Hydrophilized carbon black aqueous dispersion for use as conductive assistant in positive electrode of zinc negative electrode secondary battery, and zinc negative electrode secondary battery

Hydrophilized carbon black dispersion addresses the conductivity issues of activated carbon in zinc negative electrode batteries by enhancing dispersibility and charge/discharge capacity through surface modification with acidic functional groups.

JP2024151400APending Publication Date: 2024-10-25KYOTO UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023064658
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-12
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Activated carbon, used in zinc negative electrode secondary batteries, has poor electrical conductivity due to its hydrophobic nature, making it difficult to disperse in water at high concentrations and thus limiting the electrode's performance.

Method used

A hydrophilized carbon black aqueous dispersion is used as a conductive additive, enhancing the wettability and dispersibility of carbon black in water by modifying its surface with acidic functional groups, allowing for better electrode performance.

Benefits of technology

The hydrophilized carbon black dispersion improves the charge/discharge capacity of zinc negative electrode secondary batteries by ensuring high hydrophilicity and effective dispersion, thereby optimizing the conductive properties of the electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024151400000001
    Figure 2024151400000001
  • Figure 2024151400000002
    Figure 2024151400000002
  • Figure 2024151400000003
    Figure 2024151400000003
Patent Text Reader

Abstract

To provide a conductive assistant for a positive electrode of a zinc negative electrode secondary battery that uses an aqueous electrolyte.SOLUTION: An aqueous dispersion of hydrophilized carbon black, in which the solid content of hydrophilized carbon black is dispersed in water, is used as a conductive assistant in a positive electrode of a zinc negative electrode secondary battery.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a hydrophilized carbon black aqueous dispersion used as a conductive assistant in the positive electrode of a zinc negative electrode secondary battery, and to a zinc negative electrode secondary battery. [Background technology]

[0002] As electronic devices become smaller, thinner, and lighter, secondary batteries that can be charged at high energy density and discharged with high efficiency have been developed as power sources for electronic devices and backup batteries. Secondary batteries are also being developed as power sources for electric vehicles and distributed power storage batteries. Lithium-ion secondary batteries, which are currently the most popular secondary batteries, use organic electrolytes, so there is a risk of smoke, fire, and explosion when the battery is short-circuited. In contrast, secondary batteries using aqueous electrolytes are expected to be used in a wide range of fields due to their safety and low environmental impact. In particular, in electric vehicle applications, secondary batteries using aqueous electrolytes instead of organic electrolytes are indispensable to eliminate the risk of fire. As secondary batteries using aqueous electrolytes, zinc negative electrode secondary batteries are of high importance. In particular, zinc-carbon batteries using carbon materials for the positive electrode are attracting attention because they are lightweight and low cost. Non-patent document 1 is known as a recent report on secondary batteries using carbon and zinc for the positive and negative electrodes, respectively. According to Non-Patent Document 1, when a carbon positive electrode using activated carbon cloth is used in an electrolytic system of zinc sulfate or zinc perchlorate, the capacity is 34 and 50 Ah / kg, respectively. [Prior art documents] [Non-patent literature]

[0003] [Non-Patent Document 1] J. Eskusson et. al., Journal of the Electrochemical Society, 2022 169 020512 Summary of the Invention [Problem to be solved by the invention]

[0004] To increase the capacity of zinc-ion batteries, it is desirable to use carbon materials with a high specific surface area, such as activated carbon. However, activated carbon has poor electrical conductivity, so it is essential to incorporate an appropriate conductive additive.

[0005] In lithium ion secondary batteries using organic electrolytes, carbon black is used as a conductive assistant. However, carbon black is hydrophobic and has low wettability with water, so it is difficult to stably disperse it in water at a high concentration. This is because the amount of hydrophilic functional groups, such as acidic hydroxyl groups such as carboxyl groups and hydroxyl groups, present on the carbon black surface, which have a high affinity with aqueous media such as water molecules, is extremely small. Therefore, it has a drawback in that it is difficult to prepare a slurry in which carbon black is highly dispersed. If the dispersibility is poor, high conductivity cannot be obtained, and the original characteristics of the electrode active material cannot be exhibited. [Means for solving the problem]

[0006] In the present disclosure, a hydrophilized carbon black aqueous dispersion is used as a conductive assistant for use in a positive electrode of a zinc negative electrode secondary battery. In the hydrophilized carbon black aqueous dispersion, hydrophilized carbon black, which is a solid content, is dispersed in water.

