Resin composition, resin sheet, laminate, sheet cured product and circuit board material

A resin composition with thermoplastic resins, maleimide compounds, and polymerizable compounds addresses thermal expansion issues in circuit boards, achieving low dielectric and thermal expansion balances for improved electronic device performance.

JP2024146842APending Publication Date: 2024-10-15MITSUBISHI CHEM CORP

Patent Information

Application Number
JP2024049795
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-26
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Circuit board materials face issues with curling or warping due to large differences in linear thermal expansion coefficients between resin layers and conductors, especially in multi-layered electronic devices, necessitating a balance between low dielectric properties and low thermal expansion.

Method used

A resin composition comprising thermoplastic resins like styrene thermoplastic elastomers, maleimide compounds, and radically polymerizable compounds is formulated, with specific ratios and additives to achieve a crosslinked structure that reduces thermal expansion and maintains low dielectric properties.

Benefits of technology

The resulting cured sheets and circuit board materials exhibit an excellent balance of low dielectric properties and low thermal expansion coefficients, improving signal transmission efficiency and reducing warping and curling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146842000001
    Figure 2024146842000001
  • Figure 2024146842000002
    Figure 2024146842000002
  • Figure 2024146842000003
    Figure 2024146842000003
Patent Text Reader

Abstract

To provide a sheet cured material and a circuit board materials having excellent balance between low dielectric properties and low coefficient of linear thermal expansion and to provide a resin composition, a resin sheet and a laminate capable of producing the sheet cured material and the circuit board material having excellent balance between low dielectric properties and low coefficient of linear thermal expansion.SOLUTION: There is provided a resin composition which comprises at least one thermoplastic resin (A1) selected from the group consisting of a styrene-based thermoplastic elastomer, an olefin-based thermoplastic elastomer and an ethylene-based polymer, a maleimide compound (B) having one or more N-substituted maleimide groups in the molecule and a radical polymerizable compound (C) having two or more ethylenically unsaturated bonds in the molecule, wherein when the total amount of the thermoplastic resin (A1), the maleimide compound (B) and the radical polymerizable compound (C) is defined as 100 mass%, the content of the maleimide compound (B) is 1 mass% or more and less than 30 mass%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition, a resin sheet, a laminate, a cured sheet, and a circuit board material. [Background technology]

[0002] In recent years, as electrical and electronic devices have become more powerful and functional, communication frequencies have become higher in order to improve communication speeds and the amount of information transmitted. When a digital signal is transmitted through a circuit board, a portion of the transmitted digital signal is converted into heat within the circuit board, resulting in transmission loss. Since the amount of transmission loss is expressed as the product of the dielectric constant and the dielectric loss tangent, a material with a low dielectric constant and dielectric loss tangent, i.e., a component with low dielectric properties, is required to achieve low-loss communication. Since transmission signals in the high-frequency range in particular are more easily converted into heat, materials with even lower dielectric properties are in demand.

[0003] Known examples of materials having low dielectric properties include polyphenylene ether resin compositions containing an epoxy compound and a cyanate compound (see, for example, Patent Document 1), thermosetting resins such as maleimide resins (see, for example, Patent Document 2), and thermoplastic resins such as cyclic olefin resin compositions (see, for example, Patent Document 3). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2010-059363 A [Patent Document 2] JP 2012-255059 A [Patent Document 3] International Publication No. 2006 / 095511 Summary of the Invention [Problem to be solved by the invention]

[0005] When a circuit board material is produced by laminating a low dielectric resin and a conductor as in the above Patent Documents 1 to 3, if the difference in linear thermal expansion coefficient between the resin layer and the conductor is large, curling or warping may occur after lamination. In recent years, as electric and electronic devices have become smaller and more multi-layered, there is a demand to reduce the linear thermal expansion coefficient of the resin layer to improve curling and warping of the laminate.

[0006] Therefore, an object of the present invention is to provide a sheet cured product and a circuit board material having an excellent balance between low dielectric properties and a low linear thermal expansion coefficient, as well as a resin composition, a resin sheet, and a laminate capable of producing the sheet cured product and the circuit board material having an excellent balance between low dielectric properties and a low linear thermal expansion coefficient. [Means for solving the problem]

[0007] As a result of extensive investigations aimed at solving the above problems, the present inventors have found that the above problems can be solved by adding a specific compound to a thermoplastic resin.

[0008] The gist of the present invention is as follows. [1] A thermoplastic resin composition comprising at least one thermoplastic resin (A1) selected from the group consisting of a styrene-based thermoplastic elastomer, an olefin-based thermoplastic elastomer, and an ethylene-based polymer, a maleimide compound (B) having one or more N-substituted maleimide groups in the molecule, and a radical polymerizable compound (C) having two or more ethylenically unsaturated bonds in the molecule, a resin composition in which the content of the maleimide compound (B) is 1% by mass or more and less than 30% by mass when the total amount of the thermoplastic resin (A1), the maleimide compound (B), and the radical polymerizable compound (C) is 100% by mass. [2] The resin composition according to the above [1], wherein the thermoplastic resin (A1) comprises a styrene-based thermoplastic elastomer. [3] The resin composition according to [2] above, wherein the styrene content of the styrene-based thermoplastic elastomer is 10% by mass or more and 70% by mass or less. [4] The resin composition according to any one of the above [1] to [3], wherein the radical polymerizable compound (C) is at least one selected from the group consisting of a bifunctional aromatic vinyl compound and a trialkenyl isocyanurate compound. [5] The resin composition according to any one of the above [1] to [4], wherein the mass ratio of the maleimide compound (B) to the radically polymerizable compound (C) is (B):(C)=1:0.5 to 1:10. [6] The resin composition according to any one of the above [1] to [5], which contains a cyclic polyolefin resin copolymer (A2). [7] The resin composition according to [6], wherein the cyclic polyolefin resin copolymer (A2) is a copolymer having an alicyclic structure in a polyolefin side chain. [8] A resin sheet comprising the resin composition according to any one of the above [1] to [7]. [9] A laminate comprising the resin sheet according to [8] above, and a release film on one or both sides of the sheet.

[10] A sheet cured product obtained by curing the resin sheet described in [8] above.

[11] A circuit board material comprising an insulating layer made of the resin sheet according to [8] above and a conductor laminated thereon. Effect of the Invention

[0009] According to the present invention, it is possible to obtain a sheet cured product and a circuit board material having an excellent balance between low dielectric properties and a low linear thermal expansion coefficient, as well as a resin composition, a resin sheet, and a laminate from which the sheet cured product and the circuit board material having an excellent balance between low dielectric properties and a low linear thermal expansion coefficient can be produced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail below. However, the following description is an example of an embodiment of the present invention, and the present invention is not limited to the contents of the following description as long as it does not deviate from the gist of the present invention. In the following, when the expression "~" is used, it is used as an expression including the numerical values ​​or physical properties before and after it.

[0011] <Resin composition> A resin composition according to one embodiment of the present invention (hereinafter also referred to as "the composition") contains at least one thermoplastic resin (A1) selected from the group consisting of a styrene-based thermoplastic elastomer, an olefin-based thermoplastic elastomer, and an ethylene-based polymer, a maleimide compound (B) having one or more N-substituted maleimide groups in the molecule, and a radically polymerizable compound (C) having two or more ethylenically unsaturated bonds in the molecule. The reason why the linear thermal expansion coefficient of the cured sheet and circuit board material made from this composition is low is not clear, but it is thought that this is because, although the maleimide compound (B) alone has difficulty in undergoing a crosslinking reaction on its own due to steric hindrance, a rigid crosslinked structure is formed and molecular mobility is restricted by copolymerization of the maleimide compound (B) with the radically polymerizable compound (C) or with double bonds generated in the composition when radicals abstract hydrogen from the molecular chain during the curing reaction. It is believed that the heat resistance of the sheet cured product and the circuit board material made of this composition is also good. Although the reason for the good heat resistance is not clear, it is believed that when this composition is cured, the crosslink density is artificially increased by the maleimide compound (B) and the radical polymerizable compound (C) entangled with the thermoplastic resin (A1), and the elastic modulus is improved. Each component of the composition will now be described.

