Multilayer film and vessel
A multilayer film with a high storage modulus and specific layer composition addresses hole formation issues in thermal welding to three-dimensional paper bases, enhancing film integrity and suitability for microwaveable food containers.
Patent Information
- Application Number
- JP2023060391
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2024-10-16
AI Technical Summary
Existing multilayer films thermally welded to three-dimensionally formed paper base materials are prone to hole formation due to high temperatures during the welding process.
A multilayer film design with a high storage modulus of 0.3 MPa or more at 150°C, comprising a polyethylene resin ratio of 60% or more, and including layers such as an outer polyethylene layer, an inner layer for welding to paper, and an intermediate oxygen barrier layer, is used to suppress hole formation.
The high storage modulus and layer composition reduce hole formation and thermal shrinkage, ensuring the integrity of the welded film and container, particularly suitable for microwaveable food packaging.
Smart Images

Figure 2024147404000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a multilayer film and a container that can be heat-sealed to a paper substrate that has been previously formed into a three-dimensional shape. [Background technology]
[0002] There is known a multilayer film that is adhered to a three-dimensionally preformed paper substrate. For example, Patent Document 1 discloses a laminate film for paper containers that is adhered to paper containers. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-146996 A Summary of the Invention [Problem to be solved by the invention]
[0004] In the technology disclosed in Patent Document 1, a multilayer film is heated and bonded to a paper cup, which is a paper substrate that has been previously formed into a three-dimensional shape. Here, the paper substrate that has been previously formed into a three-dimensional shape may have a portion where the substrate is interrupted, for example, due to forming a flat substrate into a three-dimensional shape. The portion where the substrate is interrupted is sealed by heat-sealing the multilayer film. However, there is a problem in that the higher the temperature during heat-sealing, the more likely holes are to occur in the multilayer film at the portion where the substrate is interrupted.
[0005] It is therefore desirable to develop a multilayer film that is less likely to develop holes when heat-welded to a substrate that has been previously formed into a three-dimensional shape. [Means for solving the problem]
[0006] As a result of extensive research, the present inventors have found that increasing the storage modulus at high temperatures can suppress the formation of holes in a multilayer film when the multilayer film is heat-welded to a substrate that has been previously formed into a three-dimensional shape. The present invention was made based on this finding.
[0007] The multilayer film according to the present disclosure comprises a first layer which is an outer layer capable of adhering to a polyethylene-based resin material, and a second layer which is an inner layer which can be heat-sealed to a paper substrate which has been previously formed into a three-dimensional shape, the ratio of polyethylene-based resin being 60% by weight or more, and the film is characterized in that, in dynamic viscoelasticity measurement in a tensile mode in the MD direction, the film has a storage modulus of 0.3 MPa or more at a measurement temperature of 150°C.
[0008] In addition, the container according to the present disclosure is characterized in that it comprises a substrate made of paper that has been three-dimensionally formed in advance, and the above-mentioned multilayer film, and the multilayer film is heat-welded to the substrate.
[0009] According to these configurations, the storage modulus of the multilayer film at a measurement temperature of 150°C is 0.3 MPa or more, so that when the multilayer film is heat-welded to a pre-formed three-dimensional paper substrate, the occurrence of holes at the points where the substrate is interrupted can be suppressed.
[0010] Preferred embodiments of the present invention will be described below. However, the scope of the present invention is not limited to the preferred embodiments described below.
[0011] In one embodiment, the multilayer film preferably has a storage modulus of 4 MPa or less at a measurement temperature of 150° C. in the dynamic viscoelasticity measurement.
[0012] In one embodiment, the multilayer film preferably has an overall thickness of 80 μm or more and 180 μm or less.
[0013] In one embodiment, the multilayer film preferably includes a first functional layer between the first layer and the second layer.
[0014] In one embodiment of the multilayer film, the first functional layer is preferably a polyethylene resin having a polar group.
[0015] In one embodiment of the multilayer film, the polyethylene resin having a polar group is preferably an ionomer.
[0016] In one embodiment, the multilayer film preferably includes an intermediate layer between the first layer and the second layer, the intermediate layer being an oxygen barrier layer.
[0017] In one embodiment of the multilayer film, the intermediate layer preferably contains an ethylene-vinyl alcohol copolymer.
[0018] In one embodiment of the multilayer film, the second layer preferably contains an ethylene-vinyl acetate copolymer.
[0019] In one embodiment, the multilayer film is preferably irradiated with an electron beam at an exposure dose of 20 kGy to 300 kGy.
[0020] In one aspect, the container is preferably microwave-reheat-resistant.
