Film-covered transparent base plate and top plate for cooking device
By applying a light absorbing film on a transparent substrate, the combination of dielectric phase and metal phase absorbs light evenly within the visible light range, solving the problem of aesthetics and information display when the light source is turned off, and the information is clearly displayed when the light source is turned on without affecting the aesthetics.
Patent Information
- Application Number
- JP2024127630
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-07-01
- Filing Date
- 2024-08-02
- Publication Date
- 2024-10-23
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the prior art, although the use of a black glass roof can hide the internal structure of the cooking equipment, when the light source is turned on, the display information is difficult to clearly view, and the aesthetics are affected.
A light absorbing film is coated on a transparent substrate. The light absorbing film is composed of a dielectric phase and a metal phase with a band gap of 2.0 eV or more. The dielectric phase is preferably a metal oxide. The light absorbs uniformly within the visible light range through the combination of the dielectric phase and the metal phase, ensuring that the top plate appears colorless black when the light source is closed.
It realizes the beauty of maintaining the light source when it is turned off, and the information can be clearly displayed when the light source is turned on without affecting the beauty.
Smart Images

Figure 2024150747000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a film-coated transparent substrate and a top plate for a cooking appliance using the film-coated transparent substrate. [Background technology]
[0002] Conventionally, in cooking appliances such as electromagnetic cookers, radiant heater cookers, and gas cookers, a top plate made of black glass or transparent glass with a black coating is used to conceal the internal structure of the cooker. In such cooking appliances, a combination of LEDs (Light Emitting Diodes), liquid crystal displays, or liquid crystal displays with touch panel functions is sometimes used to display various information such as the power supply and heating state on the top plate.
[0003] The following Patent Document 1 discloses a top plate for a cooking device, which includes a glass plate, an inorganic pigment layer provided on the glass plate, and an indication layer provided on the inorganic pigment layer. The inorganic pigment layer contains a pigment and glass. The indication layer has a transparent resin part that transmits LED light and the like, and a heat-resistant resin part that blocks the LED light and the like. In Patent Document 1, letters, numbers, symbols, and the like are displayed by changing the shape of the transmitting part that transmits the LED light and the like, or by transmitting patterned light in the transmitting part. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2014-215018 A Summary of the Invention [Problem to be solved by the invention]
[0005] Incidentally, when an LED, a liquid crystal display, or a liquid crystal display with a touch panel function is combined with a top plate for a cooking appliance, it is required that various information be clearly visible when the light source is turned on, and that the internal structure of the cooking appliance be concealed when the light source is turned off. However, when a black-colored glass substrate is used as the top plate, although it is possible to conceal the internal structure of the cooking appliance when the light source is turned off, there is a problem that various information is difficult to see when the light source is turned on.
[0006] In regard to this point, in Patent Document 1, a black inorganic pigment layer is provided in the display area as well, thereby attempting to conceal the internal structure of the cooking appliance. However, when a black inorganic pigment layer is provided as in the top plate of Patent Document 1, the color does not become achromatic black when the light source is turned off, and aesthetics may be impaired.
[0007] An object of the present invention is to provide a film-coated transparent substrate that has excellent aesthetic appearance even when a light source is turned off, and a top plate for a cooking appliance that uses the film-coated transparent substrate. [Means for solving the problem]
[0008] The film-coated transparent substrate of the present invention comprises a transparent substrate and a light-absorbing film provided on one main surface of the transparent substrate, and is characterized in that the light-absorbing film includes a dielectric phase composed of a material having a band gap of 2.0 eV or more and 2.7 eV or less, and a metal phase.
[0009] In the present invention, the material is preferably a metal oxide.
[0010] In the present invention, it is preferable that the standard Gibbs energy of the metal element constituting the metal oxide is smaller than the standard Gibbs energy of the metal element constituting the metal phase in the Ellingham diagram.
[0011] In the present invention, the average absorption coefficient of the light absorbing film at wavelengths of 400 nm to 700 nm is 0.5 μm-1 Above, 80μm -1 It is preferable that:
[0012] In the present invention, in the light absorbing film, when the absorption coefficient at a wavelength of 436 nm is α1, the absorption coefficient at a wavelength of 546 nm is α2, and the absorption coefficient at a wavelength of 700 nm is α3, it is preferable that α1 / α2 is 0.8 or more and 2.0 or less, and α3 / α2 is 0.8 or more and 2.0 or less.
[0013] In the present invention, it is preferable that in the light absorbing film, the α1 / α2 is 0.8 or more and 1.25 or less, and the α3 / α2 is 0.8 or more and 1.25 or less.
