Method of processing workpiece

The method of fixing thermoplastic resin sheets on both sides of a workpiece with a gap between them allows for easy separation by preventing integration, addressing the challenge of separating integrated sheets.

JP2024150271APending Publication Date: 2024-10-23DISCO CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023063610
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-23

AI Technical Summary

Technical Problem

Thermoplastic resin sheets fixed on both sides of a workpiece tend to integrate through thermocompression bonding, making it difficult to separate them from the workpiece.

Method used

A method involving fixing a first and second sheet of thermoplastic resin without an adhesive layer on one and the other side of the workpiece, respectively, with a gap between them in the annular region between the workpiece and frame, using thermocompression bonding, and peeling them off after processing.

Benefits of technology

Enables easy peeling of the sheets from the workpiece by maintaining a gap between them, preventing integration and ensuring they can be easily detached even when fixed on both sides.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150271000001_ABST
    Figure 2024150271000001_ABST
Patent Text Reader

Abstract

To provide a method of processing a workpiece, in which a sheet can be easily peeled off even when the sheet is fixed to both surfaces of the workpiece.SOLUTION: A method of processing a workpiece includes: a sheet fixing step 101 including a first fixing step 111 of fixing a first sheet by thermocompression bonding to one surface of the workpiece and a frame for housing the workpiece in a central opening, and a second fixing step 112 of fixing a second sheet to the other surface of the workpiece by thermocompression bonding; a processing step 102 of performing processing including at least any one of a process, an inspection, a storage, and a transportation for the workpiece, after the sheet fixing step 101; and a peeling step 103 of peeling off the first sheet and the second sheet from the workpiece and the frame after the processing step 102. In the sheet fixing step 101, a first sheet and a second sheet are fixed to each other with a gap therebetween in a region between an outer periphery of the workpiece and an inner periphery of the frame.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for treating a workpiece. [Background technology]

[0002] In order to prevent the adhesion of foreign matter, a technique is known in which one side of a workpiece is protected with a sheet made of a thermoplastic resin that does not have an adhesive layer on both sides, and then processing such as cutting, irradiation with a laser beam, breaking, and sheet expansion, as well as inspection of the workpiece, storage of the workpiece, and transportation including conveying of the workpiece are performed (see, for example, Patent Documents 1, 2, and 3). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2021-077684 [Patent Document 2] JP 2020-077812 A [Patent Document 3] JP 2013-058671 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, when a sheet made of a thermoplastic resin is fixed to both surfaces of the substrate during processing, the sheets are integrated with each other by thermocompression bonding, which poses a problem that it becomes difficult to peel the sheets from the workpiece.

[0005] The present invention has been made in consideration of such problems, and its object is to provide a method for processing a workpiece that allows the sheet to be easily peeled off even when the sheet is fixed to both sides of the workpiece. [Means for solving the problem]

[0006] In order to solve the above-mentioned problems and achieve the object, the method for processing a workpiece of the present invention is a method for processing a workpiece, comprising a sheet fixing step of fixing a first sheet made of a thermoplastic resin having no adhesive layer to one side of the workpiece, and fixing a second sheet made of a thermoplastic resin having no adhesive layer to the other side of the workpiece, the sheet fixing step including a first fixing step of fixing the first sheet to one side of the workpiece and a frame that accommodates the workpiece in a central opening by thermocompression bonding, and a second fixing step of fixing the second sheet to the workpiece by thermocompression bonding. and a second fixing step of fixing the first sheet to the other side of the workpiece by thermocompression, wherein after the sheet fixing step, a processing step is performed on the workpiece including at least one of processing, inspection, storage, and transportation, and after the processing step, a peeling step is performed on the first sheet and the second sheet from the workpiece and the frame, and the first sheet and the second sheet are fixed with a gap between them in the sheet fixing step in the region between the outer periphery of the workpiece and the inner periphery of the frame.

[0007] In the sheet fixing step, the outer edge of the first sheet and the outer edge of the second sheet may be fixed to the frame, so that the first sheet and the second sheet are fixed with a gap between each other in the area between the outer periphery of the workpiece and the inner periphery of the frame.

[0008] In the sheet fixing step, a peeling member may be disposed between the first sheet and the second sheet in a region between an outer periphery of the workpiece and an inner periphery of the frame.

[0009] In the sheet fixing step, the second sheet may conform to an outer edge of the workpiece.

[0010] In addition, in order to solve the above-mentioned problems and achieve the object, the method for processing a workpiece of the present invention is a method for processing a workpiece, comprising a sheet fixing step of fixing a first sheet made of a thermoplastic resin having no adhesive layer to one side of the workpiece, and fixing a second sheet made of a thermoplastic resin having no adhesive layer to the other side of the workpiece, the sheet fixing step including a first fixing step of fixing the first sheet to one side of the workpiece and a frame that accommodates the workpiece in a central opening by thermocompression bonding, and a second fixing step of fixing the second sheet to the other side of the workpiece by thermocompression bonding. and a second fixing step of fixing the first sheet and the second sheet to the surface of the workpiece by thermocompression, and after the sheet fixing step, a processing step of performing a process including at least one of processing, inspection, storage, and transportation of the workpiece, and after the processing step, a peeling step of peeling the first sheet and the second sheet from the workpiece and the frame, wherein the peeling step is characterized by cutting at least one of the first sheet and the second sheet along the outer periphery of the workpiece, and then removing the first sheet and the second sheet from the workpiece and the frame.

