Semiconductor device

By enhancing the purity of oxide semiconductor films through dehydration or dehydrogenation and using metal oxide materials, the aperture ratio and reliability of thin film transistors are improved, addressing the limitations of conventional oxide semiconductor display panels.

JP2024147575AInactive Publication Date: 2024-10-16SEMICON ENERGY LAB CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2024101870
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2009-07-10
Filing Date
2024-06-25
Publication Date
2024-10-16
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional display panels using oxide semiconductors fail to improve the aperture ratio and reliability due to the use of conductive films without considering light-transmitting properties and moisture impurities in the semiconductor layers.

Method used

The method involves increasing the purity of oxide semiconductor films by reducing moisture impurities through dehydration or dehydrogenation processes, forming a gate electrode layer, gate insulating layer, and oxide semiconductor layer, and using metal oxide materials for the semiconductor device, with specific heat treatments and cooling methods to enhance the semiconductor's electrical characteristics.

Benefits of technology

This approach enhances the aperture ratio and reliability of thin film transistors by improving the electrical characteristics and reducing impurities, leading to high-performance and cost-effective semiconductor devices with improved manufacturing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024147575000001_ABST
    Figure 2024147575000001_ABST
Patent Text Reader

Abstract

To manufacture and provide a highly reliable display device that has a thin-film transistor having a high numerical aperture and stable electrical characteristics.SOLUTION: In a method of manufacturing a semiconductor device that has a thin-film transistor using a semiconductor layer including a channel formation region as an oxide semiconductor film, heat treatment (heat treatment for dehydration or dehydrogenation) for enhancing the purity of the oxide semiconductor film and for reducing moisture and the like which are impurities is performed. In addition, a gate electrode layer, a source electrode layer, and a drain electrode layer are manufactured by using a light transmissive conductive film to improve a numerical aperture.SELECTED DRAWING: Figure 9
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] A semiconductor device having a circuit configured with thin film transistors (hereinafter referred to as TFTs) and The present invention relates to a method for producing the same, and is applicable to electro-optical devices such as liquid crystal display panels and organic light-emitting devices. The present invention relates to electronic equipment incorporating a light-emitting display device having a light-emitting element as a component.

[0002] In this specification, a semiconductor device is a device that can function by utilizing semiconductor characteristics. This term refers to devices in general, and electro-optical devices, semiconductor circuits, and electronic equipment are all classified as semiconductor devices. [Background technology]

[0003] As a method of wiring metal auxiliary wiring for the transparent electrodes of electro-optical elements, The metal auxiliary wiring and the transparent electrode are wired so that they overlap to ensure electrical continuity with the transparent electrode. It is known that the above-mentioned method is used (see Patent Document 1).

[0004] The additional capacitance electrodes provided on the active matrix substrate are made of transparent materials such as ITO and SnO2. In order to reduce the electrical resistance of the additional capacitance electrode, A configuration is known in which an auxiliary wiring made of a film is provided in contact with an electrode for additional capacitance (see Patent Document 2). see).

[0005] In a field effect transistor using an amorphous oxide semiconductor film, The materials used to form the gate and drain electrodes are indium tin oxide (ITO), indium tin oxide (ITO), and indium tin oxide (ITO). Transparent electrodes such as zinc oxide, ZnO, SnO2, and Al, Ag, Cr, Ni, Mo , Au, Ti, Ta, or other metal electrodes, or metal electrodes of alloys containing these, etc. Two or more layers of these may be laminated to reduce contact resistance and improve interface strength. is known (see Patent Document 3).

[0006] A source electrode, a drain electrode and a gate electrode of a transistor using an amorphous oxide semiconductor The materials for the gate electrode and the auxiliary capacitance electrode are indium (In), aluminum (Al), and gold (Gl). (Au), silver (Ag), and other metals, as well as indium oxide (In2O3), tin oxide (SnO2 ), zinc oxide (ZnO), cadmium oxide (CdO), indium cadmium oxide (Cd In2O4), cadmium tin oxide (Cd2SnO4), zinc tin oxide (Zn2SnO4 ) and other oxide materials can be used, and the materials for the gate electrode, source electrode, and drain electrode can be It is known that the above may be the same or different (see Patent Document 4 and Patent Document 5). see). [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 2-82221 [Patent Document 2] Japanese Patent Application Publication No. 2-310536 [Patent Document 3] JP 2008-243928 A [Patent Document 4] JP 2007-109918 A [Patent Document 5] JP 2007-115807 A Summary of the Invention [Problem to be solved by the invention]

[0008] However, conventional display panels using oxide semiconductors simply use them as electrode materials to provide transparency. Therefore, the aperture ratio could not be improved. In addition, when constructing a display device using metal oxide, reliability is taken into consideration. There wasn't.

[0009] In view of the above, one embodiment of the present invention is to provide a display device including a metal oxide, which has an aperture ratio of 100 nm or less. One of the objectives is to improve the reliability while improving the speed and the reliability. [Means for solving the problem]

[0010] A semiconductor device having a thin film transistor in which a semiconductor layer including a channel formation region is an oxide semiconductor film In a method for manufacturing an electronic device, the purity of an oxide semiconductor film is increased and impurities such as moisture are reduced. In addition, a heat treatment for dehydration or dehydrogenation is performed on the oxide semiconductor film. The gate insulating layer is also protected from moisture and other impurities. The present invention reduces impurities such as moisture that are present at the interface between the oxide semiconductor film and the oxide semiconductor film.

[0011] One embodiment of the present invention disclosed in this specification is a method for manufacturing a gate electrode made of a metal oxide on a substrate having an insulating surface. a gate electrode layer is formed on the gate electrode layer, a gate insulating layer is formed on the gate insulating layer, and an oxide A semiconductor layer is formed, the oxide semiconductor layer is dehydrated or dehydrogenated, and the dehydrated or dehydrogenated forming a source electrode layer and a drain electrode layer made of a metal oxide over the oxide semiconductor layer; An oxide semiconductor layer is formed on the gate insulating layer, the oxide semiconductor layer, the source electrode layer, and the drain electrode layer. A protective insulating layer is formed in contact with a part of the insulating layer, and a pixel electrode layer made of a metal oxide is formed on the protective insulating layer. The present invention relates to a method for manufacturing a semiconductor device.

[0012] Dehydration or dehydrogenation can be performed under an oxygen atmosphere, nitrogen or rare gas (argon, helium, etc.). The substrate is heated to 350° C. or higher, preferably 400° C. or higher, in an inert gas atmosphere or under reduced pressure. Heat treatment below the strain point is performed to reduce impurities such as moisture contained in the oxide semiconductor layer.

[0013] The oxide semiconductor layer that has been dehydrated or dehydrogenated is Thermal Desorption Spectroscopy (TDS) was used for the layer. Even when measurements were taken up to 450°C using spectroscopic techniques, the two water peaks were not observed. The heat treatment conditions are set so that at least one peak appearing around 300°C is not detected. For a thin film transistor using an oxide semiconductor layer that has been dehydrated or dehydrogenated, Even when measuring up to 450°C with TDS, the water peak that appears at least around 300°C is not detected. Not done.

[0014] Then, water is again released from the oxide semiconductor layer at the heating temperature T at which the oxide semiconductor layer is dehydrated or dehydrogenated. The temperature is preferably lowered by 100°C or more than the heating temperature T until the temperature is sufficiently low so that the material does not enter the container. The material is cooled slowly to below 100°C.

[0015] In addition, the gas atmosphere when lowering the temperature from the heating temperature T is the same as the gas atmosphere heated to the heating temperature T. The atmosphere may be switched to a different gas atmosphere.

[0016] The moisture content in the film is reduced by a heat treatment for dehydration or dehydrogenation, and then the film is Cool slowly (or cool) in an atmosphere that is not prone to dew (dew point is -40°C or less, preferably -60°C or less). By using the oxide semiconductor film, the electrical characteristics of a thin film transistor can be improved and the This will realize thin-film transistors that are both highly productive and have high performance.

[0017] In this specification, the inert gas atmosphere is oxygen, nitrogen or rare gas (argon, helium, etc.). Heat treatment under a nitrogen atmosphere or reduced pressure is called heat treatment for dehydration or dehydrogenation. In this specification, dehydrogenation refers only to the desorption of H2 by this heat treatment. It is not called dehydration or dehydrogenation, but includes the elimination of H, OH, etc. We will call them that for convenience.

[0018] Under an inert gas atmosphere of nitrogen or rare gas (argon, helium, etc.), or under reduced pressure When the heat treatment is performed, the i-type oxide semiconductor layer becomes an oxygen-deficient type. This means lower resistance, i.e. N-type (N - , N + Then, the oxide semiconductor layer is By forming an oxide insulating film, the oxide semiconductor layer is made in an oxygen-excess state, resulting in a high resistance This makes it possible to obtain a thin, reliable substrate with good electrical properties. It is possible to manufacture and provide a semiconductor device having a film transistor.

[0019] Under an inert gas atmosphere of nitrogen or rare gas (argon, helium, etc.), or under reduced pressure When the atmosphere is changed to an oxygen atmosphere and then slowly cooled, the oxide semiconductor The layer becomes oxygen deficient by heat treatment, resulting in low resistance, i.e., N-type (N - , N + etc.), After that, the oxide semiconductor layer is cooled slowly in an oxygen atmosphere to make it into an oxygen-excessive state, thereby forming a high-resistance That is, it can be made into I-type.

[0020] In addition, when heat treatment for dehydration or dehydrogenation is performed in an oxygen atmosphere, the oxide semiconductor The moisture in the layer is removed and at the same time an oxygen-rich state is created.

[0021] The oxide semiconductor used in this specification is InMO3(ZnO). m (m>0) A thin film transistor is fabricated using the thin film as an oxide semiconductor layer. Indicates one or more metal elements selected from Ga, Fe, Ni, Mn, and Co. For example, M can be Ga, Ga and Ni, Ga and Fe, etc. In the oxide semiconductor, M may contain any of the above metal elements. In addition to the metal elements contained, impurity elements include Fe, Ni, other transition metal elements, or Some contain oxides of transition metals. In this specification, InMO3(ZnO ) m Among oxide semiconductors with a structure represented by (m>0), oxide semiconductors with a structure containing Ga as M The compound semiconductor is called an In-Ga-Zn-O oxide semiconductor, and the thin film is called an In-Ga-Zn- It is also called an O-based non-single crystal film.

[0022] In addition to the above, metal oxides that can be used for the oxide semiconductor layer include In-Sn-Zn-O metal oxides of the In-Al-Zn-O system, metal oxides of the Sn-Ga-Zn-O system Oxides, Al-Ga-Zn-O metal oxides, Sn-Al-Zn-O metal oxides, In-Zn-O metal oxides, Sn-Zn-O metal oxides, Al-Zn-O metal oxides Metal oxides, In-O metal oxides, Sn-O metal oxides, Zn-O metal oxides In addition, the oxide semiconductor layer made of the metal oxide may contain silicon oxide. This may be allowed.

[0023] The oxide semiconductor is preferably an oxide semiconductor containing In, more preferably an oxide semiconductor containing In and In order to make the oxide semiconductor layer i-type (intrinsic), It is effective to subject the mixture to a hydrogenation or dehydrogenation process.

[0024] In addition, when heat treatment for dehydration or dehydrogenation is performed after the formation of the oxide semiconductor layer, Depending on the conditions of the heat treatment or the material of the oxide semiconductor layer, the oxide semiconductor layer may be in an amorphous state. In some cases, the oxide semiconductor layer becomes a microcrystalline film or a polycrystalline film. For example, the amorphous structure may contain crystalline grains (nanocrystals). Even if a crystal film is formed, the oxide semiconductor layer can be made to have high resistance by making the oxide semiconductor layer in an oxygen-excess state. If it can be made into an I-type, it will be possible to obtain switching characteristics as a TFT. Cut.

[0025] However, to reduce the off-current of the TFT and achieve low power consumption, the oxide semiconductor layer must be amorphous. It is preferable that the amorphous state is maintained.

[0026] In addition, even if heat treatment for dehydration or dehydrogenation is performed after the formation of the oxide semiconductor layer, the oxide semiconductor layer does not become oxidized. In order to make the compound semiconductor layer amorphous, it is preferable to make the film thickness as thin as 50 nm or less. When the oxide semiconductor layer is formed and then subjected to heat treatment, Crystallization can be suppressed.

[0027] In addition, even if heat treatment for dehydration or dehydrogenation is performed after the formation of the oxide semiconductor layer, the oxide semiconductor layer does not become oxidized. In order to make the oxide semiconductor layer amorphous, silicon oxide (S) is added to the oxide semiconductor layer to inhibit crystallization. By including iOx (X>0), after the formation of the oxide semiconductor layer during the manufacturing process, When the film is subjected to a heat treatment, crystallization can be suppressed.

[0028] Note that the off-state current used in this specification is the current that flows through the source electrode when the transistor is in an off state. For example, in the case of an n-type transistor, the gate When the gate voltage is lower than the threshold voltage of the transistor, is the current flowing through

[0029] Also, a gate electrode layer, a source electrode layer, a drain electrode layer, a pixel electrode layer, or other electrodes Metal oxides applied to the wiring layers and other wiring layers are deposited by sputtering or vacuum deposition (electronic bipolar deposition). Using the visible light deposition method, arc discharge ion plating method, and spray method, Conductive materials that are transparent to light, such as metal oxides of the In-Sn-Zn-O system, In- Al-Zn-O metal oxides, Sn-Ga-Zn-O metal oxides, Al-Ga-Z nO-based metal oxides, Sn-Al-Zn-O-based metal oxides, In-Zn-O-based metals Oxides, Sn-Zn-O metal oxides, Al-Zn-O metal oxides, In-O metal oxides Metal oxides, Sn-O-based metal oxides, and Zn-O-based metal oxides can be used. The wiring layer or electrode layer made of the above metal oxide may contain silicon oxide.

[0030] Also, a gate electrode layer, a source electrode layer, a drain electrode layer, a pixel electrode layer, or other electrodes Other materials that can be used for the wiring layers and other wiring layers include nitrogen-containing Al-Zn-O-based non-monocrystalline Crystalline films, i.e. Al-Zn-ON non-single crystal films and nitrogen-containing Zn-ON non-single crystal films. Alternatively, a single crystal film or a nitrogen-containing Sn-Zn-ON non-single crystal film may be used. The composition ratio (atomic %) of zinc in the Zn-ON oxide semiconductor film is set to 47 atomic % or less, and the oxide The aluminum composition ratio (atomic percent) in the oxide semiconductor film is greater than that in the oxide semiconductor film. The composition ratio (atomic %) of nium is larger than the composition ratio (atomic %) of nitrogen in the light-transmitting conductive film. The composition ratio of the light-transmitting conductive film is expressed in atomic percent. ISER(EPMA:Electron Probe X-ray MicroAnaly The evaluation will be carried out by analysis using the .

[0031] A gate electrode layer, a source electrode layer, a drain electrode layer, a pixel electrode layer, or other electrode layers, By using a conductive film having a property of transmitting visible light for other wiring layers, In addition, when a light-transmitting material is used for the oxide semiconductor layer, By using the above-mentioned method, the aperture ratio can be further improved. By using a light-transmitting film for the semiconductor layer, scanning In order to increase the resolution of the displayed image by increasing the number of lines, the pixel size is reduced, but In addition, the thin film transistor can be formed of a light-transmitting material. By using a film, a wide viewing angle can be achieved even if one pixel is divided into multiple sub-pixels. A high aperture ratio can be achieved. In other words, even if a high density group of thin film transistors is arranged, the aperture ratio can be increased. The aperture ratio can be increased, and a sufficient display area can be secured. For example, When one pixel has two to four sub-pixels, the thin film transistor has light-transmitting properties. In addition, each storage capacitor is transparent, which improves the aperture ratio. can be done.

[0032] In addition, in a light-emitting display device, the components (wiring and semiconductor layer) of a thin-film transistor are transparent. By using a film with optical properties, even if multiple thin film transistors are arranged in one pixel, high In a light-emitting display device using a light-emitting element, The pixel portion has a gate electrode of a thin film transistor and The source wiring or drain wiring of another transistor is electrically connected to the For example, in a light-emitting display device, one pixel has 2 to 7 thin film transistors. Even if the thin film transistor has a storage capacitor, the thin film transistor and the storage capacitor have light-transmitting properties. A high aperture ratio can be achieved.

[0033] Also, a gate electrode layer, a source electrode layer, a drain electrode layer, a pixel electrode layer, or other electrodes If the same material is used for the layers and other wiring layers, common sputter targets and common manufacturing equipment can be used. The cost of the material and the etchant (or This reduces the cost of etching gas, resulting in reduced manufacturing costs. It is possible.

[0034] In this specification, a film that is transparent to visible light has a visible light transmittance of 75 to 100 %, and the film is also called a transparent conductive film. A source electrode layer, a drain electrode layer, a pixel electrode layer, or other electrode layers, or other wiring layers As the metal oxide to be applied, a conductive film semitransparent to visible light may be used. In contrast, translucency refers to a visible light transmittance of 50-75%.

[0035] A gate electrode layer, a source electrode layer, a drain electrode layer, a pixel electrode layer, or other electrode layers, The thickness of the other wiring layers is 30 nm to 200 nm, and the layers are transparent to visible light. It is only necessary to select a film thickness that has a thickness of 0.1 or is semi-transparent.

