Solid electrolyte sheet and all-solid battery

The layered solid electrolyte sheet with specific binder and particle size distributions addresses strength and conductivity issues in all-solid-state batteries, enhancing stability and efficiency.

JP2024146934APending Publication Date: 2024-10-15HONDA MOTOR CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024058257
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-29
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing all-solid-state batteries face challenges with long-term stability and charging/discharging efficiency due to the inclusion of porous base materials, which can cause uneven strength, cracks, and a decrease in ionic conductivity.

Method used

A solid electrolyte sheet with a layered structure is developed, featuring an inner layer with a high binder content and small particle size electrolyte material, and outer layers with lower binder content and larger particle size electrolyte material, enhancing adhesion and conductivity.

Benefits of technology

The solution improves the strength and suppresses crack generation while enhancing ionic conductivity, leading to improved stability and charge/discharge efficiency in all-solid-state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146934000001_ABST
    Figure 2024146934000001_ABST
Patent Text Reader

Abstract

To provide a solid electrolyte sheet in which the strength is improved, the occurrence of a crack is suppressed, and the ion conductivity is improved.SOLUTION: A solid electrolyte sheet includes an inner layer, a first outer layer stacked on one surface of the inner layer, and a second outer layer stacked on the other surface of the inner layer. The inner layer includes a porous base material and an inner layer solid electrolyte composition that fills the porous base material. The inner layer solid electrolyte composition contains a solid electrolyte material and binder. The first outer layer includes a first outer layer solid electrolyte composition containing a solid electrolyte material and binder. The second outer layer includes a second outer layer solid electrolyte composition containing a solid electrolyte material and binder. The inner layer solid electrolyte composition has a higher binder content than the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition. An average particle diameter of the solid electrolyte material included in the inner layer solid electrolyte composition is smaller than that of the solid electrolyte material in the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a solid electrolyte sheet and an all-solid-state battery. [Background technology]

[0002] In recent years, research and development on all-solid-state batteries that contribute to energy efficiency has been conducted to ensure that more people have access to affordable, reliable, sustainable, and advanced energy. All-solid-state batteries generally have a structure in which a solid electrolyte layer is sandwiched between a positive electrode and a negative electrode. For example, the solid electrolyte layer of a lithium-ion all-solid-state battery has a function of conducting lithium ions and a function as a separator that prevents a short circuit between the positive electrode layer (positive electrode active material layer) in the positive electrode and the negative electrode layer (negative electrode active material layer) in the negative electrode. Here, it is considered preferable that the solid electrolyte layer that serves as the separator is as thin as possible in order to improve the energy density. However, simply making it thin leads to the occurrence of cracks due to a decrease in strength, so all-solid-state batteries that contain a porous substrate to thin the solid electrolyte layer and ensure its strength are known (see Patent Document 1, etc.). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2015-153460 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, in the technology related to all-solid-state batteries, the long-term stability and improvement of charge / discharge efficiency are issues. The inclusion of a porous substrate improves the strength of the solid electrolyte layer, improving the stability of the all-solid-state battery. However, the use of a porous substrate may cause unevenness in strength, or the inclusion of a porous substrate may cause cracks or a decrease in ion conductivity.

[0005] In order to solve the above problems, the present application has as its main object to provide a solid electrolyte sheet having improved strength, suppressed cracking, and improved ionic conductivity, and an all-solid-state battery having a solid electrolyte layer having improved strength, suppressed cracking, and improved ionic conductivity, which will ultimately contribute to energy efficiency. [Means for solving the problem]

[0006] In order to solve the above problems, the present inventors have found that, in a solid electrolyte sheet having an inner layer in which a porous substrate is filled with a solid electrolyte composition containing a solid electrolyte material and a binder, and an outer layer containing a solid electrolyte composition laminated on the surface of the inner layer, it is effective to adjust the particle size of the solid electrolyte material used in the inner layer and the outer layer and the amount of the binder, and have completed the present invention. Accordingly, the present invention provides the following.

[0007] (1) A solid electrolyte sheet having an inner layer, a first outer layer laminated on one surface of the inner layer, and a second outer layer laminated on the other surface of the inner layer, the inner layer comprising a porous substrate and an inner layer solid electrolyte composition filled in the porous substrate, the inner layer solid electrolyte composition containing a solid electrolyte material and a binder, the first outer layer comprising a first outer layer solid electrolyte composition containing a solid electrolyte material and a binder, the second outer layer comprising a second outer layer solid electrolyte composition containing a solid electrolyte material and a binder, the inner layer solid electrolyte composition having a higher binder content than the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition, and an average particle size of the solid electrolyte material contained in the inner layer solid electrolyte composition being smaller than the average particle sizes of the solid electrolyte materials contained in the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition.

[0008] According to the solid electrolyte sheet of (1), the inner layer solid electrolyte composition has a high binder content and has high adhesion to the porous substrate of the inner layer, so that cracks are unlikely to occur. On the other hand, the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition have a low binder content, so that ion conductivity is improved. In addition, the inner layer solid electrolyte composition has a small average particle size of the solid electrolyte material, so that it is easy to fill the porous substrate of the inner layer and is filled at a high density, so that the strength of the solid electrolyte sheet and the effect of suppressing the occurrence of cracks are improved. Furthermore, the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition have a large average particle size of the solid electrolyte material, so that the lithium ion conductivity of the solid electrolyte sheet is improved. Therefore, according to the solid electrolyte sheet of (1), the strength is improved, the occurrence of cracks is suppressed, and the ion conductivity is improved.

[0009] (2) The solid electrolyte sheet according to (1), wherein the binder content of the first outer layer solid electrolyte composition and the binder content of the second outer layer solid electrolyte composition are within a range of 1 / 10 to 9 / 10 of the binder content of the inner layer solid electrolyte composition.