[0021] Further features and advantages of the present invention will become more apparent from the following description of exemplary and non-limiting embodiments, which are given with reference to the drawings. [Brief description of the drawings]
[0022] [Figure 1] Schematic cross-sectional view showing the layer structure of a multilayer film [Diagram 2] Schematic cross-sectional view showing the configuration of the container [Diagram 3] Trends in hole occurrence rates [Figure 4] FIG. 1 is a flow chart showing a method for manufacturing a container. [Diagram 5] Graph showing the results of storage modulus measurement DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Hereinafter, a multilayer film 10 according to an embodiment will be described with reference to the drawings. FIG. 1 is a schematic cross-sectional view showing the layer structure of the multilayer film 10. FIG. 2 is a schematic cross-sectional view showing the structure of a container 20. The multilayer film 10 includes a first layer 11, which is an outer layer that can be adhered to a polyethylene-based resin material, and a second layer 17, which is an inner layer that can be adhered to paper. In this embodiment, the multilayer film 10 includes the first layer 11 provided on the first surface side, an intermediate layer 14, and the second layer 17 provided on the second surface side, in the order listed. The second layer 17 of the multilayer film 10 is heat-welded to a paper substrate 21 that has been previously formed three-dimensionally to form the container 20.
[0024] Here, the term "polyethylene resin material" refers to a member containing a polyethylene resin. Examples of polyethylene resin materials include films and lids made of polyethylene resin. The term "polyethylene resin" refers to a polymer containing at least ethylene as a monomer unit. Examples of "polyethylene resin" include high-density polyethylene resin, medium-density polyethylene resin, low-density polyethylene resin, linear low-density polyethylene resin, modified polyethylene resin, ethylene-vinyl acetate resin (e.g., ethylene-vinyl acetate copolymer, etc.), ethylene-vinyl alcohol resin (e.g., ethylene-vinyl alcohol copolymer, etc.), ethylene-methyl acrylate resin (e.g., ethylene-methyl acrylate copolymer, etc.), ethylene-methacrylic acid resin (e.g., ethylene-methacrylic acid copolymer, etc.), ethylene-aliphatic unsaturated carboxylic acid resin, ethylene-aliphatic unsaturated carboxylic acid ester resin, ionomer resin, etc.
[0025] Examples of the "modified polyethylene resin" include polyethylene, ethylene-unsaturated carboxylic acid copolymer, and ethylene-methyl methacrylate copolymer.
[0026] Moreover, the term "polyolefin resin" refers to a polymer containing units derived from olefin. Examples of "polyolefin resin" include homopolymers of olefins such as polyethylene, polypropylene, polybutene, and poly-4-methylpentene, copolymers of two or more olefins, and copolymers of one or more olefins with different components other than olefins.
[0027] Moreover, the term "polypropylene-based resin" refers to a polymer that contains at least propylene as a monomer unit. Examples of the "polypropylene-based resin" include homopolypropylene, block polypropylene, and random polypropylene.
[0028] Examples of "modified polypropylene resins" include modified polymers obtained by graft-copolymerizing unsaturated carboxylic acids such as maleic acid and fumaric acid or their acid anhydrides onto polypropylene resins such as polypropylene, propylene-α-olefin copolymers, and terpolymers of propylene, ethylene, and α-olefins.
[0029] The abbreviations for resin names in this embodiment are shown below. PE: Polyethylene HDPE: High density polyethylene MDPE: Medium Density Polyethylene LDPE: Low density polyethylene LLDPE: Linear low density polyethylene ION: Ionomer EVA: Ethylene-vinyl acetate copolymer EVOH: Ethylene-vinyl alcohol copolymer EMA: Ethylene-methyl acrylate copolymer EMAA: Ethylene-methacrylic acid copolymer MAA: Methyl methacrylate PET: Polyethylene terephthalate PO: Polyolefin PP: Polypropylene NY: Nylon
[0030] In this embodiment, the multilayer film 10 includes an intermediate layer 14 between the first layer 11 and the second layer 17. The multilayer film 10 also includes a first functional layer 12 and a second functional layer 16 between the first layer 11 and the second layer 17. In the illustrated example, the multilayer film 10 includes, in order from the first layer 11 side, which is the outermost layer, the first functional layer 12, the intermediate layer 14, the second functional layer 16, and the second layer 17.
[0031] The first layer 11 is an outer layer that can be bonded to a polyethylene-based resin material. In this embodiment, the first layer 11 is a layer that is in direct contact with the contents of the container 20 and is preferably made of various thermoplastic resins. The first layer 11 is made of, for example, a polyolefin-based resin, a polyethylene-based resin, a polypropylene-based resin, a polyamide-based resin, a polyester-based resin, a polycarbonate-based resin, a polystyrene-based resin, a thermoplastic elastomer, or the like.
[0032] The first layer 11 desirably contains a polyethylene-based resin. The first layer 11 may contain only one type of polyethylene-based resin, or may contain two or more types of polyethylene-based resin. The first layer 11 preferably contains 60% by mass or more of the polyethylene-based resin. More preferably, the first layer 11 contains 70% by mass or more of the polyethylene-based resin. Even more preferably, the first layer 11 contains 80% by mass or more of the polyethylene-based resin.