[0012] 1.Thermoplastic resin (A1) The thermoplastic resin (A1) of the present composition is at least one selected from the group consisting of styrene-based thermoplastic elastomers, olefin-based thermoplastic elastomers, and ethylene-based polymers. The thermoplastic resin (A1) may be used alone or in combination of two or more.

[0013] Examples of the styrene-based thermoplastic elastomer include styrene-butadiene-styrene block copolymer (SBS), styrene-isoprene-styrene block copolymer (SIS), and hydrogenated versions of these, such as styrene-ethylene-butadiene-styrene block copolymer (SEBS), styrene-ethylene-propylene-styrene block copolymer (SEPS), and styrene-isobutylene-styrene block copolymer (SIBS).

[0014] The olefin-based thermoplastic elastomer contains a polyolefin (excluding cyclic polyolefins, which will be described later) as a hard segment, and a rubber component as a soft segment. The olefin-based thermoplastic elastomer may be a mixture (polymer blend) of a polyolefin and a rubber component, a cross-linked product obtained by cross-linking a polyolefin with a rubber component, or a polymer obtained by polymerizing a polyolefin with a rubber component. The polyolefin includes polypropylene, polyethylene, and the like. Examples of the rubber component include diene rubbers such as isoprene rubber, butadiene rubber, butyl rubber, propylene-butadiene rubber, acrylonitrile-butadiene rubber, and acrylonitrile-isoprene rubber; ethylene-propylene non-conjugated diene rubber; and ethylene-butadiene copolymer rubber.

[0015] The ethylene polymer includes a homopolymer of ethylene and a copolymer of ethylene and another monomer. The copolymer of ethylene and another monomer preferably contains ethylene as a main component. Here, "containing ethylene as a main component" means that the copolymer contains 50 mol % or more, preferably 60 mol % or more, of ethylene structural units. The other monomer to be copolymerized with ethylene is not particularly limited as long as it is a monomer copolymerizable with ethylene. Preferred examples of the ethylene polymer include low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), polyethylene obtained by polymerization using a metallocene catalyst, etc. Among these, it is particularly preferable to use linear low-density polyethylene (LLDPE) because of its high flexibility.

[0016] Among the above thermoplastic resins (A1), from the viewpoints of low dielectric properties and ease of processing, styrene-based thermoplastic elastomers are preferred, and styrene-ethylene-butadiene-styrene block copolymers (SEBS) are more preferred. In addition, among the above-mentioned thermoplastic resins (A1), when a combination in which the thermoplastic resin (A1) and the maleimide compound (B) and the thermoplastic resin (A1) and the radical polymerizable compound (C) are not easily reacted with each other is selected, the thermoplastic resin (A1) does not form a chemical bond with the maleimide compound (B) and the radical polymerizable compound (C), but has a structure in which the molecular chains of the thermoplastic resin (A1) and the maleimide compound (B) and the radical polymerizable compound (C) are partially and physically entangled with each other, so that the crosslink density is increased in a pseudo manner compared to the thermoplastic resin (A1) alone while maintaining the low dielectric properties of the thermoplastic resin (A1). Therefore, it is considered that the linear thermal expansion coefficient is reduced, the elastic modulus is improved, and the heat resistance is improved. From this viewpoint, the thermoplastic resin (A1), the maleimide compound (B) and the radically polymerizable compound (C) are preferably a combination that does not react with each other, and among the above-mentioned thermoplastic resins (A1), a styrene-based thermoplastic elastomer is preferred, a styrene-isobutylene-styrene block copolymer (SIBS) or a styrene-ethylene-butadiene-styrene block copolymer (SEBS) is more preferred, and a styrene-ethylene-butadiene-styrene block copolymer (SEBS) is even more preferred.

[0017] When a styrene-based thermoplastic elastomer is used as the thermoplastic resin (A1), the styrene content is preferably 10% by mass or more, more preferably 15% by mass or more, and is preferably 70% by mass or less, more preferably 60% by mass or less, even more preferably 50% by mass or less, and even more preferably 40% by mass or less. When the styrene content is within the above range, the thermoplastic resin (A1) has a low dielectric tangent and an appropriate elastic modulus, so that low dielectric properties and heat resistance can be achieved at the same time, and handling properties are also good.

[0018] The thermoplastic resin (A1) may be modified by a known method. Examples of the modified products include reaction products of the above-mentioned thermoplastic resin (A1) with at least one of an unsaturated carboxylic acid and an anhydride thereof. By modifying the thermoplastic resin (A1), the polarity of the polymer increases, and this is expected to improve adhesion to conductors such as copper foil.

[0019] Examples of at least one of the unsaturated carboxylic acid and the anhydride thereof include unsaturated carboxylic acids such as acrylic acid, methacrylic acid, α-ethylacrylic acid, maleic acid, fumaric acid, tetrahydrophthalic acid, methyltetrahydrophthalic acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid, and nadic acids, and their anhydrides. Specific examples of the acid anhydride include maleic anhydride, citraconic anhydride, and nadic anhydrides. Examples of nadic acids or their anhydrides include endo-cis-bicyclo[2.2.1]hept-2,3-dicarboxylic acid (nadic acid), methyl-endo-cis-bicyclo[2.2.1]hept-5-ene-2,3-dicarboxylic acid (methylnadic acid), and the like, and their anhydrides.

[0020] Of these unsaturated carboxylic acids and / or their anhydrides, acrylic acid, maleic acid, nadic acid, maleic anhydride and nadic anhydride are preferred. At least one of the unsaturated carboxylic acid and the anhydride thereof may be used alone or in combination of two or more kinds.

[0021] From the viewpoint of low dielectric properties, the content of the thermoplastic resin (A1) in the composition is preferably 20% by mass or more, more preferably 25% by mass or more, even more preferably 30% by mass or more, even more preferably 35% by mass or more, and particularly preferably 40% by mass or more, when the total amount of the thermoplastic resin (A1), the maleimide compound (B), and the radical polymerizable compound (C) is taken as 100% by mass. On the other hand, from the viewpoint of low linear thermal expansion coefficient, it is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less.

[0022] From the viewpoint of low dielectric properties, the content of the thermoplastic resin (A1) in the composition is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and even more preferably 85% by mass or more, of the resin components of the composition. The upper limit of the content is not particularly limited, and the resin components of the composition may be only the thermoplastic resin (A1) (100% by mass). In the present invention, the term "resin component" refers to the thermoplastic resin (A1) contained in the composition, the cyclic polyolefin resin copolymer (A2) described below, and other resins added as necessary. The term "resin component" does not include the radically polymerizable compound (C).

[0023] The storage modulus of the thermoplastic resin (A1) at 24° C. is preferably 0.1 MPa or more, more preferably 1 MPa or more, and is preferably less than 2000 MPa, more preferably less than 1500 MPa, even more preferably less than 1000 MPa, even more preferably less than 500 MPa, even more preferably less than 300 MPa, even more preferably less than 100 MPa, and even more preferably less than 50 MPa. By adjusting the storage modulus to less than the above upper limit, the flexibility of the obtained cured sheet will be good. Furthermore, by adjusting the storage modulus to be equal to or greater than the above lower limit, the heat resistance and handleability of the obtained sheet cured product are improved.

[0024] The storage modulus is a value obtained by forming the thermoplastic resin (A1) into a sheet having a thickness of 300 μm into a test piece and measuring the dynamic viscoelasticity with a viscoelasticity spectrometer. The measurement conditions may be the same as those described in the examples.

