Resin sheet and fabric laminate
A resin sheet composition with 4-methyl-1-pentene polymer and thermoplastic elastomer addresses adhesion and heat resistance issues, ensuring strong bonding and flexibility in high-temperature environments.
Patent Information
- Application Number
- JP2024049048
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-15
AI Technical Summary
Conventional resin sheets made from 4-methyl-1-pentene polymers face issues with adhesion to fabrics, affecting the texture and heat resistance, particularly in high-temperature environments, and require improvements in bonding methods to maintain flexibility and stretchability.
A resin sheet composition containing 4-methyl-1-pentene polymer and a thermoplastic elastomer with controlled storage modulus and adhesive strength, combined with a compatibilizer, to enhance adhesion and heat resistance while maintaining flexibility and stretchability.
The resin sheet achieves strong adhesion to fabrics with improved heat resistance, maintaining flexibility and stress relaxation properties, even under high temperatures and during washing or ironing.
Smart Images

Figure 2024146837000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin sheet, and more particularly to a resin sheet, a fabric laminate and a clothing item using the resin sheet, and a method for producing the fabric laminate. [Background technology]
[0002] Resin sheets using 4-methyl-1-pentene polymers, which contain 4-methyl-1-pentene as the main constituent monomer, have excellent flexibility and stretchability, and provide a pleasant feel on the skin, and are therefore expected to be widely used in a variety of applications, such as hygiene materials, clothing materials, and medical materials.
[0003] For example, Patent Document 1 (WO 2018 / 143411) discloses an example in which a sheet obtained by foaming a 4-methyl-1-pentene polymer is used as it is as a pressure supporter. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2018 / 143411 Summary of the Invention [Problem to be solved by the invention]
[0005] The present inventors focused on clothing made of a new material in which a resin sheet and a fabric are directly laminated, as a new application of a resin sheet using a 4-methyl-1-pentene polymer. However, when a conventional resin sheet as disclosed in Patent Document 1 is bonded to a fabric by thermocompression bonding, the resin sheet and the fabric material do not blend well, and it was found that there is room for improvement in terms of obtaining good adhesion. In addition, although adhesion can be improved by bonding at high temperatures, a problem occurs in that the texture of the fabric is hindered. Furthermore, when the resin sheet is used as the back or seat of a mobility chair for an automobile or the like, heat resistance is required in the interior of the vehicle where a high temperature environment in summer is expected, and when the resin sheet is used as clothing, heat resistance against washing, drying and ironing is also required. [Means for solving the problem]
[0006] The present inventors have conducted research focusing on improving adhesiveness to fabrics and heat resistance while maintaining the flexibility, stretchability, and good texture characteristic of resin sheets using 4-methyl-1-pentene polymers, and have found that some resin sheets containing 4-methyl-1-pentene polymers have good adhesiveness and heat resistance, while others do not. As a result of extensive research to distinguish between the two, the inventors have found that it is effective to devise a new index for adhesive strength and control it, and to control the storage modulus under specified conditions, and have completed the present invention.
[0007] That is, according to the present invention, there are provided the following resin sheet and related techniques.
[0008] [1] A resin sheet made of a resin composition containing a 4-methyl-1-pentene polymer (A) and a thermoplastic elastomer (B) having a melting point of 130 to 180°C, the 4-methyl-1-pentene polymer (A) contains a structural unit (a1) derived from 4-methyl-1-pentene and a structural unit (a2) derived from a linear α-olefin having 2 to 3 carbon atoms, A resin sheet having a storage modulus E' of 0.55 MPa or more and 7.0 MPa or less at 100°C when dynamic viscoelasticity is measured under conditions of a frequency of 1.59 Hz, a strain of 0.1%, a heating rate of 4°C / min, and a tensile mode in the temperature range of -60°C to 200°C. [2] A resin sheet made of a resin composition containing a 4-methyl-1-pentene polymer (A) and a thermoplastic elastomer (B) having a melting point of 130 to 180°C, the 4-methyl-1-pentene polymer (A) contains a structural unit (a1) derived from 4-methyl-1-pentene and a structural unit (a2) derived from a linear α-olefin having 2 to 3 carbon atoms, A resin sheet whose adhesive strength, measured by the following procedure, is 4N / 25mm or more and 30N / 25mm or less. [procedure] First, the resin sheet and the fabric x (thickness: 0.28 mm, basis weight: 100 g / m 2 (Materials: 89% polyester, 11% polyurethane) are layered so that the MD direction of the resin sheet is parallel to the direction in which the fabric x has the greatest elasticity, and are bonded under conditions of a pressure of 0.1 MPa, a time of 10 seconds, and a temperature of 190° C. to produce a laminate. The MD direction of the resin sheet of the laminate is set as the length direction, and the laminate is cut to a width of 25 mm to obtain a test piece. Next, the adhesive strength [N / 25 mm] of the test piece is measured when the resin sheet is peeled off from the substrate x using a tensile testing machine equipped with a thermostatic chamber at a test temperature of 100°C, a tensile speed of 300 mm / min, a peel angle of 180°, and a peel direction in the MD direction. [3] The resin sheet according to [1] or [2], wherein the Shore A hardness of at least one surface of the resin sheet immediately after measurement at 23°C in accordance with JIS K6253 is HS0, and the HS0 is 30 or more and 90 or less. [4] The resin sheet according to any one of [1] to [3], wherein the Shore A hardness of at least one surface of the resin sheet immediately after measurement, measured in accordance with JIS K6253 at 23°C, is HS0, and the Shore A hardness 15 seconds after measurement is HS1, and ΔHS, expressed as (HS0-HS1), is 3 or more and 30 or less. [5] The resin sheet according to any one of [1] to [4], wherein the resin sheet has a thickness of 0.1 mm or more and 3 mm or less. [6] The density of the resin sheet is 0.30 g / cm 3 More than 1.5g / cm 3 The resin sheet according to any one of [1] to [5] below. [7] The resin sheet according to any one of [1] to [6], wherein the Shore A hardness of the thermoplastic elastomer (B) is 30 or more and 90 or less. [8] The resin sheet according to any one of [1] to [7], wherein the thermoplastic elastomer (B) includes a thermoplastic elastomer (b1) having a functional group containing one or more atoms selected from the group consisting of oxygen, sulfur, nitrogen, and halogens. [9] The resin sheet according to any one of [1] to [8], wherein the thermoplastic elastomer (B) includes one or more thermoplastic elastomers (b2) selected from a thermoplastic polyamide-based elastomer, a thermoplastic polyurethane-based elastomer, and a thermoplastic polyester-based elastomer.
[10] The resin sheet according to any one of [1] to [9], wherein the resin composition further contains a compatibilizer (C).
[11] The resin sheet according to
[10] , wherein the compatibilizer (C) contains a modified styrene-based thermoplastic elastomer or a modified polyolefin-based thermoplastic elastomer.
[12] The content of the 4-methyl-1-pentene polymer (A) is 20 to 60 mass% based on the total amount of the resin composition, The content of the thermoplastic elastomer (B) is 20 to 80% by mass based on the total amount of the resin composition, The resin sheet according to
[10] or
[11] , wherein the content of the compatibilizer (C) is 5 to 20 mass % based on the total amount of the resin composition.
[13] The resin sheet according to any one of [1] to
[12] , wherein the thermoplastic elastomer (B) contains a thermoplastic elastomer (b3) consisting of a propylene-α-olefin copolymer containing a propylene unit and an α-olefin unit having 2 or 4 to 20 carbon atoms.
[14] The resin sheet according to any one of [1] to
[13] , wherein the thermoplastic elastomer (B) includes a thermoplastic elastomer (b4) consisting of one or more selected from a thermoplastic olefin-based elastomer, a thermoplastic styrene-based elastomer, and a compound thereof.
[15] A resin sheet according to any one of [1] to
[14] , which is used as a material for clothing.
[16] A fabric laminate having fabric bonded to at least one surface of the resin sheet described in any one of [1] to
[15] .
