Physical property conversion type bond-exchange polyester resin
The bond-exchangeable polyester resin allows adjustment of mechanical properties by generating crosslinking points through transesterification, enabling conversion between thermoplastic and thermosetting states with enhanced remoldability and recyclability.
Patent Information
- Application Number
- JP2023065527
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-10-25
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional polymer resins have fixed physical properties determined by monomer selection and crosslinking agent presence during synthesis, limiting the ability to adjust flexibility and hardness post-polymerization.
A bond-exchangeable polyester resin utilizing a linear polymer with ester bonds and hydroxyl groups, capable of generating crosslinking points through transesterification, allowing adjustment of mechanical properties via heating conditions.
Enables conversion between thermoplastic and thermosetting states, offering adjustable mechanical properties and features like remoldability and recyclability.
Smart Images

Figure 2024151806000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a property-changing bond-exchangeable polyester resin. [Background technology]
[0002] Polymer resins are broadly classified into thermoplastic resins and cross-linked resins (thermosetting resins) depending on the presence or absence of cross-linking (chemical linkages between polymer chains). When polymer chains are linked by cross-linking, the elastic modulus increases, and this elastic modulus is correlated with the cross-link density.
[0003] Patent Document 1 describes a polyester resin having a polymer main chain containing multiple ester bonds and multiple covalent cross-linking moieties containing ester bonds and hydroxyl groups (OH groups), and a cross-linked polyester resin containing an ester exchange catalyst.
[0004] Non-Patent Document 1 describes the functionalization of epoxy cured resin by introducing transesterification type bond exchange crosslinks into the network structure of the resin. In addition, Non-Patent Document 2 describes the functionalization by introducing transesterification-type bond exchange crosslinks into the network structure of polyester cured resin. However, these Non-Patent Documents only focus on the remoldability and repairability of the advantages of resins containing bond exchange crosslinks, and do not describe the conversion of the physical properties of the resin. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] WO2020 / 045439 [Non-patent literature]
[0006] [Non-Patent Document 1] Montarnal, D.; Capelot, M.; Tournilhac, F.; Leibler, L., Science, 2011, 334, 965. [Non-Patent Document 2] Hayashi, M.; Yano, R.; Takasu, A., Polym. Chem., 2019, 10, 2047. Summary of the Invention [Problem to be solved by the invention]
[0007] However, in conventional wisdom, the physical properties of the resin obtained are determined by the selection of the monomer type and the presence or absence of a crosslinking agent during synthesis. In other words, there was a problem that the flexibility and hardness of the resin were made different at the initial stage and could not be adjusted after polymerization. Therefore, in the present invention, the object is to provide a property-changing bond-exchangeable polyester resin based on the "seamless material conversion concept from thermoplastic resin to crosslinked resin" by utilizing a bond exchange reaction between molecules. Here, the property-changing bond-exchangeable polyester resin means, as described below, a property-changing bond-exchangeable polyester resin that is mainly a linear polymer, a property-changing bond-exchangeable polyester resin raw material containing a linear polymer, and a property-changing bond-exchangeable polyester resin containing a crosslinking point generated by bond exchange in the property-changing bond-exchangeable polyester resin raw material (hereinafter, sometimes referred to as a "property-changing bond-exchangeable polyester resin containing a crosslinking point"), and further includes a property-changing bond-exchangeable polyester resin containing an activated crosslinking point, in which the crosslinking point is activated. [Means for solving the problem]
[0008] The present invention which solves the above problems is as follows. [1] A linear polymer, the linear polymer comprising a component part capable of generating a crosslinking point with another linear polymer by bond exchange via a transesterification reaction. [2] The linear polymer according to [1], wherein the constituent moiety contains an ester bond and a hydroxyl group. [3] The linear polymer according to [2], wherein the number average molecular weight of the linear polymer is 5,000 or more, the proportion of the ester bonds in the linear polymer is 15 or more per molecular chain, and the proportion of the hydroxyl groups in the linear polymer is 15 or more per molecular chain. [4] A property-converting bond-exchangeable polyester resin raw material, comprising the linear polymer according to any one of [1] to [3] and an ester exchange catalyst. [5] The property-converting bond-exchangeable polyester resin raw material according to [4], wherein the molar ratio of the transesterification catalyst to the hydroxyl groups (the hydroxyl groups:the transesterification catalyst) is 0.01 to 0.15 relative to the hydroxyl groups (or ester bonds). [6] A property-changing bond-exchangeable polyester resin containing crosslinking points, which is produced by crosslinking at least a portion of the constituent parts described in any one of [1] to [3], and contains crosslinking points between the linear polymer and the other linear polymer. [7] A property-changing bond-exchangeable polyester resin containing crosslinking points according to [6], which contains crosslinking points having a predetermined maximum stress, wherein the maximum stress of the resin consisting of a linear polymer not containing crosslinking points before it contains the crosslinking points is 1 MPa or less. [8] A property-changing bond-exchangeable polyester resin containing crosslinking points according to [7], which has a Young's modulus that is 10 times or more larger than the Young's modulus of a linear polymer that does not contain the crosslinking points before the crosslinking points are contained. [9] The present invention provides a property-changing bond-exchangeable polyester resin having activated crosslinking points, in which the crosslinking points of the property-changing bond-exchangeable polyester resin having the crosslinking points described in [6] are further activated.