[0033] When the first layer 11 contains a polyethylene resin, the crosslink density of the first layer 11 can be improved by irradiating the multilayer film 10 with an electron beam from the first layer 11 side. The polyethylene contained in the first layer 11 is preferably low-density polyethylene (LDPE), and more preferably linear low-density polyethylene (LLDPE). In this way, the crosslink density of the first layer 11 can be further improved when the multilayer film 10 is irradiated with an electron beam from the first layer 11 side.
[0034] The second layer 17 is a layer that can be thermally welded to the paper substrate 21 that has been three-dimensionally formed in advance. The second layer 17 can be made of a known resin layer that exhibits a certain degree of thermal weldability. The second layer 17 is not particularly limited, but specifically can be made of, for example, a polyethylene resin, an ionomer resin, an ethylene copolymer (such as an ethylene-vinyl acetate copolymer), or a mixture of a polyethylene resin and a polypropylene resin.
[0035] The second layer 17 desirably contains ethylene-vinyl acetate copolymer (EVA). The second layer 17 preferably contains 50% by mass or more of ethylene-vinyl acetate copolymer. More preferably, the second layer 17 contains 60% by mass or more of ethylene-vinyl acetate copolymer. Even more preferably, the second layer 17 contains 70% by mass or more of ethylene-vinyl acetate copolymer. The second layer 17 may also contain a modified polyolefin-based resin having a polar group. The second layer 17 contains a modified polyolefin-based resin, which provides excellent adhesion to the paper substrate 21. The modified polyolefin-based resin preferably has a structural unit derived from a monomer having a carboxy group or a group in which two carboxy groups have been anhydridized.
[0036] The modified polyolefin resin is preferably a modified polypropylene resin or a modified polyethylene resin. The second layer 17 may contain only one type of modified polyolefin resin, or may contain two or more types of modified polyolefin resin. The second layer 17 may be composed of a modified polyolefin resin alone, or may be composed of a mixture of the modified polyolefin resin and another material. The other material is not particularly limited and may be selected arbitrarily depending on the purpose.
[0037] In this embodiment, the multilayer film 10 includes an intermediate layer 14 between the first layer 11 and the second layer 17. The function of the intermediate layer 14 is not particularly limited, but preferably provides the multilayer film 10 with gas barrier properties. "Gas barrier properties" refers to the resistance to gas permeation. The intermediate layer 14 provides the multilayer film 10 with gas barrier properties against, for example, carbon dioxide gas (CO2), nitrogen gas (N2), and oxygen gas (O2).
[0038] In this embodiment, the intermediate layer 14 is an oxygen barrier layer. The intermediate layer 14 includes an ethylene-vinyl alcohol copolymer (EVOH). Here, it is preferable to use an ethylene-vinyl alcohol copolymer having an ethylene content of 38 mol% or less, since the gas barrier property is particularly high. In addition to the ethylene-vinyl alcohol copolymer, the material included in the intermediate layer 14 is preferably polyamide MXD6, polyvinylidene chloride, or the like. Also, the intermediate layer 14 may contain an additive having gas barrier property (mica, clay, or the like). The intermediate layer 14 preferably includes 70% by mass or more of a polyethylene resin. More preferably, it includes 80% by mass or more of a polyethylene resin. Even more preferably, it includes 90% by mass or more of a polyethylene resin. The intermediate layer 14 includes, for example, 50% by mass or more of an ethylene-vinyl alcohol copolymer (EVOH).
[0039] The material and thickness of the intermediate layer 14 have a large effect on the gas barrier properties of the multilayer film 10, and therefore the material and thickness of the intermediate layer 14 must be selected within a range that provides the required gas barrier properties. The material and thickness of the intermediate layer 14 must be selected so that the oxygen transmission rate of a film made of the material and having a thickness of 5.0 ml / m2 or less, as measured according to JIS K 7126-2:2006 (constant pressure method). 2 For example, if the intermediate layer 14 is made of an ethylene-vinyl alcohol copolymer with an ethylene content of 38 mol % or less and has a thickness of 6 μm or more, the oxygen permeability is determined to be 5.0 ml / m 2 The material and thickness of the intermediate layer 14 are such that the oxygen permeability of a film made of the material and having the specified thickness is 3.0 ml / m 2 More preferably, the concentration is determined to be equal to or less than 1.0 ml / m 2 It is further preferred that the temperature is determined to be equal to or less than 1·day·atm.
[0040] In this embodiment, the multilayer film 10 includes a first adhesive layer 13 between the intermediate layer 14 and the first layer 11. The multilayer film 10 also includes a second adhesive layer 15 between the intermediate layer 14 and the second layer 17. The first adhesive layer 13 and the second adhesive layer 15 have the function of adhering adjacent layers on both sides of each other. The first adhesive layer 13 is preferably adjacent to the intermediate layer 14. The second adhesive layer 15 is preferably adjacent to the intermediate layer 14. The materials constituting the first adhesive layer 13 and the second adhesive layer 15 are selected according to the combination of the two layers to be adhered to each other, and for example, known adhesive polymers are used.
