Laminate and method for manufacturing the same

A laminate with a coating film on polyolefin resin base material, using an active energy ray-curable resin and hydrogen abstraction photoinitiator, addresses adhesion and scratch resistance issues, ensuring strong bonding and durability.

JP2024152086APending Publication Date: 2024-10-25RIKEN TECHNOS CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023066025
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-14
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Polyolefin resins suffer from insufficient scratch resistance and poor adhesion to coating films, limiting their applications, and existing solutions like active energy ray-curable compositions do not provide sufficient adhesion strength.

Method used

A laminate is produced by directly laminating a polyolefin resin base material with a coating film using an active energy ray-curable resin and a hydrogen abstraction type photoinitiator, involving steps of forming, pre-drying, and curing the coating film at elevated temperatures and irradiating with active energy rays.

Benefits of technology

The laminate achieves high adhesion strength between the polyolefin resin base material and the coating film, maintaining adhesion even after moist heat tests, suitable for surface protection and scratch resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152086000001_ABST
    Figure 2024152086000001_ABST
Patent Text Reader

Abstract

To provide a laminate in which a polyolefin resin base material and a coating film are directly laminated with sufficient adhesion strength, and a method for manufacturing the same.SOLUTION: A method for manufacturing a laminate comprises the steps of: (1) forming a wet coating film on a part or all of a surface of a polyolefin resin base material by using a coating material for forming a coating film; (2) pre-drying the wet coating film to form an uncured coating film thereby obtaining an intermediate laminate; (3) preheating the intermediate laminate to a temperature of 65°C or higher; and (4) completely curing the uncured coating film by the application of an active energy ray. The coating material comprises: (A) 100 parts by mass of an active energy ray-curable resin; and (B) 1 to 30 parts by mass of a hydrogen abstraction type photoinitiator.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate and a manufacturing method thereof. More specifically, the present invention relates to a laminate having a coating film on a part or all of the surfaces of a polyolefin resin substrate, and a manufacturing method thereof, in which the polyolefin resin substrate and the coating film are directly laminated together, and a manufacturing method thereof. [Background technology]

[0002] Conventionally, polyolefin resins such as polyethylene, polypropylene, cyclic olefin resins, and poly4-methyl-pentene-1 have been used in various fields as molded bodies such as films. In particular, cyclic olefin resins and poly4-methyl-pentene-1 films have high optical isotropy, high transparency, high heat resistance, and low moisture absorption, and are therefore widely used in the optical field. On the other hand, polyolefin resins have the disadvantage that their scratch resistance is insufficient and their applicable applications are limited. When the scratch resistance is insufficient for application to a desired application, a method of providing a coating film (hard coat) on the surface of a molded body such as a resin film to impart scratch resistance (prevent scratches) is widely used. In addition, for the formation of a coating film (hard coat) to impart scratch resistance (prevent scratches), paints mainly composed of active energy ray curable resins are often used because of their high hardness, short curing time, and high productivity. However, polyolefin resins have the disadvantage of insufficient adhesion to coating films (hard coats) formed using paints mainly composed of active energy ray curable resins. In response to this, a UV-curable composition for protecting cyclic olefin resins containing a polymerizable compound and a photopolymerization initiator, which contains a benzophenone compound and an aliphatic tertiary amine compound as the photopolymerization initiator (Patent Document 1), and a technique for providing an easy-adhesion layer containing a mixture of a polyolefin resin and a methyl methacrylate resin (Patent Document 2) have been proposed. However, the technique of Patent Document 1 is not sufficient. The technique of Patent Document 2 has the disadvantage of increasing the number of steps in order to provide an easy-adhesion layer. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2002-356505 A [Patent Document 2] JP 2016-187870 A [Patent Document 3] JP 2016-113393 A Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide a laminate having a coating film on all or part of the surfaces of a polyolefin resin substrate, and a method for producing the same, in which the polyolefin resin substrate and the coating film are directly laminated with sufficient adhesion strength, and a method for producing the same. [Means for solving the problem]

[0005] As a result of extensive research, the present inventors have found that the above object can be achieved by a specific laminate and a specific manufacturing method.

[0006] That is, various aspects of the manufacturing method of the present invention are as follows. [1]. A method for producing a laminate having a coating film on a part or all of the surfaces of a polyolefin resin substrate, comprising the steps of: The polyolefin resin substrate and the coating film are directly laminated together, (1) forming a wet coating film on a part or all of the surfaces of the polyolefin-based resin substrate using a coating material for forming the coating film, thereby obtaining an intermediate laminate 1 having the wet coating film on a part or all of the surfaces of the polyolefin-based resin substrate; (2) A step of pre-drying the wet coating film to form an uncured coating film, thereby obtaining an intermediate laminate 2 having the uncured coating film on a part or all of the surfaces of the polyolefin-based resin substrate; (3) preheating the intermediate laminate 2 to a temperature of 65° C. or higher; and (4) a step of irradiating the uncured coating film with active energy rays to completely cure the uncured coating film; wherein the coating comprises: (A) 100 parts by mass of an active energy ray-curable resin; and (B) 1 to 30 parts by mass of a hydrogen abstraction type photoinitiator; A method for producing the laminate comprising the steps of: [2]. The method for producing a laminate according to item [1], wherein the component (A) active energy ray-curable resin contains a polyfunctional (meth)acrylate. [3]. The method for producing a laminate according to item [2], wherein the polyfunctional (meth)acrylate contains a polyfunctional (meth)acrylate having an acrylic equivalent of 300 or less. [4]. The method for producing a laminate according to item [1], wherein the step (4) includes a sub-step of irradiating the intermediate laminate 2 with active energy rays from a surface opposite to the uncured coating film. [5]. The method for producing a laminate according to item [1], wherein the coating material does not contain an intramolecular cleavage type photoinitiator. [6]. The method for producing a laminate according to item [1], wherein the coating material does not contain an aliphatic tertiary amine compound. [7]. A method for producing an article comprising a laminate, the method comprising the step of producing a laminate using the method for producing a laminate according to any one of items [1] to [6].

[0007] Various aspects of the laminate of the present invention are as follows. [1]. A laminate having a coating film on a part or all of the surfaces of a polyolefin resin substrate, The polyolefin resin substrate and the coating film are directly laminated together, The coating film is (A) 100 parts by mass of an active energy ray-curable resin; and (B) 1 to 30 parts by mass of a hydrogen abstraction type photoinitiator; The coating material is made of a paint containing When a cross-cut test is performed according to JIS K 5600-5-6:1999 by cutting cross-cuts from the coating surface side of the laminate, the result is Class 0, Class 1, Class 2, or Class 3. The above laminate. [2]. The laminate according to item [1], wherein the component (A) active energy ray-curable resin contains a polyfunctional (meth)acrylate. [3]. The laminate according to item [2], wherein the polyfunctional (meth)acrylate contains a polyfunctional (meth)acrylate having an acrylic equivalent of 300 or less. [4]. The laminate according to item [1], wherein the coating material does not contain an intramolecular cleavage type photoinitiator. [5]. The laminate according to item [1], wherein the coating material does not contain an aliphatic tertiary amine compound. [6]. An article comprising a laminate, the article comprising the laminate according to any one of items [1] to [5]. Effect of the Invention

[0008] In the laminate produced by the manufacturing method of the present invention, the polyolefin resin substrate and the coating film are directly laminated with sufficient adhesion strength. That is, it is not necessary to form an easy-adhesion layer on the coating film-formed surface of the polyolefin resin substrate. In the laminate produced by the preferred manufacturing method of the present invention, the polyolefin resin substrate and the coating film are directly laminated with sufficient adhesion strength, and the sufficient adhesion strength is maintained even after a wet heat test. Therefore, the laminate produced by the manufacturing method of the present invention can be suitably used as a surface protection member or a member that forms the surface of an article (including a member of an article) that requires scratch resistance.

[0009] In the laminate of the present invention, the polyolefin resin substrate and the coating film are directly laminated with sufficient adhesion strength. In the preferred laminate of the present invention, the polyolefin resin substrate and the coating film are directly laminated with sufficient adhesion strength, and the sufficient adhesion strength is maintained even after a wet heat test. Therefore, the laminate of the present invention can be suitably used as a surface protection member or a member that forms a surface of an article (including a member of an article) that requires scratch resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] In this specification, the term "resin" is used to include a resin mixture containing two or more resins, and a resin composition containing components other than resin.