[17] The fabric has a basis weight of 75 g / m 2 ~300g / m 2 The fabric laminate according to
[16] ,
[18] The fabric laminate described in
[16] or
[17] , wherein at least a portion of the fabric laminate has a curved surface, and the radius of curvature of the curved surface is in the range of 50 mm to 150 mm.
[19] Clothing using the fabric laminate described in any one of
[16] to
[18] .
[20] The article of clothing described in
[19] , wherein the surface of the resin sheet is configured to be the surface that comes into contact with a human.
[21] A method for producing a fabric laminate, comprising the steps of: overlapping a fabric on at least one side of the resin sheet described in any one of [1] to
[15] ; and heat-sealing the fabric laminate under conditions of 140°C to 190°C and 0.1 MPa to 2.0 MPa. Effect of the Invention
[0009] According to the present invention, it is possible to provide a resin sheet that can achieve both adhesion to fabrics and heat resistance, and a technique relating to the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] In this specification, the expression "a to b" in the explanation of a numerical range means from a to b, unless otherwise specified. For example, "1 to 5% by mass" means "1% by mass to 5% by mass."
[0011] In this specification, MD direction refers to the machine direction and is intended to be the flow direction during molding of a resin sheet, and TD direction refers to the transverse direction and is intended to be the direction perpendicular to the MD direction.
[0012] <Resin sheet> The resin sheet of the present embodiment is constituted by a resin composition containing a 4-methyl-1-pentene polymer (A) and a thermoplastic elastomer (B) having a melting point of 130 to 180°C, the 4-methyl-1-pentene polymer (A) contains a structural unit (a1) derived from 4-methyl-1-pentene and a structural unit (a2) derived from a linear α-olefin having 2 to 3 carbon atoms, When dynamic viscoelasticity is measured under conditions of a frequency of 1.59 Hz, a strain of 0.1%, a heating rate of 4°C / min, and a temperature range of -60°C to 200°C in a tensile mode, the storage modulus E' at 100°C is 0.55 MPa or more and 7.0 MPa or less.
[0013] By controlling the storage modulus E', the resin sheet can achieve high levels of adhesion to fabrics and heat resistance while retaining the flexibility, stretchability, and good feel that are characteristic of resin sheets using 4-methyl-1-pentene polymer (A).
[0014] The storage modulus E' is preferably 0.55 MPa to 6.0 MPa, and more preferably 0.57 MPa to 5.0 MPa. By setting the storage modulus E' within the above numerical range, both adhesiveness and heat resistance can be more effectively achieved.
[0015] The resin sheet of the present embodiment may be constituted by a resin composition containing a 4-methyl-1-pentene polymer (A) and a thermoplastic elastomer (B) having a melting point of 130 to 180°C, in which the 4-methyl-1-pentene polymer (A) contains a structural unit (a1) derived from 4-methyl-1-pentene and a structural unit (a2) derived from a linear α-olefin having 2 to 3 carbon atoms, and may be constituted so that the adhesive strength measured by the following procedure is 4 N / 25 mm or more and 30 N / 25 mm or less.
[0016] [procedure] First, the resin sheet and the fabric x (thickness: 0.28 mm, basis weight: 100 g / m 2 (Materials: 89% polyester, 11% polyurethane) are layered so that the MD direction of the resin sheet is parallel to the direction in which the fabric x has the greatest elasticity, and are bonded under conditions of a pressure of 0.1 MPa, a time of 10 seconds, and a temperature of 190° C. to produce a laminate. The MD direction of the resin sheet of the laminate is set as the length direction, and the laminate is cut to a width of 25 mm to obtain a test piece. Next, the adhesive strength [N / 25 mm] of the test piece is measured when the resin sheet is peeled off from the substrate x using a tensile testing machine equipped with a thermostatic chamber at a test temperature of 100°C, a tensile speed of 300 mm / min, a peel angle of 180°, and a peel direction in the MD direction.
[0017] By controlling the adhesive strength, the resin sheet of the present embodiment can achieve high levels of adhesion to fabrics and heat resistance while retaining the flexibility, stretchability, stress relaxation property, and good feel that are characteristic of resin sheets using the 4-methyl-1-pentene polymer (A).
[0018] In order to obtain good adhesion to the fabric, the adhesive strength is preferably 5 N / 25 mm or more, and more preferably 6 N / 25 mm or more. The adhesive strength is preferably 25 N / 25 mm or less, more preferably 15 N / 25 mm or less, and even more preferably 12 N / 25 mm or less, in order to obtain good adhesion to the fabric while maintaining heat resistance.
[0019] Although the details of the mechanism by which such an effect is obtained are not clear, it is speculated as follows. First, when the resin sheet is heated and pressed against the fabric, part of the molten resin sheet penetrates into the weave of the fabric, bonding the resin sheet and the fabric. At this time, it is important that the thermal properties of the resin, the compatibility of the molten resin with the fabric, and the ease of impregnation are appropriate. Therefore, it is presumed that by using a predetermined storage modulus or a predetermined adhesive strength to the fabric x as an indicator of thermal behavior, it is possible to effectively control the thermal properties of the resin, its compatibility with the fabric, and its ease of impregnation, thereby improving the adhesiveness and heat resistance of the resin sheet to the fabric.
[0020] In the above procedure, the stretchability of the fabric x is calculated based on the elongation percentage defined in accordance with Method B of JIS L 1096, Fabric Testing Method for Woven and Knitted Fabrics.
[0021] The resin sheet of the present embodiment can be realized by selecting materials constituting the resin sheet, adjusting the blending amounts, or devising a method for producing the resin sheet by combining known methods, etc. For example, the selection and combination of the 4-methyl-1-pentene polymer (A) and the thermoplastic elastomer (B) may be adjusted, or the raw materials for the resin sheet may be thoroughly kneaded using a twin-screw extruder.
[0022] Next, the physical properties of the resin sheet will be described.
[0023] [Loss tangent (tanδ)] It is preferable that the resin sheet has at least one temperature showing a maximum value of loss tangent (tan δ) in the range of at least 10°C to 100°C, as determined by dynamic viscoelasticity measurement under conditions of a heating rate of 4°C / min, a frequency of 1.59 Hz, and a distortion of 0.1%, and that the maximum value of the loss tangent is at least 0.1 to 3.5.
[0024] The temperature at which the loss tangent (tan δ) of dynamic viscoelasticity shows a maximum value is preferably at least one in the range of 10°C or higher and 40°C or lower, more preferably at least one in the range of 15°C or higher and 38°C or lower, and even more preferably at least one in the range of 15°C or higher and 38°C or lower. The maximum value of the loss tangent (tan δ) of the dynamic viscoelasticity is preferably 0.2 or more and 3.0 or less, more preferably 0.2 or more and 2.5 or less, and further preferably 0.5 or more and 2.0 or less.
[0025] In this embodiment, the maximum value of the loss tangent of the 4-methyl-1-pentene polymer (a) is preferably 0.8 or more, more preferably 1.0 or more, and even more preferably 1.2 or more. In this embodiment, the maximum value of the loss tangent is preferably 3.0 or less, and more preferably 2.8 or less.
[0026] The dynamic viscoelasticity measurement can be performed, for example, by preparing a test piece of 30 mm length × 10 mm width from the resin sheet of this embodiment and using a rheometer under the following conditions: frequency 1.59 Hz, heating rate 4°C / min, measurement temperature range 0°C to 110°C, distortion amount 0.1%, chuck distance 20 mm, and tension mode.
[0027] [Shore A hardness] In this embodiment, when the Shore A hardness of at least one surface of the resin sheet immediately after measurement, measured at 23°C in accordance with JIS K6253, is defined as HS0, HS0 is preferably 30 to 90, more preferably 35 to 87, and even more preferably 38 to 85. By setting the HS0 to the lower limit or more, the mechanical properties of the resin sheet can be improved, whereas by setting the HS0 to the upper limit or less, the inherent flexibility and stress relaxation properties of the resin sheet can be improved.