[0041] In this embodiment, a first functional layer 12 is provided between the first layer 11 and the second layer 17. Also, in this embodiment, a second functional layer 16 is provided between the first layer 11 and the second layer 17. The functions of the first functional layer 12 and the second functional layer 16 are not particularly limited, but preferably, they impart heat resistance, freezing resistance, etc. to the multilayer film 10.
[0042] The first functional layer 12 is preferably a polyethylene-based resin. Preferably, the first functional layer 12 is a polyethylene-based resin having a polar group. More preferably, the polyethylene-based resin having a polar group that is the first functional layer 12 is an ionomer (ION). The first functional layer 12 preferably contains 80% by mass or more of polyethylene. More preferably, it contains 90% by mass or more of polyethylene. Even more preferably, it contains 100% by mass or more of polyethylene. In the example shown in FIG. 1, the first functional layer 12 is disposed between the first layer 11 and the first adhesive layer 13.
[0043] In this embodiment, the electron beam irradiation described below is performed from the side of the first layer 11. In this way, it is possible to effectively improve the heat resistance of the first layer 11, which is the surface that comes into contact with the contents such as food. In addition, it is possible to suppress a decrease in the adhesive strength of the second layer 17 that is thermally fused to the paper substrate.
[0044] The second functional layer 16 is preferably a polyethylene-based resin. Preferably, the second functional layer 16 is a polyethylene-based resin having a polar group. More preferably, the polyethylene-based resin having a polar group that is the second functional layer 16 is an ionomer (ION). The second functional layer 16 that is a polyethylene-based resin preferably contains 80% by mass or more of polyethylene. More preferably, it contains 90% by mass or more of polyethylene. Even more preferably, it contains 100% by mass or more of polyethylene. In the example shown in FIG. 1, the second functional layer 16 is disposed between the second adhesive layer 15 and the second layer 17.
[0045] FIG. 3 is a diagram showing the tendency of the rate of hole formation (%) during heat welding and the heat shrinkage rate (%) of the multilayer film 10 after heat welding with respect to various parameters. The upper part is a diagram showing the tendency of the rate of hole formation (%) during heat welding and the heat shrinkage rate (%) of the multilayer film 10 after heat welding with respect to the temperature in the lamination step S14 described later, i.e., the heat welding temperature (°C) when the multilayer film 10 is heat-welded to the substrate 21. The middle part is a diagram showing the tendency of the rate of hole formation (%) during heat welding and the heat shrinkage rate (%) of the multilayer film 10 after heat welding with respect to the irradiation dose (KGy) when the multilayer film 10 is irradiated with an electron beam. The lower part is a diagram showing the tendency of the rate of hole formation (%) during heat welding and the heat shrinkage rate (%) of the multilayer film 10 after heat welding with respect to the ionomer ratio (%) of the multilayer film 10.
[0046] If the heat shrinkage rate is high, the shape of the container 20 is likely to collapse when the container 20 in which the multilayer film 10 is heat-welded to the substrate 21 is heated, for example, using a microwave oven. As shown in Fig. 3, increasing the heat welding temperature (°C) can reduce the heat shrinkage rate, but the rate of hole formation increases. Increasing the exposure dose can reduce the rate of hole formation, but the heat shrinkage rate increases. Increasing the ionomer ratio can reduce the rate of hole formation and the heat shrinkage rate.
[0047] Preferably, the multilayer film 10 is irradiated with an electron beam at an exposure dose of 300 kGy or less. More preferably, the multilayer film 10 is irradiated with an electron beam at an exposure dose of 250 kGy or less. Even more preferably, the multilayer film 10 is irradiated with an electron beam at an exposure dose of 200 kGy or less. When the exposure dose of the electron beam is within this range, an increase in the heat shrinkage rate of the multilayer film 10 is suppressed.
[0048] Preferably, the multilayer film 10 is irradiated with an electron beam at an exposure dose of 50 kGy or more. More preferably, the multilayer film 10 is irradiated with an electron beam at an exposure dose of 55 kGy or more. Even more preferably, the multilayer film 10 is irradiated with an electron beam at an exposure dose of 60 kGy or more. When the exposure dose of the electron beam is within this range, it is possible to impart high heat resistance to the multilayer film 10 and prevent holes from being formed.
[0049] The reason why the crosslink density of the multilayer film 10 is improved by electron beam irradiation is not clear, but it is believed to be as follows. That is, when the multilayer film 10 is irradiated with an electron beam, the carbon-hydrogen bonds in the polyethylene of the first layer 11 of the multilayer film 10 are broken, and radicals are generated at the ends of the broken bonds. It is believed that the generated radicals come into contact with other polyethylene molecular chains due to the molecular motion of the molecular chains, extract hydrogen atoms, and bond with carbon atoms in the polyethylene molecular chains, resulting in the formation of a crosslinked structure. It is believed that a similar phenomenon occurs in the first functional layer 12 and the intermediate layer 14. However, the above-mentioned mechanism is merely a conjecture, and the scope of the present invention is not affected by its truth or falsity.
