Non-heat treated forging steel, non-heat treated forged steel and non-heat treated forged part

A non-thermal forging steel with a controlled chemical composition and parameter X addresses the challenge of achieving high strength and machinability, resulting in cost-effective production of high-strength forged parts for automotive applications.

JP2024146820APending Publication Date: 2024-10-15KOBE STEEL LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024043958
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-19
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing non-thermal forged parts face challenges in achieving high strength while maintaining excellent machinability, particularly during turning, leading to increased machining costs due to tool wear.

Method used

A non-thermal forging steel with a specific chemical composition and parameter X, defined by the formula X=[C]+0.28×[Mn]-1.03×[S]+0.323×[Cr]+1.69×[V], is developed to achieve a strength of 1060 MPa or more with improved machinability, specifically suppressing tool wear during turning.

Benefits of technology

The steel exhibits high strength and excellent machinability, reducing tool wear and machining costs, enabling the production of high-strength non-thermal forged parts suitable for automotive components like connecting rods and suspension parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146820000001
    Figure 2024146820000001
  • Figure 2024146820000002
    Figure 2024146820000002
Patent Text Reader

Abstract

To provide: a non-heat treated forged part showing high strength; non-heat treated forged steel useful for manufacturing the non-heat treated forged part, showing high strength and excellent in machinability; and non-heat treated forging steel.SOLUTION: Non-heat treated forging steel satisfies a predetermined chemical composition, and X shown by the following formula (1) is 1.09-1.37. X=[C]+0.28×[Mn]-1.03×[S]+0.323×[Cr]+1.69×[V]...(1), where [C], [Mn], [S], [Cr] and [V] show the contents of C, Mn, S, Cr and V shown by mass% in the steel, respectively, and any elements not included are assumed to be zero.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to non-heat treated forging steel, non-heat treated forging steel, and non-heat treated forged parts. [Background technology]

[0002] With the worsening of global warming and other problems, efforts to improve fuel efficiency in automobiles are accelerating. Reducing the weight of the vehicle body is an effective way to improve fuel efficiency, and to achieve this, there is a demand for high-strength automobile parts. In addition, forged parts are used for automobile parts such as connecting rods, and from the viewpoints of cost reduction and manufacturing efficiency, it is required that the forged parts for automobiles are non-tempered forged parts that are not heat-treated after forging and that exhibit high strength.

[0003] As an example of a non-heat treated steel, Patent Document 1 discloses a high-strength non-heat treated steel with excellent fracture splitting properties that has excellent hot ductility and stably forms a complete ferrite-pearlite structure when air-cooled or wind-cooled after hot forging, by controlling the range of each component, the K value defined by the prescribed formula (1), the F value defined by the formula (2), and the R value defined by the formula (3).

[0004] Patent Document 2 discloses a hot forged, untreated steel part which can ensure high strength while also ensuring excellent machinability and fracture splitting properties without relying on aging treatment or cold coining, the part satisfying specified component ranges, with 2Mn+5Mo+Cr≦3.1, C+Si / 5+Mn / 10+10P+5V≧1.8, Ceq=C+Si / 7+Mn / 5+Cr / 9+V being 0.90 to 1.10, having a hardness of HV330 or more, a yield ratio of 0.73 or more, and a ferrite-pearlite structure with 10% or less bainite.

[0005] Patent Document 3 discloses a steel material that reduces the amount of deformation near the fracture surface during fracture splitting, increases the irregularities of the fracture surface to improve fit while suppressing chipping of the fracture surface, and contains a steel material that satisfies specified component ranges, in particular a steel material that contains one or two types selected from the group consisting of Sb and Sn at specified contents, thereby reducing deformation resistance during cutting. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2010-077488 A [Patent Document 2] JP 2011-195862 A [Patent Document 3] JP 2018-035416 A Summary of the Invention [Problem to be solved by the invention]

[0007] Non-tempered forged parts are manufactured by subjecting forged steel obtained by hot forging non-tempered forging steel to machining such as cutting. The forged steel is required to have excellent machinability necessary for manufacturing non-tempered forged parts. In addition, in order to obtain high-strength non-tempered forged parts, the forged steel must exhibit high strength. However, increasing the strength reduces the machinability, which increases the cost of machining. In particular, when turning is performed as machining, it is required to suppress tool wear and reduce processing costs.

[0008] On the other hand, in Patent Document 1, the tensile strength (TS) after hot forging in the examples is at most 1008 MPa, and higher strength cannot be ensured. In Patent Document 2, machinability in drilling is considered, but machinability in turning is not considered, and further consideration is considered to be necessary to ensure excellent machinability in turning. In addition, in Patent Document 3, improvement of chip disposal in turning is considered, but compatibility with high strength is not considered, and further consideration is considered to be necessary to ensure strength.

