Curable composition, cured product of curable composition and method for producing cured product

A curable composition with a transition metal complex, silicon compound, and organic compound addresses storage stability and toughness issues, enhancing light transmittance and mechanical properties for semiconductor device applications.

JP2024151784APending Publication Date: 2024-10-25ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023065488
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Conventional curable compositions used in semiconductor devices face issues with storage stability, light transmittance at 400 nm, and toughness, leading to undesirable yellow color and decreased mechanical properties.

Method used

A curable composition comprising a transition metal complex with a pincer-type ligand, a silicon compound with SiH groups, and an organic compound with carbon-carbon double bonds, specifically designed to enhance storage stability, light transmittance, and toughness through controlled hydrosilylation reactions.

Benefits of technology

The composition achieves excellent storage stability, high transmittance of light at 400 nm, and good toughness, resulting in improved performance for semiconductor device protection and optical applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024151784000001
    Figure 2024151784000001
  • Figure 2024151784000002
    Figure 2024151784000002
  • Figure 2024151784000003
    Figure 2024151784000003
Patent Text Reader

Abstract

To provide a curable composition, a cured product and a method for producing the same, which have excellent storage stability, a high transmittance of light at a wavelength of 400 nm after curing and good toughness.SOLUTION: There is provided a curable composition which comprises: a transition metal complex (a) having a transition metal and a pincer-type ligand having two or more ligand sites containing a phosphorus atom or a nitrogen atom and a carbon-transition metal bonding site; a silicon compound (b) having at least two SiH groups in one molecule; and an organic compound (c) having at least two carbon-carbon double bonds in one molecule, in which at least one of the carbon-carbon double bonds is an internal double bond.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable composition, a cured product of the curable composition, and a method for producing the cured product. [Background technology]

[0002] Silicon-containing resins exhibit good stability due to the high bond energy of silicon-carbon bonds and the like present in the skeleton, and are therefore used in a wide range of applications, such as protective and sealing materials for semiconductor elements such as light-emitting diode elements, or materials for lenses and other optical components. In particular, silicon-containing curable compositions are used as sealing materials and protective coating materials for optical semiconductor elements in optical semiconductor devices such as light-emitting diodes (LEDs).

[0003] For example, Patent Document 1 describes a one-component millable silicone rubber composition that has excellent storage stability at 40° C. or less, contains no solvent, and hardens with an extremely small amount of platinum catalyst.

[0004] Patent Document 2 proposes a curable composition that has good reactivity, can be easily produced, has good storage stability, and has low viscosity and excellent workability. The curable composition contains a carbon-carbon double bond reactive with a SiH group and a SiH group, and is obtained by subjecting an organic compound (A) containing at least one specific divalent group reactive with a SiH group in one molecule and a compound (B) containing at least two SiH groups in one molecule to a partial hydrosilylation reaction in the presence of a hydrosilylation catalyst (C). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2021-127373 [Patent Document 2] JP 2003-321484 A Summary of the Invention [Problem to be solved by the invention]

[0006] For example, a curable composition utilizing a hydrosilylation addition reaction has excellent properties, but there is room for improvement in terms of storage stability because the addition reaction proceeds even at room temperature after the preparation of the curable composition. Even if the composition shown in Patent Document 1 has excellent storage stability, conventional resin materials have problems such as a decrease in the toughness of the obtained curable composition due to various factors such as light absorption of the transition metal complex catalyst itself, thermal deterioration, and side reactions. In other words, no curable composition has been obtained that satisfies all of the storage stability of the curable composition, high transmittance of light with a wavelength of 400 nm, which greatly affects the yellowness of the cured product obtained from the curable composition, and toughness.

[0007] Accordingly, an object of the present invention is to provide a curable composition which has excellent storage stability, high transmittance at a wavelength of 400 nm after curing, and good toughness, a cured product thereof, and a method for producing the same. [Means for solving the problem]

