Electrode active material and all-solid-state battery
An Al and Nb-based oxide electrode active material with a specific XRD peak range addresses the safety and capacity issues of Li-ion battery materials, offering a high-capacity and safe all-solid-state battery solution.
Patent Information
- Application Number
- JP2023065110
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-10-25
Smart Images

Figure 2024151622000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrode active material and an all-solid-state battery. [Background technology]
[0002] In recent years, all-solid-state batteries have been utilized as secondary batteries having high energy density (see, for example, Patent Documents 1 to 3 and Non-Patent Document 1). These all-solid-state batteries are required to be smaller, lighter, and have high capacity and high energy density, so high-capacity and high-power electrode active materials are being developed. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2022 / 080083 [Patent Document 2] International Publication No. 2014 / 038311 [Patent Document 3] International Publication No. 2022 / 185717 [Non-patent literature]
[0004] [Non-Patent Document 1] Appl. Mater. Interface. 2019;11(6): 6089-6096. Summary of the Invention [Problem to be solved by the invention]
[0005] The negative electrode material used in general Li-ion batteries is mainly graphite-based. However, since the operating potential of graphite-based batteries is close to the deposition potential of Li, there is a risk of internal short circuit due to deposition of Li during charging and discharging.
[0006] Compared with graphite-based negative electrode materials, oxide-based negative electrode materials have a higher operating potential and do not cause lithium deposition, so they can provide safe batteries that do not cause internal short circuits during charging and discharging. However, a drawback of oxide-based negative electrode materials is their low capacity.
[0007] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide a high-capacity electrode active material and an all-solid-state battery using the electrode active material. [Means for solving the problem]
[0008] The electrode active material according to the present invention includes a negative electrode active material which contains Al and Nb, belongs to the space group C2 / m, and has a main peak at 25.3° or more and 25.7° or less in XRD measurement using CuKα radiation.
[0009] In the above electrode active material, the negative electrode active material is represented by the general formula Al 2+x Nb 50 O 128+1.5x It may be one represented by a composition formula of (-0.1≦x≦0.1).
[0010] The electrode active material may further contain another negative electrode active material having a composition different from that of the negative electrode active material.
[0011] In the above electrode active material, the negative electrode active material is Al2Nb 50 O 128 and the electrode active material further comprises AlNb 11 O 29 may also include
[0012] The all-solid-state battery according to the present invention includes an oxide-based solid electrolyte layer, a first electrode layer provided on a first main surface of the oxide-based solid electrolyte layer and containing a positive electrode active material, and a second electrode layer provided on a second main surface of the oxide-based solid electrolyte layer and containing any one of the electrode active materials described above. Effect of the Invention
[0013] According to the present invention, it is possible to provide a high-capacity electrode active material and an all-solid-state battery using the electrode active material. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a basic structure of an all-solid-state battery. [Diagram 2] FIG. [Diagram 3] 1(a) and (b) are diagrams illustrating the measurement results when XRD measurement was performed using CuKα radiation. [Figure 4] FIG. 1 is a schematic cross-sectional view of an all-solid-state battery according to an embodiment. [Diagram 5] FIG. 1 is a schematic cross-sectional view of another all-solid-state battery. [Figure 6] FIG. 1 is a diagram illustrating a flow of a method for producing an all-solid-state battery. [Figure 7] 1(a) and (b) are diagrams illustrating the lamination process. [Figure 8] FIG. 4 is a schematic cross-sectional view showing the basic structure of a lithium-ion battery according to a second embodiment. [Figure 9] FIG. 2 is a diagram showing the discharge capacity of Example 1. [Figure 10] FIG. 1 shows the results of XRD measurement. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, an embodiment will be described with reference to the drawings.
[0016] (First embodiment) Fig. 1 is a schematic cross-sectional view showing a basic structure of an all-solid-state battery 100 according to a first embodiment. As illustrated in Fig. 1, the all-solid-state battery 100 has a structure in which a solid electrolyte layer 30 is sandwiched between a first internal electrode 10 (first electrode layer) and a second internal electrode 20 (second electrode layer). The first internal electrode 10 is formed on a first main surface of the solid electrolyte layer 30. The second internal electrode 20 is formed on a second main surface of the solid electrolyte layer 30. The first internal electrode 10, the solid electrolyte layer 30, and the second internal electrode 20 are sintered bodies.
