Film for cell pouch and manufacturing method thereof

The film for cell pouches, featuring a barrier and adhesive layers with a one-pass 3-coating method, addresses the issues of stress and uneven strength in conventional processes, achieving enhanced mechanical strength and formability.

JP2024149467AActive Publication Date: 2024-10-18YOUL CHON CHEMICAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024061604
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-06
Filing Date
2024-04-05
Publication Date
2024-10-18
Estimated Expiration
2044-04-05

AI Technical Summary

Technical Problem

Conventional processes for manufacturing cell pouches involve repetitive steps like coating, drying, and winding, leading to increased process defects, stress on the film, and uneven mechanical strength distribution, which affects the film's durability and formability.

Method used

A film for cell pouches is designed with a barrier layer treated on both sides, adhesive layers on both sides, and functional layers, utilizing a one-pass 3-coating method to reduce stress and maintain uniform mechanical strength, with a difference in breaking strength between longitudinal and transverse directions of 40 N/15 mm or less.

Benefits of technology

The film exhibits excellent mechanical strength, reduced stress, low deviation in mechanical properties, and improved formability, minimizing process defects and ensuring consistent performance in both directions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149467000001_ABST
    Figure 2024149467000001_ABST
Patent Text Reader

Abstract

To provide a film for a cell pouch with excellent mechanical strength, low deviation in mechanical strength due to low stress on the film, and excellent formability, and a manufacturing method thereof.SOLUTION: A film for a cell pouch comprises: a barrier layer 300 made of metal and having surface treatment on both sides; adhesive layers 200, 400 formed on both sides of the barrier layer; and functional fabric layers 100, 500 formed on both sides of the adhesive layer, where the difference between a machine direction (MD) breaking strength and a transverse direction (TD) breaking strength is 40 N / 15 mm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Disclosed herein is a film for a cell pouch and a method for producing the same. [National research and development project that supported this invention] [Project unique number]1415185612 [Subject number] 20022450 [Department name] Ministry of Trade, Industry and Energy [Name of issue management (specialized) organization] Korea Institute for Industrial Technology Evaluation and Management [Research Project Name] Material Parts Package Type (Top Company) [Research title] Development of next-generation secondary battery pouches capable of achieving more than twice the adhesive strength (60℃) [Contribution rate] 1 / 1 [Name of project execution organization] Kurimura Chemical Co., Ltd. [Research period] 2023.01.01~2023.12.31 [Background technology]

[0002] Pouch-type batteries, which are generally used in electric vehicles, have the advantage of being easier to deform and having a higher energy density than cylindrical or prismatic batteries. Such cell pouches are generally manufactured in the following order: a first step of performing a surface treatment on one side of a metal layer, a second step of performing a surface treatment on the other side of the metal layer, a third step of laminating an outer layer on one side, and a fourth step of laminating a sealant layer on the other side.

[0003] Korean Patent Publication No. 10-2016-0070468 discloses such a process. However, in such a conventional process, the processes such as coating, drying, and winding are sequentially repeated for each process, which may increase the probability of running loss and process defects occurring during feeding of the raw roll. In addition, the conventional process has a problem that the speed is slow and the stress applied to the film increases due to the repeated winding. Furthermore, the tension of the driving roll that feeds the film is high, which causes a change in the tensile curve of the film, and the mechanical strength of the film in the machine direction (MD) and the transverse direction (TD) is changed. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Korean Patent Publication No. 10-2016-0070468 [Patent Document 2] Korean Patent Publication No. 10-2022-0031820 Summary of the Invention [Problem to be solved by the invention]

[0005] An object of one aspect of the present invention is to provide a film for a cell pouch, which has excellent mechanical strength, is subjected to less stress on the film, has a small deviation in mechanical strength, and has excellent formability, and a manufacturing method thereof. [Means for solving the problem]

[0006] In one aspect of the present invention, there is provided a film for cell pouches, comprising: a barrier layer made of metal and having a surface treatment applied to both sides thereof; adhesive layers formed on both sides of the barrier layer; and functional base fabric layers formed on both sides of the adhesive layer; and the difference between the breaking strength in the longitudinal direction (MD) and the breaking strength in the transverse direction (TD) is 40 N / 15 mm or less.

[0007] In another aspect, the present invention provides a cell pouch comprising the film for a cell pouch.

[0008] In another aspect, the present invention provides a method for manufacturing a film for a cell pouch, the method including: a double-sided surface treatment step of performing a surface treatment on both sides of a metal raw material forming a barrier layer; a one-sided coating step of applying an adhesive to one side of the surface-treated metal raw material to form an adhesive layer; and a lamination step of laminating a functional raw material to one side of the adhesive layer to form a functional raw material layer. Effect of the Invention

[0009] The cell pouch film and manufacturing method thereof according to an embodiment of the present invention have excellent mechanical strength, and since stress applied to the film is small, the deviation in mechanical strength is small and the formability is excellent. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic diagram showing a cross section of a film according to an embodiment of the present disclosure. [Diagram 2] 1 is a schematic diagram of a cell pouch film manufacturing apparatus according to an embodiment of the present invention. FIG. [Diagram 3] 1 is a stress-strain curve of a film for a cell pouch according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings.