[0011] The first sheet and the second sheet may be composed of any of polyolefin, polyethylene, polypropylene, and polystyrene. Effect of the Invention

[0012] The present invention provides a gap in the annular region between the outer periphery of the workpiece and the inner periphery forming the opening of the frame, which prevents a first sheet fixed to one side and a second sheet fixed to the other side from contacting each other. This prevents the first sheet and the second sheet from being thermocompressed together and integrated when the first sheet and the second sheet are thermocompressed, so that the first sheet and the second sheet can be easily peeled off even when the first sheet and the second sheet are fixed to both sides of the workpiece. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a flowchart showing a processing procedure of the workpiece processing method according to the first embodiment. [Diagram 2]FIG. 2 is a cross-sectional view illustrating the sheet fixing step of FIG. [Diagram 3] FIG. 3 is a cross-sectional view illustrating a first example of the processing steps of FIG. [Figure 4] FIG. 4 is a cross-sectional view illustrating a second example of the processing steps of FIG. [Diagram 5] FIG. 5 is a cross-sectional view illustrating a third example of the processing steps of FIG. [Figure 6] FIG. 6 is a cross-sectional view illustrating the peeling step of FIG. [Figure 7] FIG. 7 is a cross-sectional view illustrating the peeling step of FIG. [Figure 8] FIG. 8 is a cross-sectional view illustrating a sheet fixing step in the workpiece processing method according to the second embodiment. [Figure 9] FIG. 9 is a cross-sectional view illustrating a peeling step of the workpiece processing method according to the second embodiment. [Figure 10] FIG. 10 is a cross-sectional view illustrating a peeling step of the method for treating a workpiece according to the second embodiment. [Figure 11] FIG. 11 is a cross-sectional view illustrating a sheet fixing step in the method for treating a workpiece according to the third embodiment. [Figure 12] FIG. 12 is a cross-sectional view illustrating a sheet fixing step in the workpiece processing method according to the fourth embodiment. [Figure 13] FIG. 13 is a cross-sectional view illustrating a peeling step of the workpiece processing method according to the fourth embodiment. [Figure 14] FIG. 14 is a cross-sectional view illustrating a peeling step of the workpiece processing method according to the fourth embodiment. [Figure 15] FIG. 15 is a cross-sectional view illustrating a sheet fixing step in the workpiece processing method according to the fifth embodiment. [Figure 16] FIG. 16 is a cross-sectional view illustrating a peeling step of the method for treating a workpiece according to the fifth embodiment. [Figure 17] FIG. 17 is a cross-sectional view illustrating a peeling step of the method for treating a workpiece according to the fifth embodiment. [Figure 18]FIG. 18 is a cross-sectional view illustrating a peeling step of the method for treating a workpiece according to the fifth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The form (embodiment) for carrying out the present invention will be described in detail with reference to the drawings. The present invention is not limited to the contents described in the following embodiment. Furthermore, the components described below include those that a person skilled in the art can easily imagine and those that are substantially the same. Furthermore, the configurations described below can be appropriately combined. Furthermore, various omissions, substitutions, or modifications of the configurations can be made without departing from the gist of the present invention.

[0015] [Embodiment 1] A method for processing a workpiece according to a first embodiment of the present invention will be described with reference to the drawings. Fig. 1 is a flow chart showing the procedure of the method for processing a workpiece according to the first embodiment. As shown in Fig. 1, the method for processing a workpiece according to the first embodiment includes a sheet fixing step 101, a processing step 102, and a peeling step 103.

[0016] In the first embodiment, the workpiece 1 to be processed by the workpiece processing method according to the first embodiment is a disk-shaped semiconductor wafer or an optical device wafer made of silicon, sapphire, silicon carbide (SiC), gallium arsenide, glass, or the like. The workpiece 1 has a flat surface, and chip-shaped devices are formed in each of the areas partitioned by a plurality of intersecting (orthogonal in the first embodiment) planned division lines. The workpiece 1 is divided along the planned division lines to manufacture device chips. In the present invention, the workpiece 1 may be a rectangular package substrate having a plurality of devices sealed with resin, a ceramic plate, a glass plate, or the like.

[0017] Fig. 2 is a cross-sectional view for explaining the sheet fixing step 101 in Fig. 1. As shown in Fig. 2, the sheet fixing step 101 is a step of fixing a first sheet 11 made of a thermoplastic resin having no adhesive layer to one surface 2 of the workpiece 1, and fixing a second sheet 12 made of a thermoplastic resin having no adhesive layer to the other surface 3 of the workpiece 1. In the first embodiment, the one surface 2 is the back surface of the workpiece 1, and the other surface 3 is the surface of the workpiece 1 on which the device is formed, but the present invention is not limited thereto, and the one surface 2 may be the surface of the workpiece 1 on which the device is formed, and the other surface 3 may be the back surface of the workpiece 1.

[0018] Here, the first sheet 11 and the second sheet 12 are both sheets made of a thermoplastic resin that do not have a glue layer. In this specification, the glue layer is a layer made of a synthetic resin having adhesive properties such as a pressure-sensitive adhesive.

[0019] The thermoplastic resin constituting the first sheet 11 and the second sheet 12 has a storage modulus of 1×10 at a temperature of 10° C. or higher and 30° C. or lower. 6 Pa or more 1×10 9 Pa or less, and the storage modulus at temperatures between 80°C and 100°C is 1×10 6 Pa or more 1×10 7 Pa or less.

[0020] The storage modulus, together with the loss modulus (dynamic loss modulus) and loss tangent, is measured by dynamic mechanical analysis (DMA). Specifically, the storage modulus is measured according to any of the following methods: JIS K 7244-4 (non-resonant forced vibration method), JIS K 7244-5 (bending mode), and JIS K 7244-6 (shear mode) of the Japanese Industrial Standards. According to the Japanese Industrial Standards, the storage modulus is 0.01 GPa (1×10 7 If the strength is less than 0.01 GPa or less than 5 GPa (1×10 7 Pa or more 5×10 9Pa or less), it is preferable to measure using a method according to JIS K 7244-4 (non-resonant forced vibration method), and 9 In the case where the compressive strength is greater than 1 Pa, it is preferable to measure using a method in accordance with JIS K 7244-5 (bending mode).

[0021] The storage modulus generally varies depending on the temperature during measurement and the frequency (speed) of deformation applied during measurement. More specifically, the thermoplastic resin constituting the first sheet 11 and the second sheet 12 has a storage modulus of 1×10 or less when measured under conditions of a temperature of 10° C. or more and 30° C. or less and a deformation frequency of 0.01 Hz or more and 10 Hz or less. 6 Pa or more 1×10 9 The storage modulus measured under the conditions of a temperature of 80°C to 100°C and a deformation frequency of 0.01Hz to 10Hz is 1×10 6 Pa or more 1×10 7 Pa or less.