[0014] In the present invention, the light absorbing film has an absorption coefficient at a wavelength λ of α λ The average absorption coefficient in the wavelength range of 400 nm to 700 nm is α AVE In this case, it is preferable that the absorption mean deviation M represented by the following formula (1) is 0.30 or less.
[0015]
number
[0016] In the present invention, it is preferable that a dielectric multilayer film is further provided on the light absorbing film.
[0017] In the present invention, it is preferable that the dielectric multilayer film is a laminate film in which high-refractive index films having a relatively high refractive index and low-refractive index films having a relatively low refractive index are alternately laminated, and that the high-refractive index films are the light-absorbing films.
[0018] The top plate for a cooking appliance according to the present invention comprises a film-coated transparent substrate constructed according to the present invention, the transparent substrate having a cooking surface on which a cooking utensil is placed and a back surface opposite the cooking surface, and the light-absorbing film is provided on the back surface of the transparent substrate. Effect of the Invention
[0019] According to the present invention, it is possible to provide a film-coated transparent substrate that has excellent aesthetic appearance even when the light source is turned off, and a top plate for a cooking appliance that uses the film-coated transparent substrate. [Brief description of the drawings]
[0020] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a film-coated transparent substrate according to a first embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing, in an enlarged scale, a light absorbing film constituting the film-coated transparent substrate according to the first embodiment of the present invention. [Diagram 3] FIG. 3 is a diagram showing an example of an Ellingham diagram of a metal and a metal oxide. [Figure 4] FIG. 4 is a schematic cross-sectional view showing a film-coated transparent substrate according to the second embodiment of the present invention. [Diagram 5] FIG. 5 is a schematic cross-sectional view showing a film-coated transparent substrate according to a third embodiment of the present invention. [Figure 6] FIG. 6 is a schematic cross-sectional view showing a film-coated transparent substrate according to a fourth embodiment of the present invention. [Figure 7] FIG. 7 is a schematic cross-sectional view showing a top plate for a cooker according to one embodiment of the present invention. [Figure 8] FIG. 8 is a diagram showing the absorption coefficient of the light absorbing film prepared in the example. [Figure 9] FIG. 9 is a diagram showing the absorption coefficient of the light absorbing film produced in the comparative example. [Figure 10] FIG. 10 is a diagram showing the absorption coefficients of the light-absorbing films produced in Examples 1 and 3 to 6 and Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Preferred embodiments will be described below. However, the following embodiments are merely examples, and the present invention is not limited to the following embodiments. In addition, in each drawing, components having substantially the same functions may be referred to by the same reference numerals.
[0022] [Transparent substrate with film] (First embodiment) Fig. 1 is a schematic cross-sectional view showing a film-coated transparent substrate according to a first embodiment of the present invention, and Fig. 2 is a schematic cross-sectional view showing, in an enlarged manner, a light-absorbing film constituting the film-coated transparent substrate according to the first embodiment of the present invention.
[0023] 1, the film-coated transparent substrate 1 includes a transparent substrate 2 and a light-absorbing film 3. The transparent substrate 2 has a first main surface 2a and a second main surface 2b that face each other. The light-absorbing film 3 is provided on the first main surface 2a of the transparent substrate 2.
[0024] In this embodiment, the transparent substrate 2 has a substantially rectangular plate shape. However, the transparent substrate 2 may have a substantially circular plate shape, and the shape is not particularly limited.
[0025] The transparent substrate 2 transmits light with a wavelength of 400 nm to 700 nm. The transparent substrate 2 may be colored and transparent, but is preferably colorless and transparent from the viewpoint of further enhancing aesthetics. In this specification, "transparent" means that the light transmittance in the visible wavelength range of 400 nm to 700 nm is 80% or more. Also, "colorless" means that the saturation of the transmitted light when irradiated with a D65 light source is 2 or less.
[0026] In this embodiment, the transparent substrate 2 is made of glass, although the transparent substrate 2 may be made of other materials such as ceramics as long as it is a transparent substrate.
[0027] The glass constituting the transparent substrate 2 is preferably made of glass with a high glass transition temperature and low expansion, or low expansion crystallized glass. A specific example of low expansion crystallized glass is "N-0" manufactured by Nippon Electric Glass Co., Ltd. The transparent substrate 2 may be made of borosilicate glass, alkali-free glass, aluminosilicate glass, or the like. In this case, the heat resistance of the transparent substrate 2 can be further improved, and the thermal expansion coefficient can be further reduced. Therefore, the transparent substrate 2 can be suitably used for applications such as top plates for cookware where heating and cooling are repeated.