[0036] In addition, the gate insulating layer and the oxide semiconductor film are processed continuously without being exposed to the air. It may be subjected to a continuous process (also called in-situ process or continuous deposition). By performing the treatment continuously without causing the oxide semiconductor film to be damaged, the interface between the gate insulating layer and the oxide semiconductor film is protected from water and halogen. Without being contaminated by atmospheric components or impurities suspended in the air, such as hydrocarbons, Since it is possible to form a gate insulating layer and an oxide semiconductor film, the characteristics of thin film transistors can be improved. This can reduce fluctuations.

[0037] In this specification, the term "continuous processing" refers to a process that starts with the first processing step performed by the PCVD method or the sputtering method and ends with the PC During the series of processes up to the second processing step performed by the VD method or sputtering method, the substrate to be processed is placed The atmosphere is always in a vacuum or inert gas atmosphere without coming into contact with contaminated atmosphere such as air. This refers to the fact that the atmosphere is controlled in a nitrogen or rare gas atmosphere, or in an oxygen atmosphere. By performing continuous processing, reattachment of moisture and other substances to the cleaned substrate can be avoided, and film formation can be performed. Which processing can be performed?

[0038] To carry out a series of processes from the first processing step to the second processing step in the same chamber is considered to be within the scope of continuous processing in this specification.

[0039] In addition, a series of processes from the first process to the second process are carried out in different chambers. In this case, after the first processing step is completed, the substrate is transported between chambers without being exposed to the atmosphere. The application of a second treatment is also considered to be within the scope of the continuous treatment in this specification.

[0040] Between the first and second processing steps, a substrate transfer step, an alignment step, and a slow cooling step are performed. or a step of heating or cooling the substrate to a temperature required for the second step. However, such a process is considered to be within the scope of the continuous process in this specification.

[0041] However, the first step involves processes that use liquids, such as cleaning, wet etching, and resist formation. If the first processing step is between the second processing step, it does not fall within the scope of continuous processing as used herein. Let's say that's not the case.

[0042] The structure obtained by the above manufacturing method includes a gate electrode layer and a gate A gate insulating layer is formed on the gate electrode layer, an oxide semiconductor layer is formed on the gate insulating layer, and a gate insulating layer is formed on the oxide semiconductor layer. A source electrode layer and a drain electrode layer, a gate insulating layer, an oxide semiconductor layer, a source electrode layer, and a protective insulating layer on the drain electrode layer and in contact with a part of the oxide semiconductor layer; and a metal insulating layer on the protective insulating layer. A pixel electrode layer made of an oxide. The source electrode layer, the drain electrode layer, the protective insulating layer, and the pixel electrode layer have a light-transmitting property. is a semiconductor device in which an oxide semiconductor layer and a gate electrode layer overlap.

[0043] The above configuration solves at least one of the above problems.

[0044] In the above structure, the pixel electrode layer overlaps with the oxide semiconductor layer and the gate electrode layer. The area covered by the oxide semiconductor can be used as a display area, achieving a high aperture ratio. The pixel electrode layer overlapping the gate electrode layer and the body layer may be the pixel electrode layer of an adjacent pixel. That is, the oxide semiconductor layer is electrically connected through the source electrode layer and the drain electrode layer. The pixel electrode layer does not overlap with the channel formation region of the oxide semiconductor layer, and the pixel electrode layer does not overlap with the channel formation region of the oxide semiconductor layer. The electrode layers may be configured to overlap each other.

[0045] In addition, in the terminal section where multiple terminal electrodes that connect to external terminals such as FPCs are arranged, The electrode is made of the same material as the gate electrode layer, the source electrode layer, the drain electrode layer, or the pixel electrode layer. They can be formed in the same process.

[0046] In addition, the storage capacitor of the pixel portion of the liquid crystal display device or the light-emitting display device uses the gate insulating layer as a dielectric. A capacitance wiring layer made of a conductive material having transparency to visible light and a transparent material for the visible light The capacitor wiring layer is formed of a conductive material having optical properties. The capacitance electrode layer can be formed of the same material and in the same process as the gate electrode layer. The insulating layer 12 can be formed from the same material and in the same process as the source electrode layer or the drain electrode layer.

[0047] In addition, the storage capacitor of the pixel portion of the liquid crystal display device or the light-emitting display device uses a protective insulating layer as a dielectric. a capacitance wiring layer made of a conductive material having transparency to visible light; In this case, the capacitance wiring layer may be formed of a pixel electrode layer made of a conductive material having a capacitance of 1000 .mu.m. The insulating layer 12 can be formed from the same material and in the same process as the source electrode layer or the drain electrode layer.

[0048] In addition to liquid crystal display devices, display devices having thin film transistors include those using light emitting elements. Examples of such displays include light-emitting displays that use electrophoretic display elements, and displays that use electrophoretic display elements and are also known as electronic paper. Can be obtained.

[0049] The liquid crystal display device is not particularly limited, and may be a TN liquid crystal, an IPS liquid crystal, an OCB liquid crystal, or the like. Liquid crystal, STN liquid crystal, VA liquid crystal, ECB type liquid crystal, GH liquid crystal, polymer dispersed liquid crystal, discote Among them, normally black type liquid crystal panels, e.g. For example, it is preferable to use a transmissive liquid crystal display device that employs a vertical alignment (VA) mode. There are several types of direct alignment modes, such as MVA (Multi-Dom Vertical Alignment mode, PVA (Patterned Vertical Alignment mode, ASV mode, etc. Specifically, one pixel is divided into multiple subpixels, and a pixel is placed at the center of each subpixel. By providing a convex portion on the opposing substrate, one pixel is made into a multi-domain pixel. and providing a convex portion on the opposing substrate located at the center of each subpixel, The driving method for dividing one pixel into multiple domains and achieving a wide viewing angle is the sub-pixel method. The convex portion may be provided on either or both of the opposing substrate and the element substrate. It is common to align liquid crystal molecules radially to improve the alignment control force.

[0050] In addition, the top surface of the liquid crystal driving electrode, i.e., the pixel electrode, is shaped like a comb or zigzag to reduce the voltage. The directions may be diversified. Also, one pixel may be made into a multi-domain by using optical alignment. Good too.

[0051] In addition, since thin-film transistors are easily damaged by static electricity, etc., For the line, a protection circuit for protecting the thin film transistor in the pixel area can be provided on the same substrate. The protection circuit is preferably configured using a nonlinear element using an oxide semiconductor. stomach. Effect of the Invention

[0052] In the pixel portion of a display device, a film having light-transmitting properties is used as a component of a thin film transistor. In order to increase the number of scanning lines and improve the resolution of the displayed image, pixel dimensions are reduced. In addition, a high aperture ratio can be achieved even if the thin film transistor is made of a light-transmitting material. By using a film with this property, one pixel is divided into multiple sub-pixels to achieve a wide viewing angle. Even if it is divided, a high aperture ratio can be achieved. [Brief description of the drawings]

[0053] [Figure 1] 1A to 1C are cross-sectional views showing a process of one embodiment of the present invention. [Diagram 2] 1A and 1B are a plan view and a cross-sectional view illustrating one embodiment of the present invention. [Diagram 3] 1A to 1C are cross-sectional views showing a process of one embodiment of the present invention. [Figure 4] 1A to 1C are cross-sectional views showing a process of one embodiment of the present invention. [Diagram 5] 1A to 1C are cross-sectional views showing a process of one embodiment of the present invention. [Figure 6] 1A and 1B are a plan view and a cross-sectional view illustrating one embodiment of the present invention. [Figure 7] 1A and 1B are cross-sectional views and plan views illustrating a process of one embodiment of the present invention. [Figure 8] 1A to 1C are cross-sectional views showing a process of one embodiment of the present invention. [Figure 9] 1A to 1C are cross-sectional views showing a process of one embodiment of the present invention. [Figure 10] FIG. 1 is a plan view illustrating one embodiment of the present invention. [Figure 11] FIG. 1 is a plan view illustrating one embodiment of the present invention. [Figure 12] 1A and 1B are cross-sectional views and a plan view illustrating one embodiment of the present invention. [Figure 13] FIG. 1 is a perspective view illustrating one embodiment of the present invention. [Figure 14] FIG. 1 is a block diagram showing one embodiment of the present invention. [Figure 15] 1 is a timing chart illustrating one embodiment of the present invention. [Figure 16] FIG. 2 is a diagram illustrating a pixel equivalent circuit of the semiconductor device. [Figure 17] 1A and 1B are diagrams illustrating a semiconductor device. [Figure 18] 1A and 1B are diagrams illustrating a semiconductor device. [Figure 19] 1A and 1B are diagrams illustrating a semiconductor device. [Figure 20] 1A and 1B are diagrams illustrating a semiconductor device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0054] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. The present invention is not limited to the following description, and those skilled in the art will recognize that the present invention may be modified in various ways in form and detail. The present invention is not limited to the description of the following embodiments. It is not something that can be done.

[0055] (Embodiment 1) A semiconductor device and a manufacturing method of the semiconductor device will be described with reference to FIGS. The thin film transistor 470 has a structure called a channel etch type.

[0056] FIG. 2A is a plan view of a thin film transistor 470 included in the semiconductor device, and FIG. FIG. 2(A) is a cross-sectional view taken along line C1-C2 of FIG. The transistor is a thin film transistor having a gate electrode layer 401 on a substrate 400 having an insulating surface. , a gate insulating layer 402, an oxide semiconductor layer 403, a source electrode layer 405a, and a drain electrode The electrode layer 405b covers the thin film transistor 470 and is connected to the oxide semiconductor layer 403. An oxide insulating film 407 is provided.

[0057] Also, a substrate 400 having an insulating surface, a gate electrode layer 401, a gate insulating layer 402, an oxide The semiconductor layer 403, the source electrode layer 405a, the drain electrode layer 405b, and the oxide insulating film 4 07 is made entirely of materials that are transparent to visible light. The thin film transistor 470 has a light-transmitting property, and is disposed in a pixel portion of a display device. In this case, the aperture ratio can be improved.

[0058] The oxide semiconductor layer 403 is formed by removing at least moisture or the like which is an impurity after the formation of the oxide semiconductor film. Heat treatment to reduce the amount of hydrogen (heat treatment for dehydration or dehydrogenation) is performed. After heat treatment for dehydrogenation and gradual cooling, the oxide insulating film in contact with the oxide semiconductor layer was formed. Reducing the carrier concentration in the oxide semiconductor layer by performing a process such as formation of a thin film transistor47 This will lead to improved reliability of 0.

[0059] In addition to the oxide semiconductor layer 403, the gate insulating layer 402 and the oxide semiconductor layer The interface between the oxide semiconductor layer 403 and the films provided above and below the oxide semiconductor layer 403, specifically, the gate insulating film The interface between the insulating layer 402 and the oxide semiconductor layer 403, and the interface between the oxide insulating film 407 and the oxide semiconductor layer 404 Reduce impurities such as moisture present at the interface of 03.

[0060] The manufacturing process of the thin film transistor 470 shown in FIG. 2B will be described below with reference to FIGS. A cross-sectional view is shown.

[0061] In FIG. 1A, a gate electrode layer 401 is provided over a substrate 400 having an insulating surface.

[0062] There is no significant limitation on the substrate that can be used for the substrate 400 having an insulating surface. In any case, it is necessary for the insulating surface to have sufficient heat resistance to withstand subsequent heat treatment. The substrate 400 is made of glass such as barium borosilicate glass or aluminoborosilicate glass. A substrate can be used.

[0063] In addition, for glass substrates, if the temperature of the subsequent heat treatment is high, the distortion point is 730°C or higher. For the glass substrate, for example, aluminosilicate glass, alumina Glass materials such as lumino borosilicate glass and barium borosilicate glass are used. By containing more barium oxide (BaO) than boron oxide, it is possible to obtain a more practical and durable Thermal glass is obtained. For this reason, a glass substrate containing more BaO than B2O3 is used. is preferred.

[0064] Instead of the above glass substrate, a ceramic substrate, a quartz substrate, a sapphire substrate, etc. A substrate made of an insulating material may be used, and crystallized glass may also be used.

[0065] In addition, an insulating film serving as a base film may be provided between the substrate 400 and the gate electrode layer 401. The film has a function of preventing the diffusion of impurity elements from the substrate 400. A laminated structure of one or more films selected from a silicon nitride film, a silicon oxide nitride film, and a silicon oxynitride film. It can be formed more.

[0066] The material of the gate electrode layer 401 is a conductive material that is transparent to visible light, such as In-S n-Zn-O metal oxides, In-Al-Zn-O metal oxides, Sn-Ga-Zn -O-based metal oxides, Al-Ga-Zn-O-based metal oxides, Sn-Al-Zn-O-based Metal oxides, In-Zn-O metal oxides, Sn-Zn-O metal oxides, Al-Z nO-based metal oxides, In-O-based metal oxides, Sn-O-based metal oxides, Zn-O-based The metal oxide can be applied, and the film thickness is appropriately within the range of 30 nm to 200 nm. The metal oxide film used for the gate electrode layer 401 can be formed by sputtering or vacuum deposition. The method uses a deposition method (such as electron beam deposition), an arc discharge ion plating method, and a spray method. There are.

[0067] Next, a gate insulating layer 402 is formed over the gate electrode layer 401 .

[0068] The gate insulating layer 402 is a silicon oxide layer formed by using a plasma CVD method, a sputtering method, or the like. A silicon nitride layer, a silicon oxynitride layer, or a silicon nitride oxide layer may be formed as a single layer or a stacked layer. For example, the deposition gas can be SiH4, oxygen, and nitrogen, and the plasma CVD method can be used. A silicon oxynitride layer may be formed.

[0069] Next, an oxide semiconductor film having a thickness of 2 nm to 200 nm is formed over the gate insulating layer 402. Complete.

[0070] Note that before the oxide semiconductor film is formed by a sputtering method, argon gas is introduced to the plasma Reverse sputtering is performed to generate ions, and dust adhering to the surface of the gate insulating layer 402 is removed. In reverse sputtering, the target is sputtered in an argon atmosphere without applying a voltage to the target. A voltage is applied to the substrate side using an RF power source under atmospheric pressure to form plasma near the substrate and modify the surface. It is to be noted that nitrogen, helium, oxygen, etc. may be used in place of argon.

[0071] The oxide semiconductor film was formed by sputtering using an In-Ga-Zn-O oxide semiconductor target. The oxide semiconductor film is formed by oxidizing an oxide semiconductor film under a rare gas (typically, argon) atmosphere. The sputtering method is used in a nitrogen atmosphere or in an atmosphere of rare gas (typically argon) and oxygen. It can be formed more.

[0072] The gate insulating layer 402 and the oxide semiconductor film are successively formed without exposure to air. The gate insulating layer 402 and the oxide film 403 are successively formed without exposure to the air. The interface of the semiconductor film is exposed to atmospheric components such as water and hydrocarbons, as well as impurities floating in the air. The gate insulating layer 402 and the oxide semiconductor film can be formed without being contaminated by nitrogen. Therefore, the variation in the characteristics of the thin film transistors can be reduced.

[0073] The oxide semiconductor film is then subjected to a photolithography process to form an island-shaped oxide semiconductor layer, which is an oxide semiconductor layer. The resulting semiconductor layer is then processed into a dielectric layer (first oxide semiconductor layer 430) (see FIG. 1(A)).

[0074] Next, the first oxide semiconductor layer 430 is dehydrated or dehydrogenated. The temperature of the first heat treatment for siliconization is 350° C. or higher and lower than the distortion point of the substrate, preferably 400° C. Here, the substrate is introduced into an electric furnace, which is one type of heat treatment device, and the first oxidation The compound semiconductor layer 430 is subjected to a heat treatment in an oxygen atmosphere, and then gradually The oxide semiconductor layer is cooled to obtain a second oxide semiconductor layer 431 (see FIG. 1B). From the heating temperature T at which dehydration or dehydrogenation occurs to a temperature high enough to prevent water from re-entering the system, Specifically, the temperature is gradually cooled until it is 100°C or more lower than the heating temperature T. The substrate is then gradually cooled to a temperature lower than that of the second heat treatment, and the substrate is taken out of the heat treatment apparatus. By performing heat treatment on the oxide semiconductor layer in an oxygen atmosphere, water and the like contained in the oxide semiconductor layer can be removed. At the same time, the second oxide semiconductor layer 431 can be made to have an oxygen-excessive state. Depending on the conditions of the first heat treatment or the material of the oxide semiconductor layer, the oxide semiconductor layer may be crystallized and microcrystalline. In some cases, the film may be a crystalline or polycrystalline film.

[0075] In the first heat treatment, it is preferable that the oxygen gas does not contain water, hydrogen, or the like. Alternatively, the purity of the oxygen gas introduced into the heat treatment device must be 6N (99.9999%) or higher. Preferably, the oxygen concentration is 7N (99.99999%) or more (i.e., the impurity concentration in oxygen is 1 ppm or less). It is preferable to set the concentration of the ion exchange resin to 0.1 ppm or less.

[0076] The first heat treatment is carried out within a range of 0.5 hours to 10 hours, and the temperature rise characteristic of the electric furnace is set to 0. It is preferable to set the temperature drop rate to 1°C / min or more and 20°C / min or less. The range is preferably 0.1° C. / min to 15° C. / min.