[0017] When the all-solid-state battery 100 is used as a secondary battery, one of the first internal electrode 10 and the second internal electrode 20 is used as a positive electrode, and the other is used as a negative electrode. In the present embodiment, as an example, the first internal electrode 10 is used as a positive electrode, and the second internal electrode 20 is used as a negative electrode.
[0018] The solid electrolyte layer 30 is mainly composed of a solid electrolyte having ion conductivity. The solid electrolyte of the solid electrolyte layer 30 is, for example, an oxide-based solid electrolyte having lithium ion conductivity. The solid electrolyte is, for example, a phosphate-based solid electrolyte having a NASICON structure. The phosphate-based solid electrolyte having a NASICON structure has a high electrical conductivity and is stable in the air. The phosphate-based solid electrolyte is, for example, a phosphate containing lithium. The phosphate is not particularly limited, but examples thereof include a composite lithium phosphate salt with Ti (for example, LiTi2(PO4)3). Alternatively, Ti can be partially or completely replaced with a tetravalent transition metal such as Ge, Sn, Hf, or Zr. In order to increase the Li content, it may be partially replaced with a trivalent transition metal such as Al, Ga, In, Y, or La. More specifically, for example, Li 1+x Al x Ge 2-x (PO4)3 and Li 1+x Al x Zr 2-x (PO4)3, Li 1+x Al x Ti 2-x (PO4)3, etc.
[0019] As illustrated in FIG. 2, the first internal electrode 10 has a structure in which an electrode active material 11, a solid electrolyte 12, a conductive assistant 13, and the like are dispersed. The second internal electrode 20 has a structure in which an electrode active material 21, a solid electrolyte 22, a conductive assistant 23, and the like are dispersed. The first internal electrode 10 includes the electrode active material 11, and the second internal electrode 20 includes the electrode active material 21, so that the all-solid-state battery 100 can be used as a secondary battery. The first internal electrode 10 includes the solid electrolyte 12, and the second internal electrode 20 includes the solid electrolyte 22, so that the first internal electrode 10 and the second internal electrode 20 have ion conductivity. The first internal electrode 10 includes the conductive assistant 13, and the second internal electrode 20 includes the conductive assistant 23, so that the first internal electrode 10 and the second internal electrode 20 have conductivity.
[0020] The electrode active material 11 is, for example, an electrode active material having an olivine crystal structure. An example of such an electrode active material is a phosphate containing a transition metal and lithium. The olivine crystal structure is a crystal that natural olivine has, and can be identified by X-ray diffraction.
[0021] A typical example of an electrode active material having an olivine crystal structure is LiCoPO4 containing Co. Phosphates in which the transition metal Co is substituted in this chemical formula can also be used. Here, the ratio of Li and PO4 can vary depending on the valence. Note that it is preferable to use Co, Mn, Fe, Ni, etc. as the transition metal.
[0022] A carbon material or the like is used as the conductive assistants 13 and 23. A metal may be used as the conductive assistants 13 and 23. Examples of the metal for the conductive assistant include Pd, Ni, Cu, Fe, and alloys containing these metals.
[0023] Incidentally, the negative electrode active material used in general Li-ion batteries is mainly graphite-based. However, since the operating potential of graphite-based materials is close to the deposition potential of Li, there is a risk of internal short circuit due to deposition of Li during charging and discharging. Therefore, it is considered to use an oxide-based negative electrode active material. Compared with graphite-based negative electrode active materials, oxide-based negative electrode active materials have a higher operating potential and do not cause lithium deposition, so it is possible to provide a safe battery that does not cause internal short circuit during charging and discharging. However, a drawback of oxide-based negative electrode active materials is that they have a low capacity.
[0024] In recent years, AlNb 11 O 29 However, AlNb 11 O 29 There is an ever-increasing demand for high-capacity negative electrode active materials.
