Method for manufacturing multilayer ceramic electronic component, multilayer ceramic electronic component, and circuit board
By forming a recrystallized first nickel film and a second nickel film through electrolytic plating and heat treatment, the method addresses adhesion and solder bonding issues in multilayer ceramic capacitors, ensuring stable plating films and preventing hydrogen diffusion.
Patent Information
- Application Number
- JP2024122313
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-05-19
AI Technical Summary
The formation of Ni plating layers after oxidation treatments in multilayer ceramic capacitors can lead to decreased adhesion between the protective oxide film and the Ni plating layer, and the surface of the Ni plating layer may become unstable, affecting solder wettability and bonding during board mounting.
A method involving electrolytic plating to form a first nickel film on a ceramic body, followed by heat treatment in a weak reducing atmosphere to recrystallize and release hydrogen, then forming a second nickel film with a stable surface state, ensuring adhesion and solder bondability.
The method effectively suppresses hydrogen diffusion into the ceramic body, maintains adhesion of the plating films, and ensures sufficient solder bonding, thereby enhancing the reliability of the multilayer ceramic electronic components.
Smart Images

Figure 2024147812000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a multilayer ceramic electronic component having external electrodes, a multilayer ceramic electronic component, and a circuit board using the same. [Background technology]
[0002] Generally, the manufacturing process of a multilayer ceramic capacitor includes a plating process for forming external electrodes. Hydrogen generated during this plating process tends to be absorbed and remain in the external electrodes. In a multilayer ceramic capacitor, hydrogen in the external electrodes diffuses into the ceramic body, causing problems such as a decrease in insulation resistance.
[0003] In response to this, Patent Document 1 describes a method for manufacturing a multilayer ceramic capacitor, which comprises oxidizing an external electrode body containing Cu to form a protective layer containing CuO, forming a Ni plating layer on the protective layer, performing a heat treatment at a temperature of 150°C or higher after the formation of the Ni plating layer, and forming a Sn plating layer after the heat treatment. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2016-66783 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, when forming a Ni plating layer after oxidation treatment of the external electrode body, the adhesion between the protective layer, which is an oxide film, and the Ni plating layer may decrease. Furthermore, the surface of the Ni plating layer may become unstable due to oxidation after heat treatment. Therefore, forming a Sn plating layer directly on the surface may decrease the adhesion of the Sn plating layer and decrease the wettability of the solder used for mounting on the board.
[0006] In view of the above circumstances, an object of the present invention is to provide a method for manufacturing a multilayer ceramic electronic component that is less susceptible to the adverse effects of hydrogen, has excellent adhesion of plating films on external electrodes, and is capable of ensuring sufficient solder bondability during mounting, as well as a multilayer ceramic electronic component and a circuit board using the same. [Means for solving the problem]
[0007] In order to achieve the above object, a method for manufacturing a multilayer ceramic electronic component according to one embodiment of the present invention includes a step of forming a base film made of a conductive material on a surface of a ceramic body having internal electrodes that are laminated and extended to a surface, so that the base film is connected to the internal electrodes. A first nickel film is formed on the undercoat film by electrolytic plating. After the first nickel film is formed, the first nickel film is heat-treated in a weak reducing atmosphere at a temperature equal to or higher than the temperature at which the first nickel film is recrystallized. A second nickel film is formed on the heat-treated first nickel film by electrolytic plating. In the heat treatment, a recrystallized structure having fewer dislocations and lattice defects than the crystal structure of the second nickel film is formed in the first nickel film. Furthermore, in the heat treatment, crystal grains larger than crystal grains of the second nickel film may be formed in the first nickel film.
[0008] After the first nickel film is formed, the film is heat-treated at a temperature at which the film recrystallizes, thereby releasing the hydrogen trapped in the first nickel film and the like to the outside. Furthermore, the heat-treated first nickel film is recrystallized and configured to suppress the diffusion of hydrogen, so that the intrusion of hydrogen into the ceramic body after the heat treatment is prevented. This makes it possible to suppress problems such as a decrease in insulation resistance due to the diffusion of hydrogen into the ceramic body. In addition, by forming the second nickel film on the heat-treated first nickel film, the second nickel film can be arranged on the surface side with a stable surface state with little oxidation. Therefore, when mounting the multilayer ceramic electronic component on a substrate, it is possible to suppress the decrease in solder wettability and ensure sufficient solder bondability. Furthermore, by forming a second nickel film of the same material on the heat-treated first nickel film, it is possible to sufficiently ensure the adhesion between them.
[0009] Specifically, the temperature of the heat treatment may be 450° C. or higher and 800° C. or lower. This makes it possible to obtain a first nickel film that can recrystallize the first nickel film and sufficiently release hydrogen absorbed in the first nickel film and the like while also sufficiently suppressing diffusion of hydrogen.
[0010] For example, the first nickel film may have a thickness of not less than 1.0 μm and not more than 10.0 μm. This makes it possible to obtain a first nickel film capable of sufficiently suppressing diffusion of hydrogen after heat treatment, and also makes it possible to ease the conditions of the heat treatment for releasing hydrogen.
[0011] For example, the second nickel film may have a thickness of 1.5 μm or more and 6.0 μm or less. This makes it possible to ensure sufficient wettability of the solder during mounting, and also to reduce the size of the multilayer ceramic electronic component.
[0012] For example, the thickness of the undercoat film may be 2 μm or more and 50 μm or less. This makes it possible to reliably cover the surface of the ceramic body with the base film, while also achieving miniaturization of the multilayer ceramic electronic component.
[0013] For example, the undercoat film may contain copper or an alloy thereof as a main component.