[0028] In this embodiment, when the Shore A hardness of at least one surface of the resin sheet immediately after measurement at 23°C in accordance with JIS K6253 is defined as HS0 and the Shore A hardness 15 seconds after measurement is defined as HS1, ΔHS represented by (HS0-HS1) is preferably 3 to 30, more preferably 5 to 30, and even more preferably 5 to 25. By setting ΔHS within the above-mentioned range, it becomes easier to improve the balance of the inherent flexibility, shape retention, shape conformability, and stress relaxation properties of the resin sheet while simultaneously achieving both heat resistance and adhesiveness. Also, a larger ΔHS means better stress relaxation properties.
[0029] The loss tangent and Shore A hardness of the resin sheet can be controlled within the above ranges by appropriately adjusting, for example, the type and blending ratio of the 4-methyl-1-pentene polymer (A), the presence or absence of crosslinking, the kneading method of the composition, and the like.
[0030] [MFR] The melt flow rate (MFR) of the resin sheet, measured in accordance with ASTM D1238 at 230° C. under a load of 2.16 kg, is preferably 3 to 50 g / 10 min. By setting the MFR of the resin sheet to be equal to or higher than the lower limit, the resin sheet in a molten state can easily impregnate the fabric, and can easily adhere to the fabric. On the other hand, by setting the MFR of the resin sheet to be equal to or less than the upper limit, the amount of thermal deflection is small, creep deformation is less likely to occur, and heat resistance can be easily imparted. The MFR of the resin sheet can be achieved by selecting the materials for the resin sheet and adjusting the blending amounts.
[0031] Thickness The average thickness of the resin sheet is not particularly limited, but is preferably in the range of 0.1 mm to 3 mm, more preferably in the range of 0.2 mm to 2 mm, and even more preferably in the range of 0.3 mm to 1 mm. By setting the average thickness of the resin sheet to be equal to or more than the lower limit, the resin sheet can more easily retain the flexibility, stretchability, stress relaxation property, and good texture characteristic of a resin sheet using a 4-methyl-1-pentene polymer (A) while obtaining adhesion to fabrics. On the other hand, by setting the average thickness of the resin sheet to be equal to or less than the upper limit, it is possible to improve adhesion to the fabric while maintaining good heat resistance.
[0032] [density] The density of the resin sheet measured according to ASTM D 1505 (underwater displacement method) is preferably 0.3 to 1.5 g / cm 3 and preferably 0.4 to 1.4 g / cm 3 and more preferably 0.5 to 1.2 g / cm 3 and more preferably 0.6 to 1.2 g / cm 3 It is. By setting the density of the resin sheet to the lower limit or more, it is possible to increase the mechanical strength while improving the adhesiveness and heat resistance, whereas by setting the density of the resin sheet to the upper limit or less, it is easy to impart flexibility and reduce the weight. The density of the resin sheet can be adjusted by the selection of the materials for the resin composition as well as by whether or not the resin sheet is foamed and the degree of foaming.
[0033] [form] The resin sheet of the present embodiment may be in the form of a foam containing bubbles, or may not be in the form of a foam. By using a foam, the flexibility and cushioning properties of the resin sheet can be easily improved. The expansion ratio is not particularly limited, and can be appropriately determined taking into consideration the application of the resin sheet, etc. In the present embodiment, the resin sheet being a foamed body refers to, for example, a porous body having a large number of air bubbles (cavities) inside the resin sheet.
[0034] [Resin composition] Next, the resin composition constituting the resin sheet will be described. The resin composition constituting the resin sheet contains a 4-methyl-1-pentene polymer (A) and a thermoplastic elastomer (B) having a melting point of 130 to 180°C.
[0035] [4-Methyl-1-pentene polymer (A)] The 4-methyl-1-pentene polymer (A) contains, for example, a structural unit (a1) derived from 4-methyl-1-pentene and a structural unit (a2) derived from an α-olefin having 2 to 3 carbon atoms other than 4-methyl-1-pentene.
[0036] In the 4-methyl-1-pentene polymer (A) according to this embodiment, from the viewpoint of further improving the flexibility of the resin sheet, when the sum of the structural units (a1) and (a2) is taken as 100 mol %, it is preferable that the content of the structural unit (a1) is 10 mol % or more and 90 mol % or less, and the content of the structural unit (a2) is 10 mol % or more and 90 mol % or less. In addition, in the 4-methyl-1-pentene polymer (A) according to this embodiment, from the viewpoint of improving the flexibility and mechanical properties of the resin sheet, when the sum of the structural units (a1) and (a2) is taken as 100 mol%, the content of the structural unit (a1) is more preferably 30 mol% or more and 90 mol% or less, and the content of the structural unit (a2) is more preferably 10 mol% or more and 70 mol% or less, the content of the structural unit (a1) is even more preferably 50 mol% or more and 90 mol% or less, and the content of the structural unit (a2) is even more preferably 10 mol% or more and 50 mol% or less, the content of the structural unit (a1) is even more preferably 60 mol% or more and 90 mol% or less, and the content of the structural unit (a2) is even more preferably 10 mol% or more and 40 mol% or less, and the content of the structural unit (a1) is particularly preferably 65 mol% or more and 90 mol% or less, and the content of the structural unit (a2) is particularly preferably 10 mol% or more and 35 mol% or less.
[0037] Examples of the structural unit (a2) derived from a linear α-olefin having 2 to 3 carbon atoms include ethylene and propylene, and among these, propylene is preferred because it provides flexibility, stress relaxation properties, and the like while maintaining mechanical strength.
[0038] The 4-methyl-1-pentene polymer (A) may contain structural units other than the structural units (a1) and (a2) as long as the object of the present invention is not impaired. Examples of other structural units include structural units derived from non-conjugated polyenes. Examples of the non-conjugated polyene include linear, branched or cyclic dienes having preferably 5 to 20, more preferably 5 to 10 carbon atoms, various norbornenes, norbornadienes, etc. Among these, 5-vinylidene-2-norbornene and 5-ethylidene-2-norbornene are preferred.
[0039] The 4-methyl-1-pentene polymer (A) according to this embodiment has an intrinsic viscosity [η] in decalin at 135° C. of preferably 0.01 to 5.0 dL / g, more preferably 0.1 to 4.0 dL / g, even more preferably 0.5 to 3.0 dL / g, and particularly preferably 1.0 to 2.8 dL / g, from the viewpoint of improving the mechanical strength and moldability of the resin sheet.
[0040] The density of the 4-methyl-1-pentene polymer (A) according to this embodiment, measured according to ASTM D 1505 (water displacement method), is preferably 0.810 to 0.850 g / cm 3 , more preferably 0.820 to 0.850 g / cm 3 , and more preferably 0.830 to 0.850 g / cm 3 It is.
[0041] The 4-methyl-1-pentene polymer (A) according to the present embodiment can be produced by various methods. For example, it can be produced by using known catalysts such as magnesium-supported titanium catalysts; metallocene catalysts described in International Publication No. 01 / 53369, International Publication No. 01 / 027124, JP-A-3-193796, and JP-A-02-41303; and olefin polymerization catalysts containing metallocene compounds described in International Publication No. 2011 / 055803.
[0042] The content of the 4-methyl-1-pentene polymer (A) is preferably 10 to 80 mass %, more preferably 15 to 70 mass %, and further preferably 20 to 60 mass %, based on the total amount of the resin composition, thereby making it possible to obtain a resin sheet having an excellent balance between heat resistance and adhesiveness.
[0043] [Thermoplastic elastomer (B)] The thermoplastic elastomer (B) has a melting point of 130 to 180° C. and has good compatibility with the 4-methyl-1-pentene polymer (A), which is presumably why adhesion can be easily improved.
[0044] The melting point of the thermoplastic elastomer (B) can be measured using a DSC in accordance with JIS K7121.