[0012] The embodiments of the present invention disclosed herein are merely illustrative and are not to be construed as being limited to the embodiments described herein, as the present invention may be embodied in various forms. The present invention may be modified in various ways and may have various forms, and the embodiments are not intended to limit the present invention to the specific disclosed forms, but should be understood to include all modifications, equivalents, or alternatives within the spirit and technical scope of the present invention.

[0013] In this specification, when a part "comprises" a certain component, this means that it may further include other components, rather than excluding other components, unless otherwise specified.

[0014] Similar parts are designated by the same reference numerals throughout the specification. Throughout the specification, when a part such as a film, region, plate, etc. is described as being "on" or "above" another part, this includes not only when it is directly on the other part, but also when there is another part between them. Throughout the specification, terms such as first, second, etc. are used only to describe various components, and the components should not be limited by such terms. The terms are used only to distinguish one component from another.

[0015] In this specification, the term "cell" refers to a battery, and has the broadest meaning including all types of batteries such as secondary batteries such as lithium ion batteries and lithium polymer batteries, and portable storage batteries.

[0016] In this specification, the term "cell pouch" refers to a pouch in the broadest sense, which includes all laminated films processed into a bag or box shape in consideration of gas barrier properties, bendability, electrolyte resistance, thermal adhesiveness, etc., in order to house the cell components, such as a positive electrode, a negative electrode, and a separator, impregnated with an electrolyte and contained therein.

[0017] In this specification, the term "barrier property" refers to the ability to block water vapor from entering the battery from the outside.

[0018] In this specification, "flexibility" refers to the degree of bending of a cell and / or a cell pouch, and the better the bendability, the easier the cell and / or flexible cell pouch can be bent.

[0019] Cell pouch film FIG. 1 is a schematic cross-sectional view of a film according to an embodiment of the present disclosure.

[0020] In an exemplary embodiment of the present invention, a film for a cell pouch is provided, which includes a barrier layer 300 made of metal and having surface treatment applied to both sides thereof; adhesive layers 200, 400 formed on both sides of the barrier layer; and functional raw fabric layers 100, 500 formed on both sides of the adhesive layers 200, 400; and the difference between the breaking strength in the machine direction (MD) and the breaking strength in the width direction (TD) is 40N / 15mm or less.

[0021] One embodiment of the present disclosure may provide a film for a cell pouch, which includes a sealant layer 500; an inner adhesive layer 400 laminated on the sealant layer 500; a barrier layer 300 laminated on the inner adhesive layer 400; an outer adhesive layer 200 laminated on the barrier layer 300; and an outer layer 100 formed on the outer adhesive layer 200, wherein the barrier layer 300 includes a metal layer 320 and surface treatment layers 310 and 330 uniformly coated on both sides of the metal layer 320, respectively.

[0022] In one embodiment, an extruded resin layer may be further formed between the adhesive layer and the functional raw fabric layer. The extruded resin layer may improve the bendability, adhesiveness, insulation, etc. of the pouch. The extruded resin layer includes an olefin-based resin such as a polypropylene-based resin. The extruded resin layer may have a thickness of about 5 to 80 μm. Alternatively, the extruded resin layer and the sealant layer may constitute the inner layer of the film for the cell pouch without the inner adhesive layer. When the inner adhesive layer is not provided as described above, the extruded resin layer may also serve as the inner adhesive layer.

[0023] In an embodiment, the barrier layer can block the ingress and egress of external moisture and air, and internally generated gas. The barrier layer is not particularly limited as long as it is a metal having gas barrier properties. The barrier layer may include at least one selected from a metal thin film and a metal deposition layer. In this case, the metal thin film may be a metal foil, and the metal deposition layer may be formed by vacuum deposition on a separate plastic film, for example, a film of polyethylene terephthalate (PET), polyethylene (PE), or polypropylene (PP).

[0024] In one embodiment, the difference between the breaking strength in the machine direction (MD) and the breaking strength in the transverse direction (TD) of the film is 40N / 15mm or less. More specifically, the difference between the breaking strength in the machine direction (MD) and the breaking strength in the transverse direction (TD) of the film may be 5N / 15mm or more, 10N / 15mm or more, 15N / 15mm or more, 20N / 15mm or more, 23N / 15mm or more; 40N / 15mm or less, 35N / 15mm or less, 30N / 15mm or less, 25N / 15mm or less, 23N / 15mm or less, but is not limited thereto.