[0011] In this specification, the term "film" is used interchangeably or interchangeably with "sheet." In this specification, the terms "film" and "sheet" are used for those that can be industrially wound into a roll. The term "plate" is used for those that cannot be industrially wound into a roll. In addition, in this specification, laminating a certain layer and another layer in order includes both directly laminating the layers and laminating the layers with one or more layers, such as an easy-adhesion layer (anchor coat), interposed between the layers.

[0012] In this specification, the term "more than" in relation to a numerical range means a certain number or more than a certain number. For example, 20% or more means 20% or more than 20%. The term "less than" in relation to a numerical range means a certain number or less than a certain number. For example, 20% or less means 20% or less than 20%. Furthermore, the symbol "~" in relation to a numerical range means a certain number, more than a certain number and less than another certain number, or another certain number. Here, the other certain number is a number larger than the certain number. For example, 10 to 90% means 10%, more than 10% and less than 90%, or 90%. Furthermore, the upper and lower limits of the numerical range can be arbitrarily combined, and an embodiment in which the values ​​are arbitrarily combined can be read. For example, from a statement regarding the numerical range of a certain characteristic such as "usually 10% or more, preferably 20% or more. On the other hand, it is usually 40% or less, preferably 30% or less" or "usually 10 to 40%, preferably 20 to 30%," it can be read that the numerical range of the certain characteristic is 10 to 40%, 20 to 30%, 10 to 30%, or 20 to 40% in one embodiment.

[0013] Other than in the examples, or where otherwise specified, all numerical values ​​used in the specification and claims should be understood to be modified by the term "about." Without attempting to limit the application of the doctrine of equivalents to the scope of the claims, each numerical value should be construed in light of the number of significant digits and by applying ordinary rounding techniques.

[0014] In this specification, terms specifying shapes or geometric conditions, such as parallel, orthogonal, and perpendicular, are intended to include substantially the same state in addition to their strict meanings.

[0015] 1. Manufacturing method of laminate: The manufacturing method of the present invention is a method for manufacturing a laminate having a coating film (including a hard coat; the same applies below) on a part or all of the surfaces of a polyolefin resin substrate. In the manufacturing method of the present invention, the polyolefin resin substrate and the coating film are directly laminated. That is, the manufacturing method of the present invention excludes an embodiment in which one or more separate layers such as an easy-adhesion layer (anchor coat) are interposed between the polyolefin resin substrate and the coating film.

[0016] The production method of the present invention comprises the steps of: (1) forming a wet coating film on a part or all of the surfaces of the polyolefin-based resin substrate using a coating material for forming the coating film, thereby obtaining an intermediate laminate 1 having the wet coating film on a part or all of the surfaces of the polyolefin-based resin substrate; (2) A step of pre-drying the wet coating film to form an uncured coating film, thereby obtaining an intermediate laminate 2 having the uncured coating film on a part or all of the surfaces of the polyolefin-based resin substrate; (3) preheating the intermediate laminate 2 to a temperature of 65° C. or higher; and (4) a step of irradiating the uncured coating film with active energy rays to completely cure the uncured coating film; Includes.

[0017] In the production method of the present invention, the coating material used to form the coating film contains (A) an active energy ray curable resin, and (B) a hydrogen abstraction type photoinitiator. In one typical embodiment, the coating material contains 100 parts by mass of the (A) active energy ray curable resin, and 1 to 30 parts by mass of the (B) hydrogen abstraction type photoinitiator.

[0018] Process (1) The step (1) is a step of forming a wet coating film on a part or all of the surfaces of the polyolefin resin substrate using a coating material for forming the coating film to obtain an intermediate laminate 1 having the wet coating film on a part or all of the surfaces of the polyolefin resin substrate. Here, it goes without saying that the wet coating film is directly formed on a part or all of the surfaces of the polyolefin resin substrate.

[0019] In one typical embodiment, the polyolefin-based resin substrate may be a polyolefin-based resin film.

[0020] The polyolefin-based resin film may be a single layer film or a multilayer film. When the polyolefin-based resin film is a single layer film, the resin forming the single layer film (in other words, the resin forming the coating film forming surface of the single layer film) mainly contains a polyolefin-based resin. When the polyolefin-based resin film is a multilayer film, the resin forming the coating film forming surface of the multilayer film (the resin forming the surface layer of the multilayer film on the side where the coating film is formed) mainly contains a polyolefin-based resin. When the polyolefin-based resin film is a multilayer film, the resin forming the layer other than the layer forming the coating film forming surface of the multilayer film may mainly contain a polyolefin-based resin, or may be other than the one mainly containing a polyolefin-based resin.

[0021] The polyolefin resin film may be a non-stretched film, a uniaxially stretched film, or a biaxially stretched film.

[0022] In another embodiment, the polyolefin resin substrate may be a three-dimensional molded article of a polyolefin resin. Here, the three-dimensional molded article refers to a molded article having a shape that includes a non-planar shape such as unevenness in at least a part thereof.

[0023] The three-dimensional molded body may be a single-layer three-dimensional molded body or a multi-layer three-dimensional molded body. When the three-dimensional molded body is a single-layer three-dimensional molded body, the resin forming the single-layer three-dimensional molded body mainly contains a polyolefin resin. When the three-dimensional molded body is a multi-layer three-dimensional molded body, the resin forming the coating film forming surface of the multi-layer three-dimensional molded body (the resin forming the surface layer of the multi-layer three-dimensional molded body on which the coating film is formed) mainly contains a polyolefin resin. When the three-dimensional molded body is a multi-layer three-dimensional molded body, the resin forming the layer other than the layer forming the coating film forming surface of the multi-layer three-dimensional molded body may mainly contain a polyolefin resin, or may be other than the one mainly containing a polyolefin resin.

[0024] Here, containing mainly polyolefin-based resin means that the total of the resins forming the monolayer film, the resins forming the coating film-forming surface of the multilayer film, the resins forming the monolayer three-dimensional molded body, or the resins forming the coating film-forming surface of the multilayer three-dimensional molded body is 100 mass%, and the polyolefin-based resin is usually contained in an amount of 60 mass% or more, preferably 70 mass% or more, more preferably 80 mass% or more, even more preferably 90 mass% or more, and most preferably 95 mass% or more, and typically 99 to 100 mass%.

[0025] The polyolefin resin is a resin that mainly contains structural units derived from an α-olefin and / or a cyclic olefin.

[0026] The α-olefin is an alkene having a carbon-carbon double bond at the α-position. Examples of the α-olefin include ethylene, propylene, 1-butene, 1-hexene, 1-octene, and 4-methyl-pentene-1.

[0027] The cyclic olefin is a polymerizable compound having an alicyclic structure formed by carbon atoms and having a carbon-carbon double bond in the ring. Examples of the cyclic olefin include cyclobutene, cyclopentene, cyclopentadiene, norbornene (bicyclo[2.2.1]hept-2-ene), dicyclopentadiene (tricyclo[4.3.0.12,5]deca-3,7-diene), tetracyclododecene (tetracyclo[4.4.0.12,5.17,10]deca-3-ene), and derivatives thereof.

[0028] Here, "mainly containing structural units derived from α-olefins and / or cyclic olefins" means that, with the sum of all structural units of the polyolefin resin being 100% by mass, the content of structural units derived from α-olefins and / or cyclic olefins is usually 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, still more preferably 90% by mass or more, most preferably 95% by mass or more, and typically 99 to 100% by mass.

[0029] Examples of the polyolefin resin include polyethylene resin, polypropylene resin, cyclic olefin resin, and poly-4-methyl-pentene-1 resin.

[0030] The polyethylene resin is a resin mainly containing structural units derived from ethylene. The content of structural units derived from ethylene in the polyethylene resin may be usually 50% by mass or more, preferably 60% by mass or more, more preferably 65% ​​by mass or more, and typically 70 to 100% by mass, where the sum of all structural units is 100% by mass.

[0031] Examples of the polyethylene resin include polyethylenes such as very low density polyethylene, low density polyethylene, linear low density polyethylene, medium density polyethylene, high density polyethylene, and ethylene-α-olefin copolymers such as ethylene-1-butene copolymer, ethylene-1-hexene copolymer, and ethylene-1-octene copolymer; ethylene-(meth)acrylic acid alkyl ester copolymers such as ethylene-ethyl acrylate copolymer and ethylene-methyl methacrylate copolymer; ethylene-unsaturated carboxylic acid copolymers such as ethylene-acrylic acid copolymer and ethylene-methacrylic acid copolymer; ionomer resins in which the ethylene-unsaturated carboxylic acid copolymer molecules are crosslinked with metal ions; and ethylene-vinyl acetate copolymer.