[0022] The thermoplastic resin constituting the first sheet 11 and the second sheet 12 has the above-mentioned storage modulus and has the property that the storage modulus decreases with increasing temperature, so that it does not have a glue layer and can be fixed to the surface of the workpiece 1 by thermocompression bonding by heating. 6 If the storage modulus is less than 1×10 Pa, the resin will be sticky and too adhesive, forming a glue layer. 9 If it is higher than Pa, the resin may be too hard and may not be fixed to the surface of the workpiece 1.

[0023] In the first embodiment, the thermoplastic resins constituting the first sheet 11 and the second sheet 12 are both polyolefins, such as polyethylene, polypropylene, and polystyrene. That is, the first sheet 11 and the second sheet 12 are both preferably made of polyolefin as the main material and formed into a sheet shape, that is, polyolefin-based sheets, such as polyethylene sheets, polypropylene sheets, and polystyrene sheets.

[0024] As shown in FIG. 1, the sheet fixing step 101 has a first fixing step 111 and a second fixing step 112. The first fixing step 111 is a step of fixing the first sheet 11 to one surface 2, 7 (see FIG. 2) of the workpiece 1 and the frame 6 (see FIG. 2) that houses the workpiece 1 in a central opening 9 (see FIG. 2) by thermocompression. The second fixing step 112 is a step of fixing the second sheet 12 to the other surface 3 of the workpiece 1 by thermocompression. In the second fixing step 112, in the first embodiment, the second sheet 12 is fixed to the other surfaces 3, 8 (see FIG. 2) of the workpiece 1 and the frame 6 by thermocompression. In the first embodiment, the second fixing step 112 is performed after the first fixing step 111 in the sheet fixing step 101, but the present invention is not limited to this, and the first fixing step 111 may be performed after the second fixing step 112.

[0025] Here, the frame 6 used in the method for processing a workpiece according to the first embodiment is formed in a plate shape with one surface 7 and the other surface 8 parallel to each other, and is formed in an annular shape by forming a circular opening 9 in the center having an inner diameter larger than the outer diameter of the workpiece 1. Therefore, the frame 6 can accommodate the workpiece 1 in the opening 9. In the first embodiment, the frame 6 is formed to be slightly thicker than the workpiece 1 as shown in FIG. 2, but the present invention is not limited to this, and the frame 6 may be formed to be the same thickness as the workpiece 1 or thinner than the workpiece 1. In the first embodiment, the frame 6 is made of metal, for example, SUS.

[0026] In the first embodiment, the first sheet 11 and the second sheet 12 are both formed into a sheet shape and size that fully covers the opening 9 of the frame 6 and does not protrude from the outer periphery of the frame 6. The first sheet 11 and the second sheet 12 are formed into a circular sheet shape that is, for example, larger than the outer diameter of the workpiece 1, larger than the inner diameter of the opening 9 of the frame 6, and smaller than the outer diameter of the frame 6.

[0027] In the first fixing step 111, first, the workpiece 1 and the frame 6 are placed so that the workpiece 1 is located at the center of the opening 9 of the frame 6, and the surface of the first sheet 11 is placed in contact with one surface 2, 7 of each of the workpiece 1 and the frame 6. In the first embodiment, the workpiece 1 and the frame 6 are placed on a holding table (not shown) with one surface 2, 7 exposed upward, and the first sheet 11 is placed on one surface 2, 7 of each of the workpiece 1 and the frame 6, but the present invention is not limited to this, and the first sheet 11 may be placed on a holding table (not shown), and the workpiece 1 and the frame 6 may be placed on the first sheet 11 with one surface 2, 7 facing the first sheet 11.

[0028] In a first fixing step 111, the first sheet 11 is then heated at a predetermined temperature (for example, 50 to 150° C. in the first embodiment) to soften it, while pressing the workpiece 1 and the frame 6 and the first sheet 11 in a direction to approach each other along the thickness direction with a predetermined pressing force (for example, 0.3 MPa or more in the first embodiment) for a predetermined time (for example, 30 seconds or more in the first embodiment), thereby thermocompression-bonding and fixing the first sheet 11 to one surfaces 2, 7 of the workpiece 1 and the frame 6, respectively. In this first fixing step 111, the first sheet 11 may be heated by a heat source provided inside a holding table (not shown) or inside a rectangular pressing member having a shape and size sufficient to cover the first sheet 11 in a plan view, while pressing the first sheet 11 with this pressing member, thereby thermocompression-bonding it. In addition, in this first fixing step 111, while heating the first sheet 11 with a heat source provided inside a holding table (not shown) or inside a pressing roller (not shown), a pressing roller (not shown) may be rotated and moved from one end on one surface 7 of the frame 6 through one surface 2 of the workpiece 1 to the other end on one surface 7 of the frame 6 to press the first sheet 11, thereby thermocompression bonding. In addition, in the first fixing step 111, at least one of the first sheet 11, the workpiece 1, the frame 6, and the holding table may be heated by infrared rays.

[0029] Alternatively, in this first fixing step 111, a roller (not shown) may be rotated and moved from one end on one side 7 of the frame 6 through the first sheet 11, over one side 2 of the workpiece 1, to the other end on one side 7 of the frame 6, thereby bringing the first sheet 11 into close contact with the workpiece 1 and one side 2, 7 of the frame 6, and then hot air at a predetermined temperature (for example, 150°C or higher in embodiment 1) may be blown from the side of the first sheet 11 using an industrial dryer to heat and soften the first sheet 11, and the softened first sheet 11 may be fixed by thermocompression to the workpiece 1 and one side 2, 7 of the frame 6, without pressing the first sheet 11 against the workpiece 1 and the frame 6, i.e., with a pressing force of 0 MPa.