[10] A method for producing a linear polymer according to [2], comprising a reaction of a thiol group with an epoxy group catalyzed by a transesterification catalyst, in which the molar ratio of thiol group:epoxy group is 1:0.75 to 0.75:1 (=1:1.33).
[11] The method for producing a linear polymer according to
[10] , wherein the molar ratio of the catalyst amount is 0.01 or more and 0.15 or less when the molar ratio of thiol groups:epoxy groups is 1:1.
[12] A method for producing a property-convertible bond-exchangeable polyester resin having crosslinking points, which is obtained by mixing a linear polymer having an ester bond and a hydroxyl group with an ester exchange catalyst and heating the mixture to form crosslinking points. Effect of the Invention
[0009] The property-changing bond-exchangeable polyester resin according to the present invention includes a thermosetting thermoplastic resin that does not belong to either a thermoplastic resin or a thermosetting (crosslinked) resin. In this case, a wide range of mechanical properties can be expressed depending on the heating conditions (temperature and time), so that it can be a property-changing resin. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic diagram showing (a) a property-changing bond-exchangeable polyester resin raw material and (b) a property-changing bond-exchangeable polyester resin containing crosslinking points, which are one embodiment of the present invention, and (c) an ester exchange reaction formula. [Diagram 2] FIG. 1 is a diagram showing the synthesis of a hydroxyl group-containing polyester (linear polymer). [Diagram 3] FIG. 1 shows the changes in storage modulus (G') and loss modulus (G'') of property-changing bond-exchangeable polyester resins containing crosslinking points produced at heating temperatures of (a) 100°C (Comparative Example 3), (b) 130°C (Comparative Example 4), (c) 160°C (Example 3), and (d) 190°C (Example 4). [Figure 4] FIG. 1 shows the stress-strain curves of the property-changing bond-exchangeable polyester resins containing crosslinking points produced at heating temperatures of (a) 100° C. (Comparative Example 3), 130° C. (Comparative Example 4), 160° C. (Example 3), and 190° C. (Example 4), and (b) Example 1 (linear polymer). [Diagram 5] FIG. 13 is a diagram showing a stress relaxation measurement at 200° C. of Example 4 (property-converting bond-exchangeable polyester resin containing crosslinking points). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, the embodiments of the present invention will be described with reference to the drawings. The present invention is not limited to the following embodiments, and changes, modifications, and improvements can be made without departing from the scope of the invention.
[0012] The resin obtained by the present invention is classified as a thermoplastic resin in the initial state, but is converted into a thermosetting resin by subsequent heat treatment. Furthermore, when thermal energy that activates bond exchange is applied to the final crosslinked resin (property-converting bond-exchangeable polyester resin containing crosslinking points), the constraints of the crosslinks are temporarily weakened, and the resin exhibits functions such as remolding. In other words, the resin obtained by the present invention is a thermosetting thermoplastic resin that does not belong to either a thermoplastic resin or a thermosetting (crosslinking) resin. In this case, it is a property-converting resin because it can express a wide range of mechanical properties depending on the heating conditions (temperature and time).
[0013] Specifically, the property-changing bond-exchangeable polyester resin containing crosslinking points is an invention in which intermolecular crosslinks are formed through an ester exchange reaction by adding an appropriate catalyst to a hydroxyl-containing polyester and heating it. The crosslink density can be adjusted by the degree of progress of the ester exchange reaction, and the mechanical properties of the resin can be freely adjusted even after polymer polymerization.