[0025] The present invention does not use a conventional method in which coating, drying, and winding are repeated for each process, but uses an in-line method of 1 Pass 3 Coating (1P3C) in which three or more coating processes can be performed in one facility according to the manufacturing method of the present invention. This reduces the probability of running losses and process defects that occur when feeding the raw material. In addition, according to the method of the present invention, the process speed is high and the number of windings is reduced, so the stress applied to the film is reduced, and the tension of the driving roll that feeds the film is low, so there is no change in the tensile curve of the film, and the mechanical strength of the film in the longitudinal direction (MD) and transverse direction (TD) is not changed.

[0026] In one embodiment, the functional base layer formed on one side of the adhesive layer is an outer layer made of a synthetic resin base film, and the functional base layer formed on the other side of the adhesive layer is a sealant layer made of a sealant base film.

[0027] In one embodiment, the sealant layer is an inner layer that is bonded by heat after the cells are embedded to provide sealing properties, and may include a sealing resin for thermal bonding.

[0028] In one embodiment, the film has a rupture strength in the transverse direction (TD) of 250N / 15mm or less. More specifically, the rupture strength in the transverse direction (TD) of the film may be, but is not limited to, 150N / 15mm or more, 160N / 15mm or more, 170N / 15mm or more, 180N / 15mm or more, 190N / 15mm or more, 200N / 15mm or more, 210N / 15mm or more, 220N / 15mm or more, 230N / 15mm or more, 231N / 15mm or more; 250N / 15mm or less, 240N / 15mm or less, or 231N / 15mm or less.

[0029] In one embodiment, the difference between the elongation percentage in the longitudinal direction (MD) and the transverse direction (TD) of the film is 6% or less. More specifically, the difference between the elongation percentage in the longitudinal direction (MD) and the transverse direction (TD) of the film may be, but is not limited to, 0% or more, 1% or more, 2% or more, 3% or more; 6% or less, 5% or less, 4% or less, 3% or less.

[0030] In an embodiment, the product of the difference (N / 15 mm) between the breaking strength in the machine direction (MD) and the breaking strength in the transverse direction (TD) of the film and the difference (%) between the elongation in the machine direction (MD) and the elongation in the transverse direction (TD) of the film is 240 or less. More specifically, the product of the difference (N / 15 mm) in breaking strength and the difference (%) in elongation may be 5 or more, 10 or more, 15 or more, 20 or more, 25 or more, 30 or more, 35 or more, 40 or more, 45 or more, 50 or more, 55 or more, 60 or more, 65 or more, 70 or more, 75 or more, 80 or more, 85 or more, 90 or more, 95 or more, 99 or more; 200 or less, 190 or less, 180 or less, 170 or less, 160 or less, 150 or less, 140 or less, 130 or less, 120 or less, 110 or less, 100 or less, or 99 or less, but is not limited thereto. When the product of the difference in breaking strength (N / 15mm) and the difference in elongation (%) is within the above range, the film for cell pouch has uniform physical properties in the machine direction (MD) and the transverse direction (TD), and therefore the stress applied to the film during the forming and processing process of the film for cell pouch can be uniformly distributed. This delays the phenomenon in which stress is concentrated in one direction and the occurrence of cracks is accelerated, thereby improving formability and durability.

[0031] In one embodiment, the formability in the longitudinal direction (MD) and the transverse direction (TD) of the film are both 16.5 mm or more. When a test piece cut from a film for a cell pouch is molded and its depth is measured, if none of 10 pieces out of 10 pieces at that depth are torn, the deeper depth is applied, and if even one piece is torn, the depth just before it is the maximum height and is called the formability. More specifically, the formability in the longitudinal direction (MD) and the transverse direction (TD) of the film may both be 16.5 mm or more, but is not limited thereto. The molded shape of the film for a cell pouch when molded is generally a rectangle (e.g., 190 mm wide and 90 mm long) rather than a square. For example, the formability in the longitudinal direction (MD) of the film means that the rectangular shape to be molded is 190 mm wide (TD direction) and 90 mm long (MD direction). The formability in the transverse direction (TD) means that the formed rectangular shape has a horizontal length of 190 mm (MD) and a vertical length of 90 mm (TD).

[0032] In one embodiment, the metal constituting the barrier layer, specifically, the metal constituting the metal thin film or metal deposition layer, may be one or more selected from the group consisting of aluminum (Al), iron (Fe), copper (Cu), nickel (Ni), tin (Sn), zinc (Zn), indium (In), and tungsten (W) (single metal or mixture of single metals), or an alloy of two or more selected therefrom. In one embodiment, the metal of the barrier layer is aluminum or an alloy thereof. The barrier layer is required to have properties such as barrier properties against water vapor and other gases as well as formability. Furthermore, the barrier layer may be surface-treated with phosphoric acid, chromium, or the like for corrosion resistance.