[0030] In the first embodiment, the first fixing step 111 is performed while suppressing the first sheet 11 from loosening in the thickness direction in an annular region (hereinafter referred to as annular region) between the outer periphery 4 of the workpiece 1 and the inner periphery forming the opening 9 of the frame 6. This makes it possible to more reliably fix the first sheet 11 and the second sheet 12 in the annular region with a gap therebetween so that they do not come into contact with each other after performing the second fixing step 112 described later.

[0031] In the second fixing step 112, first, the second sheet 12 is placed in contact with the other surfaces 3, 8 of the workpiece 1 and the frame 6 opposite to the surfaces 2, 7 of the workpiece 1 and the frame 6 on which the first sheet 11 is thermocompression bonded. In the first embodiment, the first sheet 11 may be placed facing upward, or the second sheet 12 may be placed facing upward.

[0032] In the second fixing step 112, the second sheet 12 is then heated at a predetermined temperature (for example, 50 to 150° C. in the first embodiment) to soften it, while pressing the workpiece 1, the frame 6, and the second sheet 12 in a direction to approach each other along the thickness direction with a predetermined pressing force (for example, 0.3 MPa or more in the first embodiment) for a predetermined time (for example, 30 seconds or more in the first embodiment), thereby fixing the second sheet 12 to the other surfaces 3, 8 of the workpiece 1 and the frame 6 by thermocompression. The heating and pressing in the second fixing step 112 are performed in the same manner as the heating and pressing in the first fixing step 111. For example, in the second fixing step 112, at least one of the second sheet 12, the workpiece 1, the frame 6, and the holding table may be heated by a heat source provided inside a holding table or a pressing member (not shown), a heat source provided inside a pressing roller (not shown), or infrared rays. The second fixing step 112 is performed while preventing the first sheet 11, which has been fixed to the workpiece 1 and one surface 2, 7 of the frame 6 by thermocompression bonding in the first fixing step 111, from peeling off.

[0033] In the first embodiment, the second fixing step 112 is performed while suppressing slackening of the second sheet 12 in the thickness direction in the annular region, similar to the first fixing step 111. This makes it possible to more reliably fix the first sheet 11 and the second sheet 12 in the annular region with a gap therebetween so that they do not come into contact with each other.

[0034] In this manner, when the sheet fixing step 101 is performed, the first sheet 11 is fixed to one surface 2, 7 of each of the workpiece 1 and the frame 6, and the second sheet 12 is fixed to the other surface 3, 8 of each of the workpiece 1 and the frame 6, as shown in Fig. 2. In the first embodiment, in the first fixing step 111 of the sheet fixing step 101, the outer edge of the first sheet 11 is fixed to the frame 6, and in the second fixing step 112 of the sheet fixing step 101, the outer edge of the second sheet 12 is fixed to the frame 6, so that the first sheet 11 and the second sheet 12 can be fixed more reliably with a gap therebetween so that they do not come into contact with each other in the annular region.

[0035] Processing step 102 is a step of carrying out processing including at least one of processing, inspection, storage, and transportation of the workpiece 1 having the first sheet 11 and the second sheet 12 fixed to both sides thereof after the sheet fixing step 101. FIG. 3 is a cross-sectional view explaining laser processing, which is a first example of processing step 102 in FIG. 1. FIG. 4 is a cross-sectional view explaining expanding processing, which is a second example of processing step 102 in FIG. 1. FIG. 5 is a cross-sectional view explaining roller breaking processing, which is a third example of processing step 102 in FIG. 1.

[0036] In the first example of the processing step 102, as shown in FIG. 3, the laser irradiator 20 aligns the focal point 22 of the laser beam 21, which is transparent to the workpiece 1, with the inside of the workpiece 1 having the first sheet 11 and the second sheet 12 fixed on both sides, and irradiates the workpiece 1 with the laser beam 21. While irradiating the workpiece 1 with the laser beam 21, the workpiece 1 and the focal point 22 of the laser beam 21 are moved relatively along the planned dividing line by a driving source (not shown), thereby laser processing the workpiece 1 with the laser beam 21 to form a modified layer along the planned dividing line inside the workpiece 1. Here, the modified layer means a region in which the density, refractive index, mechanical strength, and other physical properties are different from those of the surroundings, and examples thereof include a melting processing region, a crack region, an insulation breakdown region, a refractive index change region, and a region in which these regions are mixed. Such a modified layer, together with a crack extending from the modified layer in the vertical direction of the workpiece 1, becomes a dividing starting point for dividing the workpiece 1.

[0037] In a first example of processing step 102, in embodiment 1, a laser beam 21 is irradiated onto the workpiece 1 through the second sheet 12 from the other side 3 side to which the second sheet 12 is fixed, but the present invention is not limited to this, and the laser beam 21 may also be irradiated onto the workpiece 1 through the first sheet 11 from the one side 2 side to which the first sheet 11 is fixed.

[0038] In addition, in the first example of processing step 102, in embodiment 1, a modified layer is formed inside the workpiece 1 by irradiating the workpiece 1 with a laser beam 21 that is transparent, but the present invention is not limited to this, and a so-called ablation process may be performed in which an absorbent laser beam 21 is irradiated onto the workpiece 1 to ablate (sublimate or evaporate) the workpiece 1, to form a laser-processed groove in the workpiece 1 that serves as the starting point for division, similar to the modified layer, or the workpiece 1 may be completely divided.

[0039] In the first embodiment, the second example of the processing step 102 is performed on the workpiece 1 in which a division starting point is formed along the planned division line, such as the workpiece 1 after the first example of the processing step 102 is performed. In the second example of the processing step 102, as shown in FIG. 4, the frame 6 is fixed from the outer periphery by the frame fixing part 31 of the expanding device 30, any surface of the workpiece 1 is placed on the holding table 32, and the holding table 32 and the push-up member 33 (expansion roller 34) are raised relatively to the frame fixing part 31 that fixes the frame 6 by a lifting unit (not shown), so that the annular regions of the first sheet 11 and the second sheet 12 are pressed in the thickness direction of the workpiece 1 by the expansion roller 34. Note that in the second example of the processing step 102, the first sheet 11 side may be pressed by the expansion roller 34, or the second sheet 12 side may be pressed by the expansion roller 34. As a result, in the second example of processing step 102, the workpiece 1 is divided from the division starting point by the tensile force generated as the first sheet 11 and the second sheet 12 expand in the planar direction.