[0050] The total thickness of the multilayer film 10 is not particularly limited, but is preferably 200 μm or less. Preferably, the total thickness of the multilayer film 10 is 40 μm or more and 180 μm or less. More preferably, the total thickness of the multilayer film 10 is 80 μm or more and 140 μm or less. If the thickness of the multilayer film 10 exceeds 200 μm, heat is not easily transferred to the bonding surface when the second layer 17 is thermoformed (thermal welding) to the substrate 21, and thermoforming (thermal welding) defects may easily occur. If the thickness of the multilayer film 10 is less than 40 μm, the intermediate layer 14 becomes thin and the gas barrier property may not meet the required level. In addition, if the thickness of the multilayer film 10 is less than 40 μm, the yield of the multilayer film 10 may be low when it is manufactured.
[0051] In this embodiment, the ratio of polyethylene-based resin in the multilayer film 10 is 60% by weight or more. Preferably, the ratio of polyethylene-based resin in the multilayer film 10 is 70% by weight or more. More preferably, the ratio of polyethylene-based resin in the multilayer film 10 is 80% by weight or more. The ratio of polyethylene-based resin in the multilayer film 10 is a value calculated by dividing the total weight of the polyethylene-based resin in each layer by the total weight of the multilayer film 10.
[0052] In this embodiment, in dynamic viscoelasticity measurement in a tensile mode in the MD (machine direction), the storage modulus of the multilayer film 10 at a measurement temperature of 150°C is 0.3 MPa or more. Preferably, the storage modulus is 0.4 MPa or more. More preferably, the storage modulus is 0.5 MPa or more. Even more preferably, the storage modulus is 0.6 MPa or more.
[0053] In this embodiment, in dynamic viscoelasticity measurement in the tensile mode in the MD direction, the storage modulus of the multilayer film 10 at a measurement temperature of 150°C is 4 MPa or less. Preferably, the storage modulus is 3.7 MPa or less. More preferably, the storage modulus is 3.3 MPa or less. Even more preferably, the storage modulus is 3.0 MPa or less. In this way, an increase in the thermal shrinkage rate of the multilayer film 10 is suppressed.
[0054] The container 20 includes a paper substrate 21 that has been formed three-dimensionally in advance, and a multilayer film 10, and the multilayer film 10 is heat-sealed to the substrate 21. In this embodiment, the container 20 further includes a lid 22. The container 20 contains, for example, food or medicine as contents. As the lid 22, for example, a top film for top-seal packaging made of a polyethylene resin material or a skin film for skin-pack packaging made of an ethylene-vinyl acetate copolymer resin material is used. "Top-seal packaging" is a packaging method in which a container is filled with contents and the top film is heat-sealed to the container to preferably seal it. "Skin-pack packaging" is a packaging method in which a product is placed in a container such as a tray, a backing paper, an air cap, or a film, a heated skin film is placed on top, air is removed from below, and the skin film is brought into close contact with the surface of the food and the container to preferably seal it. In the illustrated example, the substrate 21 that has been formed three-dimensionally in advance is a paper container for top-seal packaging, and the lid 22 is a top film.
[0055] When the first layer 11 contains a polyethylene resin, the first layer 11 has oil resistance, so that damage to the substrate 21 caused by oil contained in food or the like can be avoided. In addition, since the first layer 11 is given heat resistance by electron beam crosslinking, it has sufficient heat resistance for food heated in a microwave oven, for example. Preferably, the multilayer film 10 is a multilayer film for microwave-heated food that can be used for microwave-heated food. Here, microwave-heated food means food that is cooked in a microwave oven. Also, preferably, the container 20 has microwave-heating resistance. Having microwave-heating resistance means that food can be cooked in a microwave oven. Preferably, having microwave-heating resistance means that it complies with the "Microwave High Frequency Suitability Test" and "Microwave Durability Test" specified in JIS S2029:2002. Since the container 20 has microwave-heating resistance, the container 20 can be suitably used for microwave-heated food.
[0056] The first layer 11 is heat-sealed to the lid 22. This makes it possible to seal food or the like in the space defined by the multilayer film 10 and the lid 22. For example, the multilayer film 10 has high gas barrier properties (particularly oxygen barrier properties, with an oxygen permeability of 5.0 ml / m 2 ) derived from the intermediate layer 14. 2 1·day·atm or less. Since the lid material 22 also has high gas barrier properties, food and the like can be sealed with a member having high gas barrier properties, so deterioration of the food and the like can be suppressed.
[0057] As shown in FIG. 4, the method for manufacturing the container 20 includes a substrate forming step S11, a multilayer film forming step S12, a heat softening step S13, and a lamination step S14.