[0007] The solid content concentration of the hydrophilized carbon black aqueous dispersion may be 3% by mass to 25% by mass.

[0008] In the aqueous dispersion of hydrophilized carbon black, the average particle size of agglomerates of the hydrophilized carbon black dispersed in water may be 70 nm to 200 nm.

[0009] The hydrophilized carbon black may have a total amount of acidic functional groups detected when immersed in NaOH and then subjected to neutralization titration with HCl of 0.5 mmol / g or more and 1.00 mmol / g or less, a total amount of acidic functional groups detected when immersed in Na2CO3 and then subjected to neutralization titration with HCl of 0.1 mmol / g or more and 0.30 mmol / g or less, and a total amount of acidic functional groups detected when immersed in NaHCO3 and then subjected to neutralization titration with HCl of 0.05 mmol / g or more and 0.20 mmol / g or less.

[0010] The pH of the hydrophilized carbon black aqueous dispersion may be 6.0 to 9.0.

[0011] The zinc negative electrode secondary battery of the present disclosure is A positive electrode including a positive electrode active material and hydrophilized carbon black as a conductive assistant; A zinc negative electrode; An aqueous electrolyte; Equipped with.

[0012] In a zinc negative electrode secondary battery, the positive electrode active material may be activated carbon. Effect of the Invention

[0013] The hydrophilized carbon black aqueous dispersion of the present disclosure exhibits high hydrophilicity and can be suitably used as a conductive assistant for the positive electrode of a zinc negative electrode battery. A zinc negative electrode secondary battery using the hydrophilized carbon black aqueous dispersion as a conductive assistant exhibits high charge / discharge capacity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The zinc negative electrode secondary battery of this embodiment includes a zinc negative electrode, a positive electrode, and an aqueous electrolyte. The positive electrode includes a positive electrode active material and a conductive assistant.

[0015] In this embodiment, activated carbon is used as the positive electrode active material. The activated carbon is produced by activating a carbon material with a chemical or steam.

[0016] In this embodiment, a hydrophilized carbon black aqueous dispersion is used as the conductive assistant for the positive electrode. The hydrophilized carbon black aqueous dispersion is prepared by dispersing hydrophilized carbon black in water.

[0017] Next, the hydrophilized carbon black according to this embodiment will be described.

[0018] The hydrophilized carbon black according to this embodiment has an average particle size D of the agglomerates when dispersed in water. 50 It is preferable that the thickness is 70 nm to 200 nm.

[0019] The hydrophilized carbon black according to this embodiment preferably has a total amount of functional groups detected when titrated with NaOH of 0.2 mmol / g or more and 0.60 mmol / g or less, a total amount of functional groups detected when titrated with Na2CO3 of 0.05 mmol / g or more and 0.30 mmol / g or less, and a total amount of functional groups detected when titrated with NaHCO3 of 0.05 mmol / g or more and 0.20 mmol / g or less.

[0020] The hydrophilized carbon black according to this embodiment has an average particle size D of agglomerates dispersed in water. 50 is 70 nm to 200 nm, preferably 90 nm to 160 nm, and more preferably 100 nm to 150 nm.

[0021] <Average particle size D of hydrophilized carbon black particle agglomerates 50 > In the present application, the average particle size D of the agglomerates of the hydrophilized carbon black is 50 means the value of 50% cumulative frequency on the cumulative frequency distribution curve of agglomerate particle size obtained from the degree of frequency modulation of scattered light when laser light is irradiated onto the agglomerate particle in an aqueous dispersion state using a laser diffraction / scattering particle size distribution measuring device.