[0077] As a result, the reliability of the thin film transistor to be formed later can be improved.

[0078] In addition to the heating method using an electric furnace, the first heat treatment also uses a GRT method using heated gas. A (Gas Rapid Thermal Anneal) method or L using lamp light Instantaneous heating methods such as the RTA (Lamp Rapid Thermal Anneal) method etc. can be used.

[0079] In addition, when the heat treatment apparatus is a multi-chamber type, the first heat treatment and the cooling treatment are performed in different chambers. Typically, the chamber is filled with oxygen gas and heated to 400°C or higher. In a first chamber heated to below the strain point of the substrate, an oxide semiconductor layer on the substrate is heated. Next, the container passes through a transfer chamber where oxygen gas is introduced, and is filled with oxygen and heated to 100℃ or less. The substrate that has been subjected to the first heat treatment is transferred to a second chamber, which is preferably at room temperature. By the above steps, the throughput can be improved.

[0080] In addition, the first heat treatment of the oxide semiconductor layer in an oxygen atmosphere is performed to form an island-shaped oxide semiconductor layer. In that case, the first oxide semiconductor film is After the heating and cooling processes in 1, the substrate is removed from the heating apparatus and subjected to the photolithography process. Do the following.

[0081] In addition, before the oxide semiconductor film is formed, an inert gas (nitrogen, helium, neon, or argon) is introduced. Heat treatment (400℃ or higher) in an atmosphere of rare gas such as benzene, oxygen, or reduced pressure. The gate insulation layer is then subjected to a process below the strain point of the plate to remove impurities such as hydrogen and water contained in the layer. It may also be a layer.

[0082] Next, a conductive film is formed over the gate insulating layer 402 and the second oxide semiconductor layer 431. Conductive films are formed by sputtering, vacuum deposition (electron beam deposition, etc.), and arc discharge. Ion plating or spraying is used.

[0083] The conductive film is made of a conductive material that is transparent to visible light, such as In-Sn-Z. nO-based metal oxides, In-Al-Zn-O-based metal oxides, Sn-Ga-Zn-O-based Metal oxides of Al-Ga-Zn-O system, metal oxides of Sn-Al-Zn-O system oxides, In-Zn-O metal oxides, Sn-Zn-O metal oxides, Al-Zn-O metal oxides of the In-O system, metal oxides of the Sn-O system, metal oxides of the Zn-O system An oxide can be used, and the film thickness is appropriately selected within the range of 30 nm to 200 nm. do.

[0084] Next, the second oxide semiconductor layer 431 and the conductive film are selectively formed by a photolithography process. The oxide semiconductor layer 403, the source electrode layer 405a, and the drain electrode layer 405b are selectively etched. Note that the oxide semiconductor layer is only partially etched, and a groove (a recess) is formed. In addition, the resist used in the photolithography process is an oxide semiconductor layer having the above structure. When the oxide mask is removed by oxygen ashing, the exposed region of the oxide semiconductor layer Oxygen is introduced into the

[0085] Next, an oxide insulating film 407 which serves as a protective insulating layer in contact with part of the oxide semiconductor layer 403 is formed. Thus, a thin film transistor 470 can be manufactured (see FIG. 1C). The insulating film 407 has a thickness of at least 1 nm and is formed by an acid deposition method such as a CVD method or a sputtering method. The oxide insulating film 407 can be formed by using a method that does not allow impurities such as water and hydrogen to be mixed therein. Here, the oxide insulating film 407 is formed by a sputtering method. The oxide insulating film 407 formed in contact with the oxide semiconductor layer is resistant to moisture, hydrogen ions, and OH - It is an inorganic insulating film that does not contain impurities such as those listed above and blocks their intrusion from the outside. Typically, a silicon oxide film, a silicon nitride oxide film, an aluminum oxide film, or an oxynitride film is used. An aluminum film or the like is used. A silicon nitride film or a nitride film in contact with the oxide insulating film 407 is also used. An aluminum film may be laminated. The silicon nitride film is resistant to moisture, hydrogen ions, and OH - Such as It does not contain any impurities and blocks these from entering from the outside.

[0086] In this embodiment, a silicon oxide film is formed as the oxide insulating film 407 to a thickness of 300 nm. The substrate temperature during film formation may be from room temperature to 300° C., and in this embodiment, it is set to 100° C. The silicon oxide film is formed by sputtering in a rare gas (typically argon) atmosphere. The reaction is carried out in an atmosphere of air, oxygen, or a rare gas (typically argon) and oxygen. In addition, a silicon oxide target or a silicon target can be used as the target. For example, a silicon target can be used for sputtering in an oxygen and nitrogen atmosphere. A silicon oxide film can be formed by a deposition method.

[0087] After the oxide insulating film 407 is formed, a thin film is formed under a nitrogen atmosphere or an oxygen atmosphere. Even if the transistor 470 is subjected to a second heat treatment (preferably at 150° C. or higher and lower than 350° C.), For example, the second heat treatment is performed at 250° C. for 1 hour in a nitrogen atmosphere. When the oxide semiconductor layer 403 is heated while being in contact with the oxide insulating film 407, As a result, the variation in the electrical characteristics of the thin film transistor 470 can be reduced.

[0088] (Embodiment 2) A semiconductor device different from that in Embodiment 1 and a method for manufacturing the semiconductor device will be described with reference to FIGS. The same parts as those in the first embodiment or parts having similar functions and steps are the same as those in the first embodiment. The above-mentioned process can be carried out in the above-mentioned manner, and a repeated explanation will be omitted.

[0089] 3A to 3D are cross-sectional views showing a manufacturing process of the thin film transistor 480. The thin film transistor 480 shown in FIG. 1 has a structure also called an inverted coplanar type (bottom contact type). It is one of the structures.

[0090] As in the first embodiment, a gate electrode layer 401 is provided over a substrate 400 having an insulating surface. In addition, an insulating film serving as a base film may be provided between the substrate 400 and the gate electrode layer 401 .

[0091] Next, a gate insulating layer 402 is formed on the gate electrode layer 401 in the same manner as in the first embodiment. Next, an oxide semiconductor film is formed over the gate insulating layer 402.

[0092] Next, the oxide semiconductor film is subjected to a photolithography process to form an island-shaped oxide semiconductor layer. The resulting semiconductor layer is then processed into a first oxide semiconductor layer (first oxide semiconductor layer 430) (see FIG. 3A). FIG. 3(A) is the same as FIG. 1(A).

[0093] Next, the first oxide semiconductor layer 430 is dehydrated or dehydrogenated. The temperature of the first heat treatment for siliconization is 350° C. or higher and lower than the distortion point of the substrate, preferably 400° C. Here, the substrate is introduced into an electric furnace, which is one type of heat treatment device, and the first oxidation The semiconductor layer 430 is exposed to an inert gas (nitrogen or a dilute gas such as helium, neon, or argon). Heat treatment is performed under a nitrogen atmosphere or reduced pressure to form a second oxide semiconductor layer 442. The oxide semiconductor layer is heated under an inert gas atmosphere or under reduced pressure (see FIG. 3B). Heat treatment reduces the resistance (increases the carrier concentration, preferably 1×10 18 / cm 3 Below In this way, the resistance of the oxide semiconductor layer (the second oxide semiconductor layer 442) can be reduced. do.

[0094] In the first heat treatment, nitrogen or a rare gas such as helium, neon, or argon is used. It is preferable that the nitrogen introduced into the heat treatment device does not contain water, hydrogen, etc. Or the purity of rare gases such as helium, neon, and argon is 6N or more, preferably 7N or more. (i.e., impurity concentration is 1 ppm or less, preferably 0.1 ppm or less). In this embodiment, the electric furnace containing the substrate is heated to 350° C. or higher and 600° C. or higher in a nitrogen atmosphere. After heating to 400°C or less, preferably 400°C or more to dehydrate or dehydrogenate, stops the introduction of the rare gas into the chamber and turns off the heater.

[0095] After the heating, the film is slowly cooled in an oxygen atmosphere to form a third oxide semiconductor layer 481 (FIG. 3C). (See reference 2.) From the heating temperature T at which the oxide semiconductor layer is dehydrated or dehydrogenated, water is not introduced again. In particular, the temperature must be kept at 100°C below the heating temperature T until the temperature is low enough to prevent the oxygen atmosphere from Alternatively, the temperature is lowered in an oxygen atmosphere to a temperature lower than that of the second heat treatment to be performed in the subsequent step. The substrate is gradually cooled in the atmosphere and then taken out of the heat treatment device. After the heater is turned off, oxygen is introduced into the electric furnace and the furnace is gradually cooled. It is preferable that the gas does not contain impurities such as water and hydrogen. The purity of the oxygen introduced into the bar is 6N or less, preferably 7N or less (i.e., impurities in the oxygen It is preferable to keep the concentration at 1 ppm or less, and preferably at 0.1 ppm or less.

[0096] As a result, the reliability of the thin film transistor to be formed later can be improved.

[0097] In addition, when the first heat treatment is performed under reduced pressure, oxygen is flowed into the electric furnace after the heat treatment to reduce the pressure. The pressure can then be returned to atmospheric pressure and cooled.

[0098] In addition, when the heat treatment apparatus is a multi-chamber type, the first heat treatment and the cooling treatment are performed in different chambers. Typically, the chamber is filled with nitrogen or a rare gas and has a temperature of 400 In a first chamber heated to a temperature above 100° C. but below the strain point of the substrate, an oxide semiconductor layer is deposited on the substrate. The layer is heated at a heating temperature T until it reaches a temperature where water cannot enter again. The temperature is gradually cooled until it drops by 100°C below T. Next, the temperature is lowered by 100°C by introducing nitrogen or rare gas into the carrier. A second chamber is filled with oxygen and is at a temperature below 100° C., preferably at room temperature. The substrate that has been subjected to the first heat treatment is then moved and cooled. The throughput can be improved.

[0099] In addition, the first heat treatment of the oxide semiconductor layer under an inert gas atmosphere or under reduced pressure is The oxide semiconductor film may be processed into a crystalline oxide semiconductor layer. After the first heating process and the cooling process, the substrate is removed from the heating apparatus and subjected to photolithography. The process is carried out.

[0100] In addition, before the oxide semiconductor film is formed, an inert gas (nitrogen, helium, neon, or argon) is introduced. Heat treatment (400℃ or higher) in an atmosphere of rare gas such as benzene, oxygen, or reduced pressure. The gate insulation layer is then subjected to a process below the strain point of the plate to remove impurities such as hydrogen and water contained in the layer. It may also be a layer.

[0101] Next, a conductive film is formed over the gate insulating layer 402 and the third oxide semiconductor layer 481.

[0102] The conductive film is made of a conductive material that is transparent to visible light, such as In-Sn-Z. nO-based metal oxides, In-Al-Zn-O-based metal oxides, Sn-Ga-Zn-O-based Metal oxides of Al-Ga-Zn-O system, metal oxides of Sn-Al-Zn-O system oxides, In-Zn-O metal oxides, Sn-Zn-O metal oxides, Al-Zn-O metal oxides of the In-O system, metal oxides of the Sn-O system, metal oxides of the Zn-O system An oxide can be used, and the film thickness is appropriately selected within the range of 30 nm to 200 nm. do.

[0103] Next, the third oxide semiconductor layer 481 and the conductive film are selectively formed by a photolithography process. The oxide semiconductor layer 483, the source electrode layer 405a, and the drain electrode layer 405b are selectively etched. Note that the oxide semiconductor layer is only partially etched, and a groove (a recess) is formed. In addition, the resist used in the photolithography process is an oxide semiconductor layer having the above structure. When the oxide mask is removed by oxygen ashing, the exposed region of the oxide semiconductor layer Oxygen is introduced into the

[0104] Next, the oxide insulating film 407 which serves as a protective insulating layer in contact with part of the oxide semiconductor layer 483 is formed. Thus, a thin film transistor 480 can be manufactured (see FIG. 3D). The insulating film 407 has a thickness of at least 1 nm and is formed by an acid deposition method such as a CVD method or a sputtering method. The oxide insulating film 407 can be formed by using a method that does not allow impurities such as water and hydrogen to be mixed therein. Here, the oxide insulating film 407 is formed by a sputtering method. The oxide insulating film 407 formed in contact with the oxide semiconductor layer is resistant to moisture, hydrogen ions, and OH - It is an inorganic insulating film that does not contain impurities such as those listed above and blocks their intrusion from the outside. Typically, a silicon oxide film, a silicon nitride oxide film, an aluminum oxide film, or an oxynitride film is used. An aluminum film or the like is used. An aluminum nitride film may be laminated. The silicon nitride film is resistant to moisture, hydrogen ions, and OH - etc. It does not contain impurities and blocks them from entering from the outside.

[0105] In this embodiment, a silicon oxide film is formed as the oxide insulating film 407 to a thickness of 300 nm. The substrate temperature during film formation may be from room temperature to 300° C., and in this embodiment, it is set to 100° C. The silicon oxide film is formed by sputtering in a rare gas (typically argon) atmosphere. The reaction is carried out in an atmosphere of air, oxygen, or a rare gas (typically argon) and oxygen. In addition, a silicon oxide target or a silicon target can be used as the target. For example, a silicon target can be used for sputtering in an oxygen and nitrogen atmosphere. A silicon oxide film can be formed by a deposition method.

[0106] After the oxide insulating film 407 is formed, a thin film is formed under a nitrogen atmosphere or an oxygen atmosphere. Even if the transistor 480 is subjected to a second heat treatment (preferably at 150° C. or higher and lower than 350° C.), For example, the second heat treatment is performed at 250° C. for 1 hour in a nitrogen atmosphere. When the oxide semiconductor layer 483 is heated while being in contact with the oxide insulating film 407, As a result, the variation in the electrical characteristics of the thin film transistor 480 can be reduced.

[0107] This embodiment mode can be freely combined with the first embodiment mode.

[0108] (Embodiment 3) A semiconductor device and a manufacturing method of the semiconductor device different from those in Embodiment Mode 1 and Embodiment Mode 2 will be described with reference to FIG. The following will be described. The same parts as those in the first and second embodiments or parts having similar functions. The steps and processes can be carried out in the same manner as in the first and second embodiments, and the description will be repeated. is omitted.

[0109] 4A to 4C are cross-sectional views showing a manufacturing process of the thin film transistor 440. The thin film transistor 440 shown in FIG.

[0110] As in the first embodiment, a gate electrode layer 401 is provided over a substrate 400 having an insulating surface. In addition, an insulating film serving as a base film may be provided between the substrate 400 and the gate electrode layer 401 .

[0111] Next, a gate insulating layer 402 is formed on the gate electrode layer 401 in the same manner as in the first embodiment. Next, an oxide semiconductor film is formed over the gate insulating layer 402.

[0112] Next, the oxide semiconductor film is subjected to a photolithography process to form an island-shaped oxide semiconductor layer. The resulting semiconductor layer is then processed into a first oxide semiconductor layer (first oxide semiconductor layer 430) (see FIG. 4A). FIG. 4(A) is the same as FIG. 1(A).

[0113] Next, the first oxide semiconductor layer 430 is dehydrated or dehydrogenated. The temperature of the first heat treatment for siliconization is 350° C. or higher and lower than the distortion point of the substrate, preferably 400° C. Here, the substrate is introduced into an electric furnace, which is one type of heat treatment device, and the first oxidation The semiconductor layer 430 is exposed to an inert gas (nitrogen or a dilute gas such as helium, neon, or argon). The second oxide semiconductor layer 4 is formed by heat treatment under a nitrogen atmosphere or reduced pressure and then gradually cooled. The value is 44 (see Figure 4(B)).

[0114] In the first heat treatment, nitrogen or a rare gas such as helium, neon, or argon is used. It is preferable that the nitrogen introduced into the heat treatment device does not contain water, hydrogen, etc. Or the purity of rare gases such as helium, neon, and argon must be 6N (99.9999%) or higher. Preferably, the concentration of impurities is 7N (99.99999%) or more (i.e., the impurity concentration is 1 ppm or less, In this embodiment, the substrate is introduced into the electrode. The inside of the furnace is heated to 350°C or higher and 600°C or lower, preferably 400°C or higher, in a nitrogen atmosphere. After dehydration or dehydrogenation, the heater is turned off and the material is gradually cooled. The semiconductor layer is heated in an inert gas atmosphere or under reduced pressure and then cooled slowly to obtain a low resistance (The carrier concentration is increased, preferably 1×10 18 / cm 3 (above) and the acid with low resistance The second oxide semiconductor layer 444 may be an oxide semiconductor layer.

[0115] If the heat treatment is performed under reduced pressure, the pressure should be reduced by flowing an inert gas into the electric furnace after the heat treatment. The pressure can then be returned to atmospheric pressure and cooled.

[0116] In addition, if the heat treatment equipment is a multi-chamber type, the heating process and the cooling process are performed in different chambers. Typically, the furnace is filled with nitrogen or a rare gas and is heated to 200°C or higher. In a first chamber heated to 600° C. or less, preferably 400° C. to 450° C. Then, the oxide semiconductor layer on the substrate is heated at a heating temperature T, and the temperature is set to a sufficient level so that water does not enter again. The temperature is gradually cooled to 300°C, specifically, until it is 100°C lower than the heating temperature T. Next, nitrogen or The chamber is filled with nitrogen or rare gas and is heated to 100°C or less. The heat-treated substrate is transferred to a second chamber, which is preferably at room temperature, and cooled. Through these steps, the throughput can be improved.