[0008] Means for Solving the Problems of the Prior Art As a result of intensive research by the present inventors to solve the above problems of the prior art, the present inventors have found that the above problems can be solved by the following solving means, and have completed the present invention. That is, the present invention includes the following embodiments. <1> A transition metal complex (a) having a transition metal and a pincer-type ligand having two or more ligand sites containing a phosphorus atom or a nitrogen atom and a carbon-transition metal bond site; A silicon compound (b) having at least two SiH groups in one molecule; an organic compound (c) containing at least two carbon-carbon double bonds in one molecule, at least one of which is an internal double bond; A curable composition comprising: <2> The transition metal complex (a) has the formula (a1): [ka] (In formula (a1), Ar is an aromatic hydrocarbon moiety which may have a substituent, L is a ligand moiety containing a phosphorus atom or a nitrogen atom, and [Rh] is a rhodium moiety which may have a ligand.) <1> The curable composition according to claim 1. <3> The transition metal complex (a) is Formula (a2): [ka] (In formula (a2), R 1 , R 2 , R 3 , and R 4 are each independently an aliphatic hydrocarbon group having 1 to 18 carbon atoms or an aromatic hydrocarbon group having 6 to 20 carbon atoms; R 5 , R 6 , and R 7 are each independently a hydrogen atom, an aliphatic hydrocarbon group having 1 to 18 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms; [Rh] is a rhodium moiety which may contain a ligand; any two adjacent R 5 , R 6 , and R 7 may form a ring, the aliphatic hydrocarbon group and the aromatic hydrocarbon group may be substituted, and at least one carbon may be substituted with a heteroatom. or Formula (a3): [ka] (in formula (a3), R1, R2, R3, and R4 each independently represent an aliphatic hydrocarbon group having 1 to 18 carbon atoms or an aromatic hydrocarbon group having 6 to 20 carbon atoms; R5, R6, and R7 each independently represent a hydrogen atom, an aliphatic hydrocarbon group having 1 to 18 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms; [Rh] represents a rhodium moiety which may contain a ligand; any two adjacent R5, R6, and R7 may form a ring; the aliphatic hydrocarbon group and the aromatic hydrocarbon group may be substituted; and at least one carbon may be substituted with a heteroatom). <1> or <2> The curable composition according to claim 1. <4> L in the transition metal complex (a) is a coordination site containing a phosphorus atom; 31 P-NMR chemical shift values ​​are observed below 50 ppm in the magnetic field. <2> or <3> The curable composition according to claim 1. <5> The content of the transition metal complex (a) is 10 to 1000 mass ppm based on the transition metal atom with respect to the total amount of the curable composition. <1> ~ <4> 2. The curable composition according to claim 1 . <6> The silicon compound (b) has a siloxane skeleton. <1> ~ <5> 2. The curable composition according to claim 1 . <7> The SiH group in the silicon compound (b) has an alkyl group bonded to Si. <1> ~ <6> 2. The curable composition according to claim 1 . <8> The silicon compound (b) is 1,3,5,7-tetraalkylcyclotetrasiloxane or tetrakis(dialkylsilyloxy)silane; <1> ~ <7> 2. The curable composition according to claim 1 . <9> The content of the silicon compound (b) is 5 to 95 mass% based on the total amount of the curable composition. <1> ~ <8> 2. The curable composition according to claim 1 . <10> The organic compound (c) has a monocyclic unsaturated hydrocarbon moiety. <1> ~ <9> 2. The curable composition according to claim 1 . <11> The organic compound (c) is at least one selected from the group consisting of vinylcyclohexene, limonene, myrcene, cyclooctadiene, cyclohexadiene, cyclopentadiene, and dicyclopentadiene. <1> ~ <10> 2. The curable composition according to claim 1 . <12> The content of the organic compound (c) is 5 to 95% by mass based on the total amount of the curable composition. <1> ~ <11> 2. The curable composition according to claim 1 . <13> <1> ~ <12> 2. A cured product of the curable composition according to claim 1 . <14> <1> ~ <12> 2. A method for producing a cured product, comprising a step of reacting a SiH group with a carbon-carbon double bond using the curable composition according to claim 1. Effect of the Invention

[0009] According to the present invention, it is possible to provide a curable composition which has excellent storage stability, high transmittance at a wavelength of 400 nm after curing, and good toughness, a cured product thereof, and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention (hereinafter also referred to as "the present embodiment") will be described in detail. Note that the following embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content, and the present invention can be implemented in various modified forms within the scope of its gist.

[0011] [Curable composition] The curable composition according to the present embodiment is A transition metal complex (a) having a transition metal and a pincer-type ligand having two or more ligand sites containing a phosphorus atom or a nitrogen atom and a carbon-transition metal bond site; A silicon compound (b) having at least two SiH groups in one molecule; an organic compound (c) containing at least two carbon-carbon double bonds in one molecule, at least one of which is an internal double bond; Contains. According to the present embodiment, it is possible to provide a curable composition having excellent storage stability, high transmittance of light with a wavelength of 400 nm after curing, and good toughness, a cured product thereof, and a method for producing the same.

[0012] [Transition metal complex (a)] The curable composition according to the present embodiment contains a transition metal complex (a). The transition metal complex (a) has a transition metal and a pincer ligand. The transition metal complex (a) preferably functions as a hydrosilylation catalyst.

[0013] Examples of transition metals include platinum, rhodium, iridium, iron, aluminum, palladium, nickel, titanium, etc. Among these, rhodium is preferred.

[0014] Pincer ligands have two or more ligand sites containing phosphorus or nitrogen atoms and a carbon-transition metal binding site.

[0015] The transition metal complex (a) preferably has the formula (a1): [ka] (In formula (a1), Ar is an aromatic hydrocarbon moiety which may have a substituent, L is a ligand moiety containing a phosphorus atom or a nitrogen atom, and [Rh] is a rhodium moiety which may contain a ligand.)

[0016] The transition metal complex (a) is more preferably represented by the formula (a2): [ka] (In formula (a2), R 1 , R 2 , R 3 , and R 4are each independently an aliphatic hydrocarbon group having 1 to 18 carbon atoms or an aromatic hydrocarbon group having 6 to 20 carbon atoms; R 5 , R 6 , and R 7 are each independently a hydrogen atom, an aliphatic hydrocarbon group having 1 to 18 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms; [Rh] is a rhodium moiety which may contain a ligand; any two adjacent R 5 , R 6 , and R 7 may form a ring, the aliphatic hydrocarbon group and the aromatic hydrocarbon group may be substituted, and at least one carbon may be substituted with a hetero atom.

[0017] The aliphatic hydrocarbon group having 1 to 18 carbon atoms may be linear, branched, or cyclic. Examples of the aliphatic hydrocarbon group include a methyl group, a tert-butyl group, a cyclohexyl group, and an adamantyl group.

[0018] Examples of the aromatic hydrocarbon group having 6 to 20 carbon atoms include a phenyl group, a tolyl group, a xylyl group, and a naphthyl group.