[0032] Examples of the metal ion used in the ionomer resin include lithium ion, sodium ion, potassium ion, rubidium ion, cesium ion, zinc ion, magnesium ion, and manganese ion.

[0033] The polypropylene resin is a resin mainly containing structural units derived from propylene. The content of the structural units derived from propylene in the polypropylene resin may be usually 50% by mass or more, preferably 60% by mass or more, more preferably 65% ​​by mass or more, and typically 70 to 100% by mass, where the sum of all structural units is 100% by mass.

[0034] Examples of the polypropylene-based resin include polypropylenes such as propylene homopolymers and copolymers (including block copolymers and random copolymers) of propylene and one or more α-olefins (e.g., ethylene, 1-butene, 1-hexene, 1-octene, and 4-methyl-pentene-1).

[0035] The cyclic olefin resin is a resin mainly containing structural units derived from the cyclic olefin. The content of the structural units derived from the cyclic olefin in the cyclic olefin resin may be usually 50% by mass or more, preferably 70% by mass or more, more preferably 80% by mass or more, typically 90 to 100% by mass, where the sum of all structural units is 100% by mass.

[0036] Examples of the cyclic olefin resin include copolymers of the cyclic olefin, preferably norbornene, and the α-olefin, preferably an α-olefin having 2 to 8 carbon atoms (e.g., ethylene, propylene, 1-butene, 1-pentene, 1-hexene, and 1-octene), more preferably ethylene.

[0037] The poly-4-methyl-pentene-1 resin is a resin mainly containing structural units derived from 4-methyl-pentene-1. The content of structural units derived from 4-methyl-pentene-1 in the poly-4-methyl-pentene-1 resin may be usually 50% by mass or more, preferably 70% by mass or more, more preferably 80% by mass or more, and typically 90 to 100% by mass, with the sum of all structural units being 100% by mass.

[0038] Examples of the poly-4-methyl-pentene-1 resin include poly-4-methyl-pentene-1 such as 4-methyl-pentene-1 homopolymers and copolymers (including block copolymers and random copolymers) of 4-methyl-pentene-1 with one or more α-olefins (e.g., ethylene, propylene, 1-butene, 1-hexene, 1-octene, etc.).

[0039] As the polyolefin resin, one or a mixture of two or more of these can be appropriately selected and used, taking into consideration the use of the laminate, the required properties thereof, and the preheating temperature in the above step (3).

[0040] The method of forming the polyolefin resin film using these polyolefin resins is not particularly limited, and known film forming methods can be used.The film forming method can be, for example, a method of forming a film using a calendar roll rolling film forming device equipped with a calendar roll rolling processing machine and a winding device; a method of forming a film using a T-die film forming device equipped with an extruder, a T-die, and a winding device; and a method of forming a film using an inflation film forming device equipped with an extruder, a circular die, an inflation device, and a winding device having a nip mechanism.In addition, after forming a film by these methods, it may be further uniaxially or biaxially stretched.

[0041] When the laminate is used in the optical field, particularly when it is used to protect a display faceplate or the like from scratches, damage, adhesion of contaminants, etc., films of cyclic olefin resins and poly 4-methyl-pentene-1 are preferred because they have high optical isotropy, high transparency, high heat resistance, and low moisture absorption. When the laminate is used to protect the surface of an article having a three-dimensional shape / stereoscopic shape from scratches, damage, adhesion of contaminants, etc., films of polyethylene resins and polypropylene resins are preferred because they have stretchability or flexibility.

[0042] The thickness of the polyolefin resin film can be appropriately determined taking into consideration the use of the laminate produced by the manufacturing method of the present invention, its required properties, and its handling. When the laminate is used for an application that does not require high rigidity, the thickness may be usually 10 μm or more, preferably 30 μm or more, more preferably 50 μm or more from the viewpoint of handling. On the other hand, from the viewpoint of economic efficiency, the thickness may be usually 250 μm or less, preferably 150 μm or less, more preferably 100 μm or less. When the laminate is used for an application that requires high rigidity, the thickness may be usually 200 μm or more, preferably 300 μm or more, more preferably 400 μm or more. On the other hand, from the viewpoint of meeting the demand for thinning of the article, the thickness may be usually 1500 μm or less, preferably 1000 μm or less, more preferably 700 μm or less.

[0043] The method of producing the above-mentioned three-dimensional molded body using these polyolefin resins is not particularly limited, and can use known molding methods.The above-mentioned molding methods include, for example, injection molding, blow molding, extrusion molding, and other methods, and a method of forming a thick film (sheet) using a known film forming method, and then giving the thick film (sheet) a three-dimensional shape by a three-dimensional forming method such as membrane press molding, pressure press molding, vacuum molding, and vacuum pressure molding.

[0044] The thickness of the three-dimensional molded body can be appropriately determined taking into consideration the use of the laminate produced by the manufacturing method of the present invention, its required properties, and its handleability. The thickness of the three-dimensional molded body may be usually 200 μm or more, preferably 300 μm or more, more preferably 400 μm or more, from the viewpoint of imparting the rigidity required to maintain the shape. On the other hand, from the viewpoint of responding to the demand for lightweight articles, it may be usually 1500 μm or less, preferably 1000 μm or less, more preferably 700 μm or less.

[0045] The paint for forming the coating film will be described later in "2. Paint for forming coating film".

[0046] In the above step (1), the method for forming a wet coating film on a part or all of the surfaces of the polyolefin resin substrate using the coating material for forming the coating film is not particularly limited, and a known coating method can be used.

[0047] When the polyolefin resin substrate is a polyolefin resin film, the coating method is preferably, from the viewpoint of applying the coating material productively by a roll-to-roll method, a method such as rod coating, roll coating, gravure coating, reverse coating, kiss reverse coating, and die coating.

[0048] When the polyolefin resin substrate is a three-dimensional molded article, examples of the coating method include dip coating, spray coating, spin coating, and air knife coating.

[0049] The thickness of the wet coating film formed in the above step (1) (the amount of the coating material applied) can be appropriately determined taking into account the solids concentration of the coating material, so that the thickness of the completely cured coating film formed in the below-mentioned step (4) falls within the preferred range described below.

[0050] Before the step (1), the coating film-forming surface of the polyolefin-based resin substrate may or may not be subjected to an easy-adhesion treatment such as corona treatment, plasma treatment, and ultraviolet treatment. In the preferred manufacturing method of the present invention, the adhesion strength between the polyolefin-based resin substrate and the coating film is sufficiently developed even without the easy-adhesion treatment. Therefore, in the preferred manufacturing method of the present invention, the easy-adhesion treatment can be omitted.

[0051] Process (2) The above-mentioned step (2) is a step of pre-drying the wet coating film of the above-mentioned intermediate laminate 1 to form an uncured coating film, thereby obtaining an intermediate laminate 2 having the uncured coating film on a part or all of the surfaces of the above-mentioned polyolefin resin substrate.

[0052] The preliminary drying can be carried out, for example, by passing the intermediate laminate 1 through a drying furnace set at a temperature of usually 50°C or higher, preferably 60°C or higher, more preferably 65°C or higher, even more preferably 70°C or higher, even more preferably 75°C or higher, and most preferably 80°C or higher, and at a temperature not higher than a temperature taking into consideration the heat resistance of the polyolefin resin substrate, at a line speed such that the time required for passing from the inlet to the outlet is about 0.5 to 10 minutes, preferably 1 to 5 minutes.

[0053] Process (3) The step (3) is a step of preheating the intermediate laminate 2 to a temperature of 65° C. or higher.

[0054] Without intending to be bound by theory, it is believed that by irradiating the intermediate laminate 2 with active energy rays in a preheated state, abstraction of hydrogen atoms by the hydrogen abstraction photoinitiator, component (B), occurs in sufficient quantities even on the surface of the polyolefin resin substrate in contact with the uncured coating film, forming reaction sites and improving adhesion.