[0014] A surface layer film containing tin or an alloy thereof as a main component may be formed on the second nickel film by electrolytic plating. By forming a surface film that reacts easily with solder, it is possible to more reliably ensure the solder bondability during mounting.
[0015] A multilayer ceramic electronic component according to another embodiment of the present invention includes a ceramic body and external electrodes. The ceramic body has internal electrodes that are laminated and extended to the surface. The external electrodes include an undercoat film, a first nickel film, and a second nickel film. The undercoat film is disposed on the surface of the ceramic body, is connected to the internal electrodes, and is made of a conductive material. The first nickel film is disposed on the undercoat film. The second nickel film has a higher hydrogen concentration than the first nickel film and is disposed on the first nickel film. The first nickel film has a recrystallized structure with fewer dislocations and lattice defects than the crystal structure of the second nickel film. Furthermore, the first nickel film may include crystal grains that are larger than the crystal grains of the second nickel film.
[0016] For example, the first nickel film may include a recrystallized structure. As a result, the recrystallized structure of the first nickel film suppresses the diffusion of hydrogen, and the intrusion of hydrogen into the ceramic body is prevented.
[0017] For example, the first nickel film may have a thickness of not less than 1.0 μm and not more than 10.0 μm.
[0018] For example, the second nickel film may have a thickness of 1.5 μm or more and 6.0 μm or less.
[0019] For example, the thickness of the undercoat film may be 2 μm or more and 50 μm or less.
[0020] For example, the undercoat film may contain copper or an alloy thereof as a main component.
[0021] The external electrode may further have a surface layer film disposed on the second nickel film and containing tin or an alloy thereof as a main component.
[0022] A circuit board according to yet another embodiment of the present invention includes a mounting substrate, a multilayer ceramic electronic component, and solder. The ceramic electronic component includes a ceramic body having internal electrodes that are laminated and extended to a surface, and external electrodes that are disposed on the surface of the ceramic body and connected to the internal electrodes. The solder connects the external electrodes to the mounting board. The external electrodes are a base film formed of a conductive material and disposed on the surface of the ceramic body; a first nickel film disposed on the undercoat film; a second nickel film having a higher hydrogen concentration than the first nickel film and disposed on the first nickel film. The first nickel film has a recrystallized structure with fewer dislocations and lattice defects than the crystal structure of the second nickel film. Effect of the Invention
[0023] As described above, according to the present invention, it is possible to provide a method for manufacturing a multilayer ceramic electronic component that is less susceptible to the adverse effects of hydrogen, has excellent adhesion of plating films on external electrodes, and is capable of ensuring sufficient solder bondability during mounting, as well as a multilayer ceramic electronic component and a circuit board using the same. [Brief description of the drawings]
[0024] [Figure 1] 1 is a perspective view showing a schematic diagram of a multilayer ceramic electronic component according to an embodiment of the present invention. [Diagram 2] 2 is a cross-sectional view taken along line AA' of the multilayer ceramic electronic component. FIG. [Diagram 3]2 is a cross-sectional view taken along line BB' of the multilayer ceramic electronic component. FIG. [Figure 4] 2 is a schematic cross-sectional view showing a circuit board on which the multilayer ceramic electronic component is mounted. FIG. [Diagram 5] 4 is a flowchart showing a method for manufacturing the multilayer ceramic electronic component. [Figure 6] 3A to 3C are perspective views showing a manufacturing process of the multilayer ceramic electronic component. [Figure 7] 1 is a graph showing the results of thermal desorption spectroscopy (TDS) performed on test chips in which external electrodes of different configurations are formed on the ceramic body of the above-mentioned multilayer ceramic electronic component, in which the horizontal axis indicates the test chip number and the vertical axis indicates the total amount of hydrogen desorbed from 50 mg of the test chip. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the drawings, an X-axis, a Y-axis, and a Z-axis that are mutually orthogonal are shown as appropriate, and the X-axis, the Y-axis, and the Z-axis are common to all the drawings.
[0026] [Configuration of multilayer ceramic capacitor 10] 1 to 3 are diagrams showing a multilayer ceramic capacitor 10 according to an embodiment of the present invention. Fig. 1 is a perspective view of the multilayer ceramic capacitor 10. Fig. 2 is a cross-sectional view of the multilayer ceramic capacitor 10 taken along line A-A' in Fig. 1. Fig. 3 is a cross-sectional view of the multilayer ceramic capacitor 10 taken along line B-B' in Fig. 1.
[0027] The multilayer ceramic capacitor 10 includes a ceramic body 11, a first external electrode 14, and a second external electrode 15. The ceramic body 11 typically has a first end face 11a and a second end face 11b facing the X-axis direction, a first side face 11c and a second side face 11d facing the Y-axis direction, and a first main face 11e and a second main face 11f facing the Z-axis direction. More specifically, the first end face 11a faces in one direction parallel to the X-axis direction, and the second end face 11b faces in a direction parallel to the X-axis direction and opposite to the one direction. The first side face 11c faces in one direction parallel to the Y-axis direction, and the second side face 11d faces in a direction parallel to the Y-axis direction and opposite to the one direction. The first main face 11e faces in one direction parallel to the Z-axis direction, and the second main face 11f faces in a direction parallel to the Z-axis direction and opposite to the one direction. The first end face 11a and the second end face 11b extend along the Y-axis direction and the Z-axis direction. The first side face 11c and the second side face 11d extend along the Z-axis direction and the X-axis direction. The first main face 11e and the second main face 11f extend along the X-axis direction and the Y-axis direction.