[0040] In the first embodiment, the third example of the processing step 102 is performed on the workpiece 1 in which a division starting point is formed along the planned division line, such as the workpiece 1 after the first example of the processing step 102 is performed. In the third example of the processing step 102, as shown in Fig. 5, one of the surfaces of the workpiece 1 is placed on the holding surface 44 of the elastic member 43 provided on the upper surface of the table base 42 of the holding table 41 of the roller breaking device 40, and the pressing roller 45 rotates and moves from one end of the workpiece 1 to the other end while pressing downward from above against the workpiece 1 and the frame 6 held on the holding surface 44, via the second sheet 12 from the other surface 3 side of the workpiece 1 when the first sheet 11 side is placed on the holding surface 44, or from one surface 2 side of the workpiece 1 through the first sheet 11 when the second sheet 12 side is placed on the holding surface 44. As a result, in the third example of processing step 102, a pressing force is applied to the workpiece 1 by the pressing roller 45, and an elastic force generated in the elastic member 43 by the pressing by the pressing roller 45 is applied to the workpiece 1, thereby applying an external force to the workpiece 1 from both sides and dividing it starting from the division starting point.

[0041] In the processing step 102, the workpiece 1 may be cut together with the second sheet 12 from the other surface 3 side to which the second sheet 12 is fixed, by a cutting blade, to form a cutting groove in the workpiece 1, or to completely divide the workpiece 1. In addition, in the processing step 102, for the workpiece 1 in which a division starting point is formed along the planned division line, such as the workpiece 1 after the first example of the processing step 102 is performed, a breaking blade (not shown) positioned on the planned division line of the workpiece 1 through the first sheet 11 or the second sheet 12 may be pressed against the workpiece 1 to divide the workpiece 1 from the division starting point. In addition, in the processing step 102, the workpiece 1 may be inspected by irradiating the inside of the workpiece 1 in which the first sheet 11 and the second sheet 12 are fixed to both sides, for example, with inspection light that penetrates the first sheet 11 and the second sheet 12. In addition, in the processing step 102, the workpiece 1 may be stored in a cassette (not shown). In the processing step 102, the workpiece 1 may be indirectly held by suctioning the first sheet 11 or the second sheet 12 fixed to the workpiece 1 using a transport unit (not shown), or the workpiece 1 may be indirectly held by gripping the frame 6 attached to the workpiece 1. In the processing step 102, the workpiece 1 may be transported to another device, another factory, or the like with the first sheet 11 and the second sheet 12 fixed to both sides of the workpiece 1. In the processing step 102, the present invention is not limited to these, and any processing, inspection, storage, and transportation of the workpiece 1 that can be performed when the first sheet 11 and the second sheet 12 are fixed to both sides of the workpiece 1 may be performed.

[0042] The peeling step 103 is a step of peeling the first sheet 11 and the second sheet 12 from the workpiece 1 and the frame 6 after the processing step 102. FIGS. 6 and 7 are cross-sectional views for explaining the peeling step 103 in FIG. 1. In the first embodiment, the peeling step 103 first peels the second sheet 12 from the workpiece 1 and the frame 6 as shown in FIG. 6. Specifically, in the peeling step 103, the workpiece 1 and the frame 6 are suction-held from below by the holding table 51 via the first sheet 11, and the second sheet 12 is peeled from above. In the peeling step 103, the first sheet 11 is then peeled from the workpiece 1 and the frame 6 as shown in FIG. 7. Specifically, in the peeling step 103, the workpiece 1 and the frame 6 are suction-held from below by the holding table 51, and the first sheet 11 is peeled from above. In addition, in the peeling step 103, either the first sheet 11 or the second sheet 12 may be peeled off first from the workpiece 1. In addition, in the peeling step 103, after peeling off either the first sheet 11 or the second sheet 12, processing or inspection similar to that in the processing step 102 may be performed, and then the other of the first sheet 11 or the second sheet 12 may be peeled off.

[0043] The method for processing a workpiece of embodiment 1 having the above-mentioned configuration provides a gap in the annular region (annular region) between the outer periphery 4 of the workpiece 1 and the inner circumference forming the opening 9 of the frame 6 so that the first sheet 11 fixed to one surface 2, 7 and the second sheet 12 fixed to the other surface 3, 8 do not come into contact with each other. This prevents the first sheet 11 and the second sheet 12 from being thermocompressed together and integrated when the first sheet 11 and the second sheet 12 are thermocompressed, thereby achieving the effect of allowing the first sheet 11 and the second sheet 12 to be easily peeled off even when the first sheet 11 and the second sheet 12 are fixed to both surfaces of the workpiece 1.

[0044] Furthermore, in the method for processing a workpiece according to the first embodiment, the outer edge of the first sheet 11 and the outer edge of the second sheet 12 are fixed to the frame 6 in the sheet fixing step 101, thereby fixing the first sheet 11 and the second sheet 12 with a gap between them in the annular region. Therefore, the method for processing a workpiece according to the first embodiment can more reliably fix the first sheet 11 and the second sheet 12 with a gap between them so that they do not contact each other in the annular region.

[0045] Furthermore, in the method for processing the workpiece according to embodiment 1, the first sheet 11 and the second sheet 12 are made of either polyolefin, polyethylene, polypropylene, or polystyrene, so they do not have an adhesive layer, and can be preferably fixed to the surface of the workpiece 1 by thermocompression bonding through heating.

[0046] [Embodiment 2] A method for processing a workpiece according to a second embodiment of the present invention will be described. Fig. 8 is a cross-sectional view for explaining a sheet fixing step 101 of the method for processing a workpiece according to the second embodiment. Figs. 9 and 10 are both cross-sectional views for explaining a peeling step 103 of the method for processing a workpiece according to the second embodiment. In Figs. 8, 9, and 10, the same parts as those in the first embodiment are denoted by the same reference numerals, and the description thereof will be omitted.