[0033] In one embodiment, the outer layer includes one or more resins selected from the group consisting of polyethylene terephthalate (PET) resin and nylon resin. The outer layer is required to have properties such as heat resistance, pinhole resistance, chemical resistance, abrasion resistance, moldability, and insulation. The outer layer may be composed of a plurality of layers. In one embodiment, the outer layer is made of polyethylene terephthalate (PET) resin and nylon resin.

[0034] In one embodiment, the sealant layer includes one or more polyolefin resins selected from the group consisting of polypropylene, low density polyethylene, linear low density polyethylene, very low density polyethylene, medium density polyethylene, high density polyethylene, polybutene, and ethylene / propylene copolymer. The sealant layer is required to have properties such as heat resistance, cold resistance, thermal adhesion, and formability, as well as electrolyte resistance and insulation resistance since it is a layer that comes into contact with the electrolyte. The sealant layer may be composed of multiple layers.

[0035] In one embodiment, the surface treatment layer may be a surface treatment layer based on phosphoric acid, chromium, zirconium, cerium, lanthanum, or the like to provide corrosion resistance to the metal.

[0036] In one embodiment, the adhesive layer may include one or more of an epoxy adhesive, a polyurethane adhesive, a phenolic resin adhesive, a polyester adhesive, and a polyolefin adhesive. As an example, the inner adhesive layer and the outer adhesive layer may each have a thickness of 0.5 μm to 10 μm.

[0037] In one embodiment, the barrier layer may have a thickness of 5 μm to 100 μm. If the thickness of the barrier layer is less than 5 μm, it is difficult to realize the barrier layer as a cell pouch for a secondary battery, and if the thickness of the barrier layer is more than 100 μm, the battery capacity may be rapidly reduced in a bending test of the cell pouch. In one embodiment, the outer layer may have a thickness of 5 μm to 50 μm. In one embodiment, the sealant layer may have a thickness of 5 μm to 100 μm.

[0038] In one embodiment, an extruded resin layer may be further formed between the inner adhesive layer and the sealant layer. The extruded resin layer may improve the bendability, adhesiveness, insulation, etc. of the pouch. In one embodiment, the extruded resin layer may include an olefin-based resin such as a polypropylene-based resin. In another embodiment, the inner adhesive layer may not be provided, and the extruded resin layer and the sealant layer may constitute an inner layer of the film for a cell pouch. When the inner adhesive layer is not provided as described above, the extruded resin layer may also function as the inner adhesive layer. In one embodiment, the extruded resin layer may have a thickness of 5 μm to 80 μm.

[0039] Cell Pouch The cell pouch film according to one embodiment of the present invention is excellent in gas barrier properties, bendability, electrolyte resistance, and heat adhesion, and is therefore suitable for use as a cell pouch.

[0040] In another exemplary embodiment of the present invention, a cell pouch is provided, including a film for a cell pouch according to an embodiment of the present invention.

[0041] Manufacturing method for cell pouch film In another exemplary embodiment of the present invention, there is provided a method for manufacturing a film for a cell pouch, the method including: a double-sided surface treatment step of performing a surface treatment on both sides of a metal base material on which a barrier layer is formed; a one-sided coating step of applying an adhesive to one side of the surface-treated metal base material to form an adhesive layer; and a lamination step of laminating a functional base material to one side of the adhesive layer to form a functional base material layer.

[0042] The present invention does not involve repeated processes such as coating, drying, and winding for each process, but uses an in-line method of 1 Pass 3 Coating (1P3C) in which three or more coating processes can be performed in one facility according to the manufacturing method of the present invention. This reduces the probability of running losses and process defects that occur when feeding the raw roll. In addition, according to the method of the present invention, the process speed is high and the number of windings is reduced, reducing the stress applied to the film, and the tension of the driving roll that feeds the film is low, so there is no change in the tensile curve of the film, and the mechanical strength of the film in the longitudinal direction (MD) and transverse direction (TD) is not changed.

[0043] The double-sided surface treatment step is a process of performing a surface treatment by applying a first and second coat to both sides of a metal substrate on which a metal layer is to be formed, and the double-sided surface treatment step is performed by a double-sided coating means including a first coater and a second coater.

[0044] The double-sided surface treatment step may include a web supplying process for unwinding and supplying a wound metal web; a foreign matter removing process for removing foreign matter present on the surface of the supplied metal web; a tension adjusting process for adjusting the tension of the metal web from which the foreign matter on the surface has been removed; and a double-sided coating process for coating both sides of the metal web while maintaining a constant tension.