[0010] According to the solid electrolyte sheet of (2), since the binder contents of the inner layer solid electrolyte composition, the first outer layer solid electrolyte composition, and the second outer layer solid electrolyte composition satisfy the above-mentioned relationship, the strength of the solid electrolyte sheet, the effect of suppressing crack generation, and the lithium ion conductivity are improved in a more balanced manner.

[0011] (3) The solid electrolyte sheet according to (2), wherein the binder content of the first outer layer solid electrolyte composition and the binder content of the second outer layer solid electrolyte composition are within a range of 3 / 10 to 6 / 10 of the binder content of the inner layer solid electrolyte composition.

[0012] According to the solid electrolyte sheet of (3), the binder contents of the inner layer solid electrolyte composition, the first outer layer solid electrolyte composition, and the second outer layer solid electrolyte composition satisfy the above-mentioned relationship, and therefore the strength of the solid electrolyte sheet, the effect of suppressing crack generation, and the lithium ion conductivity are improved in a more balanced manner.

[0013] (4) The solid electrolyte sheet according to any one of (1) to (3), wherein the binder content of the inner layer solid electrolyte composition is within a range of 3 to 20 mass %.

[0014] According to the solid electrolyte sheet of (4), since the binder content of the inner layer solid electrolyte composition is within the above range, the strength of the solid electrolyte sheet, the effect of suppressing crack generation, and the lithium ion conductivity are improved in a more balanced manner.

[0015] (5) The solid electrolyte sheet according to (4), wherein the binder content of the inner layer solid electrolyte composition is within a range of 3 to 9 mass %.

[0016] According to the solid electrolyte sheet of (5), since the binder content of the solid electrolyte composition for the inner layer is within the above range, the lithium ion conductivity is further improved.

[0017] (6) The solid electrolyte sheet according to (5), wherein the inner layer has a thickness in the range of 10 to 25 μm.

[0018] According to the solid electrolyte sheet of (6), since the thickness of the inner layer is within the above range, the lithium ion conductivity is further improved.

[0019] (7) The solid electrolyte sheet according to (4), wherein the binder content of the inner layer solid electrolyte composition is within a range of 10 to 20 mass %.

[0020] According to the solid electrolyte sheet of (7), since the binder content of the inner layer solid electrolyte composition is within the above range, the strength of the solid electrolyte sheet is further improved.

[0021] (8) The solid electrolyte sheet according to any one of (1) to (7), wherein a particle size distribution peak of the solid electrolyte material contained in the inner layer solid electrolyte composition is in a region where the particle size is 1 μm or less, and a particle size distribution peak of the solid electrolyte materials contained in the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition is in a region where the particle size is 1 μm or less and a region where the particle size is 3 μm or more.

[0022] According to the solid electrolyte sheet of (8), the inner layer solid electrolyte composition contains many fine particles of a solid electrolyte material having a particle size of 1 μm or less, and is therefore easily filled into the porous substrate of the inner layer. This improves the strength of the solid electrolyte sheet and the effect of suppressing the occurrence of cracks. In addition, the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition contain fine particles of a solid electrolyte material having a particle size of 1 μm or less and coarse particles of a solid electrolyte material having a particle size of 3 μm or more, and the fine particles are interposed between the coarse particles, so that the first outer layer and the second outer layer tend to be dense. This improves the lithium ion conductivity of the solid electrolyte sheet.

[0023] (9) The solid electrolyte sheet according to any one of (1) to (8), wherein the inner layer has a thickness in the range of 2 to 30 μm, and the first outer layer and the second outer layer have thicknesses in the range of 1 / 5 to 2 times the thickness of the inner layer.

[0024] According to the solid electrolyte sheet of (9), since the thicknesses of the inner layer, the first outer layer, and the second outer layer are within the above-mentioned ranges, the strength, the effect of suppressing crack generation, and the lithium ion conductivity are improved in a more balanced manner.

[0025] (10) The solid electrolyte sheet according to (9), wherein the first outer layer and the second outer layer have a thickness smaller than a thickness of the inner layer.

[0026] According to the solid electrolyte sheet of (10), the first outer layer and the second outer layer are thinner than the inner layer, so that the lithium ion conductivity is further improved.

[0027] (11) The solid electrolyte sheet according to (10), wherein the thickness of the first outer layer and the second outer layer is within a range of 1 / 5 to 4 / 5 times the thickness of the inner layer.

[0028] According to the solid electrolyte sheet of (11), the relationship between the thicknesses of the inner layer, the first outer layer, and the second outer layer is within the above range, so that the lithium ion conductivity is further improved.

[0029] (12) The solid electrolyte sheet according to any one of (9) to (11), wherein the inner layer has a thickness in the range of 10 to 25 μm.

[0030] According to the solid electrolyte sheet of (12), since the thickness of the inner layer is within the above range, the lithium ion conductivity is further improved and the electrical resistance is reduced.

[0031] (13) An all-solid-state battery comprising a positive electrode, a negative electrode, and a solid electrolyte layer disposed between the positive electrode and the negative electrode, the solid electrolyte layer being made of the solid electrolyte sheet according to any one of (1) to (125), the first outer layer being in contact with the positive electrode, and the second outer layer being in contact with the negative electrode.

[0032] According to the all-solid-state battery of (13), since the solid electrolyte layer is made of the above-mentioned solid electrolyte sheet, the strength of the solid electrolyte layer is improved, the occurrence of cracks is suppressed, and the ion conductivity is improved. Effect of the Invention

[0033] According to the present invention, it is possible to provide a solid electrolyte sheet having improved strength, suppressed cracking, and improved ion conductivity, and an all-solid-state battery having a solid electrolyte layer having improved strength, suppressed cracking, and improved ion conductivity. [Brief description of the drawings]

[0034] [Figure 1] FIG. 1 is a cross-sectional view illustrating a schematic configuration of an all-solid-state battery according to one embodiment of the present invention. [Diagram 2] 2 is a SEM photograph of a cross section of an inner layer of the solid electrolyte sheet obtained in Example 1. [Diagram 3] 2 is a SEM photograph of a cross section of a first outer layer of the solid electrolyte sheet obtained in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0035] Hereinafter, an embodiment of the present invention will be described.

