Positive electrode active material and sodium ion secondary battery

A Na-containing oxide with controlled X-ray diffraction peak intensities and crystallinity characteristics addresses the limitations of conventional P2 type structures, resulting in improved reversible capacity and performance in sodium ion secondary batteries.

JP2024151612AActive Publication Date: 2024-10-25TOYOTA JIDOSHA KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023065094
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-12
Publication Date
2024-10-25
Estimated Expiration
2043-04-12

Smart Images

  • Figure 2024151612000001_ABST
    Figure 2024151612000001_ABST
Patent Text Reader

Abstract

To disclose a positive electrode active material which has a P2 type structure and a reversible large capacity.SOLUTION: A positive electrode active material according to the present disclosure contains an Na-containing oxide. The Na-containing oxide has a P2 type structure. The Na-containing oxide at least contains, as constituent elements, Na, O and at least one element of Mn, Ni and Co. An X-ray diffraction pattern of the Na-containing oxide satisfies I1 / I2≤0.10. The X-ray diffraction pattern of the Na-containing oxide satisfies I1 / I3≤0.70. Here, the I1 represents the X-ray diffraction peak intensity derived from the (102) plane of the P2 type structure, the I2 represents the X-ray diffraction peak intensity derived from the (002) plane of the P2 type structure, and the I3 represents the X-ray diffraction peak intensity derived from the (100) plane of the P2 type structure.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application discloses a positive electrode active material and a sodium ion secondary battery. [Background technology]

[0002] Patent Documents 1 and 2 disclose Na-containing oxides having a P2 type structure and a specific chemical composition. The Na-containing oxides having a P2 type structure are used as positive electrode active materials for sodium ion secondary batteries. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2012-201588 A [Patent Document 2] JP 2017-045600 A Summary of the Invention [Problem to be solved by the invention]

[0004] Conventional positive electrode active materials having a P2 type structure have room for improvement in terms of reversible capacity. [Means for solving the problem]

[0005] The present application discloses the following aspects as means for solving the above problems. <Aspect 1> A positive electrode active material comprising a Na-containing oxide, The Na-containing oxide has a P2 type structure, The Na-containing oxide contains, as constituent elements, at least one element selected from Mn, Ni, and Co, Na, and O, The X-ray diffraction pattern of the Na-containing oxide is I 1 / I 2 ≦0.10 is satisfied, The X-ray diffraction pattern of the Na-containing oxide is I 1 / I3 ≦0.70, Above I 1 is the X-ray diffraction peak intensity originating from the (102) plane of the P2 type structure, Above I 2 is the X-ray diffraction peak intensity derived from the (002) plane of the P2 type structure, Above I 3 is the X-ray diffraction peak intensity derived from the (100) plane of the P2 type structure, Cathode active material. <Aspect 2> The positive electrode active material of embodiment 1, The X-ray diffraction pattern of the Na-containing oxide is 0.01≦I 1 / I 2 ≦0.10 is satisfied, The X-ray diffraction pattern of the Na-containing oxide is 0.01≦I 1 / I 3 Meets ≦0.70, Cathode active material. <Aspect 3> The positive electrode active material of Aspect 1 or 2, The X-ray diffraction pattern of the Na-containing oxide is 0.40°≦HW 1 Fulfilling The above HW 1 is the half-width of the X-ray diffraction peak derived from the (102) plane of the P2 type structure, Cathode active material. <Aspect 4> The positive electrode active material of Aspect 3, The X-ray diffraction pattern of the Na-containing oxide is 0.40°≦HW 1 ≦1.00°, Cathode active material. <Aspect 5> The positive electrode active material according to any one of Aspects 1 to 4, The sodium-containing oxide is Na a Mn x-p Ni y-q Co z-r M p+q+r O 2(Here, 0 < a ≤ 1.00, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W.) having a chemical composition represented by a positive electrode active material. <Aspect 6> A positive electrode active material according to any one of Aspects 1 to 5, wherein the Na-containing oxide contains at least Na, Mn, Ni, Co, and O as constituent elements, a positive electrode active material. <Aspect 7> A positive electrode active material according to any one of Aspects 1 to 4, wherein the Na-containing oxide contains at least Na, Mn, Fe, and O as constituent elements, a positive electrode active material. <Aspect 8> A sodium ion secondary battery, having a positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, wherein the positive electrode active material layer contains a positive electrode active material according to any one of Aspects 1 to 7, a sodium ion secondary battery.

Advantages of the Invention

[0006] The positive electrode active material of the present disclosure has a large reversible capacity.

Brief Description of the Drawings

[0007] [Figure 1] An example of the process for manufacturing a Na-containing oxide having a P2-type structure is shown. [Diagram 2] An example of the configuration of a sodium ion secondary battery is schematically shown. [Diagram 3] X-ray diffraction patterns of each of Examples 1 to 3 and Comparative Example 1 are shown. [Figure 4] X-ray diffraction patterns of each of Example 4 and Comparative Example 2 are shown.

Modes for Carrying Out the Invention

[0008] 1.Cathode active material The positive electrode active material according to the embodiment includes a Na-containing oxide. The Na-containing oxide has a P2 type structure. The Na-containing oxide includes, as constituent elements, at least one element selected from Mn, Ni, and Co, Na, and O. The X-ray diffraction pattern of the Na-containing oxide is I 1 / I 2 The X-ray diffraction pattern of the Na-containing oxide satisfies I 1 / I 3 ≦0.70. 1 is the X-ray diffraction peak intensity originating from the (102) plane of the P2 type structure. 2 is the X-ray diffraction peak intensity derived from the (002) plane of the P2 type structure. 3 is the X-ray diffraction peak intensity originating from the (100) plane of the P2 type structure.

[0009] 1.1 Crystal structure The Na-containing oxide according to the embodiment has at least a P2 type structure (belonging to space group P63mc) as a crystal structure. The Na-containing oxide may have a crystal structure other than the P2 type structure in addition to the P2 type structure. Examples of the crystal structure other than the P2 type structure include various crystal structures (O2 type structure, etc.) formed when Na is desorbed from the P2 type structure. The Na-containing oxide may have a P2 type structure as a main phase. The crystal structure of the Na-containing oxide as a main phase may change depending on the charge / discharge state.

[0010] 1.1.1 X-ray diffraction peak intensity The X-ray diffraction pattern of the Na-containing oxide according to the embodiment is I 1 / I 2 ≦0.10 and I 1 / I 3 ≦0.70. 1 is the X-ray diffraction peak intensity derived from the (102) plane of the P2 type structure, and I 2 is the X-ray diffraction peak intensity derived from the (002) plane of the P2 type structure, and I3 is the X-ray diffraction peak intensity originating from the (100) plane of the P2 type structure.

[0011] Conventional P2 type positive electrode active materials have a large X-ray diffraction peak intensity derived from the (102) plane and are excellent in crystallinity in all directions, including vertical, horizontal, and oblique directions. In contrast, the Na-containing oxide according to the embodiment adopts unconventional synthesis conditions, resulting in a large X-ray diffraction peak intensity I derived from the (102) plane. 1 is the X-ray diffraction peak intensity I 2 , and the X-ray diffraction peak intensity I 3 . That is, in the Na-containing oxide according to the embodiment, the X-ray diffraction peak intensity for the (102) plane in the P2 type crystal structure is decreased, and the crystallinity is decreased in the oblique direction while maintaining the P2 type structure as a whole. According to the findings of the present inventors, the Na-containing oxide having such a P2 type structure has a superior reversible capacity compared to the conventional P2 type positive electrode active material. Here, the low crystallinity for the (102) plane means that stacking faults are introduced in a specific crystal plane of the P2 type crystal structure. In the Na-containing oxide according to the embodiment, it is presumed that the reversible capacity as a positive electrode active material is increased by some action of the stacking faults.