[0045] The foreign matter removal process may include a first foreign matter removal process of removing oil by performing an electric discharge treatment on both sides of the metal web. The foreign matter removal process may further include a pinhole inspection process of checking whether pinholes have occurred on both sides of the metal web from which the oil has been removed. The foreign matter removal process may further include a second foreign matter removal process of removing foreign matter occurring on both sides of the metal web after the pinhole inspection by a roll method.

[0046] One side of the metal roll is coated with water-based and solvent-based coating liquids by a primary coater using a direct coating and reverse kiss coating (RKC) method, taking into consideration the physical properties and changes of the coating liquid. The other side of the metal roll may be coated with a secondary coating using RKC and film up / down coating methods. Meanwhile, the position of the substrate contact surface, coating roll, and doctor can be adjusted to improve the coating uniformity and work speed. In particular, a chamber method (sealed piping) is configured to precisely control the coating agent, and the viscosity of the coating agent can be adjusted and the inflow of foreign matter can be basically blocked.

[0047] Between the double-sided surface treatment step and the one-sided surface coating step of forming an adhesive layer, the method may further include a property stabilization drying step of drying the metal sheet having both sides coated thereon in a floating manner to stabilize the property; a cooling step of cooling the dried metal sheet; and a surface inspection step of inspecting the surface of the cooled metal sheet.

[0048] After the double-sided surface treatment step is completed, the metal web with the coating treatment on both sides can be dried in a floating manner to stabilize the physical properties. In this case, the drying method may be an air floating method so that the coated substrate can be dried in a non-contact manner while floating. This allows the metal web with the surface treatment on both sides to be dried while minimizing contact with components such as a feed roll. The dried metal web can then be cooled, and the surface of the cooled metal web can be inspected.

[0049] The one-side coating step for forming the adhesive layer is a process of applying an adhesive to one side of the metal base material that has been surface-treated by two coatings, and is performed by a third coater, and is prepared for lamination through processes such as drying. After applying the adhesive, the metal base material to which the adhesive has been applied is dried to form an adhesive layer, and the thickness of the dried adhesive layer is measured, and the surface of the adhesive layer is corona-treated to strengthen the adhesive force.

[0050] One embodiment of the method may further include, after the laminating step, an inner adhesive layer coating step of applying an inner adhesive to the other side of the metal sheet where the outer layer is not laminated to form an inner adhesive layer. Also, one embodiment may further include a drying step after the coating step. One embodiment may further include a step of laminating a sealant layer sheet under the inner adhesive layer.

[0051] In one embodiment, the method may include a total of two or less winding steps to prevent punctures and / or indentations from occurring on the raw material used in each step up to the outer layer lamination step. Specifically, the metal raw material may be wound up a total of two or less times. More specifically, the winding step may include a total of one winding step. In one embodiment, the winding step may be included after the outer adhesive layer coating step and before the outer layer raw material lamination step. For example, the winding step may be performed in step (10) in FIG. 2.

[0052] In one embodiment, the laminating step of laminating an outer layer raw material on the outer adhesive layer and the step of laminating a sealant layer raw material under the inner adhesive layer are each a process of laminating a functional raw material on one side of a metal raw material coated with an adhesive, and the inner side may be laminated with a sealant layer raw material for mainly stabilizing the heat resistance and cold resistance of the battery, and the outer side may be laminated with an outer layer raw material for heat resistance, pinhole resistance, abrasion resistance, etc. In one embodiment, each laminating step may be a step of laminating a previously prepared outer layer raw material or sealant raw material.

[0053] Between the third coating step and the laminating step, the method may further include an adhesive drying step of drying the adhesive-coated metal substrate to form an adhesive layer; an adhesive layer thickness measuring step of measuring the thickness of the dried adhesive layer; and an adhesive layer surface treatment step of corona-treating the surface of the adhesive layer to enhance adhesive strength.

[0054] The method may further include a surface inspection step of inspecting the surface of the sealant layer or outer layer after the laminating step.

[0055] Meanwhile, in order to minimize the occurrence of foreign objects and scratches during the process of feeding each raw material, both a Tendency structure that separates the substrate contact roll from the shaft and moves, and an integrated movable shaft structure may be applied to the guide roll. The general driving method of the guide roll is a mechanism that transmits the rotation from the motor to the shaft integrated guide roll and drives it at a 1:1 speed, while the Tensile driving method is a mechanism that separates the guide roll from the shaft and mutually compensates for the rotation speed of the fine roll, and may be applied appropriately in the required section.

[0056] Furthermore, a rewinder unit and an unwinder unit (raw material supply unit) may be separately configured so that the equipment can be operated separately when a problem occurs in the equipment causing a malfunction in the equipment operation.