[0047] The method for processing a workpiece according to the second embodiment is obtained by modifying the sheet fixing step 101 in the method for processing a workpiece according to the first embodiment, and modifying the peeling step 103 accordingly. The sheet fixing step 101 in the method for processing a workpiece according to the second embodiment is obtained by modifying the sheet fixing step 101 in the method for processing a workpiece according to the first embodiment so that a peeling member 13 (see FIG. 8) is disposed between the first sheet 11 and the second sheet 12 in the annular region, and the other configurations are the same as those in the first embodiment.

[0048] In the sheet fixing step 101 of the workpiece processing method according to the embodiment 2, the first fixing step 111 is the same as that of the embodiment 1. The second fixing step 112 of the embodiment 2 is modified such that, in the second fixing step 112 of the embodiment 1, before the second sheet 12 is placed in contact with the other surfaces 3, 8 of the workpiece 1 and the frame 6 to which the first sheet 11 is thermocompression-bonded, an annular peeling member 13 is placed in the annular region, and then the second sheet 12 is placed so as to sandwich the peeling member 13 between the first sheet 11 and the second sheet 12.

[0049] Here, the peeling member 13 used in the sheet fixing step 101 of the workpiece processing method according to the second embodiment is formed in a plate shape and is formed in an annular shape with an inner diameter slightly larger than the outer diameter of the workpiece 1 and an outer diameter slightly smaller than the inner diameter of the opening 9 of the frame 6. Therefore, the peeling member 13 can be arranged in an annular region with the workpiece 1 arranged on the inner periphery side and the frame 6 arranged on the outer periphery side. In the second embodiment, the peeling member 13 is formed to have a thickness approximately equal to that of the workpiece 1 and the frame 6 as shown in FIG. 8, but the present invention is not limited to this, and the peeling member 13 may be formed to be thinner than the workpiece 1 and the frame 6. In the second embodiment, the peeling member 13 may be formed of any material as long as it is not integrated with the first sheet 11 and the second sheet 12 by thermocompression bonding, and is formed of a material different from the first sheet 11 and the second sheet 12, and examples of the material include a sheet made of polyethylene terephthalate (PET) and a sheet of any material coated with a fluororesin. Moreover, the peeling member 13 may not have a sheet, and may be configured by coating at least one of the first sheet 11 and the second sheet 12 in a circular region with a fluororesin coating agent.

[0050] In this manner, when the sheet fixing step 101 of the second embodiment is performed, the first sheet 11 is fixed to one surface 2, 7 of each of the workpiece 1 and the frame 6, the second sheet 12 is fixed to the other surface 3, 8 of each of the workpiece 1 and the frame 6, and an annular peeling member 13 is disposed between the first sheet 11 and the second sheet 12 in the annular region, as shown in Fig. 8. In the second embodiment, by disposing the annular peeling member 13 between the first sheet 11 and the second sheet 12 in the annular region in the sheet fixing step 101, the first sheet 11 and the second sheet 12 can be more reliably fixed with a gap therebetween so that they do not come into contact with each other in the annular region by the peeling member 13.

[0051] The peeling step 103 of the method for treating a workpiece according to the second embodiment is the same as that of the first embodiment, except that in the peeling step 103 of the method for treating a workpiece according to the first embodiment, a peeling member 13 is disposed between the first sheet 11 and the second sheet 12 in the annular region before the first sheet 11 and the second sheet 12 are peeled off from above. Specifically, in the peeling step 103 of the second embodiment, first, as shown in FIG. 9, the workpiece 1, the frame 6, and the peeling member 13 are sucked and held from below by the holding table 51 via the first sheet 11, and the second sheet 12 is peeled off from above, and then, as shown in FIG. 10, the workpiece 1, the frame 6, and the peeling member 13 are sucked and held from below by the holding table 51, and the first sheet 11 is peeled off from above. Note that in the peeling step 103 of the second embodiment, either the first sheet 11 or the second sheet 12 may be peeled off from the workpiece 1 first.

[0052] The method for processing a workpiece according to the second embodiment having the above-mentioned configuration is modified so that a peeling member 13 (see FIG. 8) is disposed between the first sheet 11 and the second sheet 12 in the annular region in the sheet fixing step 101. Therefore, the method for processing a workpiece according to the second embodiment can more reliably fix the first sheet 11 and the second sheet 12 with a gap therebetween so that they do not come into contact with each other by the peeling member 13, thereby achieving the advantageous effect that the first sheet 11 and the second sheet 12 can be easily peeled off even when the first sheet 11 and the second sheet 12 are fixed to both sides of the workpiece 1.

[0053] [Embodiment 3] A method for processing a workpiece according to embodiment 3 of the present invention will be described. Fig. 11 is a cross-sectional view for explaining a sheet fixing step 101 of the method for processing a workpiece according to embodiment 3. In Fig. 11, the same parts as those in embodiments 1 and 2 are denoted by the same reference numerals, and the description thereof will be omitted.

[0054] The method for processing a workpiece according to the third embodiment is the same as the method for processing a workpiece according to the second embodiment except that the sheet fixing step 101 is changed and the peeling step 103 is accordingly changed. The other configurations are the same as those of the second embodiment.

[0055] The sheet fixing step 101 of the method for treating a workpiece according to the third embodiment is a modification of the sheet fixing step 101 of the method for treating a workpiece according to the second embodiment, in which, in the second fixing step 112, the surface of the second sheet 12 is placed in contact with the other surface 3 of the workpiece 1 to which the first sheet 11 is thermocompression-bonded and the surface of the peeling member 13, and then thermocompression-bonded, instead of the surface of the second sheet 12 being placed in contact with the other surface 3 of the workpiece 1 to which the first sheet 11 is thermocompression-bonded and the surface of the peeling member 13, and then thermocompression-bonded. In this modification, the shape and size of the second sheet 12 are changed to a shape and size that sufficiently covers the outer periphery 4 of the workpiece 1 but does not reach the opening 9 of the frame 6, for example, a circle that is larger than the outer diameter of the workpiece 1 and smaller than the inner diameter of the opening 9 of the frame 6.

