as that for the first and second times.

[0031] In addition, while Figure 1 illustrates the case where the impact position is near the weld toe 1a on the horizontal member 3a side, it may be near the weld toe 1b on the vertical member 3b side. Whether the impact position is near the weld toe on the horizontal member 3a side, the vertical member 3b side, or both is determined based on the state of external forces acting on the welded structure when in service.

[0032] [Product of maximum depth and width of impact mark] In the present invention, the maximum depth of the impact mark (D P ) and width (W P ) product (D P ×W P ) is 3.0 to 5.0 mm 2 It is preferable that the maximum depth of the impact mark (D P ) and width (W P ) is defined in a cross section perpendicular to the extending direction of the weld bead in each HP treatment, and is expressed in mm. For example, Fig. 2(b) shows the maximum depth Dp1 and width Wp1 of the first impact mark 41 and the maximum depth Dp2 and width Wp2 of the second impact mark 42.

[0033] D of each impact mark P ×W P is 3.0mm 2 If the impact depth is less than 100 mm, it is difficult to impart sufficient compressive residual stress. P ×W P is 5.0mm 2 If the impact mark is greater than D, a fatigue crack may occur at the impact mark. P ×W P 3.0~4.0mm 2 It is.

[0034] Maximum depth D P and width W P are measured as follows: maximum depth is measured using a depth gauge and width is measured using a vernier caliper.

[0035] [Welded Structures] The present invention has a significant effect of improving fatigue strength when applied to welds of welded structures used in environments where external forces are constantly acting on them. An example of such a weld is the weld that joins the tower and base of the aforementioned floating offshore wind power generation facility (not shown), which is constantly subjected to external forces from waves.

[0036] The welding method for forming the welded portion is not particularly limited, and any of shielded metal arc welding, carbon dioxide gas arc welding, and the like can be used.

[0037] [Base material] In the present invention, it is preferable that the base material portion 3 is a steel material having a plate thickness of 30 mm or more. By using steel materials for the horizontal members 3a and vertical members 3b shown in Fig. 1, the materials are relatively inexpensive, welding is easy, and the strength of the welded structure is easily ensured.

[0038] However, if the plate thickness of the steel material (for example, plate thicknesses ta and tb of the horizontal member 3a and the vertical member 3b in FIG. 1) is less than 30 mm, it may be difficult to ensure the strength of the floating offshore wind power generation facility described above, so the plate thickness of the steel material is preferably 30 mm or more. Note that the upper limit of the plate thickness is not particularly limited in the present invention, and depends on the upper limit of the range of plate thicknesses that can be normally manufactured. EXAMPLES

[0039] Using 100 mm thick YP470 grade thick steel plate (Young's modulus E: 206 GPa, Poisson's ratio ν: 0.3), a total of six fillet welded joints shown in Figure 4 were fabricated as joints No. 1 to 6 in Table 1, simulating the welded joint between the tower and base of a floating offshore power generation facility. Gas shielded arc welding was used for the fillet welding, and the welding conditions were welding current: 230 A, welding voltage: 30 V, welding speed: 34 μm / min (heat input: approximately 12.2 kJ / cm). Carbon dioxide (CO2: 100%) was used as the shielding gas. The wire used was YP470 grade wire with a diameter of 1.2 mm.

[0040] Next, for each fillet welded joint, HP treatment was performed on the base material portion 3 near the weld toe on the side of the cross member 3a, forming an impact mark 41 (see Fig. 1(a)). The distance between the impact mark 41 and the weld toe 1a was set to 1.0 mm (see Table 1). For HP treatment, a chipper with a tip shape as shown in Fig. 3 and dimensions a = 9.0 mm and b = 5.0 mm was connected to an impact device (not shown), and the impact direction was perpendicular to the steel plate surface, and the treatment was performed with air pressure at an impact frequency of 70 Hz. After the treatment, the maximum depth (D P ) x width (W P The results are shown in Table 1. Here, D P and W P The average values ​​of N pieces of measurement data obtained using a depth gauge and a vernier caliper at N=5 locations in the extension direction of the impact mark were used.

[0041] Joint No. 1 is a comparative example in which the HP treatment was performed only once, and was used for measuring the residual stress after the first HP treatment.

[0042] Joint No. 2 is a comparative example in which the HP treatment was performed only once, and was used for measuring the residual stress after the first HP treatment and a fatigue test for a predetermined number of cycles were performed in sequence.

[0043] Joint No. 3 is a comparative example in which the HP treatment was performed twice, but the impact position in the second HP treatment was removed from the vicinity of the toe, i.e., the distance between the toe 1a and the impact mark 42 (see Fig. 1(b)) was set to 3 mm (see Table 1), which is more than 2 mm. This joint was used for measuring the residual stress after the first HP treatment, a fatigue test for a specified number of cycles, and the second HP treatment were performed in that order.

[0044] Joints No. 4 to 6 are examples of the present invention in which the treatment was performed twice, and the second impact position was the same as the first, near the toe, i.e., the distance between the toe 1a and the impact mark 42 (see Fig. 1(b)) was within 2 mm (see Table 1). These were used to measure the residual stress after the first HP treatment, a fatigue test for a specified number of cycles, and the second HP treatment were performed in that order.