[0057] In addition, the present disclosure may further include an aging step as an embodiment. The aging step is a necessary step for improving the reliability of adhesive strength, electrolyte resistance, peel strength, etc., during the manufacture of the cell pouch, but since it takes a somewhat long time, an optimal aging step is essential. It is preferable from the viewpoint of productivity to manufacture the product through only one aging step for the final structure of the cell pouch. Specifically, the method may include one aging step. More specifically, the method may be a step of applying an adhesive to one side of the metal raw material that has been subjected to the surface treatment without an aging step after the both-side surface treatment step, and the aging step may be included after the sealant layer lamination step. For example, if an aging step is included in the both-side surface treatment step before the lamination step, the film in the middle of the manufacturing process may be exposed to air for a certain period of time or more, and the surface treatment agent that has not been laminated may be detached. For example, if an aging step is included in the adhesive layer formation step, a blocking phenomenon may occur in which the adhesive layer is partially reacted and then adheres to another layer.

[0058] The first intermediate structure of the film for cell pouches may have a structure of outer layer / adhesive layer / surface treatment layer / barrier layer / surface treatment layer / adhesive layer, and the second intermediate structure may have a structure of outer layer / adhesive layer / surface treatment layer / barrier layer / surface treatment layer. If it is unavoidable to carry out aging twice, it is preferable to carry out the first aging in the second intermediate structure and then the second aging in the final structure. If the first aging is carried out in the first intermediate structure, problems such as problems in the manufacturing process and deterioration of physical properties may occur. More specifically, in a product that has undergone the first aging in the first intermediate structure, the reaction of the inner adhesive layer (sealant layer side) may partially proceed, and a blocking phenomenon in which the inner adhesive layer sticks to the outer layer may occur.

[0059] Furthermore, when a sealant layer is formed after the primary maturation, an additional step for strengthening the adhesive strength of the inner adhesive layer becomes necessary, which may lead to a decrease in productivity.

[0060] Meanwhile, in order to minimize the generation of foreign matter and scratches during the feeding of the raw web, a suction roll may be applied in the tension control section, and a contact type clean roll may be applied to remove foreign matter generated during the running of the web and prevent the foreign matter from adhering to the roll and causing poor appearance (punctures, scratches, etc.).

[0061] In one embodiment, the film for the cell pouch is fed by a drive roll, and all or part of the drive roll is a suction roll. The suction roll has a plurality of holes for sucking air from its circumferential surface. By sucking air through the holes, the film is drawn into contact with the circumferential surface of the suction roll.

[0062] In one embodiment, the tension applied to the cell pouch film by the suction roll is 0.02 kgf / cm 2 ~2.5kgf / cm 2 It is.

[0063] In one embodiment, during the manufacturing process of the film for the cell pouch, the metal roll of the film for the cell pouch is wound up to two times in total.

[0064] Cell pouch film manufacturing equipment In another illustrative embodiment of the present invention, there is provided an apparatus for manufacturing a film for a cell pouch, comprising: a double-sided surface treatment means including a first coater 3 and a second coater 4 for performing a surface treatment on both sides of a metal raw material that forms a barrier layer; a third coater 7 for applying an adhesive to one side of the metal raw material that has been subjected to the surface treatment; and a lamination unit 9 for laminating a functional raw material to one side of the adhesive layer.

[0065] FIG. 2 is a schematic diagram of an apparatus for producing a film for a cell pouch according to one embodiment of the present invention.

[0066] The double-sided surface treatment means may include a raw material supply unit 1, a foreign matter removal unit 2, a tension adjustment unit, a first coater 3, and a second coater 4. The raw material supply unit 1 unwinds and supplies a wound metal raw material. The foreign matter removal unit 2 removes foreign matter present on the surface of the supplied metal raw material. The tension adjustment unit adjusts the tension of the metal raw material from which the foreign matter on the surface has been removed. The first coater 3 and the second coater 4 coat both sides of the metal raw material while maintaining a constant tension.

[0067] The foreign matter removal means 2 may include a primary foreign matter removal unit that performs discharge treatment on both sides of the metal raw material to remove oil. It may further include a pinhole inspection unit that checks for pinholes on both sides of the metal raw material from which oil has been removed. If no abnormality is found as a result of the inspection, it may further include a secondary foreign matter removal unit that removes foreign matter generated on both sides of the metal raw material by a roll method.

[0068] A property stabilization drying unit 5 may be provided between the double-sided surface treatment means and the third coater 7, which dries the metal web coated on both sides in a floating manner to stabilize the property. In this case, the drying method may be an air floating method so that the coated substrate can be dried in a non-contact manner while floating. This allows the metal web coated on both sides to be dried while minimizing contact with components such as a feed roll. The dried metal web may then be cooled by a cooling unit 6, and the surface of the cooled metal web may be inspected by a surface inspection unit.

