Antioxidant stabilizer in polymers

Herbal lignin is used as an antioxidant stabilizer in polymers to address oxidative degradation challenges, enhancing stability and compatibility, thus overcoming the limitations of traditional stabilizers.

JP2024147556AActive Publication Date: 2024-10-16RENMATIX INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024098519
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2017-09-07
Filing Date
2024-06-19
Publication Date
2024-10-16
Estimated Expiration
2038-09-07

AI Technical Summary

Technical Problem

Existing antioxidant stabilizers for polymers face challenges in providing effective protection against oxidative degradation while maintaining environmental safety and compatibility with the polymer matrix, as many heavy metal-based stabilizers are phased out due to toxicity concerns, and organic alternatives often suffer from poor compatibility and migration issues.

Method used

The use of herbal lignin, particularly switchgrass lignin, as an antioxidant stabilizer in polymers, which enhances oxidative stability by incorporating it into polymer compositions, offering improved compatibility and resistance to migration.

Benefits of technology

Herbal lignin significantly raises the oxidation onset temperature of polymers, providing enhanced protection against degradation and maintaining compatibility without the environmental hazards associated with traditional stabilizers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024147556000001_ABST
    Figure 2024147556000001_ABST
Patent Text Reader

Abstract

To provide the use of a herbaceous lignin and / or a hardwood lignin as an antioxidant stabilizer in polymers or polymer compositions, such as thermoplastic substances, thermoplastic composites, thermosetting substances, coatings, films, adhesives, personal care compositions, or any combinations thereof.SOLUTION: A composition comprises a thermoplastic polymer, and biomass that comprises a lignin. The lignin is present at a concentration from 0.5 wt.% to 1.5 wt.%. The composition contains cellulose and / or hemicellulose in an amount less than or equal to 20% based on the weight of the biomass. The lignin is preferably a hardwood lignin, and further preferably a herbaceous lignin.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application is a continuation of U.S. Provisional Patent Application No. 62 / 555,642, filed September 7, 2017. which is incorporated herein by reference in its entirety.

[0002] The present invention relates to herbaceous lignin and / or herbaceous lignin as antioxidants in polymers or polymer compositions. Specifically, the present invention relates to a polymer or polymer composition, e.g. For example, thermoplastics, thermoplastic composites, thermosets, coatings, films, adhesives , personal care compositions, or any combination thereof, as antioxidant stabilizers Uses of herbaceous lignin and / or hardwood lignin are disclosed herein. [Background technology]

[0003] The direct or indirect effects of heat and UV light can cause the degradation of most polymers, e.g. It has long been recognized that certain substances (chemical substances) are susceptible to oxidative degradation over time. This can occur early in the formulation and processing of a polymer, but the degradation of properties is more evident This can result in discoloration and loss of strength, flexibility, stiffness, scratch resistance, or gloss. The detailed mechanism of decomposition is complex, but Generally considered to be free radicals in nature, they are responsible for initiating processes, such as the synthesis of polymer chains. The process begins with the loss of a hydrogen atom (H.) from the polymer, resulting in the formation of reactive and unstable polymer free radicals ( The propagation of the free radical reaction involves the polymer free radical reaction with oxygen molecules. This reaction includes a variety of reactions, including those involving the formation of peroxy radicals (ROO·), which The peroxy radical transfers a hydrogen atom from another polymer chain to form a hydroperoxide (RO OH) and generate another polymer free radical (R·). The hydroperoxides then convert to two new free radicals (RO·) and (·OH). may split off and continue to propagate the reaction to other polymer molecules. Further reactions on adjacent polymer chains can result in branching and crosslinking. The reaction may terminate naturally by combining the -radicals, but during this period Significant degradation of the polymer may occur. The technique uses free radicals during the degradation process. This "mop-up" the nuclei, thereby bringing about the termination of radical reactions more quickly. We have developed applications for engineered additives. Such additives are usually called antioxidant stabilizers. Stabilizing polymers include polypropylene, polyethylene, polyvinyl chloride (PVC), Polyvinyl acetate (PVA), chlorinated polyethylene, polystyrene, acrylonitrile-butadiene ABS copolymer, ethylene-vinyl acetate copolymer, PVC / ABS blend, polyethylene terephthalate (PET), polycarbonate, polyurethane These include styrene, acrylic, styrene-acrylic, polyamide, nylon, elastomer, etc. , but not limited to these.

[0004] Known antioxidant stabilizers include those containing metals such as lead, barium, cadmium, tin, and the like. Recently, heavy metal salts including zinc, calcium, magnesium, and aluminum, and organometallic compounds have been used. These include compounds and complexes, most of which have environmental and / or toxicological have been phased out (or are being phased out) due to safety concerns. Other antioxidant stabilizers include: Organic phosphites and organic phosphonites, sterically hindered phenols, amines, and thioesters Includes Stell.

[0005] Stabilization of free radicals (termination of decomposition reactions) and favorable environmental and toxicological processes In addition to having a file, the stabilizer must have good compatibility with the polymer and be able to diffuse or penetrate easily. The latter problem (antioxidation) must be resistant to migration from the polymer. Additive migration and blooming) can occur with small molecule additives, especially if they have poor compatibility with the polymer. Many of the commercially available stabilizing additives lack one or more of these properties. What is needed is an economical stabilizer additive that provides all these properties. It is an additive.

[0006] The methods and compositions of the present invention are directed to these, and other important ends. Summary of the Invention

[0007] In one embodiment, a composition is provided that includes a thermoplastic polymer and biomass, the biomass The composition contains lignin, and the composition contains cellulose and and / or hemicellulose.

[0008] In one embodiment, one of hardwood lignin, softwood lignin, and herbaceous lignin. In certain embodiments, a polymer or polymer composition is provided that comprises a poly The polymer or monomer composition may further comprise acridine orange (AO). Thus, in one embodiment, a polymer or polymer composition comprising hardwood lignin is In another embodiment, a polymer or polymer composition comprising softwood lignin is provided. In yet another embodiment, a polymer or polymers comprising herbaceous lignin are provided. A composition is provided.

[0009] In certain embodiments, the disclosed polymers or polymer compositions are used in thermoplastics, thermosetting chemical materials, composites, coatings, films, adhesives, personal care compositions, or Any combination thereof is provided. Thus, for example, the disclosed thermoplastics, thermoplastics, a curable material, a composite, a coating, a film, an adhesive, a personal care composition, or These combinations are formed from the disclosed polymers or polymer compositions, or , can be made therewith.

[0010] In certain embodiments, the oxidation onset temperature of the polymer or polymer composition comprising herbaceous lignin is The degree of lignin content is 100%, except that it contains kraft lignin or hardwood lignin instead of herbaceous lignin. At least 10° C. higher than the same polymer or polymer composition.

[0011] In certain embodiments, the polymer or polymer composition comprising herbaceous lignin has a molecular weight of about 232 In one such embodiment, the polymer has an oxidation onset temperature of from about 250° C. to about 250° C. In one such embodiment, the herbaceous lignin is switchgrass lignin. be.

[0012] In certain embodiments, the polymer is a thermoplastic.

[0013] In certain embodiments, the thermoplastic material is polyethylene, polypropylene, or Includes a combination of.

[0014] In certain embodiments, the herbaceous lignin is switchgrass lignin.

[0015] Further advantages will be described in part in the description that follows and in part will be apparent from the description, or The advantages which may be obtained by the practice of the invention are particularly set forth in the appended claims. The invention is realized and achieved by the elements and combinations indicated. Both the above and the following detailed description are exemplary and explanatory only and are not intended to limit the invention as claimed. It should be understood that this does not define the [Brief description of the drawings]

[0016] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate and explain several embodiments. Together they serve to explain the principles of the invention.

[0017] [Figure 1] FIG. 1 shows the onset of oxidation temperatures, OOT, (°C) obtained at various antioxidant concentrations for various antioxidants added to polypropylene. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The present invention relates to lignin, in particular thermoplastics, thermoplastic composites, thermosets, coatings, in coatings, films, adhesives, personal care compositions, or any combination thereof. Specifically, the anti-oxidant in a polymer or polymer composite or polymer composition The present invention relates to the use of herbaceous lignin as a stabilizer for chemical reactions.

[0019] However, the present invention is not limited to the use of lignin as an antioxidant additive for polymers, Herbaceous lignin as a filler in polymer or polymer compositions (e.g., polymer composites) The fillers may also be used to enhance the effect of heat or light on the polymer composite. This provides protection from degradation caused by

[0020] The present invention is defined by the following detailed description, examples, and claims, as well as the foregoing. This can be more readily understood by referring to the following description. The present invention does not relate to any particular compositions, articles, devices, systems, It is understood that the present invention is not limited to the specific embodiments and / or methods, and as such may, of course, vary. Aspects of the invention are described and claimed in certain statutory classes, such as composition of matter statutory classes. However, this is for convenience and those skilled in the art will appreciate that each aspect of the invention may be classified as a statutory classification. It will be understood that the present invention can be described and claimed as follows.

[0021] The following description of the invention also enables teaching of the invention in its best currently known form. To this end, the skilled artisan will be able to It will be appreciated that changes and modifications can be made to various aspects of the invention described herein. It will be appreciated and understood that some of the advantages of the present invention can be achieved without utilizing other features. It will be apparent that some of the features of the invention can be obtained by selecting Thus, many modifications and adaptations to the present invention are possible for those skilled in the relevant art. , which may be desirable in certain circumstances and thus are also part of the present invention. It would be.

[0022] While the present invention may be embodied in various forms, the following description of some embodiments is provided to It is understood that the present disclosure should be considered as an illustration of the present invention, and that the specific implementations illustrated herein are illustrative of the invention. It is understood that the present disclosure is not intended to be limiting in any way. Headings are used for convenience only. are provided and should not be construed as limiting the invention in any manner. An embodiment illustrated under any heading or any portion of this disclosure may be used interchangeably with the embodiments illustrated under the same heading of this disclosure. or any embodiment illustrated under any other heading or portion of this disclosure. can be combined with.

[0023] Unless otherwise indicated herein or clearly contradicted by context, Any combination of the described elements in all possible variations is encompassed by this invention.

[0024] All publications mentioned herein are incorporated by reference and are hereby expressly incorporated by reference in their entirety. Related methods and / or materials are disclosed and described herein.

[0025] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting. It should be understood that this is not intended to be a generalization of the term. Unless otherwise defined, the terms used herein All technical and scientific terms used herein are understood to be within the skill of those in the art to which this invention pertains. As used herein and in the claims that follow, Reference is made to several terms which are defined throughout the specification.

[0026] A.Definition As used above and throughout this disclosure, the following terms mean the following unless otherwise indicated: It is to be understood that such terms have meaning.

[0027] As used in the specification and the appended claims, the singular forms "a," "an," and "the" refer to "The" is used in the plural unless the context clearly indicates otherwise. Includes the target.

[0028] As used herein, the terms "optional" and "optionally" mean any of the following: that any event, condition, element or circumstance may or may not occur; and the description includes when and how said event, condition, element, or situation occurs. This means that cases where the above is not the case are included.