[0025] Through intensive research by the present inventors, it has been found that a higher capacity can be achieved by using an oxide-based negative electrode active material that contains Al and Nb, belongs to the space group C2 / m, and has a main peak at 25.3° to 25.7° in XRD measurement using CuKα radiation. In this embodiment, the electrode active material 21 includes an oxide-based negative electrode active material that contains Al and Nb, belongs to the space group C2 / m, and has a main peak at 25.3° to 25.7° in XRD measurement using CuKα radiation.
[0026] For example, an oxide-based negative electrode active material containing Al and Nb, belonging to the space group C2 / m, and having a main peak at 25.3° to 25.7° in XRD measurement using CuKα radiation is represented by the general formula Al 2+x Nb 50 O 128+1.5x An oxide that can be expressed by (-0.1≦x≦0.1) can be used. For example, -0.1≦x≦0 or 0≦x≦0.1 may be used.
[0027] For example, Al2Nb 50 O 128 , Al1.9 Nb 50 O 127.85 , Al 2.1 Nb 50 O 128。15 For example, AlNb 11 O 29 Input / output is 250~270mAh / cm 3 whereas Al2Nb 50 O 128 Input / output is 270mAh / g~290mAh / cm 3 It is.
[0028] As an example, Figure 3(a) shows Al2Nb 50 O 128 3(a) shows the results of XRD measurement using CuKα radiation for a negative electrode active material having the composition. As shown in FIG. 3(a), although several peaks appear, the main peak (the peak with the highest intensity) appears between 25.3° and 25.7°. Note that FIG. 3(b) shows the results of XRD measurement using CuKα radiation for a negative electrode active material having the composition. 11 O 29 FIG. 3(b) is a diagram illustrating the measurement results when XRD measurement was performed using CuKα radiation on AlNb 11 O 29 In this case, the main peak appears outside the range of 25.3° to 25.7°.
[0029] The electrode active material 21 may contain an oxide-based negative electrode active material that contains Al and Nb, belongs to the space group C2 / m, and has a main peak at 25.3° to 25.7° in XRD measurement using CuKα radiation, and may also contain other negative electrode active materials with different compositions. The other negative electrode active materials are not particularly limited, but may be, for example, TiNb2O7, AlNb 11 O 29 , Li4Ti5O 12 , TiTa2O7, TiTa 1.5 Nb 0.5 O7, TiO2, Ti2Nb 10 O 29 , Li 1.3 Al 0.3 Ti 1.7(PO4)3, LiVO3, LiTiOPO4, MoNb 12 O 33 , Li 0.29 La 0.57 TiO3, Nb 16 W5O 55 , Nb2O5, NbPO5, Li3VO4, Li3V2O5, etc. can be used.
[0030] In particular, Al2Nb is used as a negative electrode active material that contains Al and Nb, belongs to the space group C2 / m, and has a main peak at 25.3° to 25.7° in XRD measurement using CuKα radiation. 50 O 128 The other negative electrode active material is AlNb 11 O 29 By using the above, a unique effect of suppressing the reaction between the active materials even when they are mixed and fired can be obtained.
[0031] In the second internal electrode 20, if the average particle size of the electrode active material 21 is too large, the resistance inside the electrode increases, and high-speed charging and discharging may become difficult. If the average particle size is too small, the reactivity during heat treatment increases, and sintering and densification of the solid electrolyte may be hindered. Therefore, the average particle size of the electrode active material 21 in the second internal electrode 20 is preferably 0.5 μm or more and 5 μm or less, more preferably 0.7 μm or more and 4.5 μm or less, and even more preferably 1 μm or more and 4 μm or less.
[0032] FIG. 4 is a schematic cross-sectional view of a stacked type all-solid-state battery 100a in which a plurality of battery units are stacked. The all-solid-state battery 100a includes a stacked chip 60 having a substantially rectangular parallelepiped shape. In the stacked chip 60, a first external electrode 40a and a second external electrode 40b are provided so as to contact two side surfaces, which are two of the four surfaces other than the upper and lower surfaces at the ends in the stacking direction. The two side surfaces may be two adjacent side surfaces, or may be two side surfaces facing each other. In this embodiment, the first external electrode 40a and the second external electrode 40b are provided so as to contact two side surfaces facing each other (hereinafter referred to as two end surfaces).