[0117] In addition, the heat treatment of the oxide semiconductor layer under an inert gas atmosphere or under reduced pressure can form island-shaped oxide films. It is also possible to perform this treatment on the oxide semiconductor film before processing it into an oxide semiconductor layer. In that case, an inactive After heat treatment of the oxide semiconductor film under a gas atmosphere or reduced pressure, The substrate is then removed from the heating apparatus and a photolithography process is performed.

[0118] In addition, before the oxide semiconductor film is formed, an inert gas (nitrogen, helium, neon, or argon) is introduced. Heat treatment (400℃ or higher) in an atmosphere of rare gas such as benzene, oxygen, or reduced pressure. The gate insulation layer is then subjected to a process below the strain point of the plate to remove impurities such as hydrogen and water contained in the layer. It may also be a layer.

[0119] Next, a conductive film is formed over the gate insulating layer 402 and the second oxide semiconductor layer 444.

[0120] The conductive film is made of a conductive material that is transparent to visible light, such as In-Sn-Z. nO-based metal oxides, In-Al-Zn-O-based metal oxides, Sn-Ga-Zn-O-based Metal oxides of Al-Ga-Zn-O system, metal oxides of Sn-Al-Zn-O system oxides, In-Zn-O metal oxides, Sn-Zn-O metal oxides, Al-Zn-O metal oxides of the In-O system, metal oxides of the Sn-O system, metal oxides of the Zn-O system An oxide can be used, and the film thickness is appropriately selected within the range of 30 nm to 200 nm. do.

[0121] Next, the second oxide semiconductor layer 444 and the conductive film are selectively formed by a photolithography process. The oxide semiconductor layer, the source electrode layer 405a, and the drain electrode layer 405 are selectively etched. Note that the oxide semiconductor layer is only partially etched to have a groove (a depression). In addition, the resist mask used in the photolithography process is When oxygen ashing is performed to remove the oxide semiconductor layer, oxygen is introduced into the exposed region of the oxide semiconductor layer. will be introduced.

[0122] Next, an oxide insulating film 407 serving as a protective insulating layer in contact with part of the oxide semiconductor layer is formed. The oxide insulating film 407 has a thickness of at least 1 nm. The oxide insulating film 407 is formed by using an appropriate method that does not allow impurities such as water and hydrogen to be mixed therein. Here, the oxide insulating film 407 is formed by a sputtering method. The oxide insulating film 407 formed in contact with the low-resistance oxide semiconductor layer is resistant to moisture and hydrogen. Ions and OH - It does not contain impurities such as nicotinamide, and blocks them from entering from the outside. An inorganic insulating film is used, typically a silicon oxide film, a silicon nitride oxide film, an aluminum oxide film, or An aluminum oxynitride film or the like is used as the insulating film 407. A bare film or an aluminum nitride film may be laminated. The silicon nitride film is resistant to moisture, hydrogen ions, OH - It does not contain impurities such as these, and blocks them from entering from the outside.

[0123] A thin film is formed on the second oxide semiconductor layer 444 by a sputtering method, a PCVD method, or the like. When the oxide insulating film 407 is formed, the oxide semiconductor layer 444 has a low resistance. In addition, the region in contact with the oxide insulating film 407 is made to have a high resistance (the carrier concentration is reduced, preferably 1 ×10 18 / cm 3 The thickness of the oxide semiconductor region can be reduced by 100 nm to 100 nm, and the thickness of the oxide semiconductor region can be reduced by 100 nm to 100 nm. The region overlapping with the source electrode layer 405a and the drain electrode layer 405b remains low in resistance. There are two low-resistance oxide semiconductor regions sandwiching a high-resistance oxide semiconductor region therebetween. During the manufacturing process of semiconductor devices, heating, slow cooling, and It is important to increase or decrease the carrier concentration in the oxide semiconductor layer by forming an oxide insulating film, etc. The oxide semiconductor layer 444 includes a high-resistance oxide semiconductor region and a low-resistance oxide semiconductor region. The oxide semiconductor layer 443 (the third oxide semiconductor layer) having the region is formed as a thin film transistor. The high resistance oxide semiconductor region can be used to fabricate the thin film transistor 440. This becomes the channel formation region of 40.

[0124] Note that the oxide semiconductor layer 443 overlapping with the drain electrode layer (and the source electrode layer) has a low By forming a resistive oxide semiconductor region, the reliability of the driver circuit is improved. Specifically, by forming a low-resistance oxide semiconductor region, The conductivity is gradually changed from the electrode layer to the low-resistance oxide semiconductor region and the channel formation region. Therefore, the drain electrode layer is connected to a high power supply potential VD When the wiring supplying D is connected, a high Even when an electric field is applied, the low-resistance oxide semiconductor region acts as a buffer, preventing a local high electric field from being applied. Therefore, the withstand voltage of the transistor can be improved.

[0125] In addition, in the oxide semiconductor layer 443 overlapping with the drain electrode layer (and the source electrode layer), By forming a resistive oxide semiconductor region, a channel formation region when a driver circuit is formed is Specifically, the low resistance oxide semiconductor region can be formed by By forming the gate insulating film, the leakage current of the transistor flowing between the drain electrode layer and the source electrode layer is reduced. The flow path is the drain electrode layer, the low resistance oxide semiconductor region on the drain electrode layer side, The order is the panel formation region, the low resistance oxide semiconductor region on the source electrode layer side, and the source electrode layer. At this time, in the channel formation region, the channel is formed from the low-resistance oxide semiconductor region on the drain electrode layer side. The leakage current flowing in the channel formation region is regulated by the gate insulating layer, which becomes highly resistive when the transistor is off. The gate electrode and the back channel region can be concentrated near the interface. The leakage current at the surface of the channel forming region that is separated from the do.

[0126] After the oxide insulating film 407 is formed, a thin film is formed under a nitrogen atmosphere or an oxygen atmosphere. Even if the transistor 440 is subjected to a second heat treatment (preferably at 150° C. or higher and lower than 350° C.), For example, the second heat treatment is performed at 250° C. for 1 hour in a nitrogen atmosphere. When the oxide semiconductor layer 443 is heated while being in contact with the oxide insulating film 407, As a result, the variation in the electrical characteristics of the thin film transistor 440 can be reduced.

[0127] This embodiment mode can be freely combined with embodiment mode 1 or 2.

[0128] (Embodiment 4) A semiconductor device and a method for manufacturing the semiconductor device will be described with reference to FIGS.

[0129] FIG. 6A is a plan view of a thin film transistor 460 included in a semiconductor device, and FIG. The thin film transistor 460 is a bottom gate. A gate electrode layer 451 is formed on a substrate 450 having an insulating surface. , a gate insulating layer 452, a source electrode layer 455a, a drain electrode layer 455b, and an oxide semiconductor layer. The thin film transistor 460 is covered with a conductor layer 453. The oxide semiconductor layer 453 is formed of In-Ga-Zn -O-based non-single crystal film is used.

[0130] The thin film transistor 460 has a gate insulating layer in the entire region including the thin film transistor 460. A layer 452 is present between the gate insulating layer 452 and a substrate 450 that is a substrate having an insulating surface. A gate electrode layer 451 is provided. A source electrode layer 455a is provided on the gate insulating layer 452. A gate insulating layer 452 and a source electrode layer 455b are provided. The oxide semiconductor layer 453 is provided over the source electrode layer 455a and the drain electrode layer 455b. Although not shown, a source electrode layer 455a and a drain electrode layer 455b are formed over the gate insulating layer 452. In addition to the electrode layer 455b, a wiring layer is provided. The wiring layer is provided outside the outer periphery of the oxide semiconductor layer 453. It extends to the side.

[0131] Also, a substrate 450 having an insulating surface, a gate electrode layer 451, a gate insulating layer 452, an oxide The semiconductor layer 453, the source electrode layer 455a, the drain electrode layer 455b, and the oxide insulating film 4 57 is made of a material that is transparent to visible light. The thin film transistor 460 has a light-transmitting property, and is disposed in a pixel portion of a display device. In this case, the aperture ratio can be improved.

[0132] The oxide semiconductor layer 453 is formed by removing at least moisture, which is an impurity, from the oxide semiconductor layer 453 after the oxide semiconductor film is formed. After the heat treatment to reduce the The oxide insulating film 457 is formed in contact with the oxide semiconductor film to form a channel formation region. Used as.

[0133] 5A to 5C are cross-sectional views showing a manufacturing process of the thin film transistor 460 shown in FIG. Shows.

[0134] A gate electrode layer 451 is provided over a substrate 450 having an insulating surface. An insulating film serving as a base film may be provided between the substrate 450 and the gate electrode layer 451. It has the function of preventing the diffusion of impurity elements from 50, and is used in silicon nitride films, silicon oxide films, and nitride oxide films. The insulating film is formed by a laminate structure of one or more films selected from a silicon film and a silicon oxynitride film. It is possible.

[0135] The material of the gate electrode layer 451 is a conductive material that is transparent to visible light, such as In-S n-Zn-O metal oxides, In-Al-Zn-O metal oxides, Sn-Ga-Zn -O-based metal oxides, Al-Ga-Zn-O-based metal oxides, Sn-Al-Zn-O-based Metal oxides, In-Zn-O metal oxides, Sn-Zn-O metal oxides, Al-Z nO-based metal oxides, In-O-based metal oxides, Sn-O-based metal oxides, Zn-O-based The metal oxide can be applied, and the film thickness is appropriately within the range of 30 nm to 200 nm. Select.

[0136] Next, a gate insulating layer 452 is formed over the gate electrode layer 451 .

[0137] The gate insulating layer 452 is a silicon oxide layer formed by using a plasma CVD method, a sputtering method, or the like. A silicon nitride layer, a silicon oxynitride layer, or a silicon nitride oxide layer may be formed as a single layer or a stacked layer. For example, the deposition gas can be SiH4, oxygen, and nitrogen, and the plasma CVD method can be used. A silicon oxynitride layer may be formed.

[0138] Next, a conductive film is formed over the gate insulating layer 452, and an island-like The resulting semiconductor layer is processed into a source electrode layer 455a and a drain electrode layer 455b (see FIG. 5A).

[0139] The conductive film is made of a conductive material that is transparent to visible light, such as In-Sn-Z. nO-based metal oxides, In-Al-Zn-O-based metal oxides, Sn-Ga-Zn-O-based Metal oxides of Al-Ga-Zn-O system, metal oxides of Sn-Al-Zn-O system oxides, In-Zn-O metal oxides, Sn-Zn-O metal oxides, Al-Zn-O metal oxides of the In-O system, metal oxides of the Sn-O system, metal oxides of the Zn-O system An oxide can be used, and the film thickness is appropriately selected within the range of 30 nm to 200 nm. do.

[0140] Next, an oxide film was formed on the gate insulating layer 452, the source electrode layer 455a, and the drain electrode layer 455b. Then, an island-shaped oxide semiconductor layer 483 (the first The photolithography process is then performed to obtain a semiconductor layer (oxide semiconductor layer 1) (see FIG. 5B). When removing the resist mask used in the photolithography process, oxygen ashing is performed, and the oxide semiconductor Oxygen is introduced into the exposed areas of the layer.

[0141] Note that before the oxide semiconductor film is formed by a sputtering method, argon gas is introduced to the plasma Reverse sputtering is performed to generate ions, and dust adhering to the surface of the gate insulating layer 452 is removed. It is preferable to do so.

[0142] The oxide semiconductor layer 483 is subjected to first heat treatment for dehydration or dehydrogenation. The temperature of the first heat treatment for hydrogenation or dehydrogenation is 350° C. or higher and lower than the distortion point of the substrate, preferably The temperature must be 400°C or higher.

[0143] The first heat treatment for dehydration or dehydrogenation is performed using an inert gas (nitrogen or helium). The gas is heated in an atmosphere of rare gases such as ammonium, neon, argon, etc., in an oxygen atmosphere, or under reduced pressure. After that, heat treatment is performed. The heating temperature T at which the oxide semiconductor layer is dehydrated or dehydrogenated is changed to The temperature must be at least 100°C lower than the heating temperature T so that water does not enter again. Alternatively, the temperature is gradually cooled to a temperature lower than that of the second heat treatment to be performed in the subsequent step. Then, the substrate is removed from the heat treatment device.

[0144] In this embodiment, the first heat treatment is performed in an oxygen atmosphere as in the first embodiment. The oxide semiconductor layer 453 is formed by slowly cooling the oxide semiconductor layer 453 in which impurities such as moisture are reduced. The combination of the first heat treatment and the slow cooling is not particularly limited, and may be any of the combinations of the first heat treatment and the slow cooling. Any one of the combinations and procedures of the second embodiment or the third embodiment may be used. Cut.

[0145] In the first heat treatment, an inert gas (nitrogen, helium, neon, argon) is used. It is preferable that the atmosphere of rare gases such as fluorine or oxygen does not contain water, hydrogen, etc. Alternatively, the purity of the gas introduced into the heat treatment device is preferably 6N (99.9999%) or more. or 7N (99.99999%) or more (i.e. impurity concentration in the atmosphere is 1 ppm or less, Preferably, the concentration is 0.1 ppm or less.

[0146] As a result, the reliability of the thin film transistor to be formed later can be improved.

[0147] In addition, the first heat treatment of the oxide semiconductor layer in an oxygen atmosphere is performed to form an island-shaped oxide semiconductor layer. In that case, the first oxide semiconductor film is After the heating and cooling processes in 1, the substrate is removed from the heating apparatus and subjected to the photolithography process. Do the following.

[0148] In addition, before the oxide semiconductor film is formed, an inert gas (nitrogen, helium, neon, or argon) is introduced. Heat treatment (400℃ or higher) in an atmosphere of rare gas such as benzene, oxygen, or reduced pressure. The gate insulation layer is then subjected to a process below the strain point of the plate to remove impurities such as hydrogen and water contained in the layer. It may also be a layer.

[0149] Next, an oxide insulating film is formed on the oxide semiconductor layer 453 by a sputtering method or a PCVD method. By forming 457, a thin film transistor 460 can be manufactured (see FIG. 5C). In this embodiment, a silicon oxide film with a thickness of 300 nm is formed as the oxide insulating film 457. The substrate temperature during film formation may be set to room temperature or higher and 300° C. or lower. In this embodiment, the substrate temperature is set to 100° C. Let us assume that.

[0150] After the oxide insulating film 457 is formed, a thin film is formed under a nitrogen atmosphere or an oxygen atmosphere. Even if the transistor 460 is subjected to a second heat treatment (preferably at 150° C. or higher and lower than 350° C.), For example, the second heat treatment is performed at 250° C. for 1 hour in a nitrogen atmosphere. When the oxide semiconductor layer 453 is heated while being in contact with the oxide insulating film 457, As a result, the variation in the electrical characteristics of the thin film transistor 460 can be reduced.

[0151] This embodiment can be freely combined with embodiment 1, embodiment 2, or embodiment 3. It is possible.

[0152] (Embodiment 5) In this embodiment, an example of a channel stop type thin film transistor 1430 will be described with reference to FIG. FIG. 7(C) shows the structure of a thin film transistor. This is an example of a plan view, and the cross-sectional view taken along the chain line Z1-Z2 in the figure corresponds to FIG. 7(B). In addition, the oxide semiconductor layer of the thin film transistor 1430 is made of an oxide semiconductor material that does not contain gallium. Here is an example of using the fee.

[0153] First, a gate electrode layer 1401 is provided over a substrate 1400 .

[0154] In addition, an insulating film serving as a base film may be provided between the substrate 1400 and the gate electrode layer 1401 . The undercoat film has a function of preventing the diffusion of impurity elements from the substrate 1400. A laminate of one or more films selected from a silicon nitride film, a silicon oxynitride film, and a silicon oxynitride film. It can be formed by structure.

[0155] The gate electrode layer 1401 is made of a conductive material that is transparent to visible light, such as In- Sn-Zn-O metal oxides, In-Al-Zn-O metal oxides, Sn-Ga-Z nO-based metal oxides, Al-Ga-Zn-O-based metal oxides, Sn-Al-Zn-O-based Metal oxides of In-Zn-O system, metal oxides of Sn-Zn-O system, metal oxides of Al- Zn-O metal oxides, In-O metal oxides, Sn-O metal oxides, Zn-O The film thickness is preferably within the range of 30 nm to 200 nm. Please choose accordingly.

[0156] Next, a gate insulating layer 1402 is formed to cover the gate electrode layer 1401. An oxide semiconductor layer is formed over the layer 1402 .

[0157] In this embodiment, a Sn-Zn-O oxide semiconductor layer is formed by sputtering. By not using gallium in the oxide semiconductor layer, expensive target This reduces costs because it is not necessary to use a kit.

[0158] Immediately after the oxide semiconductor film is formed or after the oxide semiconductor layer is processed into an island shape, Hydrogenation is carried out.