[0028] There is no particular limitation on the thickness of the transparent substrate 2. The thickness of the transparent substrate 2 can be appropriately set depending on the light transmittance, etc. The thickness of the transparent substrate 2 can be, for example, about 0.035 mm to 5 mm.
[0029] The light absorbing film 3 is provided on the first main surface 2a of the transparent substrate 2. As shown in FIG. 2, the light absorbing film 3 has a dielectric phase 4 and a metal phase 5. In this embodiment, the dielectric phase 4 is a matrix, and the metal phase 5 is dispersed in the matrix of the dielectric phase 4. However, the metal phase 5 may be exposed on the surface of the dielectric phase 4. In addition, the dielectric phase 4 and the metal phase 5 may simply be mixed, and the form of the mixture is not particularly limited. As long as a conductive path is not formed by the metal phase 5 throughout the entire light absorbing film 3, the metal phases 5 may be partially in contact with each other, and the size of the metal phase 5 may not be uniform. Such a structure can be appropriately adjusted, for example, by the charge ratio of the materials constituting the dielectric phase 4 and the metal phase 5.
[0030] The method for forming the light absorbing film 3 is not particularly limited, but may be, for example, a physical vapor deposition method (PVD method), such as a sputtering method, a pulsed laser deposition method (PLD) or an evaporation method.
[0031] In this embodiment, the dielectric phase 4 is composed of a material having a band gap of 2.0 eV or more and 2.7 eV or less. In particular, the dielectric phase 4 is preferably composed of a metal oxide having a band gap of 2.0 eV or more and 2.7 eV or less. However, the dielectric phase 4 may be composed of a metal oxynitride or metal nitride having a band gap of 2.0 eV or more and 2.7 eV or less. The band gap can be calculated, for example, from a Tauc plot.
[0032] Examples of metal oxides with a band gap of 2.0 eV or more and 2.7 eV or less include Bi2O3 (2.5 eV), Fe2O3 (2.1 eV), Fe3O4 (2.0 eV), V2O5 (2.3 eV), WO3 (2.5 eV), MoO3 (2.7 eV), and Cr2O3 (2.6 eV). However, composite oxides such as BiVO4 (2.3 eV) containing these cations may also be used. Examples of metal oxynitrides with a band gap of 2.0 eV or more and 2.7 eV or less include SrTaO2N, TiO 2-x N x etc.
[0033] The metal constituting the metal phase 5 is not particularly limited, and examples thereof include Au, Ag, Cu, Pt, Pd, Rh, Zn, Fe, Sn, Ni, and Pb. The metal phase 5 may be made of an alloy of these metals. Examples of the alloy include FeNi and CuNi.
[0034] The film-coated transparent substrate 1 according to this embodiment is characterized in that the light absorbing film 3 provided on the first main surface 2a of the transparent substrate 2 is composed of a dielectric phase 4 having a band gap of 2.0 eV or more and 2.7 eV or less, and a metal phase 5. This allows various information to be displayed clearly when the light source is turned on, and provides an excellent aesthetic appearance when the light is turned off. This can be explained as follows.
[0035] Conventionally, when a black-colored glass substrate is used for a substrate such as a top plate for a cooker, the internal structure of the cooker can be concealed when the light source such as an LED or liquid crystal display is turned off, but when the light source is turned on, various pieces of information are difficult to see. On the other hand, when a black inorganic pigment layer is provided on a transparent substrate such as a glass substrate, the color does not become achromatic black when the light source is turned off, and the aesthetic appearance may be impaired.
[0036] In this regard, conventional top plates had a problem in that the material that constitutes the inorganic pigment layer strongly absorbs the short wavelength side of visible light (purple and blue sides; high light energy) and weakly absorbs the long wavelength side (red side; low light energy), and therefore does not produce an achromatic black color.
[0037] In contrast, in the light absorbing film 3 of this embodiment, light absorption on the short wavelength side of visible light is carried out by light absorption due to the band gap of the dielectric phase 4, and light absorption on the long wavelength side is carried out by light absorption by free electrons in the metallic phase 5. Therefore, the top plate remains achromatic black even when the light is turned off, and has excellent aesthetic appearance.
[0038] More specifically, the absorption coefficient α(λ) that depends on the wavelength of light is expressed by the following formula (I).
[0039] α(λ)=α(λ) バンドギャップ型 +α(λ) 自由電子型 =A λ -n +B·λ 2 ≒C λ 0 ... Formula (I) (In formula (I), A, B, and C are constants, and n>0.)