[0009] The present disclosure has been made in consideration of the above circumstances, and an object of the present disclosure is to provide non-heat treated forged parts exhibiting high strength, such as engine parts and suspension parts, such as connecting rods for automobiles, and non-heat treated forged steel and steel for non-heat treated forging, which are useful for producing the non-heat treated forged parts and exhibit high strength and excellent machinability, particularly capable of suppressing tool wear during turning. [Means for solving the problem]

[0010] Aspect 1 of the present invention is C: 0.34~0.50% by mass, Si: 0.60~1.00% by mass, Mn: 0.90~1.40% by mass, P:0.010~0.050% by mass, S: 0.040~0.120% by mass, Cr:0.15~0.40% by mass, V:0.20~0.40% by mass, Al: more than 0 mass%, 0.010 mass% or less, N: more than 0% by mass, 0.012% by mass or less, Ni: 0.20 mass% or less (including 0 mass%) Cu: 0.20 mass% or less (including 0 mass%) Mo: 0.20 mass% or less (including 0 mass%) Ti: 0.030 mass% or less (including 0 mass%) Ca: 0.030% by mass or less (including 0% by mass), Pb: 0.10% by mass or less (including 0% by mass), Sb: 0.10 mass% or less (including 0 mass%) Te: 0.10% by mass or less (including 0% by mass), Zr: 0.005 mass% or less (including 0 mass%), Mg: 0.005% by mass or less (including 0% by mass), and REM: 0.02% by mass or less (including 0% by mass) and the balance being Fe and unavoidable impurities, The steel is a non-tempered forging steel, in which X in the following formula (1) is 1.09 to 1.37. X=[C]+0.28×[Mn]-1.03×[S]+0.323×[Cr]+1.69×[V]...(1) Here, [C], [Mn], [S], [Cr], and [V] respectively indicate the content of C, Mn, S, Cr, and V in the steel, expressed in mass%, and elements that are not contained are registered as zero.

[0011] Aspect 2 of the present invention is C: 0.34~0.50% by mass, Si: 0.60~1.00% by mass, Mn: 0.90~1.40% by mass, P:0.010~0.050% by mass, S: 0.040~0.120% by mass, Cr:0.15~0.40% by mass, V:0.20~0.40% by mass, Al: more than 0 mass%, 0.010 mass% or less, N: more than 0% by mass, 0.012% by mass or less, Ni: 0.20 mass% or less (including 0 mass%) Cu: 0.20 mass% or less (including 0 mass%) Mo: 0.20 mass% or less (including 0 mass%) Ti: 0.030 mass% or less (including 0 mass%) Ca: 0.030% by mass or less (including 0% by mass), Pb: 0.10% by mass or less (including 0% by mass), Sb: 0.10 mass% or less (including 0 mass%) Te: 0.10% by mass or less (including 0% by mass), Zr: 0.005 mass% or less (including 0 mass%), Mg: 0.005% by mass or less (including 0% by mass), and REM: 0.02% by mass or less (including 0% by mass) and the balance being Fe and unavoidable impurities, This is a non-tempered forged steel in which X in the following formula (1) is 1.09 to 1.37. X=[C]+0.28×[Mn]-1.03×[S]+0.323×[Cr]+1.69×[V]...(1) Here, [C], [Mn], [S], [Cr], and [V] respectively indicate the content of C, Mn, S, Cr, and V in the steel, expressed in mass%, and elements that are not contained are registered as zero.

[0012] Aspect 3 of the present invention is A non-heat treated forged part made by using the non-heat treated forged steel according to embodiment 2. Effect of the Invention

[0013] According to the present disclosure, it is possible to provide a non-heat treated forged part exhibiting high strength that contributes to weight reduction of a vehicle body, and a non-heat treated forged steel that is useful for producing the non-heat treated forged part, exhibiting high strength and excellent machinability, in particular capable of suppressing tool wear during turning, and a steel for non-heat treated forging. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] 1.Non-thermal forging steel The present inventors have conducted extensive research to realize a non-heat treated forged part exhibiting high strength, and a non-heat treated forged steel useful for manufacturing the non-heat treated forged part, exhibiting high strength and excellent machinability, particularly capable of suppressing tool wear during turning. As a result, they have found that controlling the chemical composition and parameter X of the non-heat treated forging steel, which is the raw material of the non-heat treated forged steel, within appropriate ranges, and in particular, as described in detail below, the range of the parameter X, the N content, and the Si content, within specified ranges, can be used to improve strength and machinability.

[0015] [High strength] [Regarding the lower limit of formula (1)] The present inventors have investigated the degree of effect of each element on the strength and machinability of steel material, and first found formula (1) as a formula for improving the strength and machinability of steel material. X=[C]+0.28×[Mn]-1.03×[S]+0.323×[Cr]+1.69×[V]...(1) Here, [C], [Mn], [S], [Cr], and [V] respectively indicate the content of C, Mn, S, Cr, and V in the steel, expressed in mass%, and elements that are not contained are registered as zero.