[0028] The first end face 11a and the second end face 11b, the first side face 11c and the second side face 11d, and the first main face 11e and the second main face 11f of the ceramic body 11 are all configured as flat surfaces. The flat surface according to the present embodiment does not have to be a strictly flat surface as long as it is recognized as flat when viewed overall, and includes, for example, a surface having a minute uneven shape or a gently curved shape.
[0029] The ceramic body 11 has ridges that interconnect the first end face 11a and the second end face 11b, the first side face 11c and the second side face 11d, and the first main face 11e and the second main face 11f. The ridges are, for example, chamfered to be rounded, but may not be chamfered.
[0030] The ceramic body 11 is made of dielectric ceramics. The ceramic body 11 has first internal electrodes 12 and second internal electrodes 13 covered with dielectric ceramics and stacked in the Z-axis direction. The multiple internal electrodes 12, 13 are each in the form of a sheet extending along the XY plane, and are alternately arranged along the Z-axis direction.
[0031] That is, the ceramic body 11 has a facing region where the internal electrodes 12, 13 face each other in the Z-axis direction with the ceramic layer 16 sandwiched therebetween. The first internal electrode 12 is extended from the facing region to the first end face 11a and connected to the first external electrode 14. The second internal electrode 13 is extended from the facing region to the second end face 11b and connected to the second external electrode 15.
[0032] With this configuration, when a voltage is applied between the first external electrode 14 and the second external electrode 15 in the multilayer ceramic capacitor 10, the voltage is applied to the multiple ceramic layers 16 in the opposing regions of the internal electrodes 12, 13. As a result, a charge corresponding to the voltage between the first external electrode 14 and the second external electrode 15 is stored in the multilayer ceramic capacitor 10.
[0033] In the ceramic body 11, a dielectric ceramic with a high dielectric constant is used to increase the capacitance of each ceramic layer 16 between the internal electrodes 12, 13. An example of a dielectric ceramic with a high dielectric constant is a material with a perovskite structure containing barium (Ba) and titanium (Ti), such as barium titanate (BaTiO3).
[0034] In addition, the dielectric ceramics may be made of compositions such as strontium titanate (SrTiO3), calcium titanate (CaTiO3), magnesium titanate (MgTiO3), calcium zirconate (CaZrO3), calcium zirconate titanate (Ca(Zr,Ti)O3), barium zirconate (BaZrO3), and titanium oxide (TiO2).
[0035] The first external electrode 14 is disposed on the surface of the ceramic body 11 and covers, for example, the first end face 11a. The second external electrode 15 is disposed on the surface of the ceramic body 11 and covers, for example, the second end face 11b. The external electrodes 14, 15 face each other in the X-axis direction with the ceramic body 11 in between and function as terminals of the multilayer ceramic capacitor 10.
[0036] The external electrodes 14, 15 extend inward in the X-axis direction from the end faces 11a, 11b of the ceramic body 11 along the principal faces 11e, 11f and the side faces 11c, 11d, respectively, and are spaced apart from each other on the principal faces 11e, 11f and the side faces 11c, 11d.
[0037] The shapes of the external electrodes 14, 15 are not limited to those shown in Figures 1 and 2. For example, the external electrodes 14, 15 may extend from the end faces 11a, 11b of the ceramic body 11 to only one of the main surfaces, and may have an L-shaped cross section parallel to the XZ plane. Furthermore, the external electrodes 14, 15 may not extend to any of the main surfaces or side surfaces.
[0038] The first external electrode 14 has a four-layer structure, and includes an undercoat film 140, a first nickel film 141, a second nickel film 142, and a surface film 143. In the first external electrode 14, the undercoat film 140, the first nickel film 141, the second nickel film 142, and the surface film 143 are laminated in this order from the inside of the ceramic body 11 side to the outside.
[0039] The second external electrode 15 has a four-layer structure, and includes an undercoat film 150, a first nickel film 151, a second nickel film 152, and a surface film 153. In the second external electrode 15, the undercoat film 150, the first nickel film 151, the second nickel film 152, and the surface film 153 are laminated in this order from the inside to the outside of the ceramic body 11.
[0040] The undercoat films 140 and 150 are formed of a conductive material. For example, the undercoat films 140 and 150 may contain Cu (copper), Ni (nickel), Ag (silver), Au (gold), Pt (platinum), Pd (palladium), Ti (titanium), Ta (tantalum), W (tungsten), or an alloy thereof as a main component. As an example, the undercoat films 140 and 150 may contain Cu or an alloy thereof as a main component. The main component refers to the component with the highest molar ratio.
[0041] The undercoat films 140 and 150 can be configured, for example, as at least one sputtered film formed by a sputtering method, at least one baked film formed by baking a conductive metal paste, etc. Also, the undercoat films 140 and 150 may be configured by combining a sputtered film and a baked film.
[0042] The first nickel films 141, 151 are films formed by electrolytic plating and disposed on the base films 140, 150. The first nickel films 141, 151 contain Ni or an alloy thereof as a main component. The first nickel films 141, 151 are films that have been subjected to heat treatment at a temperature equal to or higher than the recrystallization temperature, and contain recrystallized grains of a metal or alloy containing Ni as a main component, as will be described in detail later.
[0043] The second nickel films 142, 152 are films formed by electrolytic plating and are disposed on the first nickel films 141, 151. The second nickel films 142, 152 also contain Ni or an alloy thereof as a main component. The second nickel films 142, 152 are formed after the above heat treatment and therefore are not subjected to the above heat treatment.