[0033] In the following description, components having the same composition range, thickness range, and particle size distribution range as those of the all-solid-state battery 100 are denoted by the same reference numerals and detailed description thereof will be omitted.
[0034] In the all-solid-state battery 100a, a plurality of first internal electrodes 10 and a plurality of second internal electrodes 20 are alternately stacked with a solid electrolyte layer 30 interposed therebetween. The edges of the plurality of first internal electrodes 10 are exposed to the first end face of the stacked chip 60, but are not exposed to the second end face. The edges of the plurality of second internal electrodes 20 are exposed to the second end face of the stacked chip 60, but are not exposed to the first end face. As a result, the first internal electrodes 10 and the second internal electrodes 20 are alternately conductive to the first external electrode 40a and the second external electrode 40b. The solid electrolyte layer 30 extends from the first external electrode 40a to the second external electrode 40b. In this way, the all-solid-state battery 100a has a structure in which a plurality of battery units are stacked.
[0035] A cover layer 50 is laminated on the upper surface of the laminated structure of the first internal electrode 10, the solid electrolyte layer 30, and the second internal electrode 20 (in the example of FIG. 4, on the upper surface of the uppermost first internal electrode 10). In addition, a cover layer 50 is laminated on the lower surface of the laminated structure (in the example of FIG. 4, on the lower surface of the lowermost first internal electrode 10). The cover layer 50 is mainly composed of an inorganic material (e.g., Al2O3, ZrO2, TiO2, etc.) containing, for example, Al, Zr, Ti, etc. The cover layer 50 may contain the main component of the solid electrolyte layer 30 as a main component.
[0036] The first internal electrode 10 and the second internal electrode 20 may include a current collector layer. For example, as illustrated in FIG. 5, a first current collector layer 15 may be provided in the first internal electrode 10. Also, a second current collector layer 25 may be provided in the second internal electrode 20. The first current collector layer 15 and the second current collector layer 25 are mainly composed of a conductive material. For example, metal, carbon, etc. can be used as the conductive material of the first current collector layer 15 and the second current collector layer 25. The current collection efficiency is improved by connecting the first current collector layer 15 to the first external electrode 40a and connecting the second current collector layer 25 to the second external electrode 40b.
[0037] Next, a description will be given of a method for manufacturing the all-solid-state battery 100a illustrated in Fig. 4. Fig. 6 is a diagram illustrating a flow of the method for manufacturing the all-solid-state battery 100a.
[0038] (Production process of negative electrode active material powder) Weigh out and mix raw materials such as Al2O3 and Nb2O5. For example, Al 2+x Nb 50 O 128+1.5x The mixture is weighed out so that (-0.1≦x≦0.1) is obtained, and then crushed and mixed. After mixing, the mixture is calcined at 1100℃ in air, and the calcined powder is crushed again. After that, it is heat-treated at 1300℃ in air to obtain the target Al. 2+x Nb 50 O 128+1.5x A composite powder of (-0.1≦x≦0.1, 0≦y<25) is obtained. The composite powder is crushed again and then sieved through a #150 stainless steel mesh to obtain the negative electrode active material powder.
[0039] The firing temperature during synthesis is preferably 1100°C or higher and 1450°C or lower, more preferably 1150°C or higher and 1400°C or lower, and even more preferably 1200°C or higher and 1350°C or lower.
[0040] (Process for producing raw powder for solid electrolyte layer) First, a raw material powder for the solid electrolyte layer constituting the above-mentioned solid electrolyte layer 30 is prepared. For example, the raw material powder for the solid electrolyte layer can be prepared by mixing raw materials, additives, etc., and using a solid-phase synthesis method, etc. The obtained raw material powder can be adjusted to a desired average particle size by dry pulverizing. For example, the desired average particle size is adjusted using a planetary ball mill using 5 mmφ ZrO2 balls.
