Electrophotographic image forming system, electrophotographic image forming apparatus, developing sleeve, developing roller, and image forming method
The use of a silicon-enhanced aluminum alloy developing sleeve and oppositely charged toner additives addresses fogging and toner spillage issues in electrophotographic image forming systems, particularly in high humidity environments, by maintaining optimal toner charge levels.
Patent Information
- Application Number
- JP2023066086
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-25
AI Technical Summary
Existing electrophotographic image forming systems experience fogging and toner spillage due to insufficient charge on toner in high temperature and humidity environments, particularly in southern China and Southeast Asia, despite conventional methods to maintain charge levels.
Incorporating a developing sleeve made of an aluminum alloy with a silicon content of more than 0.6% by mass and using a developer with toner containing an external additive charged to an opposite polarity to the toner, which enhances charge retention and reduces leakage.
The solution effectively suppresses fogging and toner spillage by maintaining adequate charge levels on toner, even in high temperature and humidity conditions, ensuring high-quality image formation.
Smart Images

Figure 2024152108000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrophotographic image forming system, an electrophotographic image forming apparatus, a developing sleeve, a developing roller, and an image forming method, and more particularly to an electrophotographic image forming system and the like that suppresses fogging in a formed image and suppresses toner spillage in an electrophotographic image forming apparatus. [Background technology]
[0002] In recent years, in electrophotographic copying machines and printers, developers using toner for developing electrostatic images (hereinafter, simply referred to as "toner") have become mainstream because of their advantage in high-speed development. In detail, an electrostatic image is formed on a photoconductor by a laser, and the electrostatic image is developed using the charged toner.
[0003] A developing sleeve is known as a means for transporting toner to, for example, a photoconductor. Charged toner is attached to the developing sleeve, or the toner is attached to the developing sleeve and then charged, and the developing sleeve is rotated, whereby the charged toner can be transported to the photoconductor.
[0004] Therefore, the toner must have a desired charge amount during development, and must be held on the developing sleeve by image force.
[0005] If the toner does not have a sufficient charge when it is transported to the photoconductor, the toner will adhere to the non-electrostatic image areas (non-image areas) of the photoconductor, resulting in the formation of unintended image areas, known as "fogging."
[0006] In addition, when the charged toner comes into contact with the developing sleeve (metal), an attractive force acts on it, in other words, the surface of the developing sleeve acts as a mirror, and an attractive force acts on the opposite side of the toner, similar to that when there is an opposite charge. This is called "image force." If the image force decreases, the toner cannot be sufficiently held on the developing sleeve, and toner spills out.
[0007] In order for the toner to have a desired charge amount during development, it is necessary to increase the charge amount itself at the time of charging, or to maintain the charge amount of the toner (suppress a decrease in the charge amount). Therefore, technologies have been proposed to specify the surface roughness of the conductive layer of the developing sleeve (Patent Document 1), to specify the material of the surface layer of the regulating member (Patent Document 2), or to specify the external additives of the toner (Patent Document 3).
[0008] However, these conventional methods were not suitable for the high temperature and humidity environments of southern China and Southeast Asia, and therefore there still exist problems such as fog and toner spillage during continuous printing due to the decrease in the charge of the toner during development in high temperature and humidity environments. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Japanese Patent Application Publication No. 08-179620 [Patent Document 2] Japanese Patent Application Publication No. 05-188652 [Patent Document 3] JP 2007-34164 A Summary of the Invention [Problem to be solved by the invention]
[0010] The present invention has been made in consideration of the above problems and circumstances, and the problem to be solved is to provide an electrophotographic image forming system, an electrophotographic image forming apparatus, a developing sleeve, a developing roller, and an image forming method that suppress fog in formed images and suppress toner spillage within the electrophotographic image forming apparatus. [Means for solving the problem]
[0011] In order to solve the above-mentioned problems, the present inventors have investigated the causes of the above-mentioned problems, and as a result, have found that in an electrophotographic image forming system, when the developing sleeve contains an aluminum alloy containing more than 0.6% by mass of silicon, and the developer contains a toner for developing an electrostatic image having an external additive, and the external additive is charged with a polarity opposite to that of the toner for developing an electrostatic image, fogging in the formed image can be suppressed and toner spillage within the electrophotographic image forming apparatus can be suppressed, thereby arriving at the present invention. That is, the above-mentioned problems of the present invention are solved by the following means.