[0044] The surface films 143, 153 are films formed by electrolytic plating and are disposed on the second nickel films 142, 152. The surface films 143, 153 contain, for example, Sn (tin) or an alloy thereof as a main component, which enhances the reactivity of the external electrodes 14, 15 with the solder during soldering for mounting the multilayer ceramic capacitor 10 on a mounting board, thereby enabling them to be sufficiently bonded to each other.
[0045] [Configuration of circuit board 100] FIG. 4 is a cross-sectional view showing the circuit board 100 of this embodiment, and is a view showing a cross section corresponding to FIG.
[0046] As shown in FIG. 4, the circuit board 100 includes a mounting board 110 and a multilayer ceramic capacitor. 10, a first solder H1 and a second solder H2.
[0047] The mounting substrate 110 is a substrate on which the multilayer ceramic capacitor 10 is mounted, and may have a circuit (not shown) formed thereon. The mounting substrate 110 has a mounting surface 110a facing the multilayer ceramic capacitor 10, and a first land L1 and a second land L2 formed on the mounting surface 110a for connection to the circuit substrate 100.
[0048] The first solder H1 connects the first land L1 of the mounting board 110 to the first external electrode 14. The second solder H2 connects the second land L2 of the mounting board 110 to the second external electrode 15. These solders H1, H2 are formed, for example, by solder paste applied to the lands L1, L2 melting and wetting onto the external electrodes 14, 15.
[0049] In the multilayer ceramic capacitor 10, the surface films 143, 153 react favorably with the solder, facilitating the wetting up of the solder, and the first solder H1 and second solder H2 can be joined to the external electrodes 14, 15 sufficiently.
[0050] Furthermore, the wetting of the solder is affected not only by the surface films 143, 153 but also by the surface condition of the layer below them. In this embodiment, the second nickel films 142, 152 that have not been subjected to heat treatment are provided below the surface films 143, 153, so that the solder wettability can be maintained well.
[0051] The detailed effects of the first nickel films 141, 151 and the second nickel films 142, 152 will be described later.
[0052] [Method of manufacturing multilayer ceramic capacitor 10] Fig. 5 is a flowchart showing a method for manufacturing the multilayer ceramic capacitor 10. Fig. 6 is a diagram showing a manufacturing process of the multilayer ceramic capacitor 10. The method for manufacturing the multilayer ceramic capacitor 10 will be described below along Fig. 5 with reference to Fig. 6 as needed.
[0053] (Step S01: Preparation of ceramic body 11) In step S01, a first ceramic sheet S1, a second ceramic sheet S2 and a third ceramic sheet S3 are laminated and fired as shown in FIG.
[0054] The ceramic sheets S1, S2, and S3 are formed as unfired dielectric green sheets mainly composed of dielectric ceramics. An unfired first internal electrode 12u corresponding to the first internal electrode 12 is formed on the first ceramic sheet S1, and an unfired second internal electrode 13u corresponding to the second internal electrode 13 is formed on the second ceramic sheet S2. No internal electrode is formed on the third ceramic sheet S3.
[0055] In the green ceramic body 11u shown in Fig. 6, the ceramic sheets S1 and S2 are alternately laminated, and a third ceramic sheet S3 is laminated on the top and bottom surfaces in the Z-axis direction. The green ceramic body 11u is integrated by pressing the ceramic sheets S1, S2, and S3 together. The number of the ceramic sheets S1, S2, and S3 is not limited to the example shown in Fig. 6.
[0056] Although the above describes the unsintered ceramic body 11u corresponding to one ceramic body 11, in reality, a laminated sheet is formed as a large sheet that is not separated into individual pieces, and then the laminated sheet is separated into individual ceramic bodies 11u.
[0057] The ceramic body 11 shown in Figs. 1 to 3 is produced by sintering the unsintered ceramic body 11u. The firing temperature can be determined based on the sintering temperature of the ceramic body 11u. For example, when a barium titanate-based material is used as the dielectric ceramic, the firing temperature can be set to about 1000 to 1300°C. Furthermore, the firing can be performed, for example, in a reducing atmosphere or a low oxygen partial pressure atmosphere.
[0058] (Step S02: Formation of undercoat films 140 and 150) In step S02, base films 140, 150 made of a conductive material are formed on the surfaces of the ceramic body 11 so as to be connected to the internal electrodes 12, 13. In this embodiment, the base films 140, 150 are formed so as to cover the first end face 11a and the second end face 11b.
[0059] The base films 140, 150 are formed by applying a conductive paste to the end faces 11a, 11b of the ceramic body 11 by, for example, a dipping method, a printing method, or the like, and baking the paste. In this case, the conductive material constituting the base films 140, 150 may contain, for example, Cu, Ni, Ag, Au, Pt, Pd, or an alloy thereof as a main component.
[0060] Alternatively, the undercoat films 140 and 150 may be formed by a sputtering method. In this case, the conductive material constituting the undercoat films 140 and 150 may contain, for example, Ti, Ni, Ag, Au, Pt, Pd, Ta, W, or an alloy thereof as a main component.
[0061] The thickness of the undercoat films 140, 150 can be set to 2 μm or more and 50 μm or less. This allows the end faces 11a, 11b to be reliably covered by the undercoat films 140, 150 while miniaturizing the multilayer ceramic capacitor 10. The thickness of the undercoat films 140, 150 can be, for example, the thickness of the region on the end faces 11a, 11b, and can be the dimension along the X-axis direction of the center in the Z-axis direction and the Y-axis direction.
[0062] (Step S03: Forming first nickel films 141, 151) In step S03, first nickel films 141, 151 are formed on the undercoat films 140, 150. The first nickel films 141, 151 contain Ni or an alloy thereof as a main component, and are formed by electrolytic plating.