[0012] In the X-ray diffraction pattern of the Na-containing oxide according to the embodiment, the X-ray diffraction peak intensity I 1 and the X-ray diffraction peak intensity I originating from the (002) plane of the P2 type structure 2 Comparison with I 1 / I 2 But, I 1 / I 2 In the X-ray diffraction pattern of the Na-containing oxide according to the embodiment, the X-ray diffraction peak intensity I 1 and the X-ray diffraction peak intensity I originating from the (100) plane of the P2 structure 3 Comparison with I 1 / I 3 I 1 / I3 The X-ray diffraction pattern satisfies 0.01≦I≦0.70. 1 / I 2 ≦0.10, 0.02≦I 1 / I 2 ≦0.10 or 0.03≦I 1 / I 2 ≦0.10 and 0.01≦I 1 / I 3 ≦0.70, 0.05≦I 1 / I 3 ≦0.70, 0.10≦I 1 / I 3 ≦0.70, 0.15≦I 1 / I 3 ≦0.70, 0.20≦I 1 / I 3 ≦0.70 or 0.20≦I 1 / I 3 ≦0.65 may be satisfied.

[0013] 1.1.2 Half-width of X-ray diffraction peak As described above, the Na-containing oxide according to the embodiment has low crystallinity on the (102) plane of the P2 type structure. For example, the X-ray diffraction pattern of the Na-containing oxide according to the embodiment has a crystallinity of 0.40°≦HW 1 Here, the HW 1 is the half-width of the X-ray diffraction peak derived from the (102) plane of the P2 type structure. 1 0.40°≦HW 1 ≦1.00°, 0.45°≦HW 1 ≦1.00°, 0.50°≦HW 1 ≦1.00°, 0.55°≦HW 1 ≦1.00° or 0.60°≦HW 1 ≦1.00°. There are no particular limitations on the half-value width of the X-ray diffraction peak derived from the (002) plane of the P2 type structure or the half-value width of the X-ray diffraction peak derived from the (100) plane.

[0014] 1.1.3 Measurement method for X-ray diffraction peak intensity and half-width In the present application, the terms "X-ray diffraction pattern of Na-containing oxide", "X-ray diffraction peak intensity" and "half width of X-ray diffraction peak" refer to those obtained under the following conditions. That is, an X-ray diffraction pattern is obtained by performing 2θ / θ scan on Na-containing oxide using an X-ray diffractometer (Rigaku, fully automatic multipurpose X-ray diffractometer SmartLab) with CuKα as a radiation source, tube voltage 45 kV, tube current 200 mA, step width 0.02°, and scan speed 1° / min. In the X-ray diffraction pattern, the X-ray diffraction peak derived from the (102) plane of the P2 type structure typically appears at 38.9°±0.5° (however, this may vary depending on the transition metal composition, Na amount, etc.). Also, the X-ray diffraction peak derived from the (002) plane of the P2 type structure typically appears at 15.9°±0.5° (however, this may vary depending on the transition metal composition, Na amount, etc.). In addition, the X-ray diffraction peak originating from the (100) plane of the P2 type structure typically appears at 36°±0.5° (however, this can vary depending on the transition metal composition, the amount of Na, etc.). After subtracting the background value near the peak from the X-ray diffraction pattern, the above I was calculated from the intensity of each X-ray diffraction peak. 1 / I 2 , I 1 / I 3 The half-width HW of the X-ray diffraction peak originating from the (002) plane was calculated. 1 Request.

[0015] 1.1.4 Crystallites The Na-containing oxide according to an embodiment may be a single crystal consisting of one crystallite, or may be a polycrystal having a plurality of crystallites. For example, the surface of the Na-containing oxide according to an embodiment may be composed of a plurality of crystallites. In other words, the Na-containing oxide may have a structure in which a plurality of crystallites are connected to each other on the surface. When the surface of the Na-containing oxide is composed of a plurality of crystallites, a crystal grain boundary is present on the surface. Here, the crystal grain boundary may be an inlet and an outlet of intercalation. That is, when the Na-containing oxide is a polycrystal having a plurality of crystallites, the effect of increasing the number of inlets and outlets of intercalation to reduce the reaction resistance, the effect of shortening the distance of movement of sodium ions to reduce the diffusion resistance, the effect of reducing the absolute amount of expansion and contraction during charging and discharging, and the effect of making it difficult for cracks to occur can be expected. The size of the crystallite may be large or small, but it is considered that the smaller the size of the crystallite, the more the crystal grain boundaries will be, and the more likely the above-mentioned advantageous effects will be exhibited. For example, when the diameter of the crystallite constituting the Na-containing oxide is less than 1 μm, higher performance is likely to be obtained. The "crystallite" and "diameter of the crystallite" can be determined by observing the surface of the Na-containing oxide with a scanning electron microscope (SEM) or a transmission electron microscope (TEM). That is, when the surface of the Na-containing oxide is observed and one closed region surrounded by the grain boundary is observed, the region is regarded as a "crystallite". The maximum Feret diameter of the crystallite is determined and regarded as the "diameter of the crystallite". If the Na-containing oxide is composed of a single crystal, the particle itself can be said to be one crystallite, and the maximum Feret diameter of the particle is the "diameter of the crystallite". Alternatively, the diameter of the crystallite can be determined by EBSD or XRD. For example, the diameter of the crystallite can be determined based on the Scherrer formula from the half-width of the diffraction line of the XRD pattern. If the diameter of the crystallite specified by any method is less than 1 μm, the Na-containing oxide is likely to exhibit higher performance. The crystallite constituting the Na-containing oxide may have a first surface exposed on the surface of the oxide, and the first surface may be planar. That is, the surface of the Na-containing oxide may have a structure in which a plurality of planes are connected.As described later, when producing a Na-containing oxide, crystallites having a planar first surface can be easily obtained by growing the crystallites on the surface of the particles until one crystallite and another crystallite are connected to each other.

[0016] 1.2 Chemical composition The Na-containing oxide according to one embodiment contains, as constituent elements, at least one element selected from Mn, Ni, and Co, Na, and O. The Na-containing oxide is particularly likely to achieve higher performance when it contains, as constituent elements, at least Na, Mn, one or both of Ni and Co, and O, and particularly when it contains, as constituent elements, at least Na, Mn, Ni, Co, and O. Alternatively, the Na-containing oxide is also likely to achieve higher performance when it contains, as constituent elements, at least Na, Mn, Fe, and O.

[0017] In one embodiment, the Na-containing oxide having a P2 type structure is Na a Mn x-p Ni y-q Co z-r M p+q+r O 2(Here, 0 < a ≤ 1.00, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W. ) It may have a chemical composition represented by. When the Na-containing oxide has such a chemical composition, the P2-type structure is likely to be maintained. In the above chemical composition, a is greater than 0, and may be 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, 0.50 or more, or 0.60 or more, and is at most 1.00, and may be 0.90 or less, 0.80 or less, or 0.70 or less. Also, x is 0 or more, and may be 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, or 0.50 or more, and is at most 1.00, and may be 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, or 0.50 or less. Also, y is 0 or more, and may be 0.10 or more or 0.20 or more, and is at most 1.00, and may be 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, 0.30 or less, or 0.20 or less. Also, z is 0 or more, and may be 0.10 or more, 0.20 or more, or 0.30 or more, and is at most 1.00, and may be 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, or 0.30 or less. The element M has little contribution to charge and discharge. In this regard, in the above chemical composition, when p + q + r is less than 0.17, a high charge and discharge capacity is likely to be ensured. p + q + r may be 0.16 or less, 0.15 or less, 0.14 or less, 0.13 or less, 0.12 or less, 0.11 or less, or 0.10 or less. On the other hand, when the element M is included, the P2-type structure is likely to be stabilized. In the above chemical composition, p + q + r is 0 or more, and may be 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, 0.05 or more, 0.06 or more, 0.07 or more, 0.08 or more, 0.09 or more, or 0.10 or more. The composition of O is approximately 2, but is not necessarily exactly 2.0 and is indefinite.