[0055] Examples of the preheating method include a method in which the predrying temperature in step (2) is set to 65° C. or higher to perform both predrying of the wet coating film (a step of converting the intermediate laminate 1 into the intermediate laminate 2) and preheating of the intermediate laminate 2; and a method using a non-contact heating device such as a flash lamp annealing device or an excimer laser annealing device. When the polyolefin resin substrate is a polyolefin resin film, the preheating method may be a method in which the intermediate laminate 2 is wrapped around a preheating roll set to a temperature of 65° C. or higher and conveyed. Furthermore, the preheating method may be a combination of these methods.

[0056] The preheating temperature may be preferably 70° C. or higher, more preferably 75° C. or higher, and even more preferably 80° C. or higher. Meanwhile, the preheating temperature is a temperature or lower taking into consideration the heat resistance of the polyolefin resin substrate. The preheating temperature may be preferably 120° C. or lower, and more preferably 100° C. or lower.

[0057] Process (4) The step (4) is a step of irradiating the intermediate laminate 2 preheated in the step (3) with active energy rays to completely cure the uncured coating film. The irradiation may be performed from the surface of the intermediate laminate 2 on the uncured coating film side, or from the surface opposite the uncured coating film. From the viewpoint of adhesion between the polyolefin resin substrate and the coating film, particularly adhesion after a moist heat test, the irradiation is preferably performed from the surface of the intermediate laminate 2 opposite the uncured coating film.

[0058] Without intending to be bound by theory, the hydrogen abstraction type photoinitiator (B) is a compound that also functions as an ultraviolet absorber. Therefore, it is considered that by irradiating the surface of the intermediate laminate 2 opposite to the uncured coating film, among the hydrogen abstraction type photoinitiators (B) contained in the uncured coating film, the one present in the vicinity of the polyolefin resin substrate in the uncured coating film acts preferentially, thereby sufficiently improving adhesion.

[0059] On the other hand, the irradiation is preferably performed from the surface of the intermediate laminate 2 on the side of the uncured coating film, from the viewpoint of web handleability or the inconvenience of irradiating the active energy rays from the back side of the uncured coating film that is not cured at all, and from the viewpoint of completely curing the uncured coating film with a minimum amount of irradiation and preventing coloring (yellowing) of the coating film. Therefore, one of the more preferred embodiments is to perform the irradiation so as to include a sub-step (4-1) of irradiating from the surface of the intermediate laminate 2 opposite to the uncured coating film side and a sub-step (4-2) of irradiating from the surface of the uncured coating film side. The sub-steps (4-1) and (4-2) may be performed simultaneously, the sub-step (4-1) may be performed first, and the sub-step (4-2) may be performed first, and the sub-step (4-1) may be performed first. From the viewpoint of web handling properties and the inconveniences of the above-mentioned apparatus, it is more convenient to carry out the above-mentioned sub-step (4-1) after carrying out the above-mentioned sub-step (4-2).

[0060] The cumulative dose of the irradiation can be appropriately selected and determined from the viewpoint of completely curing the uncured coating film and from the viewpoint of preventing coloring (yellowing) of the coating film, taking into consideration the thickness of the coating film. The cumulative dose is usually 10 to 10,000 mJ / cm 2 , preferably 300 to 3000 mJ / cm 2 , more preferably 400 to 2000 mJ / cm 2 , and more preferably 500 to 1500 mJ / cm 2 , and most preferably 600 to 1200 mJ / cm 2Here, when the sub-step (4-1) and the sub-step (4-2) are included, the integrated irradiation amount is the total integrated irradiation amount of the sub-step (4-1) and the sub-step (4-2).

[0061] When performing either the substep (4-1) or the substep (4-2) and then the other substep, from the viewpoint of allowing the component (B) hydrogen abstraction photoinitiator to remain without being consumed in the earlier substep and to function effectively in the later substep, it is one of the preferred embodiments to suppress the integrated irradiation dose in the earlier substep to a relatively low level (usually 10 to 70%, preferably 20 to 60% of the desired total integrated irradiation dose).

[0062] The thickness of the completely cured coating film formed in the above step (4) can be appropriately determined taking into consideration the use of the laminate produced by the manufacturing method of the present invention, its required properties, and handling. The thickness of the coating film may be usually 0.1 μm or more, preferably 0.5 μm or more, more preferably 1 μm or more, even more preferably 2 μm or more, and most preferably 3 μm or more, from the viewpoint of surface hardness and scratch resistance. On the other hand, when the polyolefin resin substrate is the polyolefin resin film, the thickness of the coating film may be usually 60 μm or less, preferably 30 μm or less, more preferably 20 μm or less, and even more preferably 10 μm or less, from the viewpoint of maintaining good bending resistance of the laminate and making it easy to handle as a film roll, and from the viewpoint of suppressing curling. When the polyolefin resin substrate is the three-dimensional molded body, the thickness of the coating film may be usually 60 μm or less, preferably 30 μm or less, more preferably 20 μm or less, and even more preferably 10 μm or less, from the viewpoint of workability when forming the wet coating film in the above step (1).

[0063] After the step (4), an aging treatment may be carried out to stabilize the properties of the laminate.

[0064] 2. Paint for film formation: The production method of the present invention uses a coating material containing the above (A) active energy ray curable resin and the above (B) hydrogen abstraction type photoinitiator as the coating material for forming the coating film. In one typical embodiment, the production method of the present invention uses a coating material containing 100 parts by mass of the above (A) active energy ray curable resin and 1 to 30 parts by mass of the above (B) hydrogen abstraction type photoinitiator.

[0065] (A) Active energy ray curable resin: The coating material contains the above-mentioned component (A) active energy ray curable resin. The above-mentioned component (A) active energy ray curable resin functions to form a coating film by being polymerized and cured by active energy rays such as ultraviolet rays and electron beams.

[0066] Examples of the component (A) active energy ray-curable resin include compounds having a (meth)acryloyl group, compounds having an allyl group, compounds having a thiol group, compounds having a vinyl ether group, N-substituted (meth)acrylamide compounds, and aromatic vinyl compounds.

[0067] The compound having the (meth)acryloyl group is a compound having one or more acryloyl groups (-CO-CH=CH2) or methacryloyl groups (-CO-C(CH3)=CH2) in one molecule. The number of (meth)acryloyl groups in the compound having the (meth)acryloyl group in one molecule may be preferably 2 or more, more preferably 3 or more, from the viewpoint of the curability of the coating material. On the other hand, from the viewpoint of the crack resistance of the coating film, it may be usually 20 or less, preferably 12 or less, more preferably 8 or less. In this specification, the (meth)acryloyl group means an acryloyl group or a methacryloyl group.

[0068] Examples of the compound having a (meth)acryloyl group include (meth)acryloyl group-containing prepolymers or oligomers such as polyurethane (meth)acrylate, polyester (meth)acrylate, polyacryl (meth)acrylate, epoxy (meth)acrylate, polyalkylene glycol poly(meth)acrylate, and polyether (meth)acrylate; compounds having one (meth)acryloyl group in one molecule such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, hydroxyethyl (meth)acrylate, and hydroxypropyl (meth)acrylate; ethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, and the like. Examples of the compound include (meth)acrylate, 1,6-hexanediol di(meth)acrylate, polyethylene glycol di(meth)acrylate, 2,2'-bis(4-(meth)acryloyloxypolyethyleneoxyphenyl)propane, and 2,2'-bis(4-(meth)acryloyloxypolypropyleneoxyphenyl)propane, which have two (meth)acryloyl groups in one molecule; trimethylolpropane tri(meth)acrylate, and trimethylolethane tri(meth)acrylate, which have three (meth)acryloyl groups in one molecule; pentaerythritol tetra(meth)acrylate, which has four (meth)acryloyl groups in one molecule; and dipentaerythritol hexaacrylate, which has six (meth)acryloyl groups in one molecule. In this specification, (meth)acrylate means acrylate or methacrylate.

[0069] The compound having an allyl group is a compound having one or more allyl groups (2-propenyl group: -CH2-CH=CH2) in one molecule. The number of allyl groups in the compound having an allyl group may be preferably 2 or more, more preferably 3 or more, in terms of the curability of the coating material. On the other hand, in terms of the crack resistance of the coating film, it may be usually 20 or less, preferably 12 or less, more preferably 8 or less.