[0029] As used herein, the phrase "sufficient for" (e.g., "a sufficient condition for" or "sufficient for" ") refers to such value or condition that is capable of performing the function or property for which such value or condition is expressed. As pointed out below, the exact values ​​or specific conditions required may vary. Depending on recognized variables, such as the materials and / or processing conditions employed, various embodiments may be used. may differ from the above.

[0030] The term "by weight," when used in conjunction with an ingredient, means that the ingredient is included, unless otherwise specified. The weight of the formulation or composition is based on the total weight of the formulation or composition to be used. When an element or component is said to be present in an amount of 8% by weight, this percentage represents 100% of the total composition. It is understood that the weight percentages of the ingredients are relative to the proportions. In some cases, the weight percentages of the ingredients include water. "Dry basis" refers to the weight of the composition excluding the total weight of the composition (e.g. For example, less than about 1%, less than about 0.5%, less than about 0.1%, by weight based on the total weight of the composition. less than about 0.05% or about 0% water).

[0031] Unless otherwise indicated, the use of numerical values ​​for the various quantitative values ​​specified in this application is within the scope of the described ranges. The values ​​are approximate, as if both the minimum and maximum values ​​in the range were preceded by the word "about." In this way, slight deviations from the values ​​described can be used. Any number of different values ​​can be used to achieve substantially the same results as the values ​​stated. All values ​​between the minimum and maximum values ​​listed, and the possibilities formed by such values For example, a range in which an ingredient is between 2% and 10% is intended to be a continuous range inclusive of all ranges. The disclosure that the amine may be present in amounts of 2% to 9%, 2% to 8%, 3% to 10%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, % to 9%, 4% to 5%, etc. Any and all values ​​that can be formed by dividing all other listed values ​​by Ratios (and ranges of such ratios) are also disclosed. Thus, one of skill in the art will be able to Such ratios, ranges, and ranges of ratios are expressly derived from the numerical values ​​presented herein. In all cases, such ratios, ranges and ratio ranges are within the scope of the various embodiments of the present invention. They will understand that it expresses attitude.

[0032] If you want to disclose numbers, for example 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, Such numbers may be followed by the statement: "Each of such numbers may be preceded by the term 'about', "at least about," or "less than about," and using any of the preceding numerical values. By themselves, open-ended ranges can be listed, or in combination, closed-ended ranges can be listed. "This sentence can be used with each of the numbers above by itself (e.g. 4), Begin with the word "about" (e.g., about 8) and use the phrase "at least about" (e.g., at least may begin with about 2), may begin with the phrase "less than about" (e.g., less than about 7), or To define a range (e.g., 2 to 9, about 1 to 4, 8 to about 9, about 1 to about 10, etc.), The preceding words or phrases may be used with or without any of them, in any combination, Additionally, when a range is stated as "up to about X" (where X is a number), this phrase is equivalent to combining "about X" and "less than about X" instead. For example, "about "10 or less" is the same as "about 10, or less than about 10." Interchangeable range descriptions are contemplated. Other range formats are disclosed herein, but the differences in format are not intended to be construed as limiting the scope of the invention. should not be construed to mean that there is a difference in substance.

[0033] As used herein, the term "substantially free" means about 1% by weight of the total composition. %, for example, less than about 0.5% by weight, less than about 0.1% by weight, less than about 0.05% by weight, refers to a composition having less than about 0.01% by weight of the recited material.

[0034] As used herein, the term "substantially free" (when not used as the phrase "substantially free") "Qualitatively," when used in reference to a composition, means at least about 60% by weight of the total composition. % by weight, e.g., at least about 65%, at least about 70%, at least about 75%, At least about 80%, at least about 85%, at least about 90%, at least about 91%, or at least At least about 92%, at least about 93%, at least about 94%, at least about 95%, at least about 96%, at least about 97%, at least about 98%, at least about 99%, or Refers to approximately 100% of a particular property or component.

[0035] As used herein, "continuous" means uninterrupted or continuous during a process. indicates a process that is interrupted, paused, or stopped only temporarily. The developing material (cellulose-containing composite material) is fed into the device without interruption or substantially without interruption. If the composite material is fed in a batch process, or if the processing is not done in a batch process, the process is "Continuous."

[0036] A supercritical fluid is a liquid that exists at a temperature above its critical temperature and at a pressure above its critical pressure. A supercritical fluid is a fluid that reaches its "critical point," i.e., when the liquid and vapor (gas) phases are mutually exclusive. The point at which equilibrium can exist is called the critical pressure or temperature. From this point on, the distinction between liquid and gas phases disappears. A supercritical fluid has the solvent properties of a liquid as well as the properties of a gas. Therefore, supercritical fluid extraction has the advantage of high permeability and good This has the advantage of efficient solvation.

[0037] The reported critical temperatures and pressures are: for pure water, the critical temperature is about 374.2°C, and for The critical pressure is about 221 bar, and for carbon dioxide, the critical temperature is about 31°C and the critical pressure is The pressure is about 72.9 atmospheres (about 1072 psig). Near-critical water is water at temperatures above about 300°C. A temperature below the critical temperature (374.2°C) and low enough to ensure that all fluids are in the liquid phase Subcritical water is water that has a temperature below about 300°C and is in a state where all of the fluid is in the liquid phase. Subcritical water has a temperature greater than about 250°C and less than about 300°C. C., and in most cases, subcritical water has a temperature of about 250.degree. C. to about 280.degree. C. The term "high temperature, high pressure water" is used herein as near-critical water or sub-critical water, or at least Any temperature of at least about 50° C. (preferably at least about 100° C., at least about 150° C.) °C, at least about 200 °C, at least about 250 °C, at least about 300 °C, or at least at least about 350° C.), but below supercritical (e.g., below about 374° C.), in water (e.g., It is defined as the pressure at which all water (in water) is in a liquid state.

[0038] As used herein, a fluid that is "supercritical" (e.g., supercritical water, supercritical CO 2 N (e.g., argon, nitrogen, nitrogen dioxide, etc.) refer to fluids that are supercritical when they exist in pure form under certain conditions of temperature and pressure. For example, water may be pure or may be a mixture (e.g., water and ethanol, water and CO 2 and Whether present as a liquid, liquid phase, or liquid phase, "supercritical water" is defined as water that has a temperature of at least about 374.2°C and and water present at a pressure of at least about 221 bar. "Water and supercritical carbon dioxide mixture" refers to any supercritical phase, whether or not it contains water. , and whether the aqueous phase contains any carbon dioxide or not, Denotes a mixture of water and carbon dioxide at temperatures and pressures that are high but below the critical point of water For example, subcritical water and supercritical CO 2 The mixture is heated to a temperature of about 250°C to about 280°C. It may have a pressure of at least about 225 bar.

[0039] The term "supercritical hydrolysis" refers to the hydrolysis of one or more fluids under supercritical conditions (i.e., This refers to the hydrolysis reaction brought about by a hydrolysis reaction (hydrolysis of a liquid).

[0040] Unless clearly contradicted by context, all pressures disclosed herein are gauge pressures.

[0041] As used herein, "fluid" means a vapor or liquid or both.

[0042] As used herein, a "slurry" refers to a mixture of insoluble or partially soluble solids and a granular solid. Flowable or pumpable mixtures with the body, e.g. suspended fragments in water or bio Refers to the particles of mass.

[0043] As used herein, "herbaceous lignin" refers to lignin derived from herbaceous biomass. Herbaceous biomass includes switchgrass, silvergrass, turfgrass, and ornamental Grasses and cereal grains, such as sorghum, barley, and wheat. Herbaceous lignin is divided into three molar groups: Norignol (Lignin Syringyl-S, Lignin Iacyl-G, and Lignin H They are composed of hydroxyphenyl-H subunits, and usually have more H subunits than non-herbaceous plants. Herbaceous lignin has more ether bonds in the lignin. The large amount of hydroxycinnamic acid units, e.g. ferulic acid and p-coumaric acid, Further distinction is made.

[0044] As used herein, a "composite" refers to a material in which the constituent components have different physical or chemical properties. An article or material made from two or more components. "Composition" includes lignin-containing composites, such as polymer-lignin composites.

[0045] A "synthetic polymer" is a polymer that is not naturally occurring, but is instead made artificially. Synthetic polymers are polymers that are either man-made or machine-made. Examples of synthetic polymers include homopolymers. Polymers such as polyethylene, polypropylene, etc., and copolymers such as ethylene vinyl acetate, styrene-butadiene, etc. Synthetic polymers include various types of polymers, such as thermosetting polymers and thermoplastic polymers. The structural form of a polymer, or synthetic polymer (e.g., isotactic, syndiotactic, Polyolefins are classified as high density or low density polymers. polymers (e.g., low density polyethylene, high density polyethylene, etc.) Includes:

[0046] As used herein, the term "polymer-lignin complex" refers to a polymer that contains lignin. The term "composite" refers to a composite in which each of these components is greater than 0% by weight based on the weight of the dry composite, and up to As used herein, the term "polymer-lignin" refers to a polymer that is present in an amount ranging from 0.1 to 100% by weight. "Complexes" refers to naturally occurring composites, such as wood, lignocellulosic biomass, cellulosic biomass, and the like. from cellulose-hemicellulose complexes, or wood or lignocellulosic biomass It does not contain any constituents such as cellulose or hemicellulose, or even wood (poly In addition to the polymer and lignin components, polymers may be present as additional components. Specific examples of lignin complexes are described elsewhere herein and are used herein. This represents the meaning of "cellulose-polymer composite" as used herein.

[0047] As used herein, "grinding" refers to any mechanical means for reducing the size of a solid. By this is meant methods such as crushing, grinding, impact grinding, and the like.

[0048] As used herein, the terms "ambient temperature" and "ambient pressure" refer to temperatures at normal (usually, but not necessarily This refers to room temperature and pressure (unadjusted, if not regulated). Such conditions may vary. Because of the nature of the temperature and pressure, the terms are used only to convey approximate temperatures and pressures. In this specification, ambient temperature is taken to mean a temperature of 20°C ± 5°C and ambient pressure is , is interpreted to mean a pressure of 1 bar (1 atmosphere) ± 0.2 bar (0.2 atmospheres).

[0049] As used herein, the term "glass transition temperature" or Tg refers to the temperature at which a glassy polymer becomes polymerized. -Temperatures above which chain segments undergo motion (and from a "glassy" state to melt or As used herein, this refers to the transition to a rubbery state using a heating rate of 10° C. / min. Tg, measured by differential scanning calorimetry (DSC), is the midpoint of the heat flow vs. temperature transition. The point is taken as the Tg value.

[0050] As used herein, a "C1-05 alcohol" refers to an alcohol containing 1 to 5 carbon atoms. Examples of C1-05 alcohols are methanol, ethanol, n-propanol, propanol, isopropanol, n-butanol, s-butanol, t-butanol, i -Butanol, n-pentanol, 2-pentanol, 3-pentanol, 2-methyl- 1-butanol, 2-methyl-2-butanol, 3-methyl-1-butanol, 3-methyl 2,2-dimethyl-1-propanol, and 2,2-dimethyl-1-propanol. Mixtures of one or more of these alcohols may be used, including but not limited to:

[0051] B. Polymers and Polymer Compositions In one embodiment, a composition is disclosed that includes a thermoplastic polymer and biomass, the biomass being The composition contains lignin, and the composition contains cellulose and and / or hemicellulose.