[0159] The first heat treatment for dehydration or dehydrogenation is performed using an inert gas (nitrogen or helium). The gas is heated in an atmosphere of rare gases such as ammonium, neon, argon, etc., in an oxygen atmosphere, or under reduced pressure. The temperature of the first heat treatment is 350° C. or higher and lower than the distortion point of the substrate, preferably 4 After that, the heating temperature T at which the oxide semiconductor layer is dehydrated or dehydrogenated is set to 00° C. or higher. Then, heat the container to a temperature that is high enough to prevent water from entering again, specifically, 100°C higher than the heating temperature T. Or, gradually cool it down to a temperature lower than that of the second heat treatment to be performed in the subsequent step. After cooling, the substrate is removed from the heat treatment device.

[0160] In this embodiment, the first heat treatment is performed in an oxygen atmosphere as in the first embodiment. The oxide semiconductor layer 1403 is obtained by gradually cooling the oxide semiconductor layer 1403 in which impurities such as moisture are reduced. (See FIG. 7(A)). The combination of the first heat treatment and the slow cooling is not particularly limited. Any one combination and method of embodiment 1, embodiment 2, or embodiment 3 The order can be used.

[0161] In the first heat treatment, an inert gas (nitrogen, helium, neon, argon) is used. It is preferable that the atmosphere of rare gases such as fluorine or oxygen does not contain water, hydrogen, etc. Alternatively, the purity of the gas introduced into the heat treatment device is set to 6N or more, preferably 7N or more (i.e. It is preferable to keep the impurity concentration in the atmosphere at 1 ppm or less, preferably 0.1 ppm or less. I wish.

[0162] As a result, the reliability of the thin film transistor to be formed later can be improved.

[0163] In addition, the first heat treatment of the oxide semiconductor layer in an oxygen atmosphere causes the oxide semiconductor layer to have an island shape. In that case, the first oxide semiconductor film is After the heating and cooling processes in 1, the substrate is removed from the heating apparatus and subjected to the photolithography process. Do the following.

[0164] In addition, before the oxide semiconductor film is formed, an inert gas (nitrogen, helium, neon, or argon) is introduced. Heat treatment (400℃ or higher) in an atmosphere of rare gas such as benzene, oxygen, or reduced pressure. The gate insulation layer is then subjected to a process below the strain point of the plate to remove impurities such as hydrogen and water contained in the layer. It may also be a layer.

[0165] Next, a channel protective layer 1418 is provided over and in contact with the oxide semiconductor layer 1403. By providing the oxide semiconductor protective layer 1418, Damage during the process (film loss due to plasma or etching agent during etching, etc.) Therefore, the reliability of the thin film transistor 1430 can be improved. can.

[0166] In addition, after the heat treatment for dehydration or dehydrogenation, the A protective layer 1418 can also be formed on the substrate. By doing so, the interface is free from atmospheric components such as water and hydrocarbons, as well as impurities suspended in the air. The oxide semiconductor layer 1403 and the channel protection layer 1418 are formed without being contaminated by oxygen. Therefore, the variation in the characteristics of the thin film transistors can be reduced.

[0167] The channel protection layer 1418 is made of an inorganic material containing oxygen (silicon oxide, silicon oxynitride, nitride, etc.). The material used for the thin film is silicon oxide. The method of fabrication is plasma CVD or thermal CVD. The channel protection layer 1418 can be formed by a vapor deposition method or a sputtering method such as After the film is formed, the shape is processed by etching. Here, the silicon oxide film is formed by the sputtering method. The channel is then formed by etching using a mask in a photolithography process. A protective layer 1418 is formed. In addition, the resist mask used in the photolithography process is When oxygen ashing is performed to remove the mask, oxygen is introduced into the exposed region of the oxide semiconductor layer. An element is introduced.

[0168] Next, a conductive film is formed over the channel protective layer 1418 and the oxide semiconductor layer 1403.

[0169] The conductive film is made of a conductive material that is transparent to visible light, such as In-Sn-Z. nO-based metal oxides, In-Al-Zn-O-based metal oxides, Sn-Ga-Zn-O-based Metal oxides of Al-Ga-Zn-O system, metal oxides of Sn-Al-Zn-O system oxides, In-Zn-O metal oxides, Sn-Zn-O metal oxides, Al-Zn-O metal oxides of the In-O system, metal oxides of the Sn-O system, metal oxides of the Zn-O system An oxide can be used, and the film thickness is appropriately selected within the range of 30 nm to 200 nm. do.

[0170] Next, the conductive film is selectively etched using a mask in a photolithography process. The source electrode layers 1405a and 1405b are formed on the channel protection layer 1418 and the oxide semiconductor layer 1403. A drain electrode layer 1405b is formed on each of the thin film transistors 1430 (FIG. 7(B)).

[0171] This embodiment can be freely combined with embodiment 1, embodiment 2, or embodiment 3. It is possible.

[0172] (Embodiment 6) In this embodiment mode, a liquid crystal display device in which the thin film transistor shown in Embodiment 1 is arranged in a pixel portion is An example of the device is shown in Figs. 8, 9, 10, 11, 12, 13, 14, and 15. This is explained below.

[0173] In FIG. 8A, a light-transmitting substrate 100 is made of barium borosilicate glass or aluminum. A glass substrate such as borosilicate glass can be used. 1000mm x 1200mm, 1100mm x 1250mm, 1150mm x 130 A large-area substrate such as 0 mm may be used. By using a large-area substrate, A plurality of liquid crystal display devices can be manufactured by the above method, and the manufacturing cost can be reduced. A 600mm x 720mm glass substrate is used.

[0174] Next, a conductive film having a translucency to visible light is formed on the entire surface of the substrate 100, and then a first film is formed on the conductive film. A photolithography process is carried out, a resist mask is formed, and unnecessary parts are removed by etching. The wiring and electrodes (gate wiring including the gate electrode layer 101, the capacitance wiring 108, and At this time, a taper is formed at least at the end of the gate electrode layer 101. Etch to form features.

[0175] When using a large-area substrate, the photomask for the photolithography process is expensive. In order to form the resist mask, the resist mask may be formed by an inkjet method. The jet method can reduce the manufacturing cost. In at least one step of the photolithography process, a resist mask is applied by the inkjet method. It may be formed.

[0176] A gate wiring including a gate electrode layer 101, a capacitance wiring 108, and a first terminal 121 of a terminal portion is a conductive material that is transparent to visible light, such as an In-Sn-Zn-O metal oxide. In-Al-Zn-O metal oxides, Sn-Ga-Zn-O metal oxides, Al -Ga-Zn-O metal oxides, Sn-Al-Zn-O metal oxides, In-Zn- O-based metal oxides, Sn-Zn-O-based metal oxides, Al-Zn-O-based metal oxides, I By applying nO-based metal oxides, Sn-O-based metal oxides, and Zn-O-based metal oxides, The thickness of the conductive film is appropriately selected within the range of 30 nm to 200 nm. deposition method, vacuum deposition method (electron beam deposition method, etc.), arc discharge ion plating method, The inkjet method is used to form the inkjet printhead. This eliminates the need for a photolithography process, achieving further cost reductions.

[0177] In this embodiment, the conductive film is formed by sputtering using an In-Sn-O target. After the conductive film is formed, it is made into a low-resistance conductive film. The target is made of a target material attached to a backing plate (target The target is attached to a backing plate. When attaching the get, the target is divided and bonded to one backing plate. If the target is divided, the size of the target when it is attached to the backing plate can be reduced. Such a divided target can be used to form the thin film on a large-area substrate. In the case of depositing a film, the target is enlarged accordingly, and the present invention can be particularly suitably used for this purpose. Of course, one target may be attached to one backing plate.

[0178] There are two types of sputtering: RF sputtering, which uses a high-frequency power source for the sputtering power supply, and DC sputtering. There is also the pulsed DC sputtering method, which applies a pulsed bias. The DC sputtering method is mainly used for depositing insulating films, while the DC sputtering method is mainly used for depositing metal films. It is used in.

[0179] There are also multi-target sputtering devices that can accommodate multiple targets of different materials. The equipment can deposit layers of different materials in the same chamber, or multiple types of films in the same chamber. It is also possible to form a film by discharging two or more materials at the same time.

[0180] Also, a sputtering apparatus using a magnetron sputtering method equipped with a magnet mechanism inside the chamber and ECR sputtering using plasma generated by microwaves without glow discharge. There is a sputtering apparatus that uses this method.

[0181] In addition, in a film formation method using a sputtering method, a target material and a sputtering gas component are mixed during film formation. Reactive sputtering is a method of forming thin films of compounds by chemically reacting them with each other, and There is also a bias sputtering method in which a voltage is also applied to the substrate.

[0182] Next, a gate insulating layer 102 is formed on the entire surface of the gate electrode layer 101. 02 is a method using sputtering or PCVD, etc., with a film thickness of 50 nm to 250 nm. The gate insulating layer 102 is a silicon oxide film, a silicon oxynitride film, or a silicon nitride oxide film. , silicon nitride film, tantalum oxide film, etc. are used as inorganic insulating films, and a single layer made of these materials is used. Or, it is formed as a laminated structure.

[0183] In this embodiment, monosilane gas ( SiH4), nitrous oxide (N2O) and rare gases are introduced and heated at high pressures of 10 Pa to 30 Pa. A high-density plasma is generated to form a gate insulating layer 102 having a thickness of 100 nm on the gate electrode layer 101. The gate insulating layer 102 is a silicon oxynitride film. , High density plasma device is 1×10 11 / cm 3 A device that can achieve a plasma density of For example, a microwave power of 3kW to 6kW is applied to generate plasma. When forming the insulating film, the monosilane gas (Si The flow ratio of H4) to nitrous oxide (N2O) should be in the range of 1:10 to 1:200. The rare gases introduced into the chamber are helium, argon, krypton, and xenon. Among them, it is preferable to use argon, which is inexpensive.

[0184] In addition, the gate insulating layer 102 obtained by the high density plasma device has a constant film thickness. It has excellent step coverage. In addition, by forming an insulating film using a high-density plasma device, The thickness can be precisely controlled.

[0185] The insulating film obtained by the high-density plasma device is different from that obtained by the conventional parallel plate type PCVD device. The etching rates of the insulating films are significantly different from those of the insulating films used in the past. In this case, the insulating film obtained by the conventional parallel plate type PCVD equipment is 10% or more or 2 0% slower, and the insulating film obtained by the high-density plasma device can be said to be a dense film.

[0186] Next, an oxide semiconductor film (In-Ga-Zn-O-based non-single crystal film) is formed on the gate insulating layer 102. After the plasma treatment, the In-Ga-Zn-O non-single crystal film is formed without exposure to the atmosphere. Deposition of the film is useful in that it prevents dust and moisture from adhering to the interface between the gate insulating layer and the semiconductor film. Here, an oxide semiconductor target ( In-Ga-Zn-O oxide semiconductor target (In2O3:Ga2O3:ZnO=1 The molar ratio was 1:1, the distance between the substrate and the target was 170 mm, and the pressure was 0 .4Pa, direct current (DC) power supply 0.5kW, oxygen only, argon only, or argon and oxygen The film is formed in a nitrogen atmosphere. If a pulsed direct current (DC) power supply is used, dust can be reduced and the film can be formed more efficiently. This is also preferable because the thickness distribution is uniform. The thickness of the In-Ga-Zn-O non-single crystal film is 2n The oxide semiconductor film is an In-Ga-Zn-O oxide semiconductor film. Using a target, a 50 nm thick In-Ga-Zn-O non-single crystal film was formed by sputtering. In order to maintain the amorphous state, it is preferable to make the film thickness 50 nm or less. In the case of a thin-film transistor of the N-type, the thin film is further etched, and the thin film is That is, the film thickness of the channel formation region is 30 nm or less, and the final thin-film transistor The thickness of the thin film region of the capacitor is 5 nm to 20 nm. The channel width of the thin film transistor is preferably 0.5 μm or more and 10 μm or less.

[0187] In addition, the target is attached to a backing plate (a plate for attaching the target). The substrate is then attached to the substrate and vacuum packed. In order to obtain the electrical characteristics of the diode, it is necessary to avoid exposing it to moisture in the air as much as possible. It is preferable to place the backing plate with the target material attached in a sputtering apparatus. This is not limited to installation in a sputtering device, but also applies when manufacturing targets or when backing up targets. When bonding to the plate and before vacuum packaging, the target is to avoid atmospheric moisture as much as possible. It is preferable to prevent the two devices from touching each other.

[0188] Next, a second photolithography process is performed to form a resist mask, and the oxide semiconductor film For example, wet etching is performed using a solution of phosphoric acid, acetic acid, and nitric acid. In this manner, unnecessary portions are removed to form the first oxide semiconductor layer 133 (see FIG. 8A). The etching here is not limited to wet etching, but may be dry etching. It's fine.

[0189] The etching gas used in dry etching is a gas containing chlorine (chlorine-based gas, e.g. For example, chlorine (Cl2), boron chloride (BCl3), silicon chloride (SiCl4), carbon tetrachloride (CC l4) etc.) are preferred.

[0190] In addition, gases containing fluorine (fluorine-based gases, such as carbon tetrafluoride (CF4) and sulfur fluoride (SF 6), nitrogen fluoride (NF3), trifluoromethane (CHF3), etc.), oxygen (O2), Gases with rare gases such as helium (He) and argon (Ar) added to these gases, etc. It can be used.

[0191] As a dry etching method, parallel plate type RIE (Reactive Ion Etch) ing method and ICP (Inductively Coupled Plasma) A combined plasma etching method can be used. It is possible to etch into the desired shape. The etching conditions (the amount of power applied to the coil-type electrode, the amount of power applied to the electrode on the substrate side) were set so that The amount of power used, the temperature of the electrode on the substrate, etc. are adjusted appropriately.

[0192] The etching solution used for wet etching is a mixture of phosphoric acid, acetic acid, and nitric acid. Alternatively, ITO07N (manufactured by Kanto Chemical Co., Ltd.) may be used.

[0193] In addition, the etching solution after wet etching is washed away together with the etched material. The waste etching solution containing the removed material is purified to remove the contained material. The indium, etc. contained in the oxide semiconductor layer may be reused from the waste liquid after the etching. By recovering and reusing materials, resources can be used more effectively and costs can be reduced. .

[0194] In order to etch the desired shape, the etching conditions (etching Adjust the etching conditions (liquid, etching time, temperature, etc.) as appropriate.

[0195] Next, the first oxide semiconductor layer 133 is subjected to a first heat treatment for dehydration or dehydrogenation. The first oxide semiconductor layer 133 is subjected to a first heat treatment in an oxygen atmosphere, and then The mixture is slowly cooled under nitrogen atmosphere.

[0196] The first heat treatment is, for example, a heat treatment at 650° C. for 1 hour in an oxygen atmosphere. The temperature T at which the semiconductor layer is dehydrated or dehydrogenated must be sufficiently low so that water does not enter again. The second oxide semiconductor is then cooled to a temperature, specifically, until the temperature is 100° C. lower than the heating temperature T. A conductor layer 134 is formed. Alternatively, the temperature is set to a temperature lower than that of the second heat treatment to be performed in a later step. The oxide semiconductor layer is heated in an oxygen atmosphere. By this treatment, impurities such as water contained in the oxide semiconductor layer can be removed, and at the same time, Then, the second oxide semiconductor layer 134 is made to have an oxygen excess state (see FIG. 8B). Depending on the heat treatment conditions or the material of the oxide semiconductor layer, the oxide semiconductor layer may be crystallized to become a microcrystalline film or a polycrystalline film. In some cases, a crystalline film may be formed.

[0197] Next, the light-transmitting conductive film 132 is formed over the second oxide semiconductor layer 134 by a sputtering method or a vacuum deposition method. Vapor deposition (electron beam vapor deposition, etc.), arc discharge ion plating, and spraying , or the inkjet method (see FIG. 8(C)).

[0198] The light-transmitting conductive film 132 is formed of a material that transmits visible light, for example For example, metal oxides of the In-Sn-Zn-O system, metal oxides of the In-Al-Zn-O system, and Sn- Ga-Zn-O metal oxides, Al-Ga-Zn-O metal oxides, Sn-Al-Z nO-based metal oxides, In-Zn-O-based metal oxides, Sn-Zn-O-based metal oxides , Al-Zn-O based metal oxides, In-O based metal oxides, Sn-O based metal oxides, Zn-O-based metal oxides can be used, and the film thickness ranges from 30 nm to 200 nm. Select appropriately within the range.

[0199] In this embodiment, before the formation of the light-transmitting conductive film 132, the conductive film 132 is dehydrated or dehydrogenated. However, the present invention is not limited to the above-mentioned example, and the first heat treatment may be performed on the conductive film 132 having a light-transmitting property. After the light-transmitting conductive film 132 is formed, a first heat treatment may be performed. By performing heat treatment, the oxide semiconductor layer is dehydrated or dehydrogenated, and at the same time, a light-transmitting This may also serve as heat treatment for improving the crystallinity of the conductive film 132 and reducing its resistance.