[0014] In addition, in the property-changing bond-exchangeable polyester resin containing crosslinking points, ester bonds, hydroxyl groups, and (ester exchange) catalysts are present, so reheating activates the bond exchange via the ester exchange reaction. Because the bond exchange temporarily activates molecular mobility, the resin exhibits useful functions such as remoldability, despite being a crosslinked resin.
[0015] That is, the resin obtained by the present invention is classified as a thermoplastic resin (property-changing bond-exchangeable polyester resin) in the initial state, but is converted into a thermosetting resin (property-changing bond-exchangeable polyester resin containing crosslinking points) by subsequent heat treatment. Furthermore, when thermal energy that activates bond exchange is applied to the property-changing bond-exchangeable polyester resin containing crosslinking points, the constraint of the crosslinking is temporarily weakened, and the property-changing bond-exchangeable polyester resin containing the activated crosslinking points exhibits functions such as remoldability.
[0016] As shown in Fig. 1(a), a linear polymer 2 contains a constituent part 6 that can generate a crosslinking point 7 with another linear polymer 2' by bond exchange via a transesterification reaction, and the constituent part 6 contains a hydroxyl group 4 and an ester bond 5. On the other hand, a property-changing bond-exchangeable polyester resin raw material 1 contains a linear polymer 2 (2') and a predetermined amount of a transesterification catalyst 3. As shown in Fig. 1(b), when a crosslinking point 7 (7') is generated by bond exchange via a transesterification reaction, the property-changing bond-exchangeable polyester resin raw material 1 becomes a property-changing bond-exchangeable polyester resin 8 containing a crosslinking point.
[0017] As shown in Fig. 1(c), the transesterification reaction occurs when the OH group (hydroxyl group) bonded to R2 attacks the R1-0 (C=0) bond of one of the many ester bonds present nearby due to the action of heat (Δ) and the transesterification catalyst (cat.) present nearby. The transesterification reaction then produces a crosslinking point where, for example, a linear polymer 2 is crosslinked with another linear polymer 2', and the property-changing bond-exchangeable polyester resin 8 containing the crosslinking point has a predetermined strength compared to the property-changing bond-exchangeable polyester resin raw material 1, corresponding to the crosslinking point formed. EXAMPLES
[0018] <Synthesis of hydroxyl group-containing polyester (linear polymer)> A hydroxyl-containing linear polyester (linear polymer) was prepared by a thiol-epoxy click reaction using tin octoate (Sn(Oct)2) as a catalyst, using a dithiol monomer (2-SH, Ethylene glycol bis(3-mercaptopropionate)) and a diepoxy monomer (2-epoxy, 2,2-Bis(4-glycidyloxyphenyl)propane) with an ester bond as shown in Figure 2 as starting materials. The epoxy ring-opening reaction generates new hydroxyl groups, so the linear polymer obtained has an inherent ester bond and hydroxyl group. The reaction was carried out by mixing the materials in a molar ratio of thiol group:epoxy group:Sn(Oct)2=1:1:0.05 and heating at 100oC for 24 hours.
[0019] The progress of the reaction was monitored by proton nuclear magnetic resonance spectroscopy ( 1 The molecular weight was confirmed by H-NMR measurement. The number average molecular weight measured by gel permeation chromatography (GPC) was about 8000. The obtained sample is referred to as Example 1 below. Regarding the diepoxy monomer, many other types of difunctional monomers can be used, such as 1,7-octadiene diepoxide, 1,5-hexadiene diepoxide, 1,4-butanediol diglycidyl ether, and 2,2'-(2,2,3,3,4,4,5,5-octafluorohexane-1,6-diyl)bis(oxirane). Regarding the dithiol monomer, many other types of difunctional monomers with ester bonds can be used, such as tetraethylene glycol bis(3-mercaptopropionate) and polyethylene glycol bis(3-mercaptopropionate).
[0020] The polyester obtained in Example 1 is a non-crosslinked polymer that is easily dissolved in a good solvent and behaves as a thermoplastic resin. It has also been found that if the above polymerization is carried out at 140°C or higher for 24 hours, polymerization and crosslinking (ester exchange reaction) proceed simultaneously, making it impossible to convert the thermoplastic resin into a thermosetting resin (Comparative Example 1). As another control experiment, in the reaction of a dicarboxylic acid compound (adipic acid) with the above diepoxy monomer at 100°C, polymerization and crosslinking (ester exchange reaction) proceed simultaneously, and no linear polyester was obtained (Comparative Example 2). In other words, it can be said that the reaction of a thiol group with an epoxy group is optimal for obtaining a hydroxyl group-containing linear polyester (linear polymer).