[0016] Furthermore, the range of X was investigated to achieve a strength (TS) of 1060 MPa or more of the forged steel obtained by hot forging the non-tempered forging steel. As a result, it was found that X needs to be 1.09 or more to achieve a strength (TS) of 1060 MPa or more of the forged steel. From the viewpoint of obtaining a higher strength, X is preferably 1.10 or more, more preferably 1.11 or more. The upper limit of X is determined from the viewpoint of ensuring excellent machinability, as described below.

[0017] [N content] If the N content is high (more than 0.012 mass%), N bonds with V before hot forging, forming coarse V carbonitrides and reducing the amount of dissolved vanadium. As a result, the amount of fine V carbides precipitated in ferrite, which contributes to improving strength, decreases, and the strength of the part decreases. V carbonitrides obtained by bonding with N precipitate at a higher temperature than V carbides. If V carbonitrides are formed at a high temperature, as mentioned above, the amount of fine V carbides precipitated decreases, and V does not contribute to improving strength. Therefore, it is necessary to suppress the amount of N in order to improve strength.

[0018] [Machinability] [Regarding the upper limit of formula (1)] The present inventors have also investigated the range of X in the above formula (1) from the viewpoint of improving machinability, particularly suppressing tool wear during turning, and have found that it is preferable to set X in the following formula (1) to 1.37 or less. X=[C]+0.28×[Mn]-1.03×[S]+0.323×[Cr]+1.69×[V]...(1) Here, [C], [Mn], [S], [Cr], and [V] respectively indicate the content of C, Mn, S, Cr, and V in the steel, expressed in mass%, and elements that are not contained are registered as zero.

[0019] If the value of X represented by the above formula (1) is too large, exceeding 1.37, the strength of the forged steel becomes too high, and the machinability (suppression of tool wear) of the forged steel during part processing decreases. X is preferably 1.35 or less, and more preferably 1.33 or less.

[0020] [Si content] Conventionally, research has been conducted on the effect of Si addition on machinability in hot tool steels (420 to 500 Hv) that are often used after tempering 5% by mass Cr steel, carburized equivalent quenched materials with a hardness of about 700 Hv, cold tool steels, and the like. In these steels, both cases in which Si improves and worsens machinability have been confirmed. The reason why both cases have been confirmed is thought to be due to material components other than Si and cutting methods, etc. On the other hand, in steels with the strength level according to this embodiment, the effect of Si on machinability has not been investigated, and the effect has not been made clear. Therefore, the inventors have conducted research on the chemical composition of this embodiment, and have found that when turning is performed as cutting with the chemical composition of this embodiment, by increasing the Si content, Si in the steel adheres to the tool during turning of the forged steel, suppressing tool wear, that is, improving the machinability of the forged steel.

[0021] It has been discovered that by using a non-heat treated forging steel in which the above-mentioned parameter X and the contents of N and Si in the chemical composition are within the specified ranges, a forged steel exhibiting high strength with a TS of 1060 MPa or more and good machinability in turning during part processing (reduced tool wear) can be obtained by hot forging and cooling under normal conditions without adding any special processes, and that the non-heat treated forged parts obtained by turning the forged steel exhibit high strength.

[0022] The range of each component is described in detail below. Note that, with respect to the content of an element shown in this specification, the expression "(numerical value) mass% or less (including 0 mass%)" means that it includes not only the case where it is intentionally added and the case where it is 0 mass%, but also the case where it is not intentionally added, that is, the case where the content is at the level of an unavoidable impurity.

[0023] [C:0.34~0.50% by mass] C is a solid solution strengthening element necessary for ensuring strength. If the C content is too low, the strength decreases. From this viewpoint, the C content must be 0.34 mass% or more. The C content is preferably 0.36 mass% or more, and more preferably 0.38 mass% or more. However, if the C content is excessive, the strength becomes excessively high and the machinability deteriorates. From this viewpoint, the C content must be 0.50 mass% or less. The C content is preferably 0.48 mass% or less, and more preferably 0.45 mass% or less.

[0024] [Si:0.60~1.00% by mass] Si is an important element in this embodiment. Si is useful as a deoxidizing element during steel smelting, and as described above, it adheres to tools during turning and suppresses tool wear, thereby improving the machinability of the steel. From this viewpoint, the Si content needs to be 0.60 mass% or more. The Si content is preferably 0.62 mass% or more, and more preferably 0.65 mass% or more. However, if the Si content is excessive, the amount of decarburization increases after hot forging, causing a decrease in fatigue strength. From this viewpoint, the Si content needs to be 1.00 mass% or less. The Si content is preferably 0.90 mass% or less, and more preferably 0.80 mass% or less. It is presumed that the Si content in Patent Document 2 is low, and the effect of suppressing tool wear during turning cannot be obtained.