[0036] FIG. 1 is a cross-sectional view of an all-solid-state battery 1 according to one embodiment of the present invention. As shown in FIG. 1, the all-solid-state battery 1 includes a positive electrode 10, a negative electrode 20, and a solid electrolyte layer 30. The all-solid-state battery 1 is a laminate in which the positive electrode 10, the solid electrolyte layer 30, and the negative electrode 20 are laminated in this order. The all-solid-state battery 1 according to the embodiment is a lithium-ion all-solid-state battery. Note that the all-solid-state battery in this specification refers to a battery that has been made into an all-solid state. The positive electrode 10 has a positive electrode layer 11 and a positive electrode current collector 12. The positive electrode layer 11 is disposed on the side of the solid electrolyte layer 30. The positive electrode current collector 12 constitutes the surface of the all-solid-state battery 1 on the positive electrode 10 side.

[0037] The positive electrode layer 11 includes a positive electrode active material. The positive electrode active material used in the positive electrode layer 11 is not particularly limited, and may be any material that functions as a positive electrode of the all-solid-state battery 1. Specific examples of the positive electrode active material include sulfide-based materials such as titanium sulfide (TiS2), molybdenum sulfide (MoS2), iron sulfide (FeS, FeS2), copper sulfide (CuS), and nickel sulfide (Ni3S2). Also, examples of oxide-based materials include bismuth oxide (Bi2O3), bismuth lead oxide (Bi2Pb2O5), copper oxide (CuO), vanadium oxide (VO), and the like. 13 ), lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2), Li(NiCoMn)O2, Li(NiCoAl)O2, Li(NiCo)O2, etc. Also, these can be used in combination.

[0038] The positive electrode current collector 12 has a function of collecting current from the positive electrode layer 11. The positive electrode current collector 12 is a foil-shaped member made of an electrode material having electrical conductivity. The electrode material used for the positive electrode current collector 12 is not particularly limited as long as it is a material having electrical conductivity, and examples thereof include vanadium, aluminum, stainless steel, gold, platinum, manganese, iron, titanium, etc., with aluminum being preferred among them. The shape and thickness of the positive electrode current collector 12 are not particularly limited as long as they are capable of collecting current from the positive electrode layer 11.

[0039] The negative electrode 20 has a negative electrode layer 21 and a negative electrode current collector 22. The negative electrode layer 21 is disposed on the solid electrolyte layer 30 side. The negative electrode current collector 22 constitutes the surface of the all-solid-state battery 1 on the negative electrode 20 side.

[0040] The negative electrode layer 21 may contain a negative electrode active material. The negative electrode active material used in the negative electrode layer 21 is not particularly limited as long as it functions as the negative electrode of the all-solid-state battery 1, but it is preferable that the negative electrode active material contains at least one of a Li-based material and a Si-based material. Specific examples of the negative electrode active material include carbon materials, specifically, artificial graphite, graphite carbon fiber, resin-calcined carbon, pyrolytic vapor-grown carbon, coke, mesocarbon microbeads (MCMB), furfuryl alcohol resin-calcined carbon, polyacene, pitch-based carbon fiber, vapor-grown carbon fiber, natural graphite, and non-graphitizable carbon. Alternatively, the negative electrode active material may be a mixture of these materials. In addition, as the negative electrode active material, metals that form an alloy with lithium or alloys that combine these metals with other elements or compounds can be used. Examples of metals that form an alloy with lithium include metallic indium, metallic aluminum, and metallic silicon. Furthermore, metallic lithium can be used as the negative electrode layer 21.

[0041] The negative electrode current collector 22 has a function of collecting current from the negative electrode layer 21. The negative electrode current collector 22 is a foil-shaped member made of an electrode material having electrical conductivity. The electrode material used for the negative electrode current collector 22 is not particularly limited as long as it is a material having electrical conductivity, and examples thereof include vanadium, stainless steel, manganese, iron, titanium, copper, nickel, cobalt, zinc, etc., among which copper and nickel are preferable because they have excellent electrical conductivity and current collecting properties. The shape and thickness of the negative electrode current collector 22 are not particularly limited as long as they are capable of collecting current from the negative electrode layer 21.

[0042] The solid electrolyte layer 30 has an inner layer 31, a first outer layer 32 laminated on one surface of the inner layer 31, and a second outer layer 33 laminated on the other surface of the inner layer 31. The first outer layer 32 is disposed at a position where it contacts the positive electrode 10, and the second outer layer 33 is disposed at a position where it contacts the negative electrode 20. The thickness of the inner layer 31 may be, for example, within a range of 2 to 30 μm, or may be within a range of 10 to 25 μm. The thicknesses of the first outer layer 32 and the second outer layer 33 may be, for example, within a range of 1 / 5 to 2 times the thickness of the inner layer 31. From the viewpoint of improving the lithium ion conductivity of the solid electrolyte layer 30, the thicknesses of the first outer layer 32 and the second outer layer 33 may be thinner than the thickness of the inner layer 31, and the thicknesses of the first outer layer 32 and the second outer layer 33 may be within a range of 1 / 5 to 4 / 5 times the thickness of the inner layer 31.

[0043] The inner layer 31 includes a porous substrate (not shown) and an inner layer solid electrolyte composition (not shown) filled in the porous substrate. The inner layer 31 may be composed only of a porous substrate filled with the inner layer solid electrolyte composition. The inner layer solid electrolyte composition contains a solid electrolyte material and a binder. The inner layer solid electrolyte composition may be composed only of a solid electrolyte material and a binder.

[0044] The first outer layer 32 includes a first outer layer solid electrolyte composition containing a solid electrolyte material and a binder. The first outer layer 32 may be composed of only the first outer layer solid electrolyte composition. The second outer layer 33 includes a second outer layer solid electrolyte composition containing a solid electrolyte material and a binder. The second outer layer 33 may be composed of only the second outer layer solid electrolyte composition. The first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition may be composed of only the solid electrolyte material and a binder. The first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition may be the same.