[0200] Next, a third photolithography process is performed to form a resist mask and to form a The unnecessary portions are removed to form the source electrode layer 105a, the drain electrode layer 105b, and the capacitance electrode 13. 5 and the second terminal 122 are formed. In this etching process, the oxide semiconductor layer is exposed. The exposed region is also partially etched, resulting in the oxide semiconductor layer 103 having a recess. A region of the oxide semiconductor layer 103 that does not overlap with the electrode layer 105a and the drain electrode layer 105b is In FIG. 8D, the source electrode layer 105a and the drain electrode layer 105b are 105b and the oxide semiconductor layer are etched at the same time by dry etching. , the source electrode layer 105a, the drain electrode layer 105b, and the end portion (gate The ends of the first and second electrodes 101 (located above the first and second electrodes 102) coincide with each other to form a continuous structure.

[0201] In the third photolithography process, the source electrode layer 105a or the drain electrode layer 105b is The second terminal 122 made of the same material as the electrode layer 105b is left in the terminal portion. 22 is electrically connected to the source wiring (the source wiring including the source electrode layer 105a). .

[0202] In the third photolithography process, the source electrode layer 105a or the drain electrode layer 105b is The capacitance electrode 135, which is made of the same material as the electrode layer 105b, is formed by using the gate insulating layer 102 as a dielectric. , and forms a storage capacitor together with the capacitor wiring 108.

[0203] Also, a resist having regions of multiple thicknesses (typically two types) formed by a multi-tone mask is used. By using a photomask, the number of resist masks can be reduced, which simplifies the process and reduces Cost reduction is possible.

[0204] Next, the resist mask is removed. When removing the resist mask, oxygen ashing is performed. Then, oxygen is introduced into an exposed region of the oxide semiconductor layer 103. A first protective insulating layer 107 is formed to be a protective insulating layer in contact with a part of the conductor layer 103. The protective insulating layer 107 is typically a silicon oxide film, a silicon oxynitride film, an aluminum oxide film, or Alternatively, an aluminum oxynitride film or the like is used. Of course, the first protective insulating layer 107 has a light-transmitting property. It is an insulating film having the above structure.

[0205] Next, after the first protective insulating layer 107 is formed, heat treatment may be performed. The heating may be performed in a hydrogen atmosphere or a nitrogen atmosphere at a temperature of 150° C. or higher and lower than 350° C. When the heat treatment is performed, the oxide semiconductor layer 103 is heated in a state in contact with the first protective insulating layer 107. This increases the resistance of the oxide semiconductor layer 103, thereby improving the electrical characteristics of the transistor. This heat treatment (preferably The temperature is not particularly limited to 150° C. or higher and lower than 350° C. after the formation of the first protective insulating layer 107. The heat treatment during the resin film formation and the low resistance of the light-transmitting conductive film are not performed. By combining this with the heat treatment for increasing the temperature, the number of steps can be reduced.

[0206] Through the above steps, the thin film transistor 170 can be fabricated.

[0207] Next, the second protective insulating layer 131 is formed (see FIG. 9(A)). 31 is water, hydrogen ions, OH - It does not contain impurities such as The inorganic insulating film used is a silicon nitride film, an aluminum nitride film, a silicon oxide nitride film, and a silicon nitride film. Of course, the second protective insulating layer 131 is made of a material having a light-transmitting property. It is an insulating film having the above structure.

[0208] The second protective insulating layer 131 is a gate insulating layer provided below the second protective insulating layer 131. It is preferable that the insulating film 102 is in contact with the insulating film 102 or the insulating film serving as the base. Molecular weight, hydrogen ions, and OH - In particular, the second The gate insulating layer 102 in contact with the protective insulating layer 131 or the insulating film serving as the base is a silicon nitride film. It is valid if

[0209] Next, a fourth photolithography process is performed to form a resist mask and a first protective insulating film is formed. The drain is formed by etching the layer 107, the second protective insulating layer 131, and the gate insulating layer 102. A contact hole 125 is formed that reaches the contact electrode layer 105b. The contact hole 127 reaches the second terminal 122 by the wiring, and the contact hole 128 reaches the first terminal 121 by the wiring. A contact hole 126 is also formed. The cross-sectional view at this stage is shown in FIG. The plan view at this stage corresponds to FIG. 10, and the cut is taken along the dashed lines A1-A2 and B1-B2 in FIG. The cross-sectional view corresponds to FIG. 9(B). Also, as shown in FIG. 10, A contact hole 124 reaching the capacitance electrode 135 is also formed.

[0210] Next, after removing the resist mask, a light-transmitting conductive film is formed. The conductive film material is indium oxide (In2O3) or an indium oxide tin oxide alloy. (In2O3-SnO2, abbreviated as ITO) is deposited by sputtering or vacuum deposition. As another material for the conductive film, a nitrogen-containing Al-Zn-O-based non-single crystal film, i.e. That is, Al-Zn-ON type non-single crystal film, Zn-ON type non-single crystal film containing nitrogen, and nitrogen It is also possible to use a Sn-Zn-ON type non-single crystal film containing Al-Zn-O- The composition ratio (atomic %) of zinc in the N-based oxide semiconductor film is set to 47 atomic % or less, and the oxide semiconductor film The composition ratio (atomic percent) of aluminum in the oxide semiconductor film is larger than that in the oxide semiconductor film. The composition ratio (atomic %) of nitrogen in the light-transmitting conductive film is larger than that in the light-transmitting conductive film. Etching of such materials is done with solutions based on hydrochloric acid. Since etching tends to leave residue, indium oxide and nitrogen oxide are used to improve etching processability. A lead alloy (In2O3-ZnO) may also be used. Also, a conductive film with light transmission can be made to have low resistance. In the case where heat treatment is performed to change the resistance of the oxide semiconductor layer 103, the resistance of the oxide semiconductor layer 103 is increased. This can also be used as a heat treatment to improve the electrical characteristics of the do.

[0211] Next, a fifth photolithography process is performed to form a resist mask and to form a The pixel electrode layer 110 is formed by removing unnecessary portions of the first through contact holes formed in the first protective insulating layer 107 and the second protective insulating layer 131. 3 and electrically connects to the capacitance electrode 135 .

[0212] In the fifth photolithography process, the first terminal 121 and the second terminal 1 22 is covered with a resist mask, and the light-transmitting conductive films 128 and 129 formed on the terminal portions are The light-transmitting conductive films 128 and 129 are electrodes or wiring used for connection with an FPC. The light-transmitting conductive film 128 formed on the first terminal 121 is a gate wiring The transparent electrode formed on the second terminal 122 serves as a terminal electrode for connection that functions as an input terminal for the The conductive film 129 having optical properties is a terminal electrode for connection that functions as an input terminal of a source wiring. be.

[0213] Next, the resist mask is removed, and the cross-sectional view at this stage is shown in FIG. The plan view at this stage corresponds to FIG. 11, and the cut is made along the dashed lines A1-A2 and B1-B2 in FIG. 9(C) is a cross-sectional view of the pixel electrode layer 110. A channel formation region and a gate electrode layer 101 of the thin film transistor 170 connected to Although an example of overlapping is shown, this is not particularly limited, and the channel forming region of the thin film transistor 170 may be The thin film transistor may be configured to overlap with the pixel electrode layer of an adjacent pixel that is not connected to the thin film transistor. A light-transmitting conductive film, which is a pixel electrode in this embodiment, is formed so as to overlap the channel forming region of the pixel electrode 170. By forming the pole layer 110, a bias voltage is applied to check the reliability of the thin film transistor. - In the thermal stress test (hereinafter referred to as BT test), the thin film transistor This can reduce the amount of change in the threshold voltage of the resistor 170.

[0214] 12(A) and 12(B) are a plan view and a cross-sectional view of the gate line terminal portion at this stage. 12A is a cross-sectional view taken along line E1-E2 in FIG. 12B. In FIG. 12(A), the first protective insulating layer 154 and the second protective insulating layer 1 The light-transmitting conductive film 155 formed on the substrate 57 is a connection terminal that functions as an input terminal. In FIG. 12(A), the terminal portion is made of the same material as the gate wiring. A first terminal 151 to be connected to the source line and a connection electrode layer 153 made of the same material as the source line are connected to the gate. The light-transmitting conductive film 155 overlaps the insulating film 152 and provides electrical continuity. In FIG. 9C, the light-transmitting conductive film 128 and the first terminal 121 are in contact with each other. The portion where the light-transmitting conductive film 155 and the first terminal 151 are in contact with each other in FIG. This corresponds to the part that is

[0215] 12(C) and 12(D) show a source line terminal portion different from that shown in FIG. 9(C). 12(C) shows a plan view and a cross-sectional view of the source wiring terminal portion. This corresponds to a cross-sectional view taken along line F1-F2 in FIG. A light-transmitting conductive film 1 formed on the first protective insulating layer 154 and the second protective insulating layer 157 55 is a terminal electrode for connection that functions as an input terminal. In the terminal portion, an electrode layer 156 made of the same material as the gate wiring is electrically connected to the source wiring. The electrode layer 15 overlaps a second terminal 150 connected to the gate insulating layer 152. 6 is not electrically connected to the second terminal 150, and the electrode layer 156 is connected to the second terminal 150. By setting different potentials, such as floating, GND, or 0V, you can reduce noise. A capacitance for preventing electrostatic discharge or a capacitance for preventing static electricity can be formed. A conductive film having a light-transmitting property is formed through the first protective insulating layer 154 and the second protective insulating layer 157. 155 and is electrically connected.

[0216] A plurality of gate lines, source lines, and capacitance lines are provided according to the pixel density. In addition, in the terminal section, a first terminal has the same potential as the gate wiring, a second terminal has the same potential as the source wiring, The terminal 2 and the third terminal of the same potential as the capacitance wiring are arranged in a row. The number of terminals may be any number and may be determined appropriately by the implementer.

[0217] In this way, five photolithography steps were performed using five photomasks to produce the bottom A pixel thin-film transistor having a thin-film transistor 170 which is a gate type thin-film transistor. Then, these are connected to the matrix corresponding to each pixel. By arranging the pixels in a rectangular shape, an active matrix display device can be created. For the sake of convenience, in this specification, such a substrate is referred to as an actuator. This is called an active matrix substrate.

[0218] When manufacturing an active matrix type liquid crystal display device, an active matrix substrate A liquid crystal layer is provided between the active matrix substrate and a counter substrate having a counter electrode. The counter electrode is fixed to the counter substrate. A fourth terminal electrically connected to the common electrode is provided on the active matrix substrate. This fourth terminal is used to set the common electrode to a fixed potential, such as GND or 0V. This is a terminal for

[0219] The configuration of the storage capacitor is not limited to that shown in the present embodiment. For example, a capacitor line may be provided. First, the pixel electrode layer is overlapped with the gate wiring of the adjacent pixel via the protective insulating layer and the gate insulating layer. A storage capacitor may be formed by using the same.

[0220] In addition, the method of providing a liquid crystal layer between the active matrix substrate and the opposing substrate and sealing it is There are two methods: the drip method and the liquid crystal injection method. A liquid crystal layer is placed between the active matrix substrate and the opposing substrate. An example of a liquid crystal display panel with an FPC 1924 attached is shown in FIG. In the display panel 1908, a first substrate 1920 on which a pixel electrode layer is provided and a first The substrate 1920 and the opposing second substrate 1923 are bonded together with a sealant 1922. The sealant 1922 is formed to surround the display portion 1921, and the first substrate 1920 A liquid crystal layer is provided in the area surrounded by the first substrate 1923 and the sealant 1922. The liquid crystal sealing method for the display panel 1908 shown in FIG. 3(A) uses a liquid crystal dropping method, and the substrate is placed under reduced pressure. The gap between the pair of substrates is made by using a spacer, specifically a spherical spacer or a pillar. The gap is held in place by a spacer or a filler contained in the sealing material. The LCD mode (TN mode, VA mode, IPS mode) that drives the display panel 1908 However, in the IPS mode, electrodes are provided on the second substrate. In other liquid crystal modes, a counter electrode is often provided on the second substrate. In this case, when the pair of substrates are attached, the opposing electrodes and the terminal electrodes provided on the first substrate are Connections are also made to ensure continuity.

[0221] FIG. 13(B) shows the structure of a panel manufactured using a liquid crystal sealing method different from that in FIG. 13(A). In FIG. 13(B), the same reference numerals are used for the parts common to FIG. 13(A). The display panel shown in FIG. 13B is a liquid crystal injection panel formed with a first sealant 1925. After injecting liquid crystal from the opening by using a liquid crystal injection method, the liquid crystal injection opening is covered with a second seal material 1926. It is sealed with.

[0222] FIG. 13(C) shows an example of a panel configuration different from that of FIG. 13(A). ), the same reference numerals are used for the parts common to FIG. 13(A). The panel in FIG. 13(C) is A driver IC 1927 for driving the display unit is mounted on the first substrate 1920 . The driving IC 1927 is mounted on the first substrate 1920 to achieve circuit integration.

[0223] If necessary, the display panels shown in Figs. 13(A), 13(B), and 13(C) may be Desired optical films, such as polarizers, anti-reflection films, color filters, etc., are appropriately installed. can.

[0224] Regarding the configuration of a block diagram of an active matrix type liquid crystal display device corresponding to FIG. 13(C), FIG. 14A shows a display portion 1301 and a display device 1302 provided on a substrate 1300. The configuration of the driving unit 1302 connected from outside the substrate 1300 is shown. 1302 includes a signal line driver circuit 1303, a scanning line driver circuit 1304, etc. The display unit 1301 has a plurality of pixels 1305 arranged in a matrix.

[0225] In FIG. 14A, a scanning line driver circuit 1304 is connected to an external connection terminal 1309. The signal line driver circuit 1303 supplies a scanning signal to the scanning line 1306. 09 to the signal line 1308. The scanning signal from the scanning line 1306 Thus, the scanning signal is sent so that the pixels 1305 are selected in sequence from the first row of the scanning line 1306. Supply the number.

[0226] In this embodiment, the driving unit 1302 is formed outside the substrate 1300. The moving part 1302 is bonded by the TAB (Tape Automated Bonding) method. It can be mounted on a flexible printed circuit (FPC). Alternatively, the driving unit 1302 may be implemented by a COG (Chip on Glass) method. It is possible to mount it on the substrate 1300 using this.

[0227] In this embodiment, the driving unit 1302 is formed outside the substrate 1300. The driving unit 1302 is formed of a transistor using a single crystal semiconductor. 302 is a device that improves the drive frequency, reduces power consumption by reducing the drive voltage, and reduces the variation of the output signal. In addition, the scanning line driver circuit 1304 and the signal line driver circuit 1303 are A signal, a voltage, a current, or the like is input to these via an external connection terminal 1309 .

[0228] In FIG. 14A, the scanning line driver circuit 1304 includes G1 to G n n scan lines The signal line driver circuit 1303 is connected to a RGB (RGB) When considering a configuration of three pixels (red, green, and blue), the signal line corresponding to R is S R1 ~S Rm m lines and the signal line S corresponding to G G1 or signal line S Gm m and B Corresponding S B1 ~S Bm In other words, a total of 3m signal lines are connected. As shown in FIG. 13B, a pixel 1305 has a signal line for each color element, and each color element is connected to a corresponding pixel. By supplying data to the pixel elements via signal lines, it becomes possible to reproduce the desired color.

[0229] The timing chart shown in FIG. 15 includes a frame period and a row selection period (a period during which the image of the display device is displayed). The scanning line 1306 (representatively, G1, G2, G3) is scanned in a period corresponding to the scanning time for one row. n ) A scanning signal for scanning the image, and a signal line 1308 (representatively, S R1 ) data signal, It shows.

[0230] In the block diagram shown in FIG. 14, the transistors provided in each pixel are thin-film transistors. The transistor 170 is an n-channel transistor. Regarding the driving of pixels when controlling the on / off of n-channel transistors, This is an explanation of the above.

[0231] In the timing chart of FIG. 15, one frame corresponds to a period for displaying one screen's worth of image. The frame period should be at least 1 / 120 so that viewers do not experience any residual image when viewing moving images. seconds (≒8.3 ms) (preferably 1 / 240 seconds), and the number of scanning lines is n. Therefore, the row selection period is 1 / (120×n) seconds. The number is 2000 (4096 x 2160 pixels, 3840 x 2160 pixels, etc., so-called 4k2 Considering a display device with a 1000-pixel image (assuming 1000-pixel images), the delay of the signal due to wiring is not taken into consideration. In this case, the row selection period corresponds to 1 / 240000 seconds (≈4.2 μs).

[0232] In this way, even if the number of scanning lines is increased, for example to 2000, the number of lines arranged in each pixel is Since the thin film transistor 170 has a light-transmitting property, a high aperture ratio can be realized. do.

[0233] In an active matrix type liquid crystal display device (e.g., TN type), By driving the arranged pixel electrode layers, a display pattern is formed on the screen. Alternatively, a voltage is applied between a selected pixel electrode layer and a counter electrode corresponding to the pixel electrode layer. This causes optical modulation of the liquid crystal layer disposed between the pixel electrode layer and the counter electrode, This optical modulation is perceived by the observer as a display pattern.

[0234] In a TN type liquid crystal display device, the liquid crystal is twisted 90 degrees between a pair of substrates, and the polarizing element The absorption axis direction of the element is arranged to be almost parallel to or almost perpendicular to the rubbing direction. In TN type liquid crystal display devices, when no voltage is applied to the pixel electrode layer, light from a backlight or the like is emitted. The incident light from the light source is linearly polarized by the polarizing element on the light source side, and this linear polarization is oriented along the twist of the liquid crystal layer. If the transmission axis of the other polarizing element is aligned with the azimuth of the linearly polarized light, the light propagates in a linear manner. All linearly polarized light is emitted, resulting in a white display (normally white display).