[0058] The substrate forming step S11 is a step of forming a substrate 21 having a three-dimensional shape from a planar paper material. A known forming method can be used for the substrate forming step S11. Examples of such forming methods include vacuum forming, pressure forming, vacuum pressure forming, match forming forming, and press forming. As the paper material, recycled paper pulp, virgin pulp, and pulp obtained by appropriately mixing these may be used. The container 20 may be formed into a three-dimensional shape by assembling paperboard by cutting it into a desired shape, or may be formed using a mold.
[0059] The multilayer film forming step S12 is a step of forming a multilayer film 10 having a first layer 11, an intermediate layer 14, and a second layer 17 in the order described above. For example, co-extrusion molding is used as the multilayer film forming step S12. That is, the materials constituting the first layer 11, the first functional layer 12, the intermediate layer 14, the second functional layer 16, and the second layer 17 are extruded from an extruder and discharged from a T-die to form the multilayer film 10 having the above configuration. As another forming method, the multilayer film 10 may be formed by a method in which the first layer 11, the first functional layer 12, the intermediate layer 14, the second functional layer 16, and the second layer 17, which are formed into a film shape for each layer, are heat-welded to each other. The multilayer film 10 may also be formed by bonding the layers together using an adhesive by any of a dry lamination method, a hot melt lamination method, and a wet lamination method. In the illustrated example, the multilayer film forming step S12 is performed after the substrate forming step S11, but the order may be reversed or they may be performed in parallel.
[0060] The heat-softening step S13 is a step of heating and softening the multilayer film 10. In this embodiment, the substrate 21 is placed in the lower mold of a mold, and the multilayer film 10 is placed on a hot plate 30, which is the upper mold of the mold, so that the second layer 17 side faces the substrate 21, and is heated and softened at 120°C to 150°C.
[0061] The laminating step S14 is a step of thermally welding the multilayer film 10 softened in the heat-softening step S13 by bringing the second layer 17 into contact with the substrate 21. In this embodiment, the upper mold on which the multilayer film 10 is arranged is lowered to bring the second layer 17 of the multilayer film 10 into contact with the substrate 21 arranged in the lower mold, and a pressure of 1.0 kgf to 2.5 kgf, preferably 1.5 kgf to 2.0 kgf is applied, and this state is maintained for 1 to 5 seconds, thereby thermally welding the multilayer film 10 and the substrate 21.
[0062] Other embodiments Other embodiments of the multilayer film 10 and the container 20 according to the present invention will be described below. Note that the configurations disclosed in the following respective embodiments can be applied in combination with the configurations disclosed in other embodiments, unless a contradiction occurs.
[0063] In the above embodiment, an example has been described in which the multilayer film 10 includes the first layer 11, the first functional layer 12, the first adhesive layer 13, the intermediate layer 14, the second adhesive layer 15, the second functional layer 16, and the second layer 17. However, in the multilayer film 10 according to the present invention, the presence or absence of the first functional layer 12 and the second functional layer 16 is optional. Also, for example, the first functional layer 12 and the second functional layer 16 may be provided concentrated on one side of the intermediate layer 14 in the stacking direction. Also, for example, two layers having a different function from the intermediate layer 14 may be further provided symmetrically with respect to the intermediate layer 14 on both sides of the intermediate layer 14 in the stacking direction.
[0064] Known additives may be added to the polymeric materials used in each layer constituting the multilayer film 10 of the present invention. Examples of such additives include plasticizers, antioxidants, flame retardants, stabilizers, UV absorbers, antistatic agents, lubricants, water repellents, and oil repellents.
[0065] In the above embodiment, the container manufacturing method includes the base material forming step S11, the multilayer film forming step S12, the heat softening step S13, and the laminating step S14, but other steps may be included. For example, a lid material forming step, a gravure printing step, etc. may be further included.
[0066] Regarding other configurations, it should be understood that the embodiments disclosed in this specification are illustrative in all respects and that the scope of the present invention is not limited thereto. A person skilled in the art would easily understand that appropriate modifications are possible without departing from the spirit of the present invention. Therefore, other embodiments modified without departing from the spirit of the present invention are naturally included in the scope of the present invention.
[0067] The present invention will be described in more detail below with reference to specific examples, although the present invention is not limited to the following examples.
[0068] The multilayer films of Samples 1 to 8 below were produced, and then subjected to dynamic mechanical analysis (DMA) and a hole inspection.