[0022] For each oxidized carbon black aqueous dispersion, a laser Doppler particle size distribution analyzer (Microtrac, MT3300) was used to measure the particle size of the carbon black particle aggregates, and a cumulative frequency distribution curve was created. The value of the 50% cumulative frequency from the cumulative frequency distribution curve was determined as the average particle size (D 50 ) was calculated.

[0023] The average particle size of the above-mentioned agglomerates D 50 Within the above range, the powder can be suitably dispersed in an aqueous medium and can be suitably used as a conductive assistant. The average particle size of the above agglomerates D 50 is considered to be a characteristic related to the size of the agglomerates of the hydrophilized carbon black particles when dispersed in an aqueous medium. 50 If the average particle diameter D of the carbon black agglomerates is less than 70 nm, when the carbon black is used as a conductive additive, the particle diameter is small, and when the carbon black is added between the electrode active materials, it becomes difficult to manufacture the electrode. 50 If the particle size exceeds 200 nm, the agglomerates of the hydrophilized carbon black are more likely to come into contact with each other in an aqueous medium, and the hydrophilized carbon black tends to aggregate in the aqueous dispersion, resulting in a decrease in dispersibility and a decrease in electrical conductivity.

[0024] In addition, it is essential that the surface of hydrophilic carbon black is modified with -COOH groups, -OH groups, -COC=O groups, or the like, and such surface acidic functional groups can generally be quantified by Bohem's method.

[0025] This method is widely used for activated carbon, and classifies and quantifies the acidic oxygen functional groups on the surface of activated carbon by acid / base titration. The analytical method is as follows: first, the sample is dried at 105°C to a constant weight to remove moisture, then 1 g is accurately weighed and immersed in 50 ml of an alkaline aqueous solution. Three types of alkaline aqueous solutions are used: NaOH (sodium hydroxide), Na2CO3 (sodium carbonate), and NaHCO3 (sodium bicarbonate), all with a concentration of 0.1 N (mol / L). This immersion solution is stored in an Erlenmeyer flask, the opening is sealed, and after shaking for 24 hours, the sample is filtered and removed, 10 ml of the immersion solution is weighed with a pipette and titrated with 1 N HCl. The titration is performed three times, and the average value is used. The amount of surface acidic functional groups of the sample is calculated from the difference between this value and the alkaline titration value of the blank.

[0026] The surface acidic oxygen functional groups that react with the types of alkali are as follows: NaOH: -OH (phenolic hydroxyl group), -COC=O (lactone group) -COOH (carboxy group) Na2CO3: -COC=O (lactone group), -COOH (carboxy group) NaHCO3: -COOH (carboxy group)

[0027] Therefore, the total amount of acidic functional groups is calculated from the titration value of NaOH, and the difference between the amount of surface acidic oxygen functional groups calculated from the titration values ​​of NaOH and Na2CO3 corresponds to the amount of -OH (phenolic hydroxyl group), and the difference between the amount of surface acidic oxygen functional groups calculated from the titration values ​​of NaOH and Na2CO3 corresponds to the amount of -OH (phenolic hydroxyl group). 3と The difference in the amount of surface acidic oxygen functional groups calculated from the titration value of NaHCO3 corresponds to the amount of -COC=O (lactone group), and the amount of surface acidic oxygen functional groups calculated from the titration value of NaHCO3 corresponds to the amount of -COOH (carboxy group).

[0028] The hydrophilized carbon black of the present embodiment has a total acidic functional group amount of 0.5 mmol / g to 1.00 mmol / g when immersed in NaOH and then titrated with HCl for neutralization, a total acidic functional group amount of 0.1 mmol / g to 0.30 mmol / g when immersed in Na2CO3 and then titrated with HCl for neutralization, and a total acidic functional group amount of 0.05 mmol / g to 0.20 mmol / g when immersed in NaHCO3 and then titrated with HCl for neutralization. With the above-mentioned surface acidic functional groups, it can exhibit excellent performance as a conductive assistant. Even if the amount of functional groups is less than these, it can be effective as a conductive assistant, but the performance is not much different from that of general carbon black. If the amount of functional groups is higher than these, the pH of the aqueous solution decreases, and the performance as a battery deteriorates.