[0021] <Production of property-changing bond-exchangeable polyester resin containing crosslinking points> Since the Sn(Oct)2 mixed during polymerization also acts as a catalyst for the ester exchange reaction, it was not removed but was used as it was as a raw material for a property-changing bond-exchangeable polyester resin (Example 2), to produce a property-changing bond-exchangeable polyester resin containing crosslinking points. The polyester (linear polymer) obtained in Example 1 was heat-treated (under vacuum) at four temperatures, 100°C (Comparative Example 3), 130°C (Comparative Example 4), 160°C (Example 3), and 190°C (Example 4), without purification. Below, we will explain the results of the time-resolved dynamic viscoelasticity measurement to investigate the progress of the crosslinking reaction under heating, the swelling extraction test to investigate the gel component, and the tensile test to investigate the change in mechanical properties.
[0022] Measurement conditions: Measurements were performed using MCR302 (Anton Paar). Changes in storage modulus (G´) and loss modulus (G´´) were tracked under a N2 gas atmosphere. The measurement frequency was 1 Hz and the strain was 0.5%. Results: Figure 3 shows the changes in G' and G" within 24 hours. At 100°C (Comparative Example 3), G' is always below G", indicating that sufficient crosslinking does not proceed under these conditions. On the other hand, at temperatures above 130°C (Comparative Example 4, Examples 3 and 4), a cross-point where G' = G" is observed at a certain time, indicating that crosslinking proceeds with time. The time at which the cross-point is reached is the gelation time (t gel ) and is used as an index of the rate at which crosslinking progresses.
[0023] t gel was 13.8 hours (=830 minutes) for the 130°C reaction (Comparative Example 4), 2.5 hours (=150 minutes) for the 160°C reaction (Example 3), and 0.4 hours (=24 minutes) for the 190°C reaction (Example 4). In other words, the higher the temperature, the faster the crosslinking rate, and the more efficiently the intermolecular ester exchange reaction proceeds. In addition, G' after 24 hours was 0.053 MPa for the 100°C reaction (Comparative Example 3), 0.49 MPa for the 130°C reaction (Comparative Example 4), 1.5 MPa for the 160°C reaction (Example 3), and 6.1 MPa for the 190°C reaction (Example 4). Since the value of G' reflects the crosslinking density, it can be seen that when crosslinking is performed at a high temperature, the crosslinking density increases along with the increase in the crosslinking rate.
[0024] <Swelling extraction test> The results of the swelling and extraction test of the samples reacted with Example 1 at 100°C (Comparative Example 3), 130°C (Comparative Example 4), 160°C (Example 3), and 190°C (Example 4) for 24 hours are described below. Tetrahydrofuran was used as the solvent, and the sample was immersed in it for 24 hours, after which the solvent was replaced. This procedure was repeated three times. After the three times, the swollen sample was taken out and dried in vacuum, and the dry weight (m d The initial weight (m i ) compared with the gel fraction (f gel ) was defined as formula (1) and calculated (unit: %). (Number 1) JPEG2024151806000002.jpg1055
[0025] All samples treated at 100°C (Comparative Example 3) and 130°C (Comparative Example 4) for 24 hours were dissolved, andgel The crosslinking rate was 0%. This result indicates that crosslinking was not sufficiently formed in the entire system. On the other hand, the samples treated at 160°C (Example 3) and 190°C (Example 4) for 24 hours both showed f gel The cross-linking rate was 95% or more, and it was confirmed that cross-linking was formed throughout the entire system. From these results, it can be said that the conversion from a non-cross-linked state to a cross-linked state was achieved.
[0026] <Mechanical properties> Measurement conditions: Measurement was performed at room temperature using an AGS-500NX (SHIMADZU). The tensile speed was 100 mm / min. The test specimen was a dumbbell-shaped specimen with a thickness of 0.5 mm, a gauge width of 4 mm, and a gauge length of 13 mm. Results: Figure 4 shows the stress-strain curves for samples of Example 1 that were reacted for 24 hours at 100°C (Comparative Example 3), 130°C (Comparative Example 4), 160°C (Example 3), and 190°C (Example 4). For comparison, the results of Example 1 that was not heat-treated are also shown. The vertical axis is the nominal stress, and the horizontal axis is the nominal strain. Table 1 summarizes the Young's modulus (calculated in the 5% strain region) and maximum stress of each sample. (Table 1) TIFF2024151806000003.tif32135
[0027] The stress-strain curve after 24 hours of treatment at 100°C is equivalent to that of the untreated Example 1, and it is understood that crosslinking has not progressed at all. At 130°C (Comparative Example 4), although there is a slight increase in stress, the effect of crosslinking is not observed. On the other hand, the samples heat-treated at 160°C (Example 3) and 190°C (Example 4) show a significant increase in Young's modulus and maximum stress, and it is understood that crosslinking has progressed sufficiently. In addition, the sample treated at 190°C (Example 4) has a Young's modulus (320 MPa) that is significantly larger than the value of a typical rubber material (1-10 MPa), and exhibits the behavior of a glassy crosslinked resin. From the above results, it was found that the mechanical properties can be significantly modified by conversion from a non-crosslinked linear polymer state via intermolecular bond exchange. It was also shown that the degree of modification can be adjusted by the heating temperature.