[0063] (Step S04: Heat treatment) In step S04, after the first nickel films 141, 151 are formed, a heat treatment is performed in a weak reducing atmosphere. In this embodiment, a weak reducing atmosphere means an atmosphere with an oxygen concentration of 30 ppm or less. This prevents the first nickel films 141, 151 from being excessively oxidized. The temperature of the heat treatment is equal to or higher than the temperature at which the first nickel films 141, 151 are recrystallized, and specifically, can be set to 450° C. or higher and 800° C. or lower. The time of the heat treatment can be, for example, 5 minutes or higher and 30 minutes or lower.
[0064] (Step S05: Forming second nickel films 142, 152) In step S05, second nickel films 142, 152 are formed on the heat-treated first nickel films 141, 151. The second nickel films 142, 152 contain Ni or an alloy thereof as a main component, and are formed by electrolytic plating.
[0065] (Step S06: Formation of surface films 143, 153) In step S06, surface films 143, 153 are formed on the second nickel films 142, 152. The surface films 143, 153 contain, for example, Sn or an alloy thereof as a main component, and are formed by electrolytic plating.
[0066] The thickness of the surface films 143, 153 may be 3 μm or more and 10 μm or less, thereby ensuring sufficient reactivity with solder while miniaturizing the multilayer ceramic capacitor 10. The thickness of the surface films 143, 153 may be, for example, the thickness of the region on the end faces 11a, 11b, and may be the dimension along the X-axis direction of the center portion in the Z-axis direction and the Y-axis direction.
[0067] In this manner, the multilayer ceramic capacitor 10 is manufactured.
[0068] [Detailed description of external electrodes 14 and 15] The plating process by electrolytic plating for forming the first nickel films 141, 151, the second nickel films 142, 152, and the surface films 143, 153 generates hydrogen, which has a strong effect of deteriorating the ceramic body 11. The hydrogen generated in the plating process is likely to be absorbed in the base films 140, 150, the first nickel films 141, 151, the second nickel films 142, 152, and the surface films 143, 153 of the external electrodes 14, 15.
[0069] When the hydrogen absorbed in the external electrodes 14, 15 diffuses into the ceramic body 11 and reaches the opposing regions of the internal electrodes 12, 13, the insulation resistance of the ceramic layers 16 between the internal electrodes 12, 13 decreases, which makes the multilayer ceramic capacitor 10 more susceptible to insulation failure.
[0070] The hydrogen absorbed in the external electrodes 14, 15 is not limited to hydrogen generated in the plating process, but may be, for example, hydrogen contained in moisture such as water vapor in the atmosphere, etc. Furthermore, the hydrogen absorbed in the external electrodes 14, 15 may be in any state that hydrogen can be in, such as hydrogen atoms, hydrogen ions, or hydrogen isotopes.
[0071] In this embodiment, a heat treatment is performed in step S04 after the formation of the first nickel films 141, 151 in step S03, whereby hydrogen absorbed in the first nickel films 141, 151, etc. is released to the outside and removed.
[0072] Furthermore, this heat treatment promotes recrystallization of the first nickel films 141, 151, and the first nickel films 141, 151 are configured to suppress the diffusion of hydrogen. In other words, the first nickel films 141, 151 include a recrystallized structure. As a result, even if hydrogen is generated during the formation of the second nickel films 142, 152 and the surface films 143, 153, the first nickel films 141, 151 suppress the diffusion of the hydrogen, and prevent the hydrogen from entering the ceramic body 11. The penetration of hydrogen from the outside of the multilayer ceramic capacitor 10 is also prevented. As a result, the diffusion of hydrogen into the ceramic body 11 is suppressed in the multilayer ceramic capacitor 10.
[0073] The recrystallized structure of the first nickel films 141, 151 can be confirmed as a crystal structure with fewer dislocations and lattice defects compared to the second nickel films 142, 152. The recrystallized structure of the first nickel films 141, 151 has larger crystal grains compared to the second nickel films 142, 152. As a method for confirming these crystal structures, for example, a method can be used in which the target surface is chemically polished and then observed at 500 to 5000 times magnification using an optical microscope or a scanning electron microscope (SEM).
[0074] For example, a method for verifying the recrystallized structure of the first nickel films 141, 151 is to first check the structures of the first nickel films 141, 151 and the second nickel films 142, 152, then subject the second nickel films 142, 152 to a heat treatment (referred to as a verification heat treatment) similar to that in step S04, and compare the structure of the second nickel films 142, 152 after the verification heat treatment with the structure of the first nickel films 141, 151 before the verification heat treatment. If the structure of the second nickel films 142, 152 after the verification heat treatment has changed to a structure similar to the structure of the first nickel films 141, 151 before the verification heat treatment, it can be verified that the first nickel films 141, 151 have become recrystallized structures by the heat treatment in step S04.
[0075] That is, in this embodiment, the release of hydrogen absorbed in ceramic body 11, undercoat films 140, 150, and first nickel films 141, 151, and the formation of the diffusion suppression layer that suppresses the diffusion of hydrogen are performed in the same heat treatment process. Therefore, a configuration that is resistant to the adverse effects of hydrogen can be obtained while minimizing the thermal load on ceramic body 11 and the like associated with the release of hydrogen and the formation of the diffusion suppression layer.
[0076] The thickness of the first nickel films 141, 151 can be, for example, 1.0 μm to 10.0 μm, more preferably 1.0 μm to 4.5 μm. The thickness of the first nickel films 141, 151 can be, for example, the thickness of the region on the end faces 11a, 11b, and can be the dimension along the X-axis direction of the center in the Z-axis direction and the Y-axis direction.