[0025] The density of the thermoplastic resin (A1) is 0.98 g / cm 3 Less than 0.95 g / cm is preferred. 3 Less than 0.91 g / cm is more preferable. 3 On the other hand, the lower limit of the density is not particularly limited, but is preferably 0.80 g / cm3 or less. 3 The above is preferred. When the density is equal to or less than the above value, the flexibility of the obtained cured sheet is good.

[0026] The density can be measured in accordance with ASTM D792 by forming the thermoplastic resin (A1) into a sheet having a thickness of 300 μm into a test piece.

[0027] The dielectric loss tangent of the thermoplastic resin (A1) at 10 GHz is preferably less than 0.003, more preferably less than 0.002, and even more preferably less than 0.001. On the other hand, the lower limit is not particularly limited as long as it is 0 or more. The smaller the dielectric tangent, the smaller the dielectric loss, and therefore when the composition is used as a circuit board material, the transmission efficiency and speed of electric signals can be increased.

[0028] The dielectric tangent is a value obtained by forming the thermoplastic resin (A1) into a sheet having a thickness of 300 μm into a test piece and measuring it at a temperature of 23° C. and a frequency of 10 GHz in accordance with JIS C2565:1992.

[0029] 2. Cyclic polyolefin resin copolymer (A2) The present composition may contain a cyclic polyolefin resin copolymer (A2) for the purposes of improving heat resistance, reducing the dielectric tangent, reducing the linear thermal expansion coefficient, reducing tackiness, and the like. The reason why the heat resistance, linear thermal expansion coefficient, tackiness, etc. are improved is not clear, but it is thought that this is because the inclusion of the cyclic polyolefin resin copolymer (A2) together with the thermoplastic resin (A1) introduces a rigid skeleton into the molecule. The cyclic polyolefin resin copolymer (A2) is a copolymer having an alicyclic structure, specifically, a copolymer having an alicyclic structure in the side chain of polyolefin.Preferable examples of the alicyclic structure include cycloalkane, bicycloalkane, polycyclic compound, etc.Among these, cycloalkane is preferred, and cyclohexane is more preferred. The alicyclic structure is more preferably an alicyclic structure generated by hydrogenation of an aromatic ring contained in a hydrogenated aromatic vinyl polymer block unit described below.

[0030] The cyclic polyolefin resin copolymer (A2) preferably has a crystal melting peak temperature of less than 100°C. The crystalline melting peak temperature of the cyclic polyolefin resin copolymer (A2) is preferably 50° C. or higher, more preferably 60° C. or higher, and even more preferably 65° C. or higher. The crystalline melting peak temperature of the cyclic polyolefin resin copolymer (A2) is preferably 90° C. or lower, and more preferably 85° C. or lower. The crystalline melting peak temperature in the present invention is the temperature at which a crystalline melting peak is detected in differential scanning calorimetry (DSC) measured at a heating rate of 10° C. / min. The cyclic polyolefin resin copolymer (A2) used in the present resin composition may have a crystalline melting peak at less than 100° C., and may have a crystalline melting peak at two points, for example, less than 100° C. and 100° C. or higher.

[0031] Examples of known cyclic polyolefins include hydrogenated ring-opening polymers having repeating units derived from monocyclic norbornene monomers or polycyclic norbornene monomers (e.g., International Publication Nos. WO 2012 / 046443 and WO 2012 / 033076). These cyclic polyolefins have an alicyclic structure in the polymer main chain, and either do not have a crystalline melting peak temperature below 100° C. or are amorphous. The crystallinity of a polymer usually varies depending on the regularity of the molecular structure and steric hindrance. Polymers having alicyclic structures in their side chains or main chains are difficult to crystallize due to the large steric hindrance, and tend to become amorphous. On the other hand, the cyclic polyolefin resin copolymer (A2) of the present resin composition exhibits crystallinity due to the structure of the hydrogenated conjugated diene polymer block unit described later, and has an alicyclic structure in the polyolefin side chain, so that the crystalline melting peak temperature can be made to be less than 100°C.

[0032] The melt flow rate (MFR) of the cyclic polyolefin resin copolymer (A2) is not particularly limited, but is usually 0.1 g / 10 min or more, and from the viewpoint of molding method and appearance of molded product, it is preferably 0.5 g / 10 min or more. The melt flow rate (MFR) is usually 200 g / 10 min or less, and from the viewpoint of material strength, it is preferably 100 g / 10 min or less, more preferably 90.0 g / 10 min or less. By setting the MFR within the above range, compatibility with the thermoplastic resin (A1) is improved. The MFR is determined in accordance with ISO R1133, by measuring at a temperature of 230°C and a load of 2.16 kg.

[0033] As the cyclic polyolefin resin copolymer (A2) used in the present resin composition, from the viewpoint of low dielectric properties, a cyclic polyolefin containing at least one type of hydrogenated aromatic vinyl polymer block unit and at least one type of hydrogenated conjugated diene polymer block unit (hereinafter also referred to as "cyclic polyolefin (a)"), or a modified product of the cyclic polyolefin (a) with at least one of an unsaturated carboxylic acid and an anhydride thereof is preferred.

[0034] For purposes of this invention, "block" refers to a polymeric segment of a copolymer that exhibits microphase separation from structurally or compositionally distinct polymeric segments of the copolymer. Microphase separation occurs due to the immiscibility of the polymeric segments in the block copolymer. Microphase separation and block copolymers are extensively discussed in "Block Copolymers - Designer Soft Materials" in the February 1999 issue of PHYSICS TODAY, pp. 32-38.

[0035] Examples of the cyclic polyolefin (a) include a diblock copolymer consisting of a hydrogenated aromatic vinyl polymer block unit (hereinafter also referred to as "block A") and a hydrogenated conjugated diene polymer block unit (hereinafter also referred to as "block B"), a triblock copolymer containing two or more of at least one of block A and block B, a tetrablock copolymer, and a pentablock copolymer. The cyclic polyolefin (a) preferably contains at least two blocks A, and suitable examples thereof include an ABA type, an ABAB type, and an ABABA type.

[0036] In addition, the cyclic polyolefin (a) preferably contains a segment made of a hydrogenated aromatic vinyl polymer at each end. For this reason, the hydrogenated block copolymer of the present resin composition preferably has at least two hydrogenated aromatic vinyl polymer block units (blocks A) and at least one hydrogenated conjugated diene polymer block unit (block B) between the two hydrogenated aromatic vinyl polymer block units (blocks A). From these viewpoints, the cyclic polyolefin (a) is more preferably an ABA type or an ABABA type.

[0037] The content of the hydrogenated aromatic vinyl polymer block unit (block A) in the cyclic polyolefin (a) is preferably 30 to 99 mol %, more preferably 40 to 90 mol %, still more preferably 50 mol % or more, and even more preferably 60 mol % or more. If the ratio of the hydrogenated aromatic vinyl polymer block unit (block A) is equal to or higher than the lower limit, the rigidity is not decreased and the heat resistance and the linear thermal expansion coefficient are also good. On the other hand, if the ratio is equal to or lower than the upper limit, the flexibility is good.

[0038] The content of the hydrogenated conjugated diene polymer block unit (block B) in the cyclic polyolefin (a) is preferably 1 to 70 mol %, more preferably 10 to 60 mol %, still more preferably 50 mol % or less, and even more preferably 40 mol % or less. When the ratio of the hydrogenated conjugated diene polymer block unit (block B) is equal to or higher than the lower limit, the flexibility is good. On the other hand, when the ratio is equal to or lower than the upper limit, the rigidity is not decreased and the heat resistance and the linear thermal expansion coefficient are also good.

[0039] The hydrogenated aromatic vinyl polymer block unit and the hydrogenated conjugated diene polymer block unit constituting the cyclic polyolefin (a) can be obtained by hydrogenating a polymer block composed of an aromatic vinyl monomer and a conjugated diene monomer such as 1,3-butadiene, which will be described in detail later. Also, the cyclic polyolefin (a) is preferably a block copolymer having no functional groups. The term "no functional groups" means that the block copolymer has no functional groups, i.e., no groups containing atoms other than carbon and hydrogen atoms.