[0040] In other words, the absorption coefficient due to the band gap of the dielectric phase 4, which is responsible for absorbing light on the short wavelength side of visible light, is proportional to the nth power of the inverse of the wavelength, and the absorption coefficient due to free electrons in the metallic phase 5, which is responsible for absorbing light on the long wavelength side, is proportional to the square of the wavelength. Therefore, the absorption coefficient α(λ) of the light absorbing film 3, which is expressed as the sum of these, is generally independent of wavelength and tends to be a constant value at any wavelength.
[0041] In this way, the film-coated transparent substrate 1 having the light absorbing film 3 can uniformly absorb light, particularly in almost the entire visible light range. Therefore, the film-coated transparent substrate 1 can be achromatic black when the light source is turned off, and has excellent aesthetic appearance. Therefore, the film-coated transparent substrate 1 can be suitably used for applications such as a top plate for a cooking device and a cover glass for a display.
[0042] In the present invention, the band gap of the dielectric phase 4 is preferably 2.5 eV or less, and more preferably 2.3 eV or less, in which case light can be absorbed more uniformly independent of wavelength, and the aesthetic quality of the film-coated transparent substrate 1 can be further improved.
[0043] The band gap of the dielectric phase 4 is preferably an indirect transition type. In this case, light can be absorbed more uniformly independent of wavelength, and the aesthetic quality of the film-coated transparent substrate 1 can be further improved.
[0044] In addition, it is preferable that the light absorbing film 3 has a chemical stability that allows the coexistence of the dielectric phase 4 and the metal phase 5. In this regard, when the dielectric phase 4 is composed of a metal oxide, a preferable combination of the dielectric phase 4 and the metal phase 5 can be determined according to the Ellingham diagram shown in FIG.
[0045] In the Ellingham diagram shown in FIG. 3, the lower the standard Gibbs energy of each metal element, the more stable the oxide state is, and the higher the standard Gibbs energy of each metal element, the more stable the metal state is. For example, this means that metal Ag can exist stably in the oxide of Fe, but metal Fe cannot exist stably in the oxides of Bi, Cu, and Ag (it is easily oxidized). Therefore, it is preferable that the standard Gibbs energy of the metal element constituting the dielectric phase 4 is smaller than the standard Gibbs energy of the metal element constituting the metal phase 5. In this case, the chemical stability that allows the dielectric phase 4 and the metal phase 5 to coexist can be further improved, and the aesthetics of the film-coated transparent substrate 1 can be further improved. Note that the Ellingham diagram in FIG. 3 is an example and can be applied to other metals.
[0046] From this viewpoint, as a preferred combination of the dielectric phase 4 and the metal phase 5, for example, when an oxide of a base metal such as PbO or Bi2O3 is used for the dielectric phase 4, it is preferable to use Au, Ag, Cu, Pt, Pd, Rh, or the like for the metal phase 5. When an oxide of a noble metal such as V2O5 or Cr2O3 is used for the dielectric phase 4, it is further preferable to use Zn, Fe, Sn, Ni, Pb, or the like for the metal phase 5.
[0047] Specific examples of preferred combinations of the dielectric phase 4 and the metal phase 5 include Fe2O3 and Ag, Bi2O3 and Cu, PbO and Pt, Cr2O3 and Pb, BiVO4 and Ag, V2O5 and FeNi, SrTaO2N, and CuNi.
[0048] It is preferable that the metal phase 5 is dispersed in the dielectric phase 4 as a matrix as in this embodiment. In this case, the insulating property of the light absorbing film 3 can be further improved. Therefore, in this case, it can be suitably used for a display having a touch panel function, or a top plate for a cooker having a built-in display having a touch panel function.
[0049] In the light absorbing film 3, the volume ratio of the metal phase 5 to the whole (metal phase 5 / (dielectric phase 4+metal phase 5)) is preferably 0.3 or more, more preferably 0.5 or more, and preferably 0.8 or less, more preferably 0.7 or less. When the volume ratio (metal phase 5 / (dielectric phase 4+metal phase 5)) is equal to or more than the lower limit, the insulating properties of the light absorbing film 3 can be further improved. When the volume ratio (metal phase 5 / (dielectric phase 4+metal phase 5)) is equal to or less than the upper limit, more sufficient absorption can be obtained at wavelengths that are likely to cause optical interference.