[0012] 1. An electrophotographic imaging system having a developing sleeve for transporting a developer, the developing sleeve comprises an aluminum alloy containing more than 0.6% by weight of silicon; the developer contains a toner for developing an electrostatic image having an external additive, The external additive is charged with a polarity opposite to that of the toner for developing an electrostatic image. 23. An electrophotographic imaging system comprising:
[0013] 2. The developer is a one-component developer. 2. The electrophotographic imaging system of claim 1.
[0014] 3. The silicon content is within the range of 0.8 to 12.6 mass% based on the total mass of the aluminum alloy. 2. The electrophotographic imaging system of claim 1.
[0015] 4. The copper content is 2.0 mass% or less based on the total mass of the aluminum alloy. 2. The electrophotographic imaging system of claim 1.
[0016] 5. The external additive is an inorganic particle. 2. The electrophotographic imaging system of claim 1.
[0017] 6. The inorganic particles are titanic acid compounds. 6. The electrophotographic imaging system of claim 5.
[0018] 7. An electrophotographic imaging system having a developing sleeve for transporting a developer, the developing sleeve comprises an aluminum alloy containing more than 0.6% by weight of silicon; the developer contains a toner for developing an electrostatic image having an external additive, The external additive is titanium strontium oxide. 23. An electrophotographic imaging system comprising:
[0019] 8. An electrophotographic image forming apparatus including at least a developing sleeve for transporting the developer, The electrophotographic image forming system according to any one of claims 1 to 7, 2. An electrophotographic image forming apparatus comprising:
[0020] 9. The electrophotographic image forming apparatus according to claim 8 is provided with The developing sleeve is characterized by the above.
[0021] 10. Having the developing sleeve described in item 9 A developing roller characterized by:
[0022] 11. The electrophotographic image forming system according to any one of claims 1 to 7 is used. 1. An image forming method comprising: Effect of the Invention
[0023] According to the above-mentioned means of the present invention, it is possible to provide an electrophotographic image forming system, an electrophotographic image forming apparatus, a developing sleeve, a developing roller, and an image forming method, which are capable of suppressing fogging in an image formed and suppressing toner spillage in an electrophotographic image forming apparatus.
[0024] Although the mechanism by which the effects of the present invention are manifested or the mechanism by which the effects of the present invention are acted upon has not been clearly understood, it is speculated as follows.
[0025] In order to prevent fogging and toner spillage, the toner needs to have a desired charge amount during development. Methods for obtaining a toner with a desired charge amount during development include increasing the charge amount itself during charging, or maintaining the charge amount of the toner (suppressing a decrease in the charge amount).
[0026] Although the mechanism is not yet clear, it is believed that the charge amount of a toner changes depending on temperature and humidity. In particular, in a high-temperature and high-humidity environment, it is difficult to obtain a sufficient charge amount, and most toners are weakly charged relative to the desired charge amount.
[0027] In addition, in a high humidity environment, water can get into the inside of the image forming device and adhere to the surface of the developing sleeve. If charged toner adheres to the water, the charge leaks through the water, and the charge on the toner is likely to decrease.
[0028] In particular, in image forming devices compatible with one-component developers, the toner is triboelectrically charged by passing between the developing sleeve and the regulating member, and therefore, if water is adsorbed to the regulating member in addition to the surface of the developing sleeve, the leakage of charge increases further, and the charge amount of the toner is likely to decrease.
[0029] Therefore, the electrophotographic image forming system of the present invention, by combining the electrophotographic image forming apparatus of the present invention with a specific toner, increases the charge amount itself during charging and suppresses the decrease in the charge amount of the toner.