[0019] R 1 , R 2 , R 3 , and R 4 The aliphatic hydrocarbon group in is preferably branched or cyclic. The number of carbon atoms in the aliphatic hydrocarbon group is preferably 3 to 10, and more preferably 3 to 8. 1 , R 2 , R 3 , and R 4 is preferably a branched or cyclic aliphatic hydrocarbon group having 3 to 10 carbon atoms, and more preferably a tert-butyl group or a cyclohexyl group.

[0020] R 5 , R 6 , and R 7 is preferably a hydrogen atom.

[0021] Rh in [Rh] is not particularly limited and may be monovalent or trivalent. [Rh] includes, for example, RhCl2, RhBr2, Rh(Cl)(Br), RhH2, RhH(OH), Rh(OH)2, RhHCl, RhHBr, RhH(Me), RhH(OAc), Rh(OAc)2, RhH(acac), RhH(SPh), RhCl(Me), RhBr(Me), RhI(Me), RhCl(CH2Ph), and RhBr(CH2Ph).

[0022] Examples of the complex represented by formula (a2) include (2,6-bis(di-tert-butylphosphinomethyl)phenyl)acetylacetonate hydridorodium, (2,6-bis(di-tert-butylphosphinomethyl)phenyl)acetatohydridorodium, (2,6-bis(di-cyclohexylphosphinomethyl)phenyl)acetylacetonate hydridorodium, (2,6-bis(di-cyclohexylphosphinomethyl)phenyl)acetatohydridorodium, (2,6-bis(di-phenylphosphinomethyl)phenyl)acetylacetonate hydridorodium, (2,6-bis(di-phenylphosphinomethyl)phenyl)acetatohydridorodium, and the like.

[0023] The transition metal complex (a) preferably has the formula (a3): [ka] (In formula (a3), R1, R2, R3, and R4 are each independently an aliphatic hydrocarbon group having 1 to 18 carbon atoms or an aromatic hydrocarbon group having 6 to 20 carbon atoms; R5, R6, and R7 are each independently a hydrogen atom, an aliphatic hydrocarbon group having 1 to 18 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms; [Rh] is a rhodium moiety which may contain a ligand; any two adjacent R5, R6, and R7 may form a ring; the aliphatic hydrocarbon group and the aromatic hydrocarbon group may be substituted; and at least one carbon may be substituted with a heteroatom.)

[0024] In the formula (a3), the aliphatic hydrocarbon group having 1 to 18 carbon atoms, the aromatic hydrocarbon group having 6 to 20 carbon atoms, and [Rh] have the same meaning as in the formula (a2).

[0025] Examples of the complex represented by formula (a3) ​​include bis(acetato)aqua[4,6-bis(4-isopropyl-2-oxazolin-2-yl)-m-xylene]rhodium, bis(acetato)aqua[4,6-bis(4-isopropyl-2-oxazolin-2-yl)-benzene]rhodium, bis(acetato)aqua[4,6-bis(4-phenyl-2-oxazolin-2-yl)-benzene]rhodium, acetylacetonato(aqua)[4,6-bis(4-isopropyl-2-oxazolin-2-yl)-m-xylene]rhodium, acetylacetonato(aqua)[4,6-bis(4-isopropyl-2-oxazolin-2-yl)-benzene]rhodium, and acetylacetonato(aqua)[4,6-bis(4-phenyl-2-oxazolin-2-yl)-benzene]rhodium.

[0026] (Method for producing transition metal complex (a)) The method for producing the transition metal complex (a) can be, for example, to react a halogenated transition metal with a pincer ligand to obtain a halogenated hydride transition metal complex having a pincer ligand. The halogenated hydride complex may also be reacted with an alkali metal compound such as sodium acetylacetonate to substitute the ligand bonded to the transition metal. The pincer ligand may be represented by the formula (a2-1): [ka] (In formula (a2-1), R 1 , R 2 , R 3 , and R 4 are each independently an aliphatic hydrocarbon group having 1 to 18 carbon atoms or an aromatic hydrocarbon group having 6 to 20 carbon atoms; R 5 , R 6 , and R 7are each independently a hydrogen atom, an aliphatic hydrocarbon group having 1 to 18 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms, and any two adjacent R 5 , R 6 , and R 7 may form a ring, the aliphatic hydrocarbon group and the aromatic hydrocarbon group may be substituted, and at least one carbon may be substituted with a heteroatom.

[0027] (Mixing ratio of transition metal complex (a)) The amount of the transition metal complex (a) used is not particularly limited as long as it is an effective amount as a catalyst, but is preferably 0.1 to 10,000 ppm based on the transition metal atom relative to the total amount of the curable composition, and more preferably 10 to 1,000 ppm from the viewpoint of both suppressing coloring and high reaction activity. By using the transition metal complex (a) in the above range, the time required for the curing reaction becomes appropriate, and coloring of the cured product tends to be further suppressed.

[0028] <Silicon compounds (b)> The silicon compound (b) has at least two SiH groups in one molecule. Because the silicon compound (b) has two SiH groups, it reacts with the organic compound (c) containing at least two carbon-carbon double bonds in one molecule, which will be described later, to form a network-like cured product.

[0029] The silicon compound (b) preferably has a siloxane skeleton, which can enhance the heat resistance of the cured product of the curable composition.

[0030] The SiH group in the silicon compound (b) preferably has an alkyl group bonded to Si. The alkyl group is not particularly limited, but may be, for example, an alkyl group having 1 to 10 carbon atoms (preferably 1 to 4 carbon atoms). Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an n-butyl group, and a tert-butyl group.