[0052] The present invention relates to lignin, for example hardwood lignin, softwood lignin, herbaceous lignin, or provides polymers or polymer compositions comprising these combinations. In the present invention, the polymer or polymer composition further comprises acridine orange (AO). In certain embodiments, hardwood lignin, softwood lignin, and / or herbaceous lignin can be used. The lignin is prepared by the disclosed process.

[0053] Without wishing to be bound by any theory, it is believed that the composition of lignin varies from species to species. Briefly, the three monolignol monomers are the precursors of lignin and All of these are methoxylated to various degrees. These include p-coumaryl alcohol, coumarin, These lignols include niferyl alcohol and sinapyl alcohol. The phenylpropanoids p-hydroxyphenyl (H), guaiacyl (G), and cyclohexyl (C) are It is incorporated into lignin in the form of linoleic acid (S). Gymnosperms contain almost entirely G and small amounts of Dicotyledonous angiosperms have lignin composed of H, whereas dicotyledonous angiosperms are mostly a mixture of G and S. Finally, monocotyledonous lignins contain all three (i.e., H, G, and Many herbs have mostly G, but some palms have mostly S. All lignins contain small amounts of incomplete or modified monolignols. Other monomers are prominent in woody plants.

[0054] In certain embodiments, the lignin is substantially free of cellulose. Thus, for example, , the lignin is less than about 20% by weight, less than about 15% by weight, less than about 1% by weight, based on the total weight of the lignin. % cellulose, less than about 5% cellulose, or less than about 1% cellulose. Cut.

[0055] In certain embodiments, the lignin is substantially free of hemicellulose. For example, the lignin may be present in an amount of less than about 20% by weight, less than about 15% by weight, based on the total weight of the lignin. Contains less than about 10% by weight, less than about 5% by weight, or less than about 1% by weight hemicellulose. It is possible.

[0056] In certain embodiments, the lignin is either cellulose or hemicellulose. Thus, for example, lignin is substantially free of both cellulose and hemicellulose. The total weight of the lignin is less than about 20%, less than about 15%, or less than about 10% by weight. %, less than about 5% by weight, or less than about 1% by weight.

[0057] The present invention also provides a polymer or polymer composition comprising a biomass consisting essentially of lignin. Thus, in certain embodiments, the biomass provides a composition comprising: Based on, at least about 60%, at least about 65%, at least about 70%, at least At least about 75%, at least about 80%, at least about 85%, at least about 90%, at least at least about 91%, at least about 92%, at least about 93%, at least about 94%, at least about 95%, at least about 96%, at least about 97%, at least about 98%, The lignin content is about 99%, or about 100%.

[0058] A polymer-lignin composite comprises at least one polymer and lignin. Each of the components and the lignin component is greater than 0% by weight based on the weight of the dry composite. In one embodiment, at least two components are present in an amount ranging from 0.1 to 100% by weight. Each of the components is present in an amount ranging from at least 2% by weight to at most 98% by weight based on the weight of the composite. In one embodiment, each of the at least two components is present in an amount ranging from about 100 to about 1500 by weight of the composite. Based on the total amount of the stearate, the stearate is present in an amount ranging from at least 5% to at most 95% by weight.

[0059] Lignin (e.g., herbaceous lignin or hardwood lignin) can be used in any suitable amount to form the polyolefin. The polymer may be used in a polymer or polymer composition, such as a thermoplastic polymer. ,The amount is 0.01, 0.02, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0 .6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6 , 1.7, 1.8, 1.9, 2, 2.2, 2.4, 2.6, 2.8, 3, 3.2, 3.4 , 3.6, 3.8, 4, 4.2, 4.4, 4.6, 4.8, 5, 5.5, 6, 6.5, 7 , 7.5, 8, 8.5, 9, 9.5, 10, 11, 12, 13, 14, 15, 16, 18 , 20, 22, 24, 26, 28, 30, 32, 34, 36, 38, 40, 42, 44, 46, 48, 50, 55, 60, 65, 70, 75, 80, 85, 90, or 95 (weight Each of the above numbers may be preceded by the words "about," "at least about," " or "less than about" and any of the above numerical values ​​may be used alone. open-ended ranges or combined to provide closed-ended ranges. For example, lignin can be present in a polymer or polymer composition at a concentration of 0.1 to 3.0% by weight. Alternatively, it may be used in an amount of 0.3 to 2.0% by weight, or 10 to 60% by weight. Lignin may be obtained from biomass as described elsewhere herein. Suitable biomass includes switchgrass, silvergrass, turfgrass, broad-leaved grass, and These include, but are not limited to, leafy trees, ornamental grasses, and cereal grains such as sorghum, barley, and wheat. As disclosed herein, lignin is a polymer or polymer composition. is present in a coating, film, adhesive, or personal care composition. The present invention can be used in any composition for antioxidant purposes, including, but not limited to, ethylhexyl esters such as ethylhexyl esters.

[0060] Thus, in certain embodiments, the polymer or polymer composition is a thermoplastic, Thermosets, composites, coatings, films, adhesives, personal care compositions, or any combination thereof.

[0061] In certain embodiments, the oxidation onset temperature of the polymer or polymer composition comprising herbaceous lignin is The degree of lignin content is 100%, except that it contains kraft lignin or hardwood lignin instead of herbaceous lignin. At least 10° C. higher than the same polymer or polymer composition.

[0062] In certain embodiments, the polymer or polymer composition is subjected to acid treatment at a temperature of about 232° C. to about 250° C. In one such embodiment, the polymer is polypropylene. In one such embodiment, the herbaceous lignin is switchgrass lignin.

[0063] In certain embodiments, the polymer or polymer composition is a thermoplastic.

[0064] In certain embodiments, the thermoplastic material is polyethylene, polypropylene, or Includes a combination of.

[0065] Other suitable components of the polymer or polymer composition include fillers (e.g., talc, calcium carbonate, etc. calcium, glass fiber, etc.), colorants (e.g. inorganic pigments, e.g. titanium dioxide, carbon black, metal salts, etc., or organic colorants, e.g. phthalocyanine blue), and others. Additives such as compatibilizers (e.g. graft modified polymers, block copolymers, silanes etc.), processing aids (e.g. waxes, lubricants, zinc stearate, etc.), wear resistance aids ( Lubricants such as polytetrafluoroethylene, PTFE, oil, silicone, etc. ), antiblocking aids (e.g., talc), antistatic agents (metals, e.g., stainless steel fibers, ionic salts, etc.), nucleating agents (e.g. sorbitol, minerals, metal salts, etc.), Flame retardants (bromine-containing compounds, phosphorus-containing compounds, magnesium hydroxide, etc.), Or it can be any combination thereof.

[0066] The polymer to be stabilized (or the polymer of the polymer-lignin complex) can be any polymer. - for example, thermosetting polymers, thermoplastic polymers, coatings, films, adhesives, personal care compositions, or combinations thereof. In certain embodiments, the polymer may be a thermoplastic polymer. In certain embodiments, the polymer may be polyethylene, polypropylene, or the like. pyrene, polyesters (e.g., poly(ethylene terephthalate)), polyamides (e.g., polyamides, including, for example, aliphatic, aromatic or semi-aromatic polyamides, or any combination thereof. The stabilizing polymer may comprise, consist essentially of, or consist of polypropylene. , polyethylene, polyvinyl chloride (PVC), polyvinyl acetate (PVA), chlorinated polyethylene Styrene, polystyrene, acrylonitrile-butadiene-styrene (ABS) copolymer , ethylene-vinyl acetate copolymer, PVC / ABS blend, polyethylene terephthalate (PET), Polycarbonate, Polyurethane, Acrylic, Styrene-Acrylic, Polyurethane These include, but are not limited to, polyamides, nylons, elastomers, and the like. Any of the polymers herein may be used alone or in any combination (e.g., with other synthetic The polymer may be present in the form of a solvent or a carrier. It may be present as bulk (dry) polymer without any solvent or in a solvent solution. It may be in a liquid or dispersion, or in an aqueous solution or dispersion, or in a dry film. Thus, in various embodiments, the stabilizer may be present as a coating or a stabilizing agent. The polymer to be cured is processed at a temperature (i.e., melting or softening) below the scorch point of lignin. In various alternative embodiments, the stabilized polymer may be a polymer having a The mer can be a polymer that has a processing temperature of less than about 400°C.

[0067] The activity of antioxidants was measured according to ASTM 2009-02 (charcoal by differential scanning calorimetry (DSC) The standard test method for hydrogen oxidation onset temperature can be used to evaluate the lignin content of herbaceous lignin. For example, switchgrass lignin has a higher resistance to oxidative degradation of the polymer than other lignins. For example, at a concentration of 1.0 wt%, switchgrass lignin provides excellent protection against Usually, polypropylene (Bapolene® 4012F, Bamberger Pol The oxidation onset temperature of the same polymer was (compared to hardwood lignin and kraft lignin at the same concentration at about 230°C) Raise the temperature from about 200°C to about 244°C.

[0068] In certain embodiments, the composition comprises kraft lignin or broadleaf lignin instead of herbaceous lignin. It has an oxidation onset temperature at least 10°C higher than an identical composition except that it contains wood lignin. do.

[0069] 1. Herbaceous lignin In certain embodiments, the lignin is herbaceous lignin. In certain embodiments, the herbaceous lignin is switchgrass lignin. A large amount of hydroxycinnamic acid units ether-linked to ferulic acid and p-chloro For example, herbaceous lignin contains p-hydroxyphenyl, guaiacinamide units. The copolymer may contain a mixture of syringyl, cyclic, and syringyl units.

[0070] In certain embodiments, the herbaceous lignin has a particle size of less than about 600 μm, about Less than 550 μm, less than about 500 μm, less than about 450 μm, less than about 400 μm, about 350 μm m or less, less than about 300 μm, less than about 250 μm, less than about 200 μm, less than about 150 μm, Less than about 125 μm, Less than about 100 μm, Less than about 75 μm, Less than about 50 μm, Less than about 25 μm Average particle size d of less than about 10 μm or less than about 5 μm (50) has.

[0071] In certain embodiments, herbaceous lignin can be obtained by hydrolysis of herbaceous biomass with a fluid, e.g. For example, it can be obtained by subcritical, near-critical, or supercritical hydrolysis. Examples of fluids are water, methanol, etc. ethanol, propanol, butanol, carbon dioxide, sulfur dioxide, or The present invention includes, but is not limited to, any combination of these. The decomposition is supercritical hydrolysis. As described in further detail herein, the preparation process includes a pretreatment In certain embodiments, a pretreatment step may be included, but such a pretreatment step is not required. The process may include treatment steps, as further detailed herein.