[0040] The monomers for forming the aromatic vinyl polymer block unit and the conjugated diene polymer block unit before hydrogenation will be described below.

[0041] (Aromatic vinyl monomer) The aromatic vinyl monomer serving as a raw material for the aromatic vinyl polymer block unit before hydrogenation is a monomer represented by the following general formula (1).

[0042] [ka]

[0043] In the above general formula (1), R is a hydrogen atom or an alkyl group, and Ar is a phenyl group, a halophenyl group, an alkylphenyl group, an alkylhalophenyl group, a naphthyl group, a pyridinyl group, or an anthracenyl group.

[0044] When R is an alkyl group, the carbon number is preferably 1 to 6, and the alkyl group may be mono- or polysubstituted with functional groups such as a halo group, a nitro group, an amino group, a hydroxyl group, a cyano group, a carbonyl group, and a carboxyl group. Moreover, the above Ar is preferably a phenyl group or an alkylphenyl group, and more preferably a phenyl group.

[0045] Examples of aromatic vinyl monomers include styrene, α-methylstyrene, vinyltoluene (including all isomers, with p-vinyltoluene being particularly preferred), ethylstyrene, propylstyrene, butylstyrene, vinylbiphenyl, vinylnaphthalene, vinylanthracene (including all isomers), and mixtures thereof. Among these, styrene is preferred.

[0046] (Conjugated Diene Monomer) The conjugated diene monomer serving as the raw material of the conjugated diene polymer block unit before hydrogenation is not particularly limited as long as it is a monomer having two conjugated double bonds. Examples of conjugated diene monomers include 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2-methyl-1,3-pentadiene and similar compounds, and mixtures thereof. Among these, 1,3-butadiene is preferred from the viewpoint of obtaining a block having a high structural regularity and being easily crystallized.

[0047] When 1,3-butadiene is used as the conjugated diene monomer, its polymer, polybutadiene, contains 1,4-bond units ([-CH2-CH=CH-CH2-]) and 1,2-bond units ([-CH2-CH(CH=CH2)-]), and the former gives a structure similar to the repeating unit of polyethylene (ethylene structure) upon hydrogenation, and the latter gives a structure similar to the repeating unit when 1-butene is polymerized (1-butene structure). Therefore, the hydrogenated conjugated diene polymer block in the present resin composition preferably contains at least one of an ethylene structure and a 1-butene structure. Furthermore, when isoprene is used as the conjugated diene monomer, its polymer, polyisoprene, contains 1,4-bond units ([-CH2-C(CH3)=CH-CH2-]), 3,4-bond units ([-CH2-CH(C(CH3)=CH2)-]), and 1,2-bond units ([-CH2-C(CH3)(CH=CH2)-]), and contains at least one of the three types of repeating units obtained by hydrogenation.

[0048] (Block structure) The cyclic polyolefin (a) is preferably produced by hydrogenation of a multiblock copolymer such as a triblock copolymer, a tetrablock copolymer, or a pentablock copolymer, such as SBS, SBSB, SBSBS, SBSBSB, SIS, SISIS, and SISBS (where S is polystyrene, B is polybutadiene, and I is polyisoprene). The block may be a linear block or may be branched. When branched, the polymerization chain may be bonded at any position along the backbone of the copolymer. In addition to a linear block, the block may be a tapered block or a star block.

[0049] The block copolymer constituting the cyclic polyolefin (a) before hydrogenation may contain one or more additional block units other than the aromatic vinyl polymer block unit and the conjugated diene polymer block unit. For example, in the case of a triblock copolymer, these additional block units may be bonded to any position of the triblock polymer backbone.

[0050] A preferred example of the hydrogenated aromatic vinyl polymer block unit is hydrogenated polystyrene, and a preferred example of the hydrogenated conjugated diene polymer block unit is hydrogenated polybutadiene or hydrogenated polyisoprene, with hydrogenated polybutadiene being more preferred. A preferred embodiment of the cyclic polyolefin (a) is a hydrogenated triblock or pentablock copolymer of styrene and butadiene, with a hydrogenated triblock copolymer being more preferred.

[0051] (Hydrogenation level) The cyclic polyolefin (a) is a polyolefin in which the aromatic rings derived from styrene and the like are hydrogenated in addition to the double bonds derived from conjugated dienes such as butadiene, and is substantially completely hydrogenated. Specifically, it refers to a polyolefin that has achieved the following hydrogenation levels: The hydrogenation level of the hydrogenated aromatic vinyl polymer block unit is preferably 90% or more, more preferably 95% or more, further preferably 98% or more, and particularly preferably 99.5% or more. The hydrogenation level of the hydrogenated conjugated diene polymer block unit is preferably 95% or more, more preferably 99% or more, and even more preferably 99.5% or more. Such a high level of hydrogenation reduces dielectric loss and also provides good stiffness and heat resistance. The hydrogenation level of the hydrogenated aromatic vinyl polymer block unit refers to the proportion of the aromatic vinyl polymer block unit saturated by hydrogenation, and the hydrogenation level of the hydrogenated conjugated diene polymer block unit refers to the proportion of the conjugated diene polymer block unit saturated by hydrogenation. The hydrogenation level of each block unit is determined using proton NMR.

[0052] The cyclic polyolefin resin copolymer (A2) may be used alone or in combination of two or more kinds. As the cyclic polyolefin resin copolymer (A2) in the present resin composition, commercially available products can be used, specifically, TEFABLOC (registered trademark) manufactured by Mitsubishi Chemical Corporation can be mentioned.

[0053] When the composition contains a cyclic polyolefin resin copolymer (A2), the content thereof is preferably 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more of the resin components of the composition from the viewpoints of reducing the linear thermal expansion coefficient and reducing tackiness. On the other hand, the upper limit is preferably 40% by mass or less, more preferably 38% by mass or less, and even more preferably 35% by mass or less from the viewpoints of flexibility and adhesion to the substrate.

[0054] 3. Maleimide Compound (B) The maleimide compound (B) of the present composition has one or more N-substituted maleimide groups in the molecule.

[0055] Examples of the maleimide compound (B) include aromatic maleimide compounds having one N-substituted maleimide group in the molecule, such as N-phenylmaleimide, N-(2-methylphenyl)maleimide, N-(4-methylphenyl)maleimide, N-(2,6-dimethylphenyl)maleimide, N-(2,6-diethylphenyl)maleimide, N-(2-methoxyphenyl)maleimide, N-benzylmaleimide, N-dodecylmaleimide, N-isopropylmaleimide, and N-cyclohexylmaleimide; bis(4-maleimidophenyl)methane, bis(4-maleimidophenyl)ether, bis(4-maleimidophenyl)sulfone, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenyl aromatic bismaleimide compounds having two N-substituted maleimide groups in the molecule, such as nylene bismaleimide, m-phenylene bismaleimide, 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane, bis(3-ethyl-5-methyl-4-maleimidophenyl)methane, 1,4-bis(maleimido)butane, and N,N'-(phenylene-di-(2,2-propylidene)-di-p-phenylene)bismaleimide; aromatic polymaleimide compounds having three or more N-substituted maleimide groups in the molecule, such as polyphenylmethane maleimide and biphenyl aralkyl maleimide; and aliphatic maleimide compounds, such as 1,6-bismaleimide-(2,2,4-trimethyl)hexane and pyrrolidine binder type long chain alkyl bismaleimide. The maleimide compound (B) may be used alone or in combination of two or more kinds.

[0056] The present composition preferably contains the maleimide compound (B) in an amount of 1% by mass or more and less than 30% by mass, when the total amount of the thermoplastic resin (A1), the maleimide compound (B) and the radically polymerizable compound (C) is taken as 100% by mass. The content of the maleimide compound (B) is more preferably 3% by mass or more, even more preferably 5% by mass or more, and even more preferably 10% by mass or more, based on the total amount, from the viewpoint of a low linear thermal expansion coefficient, while it is more preferably 25% by mass or less, and even more preferably 20% by mass or less, from the viewpoint of low dielectric properties.