[0069] Between the third coater 7 and the laminating unit 9, there may further be included an adhesive drying unit 8 for drying the adhesive-coated metal substrate to form an adhesive layer; an adhesive layer measuring unit for measuring the thickness of the dried adhesive layer; and an adhesive layer surface treatment unit for corona-treating the surface of the adhesive layer to strengthen the adhesive force.

[0070] The laminating section 9 may further include a surface inspection section for inspecting the surfaces of the sealant layer and the outer layer.

[0071] Between the laminating unit 9 and the final rewinding unit (End, 2nd Rewind) in Figure 2, a fourth coater (not shown) that applies adhesive to the other side of the surface-treated metal raw material, a drying unit (not shown), a functional layer laminating unit (not shown), an extrusion unit (including co-extrusion) (not shown), etc. may be added as necessary. EXAMPLES

[0072] The present invention will now be described in detail with reference to preferred embodiments so that those skilled in the art can easily practice the present invention. However, the present invention may be embodied in many different forms and should not be construed as limited to the embodiments set forth herein.

[0073] <Production Example 1> Production of film for cell pouches Both sides of the aluminum foil metal roll that forms the barrier layer were coated with a first and second coating to perform surface treatment. The metal roll with both sides coated was then dried using a floating method to stabilize the physical properties. The dried metal roll was then cooled, and a urethane adhesive was applied to one side of the metal roll that had been subjected to the surface treatment using a third coater to form an adhesive layer. A PET / nylon film prepared in advance was then laminated to one side of the adhesive layer to form an outer layer. An adhesive was applied to the other side of the adhesive layer, and a sealant layer was formed by laminating an unstretched polypropylene film, and a film for a cell pouch was manufactured and wound up (Example 1: a sample taken at 700 m from the paper tube part of a roll that had been wound up to a total of 2,000 m; Example 2: a sample taken at 1,300 m from the paper tube part of a roll that had been wound up to a total of 2,000 m; Example 3: a sample taken at 1,900 m from the paper tube part of a roll that had been wound up to a total of 2,000 m).

[0074] <Production Example 2> Production of film for cell pouches One side of the aluminum foil metal roll on which the barrier layer is formed is subjected to a first coating and surface treatment, and then it is wound up after drying. The other side of the aluminum foil metal roll on which the barrier layer is formed is subjected to a second coating and surface treatment, and then it is wound up after drying. One side of the aluminum foil metal roll on which both sides have been surface-treated is coated with a urethane adhesive, and after drying, a previously prepared PET / nylon film is laminated to form an outer layer and wound up. Next, the inner surface is coated with an adhesive, and after drying, an inner layer (sealant film) is laminated and wound up (Comparative Example 1: A sample at 700 m from the paper tube part on a roll wound up to a total of 2,000 m; Comparative Example 2: A sample at 1,300 m from the paper tube part on a roll wound up to a total of 2,000 m; Comparative Example 3: A sample at 1,900 m from the paper tube part on a roll wound up to a total of 2,000 m).

[0075] <Experimental Example 1> Evaluation of the difference between the physical properties in the machine direction (MD) and the transverse direction (TD) of the film The cell pouch films produced in Production Examples 1 and 2 were evaluated for the difference between the physical properties in the machine direction (MD) and the physical properties in the transverse direction (TD).

[0076] More specifically, specimens measuring 130 mm x 15 mm were cut from the wound roll in both the machine direction (MD) and the transverse direction (TD). The tensile strength of the specimens was measured at a stretching speed of 50 mm / min and a grip distance of 50 mm using a universal testing machine manufactured by UTM (Instron) in accordance with ASTM D638. The breaking strength, which is the strength at the time when the specimen broke, was measured, and a 30 mm length was marked in the middle of the specimen, and the length elongated after breaking was measured and evaluated to measure the elongation percentage.

[0077] The results are shown in Figure 3 and the following Tables 1 and 2. Figure 3 is a stress-strain curve of the cell pouch film according to one embodiment of the present invention.

[0078] [Table 1]

[0079] [Table 2]

[0080] From FIG. 3 and Tables 1 and 2, it can be seen that the cell pouch film according to the present invention has excellent mechanical strength and a low deviation in mechanical strength.

[0081] <Experimental Example 2> Evaluation of the difference between formability in the machine direction (MD) and the transverse direction (TD) of the film The cell pouch films produced in Production Examples 1 and 2 were evaluated for the difference between the physical properties in the machine direction (MD) and the physical properties in the transverse direction (TD).

[0082] More specifically, a test piece measuring 266mm x 240mm was taken from the roll in both the machine direction (MD) and transverse direction (TD). The test piece was molded into a rectangle (190mm horizontal, 90mm vertical) (the moldability was evaluated in 1 cup using chrome-coated high moldable pouch moldability evaluation equipment, and the R value was various, but the standard corner R value was 4).