[0041] (Cover layer raw powder preparation process) First, the raw material powder of the ceramics constituting the above-mentioned cover layer 50 is prepared. For example, the raw material powder for the cover layer can be prepared by mixing the raw materials, additives, etc., and using a solid-phase synthesis method, etc. The obtained raw material powder can be adjusted to a desired average particle size by dry pulverizing. For example, the desired average particle size is adjusted using a planetary ball mill using 5 mmφ ZrO2 balls.
[0042] (Internal electrode paste manufacturing process) Next, the internal electrode paste for producing the first internal electrode 10 and the second internal electrode 20 is produced. For example, the internal electrode paste can be obtained by uniformly dispersing the conductive assistant, the electrode active material, the solid electrolyte material, the sintering assistant, the binder, the plasticizer, and the like in water or an organic solvent. The raw material powder for the solid electrolyte layer described above may be used as the solid electrolyte material. The conductive assistant may be a carbon material or the like. The conductive assistant may be a metal. Examples of the metal of the conductive assistant include Pd, Ni, Cu, Fe, and alloys containing these. Pd, Ni, Cu, Fe, alloys containing these, and various carbon materials may also be used. When the first internal electrode 10 and the second internal electrode 20 have different compositions, the internal electrode pastes may be produced separately. When the electrode active material 21 of the second internal electrode 20 contains a plurality of types of negative electrode active materials, the plurality of types of negative electrode active materials may be contained in the internal electrode paste.
[0043] The internal electrode paste contains, as a sintering aid, one or more glass components such as Li-BO based compounds, Li-Si-O based compounds, Li-CO based compounds, Li-SO based compounds, and Li-PO based compounds.
[0044] (External electrode paste manufacturing process) Next, an external electrode paste for producing the above-mentioned first external electrode 40a and second external electrode 40b is prepared. For example, the external electrode paste can be obtained by uniformly dispersing a conductive material, a glass frit, a binder, a plasticizer, etc. in water or an organic solvent.
[0045] (Solid electrolyte green sheet manufacturing process) The raw material powder for the solid electrolyte layer is uniformly dispersed in an aqueous or organic solvent together with a binder, a dispersant, a plasticizer, etc., and wet-pulverized to obtain a solid electrolyte slurry having a desired average particle size. At this time, a bead mill, a wet jet mill, various kneaders, a high-pressure homogenizer, etc. can be used, and it is preferable to use a bead mill from the viewpoint of simultaneously adjusting the particle size distribution and dispersing. A binder is added to the obtained solid electrolyte slurry to obtain a solid electrolyte paste. The obtained solid electrolyte paste is coated to produce a solid electrolyte green sheet 51. The coating method is not particularly limited, and a slot die method, a reverse coat method, a gravure coat method, a bar coat method, a doctor blade method, etc. can be used. The particle size distribution after wet-pulverization can be measured, for example, using a laser diffraction measurement device using a laser diffraction scattering method.
[0046] (Lamination process) As illustrated in FIG. 7(a), the internal electrode paste 52 is printed on one side of the solid electrolyte green sheet 51. In the area on the solid electrolyte green sheet 51 where the internal electrode paste 52 is not printed, the reverse pattern 53 is printed. The reverse pattern 53 can be the same as the solid electrolyte green sheet 51. A plurality of printed solid electrolyte green sheets 51 are alternately shifted and stacked. As illustrated in FIG. 7(b), a laminate is obtained by pressing the cover sheets 54 from above and below in the stacking direction. In this case, a laminate having a substantially rectangular parallelepiped shape is obtained so that the internal electrode paste 52 is exposed alternately on two end faces of the laminate. The cover sheet 54 can be formed by applying the raw material powder for the cover layer in the same manner as in the solid electrolyte green sheet preparation process. The cover sheet 54 is formed to be thicker than the solid electrolyte green sheet 51. It may be made thicker during coating, or it may be made thicker by stacking multiple coated sheets.
[0047] Next, the external electrode paste 55 is applied to each of the two end faces by a dipping method or the like, and then dried. This provides a molded body for forming the all-solid-state battery 100a.