[0235] In addition, in the case of a full-color liquid crystal display device, a color filter is provided and the pixel electrode layer is When no voltage is applied to the pixel electrode layer, the color display is achieved. The incident light is linearly polarized by the polarizing element on the light source side, and the average alignment of the liquid crystal molecular axes in the liquid crystal layer The direction of the unit vector is almost perpendicular to the substrate surface, so the light source side The azimuth angle of linearly polarized light propagates unchanged and coincides with the absorption axis of the other polarizing element, resulting in a black display. It becomes.

[0236] Although an example of a TN type liquid crystal display device has been shown in this embodiment, the present invention is not limited thereto, and various The present invention can be applied to various modes of liquid crystal display devices. For example, the method of improving the viewing angle characteristics In this method, an electric field is applied to the liquid crystal layer in a direction parallel to the main surface of the substrate (also known as IPS). In addition, nematic liquid crystals with negative dielectric anisotropy can be used as liquid crystal materials. This method can be applied to a method using a vertical alignment film as the alignment film. The method of using a vertical alignment film is one of the voltage controlled birefringence (ECB) methods. The birefringence of the crystal molecules is utilized to control the transmittance.

[0237] In addition, as a method for improving the response speed, ferroelectric liquid crystals and antiferroelectric liquid crystals are used to display moving images. The response speed of the liquid crystal layer may be improved so as to meet the display requirements.

[0238] Alternatively, a liquid crystal that exhibits a blue phase without using an alignment film may be used. The blue phase is one of the liquid crystal phases. When the temperature of cholesteric liquid crystal is increased, the phase immediately transitions from the cholesteric phase to the isotropic phase. The blue phase appears only in a narrow temperature range, so it is necessary to improve the temperature range. In order to achieve this, a liquid crystal composition containing 5% by weight or more of a chiral agent is used in the liquid crystal layer. The liquid crystal composition containing the liquid crystal exhibiting the blue phase and the chiral agent has a short response speed of 1 msec or less. Since it is optically isotropic, no alignment treatment is required, and the viewing angle dependency is small.

[0239] In addition, OCB (Optical Compensate Birefringence) The OCB mode can also be applied to transmissive LCD devices that use a pair of The response speed of the liquid crystal layer between the substrates is improved by setting the liquid crystal layer in a state called bend alignment. The pretilt angle of the first alignment film in contact with the liquid crystal layer and the pretilt angle of the second alignment film in contact with the liquid crystal layer are The pretilt angle of the film is reversed to form a bend alignment. It is necessary to transition the liquid crystal from its initial splay alignment to a state called bend alignment.

[0240] It can also be applied to a transmissive liquid crystal display device that employs a vertical alignment mode. In a transmissive liquid crystal display device that uses the mode, one pixel is divided into multiple sub-pixels, and each By providing a convex portion on the opposing substrate located at the center of each pixel, one pixel can be divided into multiple domains (multi-domain). This driving method may be a sub-pixel domain driving method to achieve a wide viewing angle. This is called wheel drive.

[0241] To achieve a wide viewing angle, sub-pixel driving is used, dividing one pixel into multiple sub-pixels. However, since the thin film transistor 170 arranged in each pixel has light transmission properties, a high aperture ratio can be achieved. It is possible to achieve this.

[0242] In addition, when displaying moving images on a liquid crystal display device, the response of the liquid crystal molecules themselves is slow, resulting in image retention. In order to improve the moving image characteristics of a liquid crystal display device, In one embodiment, a driving technique known as black insertion is used, in which a full black display is performed every other frame.

[0243] In addition, the vertical synchronous frequency is increased by 1.5 or 2 times to improve the video characteristics. There is also a driving technology called double speed driving.

[0244] In addition, in order to improve the video characteristics of liquid crystal display devices, multiple LEDs (light emitting diodes) are used as backlights. A surface light source is formed by using a diode) light source or multiple EL light sources, etc., and a surface light source is formed. There is also a driving technology that drives each light source to light intermittently within one frame period. In addition, three or more types of LEDs may be used, or white-emitting LEDs may be used. Since multiple LEDs can be controlled, the LE can be switched according to the timing of the optical modulation of the liquid crystal layer. The timing of the LEDs can also be synchronized. This is particularly useful when displaying images with a large proportion of black areas occupying the entire screen. This has the effect of reducing power consumption.

[0245] By combining these driving technologies, the display characteristics such as the video characteristics of the LCD device can be improved. can be improved compared to the conventional method.

[0246] The n-channel transistor disclosed in this specification has an oxide semiconductor film as a channel formation region. These drive technologies can be combined due to their good dynamic characteristics. do.

[0247] By forming the thin film transistor using an oxide semiconductor, the manufacturing cost can be reduced. In particular, the heat treatment for dehydration or dehydrogenation removes the moisture, which is an impurity, In order to reduce these and increase the purity of the oxide semiconductor film, the dew point in the film formation chamber has been lowered. Even without using a special sputtering device or an ultra-high purity oxide semiconductor target, good electrical characteristics can be obtained. Thus, a semiconductor device having a thin film transistor with good properties and high reliability can be manufactured.

[0248] The oxide semiconductor layer in the channel formation region is a high resistance region, so that the electrical resistance of the thin film transistor is The electrical characteristics are stabilized and the increase in the off-current can be prevented. It is possible to obtain a semiconductor device having a good and reliable thin film transistor.

[0249] This embodiment mode can be implemented in appropriate combination with the configurations described in other embodiments. It is.

[0250] (Embodiment 7) An example of a light-emitting display device is shown as a semiconductor device. is shown using a light-emitting element that uses electroluminescence. The light-emitting element that uses the light-emitting material is classified into two types according to whether the light-emitting material is an organic compound or an inorganic compound. Generally, the former is called an organic EL element and the latter an inorganic EL element.

[0251] In an organic EL element, electrons and holes are released from a pair of electrodes by applying a voltage to the light-emitting element. are injected into layers containing light-emitting organic compounds, causing a current to flow. The rears (electrons and holes) recombine to form an excited state in the light-emitting organic compound. When the excited state returns to the ground state, light is emitted. Such a light-emitting element is called a current-excitation type light-emitting element.

[0252] Inorganic EL elements are divided into dispersion-type inorganic EL elements and thin-film-type inorganic EL elements according to their element structure. Dispersion-type inorganic EL elements have a light-emitting layer in which particles of a light-emitting material are dispersed in a binder. The emission mechanism is a donor-acceptor reaction that utilizes the donor and acceptor levels. Thin-film inorganic EL elements are made by sandwiching a light-emitting layer between dielectric layers. The structure is sandwiched between electrodes, and the light emission mechanism utilizes the inner shell electron transition of metal ions. In this example, the light-emitting element is an organic EL element. do.

[0253] FIG. 16 shows an example of a pixel configuration to which digital time gray scale driving can be applied as an example of a semiconductor device. This is a diagram.

[0254] The configuration of a pixel to which digital time gray scale driving can be applied and the operation of the pixel will be described. The figure shows an n-channel transistor that uses an oxide semiconductor layer as a channel formation region in one pixel. Here is an example of using two of them.

[0255] The pixel 6400 includes a switching transistor 6401, a driving transistor 6402, The switching transistor 64 has a light emitting element 6404 and a capacitor element 6403. 01 has a gate connected to a scanning line 6406 and a first electrode (one of the source and drain electrodes) The first electrode (the other of the source electrode and the drain electrode) is connected to a signal line 6405, and the second electrode (the other of the source electrode and the drain electrode) is connected to a drive The driving transistor 6402 is connected to the gate of the driving transistor 6402. The gate is connected to a power supply line 6407 via a capacitor element 6403, and the first electrode is connected to a power supply line 640 7, and the second electrode is connected to the first electrode (pixel electrode layer) of the light-emitting element 6404. The second electrode of the light emitting element 6404 corresponds to a common electrode 6408. It is electrically connected to a common potential line formed on one substrate.

[0256] A low power supply potential is set to the second electrode (common electrode 6408) of the light emitting element 6404. Note that the low power supply potential is a low power supply potential with respect to the high power supply potential set to the power supply line 6407. Potential < High power supply potential. For example, GND, 0V, etc. are set as low power supply potential. The potential difference between the high power supply potential and the low power supply potential is applied to the light emitting element 6404. In order to make the light emitting element 6404 emit light by passing a current through the light emitting element 6404, a high power supply potential and the low power supply potential is set to be equal to or higher than the forward threshold voltage of the light emitting element 6404. Each potential is set.

[0257] The capacitor 6403 is omitted by substituting the gate capacitance of the driving transistor 6402. It is also possible to set the gate capacitance of the driving transistor 6402 as A capacitance may be formed between the region and the gate electrode.

[0258] In the case of a voltage input voltage driving method, the gate of the driving transistor 6402 is The driving transistor 6402 is in two states, either fully on or fully off. A video signal is inputted, that is, the driving transistor 6402 is operated in a linear region. In order to operate the driving transistor 6402 in a linear region, the voltage of the power supply line 6407 must be higher than that of the driving transistor 6402. A high voltage is applied to the gate of the driving transistor 6402. A voltage equal to or higher than (power supply line voltage + Vth of the driving transistor 6402) is applied.

[0259] In addition, when analog gray scale driving is performed instead of digital time gray scale driving, the input of the signal is different. By doing so, the same pixel configuration as in FIG. 16 can be used.

[0260] In the case of performing analog gradation driving, a light emitting element 6404 is connected to the gate of a driving transistor 6402. A voltage equal to or higher than the forward voltage of the light emitting element 6401 and the Vth of the driving transistor 6402 is applied. The forward voltage in 04 refers to the voltage required to achieve the desired brightness, and should be at least 100% forward voltage. In addition, the video transistor 6402 is designed to operate in the saturation region. By inputting an optical signal, a current can be passed through the light emitting element 6404. In order to operate the transistor 6402 in the saturation region, the potential of the power supply line 6407 is The gate potential of the light emitting element 6402 is set higher than that of the gate of the transistor 6403. Analog gradation drive can be performed by passing a current corresponding to a video signal through 6404.

[0261] Note that the pixel configuration shown in FIG. 16 is not limited to this. For example, A switch, a resistive element, a capacitive element, a transistor, a logic circuit, or the like may be added.

[0262] Next, the configuration of the light emitting element will be described with reference to FIG. 17. Here, the driving TFT is The cross-sectional structure of a pixel will be described using the example of the type shown in Figure 17(A), (B), and (C). The driving TFTs 7001, 7011, and 7021 used in the semiconductor device are the same as those in the first embodiment. The thin-film transistor shown in Fig. 1 can be fabricated in the same manner as the thin-film transistor shown in Fig. 1. In addition, the thin film transistor shown in the second embodiment or the third embodiment is used as a driving transistor. Can also be applied as FT7001, 7011, 7021.

[0263] The light emitting element only needs to have at least one of the anode and cathode transparent in order to extract light. Then, a thin film transistor and a light emitting element are formed on the substrate, and light is taken from the surface opposite to the substrate. Top emission, bottom emission, and side emission. There are light-emitting elements with a double-sided emission structure that emits light from the side of the pixel. The present invention can also be applied to optical elements.

[0264] A light emitting element having a top emission structure will be described with reference to FIG.

[0265] In FIG. 17A, a driving TFT 7001 is an n-type TFT, and light emitted from a light-emitting element 7002 is FIG. 17A shows a cross-sectional view of a pixel when the light emitting element 70 The cathode 7003 of the TFT 7002 is electrically connected to the driving TFT 7001. A light-emitting layer 7004 and an anode 7005 are laminated on the TFT 7001 in this order. It is covered with a protective insulating layer 7006 made of a silicon nitride film or an aluminum nitride film, and further covered with a planarizing insulating layer 7006. The cathode 7003 is covered with a conductive film 7007 that has a small work function and reflects light. Various materials can be used for the conductive film. For example, Ca, Al, MgAg, AlL The light-emitting layer 7004 may be composed of a single layer or a plurality of layers. If it is made up of multiple layers, the cathode 7003, an electron injection layer, an electron transport layer, a light-emitting layer, a hole transport layer, and a hole injection layer are laminated in this order. It is not necessary to provide all of these layers. The anode 7005 has a light-transmitting property. The conductive material is formed using a conductive material such as tungsten oxide, indium oxide, Indium zinc oxide containing tungsten, indium oxide containing titanium oxide, titanium oxide Indium tin oxide (ITO) containing tin, in ... A light-transmitting conductive film such as indium zinc oxide or indium tin oxide with silicon oxide added may also be used.

[0266] Moreover, the cathode 7003 is insulated from the cathode 7008 of the adjacent pixel by a partition wall 7009 . In addition, the cathode 7008 of the adjacent pixels is insulated from the oxide semiconductor layer of the driving TFT 7001 by the gate insulating layer. The layer overlaps the edge layer. By forming the cathode 7008 of the adjacent pixels so that In the bias-thermal stress test (hereinafter referred to as BT test) to check the reliability, The change in the threshold voltage of the driving TFT7001 before and after the T test can be reduced. do.

[0267] The region where the light-emitting layer 7004 is sandwiched between the cathode 7003 and the anode 7005 constitutes the light-emitting element 7002. In the case of the pixel shown in FIG. 17A, the light emitted from the light emitting element 7002 is The light is emitted toward the anode 7005 as indicated by the mark.

[0268] Next, a light emitting element having a bottom emission structure will be described with reference to FIG. When 011 is an n-type light emitting element and light emitted from the light emitting element 7012 is emitted to the cathode 7013 side, FIG. 17B shows a cross-sectional view of a pixel. A cathode 7013 of a light-emitting element 7012 is formed on a light-transmitting conductive film 7017. A light-emitting layer 7014 and an anode 7015 are laminated in this order on the cathode 7013. When the anode 15 has a light-transmitting property, a shielding layer for reflecting or blocking light is provided so as to cover the anode. The cathode 7013 may have a film 7016 formed thereon, as in the case of FIG. Various conductive materials with small thermal coefficients can be used. However, the thickness of the material should be The thickness is set to a level that allows light to pass through (preferably, about 5 nm to 30 nm). For example, a 20 nm film An aluminum film having a thickness of 700 nm can be used as the cathode 7013. 17(A), even if it is composed of a single layer, multiple layers are laminated. The anode 7015 does not need to transmit light, but as shown in FIG. As in the case of 17(A), the insulating film 17 can be formed using a conductive material having light-transmitting properties. The shielding film 7016 may be made of, for example, a metal that reflects light, but is not limited to a metal film. For example, a resin containing a black pigment may be used.

[0269] Moreover, the cathode 7013 is insulated from the cathode 7018 of the adjacent pixel by a partition wall 7019 . In addition, the cathode 7018 of the adjacent pixel is insulated from the oxide semiconductor layer of the driving TFT 7011 by the gate insulating layer. The layer overlaps the edge layer. By forming the cathode 7018 of the adjacent pixels so that In the bias-thermal stress test (hereinafter referred to as BT test) to check the reliability, The change in the threshold voltage of the driving TFT7011 before and after the T test can be reduced. do.

[0270] The region where the light-emitting layer 7014 is sandwiched between the cathode 7013 and the anode 7015 is the light-emitting element 7012. In the case of the pixel shown in FIG. 17B, the light emitted from the light-emitting element 7012 corresponds to The light is emitted toward the cathode 7013 as shown by the arrow.

[0271] In addition, since the driving TFT 7011 has a light-transmitting property, the light emitting element 7012 of the pixel adjacent thereto The light emitted from the light emitting element passes through the driving TFT 7011 and reaches the cathode 7012 as shown by the arrow. Eject towards 013.

[0272] Next, a light emitting element having a dual emission structure will be described with reference to FIG. In this example, a conductive film 7027 having a light-transmitting property and electrically connected to the driving TFT 7021 is formed on the substrate 7022. A cathode 7023 of the light-emitting element 7022 is formed, and a light-emitting layer 7024 is formed on the cathode 7023. The anode 7025 is laminated in order. The cathode 7023 is, as in the case of FIG. Various conductive materials with small thermal coefficients can be used. However, the thickness of the material should be For example, the cathode 7023 is made of Al having a thickness of 20 nm. The light-emitting layer 7024 can be formed of a single layer, as in FIG. The anode 70 may be configured as a single layer or as a laminate of multiple layers. 25 can be formed using a light-transmitting conductive material, as in FIG. 17(A). do.

[0273] Moreover, the cathode 7023 is insulated from the cathode 7028 of the adjacent pixel by a partition wall 7029 . In addition, the cathode 7028 of the adjacent pixel is insulated from the oxide semiconductor layer of the driving TFT 7021 by the gate insulating layer. The layer overlaps the edge layer. By forming the cathode 7028 of the adjacent pixels so that In the bias-thermal stress test (hereinafter referred to as BT test) to check the reliability, The change in the threshold voltage of the driving TFT7021 before and after the T test can be reduced. do.

[0274] The overlapping portion of the cathode 7023, the light-emitting layer 7024, and the anode 7025 constitutes the light-emitting element 70. In the case of the pixel shown in FIG. 17C, the light emitted from the light emitting element 7022 is is emitted toward both the anode 7025 side and the cathode 7023 side as indicated by the arrows.