[0045] In the second HP treatment, the same method as in the first HP treatment was used, except that the impact position was as shown in Table 1. After the second HP treatment, the maximum depth (D P ) x width (W P The results are shown in Table 1.

[0046] The fatigue test was carried out by a tension-compression fatigue test method as shown in FIG. The predetermined number of cycles was set to 300,000 (see Table 1). As described above, this corresponds to the predetermined period of time for the floating offshore wind power generation facility to be in service, which is 3 years. The second HP treatment was carried out after the predetermined number of cycles had elapsed.

[0047] The residual stress was measured using X-rays on the surface of the base material 0.2 mm away from the toe. The results are shown in Table 1.

[0048] From Table 1, the following can be seen. That is, the first HP treatment introduced compressive residual stress of the above-mentioned suitable level (-400 to -200 MPa) into the target region (Joint No. 1 Comparative Example). However, the absolute value of the compressive residual stress decreased by carrying out a fatigue test for a specified number of cycles (Joint No. 2 Comparative Example). In this case, even if a second HP treatment was carried out, if the impact position was outside the range of the present invention, the compressive residual stress was not improved (Joint No. 3 Comparative Example). In contrast, by carrying out a second HP treatment at an impact position within the range of the present invention, the compressive residual stress was improved to the above-mentioned suitable level (Joints Nos. 4 to 6 Inventive Examples).

[0049] In this way, it was verified that the present invention can maintain the compressive residual stress on the base material surface near the weld toe of a welded structure that is repeatedly subjected to external forces at a suitable level, thereby improving fatigue strength.

[0050] [Table 1] [Explanation of symbols]

[0051] 1 Welding 1a, 1b Weld toe (toe) 2. Weld bead extension direction 3 Base metal part 3a Horizontal member 3b Vertical member 41, 42 Impact marks (1st, 2nd)

Claims

1. A method for improving fatigue strength of a welded part, comprising the steps of: forming linear impact indentations in a base metal portion near a weld toe of the welded part by hammer peening, the linear impact indentations being continuous in an extending direction of a weld bead; and then, after a prescribed period of time, forming similar linear impact indentations again in the base metal portion near the weld toe.

2. 2. The method for improving fatigue strength of a welded portion according to claim 1, wherein the predetermined period is three years or less.

3. 2. The method for improving fatigue strength of a welded portion according to claim 1, wherein the predetermined period is from 0.5 to 3 years.

4. 4. The method for improving fatigue strength of a welded portion according to claim 1, wherein a distance between the impact mark and the weld toe is within 1.0 mm.

5. The maximum depth of the impact mark (D P ) and width (W P ) product (D P ×W P ) is 3.0 to 5.0 mm 2 The method for improving fatigue strength of a welded portion according to any one of claims 1 to 3, characterized in that

6. The maximum depth of the impact mark (D P ) and width (W P ) product (D P ×W P ) is 3.0 to 5.0 mm 2 5. The method for improving fatigue strength of a welded portion according to claim 4,

7. The method for improving fatigue strength of a welded portion according to any one of claims 1 to 3, characterized in that the welded portion is a welded portion that joins a tower and a base of a floating offshore wind power generation facility.

8. The method for improving fatigue strength of a welded portion according to claim 4, characterized in that the welded portion is a welded portion that joins a tower and a base of a floating offshore wind power generation facility.

9. The method for improving fatigue strength of a welded portion according to claim 5, characterized in that the welded portion is a welded portion that joins a tower and a base of a floating offshore wind power generation facility.

10. The method for improving fatigue strength of a welded portion according to claim 6, characterized in that the welded portion is a welded portion that joins a tower and a base of a floating offshore wind power generation facility.

11. The method for improving fatigue strength of a welded portion according to any one of claims 1 to 3, characterized in that the base material portion is a steel material with a plate thickness of 30 mm or more.

12. 5. The method for improving fatigue strength of a welded portion according to claim 4, wherein the base material portion is a steel material having a plate thickness of 30 mm or more.

13. 6. The method for improving fatigue strength of a welded portion according to claim 5, wherein the base material portion is a steel material having a plate thickness of 30 mm or more.

14. 7. The method for improving fatigue strength of a welded portion according to claim 6, wherein the base material portion is a steel material having a plate thickness of 30 mm or more.

15. 8. The method for improving fatigue strength of a welded portion according to claim 7, wherein the base material portion is a steel material having a plate thickness of 30 mm or more.

16. 9. The method for improving fatigue strength of a welded joint according to claim 8, wherein the base material is a steel material having a plate thickness of 30 mm or more.

17. The method for improving fatigue strength of a welded portion according to claim 9, wherein the base material portion is a steel material having a plate thickness of 30 mm or more.

18. The method for improving fatigue strength of a welded portion according to claim 10, wherein the base material portion is a steel material having a plate thickness of 30 mm or more.

Citation Information

Patent Citations

  • Peening method and apparatus for improving fatigue characteristic of welded joint, peening apparatus for improving the fatigue characteristics and welded structure excellent in fatigue resistance

    JP2010029897A

  • Method for repairing fatigue cracking of steel structure

    JP2010125534A

  • Peening construction method and weld joint using the same

    JP2011167693A

  • Method for manufacturing weld joint and weld joint

    JP2018108601A

  • Method for improving fatigue life of weld zone in existing bridge and for repairing crack in weld zone therein

    JP2021023947A