[0057] The content of the maleimide compound (B) is preferably 1% by mass or more and less than 30% by mass based on the total mass of the composition. From the viewpoint of a low linear thermal expansion coefficient, the content of the maleimide compound (B) is more preferably 3 mass% or more, further preferably 5 mass% or more, and even more preferably 10 mass% or more based on the total mass of the composition, while from the viewpoint of low dielectric properties, it is more preferably 25 mass% or less, and even more preferably 20 mass% or less.

[0058] 4. Radical polymerizable compound (C) The radical polymerizable compound (C) is a compound having two or more ethylenically unsaturated bonds in the molecule. The radical polymerizable compound (C) may be either bifunctional or trifunctional or higher.

[0059] Examples of the bifunctional radically polymerizable compound (C) include bifunctional aromatic vinyl compounds such as divinylbenzene, divinylnaphthalene, and divinylbiphenyl; ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetrapropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, ethoxylated polypropylene glycol di(meth)acrylate, and the like. difunctional aliphatic (meth)acrylate compounds such as 2-methyl-1,3-propanediol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 3-methyl-1,5-pentanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 2-butyl-2-ethyl-1,3-propanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, glycerin di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, and ethoxylated 2-methyl-1,3-propanediol di(meth)acrylate;Cyclohexanedimethanol di(meth)acrylate, ethoxylated cyclohexanedimethanol di(meth)acrylate, propoxylated cyclohexanedimethanol di(meth)acrylate, ethoxylated propoxylated cyclohexanedimethanol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, ethoxylated tricyclodecane dimethanol di(meth)acrylate, propoxylated tricyclodecane dimethanol di(meth)acrylate, ethoxylated propoxylated tricyclodecane dimethanol di(meth)acrylate Bifunctional alicyclic (meth)acrylate compounds such as chlodecane dimethanol di(meth)acrylate, ethoxylated hydrogenated bisphenol A di(meth)acrylate, propoxylated hydrogenated bisphenol A di(meth)acrylate, ethoxylated propoxylated hydrogenated bisphenol A di(meth)acrylate, ethoxylated hydrogenated bisphenol F di(meth)acrylate, propoxylated hydrogenated bisphenol F di(meth)acrylate, and ethoxylated propoxylated hydrogenated bisphenol F di(meth)acrylate; ethylenedioxylated bisphenol A di(meth)acrylate, propoxylated bisphenol A di(meth)acrylate, ethoxylated propoxylated bisphenol A di(meth)acrylate, ethoxylated bisphenol F di(meth)acrylate, propoxylated bisphenol F di(meth)acrylate, ethoxylated propoxylated bisphenol F di(meth)acrylate, ethoxylated bisphenol AF di(meth)acrylate, propoxylated bisphenol AF di(meth)acrylate, ethoxylated propoxylated bis Examples of the difunctional aromatic (meth)acrylate compounds include phenol AF di(meth)acrylate, ethoxylated fluorene type di(meth)acrylate, propoxylated fluorene type di(meth)acrylate, and ethoxylated propoxylated fluorene type di(meth)acrylate; and difunctional heterocyclic (meth)acrylate compounds include ethoxylated isocyanuric acid di(meth)acrylate, propoxylated isocyanuric acid di(meth)acrylate, and ethoxylated propoxylated isocyanuric acid di(meth)acrylate.

[0060] Examples of the trifunctional or higher radical polymerizable compound (C) include triallyl cyanurate and triallyl isocyanurate compounds such as triallyl cyanurate and triallyl isocyanurate; trimethylolpropane tri(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, propoxylated trimethylolpropane tri(meth)acrylate, ethoxylated propoxylated trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, ethoxylated pentaerythritol tri(meth)acrylate, propoxylated pentaerythritol tri(meth)acrylate, and ethoxylated propoxylated pentaerythritol tri(meth)acrylate. polyfunctional aliphatic (meth)acrylate compounds such as pentaerythritol tetra(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, propoxylated pentaerythritol tetra(meth)acrylate, ethoxylated propoxylated pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetraacrylate, and dipentaerythritol hexa(meth)acrylate; and polyfunctional heterocyclic (meth)acrylate compounds such as ethoxylated isocyanuric acid tri(meth)acrylate, propoxylated isocyanuric acid tri(meth)acrylate, and ethoxylated propoxylated isocyanuric acid tri(meth)acrylate. The radical polymerizable compound (C) may be used alone or in combination of two or more kinds.

[0061] Among the above, when a styrene-based thermoplastic elastomer is used as the thermoplastic resin (A1), from the viewpoint of optimizing the phase-separated structure of the resulting resin composition and cured product, at least one selected from the group consisting of a bifunctional aromatic vinyl compound and a trialkenyl isocyanurate compound is preferred, and among these, divinylbenzene or triallyl isocyanurate is more preferred.

[0062] The radical polymerizable compound (C) preferably has no polar functional group or has a small number of polar functional groups in the molecule. When the radical polymerizable compound (C) has a cyclic structure, it is preferable that the substituent has no polar functional group or has a small number of polar functional groups. When the amount of polar functional groups is small, the compatibility with the thermoplastic resin (A1) becomes good, and the dielectric loss tangent of the obtained sheet cured product also becomes low. The polar functional group means a functional group having a negative atom (e.g., nitrogen, oxygen, chlorine, fluorine, etc.) and having a net dipole. Examples of the functional group include an ester group, a carbonyl group, a carboxyl group, a hydroxyl group, an amide group, and an amino group. When the radical polymerizable compound (C) has an ester group, the polar functional group equivalent of the radical polymerizable compound (C) (molecular weight of the radical polymerizable compound (C) / molecular weight of the polar functional group (total amount when there are multiple polar functional groups)) is preferably 2 or more, more preferably 3 or more, even more preferably 4 or more, even more preferably 5 or more, and still more preferably 6 or more.

[0063] The mass average molecular weight (Mw) of the radical polymerizable compound (C) in the present composition is preferably 100 or more, more preferably 120 or more, while it is preferably 4000 or less, more preferably 3000 or less, even more preferably 2000 or less, even more preferably 1000 or less, particularly preferably 800 or less, and even more preferably 600 or less. When the mass average molecular weight (Mw) of the radically polymerizable compound (C) is within the above range, the molecular chains of the thermoplastic resin (A1), the maleimide compound (B), and the radically polymerizable compound (C) are more likely to entangle with each other during curing, making it easier to increase the crosslinking density in a pseudo manner. As a result, the linear thermal expansion coefficient of the obtained sheet cured product is more likely to be low and the heat resistance is also good. In addition, when the crosslinking agent is not partially crosslinked or polymerized, the "mass average molecular weight (Mw) of the radically polymerizable compound (C)" means the molecular weight of the compound used as the radically polymerizable compound (C).

[0064] The present composition preferably contains the radical polymerizable compound (C) in an amount of 1% by mass or more and 70% by mass or less, when the total amount of the thermoplastic resin (A1), the maleimide compound (B) and the radical polymerizable compound (C) is taken as 100% by mass. The content of the radical polymerizable compound (C) is more preferably 3% by mass or more, even more preferably 5% by mass or more, and even more preferably 10% by mass or more, based on the total amount, from the viewpoint of low linear thermal expansion coefficient and heat resistance, while from the viewpoint of low dielectric properties, it is more preferably 65% ​​by mass or less, even more preferably 60% by mass or less, even more preferably 55% by mass or less, and particularly preferably 50% by mass or less.

[0065] The content of the radically polymerizable compound (C) is preferably from 1% by mass to 70% by mass, based on the total mass of the composition. From the viewpoints of low linear thermal expansion coefficient and heat resistance, the content of the radical polymerizable compound (C) is more preferably 3 mass% or more, even more preferably 5 mass% or more, and even more preferably 10 mass% or more based on the total mass of the composition, while from the viewpoint of low dielectric properties, it is more preferably 65 mass% or less, even more preferably 60 mass% or less, even more preferably 55 mass% or less, and particularly preferably 50 mass% or less.