[0025] [Mn:0.90~1.40% by mass] Mn can ensure the strength of steel material by solid solution strengthening. To achieve this effect, the Mn content is set to 0.90 mass% or more. The Mn content is preferably 0.92 mass% or more, and more preferably 0.95 mass% or more. However, if the Mn content is excessive, supercooled structures such as bainite are generated, and the strength is rather reduced. From this viewpoint, the Mn content needs to be set to 1.40 mass% or less. The Mn content is preferably 1.30 mass% or less, and more preferably 1.20 mass% or less.

[0026] [P:0.010~0.050% by mass] P has the effect of enhancing fracture splitting properties during the manufacture of parts such as connecting rods. From this viewpoint, the P content is set to 0.010% by mass or more. The P content is preferably 0.015% by mass or more, and more preferably 0.020% by mass or more. However, excessive P content may induce casting defects such as cracks during continuous casting. From this viewpoint, the P content is set to 0.050% by mass or less. The P content is preferably 0.045% by mass or less, more preferably 0.040% by mass or less, and even more preferably 0.035% by mass or less.

[0027] [S:0.040~0.120% by mass] S hardly dissolves in steel, but forms sulfides such as MnS, and has the effect of enhancing chip separation by concentrating stress on the sulfides during cutting. From this viewpoint, the S content needs to be 0.040% by mass or more. The S content is preferably 0.050% by mass or more, and more preferably 0.055% by mass or more. However, excessive S content can cause continuous casting cracks, hot forging cracks, and reduced fatigue strength. Therefore, the S content needs to be 0.120% by mass or less. The S content is preferably 0.100% by mass or less, and more preferably 0.080% by mass or less.

[0028] [Cr:0.15~0.40% by mass] Cr can ensure the strength of the steel material by solid solution strengthening. Therefore, the Cr content is set to 0.15 mass% or more. The Cr content is preferably 0.16 mass% or more, and more preferably 0.18 mass% or more. However, if the Cr content is excessive, supercooled structures such as bainite are generated, which reduces the strength. From this viewpoint, the Cr content needs to be set to 0.40 mass% or less. The Cr content is preferably 0.38 mass% or less, and more preferably 0.35 mass% or less.

[0029] [V:0.20~0.40% by mass] V is an element necessary for ensuring strength, and can strengthen ferrite by becoming V carbide in steel and finely precipitating in ferrite during cooling after forging. From this viewpoint, the V content needs to be 0.20 mass% or more. The V content is preferably 0.25 mass% or more, and more preferably 0.30 mass% or more. However, if the V content is excessive, the above effects are saturated, the cost of adding it is not worth it, and hot workability is hindered, resulting in deterioration of manufacturability. From this viewpoint, the V content needs to be 0.40 mass% or less. The V content is preferably 0.39 mass% or less, and more preferably 0.37 mass% or less.

[0030] [Al: more than 0 mass%, 0.010 mass% or less] Al is useful as a deoxidizing element during steel smelting. When an appropriate amount of Al is contained, an Al-Si-Ca composite oxide that is effective for machinability (suppression of tool wear) is formed. Therefore, the Al content may be more than 0 mass%. However, if Al is contained in excess, a hard oxide of Al alone is formed, which deteriorates machinability. From this viewpoint, the Al content must be 0.010 mass% or less. The Al content is preferably 0.008 mass% or less, and more preferably 0.005 mass% or less.

[0031] [N: more than 0 mass%, 0.012 mass% or less] If the N content is high, as described above, N bonds with V before hot forging to form coarse V carbonitrides. The formation of V carbonitrides reduces the amount of dissolved V, and the amount of fine V carbides in ferrite that precipitate after the formation of V carbonitrides and contribute to improving strength is reduced, resulting in a decrease in the strength of the part. From this perspective, the N content must be 0.012 mass% or less. The N content is preferably 0.010 mass% or less, and more preferably 0.008 mass% or less.

[0032] [Balance: Fe and unavoidable impurities] In a preferred embodiment, the balance is Fe and unavoidable impurities. As unavoidable impurities, the inclusion of trace elements (e.g., As, Sb, Sn, etc.) brought in due to the conditions of raw materials, materials, manufacturing facilities, etc. is permitted. In this specification, the unavoidable impurities also include any element in an amount within the range shown below. Therefore, the "unavoidable impurities" in the above "balance: Fe and unavoidable impurities" is a concept excluding any element at the unavoidable impurity level below. Ni≦0.02 mass%, Cu≦0.02 mass%, Mo≦0.01 mass%, Ti≦0.007 mass%, Ca≦0.0009 mass%, Pb≦0.00002 mass%, Sb≦0.0004 mass%, Te≦0.0001 mass%, Zr≦0.0002 mass%, Mg≦0.0001 mass%, REM≦0.0001 mass%

[0033] The chemical composition in this embodiment does not necessarily include the elements described below. Any other elements may be further included as long as the desired characteristics can be maintained. By including the optional elements described below as necessary, the strength and the like can be further increased.