[0072] In certain embodiments, the herbaceous lignin is obtained by hydrolysis, e.g., supercritical hydrolysis. Hydrolysis can be achieved by varying pressures, e.g., 1, 5, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 125, 130, 140, 150, 160, 17 0, 175, 180, 190, 200, 210, 220, 221, 225, 230, 24 0, 250, 260, 270, 275, 280, 290, 300, 310, 320, 32 5, 330, 340, 350, 360, 370, 375, 380, 390, 400, 42 0, 440, 450, 460, 475, 480, 500, 525, 550, 575, 60 0, 625, 650, 675, 700, 725, 750, 775, or 800 (bar The hydrolysis can be carried out at temperatures such as 374, 375, 380, 39 0, 400, 410, 420, 430, 440, 450, 460, 470, 480, 49 0, 500, 510, 520, 530, 540, 550, 560, 570, or 575 (° C.). Each of the above numbers may be preceded by the words "about," "at least The above numerical values ​​may be used alone to indicate the amount of the List open-ended ranges or combine them to list closed-ended ranges Thus, in certain embodiments, the herbaceous lignin can reduce the herbaceous biomass by about 3 For fluids with temperatures between 40°C and 400°C and pressures between 225 bar and 250 bar. It is obtained by exposure.

[0073] Traditionally, antioxidants for polymers are provided as additives, typically at 0.05-10 wt.%. (solids on solids) range for use as an antioxidant in polymers. The herbaceous lignins disclosed herein (e.g., switchgrass lignin) can also be used as polymer additives. However, as disclosed herein and further described below, As such, herbaceous lignin also acts as a polymer filler (or thickener) that acts as an antioxidant. Therefore, the herbaceous lignin content is as high as 95% by weight. There are cases.

[0074] The polymer-lignin composite comprises at least one polymer and herbaceous lignin. Each of the polymeric and herbaceous lignin components is 0.05 wt., based on the weight of the dry composite. In one embodiment, the glycerol is present in an amount ranging from greater than 100% by weight up to less than 100% by weight. Each of the two components is present in an amount of at least 2% by weight and at most 9% by weight based on the weight of the composite. 8% by weight. In one embodiment, each of the at least two components is present in an amount ranging from at least 5% by weight to at most 95% by weight based on the weight of the composite .

[0075] Herbaceous lignin (e.g., switchgrass lignin) can be used in any suitable amount as a polymer or or polymer compositions, such as thermoplastic polymers. For example, the amount ,0.01,0.02,0.05,0.1,0.2,0.3,0.4,0.5,0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1. 7, 1.8, 1.9, 2, 2.2, 2.4, 2.6, 2.8, 3, 3.2, 3.4, 3. 6, 3.8, 4, 4.2, 4.4, 4.6, 4.8, 5, 5.5, 6, 6.5, 7, 7. 5, 8, 8.5, 9, 9.5, 10, 11, 12, 13, 14, 15, 16, 18, 20 , 22, 24, 26, 28, 30, 32, 34, 36, 38, 40, 42, 44, 46, 48, 50, 55, 60, 65, 70, 75, 80, 85, 90, or 95 (by weight) Each of the above numbers may be preceded by the terms "about," "at least about," and The above figures may be used alone to indicate open ended transactions. Ended ranges may be written or combined to write close-ended ranges. For example, herbaceous lignin may be present in a polymer or polymer composition at a concentration of 0.1 to 3.0% by weight. It can be used in an amount of 0.3 to 2.0% by weight, or 10 to 60% by weight. The lignin is derived from herbaceous biomass as described elsewhere herein. Suitable biomass includes switchgrass, Miscanthus sinensis (silvergrass), These include turfgrasses, ornamental grasses, and cereals such as sorghum, barley, and wheat, but are not limited to these. As disclosed herein, herbaceous lignin may be used as a polymer or polymer composition. The composition is present in a coating, film, adhesive, or personal care composition. The composition may be used in any composition for antioxidant purposes, including those containing

[0076] Herbaceous lignin is 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8 , 0.9, 1.0, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 , 2.0, 2.2, 2.4, 2.6, 2.8, 3.0, 3.5, 4.0, 4.5, 5.0 , 5.5, 6.0, 6.5, 7.0, 7.5, 8.0, 8.5, 9.0, 9.5, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 25, 30, 40, 5 0 (micrometers), the diameter / maximum dimension. Each of the terms may be preceded by the term "about," "at least about," or "less than about." Any of the above values ​​may be used alone or in combination to describe an open-ended range. The range of close ends can also be listed. For example, herbaceous lignin is 1. Average particle size (micrometers) of 0 to 10.0 or 2 to 8 micrometers It is possible.

[0077] Herbaceous lignin is 0.1, 0.5, 1.0, 1.5, 2.0, 5.0, 6.0, 7.0 , 8.0, 9.0, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 2 The carbohydrate content may be 0, 25, 30, 40, or 50%. Each of the above may be preceded by the term "about," "at least about," or "less than about." Any of the above numerical values ​​may be used alone or in combination to describe an open-ended range. For example, herbaceous lignin has a close-end range of 1.0 It may have a carbohydrate content of 15.0, or 2-8%.

[0078] Biomass, including switchgrass biomass, is typically made up of cellulose, hemicellulose, and lignin. Herbaceous lignin is obtained, for example, by hydrolyzing herbaceous biomass with a fluid. The cellulose can be derived from herbaceous biomass by any suitable method, including by Hydrolysis can involve one or more steps (2, 3, 4, 5, 6, 7, 8, or 9 or more). The temperatures, pressures, and times described herein include It can be applied to any single step. For example, the hydrolysis process is carried out in two steps. The first step may be carried out at temperatures, pressures, and residence times as disclosed herein. and the second step is carried out at any of the temperatures, pressures, and times disclosed herein. has.

[0079] The fluids are water, methanol, ethanol, propanol, butanol, carbon dioxide, diacid or any combination thereof. In an embodiment, the fluid comprises, consists of, or consists essentially of water.

[0080] In certain embodiments, the herbaceous biomass (e.g., switchgrass) is grown in a subcritical, near-critical, or This process involves subjecting herbaceous biomass to a first temperature and and pretreating the biomass under a first pressure for a first period of time, thereby forming a pretreated biomass. As used herein, a pretreatment step typically involves the removal of wastewater from biomass. Extracting hemicellulose (if present) while extracting cellulose (if present) ) and lignin (i.e., the product of the pretreatment step is referred to herein as "pretreated biomass"). The process involves subjecting the pretreated biomass to a second temperature and a second pressure. In some embodiments, the method further comprises treating the substrate under a force for a second period of time. The process includes a treatment step and does not include a pretreatment step. In other words, as defined herein Herbaceous biomass that has not been subjected to a pretreatment process involving a fluid is subjected to a treatment process involving a fluid. Prior to the treatment step, the herbaceous biomass may be comminuted (e.g., by mechanical means, e.g., For example, by crushing, grinding, crushing by impact, etc., or by explosive decompression, e.g. steam explosion. This grinding is not considered a pretreatment step as used herein. When using a fluid containing The method may include treating the herbaceous biomass with

[0081] In some embodiments, if desired, the herbaceous biomass is typically about 600 microns. Average particle size d less than 500 micrometers or less than 500 micrometers (50) To manufacture For this reason, size reduction may be performed prior to subcritical, near supercritical, or supercritical hydrolysis. In certain embodiments, size reduction may be achieved by culturing herbaceous biomass in the presence of ammonia. In certain embodiments, the size reduction comprises exploding the grass in the presence of sulfur dioxide. This involves exploding the biomass, although size reduction may not be necessary.

[0082] In certain embodiments, subcritical, near supercritical, or supercritical hydrolysis or the like as described herein may be used. Any other hydrolyzable (e.g., enzymatic) herbaceous biomass shown is measured by light scattering. The average particle size d is less than about 600 μm or less than about 500 μm. (50) , for example, the average Particle size, d (50) are 5, 10, 25, 50, 75, 100, 125, 150, 200, 250, 300, 350, 400, 450, 500, 550, 600 (micrometers Each of the foregoing numbers may be preceded by the words "about," "at least about," or "less than approximately" may be added, and any of the above figures may be used to open a single can be combined to describe a closed-ended range. For example, the average particle diameter d (50) is about 50μm to about 600μm, about 50μm to about 50 0 μm, about 50 μm to about 450 μm, about 25 μm to about 250 μm, or about 100 μm to It can be about 400 μm.

[0083] In certain embodiments, the size-reduced herbaceous biomass preferably comprises the size-reduced herbaceous biomass described herein. is mixed with a fluid, e.g., a fluid that comprises, consists of, or consists essentially of water, The mixture is then hydrolyzed at a temperature of at least about 100° C. In this embodiment, the mixture or the fluid in contact with the mixture itself may be heated to 100, 120, 140° C. , 150℃, 160℃, 170℃, 180℃, 190℃, 200℃, 210℃, 220℃ , 230℃, 240℃, 250℃, 260℃, 280℃, 300℃, 320℃, 340℃ , 350℃, 360℃, 370℃, 374.2℃, 380℃, 390℃, 400℃, 41 0℃, 420℃, 440℃, 450℃, 460℃, 480℃, 500℃, 520℃, 54 The temperature (°C) is 0°C, 560°C, 580°C, or 600°C. may be preceded by the words "about," "at least about," or "less than about," Numerical values ​​may be used alone or in combination to provide open-ended ranges. The range of the rose end can be described. For example, the mixture can be heated to 190°C to 374°C. Alternatively, the mixture may be hydrolyzed at a temperature between 374° C. and 500° C., or The mixture may be hydrolyzed at a temperature of greater than 500° C. In certain embodiments, the mixture may be hydrolyzed at a temperature of greater than 100° C. Hydrolysis at temperatures between 500°C and 500°C under sufficient pressure to ensure that all fluids are in liquid form. In some such embodiments, the mixture is substantially free of exogenous acids. In some such embodiments, the mixture is substantially free of Ci-05 alcohols. If desired, one or more preheat steps can also be used in each embodiment.

[0084] In certain embodiments, the herbaceous biomass comprises, consists of, or is composed of, for example, water. and mixing the mixture with a fluid essentially consisting of the mixture, the mixture being subjected to supercritical hydrolysis, and The article is heated to a temperature of at least about 374° C., for example, from about 374.2° C. to about 575° C., and The mixture is subjected to a pressure of at least about 221 bar for a period of time sufficient to produce at least one C6 sugar. When the mixture is subjected to supercritical hydrolysis, the water in contact with the mixture is heated to a temperature of at least about 374°C. The water in contact with the mixture has temperatures of 374, 375, 380, 390, 400, 41 0, 420, 430, 440, 450, 460, 470, 480, 490, 500, 51 The temperatures are 0, 520, 530, 540, 550, 560, 570, and 575°C. Each of the foregoing numbers may be preceded by the word "about," "at least about," or "less than about." Any of the above values ​​may be used alone to describe an open-ended range, or or combinations of compounds may be used to describe the close-ended range. The water in contact has a temperature bounded by any two of the aforementioned endpoints. For example, water can be heated at temperatures ranging from about 374°C to about 575°C, from about 374°C to about 450°C, 400°C to about 520°C, or about 375°C to about 430°C, In certain embodiments, the pressure may be at least about 221 bar. The water may have a temperature greater than 575° C. and be under a pressure of at least about 221 bar. In some such embodiments, the mixture is substantially free of exogenous acid. In some such embodiments, the mixture is substantially free of C1-05 alcohols. If desired, an additional preheat step can also be used in each embodiment.