[0056] In this modification, the shape and size of the second sheet 12 to be peeled off in the peeling step 103 of the method for treating a workpiece according to embodiment 3 is changed from that in the peeling step 103 of the method for treating a workpiece according to embodiment 2. In the peeling step 103 of the method for treating a workpiece according to embodiment 3, since the second sheet 12 is smaller than the first sheet 11, it is preferable to peel the second sheet 12 off the workpiece 1 before the first sheet 11.

[0057] The method for processing a workpiece of embodiment 3 having the above-mentioned configuration is the method for processing a workpiece of embodiment 2 in which the shape and size of the second sheet 12 that is thermocompression bonded to the other surface 3 of the workpiece 1 is made smaller, and therefore has the same effect as the method for processing a workpiece of embodiment 2.

[0058] [Embodiment 4] A method for processing a workpiece according to embodiment 4 of the present invention will be described. Fig. 12 is a cross-sectional view for explaining a sheet fixing step 101 of the method for processing a workpiece according to embodiment 4. Figs. 13 and 14 are both cross-sectional views for explaining a peeling step 103 of the method for processing a workpiece according to embodiment 4. In Figs. 12, 13, and 14, the same parts as those in embodiments 1 to 3 are denoted by the same reference numerals, and the description thereof will be omitted.

[0059] The method for processing a workpiece according to the fourth embodiment is the same as the method for processing a workpiece according to the first embodiment except that the sheet fixing step 101 is changed and the peeling step 103 is accordingly changed. The other configurations are the same as those of the first embodiment.

[0060] The sheet fixing step 101 of the method for processing a workpiece according to the fourth embodiment is a modification of the sheet fixing step 101 of the method for processing a workpiece according to the first embodiment, in which the second sheet 12 is placed in contact with the other surface 3 of the workpiece 1 to which the first sheet 11 is thermocompressed and then thermocompressed, instead of being placed in contact with the other surface 3 of the workpiece 1 to which the first sheet 11 is thermocompressed and then thermocompressed, in the second fixing step 112. In this modification, the shape and size of the second sheet 12 are changed to be the same as the outer periphery 4 (outer edge) of the workpiece 1 in a plan view within a predetermined error range. In the fourth embodiment, since the second sheet 12 does not protrude from the outer periphery 4 (outer edge) of the workpiece 1 in this way, the first sheet 11 and the second sheet 12 can be more reliably fixed in the annular region with a gap therebetween so that they do not come into contact with each other.

[0061] In making this change, the shape and size of the second sheet 12 to be peeled off is changed in peeling step 103 of the method for treating a workpiece according to embodiment 4 from that in embodiment 1. In peeling step 103 of the method for treating a workpiece according to embodiment 4, since the second sheet 12 is smaller than the first sheet 11, it is preferable to peel the second sheet 12 off the workpiece 1 before the first sheet 11 as shown in Fig. 13, and then peel the first sheet 11 off the workpiece 1 as shown in Fig. 14.

[0062] The method for processing a workpiece of embodiment 4 having the above-mentioned configuration is the method for processing a workpiece of embodiment 1, except that the shape and size of the second sheet 12 that is thermocompression bonded to the other surface 3 of the workpiece 1 is changed to be the same as the outer periphery 4 (outer edge) of the workpiece 1, and therefore has the same effect as the method for processing a workpiece of embodiment 1.

[0063] [Embodiment 5] A method for processing a workpiece according to embodiment 5 of the present invention will be described. Fig. 15 is a cross-sectional view for explaining a sheet fixing step 101 of the method for processing a workpiece according to embodiment 5. Figs. 16, 17, and 18 are all cross-sectional views for explaining a peeling step 103 of the method for processing a workpiece according to embodiment 5. In Figs. 15, 16, 17, and 18, the same parts as those in embodiments 1 to 4 are designated by the same reference numerals, and the description thereof will be omitted.

[0064] The method for processing a workpiece according to the fifth embodiment is obtained by modifying the sheet fixing step 101 and the peeling step 103 in the method for processing a workpiece according to the first embodiment.

[0065] The sheet fixing step 101 of the workpiece processing method according to the fifth embodiment is a modification of the sheet fixing step 101 of the workpiece processing method according to the first embodiment, in which the first sheet 11 and the second sheet 12 do not need to be fixed with a gap that prevents them from contacting each other in the annular region. If the first sheet 11 and the second sheet 12 are not thermocompressed to each other in the annular region in the sheet fixing step 101 of the fifth embodiment, the peeling step 103 is the same as in the first embodiment. On the other hand, if the first sheet 11 and the second sheet 12 are thermocompressed to each other in the annular region in the sheet fixing step 101 of the fifth embodiment, as shown in FIG. 15, the peeling step 103 is modified from that of the first embodiment.

[0066] In embodiment 5, when the first sheet 11 and the second sheet 12 are thermally pressed together in the annular region in the sheet fixing step 101, in the peeling step 103, at least one of the first sheet 11 or the second sheet 12 is cut along the outer periphery 4 of the workpiece 1, and then the first sheet 11 and the second sheet 12 are removed from the workpiece 1 and the frame 6.

[0067] In the fifth embodiment, when the first sheet 11 and the second sheet 12 are thermocompression bonded to each other in the annular region in the sheet fixing step 101, the peeling step 103 specifically includes first cutting the second sheet 12 along the outer periphery 4 of the workpiece 1 by a laser irradiator 60 as shown in Fig. 16. In the peeling step 103, a focus point 62 of a laser beam 61 absorbent for the second sheet 12 is aligned with the upper surface of the second sheet 12, and the laser beam 61 is irradiated while the second sheet 12 and the focus point 62 of the laser beam 61 are moved relatively along the outer periphery 4 of the workpiece 1 by a driving source (not shown), thereby ablation processing the second sheet 12 along the outer periphery 4 of the workpiece 1 with the laser beam 61, thereby cutting an inner periphery 12-1 of the second sheet 12 inside the outer periphery 4 of the workpiece 1 and an outer periphery 12-2 of the second sheet 12 outside the outer periphery 4 of the workpiece 1. The cutting position of the second sheet 12 is not limited to the outer periphery 4 of the workpiece 1, and may be outside or inside the outer periphery 4 of the workpiece 1. In the peeling step 103, the inner periphery 12-1 of the first sheet 11 and the second sheet 12, which are thermocompression-bonded to each other, is separated from the first sheet 11 and the outer periphery 12-2, which are thermocompression-bonded to each other. In the fifth embodiment, the second sheet 12 is cut into the inner periphery 12-1 and the outer periphery 12-2 by the laser beam 61, but the present invention is not limited to this, and the second sheet 12 may be cut into the inner periphery 12-1 and the outer periphery 12-2 by other means such as a cutter or a cutting blade. In addition, not only the second sheet 12 but also the first sheet 11 may be cut.