[0018] 1.3 Shape The P2 type structure is a hexagonal crystal system, has a large diffusion coefficient of Na ions, and is likely to grow crystals in a specific direction. In particular, when at least one of Mn, Ni, and Co is included as a transition metal element constituting the P2 type structure, the crystals tend to grow in a plate-like shape in a specific direction. Therefore, the Na-containing oxide having the P2 type structure usually becomes a plate-like particle with a large aspect ratio in which the crystal growth direction is biased in a specific direction. The Na-containing oxide according to one embodiment may be such a plate-like particle or may be a spherical particle. When the Na-containing oxide is a spherical particle, the reaction resistance decreases due to the reduction in crystallite size, and the diffusion resistance inside the particle tends to decrease. Furthermore, when applied to a secondary battery or the like, it is considered that the degree of bending is reduced by spheroidization, and the sodium ion conduction resistance decreases. As a result, for example, the rate characteristics are improved and the reversible capacity is likely to increase. In addition, in this application, the "spherical particle" means a particle having a circularity of 0.80 or more. The circularity of the particles may be 0.81 or more, 0.82 or more, 0.83 or more, 0.84 or more, 0.85 or more, 0.86 or more, 0.87 or more, 0.88 or more, 0.89 or more, or 0.90 or more. The circularity of the particles is 4πS / L 2 Here, S is the orthogonal projected area of ​​the particle, and L is the perimeter of the orthogonal projected image of the particle. The circularity of a particle can be determined by observing the appearance of the particle with a scanning electron microscope (SEM), a transmission electron microscope (TEM), or an optical microscope. When a particle is composed of multiple particles, the circularity is measured, for example, as an average value as follows.

[0019] (1) First, the particle size distribution of the particles is measured. Specifically, the particle size at 10% cumulative value (D10) and the particle size at 90% cumulative value (D90) in the volume-based particle size distribution are determined by a laser diffraction / scattering method. (2) Regarding the appearance of the particles whose particle size distribution has been measured, images are observed using a SEM, TEM, or optical microscope, and from the particles contained in the images, 100 particles having a circle equivalent diameter (the diameter of a circle having the same area as the orthogonal projected area of ​​the particle) equal to or greater than D10 and equal to or less than D90 as determined in (1) are randomly selected. (3) The circularity of each of the 100 extracted particles is determined by image processing, and the average value is regarded as the "circularity of the particle."

[0020] The Na-containing oxide according to one embodiment may be a solid particle, a hollow particle, or a particle having a void. The size of the Na-containing oxide particles is not particularly limited, but it is considered that a smaller size is more advantageous. For example, the average particle diameter (D50) of the Na-containing oxide particles may be 0.1 μm or more and 10 μm or less, 1.0 μm or more and 8.0 μm or less, or 2.0 μm or more and 6.0 μm or less. The average particle diameter (D50) is the particle diameter (D50, median diameter) at an integrated value of 50% in the volume-based particle size distribution by a laser diffraction / scattering method.

[0021] 1.4 Other As described above, the positive electrode active material according to the embodiment has an excellent reversible capacity by including the specific Na-containing oxide. As described above, stacking faults are introduced in a specific crystal plane of the Na-containing oxide, and the stacking faults may lead to an improvement in the reversible capacity. The positive electrode active material according to the embodiment may be composed of only the Na-containing oxide, or may include other positive electrode active materials (other positive electrode active materials) in addition to the Na-containing oxide. From the viewpoint of further enhancing the above effect, the ratio of other positive electrode active materials in the entire positive electrode active material may be small. For example, the content of the Na-containing oxide may be 50% by mass or more and 100% by mass or less, 60% by mass or more and 100% by mass or less, 70% by mass or more and 100% by mass or less, 80% by mass or more and 100% by mass or less, 90% by mass or more and 100% by mass or less, 95% by mass or more and 100% by mass or less, or 99% by mass or more and 100% by mass or less.

[0022] 2. Manufacturing method of positive electrode active material The Na-containing oxide according to the above embodiment can be produced, for example, by the following method. As shown in FIG. 1, the method for producing a Na-containing oxide having a P2 type structure according to one embodiment is as follows: S1: Obtaining a precursor comprising at least one element of Mn, Ni and Co; S2: Coating the surface of the precursor with a Na source to obtain a composite; S3: sintering the composite to obtain a Na-containing oxide having a P2 type structure. S3-1: Pre-firing the composite at a temperature of 300° C. or more and less than 700° C. for 2 hours or more and 10 hours or less; S3-2: Following the preliminary firing, the composite is subjected to a main firing at a temperature of 700° C. or more and 1100° C. or less for a period of 30 minutes to 48 hours or less; and S3-3: Following the main sintering, the composite is heated to a temperature T 1 from 100°C or less T 2 and rapidly cooling until the temperature reaches a temperature of 100.degree.

[0023] 2.1 S1 In S1, a precursor containing at least one element of Mn, Ni, and Co is obtained. The precursor may contain at least Mn, one or both of Ni and Co, or may contain at least Mn, Ni, and Co. The precursor may be a salt containing at least one element of Mn, Ni, and Co. For example, the precursor may be at least one of carbonate, sulfate, nitrate, and acetate. Alternatively, the precursor may be a compound other than a salt. For example, the precursor may be a hydroxide. The precursor may be a hydrate. The precursor may be a combination of multiple types of compounds. The precursor may have various shapes. For example, the precursor may be particulate, or may be spherical particles as described later. The particle size of the particles made of the precursor is not particularly limited.

[0024] In S1, a precipitate as the precursor may be obtained by a coprecipitation method using an ion source capable of forming a precipitate in an aqueous solution with transition metal ions and a transition metal compound containing at least one element selected from Mn, Ni, and Co. This makes it easier to obtain spherical particles as the precursor. The "ion source capable of forming a precipitate in an aqueous solution with transition metal ions" may be at least one selected from, for example, sodium salts such as sodium carbonate and sodium nitrate, sodium hydroxide, and sodium oxide. The transition metal compound may be the above salt or hydroxide containing at least one element selected from Mn, Ni, and Co. Specifically, in S1, the ion source and the transition metal compound may be prepared as solutions, and the solutions may be dropped and mixed to obtain a precipitate as the precursor. In this case, for example, water is used as the solvent. In this case, various sodium compounds may be used as the base, and an aqueous ammonia solution or the like may be added to adjust the basicity. In the case of the coprecipitation method, for example, an aqueous solution of a transition metal compound and an aqueous solution of sodium carbonate are prepared, and the aqueous solutions are dropped and mixed to obtain a precipitate as the precursor. Alternatively, the precursor can be obtained by a sol-gel method, and in particular, by a coprecipitation method, spherical particles can be easily obtained as the precursor.

[0025] In S1, the precursor may contain element M. Element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W. These elements M have, for example, a function of stabilizing the P2 type structure. The method of obtaining a precursor containing element M is not particularly limited. When the precursor is obtained by coprecipitation in S1, for example, an aqueous solution of a transition metal compound containing at least one of Mn, Ni, and Co, an aqueous solution of sodium carbonate, and an aqueous solution of a compound of element M are prepared, and each aqueous solution is dropped and mixed to obtain a precursor containing element M together with at least one element of Mn, Ni, and Co. Alternatively, in the manufacturing method of the present disclosure, element M may not be added in S1, and element M may be doped when Na-doping baking is performed in S2 and S3 described later.

[0026] 2.2 S2 In S2, the surface of the precursor obtained in S1 is coated with a Na source to obtain a composite. The Na source may be a salt containing Na, such as a carbonate or a nitrate, or may be a compound other than a salt, such as sodium oxide or sodium hydroxide. In S2, the amount of the Na source coated on the surface of the precursor may be determined taking into account the amount of Na lost during the subsequent calcination.

[0027] In S2, the coverage of the Na source on the surface of the precursor is not particularly limited. For example, in S2, the above-mentioned composite may be obtained by covering 40 area% or more, 50 area% or more, 60 area% or more, or 70 area% or more of the surface of the above-mentioned precursor with the Na source. Here, when the precursor obtained by S1 is a spherical particle, and the composite obtained by S2 is obtained by covering 40 area% or more of the surface of the precursor with the Na source, the Na-containing oxide having the P2 type structure is likely to become a spherical particle in S3 described later. If the coverage of the Na source is small, when the composite is fired, the P2 type crystal is likely to grow abnormally on the surface of the composite, and the Na-containing oxide is likely to become a plate-like. If the coverage of the Na source is large, when the composite is fired, the crystallites of the P2 type crystal are likely to become small, and the Na-containing oxide is likely to become a spherical particle corresponding to the shape of the precursor.

[0028] In S2, the method for coating the surface of the precursor with the Na source is not particularly limited. As described above, when 40% or more of the area of ​​the surface of the precursor is coated with the Na source, various methods can be used. For example, a tumbling fluidized coating method or a spray drying method can be used. That is, a coating solution in which a Na source is dissolved is prepared, and the coating solution is brought into contact with the surface of the precursor, and dried at the same time or after the contact. By adjusting the coating conditions (temperature, time, number of times, etc.), 40% or more of the area of ​​the surface of the precursor can be coated with the Na source.