[0085] In embodiments where the mixture is subjected to subcritical, near supercritical, or supercritical hydrolysis, the hydrolysis may be carried out by: 1, 5, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 1 20, 125, 130, 140, 150, 160, 170, 175, 180, 190, 2 00, 210, 220, 221, 225, 230, 240, 250, 260, 270, 2 75, 280, 290, 300, 310, 320, 325, 330, 340, 350, 3 60, 370, 375, 380, 390, 400, 420, 440, 450, 460, 4 75, 480, 500, 525, 550, 575, 600, 625, 650, 675, 7 The pressure is 0, 725, 750, 775, or 800 (bar). Each of the above may be preceded by the word "about," "at least about," or "less than about." Any of the above numerical values ​​may be used alone or in combination to describe an open-ended range. For example, the pressure is approximately 221 bar. ~800bar, 230bar~500bar, 325bar~750bar In certain embodiments, the pressure may be from about 275 bar to about 350 bar. The force may be greater than 800 bar.

[0086] In certain embodiments where the mixture is subjected to near-supercritical or supercritical hydrolysis, as the hydrolysis continues, Between are 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1 .0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2 .0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, 6.0, 7.0, 8.0, 9 .0, 10.0, 15, 20, 30, 40, 50, 60, 70, 80, 90, 100, 1 20, 140, 160, 180, 200, 220, 240, 260, 280, or 30 Each of the foregoing numbers may be preceded by the words "about," "at least about," or " "less than about" may be used in an open-ended statement by itself using any of the above numerical values. Ranges can be written or combined to write close-ended ranges. For example, the duration is about 0.1 seconds to about 10 seconds, about 0.1 seconds to about 5 seconds, about 0.1 seconds to about 0.3 seconds , about 1.1 seconds to about 5 seconds, or about 0.9 seconds to about 9 seconds. In the preferred embodiment, the duration is greater than 10 seconds. The mixture is subjected to a lower temperature (e.g., about 0.1 seconds to about 1.4 seconds). In certain embodiments, the duration of hydrolysis is 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 6, 7, 8, 9, 10, 15, 20, 25, 30 , 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, or 300 (minutes). Each of the foregoing numbers may be preceded by the word "about," "at least about," or "less than about" and any of the above numerical values ​​may be used alone. open-ended ranges or combined to provide closed-ended ranges. Cut.

[0087] In certain embodiments, the mixture containing herbaceous biomass to be subsequently hydrolyzed comprises C1-0 5. Substantially free of alcohol. In certain embodiments, the mixture is substantially free of exogenous acids. Optionally, in each embodiment, one or more preheating steps may also be performed prior to hydrolysis. In another embodiment, the mixture can be used in ) any C1-05 alcohol, exogenous acid, or any combination thereof.

[0088] In certain embodiments, the solids content of the mixture based on the total weight of the mixture is about 1% by weight or more, e.g. For example, 1% to 40% by weight. The solid content of the mixture is 1, 2, 3, 4, 5, 6, 7, 8 , 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 2 2, 23, 24, 25, 26, 27, 28, 29, 30, 32, 34, 36, 38, 40 Each of the foregoing numbers may be preceded by the words "about," "at least "at least about," "less than about," or "less than about" may be used to indicate any of the numerical values ​​listed above. Alone to describe open-ended ranges or in combination to describe closed-ended ranges For example, the solid content of the mixture can be about 10% by weight to about 29% by weight, about 15% by weight, or about 29% by weight. % to about 29% by weight, about 10% to about 18% by weight, or about 24% to about 27% by weight It can be said that:

[0089] 2. Hardwood lignin In certain embodiments, the lignin is a hardwood lignin. For example, the hardwood lignin may be In another particular embodiment, the aryl group may include a mixture of guaiacyl, syringyl, and syringyl units. Therefore, hardwood lignin cannot contain p-hydroxyphenyl.

[0090] In certain embodiments, the hardwood lignin has a particle size of less than about 600 μm as measured by light scattering; Less than about 550 μm, less than about 500 μm, less than about 450 μm, less than about 400 μm, less than about 350 Less than μm, Less than about 300 μm, Less than about 250 μm, Less than about 200 μm, Less than about 150 μm , less than about 125 μm, less than about 100 μm, less than about 75 μm, less than about 50 μm, about 25 μm Average particle size d of less than about 10 μm, or less than about 5 μm (50) has.

[0091] In certain embodiments, hardwood lignin can be prepared by hydrolysis of biomass with a fluid, e.g., by hydrolysis of chloroform. It is obtained by supercritical, near-critical, or supercritical hydrolysis. Examples of fluids are water, methanol, and alcohol, ethanol, propanol, butanol, carbon dioxide, sulfur dioxide, or any of the above. In certain embodiments, the hydrolysis may include, but is not limited to, any combination of is supercritical hydrolysis. As further detailed herein, the preparation process includes a pretreatment step However, such a pretreatment step is not required. The process may include processing steps, as further detailed herein.

[0092] In certain embodiments, the hardwood lignin is obtained by hydrolysis, e.g., supercritical hydrolysis. Hydrolysis can be achieved by varying the pressure, e.g., 1, 5, 10, 20, 30, 40, 50, 60, 70 , 80, 90, 100, 110, 120, 125, 130, 140, 150, 160, 1 70, 175, 180, 190, 200, 210, 220, 221, 225, 230, 2 40, 250, 260, 270, 275, 280, 290, 300, 310, 320, 3 25, 330, 340, 350, 360, 370, 375, 380, 390, 400, 4 20, 440, 450, 460, 475, 480, 500, 525, 550, 575, 6 00, 625, 650, 675, 700, 725, 750, 775, or 800(ba The hydrolysis can be carried out at temperatures such as 374, 375, 380, 3 90, 400, 410, 420, 430, 440, 450, 460, 470, 480, 4 90, 500, 510, 520, 530, 540, 550, 560, 570, or 57 Each of the above numbers may be preceded by the words "about," "at least The term "about" or "less than about" may be used alone to refer to any of the numerical values ​​listed above. You can list open-ended ranges or combine them to list closed-ended ranges. Thus, in certain embodiments, hardwood lignin can reduce biomass to about 34%. The fluid has a temperature of 0°C to about 400°C and a pressure of about 225 bar to about 250 bar. This is obtained by subtracting

[0093] Traditionally, antioxidants for polymers are provided as additives, typically at 0.05-10 wt.%. (solids on solids) range for use as an antioxidant in polymers. The hardwood lignins disclosed herein may also be utilized in this manner as polymer additives. However, as disclosed herein and further described below, hardwood lignins are still It may also be utilized as a polymeric filler (or extender) that also functions as an antioxidant. Thus, the hardwood lignin content can be as high as 95% by weight.

[0094] The polymer-lignin composite comprises at least one polymer and hardwood lignin. Each of the polymer component and the hardwood lignin component comprises, based on the weight of the dry composite, In one embodiment, the at least one hydroxypropyl ester is present in an amount ranging from greater than 0% to less than 100% by weight. Each of at least two components is present in an amount of at least 2% by weight, based on the weight of the composite, and at most In one embodiment, each of the at least two components is present in an amount ranging from 98% by weight to 100% by weight. is present in an amount ranging from at least 5% by weight to at most 95% by weight based on the weight of the composite. do.

[0095] The hardwood lignin can be used in any suitable amount as a polymer or polymer composition, such as a thermoplastic polymer. For example, amounts of 0.01, 0.02, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1. 1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.2, 2.4, 2.6, 2.8, 3, 3.2, 3.4, 3.6, 3.8, 4, 4.2, 4.4, 4.6, 4.8, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10 , 11, 12, 13, 14, 15, 16, 18, 20, 22, 24, 26, 28, 30, 32, 34, 36, 38, 40, 42, 44, 46, 48, 50, 55, 60, 65, 7 It can be 0, 75, 80, 85, 90, or 95 (wt%). each may be preceded by the term "about," "at least about," or "less than about," Any of the above values ​​may be used alone or in combination to describe an open-ended range. For example, hardwood lignin is a polymer or 0.1 to 3.0% by weight, or 0.3 to 2.0% by weight, or The hardwood lignin may be used in an amount of 10 to 60% by weight. As disclosed herein, the present invention can be obtained from biomass as described elsewhere herein. Thus, hardwood lignin is a polymer or polymer composition that can be used in coatings, films, and adhesives. Any composition for antioxidant purposes, including compositions present in adhesives, or personal care compositions. It can be used in compositions.

[0096] Hardwood lignin is 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0. 8, 0.9, 1.0, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1. 9, 2.0, 2.2, 2.4, 2.6, 2.8, 3.0, 3.5, 4.0, 4.5, 5. 0, 5.5, 6.0, 6.5, 7.0, 7.5, 8.0, 8.5, 9.0, 9.5, 10 , 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 25, 30, 40, 50 (micrometers), the diameter / maximum dimension. Each numerical value may be preceded by the term "about," "at least about," or "less than about." Any of the above values ​​may be used alone to describe an open-ended range, or in combination. For example, hardwood lignin has the following close-end range: Average particle size (micrometers) of 1.0 to 10.0 or 2 to 8 micrometers It is possible to have.

[0097] Hardwood lignin is 0.1, 0.5, 1.0, 1.5, 2.0, 5.0, 6.0, 7. 0, 8.0, 9.0, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, The carbohydrate content may be 20, 25, 30, 40, or 50%. Each of the terms may be preceded by the term "about," "at least about," or "less than about." Any of the above values ​​may be used alone or in combination to describe an open-ended range. For example, hardwood lignin has a range of 1 It can have a carbohydrate content of .0-15.0, or 2-8%.

[0098] Biomass typically contains cellulose, hemicellulose, and lignin. The lignin can be extracted by any suitable method, including, for example, hydrolyzing the biomass with a fluid. Hydrolysis can be carried out in one or more steps. (2, 3, 4, 5, 6, 7, 8, or 9 or more hydrolysis steps). The temperatures, pressures, and times described can be applied to any single step. For example, the hydrolysis process can be carried out in two steps, the first of which is described herein. and the second step has any of the temperatures, pressures, and residence times disclosed herein. With any of the temperatures, pressures, and times indicated.

[0099] The fluids are water, methanol, ethanol, propanol, butanol, carbon dioxide, diacid or any combination thereof. In an embodiment, the fluid comprises, consists of, or consists essentially of water.

[0100] In certain embodiments, the biomass is subjected to subcritical, near-critical, or supercritical hydrolysis. The process includes pretreating biomass at a first temperature and a first pressure for a first period of time, This can include a pretreatment step, thereby forming a pretreated biomass. The pretreatment steps used usually involve the extraction of hemicellulose (if present) from the biomass. while leaving behind the cellulose (if present) and lignin (i.e., pretreatment The product of the pretreatment process is referred to herein as "pretreated biomass." and treating the biomass at a second temperature and a second pressure for a second period of time. In some embodiments, the process includes a treatment step, and may further include a pretreatment step. In other words, biomass that has not been subjected to a pretreatment step as defined herein does not include However, prior to the treatment step, the biomass may be crushed. Burrs (e.g. by mechanical means, e.g. crushing, grinding, crushing by impact, etc., or by explosion) This comminution is referred to as a pretreatment process as used herein. When a fluid containing supercritical water is used, the process is not considered a This may include treating the biomass with supercritical water without a pretreatment step being performed.