[0069] The resins constituting Samples 1 to 8 are as follows. (Sample 1) First layer: PE, thickness 20μm (Product number: Yumerit 4040FC: manufactured by Ube Maruzen Polyethylene Co., Ltd.) First functional layer: EVA, thickness 24μm (Product number: Evaflex V5714C: manufactured by Dow Mitsui Polychemicals Co., Ltd.) First adhesive layer: PE, thickness 8μm Middle layer: EVOH, thickness 20μm (Product number: EVAL XEP-1393B: manufactured by Kuraray Co., Ltd.) Second adhesive layer: PE, thickness 8μm (Product number: Admer NF536: manufactured by Mitsui Chemicals, Inc.) Second layer: EVA, thickness 20μm (Product number: Evaflex V5714C: manufactured by Dow Mitsui Polychemicals Co., Ltd.) (Sample 2) First layer: PE, thickness 20μm (Product number: Yumerit 4040FC: manufactured by Ube Maruzen Polyethylene Co., Ltd.) First functional layer: EVA, thickness 24μm (Product number: Evaflex V5716RC: manufactured by Dow Mitsui Polychemicals Co., Ltd.) First adhesive layer: PE, thickness 8μm Middle layer: EVOH, thickness 20μm (Product number: EVAL XEP-1393B: manufactured by Kuraray Co., Ltd.) Second adhesive layer: PE, thickness 8μm (Product number: Admer NF536: manufactured by Mitsui Chemicals, Inc.) Second layer: EVA, thickness 20μm (Product number: Evaflex V5714C: manufactured by Dow Mitsui Polychemicals Co., Ltd.) (Sample 3) First layer: PE, thickness 20μm (Product number: Yumerit 4040FC: manufactured by Ube Maruzen Polyethylene Co., Ltd.) First functional layer: ION thickness 24μm (Product number: Himilan 1601: manufactured by Mitsui Dow Polychemicals Co., Ltd.) First adhesive layer: PE, thickness 8μm Middle layer: EVOH, thickness 20μm (Product number: EVAL XEP-1393B: manufactured by Kuraray Co., Ltd.) Second adhesive layer: PE, thickness 8μm (Product number: Admer NF536: manufactured by Mitsui Chemicals, Inc.) Second layer: EVA, thickness 20μm (Product number: Evaflex V5714C: manufactured by Dow Mitsui Polychemicals Co., Ltd.) (Sample 4) First layer: PE, thickness 20μm (Product number: Yumerit 4040FC: manufactured by Ube Maruzen Polyethylene Co., Ltd.) First functional layer: ION thickness 24μm (Product number: Himilan 1855: manufactured by Mitsui Dow Polychemicals Co., Ltd.) First adhesive layer: PE, thickness 8μm Middle layer: EVOH, thickness 20μm (Product number: EVAL XEP-1393B: manufactured by Kuraray Co., Ltd.) Second adhesive layer: PE, thickness 8μm (Product number: Admer NF536: manufactured by Mitsui Chemicals, Inc.) Second layer: EVA, thickness 20μm (Product number: Evaflex V5714C: manufactured by Dow Mitsui Polychemicals Co., Ltd.) (Sample 5) First layer: PP, thickness 44μm (Product number: Noblen WF836DG3: manufactured by Sumitomo Chemical Co., Ltd.) First adhesive layer: PP, thickness 8μm (Product number: Admer QF551: manufactured by Mitsui Chemicals, Inc.) Middle layer: EVOH, thickness 20μm (Product number: EVAL XEP-1393B: manufactured by Kuraray Co., Ltd.) Second adhesive layer: PE, thickness 8μm (Product number: Admer NF536: manufactured by Mitsui Chemicals, Inc.) Second layer: EVA, thickness 20μm (Product number: Evaflex V5714C: manufactured by Dow Mitsui Polychemicals Co., Ltd.) (Sample 6) First layer: PP, thickness 20μm (Product number: Noblen WF836DG3: manufactured by Sumitomo Chemical Co., Ltd.) First adhesive layer: PP, thickness 8μm (Product number: Admer QF551: manufactured by Mitsui Chemicals, Inc.) First functional layer: NY thickness 24μm (Product number: Ultramid B40L09: BASF Japan Ltd.) Middle layer: EVOH, thickness 20μm (Product number: EVAL XEP-1393B: manufactured by Kuraray Co., Ltd.) Second adhesive layer: PE, thickness 8μm (Product number: Admer NF536: manufactured by Mitsui Chemicals, Inc.) Second layer: EVA, thickness 20μm (Product number: Evaflex V5714C: manufactured by Dow Mitsui Polychemicals Co., Ltd.) (Sample 7) First layer: PE, thickness 20μm (Product number: Yumerit 4040FC: manufactured by Ube Maruzen Polyethylene Co., Ltd.) First adhesive layer: PE, thickness 8μm (Product number: Admer NF536: manufactured by Mitsui Chemicals, Inc.) First functional layer: NY thickness 24μm (Product number: Ultramid B40L09: BASF Japan Ltd.) Middle layer: EVOH, thickness 20μm (Product number: EVAL XEP-1393B: manufactured by Kuraray Co., Ltd.) Second adhesive layer: PE, thickness 8μm (Product number: Admer NF536: manufactured by Mitsui Chemicals, Inc.) Second layer: EVA, thickness 20μm (Product number: Evaflex V5714C: manufactured by Dow Mitsui Polychemicals Co., Ltd.) (Sample 8) First layer: PET, thickness 20μm (Product number: BR8040: SK Chemicals) First adhesive layer: Modified PO, thickness 8 μm (Product number: Admer SF728: manufactured by Mitsui Chemicals, Inc.) First functional layer: NY thickness 24μm (Product number: Ultramid B40L09: BASF Japan Ltd.) Middle layer: EVOH, thickness 20μm (Product number: EVAL XEP-1393B: manufactured by Kuraray Co., Ltd.) Second adhesive layer: PE, thickness 8μm (Product number: Admer NF536: manufactured by Mitsui Chemicals, Inc.) Second layer: EVA, thickness 20μm (Product number: Evaflex V5714C: manufactured by Dow Mitsui Polychemicals Co., Ltd.)