[0077] By making the thickness of the first nickel film 141, 151 1.0 μm or more, the first nickel film 141, 151 sufficiently covers the undercoat film 140, 150, and the diffusion of hydrogen can be effectively suppressed. In addition, the components of the undercoat film 140, 150 are less likely to diffuse to the surface of the first nickel film 141, 151, and the adhesion between the surface and the second nickel film 142, 152 is improved. By making the thickness of the first nickel film 141, 151 10.0 μm or less, the amount of hydrogen generated by the formation of the first nickel film 141, 151 can be suppressed, and the condition of the heat treatment for releasing hydrogen can be relaxed. Furthermore, by making the thickness of the first nickel film 141, 151 4.5 μm or less, the thickness of the external electrodes 14, 15 can be suppressed, and the multilayer ceramic capacitor 10 can be made smaller.
[0078] Here, the heat-treated surface of the first nickel film 141, 151 is prone to formation of an oxide film and is in an unstable state. If the surface film 143, 153 is formed directly on such a first nickel film 141, 151, the wettability of the solder may decrease in the mounting process using solder, and good solder bonding may not be obtained.
[0079] Furthermore, if the surface films 143, 153 are formed on the unstable surfaces of the first nickel films 141, 151, the adhesion of the surface films 143, 153 may decrease, causing problems such as peeling of the surface films 143, 153.
[0080] Therefore, in this embodiment, the second nickel films 142, 152 are formed on the heat-treated first nickel films 141, 151. By arranging the second nickel films 142, 152, which are less susceptible to oxidation, on the surface layer side, it is possible to suppress a decrease in the wettability of the solder.
[0081] Moreover, since the second nickel films 142, 152 use the same type of metal or alloy as the first nickel films 141, 151, it is possible to ensure sufficient adhesion between the first nickel films 141, 151 and the second nickel films 142, 152. Furthermore, since the surface films 143, 153 are formed on the second nickel films 142, 152 which are less affected by oxide films and the like, it is possible to ensure sufficient adhesion between the second nickel films 142, 152 and the surface films 143, 153. This makes it possible to increase the adhesion of the plating films of the external electrodes 14, 15 and prevent the plating films from peeling off.
[0082] Furthermore, the hydrogen concentration in the first nickel films 141, 151 decreases due to the heat treatment. Meanwhile, the second nickel films 142, 152 absorb hydrogen generated in the plating process after the heat treatment. Therefore, the hydrogen concentration in the second nickel films 142, 152 becomes higher than the hydrogen concentration in the first nickel films 141, 151. Note that the hydrogen concentration can be expressed as the concentration (mol %) of hydrogen when nickel or its alloy, which is the main component of the nickel film, is taken as 100 mol %.
[0083] The hydrogen concentration is measured by, for example, secondary ion mass spectrometry (SIMS). As a sample for measuring the hydrogen concentration, for example, a multilayer ceramic capacitor 10 cut parallel to the XZ plane can be used. The cross section of the sample is mirror-polished using, for example, diamond paste, etc., so as to obtain a smoothness sufficient for measurement.
[0084] The thickness of the second nickel films 142, 152 can be, for example, 1.5 μm or more and 6.0 μm or less. The thickness of the second nickel films 142, 152 can be, for example, the thickness of the region on the end faces 11a, 11b, and can be the dimension along the X-axis direction of the center in the Z-axis direction and the Y-axis direction.
[0085] By setting the thickness of the second nickel films 142, 152 to 1.5 μm or more, the second nickel films 142, 152 are configured to sufficiently cover the heat-treated first nickel films 141, 151. This ensures sufficient wettability of the solder during mounting and enhances the adhesion of the surface films 143, 153. By setting the thickness of the second nickel films 142, 152 to 6.0 μm or less, the thickness of the external electrodes 14, 15 is suppressed, and the multilayer ceramic capacitor 10 can be made smaller in size.
[0086] Next, test results will be shown to further explain the effects of this embodiment.
[0087] [Test example] Thermal desorption spectroscopy (TDS) was performed on test chips in which external electrodes of different configurations were formed on the ceramic body 11. In the TDS, the amount of hydrogen desorbed from 50 mg of the test chip (about 8 electronic components) was measured while increasing the temperature from 100°C to 1000°C.
[0088] 7 is a graph showing the results of TDS, with the horizontal axis showing the test chip number and the vertical axis showing the total amount of hydrogen desorbed from 50 mg of test chips. Specifically, the vertical axis shows the relative amount of the number of hydrogen molecules desorbed from each 50 mg test chip, based on the number of hydrogen molecules desorbed from 50 mg of test chip 1.
[0089] The test chip was made by forming a 40 μm thick base film, mainly composed of Cu, on a ceramic body, and then forming a predetermined plating film on the base film. The size of the ceramic body is about 1.5 mm in the X-axis direction, about 0.7 mm in the Y-axis direction, and about 0.7 mm in the Z-axis direction.
[0090] Test chips 1 to 3 all have a first nickel film with a thickness of 3 μm. Test chip 1 has an external electrode made of an undercoat film and the first nickel film, and has not been subjected to heat treatment. Test chip 2 has external electrodes made of an undercoat film and a first nickel film, and after the first nickel film is formed, it is heat-treated in a weak reducing atmosphere at 450 to 550°C for 20 minutes. Test chip 3 has external electrodes made of an undercoat film, a first nickel film, and a second nickel film, and after the first nickel film is formed, it is heat-treated under the same conditions as test chip 2. The thickness of the second nickel film of test chip 3 is 6 μm.