[0031] The silicon compound (b) is preferably a cyclic siloxane. The silicon compound (b) preferably has a 4- to 10-membered cyclic siloxane structure, more preferably has a 6- to 8-membered cyclic siloxane structure, and further preferably has an 8-membered cyclic siloxane structure.

[0032] In the case of a cyclic siloxane, the silicon compound (b) is preferably a 1,3,5,7-tetraalkylcyclotetrasiloxane, and more preferably 1,3,5,7-tetramethylcyclotetrasiloxane.

[0033] The silicon compound (b) is preferably a branched siloxane.The silicon compound (b) is preferably a 4-substituted dialkylsilyloxysilane.

[0034] In the case of a branched siloxane, the silicon compound (b) is preferably tetrakis(dialkylsilyloxy)silane, and more preferably tetrakis(dimethylsilyloxy)silane.

[0035] Among the above, the silicon compound (b) is preferably 1,3,5,7-tetraalkylcyclotetrasiloxane or tetrakis(dialkylsilyloxy)silane, and more preferably 1,3,5,7-tetramethylcyclotetrasiloxane or tetrakis(dimethylsilyloxy)silane.

[0036] The content of the silicon compound (b) is preferably from 5 to 95% by mass, more preferably from 10 to 90% by mass, and preferably from 20 to 80% by mass, based on the total amount of the curable composition.

[0037] <Organic compounds (c)> The organic compound (c) contains at least two carbon-carbon double bonds in one molecule, at least one of which is an internal double bond. The organic compound (c) contains at least two carbon-carbon double bonds in one molecule, and thus forms a crosslinked structure by reaction with the silicon compound (b).

[0038] In the organic compound (c), at least one of the carbon-carbon double bonds is an internal double bond. The term "internal double bond" refers to a carbon-carbon double bond in which at least one carbon is bonded to each of the two carbons forming the double bond. Since the internal double bond exhibits a lower activity against hydrosilylation than the terminal double bond, the organic compound (c) can have an internal double bond at least one of the carbon-carbon double bonds, thereby improving the storage stability. From the viewpoint of further improving the storage stability, it is preferable that the portion containing the internal double bond is not a norbornene portion. In addition, from the viewpoint of further improving the storage stability, it is preferable that at least two of the carbon-carbon double bonds in the organic compound (c) are internal double bonds, and it is more preferable that all of the carbon-carbon double bonds are internal double bonds.

[0039] The organic compound (c) preferably has a monocyclic unsaturated hydrocarbon moiety as a moiety containing an internal double bond. Examples of the monocyclic unsaturated hydrocarbon moiety include a cyclohexene moiety, a cyclohexadiene moiety, a cyclopentene moiety, a cyclopetadiene moiety, a cycloheptene moiety, a cyclooctene moiety, and a cyclooctadiene moiety.

[0040] The organic compound (c) preferably has one terminal double bond.

[0041] Examples of the organic compound (c) include vinylcyclohexene, limonene, myrcene, cyclooctadiene, cyclohexadiene, cyclopentadiene, and dicyclopentadiene. Among these, vinylcyclohexene or limonene is preferable.

[0042] The content of the organic compound (c) is preferably 5 to 95 mass %, more preferably 10 to 90 mass %, and preferably 20 to 80 mass %, based on the total amount of the curable composition.

[0043] In the curable composition of this embodiment, the combination of the silicon compound (b) and the organic compound (c) makes it possible to realize high storage stability and good transparency to 400 nm light and good toughness of the cured product obtained from the curable composition of this embodiment.

[0044] With regard to the ratio of silicon compound (b) to organic compound (c) in the curable composition according to this embodiment, the molar ratio of Si-H groups in silicon compound (b) to carbon-carbon unsaturated bonds in organic compound (c) [[Si-H groups (mol) in silicon compound (b)] / [carbon-carbon unsaturated bonds (mol) in organic compound (c)]] is preferably 0.5 to 2.0, more preferably 0.6 to 1.4, and even more preferably 0.8 to 1.2, from the viewpoint of obtaining better toughness.

[0045] The curable composition of the present embodiment may contain, in addition to the above components, an adhesion improver, an antioxidant, a viscosity modifier, a hardness modifier, or other components as necessary.

[0046] <Adhesion improver> The curable composition of the present embodiment further contains an adhesion improver, and thus tends to have improved adhesion to the substrate. The adhesion improver is not particularly limited, but examples thereof include acrylic silane coupling agents, epoxy silane coupling agents, and silane coupling agents having a norbornyl group. Examples of acrylic silane coupling agents include methacrylopropyl trimethoxysilane, methacrylopropyl dimethoxysilane, methacrylopropyl triethoxysilane, methacrylopropyl diethoxysilane, acrylopropyl trimethoxysilane, acrylopropyl dimethoxysilane, acrylopropyl triethoxysilane, and acrylopropyl diethoxysilane. Examples of epoxy silane coupling agents include glycidyl propyl trimethoxysilane and glycidyl propyl triethoxysilane. Examples of silane coupling agents having a norbornyl group include norbornyl ethyl trimethoxysilane, norbornyl ethyl dimethoxysilane, norbornyl ethyl triethoxysilane, and norbornyl ethyl diethoxysilane. These may be used alone or in combination of two or more.

[0047] From the viewpoint of further improving the adhesion to the adherend, the content of the adhesion improver is preferably 0.1 to 10 mass %, and more preferably 1 to 5 mass %, based on the total amount of the curable composition.