[0066] From the viewpoint of a balance between low dielectric properties and a low linear thermal expansion coefficient, the mass ratio of the maleimide compound (B) to the radically polymerizable compound (C) in the composition is preferably (B):(C)=1:0.5 to 1:10, more preferably 1:0.8 to 1:8, and even more preferably 1:1 to 1:5.

[0067] 5.Organic peroxide (D) The present composition may contain an organic peroxide (D) for the purpose of accelerating the curing reaction. Examples of the organic peroxide include those belonging to the group of hydroperoxides, dialkyl peroxides, diacyl peroxides, peroxy esters, and ketone peroxides. Specific examples of the peroxides include hydroperoxides such as cumene hydroperoxide and tert-butyl hydroperoxide; dialkyl peroxides such as dicumyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane and 2,5-bis(tert-butylperoxy)-2,5-dimethyl-3-hexyne; diacyl peroxides such as lauryl peroxide and benzoyl peroxide; peroxy esters such as tert-butyl peroxyacetate, tert-butyl peroxybenzoate and tert-butylperoxyisopropyl carbonate; and ketone peroxides such as cyclohexanone peroxide. The organic peroxide (D) may be used alone or in combination of two or more kinds.

[0068] The content of the organic peroxide (D) in the composition is preferably from 0.01 to 5 parts by mass, more preferably from 0.05 to 3 parts by mass, and even more preferably from 0.1 to 1 part by mass, per 100 parts by mass of the total amount of the thermoplastic resin (A1), the maleimide compound (B), and the radically polymerizable compound (C). When the content of the organic peroxide (D) is within the above range, the curing reaction can be promoted while the dielectric properties of the sheet cured product can be maintained at a low level.

[0069] 6. Solvent (E) When a resin sheet is produced from the present composition through a coating step, the composition may contain a solvent (E). The solvent (E) is not particularly limited as long as it can uniformly dissolve the thermoplastic resin (A1), the maleimide compound (B), and the radical polymerizable compound (C), and examples of the solvent include toluene, cyclohexane, tetrahydrofuran, and xylene. The solvent (E) may be used alone or in combination of two or more kinds.

[0070] The solvent (E) preferably has a boiling point of 200° C. or lower so that it volatilizes when the resin sheet is dried.

[0071] From the viewpoint of film-formability, the content of the solvent (E) in the present composition is preferably from 100 parts by mass to 500 parts by mass, and more preferably from 200 parts by mass to 400 parts by mass, per 100 parts by mass of the total amount of the thermoplastic resin (A1), the maleimide compound (B) and the radically polymerizable compound (C).

[0072] 7. Other Ingredients The composition may contain, as components other than those described above, a thermoplastic elastomer other than the thermoplastic resin (A1), a crosslinking agent other than the maleimide compound (B) and the radically polymerizable compound (C), an ultraviolet absorber, an antistatic agent, an antioxidant, a coupling agent, a plasticizer, a flame retardant, a colorant, a dispersant, an emulsifier, an elasticity reducing agent, a diluent, an antifoaming agent, an ion trapping agent, a thickener, a leveling agent, inorganic particles, organic particles, etc. These components may be used alone or in combination of two or more.

[0073] Examples of crosslinking agents other than the maleimide compound (B) and the radically polymerizable compound (C) include epoxy compounds.

[0074] Examples of inorganic particles include calcium carbonate, magnesium carbonate, barium carbonate, magnesium sulfate, barium sulfate, calcium sulfate, zinc oxide, magnesium oxide, calcium oxide, titanium oxide, aluminum oxide, zinc oxide, alumina, aluminum hydroxide, hydroxyapatite, silica, magnesium silicate, mica, talc, kaolin, clay, glass powder, asbestos powder, zeolite, and clay silicate. Examples of the organic particles include (meth)acrylate-based resin particles, styrene-based resin particles, silicone-based resin particles, nylon-based resin particles, polyethylene-based resin particles, benzoguanamine-based resin particles, and urethane-based resin particles.

[0075] When inorganic particles or organic particles are contained, the content is preferably 1 part by mass or more and 2000 parts by mass or less, more preferably 25 parts by mass or more and 175 parts by mass or less, and even more preferably 50 parts by mass or more and 150 parts by mass or less, per 100 parts by mass of the total amount of the thermoplastic resin (A1), the maleimide compound (B) and the radical polymerizable compound (C). When the content of the inorganic particles or organic particles is equal to or more than the lower limit, the dielectric properties of the sheet cured product can be further reduced, and the linear thermal expansion coefficient of the sheet cured product can be reduced, so that peeling from the substrate is unlikely to occur when used as a circuit board material. On the other hand, when the content of the inorganic particles or organic particles is equal to or less than the upper limit, the moldability of the sheet cured product is good.

[0076] <Resin sheet> A resin sheet according to one embodiment of the present invention (hereinafter also referred to as "the present resin sheet") is obtained by forming the present composition in an uncured state into a sheet shape.

[0077] The thickness of the present resin sheet after curing is preferably from 10 to 500 μm, more preferably from 50 to 400 μm, and even more preferably from 100 to 350 μm. When the thickness of the resin sheet after curing is equal to or greater than the lower limit, the sheet has good handleability, whereas when the thickness is equal to or less than the upper limit, the sheet has good conformability to uneven surfaces of the circuit board when the resin sheet is used as a circuit board material. The above thickness was measured with a micrometer on the cured product obtained by heat pressing the resin sheet at 200° C. and 2 MPa for 30 minutes.

[0078] The relative dielectric constant of the resin sheet after curing is preferably equal to or less than 4, more preferably equal to or less than 3, and even more preferably equal to or less than 2.5. On the other hand, there is no particular lower limit to the relative dielectric constant, and it is sufficient if it is equal to or greater than 1. The dielectric loss tangent of the resin sheet after curing is preferably 0.003 or less, more preferably 0.002 or less, and even more preferably 0.0015 or less. On the other hand, the lower limit of the dielectric loss tangent is not particularly limited, and it is sufficient that it is 0 or more. The above-mentioned dielectric constant and dielectric tangent were determined by measuring the cured material obtained by heat pressing the resin sheet at 200°C and 2 MPa for 30 minutes as a test piece at a temperature of 23°C and a frequency of 10 GHz in accordance with JIS C2565:1992.

[0079] The average linear thermal expansion coefficient of the resin sheet at 0 to 140°C after curing is preferably 300 ppm / K or less, more preferably 250 ppm / K or less, even more preferably 200 ppm / K or less, even more preferably 150 ppm / K or less, and particularly preferably 100 ppm / K or less. By having the average linear thermal expansion coefficient be equal to or less than the above upper limit, the difference with the linear thermal expansion coefficient of a conductor such as copper foil can be reduced, and curling or warping when laminated with a conductor can be suppressed. Although there is no particular lower limit for the coefficient of linear thermal expansion, it is preferably 10 ppm / K or more from the viewpoint of preventing peeling from the conductor or deformation when the sheet cured product is used as a circuit board material. The linear thermal expansion coefficient can be measured by thermomechanical analysis according to JIS K7197 (2012) using a test piece of the cured product obtained by heat pressing the resin sheet at 200°C and 2MPa for 30 minutes. Specifically, a thermal analyzer "TMA 841" (Mettler Toledo) was used to measure the sample shape, which was 5 mm wide x 16 mm long, starting from 30°C and heating to 100°C at 5°C / min, then cooling to 0°C once, and then heating to 150°C again. The dimensional change during the reheating process was measured, and the average value of the thermal expansion coefficient in the in-plane direction from 0 to 140°C was calculated based on the results.