[0028] <Evaluation of bond exchange properties of polyester resin with cross-linking sites and changeable physical properties> The sample of Example 1 (linear polymer) was used, and the results of evaluation of the bond exchange properties for a crosslinked resin (property-changing bond exchangeable polyester resin having crosslinking points, Example 4) after heat treatment at 190°C for 24 hours are shown below. Measurement conditions: Measurement was performed at 190°C using MCR302 (Anton Paar). Stress relaxation measurements were performed on disk-shaped samples with a diameter of 8 mm and a thickness of 1 mm under a shear strain of 3%. The measurements were performed in a N2 gas atmosphere.
[0029] Results: Figure 5 shows the results of stress relaxation measurements at 200°C. The vertical axis shows stress (σ) normalized by the initial stress (σ0), and the horizontal axis shows the elapsed time (seconds). Despite being a fully crosslinked resin with almost no gel components, significant stress relaxation was observed. This result suggests the progression of bond exchange via transesterification in the crosslinked network. As bond exchange occurs, the material also shows reshapeability and mechanical recyclability using a hot press. Specifically, in Example 1, the molar ratio of thiol group:epoxy group:Sn(Oct)2 was fixed at 1:1:0.05, but the results when the ratios were changed are shown below. As series A, thiol group:epoxy group=1:X (X=0.25, 0.5, 0.75) was prepared, and as series B, samples were prepared in which the ratio was changed to thiol group:epoxy group=X:1 (X=0.25, 0.5, 0.75). In addition, in the above series A and B, the catalyst was fixed to epoxy group:epoxy group:Sn(Oct)2=1:0.05 relative to the epoxy group. As series C, samples were prepared in which the thiol group:epoxy group=1:1 ratio was fixed, and the tin catalyst was changed to thiol group:epoxy group:Sn(Oct)2=1:1:X (X=0.01, 0.025, 0.1, 0.2). After mixing the necessary compounds, the polymerisation reaction is carried out at 100°C for 24 hours as a common operation, followed by heat treatment for cross-linking at 160°C for 24 hours.
[0030] <Other Feed Ratios for Linear Polymers> Table 2-4 shows the results of the above three series. The item "Polymerization result" shows the state of the sample after the polymerization reaction. "Soluble" means that the polymer produced is soluble in tetrahydrofuran, which is a good solvent. "Insoluble" means that the polymer did not dissolve, and indicates the result of the polymerization reaction and the crosslinking reaction proceeding simultaneously. In this case, the thermoplastic resin cannot be converted to a thermosetting resin, and is therefore not suitable for the present invention. "Heterogeneous" means that the catalyst aggregated to form a heterogeneous mixture. The item "Heat treatment result" indicates the result of heat treatment for crosslinking at 160°C for 24 hours after the polymerization reaction. The meanings of "soluble," "insoluble," and "heterogeneous" are as described above. In the <Conversion Possible> section, if the <Polymerization Result> is "soluble", indicating the properties of a thermoplastic resin, and the <Heat Treatment Result> is "insoluble", indicating the properties of a thermosetting resin, then the result will be marked "Yes", and all other results will be marked "No".
[0031] (Table 2) Series A: Thiol group:Epoxy group=1:X (X=0.25, 0.5, 0.75) JPEG2024151806000004.jpg22135 (Table 3) Series B: Thiol group: Epoxy group = X:1 (X=0.25, 0.5, 0.75) JPEG2024151806000005.jpg22135 (Table 4) Series C: Thiol group:Epoxy group:Sn(Oct)2=1:1:X JPEG2024151806000006.jpg27135
[0032] To summarize the above results, when the ratio of thiol groups is extremely low compared to the chemical equivalent, the polymer is polymerized, but no crosslinked product is obtained after heat treatment. The reason for this is that the molecular weight of the polymer produced is too small. Also, when the ratio of thiol groups is extremely high compared to the chemical equivalent, homopolymerization of the epoxy compound proceeds and a crosslinked product is produced during the reaction at 100°C. As for the catalyst, it was found that when the ratio is too high, it does not mix uniformly with the other components and a white-colored crosslinked product is produced.