[0050] The average absorption coefficient of the light absorbing film 3 at wavelengths of 400 nm to 700 nm is preferably 0.5 μm -1 More preferably, 10 μm -1 More than 80μm, preferably -1 Less than or equal to 70 μm, more preferably -1 or less. When the average absorption coefficient is equal to or greater than the lower limit, for example, when used in a top plate for a cooker, the internal structure of the cooker can be more reliably concealed. On the other hand, when the average absorption coefficient is equal to or less than the upper limit, various information can be more reliably and clearly displayed when the light source is turned on. The absorption coefficient of the light absorbing film 3 is derived from measurements of transmittance and reflectance using spectroscopic ellipsometry or a spectrophotometer, and is measured from the light absorbing film 3 side in a state where it is laminated on the transparent substrate 2.
[0051] In addition, in the light absorbing film 3, when the absorption coefficient at a wavelength of 436 nm is α1, the absorption coefficient at a wavelength of 546 nm is α2, and the absorption coefficient at a wavelength of 700 nm is α3, it is preferable that α1 / α2 is 0.8 or more and 2.0 or less, and α3 / α2 is 0.8 or more and 2.0 or less. It is more preferable that α1 / α2 is 0.8 or more and 1.25 or less, and α3 / α2 is 0.8 or more and 1.25 or less. In this case, it is possible to achieve a more achromatic black color when the light source is turned off, and it is possible to achieve a more aesthetically pleasing appearance.
[0052] In addition, in the light absorbing film, the absorption coefficient at wavelength λ is defined as α, and the average absorption coefficient at wavelengths of 400 nm to 700 nm is defined as α AVE When the light source is turned off, it is preferable that the absorption mean deviation M represented by the following formula (1) is 0.30 or less. In this case, a more achromatic black color can be obtained when the light source is turned off, and the appearance can be further improved.
[0053]
number
[0054] In the present invention, the content of the metal constituting the metal phase 5 in the light absorbing film 3 is, in mole %, preferably 5% or more, more preferably 10% or more, even more preferably 12% or more, preferably 80% or less, more preferably 70% or less, even more preferably 60% or less, and particularly preferably 55% or less. If the content of the metal constituting the metal phase 5 in the light absorbing film 3 is smaller than the lower limit, the α1 / α2 may become too large, the α3 / α2 may become too small, and the absorption mean deviation M may become too large. On the other hand, if the content of the metal constituting the metal phase 5 in the light absorbing film 3 is larger than the upper limit, the sheet resistance may be easily reduced. In addition, the α1 / α2 may become too small, the α3 / α2 may become too large, and the absorption mean deviation M may become too large.
[0055] The thickness of the light absorbing film 3 is not particularly limited, but is preferably 5 nm or more, more preferably 10 nm or more, and preferably 2 μm or less, more preferably 1 μm or less. When the thickness of the light absorbing film 3 is within the above range, various information can be displayed more clearly when the light source is turned on, and the appearance can be improved when the light is turned off.
[0056] Saturation C of the transmitted light through the film-coated transparent substrate 1 * T is preferably 2 or less, more preferably 1 or less, and further preferably 0.5 or less.* R is preferably 2 or less, more preferably 1 or less, and further preferably 0.5 or less. * is the chroma C when illuminated with a D65 light source in the L*a*b* color system adopted in JIS Z 8781-4:2013. * In addition, chroma C * is chromaticity a * and b * More demanding, C * =((a * ) 2 +(b * ) 2 ) 1 / 2 In this case, it is possible to achieve a more achromatic black color when the light source is turned off, and it is possible to achieve an even more aesthetically pleasing appearance.
[0057] In order to make the boundary between the display area A and the non-display area B, which will be described later, even less visible, the brightness (L * The absolute value of the difference between the saturation (C * The absolute value of the difference between the above values is preferably 0.7 or less, and more preferably 0.4 or less.
[0058] The sheet resistance of the light absorbing film 3 is preferably 10 6 Ω / □ or more, preferably 10 8 Ω / □ or more. In this case, since the light absorbing film 3 is insulating, when it is used as a cover glass for an image display device or a top plate for a cooking appliance, even if a touch panel is added, the change in capacitance due to finger contact, which is necessary for a capacitive touch sensor, is maintained, and the touch panel can function. The sheet resistance can be measured by the method specified in ASTM D257 or JIS K 6271-6 (2008).
[0059] (Second, third and fourth embodiments) Fig. 4 is a schematic cross-sectional view showing a film-coated transparent substrate according to a second embodiment of the present invention. As shown in Fig. 4, in a film-coated transparent substrate 21, a dielectric multilayer film 6 is further provided on a light absorbing film 3. The other points are the same as those in the first embodiment.