[0034] [Ni: 0.20 mass% or less (including 0 mass%)] Ni may not be contained. Alternatively, the above amount of Ni may be contained as necessary. That is, Ni: 0 to 0.20 mass%. By including Ni, the strength of the steel material can be ensured by solid solution strengthening. From the viewpoint of exerting this effect, the Ni content may be more than 0.02 mass%. However, if the Ni content is excessive, the strength becomes excessively high and the machinability deteriorates. From this viewpoint, the Ni content needs to be 0.20 mass% or less. The Ni content is preferably 0.10 mass% or less, and more preferably 0.05 mass% or less.

[0035] [Cu: 0.20% by mass or less (including 0% by mass)] Cu may not be contained. Alternatively, the above amount of Cu may be contained as necessary. That is, Cu: 0 to 0.20 mass%. By containing Cu, the strength of the steel material can be ensured by solid solution strengthening. From the viewpoint of exerting this effect, the Cu content may be more than 0.02 mass%. However, if the Cu content is excessive, hot workability is hindered and manufacturability is deteriorated. From this viewpoint, the Cu content needs to be 0.20 mass% or less. The Cu content is preferably 0.10 mass% or less, and more preferably 0.05 mass% or less.

[0036] [Mo: 0.20% by mass or less (including 0% by mass)] Mo may not be contained. Alternatively, the above amount of Mo may be contained as necessary. That is, Mo: 0 to 0.20 mass%. By including Mo, the strength of the steel material can be ensured by solid solution strengthening. From the viewpoint of exerting this effect, the Mo content may be more than 0.01 mass%. However, if the Mo content is excessive, the strength becomes excessively high and the machinability deteriorates. From this viewpoint, the Mo content needs to be 0.20 mass% or less. The Mo content is preferably 0.10 mass% or less, and more preferably 0.05 mass% or less.

[0037] [Ti: 0.030 mass% or less (including 0 mass%)] Ti may not be contained. Alternatively, the above amount of Ti may be contained as necessary. That is, Ti: 0 to 0.030 mass%. The inclusion of Ti reduces the toughness of the steel material and has the effect of enhancing fracture splitting property during the manufacture of parts such as connecting rods. From the viewpoint of exerting this effect, the Ti content may be more than 0.007 mass%. However, if the Ti content is excessive, supercooled structures such as bainite are generated when parts are manufactured by normal hot forging, and the toughness increases and the fracture splitting property decreases. From this viewpoint, the Ti content needs to be 0.030 mass% or less. The Ti content is preferably 0.025 mass% or less, more preferably 0.020 mass% or less.

[0038] [Ca: 0.030% or less by mass (including 0% by mass)] Ca may not be contained. Alternatively, the above amount of Ca may be contained as necessary. That is, Ca: 0 to 0.030 mass%. Ca is a machinable element, and by including Ca, it has the effect of improving machinability by effects such as the formation of a Bellague (tool protective film). From the viewpoint of exerting this effect, the Ca content may be more than 0.0009 mass%. However, even if the Ca content is excessive, the above effect saturates and costs increase. From this viewpoint, the Ca content needs to be 0.030 mass% or less. The Ca content is preferably 0.025 mass% or less, and more preferably 0.020 mass% or less.

[0039] [Pb: 0.10% by mass or less (including 0% by mass)] [Sb: 0.10% by mass or less (including 0% by mass)] [Te: 0.10% by mass or less (including 0% by mass)] Pb, Sb, and Te may not be included. Alternatively, for example, one or more selected from the group consisting of Pb, Sb, and Te may be contained in the above amount. That is, one or more of Pb: 0 to 0.10 mass%, Sb: 0 to 0.10 mass%, and Te: 0 to 0.10 mass% may be satisfied. Pb, Sb, and Te are all elements effective for improving chip disposability during processing. To achieve this effect, the contents of Pb, Sb, and Te may be more than 0.00002 mass%, more than 0.0004 mass%, and more than 0.0001 mass%, respectively. However, if the contents of Pb, Sb, and Te are too high, the strength and hot workability are reduced, so that each content is preferably 0.10 mass% or less. Each content is preferably 0.05 mass% or less, and more preferably 0.01 mass% or less.