[0048] (Firing process) Next, the obtained laminate is fired. The firing conditions are not particularly limited, and may be in an oxidizing or non-oxidizing atmosphere, and the maximum temperature is preferably 400°C to 1000°C, more preferably 500°C to 900°C, etc. In order to sufficiently remove the binder before the maximum temperature is reached, a step of maintaining the temperature in an oxidizing atmosphere at a temperature lower than the maximum temperature may be provided. In order to reduce process costs, it is desirable to fire at as low a temperature as possible. After firing, a reoxidation treatment may be performed. Through the above steps, an all-solid-state battery 100a is produced.
[0049] In addition, a collector layer can be formed in the first internal electrode 10 and the second internal electrode 20 by sequentially stacking an internal electrode paste, a collector paste containing a conductive material, and an internal electrode paste.
[0050] Second embodiment Fig. 8 is a schematic cross-sectional view showing the basic structure of a lithium ion battery 200 according to the second embodiment. As illustrated in Fig. 8, the lithium ion battery 200 has a structure in which an electrolytic solution 120 is disposed on a Li metal 110 functioning as a counter electrode, a mixed electrode 130 is disposed on the electrolytic solution 120, and a current collecting foil 140 is disposed on the mixed electrode 130. The electrolytic solution 120 is held in a separator or the like.
[0051] The Li metal 110 functions as a negative electrode. The mixed electrode 130 functions as a positive electrode. The mixed electrode 130 contains the electrode active material contained in the second internal electrode 20 described in the first embodiment. However, the mixed electrode 130 is not a sintered body, but is formed by applying a slurry containing the electrode active material and drying it. The current collector foil 140 is not particularly limited as long as it is a conductive material, and is, for example, a metal foil such as aluminum. The electrolyte 120 is not particularly limited as long as it contains an electrolyte that can conduct lithium ions.
[0052] In this embodiment, since the mixed electrode 130 contains the electrode active material of the second internal electrode 20 described in the first embodiment, a high capacity can be realized. Furthermore, since the firing process is not required in this embodiment, even if two or more types of negative electrode active materials are contained in the mixed electrode 130, the reaction between the negative electrode active materials can be suppressed. EXAMPLES
[0053] A lithium ion battery was fabricated according to the following embodiment, and its characteristics were examined.
[0054] Example 1 Al2Nb 50 O 128 The raw materials were weighed, crushed and mixed to obtain the composition ratio. After mixing, the mixture was calcined at 1100℃ in air, and the calcined powder was crushed again and further heat-treated at 1300℃ in air to obtain the desired Al2Nb 50 O 128 A synthetic powder was obtained. The synthetic powder was crushed again and then sieved through a #150 stainless steel mesh to obtain a negative electrode active material powder. A major peak was confirmed at 25.6° by XRD measurement using CuKα radiation. In addition, Rietveld analysis confirmed that it belonged to the space group C2 / m.
[0055] A coating slurry was prepared by mixing the negative electrode active material powder, PVdF binder, and acetylene black in a weight ratio of 80:10:10 and diluting it with NMP, and a coating film was formed on an aluminum foil. A negative electrode half cell was constructed with a metallic lithium foil placed on the counter electrode with a separator in between, and sealed in a 2032 coin cell using 1M LiPF6 EC:DEC (1:2 vol%) as the electrolyte. DEC is diethyl carbonate. EC is ethylene carbonate.
[0056] Example 2 In Example 2, Al 1.9 Nb 50 O 127.85 The negative electrode active material powder having the composition ratio was synthesized under the same manufacturing conditions as in Example 1. In addition, a main peak was confirmed at 25.7° by XRD measurement using CuKα radiation. In addition, it was confirmed by Rietveld analysis that it belongs to the space group C2 / m.
[0057] Example 3 In Example 3, Al 2.1 Nb 50 O 128。15 The negative electrode active material powder having the composition ratio was synthesized under the same manufacturing conditions as in Example 1. In addition, a main peak was confirmed at 25.4° by XRD measurement using CuKα radiation. In addition, it was confirmed by Rietveld analysis that it belongs to the space group C2 / m.