[0029] In S2, the precursor may be coated with an M source together with a Na source. For example, in S2, the precursor obtained in S1, a Na source, and an M source containing at least one element M selected from B, Mg, Al, K, Ca, Ti, V, Cr, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W may be mixed to obtain a composite. The M source may be, for example, a salt containing the element M, such as a carbonate or sulfate, or a compound other than a salt, such as an oxide or hydroxide. The amount of the M source relative to the precursor may be determined depending on the chemical composition of the Na-containing oxide after firing.

[0030] 2.3 S3 In S3, the composite obtained in S2 is calcined to obtain a Na-containing oxide having a P2 type structure. S3 includes the above S3-1, S3-2, and S3-3.

[0031] 2.3.1 S3-1 In S3-1, the composite is pre-fired at a temperature of 300° C. or more and less than 700° C. for 2 hours to 10 hours. In S3-1, the composite may be optionally molded and then pre-fired. The pre-fire is performed at a temperature lower than that of the main firing. If the pre-fire in S3-1 is insufficient, the formation of the P2 phase may be insufficient in the finally obtained Na-containing oxide. In S3-1, the pre-fire temperature is 300° C. or more and less than 700° C., and the pre-fire time is 2 hours to 10 hours, so that the composite can be pre-fired sufficiently, and the X-ray diffraction pattern of the Na-containing oxide having a P2 type structure obtained through S3-2 and S3-3 described later is the same as that of the above I phase. 1 / I 2 or I 1 / I 3The pre-firing temperature may be 400°C or more and less than 700°C, 450°C or more and less than 700°C, 500°C or more and less than 700°C, 550°C or more and less than 700°C, or 550°C or more and less than 650°C. The pre-firing time may be 2 hours or more and less than 8 hours, 3 hours or more and less than 8 hours, 4 hours or more and less than 8 hours, 5 hours or more and less than 8 hours, or 5 hours or more and less than 7 hours. The pre-firing atmosphere is not particularly limited, and may be, for example, an oxygen-containing atmosphere.

[0032] 2.3.2 S3-2 In S3-2, following the above pre-firing, the composite is subjected to main firing at a temperature of 700°C to 1100°C for 30 minutes to 10 hours. In S3-2, the main firing temperature of the composite is 700°C to 1100°C, preferably 800°C to 1000°C. If the main firing temperature is too low, the P2 phase is not generated, and if the main firing temperature is too high, the O3 phase and the like are likely to be generated instead of the P2 phase. The temperature rise condition from the pre-firing temperature to the main firing temperature is not particularly limited. The main firing time is not particularly limited, and may be, for example, 30 minutes to 48 hours. However, the shape of the Na-containing oxide can be controlled by the main firing time. As described above, in the method of the present disclosure, when the coverage of the Na source in the composite is 40 area % or more, when the composite is fired, P2 type crystals with small crystallites are likely to be formed on the surface. In the method of the present disclosure, the P2 type crystals are grown along the surface of the particles so as to connect one P2 type crystallite with another P2 type crystallite, so that the shape of the Na-containing oxide corresponds to the shape of the precursor. For example, when the precursor is a spherical particle, the Na-containing oxide can also be a spherical particle. If the firing time is too short, the generation of the P2 phase is insufficient. On the other hand, if the firing time is too long, the P2 phase grows excessively, resulting in plate-like particles rather than spherical ones. As far as the present inventors have confirmed, spherical particles of the Na-containing oxide are easily obtained when the firing time is 30 minutes or more and 3 hours or less. The Na-containing oxide obtained after firing may have a structure in which a plurality of crystallites are present on the surface and the crystallites are connected to each other.

[0033] 2.3.3 S3-3 In S3-3, following the main sintering, the composite is heated to a temperature T 1 from 100°C or less T 2 The above pre-baking and main baking are performed, for example, in a heating furnace. In step S3-3, for example, after the main baking of the composite is performed in the heating furnace, the composite is heated to an arbitrary temperature T 1 Cool to the temperature T 1 After this, the baked product is removed from the furnace and heated to any temperature T below 100°C. 2 Rapid cooling is performed outside the furnace until the temperature T 1 is any temperature above 200° C., and may be any temperature above 250° C. 2 is any temperature below 100°C, may be any temperature below 50°C, or may be the cooling end temperature. 1 from temperature T 2 In a certain temperature range between the temperatures, moisture easily penetrates between the layers of the P2 type structure due to atomic vibrations and molecular motions. When cooling the composite (Na-containing oxide having a P2 type structure) after the main firing, it is considered that the amount of moisture that penetrates between the layers of the P2 type structure can be reduced by shortening the time during which the composite is in the temperature range in which moisture easily penetrates (i.e., by cooling quickly). In this regard, in step S3-3, when cooling the composite after the main firing, an arbitrary temperature T 1 Any temperature T below 100°C 2 The temperature is then cooled in a dry atmosphere outside the furnace until the temperature T 1 from temperature T 2 The cooling rate during the cooling process is high (e.g., 20°C / min or more), which makes it difficult for moisture to penetrate between the layers of the P2 type structure, and the collapse of the P2 type structure can be suppressed. As a result, the X-ray diffraction pattern of the Na-containing oxide having the P2 type structure obtained through S3-3 is similar to that of the above-mentioned I 1 / I 2 or I 1 / I 3 It is likely to satisfy the above.

[0034] By the above method, a compound having a P2 type structure, a predetermined chemical composition, and the above I 1 / I 2 or I 1 / I 3 It is possible to produce a Na-containing oxide that satisfies the above requirements.

[0035] 3. Sodium-ion secondary battery The positive electrode active material according to the embodiment includes the specific Na-containing oxide. The positive electrode active material can be used, for example, as a positive electrode active material of a sodium ion secondary battery. FIG. 2 shows a schematic configuration of a sodium ion secondary battery according to an embodiment. As shown in FIG. 2, a sodium ion secondary battery 100 according to an embodiment has a positive electrode active material layer 10, an electrolyte layer 20, and a negative electrode active material layer 30. Here, the positive electrode active material layer 10 includes the positive electrode active material according to the embodiment.

[0036] 3.1 Cathode active material layer The positive electrode active material layer 10 includes at least the positive electrode active material according to the above embodiment, and may further include an electrolyte, a conductive assistant, a binder, and the like. Furthermore, the positive electrode active material layer 10 may further include various additives. The content of each of the positive electrode active material, electrolyte, conductive assistant, binder, and the like in the positive electrode active material layer 10 may be appropriately determined according to the intended battery performance. For example, the content of the positive electrode active material may be 40 mass% or more, 50 mass% or more, or 60 mass% or more, and may be 100 mass% or less, or 90 mass% or less, with the entire positive electrode active material layer 10 (total solid content) being 100 mass%. The shape of the positive electrode active material layer 10 is not particularly limited, and may be, for example, a sheet-like positive electrode active material layer 10 having a substantially flat surface. The thickness of the positive electrode active material layer 10 is not particularly limited, and may be, for example, 0.1 μm or more or 1 μm or more, and may be 2 mm or less or 1 mm or less.

[0037] 3.1.1 Cathode active material The positive electrode active material is as described above. That is, the positive electrode active material contains a Na-containing oxide, which has a P2 type structure and contains, as constituent elements, at least one element selected from Mn, Ni, and Co, Na, and O, and further contains I 1 / I 2 and I 1 / I 3 As described above, the positive electrode active material may be composed of only the Na-containing oxide, or may contain other positive electrode active materials (other positive electrode active materials) in addition to the Na-containing oxide. From the viewpoint of further enhancing the effect of the technology of the present disclosure, the proportion of other positive electrode active materials in the entire positive electrode active material may be small. For example, the content of the Na-containing oxide may be 50% by mass or more and 100% by mass or less, 60% by mass or more and 100% by mass or less, 70% by mass or more and 100% by mass or less, 80% by mass or more and 100% by mass or less, 90% by mass or more and 100% by mass or less, 95% by mass or more and 100% by mass or less, or 99% by mass or more and 100% by mass or less, based on the entire positive electrode active material being 100% by mass.