[0030] The electrophotographic image forming apparatus of the present invention has a developer transport means, and the developer transport means includes a developing sleeve having a metal part, and the metal part contains an aluminum alloy, and the silicon content is more than 0.6 mass % based on the total mass of the aluminum alloy. It is believed that when the silicon content exceeds 0.6 mass %, silicon (Si) crystals are precipitated, increasing the resistance value of the metal portion, thereby making it possible to suppress leakage of the toner charge.
[0031] The developer according to the present invention includes a toner for developing electrostatic images having an external additive. The external additive is charged with a polarity opposite to that of the toner for developing electrostatic images. More specifically, the developer according to the present invention is composed of at least a toner for developing electrostatic images including toner particles having an external additive attached to the surface of a toner base particle, and the polarity sign (±) of the charge of the external additive when the external additive and the Image Society of Japan standard carrier N-01 are shaken at a rotation speed of 200 rpm for 10 minutes and triboelectrically charged is opposite to the polarity sign (±) of the charge of the toner for developing electrostatic images when the toner for developing electrostatic images and the Image Society of Japan standard carrier N-01 are shaken at a rotation speed of 200 rpm for 10 minutes and triboelectrically charged. In other words, a combination of an external additive and a toner base particle (toner particle) that exhibits an opposite polarity in the triboelectric charge with the standard carrier is used, which is believed to further increase the amount of charge generated by friction between the external additive and the toner base particle (toner particle). It is believed that the effects of the present invention can be obtained through a similar mechanism whether the developer is a one-component developer or a two-component developer. [Brief description of the drawings]
[0032] [Figure 1] Schematic diagram showing an example of a developing roller [Diagram 2] Schematic cross-sectional view showing an example of a developing sleeve [Diagram 3] FIG. 1 is a schematic cross-sectional view showing an example of a developing roller in which a metal portion and a shaft are integrated together. [Figure 4] 1 is a schematic cross-sectional view showing an example of a developing device; [Diagram 5] 1 is a schematic cross-sectional view showing an example of a full-color image forming apparatus. [Figure 6] Schematic diagram showing where the black ratio is calculated in the evaluation of fogging DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] The electrophotographic image forming system of the present invention is an electrophotographic image forming system including a developing sleeve that transports a developer, the developing sleeve containing an aluminum alloy containing more than 0.6% by mass of silicon, the developer including a toner for developing an electrostatic image having an external additive, and the external additive being charged with a polarity opposite to that of the toner for developing an electrostatic image. This feature is a technical feature common to or corresponding to the following embodiments.
[0034] In an embodiment, from the viewpoint of obtaining the effects of the present invention significantly, the developer is preferably a one-component developer.
[0035] In an embodiment, from the viewpoint of obtaining a sufficient resistance value of the metal part and suppressing peeling of the coating layer, the silicon content is preferably within the range of 0.8 to 12.6 mass % with respect to the total mass of the aluminum alloy.
[0036] In an embodiment, from the viewpoint of facilitating molding and obtaining a sufficient resistance value of the metal part, the copper content is preferably 2.0 mass% or less with respect to the total mass of the aluminum alloy. When copper is added to an aluminum alloy, it becomes soft and easy to mold. However, copper has a property of easily absorbing water. Therefore, by making the copper content 2.0 mass% or less, it is possible to suppress the decrease in the resistance value of the metal part due to the influence of the absorbed moisture, and the effect can be obtained sufficiently.
[0037] In an embodiment, from the viewpoint of the chargeability of the toner, the external additive is preferably an inorganic particle, and the inorganic particle is more preferably a titanic acid compound.
[0038] The electrophotographic image forming system of the present invention is an electrophotographic image forming system including a developing sleeve that transports a developer, the developing sleeve containing an aluminum alloy containing more than 0.6% by mass of silicon, the developer including a toner for developing an electrostatic charge image having an external additive, and the external additive being strontium titanium oxide.
[0039] The electrophotographic image forming apparatus of the present invention is an electrophotographic image forming apparatus including at least a developing sleeve for transporting the developer, and is characterized in that it is used in the electrophotographic image forming system of the present invention.