[0101] In some embodiments, if desired, the biomass is typically about 600 micrometers. Average particle size d less than 100 μm or less than 500 μm (50) In order to manufacture The size reduction described above may be carried out prior to subcritical, near supercritical, or supercritical hydrolysis. In certain embodiments, the size reduction is achieved by exploding the biomass in the presence of ammonia. In certain embodiments, the size reduction comprises exploding the biomass in the presence of sulfur dioxide. However, size reduction may not be necessary.

[0102] In certain embodiments, subcritical, near supercritical, or supercritical hydrolysis or the like as described herein may be used. Any other hydrolyzed (e.g., enzymatic) biomass shown was measured by light scattering. Average particle size d of less than about 600 μm or less than about 500 μm (50) , e.g., average particle size , d (50) 5, 10, 25, 50, 75, 100, 125, 150, 200, 250 , 300, 350, 400, 450, 500, 550, 600 (micrometers, μm Each of the foregoing numbers may be preceded by the word "about," "at least about," or "Less than about" may be used, and any of the above numerical values ​​may be used alone to form an open-ended statement. ranges can be written, or combined to write close-ended ranges. For example, the average particle size d (50) is about 50μm to about 600μm, about 50μm to about 500μm , about 50 μm to about 450 μm, about 25 μm to about 250 μm, or about 100 μm to about 40 It can be set to 0 μm.

[0103] In certain embodiments, the size-reduced biomass as described herein is preferably a fluid. , for example, with a fluid that comprises, consists of, or consists essentially of water, thereby A mixture is formed, and the mixture is hydrolyzed at a temperature of at least about 100° C. In the form, the mixture or the fluid in contact with the mixture itself is heated to 100, 120, 140 °C, 15 0℃, 160℃, 170℃, 180℃, 190℃, 200℃, 210℃, 220℃, 23 0℃, 240℃, 250℃, 260℃, 280℃, 300℃, 320℃, 340℃, 35 0℃, 360℃, 370℃, 374.2℃, 380℃, 390℃, 400℃, 410℃, 420℃, 440℃, 450℃, 460℃, 480℃, 500℃, 520℃, 540℃, The temperature (°C) is 560°C, 580°C, or 600°C. may be preceded by the words "about," "at least about," or "less than about," and Either can be used alone to describe an open-ended range, or in combination to describe a closed For example, the mixture can be heated at temperatures between 190°C and 374°C. Alternatively, the mixture may be hydrolyzed at a temperature between 374°C and 500°C, or In certain embodiments, the mixture may be hydrolyzed at a temperature of from 100° C. to 50° C. At a temperature of 00°C, all fluids are hydrolyzed under sufficient pressure to ensure that they are in liquid form. In some such embodiments, the mixture is substantially free of exogenous acids. In such embodiments, the mixture is substantially free of Ci-05 alcohols. Accordingly, in each embodiment, one or more preheat steps may also be used.

[0104] In certain embodiments, the biomass comprises, consists of, or essentially consists of, e.g., water. and mixing the mixture with a fluid that is Temperatures of at least about 374° C., for example from about 374.2° C. to about 575° C., and at least A pressure of about 221 bar is applied for a time sufficient to produce at least one C6 sugar. When the mixture is subjected to supercritical hydrolysis, the water in contact with the mixture has a temperature of at least about 374° C. Water in contact with the mixture has 374, 375, 380, 390, 400, 410, 4 20, 430, 440, 450, 460, 470, 480, 490, 500, 510, 5 20, 530, 540, 550, 560, 570, 575 (℃). Each numerical value may be preceded by the word "about," "at least about," or "less than about." Any of the above values ​​may be used alone to describe an open-ended range, or in combination. Therefore, the range of the close end can be described by combining the The water to be treated must have a temperature bounded by any two of the aforementioned endpoints. For example, water can be heated at temperatures between about 374°C and about 575°C, between about 374°C and about 450°C, and between about 400°C and about ℃ to about 520 ℃, or about 375 ℃ to about 430 ℃, in each case , and may be under a pressure of at least about 221 bar. In certain embodiments, the water is It may have a temperature greater than 575° C. and be under a pressure of at least about 221 bar. In some such embodiments, the mixture is substantially free of exogenous acid. In such embodiments, the mixture is substantially free of C1-05 alcohols. Optionally, in each embodiment, an additional preheat step may also be used.

[0105] In embodiments where the mixture is subjected to subcritical, near supercritical, or supercritical hydrolysis, the hydrolysis may be carried out by: 1, 5, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 1 20, 125, 130, 140, 150, 160, 170, 175, 180, 190, 2 00, 210, 220, 221, 225, 230, 240, 250, 260, 270, 2 75, 280, 290, 300, 310, 320, 325, 330, 340, 350, 3 60, 370, 375, 380, 390, 400, 420, 440, 450, 460, 4 75, 480, 500, 525, 550, 575, 600, 625, 650, 675, 7 The pressure is 0, 725, 750, 775, or 800 (bar). Each of the above may be preceded by the word "about," "at least about," or "less than about." Any of the above numerical values ​​may be used alone or in combination to describe an open-ended range. For example, the pressure is approximately 221 bar. ~800bar, 230bar~500bar, 325bar~750bar In certain embodiments, the pressure may be from about 275 bar to about 350 bar. The force may be greater than 800 bar.

[0106] In certain embodiments where the mixture is subjected to near-supercritical or supercritical hydrolysis, as the hydrolysis continues, Between are 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1 .0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2 .0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, 6.0, 7.0, 8.0, 9 .0, 10.0, 15, 20, 30, 40, 50, 60, 70, 80, 90, 100, 1 20, 140, 160, 180, 200, 220, 240, 260, 280, or 30 Each of the foregoing numbers may be preceded by the words "about," "at least about," or " "less than about" may be used in an open-ended statement by itself using any of the above numerical values. Ranges can be written or combined to write close-ended ranges. For example, the duration is about 0.1 seconds to about 10 seconds, about 0.1 seconds to about 5 seconds, about 0.1 seconds to about 0.3 seconds , about 1.1 seconds to about 5 seconds, or about 0.9 seconds to about 9 seconds. In the preferred embodiment, the duration is greater than 10 seconds. The mixture is subjected to a lower temperature (e.g., about 0.1 seconds to about 1.4 seconds). In certain embodiments, the duration of hydrolysis is 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 6, 7, 8, 9, 10, 15, 20, 25, 30 , 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, or 300 (minutes). Each of the foregoing numbers may be preceded by the word "about," "at least about," or "less than about" and any of the above numerical values ​​may be used alone. open-ended ranges or combined to provide closed-ended ranges. Cut.

[0107] In certain embodiments, the mixture containing the biomass to be subsequently hydrolyzed contains C1-05 arsenic. In certain embodiments, the mixture is substantially free of exogenous acids. Optionally, in each embodiment, one or more preheating steps may also be used prior to hydrolysis. In another embodiment, the mixture may be any of the following: any C1-05 alcohol, exogenous acid, or any combination thereof.

[0108] In certain embodiments, the solids content of the mixture based on the total weight of the mixture is about 1% by weight or more, e.g. For example, 1% to 40% by weight. The solid content of the mixture is 1, 2, 3, 4, 5, 6, 7, 8 , 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 2 2, 23, 24, 25, 26, 27, 28, 29, 30, 32, 34, 36, 38, 40 Each of the foregoing numbers may be preceded by the words "about," "at least "at least about," "less than about," or "less than about" may be used to indicate any of the numerical values ​​listed above. Alone to describe open-ended ranges or in combination to describe closed-ended ranges For example, the solid content of the mixture can be about 10% by weight to about 29% by weight, about 15% by weight, or about 29% by weight. % to about 29% by weight, about 10% to about 18% by weight, or about 24% to about 27% by weight It can be said that:

[0109] C. Methods of Manufacturing Polymers and Polymer Compositions The present invention provides a method for producing a polymer or polymer composition, the method comprising the steps of: lignin, e.g., herbaceous or hardwood lignin, and a polymeric carrier. Examples of polymeric carriers include polypropylene, ethylene, polyvinyl chloride (PVC ), polyvinyl acetate (PVA), chlorinated polyethylene, polystyrene, acrylonitrile -Butadiene-styrene (ABS) copolymer, ethylene-vinyl acetate copolymer, PV C / ABS blend, polyethylene terephthalate (PET), polycarbonate, poly Urethane, acrylic, styrene-acrylic, polyamide, nylon, elastomer, and and any combination thereof.

[0110] The process of the present invention includes, but is not limited to, tubular reactors, digesters (vertical, horizontal, or inclined), etc. The digester may be carried out in any suitable reactor, including, but not limited to, any of the above. The digester system described in Patent No. 8,057,639B includes a digester system and a steam explosion unit.

[0111] Thus, for example, in certain embodiments, lignin is a cellulose derivative comprising: (a)(i) cellulose and and (ii) a first liquid fraction. (b) providing a biomass; and (b) mixing a first solids content with water to form a slurry. and (c) (in certain embodiments, for residence times of about 20 seconds to about 45 seconds) about 225b Preheat the slurry to a temperature of about 340°C to about 400°C at a pressure of about 250 bar. and is obtained by:

[0112] In certain embodiments, the lignin is obtained by hydrolysis, for example by supercritical hydrolysis. Hydrolysis can be performed at various pressures, e.g., 1, 5, 10, 20, 30, 40, 50, 60, 70, 80 , 90, 100, 110, 120, 125, 130, 140, 150, 160, 170, 175, 180, 190, 200, 210, 220, 221, 225, 230, 240, 250, 260, 270, 275, 280, 290, 300, 310, 320, 325, 330, 340, 350, 360, 370, 375, 380, 390, 400, 420, 440, 450, 460, 475, 480, 500, 525, 550, 575, 600, At 625, 650, 675, 700, 725, 750, 775, or 800 (bar) Hydrolysis can be carried out at temperatures such as 374, 375, 380, 390, 400, 410, 420, 430, 440, 450, 460, 470, 480, 490, 500, 510, 520, 530, 540, 550, 560, 570, or 575 (℃ Each of the foregoing numbers may be preceded by the word "about," "at least about," or "less than about" and any of the above numerical values ​​may be used alone. open-ended ranges or combined to provide closed-ended ranges. Thus, in certain embodiments, lignin can be obtained by subjecting biomass to oxidation at temperatures between about 340° C. and about 40° C. By exposing it to a fluid having a temperature of 0°C and a pressure of about 225 bar to about 250 bar. It can be obtained.

[0113] In certain embodiments, the process includes hydrolysis (e.g., supercritical hydrolysis) and collecting the product. Although the methods disclosed herein can be carried out continuously, in alternative embodiments, they can be carried out in batch or can be carried out as a semi-batch process.