[0040] [Zr: 0.005 mass% or less (including 0 mass%)] [Mg: 0.005% by mass or less (including 0% by mass)] [REM: 0.02% by mass or less (including 0% by mass)] Zr, Mg, and REM may not be included. Alternatively, for example, one or more selected from the group consisting of Zr, Mg, and REM may be contained in the above amounts. That is, one or more of Zr: 0 to 0.005 mass%, Mg: 0 to 0.005 mass%, and REM: 0 to 0.02 mass% may be satisfied. Zr, Mg, and REM are all elements effective for improving the fracture splitting properties of parts. To exert this effect, the contents of Zr, Mg, and REM may be more than 0.0002 mass%, more than 0.0001 mass%, and more than 0.0001 mass%, respectively. However, if the contents of Zr, Mg, and REM are too high, the effect is saturated, so that the contents of Zr and Mg are preferably 0.005 mass% or less, and the REM content is preferably 0.02 mass% or less. The content of each of Zn and Mg is more preferably 0.004% by mass or less, and even more preferably 0.003% by mass or less, and the content of REM is more preferably 0.01% by mass or less, and even more preferably 0.005% by mass or less. Note that the REM includes lanthanoid elements (15 elements from La to Lu), Sc (scandium), and Y (yttrium).

[0041] [X represented by the following formula (1) is 1.09 to 1.37 X=[C]+0.28×[Mn]-1.03×[S]+0.323×[Cr]+1.69×[V]...(1) Here, [C], [Mn], [S], [Cr], and [V] indicate the contents of C, Mn, S, Cr, and V in the steel, respectively, expressed in mass%, and elements that are not included are considered to be zero.] As described above, the present inventors have studied the degree of influence of each of the above elements on the strength and machinability of steel and found formula (1) as a formula for improving the strength and machinability of steel. In order to achieve a strength (TS) of 1060 MPa or more of forged steel (forged material), X needs to be 1.09 or more. From the viewpoint of obtaining higher strength, X is preferably 1.10 or more, more preferably 1.11 or more. On the other hand, if the value of X is too large, the strength of the forged steel becomes too high, and the machinability (tool wear) during processing of the forged steel parts decreases. Therefore, X is set to 1.37 or less. X is preferably 1.35 or less, more preferably 1.33 or less.

[0042] (Production method of non-thermal forging steel) The non-tempered forging steel according to the present embodiment can be manufactured by the following method. First, a steel satisfying the above-mentioned chemical composition is melted and cast. The casting method is not particularly limited, and a commonly used method may be adopted. For example, an ingot casting method or a continuous casting method may be adopted. After casting, hot blooming may be performed as necessary. Blooming may include a soaking treatment before blooming. Blooming conditions are not particularly limited, and a commonly used method may be adopted. For example, blooming may be performed at 1000°C to 1250°C. Conditions for hot rolling performed after blooming are also not particularly limited, and a commonly used method may be adopted. For example, hot rolling may be performed at 850°C to 1200°C. In addition, processing may be performed by forging and stretching instead of hot rolling.

[0043] 2.Non-thermal forged steel The non-heat treated forging steel according to this embodiment has the same chemical composition as the above-mentioned non-heat treated forging steel and the range of the parameter X. Since the non-heat treated forging steel according to this embodiment has a chemical composition and a parameter X within a predetermined range, it exhibits high strength and excellent machinability in which tool wear is suppressed when cutting, particularly when turning, is performed.

[0044] (Production method of non-thermal forged steel) The non-tempered forging steel according to this embodiment can be obtained by hot forging the non-tempered forging steel. The structure of non-tempered forging steel is generally mainly affected by the heating temperature before hot forging and the cooling rate after hot forging, but the non-tempered forging steel according to this embodiment has a chemical composition and a parameter X range that are appropriately controlled, so that if hot forging is performed under normal conditions, a non-tempered forging steel having desired properties can be obtained. For example, the heating temperature before hot forging can be 1150 to 1350°C, and the cooling rate after hot forging, for example, the average cooling rate from 800°C to 500°C can be 0.8 to 3.0°C / sec.

[0045] (characteristic) The non-heat treated forged steel according to this embodiment exhibits high strength, and non-heat treated forged parts obtained by machining the non-heat treated forged steel also have sufficient strength as parts. In this embodiment, the non-heat treated forged steel having high strength and "sufficient strength as parts" means that the TS evaluated in the examples described later is 1060 MPa or more, preferably 1065 MPa or more, and more preferably 1070 MPa or more.

[0046] As described above, the non-heat treated forged steel according to this embodiment has excellent machinability, particularly excellent tool wear resistance. In the present invention, "excellent tool wear resistance" means that the maximum wear amount (Vbmax) on the flank after cutting 5000 m with a cermet tool, as evaluated in the examples described later, is 120 μm or less. The Vbmax is preferably 117 μm or less, more preferably 115 μm or less.

[0047] 3.Non-thermal forged parts The present disclosure also includes a non-heat treated forged part produced using the non-heat treated forging steel (made using the non-heat treated forging steel). The chemical composition of the non-heat treated forged part is the same as the chemical composition of the non-heat treated forging steel described above, and is also the same as the chemical composition of the non-heat treated forging steel.

[0048] Specific examples of the non-heat treated forged parts according to this embodiment include forged parts such as connecting rods, lower arms, and crankshafts used in engines and chassis of transport vehicles such as automobiles and ships.