[0045] The thermoplastic elastomer (B) preferably has a Shore A hardness of 30 to 90. By setting the Shore A hardness of the thermoplastic elastomer (B) within the above range, flexibility and stress relaxation properties can be easily imparted.
[0046] The Shore A hardness of the thermoplastic elastomer (B) can be measured in accordance with JIS K6253.
[0047] (Thermoplastic elastomer (b1)) The thermoplastic elastomer (B) may contain a thermoplastic elastomer (b1) having a polar group. The polar group may be, for example, a functional group containing one or more atoms selected from the group consisting of oxygen, sulfur, nitrogen, and halogen.Specific examples include a carboxyl group, a carboxylic anhydride group, a carboxylic ester group, a hydroxyl group, an epoxy group, an amide bond, a nitrile group, a cyano group, an amino group, an imide group, an isocyanate group, an acetyl group, a thiol group, an alkoxy group, a thioether group, a sulfone group, a phosphone group, a nitro group, a urethane bond, a methoxycarbonyl group, an acetoxy group, and a halogen atom.Among these, a carboxylic anhydride group, a carboxylic ester group, a hydroxyl group, an amide bond, a nitrile group, an amino group, a sulfone group, a urethane bond, and a halogen atom are preferred, and a carboxylic ester group, an amide bond, and a urethane bond are more preferred.
[0048] (Thermoplastic elastomer (b2)) The thermoplastic elastomer (B) may contain, for example, a thermoplastic elastomer (b2) containing one or more kinds selected from the group consisting of a thermoplastic polyurethane elastomer, a thermoplastic polyamide elastomer, and a thermoplastic polyester elastomer. The thermoplastic elastomer (b2) may have a polar group.
[0049] In addition, as the thermoplastic elastomer (b2), commercially available products may be used. Specific examples of the thermoplastic polyurethane elastomers include Elastollan manufactured by BASF, Vantex manufactured by DIC Covestro Polymer, and Fortimo manufactured by Mitsui Chemicals, Inc.; examples of the thermoplastic polyamide elastomers include Pebax manufactured by Arkema, UBESTA XPA manufactured by Ube Industries, Ltd., and Diamide manufactured by Polypla-Evonik, Inc.; and examples of the thermoplastic polyester elastomers include Pelprene manufactured by Toyobo, Hytrel manufactured by DuPont, and Arnitel manufactured by DSM, Inc.
[0050] (Thermoplastic elastomer (b3)) The thermoplastic elastomer (B) may include, for example, a thermoplastic elastomer (b3) (excluding the thermoplastic elastomers (b1) and (b2)) consisting of a propylene-α-olefin copolymer containing a propylene unit and an α-olefin unit having 2 or 4 to 20 carbon atoms.
[0051] Examples of α-olefins having 2 or 4 to 20 carbon atoms include ethylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, etc. Among these, from the viewpoint of imparting flexibility, α-olefins having 2 or 4 to 12 carbon atoms are preferred, and ethylene, 1-butene, 1-hexene, and 1-octene are more preferred. In the propylene-α-olefin copolymerization, a monomer having an unsaturated bond can be copolymerized as necessary. Examples of the monomer having an unsaturated bond include one or more selected from conjugated diolefins such as butadiene and isoprene, non-conjugated diolefins such as 1,4-hexadiene, cyclic diene compounds such as dicyclopentadiene and norbornene derivatives, and acetylenes.
[0052] (Thermoplastic elastomer (b4)) The thermoplastic elastomer (B) may further contain a thermoplastic elastomer (b4) consisting of one or more selected from the group consisting of a thermoplastic olefin-based elastomer (excluding the thermoplastic elastomers (b1) and (b3)), a thermoplastic styrene-based elastomer, and a compound thereof. The thermoplastic elastomer (b4) may be partially crosslinked. By using the thermoplastic elastomer (b4) in combination with one or more selected from the thermoplastic elastomers (b1) to (b3), flexibility can be easily obtained while maintaining good heat resistance. In particular, flexibility can be easily felt immediately after contacting the resin sheet of the present embodiment. The thermoplastic elastomer (b4) is preferably a compound of a thermoplastic olefin-based elastomer (excluding the thermoplastic elastomers (b1) and (b3)) and a thermoplastic styrene-based elastomer.
[0053] The content of the thermoplastic elastomer (B) is preferably 20 to 90 mass %, more preferably 30 to 85 mass %, and further preferably 40 to 80 mass %, based on the total amount of the resin composition, thereby making it possible to obtain a resin sheet having superior adhesiveness and heat resistance. The total amount of the thermoplastic elastomers (b1) to (b4) is preferably 60% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, based on the total amount of the thermoplastic elastomer (B), and may be 100% by mass. When the thermoplastic elastomer (b4) is used in combination with at least one of the thermoplastic elastomers (b1) to (b3), the content of the thermoplastic elastomer (b4) is preferably 5% by mass or more, more preferably 10% by mass or more, and from the viewpoint of further improving the adhesiveness at room temperature, preferably 25% by mass or more, more preferably 30% by mass or more. On the other hand, the content of the thermoplastic elastomer (b4) is preferably 60% by mass or less, more preferably 50% by mass or less, and from the viewpoint of further improving the heat resistance, preferably 30% by mass or less, based on the total amount of the thermoplastic elastomers (b1) to (b3).
[0054] The total content of the 4-methyl-1-pentene polymer (A) and the thermoplastic elastomer (B) is preferably 60% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and even more preferably 95% by mass or more, or may be 100% by mass, based on the total amount of the resin composition. This makes it possible to obtain a resin sheet having superior adhesion, flexibility, stress relaxation, and heat resistance.
[0055] The resin sheet according to this embodiment may further contain a compatibilizer (C).
[0056] [Compatibilizer (C)] The compatibilizer (C) is used to improve the compatibility and adhesion between the 4-methyl-1-pentene polymer (A) and the thermoplastic elastomer (B). That is, the compatibilizer (C) has a site that is compatible with each of the 4-methyl-1-pentene polymer (A) and the thermoplastic elastomer (B), and this allows the 4-methyl-1-pentene polymer (A) and the thermoplastic elastomer (B) to be finely dispersed more uniformly.
[0057] The compatibilizer (C) may be one or more selected from modified styrene-based thermoplastic elastomers, modified polyolefin-based thermoplastic elastomers, and the like.
[0058] Examples of the styrene-based thermoplastic elastomer include hydrogenated styrene-isoprene block copolymer (SEPS), hydrogenated styrene-butadiene block copolymer (SEBS), and hydrogenated styrene-isoprene-butadiene block copolymer (SEEPS). The styrene thermoplastic elastomer preferably has a styrene content of 40% by mass or less, and more preferably from 15 to 35% by mass.
[0059] The polyolefin thermoplastic elastomer may be a propylene copolymer having a Shore A hardness in the range of 30 to 80. As a commercially available product of such a propylene copolymer, for example, Vistamaxx 6202 manufactured by ExxonMobil Chemical Corporation may be suitably used.
[0060] The modified material may be obtained by chemical modification through a graft reaction of an unsaturated carboxylic acid or a derivative thereof. Examples of the unsaturated carboxylic acid or its derivative to be grafted include unsaturated carboxylic acids such as maleic acid, fumaric acid, tetrahydrophthalic acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid, nadic acid, acrylic acid, and methacrylic acid, as well as derivatives thereof, such as the acid anhydrides, imides, amides, and esters of the unsaturated carboxylic acids. Commercially available products may be used as the modified products, and specifically, preferred modified products of styrene-based thermoplastic elastomers include Tuftec M1943 (maleic anhydride graft modified SEBS) manufactured by Asahi Kasei Corporation and Tuftec MP10 (amine modified SEBS) manufactured by Asahi Kasei Corporation.
[0061] The content of the compatibilizer (C) is preferably 5 to 20 mass %, more preferably 7 to 15 mass %, and further preferably 10 to 12 mass %, based on the total amount of the resin composition.