[0045] The porous substrate included in the inner layer 31 is preferably a woven fabric or a nonwoven fabric. Woven fabric or nonwoven fabric has a suitable porosity and thickness, and is easily filled with the inner layer solid electrolyte composition. The material of the porous substrate is not particularly limited, and may be any material that can form a self-supporting sheet. Examples of the material include polyethylene terephthalate (PET), polyamide (nylon), aromatic polyamide (aramid), Al2O3, glass, and the like. The porous substrate is preferably made of heat-resistant fibers. By forming the porous substrate from heat-resistant fibers, it is possible to suppress short circuits even when pressing is performed at a high temperature exceeding 200°C in the manufacturing process of the all-solid-state battery 1. In addition, the solid electrolyte layer 30 can be sintered by high-temperature pressing, and as a result, the interface resistance is reduced and the output of the battery can be improved. The porosity of the porous substrate may be within a range of 65 to 90%. By having the porosity within this range, it is easy to fill the inner layer solid electrolyte composition inside the porous substrate.

[0046] The solid electrolyte materials and the substances used as binders in the inner layer solid electrolyte composition contained in the inner layer 31, the first outer layer solid electrolyte composition contained in the first outer layer 32, and the second outer layer solid electrolyte composition contained in the second outer layer 33 may be the same. By using the same substances, the adhesion between the inner layer 31 and the first outer layer 32 and second outer layer 33 is increased.

[0047] The solid electrolyte material is not particularly limited as long as it is capable of conducting lithium ions between the positive electrode 10 and the negative electrode 20. For example, oxide-based electrolytes and sulfide-based electrolytes can be used as the solid electrolyte material. The solid electrolyte material preferably contains lithium element. Among them, a material containing at least lithium sulfide as the first component and synthesized from one or more compounds selected from the group consisting of silicon sulfide, phosphorus sulfide, and boron sulfide as the second component is preferable, and Li2S-P2S5 is particularly preferable from the viewpoint of lithium ion conductivity.

[0048] When the solid electrolyte material is a sulfide-based electrolyte, it may further contain sulfides such as SiS2, GeS2, B2S3, etc. In addition, Li3PO4, halogens, halogen compounds, etc. may be added to the solid electrolyte as appropriate.

[0049] In the case where the solid electrolyte material is a lithium ion conductor made of an inorganic compound, for example, Li3N, LISICON, LIPON (Li 3+y PO 4-x N x ), Thio-LISICON (Li 3.25 Ge 0.25 P 0.75 S4), Li2O-Al2O3-TiO2-P2O5 (LATP), etc.

[0050] The solid electrolyte material may have an amorphous, glassy, ​​crystalline (crystallized glass) structure, etc. When the solid electrolyte material is a sulfide-based solid electrolyte made of Li2S-P2S5, the lithium ion conductivity of the amorphous body is 10 -4 Scm -1 On the other hand, the lithium ion conductivity of the crystalline material is about 10 -3 Scm -1 That's about it.

[0051] The solid electrolyte material preferably contains at least one of phosphorus and sulfur, which can improve the lithium ion conductivity of the resulting all-solid-state battery 1.

[0052] The binder is capable of adhering to the porous substrate of the inner layer 31, the positive electrode 10, and the negative electrode 20, and also capable of adhering the solid electrolyte material. As the binder, for example, one containing an adhesive resin exhibiting adhesiveness is preferable. As the binder, for example, a fluorine-based polymer, a (meth)acrylic thermoplastic resin, a silicone resin, a urethane resin, a nitrile resin, a polyester resin, a cellulose resin, a styrene resin, a styrene butadiene resin, a vinyl acetate resin, a fluoroethylene resin, a polyvinyl ether, a rubber, etc. are listed. It should be noted that "(meth)acrylic" is a general term for acrylic and methacrylic.

[0053] The inner layer solid electrolyte composition contained in the inner layer 31 of the solid electrolyte layer 30 has a higher binder content than the first outer layer solid electrolyte composition contained in the first outer layer 32 and the second outer layer solid electrolyte composition contained in the second outer layer 33. Since the inner layer solid electrolyte composition has a high binder content, it has high adhesion to the porous substrate. Thus, the strength of the solid electrolyte layer 30 is improved. On the other hand, since the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition have a low binder content, the ion conductivity of the first outer layer 32 and the second outer layer 33 is improved. Therefore, according to the all-solid-state battery 1 of this embodiment, it is possible to achieve both improvement in the strength of the solid electrolyte layer 30 and improvement in lithium ion conductivity by containing a porous substrate.

[0054] The binder content of the inner layer solid electrolyte composition is not particularly limited, but may be within a range of 3 to 20 mass%. The binder contents of the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition are not particularly limited, but may be within a range of 1 / 10 to 9 / 10, or may be within a range of 3 / 10 to 6 / 10, of the binder content of the inner layer solid electrolyte composition. When the binder contents of the inner layer solid electrolyte composition, the first outer layer solid electrolyte composition, and the second outer layer solid electrolyte composition are within the above ranges, the strength and lithium ion conductivity of the solid electrolyte layer 30 are improved in a more balanced manner. From the viewpoint of improving the lithium ion conductivity of the solid electrolyte layer 30, the binder content of the inner layer solid electrolyte composition may be within a range of 3 to 8 mass%. From the viewpoint of improving the strength of the solid electrolyte layer 30, the binder content of the inner layer solid electrolyte composition may be within a range of 10 to 20 mass%.