[0048] <Antioxidants> The curable composition of the present embodiment may contain an antioxidant. Examples of the antioxidant include 2,6-di-t-butyl-4-methylphenol, 2,5-di-t-amylhydroquinone, 2,5-di-t-butylhydroquinone, 4,4'-butylidenebis(3-methyl-6-t-butylphenol), 2,2'-methylenebis(4-methyl-6-t-butylphenol), 2,2'-methylenebis(4-ethyl-6-t-butylphenol), Irganox1010, Irganox1035, and Irganox3114. These may be used alone or in combination of two or more.

[0049] The content of the antioxidant is preferably 10 to 10,000 ppm, and more preferably 100 to 5,000 ppm, based on the total amount of the curable composition.

[0050] <Viscosity modifier / hardness modifier> In order to adjust the viscosity of the curable composition of this embodiment or the hardness of a cured product obtained from the curable composition of this embodiment, a linear diorganopolysiloxane or a network organopolysiloxane having an alkenyl group or SiH bonded to a silicon atom; a non-reactive linear or cyclic diorganopolysiloxane (i.e., having no alkenyl group or SiH bonded to a silicon atom), a silphenylene compound, or the like may be blended as a viscosity modifier and / or hardness modifier.

[0051] <Other additives> In order to ensure a pot life, an addition reaction inhibitor such as 1-ethynylcyclohexanol, 3,5-dimethyl-1-hexyn-3-ol, etc. may be blended in. Furthermore, to improve strength, an inorganic filler such as fumed silica may be blended in so far as it does not affect transparency, and dyes, pigments, flame retardants, etc. may be blended as necessary.

[0052] Furthermore, a light stabilizer can be used to impart resistance to photodegradation caused by light energy such as sunlight and fluorescent lamps. As the light stabilizer, a hindered amine stabilizer that captures radicals generated by photooxidation degradation is suitable, and by using it in combination with an antioxidant, the antioxidant effect tends to be further improved. Specific examples of light stabilizers include bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate and 4-benzoyl-2,2,6,6-tetramethylpiperidine. A plasticizer may also be added to prevent cracking. Other addition reaction conditions, the use of solvents, etc. are not particularly limited and normal conditions can be adopted.

[0053] [Production of Curable Composition] The curable composition according to the present embodiment can be produced by mixing in advance and partially hydrosilylating the transition metal complex (a) and the silicon compound (b) in the presence of the organic compound (c). The reaction can be carried out by simply mixing, or by heating. From the viewpoint of suppressing the volatilization of the compound and reducing the generation of bubbles in the cured product, the method of partially reacting in advance by heating is preferred.

[0054] The reaction temperature is preferably 30 to 180° C., more preferably 60 to 150° C., and further preferably 80 to 120° C. If the reaction temperature is low, the reaction time for sufficient reaction becomes long, and if the reaction temperature is high, it tends to be difficult to carry out the reaction.

[0055] The reaction may be carried out at a constant temperature, but if necessary, the temperature may be changed in multiple steps or continuously.

[0056] After the reaction, the volatile matter may be removed by maintaining the mixture at room temperature or under heating under normal or reduced pressure.

[0057] [Cured product] The cured product according to this embodiment is obtained by curing the curable composition according to the above embodiment. The curable composition is cured by forming a network structure through hydrosilylation of the silicon compound (b), which is a component of the curable composition, with the organic compound (c). More specifically, curing proceeds by reacting the SiH group with the carbon-carbon double bond.

[0058] The internal transmittance of the cured product according to this embodiment to light having a wavelength of 400 nm is preferably 80% or more, more preferably 85% or more, and even more preferably 90 to 99%. The method for measuring the internal transmittance to light having a wavelength of 400 nm is the method described in the Examples.

[0059] The tensile modulus of the cured product according to this embodiment is preferably 50 MPa or more, more preferably 100 MPa or more, and even more preferably 200 MPa or more. The upper limit of the tensile modulus is not particularly limited, but may be, for example, 1000 MPa or less. The tensile modulus is measured by the method described in the Examples.

[0060] The breaking energy of the cured product according to this embodiment is preferably 0.10 J or more, more preferably 0.15 J or more, and even more preferably 0.20 J or more. The breaking energy is not particularly limited in its upper limit, but may be, for example, 10 J or less. The breaking energy is measured by the method described in the examples.

[0061] [Method of manufacturing the cured product] The method for producing a cured product according to this embodiment includes a step of reacting a SiH group with a carbon-carbon double bond using the curable composition according to this embodiment. This step is carried out by heating the curable composition according to this embodiment. The heating temperature is preferably 100 to 300°C, and more preferably 150 to 250°C.

[0062] The method for producing a cured product according to this embodiment may include a step of mixing the transition metal complex (a), the silicon compound (b), and the organic compound (c), and optionally other components, to prepare a curable composition.

[0063] The curable composition of the present invention and its cured product can be suitably used for protecting, sealing, and adhering semiconductor elements such as light-emitting diode elements, changing or adjusting the wavelength of light emitted from light-emitting diode elements, and for applications such as lenses, etc. Furthermore, the cured product of the present invention can also be suitably used for applications such as lens materials, materials for optical devices and optical components, various optical materials such as display materials, insulating materials for electronic devices and electronic components, coating materials, etc. EXAMPLES

[0064] The present embodiment will be described in more detail below with reference to examples, but the present embodiment is not limited to the following examples. The methods for measuring and evaluating physical properties in the examples and comparative examples are as follows.