[0038] 3.1.2 Electrolytes The electrolyte that can be contained in the positive electrode active material layer 10 may be a solid electrolyte, a liquid electrolyte (electrolytic solution), or a combination of these. The solid electrolyte may be any known solid electrolyte for sodium ion secondary batteries. The solid electrolyte may be an inorganic solid electrolyte or an organic polymer electrolyte. In particular, inorganic solid electrolytes are excellent in ion conductivity and heat resistance. Examples of inorganic solid electrolytes include Na 3 Zr 2 PSi 2 O 12 OrNa 2 O-11Al 2 O 3 Oxides such as NaBH 4 , NaB 10 H 10 , NaCB 9 H 10 , NaCB 11 H 12 , NaB 12 Cl 12Hydrides and borides such as Na 3 P.S. 4 , Na 3 SbS 4 , Na 2.88 Sb 0.88 W 0.12 S 4 Sulfides such as NaPF 6 , NaBF 4 The solid electrolyte may be, for example, particulate. Only one type of solid electrolyte may be used alone, or two or more types may be used in combination. The electrolytic solution may contain, for example, sodium ions as carrier ions. The electrolytic solution may be an aqueous electrolytic solution or a non-aqueous electrolytic solution. The composition of the electrolytic solution may be the same as that of the electrolytic solution of a sodium ion secondary battery known in the art. For example, the electrolytic solution may be a carbonate-based solvent in which a sodium salt is dissolved at a predetermined concentration. Examples of the carbonate-based solvent include fluoroethylene carbonate (FEC), ethylene carbonate (EC), diethyl carbonate (DEC), and dimethyl carbonate (DMC). Examples of the sodium salt include NaPF 6 etc.

[0039] 3.1.3 Conductive additives Examples of the conductive assistant that may be included in the positive electrode active material layer 10 include carbon materials such as vapor grown carbon fiber (VGCF), acetylene black (AB), ketjen black (KB), carbon nanotubes (CNT), and carbon nanofibers (CNF); and metal materials such as nickel, aluminum, and stainless steel. The conductive assistant may be, for example, particulate or fibrous, and the size is not particularly limited. Only one type of conductive assistant may be used alone, or two or more types may be used in combination.

[0040] 3.1.4 Binders Examples of binders that can be included in the positive electrode active material layer 10 include butadiene rubber (BR)-based binders, butylene rubber (IIR)-based binders, acrylate butadiene rubber (ABR)-based binders, styrene butadiene rubber (SBR)-based binders, polyvinylidene fluoride (PVdF)-based binders, polytetrafluoroethylene (PTFE)-based binders, polyimide (PI)-based binders, etc. Only one type of binder may be used alone, or two or more types may be used in combination.

[0041] 3.2 Electrolyte layer The electrolyte layer 20 contains at least an electrolyte. When the sodium ion secondary battery 100 is a solid-state battery (a battery containing a solid electrolyte, which may be a battery partially using a liquid electrolyte in combination, or an all-solid-state battery not containing a liquid electrolyte), the electrolyte layer 20 contains a solid electrolyte and may further contain a binder or the like. In this case, the content of the solid electrolyte and the binder or the like in the electrolyte layer 20 is not particularly limited. On the other hand, when the sodium ion secondary battery 100 is an electrolyte battery, the electrolyte layer 20 contains an electrolyte solution and may further have a separator or the like for holding the electrolyte solution and preventing contact between the positive electrode active material layer 10 and the negative electrode active material layer 30. The thickness of the electrolyte layer 20 is not particularly limited, and may be, for example, 0.1 μm or more or 1 μm or more, and may be 2 mm or less or 1 mm or less.

[0042] The electrolyte contained in the electrolyte layer 20 may be appropriately selected from those exemplified as electrolytes that may be contained in the positive electrode active material layer 10. The binder that may be contained in the electrolyte layer 20 may also be appropriately selected from those exemplified as binders that may be contained in the positive electrode active material layer 10. Each of the electrolytes and binders may be used alone or in combination of two or more. The separator may be any separator that is normally used in sodium ion secondary batteries, and examples of the separator include those made of resins such as polyethylene (PE), polypropylene (PP), polyester, and polyamide. The separator may have a single layer structure or a multi-layer structure. Examples of the multi-layer separator include a separator with a two-layer structure of PE / PP, or a separator with a three-layer structure of PP / PE / PP or PE / PP / PE. The separator may be made of a nonwoven fabric such as a cellulose nonwoven fabric, a resin nonwoven fabric, or a glass fiber nonwoven fabric.

[0043] 3.3 Negative electrode active material layer The negative electrode active material layer 30 includes at least a negative electrode active material, and may further include an electrolyte, a conductive assistant, a binder, and the like. Furthermore, the negative electrode active material layer 30 may further include various additives. The contents of the negative electrode active material, electrolyte, conductive assistant, binder, and the like in the negative electrode active material layer 30 may be appropriately determined according to the intended battery performance. For example, the content of the negative electrode active material may be 40 mass% or more, 50 mass% or more, or 60 mass% or more, and may be 100 mass% or less, or 90 mass% or less, with the entire negative electrode active material layer 30 (total solid content) being 100 mass%. The shape of the negative electrode active material layer 30 is not particularly limited, and may be, for example, a sheet-like negative electrode active material layer having a substantially flat surface. The thickness of the negative electrode active material layer 30 is not particularly limited, and may be, for example, 0.1 μm or more or 1 μm or more, and may be 2 mm or less or 1 mm or less.

[0044] As the negative electrode active material, various substances having a potential (charge / discharge potential) for absorbing and releasing sodium ions that is lower than that of the positive electrode active material of the present disclosure can be adopted. The negative electrode active material may be, for example, an inorganic negative electrode active material such as metallic sodium, an organic compound negative electrode active material, or a combination of these. Only one type of negative electrode active material may be used alone, or two or more types may be used in combination. The shape of the negative electrode active material may be a general shape as a negative electrode active material for a battery. For example, the negative electrode active material may be in a particulate form. The negative electrode active material particles may be primary particles, or may be secondary particles in which a plurality of primary particles are aggregated. The average particle diameter (D50) of the negative electrode active material particles may be, for example, 1 nm or more, 5 nm or more, or 10 nm or more, and may be 500 μm or less, 100 μm or less, 50 μm or less, or 30 μm or less. Alternatively, the negative electrode active material may be in a sheet form (foil form, film form) such as sodium foil. That is, the negative electrode active material layer 30 may be made of a sheet of negative electrode active material.

[0045] Examples of the electrolyte that may be contained in the negative electrode active material layer 30 include the above-mentioned solid electrolyte, electrolytic solution, or a combination thereof. Examples of the conductive assistant that may be contained in the negative electrode active material layer 30 include the above-mentioned carbon material and metal material. The binder that may be contained in the negative electrode active material layer 30 may be appropriately selected from, for example, those exemplified as the binder that may be contained in the above-mentioned positive electrode active material layer 10. The electrolyte and the binder may each be used alone, or two or more types may be used in combination.

[0046] 3.4 Positive electrode current collector As shown in FIG. 2, the sodium ion secondary battery 100 may include a positive electrode collector 40 in contact with the positive electrode active material layer 10. The positive electrode collector 40 may be any of those generally used as a positive electrode collector for a battery. The positive electrode collector 40 may be in the form of a foil, a plate, a mesh, a punched metal, a foam, or the like. The positive electrode collector 40 may be made of a metal foil or a metal mesh. In particular, a metal foil is excellent in terms of ease of handling. The positive electrode collector 40 may be made of a plurality of foils. Examples of metals constituting the positive electrode collector 40 include Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, stainless steel, and the like. In particular, from the viewpoint of ensuring oxidation resistance, the positive electrode collector 40 may contain Al. The positive electrode collector 40 may have some kind of coating layer on its surface for the purpose of adjusting resistance, etc. The positive electrode current collector 40 may be a metal foil or a substrate plated or vapor-deposited with the above metal. When the positive electrode current collector 40 is made of a plurality of metal foils, some layer may be present between the plurality of metal foils. The thickness of the positive electrode current collector 40 is not particularly limited. For example, it may be 0.1 μm or more or 1 μm or more, and may be 1 mm or less or 100 μm or less.