[0070] Examples of the compound having an allyl group include compounds having an allyl ether group (-O-CH2-CH=CH2), such as glycerin diallyl ether, trimethylolpropane diallyl ether, and pentaerythritol triallyl ether; compounds having an allyl ester group (-CO-CH2-CH=CH2), such as diallyl maleate, diallyl adipate, triallyl citrate, and triallyl trimellitate; allyl isocyanurate compounds, such as 1,3,5-tri-2-propenyl-1,3,5-triazine-2,4,6(1H,3H,5H)-trione; and allyl glycidyl compounds, such as glycerin diallyl monoglycidyl ether, allyl glycidyl phthalate, and allyl glycidyl hexahydrophthalate.

[0071] The compound having the thiol group is a compound having one or more selected from the group consisting of a primary thiol group, a secondary thiol group, and a tertiary thiol group in one molecule.The number of thiol groups in the compound having the thiol group in one molecule may be preferably 2 or more, more preferably 3 or more, from the viewpoint of the curability of the coating material.On the other hand, from the viewpoint of the crack resistance of the coating film, it may be usually 20 or less, preferably 12 or less, more preferably 8 or less.

[0072] Examples of the compound having a thiol group include compounds having one primary thiol group in one molecule, such as 3-mercaptopropionic acid, 2-ethylhexyl-3-mercaptopropionate, n-octyl-3-mercaptopropionate, 3-methoxybutyl-3-mercaptopropionate, and stearyl-3-mercaptopropionate; compounds having two primary thiol groups in one molecule, such as tetraethylene glycol bis(3-mercaptopropionate); compounds having three primary thiol groups in one molecule, such as trimethylolpropane tris(3-mercaptopropionate) and tris-((3-mercaptopropionyloxy)-ethyl)-isocyanurate; Compounds having four primary thiol groups in one molecule, such as dipentaerythritol hexakis (3-mercaptopropionate); compounds having six primary thiol groups in one molecule, such as dipentaerythritol hexakis (3-mercaptopropionate); compounds having two secondary thiol groups in one molecule, such as 1,4-bis (3-mercaptobutyryloxy) butane; compounds having three secondary thiol groups in one molecule, such as 1,3,5-tris (2- (3-sulfanylbutanoyloxy) ethyl) -1,3,5-triazinane-2,4,6-trione and trimethylolpropane tris (3-mercaptobutyrate); and compounds having four secondary thiol groups in one molecule, such as pentaerythritol tetrakis (3-mercaptobutyrate).

[0073] The compound having the vinyl ether group is a compound having one or more vinyl ether groups (-O-CH=CH2) in one molecule. The number of vinyl ether groups in the compound having the vinyl ether group may be preferably 2 or more, more preferably 3 or more, in terms of the curability of the coating material. On the other hand, in terms of the crack resistance of the coating film, it may be usually 20 or less, preferably 12 or less, more preferably 8 or less.

[0074] Examples of the compound having a vinyl ether group include compounds having one vinyl ether group in one molecule, such as methyl vinyl ether, ethyl vinyl ether, n-propyl vinyl ether, n-butyl vinyl ether, and 2-ethylhexyl vinyl ether; compounds having two vinyl ether groups in one molecule, such as diethylene glycol divinyl ether, dipropylene glycol divinyl ether, triethylene glycol divinyl ether, 1,4-cyclohexanedimethanol divinyl ether, 1,4-butanediol divinyl ether, and 1,6-hexanediol divinyl ether; and compounds having three vinyl ether groups in one molecule, such as trimethylolpropane trivinyl ether.

[0075] Examples of the N-substituted (meth)acrylamide compound include (meth)acryloylmorpholine, N,N-diethyl(meth)acrylamide, and N-hydroxyethyl(meth)acrylamide.

[0076] Examples of the aromatic vinyl compound include styrene, α-methylstyrene, and 4-methylstyrene.

[0077] As the component (A) active energy ray-curable resin, from the viewpoint of the curability of the coating film, the compound having the (meth)acryloyl group is preferred, and the compound having the (meth)acryloyl group and having two or more (meth)acryloyl groups in one molecule (hereinafter sometimes referred to as a "polyfunctional (meth)acrylate") is more preferred, and a compound having three or more (meth)acryloyl groups in one molecule (polyfunctional (meth)acrylate having three or more (meth)acryloyl groups in one molecule) is even more preferred.

[0078] As the active energy ray-curable resin of component (A), from the viewpoint of adhesion between the polyolefin resin substrate and the coating film, particularly adhesion after a wet heat test, polyfunctional (meth)acrylates having an acrylic equivalent of 300 or less are preferred, and compounds having three or more (meth)acryloyl groups in one molecule (polyfunctional (meth)acrylates having three or more (meth)acryloyl groups in one molecule) and having an acrylic equivalent of 300 or less are even more preferred.

[0079] The acrylic equivalent is defined by the following formula (1). A = M / χ (1) In formula (1), A is the acrylic equivalent, M is the molecular weight of the compound, and χ is the number of (meth)acryloyl groups in one molecule.

[0080] Here, the molecular weight of a compound is the molecular weight calculated from the molecular formula when the molecular formula of the compound can be determined. When the molecular formula of a compound cannot be determined, such as a prepolymer or oligomer of polyurethane (meth)acrylate, the molecular weight is the number average molecular weight (Mn) calculated in terms of polystyrene obtained from a differential molecular weight distribution curve (hereinafter sometimes abbreviated as GPC curve) measured by gel permeation chromatography (hereinafter sometimes abbreviated as GPC).

[0081] The measurement of GPC was performed using a high-performance liquid chromatography system "HLC-8320 (trade name)" of Tosoh Corporation (a system including a degasser, a liquid delivery pump, an autosampler, a column oven, and an RI (differential refractive index) detector) as a system; two Shodex GPC columns "KF-806L (trade name)", one each of "KF-802 (trade name)" and "KF-801 (trade name)", a total of four columns were connected in the order of KF-806L, KF-806L, KF-802, and KF-801 from the upstream side and used; tetrahydrofuran (without stabilizer) for high-performance liquid chromatography of Wako Pure Chemical Industries, Ltd. was used as the mobile phase; it can be carried out under the conditions of a flow rate of 1.0 milliliter / minute, a column temperature of 40°C, a sample concentration of 1 milligram / milliliter, and a sample injection volume of 100 microliters. The elution amount at each retention volume can be determined from the detection amount of the RI detector assuming that the molecular weight dependence of the refractive index of the measurement sample is absent. Also, a calibration curve from the retention volume to the polystyrene-converted molecular weight can be created using commercially available standard polystyrene. It should be noted that it should be appropriately selected so that the measured value is interpolated in the calibration curve. As the analysis program, "TOSOH HLC-8320GPC EcoSEC (trade name)" of Tosoh Corporation can be used. Regarding the theory of GPC and the actual measurement, reference can be made to reference books such as "Size Exclusion Chromatography, High-Performance Liquid Chromatography of Polymers, Author: Sadao Mori, First Edition, First Printing, December 10, 1991" by Kyoritsu Shuppan Co., Ltd., and "Synthetic Polymer Chromatography, Editors: Hajime Ohtani, Tatsuya Takasaki (the upper part of '崎' is '立'), First Edition, First Printing, July 25, 2013" by Ohmsha, Ltd.

[0082] The acrylic equivalent of the above polyfunctional (meth)acrylate is preferably 300 or less, more preferably 270 or less, still more preferably 240 or less, even more preferably 200 or less, and most preferably 160 to 85, from the viewpoint of the adhesion between the above polyolefin resin film and the above coating film, particularly the adhesion after the damp heat test.

[0083] When a mixture of two or more types of polyfunctional (meth)acrylates is used as the polyfunctional (meth)acrylate, the acrylic equivalent of the mixture calculated from the acrylic equivalent of each polyfunctional (meth)acrylate and its blending ratio (mass ratio) should be within the above-mentioned range.

[0084] The acrylic equivalent of the mixture can be calculated by the following formula (2). Am=a1×w1+a2×w2+a3×w3+······(2) Here, Am is the acrylic equivalent of the mixture, a1, a2, a3... are the acrylic equivalents of each polyfunctional (meth)acrylate, and w1, w2, w3... are the blending ratios (mass ratios) of each polyfunctional (meth)acrylate.