[0275] In addition, since the driving TFT 7021 has a light-transmitting property, the light emitting element 7022 of the pixel adjacent thereto The light emitted from the light emitting element passes through the driving TFT 7021 and reaches the cathode 7022 as shown by the arrow. Eject towards 023.

[0276] In this embodiment, the pixel electrode layer is a cathode, and the TFT channel of the adjacent pixel is formed. However, the present invention is not limited to the above and may be applied to the channel of the TFT to which the cathode is electrically connected. It may be configured so as to overlap with the panel forming region.

[0277] Although the organic EL element has been described as the light-emitting element here, inorganic EL elements can also be used as the light-emitting element. It is also possible to provide an L element.

[0278] In addition, the thin film transistor (driving TFT) that controls the driving of the light-emitting element and the light-emitting element are electrically However, a current control TFT is connected between the driving TFT and the light emitting element. The configuration may be such that the input / output terminals are connected to each other.

[0279] The semiconductor device is not limited to the configuration shown in FIG. 17, and may be any of the configurations disclosed in this specification. Various modifications based on the technical concept are possible.

[0280] Through the above steps, a highly reliable light-emitting display device (display panel) can be manufactured as a semiconductor device. It is possible.

[0281] This embodiment mode can be implemented in appropriate combination with the configurations described in other embodiments. It is.

[0282] (Embodiment 8) A semiconductor device including a thin film transistor manufactured by the process shown in any one of Embodiments 1 to 7. The semiconductor device can be applied to various electronic devices (including gaming machines). Examples of such devices include television sets (also called televisions or television receivers), computers, and Computer monitors, digital cameras, digital video cameras, and other cameras, digital photo frames, mobile phones (also called mobile phones or mobile phone devices), portable game machines , portable information terminals, audio playback devices, large game machines such as pachinko machines, etc.

[0283] FIG. 18A shows an example of a mobile phone 1000. The mobile phone 1000 has a housing. In addition to the display unit 1002 incorporated in the 1001, the operation buttons 1003 and the external connection port 10 04, speaker 1005, microphone 1006, etc.

[0284] The mobile phone 1000 shown in FIG. 18A displays information by touching a display unit 1002 with a finger or the like. In addition, operations such as making a phone call or sending an e-mail can be performed without using the display. This can be done by touching the display unit 1002 with a finger or the like.

[0285] The screen of the display unit 1002 has three main modes. The first is a display mode that is mainly used for displaying images. The first mode is a display mode, the second is an input mode for inputting information such as characters, and the third mode is a display mode. This is a display + input mode that combines the display mode and the input mode.

[0286] For example, when making a call or composing an e-mail, the display unit 1002 is used for inputting characters. The main character input mode is to input characters displayed on the screen. It is preferable to display a keyboard or number buttons on most of the screen of the display unit 1002. I wish.

[0287] In addition, the mobile phone 1000 may include a sensor for detecting tilt, such as a gyro or an acceleration sensor. By providing a detection device having the above configuration, the orientation of the mobile phone 1000 (portrait or landscape) can be determined and the display The screen display of the display unit 1002 can be automatically switched.

[0288] The screen mode can be changed by touching the display unit 1002 or by operating the housing 1001. This is done by operating the button 1003. Also, depending on the type of image displayed on the display unit 1002, For example, the image signal to be displayed on the display unit is a moving image. If it is data, the mode is switched to display mode, and if it is text data, the mode is switched to input mode.

[0289] In the input mode, the optical sensor of the display unit 1002 detects a signal and displays If there is no input by touch operation of the part 1002 for a certain period of time, the screen mode is changed to the input mode. Alternatively, the display mode may be switched from the normal mode to the display mode.

[0290] The display unit 1002 can also function as an image sensor. Identity authentication can be performed by touching the palm or fingers to 02 and capturing an image of the palm print, fingerprint, etc. In addition, a backlight that emits near-infrared light for the display unit or a sensing device that emits near-infrared light for the display unit By using a light source, it is also possible to image finger veins, palm veins, etc.

[0291] A plurality of thin film transistors shown in Embodiment 1 are provided in the display portion 1002. Since the transistors and wirings are transparent, when a light sensor is provided in the display portion 1002, This is effective because the thin-film transistors and wiring do not block the incident light. When using a backlight that emits light or a sensing light source that emits near-infrared light, This is preferable because the thin film transistors and wiring are not shaded by light even if the thin film transistors and wiring are not shaded by light.

[0292] FIG. 18(B) is also an example of a mobile phone. The portable information terminal shown in FIG. 18(B) is It can have multiple functions. For example, in addition to the telephone function, it can have a built-in computer and perform various functions. It can also be equipped with various data processing functions.

[0293] The portable information terminal shown in FIG. 18B has two housings, a housing 1800 and a housing 1801. The housing 1800 includes a display panel 1802, a speaker 1803, a microphone, and the like. 1804, pointing device 1806, camera lens 1807, external connection The housing 1801 is equipped with a keyboard 1810, an external memory slot, etc. The housing 1801 includes a housing 1801 and a switch 1811. The housing 1801 includes an antenna.

[0294] The display panel 1802 is equipped with a touch panel, and in FIG. A plurality of operation keys 1805 are indicated by dotted lines.

[0295] In addition to the above configuration, a non-contact IC chip, a small recording device, etc. may be built in. .

[0296] The display device can be used in a display panel 1802, and the display direction can be changed depending on the usage mode. Also, a camera lens 1807 is provided on the same surface as the display panel 1802. The speaker 1803 and microphone 1804 are Not only voice calls, but also video calls, recording, playback, etc. are possible. The housing 1801 slides and is folded from the unfolded state shown in FIG. 18(B) to the folded state. The device can be made compact and portable.

[0297] The external connection terminal 1808 can be connected to various cables such as AC adapters and USB cables. It is possible to charge the battery and to communicate data with a personal computer, etc. By inserting a recording medium into the memory slot 1811, it is possible to store and transfer a larger amount of data. do.

[0298] In addition to the above functions, it also has infrared communication function, TV reception function, etc. Good too.

[0299] FIG. 19A shows an example of a television device 9600. The display unit 9603 is incorporated in the housing 9601. In addition, the stand 9605 supports the housing 9601. This shows a configuration in which the above is supported.

[0300] The television device 9600 can be operated using an operation switch on the housing 9601 or a separate remote control. This can be done by the remote control operation device 9610. The channel and volume can be controlled by the 9609, and the display 9603 shows In addition, the remote control unit 9610 can control the video. A display portion 9607 for displaying information output from 9610 may be provided.

[0301] The television device 9600 includes a receiver and a modem. It can receive more general television broadcasts, and can also be connected to a modem via wired or wireless connection. By connecting to a network, communication can be one-way (sender to receiver) or two-way. It is also possible to communicate information (between a sender and a receiver, or between receivers).

[0302] The display portion 9603 is provided with a plurality of light-transmitting thin film transistors described in Embodiment 1. In order to achieve this, the number of scanning lines is increased. For example, the number of scanning lines is increased to 2000 (4096 x 216 The resolution of the displayed image is assumed to be 3840 x 2160 pixels, 3840 x 2160 pixels, or other so-called 4k2k images. The aperture ratio can be increased even when increasing the resolution. When the size exceeds 10 inches, 60 inches, or even 120 inches, the translucency is required. Since the wiring resistance of the wiring may become a problem, a low-resistance gold It is preferable to provide a metal wiring as an auxiliary wiring.

[0303] FIG. 19B shows an example of a digital photo frame 9700. The photo frame 9700 includes a display unit 9703 built into a housing 9701. The unit 9703 is capable of displaying various images, for example images captured by a digital camera. By displaying the image data, it can function like a normal photo frame.

[0304] The Digital Photo Frame 9700 is equipped with an operation unit, external connection terminals (USB terminal, US A terminal that can be connected to various cables such as B cable, etc., and a recording medium insertion section, etc. These components may be installed on the same surface as the display unit, but they may be installed on the side or back. It is preferable to have a digital photo frame with a built-in memory card because it improves the design. A memory that stores image data taken with a digital camera is inserted into the body insertion section to store the image data. The captured image data can be displayed on the display portion 9703 .

[0305] The digital photo frame 9700 may also be configured to transmit and receive information wirelessly. It is also possible to wirelessly import and display desired image data.

[0306] FIG. 20 shows a portable gaming machine, which is composed of two cabinets, a cabinet 9881 and a cabinet 9891. The housing 9881 includes a display unit 988 and a connector 9893 for connecting the display unit 988 to the housing 9881 in an openable and closable manner. 2 is incorporated in the housing 9891, and a display unit 9883 is incorporated in the housing 9891. The portable gaming machine shown in the figure also includes a speaker unit 9884, a recording medium insertion unit 9886, LEDs, Lamp 9890, input means (operation keys 9885, connection terminal 9887, sensor 9888 (force , displacement, position, velocity, acceleration, angular velocity, rotation speed, distance, light, liquid, magnetism, temperature, chemicals, Sound, time, hardness, electric field, current, voltage, power, radiation, flow rate, humidity, gradient, vibration, odor It is equipped with a microphone 9889) and a function to measure infrared rays. Of course, the configuration of the portable gaming machine is not limited to the above, and may be at least as described in this specification. It is sufficient that the device is equipped with semiconductor devices, and other auxiliary equipment may be provided as appropriate. The portable game machine shown in FIG. 20 can be used to play a game using a program or data recorded on a recording medium. It also has the function of reading data and displaying it on the display unit, and of sharing information with other portable gaming machines via wireless communication. The functions of the portable gaming machine shown in FIG. 20 are not limited to these. , can have a variety of functions.

[0307] As described above, the light-transmitting thin film transistor can be used for the displays of various electronic devices. The light-transmitting thin film transistor can be disposed in the display unit or the display panel. By using it as a switching element for a panel, a signal processing device with a display section having a high aperture ratio can be realized. It is possible to provide highly reliable electronic equipment.

[0308] This embodiment mode can be implemented in appropriate combination with the configurations described in other embodiments. It is. [Explanation of symbols]

[0309] 100 Substrates 101 Gate electrode layer 102 Gate insulating layer 103 Oxide semiconductor layer 105a Source electrode layer 105b Drain electrode layer 107 First protective insulating layer 108 Capacitance wiring 110 Pixel electrode layer 121 Terminal 122 Terminal 124 Contact Hole 125 Contact Hole 126 Contact Hole 127 Contact Hole 128 Light-transmitting conductive film 129 Light-transmitting conductive film 131 Second protective insulating layer 132 Light-transmitting conductive film 133 First oxide semiconductor layer 134 Second oxide semiconductor layer 135 Capacitive electrode 150 Terminals 151 Terminal 152 Gate Insulation Layer 153 Connection electrode layer 154 First protective insulating layer 155 Light-transmitting conductive film 156 Electrode layer 157 Second protective insulating layer 170 Thin-film transistor 400 Substrates 401 Gate electrode layer 402 Gate insulating layer 403 Oxide semiconductor layer 405a Source electrode layer 405b Drain electrode layer 407 Oxide insulating film 430 First oxide semiconductor layer 431 Second oxide semiconductor layer 440 Thin Film Transistor 442 Second oxide semiconductor layer 443 Oxide Semiconductor Layer 444 Second oxide semiconductor layer 450 Substrate 451 Gate electrode layer 452 Gate insulation layer 453 Oxide Semiconductor Layer 455a Source electrode layer 455b Drain electrode layer 457 Oxide insulating film 460 Thin Film Transistor 470 Thin Film Transistor 480 Thin Film Transistor 481 Oxide Semiconductor Layer 483 Oxide Semiconductor Layer 1000 Mobile Phones 1001 Case 1002 Display section 1003 Operation button 1004 External connection port 1005 Speaker 1006 Mike 1300 Board 1301 Display section 1302 Drive unit 1303 Signal line driver circuit 1304 Scanning line driver circuit 1305 pixels 1306 Scan Lines 1308 Signal Line 1309 External connection terminal 1400 Board 1401 Gate electrode layer 1402 Gate insulation layer 1403 Oxide semiconductor layer 1405a Source electrode layer 1405b Drain electrode layer 1418 Channel Protection Layer 1430 Thin-film transistor 1800 Case 1801 Case 1802 Display Panel 1803 Speaker 1804 Microphone 1805 Operation key 1806 Pointing Device 1807 Camera Lenses 1808 External connection terminal 1810 Keyboard 1811 External memory slot 1908 Display Panel 1920 Board 1921 Display section 1922 Sealing material 1923 PCB 1924 FPC 1925 First sealing material 1926 Second sealing material 1927 Driver IC 6400 pixels 6401 Switching transistor 6402 Driving transistor 6403 Capacitor 6404 Light emitting element 6405 Signal Line 6406 scan lines 6407 Power line 6408 Common electrode 7001 Driving TFT 7002 Light emitting element 7003 Cathode 7004 Light-emitting layer 7005 Anode 7006 Protective insulation layer 7007 Flattening insulating film 7008 Cathode 7009 Bulkhead 7011 Driving TFT 7012 Light emitting element 7013 Cathode 7014 Light-emitting layer 7015 Anode 7016 Shielding membrane 7017 Light-transmitting conductive film 7018 Cathode 7019 Bulkhead 7021 Driving TFT 7022 Light emitting element 7023 Cathode 7024 Light-emitting layer 7025 Anode 7027 Light-transmitting conductive film 7028 Cathode 7029 Bulkhead 9600 Television Equipment 9601 Case 9603 Display section 9605 Stand 9607 Display section 9609 Operation key 9610 Remote control device 9700 Digital Photo Frame 9701 Case 9703 Display section 9881 Case 9882 Display section 9883 Display section 9884 Speaker section 9885 Operation key 9886 Recording medium insertion section 9887 Connection terminal 9888 Sensor 9889 Microphone 9890 LED Lamp 9891 Case 9893 Connection section

Claims

1. A substrate; a first conductive layer having a region in contact with the upper surface of the substrate and a region functioning as a gate electrode; a second conductive layer having an area in contact with the upper surface of the substrate and having the same material as the first conductive layer; a first insulating layer having a region located above the first conductive layer and functioning as a gate insulating layer; a semiconductor layer having a region located above the first insulating layer and having a channel formation region; a third conductive layer having a region in contact with an upper surface of the semiconductor layer and functioning as one of a source electrode and a drain electrode; a fourth conductive layer having a region in contact with an upper surface of the semiconductor layer and functioning as the other of the source electrode and the drain electrode; a second insulating layer having a region located above the second conductive layer and a region located above the third conductive layer; a fifth conductive layer having a region in contact with an upper surface of the second insulating layer and a region functioning as a pixel electrode layer; the fifth conductive layer is electrically connected to the third conductive layer; an area where the third conductive layer overlaps with the first conductive layer in a plan view is smaller than an area where the fourth conductive layer overlaps with the first conductive layer; the third conductive layer has a first region overlapping the first conductive layer and sandwiched between the fourth conductive layers in a plan view; a width of the third conductive layer in the first region is smaller than a width of the fourth conductive layer in a region overlapping with the first conductive layer; In a plan view, the second conductive layer has a region extending in a first direction and a second region intersecting the fourth conductive layer; A semiconductor device, wherein a width of the second conductive layer in the second region is greater than a width of the third conductive layer in the first region.

2. A substrate; a first conductive layer having a region in contact with the upper surface of the substrate and a region functioning as a gate electrode; a second conductive layer having an area in contact with the upper surface of the substrate and having the same material as the first conductive layer; a first insulating layer having a region located above the first conductive layer and functioning as a gate insulating layer; a semiconductor layer having a region located above the first insulating layer and having a channel formation region; a third conductive layer having a region in contact with an upper surface of the semiconductor layer and functioning as one of a source electrode and a drain electrode; a fourth conductive layer having a region in contact with an upper surface of the semiconductor layer and functioning as the other of the source electrode and the drain electrode; a second insulating layer having a region located above the second conductive layer and a region located above the third conductive layer; a fifth conductive layer having a region in contact with an upper surface of the second insulating layer and a region functioning as a pixel electrode layer; the fifth conductive layer is electrically connected to the third conductive layer; an area where the third conductive layer overlaps with the first conductive layer in a plan view is smaller than an area where the fourth conductive layer overlaps with the first conductive layer; the third conductive layer has a first region overlapping the first conductive layer and sandwiched between the fourth conductive layers in a plan view; a width of the third conductive layer in the first region is smaller than a width of the fourth conductive layer in a region overlapping with the first conductive layer; In a plan view, the second conductive layer has a region extending in a first direction and a second region intersecting the fourth conductive layer; a width of the second conductive layer in the second region is greater than a width of the third conductive layer in the first region; When viewed in a cross-section in a channel length direction, the semiconductor layer has a third region overlapping with the third conductive layer and a fourth region between the third conductive layer and the fourth conductive layer, A semiconductor device, wherein the thickness of the semiconductor layer in the fourth region is smaller than the thickness of the semiconductor layer in the third region.

Citation Information

Patent Citations

  • Thin film transistor substrate for liquid crystal display device

    JP2001194688A

  • Transistor and display device provided with the transistor

    JP2002190605A

  • Thin-film transistor substrate and manufacturing method therefor

    JP2005277428A

  • Liquid crystal display

    JP2006330472A

  • Array substrate for liquid crystal display device and manufacturing method thereof