[0091] Test chips 4 to 6 all have a first nickel film with a thickness of 6 μm. Test chip 4 has external electrodes made of an undercoat film and the first nickel film, and has not been subjected to heat treatment. Test chip 5 has external electrodes made of an undercoat film and the first nickel film, and after the formation of the first nickel film, has been heat treated under the same conditions as test chip 2. Test chip 6 has external electrodes made of an undercoat film, the first nickel film, and the second nickel film, and after the formation of the first nickel film, has been heat treated under the same conditions as test chip 2. The thickness of the second nickel film of test chip 6 is 6 μm.
[0092] Each of the test chips 7 to 9 has a first nickel film having a thickness of 10 μm. The test chip 7 has external electrodes made of an undercoat film and the first nickel film, and has not been subjected to heat treatment. The test chip 8 has external electrodes made of an undercoat film and the first nickel film, and after the formation of the first nickel film, it has been heat treated under the same conditions as the test chip 2. The test chip 9 has external electrodes made of an undercoat film, the first nickel film, and the second nickel film, and after the formation of the first nickel film, it has been heat treated under the same conditions as the test chip 2. The thickness of the second nickel film of the test chip 9 is 6 μm.
[0093] Referring to Figure 7, comparing the results of test chip 1, which was not heat-treated, and test chip 2, which was heat-treated, it was found that the amount of hydrogen desorption from test chip 2 was significantly reduced. The results were similar for test chips 4 and 5, and test chips 7 and 8. A small amount of hydrogen desorption in TDS means that the test chip contained a small amount of hydrogen. In other words, these results show that hydrogen absorbed in the first nickel film etc. is released to the outside by heat treatment.
[0094] In the test chips 4 and 7 having the first nickel films of 6 μm and 10 μm, the amount of hydrogen desorbed was significantly larger than that in the test chip 1 having the first nickel film of 3 μm. This shows that the amount of hydrogen absorbed in the first nickel film etc. increases when the first nickel film is formed thicker.
[0095] On the other hand, in test chips 5 and 8, which had a first nickel film of 6 μm and 10 μm and were subjected to heat treatment, the amount of hydrogen desorbed was significantly reduced compared to test chips 4 and 7, which were not subjected to heat treatment. This shows that even when the first nickel film is formed to a thickness of 6 μm or 10 μm, the absorbed hydrogen can be sufficiently released by heat treatment.
[0096] Test chip 3, which had the second nickel film, had a larger amount of hydrogen desorption than test chip 2, which did not have the second nickel film. Similar results were obtained for test chips 6 and 5, and test chips 9 and 8. This shows that when the second nickel film is formed after heat treatment, hydrogen is absorbed in the external electrodes.
[0097] Next, to confirm whether the adverse effects of hydrogen are suppressed by heat treatment, a highly accelerated limit test (HALT) was performed on each test chip. In the HALT, ten chips of each test chip 1 to 9 were prepared, and a voltage of 200 V was applied under the conditions of 150°C and 400 hours, and the number of chips with insulation failure was counted.
[0098] As a result, all ten test chips 1, 4 and 7, which were not subjected to heat treatment after the formation of the first nickel film, showed insulation defects. On the other hand, none of the test chips 2, 3, 5, 6, 8 and 9, which were subjected to heat treatment after the formation of the first nickel film, showed insulation defects.
[0099] From these results, it was found that if heat treatment was not performed, hydrogen absorbed in the external electrodes would diffuse to the opposing regions of the ceramic body due to high temperatures and high voltage application, and insulation resistance would be easily reduced. On the other hand, when heat treatment was performed as in the case of test chips 2, 3, 5, 6, 8 and 9, it was found that the decrease in insulation resistance due to hydrogen was suppressed even under severe conditions.
[0100] In particular, after the heat treatment, insulation failure was also suppressed for the test chips 3, 6, and 9 on which the second nickel film was formed. This shows that even if the external electrodes absorb hydrogen due to the formation of the second nickel film, the heat-treated first nickel film is configured to suppress the diffusion of hydrogen, and the adverse effects of hydrogen on the ceramic body are suppressed.
[0101] Furthermore, when 10 test chips each of 3, 6, and 9 were coated with a 4 μm tin plating film and soldered to a board by reflow, the solder wettability of all chips was good and no mounting failure occurred. Furthermore, when the external electrodes of these test chips 3, 6, and 9 were checked visually and with a stereo microscope, no peeling of the plating film was confirmed for any of the chips.
[0102] Therefore, according to this embodiment, a multilayer ceramic capacitor can be obtained which is less susceptible to the adverse effects of hydrogen, has good adhesion of the plating film, and can ensure sufficient bondability with the solder.
[0103] As can be seen from the TDS results in Fig. 7, in order to reduce the amount of hydrogen generated, it is possible to reduce the number of plating film layers. On the other hand, in this embodiment, the second nickel film is provided after the first nickel film is heat-treated at a temperature that recrystallizes the first nickel film. As a result, according to this embodiment, the first nickel film functions as a diffusion suppression layer that suppresses the diffusion of hydrogen, suppressing the adverse effects of hydrogen, while solving the problems of adhesion to the surface film and wettability of solder.
[0104] Although the embodiment of the present invention has been described above, the present invention is not limited to the above-described embodiment, and it goes without saying that various modifications can be made without departing from the spirit of the present invention.
[0105] The configuration of the external electrode according to the present invention is not limited to the four-layer structure as in the above embodiment, and may have at least three layers, namely, the undercoat film, the first nickel film, and the second nickel film. For example, the external electrode according to the present invention may have a five-layer or more structure.