[0055] In this embodiment, the average particle diameter of the solid electrolyte material contained in the inner layer solid electrolyte composition is smaller than the average particle diameter of the solid electrolyte material contained in the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition. A solid electrolyte material having a small average particle diameter can be easily filled into a porous substrate because a large number of particles can be filled per unit volume. Therefore, by reducing the average particle diameter of the solid electrolyte material contained in the inner layer solid electrolyte composition, the solid electrolyte material can be densely filled into the porous substrate of the inner layer 31. On the other hand, the number of contact points between particles per unit volume increases, so that the lithium ion conductivity tends to be poor. Therefore, by increasing the average particle diameter of the solid electrolyte material contained in the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition, the ion conductivity of the first outer layer 32 and the second outer layer 33 is improved. The average particle diameter of the solid electrolyte material contained in the inner layer solid electrolyte composition may be in the range of 0.5 to 1.5 μm, or may be in the range of 0.5 to 1.0 μm. The average particle size of the solid electrolyte material contained in the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition may be in the range of 2.0 to 10.0 μm, or may be in the range of 2.0 to 5.0 μm. The particle size of the solid electrolyte material is the longest diameter of the solid electrolyte material measured from a cross-sectional SEM photograph of the cross section of the solid electrolyte layer 30 taken with a SEM (scanning electron microscope), and the average particle size is the number average value.

[0056] The particle size distribution of the solid electrolyte material contained in the inner layer solid electrolyte composition may have a peak in a region where the particle diameter is 1 μm or less. The particle size distribution may be based on the number of the longest diameter of the solid electrolyte material measured from a cross-sectional SEM photograph of the solid electrolyte layer 30. In this case, the inner layer solid electrolyte composition contains many solid electrolyte material fine particles having a particle diameter of 1 μm or less, so that the porous substrate of the inner layer 31 is easily filled with the solid electrolyte material. This improves the strength of the solid electrolyte layer 30. The particle size distribution of the solid electrolyte material contained in the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition may have a peak in a region where the particle diameter is 1 μm or less and a region where the particle diameter is 3 μm or more. In this case, the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition contain solid electrolyte material fine particles having a particle diameter of 1 μm or less and solid electrolyte material coarse particles having a particle diameter of 3 μm or more, so that the first outer layer 32 and the second outer layer 33 tend to be dense due to the fine particles being interposed between the coarse particles. This improves the lithium ion conductivity of the solid electrolyte layer 30. The upper limit of the particle size of the solid electrolyte material contained in the first outer layer 32 and the second outer layer 33 is equal to or less than the thickness of the first outer layer 32 and the second outer layer 33 .

[0057] The all-solid-state battery 1 can be manufactured, for example, by placing a first outer layer 32 of a solid electrolyte sheet (solid electrolyte layer 30) in which a first outer layer 32, an inner layer 31, and a second outer layer 33 are laminated in this order on a positive electrode layer 11 of a positive electrode sheet (positive electrode 10) in which a positive electrode layer 11 and a positive electrode current collector 12 are laminated, and then placing a negative electrode layer 21 of a negative electrode sheet (negative electrode 20) in which a negative electrode layer 21 and a negative electrode current collector 22 are laminated on the solid electrolyte sheet, and then performing press bonding. As the press bonding, high-temperature press bonding exceeding 200°C may be performed.

[0058] The solid electrolyte sheet can be produced by the following methods (1) to (3) using, for example, a porous substrate, an inner layer forming slurry for forming the inner layer 31, and an outer layer forming slurry for forming the first outer layer and the second outer layer. The inner layer forming slurry and the outer layer forming slurry each contain a solvent, a solid electrolyte, and a binder. The inner layer forming slurry has a higher binder content than the outer layer forming slurry.

[0059] (1) Impregnation (dip) method The porous substrate is impregnated with an inner layer forming slurry, and then the porous substrate is pulled out of the inner layer forming slurry and dried to form an inner layer member having a porous substrate (inner layer 31) filled with an inner layer solid electrolyte composition. Next, the obtained inner layer member is impregnated with an outer layer forming slurry, and then the inner layer member is pulled out of the outer layer forming slurry and dried to form outer layers (first outer layer 32, second outer layer 33) on both sides of the inner layer 31 of the inner layer member.

[0060] (2) Coating method The outer layer forming slurry is applied onto the support sheet and dried to form the first outer layer 32. Next, the inner layer forming slurry is applied onto the first outer layer 32, and then a porous substrate is placed on the coating layer of the inner layer forming slurry, and the coating layer is absorbed into the porous substrate, followed by drying to form a porous substrate (inner layer 31) filled with the inner layer solid electrolyte composition. Next, the outer layer forming slurry is applied onto the inner layer 31 and dried to form the second outer layer 33. For example, an aluminum foil or a stainless steel foil can be used as the support sheet. For example, a die coater method can be used as a method for applying the outer layer forming slurry and the inner layer forming slurry.

[0061] (3) Transfer method An inner layer sheet having an inner layer 31 in which an inner layer solid electrolyte composition is filled on a porous substrate is prepared. Also, an outer layer transfer sheet in which a peelable outer layer (first outer layer 32, second outer layer 33) is formed on a support sheet is prepared. The inner layer sheet can be obtained, for example, by impregnating a porous substrate with a slurry for forming an inner layer, then pulling the porous substrate out of the slurry for forming an inner layer, and then drying it, or by applying a slurry for forming an inner layer to a porous substrate, and then drying it. The outer layer transfer sheet can be obtained, for example, by applying a slurry for forming an outer layer on a support sheet, and then drying it. For example, an aluminum foil or a stainless steel foil can be used as the support sheet. The outer layer surfaces of the outer layer transfer sheet are placed on both side surfaces of the inner layer sheet, and the outer layers (first outer layer 32, second outer layer 33) are transferred and integrated onto both sides of the inner layer 31 by pressing, and then the support sheet is peeled off and removed.

[0062] The impregnation method (1) is easier to reduce the amount of binder than the coating method (2) and the transfer method (3). On the other hand, the coating method (2) and the transfer method (3) are easier to adjust the thickness of the outer layer (first outer layer 32, second outer layer 33) than the impregnation method (1).