[0080] <Laminate> In order to improve the handling properties of the present resin sheet, it is preferable to provide a release film on one or both surfaces to form a laminate. As the release film, for example, a resin film mainly composed of polyolefin such as polyethylene or polypropylene, polyester such as polyethylene terephthalate or polyethylene naphthalate, polyimide, polycarbonate, etc. can be used. The peel strength may be adjusted by applying a silicone resin release agent or the like. The thickness of the release film is preferably from 1 to 300 μm, more preferably from 5 to 200 μm, further preferably from 10 to 150 μm, and even further preferably from 20 to 120 μm. The surface of the release film that comes into contact with the resin sheet may be subjected to a matte treatment, a corona treatment, or an antistatic treatment.

[0081] The laminate may be a wound body wound around a core. In the wound body according to one embodiment of the present invention, the length of the laminate is preferably 10 m or more, more preferably 20 m or more. When the resin sheet is used as a flexible laminate or a stretchable laminate, for example, the length of the laminate is 10 m or more, so that electronic components can be continuously produced, and the continuous film forming property is excellent. The upper limit of the length is not particularly limited, but is preferably 1000 m or less. The material of the core is not particularly limited, but examples thereof include paper, resin-impregnated paper, acrylonitrile / butadiene / styrene copolymer (ABS resin), fiber-reinforced plastic (FRP), phenolic resin, resin containing inorganic matter, etc. An adhesive may be used for the core.

[0082] <Method of manufacturing resin sheet> Hereinafter, a method for producing the present resin sheet will be described, but the method for producing the present resin sheet is not limited to the following method.

[0083] [First manufacturing method] The first method for producing a resin sheet includes a coating liquid preparation step of preparing a coating liquid containing a resin composition, and a molding step of molding the coating liquid into a sheet.

[0084] (1) Coating fluid preparation process In the coating solution preparation step, the thermoplastic resin (A1), the maleimide compound (B), the radically polymerizable compound (C), and the cyclic polyolefin resin copolymer (A2), which is added as needed, the organic peroxide (D), the solvent (E), and other components are stirred and mixed uniformly to obtain the coating solution. For mixing, a general mixing / stirring device such as a mixer, blender, three-roll kneader, ball mill, kneader, single-screw kneader or twin-screw kneader can be used, and heating may be performed during mixing, if necessary.

[0085] (2) Molding process In the forming step, the coating liquid is formed into a sheet to obtain a resin sheet. The coating liquid can be formed into a sheet by a known method. For example, the method may be a doctor blade method, a solvent casting method, or an extrusion film forming method. A preferred forming method includes a method including the following (2-1) coating step and (2-2) drying step.

[0086] (2-1) Coating process In the coating step, a coating liquid is applied to the surface of a release film to form a coating film. The coating method may be a common method such as a dip method, a spin coating method, a spray coating method, a blade method, etc. For coating, a coating device such as a spin coater, a slit coater, a die coater, a blade coater, etc. can be used, and this makes it possible to uniformly form a coating film of a predetermined thickness on the release film.

[0087] (2-2) Drying process In the drying step, the solvent is removed from the coating film formed above. The drying temperature is not particularly limited, but is usually 10 to 150° C., preferably 25 to 120° C., and more preferably 30 to 110° C. When the drying temperature is equal to or lower than the upper limit, the crosslinking reaction of the maleimide compound (B) and the radical polymerizable compound (C) in the coating film is suppressed. When the drying temperature is equal to or higher than the lower limit, foaming of the resin sheet is suppressed, and the solvent can be effectively removed, improving productivity. The drying time can be appropriately adjusted depending on the state of the coating film, the drying environment, etc. The drying time is preferably 1 minute or more, more preferably 2 minutes or more, even more preferably 5 minutes or more, even more preferably 10 minutes or more, particularly preferably 20 minutes or more, and most preferably 30 minutes or more. On the other hand, the drying time is preferably 4 hours or less, more preferably 3 hours or less, and even more preferably 2 hours or less. By setting the drying time to the above lower limit or more, the solvent can be sufficiently removed, whereas by setting the drying time to the above upper limit or less, the productivity can be improved and the production cost can be suppressed. The solvent in the resin composition can be removed by a known heating method such as using a hot plate, a hot air oven, an IR heating oven, a vacuum dryer, or a high-frequency heater.

[0088] From the viewpoints of preventing contamination of the surface of the resin sheet and of handling properties, a release film may be laminated on the resin sheet after the drying step.

[0089] [Second manufacturing method] The second method for producing the resin sheet includes a film-forming step of extruding a resin composition onto a release film.

[0090] In the film-forming process, the thermoplastic resin (A1), the maleimide compound (B), the radically polymerizable compound (C), and the cyclic polyolefin resin copolymer (A2) added as required, the organic peroxide (D), and other components are kneaded in a single-screw extruder or a twin-screw extruder, and extruded onto a release film using an extruder or the like under temperature conditions that are equal to or higher than the melting point of the thermoplastic resin (A1) and lower than the crosslinking temperature of the maleimide compound (B) and the radically polymerizable compound (C) to form a film. The extrusion method of the resin composition is not particularly limited, but more specifically, T-die molding can be mentioned.

[0091] <Cured sheet> A sheet cured product according to one embodiment of the present invention (hereinafter also referred to as a "main cured product") is obtained by curing the above-mentioned resin sheet.

[0092] The curing temperature of the resin sheet may be any temperature at which the thermoplastic resin (A1) does not flow and at which the crosslinking reaction of the maleimide compound (B) and the radical polymerizable compound (C) proceeds, and is preferably 120 to 300°C, more preferably 140 to 250°C, and even more preferably 150 to 220°C. The curing time for the resin sheet is not particularly limited, but is preferably 10 minutes to 1 hour.

[0093] <Applications of the resin composition, resin sheet, and cured sheet> Applications of the resin composition, resin sheet and cured sheet of the present invention include, for example, copper foil laminates, stretchable substrates, flexible printed circuit boards, multilayer printed wiring boards, circuit board materials for electric and electronic devices such as capacitors, underfill materials, interchip fills for 3D-LSI, insulating sheets, vibration damping materials, adhesives, solder resists, semiconductor encapsulants, hole filling resins, and component embedding resins, but are not limited thereto.

[0094] <Circuit board materials> The resin sheet according to one embodiment of the present invention can be used as a circuit board material by laminating it with a conductor.

[0095] The conductor may be a metal foil made of a conductive metal such as copper or aluminum, or an alloy containing such a metal, or a metal layer formed by plating or sputtering.

[0096] When used as a circuit board material for electric / electronic devices, the resin sheet preferably has a thickness of 10 μm or more and 500 μm or less, and the conductor preferably has a thickness of 0.2 μm or more and 70 μm or less.

[0097] <Method of manufacturing circuit board materials> The circuit board material of the present invention can be produced, for example, by the following method. After laminating the resin sheet according to an embodiment of the present invention on a conductor, the resin sheet is heat cured to form an insulating layer, on which a conductor is further laminated, and a required number of such layers are laminated.

[0098] The curing temperature of the resin sheet may be any temperature at which the thermoplastic resin (A1) does not flow and at which the crosslinking reaction of the maleimide compound (B) and the radical polymerizable compound (C) proceeds. Specifically, the curing temperature of the resin sheet is preferably 120 to 300°C, more preferably 140 to 250°C, and further preferably 150 to 220°C. The curing time of the resin sheet is not particularly limited, but is preferably from 10 minutes to 1 hour.

[0099] The lamination of the resin sheet and the conductor may be performed by directly laminating a conductive metal foil on the resin sheet, by bonding the resin sheet and the conductive metal foil with an adhesive, by forming a conductive metal layer by plating or sputtering, or by combining these methods. The method may also include a step of drilling holes in the cured layer to form via holes, and a step of roughening the surface of the cured layer. EXAMPLES

[0100] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following examples and comparative examples, various physical properties were measured by the following methods.