[0106] Furthermore, the present invention is applicable not only to multilayer ceramic capacitors but also to general multilayer ceramic electronic components having external electrodes. Examples of multilayer ceramic electronic components to which the present invention can be applied include, in addition to multilayer ceramic capacitors, chip varistors, chip thermistors, and multilayer inductors. [Explanation of symbols]
[0107] 10...Multilayer ceramic capacitors (multilayer ceramic electronic components) 11…Ceramic body 12,13…Internal electrode 14,15...External electrode 140,150...Base film 141,151…First nickel film 142, 152…Second nickel film 143,153...Surface membrane
Claims
1. forming a base film made of a conductive material on a surface of a ceramic body having internal electrodes that are laminated and drawn out to a surface, the base film being connected to the internal electrodes; forming a first nickel film on the undercoat film by electrolytic plating; After the first nickel film is formed, a heat treatment is performed in a weak reducing atmosphere at a temperature at which the first nickel film is recrystallized or higher; forming a second nickel film on the heat-treated first nickel film by electrolytic plating; In the heat treatment, a recrystallized structure having fewer dislocations and lattice defects than the crystal structure of the second nickel film is formed in the first nickel film. A method for manufacturing multilayer ceramic electronic components.
2. 2. A method for producing a multilayer ceramic electronic component according to claim 1, comprising the steps of: In the heat treatment, crystal grains larger than the crystal grains of the second nickel film are formed in the first nickel film. A method for manufacturing multilayer ceramic electronic components.
3. 3. A method for producing a multilayer ceramic electronic component according to claim 1, further comprising the steps of: The temperature of the heat treatment is 450° C. or more and 800° C. or less. A method for manufacturing multilayer ceramic electronic components.
4. A method for producing a multilayer ceramic electronic component according to any one of claims 1 to 3, comprising the steps of: The thickness of the first nickel film is 1.0 μm or more and 10.0 μm or less. A method for manufacturing multilayer ceramic electronic components.
5. A method for producing a multilayer ceramic electronic component according to any one of claims 1 to 4, comprising the steps of: The thickness of the second nickel film is 1.5 μm or more and 6.0 μm or less. A method for manufacturing multilayer ceramic electronic components.
6. A method for producing a multilayer ceramic electronic component according to any one of claims 1 to 5, comprising the steps of: The thickness of the undercoat film is 2 μm or more and 50 μm or less. A method for manufacturing multilayer ceramic electronic components.
7. A method for producing a multilayer ceramic electronic component according to any one of claims 1 to 6, comprising the steps of: The undercoat film contains copper or an alloy thereof as a main component. A method for manufacturing multilayer ceramic electronic components.
8. A method for producing a multilayer ceramic electronic component according to any one of claims 1 to 7, comprising the steps of: A surface layer film containing tin or an alloy thereof as a main component is formed on the second nickel film by electrolytic plating. A method for manufacturing multilayer ceramic electronic components.
9. a ceramic body having internal electrodes that are laminated and drawn out to a surface; a base film that is disposed on the surface of the ceramic body, is connected to the internal electrodes, and is made of a conductive material; a first nickel film disposed on the undercoat film; a second nickel film having a higher hydrogen concentration than the first nickel film and disposed on the first nickel film; an external electrode having Equipped with The first nickel film has a recrystallized structure having fewer dislocations and lattice defects than the crystal structure of the second nickel film. Multilayer ceramic electronic components.
10. 10. The multilayer ceramic electronic component according to claim 9, The first nickel film includes crystal grains that are larger than the crystal grains of the second nickel film. Multilayer ceramic electronic components.
11. 11. The multilayer ceramic electronic component according to claim 9, The thickness of the first nickel film is 1.0 μm or more and 10.0 μm or less. Multilayer ceramic electronic components.
12. 12. The multilayer ceramic electronic component according to claim 9, The thickness of the second nickel film is 1.5 μm or more and 6.0 μm or less. Multilayer ceramic electronic components.
13. 13. The multilayer ceramic electronic component according to claim 9, The thickness of the undercoat film is 2 μm or more and 50 μm or less. Multilayer ceramic electronic components.
14. 14. The multilayer ceramic electronic component according to claim 9, The undercoat film contains copper or an alloy thereof as a main component. Multilayer ceramic electronic components.
15. 15. The multilayer ceramic electronic component according to claim 9, The external electrode further has a surface layer film disposed on the second nickel film and containing tin or an alloy thereof as a main component. Multilayer ceramic electronic components.
16. A mounting board; a laminated ceramic electronic component including a ceramic body having internal electrodes that are laminated and extended to a surface, and external electrodes that are disposed on the surface of the ceramic body and connected to the internal electrodes; Solder that connects the external electrodes and the mounting substrate; Equipped with The external electrode is a base film formed of a conductive material and disposed on the surface of the ceramic body; a first nickel film disposed on the undercoat film; a second nickel film having a higher hydrogen concentration than the first nickel film and disposed on the first nickel film; The first nickel film has a recrystallized structure having fewer dislocations and lattice defects than the crystal structure of the second nickel film. Circuit board.
Citation Information
Patent Citations
Ceramic electronic parts and manufacture thereof
JP1992022115A
Electronic parts and manufacturing method thereof
JP2006339536A
Electronic component, mounting structure thereof, and manufacturing method thereof
JP2007043144A
Multilayer capacitor manufacturing method and multilayer capacitor
JP2011253952A
Multilayer ceramic capacitor and method of manufacturing the same
JP2016066783A