[0085] In one embodiment, the component (A) active energy ray curable resin may not contain any active energy ray curable resin other than the compound having the (meth)acryloyl group (hereinafter, sometimes referred to as "other active energy ray curable resins"), for example, any one or more selected from a compound having an allyl group, a compound having a thiol group, a compound having a vinyl ether group, an N-substituted (meth)acrylamide compound, and an aromatic vinyl compound. Here, "not containing any one of the other active energy ray curable resins" means that the resin is not intentionally blended. Therefore, "not containing any one of the other active energy ray curable resins" can also be rephrased as "the amount of the resin is usually less than 0.1% by mass, preferably 0.01% by mass or less, more preferably 0.001% by mass or less, based on 100% by mass of the total of the component (A) active energy ray curable resins."

[0086] In one embodiment, the compound having the (meth)acryloyl group may not have any one or more functional groups selected from an amino group, a mercapto group, a vinyl group, an epoxy group, an allyl group, a thiol group, a vinyl ether group, an isocyanate group, and a hydrolyzable group. In one embodiment, the compound having the (meth)acryloyl group may not have any functional groups other than the (meth)acryloyl group and the hydroxyl group.

[0087] As the component (A), the active energy ray-curable resin, one or a mixture of two or more of these can be used.

[0088] (B) Hydrogen abstraction photoinitiator: The coating material contains the component (B) hydrogen abstraction type photoinitiator. The component (B) hydrogen abstraction type photoinitiator is a compound that absorbs light of a specific wavelength, becomes excited, and abstracts hydrogen from surrounding hydrogen donors to generate radicals. The component (B) hydrogen abstraction type photoinitiator functions to polymerize and cure the component (A) active energy ray curable resin by generating radicals.

[0089] Examples of the component (B) hydrogen abstraction type photoinitiator include benzophenone-based compounds, anthraquinone-based compounds, thioxanthone-based compounds, and hexaarylbisimidazoles.

[0090] Examples of the benzophenone compounds include benzophenone, methyl-o-benzoylbenzoate, 4-methylbenzophenone, 4,4'-bis(diethylamino)benzophenone, methyl o-benzoylbenzoate, 4-phenylbenzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone, and 2,4,6-trimethylbenzophenone.

[0091] Examples of the anthraquinone compounds include methylanthraquinone, 2-ethylanthraquinone, 2-t-butylanthraquinone, and 2-amylanthraquinone.

[0092] Examples of the thioxanthone compounds include thioxanthone, 2,4-diethylthioxanthone, and 2,4-diisopropylthioxanthone.

[0093] Among these, benzophenone-based compounds are preferred from the viewpoint of suppressing coloration of the coating film.

[0094] As the component (B), the hydrogen abstraction type photoinitiator, one or a mixture of two or more of these can be used.

[0095] The amount of the hydrogen abstraction type photoinitiator (B) may be, from the viewpoint of adhesion between the polyolefin resin substrate and the coating film, usually 1 part by mass or more, preferably 2 parts by mass or more, more preferably 3 parts by mass or more, and even more preferably 4 parts by mass or more, relative to 100 parts by mass of the active energy ray-curable resin (A) above, while from the viewpoint of suppressing coloration of the coating film, it may be usually 30 parts by mass or less, preferably 20 parts by mass or less, and more preferably 12 parts by mass or less.

[0096] The coating material may further contain other optional components other than the component (A) active energy ray curable resin and the component (B) hydrogen abstraction type photoinitiator, as long as the purpose of the present invention is not violated. Examples of the other optional components include additives such as defoamers, leveling agents, surfactants, thixotropy imparting agents, antistatic agents, antifouling agents, printability improvers, antioxidants, weather resistance stabilizers, light resistance stabilizers, ultraviolet absorbers (excluding compounds corresponding to the component (B) hydrogen abstraction type photoinitiators), photoinitiators other than hydrogen abstraction type, heat stabilizers, inorganic particles, organic particles, inorganic colorants, and organic colorants. As the other optional components, one or a mixture of two or more of these can be used. The amount of the other optional components is not particularly limited, as long as the purpose of the present invention is not violated, since the other optional components are optional components. The amount of the other optional components added may usually be 10 parts by mass or less, 5 parts by mass or less, 1 part by mass or less, or about 0.01 to 10 parts by mass, relative to 100 parts by mass of the active energy ray-curable resin (A) above.

[0097] The coating material may not contain any one or more of the other optional components. Here, not containing any one of the other optional components means that any one of the other optional components is not intentionally blended. Therefore, not containing any one of the other optional components can be rephrased as the blending amount of the other optional components is usually less than 0.1 parts by mass, preferably 0.01 parts by mass or less, more preferably 0.001 parts by mass or less, relative to 100 parts by mass of the component (A) active energy ray curable resin.

[0098] In one preferred embodiment, the coating material may not contain an intramolecular cleavage type photoinitiator from the viewpoint of adhesion between the polyolefin resin substrate and the coating film, particularly adhesion after a wet heat test. The intramolecular cleavage type photoinitiator is a compound that absorbs light of a specific wavelength, cleaves a bond at a specific site, and generates a radical at the cleavage site. Here, not containing the intramolecular cleavage type photoinitiator means that the intramolecular cleavage type photoinitiator is not intentionally blended. Therefore, not containing the intramolecular cleavage type photoinitiator can also be rephrased as the amount of the intramolecular cleavage type photoinitiator blended is usually less than 0.1 parts by mass, preferably 0.01 parts by mass or less, and more preferably 0.001 parts by mass or less, relative to 100 parts by mass of the component (A) active energy ray curable resin.

[0099] Without intending to be bound by theory, it is believed that the intramolecular cleavage photoinitiator absorbs energy from the excited state of the hydrogen abstraction photoinitiator of component (B) and returns it to the ground state, thereby suppressing the abstraction of hydrogen atoms from the surface of the polyolefin resin substrate that is in contact with the uncured coating film.

[0100] In one preferred embodiment, the coating material may not contain an aliphatic tertiary amine compound from the viewpoint of adhesion between the polyolefin resin substrate and the coating film, particularly adhesion after a wet heat test. Here, "not containing an aliphatic tertiary amine compound" means that the aliphatic tertiary amine compound is not intentionally blended. Therefore, "not containing an aliphatic tertiary amine compound" can be rephrased as "the amount of the aliphatic tertiary amine compound is usually less than 0.1 parts by mass, preferably 0.01 parts by mass or less, more preferably 0.001 parts by mass or less, relative to 100 parts by mass of the component (A) active energy ray curable resin. In this embodiment, the aliphatic tertiary amine compound that is also the component (A) active energy ray curable resin is the aliphatic tertiary amine compound. That is, in this embodiment, the component (A) active energy ray curable resin excludes the aliphatic tertiary amine compound.

[0101] In another preferred embodiment, the coating material may not contain an amine compound from the viewpoint of adhesion between the polyolefin resin substrate and the coating film, particularly adhesion after a wet heat test. Here, not containing the amine compound means that the amine compound is not intentionally blended. Therefore, not containing the amine compound can be rephrased as the blending amount of the amine compound is usually less than 0.1 parts by mass, preferably 0.01 parts by mass or less, more preferably 0.001 parts by mass or less, relative to 100 parts by mass of the component (A) active energy ray curable resin. In this embodiment, the amine compound that is also the component (A) active energy ray curable resin is the amine compound. That is, in this embodiment, the component (A) active energy ray curable resin excludes the amine compound.

[0102] The coating material may contain a solvent as desired to dilute it to a concentration that is easy to apply. The solvent is not particularly limited as long as it does not react with the component (A) active energy ray curable resin, the component (B) hydrogen abstraction type photoinitiator, and other optional components, or catalyze (promote) the self-reaction (including deterioration reaction) of these components. Examples of the solvent include 1-methoxy-2-propanol, ethyl acetate, n-butyl acetate, toluene, methyl ethyl ketone, methyl isobutyl ketone, diacetone alcohol, and acetone. The solvent may be one of these or a mixture of two or more of them.

[0103] The above coating material can be obtained by mixing and stirring these components.

[0104] 3.Laminate The laminate of the present invention is a laminate having a coating film on a part or all of the surfaces of a polyolefin resin substrate. In the laminate of the present invention, the polyolefin resin substrate and the coating film are directly laminated. That is, the laminate of the present invention does not include an embodiment in which one or more layers such as an easy-adhesion layer (anchor coat) are interposed between the polyolefin resin substrate and the coating film.

[0105] The coating film of the laminate of the present invention is formed from a coating material containing (A) an active energy ray-curable resin and (B) a hydrogen abstraction type photoinitiator. In one typical embodiment, the coating material contains 100 parts by mass of the (A) active energy ray-curable resin and 1 to 30 parts by mass of the (B) hydrogen abstraction type photoinitiator.