[0062] In the present embodiment, when the compatibilizer (C) is used, the content of the 4-methyl-1-pentene polymer (A) is preferably 40 to 75 mass% relative to the total amount of the resin composition, the content of the thermoplastic elastomer (B) is preferably 20 to 60 mass% relative to the total amount of the resin composition, and the content of the compatibilizer (C) is preferably 5 to 20 mass% relative to the total amount of the resin composition. More preferably, the content of the 4-methyl-1-pentene polymer (A) is 40 to 55 mass% relative to the total amount of the resin composition, the content of the thermoplastic elastomer (B) is 40 to 60 mass% relative to the total amount of the resin composition, and the content of the compatibilizer (C) is preferably 5 to 15 mass% relative to the total amount of the resin composition.
[0063] The combination of the 4-methyl-1-pentene polymer (A), the thermoplastic elastomer (b1), and the compatibilizer (C) can further improve the compatibility, and is more preferable from the viewpoint of improving the adhesiveness.
[0064] [Other ingredients] The resin sheet according to the present embodiment may contain components other than the 4-methyl-1-pentene polymer (A), the thermoplastic elastomer (B), and the compatibilizer (C) as necessary, within a range that does not impair the effects of the present invention. The resin sheet according to this embodiment may contain additives such as foaming agents, foaming modifiers, heat stabilizers, antioxidants, UV absorbers, pigments, antistatic agents, copper damage inhibitors, flame retardants, neutralizing agents, plasticizers, nucleating agents, weather stabilizers, light stabilizers, anti-aging agents, fatty acid metal salts, softeners, dispersants, colorants, lubricants, natural oils, synthetic oils, and waxes.
[0065] The foaming agent includes chemical foaming agents and physical foaming agents. Examples of chemical foaming agents include sodium bicarbonate, ammonium bicarbonate, various carboxylates, sodium borohydride, azodicarboxamide, N,N-dinitrosopentamethylenetetramine, P,P-oxybis(benzenesulfonyl hydrazide), azobisisobutyronitrile, paratoluenesulfonyl hydrazide, and sodium hydrogen carbonate. The physical foaming agent may be carbon dioxide, nitrogen, or a mixture of carbon dioxide and nitrogen, any of which may be supplied in a gaseous, liquid or supercritical state.
[0066] The foaming modifier may be one or more selected from low density polyethylene, medium density polyethylene, high density polyethylene, high pressure low density polyethylene, polypropylene, poly-1-butene, poly-4-methyl-1-pentene, poly-3-methyl-1-butene, ethylene-α-olefin copolymer, propylene-α-olefin copolymer, and 1-butene-α-olefin copolymer.
[0067] [Manufacturing method of resin sheet] The resin sheet of this embodiment can be produced by mixing or melt-kneading the raw materials 4-methyl-1-pentene polymer (A), thermoplastic elastomer (B) having a melting point of 130 to 180°C, and other optional components by a known method such as dry blending, a tumbler mixer, a Banbury mixer, a single-screw extruder, a twin-screw extruder, a high-speed twin-screw extruder, or a heat roll to prepare a resin composition, and extruding the resin composition into a sheet by a known method. The extruded sheet is cooled by a cooling roll and taken up by a take-up machine.
[0068] Examples of the method for foaming the resin sheet include the following methods. When a chemical foaming agent is used, a resin composition other than the chemical foaming agent is charged into an extruder together with the chemical foaming agent, and the mixture is mixed uniformly, and then foamed while being extruded into a sheet. In addition, when carbon dioxide is used as a physical foaming agent, a method can be mentioned in which the resin composition is charged into an extrusion molding machine, kneaded in the extrusion molding machine, and after the resin composition is plasticized, carbon dioxide is directly injected into the extrusion molding machine to foam the resin composition while extruding it into a sheet.
[0069] <Fabric laminate> The fabric laminate of this embodiment is a resin sheet composed of a resin composition containing a 4-methyl-1-pentene polymer (A) and a thermoplastic elastomer (B) having a melting point of 130 to 180°C, the 4-methyl-1-pentene polymer (A) containing a structural unit (a1) derived from 4-methyl-1-pentene and a structural unit (a2) derived from a linear α-olefin having 2 to 3 carbon atoms, and a fabric is bonded to at least one surface of the resin sheet having an adhesive strength measured by the above procedure of 4 N / 25 mm or more and 30 N / 25 mm or less. This makes it possible to realize a fabric laminate that makes use of the flexibility and texture of the fabric while obtaining new functions such as flexibility and stress relaxation properties of the resin sheet of this embodiment.
[0070] The fabric is a material obtained by processing fibers such as natural fibers, synthetic fibers, and chemical fibers into thin pieces, and examples of the fabric include woven fabrics such as woven cloth, nonwoven fabrics, etc. Specific examples of the fabric include knitted fabrics having weft knitting structures such as plain knit, milling, smooth, and double knit, knitted fabrics having warp knitting structures such as tricot and raschel, and woven fabrics having structures such as plain weave, twill, and satin.
[0071] From the viewpoints of adhesion to the resin sheet and maintaining the properties of the resin sheet, the thickness of the material is preferably 0.2 to 1.0 mm, more preferably 0.2 to 0.8 mm, and even more preferably 0.2 to 0.6 mm.
[0072] The basis weight of the fabric is not particularly limited from the viewpoint of adhesiveness and heat resistance, but is preferably 75 to 300 g / m2 from the viewpoint of handling, etc. 2 It is preferable that the thickness is 90 to 250 g / m 2 More preferably, the thickness is 100 to 200 g / m 2 It is even more preferable that:
[0073] In addition, the fabric preferably has elasticity. Specifically, the fabric preferably has a maximum elongation of 10 to 300% in the direction of maximum elasticity.
[0074] Fabric materials include natural fibers such as cotton, linen, wool, and silk; regenerated fibers such as rayon and cupra; semi-synthetic fibers such as acetate and triacetate; synthetic fibers such as nylon, polyester, polyurethane, acrylic, and rayon; and chemical fiber products made from blends of these synthetic fibers. Of these, synthetic fibers are preferred, and one or more types selected from nylon, polyester, polyurethane, acrylic, and rayon are more preferred.
[0075] The fabric laminate may be a resin sheet having fabrics laminated on both sides thereof. In this case, the fabric on one side of the resin sheet and the fabric on the other side of the resin sheet may be made of the same material or different materials.
[0076] Furthermore, the fabric laminate of this embodiment may have at least a partially curved surface, and the radius of curvature of the curved surface may be in the range of 50 mm to 150 mm. This allows the fabric laminate of this embodiment to easily conform to a curved surface. Examples of curved surfaces include rounded parts of the human body, such as the head, chest, elbows, and knees. Examples of clothing to be worn on curved surfaces include hats, hoods, brassieres, underwear, and supports.
[0077] The thickness of the fabric laminate of this embodiment is appropriately adjusted taking into consideration flexibility, processability, ease of sewing, and the like.
[0078] [Method of manufacturing fabric laminate] The method of manufacturing the fabric laminate includes the following steps. (Step) A fabric is laid on at least one surface of the resin sheet, and heat-sealed under conditions of 140° C. to 190° C. and 0.1 MPa to 2.0 MPa to obtain a fabric laminate. This makes it possible to obtain a fabric laminate while maintaining the properties of the resin sheet of this embodiment.
[0079] A pressurizing time of 1 second to 10 minutes provides good production efficiency. In addition, when performing thermal bonding, it is important to consider the factors of temperature, pressure, and time, and as a thermal bonding method that realizes this, for example, a heat press method can be used. Furthermore, it is more preferable to use a method in which the fabric and the resin sheet are thermally bonded continuously using an interlining bonding press machine. Examples of commercially available products of such thermal bonding press machines include a flat plate press manufactured by Hashima Co., Ltd. and a linear interlining bonding press device.