[0029] Next, the hydrophilized carbon black aqueous dispersion according to this embodiment will be described.

[0030] The hydrophilized carbon black aqueous dispersion according to this embodiment has a solid content concentration of preferably 3% by mass to 25% by mass, more preferably 5% by mass to 20% by mass, and further preferably 6% by mass to 15% by mass.

[0031] The hydrophilized carbon black aqueous dispersion according to this embodiment, when used as a conductive assistant, can easily exhibit suitable dispersibility because the solid content concentration is within the above range.

[0032] In the hydrophilized carbon black aqueous dispersion according to the present embodiment, the aqueous medium may be water or a medium containing water as a main component and further a water-soluble organic solvent, and is preferably composed of water alone. Examples of water constituting the aqueous medium include purified water such as ion-exchanged water (deionized water) and distilled water.

[0033] In a zinc negative electrode battery, since the zinc metal of the negative electrode is an amphoteric element, in consideration of its reactivity, the hydrophilized carbon black aqueous dispersion according to this embodiment preferably has a pH of 6.0 to 9.0, more preferably 6.5 to 8.5, and even more preferably 7.0 to 8.0.

[0034] The hydrophilized carbon black aqueous dispersion according to the present embodiment can be suitably used as a conductive assistant when its pH is within the above range. If the pH of the hydrophilized carbon black aqueous dispersion is less than 6.0, dissociation of the acidic functional groups imparted to the hydrophilized carbon black surface is hindered, and the electrical repulsive action of the particle surface is lost, making the particles more likely to aggregate. If the pH of the hydrophilized carbon black aqueous dispersion exceeds 9.0, the ion concentration in the dispersion becomes excessive, making the particles more likely to aggregate due to salting out, and the particles more likely to absorb carbon dioxide gas in the air, making the pH of the dispersion more unstable.

[0035] Next, a method for producing the hydrophilized carbon black aqueous dispersion according to this embodiment will be described.

[0036] The method for producing a hydrophilized carbon black aqueous dispersion according to this embodiment includes: gradually adding 30 to 500 parts by mass of a hydrophilizing agent to 100 parts by mass of carbon black in an aqueous medium to obtain a hydrophilized product; centrifuging the obtained hydrophilized product to obtain an average particle size D of agglomerates dispersed in water; 50 The method is characterized in that an aqueous dispersion of hydrophilized carbon black having a particle size of 70 nm to 200 nm is obtained.

[0037] In the method for producing a hydrophilized carbon black aqueous dispersion according to the present embodiment, the carbon black to be hydrophilized is not particularly limited. The hydrophilized carbon black aqueous dispersion can be obtained by subjecting commercially available carbon black to an oxidation treatment and then dispersing the carbon black in water.

[0038] Examples of commercially available carbon black include Seast 5H, 3H, NH, 116HM, 116, Toka Black #5500, #4500, and #4400 manufactured by Tokai Carbon Co., Ltd., F-200 and SUNBLACK 270 manufactured by Asahi Carbon Co., Ltd., Dia Black SA, N234, II (IISAF), N (N339), SH (HAF), MA600, #20, #3050, and #3230 manufactured by Mitsubishi Chemical Corporation, Show Black N234, N339, MAF, VULCANXC 72, and BLACK PEARLS 480 manufactured by Cabot Corporation, Niteron #200IS and #10 manufactured by Shin-Nichika Carbon Co., Ltd., Denka Black FX-35 and HS-100 manufactured by Denka Co., Ltd., and Colour Black manufactured by Evonik Degussa. Examples of the ink may include one or more selected from FW200, FW2, FW285, FW1, FW18, S170, S160, Special Black 6, 5, 4, 4A, Printex U, V, 140U, 140V, L6, 3, HIBLACK 40B1, 40B2, 420B, 150B, Corax HP1107, HP130, N234, N339, N351, MAF, N550, Purex HS55, HS45, Columbian Raven 820, Conductex 7055ULTRA, and the like.