[0040] The developing sleeve of the present invention is characterized in that it is provided in the electrophotographic image forming apparatus of the present invention. The developing roller of the present invention is characterized by having the developing sleeve of the present invention. The image forming method of the present invention is characterized by using the electrophotographic image forming system of the present invention.
[0041] The present invention, its components, and embodiments for carrying out the present invention will be described in detail below. In this application, the symbol "to" is used to mean that the numerical values before and after the symbol "to" are included as the lower limit and upper limit.
[0042] 1. Overview of the Invention The electrophotographic image forming system of the present invention is an electrophotographic image forming system including a developing sleeve that transports a developer, the developing sleeve containing an aluminum alloy containing more than 0.6% by mass of silicon, the developer including a toner for developing an electrostatic image having an external additive, and the external additive being charged with a polarity opposite to that of the toner for developing an electrostatic image. In addition, "charged to the opposite polarity" means that the developer is composed of an electrostatic image developing toner containing toner particles having an external additive adhered to the surface of the toner base particles, and when the external additive and the Image Society of Japan standard carrier N-01 are shaken at a rotation speed of 200 rpm for 10 minutes and frictionally charged, the polarity sign (±) of the charge of the external additive is opposite to the polarity sign (±) of the charge of the electrostatic image developing toner when the Image Society of Japan standard carrier N-01 is shaken at a rotation speed of 200 rpm for 10 minutes and frictionally charged.
[0043] That is, the electrophotographic image forming system of the present invention is characterized by combining the electrophotographic image forming apparatus of the present invention with a specific toner.
[0044] The electrophotographic image forming apparatus of the present invention is an electrophotographic image forming apparatus including at least a developing sleeve for transporting a developer, and is characterized in that it is used in the above-mentioned electrophotographic image forming system.
[0045] In detail, the developer transport means comprises a developing sleeve having a metal part, the metal part contains an aluminum alloy, and the silicon content is more than 0.6 mass% relative to the total mass of the aluminum alloy.
[0046] The electrophotographic image forming apparatus of the present invention (hereinafter, also simply referred to as "image forming apparatus") forms an image by an electrophotographic method. In general, an electrophotographic image forming apparatus has a charging means for charging the surface of an image holder, an electrostatic image forming means for forming an electrostatic image on the surface of the charged image holder, a developing means for developing the electrostatic image formed on the surface of the image holder as a toner image, a transfer means for transferring the toner image formed on the surface of the image holder to the surface of a recording medium, and a fixing means for fixing the toner image transferred to the surface of the recording medium.
[0047] In the image forming apparatus according to the embodiment, the developing means includes a means for transporting the developer to, for example, the surface of an image carrier (photoconductor) or another developing roller, etc. The means includes a developing sleeve having a metal portion.
[0048] The developing sleeve, developing roller, electrophotographic image forming apparatus, electrophotographic image forming system, and image forming method of the present invention will be described in this order.
[0049] 2. Overview of the developing sleeve The developing sleeve of the present invention is characterized in that it is provided in the electrophotographic image forming apparatus of the present invention. In detail, the developer transport device is provided on a means for transporting a developer, has a metal part, and is characterized in that the metal part contains an aluminum alloy and has a silicon content of more than 0.6 mass% relative to the total mass of the aluminum alloy.
[0050] It is believed that this provides the metal portion with a sufficient resistance value (electrical resistance value), making it possible to suppress leakage of the toner charge.
[0051] 3. Structure of the developing sleeve In the present invention, the term "developing sleeve" refers to a means that carries a developer and has a function of transporting the developer to another adjacent developing sleeve or a photoconductor on which an electrostatic image is formed. The developing sleeve has at least a columnar or cylindrical metal part. The developing sleeve is attached to a developing device with a "flange" or "shaft" attached as necessary. The developing sleeve with the flange or shaft attached is called a "developing roller."
[0052] In the present invention, the term "flange" refers to a part that is different in shape from a columnar or cylindrical shape and is made of a different material than the metal part, and the term "shaft" refers to a cylindrical part that is joined to the "flange" and transmits power from the motor to the developing sleeve.