[0047] 3.5 Negative electrode current collector As shown in FIG. 2, the sodium ion secondary battery 100 may include a negative electrode current collector 50 in contact with the negative electrode active material layer 30. The negative electrode current collector 50 may be any of those commonly used as a negative electrode current collector for a battery. The negative electrode current collector 50 may be in the form of a foil, a plate, a mesh, a punched metal, a foam, or the like. The negative electrode current collector 50 may be a metal foil or a metal mesh, or may be a carbon sheet. In particular, the metal foil is excellent in terms of ease of handling. The negative electrode current collector 50 may be made of a plurality of foils or sheets. Examples of metals constituting the negative electrode current collector 50 include Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, stainless steel, and the like. In particular, from the viewpoint of ensuring reduction resistance, the negative electrode current collector 50 may contain at least one metal selected from Cu, Ni, and stainless steel. The negative electrode current collector 50 may have some kind of coating layer on its surface for the purpose of adjusting the resistance, etc. Also, the negative electrode current collector 50 may be a metal foil or a base material on which the above-mentioned metal is plated or vapor-deposited. Also, when the negative electrode current collector 50 is made of a plurality of metal foils, some kind of layer may be present between the plurality of metal foils. The thickness of the negative electrode current collector 50 is not particularly limited. For example, it may be 0.1 μm or more or 1 μm or more, and may be 1 mm or less or 100 μm or less.

[0048] 3.6 Other matters In addition to the above configuration, the sodium ion secondary battery 100 may have obvious configurations as a secondary battery, such as tabs and terminals. The sodium ion secondary battery 100 may have each of the above configurations housed inside an exterior body. Any known exterior body for a battery can be used as the exterior body. In addition, a plurality of batteries 100 may be electrically connected in any way and stacked in any way to form an assembled battery. In this case, the assembled battery may be housed inside a known battery case. The sodium ion secondary battery 100 may also have obvious configurations such as necessary terminals. The shape of the sodium ion secondary battery 100 may be, for example, a coin type, a laminate type, a cylindrical type, a square type, or the like.

[0049] The sodium ion secondary battery 100 can be manufactured by applying a known method, except for using the above-mentioned specific positive electrode active material. For example, it can be manufactured as follows. However, the manufacturing method of the sodium ion secondary battery 100 is not limited to the following method, and each layer may be formed by, for example, dry molding or the like. (1) The positive electrode active material constituting the positive electrode active material layer is dispersed in a solvent to obtain a positive electrode layer slurry. The solvent used in this case is not particularly limited, and water or various organic solvents can be used. The positive electrode layer slurry is applied to the surface of a positive electrode current collector using a doctor blade or the like, and then dried to form a positive electrode active material layer on the surface of the positive electrode current collector, thereby forming a positive electrode. (2) The negative electrode active material constituting the negative electrode active material layer is dispersed in a solvent to obtain a negative electrode layer slurry. The solvent used in this case is not particularly limited, and water or various organic solvents can be used. The negative electrode layer slurry is applied to the surface of the negative electrode current collector using a doctor blade or the like, and then dried to form a negative electrode active material layer on the surface of the negative electrode current collector, thereby forming a negative electrode. (3) The layers are laminated so that the electrolyte layer (solid electrolyte layer or separator) is sandwiched between the negative electrode and the positive electrode to obtain a laminate having the negative electrode current collector, the negative electrode active material layer, the electrolyte layer, the positive electrode active material layer, and the positive electrode current collector in this order. Other members such as terminals are attached to the laminate as necessary. (4) The laminate is housed in a battery case, and in the case of an electrolyte battery, the battery case is filled with electrolyte, and the laminate is immersed in the electrolyte and sealed in the battery case to form a secondary battery. In the case of an electrolyte battery, the electrolyte may be impregnated in the negative electrode active material layer, the separator, and the positive electrode active material layer at the above step (3).

[0050] 4. Method for increasing the reversible capacity of sodium-ion secondary batteries The technology of the present disclosure also has an aspect of being a method for increasing the reversible capacity of a sodium ion secondary battery. That is, the method for increasing the reversible capacity of a sodium ion secondary battery of the present disclosure is characterized in that the positive electrode active material of the present disclosure is used in the positive electrode active material layer of the sodium ion secondary battery.

[0051] 5. Vehicles equipped with sodium-ion secondary batteries As described above, the positive electrode active material of the present disclosure has excellent reversible capacity and is suitable as a positive electrode active material for a sodium ion secondary battery. Such a sodium ion secondary battery having a large reversible capacity can be suitably used in at least one vehicle selected from, for example, a hybrid vehicle (HEV), a plug-in hybrid vehicle (PHEV), and an electric vehicle (BEV). That is, the technology of the present disclosure also has an aspect of a vehicle having a sodium ion secondary battery, the sodium ion secondary battery having a positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, and the positive electrode active material layer contains the positive electrode active material of the present disclosure. EXAMPLES

[0052] As described above, one embodiment of the positive electrode active material and the sodium ion secondary battery has been described, but various modifications are possible without departing from the spirit of the present invention. The technology of the present disclosure will be described in more detail below with reference to examples, but the technology of the present disclosure is not limited to the following examples.

[0053] 1. Preparation of Positive Electrode Active Material 1.1 Example 1 1.1.1 Preparation of precursor (1) MnSO 4 5H 2 O, NiSO 4 6H 2 O, CoSO 4 7H 2 The first solution was obtained by weighing out the desired composition ratio of O and dissolving it in distilled water to a concentration of 1.2 mol / L. 2 CO 3was dissolved in distilled water to a concentration of 1.2 mol / L to obtain a second solution. (2) 1000 mL of pure water was placed in a reaction vessel (with a baffle plate), and 500 mL of the first solution and 500 mL of the second solution were each added dropwise at a rate of about 4 mL / min. (3) After the dropwise addition was completed, the mixture was stirred at room temperature at a stirring speed of 150 rpm for 1 hour to obtain a product. (4) The product was washed with pure water, subjected to solid-liquid separation using a centrifuge, and the precipitate was collected. (5) The obtained precipitate was dried overnight at 120°C, crushed in a mortar, and then fine particles were removed by air classification to obtain precursor particles. The precursor particles were a composite salt containing Mn, Ni, and Co, and were spherical particles with a circularity of 0.86.

[0054] 1.1.2 Preparation of the complex (1) Na to 1150g / L 2 CO 3 After weighing out and distilled water, stir using a stirrer until completely dissolved. 2 CO 3 An aqueous solution was prepared. (2) The above Na 2 CO 3 The aqueous solution and the above-mentioned precursor particles are mixed together to obtain a mixture having a composition of Na 0.7 Mn 0.5 Ni 0.2 Co 0.3 O 2 The components were weighed and mixed so as to obtain a slurry. (3) The above slurry was air-dried by spray drying to obtain a composite. Specifically, a DL410 spray dryer was used, with a slurry delivery rate of 30 mL / min, an inlet temperature of 200°C, and a circulating air volume of 0.8 m 3 The above slurry was dried by air flow under the conditions of 0.3 MPa spray pressure at 1000 rpm, and the surface of the precursor particles was coated with Na. 2 CO 3 The precursor particles were coated with Na to obtain a composite. In the composite, 77% of the surface area of ​​the precursor particles was Na 2 CO 3 It was covered with.

[0055] 1.1.3 Firing of the composite The composite was placed in an alumina crucible and sintered in an air atmosphere to obtain a Na-containing oxide having a P2 structure under the following sintering conditions (1) to (7). (1) An alumina crucible containing the above composite is placed in a heating furnace in an air atmosphere. (2) The temperature inside the heating furnace is raised from room temperature (25°C) to 600°C in 115 minutes. (3) The temperature in the heating furnace is kept at 600°C for 360 minutes to perform pre-baking. (4) After preliminary firing, the temperature inside the heating furnace is raised from 600°C to 950°C in 140 minutes. (5) The temperature in the heating furnace is kept at 950°C for 60 minutes to perform the main firing. (6) After the main firing, the temperature in the heating furnace is lowered from 950°C to 250°C in 140 minutes. (7) Remove the alumina crucible from the heating furnace at 250°C and allow it to cool in a dry atmosphere outside the furnace until it reaches 25°C in 10 minutes.