[0065] [ 1 H-NMR measurement, 31 P-NMR measurement] NMR measurements were performed using a nuclear magnetic resonance spectrometer "ECZ400S" manufactured by JEOL Ltd. and a TFH probe as follows. A sample was mixed with 0.02 g of sample and 1 g of deuterated toluene. 1 H-NMR or 31 P-NMR measurements were performed. In addition, 1 In the H-NMR measurement, the reference peak of the deuterated solvent was set to 2.08 ppm, and the measurement was performed with 32 accumulations. 31 In the P-NMR measurement, the peak observed in 85% phosphoric acid was set as the standard (0 ppm), and the measurement was performed with 128 accumulations.

[0066] [Internal transmittance of light with a wavelength of 400 nm] For the curable compositions and cured products prepared in the examples and comparative examples, the transmittance of light from 350 to 800 nm was measured with an optical path length of 1.0 mm using a transmittance measuring device (spectrophotometer "U-4100" manufactured by Hitachi High-Technologies Corporation), and the internal transmittance (%) of light with a wavelength of 400 nm was extracted.

[0067] [Storage stability test] 200 mg of the oily curable compositions prepared in the Examples and Comparative Examples were placed in a 9 mL sample bottle and allowed to stand at 40° C. for 10 days. The internal transmittance of the curable compositions at a wavelength of 400 nm was then measured, and the properties were further evaluated. For the liquid curable compositions before and after the above test, the transmittance of light from 350 to 800 nm with an optical path length of 1.0 mm was measured using a transmittance measuring device (spectrophotometer "U-4100" manufactured by Hitachi High-Technologies Corporation), and the internal transmittance (%) of light with a wavelength of 400 nm was extracted. The degree of decrease ΔT (%) in the internal transmittance of light with a wavelength of 400 nm before and after the test was calculated using the following formula. ΔT(%) = [Transmittance of light with a wavelength of 400 nm before the test (%)] - [Transmittance of light with a wavelength of 400 nm after the test (%)] The properties of the curable compositions after the above tests were evaluated according to the following criteria. <Standards> A: It was a fluid liquid. B: Partially solidified C: Completely solidified

[0068] [Tensile test (tensile modulus, breaking energy)] Using a precision universal testing machine "AG-5000D" manufactured by Shimadzu Corporation, a tensile test was performed at 25°C with a chuck distance of 1.5 cm and a 500 kgf load cell at a tensile speed of 1 mm per minute to determine the tensile modulus, tensile elongation, and breaking energy. The breaking energy was the energy up to the breaking point. The test sample used was a rectangular sample with a long side of 5.0 cm, a short side of 0.5 cm, and a thickness of 1.0 mm.

[0069] [Synthesis of transition metal complex (a)] [Synthesis Example 1] A magnetic stirrer and a condenser were set in a 30 mL Schlenk flask. 182 mg (0.69 mmol) of rhodium(III) chloride trihydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 385 mg (1.0 mol) of 1,3-bis(di-tert-butylphosphinomethyl)benzene (manufactured by Sigma-Aldrich Co., Ltd.), 5.0 mL of isopropanol, and 0.25 mL of water were added to the flask and stirred at 25°C under a nitrogen atmosphere. After stirring at 25°C for 24 hours, the mixture was heated and stirred at 85°C in an oil bath for 8 hours. After heating, the reaction solution was filtered while still at 85°C, and the filtrate was recrystallized at -10°C to recover 210 mg (0.39 mmol) of (2,6-bis(di-tert-butylphosphinomethyl)phenyl)chlorohydridorhodium. Regarding the compound obtained, 1H-NMR (7.2~6.8ppm(Ar-H), 3.2~2.8ppm(Ar-CH2-), 1.4~1.1ppm(tBu), -27.3~-27.7ppm(Rh-H)) 31 P-NMR (75.0 ppm, J Rh - P Its generation was confirmed at a frequency of 117 Hz. The obtained (2,6-bis(di-tert-butylphosphinomethyl)phenyl)chlorohydridorodium (53.3 mg, 0.10 mmol), sodium acetylacetonate hydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) (0.10 mol) and chloroform (1.0 mL) were mixed and stirred at 25°C for 3 hours under a nitrogen atmosphere. After filtering the reaction solution, the filtrate was recrystallized at -10°C to recover 32.2 mg of (2,6-bis(di-tert-butylphosphinomethyl)phenyl)acetylacetonate hydridorodium (hereinafter also referred to as "transition metal complex (a1)"). Regarding the obtained compound, 1 H-NMR (7.2~6.6ppm(Ar-H), 5.4~5.1ppm(C-H), 3.4~2.7ppm(Ar-CH2-), 1.8~1.6ppm(Me), 1.4~1.1ppm(tBu), -19.1~-19.5ppm(Rh-H)) 31 P-NMR (78.6 ppm, J Rh - P Its generation was confirmed at a frequency of 117 Hz.

[0070] Example 1 In a flask equipped with a stirrer and a cooling tube, 1.51 g (6.28 mmol) of 1,3,5,7-tetramethylcyclotetrasiloxane (manufactured by Tokyo Chemical Industry Co., Ltd., hereinafter also referred to as "D4H") as compound (b), 1.13 g (10.5 mmol) of 4-vinylcyclohexene (manufactured by Tokyo Chemical Industry Co., Ltd., hereinafter also referred to as "VCH") as compound (c), and 2.0 mg (corresponding to 100 ppm in terms of rhodium atoms) of the transition metal complex (a1) obtained in Synthesis Example 1 as transition metal complex (a) were added, and the mixture was heated to 100°C in an oil bath under a nitrogen atmosphere and stirred. After heating at 100°C for 2 hours, the mixture was cooled to room temperature to obtain an oily curable composition. Regarding the obtained curable composition,1 The complete consumption of the raw material was confirmed by H-NMR measurement. In addition, the peak of the methyl group bonded to Si was observed in the region of 0 to 0.3 ppm, the peak of the compound (c) after the reaction was observed in the region of 0.3 to 2.7 ppm, and the peak of the vinyl group remaining in the compound (c) after the reaction was observed in the region of 4.5 to 6.5 ppm. The obtained curable composition was stirred and degassed, and then 2.00 g of the curable composition was poured into a 5 cmΦ aluminum cup and degassed under reduced pressure, and then preheated for 1 hour in an oven adjusted to 200° C. It was further heated for 2 hours in an oven adjusted to 220° C. to produce a cured product with a thickness of 1.0 mm.