[0039] The method for hydrophilizing the carbon black is not particularly limited, and examples of the method include a method using an oxidizing agent, an azotizing agent, a surfactant, or a microcapsule as a hydrophilizing agent.

[0040] For example, there can be mentioned a method in which carbon black is added to an aqueous solution of an oxidizing agent such as an alkali metal salt or an ammonium salt, such as hypochlorite, chlorite, chlorate, persulfate, perborate or percarbonate, to carry out oxidation.

[0041] Examples of a method for hydrophilizing carbon black include a method of treating the carbon black with an oxidizing agent such as hydrogen peroxide, ozone, ozone water, M2O2 (M is an alkali metal), dichromate, or permanganate.

[0042] Furthermore, examples of methods for hydrophilizing carbon black include a method of carrying out a diazo coupling treatment, such as a method using an azotizing agent in which p-nitrobenzoic acid is azotized with nitrous acid, and the azotized product is bonded to the surface of the carbon black.

[0043] Other examples of methods for hydrophilizing carbon black include a method using a surfactant in which carbon black is treated with a surfactant, and a microcapsule method in which a polymer is microencapsulated on the surface of carbon black and then dispersed in water.

[0044] The method for hydrophilizing the carbon black may be any method that can disperse the resulting hydrophilized product well in an aqueous medium, and a method of oxidation with an oxidizing agent is preferred.

[0045] The aqueous medium may be water or a medium containing water as the main component and further containing a water-soluble organic solvent, and is preferably composed of water alone.

[0046] The water constituting the aqueous medium includes purified water such as ion-exchanged water (deionized water) and distilled water.

[0047] In order to improve dispersibility, a surfactant may be added to the aqueous medium as necessary. The surfactant may be any of anionic, nonionic, and cationic surfactants.

[0048] The hydrophilization treatment of carbon black is preferably carried out by stirring and mixing the hydrophilization solution obtained by stirring and mixing a hydrophilizing agent and an aqueous medium with carbon black in a disperser to form a slurry.

[0049] Examples of the dispersing machine include a high-pressure homogenizer, a sand mill, a dyno mill, a ball mill, a paint shaker, an ultrasonic dispersing machine, a dispersing machine that disperses by cavitation effect in a high-pressure chamber, etc. Dispersion treatment may also be performed using a stirrer using a normal stirring blade, a high-speed dispersing machine, an emulsifying machine, etc.

[0050] In the method for producing a hydrophilized carbon black aqueous dispersion according to this embodiment, it is preferable to obtain an oxidation treatment product by gradually adding 30 to 500 parts by mass of a hydrophilizing agent to 100 parts by mass of carbon black in an aqueous medium. The amount of the hydrophilizing agent added to 100 parts by mass of carbon black is 30 to 500 parts by mass, preferably 100 to 500 parts by mass, and more preferably 150 to 500 parts by mass.

[0051] In the method for producing a hydrophilized carbon black aqueous dispersion according to this embodiment, when the amount of the hydrophilizing agent added per 100 parts by mass of carbon black is within the above range, the surface of the carbon black can be suitably hydrophilized.

[0052] In the method for producing a hydrophilized carbon black aqueous dispersion according to the present embodiment, the hydrophilizing agent is added successively in small amounts to 100 parts by mass of carbon black. The hydrophilizing agent may be added continuously in small amounts to the carbon black, or may be added in small amounts at time intervals (intermittently). The hydrophilizing agent may be added continuously in small amounts as described above, but when the hydrophilizing agent is added intermittently in small amounts, it is preferable to add 1 / 10 to 1 / 2 of the total amount to be added, more preferably 1 / 10 to 1 / 3 of the total amount to be added, and even more preferably 1 / 10 to 1 / 5 of the total amount to be added.

[0053] In the method for producing a hydrophilized carbon black aqueous dispersion according to this embodiment, the hydrophilizing agent may be added continuously in small amounts (regardless of the number of times) to 100 parts by mass of carbon black as described above. However, when the hydrophilizing agent is added intermittently in small amounts, it is preferable to add the hydrophilizing agent in 2 to 10 parts, more preferably in 3 to 10 parts, and even more preferably in 5 to 10 parts.