[0049] (Manufacturing method for non-thermal refined forged parts) The non-thermal treated forged parts according to the present embodiment can be obtained by using the non-thermal treated forged steel. The non-thermal treated forged parts according to the present embodiment can be obtained by forming the non-thermal treated forged steel into a desired part shape by performing machining including cutting. The non-thermal treated forged steel according to the present embodiment exhibits excellent machinability when cutting as a machining process, and can sufficiently suppress tool wear. As a result, the period until tool replacement can be extended, which contributes to improving the productivity of the non-thermal treated forged parts. Examples of tools used for the cutting include those generally used in cutting processes, such as those made of cemented carbide, high-speed steel, cermet, ceramics, cBN (Cubic Boron Nitride), etc. When the non-thermal treated forged part is a connecting rod, from the viewpoint of reducing the part manufacturing cost, a method of cold fracture separation can be adopted in which the non-thermal treated forged steel is machined and then the large end portion is made into two approximately semicircular parts. EXAMPLES

[0050] The present invention will be described in more detail below with reference to examples. The present invention is not limited to the following examples, and can be practiced with appropriate modifications within the scope of the above and below-mentioned aims, and all such modifications are included in the technical scope of the present invention.

[0051] For Nos. A to D, F and G in Table 1, a small melting furnace (capacity 150 kg / ch) was used to melt and cast the steel according to the usual melting method, and then the steel was forged and stretched at a heating temperature of 1200°C to obtain square bars having a cross section perpendicular to the longitudinal direction of a square with each side measuring 20 mm and a length of 1100 mm, and round bars having a cross section perpendicular to the longitudinal direction of a diameter of 27 mm and a length of 1100 mm, which correspond to non-tempered forging steel.

[0052] For No. E in Table 1, melting, casting, blooming, and hot rolling were performed in the usual manner using an actual machine to obtain a round bar having a cross section perpendicular to the longitudinal direction of 34 mm in diameter, which corresponds to non-tempered forging steel. In Table 1 and Table 2 described later, underlined values ​​indicate values ​​outside the range of components and the like specified in this embodiment. In addition, "unavoidable impurities" in Table 1 may also include any element at the level of inevitable impurities described above.

[0053] Using square bars or round bars corresponding to the above non-tempered forging steel, the following tensile test and machinability evaluation were carried out.

[0054] (1) Tensile test First, test pieces for tensile tests were prepared as follows. A square bar with a square of 20 mm or a round bar with a diameter of 34 mm was cut perpendicular to the longitudinal direction to a length of 100 mm. The square bar or round bar with a length of 100 mm was held at 1250°C for 10 minutes, then removed from the furnace and immediately press-forged in a direction perpendicular to the rolling direction to compress the square bar to a thickness of 8 mm and the round bar to a thickness of 10 mm. After that, the test pieces were left to cool or air-blast-cooled so that the cooling rate between 800°C and 500°C was 1.4 to 1.9°C / s, and then cooled to room temperature to obtain forged steel.

[0055] Test piece samples were taken from the obtained forged steel at a location that satisfied all of the following conditions: the center in the longitudinal direction, the center in the thickness direction, and the center in the width direction. The test piece samples were processed into No. 14B test pieces as specified in JIS Z 2241 (2005). The longitudinal direction of the No. 14B test piece was aligned with the longitudinal direction of the square bar, and the tensile force was also aligned with the same direction. The tensile test was carried out at room temperature according to JIS Z 2241 (2005). When the TS was 1060 MPa or more, the test piece was evaluated as having sufficient strength for use as a part and was deemed to have passed the test. The test results are shown in Table 2.

[0056] (2) Machinability evaluation The machinability of Nos. A to E and G was evaluated by the following machinability test. First, test pieces for machinability evaluation were prepared as follows. A round bar with a diameter of 27 mm or a round bar with a diameter of 34 mm was turned on a lathe to obtain a round bar with a diameter of 25 mm. The round bar with a diameter of 25 mm was again held at 1200°C for 1 hour, and then subjected to air blast cooling at a cooling rate of 1.0 to 1.2°C / s between 800°C and 500°C to obtain a test piece for machinability evaluation simulating forged steel.