[0114] Herbaceous biomass (e.g., switchgrass) was used “as is” for hydrolysis. or by, for example, washing, mechanical preparation (e.g., grinding, shredding, crushing, etc.), Or, it may be suitably prepared by any combination thereof.

[0115] Other processes suitable for preparing the herbaceous lignin of the present invention may also be used.

[0116] The herbaceous lignin of the present invention can be generally produced by the above-mentioned treatment steps by using a suitable solvent. Extraction with a suitable solvent This process is referred to herein as the "extraction process" or "extraction." For example, the solvent is an alkaline aqueous solution. The amount of base in the alkaline aqueous solution can be, for example, an aqueous sodium hydroxide solution. The amount of the alkaline aqueous solution may be about 0.1% by weight or more, and the maximum amount is not particularly limited. The amount of base in the solution can be about 3% by weight or less, and there is no particular limit to the minimum amount. The remainder of the base usually comprises or consists of water. For example, the amount of base may be 0.1, 0.3, 0.5, 0.7, 0.9, 1.2, 1.4, 1.8, 2, 2.2, 2.4, 2.6, 2.8, 3( Each of the foregoing numbers may be preceded by the words "about," "at least about," " or "less than about" may be used, and any of the above numerical values ​​may be used alone. You can specify a range of open ends or combine them to specify a range of closed ends. For example, the amount of base may be about 0.9% by weight or more, about 1.7% by weight to about 2.6% by weight, It can be about 2.8% to about 3% by weight, or about 0.9% to about 1.2% by weight. Preferably, the alkaline aqueous solution is about 1% by weight.

[0117] Other suitable extraction solvents include aqueous organic solvents, such as dioxane, acetone, ethanol, At least one of methanol, propanol, or butanol in water is included Organic solvents in aqueous organic solvents (dioxane, acetone, ethanol, methanol, propane, etc.) The amount of alcohol, butanol, or a combination thereof is about 80% by volume or more. The amount of the organic solvent can be about 99.5% by volume or less, and there is no particular upper limit. The balance may contain water or may consist of water. For example, an aqueous organic solvent may be used. The amount of organic solvent in the 99, 99.5 (volume percent). Each of the foregoing numbers may be preceded by the word "about." "at least about," or "less than about," and using any of the preceding numerical values. In this case, open-ended ranges may be listed alone or in combination with closed-ended ranges. For example, the amount of organic solvent in the aqueous organic solvent is about 86% by volume or less. , about 88% by volume to about 94% by volume, about 90% by volume to about 92% by volume, or about 94% by volume to about The preferred amount of organic solvent in water is about 90% by volume or about 96% by volume. It is 96% by volume.

[0118] In certain embodiments, the yield of herbaceous lignin is at least 30% of the theoretical yield. In certain embodiments, the yield (%) of the herbaceous lignin is 30, 35, 40, 40% of the theoretical yield. 5, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, or 99% Each of the foregoing numbers may be preceded by the word "about," "at least about," or "less than about." Any of the above values ​​may be used alone to describe an open-ended range. or combinations can be used to describe close-ended ranges. In embodiments, the yield of herbaceous lignin is at least about 70% of the theoretical yield, or at least about 10% of the theoretical yield. At least about 85%.

[0119] D. product In some embodiments, the present invention relates to a product produced by the methods described herein. Regarding.

[0120] In some embodiments, the stabilizing polymer is polypropylene, ethylene, polyvinyl chloride. Polyvinyl (PVC), polyvinyl acetate (PVA), chlorinated polyethylene, polystyrene, acrylic ABS copolymer, ethylene-vinyl acetate copolymer Rimer, PVC / ABS blend, polyethylene terephthalate (PET), polycarbonate Polyurethane, Acrylic, Styrene-Acrylic, Polyamide, Nylon, Elastomer tomers, and any combination thereof.

[0121] In some embodiments, the stabilizing coating is any of the aforementioned polymers, or Architectural and industrial coatings, which may include any combination thereof Includes.

[0122] In some embodiments, the herbaceous lignin, such as switchgrass, can be one or more Used in combination with another antioxidant. Suitable antioxidants include IRGANOX 101 0, IRGANOX B225, IRGAFOS 168, and other phosphites, phosphatides, phenols, sterically hindered phenols, amines, thioesters, or any combination thereof This includes.

[0123] In some embodiments, the lignin-containing cellulose esters include those containing herbaceous lignin (e.g., switchgrass lignin). The oxidation onset temperatures (OOT) of the polymers are 150, 155, 160, 165, 170, and 1 75, 180, 185, 190, 195, 200, 205, 210, 215, 220, 2 22, 225, 227, 230, 231, 232, 233, 234, 235, 236, 2 37, 238, 239, 240, 241, 242, 243, 244, 245, 246, 2 47, 248, 249, 250, 252, 255, 257, 260, 262, 265, 2 67, 270, 275, 280, 285, 290, 295, 300, 305, 310, 3 15, 320, 325, 330, 335, 340, 345, 350, 355, 360, 3 65, 370, 380, 390, 400, 410, 420, 430, 440, or 45 0 (°C). Each of the above numbers may be preceded by the words "about," "at least about " or "less than about" may be used, and any of the above numerical values ​​may be used alone. You can specify open-ended ranges or combine them to specify closed-ended ranges. can.

[0124] In some embodiments, the lignin-containing cellulose esters include those containing herbaceous lignin (e.g., switchgrass lignin). The oxidation onset temperature of the polymer was higher for kraft lignin or hardwood lignin instead of herbaceous lignin. at least 1, 2, 4, 6, 8, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 90, 100, 120, 140, 160, 180, 190, 200, 210, 220, 12, 14, 16, 18, 20, 22, 24, 26, 28, 30, 32, 34, 36, 3 8, 40, 42, 44, 46, 48, 50, 52, 54, 56, 58, 60, 62, 64 , 66, 68, 70, 72, 74, 76, 78, 80, 82, 84, 86, 88, 90, 92, 94, 96, 98, or 100 (°C) higher.

[0125] E. Illustrative Provisions Some embodiments of the methods or products disclosed herein are described in the following clauses: Any combination of these provisions (or portions thereof) may be made and is hereby incorporated by reference in its entirety. It is possible to define embodiments of the methods or products shown.

[0126] Clause 1: A polymer or polymer composition comprising herbaceous lignin.

[0127] Clause 2: The polymer or polymer composition may be a thermoplastic, a thermoset, a composite, A coating, a film, an adhesive, a personal care composition, or any combination thereof. 2. The polymer or polymer composition according to claim 1,

[0128] Clause 3: The oxidation onset temperature of a polymer or polymer composition containing herbaceous lignin is The same polymers but containing kraft lignin or hardwood lignin instead of lignin. 2. The polymer or polymer composition of claim 1, wherein the temperature is at least 10° C. higher than

[0129] Clause 4: The polymer or polymer of clause 1 having an oxidation onset temperature of about 232°C to about 250°C. In one such embodiment, the polymer or polymer composition comprises a herbaceous lignin. In one such embodiment, the polymer or The polymer composition is a polypropylene polymer containing switchgrass lignin.

[0130] Clause 5: The polymer or polymer composition is a thermoplastic. Clause 2, 3, or 4 2. The polymer or polymer composition according to claim 1 .

[0131] Clause 6: The thermoplastic material is polyethylene, polypropylene, or a combination thereof. 6. The polymer or polymer composition according to clause 5, comprising

[0132] Clause 7: The thermoplastic material comprises polypropylene and the herbaceous lignin is 0.5 to 1.5% by weight. In one such embodiment, the polymer or polymer composition is present in a concentration of In this case, the thermoplastic material contains polypropylene and the herbaceous lignin is 0.5-1.5% by weight. Switchgrass lignin is present in high concentrations.

[0133] Clause 8: A coating composition comprising herbaceous lignin at a concentration of 0.5 to 2.0% by weight or film.

[0134] Clause 9: A personal care composition comprising herbaceous lignin at a concentration of 0.5 to 2.0% by weight.

[0135] Clause 10: The biomass contains lignin, and the composition comprises 20% or more by weight of the biomass. Thermoplastic polymers and biomass containing cellulose and / or hemicellulose in the amounts below. A composition comprising omas.

[0136] Clause 11: The thermoplastic polymer according to clause 10, having a processing temperature of less than about 400° C. Composition of.

[0137] Clause 12: Thermoplastic polymers are polyethylene, polypropylene, or combinations thereof. 11. The composition according to clause 10, which is a combination.

[0138] Clause 13: The composition of clause 10, wherein the lignin is hardwood lignin.

[0139] Clause 14: The composition of clause 10, wherein the lignin is a herbaceous lignin.

[0140] Clause 15: The lignin comprises a mixture of guaiacyl and syringyl units. 1. The composition according to claim 0.

[0141] Clause 16: The composition according to clause 10, having an oxidation onset temperature of about 232°C to about 250°C. .

[0142] Clause 17: The lignin has an average particle size of about 2 micrometers to about 8 micrometers. 11. The composition according to clause 10,

[0143] Clause 18: The composition of clause 10, wherein the lignin is prepared by supercritical hydrolysis.

[0144] Clause 19: Lignin is produced by subjecting biomass to a temperature of about 340°C to about 400°C and a temperature of about 225°C. The method according to claim 10, which is prepared by exposing the material to a fluid having a pressure of about 250 bar. The composition described above.

[0145] Clause 20: The polymer is polypropylene, and the lignin is from about 0.5% by weight to about 1.5% by weight. 11. The composition of claim 10, wherein the composition is present in a concentration of

[0146] Clause 21: A coating composition or film comprising the composition of clause 10.

[0147] Clause 22: A personal care composition comprising the composition of clause 10.

[0148] Clause 23: The method includes: (a) treating biomass at a temperature of about 340° C. to about 400° C. and about 225° C. obtaining lignin by exposing the lignin to a fluid having a pressure of from about 250 bar to about 250 bar; (b) mixing the lignin with a thermoplastic polymer. Manufacturing method.

[0149] Clause 24: The thermoplastic polymer according to clause 23, having a processing temperature of less than about 400°C. method.

[0150] Clause 25: Thermoplastic polymers are polyethylene, polypropylene, or combinations thereof. 24. The method according to claim 23,

[0151] Clause 26: The method of clause 23, wherein the lignin is hardwood lignin.

[0152] Clause 27: The method of clause 23, wherein the lignin is herbaceous lignin.

[0153] Clause 28: The composition according to clause 23, having an oxidation onset temperature of about 232°C to about 250°C. How to.

[0154] Clause 29: The lignin has an average particle size of about 2 micrometers to about 8 micrometers. 24. The method according to claim 23.