[0054] In the method for producing a hydrophilized carbon black aqueous dispersion according to this embodiment, the hydrophilizing agent is added successively in small amounts to 100 parts by mass of carbon black. The hydrophilizing agent may be added continuously in small amounts as described above, but when the hydrophilizing agent is added intermittently in small amounts, it is preferably added once every 5 to 90 minutes, more preferably once every 5 to 60 minutes, and even more preferably once every 5 to 30 minutes.

[0055] In the method for producing a hydrophilized carbon black aqueous dispersion according to this embodiment, the hydrophilizing agent is added gradually in small amounts to 100 parts by mass of carbon black, rather than all at once, as described above, thereby suppressing exothermic runaway that accompanies the addition of a hydrophilizing agent such as an oxidizing agent, and effectively using the hydrophilizing agent to perform hydrophilization. In addition, since the concentration of the hydrophilizing agent can be kept low, it is possible to slow down the hydrophilization reaction rate, such as the oxidation reaction rate, and it is possible to suppress the hydrophilizing agent from decomposing before coming into contact with the carbon black surface and the hydrophilization reaction from proceeding locally.

[0056] In the method for producing a hydrophilized carbon black aqueous dispersion according to this embodiment, the temperature during the oxidation treatment is preferably 50 to 100°C, more preferably 60 to 90°C, and even more preferably 60 to 80°C.

[0057] In the method for producing a hydrophilized carbon black aqueous dispersion according to this embodiment, the oxidation treatment time is preferably from 2 to 24 hours, more preferably from 3 to 12 hours, and even more preferably from 4 to 10 hours.

[0058] In the method for producing the hydrophilized carbon black aqueous dispersion according to this embodiment, after the oxidation treatment, residual salt may be further separated using an ultrafiltration membrane.

[0059] In the method for producing a hydrophilized carbon black aqueous dispersion according to this embodiment, the hydrophilized product obtained by the above treatment is preferably fed at a flow rate of 3 kg / min to 8 kg / min and centrifuged, more preferably fed at a flow rate of 3.5 kg / min to 7.5 kg / min and centrifuged, and further preferably fed at a flow rate of 4.0 kg / min to 7.0 kg / min and centrifuged.

[0060] In the method for producing a hydrophilized carbon black aqueous dispersion according to this embodiment, the hydrophilization treated product is fed at the above flow rate and centrifuged, whereby particles other than carbon black, called grit, which are contained in the carbon black, can be removed.

[0061] The supernatant obtained by the above-mentioned centrifugation treatment may be used as it is as the desired hydrophilized carbon black aqueous dispersion, or may be further treated with an ultrafiltration membrane to remove excess salts in the supernatant and remove the aqueous medium, thereby concentrating the supernatant to a desired concentration.

[0062] The above describes a method for obtaining a hydrophilized carbon black aqueous dispersion by oxidizing commercially available carbon black and dispersing it in water. On the other hand, commercially available black ink for inkjet printers is generally a hydrophilized carbon black aqueous dispersion. It is also possible to use a commercially available black ink for inkjet printers as a conductive assistant for the positive electrode of a zinc negative electrode secondary battery. EXAMPLES

[0063] The present embodiment will be described in more detail below with reference to examples, but the present embodiment is not limited to the aspects of these examples.

[0064] Example 1 Activated carbon was used as the positive electrode active material. Mesocarbon microbeads (MCMB) activated with KOH were used as the activated carbon. Specifically, water and acetone were added to a mixture of 10 g of mesocarbon microbeads manufactured by Osaka Gas Chemicals Co., Ltd. and a predetermined amount of potassium hydroxide (KOH: activation aid), and the mixture was mixed uniformly to form a slurry. Next, the slurry was heated from room temperature to 850°C at a temperature increase rate of 10°C / min in a nitrogen gas atmosphere, and kept at the same temperature for 1 hour. The reaction product was then cooled to 100°C or less, washed with water, and dried after removing residual alkali.