[0106] The coating film of the laminate of the present invention, the paint for forming the same, and the polyolefin resin substrate constituting the laminate of the present invention have been described in "1. Manufacturing method of laminate" and "2. Paint for forming coating film."

[0107] The laminate of the present invention is formed by directly laminating the polyolefin resin substrate and the coating film with sufficient adhesion strength. When a cross-cut test is performed according to JIS K5600-5-6:1999, in which cross-cut cuts are made from the coating film side of the laminate, the laminate of the present invention is preferably classified as Class 0, Class 1, Class 2, or Class 3, more preferably Class 0, Class 1, or Class 2, even more preferably Class 0 or Class 1, and most preferably Class 0.

[0108] The method for producing the laminate of the present invention is not particularly limited and may be any production method. A preferred method for producing the laminate of the present invention is the method described above in "1. Production method of laminate" (production method of the present invention).

[0109] 4.Goods The article of the present invention is an article including a laminate. Here, the laminate is a laminate produced by the manufacturing method of the present invention, or a laminate of the present invention. In one typical embodiment of the article of the present invention, a part or all of the surface of the article is formed by the coating film of the laminate. In another embodiment of the article of the present invention, the coating film of the laminate forms a portion of the surface of the article where scratch resistance is required.

[0110] Examples of the articles of the present invention include image display devices such as televisions, personal computers, tablet-type information devices, and smartphones, as well as their display panels and housings; vehicle windows, vehicle bodies, windshields, roof windows, and instrument panels; refrigerators, washing machines, cupboards, wardrobes, show windows, and the panels that constitute these; and window glass, head-up displays, electronic signs, and solar cells for buildings. EXAMPLES

[0111] The present invention will be described below with reference to examples, but the present invention is not limited to these.

[0112] Measurement method (a) Grid test: According to JIS K5600-5-6:1999, 100 grids (1 grid = 1 mm x 1 mm) were cut into the laminate from the coating layer side, and then adhesion test tape was applied to the grids, rubbed with fingers, and peeled off to perform a grid test (evaluation of adhesion between the resin film and the coating). The evaluation criteria were in accordance with Table 1 of the above JIS standard. Category 0: The edges of the cut are completely smooth and there are no peeling marks on any of the grids. Category 1: Small separations of the coating at the intersections of cuts. No more than 5% of the cross-cut area is affected. Category 2: The coating has flaked along the edges of the cuts and / or at the intersections. Clearly more than 5% but not more than 15% of the cross-cut area is affected. Category 3: The coating has suffered partial or complete major flaking along the edges of the cuts and / or partial or complete flaking of various areas of the mesh. Cross-cut areas are affected in areas significantly greater than 15% but not more than 35%. Category 4: The coating has suffered partial or complete major flaking along the edges of the cuts and / or partial or complete flaking in several areas. Cross-cut areas are clearly more than 35% affected but not more than 65% affected. Category 5: When the degree of peeling exceeds category 4.

[0113] (b) Cross-cut test after heat and humidity test: The laminate was treated in a thermo-hygrostat at a temperature of 60° C. and a relative humidity of 90% for 500 hours, and then a cross-cut test after a wet heat test was carried out in the same manner as in the above test (a) cross-cut test.

[0114] (C) Pencil hardness: In accordance with JIS K5600-5-4:1999, the pencil hardness of the coating surface of the laminate was measured using a "Uni" (product name) pencil from Mitsubishi Pencil Co., Ltd., under conditions of a test length of 25 mm and a load of 750 g. The occurrence of scratches was judged by visually observing the sample surface under a fluorescent lamp at a position 50 cm away from the lamp.

[0115] (d) Yellowness index; The yellowness index was measured using a colorimeter "SolidSpec-3700 (product name)" manufactured by Shimadzu Corporation in accordance with JIS K7105:1981.

[0116] Raw materials used (P) Polyolefin resin substrate: (P-1) Zeonoafilm ZF-16 (product name) is a cyclic olefin resin film manufactured by Zeon Corporation. It has a thickness of 100 μm and is a type that has not been treated for easy adhesion. The wettability index of the coating surface of the resin film measured immediately before the production of the laminate was 38 mN / m. (P-2) Using polypropylene "F-730NV (trade name)" manufactured by Prime Polymer Co., Ltd., a 50 μm thick polypropylene film was produced using a T-die film-producing device equipped with a 40 mm extruder, a T-die, and a take-up device, with the T-die outlet resin temperature at 250° C. No adhesion treatment was performed. The wettability index of the coating surface of the resin film measured immediately before producing the laminate was 37 mN / m.

[0117] (A) Active energy ray curable resin: (A-1) "KAYARAD DPHA (product name)" by Nippon Kayaku Co., Ltd. A mixture of dipentaerythritol hexaacrylate and dipentaerythritol pentaacrylate. Since the mixture has 0.63 mol / kg of hydroxyl groups, the mass ratio of dipentaerythritol hexaacrylate (acrylic equivalent 96) is 0.67, the mass ratio of dipentaerythritol pentaacrylate (acrylic equivalent 105) is 0.33, and the acrylic equivalent of the mixture is calculated to be 99. (A-2) Pentaerythritol triacrylate. CAS number 3524-68-3, acrylic equivalent 99. (A-3) Pentaerythritol tetraacrylate. CAS number 4986-89-4, acrylic equivalent 88. (A-4) "Art Resin UN-954 (product name)" multifunctional urethane (meth)acrylate from Negami Chemical Industrial Co., Ltd. Solid content 60% by mass, number of functional groups (number of (meth)acryloyl groups per molecule; same below), number average molecular weight 2000, mass average molecular weight 4800, Z-average molecular weight 9600, acrylic equivalent 333. (A-5) "Art Resin UN-952 (product name)" multifunctional urethane (meth)acrylate from Negami Chemical Industries, Ltd. Solid content 60% by mass, number of functional groups 10, number average molecular weight 2500, mass average molecular weight 9100, Z-average molecular weight 23000, acrylic equivalent 250. (A-6) Multifunctional urethane (meth)acrylate "U-6LPA (product name)" from Shin-Nakamura Chemical Co., Ltd. Functional group number 6, number average molecular weight 1050, mass average molecular weight 1420, Z-average molecular weight 2080, acrylic equivalent 175. (A-7) Glycerin diglycidyl ether acrylic acid adduct "Epoxy Ester 80MFA (product name)" from Kyoeisha Chemical Co., Ltd. Functional group number: 2, acrylic equivalent: 174. (A-8) Ditrimethylolpropane tetraacrylate "Aronix M-408 (trade name)" from Toagosei Co., Ltd. CAS number 94108-97-1, acrylic equivalent 117.

[0118] (B) Hydrogen abstraction photoinitiator (B-1) 4-Methylbenzophenone. CAS number 134-84-9. (B-2) 2,4-Diethylthioxanthone. CAS number 82799-44-8.

[0119] (C) Photoinitiators other than hydrogen abstraction type (C-1) IGM Resins' α-hydroxyalkylphenone photoinitiator (1-hydroxycyclohexyl-phenyl ketone) "Omnirad 184 (trade name)". Intramolecular cleavage type photoinitiator.

[0120] (D) Other ingredients (D-1) Aliphatic tertiary amine compound (N-(2-dimethylaminoethyl)acrylamide). CAS number 925-76-8

[0121] Example 1 (a) Preparation of coating material for film formation 100 parts by mass of the above (A-1), 5 parts by mass of the above (B-1), and a 1:1 (mass ratio) mixed solvent of methyl ethyl ketone and 1-methoxy-2-propanol were mixed and stirred to obtain a coating material for forming a coating film with a solid content of 30 mass %. (b) Process (1) Using this coating material for forming a coating film, a film Mayer bar type coating device was used to form a wet coating film on one side of the above (P-1) so that the thickness after curing would be 8 μm, and an intermediate laminate 1 having the wet coating film on one side of the above (P-1) was obtained. (c) Step (2) and Step (3) Next, the intermediate laminate 1 was passed through a drying furnace set at an internal temperature of 80°C at a line speed such that the time required for passing from the entrance to the exit was 1 minute to dry the wet coating film, thereby obtaining an intermediate laminate 2 having an uncured coating film on one side of the (P-1) and preheating it to a temperature of 80°C. (d) Process (4) Next, the uncured coating film of the intermediate laminate 2 was completely cured using a curing device whose conceptual diagram is shown in Figure 1. In this curing device, a high-pressure mercury lamp type ultraviolet irradiation device 1 and a specular metal roll 3, and a high-pressure mercury lamp type ultraviolet irradiation device 2 and a specular metal roll 4 are arranged facing each other, and first irradiation is performed from the surface of the intermediate laminate 2 on the uncured coating film side (sub-step (4-2) using the high-pressure mercury lamp type ultraviolet irradiation device 1), and then irradiation is performed from the surface of the intermediate laminate 2 opposite to the uncured coating film surface (sub-step (4-1) using the high-pressure mercury lamp type ultraviolet irradiation device 2). In Example 1, the accumulated light amount from the high-pressure mercury lamp type ultraviolet irradiation device 1 was 800 mJ / cm2. 2 The mirror-finished metal roll 3 was treated at a temperature of 80° C. to obtain a laminate having a coating film (completely cured coating film) on one side of the above (P-1). At this time, irradiation with a high-pressure mercury lamp type ultraviolet irradiation device 2 was not performed. In addition, the mirror-finished metal roll 4 was not heated. (e) Evaluation of the laminate The above tests (a) to (d) were carried out, and the results are shown in Table 1.