[0058] Comparative Example 1 In Comparative Example 1, AlNb 11 O 29 The negative electrode active material powder having the composition ratio was synthesized under the same manufacturing conditions as in Example 1. In addition, a main peak was confirmed at 24.9° by XRD measurement using CuKα radiation. In addition, it was confirmed by Rietveld analysis that it belongs to the space group C2 / m.
[0059] Comparative Example 2 In Comparative Example 2, Al 1.8 Nb 50 O 127.7The negative electrode active material powder having the composition ratio was synthesized under the same manufacturing conditions as in Example 1. In addition, a main peak was confirmed at 25.8° by XRD measurement using CuKα radiation. In addition, it was confirmed by Rietveld analysis that it belongs to the space group C2 / m.
[0060] Comparative Example 3 In Comparative Example 3, Al 2.2 Nb 50 O 128.3 The negative electrode active material powder having the composition ratio was synthesized under the same manufacturing conditions as in Example 1. In addition, a main peak was confirmed at 24.8° by XRD measurement using CuKα radiation. In addition, it was confirmed by Rietveld analysis that it belongs to the space group C2 / m.
[0061] (Single-phase rate) The single-phase ratio of the negative electrode active material was measured for each of Examples 1 to 3 and Comparative Examples 1 to 3. The single-phase ratio was calculated from the peak intensity ratio of the main phase and the secondary phase obtained by Rietveld analysis. Specifically, it was calculated as: strength of the negative electrode active material / (strength of the negative electrode active material+strength of the secondary phase)×100. The single-phase ratio was 100% in Example 1, 93% in Example 2, and 94% in Example 3, 100% in Comparative Example 1, 76% in Comparative Example 2, and 71% in Comparative Example 3.
[0062] If the single-phase ratio was 90% or more, the single-phase ratio was judged as pass "○", and if the single-phase ratio was less than 90%, the single-phase ratio was judged as fail "×". The single-phase ratios of Examples 1 to 3 were judged as pass "○". On the other hand, the single-phase ratios of Comparative Examples 2 and 3 were judged as fail "×". This is because it is believed that the discharge capacity decreases due to the inclusion of a large amount of phases other than the main phase (materials having a main peak between 25.3° and 25.7°).
[0063] (discharge capacity) The discharge capacity was measured for each of Examples 1 to 3 and Comparative Examples 1 to 3. The discharge capacity was measured in a thermostatic chamber at 25° C. with a cutoff potential of 1.0 V to 3.0 V (vs. Li / Li +The discharge capacity was measured by performing CC charging and discharging at 0.2 C with a discharge current of 1312 mAh / cm in Example 1. 3 In Example 2, it is 1209 mAh / cm 3 In Example 3, it is 1221 mAh / cm 3 In Comparative Example 1, it is 1122 mAh / cm 3 and in Comparative Example 2, 1076 mAh / cm 3 In Comparative Example 3, it was 1022 mAh / cm 3 The results of Example 1 are shown in FIG.
[0064] Discharge capacity is 1200mAh / cm 3 If the discharge capacity is more than 1200mAh / cm, the discharge capacity is judged as "pass" (○). 3 If the angle was less than 25.3°, the discharge capacity was judged as a failure "x". The discharge capacities of Examples 1 to 3 were judged as a pass "◯". On the other hand, the discharge capacities of Comparative Examples 1 to 3 were judged as a failure "x". This is thought to be because the capacity was reduced by including a large amount of phases other than the main phase (materials having a main peak at 25.3° or more and 25.7° or less).
[0065] The results are shown in Table 1. [Table 1]
[0066] From the above results, it was confirmed that high capacity was achieved by the negative electrode active materials of Examples 1 to 3. Next, the cycle characteristics and rate characteristics were also examined.
[0067] (Cycle characteristics) The cycle characteristics were measured for each of Examples 1 to 3 and Comparative Examples 1 to 3. The cycle characteristics were measured in a thermostatic chamber at 25° C. with a cutoff potential of 1.0 V to 3.0 V (vs. Li / Li +After 30 cycles of CC charging and discharging at 0.2 C as a constant current (C), the capacity retention rate was calculated from the initial discharge capacity to evaluate. The capacity retention rate after 30 cycles was 88.4% in Example 1, 87.2% in Example 2, 86.9% in Example 3, 90.3% in Comparative Example 1, 76.4% in Comparative Example 2, and 78.7% in Comparative Example 3.