[0071] Example 2 A curable composition and a cured product were obtained in the same manner as in Example 1, except that bis(acetato)aqua[(S,S)-4,6-bis(4-isopropyl-2-oxazolin-2-yl)-m-xylene]rhodium (manufactured by Tokyo Chemical Industry Co., Ltd., hereinafter also referred to as "transition metal complex (a2)") was used as the transition metal complex (a). Detailed results are shown in Table 1. Regarding the obtained curable composition, 1 The complete consumption of the raw material was confirmed by H-NMR measurement. In addition, the peak of the methyl group bonded to Si was observed in the region of 0 to 0.3 ppm, the peak of the compound (c) after the reaction was observed in the region of 0.3 to 2.7 ppm, and the peak of the vinyl group remaining in the compound (c) after the reaction was observed in the region of 4.5 to 6.5 ppm.

[0072] Example 3 A curable composition was obtained in the same manner as in Example 1, except that tetrakis(dimethylsilyloxy)silane (manufactured by Tokyo Chemical Industry Co., Ltd.) was used as compound (b). A cured product having a thickness of 1.0 mm was produced from the obtained curable composition, but the obtained cured product had a strength sufficient for a tensile test. The detailed results are shown in Table 1. Regarding the obtained curable composition, 1The complete consumption of the raw material was confirmed by H-NMR measurement. In addition, the peak of the methyl group bonded to Si was observed in the region of 0 to 0.3 ppm, the peak of the compound (c) after the reaction was observed in the region of 0.5 to 2.5 ppm, and the peak of the vinyl group remaining in the compound (c) after the reaction was observed in the region of 4.5 to 6.5 ppm.

[0073] Example 4 A curable composition was obtained in the same manner as in Example 2, except that tetrakis(dimethylsilyloxy)silane (manufactured by Tokyo Chemical Industry Co., Ltd.) was used as compound (b). A cured product having a thickness of 1.0 mm was produced from the obtained curable composition, but the obtained cured product had a strength sufficient for a tensile test. Detailed results are shown in Table 1. Regarding the obtained curable composition, 1 The complete consumption of the raw material was confirmed by H-NMR measurement. In addition, the peak of the methyl group bonded to Si was observed in the region of 0 to 0.3 ppm, the peak of the compound (c) after the reaction was observed in the region of 0.5 to 2.5 ppm, and the peak of the vinyl group remaining in the compound (c) after the reaction was observed in the region of 4.5 to 6.5 ppm.

[0074] Example 5 A curable composition and a cured product were obtained in the same manner as in Example 1, except that (R)-(+)-limonene (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used as the compound (c). Detailed results are shown in Table 1. Regarding the obtained curable composition, 1 The complete consumption of the raw materials was confirmed by H-NMR measurement. In addition, the peak of the methyl group bonded to Si was observed in the region of 0 to 0.3 ppm, the peak of the compound (c) after the reaction was observed in the region of 0.3 to 2.7 ppm, and the peak of the vinyl group remaining in the compound (c) after the reaction was observed in the region of 4.3 to 6.5 ppm.

[0075] Comparative Example 1 A curable composition and a cured product were obtained in the same manner as in Example 1, except that a xylene solution of Karstedt catalyst equivalent to 3.0% by weight of platinum atoms (manufactured by Umicore Japan, hereinafter also referred to as "catalyst c") was used as the catalyst in an amount of 20 ppm in terms of platinum atoms. Detailed results are shown in Table 1. Regarding the obtained curable composition, 1 The complete consumption of the raw material was confirmed by H-NMR measurement. In addition, the peak of the methyl group bonded to Si was observed in the region of 0 to 0.3 ppm, the peak of the compound (c) after the reaction was observed in the region of 0.3 to 2.7 ppm, and the peak of the vinyl group remaining in the compound (c) after the reaction was observed in the region of 4.5 to 6.5 ppm.

[0076] Comparative Example 2 A curable composition was obtained in the same manner as in Comparative Example 1, except that tetrakis(dimethylsilyloxy)silane (manufactured by Tokyo Chemical Industry Co., Ltd.) was used as the compound (b). The detailed results are shown in Table 1. Regarding the obtained curable composition, 1 The complete consumption of the raw material was confirmed by H-NMR measurement. In addition, the peak of the methyl group bonded to Si was observed in the region of 0 to 0.3 ppm, the peak of the compound (c) after the reaction was observed in the region of 0.5 to 2.5 ppm, and the peak of the vinyl group remaining in the compound (c) after the reaction was observed in the region of 4.5 to 6.5 ppm.

[0077] Comparative Example 3 A composition was obtained in the same manner as in Comparative Example 1, except that (R)-(+)-limonene (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used as compound (c). However, the composition remained in an oily state even after heating at 220°C for 2 hours, and no cured product was obtained. Detailed results are shown in Table 1.