[0070] "Dynamic viscoelasticity measurement" The storage modulus was measured by dynamic mechanical analysis (DMA) under the following conditions:
[0071] (Measurement conditions) - Multilayer film shape: length 20mm, width 4mm, thickness 100μm Test equipment model: DMA7100 (Hitachi High-Tech Fielding Corporation) ·Measurement temperature: 200℃ Measurement mode: Tensile Frequency: 10Hz ·Minimum tension: 50mN Tension Gain: 1.2 Initial force amplitude: 50mN
[0072] 5 shows a graph of the measurement results of the storage modulus (MPa) versus the measurement temperature (23°C to 200°C) for samples 1 to 8. The reason why the graphs for the measurement results for samples 5, 6, and 7 are interrupted before reaching 200°C is that the multilayer film broke during the measurement.
[0073] "Hole inspection" The multilayer films of samples 1 to 8 were heat-welded to paper containers formed three-dimensionally from flat substrates to create test pieces, and a hole inspection was performed. The shape of the test piece (paper container) and the judgment method for the hole inspection are shown below.
[0074] (Shape of paper container) Approximately rectangular container with a length of 130 mm, width of 90 mm, and depth of 40 mm
[0075] (Judgment method) Ageless Seal Check (manufactured by Mitsubishi Gas Chemical Company, Inc.) was sprayed onto the surface of the multi-layer film of the container, and the container was visually inspected for leakage from the back side after one hour had passed. In Table 1 below, in the item for judging holes, cases where there was no leakage are indicated by "O" and cases where there was leakage are indicated by "X".
[0076] The outline of the configuration of Samples 1 to 8, as well as the results of the dynamic viscoelasticity measurement and the hole formation test, are shown in Table 1 below.
[0077] [Table 1]
[0078] As shown in Table 1, the results of the hole formation evaluation were good for samples 5 to 8, which have a polyethylene resin ratio of 60% by weight or more and a storage modulus of 0.3 MPa or more and 4 MPa or less at a measurement temperature of 150°C. The reason why hole formation can be suppressed, although it is only a guess, is thought to be that the storage modulus at high temperatures does not become too small, which suppresses the elongation of the multilayer film when the temperature rises, making it easier for the multilayer film to remain at the places where the paper base material is interrupted. Also, it is thought that the storage modulus at high temperatures does not become too large, which allows the multilayer film to elongate sufficiently when the temperature rises, making the multilayer film less likely to tear. [Industrial Applicability]
[0079] The present invention can be used, for example, in food packaging applications. [Explanation of symbols]
[0080] 10: Multilayer film 11:First layer 12:First functional layer 14: Middle class 17:Second layer 20: Container 21: Base material
Claims
1. The sheet has a first layer which is an outer layer that can be bonded to a polyethylene resin material, and a second layer which is an inner layer that can be heat-sealed to a paper substrate that has been previously formed into a three-dimensional shape, The ratio of polyethylene resin is 60% by weight or more, A multilayer film having a storage modulus of 0.3 MPa or more at a measurement temperature of 150°C in dynamic viscoelasticity measurement in a tensile mode in the MD direction.
2. 2. The multilayer film according to claim 1, wherein the storage modulus at a measurement temperature of 150°C is 4 MPa or less in the dynamic viscoelasticity measurement.
3. 2. The multilayer film of claim 1, having a total thickness of 80 μm or more and 180 μm or less.
4. The multilayer film of claim 1 , further comprising a first functional layer between the first layer and the second layer.
5. The multilayer film according to claim 4 , wherein the first functional layer is a polyethylene-based resin having a polar group.
6. The multilayer film according to claim 5 , wherein the polyethylene resin having a polar group is an ionomer.
7. 2. The multilayer film of claim 1, further comprising an intermediate layer between said first layer and said second layer, said intermediate layer being an oxygen barrier layer.
8. The multilayer film of claim 7, wherein the intermediate layer comprises an ethylene-vinyl alcohol copolymer.
9. The multilayer film of claim 1 , wherein the second layer comprises an ethylene vinyl acetate copolymer.
10. The multilayer film according to claim 1 , which has been irradiated with electron beams at a dose of 50 kGy to 300 kGy.
11. A container comprising: a substrate made of paper that has been three-dimensionally formed in advance; and the multilayer film according to any one of claims 1 to 10, wherein the multilayer film is heat-welded to the substrate.
12. 12. The container of claim 11, which is microwave-resistant.
Citation Information
Patent Citations
Laminate film for paper container and laminate paper container
JP2020146996A