[0060] The dielectric multilayer film 6 is a laminated film in which low-refractive-index films 7 having a relatively low refractive index and high-refractive-index films 8 having a relatively high refractive index are alternately laminated in this order. In this embodiment, the number of laminated layers in the dielectric multilayer film 6 is six.
[0061] The material of the low refractive index film 7 may be, for example, silicon oxide as in this embodiment, or aluminum oxide.
[0062] Examples of materials for the high refractive index film 8 include niobium oxide, titanium oxide, zirconium oxide, hafnium oxide, tantalum oxide, silicon nitride, aluminum oxide, and aluminum nitride, as in this embodiment.
[0063] Fig. 5 is a schematic cross-sectional view showing a film-coated transparent substrate according to a third embodiment of the present invention. As shown in Fig. 5, in a film-coated transparent substrate 31, a dielectric multilayer film 16 including a light absorbing film 3 is provided on a first main surface 2a of a transparent substrate 2. Other points are the same as those of the first embodiment.
[0064] In the dielectric multilayer film 16, low refractive index films 7 having a relatively low refractive index and light absorbing films 3 serving as high refractive index films having a relatively high refractive index are alternately laminated in this order. In this embodiment, the number of laminated layers in the dielectric multilayer film 16 is six. Note that the light absorbing films 3 are the light absorbing films 3 described in the first embodiment, and the low refractive index films 7 are the low refractive index films 7 described in the second embodiment. Note that at least one layer of the three light absorbing films 3 may be the high refractive index film 8 described in the second embodiment.
[0065] Fig. 6 is a schematic cross-sectional view showing a film-coated transparent substrate according to a fourth embodiment of the present invention. As shown in Fig. 6, in a film-coated transparent substrate 41, two light absorbing films 3 are provided on a transparent substrate 2, and a dielectric multilayer film 6 is further provided between the transparent substrate 2 and the light absorbing film 3 and between the two light absorbing films. Other points are the same as those of the second embodiment.
[0066] In the second, third and fourth embodiments, the light absorbing film 3 provided on the first main surface 2a of the transparent substrate 2 is composed of a dielectric phase 4 having a band gap of 2.0 eV or more and 2.7 eV or less, and a metal phase 5. Therefore, when the light source is turned on, various information can be displayed clearly, and when the light is turned off, an excellent aesthetic appearance can be achieved.
[0067] Also, a dielectric multilayer film 6 may be provided on the light absorbing film 3 as in the second embodiment, a dielectric multilayer film 16 including a light absorbing film 3 may be provided on the transparent substrate 2 as in the third embodiment, or two light absorbing films 3 may be provided on the transparent substrate 2, and a dielectric multilayer film 6 may be provided between the transparent substrate 2 and the light absorbing film 3 and between the two light absorbing films as in the fourth embodiment. In this way, when the dielectric multilayer films 6, 16 are provided, for example, an anti-reflection function can be further imparted. In this case, the contrast of the display can also be improved.
[0068] [Cooking equipment top plate] 7 is a schematic cross-sectional view showing a top plate for a cooking appliance according to one embodiment of the present invention, As shown in Fig. 7, a top plate 51 for a cooking appliance includes a transparent substrate 1 with a film.
[0069] In the top plate 51 for a cooker, the second main surface 2b of the transparent substrate 2 constituting the film-coated transparent substrate 1 is the cooking surface. Meanwhile, the first main surface 2a of the transparent substrate 2 constituting the film-coated transparent substrate 1 is the back surface. The cooking surface is the surface on which a cooking utensil such as a pot or frying pan is placed. The back surface is the surface facing the light source 52 such as an LED or a display and the heating device inside the cooker. Therefore, the cooking surface and the back surface are in a front-back relationship. In this embodiment, the transparent substrate 2 is a glass substrate.
[0070] A light absorbing film 3 is provided on the back surface (first main surface 2a) of the transparent substrate 2. A heat resistant resin layer 53 is provided on the light absorbing film 3. The heat resistant resin layer 53 may be provided between the transparent substrate 2 and the light absorbing film 3. In this embodiment, an area where the heat resistant resin layer 53 is not provided in a plan view is defined as a display area A. An area where the heat resistant resin layer 53 is provided in a plan view is defined as a non-display area B.
[0071] The heat-resistant resin layer 53 is a light-shielding layer. Therefore, by providing the heat-resistant resin layer 53, the concealment of the internal structure of the cooking device can be more reliably improved. The heat-resistant resin layer 53 can be composed of a heat-resistant resin such as a silicone resin and a coloring pigment or the like. The heat-resistant resin layer 53 does not necessarily have to be provided.