[0068] In the fifth embodiment, next, in the peeling step 103, as shown in Fig. 17, the workpiece 1 and frame 6 are suction-held from below by the holding table 51 via the first sheet 11, and the inner peripheral portion 12-1 is peeled off from the workpiece 1 from above. In the peeling step 103, then, as shown in Fig. 18, the workpiece 1 and frame 6 are suction-held from below by the holding table 51, and the first sheet 11 and the outer peripheral portion 12-2 are peeled off from the workpiece 1 and frame 6 from above.

[0069] In embodiment 5, in sheet fixing step 101, only the first sheet 11 is thermocompression bonded to the frame 6, and in peeling step 103, the second sheet 12 is cut into an inner periphery 12-1 and an outer periphery 12-2, the inner periphery 12-1 of the second sheet 12 is peeled off, and then the first sheet 11 and the outer periphery 12-2 of the second sheet 12 are peeled off; however, the present invention is not limited to this, and it is also possible that in sheet fixing step 101, only the second sheet 12 is thermocompression bonded to the frame 6, and in peeling step 103, the first sheet 11 is cut into an inner periphery 12-1 and an outer periphery 12-2, the inner periphery of the first sheet 11 is peeled off, and then the second sheet 12 and the outer periphery of the first sheet 11 are peeled off.

[0070] The method for processing a workpiece of embodiment 5 having the above-mentioned configuration has the effect that even if the first sheet 11 fixed to one surface 2, 7 and the second sheet 12 fixed to the other surface 3, 8 are thermocompressed together and integrated in the annular region (annular region) between the outer periphery 4 of the workpiece 1 and the inner circumference forming the opening 9 of the frame 6, in the peeling step 103, at least one of the first sheet 11 or the second sheet 12 is cut along the outer periphery 4 of the workpiece 1, and then the first sheet 11 and the second sheet 12 are removed from the workpiece 1 and the frame 6, even if the first sheet 11 and the second sheet 12 are fixed to both sides of the workpiece 1, the first sheet 11 and the second sheet 12 can be easily peeled off.

[0071] It should be noted that the present invention is not limited to the above-described embodiment, and various modifications can be made without departing from the gist of the present invention. [Explanation of symbols]

[0072] 1 Workpiece 2,7 One side 3,8 The other side 4. Outer circumference 6 Frames 9 aperture 11 Sheet 1 12 2nd Sheet 13 Peeling member 101 Seat fixing step 102 Processing Steps 103 Peeling step 111 First Fixation Step 112 Second Fixation Step

Claims

1. A method for processing a workpiece, comprising a sheet fixing step of fixing a first sheet made of a thermoplastic resin having no adhesive layer to one surface of the workpiece, and fixing a second sheet made of a thermoplastic resin having no adhesive layer to the other surface of the workpiece, The sheet fixing step includes: a first fixing step of fixing the first sheet by thermocompression to one surface of the workpiece and a frame that accommodates the workpiece in a central opening; a second fixing step of fixing the second sheet to the other surface of the workpiece by thermocompression; having A processing step of performing a process including at least one of processing, inspection, storage, and transportation of the workpiece after the sheet fixing step; a peeling step of peeling the first sheet and the second sheet from the workpiece and the frame after the processing step; Equipped with A method for processing a workpiece, characterized in that in the sheet fixing step, the first sheet and the second sheet are fixed to each other with a gap in the area between the outer periphery of the workpiece and the inner periphery of the frame.

2. The method for processing a workpiece as described in claim 1, characterized in that in the sheet fixing step, the outer edge of the first sheet and the outer edge of the second sheet are fixed to the frame, thereby fixing the first sheet and the second sheet with a gap between them in the area between the outer periphery of the workpiece and the inner periphery of the frame.

3. 2. The method for processing a workpiece according to claim 1, wherein in the sheet fixing step, a peeling member is disposed between the first sheet and the second sheet in the region between the outer periphery of the workpiece and the inner periphery of the frame.

4. 2. The method of claim 1, wherein in said sheet fixing step, said second sheet is conformal to an outer edge of said workpiece.

5. A method for processing a workpiece, comprising a sheet fixing step of fixing a first sheet made of a thermoplastic resin having no adhesive layer to one surface of the workpiece, and fixing a second sheet made of a thermoplastic resin having no adhesive layer to the other surface of the workpiece, The sheet fixing step includes: a first fixing step of fixing the first sheet by thermocompression to one surface of the workpiece and a frame that accommodates the workpiece in a central opening; a second fixing step of fixing the second sheet to the other surface of the workpiece by thermocompression; having A processing step of performing a process including at least one of processing, inspection, storage, and transportation of the workpiece after the sheet fixing step; a peeling step of peeling the first sheet and the second sheet from the workpiece and the frame after the processing step; Equipped with The method for processing a workpiece is characterized in that the peeling step includes cutting at least one of the first sheet or the second sheet along the outer periphery of the workpiece, and then removing the first sheet and the second sheet from the workpiece and the frame.

6. 6. The method for treating a workpiece according to claim 1, wherein the first sheet and the second sheet are made of any one of polyolefin, polyethylene, polypropylene, and polystyrene.

Citation Information

Patent Citations

  • Breaking device

    JP2013058671A

  • Method for fabricating plate-like object

    JP2020077812A

  • Processing method for wafer

    JP2021077684A