[0053] 1 is a schematic diagram showing an example of a developing roller 18. It is preferable that the developing roller 18 has flanges 16 or shafts 17 attached to both ends of a developing sleeve 11 having a metal portion.
[0054] In the present invention, the developing sleeve may have a coating layer in addition to the metal portion. Fig. 2 is a schematic cross-sectional view showing an example of a developing sleeve. The developing sleeve 11 shown in Fig. 2(a) is composed only of a metal part 12. As shown in Fig. 2(b), the developing sleeve 11 preferably has a coating layer 13 on the outer peripheral surface of the metal part 12. As shown in Fig. 2(c), the coating layer 13 may be formed of two layers, a lower layer 14 and an upper layer 15. The lower layer 14 and the upper layer 15 may each be formed of multiple layers.
[0055] Generally, a flange is attached to the developing sleeve for the purpose of attaching the shaft to the developing sleeve. Therefore, if the metal part of the developing sleeve and the shaft are made of the same material and are integrated with each other, it is not necessarily necessary to provide a flange. 3 is a schematic cross-sectional view showing an example of a developing roller in which the metal portion and the shaft are integrated. The developing roller 18 has a shaft 17 at both ends of a developing sleeve 11 having, for example, a cylindrical metal portion 12. The metal portion 12 and the shaft 17 are integrated. The developing sleeve 11 preferably has a coating layer 13 on the outer circumferential surface of the metal portion 12.
[0056] (1) Metal parts The metal part according to the present invention is characterized in that it contains an aluminum alloy and has a silicon content of more than 0.6 mass% relative to the total mass of the aluminum alloy. The silicon content is preferably within a range of 0.80 to 12.60 mass%, more preferably within a range of 0.80 to 9.20 mass%, and even more preferably within a range of 0.81 to 9.20 mass%, relative to the total mass of the aluminum alloy.
[0057] It is believed that when the silicon content exceeds 0.6 mass %, silicon (Si) crystals are precipitated, increasing the resistance value of the metal portion, thereby making it possible to suppress leakage of the toner charge. In addition, by making the silicon content 0.8% by mass or more, silicon crystals are uniformly dispersed in the aluminum (Al) and the resistance value of the metal part becomes uniform, which is believed to further suppress the leakage of the toner charge.
[0058] On the other hand, by keeping the silicon content at 12.6 mass% or less, the temperature is below the eutectic point of silicon (Si) in the Al-Si system. This prevents the silicon crystal size from becoming too large, making the surface of the metal part relatively smooth, improving adhesion between the metal part and the coating layer and preventing the coating layer from peeling off.
[0059] The metal portion may further contain other metal components such as copper, iron, chromium, and nickel in addition to silicon. It is preferable that the material of the metal part is soft and easy to mold (workability, productivity), and therefore the aluminum alloy further contains copper. However, copper is prone to adsorb water, and when copper adsorbs water, the resistance value of the metal part is likely to decrease. Therefore, the copper content is preferably 2.0 mass% or less, and more preferably within the range of 0.2 to 1.2 mass%, based on the total mass of the aluminum alloy.
[0060] The metal part may further contain a conductive material in addition to the aluminum alloy. Examples of the conductive material include copper alloy, stainless steel (iron and chromium alloy), iron plated with chromium or nickel, conductive synthetic resin, etc. The metal part preferably contains 80 mass % or more of the aluminum alloy, and more preferably 100 mass %.
[0061] The type and amount of elements contained in the metal portion can be measured by high-frequency inductively coupled plasma atomic emission spectrometry.
[0062] Inductively Coupled Plasma Atomic Emission Spectroscopy (ICPAS) is a method in which a solution sample in which metals are dissolved in acid or alkali is sprayed into Ar plasma. The excited light is then split into individual wavelengths, and the type and content of elements are quantified from the light intensity. With this method, there is a linear relationship between light intensity and content from trace to high concentrations, and each element can be analyzed simultaneously.
[0063] As a measuring device for high frequency inductively coupled plasma optical emission spectrometry, for example, "ULTIMA2000" (manufactured by Horiba, Ltd.) can be used.