[0122] Examples 2-9, 11-15 A laminate having a coating film (completely cured coating film) on one side of the above (P-1) was obtained in the same manner as in Example 1, except that the composition of the coating material for forming the coating film was changed as shown in Table 1. The above tests (a) to (d) were carried out. The results are shown in Table 1 or 2.

[0123] Example 10 The composition of the paint for forming the coating film was changed as shown in Table 1, and the conditions for the process of completely curing the uncured coating film were changed to an integrated light dose of 400 mJ / cm using a high-pressure mercury lamp type ultraviolet irradiation device 1. 2 The temperature of the mirror-finished metal roll 3 was 80° C., and the cumulative light quantity from the high-pressure mercury lamp-type ultraviolet irradiation device 2 was 400 mJ / cm.2 A laminate having a coating film (completely cured coating film) on one side of the above (P-1) was obtained in the same manner as in Example 1, except that the temperature of the mirror-finished metal roll 4 was changed to 80° C. The above tests (a) to (d) were carried out. The results are shown in Table 1.

[0124] Example 16 Except for using the above (P-2) instead of the above (P-1), a laminate having a coating film (completely cured coating film) on one side of the above (P-2) was obtained in the same manner as in Example 1. The above tests (a) to (d) were carried out. The results are shown in Table 2.

[0125] Examples 17-24 A laminate having a coating film (completely cured coating film) on one side of the above (P-1) was obtained in the same manner as in Example 1, except that the formulation of the coating material for forming the coating film and the conditions for the process of completely curing the uncured coating film were changed as shown in Table 1. The above tests (a) to (d) were carried out. The results are shown in Table 2.

[0126] [Table 1]

[0127] [Table 2]

[0128] It was found that the laminate produced by the manufacturing method of the present invention has a coating film (hard coat) formed by using a coating material mainly composed of an active energy ray curable resin directly laminated on the surface of the polyolefin resin substrate, and yet the two are laminated with sufficient adhesive strength. Furthermore, it was found that the laminate produced by the preferred manufacturing method of the present invention maintains sufficient adhesive strength even after a wet heat test.

[0129] Furthermore, for the laminates of Example 1 and Example 18, the total light transmittance (unit: %) was measured according to JIS K 7361-1:1997 using a turbidity meter "NDH2000 (product name)" manufactured by Nippon Denshoku Industries Co., Ltd. The results were 90.5% for Example 1 and 90.3% for Example 2, demonstrating that the laminates have transparency suitable for use in the optical field.

[0130] In the manufacturing method of the present invention, sufficient adhesion strength is exhibited even when a polyolefin-based resin substrate is used as the resin substrate, so it will be obvious to those skilled in the art that the method is also useful when forming a coating film (hard coat) directly on the surface of a resin substrate other than a polyolefin-based resin substrate using a coating material mainly composed of an active energy ray curable resin. Examples of such embodiments are summarized as follows. In addition, it goes without saying that the invention can be carried out by replacing the "polyolefin-based resin substrate" in the description of the manufacturing method of the present invention with the "resin substrate". [1]. A method for producing a laminate having a coating film on a part or all of the surfaces of a resin substrate, comprising the steps of: The resin substrate and the coating film are directly laminated together, (1) forming a wet coating film on a part or all of the surfaces of the resin substrate using a coating material for forming the coating film, thereby obtaining an intermediate laminate 1 having the wet coating film on a part or all of the surfaces of the resin substrate; (2) a step of pre-drying the wet coating film to form an uncured coating film, thereby obtaining an intermediate laminate 2 having the uncured coating film on a part or all of the surfaces of the resin substrate; (3) preheating the intermediate laminate 2 to a temperature of 65° C. or higher; and (4) a step of irradiating the uncured coating film with active energy rays to completely cure the uncured coating film; wherein the coating comprises: (A) 100 parts by mass of an active energy ray-curable resin; and (B) 1 to 30 parts by mass of a hydrogen abstraction type photoinitiator; A method for producing the laminate, comprising: However, this does not include the resin substrate on which the coating film is formed, the surface being formed from a polyolefin resin. [2]. The method for producing a laminate according to item [1], wherein the component (A) active energy ray-curable resin contains a polyfunctional (meth)acrylate. [3]. The method for producing a laminate according to item [2], wherein the polyfunctional (meth)acrylate contains a polyfunctional (meth)acrylate having an acrylic equivalent of 300 or less. [4]. The method for producing a laminate according to item [1], wherein the step (4) includes a sub-step of irradiating active energy rays from at least a surface of the intermediate laminate 2 opposite to the uncured coating film. [5]. The method for producing a laminate according to item [1], wherein the coating material does not contain an intramolecular cleavage type photoinitiator. [Brief description of the drawings]

[0131] [Figure 1] FIG. 2 is a conceptual diagram of an ultraviolet irradiation device used in the examples. [Explanation of symbols]

[0132] 1: Mirror-finished metal roll a 2: Mirror-finished metal roll b 3: Ultraviolet irradiation device a 4: Ultraviolet irradiation device b 5: An intermediate laminate having an uncured coating film on one side of a polyolefin resin film 6: Uncured coating surface side of the intermediate laminate 7: Web running direction

Claims

1. A method for producing a laminate having a coating film on a part or all of the surfaces of a polyolefin resin substrate, comprising the steps of: The polyolefin resin substrate and the coating film are directly laminated together, (1) A step of forming a wet coating film on a part or all of the surfaces of the polyolefin-based resin substrate using a coating material for forming the coating film, thereby obtaining an intermediate laminate 1 having the wet coating film on a part or all of the surfaces of the polyolefin-based resin substrate; (2) A step of pre-drying the wet coating film to form an uncured coating film, thereby obtaining an intermediate laminate 2 having the uncured coating film on a part or all of the surfaces of the polyolefin-based resin substrate; (3) preheating the intermediate laminate 2 to a temperature of 65° C. or higher; and (4) A step of irradiating the uncured coating film with active energy rays to completely cure the uncured coating film; wherein the coating comprises: (A) 100 parts by mass of an active energy ray-curable resin; and (B) Hydrogen abstraction type photoinitiator 1 to 30 parts by mass; A method for producing the laminate comprising the steps of:

2. The method for producing a laminate according to claim 1 , wherein the component (A) active energy ray curable resin contains a polyfunctional (meth)acrylate.

3. The method for producing a laminate according to claim 2 , wherein the polyfunctional (meth)acrylate includes a polyfunctional (meth)acrylate having an acrylic equivalent of 300 or less.

4. The method for producing a laminate according to claim 1 , wherein the step (4) includes a sub-step of irradiating the intermediate laminate (2) with active energy rays from a surface opposite to the uncured coating film.

5. The method for producing a laminate according to claim 1 , wherein the coating material does not contain an intramolecular cleavage type photoinitiator.

6. The method for producing a laminate according to claim 1 , wherein the coating material does not contain an aliphatic tertiary amine compound.

7. A method for producing an article comprising a laminate, the method comprising the step of producing a laminate using the method for producing a laminate according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Ultraviolet-curable composition and resin molded article coated with the same

    JP2002356505A

  • Photoradical polymerization initiator

    JP2016113393A

  • Hard coat film

    JP2016187870A