[0080] The resin sheet of the present embodiment can provide good adhesion and heat resistance regardless of the stretch direction and other characteristics of the fabric, regardless of the direction in which the sheet is adhered to the fabric.
[0081] <Application> The resin sheet and fabric laminate according to the present embodiment are widely used regardless of the field. For example, mobility products such as automobile parts, railway parts, aircraft parts, ship parts, bicycle parts, etc.; electronic devices; household electrical appliances; audio equipment; camera equipment; precision equipment; game equipment; VR equipment; civil engineering and construction products such as civil engineering parts, building parts, and building materials; household goods such as furniture and bedding; daily necessities such as kitchen utensils, toiletries, and stationery; leisure products such as outdoor products and backpacks; agricultural products such as gardening; apparel products (clothes, underwear, and undergarments (for example, bras, shoulder pads, and corrective underwear)). It can be used for: core materials for clothing (such as clothing core materials, hats, belts, linings for school bags, business card holders, glasses, etc.), footwear supplies (various insoles, shoe lining materials, various equipment, shoes, shoelaces, etc.), decorative products such as accessories and small portable miscellaneous items; medical supplies, health care supplies, etc.; sports supplies such as sporting goods; education and toy supplies such as books and toys; packaging supplies, etc.; cosmetic supplies such as face washes and makeup supplies; lighting supplies such as LED lighting; aquaculture supplies such as fisheries supplies; safety supplies such as child seats; music supplies; pet supplies; fishing supplies, etc.
[0082] In particular, the resin sheet and the fabric laminate are preferably used as clothing, clothing materials, and clothing components. In this case, in order to exhibit the good feel that is peculiar to the resin sheet using the 4-methyl-1-pentene polymer (A), it is preferable that the surface on the resin sheet side is configured to directly contact human skin. The clothing material is more preferably used for general clothing, underwear, undergarments, hats, shoes, and other fabric-based items. The clothing material is intended to be a part of such clothing items, such as underwear innerwear and shoe insoles. In particular, it is suitable for use as a member to be worn on rounded parts of the human body, such as a hat, a hood, a brassiere, underwear, a supporter, etc. When the resin sheet and fabric laminate are applied to clothing, the resin sheet and fabric laminate can appropriately follow the movements and shape of a person's body, and have good strength against tension and the like.
[0083] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above may also be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. EXAMPLES
[0084] The present embodiment will be described in detail below with reference to examples and comparative examples, but the present embodiment is not limited to the descriptions of these examples.
[0085] (1)Measurement method Composition of 4-methyl-1-pentene polymer (A) The contents of 4-methyl-1-pentene and α-olefin in 4-methyl-1-pentene polymers are 13 Quantitative analysis was performed using C-NMR.
[0086] (2) Raw materials [4-Methyl-1-pentene polymer (A)] Copolymer of 4-methyl-1-pentene and propylene (content of 4-methyl-1-pentene-derived structural units (a1): 72 mol%, content of propylene-derived structural units (a2): 28 mol%) Glass transition temperature: 30°C, intrinsic viscosity [η] in decalin at 135°C: 1.5 dL / g, MFR: 10 g / 10 min
[0087] [Thermoplastic elastomer (B)] Thermoplastic elastomer (B)-1: "Hybra 7311F" hydrogenated styrene-based thermoplastic elastomer (SEEPS), manufactured by Kuraray Co., Ltd., no polar groups, no melting point, Shore A hardness 41 (Thermoplastic elastomer (b1) or (b2)) Thermoplastic elastomer (B)-2: "Pelprene P-30B" Thermoplastic polyester elastomer (TPEE), manufactured by Toyobo Co., Ltd., polar bond = ester bond, melting point 160°C, Shore A hardness 71 Thermoplastic elastomer (B)-3: "Fortimo XET-T1085" Thermoplastic polyurethane elastomer (TPU), manufactured by Mitsui Chemicals, polar bond = urethane bond, melting point 149°C, Shore A hardness 85 Thermoplastic elastomer (B)-4: "Pebax 2533" Thermoplastic polyether block amide copolymer (TPAE), manufactured by Arkema, polar bond = amide bond, melting point 134°C, Shore A hardness 75 (Thermoplastic elastomer (b3)) Thermoplastic elastomer (B)-5: Propylene-ethylene copolymer synthesized in Synthesis Example 1 below, 1-butene unit (19.0 mol / %), ethylene unit (13.0 mol%), propylene unit (68.0 mol%), melting point 160°C, Shore A hardness 72 (Thermoplastic elastomer (b4)) Thermoplastic elastomer (B)-6: "Milastomer 5020NS" partially crosslinked thermoplastic elastomer, manufactured by Mitsui Chemicals, no polar group, melting point 160°C, Shore A hardness 53 Thermoplastic elastomer (B)-7: "Arneston JH28NS" mineral oil-containing styrene-based elastomer compound, manufactured by Kuraray Plastics, no polar groups, no melting point, Shore A hardness 30
[0088] <Synthesis Example 1> Synthesis of Thermoplastic Elastomer (B)-5 A 2000 ml polymerization reactor that had been thoroughly purged with nitrogen was charged with 917 ml of dry hexane, 85 g of 1-butene, and triisobutylaluminum (1.0 mmol) at room temperature, and the temperature inside the polymerization reactor was then raised to 65° C. The pressure inside the system was increased to 0.77 MPa with propylene, and then the pressure inside the system was adjusted to 0.78 MPa with ethylene. Next, dimethylmethylene (3-tert-butyl-5-methylcyclopentadienyl) fluorenyl zirconium dichloride and a toluene solution of methylaluminoxane (manufactured by Tosoh Finechem Co., Ltd.) were mixed to prepare a toluene solution containing aluminum atoms and zirconium atoms in a ratio of aluminum atoms / zirconium atoms = 300 / 1 (molar ratio), and then an amount of the toluene solution containing 0.002 mmol of zirconium atoms (hence, an amount containing 0.6 mmol of aluminum atoms) was taken and added to a polymerization vessel, and polymerization was carried out for 20 minutes while maintaining the internal temperature at 65 ° C and the internal pressure at 0.78 MPa with ethylene, and the polymerization was terminated by adding 20 ml of methanol. After depressurization, the polymer was precipitated from the polymerization solution in 2 L of methanol and dried under vacuum at 130 ° C for 12 hours to obtain 60.4 g of a powdery copolymer. Next, the above process was scaled up and carried out to obtain a sufficient amount of copolymer. The obtained copolymer was mixed with 500 ppm of antioxidant Irganox 1076 and 500 ppm of Irgafos 168, extruded at a cylinder temperature of 210°C using a single-screw extruder, and the molten strand discharged from the round hole die was cooled and solidified in a water bath, and then cut with a strand cutter to obtain pellets. The pellets were used as thermoplastic elastomer (B)-5.
[0089] [Compatibilizer (C)] Compatibilizer (C): Amine-modified SEBS "Tuftec MP10" manufactured by Asahi Kasei Corporation, styrene content 30%
[0090] [others] Inorganic foaming agent: Polythrene "EE275F" manufactured by Eiwa Chemical Industry Co., Ltd.
[0091] [material] Fabric x: Thickness: 0.28mm, Weight: 100g / m 2 Material: 89% polyester, 11% polyurethane Fabric thickness: 0.42mm, weight: 160g / m 2 Material: 39% polyester, 32% acrylic, 21% rayon, 8% polyurethane Fabric thickness: 0.50mm, weight: 190g / m 2 Material: 52% cotton, 41% acrylic, 7% polyurethane
[0092] (3) Preparation of resin sheet <Examples 1 to 4> The molding machine used was a device equipped with a single-screw extruder (cylinder inner diameter D: 20 mm, full-flight screw, L / D: 28 mm when L is the effective screw length), a T-die (die width: 300 mm, lip opening: 0.4 to 1.0 mm), a cooling roll (outer diameter 200 mm, made of steel with mirror-finished hard chrome plating surface treatment, water-cooled), and a take-up machine. First, the raw materials were dry blended in the ratio shown in Table 1 (the units in the table are parts by weight), and the resulting mixture was placed in a hopper. The raw material components were melted and kneaded under conditions of a temperature of 160-230°C in each part of the cylinder and a screw rotation speed of 60-100 rpm, and extruded from a T-die to give an extrusion rate of 1.5-3.5 kg / hr. The extruded sheet-like mixture was cooled with a cooling roll (water passing through the roll interior temperature: 20°C) and taken up using a take-up machine (take-up speed: 0.4-0.6 m / min) to obtain a resin sheet (non-foamed sheet) with a sheet width of approximately 270 mm and a thickness of 0.5 mm.