[0101] <Raw materials> [Thermoplastic resin (A1)] a1-1: styrene-ethylene-butadiene-styrene block copolymer (SEBS: Asahi Kasei Corporation, "Tuftec H1052"), styrene content 20% by mass, storage modulus (24°C) = 6.2 MPa, density = 890 g / cm 3 [Cyclic polyolefin resin copolymer (A2)] a2-1: Cyclic polyolefin copolymer (HSEBS: Mitsubishi Chemical Corporation, "TEFABLOCK CP CP402"), hydrogenated aromatic vinyl polymer block unit (hydrogenated polystyrene with a hydrogenation level of 99% or more): content 67 mol%, hydrogenated conjugated diene polymer block unit (hydrogenated polybutadiene with a hydrogenation level of 99% or more): content 33 mol%, block structure: pentablock structure, total hydrogenation level: 99% or more, crystal melting peak temperature: 75°C, MFR (230°C, 2.16 kg): 85g / 10 min

[0102] [Maleimide compound (B)] b-1: Maleimide resin (manufactured by Nippon Kayaku Co., Ltd., "MIR-5000-60T") b-2: Bis(3-ethyl-5-methyl-4-maleimidophenyl)methane (K.I. Chemicals, "BMI-70") b-3: 1,4-bis(maleimido)butane (Tokyo Chemical Industry Co., Ltd.) b-4: Maleimide resin (manufactured by Nippon Kayaku Co., Ltd., "MIR-3000-70MT")

[0103] [Radical polymerizable compound (C)] c-1: A mixture of 96% divinylbenzene and 4% ethylvinylbenzene (manufactured by Nippon Steel Chemical & Material Co., Ltd., "DVB960"), mass average molecular weight (Mw): 131 c-2: Triallyl isocyanurate (TAIC: manufactured by Shinryo Corporation), mass average molecular weight (Mw): 250

[0104] [Organic peroxide (D)] d-1: 2,5-dimethyl-2,5-di-(tert-butylperoxyl)-hexyne-3 (manufactured by NOF Corporation, "Perhexyne 25B")

[0105] Solvent e-1: Toluene (content > 99.0% by mass)

[0106] <Example 1> The raw materials were mixed in the ratio shown in Table 1, and heated at about 80°C to completely dissolve the raw materials to prepare a resin composition. The prepared resin composition was spread in a sheet shape on the release-treated surface of a 50 μm-thick release film (PET film manufactured by Mitsubishi Chemical Corporation) that had been subjected to a silicone release treatment to obtain a resin sheet. The thickness of the resin sheet was adjusted so that the thickness of the sheet after curing was about 300 μm. The resin sheet spread on the release film was dried in an oven at 100°C for 1 hour, and then a 50μm-thick release film (PET film manufactured by Mitsubishi Chemical Corporation) treated with silicone release was laminated on the resin sheet so that the release-treated surface was on the resin sheet side to form a laminate. The laminate was held for 30 minutes under a pressure of about 2MPa in a heat press machine at 200°C to completely cure the resin sheet, and the release films on both sides were peeled off to obtain a sheet cured product. The dielectric properties and linear thermal expansion coefficient of the obtained sheet cured product were evaluated.

[0107] <Examples 2 to 15 and Comparative Examples 1 to 5> A sheet cured product was produced in the same manner as in Example 1, except that the raw materials were mixed according to the ratios shown in Tables 1 and 2. In Comparative Examples 2 and 5, the cured sheets foamed during curing, so that film formation was not possible. In the other examples and comparative examples, the dielectric properties and linear thermal expansion coefficients of the obtained cured sheets were evaluated.

[0108] <Measurement method> (1) Dielectric properties The in-plane relative dielectric constant and dielectric loss tangent of the cured sheet were measured in TE mode using a cavity resonator (manufactured by AET) and a network analyzer MS46 122B (manufactured by Anritsu). The measurement frequency was 10 GHz.

[0109] (2) Linear thermal expansion coefficient The linear thermal expansion coefficient of the cured sheet was measured by thermomechanical analysis according to JIS K7197 (2012). Specifically, a thermal analyzer "TMA 841" (Mettler Toledo) was used, with a sample shape of 5 mm wide x 16 mm long, and the temperature was raised from 30°C to 100°C at 5°C / min. The sample was cooled to 0°C once, and then reheated to 150°C. The dimensional change during the reheating process was measured, and the average thermal expansion coefficient in the in-plane direction from 0 to 140°C was calculated based on the results.

[0110] [Table 1]

[0111] [Table 2]

[0112] Examples 1 to 15 and Comparative Examples 1 and 2 demonstrate that by adding a maleimide compound (B) and a radically polymerizable compound (C) to a thermoplastic resin (A1), a sheet cured product having an excellent balance of low dielectric properties and a low linear thermal expansion coefficient can be obtained.

[0113] Moreover, it was shown from Examples 1 to 15 and Comparative Examples 3 to 5 that when the maleimide compound (B) was 30% by mass or more, the dielectric properties were deteriorated.

[0114] Examples 3, 5 and 6 demonstrated that the balance between the dielectric properties and the linear thermal expansion coefficient can be adjusted by adjusting the mass ratio of the maleimide compound (B) and the radically polymerizable compound (C).

[0115] In the above examples, there are no examples in which an olefin-based thermoplastic elastomer or an ethylene-based polymer is used as the thermoplastic resin (A1). However, based on the mechanism in which the molecular chains of the thermoplastic resin (A1), the maleimide compound (B), and the radically polymerizable compound (C) are entangled with each other, a good balance between low dielectric properties and a low linear thermal expansion coefficient can be achieved, and therefore, the same effects as those of a styrene-based thermoplastic elastomer can be expected.

Claims

1. The present invention comprises at least one thermoplastic resin (A1) selected from the group consisting of a styrene-based thermoplastic elastomer, an olefin-based thermoplastic elastomer, and an ethylene-based polymer, a maleimide compound (B) having one or more N-substituted maleimide groups in the molecule, and a radical polymerizable compound (C) having two or more ethylenically unsaturated bonds in the molecule, a content of the maleimide compound (B) being 1 mass% or more and less than 30 mass% when the total amount of the thermoplastic resin (A1), the maleimide compound (B), and the radical polymerizable compound (C) is 100 mass%.

2. The resin composition according to claim 1 , wherein the thermoplastic resin (A1) comprises a styrene-based thermoplastic elastomer.

3. The resin composition according to claim 2 , wherein the styrene content of the styrene-based thermoplastic elastomer is 10% by mass or more and 70% by mass or less.

4. The resin composition according to claim 1, wherein the radical polymerizable compound (C) comprises at least one selected from the group consisting of a bifunctional aromatic vinyl compound and a trialkenyl isocyanurate compound.

5. The resin composition according to claim 1, wherein the mass ratio of the maleimide compound (B) to the radical polymerizable compound (C) is (B):(C)=1:0.5 to 1:

10.

6. The resin composition according to claim 1, comprising a cyclic polyolefin resin copolymer (A2).

7. The resin composition according to claim 6, wherein the cyclic polyolefin resin copolymer (A2) is a copolymer having an alicyclic structure in a polyolefin side chain.

8. A resin sheet comprising the resin composition according to any one of claims 1 to 7.

9. A laminate comprising the resin sheet according to claim 8 and a release film on one or both surfaces thereof.

10. A sheet cured product obtained by curing the resin sheet according to claim 8.

11. A circuit board material comprising an insulating layer made of the resin sheet according to claim 8 and a conductor laminated thereon.

Citation Information

Patent Citations

  • Polyphenylene ether resin composition, prepreg, metal-clad laminate, and printed wiring board

    JP2010059363A

  • Resin composition, prepreg, laminate, resin sheet, printed wiring board and semiconductor device

    JP2012255059A

  • Cyclic olefin resin composition, and substrate provided from said resin composition

    WO2006095511A1

Cited By

  • Release film

    JP2026098851A

  • Release film

    JP7828423B1

  • Release film

    WO2026121274A1