[0078] Comparative Example 4 A composition was obtained by the same procedure as in Example 1, except that chlorotris(triphenylphosphine)rhodium(I) (manufactured by Tokyo Chemical Industry Co., Ltd., hereinafter also referred to as "transition metal complex (c1)") was used as a catalyst in an amount of 100 ppm in terms of rhodium atom, but no consumption of the vinyl compound was observed. Detailed results are shown in Table 1.

[0079] Comparative Example 5 A composition was obtained by the same operation as in Example 1, except that a transition metal complex (hereinafter also referred to as "transition metal complex (c2)") obtained by mixing (R)-(6,6'-dimethoxybiphenyl-2,2'-diyl)bis[bis(3,4,5-trimethoxyphenyl)phosphine] (manufactured by Sigma-Aldrich Co., Ltd.) and di-μ-chlorotetrakis(η-ethylene)dirhodium (manufactured by Fujifilm Wako Pure Chemical Co., Ltd.) in a molar ratio of 2:1 was used as a catalyst in an amount of 100 ppm in terms of rhodium atoms, but no consumption of the vinyl compound was observed. Detailed results are shown in Table 1. The transition metal complex (a4) was synthesized by citing the synthesis method disclosed in the literature "J.Am.Chem.Soc.,2014,136,34,12064-12072".

[0080] [Table 1]

[0081] The abbreviations in the table have the following meanings: D4H: 1,3,5,7-tetramethylcyclotetrasiloxane TDMSS: Tetrakis(dimethylsilyloxy)silane a1: Transition metal complex (a1) a2: Transition metal complex (a2) Catalyst C: Karstedt catalyst c1: Transition metal complex (c1) c2: Transition metal complex (c1) VCH: 4-vinylcyclohexene LM: Limonene

Claims

1. A transition metal complex (a) having a transition metal and a pincer-type ligand having two or more ligand sites containing a phosphorus atom or a nitrogen atom and a carbon-transition metal bond site; A silicon compound (b) having at least two SiH groups in one molecule; an organic compound (c) containing at least two carbon-carbon double bonds in one molecule, at least one of which is an internal double bond; A curable composition comprising:

2. The transition metal complex (a) is represented by the formula (a1): 【Chemistry 1】 (In formula (a1), Ar is an aromatic hydrocarbon moiety which may have a substituent, L is a ligand moiety containing a phosphorus atom or a nitrogen atom, and [Rh] is a rhodium moiety which may contain a ligand.)

3. The transition metal complex (a) is Formula (a2): 【Chemistry 2】 (In formula (a2), R 1 , R 2 , R 3 , and R 4 are each independently an aliphatic hydrocarbon group having 1 to 18 carbon atoms or an aromatic hydrocarbon group having 6 to 20 carbon atoms; R 5 , R 6 , and R 7 are each independently a hydrogen atom, an aliphatic hydrocarbon group having 1 to 18 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms; [Rh] is a rhodium moiety which may contain a ligand; any two adjacent R 5 , R 6 , and R 7 may form a ring, the aliphatic hydrocarbon group and the aromatic hydrocarbon group may be substituted, and at least one carbon may be substituted with a heteroatom. or Formula (a3): 【Chemistry 3】 (In formula (a3), R 1 , R 2 , R 3 , and R 4 are each independently an aliphatic hydrocarbon group having 1 to 18 carbon atoms or an aromatic hydrocarbon group having 6 to 20 carbon atoms; R 5 , R 6 , and R 7 are each independently a hydrogen atom, an aliphatic hydrocarbon group having 1 to 18 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms; [Rh] is a rhodium moiety which may contain a ligand; any two adjacent R 5 , R 6 , and R 7 wherein each of the aliphatic and aromatic hydrocarbon groups may be substituted, and at least one carbon may be substituted with a heteroatom.

4. L in the transition metal complex (a) is a coordination site containing a phosphorus atom, 31 3. The curable composition according to claim 2, wherein the P-NMR chemical shift values ​​are observed below 50 ppm in the field.

5. The curable composition according to claim 1, wherein the content of the transition metal complex (a) is 10 to 1000 ppm by mass based on the transition metal atom with respect to the total amount of the curable composition.

6. The curable composition according to claim 1 , wherein the silicon compound (b) has a siloxane skeleton.

7. The curable composition of claim 1 , wherein the SiH group in the silicon compound (b) has an alkyl group bonded to Si.

8. The curable composition according to claim 1, wherein the silicon compound (b) is a 1,3,5,7-tetraalkylcyclotetrasiloxane or a tetrakis(dialkylsilyloxy)silane.

9. The curable composition according to claim 1, wherein the content of the silicon compound (b) is 5 to 95 mass % based on the total amount of the curable composition.

10. The curable composition of claim 1 , wherein the organic compound (c) has a monocyclic unsaturated hydrocarbon moiety.

11. The curable composition according to claim 1, wherein the organic compound (c) is at least one selected from the group consisting of vinylcyclohexene, limonene, myrcene, cyclooctadiene, cyclohexadiene, cyclopentadiene, and dicyclopentadiene.

12. The curable composition according to claim 1, wherein the content of the organic compound (c) is 5 to 95 mass % based on the total amount of the curable composition.

13. A cured product of the curable composition according to any one of claims 1 to 12.

14. A method for producing a cured product, comprising a step of reacting a SiH group with a carbon-carbon double bond using the curable composition according to any one of claims 1 to 12.

Citation Information

Patent Citations

  • Curable composition, cured product and method for producing the same

    JP2003321484A

  • One-component millable type silicone rubber composition and cured product of the same