[0063] In the solid electrolyte layer 30 used in the all-solid-state battery 1 according to this embodiment, the inner layer solid electrolyte composition contained in the inner layer 31 has a high binder content and has high adhesion to the porous substrate of the inner layer 31, so that cracks are unlikely to occur. On the other hand, the first outer layer solid electrolyte composition contained in the first outer layer 32 and the second outer layer solid electrolyte composition contained in the second outer layer 33 have a low binder content, so that ion conductivity is improved. In addition, the inner layer solid electrolyte composition has a small average particle diameter of the solid electrolyte material, so that it is easy to fill the porous substrate of the inner layer 31 and is filled at a high density, so that the strength of the solid electrolyte layer 30 and the effect of suppressing the occurrence of cracks are improved. Furthermore, the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition have a large average particle diameter of the solid electrolyte material, so that the lithium ion conductivity of the solid electrolyte layer 30 is improved. Therefore, the solid electrolyte layer 30 has improved strength, suppressed the occurrence of cracks, and improved ion conductivity. Furthermore, since the all-solid-state battery 1 according to this embodiment has the above-mentioned solid electrolyte layer 30, the stability and charge / discharge efficiency are improved over a long period of time.

[0064] Although the specific embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and even if modifications and improvements are made within the scope of the present invention, they are included in the scope of the present invention. For example, in this embodiment, as a method for manufacturing the all-solid-state battery 1, a method for integrally pressing and bonding a laminate in which each layer is arranged in order is exemplified, but the method for manufacturing the all-solid-state battery 1 is not limited to this. For example, the all-solid-state battery 1 may be manufactured as follows. First, the positive electrode layer 11 of the positive electrode sheet in which the positive electrode layer 11 and the positive electrode current collector 12 are laminated and the first outer layer sheet are press-bonded to prepare a positive electrode-first outer layer laminate sheet, and the negative electrode layer 21 of the negative electrode sheet in which the negative electrode layer 21 and the negative electrode current collector 22 are laminated and the second outer layer sheet are press-bonded to prepare a negative electrode-second outer layer laminate sheet. Next, an inner layer sheet is prepared, and the first outer layer 32 of the positive electrode-first outer layer laminate sheet is press-bonded to one surface of the inner layer sheet, and the second outer layer 33 of the negative electrode-second outer layer laminate sheet is press-bonded to the other surface of the inner layer sheet. In this way, an electrode laminate sheet is obtained in which a positive electrode sheet, a solid electrolyte sheet, and a negative electrode sheet are laminated in this order. The inner layer solid electrolyte composition of the inner layer sheet may have a binder content in the range of 10 to 20 mass %. The average particle size of the solid electrolyte contained in the inner layer solid electrolyte composition may be in the range of 0.5 to 1.0 μm. The thickness of the inner layer sheet may be in the range of 5 to 15 μm. The outer layer solid electrolyte compositions of the first outer layer sheet and the second outer layer sheet may have a binder content in the range of 5 to 20 mass %. The average particle size of the solid electrolyte contained in the outer layer solid electrolyte composition may be in the range of 2.0 to 5.0 μm. The thickness of the first outer layer sheet and the second outer layer sheet may be in the range of 5 to 20 μm. EXAMPLES

[0065] [Example 1] (Preparation of solid electrolyte sheet) A slurry for forming an inner layer was prepared by adding 51 parts by mass of fine powder of sulfide-based solid electrolyte (average particle size: 0.7 μm) and 3 parts by mass of SBR (styrene butadiene rubber)-based binder to 46 parts by mass of solvent and mixing them. A slurry for forming an outer layer was prepared by adding 10.5 parts by mass of fine powder of sulfide-based solid electrolyte (average particle size: 0.7 μm), 41.9 parts by mass of coarse powder of sulfide-based solid electrolyte (average particle size: 3.0 μm), and 1.6 parts by mass of SBR-based binder to 46 parts by mass of solvent and mixing them.

[0066] A nonwoven fabric (material: PET, thickness: 10 μm, porosity: 75%, average fiber diameter: 3.0 μm) was immersed in the inner layer forming slurry, pulled out from the inner layer forming slurry, and then dried. In this way, an inner layer member was produced in which the nonwoven fabric was filled with an inner layer solid electrolyte composition containing fine particles of a sulfide-based solid electrolyte and a binder. The thickness of the obtained inner layer member was 30 μm. The obtained inner layer member was immersed in the outer layer forming slurry, pulled out from the outer layer forming slurry, and then dried. In this way, a three-layered solid electrolyte sheet was produced in which outer layers (thickness: 20 μm) containing an outer layer composition containing fine and coarse powders of a sulfide-based solid electrolyte and a binder were laminated on both surfaces of the inner layer.

[0067] The cross section of the obtained solid electrolyte sheet was observed using a scanning electron microscope (SEM). Fig. 2 shows a cross-sectional SEM photograph of the inner layer of the solid electrolyte sheet, and Fig. 3 shows a cross-sectional SEM photograph of the first outer layer of the solid electrolyte sheet layer. From the cross-sectional SEM photograph of Fig. 2, it was confirmed that in the inner layer 31, sulfide-based solid electrolyte fine particles 301 are closely adhered to the periphery of the PET fibers 311 of the nonwoven fabric, and the sulfide-based solid electrolyte fine particles 301 are densely packed inside the nonwoven fabric. From the cross-sectional SEM photograph of Fig. 3, it was confirmed that in the first outer layer 32, the sulfide-based solid electrolyte layer is formed by the sulfide-based solid electrolyte fine particles 301 being interposed between the sulfide-based solid electrolyte coarse particles 302.

[0068] [Example 2] A sulfide-based solid electrolyte fine powder (average particle size: 0.7 μm) and an SBR-based binder were mixed in a solvent at a ratio such that the content of the SBR-based binder in the solid content was 3 mass % to prepare an inner layer forming slurry. A nonwoven fabric (material: PET, thickness: 10 μm, porosity: 75%, average fiber diameter: 3.0 μm) was immersed in the inner layer forming slurry, and then pulled out of the inner layer forming slurry to allow the inner layer forming slurry to adhere to the nonwoven fabric, followed by drying to obtain an inner layer member having a thickness of 30 μm.