[0093] <Examples 5 to 7> An apparatus equipped with a twin-screw extruder (cylinder inner diameter D: 30 mm, kneading screw), a strand die (die hole: 4 mm, number of holes: 2), a main raw material feeder (type: waving feeder), a cooling method (water bath cooling), and a pelletizer was used. First, the raw materials were dry-blended in the ratio shown in Table 1 (the units in the table are parts by mass), and the obtained dry blend was fed into a feeder. The raw material components were melted and kneaded under conditions of a temperature of 140-200°C in each part of the cylinder and a screw rotation speed of 60-90 rpm, and pelletized to an extrusion rate of 6.0-11.0 kg / hr. Next, in order to mold a resin sheet, a single screw extruder equipped with the same T-die, cooling roll, and take-off machine as those used in Examples 1 to 4 above was used. The pellets obtained from the twin-screw extruder were fed into the hopper of the single-screw extruder. The individual raw material components were melted and kneaded under conditions of a temperature of 160-230°C in each part of the cylinder of the single-screw extruder and a screw rotation speed of 60-100 rpm, and extruded from a T-die to give an extrusion rate of 1.5-3.5 kg / hr. The extruded sheet-like mixture was cooled with a cooling roll (water passing through the roll interior temperature: 20°C) and taken up using a take-up machine (take-up speed: 0.4-0.6 m / min) to obtain a resin sheet (non-foamed sheet) with a sheet width of approximately 270 mm and a thickness of 0.5 mm.
[0094] <Examples 8, 9, 13 to 16> Using the same single-screw extruder equipped with a T-die, cooling roll, and take-off machine as used in Examples 1 to 4, the raw materials were dry-blended according to the composition shown in Table 1 (the units in the table are parts by mass), and the resulting mixture was charged into the hopper of the single-screw extruder. The raw materials were melted and kneaded under conditions of a temperature of 150 to 240°C in each part of the cylinder and a screw rotation speed of 60 to 80 rpm, and extruded from the T-die to an extrusion rate of 2.0 to 2.5 kg / hr. The extruded sheet-like mixture was cooled with a cooling roll (water passing temperature inside the roll: 20°C) and taken up using a take-off machine (take-off speed: 0.4 to 0.6 m / min) to obtain a resin sheet (foamed sheet) with a sheet width of about 270 mm and a thickness of 0.5 mm.
[0095] <Examples 10 to 12> The inorganic foaming agents shown in Table 1 were also dry-blended, and the resulting mixture was placed in the hopper of a single-screw extruder equipped with the same T-die, cooling roll, and take-off machine as those used in Examples 1 to 4. The individual components were melted and kneaded under conditions of a temperature of 140 to 220°C in each part of the cylinder of the single-screw extruder and a screw rotation speed of 60 to 80 rpm, and extruded from the T-die to an extrusion rate of 1.5 to 2.5 kg / hr. The extruded sheet-like mixture was cooled with a cooling roll (water passing through the roll at 20°C) and taken up using a take-off machine (take-off speed 0.4 to 0.6 m / min) to obtain a resin sheet (foamed sheet) with a sheet width of approximately 270 mm and a thickness of 0.5 mm.
[0096] <Comparative Examples 1 and 2> Using the raw materials in the compositions shown in Table 1 (the units in the table are parts by mass), a resin sheet having a sheet width of about 270 mm and a thickness of 0.5 mm was obtained under the same conditions as in Example 1.
[0097] (4) Measurement of physical properties The following measurements were carried out using each of the resin sheets obtained in (3) above. The results are shown in Table 1.
[0098] [Solid Viscoelasticity] The obtained resin sheet was cut into a rectangular shape (length 30 mm × width 10 mm) to prepare a test piece. Next, the temperature dependence of dynamic viscoelasticity was measured for the obtained test piece in the temperature range of -60°C to 200°C using a TA Instruments RSA-III under the conditions of a chuck distance of 20 mm, a frequency of 1.59 Hz, a strain amount of 0.1%, a heating rate of 4°C / min, and a tensile mode. The loss tangent (tan δ) value at 30°C and the storage modulus E' (MPa) value at 100°C were obtained.
[0099] [Adhesive strength] First, the resin sheet and the fabric x (thickness: 0.28 mm, basis weight: 100 g / m 2, material; polyester 89% by mass, polyurethane 11% by mass) were stacked in the order of fabric x / resin sheet / fabric x so that the MD direction of the resin sheet was parallel to the direction in which fabric x had the greatest elasticity, and a heat seal tester (Tester Sangyo Co., Ltd., thermal gradient heat seal tester, model number TP-701-G) was used to heat seal the area to be heat sealed to a rectangle of 10 mm in the MD direction of the resin sheet and 50 mm in the TD direction of the resin sheet under conditions of a pressure of 0.1 MPa, a time of 10 seconds, and a temperature of 190 ° C. on both the upper and lower heat seal bars of the heat seal tester, to obtain a laminate. As a test piece for measuring adhesive strength, the laminate was cut to a test piece width of 25 mm so that the MD direction of the resin sheet of the laminate was the length direction of the test piece, and a test piece was obtained. The adhesive strength [N / 25mm] of the test piece was measured when the resin sheet was peeled from the fabric x on the side that had been in contact with the upper heat seal bar of the heat seal tester at an environmental temperature of (i) 23°C, (ii) 100°C, a tensile speed of 300mm / min, a peel angle of 180°, and a peel direction in the MD direction of the test piece. Furthermore, the adhesive strength was measured in the same manner when fabric y or fabric z was used instead of fabric x. (conditions) Test piece shape: Strip shape, width 25mm (common) Test piece direction: Resin sheet: MD direction, Fabric: Direction with greatest elasticity (common) Distance between chucks: 30mm (common) Tensile testing machine: Tensilon universal testing machine with thermostatic chamber Tensile speed: 300 mm / min (common) Test temperature: (i) 23°C, (ii) 100°C (held for 10 minutes after reaching the set temperature) Number of measurements: n=1
[0100] [Surface hardness measurement] Using the obtained resin sheet, a test piece was prepared under the following conditions, and the Shore A hardness was measured. Test standard: JIS K6253 Test temperature: 23℃ Thickness of specimen: 7mm Equipment: Shore A hardness tester A number of sheets were stacked together to form a test piece with a total thickness of 7 mm. Using the test piece, the Shore A hardness tester was used to read the value immediately after the indenter started to contact (HS0) and the value 15 seconds after the indenter started to contact (HS1). Furthermore, the change in Shore A hardness, ΔHS, defined by the following formula (1), was calculated. ΔHS = (HS0) - (HS1) (1)
[0101] [density] According to ASTM D 1505 (underwater displacement method), the density (g / cm) of each resin sheet was calculated from the mass measured in water and air using an ALFA MIRAGE electronic specific gravity meter MD-300S. 3 ) was calculated.
[0102] [Melt flow rate (MFR)] The melt flow rate (MFR) of the resin sheet was measured at 230° C. under a load of 2.16 kg in accordance with ASTM D1238.
[0103] (5) Evaluation The resin sheets obtained in (3) above were subjected to the following evaluations. The results are shown in Table 1.