[0033] Based on the above results, the average molecular weight of the linear polymer 2(2') is preferably 5000 or more from the viewpoint of obtaining a crosslinked product after heat treatment. From the viewpoint of crosslinking efficiency, the proportion of the ester bonds 5 in the linear polymer 2 (2') is preferably 15 or more, more preferably 25 or more per molecular chain. That is, the molar ratio of the hydroxyl groups to the ester bonds in the linear polymer is 1:0.75 to 0.75:1 (=1:1.33). From the viewpoint of forming a crosslinked body colored white without being uniformly mixed with other components, the predetermined content of the transesterification catalyst 3 is preferably a molar ratio to the thiol group or epoxy group of 0.01 to 0.15, more preferably 0.025 to 0.10. [Industrial Applicability]
[0034] By utilizing the remolding processability and mechanical recyclability using a hot press that the physical property conversion type bond exchangeable polyester resin has, it can be used as a reinforcing plate whose elastic modulus can be adjusted, for example, when the reinforcing plate is pressure-bonded with a thermosetting adhesive. [Explanation of symbols]
[0035] 1: Physical property conversion type bond exchange polyester resin raw material 2, 2´: Linear polymer 3: Transesterification catalyst 4: Hydroxyl group 5: Ester bond 6: Component parts 7, 7´: Cross-linking points formed 8: Property-changing bond-exchangeable polyester resin containing crosslinking points
Claims
1. A linear polymer, the linear polymer comprising a moiety capable of forming a crosslinking point with another linear polymer by bond exchange via a transesterification reaction.
2. The linear polymer of claim 1 , wherein the moiety comprises an ester bond and a hydroxyl group.
3. 3. The linear polymer according to claim 2, wherein the number average molecular weight of the linear polymer is 5,000 or more, the number of ester bonds per molecular chain in the linear polymer is 15 or more, and the number of hydroxyl groups per molecular chain in the linear polymer is 15 or more.
4. A property-changing bond-exchangeable polyester resin raw material comprising the linear polymer according to any one of claims 1 to 3 and an ester exchange catalyst.
5. The property-converting bond-exchangeable polyester resin raw material according to claim 4, wherein the molar ratio of the transesterification catalyst to the hydroxyl groups (the hydroxyl groups:the transesterification catalyst) is 0.01 to 0.
15.
6. A property-changing bond-exchangeable polyester resin containing crosslinking points, which includes crosslinking points between the linear polymer and the other linear polymer, produced by crosslinking at least a portion of the components described in any one of claims 1 to 3.
7. A property-changing bond-exchangeable polyester resin containing crosslinking points as described in claim 6, which is a property-changing bond-exchangeable polyester resin containing crosslinking points having a predetermined maximum stress, wherein the maximum stress of the resin consisting of a linear polymer that does not contain the crosslinking points before it comes to contain the crosslinking points is 1 MPa or less.
8. The property-changing bond-exchangeable polyester resin containing the crosslinking points described in claim 7 has a Young's modulus that is 10 times or more greater than the Young's modulus of a linear polymer that does not contain the crosslinking points before the crosslinking points are contained.
9. A property-changing bond-exchangeable polyester resin containing activated crosslinking points, which is obtained by further activating the crosslinking points of the property-changing bond-exchangeable polyester resin containing the crosslinking points according to claim 6 .
10. The method for producing a linear polymer according to claim 2, comprising a reaction of thiol groups with epoxy groups catalyzed by a transesterification catalyst, the molar ratio of thiol groups:epoxy groups being 1:0.75 to 0.75:
1.
11. The method for producing a linear polymer according to claim 10, wherein the molar ratio of the catalyst amount is 0.01 or more and 0.15 or less when the molar ratio of thiol group:epoxy group is 1:
1.
12. A method for producing a property-changing bond-exchangeable polyester resin having crosslinking points, which is obtained by mixing a linear polymer having ester bonds and hydroxyl groups with an ester exchange catalyst and heating the mixture to form crosslinking points.
Citation Information
Patent Citations
Soft crosslinked polyester resin / film exhibiting self-adhesive property, re-formability, and flaw-repairing property, and production method therefor