[0069] A sulfide-based solid electrolyte coarse powder (average particle size: 3.0 μm) and an SBR-based binder were mixed in a solvent at a ratio such that the content of the SBR-based binder in the solid content was 1.6 mass % to prepare a slurry for forming an outer layer. An inner layer member was immersed in this slurry for forming an outer layer, and then pulled out of the slurry for forming an inner layer. The slurry for forming an outer layer was adhered to the inner layer member, and then dried to produce a solid electrolyte sheet having an inner layer thickness of 30 μm and first and second outer layers each having a thickness of 20 μm.

[0070] [Examples 3 and 4] A solid electrolyte sheet was produced in the same manner as in Example 2, except that the inner layer forming slurry and the outer layer forming slurry were applied so that the inner layer had a thickness as shown in Table 1 below.

[0071] [Comparative Example 1] A solid electrolyte sheet was produced in the same manner as in Example 2, except that the inner layer forming slurry was a slurry containing a coarse powder (average particle size: 3.0 μm) of a sulfide-based solid electrolyte and an SBR-based binder in such a ratio that the content of the SBR-based binder in the solid content was 1.6 mass% (used as the outer layer forming slurry in Example 2), and the outer layer forming slurry was a slurry containing a fine powder (average particle size: 0.7 μm) of a sulfide-based solid electrolyte and an SBR-based binder in such a ratio that the content of the SBR-based binder in the solid content was 3.0 mass% (used as the inner layer forming slurry in Example 2).

[0072] [evaluation] (1) Cross-section observation The cross sections of the solid electrolyte sheets obtained in Examples 1 to 3 were observed using an SEM. As a result, it was confirmed that the inside of the nonwoven fabric of the inner layer was densely filled with sulfide-based solid electrolyte fine particles. It was also confirmed that the first outer layer had a layer of sulfide-based solid electrolyte formed by the presence of sulfide-based solid electrolyte fine particles 301 between sulfide-based solid electrolyte coarse particles 302.

[0073] (2) Performance evaluation of all-solid-state battery cells Using each of the above solid electrolyte sheets, an all-solid-state battery cell was fabricated according to the following procedure.

[0074] [Preparation of positive electrode sheet] An aluminum foil with a thickness of 12.0 μm was prepared as a positive electrode current collector. 60.0 parts by mass of lithium nickel cobalt manganese composite oxide (NCM622) was used as a positive electrode active material, 35.8 parts by mass of a sulfide solid electrolyte was used as a solid electrolyte, 2.9 parts by mass of acetylene black (DENKA BLACK Li-100, manufactured by Denka Co., Ltd.) was used as a conductive additive, and 1.3 parts by mass of an SBR (styrene butadiene rubber) binder was used. The mixture was dispersed in a solvent to prepare a positive electrode active material slurry. The obtained positive electrode active material slurry was applied to both sides of a positive electrode current collector so that the basis weight after drying was 27.4 mg / cm. 2 The mixture was applied using a bar coater so as to obtain a positive electrode layer, which was then dried to prepare a positive electrode sheet.

[0075] [Preparation of negative electrode sheet] A copper foil with a thickness of 10 μm was prepared as a negative electrode current collector, and a metallic lithium foil with a thickness of 6.5 μm was laminated on the surface of the copper foil as a negative electrode layer to prepare a negative electrode sheet.

[0076] [Fabrication of all-solid-state battery cells] The positive electrode sheet, the solid electrolyte sheet, and the negative electrode sheet obtained above were cut into a size of 120 mm x 30 mm, and the positive electrode piece, the solid electrolyte piece, and the negative electrode piece obtained were stacked and press-bonded to prepare an electrode laminate. An all-solid-state battery cell was produced using the obtained electrode laminate.

[0077] [Cell charge / discharge test] Using the all-solid-state battery cell obtained as described above, a charge / discharge test was performed in the range of 2.65 to 4.3 V. The cells in which the second charge / discharge capacity was 95% or more of the first charge / discharge capacity were marked with "○". The cells in which the second charge / discharge capacity was less than 95% were marked with "×". The results are shown in Table 1.

[0078] [Cell resistance] After the above charge / discharge test, the all-solid-state battery cell was charged to a SOC (state of charge) of 50%, and the cell resistance was measured. The results are shown in Table 1.

[0079] [Table 1]

[0080] From the results in Table 1, it can be seen that the all-solid-state battery cells using the solid electrolyte sheets of Examples 2 to 4, in which the binder content and the average particle size of the solid electrolyte material are within the ranges of the present invention, have high charge / discharge efficiency and low cell resistance in the second cycle. In particular, it can be seen that the all-solid-state battery cells using the solid electrolyte sheets of Examples 3 to 4, in which the thickness of the inner layer is 25 μm or less and the thicknesses of the first outer layer and the second outer layer are 7 μm or less, have a further reduced cell resistance. On the other hand, the all-solid-state battery cell using the solid electrolyte sheet of Comparative Example 1, in which the binder content of the inner layer solid electrolyte composition is low and the average particle size of the solid electrolyte material contained in the inner layer solid electrolyte composition is large, was short-circuited at the time of the second cycle and was unable to charge / discharge.

[0081] [Example 5] As the first and second outer layer sheets, 7 μm-thick sheets containing a sulfide-based solid electrolyte coarse powder (average particle size: 3.0 μm) and an SBR binder with an SBR binder content of 5.0 mass% were prepared. As the inner layer sheet, a 10 μm-thick sheet containing a sulfide-based solid electrolyte fine powder (average particle size: 0.7 μm) and an SBR binder with an SBR binder content of 10 mass% was prepared.