[0056] The fired product after cooling was pulverized in a mortar in a dry atmosphere to obtain Na-containing oxide particles having a P2 type structure.

[0057] 1.2 Example 2 A composite was obtained in the same manner as in Example 1. The obtained composite was placed in an alumina crucible and fired in an air atmosphere, and the fired product after cooling was pulverized in a dry atmosphere to obtain a Na-containing oxide having a P2 type structure. The firing conditions were as follows (1) to (7). (1) An alumina crucible containing the above composite is placed in a heating furnace in an air atmosphere. (2) The temperature inside the heating furnace is raised from room temperature (25°C) to 600°C in 115 minutes. (3) The temperature in the heating furnace is kept at 600°C for 360 minutes to perform pre-baking. (4) After preliminary firing, the temperature inside the heating furnace is raised from 600°C to 925°C in 130 minutes. (5) The temperature in the heating furnace is kept at 925°C for 60 minutes to carry out the main firing. (6) After the main firing, the temperature in the heating furnace is lowered from 925°C to 250°C in 135 minutes. (7) Remove the alumina crucible from the heating furnace at 250°C and allow it to cool in a dry atmosphere outside the furnace until it reaches 25°C in 10 minutes.

[0058] 1.3 Example 3 A composite was obtained in the same manner as in Example 1. The obtained composite was placed in an alumina crucible and fired in an air atmosphere, and the fired product after cooling was pulverized in a dry atmosphere to obtain a Na-containing oxide having a P2 type structure. The firing conditions were as follows (1) to (7). (1) An alumina crucible containing the above composite is placed in a heating furnace in an air atmosphere. (2) The temperature inside the heating furnace is raised from room temperature (25°C) to 600°C in 115 minutes. (3) The temperature in the heating furnace is kept at 600°C for 360 minutes to perform pre-baking. (4) After preliminary firing, the temperature inside the heating furnace is raised from 600°C to 900°C in 120 minutes. (5) The temperature in the heating furnace is kept at 900°C for 60 minutes to perform the main firing. (6) After the main firing, the temperature in the heating furnace is lowered from 900°C to 250°C in 130 minutes. (7) Remove the alumina crucible from the heating furnace at 250°C and allow it to cool in a dry atmosphere outside the furnace until it reaches 25°C in 10 minutes.

[0059] 1.4 Comparative Example 1 Precursor particles were obtained in the same manner as in Example 1. The precursor particles and Na 2 CO 3 And, Na 0.7 Mn 0.5 Ni 0.2 Co 0.3 O 2 The precursor and Na were weighed out to have the following composition: 2 CO 3 The composite was obtained by mixing the above in a mortar. In the composite, 24% by area of ​​the surface of the precursor particles was Na 2 CO 3The obtained composite was placed in an alumina crucible and sintered in an air atmosphere. After cooling, the sintered product was pulverized in a dry atmosphere to obtain a Na-containing oxide having a P2 structure. The sintering conditions were as follows: (1) to (7). (1) An alumina crucible containing the above composite is placed in a heating furnace in an air atmosphere. (2) The temperature inside the heating furnace is raised from room temperature (25°C) to 600°C in 115 minutes. (3) The temperature in the heating furnace is kept at 600°C for 360 minutes to perform pre-baking. (4) After preliminary firing, the temperature inside the heating furnace is raised from 600°C to 900°C in 120 minutes. (5) The temperature in the heating furnace is kept at 900°C for 720 minutes to carry out the main firing. (6) After the main firing, the temperature in the heating furnace is lowered from 900°C to 250°C in 130 minutes. (7) Remove the alumina crucible from the heating furnace at 250°C and allow it to cool in a dry atmosphere outside the furnace until it reaches 25°C in 10 minutes.

[0060] 1.5 Example 4 1.5.1 Preparation of precursor (1) MnSO 4 5H 2 O, FeSO 4 7H 2 The first solution was obtained by weighing out the desired composition ratio of O and dissolving it in distilled water to a concentration of 1.2 mol / L. 2 CO 3 was dissolved in distilled water to a concentration of 1.2 mol / L to obtain a second solution. (2) 1000 mL of pure water was placed in a reaction vessel (with a baffle plate), and 500 mL of the first solution and 500 mL of the second solution were each added dropwise at a rate of about 4 mL / min. (3) After the dropwise addition was completed, the mixture was stirred at room temperature at a stirring speed of 150 rpm for 1 hour to obtain a product. (4) The product was washed with pure water, subjected to solid-liquid separation using a centrifuge, and the precipitate was collected. (5) The obtained precipitate was dried overnight at 120°C, crushed in a mortar, and then fine particles were removed by air classification to obtain precursor particles. The precursor particles were a composite salt containing Mn and Fe, and were spherical particles with a circularity of 0.86.

[0061] 1.5.2 Preparation of the complex (1) Na to 1150g / L 2 CO 3 After weighing out and distilled water, stir using a stirrer until completely dissolved. 2 CO 3 An aqueous solution was prepared. (2) The above Na 2 CO 3 The aqueous solution and the above-mentioned precursor particles are mixed together to obtain a mixture having a composition of Na 0.7 Mn 0.5 Fe 0.5 O 2 The components were weighed and mixed so as to obtain a slurry. (3) The above slurry was air-dried by spray drying to obtain a composite. Specifically, a DL410 spray dryer was used, with a slurry delivery rate of 30 mL / min, an inlet temperature of 200°C, and a circulating air volume of 0.8 m 3 The above slurry was dried by air flow under the conditions of 0.3 MPa spray pressure at 1000 rpm, and the surface of the precursor particles was coated with Na. 2 CO 3 The precursor particles were coated with Na to obtain a composite. In the composite, 77% of the surface area of ​​the precursor particles was Na 2 CO 3 It was covered with.

[0062] 1.5.3 Firing of the composite The composite was placed in an alumina crucible and fired in an air atmosphere, and the fired product after cooling was pulverized in a dry atmosphere to obtain a Na-containing oxide having a P2 type structure. The firing conditions were the same as those of Example 3 (1) to (7). That is, the furnace was heated (heated from 25°C to 600°C in 115 minutes), pre-fired in the furnace (held at 600°C for 360 minutes), heated in the furnace (heated from 600°C to 900°C in 120 minutes), fired in the furnace (held at 900°C for 60 minutes), cooled in the furnace (cooled from 900°C to 250°C in 130 minutes), and cooled outside the furnace (cooled from 250°C to 25°C in 10 minutes) to obtain a Na-containing oxide having a P2 type structure.

[0063] 1.6 Comparative Example 2 Precursor particles were obtained in the same manner as in Example 4. The precursor particles and Na 2 CO 3 And, Na 0.7 Mn 0.5 Fe 0.5 O 2 The precursor and Na were weighed out to have the following composition: 2 CO 3 The composite was obtained by mixing the above in a mortar. In the composite, 26% by area of ​​the surface of the precursor particles was Na 2 CO 3 The obtained composite was subjected to the same conditions (1) to (7) as those of Comparative Example 1, namely, furnace heating (heating from 25°C to 600°C in 115 minutes), furnace pre-firing (holding at 600°C for 360 minutes), furnace heating (heating from 600°C to 900°C in 120 minutes), furnace main firing (holding at 900°C for 720 minutes), furnace cooling (cooling down from 900°C to 250°C in 130 minutes), and cooling outside the furnace (cooling down from 250°C to 25°C in 10 minutes), and the calcined product after cooling was pulverized in a dry atmosphere to obtain a Na-containing oxide having a P2 type structure.

[0064] 2. Evaluation of positive electrode active material 2.1 Elemental analysis Elemental analysis was carried out to identify the chemical composition of each of the positive electrode active materials of Examples 1 to 4 and Comparative Examples 1 and 2. The results are shown in Table 1 below.