[0057] In the machinability test, an NC lathe was used as a test machine, and the above-mentioned test pieces for machinability evaluation (test pieces with a diameter of 25 mm and a length of 100 mm) were turned under the following cutting test conditions. Then, on the flank face of the cermet tool used for cutting, the maximum wear amount (Vbmax) after cutting 5000 m was determined for Nos. A to E, and the maximum wear amount (Vbmax) after cutting 10000 m was determined for No. G. In the present invention, when the maximum wear amount (Vbmax) after cutting 5000 m was 120 μm or less, it was evaluated as having excellent machinability and was deemed to have passed. The test results are shown in Table 2. Cutting test (peripheral turning test) conditions Tool: Cermet (Tungaloy DNMA150404-NS520) Holder: DJNR / L 2525 Cutting speed: 200m / min Feed rate: 0.1mm / rev Depth of cut: 0.5mm Initial scale removal amount: 3.0mm Lubrication: WET

[0058] [Table 1]

[0059] [Table 2]

[0060] From Tables 1 and 2, the following can be seen. Nos. A, B, and G are inventive examples that satisfy all the requirements in the embodiments of the present invention. That is, since each component and X shown in formula (1) are all within the specified range, TS was 1060 MPa or more, and Vbmax was 120 μm or less. Note that for No. G, the cutting distance was 10,000 m, which is different from the cutting test conditions for the other examples. However, since the cutting distance was longer than the 5,000 m of the other examples and the cutting test was performed under sufficiently severe conditions, and Vbmax was 89 μm, it is assumed that Vbmax will be 120 μm or less even when the cutting distance is 5,000 m.

[0061] In contrast, Nos. C to F are comparative examples that do not satisfy any of the requirements in the embodiments of the present invention. That is, No. C exceeded the upper limit of the range defined by X shown in formula (1), and had poor machinability.

[0062] No. D was below the lower limit of the range defined by X in formula (1) and had poor strength.

[0063] No. E had an insufficient Si content and was poor in machinability.

[0064] No. F had an excessive N content and was inferior in strength.

Claims

1. C: 0.34 to 0.50% by mass, Si: 0.60 to 1.00% by mass, Mn: 0.90 to 1.40% by mass, P: 0.010 to 0.050% by mass, S: 0.040 to 0.120% by mass, Cr: 0.15 to 0.40% by mass, V: 0.20 to 0.40% by mass, Al: more than 0 mass%, 0.010 mass% or less, N: more than 0 mass%, 0.012 mass% or less, Ni: 0.20 mass% or less (including 0 mass%), Cu: 0.20 mass% or less (including 0 mass%), Mo: 0.20 mass% or less (including 0 mass%), Ti: 0.030 mass% or less (including 0 mass%), Ca: 0.030% by mass or less (including 0% by mass), Pb: 0.10% by mass or less (including 0% by mass), Sb: 0.10 mass% or less (including 0 mass%), Te: 0.10 mass% or less (including 0 mass%), Zr: 0.005 mass% or less (including 0 mass%), Mg: 0.005% by mass or less (including 0% by mass), and REM: 0.02% by mass or less (including 0% by mass) and the balance being Fe and unavoidable impurities, A non-tempered forging steel, in which X in the following formula (1) is 1.09 to 1.

37. X=[C]+0.28×[Mn]-1.03×[S]+0.323×[Cr]+1.69×[V]...(1) Here, [C], [Mn], [S], [Cr], and [V] respectively indicate the contents of C, Mn, S, Cr, and V in the steel, expressed in mass%, and elements that are not contained are registered as zero.

2. C: 0.34 to 0.50% by mass, Si: 0.60 to 1.00% by mass, Mn: 0.90 to 1.40% by mass, P: 0.010 to 0.050% by mass, S: 0.040 to 0.120% by mass, Cr: 0.15 to 0.40% by mass, V: 0.20 to 0.40% by mass, Al: more than 0 mass%, 0.010 mass% or less, N: more than 0 mass%, 0.012 mass% or less, Ni: 0.20 mass% or less (including 0 mass%), Cu: 0.20 mass% or less (including 0 mass%), Mo: 0.20 mass% or less (including 0 mass%), Ti: 0.030 mass% or less (including 0 mass%), Ca: 0.030% by mass or less (including 0% by mass), Pb: 0.10% by mass or less (including 0% by mass), Sb: 0.10 mass% or less (including 0 mass%), Te: 0.10 mass% or less (including 0 mass%), Zr: 0.005 mass% or less (including 0 mass%), Mg: 0.005% by mass or less (including 0% by mass), and REM: 0.02% by mass or less (including 0% by mass) and the balance being Fe and unavoidable impurities, A non-tempered forged steel, in which X in the following formula (1) is 1.09 to 1.

37. X=[C]+0.28×[Mn]-1.03×[S]+0.323×[Cr]+1.69×[V]...(1) Here, [C], [Mn], [S], [Cr], and [V] respectively indicate the content of C, Mn, S, Cr, and V in the steel, expressed in mass%, and elements that are not contained are registered as zero.

3. A non-heat treated forged part made using the non-heat treated forged steel according to claim 2.

Citation Information

Patent Citations

  • High strength non-heat-treated steel for fracture partition, and steel component for fracture partition

    JP2010077488A

  • Hot-forged non-heat treated steel part and hot-forgeable non-heat treated steel used for the same

    JP2011195862A

  • Hot rolled steel for steel component excellent in fittability and machinability of fracture surfaces each other after fracture separation and steel component