[0082] The positive electrode layer of the positive electrode sheet prepared in the performance evaluation of the all-solid-state battery cell was press-bonded to the first outer layer sheet to prepare a positive electrode-first outer layer laminate sheet. Similarly, the negative electrode layer 21 of the negative electrode sheet prepared in the performance evaluation of the all-solid-state battery cell was press-bonded to the second outer layer sheet to prepare a negative electrode-second outer layer laminate sheet. Next, the first outer layer of the positive electrode-first outer layer laminate sheet was bonded to one surface of the inner layer sheet, and the second outer layer of the negative electrode-second outer layer laminate sheet was bonded to the other surface of the inner layer sheet to obtain an electrode laminate sheet in which the positive electrode sheet, the solid electrolyte sheet, and the negative electrode sheet were laminated in this order. The obtained electrode laminate sheet was cut to a size of 120 mm x 30 mm, and the obtained electrode laminate was used to prepare an all-solid-state battery cell.

[0083] [Example 6, Comparative Examples 2 to 3] An all-solid-state battery cell was produced in the same manner as in Example 5, except that, as the first outer layer sheet and the second outer layer sheet, sheets containing a sulfide-based solid electrolyte having an average particle size shown in Table 2 below and an SBR-based binder in a ratio such that the content of the SBR-based binder is the value shown in Table 2 below were used, and as the inner layer sheet, sheets containing a sulfide-based solid electrolyte having an average particle size shown in Table 2 below and an SBR-based binder in a ratio such that the content of the SBR-based binder is the value shown in Table 2 below were used.

[0084] [evaluation] The all-solid-state battery cells obtained in Examples 5 and 6 and Comparative Examples 2 and 3 were evaluated in the same manner as in the performance evaluation of the all-solid-state battery cells described above. The results are shown in Table 2 below.

[0085] [Table 2]

[0086] From the results in Table 2, it can be seen that the all-solid-state battery cells using the solid electrolyte sheets of Examples 5 and 6, in which the binder content and the average particle size of the solid electrolyte material are within the ranges of the present invention, have high charge / discharge efficiency and low cell resistance in the second cycle. On the other hand, the all-solid-state battery cells using the solid electrolyte sheets of Comparative Examples 2 and 3, in which the binder content of the inner layer solid electrolyte composition is low and the average particle size of the solid electrolyte material contained in the inner layer solid electrolyte composition is large, have high charge / discharge efficiency in the second cycle but high cell resistance. [Explanation of symbols]

[0087] 1 All-solid-state battery 10 positive electrode 11 Positive electrode layer 12 Positive electrode current collector 20 negative electrode 21 Negative electrode layer 22 Negative electrode current collector 30 Solid electrolyte layer 31 Inner layer 32 1st outer layer 33 Second outer layer 301 Sulfide solid electrolyte fine particles 302 Sulfide solid electrolyte coarse particles 311 Nonwoven PET fiber

Claims

1. The insulating sheet has an inner layer, a first outer layer laminated on one surface of the inner layer, and a second outer layer laminated on the other surface of the inner layer, the inner layer includes a porous substrate and an inner layer solid electrolyte composition filled in the porous substrate, the inner layer solid electrolyte composition containing a solid electrolyte material and a binder, the first outer layer includes a first outer layer solid electrolyte composition containing a solid electrolyte material and a binder, the second outer layer includes a second outer layer solid electrolyte composition containing a solid electrolyte material and a binder, the inner layer solid electrolyte composition has a higher binder content than the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition, a mean particle size of a solid electrolyte material contained in the inner layer solid electrolyte composition is smaller than mean particle sizes of solid electrolyte materials contained in the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition.

2. 2. The solid electrolyte sheet according to claim 1, wherein a binder content of the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition is within a range of 1 / 10 to 9 / 10 of a binder content of the inner layer solid electrolyte composition.

3. 3. The solid electrolyte sheet according to claim 2, wherein a binder content of the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition is within a range of 3 / 10 to 6 / 10 of a binder content of the inner layer solid electrolyte composition.

4. 2. The solid electrolyte sheet according to claim 1, wherein the binder content of the inner layer solid electrolyte composition is within a range of 3 to 20 mass %.

5. 5. The solid electrolyte sheet according to claim 4, wherein the binder content of the inner layer solid electrolyte composition is in the range of 3 to 9 mass %.

6. The solid electrolyte sheet according to claim 5, wherein the inner layer has a thickness in the range of 10 to 25 μm.

7. 5. The solid electrolyte sheet according to claim 4, wherein the binder content of the inner layer solid electrolyte composition is in the range of 10 to 20 mass %.

8. 2. The solid electrolyte sheet according to claim 1, wherein a particle size distribution peak of the solid electrolyte material contained in the inner layer solid electrolyte composition is in a region where the particle size is 1 μm or less, and a particle size distribution peak of the solid electrolyte materials contained in the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition is in a region where the particle size is 1 μm or less and a region where the particle size is 3 μm or more.

9. 2. The solid electrolyte sheet according to claim 1, wherein the thickness of the inner layer is within a range of 2 to 30 μm, and the thicknesses of the first outer layer and the second outer layer are within a range of 1 / 5 to 2 times the thickness of the inner layer.

10. The solid electrolyte sheet according to claim 9 , wherein the first outer layer and the second outer layer have a thickness less than a thickness of the inner layer.

11. The solid electrolyte sheet according to claim 10, wherein the thickness of the first outer layer and the second outer layer is within a range of 1 / 5 to 4 / 5 times the thickness of the inner layer.

12. The solid electrolyte sheet according to claim 9, wherein the thickness of the inner layer is in the range of 10 to 25 μm.

13. An all-solid-state battery comprising a positive electrode, a negative electrode, and a solid electrolyte layer disposed between the positive electrode and the negative electrode, The solid electrolyte layer is made of the solid electrolyte sheet according to any one of claims 1 to 5, and is disposed at a position where the first outer layer is in contact with the positive electrode and the second outer layer is in contact with the negative electrode.

Citation Information

Patent Citations

  • Solid electrolyte sheet, all-solid lithium ion battery, and method of manufacturing solid electrolyte sheet