[0083] When the depth was measured after molding, if none of the 10 pieces at that depth had any tears, the deeper depth was applied. If even one piece had a tear, the depth just before that was used as the maximum height and defined as formability.

[0084] The formability in the longitudinal direction (MD) means that the rectangular shape to be formed has a horizontal length of 190 mm (TD direction) and a vertical length of 90 mm (MD direction). The formability in the transverse direction (TD) means that the rectangular shape to be formed has a horizontal length of 190 mm (MD direction) and a vertical length of 90 mm (TD direction). The results are shown in Table 3 below.

[0085] [Table 3]

[0086] From Table 3, it can be seen that the cell pouch film according to the present invention has the best formability.

[0087] Although the exemplary embodiment of the present invention has been described in conjunction with the preferred embodiment mentioned above, various modifications and variations can be made without departing from the spirit and scope of the invention, and it is therefore intended that the appended claims cover such modifications and variations as fall within the spirit and scope of the present invention. [Explanation of symbols]

[0088] 1: Original fabric supply section 2: Foreign matter removal means 3: 1st coater 4: 2nd coater 5: Physical property stabilization drying section 6: Cooling section 7: 3rd coater 8: Adhesive drying section 9: Lamination section 10: Final winding section 100: Outer layer 200: Outer adhesive layer 300: Barrier layer 310: Surface treatment layer 320: Metal layer 330: Surface treatment layer 400: Inner adhesive layer 500: Sealant layer

Claims

1. A barrier layer made of metal and having a surface treatment applied to both sides; Adhesive layers formed on both sides of the barrier layer; and functional base layers formed on both sides of the adhesive layer; A film for cell pouches, the difference between the breaking strength in the machine direction (MD) and the breaking strength in the width direction (TD) being 40 N / 15 mm or less.

2. The functional base layer formed on one side of the adhesive layer is an outer layer made of a synthetic resin base layer, 2. The film for cell pouches according to claim 1, wherein the functional raw material layer formed on the other side of the adhesive layer is a sealant layer made of a sealant raw material.

3. 2. The strong pouch film of claim 1, wherein the film has a breaking strength in the cross direction (TD) of 250 N / 15 mm or less.

4. 2. The film for cell pouches according to claim 1, wherein the difference between the elongation percentage in the machine direction (MD) and the elongation percentage in the width direction (TD) of the film is 6% or less.

5. 2. The film for cell pouches according to claim 1, wherein the product of the difference (N / 15 mm) between the breaking strength in the longitudinal direction (MD) of the film and the breaking strength in the transverse direction (TD) of the film and the difference (%) between the elongation percentage in the longitudinal direction (MD) of the film and the elongation percentage in the transverse direction (TD) of the film is 240 or less.

6. The film for cell pouches according to claim 1 , wherein the formability in both the machine direction (MD) and the width direction (TD) of the film is 16.5 mm or more.

7. the metal of the barrier layer is aluminum or an alloy thereof; the outer layer comprises one or more resins selected from the group consisting of polyethylene terephthalate resins and nylon resins, 3. The film for cell pouches according to claim 2, wherein the sealant layer comprises one or more polyolefin resins selected from the group consisting of polypropylene, low density polyethylene, linear low density polyethylene, very low density polyethylene, medium density polyethylene, high density polyethylene, polybutene, and ethylene / propylene copolymer.

8. A cell pouch comprising the film for a cell pouch according to any one of claims 1 to 7.

9. A double-sided surface treatment step of performing a surface treatment on both sides of the metal sheet on which the barrier layer is formed; A step of coating one side of the surface-treated metal sheet by applying an adhesive to the one side of the sheet to form an adhesive layer; and The method for producing a film for a cell pouch according to any one of claims 1 to 7, further comprising: laminating a functional raw material on one side of the adhesive layer to form a functional raw material layer.

10. The method for producing a film for a cell pouch according to claim 9 , wherein the film for the cell pouch is fed by a driving roll, and all or a part of the driving roll is a suction roll.

11. The tension applied to the cell pouch film by the suction roll is 0.02 kgf / cm 2 ~2.5kgf / cm 2 The method for producing a film for a cell pouch according to claim 10,

12. The method for producing a film for a cell pouch according to claim 10, wherein the metal raw material film for the cell pouch is wound up a total of two times or less in the process for producing the film for the cell pouch.

Citation Information

Patent Citations

  • Multilayer film, package material, and battery

    JP2015107583A

  • Battery-packaging material

    JP2016207665A

  • Method for producing functional layer

    WO2023286646A1

  • Cell pouch and method of manufacturing the same

    KR1020160070468A

  • Primer layer composition, secondary battery pouch film using the same, and method for manufacturing the same

    KR1020220031820A