[0072] A light source 52 such as a display or an LED is provided below the film-coated transparent substrate 1. The light source 52 is a member provided to display information in the display area A. The information displayed in the display area A is not particularly limited, and examples include information indicating the state of the cooker, such as that the power is on or that heating is in progress, and information such as time.
[0073] In the display region A, light from the light source 52 passes through the light absorbing film 3 and the transparent substrate 2 and is emitted to the outside. In the non-display region B, the light from the light source 52 is blocked by the heat-resistant resin layer 53. Therefore, in the display region A, by transmitting the light from the light source 52, letters, numbers, symbols, etc. can be displayed.
[0074] The top plate 51 for the cooker includes a transparent substrate 1 with a film. Therefore, when the light source 52 is turned on, various pieces of information can be displayed clearly, and when the light is turned off, the appearance is excellent. In addition, the structure inside the cooker can be concealed while the boundary between the display area and the non-display area can be made difficult to see. A display with a touch panel function may be built into the cooker.
[0075] The present invention will be described in more detail below with reference to examples. However, the following examples are merely illustrative and the present invention is not limited to the following examples in any way.
[0076] (Examples 1 to 2) In Example 1, a mixed target of Ag and FeO was used to form a light absorbing film 3 on a glass substrate, which is a transparent substrate 2, by pulsed laser deposition (PLD). The Ag content in the mixed target was 60 mol %. The substrate temperature was 300° C., and the oxygen partial pressure was 0.5 Pa. The Ag content in the light absorbing film 3 was 45 mol %.
[0077] In Example 2, a mixed target of Cu and Bi2O3 was used to form a light absorbing film 3 on a glass substrate, which is a transparent substrate 2, by pulsed laser deposition (PLD). The Cu content in the mixed target was 30 mol %. The substrate temperature was 350°C, and the oxygen partial pressure was less than 0.1 Pa. The Cu content in the light absorbing film 3 was 30 mol %.
[0078] The band gap of Fe2O3 is 2.1 eV, and the band gap of Bi2O3 is 2.5 eV.
[0079] Fig. 8 is a diagram showing the absorption coefficients of the light absorbing film 3 of Ag and Fe2O3 and the light absorbing film 3 of Cu and Bi2O3 at wavelengths of 400nm to 700nm. From Fig. 8, it can be seen that the absorption coefficients of the light absorbing film 3 of Ag and Fe2O3 and the light absorbing film 3 of Cu and Bi2O3 are almost constant at wavelengths of 400nm to 700nm. In addition, in the light absorbing film 3 of Ag and Fe2O3, α1 / α2 was 1.05, α3 / α2 was 1.00, and the average absorption deviation M was 0.02, and in the light absorbing film 3 of Cu and Bi2O3, α1 / α2 was 1.22, α3 / α2 was 0.84, and the average absorption deviation M was 0.26.
[0080] When the electrical resistance of the Ag and Fe2O3 light absorbing film 3 was measured by a direct current two-terminal method using platinum electrodes, the sheet resistance was 1.2×10 8 The sheet resistance of Cu and Bi2O3 was 3.4×10 13 It was Ω / □.
[0081] Furthermore, the absorption coefficient of the light absorbing film 3 made of Cu and Bi2O3 was slightly decreased when heated to 150°C or higher in the air. On the other hand, the light absorbing film 3 made of Ag and Fe2O3 was stable up to about 400°C. To further improve the heat resistance, a high melting point material such as Al2O3 may be further added to the light absorbing film 3.
[0082] Comparative Example 1 In Comparative Example 1, a light absorbing film was formed on a glass substrate by pulsed laser deposition (PLD) using a mixed target of Ag and TiO2. The substrate temperature was 600°C and the oxygen partial pressure was 0.5 Pa. The band gap of TiO2 was 2.8 eV.
[0083] FIG. 9 is a graph showing the absorption coefficients of Ag and TiO2 light absorbing films at wavelengths of 400 nm to 700 nm. From FIG. 9, it can be seen that in the Ag and TiO2 light absorbing films, the absorption coefficients increase with increasing wavelength, and the absorption coefficients are not constant at wavelengths of 400 nm to 700 nm. In addition, α1 / α2 was 0.79, α3 / α2 was 2.51, and the absorption mean deviation M was 0.36. This shows that when the band gap of the dielectric phase is larger than 2.7 eV, it is difficult to maintain a constant absorption coefficient over the entire visible light range.