[0065] The obtained KOH-activated mesocarbon microbeads were mixed with a CMC solution of SBR as a binder. A paste was prepared by adding 10% by weight of Aqua-Black (solid concentration 15%), a hydrophilic carbon black aqueous dispersion made by Tokai Carbon Co., Ltd., as a conductive assistant, to the KOH-activated mesocarbon microbeads as a solid content. This paste was applied to a graphite sheet in an amount of 10 mg / cm. 2 The amount of the binder was 8 parts by weight per 100 parts by weight of the obtained carbon positive electrode material for zinc negative electrode batteries.

[0066] A bipolar sealed cell was assembled using the electrode (positive electrode) prepared as above, a metal zinc foil (negative electrode) as the counter electrode, and a 4M-KOH solution saturated with zinc oxide as the electrolyte, and a charge-discharge test was performed. In the charge-discharge test, a charge-discharge cycle test was performed at a constant current of 0.2 mA / gr and in a voltage range of 0.5 to 1.5 V.

[0067] Comparative Example 1 A zinc negative electrode battery was prepared in the same manner as in Example 1, except that the conductive assistant in Example 1 was replaced with Denka Black, a general-purpose conductive assistant that was not hydrophilized, and a charge / discharge test was carried out.

[0068] Example 2 In Example 1, KOH-activated mesocarbon microbeads with different specific surface areas were prepared in the same manner as in Example 1, except that the amount of activation aid added was changed. A zinc negative electrode battery was prepared in the same manner as in Example 1, and a charge / discharge test was performed.

[0069] Comparative Example 2 In Example 2, a zinc negative electrode battery was prepared in the same manner as in Example 1, except that the conductive assistant was replaced with Denka Black, a general-purpose conductive assistant that was not hydrophilized, and a charge / discharge test was performed.

[0070] The results of the above Examples 1 and 2 and Comparative Examples 1 and 2 are shown in Table 1. From Table 1, when the specific surface area of ​​the KOH-activated mesocarbon microbeads, which are active materials, is the same, the zinc negative electrode secondary battery using the hydrophilized carbon black aqueous dispersion of Example 1 as a conductive assistant of the positive electrode has a larger discharge capacity than the zinc negative electrode secondary battery using denka black as a conductive assistant of Comparative Example 1. Similarly, the zinc negative electrode secondary battery using the hydrophilized carbon black aqueous dispersion of Example 2 as a conductive assistant of the positive electrode has a larger discharge capacity than the zinc negative electrode secondary battery using denka black as a conductive assistant of Comparative Example 2. In addition, when Examples 1 and 2 are compared, when the amount of the hydrophilized carbon black aqueous dispersion, which is the conductive assistant of the positive electrode, added is the same, the discharge capacity also increases as the specific surface area of ​​the KOH-activated mesocarbon microbeads, which are active materials, increases.

[0071] [Table 1]

[0072] Example 3 In Example 1, no KOH activation aid was added, and mesocarbon microbeads activated with water vapor at 900°C for 1 hour were used as the active material, and a zinc negative electrode battery was prepared in the same manner as in Example 1, and a charge-discharge test was performed. At this time, 10% by weight of Aqua-Black (solid content concentration 15%) manufactured by Tokai Carbon Co., Ltd., which is an aqueous dispersion of hydrophilized carbon black, was added as solid content.

[0073] Example 4 A zinc negative electrode battery was prepared in the same manner as in Example 3, except that Aqua-Black (solid content concentration 15%) manufactured by Tokai Carbon Co., Ltd., which is an aqueous dispersion of hydrophilized carbon black, was added at 20% as solid content, and a charge / discharge test was performed.

[0074] Example 5 A zinc negative electrode battery was prepared in the same manner as in Example 3, except that Aqua-Black (solid content concentration 15%) manufactured by Tokai Carbon Co., Ltd., which is an aqueous dispersion of hydrophilized carbon black, was added at 30% as solid content, and a charge / discharge test was performed.

[0075] Comparative Example 3 A zinc negative electrode battery was prepared in the same manner as in Example 3, except that the conductive additive in Example 3 was replaced with Denka Black, which is a general-purpose conductive additive, and a charge / discharge test was carried out.