[0155] The invention is further defined in the following examples, in which all proportions and parts are the same unless otherwise stated. While these examples illustrate preferred embodiments of the invention, It is given by way of example only and should not be construed as limiting in any way. It should be understood that the above description and these examples are not intended to be limiting of the present invention. features can be ascertained, and various modifications of the present invention may be made without departing from their spirit and scope. Various changes and modifications can be made to adapt to different applications and conditions. EXAMPLES

[0156] F. Working Example 1. Example 1 This example shows the effect of switchgrass lignin as an antioxidant for polypropylene. and compare it with hardwood and kraft lignins, as well as commercial antioxidants. All samples were analyzed according to ASTM 2009-02 (hydrocarbon analysis by differential scanning calorimetry (DSC)). The ASTM 2009-02 standard test method for the oxidation initiation temperature of metals is used to evaluate the It is believed that the higher the oxidation onset temperature (OOT), the greater the stability against oxidative decomposition. All samples were made of polypropylene, specifically Bapolene® 4012F (Bamboo Prepared using Sigma-Aldrich Polymer, Inc., Houston, TX, USA. It is 12.0g / 10min (ASTM D-1238, 230C / 2,160g). It is commercially available as a blended / extrusion grade polypropylene with a melt flow of 1. Blended with polypropylene, lignin antioxidant or commercial antioxidant, and processed 0.5% by weight zinc stearate as auxiliary agent) and co-rotating 20mm twin screws The samples were extruded to produce pellets, which were then cut into small discs ( The samples were cut into pieces (approximately 2.6 mg) and accurately weighed for OOT testing (run in triplicate). The measurements were performed in air using a DSC with Tzero aluminum pans (TA Instruments). The samples were separately tested at 50 mL / min. The samples were equilibrated at 50 °C before increasing the temperature at a rate of 20 °C / min with an air flow of 100 °C. Various amounts of each test antioxidant (0, 0.1, 0.3, 0.5 or 0.6 , and 1.0 wt. %.

[0157] FIG. 1 shows the OOT (° C.) obtained at each antioxidant loading level for each antioxidant added. Referring to the legend of Figure 1, the antioxidants tested were:

[0158] Base - No antioxidant added (i.e., 0 wt.% antioxidant)

[0159] EBS / Omno(50%) - Added antioxidant is 50% ethylene bisstearamide. The lignin content was 50% and 50% hardwood lignin.

[0160] Irg1010 / Omno(40%) - The antioxidant added is Irganox 10 10 contained 60% and hardwood lignin 40%.

[0161] Irganox - The antioxidant added was Irganox 1010.

[0162] IrgB225 / Omno(30%) - The added antioxidant is Irganox B2 25 contained 70% and hardwood lignin 30%.

[0163] Kraft-added antioxidant was kraft lignin.

[0164] The antioxidant added to Omno was hardwood lignin.

[0165] Switchgrass Omno-The antioxidant added was switchgrass lignin.

[0166] [Irganox 1010 is pentaerythritol tetrakis(3-(3,5-di -tert-Butyl-4-hydroxyphenyl)propionate, sterically hindered phenol ;Irganox B225 = Irganox 1010 and Irgafos 168 Melt blend; Irgafos 168 = Tris(2,4-ditert-butyl phosphite) phenyl), phosphite stabilizer]

[0167] Both hardwood lignin and switchgrass lignin were processed using 5 micrometer diameter / max. It was pre-milled to a larger average particle size.

[0168] OOT is higher than that of the base case (base: polypropylene containing no antioxidants). Therefore, the data show that at the 1.0 wt% additive concentration, all lignins are antioxidant stable. Switchgrass lignin has shown some effectiveness as a lignin sulphate .... The OOT is significantly improved compared to lignin and hardwood lignin. At the same concentration in the same polymer, the hardwood lignin and kraft lignin are approximately 230°C), switchgrass lignin typically reduces the OOT of polypropylene by about From 200°C to about 244°C. Furthermore, the extrapolation of the curves shows that the concentration of lignin (antioxidant As the concentration of α-tocopherol increases, the improvement is likely to be much greater. vinegar.

[0169] Commercially viable performance is achieved with Irganox 10 at normal use concentration (0.3 wt%). 10, such performance is slightly This should be achieved with high use concentrations of switchgrass lignin. The specialty chemicals used are usually expensive, but even a small increase in their use concentration is commercially prohibitive. may not be possible.

[0170] 2. Example 2 The components of Masterbatch (MB) AF are shown in Table 1. JPEG2024147556000002.jpg70165

[0171] The components of an exemplary composition are shown in Table 2 (weight %) and Table 3 (grams). (Note: Per pellet. (The mat holds 500g). JPEG2024147556000003.jpg253147JPEG2024147556000004.jpg233158JPEG2024147556000005.jpg229158JPEG2024147556000006.jpg140154 JPEG2024147556000007.jpg232152JPEG2024147556000008.jpg229159JPEG2024147556000009.jpg229157JPEG2024147556000010.jpg229155

[0172] The total amounts (in grams) of each ingredient used are shown in Table 4. JPEG2024147556000011.jpg152124

[0173] 3. Example 3 The components of the exemplary compositions are shown in Table 5 (weight %) and Table 6 (grams). (Note: Per pellet. (The mat holds 500g). JPEG2024147556000012.jpg75169JPEG2024147556000013.jpg101169

[0174] The total amounts (in grams) of each ingredient used are shown in Table 7. JPEG2024147556000014.jpg67153

[0175] The oxidation onset temperature of the composition of Example 3 is shown in Table 8 (approximately 2.5 mg sample; air, 50 mL / min, ramp rate of 20°C per minute to 310°C). JPEG2024147556000015.jpg92166

[0176] 4. Example 4 A summary of the oxidation onset temperatures (OOT) of exemplary compositions is provided in Table 9 and FIG. JPEG2024147556000016.jpg243144JPEG2024147556000017.jpg17398

[0177] 5. Example 5 The results of UV testing of exemplary compositions are shown in Tables 10 and 11 and in Figures 3A and 3B. As shown. JPEG2024147556000018.jpg253149JPEG2024147556000019.jpg191152JPEG2024147556000020.jpg51148

[0178] 6. Example 6 The results of thermal testing of exemplary compositions are shown in Tables 12-14 and Figures 4A-C. JPEG2024147556000021.jpg225143JPEG2024147556000022.jpg222138JPEG2024147556000023.jpg206149 JPEG2024147556000024.jpg208137JPEG2024147556000025.jpg226148JPEG2024147556000026.jpg224129 JPEG2024147556000027.jpg211152JPEG2024147556000028.jpg214145JPEG2024147556000029.jpg222155 JPEG2024147556000030.jpg224127JPEG2024147556000031.jpg205154JPEG2024147556000032.jpg203130

[0179] 7. Example 7 The results of standard Oxidation Onset Temperature (OOT) testing of exemplary compositions are shown in Tables 15, 16, and 17. Shown in Figure 5. JPEG2024147556000033.jpg246149JPEG2024147556000034.jpg244119JPEG2024147556000035.jpg253154

[0180] 8. Example 8 Data corresponding to the Oxidation Onset Temperature (OOT) tests of exemplary compositions are shown in Table 17, respectively. i to xii and Figures 6A to L. JPEG2024147556000036.jpg57165JPEG2024147556000037.jpg36165JPEG2024147556000038.jpg43165 JPEG2024147556000039.jpg51165JPEG2024147556000040.jpg87166JPEG2024147556000041.jpg54166 JPEG2024147556000042.jpg44166JPEG2024147556000043.jpg77168JPEG2024147556000044.jpg84167 JPEG2024147556000045.jpg50167JPEG2024147556000046.jpg43164JPEG2024147556000047.jpg63164

[0181] Although preferred forms of the invention have been disclosed, they may be modified without departing from the spirit and scope of the invention. It will be appreciated by those skilled in the art that various changes and modifications can be made which achieve some of the advantages of the present invention. It will be apparent to those skilled in the art that the appended claims are to be construed as constituting the true spirit and scope of the present invention. All such equivalent variations that fall within the scope of the present invention are intended to be encompassed by the appended claims. The scope of application shall be determined by the

[0182] Ranges for physical properties, e.g., molecular weight, or chemical properties, e.g., chemical formula, are set forth herein. When used herein, all combinations and subcombinations of the scope of specific embodiments therein are intended to cover all combinations and subcombinations of the scope of specific embodiments therein. It is intended to include combinations.

[0183] The disclosure of each patent, patent application, and publication cited or described in this document is incorporated herein by reference in its entirety. It is incorporated herein by reference.

[0184] Various modifications and variations in the present invention may be made without departing from the scope or spirit of the present invention. It will be apparent to one skilled in the art that other embodiments of the present invention may be used in the methods disclosed herein. These features will be apparent to those skilled in the art from consideration of the specification and practice of the invention. It is intended that the following claims be construed as being illustrative only, with the true scope and spirit of the invention being indicated by the following claims. It is intended that the

Claims

1. A composition comprising a thermoplastic polymer and biomass, the biomass being lignin. said composition comprising cellulose in an amount of 20% or less by weight of said biomass and and / or hemicellulose.

2. 10. The composition of claim 1, wherein the thermoplastic polymer has a processing temperature of less than about 400°C. thing.

3. The thermoplastic polymer may be polyethylene, polypropylene, or a combination thereof.

2. The composition of claim 1 ,

4. 2. The composition of claim 1, wherein the lignin is a hardwood lignin.

5. The composition of claim 1 , wherein the lignin is an herbaceous lignin.

6. 2. The method of claim 1, wherein the lignin comprises a mixture of guaiacyl and syringyl units. The composition described above.

7. 10. The composition of claim 1 having an oxidation onset temperature of from about 232°C to about 250°C.

8. The lignin has an average particle size of about 2 micrometers to about 8 micrometers. The composition of claim 1.

9. 10. The composition of claim 1, wherein the lignin is prepared by supercritical hydrolysis.

10. The lignin is prepared by subjecting biomass to a temperature of about 340° C. to about 400° C. and a pressure of about 225 bar to about 400 bar.

10. The composition of claim 1, which is prepared by exposing it to a fluid having a pressure of about 250 bar. Composition.

11. The polymer is polypropylene and the lignin is from about 0.5% to about 1.5% by weight. %. The composition of claim 1 .

12. A coating composition or film comprising the composition of claim 1.

13. A personal care composition comprising the composition of claim 1.

14. 13. A method for producing the composition of claim 1, said method comprising: (a) subjecting biomass to a temperature of about 340° C. to about 400° C. and a pressure of about 225 bar to about 250 bar; obtaining lignin by exposing the lignin to a fluid having a pressure of 1000 argon; (b) mixing the lignin with the thermoplastic polymer; A method comprising:

15. 15. The method of claim 14, wherein the thermoplastic polymer has a processing temperature of less than about 400°C. Law.

16. The thermoplastic polymer may be polyethylene, polypropylene, or a combination thereof. The method of claim 14, wherein

17. 15. The method of claim 14, wherein the lignin is a hardwood lignin.

18. 15. The method of claim 14, wherein the lignin is a herbaceous lignin.

19. The method of claim 14, wherein the composition has an oxidation onset temperature of about 232° C. to about 250° C. Law.

20. The lignin has an average particle size of about 2 micrometers to about 8 micrometers. The method of claim 14.

Citation Information

Patent Citations

  • Degradable polymers and polymer products

    JP1998501295A

  • Antioxidant for resin

    JP2005041969A

  • Antibacterial resin composition

    JP2011219716A

  • Production of lignin from lignocellulosic biomass

    JP2014513740A

  • High Purity Lignin, Lignin Compositions, and Higher Structure Lignin

    JP2016512285A