[0104] [Heat resistance (heat deflection test)] A test piece was cut out from the resin sheet so that the size was 50 mm wide and 340 mm long, and the longitudinal direction of the test piece was the MD direction. The obtained test piece was bridged from one side to the other side of the edge of a stainless steel container (inner size: depth 86 mm, width 320 mm, length 320 mm, square type) so that the test piece would not loosen under its own weight, and the edge of the container and the 10 mm long parts from each end of both ends of the test piece were fixed using heat-resistant adhesive tape. Next, the container with the test piece fixed was placed in a hot air circulation dryer (ISUZU Soyokaze) at 100 ° C for 15 minutes to be heat-treated. Thereafter, the container with the test piece fixed was taken out of the dryer and left at room temperature for 1 hour, and the thermal deflection of the test piece was evaluated as follows. The vertical distance from the center of the test piece (a point 160 mm from the edge of the container) to the bottom of the container was defined as D0 (mm) immediately before heat treatment at 100°C for 15 minutes, and D1 immediately after leaving the test piece at room temperature for 1 hour after the specified heat treatment. D0 (mm) and D1 (mm) were measured and the amount of thermal deflection ΔD (mm) was calculated using the following formula (2). ΔD = D0 - D1 (2) The smaller the thermal deflection amount ΔD (mm), the better the heat resistance of the resin sheet.
[0105] In addition, each resin sheet of the embodiment and the fabric x were overlapped so that the MD direction of the resin sheet was parallel to the direction in which the elasticity of the fabric x was greatest, and heat-sealed under conditions of a pressure of 0.1 MPa, a time of 10 seconds, and a temperature of 190°C to obtain a fabric laminate, and then the appearance, adhesion, and feel were verified. As a result, the feel and color of the fabric were maintained, and no separation was observed at the interface between the fabric and the resin sheet, and the fabric was well bonded. In addition, even when the fabric laminate was washed or dried, or a load such as tension was applied, the fabric and the resin sheet were well bonded without peeling. Furthermore, immediately after pulling with one hand, when the fabric laminate was pulled and held with one hand, there was a feeling that the tension was decreasing over time, and stress relaxation was maintained. On the other hand, in the laminate using the resin sheet of the comparative example, separation or the like was observed at the interface between the fabric and the resin sheet in some cases.
[0106] [Table 1]
Claims
1. A resin sheet made of a resin composition containing a 4-methyl-1-pentene polymer (A) and a thermoplastic elastomer (B) having a melting point of 130 to 180°C, the 4-methyl-1-pentene polymer (A) contains a structural unit (a1) derived from 4-methyl-1-pentene and a structural unit (a2) derived from a linear α-olefin having 2 to 3 carbon atoms, A resin sheet having a storage modulus E' of 0.55 MPa or more and 7.0 MPa or less at 100°C when dynamic viscoelasticity is measured under conditions of a frequency of 1.59 Hz, a strain of 0.1%, a temperature rise rate of 4°C / min, and a tensile mode in a temperature range of -60°C to 200°C.
2. A resin sheet made of a resin composition containing a 4-methyl-1-pentene polymer (A) and a thermoplastic elastomer (B) having a melting point of 130 to 180°C, the 4-methyl-1-pentene polymer (A) contains a structural unit (a1) derived from 4-methyl-1-pentene and a structural unit (a2) derived from a linear α-olefin having 2 to 3 carbon atoms, A resin sheet having an adhesive strength of 4 N / 25 mm or more and 30 N / 25 mm or less, as measured by the following procedure. [procedure] First, the resin sheet and the fabric x (thickness: 0.28 mm, basis weight: 100 g / m 2 (Material: 89% polyester, 11% polyurethane) are layered so that the MD direction of the resin sheet is parallel to the direction in which the fabric x has the greatest elasticity, and are bonded under conditions of a pressure of 0.1 MPa, a time of 10 seconds, and a temperature of 190° C. to produce a laminate. The MD direction of the resin sheet of the laminate is the length direction, and the laminate is cut to a width of 25 mm to obtain a test piece. Next, the adhesive strength [N / 25 mm] of the test piece is measured when the resin sheet is peeled off from the fabric x using a tensile testing machine equipped with a thermostatic chamber at a test temperature of 100°C, a tensile speed of 300 mm / min, a peel angle of 180°, and a peel direction in the MD direction.
3. 3. The resin sheet according to claim 1 or 2, wherein the Shore A hardness of at least one surface of the resin sheet immediately after measurement, measured at 23 ° C. in accordance with JIS K6253, is HS0, and the Shore A hardness is HS0 of 30 or more and 90 or less.
4. 3. The resin sheet according to claim 1 or 2, wherein the Shore A hardness of at least one surface of the resin sheet immediately after measurement at 23 ° C. in accordance with JIS K6253 is HS0 and the Shore A hardness 15 seconds after measurement is HS1, ΔHS represented by (HS0-HS1) is 3 or more and 30 or less.
5. The resin sheet according to claim 1 or 2, wherein the resin sheet has a thickness of 0.1 mm or more and 3 mm or less.
6. The density of the resin sheet is 0.30 g / cm 3 Above, 1.5g / cm 3 The resin sheet according to claim 1 or 2, wherein:
7. The resin sheet according to claim 1 or 2, wherein the thermoplastic elastomer (B) has a Shore A hardness of 30 or more and 90 or less.
8. The thermoplastic elastomer (B) includes a thermoplastic elastomer (b1) having a functional group containing one or more atoms selected from the group consisting of oxygen, sulfur, nitrogen, and halogen. The resin sheet according to claim 1 or 2.
9. 3. The resin sheet according to claim 1, wherein the thermoplastic elastomer (B) comprises one or more thermoplastic elastomers (b2) selected from a thermoplastic polyamide-based elastomer, a thermoplastic polyurethane-based elastomer, and a thermoplastic polyester-based elastomer.
10. The resin sheet according to claim 8 , wherein the resin composition further comprises a compatibilizer (C).
11. The resin sheet according to claim 10, wherein the compatibilizer (C) comprises a modified styrene-based thermoplastic elastomer or a modified polyolefin-based thermoplastic elastomer.
12. The content of the 4-methyl-1-pentene polymer (A) is 20 to 60% by mass based on the total amount of the resin composition, The content of the thermoplastic elastomer (B) is 20 to 80% by mass based on the total amount of the resin composition, The resin sheet according to claim 10, wherein the content of the compatibilizer (C) is 5 to 20 mass% with respect to the total amount of the resin composition.
13. The resin sheet according to claim 1 or 2, wherein the thermoplastic elastomer (B) comprises a thermoplastic elastomer (b3) consisting of a propylene-α-olefin copolymer containing a propylene unit and an α-olefin unit having 2 or 4 to 20 carbon atoms.
14. The thermoplastic elastomer (B) comprises a thermoplastic elastomer (b4) consisting of one or more selected from a thermoplastic olefin-based elastomer, a thermoplastic styrene-based elastomer, and a compound thereof. The resin sheet according to claim 1 or 2.
15. The resin sheet according to claim 1 or 2, which is used as a material for clothing.
16. A fabric laminate comprising the resin sheet according to claim 1 or 2 and a fabric laminated to at least one surface of the resin sheet.
17. The fabric has a basis weight of 75 g / m 2 Up to 300 g / m 2 17. The fabric laminate of claim 16,
18. The fabric laminate according to claim 16, wherein at least a portion of the fabric laminate has a curved surface, and the radius of curvature of the curved surface is in the range of 50 mm to 150 mm.
19. A garment comprising the fabric laminate according to claim 16.
20. The article of clothing according to claim 19 , wherein the surface of the resin sheet is configured to be in contact with a human body.
21. A method for producing a fabric laminate, comprising the steps of overlapping a fabric on at least one surface of the resin sheet according to claim 1 or 2, and heat-sealing the fabric laminate under conditions of 140°C to 190°C and 0.1 MPa to 2.0 MPa.
Citation Information
Patent Citations
Foam body, polyolefin-based foam sheet and complex
WO2018143411A1