[0084] It was confirmed that the film-attached transparent substrates of Examples 1 and 2 could display various information clearly when the light source was turned on, and had excellent aesthetics when the light was turned off. On the other hand, in Comparative Example 1, the aesthetics were impaired when the light source was turned off.
[0085] (Examples 3 to 6 and Comparative Example 2) In Examples 3 to 6, the light absorbing film 3 was formed in the same manner as in Example 1, except that the Ag content in the mixed target of Ag and FeO and the Ag content in the light absorbing film 3 were changed as shown in the following Table 1. In Comparative Example 2, the light absorbing film was formed in the same manner as in Example 1, except that a target of FeO not containing Ag was used. In addition, the following Table 1 also shows α1 / α2, α3 / α2, absorption mean deviation M, and sheet resistance in each of the Examples and Comparative Examples.
[0086] [Table 1]
[0087] Fig. 10 is a diagram showing the absorption coefficients at wavelengths of 400 nm to 700 nm of the light absorbing films of Examples 1, 3 to 6, and Comparative Example 2. It can be seen from Fig. 10 that the absorption coefficients are almost constant at wavelengths of 400 nm to 700 nm in the light absorbing films of Examples 3 to 6 as well. It can also be seen from Fig. 10 that the absorption coefficient of the light absorbing film of Comparative Example 2 decreases with increasing wavelength, and the absorption coefficient is not constant at wavelengths of 400 nm to 700 nm.
[0088] It was also confirmed that the film-attached transparent substrates of Examples 3 to 6 could display various information clearly when the light source was turned on, and had excellent aesthetics when the light was turned off. On the other hand, in Comparative Example 2, the aesthetics were impaired when the light source was turned off. [Explanation of symbols]
[0089] 1, 21, 31, 41...Transparent substrate with film 2...Transparent substrate 2a…First main surface 2b…Second main surface 3...Light absorbing film 4. Dielectric phase 5...metallic phase 6,16...Dielectric multilayer film 7...Low refractive index film 8...High refractive index film 51...Cooking equipment top plate 52...Light source 53...Heat-resistant resin layer
Claims
1. A transparent substrate; a light absorbing film provided on one main surface of the transparent substrate; Equipped with The light absorbing film includes a dielectric phase composed of a metal oxide and a metal phase, A transparent substrate with a film, wherein in an Ellingham diagram, the standard Gibbs energy of a metal element constituting the metal oxide is smaller than the standard Gibbs energy of a metal element constituting the metal phase.
2. The average absorption coefficient of the light absorbing film at wavelengths of 400 nm to 700 nm is 0.5 μm -1 Above, 80μm -1 The film-attached transparent substrate according to claim 1 , wherein:
3. 3. The film-coated transparent substrate according to claim 1 or 2, wherein, in the light absorbing film, when an absorption coefficient at a wavelength of 436 nm is α1, an absorption coefficient at a wavelength of 546 nm is α2, and an absorption coefficient at a wavelength of 700 nm is α3, α1 / α2 is 0.8 or more and 2.0 or less, and α3 / α2 is 0.8 or more and 2.0 or less.
4. 4. The film-attached transparent substrate according to claim 3, wherein in the light-absorbing film, the α1 / α2 is 0.8 or more and 1.25 or less, and the α3 / α2 is 0.8 or more and 1.25 or less.
5. In the light absorbing film, the absorption coefficient at the wavelength λ is α λ and the average absorption coefficient in the wavelength range of 400 nm to 700 nm is α AVE 5. The film-attached transparent substrate according to claim 1, wherein, when the average absorption deviation M is expressed by the following formula (1), it is 0.30 or less: [0010]
6. 6. The film-coated transparent substrate according to claim 1, further comprising a dielectric multilayer film provided on said light-absorbing film.
7. the dielectric multilayer film is a laminated film in which high-refractive-index films having a relatively high refractive index and low-refractive-index films having a relatively low refractive index are alternately laminated, The film-attached transparent substrate according to claim 6 , wherein the high refractive index film is the light absorbing film.
8. A film-attached transparent substrate according to any one of claims 1 to 7 is provided, The transparent substrate has a cooking surface on which a cooking utensil is placed and a back surface opposite to the cooking surface, A top plate for a cooking appliance, the light absorbing film being provided on the back surface of the transparent substrate.
Citation Information
Patent Citations
Solar selective absorption coating
CN102653151A
Spectral filter
JP1989222204A
Colored transparent material
JP1995330379A
Colored film coated glass article
JP1998087343A
Method for manufacturing colored film-coated glass article and colored film-coated glass article