[0076] The results of Examples 3 to 5 and Comparative Example 3 are shown in Table 2. From Table 2, the zinc negative electrode secondary batteries using the hydrophilized carbon black aqueous dispersions of Examples 3 to 5 as the conductive assistant of the positive electrode have a larger discharge capacity than the zinc negative electrode secondary battery using denka black as the conductive assistant of the positive electrode of Comparative Example 3. Furthermore, when Examples 3 to 5 are compared, the discharge capacity increases as the amount of the hydrophilized carbon black aqueous dispersion added, which is the conductive assistant of the positive electrode, increases.

[0077] [Table 2]

[0078] The particle size distribution and the amount of functional groups measured by Bohem's neutralization titration method for the carbon black used in Examples 1 and 2 and Comparative Examples 1 and 2 are shown in Table 3. The particle size distribution was measured using an MT-3300II manufactured by Microtrackbell Co., Ltd. From Table 3, the average particle size D 50 is the average particle diameter D of the Denka Black of Comparative Example 1 50Moreover, the hydrophilized carbon black of Example 1 has a larger amount of acidic functional groups such as -OH groups and -COOH groups than the Denka black of Comparative Example 1.

[0079] [Table 3]

[0080] In summary, the hydrophilized carbon black of this embodiment has a surface modified with acidic functional groups such as -OH and -COOH groups, and exhibits good dispersibility in an aqueous medium. By using the hydrophilized carbon black aqueous dispersion of this embodiment as a positive electrode conductive assistant in a zinc negative electrode secondary battery, a secondary battery with high charge / discharge capacity can be realized. [Industrial Applicability]

[0081] The hydrophilized carbon black aqueous dispersion of the present disclosure is suitable as a conductive assistant for the positive electrode of a zinc negative electrode secondary battery, particularly when a high-surface-area carbon material such as activated carbon is used in the positive electrode.

[0082] The zinc negative electrode secondary battery using the hydrophilized carbon black aqueous dispersion of the present disclosure as a positive electrode conductive assistant has a high charge / discharge capacity. The zinc negative electrode secondary battery of the present disclosure can be used as a power source or backup for electronic devices, a power source for electric vehicles, and a distributed power storage device.

Claims

1. The hydrophilized carbon black aqueous dispersion is a solid component, hydrophilized carbon black, dispersed in water, and is used as a conductive auxiliary agent in a positive electrode of a zinc negative electrode secondary battery.

2. 2. The hydrophilized carbon black aqueous dispersion according to claim 1, wherein a solid content concentration is from 3% by mass to 25% by mass.

3. 2. The hydrophilized carbon black aqueous dispersion according to claim 1, wherein an average particle size of agglomerates of the hydrophilized carbon black dispersed in water is 70 nm to 200 nm.

4. 2. The hydrophilized carbon black aqueous dispersion according to claim 1, wherein the hydrophilized carbon black has a total acidic functional group content of 0.5 mmol / g or more and 1.00 mmol / g or less when immersed in NaOH and then subjected to neutralization titration with HCl, and 2 CO 3 When the sample is immersed in a solution of 0.1 mmol / g or more and titrated with HCl to neutralize the acidic functional group, the amount of the acidic functional group detected is 0.1 mmol / g or more and 0.30 mmol / g or less, and NaHCO 3 and then subjected to neutralization titration with HCl, the amount of acidic functional groups being 0.05 mmol / g or more and 0.20 mmol / g or less.

5. 2. The hydrophilized carbon black aqueous dispersion according to claim 1, wherein the pH of the hydrophilized carbon black aqueous dispersion is from 6.0 to 9.

0.

6. A zinc negative electrode secondary battery comprising a positive electrode containing a positive electrode active material and the hydrophilized carbon black according to any one of claims 1 to 5 as a conductive assistant, a zinc negative electrode, and an aqueous electrolyte.

7. 7. The zinc negative electrode secondary battery according to claim 6, The positive electrode active material is activated carbon.