[0065] 2.2 Identification of crystal structure by X-ray diffraction measurement For each of the positive electrode active materials of Examples 1 to 4 and Comparative Examples 1 to 2, an X-ray diffraction measurement was performed using CuKα as a radiation source to obtain an X-ray diffraction pattern. FIG. 3 shows the X-ray diffraction patterns of each of Examples 1 to 3 and Comparative Example 1. FIG. 4 shows the X-ray diffraction patterns of each of Example 3 and Comparative Example 2. As shown in FIGS. 3 and 4, it can be seen that all of the positive electrode active materials of Examples 1 to 4 and Comparative Examples 1 to 2 have a P2 type structure belonging to the space group P63mc. Also, as shown in FIG. 3, the positive electrode active materials of Examples 1 to 3 have a lower X-ray diffraction peak intensity derived from the (102) plane compared to the positive electrode active material of Comparative Example 1, and it can be seen that stacking faults are introduced in the (102) plane. Also, as shown in FIG. 4, the positive electrode active material of Example 4 has a lower X-ray diffraction peak intensity derived from the (102) plane compared to the positive electrode active material of Comparative Example 2, and it can be seen that stacking faults are introduced in the (102) plane. Table 1 below shows the X-ray diffraction peak intensity I originating from the (102) plane of the P2 type structure for each of Examples 1 to 4 and Comparative Examples 1 and 2. 1 and the X-ray diffraction peak intensity I originating from the (002) plane of the P2 type structure 2 Comparison with I 1 / I 2 , the X-ray diffraction peak intensity I 1 and the X-ray diffraction peak intensity I originating from the (100) plane of the P2 structure 3 Comparison with I 1 / I 3 , and the half-width HW of the X-ray diffraction peak originating from the (102) plane 1 Shows.

[0066] 3. Preparation of evaluation cells Coin cells were produced using the positive electrode active materials of each of Examples 1 to 4 and Comparative Examples 1 and 2. The procedure for producing the coin cells was as follows. (1) The positive electrode active material, acetylene black (AB) as a conductive additive, and polyvinylidene fluoride (PVdF) as a binder were weighed out so that the mass ratio of the positive electrode active material:AB:PVdF=85:10:5, and dispersed and mixed in N-methyl-2-pyrrolidone to obtain a positive electrode mixture slurry. The positive electrode mixture slurry was applied onto an aluminum foil and vacuum dried overnight at 120°C to obtain a positive electrode, which is a laminate of a positive electrode active material layer and a positive electrode current collector. (2) The electrolyte was a 1:1 mixture of EC and DEC by volume, to which NaPF was added to give a concentration of 1M. 6 The above was dissolved and used. (3) Metallic sodium foil was prepared as the negative electrode. (4) A coin cell (CR2032) was prepared using the positive electrode, electrolyte, and negative electrode.

[0067] 4.Charge / Discharge Characteristics Evaluation (1) The reversible capacity of each of the coin cells of Examples 1 to 3 and Comparative Example 1 was measured by charging and discharging at 0.1 C (1 C = 160 mA / g) in a voltage range of 1.0 to 4.5 V in a thermostatic chamber maintained at 25° C. The results are shown in Table 1 below. (2) The reversible capacity of each of the coin cells of Example 4 and Comparative Example 2 was measured by charging and discharging at 0.1 C (1 C = 190 mA / g) in a voltage range of 1.0 to 4.3 V in a thermostatic chamber maintained at 25° C. The results are shown in Table 1 below.

[0068] 5. Evaluation Results For each of Examples 1 to 4 and Comparative Examples 1 and 2, I identified from the X-ray diffraction patterns 1 / I 2 , I 1 / I 3 and half-width HW 1 and the reversible capacity of the evaluation cell.

[0069] [Table 1]

[0070] As is clear from the results shown in Table 1, I1 / I 2 and I 1 / I 3 The positive electrode active materials according to Examples 1 to 3, in which the number of stacking faults on the (102) plane of the P2 type structure is relatively small, have a relatively large number of stacking faults. 1 / I 2 and I 1 / I 3 The reversible capacity is larger than that of the positive electrode active material of Comparative Example 1, which has a relatively large number of stacking faults in the (102) plane of the P2 structure. The same is true for Example 4 and Comparative Example 2, which have different transition metal species from Examples 1 to 3 and Comparative Example 1.

[0071] 6. Supplementary Information In the above examples, the precursor is obtained by coprecipitation, but the precursor can be obtained by other methods. In the above examples, the surface of the precursor is coated with a Na source by spray drying to obtain a composite, but the composite can be obtained by other methods. In the above examples, the Na-containing oxide having a P2 type structure is exemplified as having a predetermined chemical composition, but the chemical composition of the Na-containing oxide is not limited to this. The Na-containing oxide may be doped with an element M other than Mn, Ni, and Co. The element M is as described in the embodiment.

[0072] 7. Summary As described above, in a positive electrode active material containing a Na-containing oxide, if the Na-containing oxide satisfies the following requirements (1) to (4), it can be said that the reversible capacity of the positive electrode active material is increased. (1) The sodium-containing oxide has a P2 type structure. (2) The Na-containing oxide contains at least one element selected from the group consisting of Mn, Ni, and Co, Na, and O as constituent elements. (3) The X-ray diffraction pattern of the Na-containing oxide is I 1 / I 2 ≦0.10. (4) The X-ray diffraction pattern of the Na-containing oxide is I 1 / I 3≦0.70. Here, the above I 1 is the X-ray diffraction peak intensity derived from the (102) plane of the P2 type structure, and I 2 is the X-ray diffraction peak intensity derived from the (002) plane of the P2 type structure, and I 3 is the X-ray diffraction peak intensity originating from the (100) plane of the P2 type structure. [Explanation of symbols]

[0073] 100 Sodium-ion secondary battery 10 Cathode active material layer 20 Electrolyte layer 30 Negative electrode active material layer 40 Positive electrode current collector 50 Negative electrode current collector

Claims

1. A positive electrode active material comprising a Na-containing oxide, The Na-containing oxide has a P2 type structure, The Na-containing oxide contains, as constituent elements, at least one element selected from Mn, Ni, and Co, Na, and O, The X-ray diffraction pattern of the Na-containing oxide is I 1 / I 2 ≦0.10 is satisfied, The X-ray diffraction pattern of the Na-containing oxide is I 1 / I 3 ≦0.70 is satisfied, I 1 is the X-ray diffraction peak intensity derived from the (102) plane of the P2 type structure, I 2 is the X-ray diffraction peak intensity derived from the (002) plane of the P2 type structure, I 3 is the X-ray diffraction peak intensity derived from the (100) plane of the P2 type structure; Cathode active material.

2. The positive electrode active material according to claim 1 , The X-ray diffraction pattern of the Na-containing oxide is 0.01≦I 1 / I 2 ≦0.10 is satisfied, The X-ray diffraction pattern of the Na-containing oxide is 0.01≦I 1 / I 3 ≦0.70, Cathode active material.

3. The positive electrode active material according to claim 1 , The X-ray diffraction pattern of the Na-containing oxide is 0.40°≦HW 1 Fulfilling The HW 1 is the half-width of the X-ray diffraction peak derived from the (102) plane of the P2 type structure; Cathode active material.

4. The positive electrode active material according to claim 3, The X-ray diffraction pattern of the Na-containing oxide is 0.40°≦HW 1 ≦1.00° is satisfied, Cathode active material.

5. The positive electrode active material according to claim 1 , The Na-containing oxide is Na a Mn x-p Ni y-q Co z-r M p+q+r O 2 (wherein 0<a≦1.00, x+y+z=1, and 0≦p+q+r<0.17; and element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W), Cathode active material.

6. The positive electrode active material according to claim 1 , The Na-containing oxide contains at least Na, Mn, Ni, Co and O as constituent elements. Cathode active material.

7. The positive electrode active material according to claim 1 , The Na-containing oxide contains at least Na, Mn, Fe, and O as constituent elements. Cathode active material.

8. A sodium ion secondary battery, A positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, The positive electrode active material layer comprises the positive electrode active material according to any one of claims 1 to 7. Sodium ion secondary battery.

Citation Information

Patent Citations

  • Composite metal oxide and sodium secondary battery

    JP2009209037A

  • Doped nickelate material

    JP2017521342A

  • Positive electrode active material, sodium ion secondary battery, and manufacturing method for the positive electrode active material

    JP2023181098A

  • Cathode active material, cathode including the cathode active material, and sodium secondary battery including the cathode

    US20150111097A1

  • Complex metal oxide, positive electrode active material for sodium secondary battery, positive electrode for sodium secondary battery, and the sodium secondary battery

    JP2012201588A