[0068] If the capacity retention rate after 30 cycles was 80% or more, the cycle characteristics were judged as pass "○", and if the capacity retention rate after 30 cycles was less than 80%, the cycle characteristics were judged as fail "×". The cycle characteristics of Examples 1 to 3 were judged as pass "○". On the other hand, the cycle characteristics of Comparative Examples 2 and 3 were judged as fail "×". This is thought to be because the electrode had significant cycle deterioration due to the inclusion of a large amount of phase other than the main phase (material having a main peak at 25.3° or more and 25.7° or less).
[0069] Next, the discharge capacity of an electrode active material in which two types of negative electrode active materials were mixed was examined.
[0070] Example 4 In Example 4, Al2Nb 50 O 128 The negative electrode active material is AlNb 11 O 29 The discharge capacity of the mixture was measured using the negative electrode active material. 3 , which was higher than the discharge capacity of Comparative Example 1. As shown in FIG. 10, peak intensities were measured in an XRD measurement using CuKα radiation. The sum of the peak intensity at 25.6° and the peak intensity at 26.0° was set to 100, and the ratio (%) of each peak intensity was measured. The peak intensity ratio at 25.6° was 32%, and the peak intensity ratio at 26.0° was 68%. The results are shown in Table 2. [Table 2]
[0071] Example 5 In Example 5, Al2Nb50 O 128 The negative electrode active material is AlNb 11 O 29 The negative electrode active material was mixed and sintered. In an XRD measurement using CuKα radiation, the peak intensity was measured. The sum of the peak intensity at 25.6° and the peak intensity at 26.0° was taken as 100, and the ratio (%) of each peak intensity was measured. A peak at 25.6° was confirmed, and even after mixing and sintering, Al2Nb 50 O 128 The presence of Al2Nb 50 O 128 The negative electrode active material is AlNb 11 O 29 It was confirmed that the reaction between the active materials was suppressed even when the negative electrode active material was mixed and fired. The results are shown in Table 3. [Table 3]
[0072] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to such specific embodiments, and various modifications and variations are possible within the scope of the gist of the present invention described in the claims. [Explanation of symbols]
[0073] 10 1st internal electrode 11 Electrode active material 12 Solid electrolyte 13 Conductive additives 15 First current collector layer 20 Second internal electrode 21 Electrode active material 22 Solid electrolyte 23 Conductive additives 25 Second collector layer 30 Solid electrolyte layer 40a First external electrode 40b 2nd external electrode 50 Cover Layer 51 Solid electrolyte green sheet 52 Internal electrode paste 53 Reverse pattern 54 Cover Sheet 55 External electrode paste 60 Stacked Chips 100,100a solid state battery 110 Li metal 120 Electrolyte 130 Mixed electrode 140 Current collecting foil 200 Lithium-ion battery
Claims
1. The electrode active material includes a negative electrode active material which contains Al and Nb, belongs to the space group C2 / m, and has a main peak at 25.3° or more and 25.7° or less in XRD measurement using CuKα radiation.
2. The negative electrode active material is represented by the general formula Al 2+x Nb 50 O 128+1.5x The electrode active material according to claim 1, which is represented by a composition formula of (-0.1≦x≦0.1).
3. The electrode active material according to claim 1 , further comprising another negative electrode active material having a different composition from the negative electrode active material.
4. The negative electrode active material is Al 2 Nb 50 O 128 and The electrode active material further comprises AlNb 11 O 29 The electrode active material of claim 3 comprising:
5. An oxide-based solid electrolyte layer; a first electrode layer provided on a first main surface of the oxide-based solid electrolyte layer and including a positive electrode active material; A second electrode layer provided on a second main surface of the oxide-based solid electrolyte layer and containing the electrode active material according to claim 1 .
Citation Information
Patent Citations
All-solid cell
WO2014038311A1
Electrode active material for electrochemical element and method for producing same, electrode material for electrochemical element, electrode for electrochemical element, electrochemical element, and mobile object