[0064] The outer diameter of the metal part is preferably within a range of 5 to 30 mm, and more preferably within a range of 10 to 20 mm. In addition, the metal part is preferably a member that leaks electric charge accumulated on the surface of the developing sleeve, and therefore has a specific resistance of 1×10 4 The resistivity is preferably Ω·cm or less. The resistivity can be measured by a known method.
[0065] The shape of the metal part is not particularly limited, and may be a columnar or cylindrical shape. However, from the above viewpoint and from the viewpoint of weight reduction, it is preferable that the metal part is a hollow cylinder and a flange is attached. It is also preferable that a shaft (shaft part) is attached to the flange. When it is cylindrical, the thickness of the metal part is preferably within the range of 0.8 to 2.0 mm. The material and shape of the flange and shaft are not particularly limited, and they do not necessarily have to be made of the same material as the metal portion.
[0066] (2) Covering layer The developing sleeve of the present invention preferably has a coating layer on the outer circumferential surface of the shaft. By having the coating layer, the photoconductor (image carrier) and the developing sleeve can be brought close to each other, and the toner can be efficiently transported to the photoconductor. In more detail, by having the coating layer, the developing sleeve can be given appropriate hardness and elasticity, and the developing sleeve can be pressed against the photoconductor with an appropriate nip width and nip pressure.
[0067] The Asker C hardness of the coating layer is preferably within a range of 20 to 100. The Asker C hardness conforms to Asker C type SRIS (Japan Rubber Association Standard) 0101 and can be measured by an Asker Rubber Hardness Tester (manufactured by Kobunshi Keiki Co., Ltd.) using a separately prepared test piece.
[0068] The thickness of the coating layer is preferably within the range of 1 to 30 μm, and more preferably within the range of 5 to 20 μm. The resistance of the coating layer is 1×10 4 ~1×10 10 It is preferable that the resistivity is in the range of Ω·cm.
[0069] The coating layer can be formed, for example, by applying a coating liquid prepared by appropriately mixing a conductive agent (electronic conductive agent or ionic conductive agent) and a resin, and optionally a non-conductive filler, to the outer circumferential surface of the shaft. The coating liquid is then dried, and if desired, heated and cured. However, the method of forming the coating layer is not limited to this, and will be described in detail later.
[0070] (2.1) Resin for coating layer The resin of the coating layer is not particularly limited, and examples thereof include silicone copolymerized polyurethane, siloxane-modified polyurethane, acrylic resin, urea resin, melamine resin, alkyd resin, modified alkyd resin such as phenol-modified or silicone-modified, oil-free alkyd resin, silicone resin, fluororesin, phenolic resin, polyamide, epoxy resin, polyester, maleic acid resin, urethane resin, etc. Among these, silicone copolymerized polyurethane, siloxane-modified polyurethane, acrylic resin, or polyamide is preferable from the viewpoint of self-film reinforcement, toner chargeability, etc. Among these, siloxane-modified polyurethane is preferable from the viewpoint of abrasion resistance.
[0071] (2.1.1) Urethane resin Urethane resin is a resin obtained by reacting urethane raw materials containing polyhydroxy compounds and isocyanate compounds. For example, it can be obtained by crosslinking prepolymers or by reacting polyol with polyisocyanate using the one-shot method.
[0072] Examples of polyhydroxy compounds include polyols used in the production of general flexible polyurethane foams and urethane elastomers, such as polyether polyols, polyester polyols, polyether polyester polyols, polyolefin polyols such as polybutadiene polyols and polyisoprene polyols, and so-called polymer polyols obtained by polymerizing ethylenically unsaturated monomers in polyols, each of which has a polyhydroxyl group at its end.
[0073] Also, examples of isocyanate compounds include polyisocyanates that are similarly used in the manufacture of general soft polyurethane foams and urethane elastomers. For example, toluene diisocyanate (TDI), crude TDI, 4,4'-diphenylmethane diisocyanate (MDI), crude MDI, aliphatic polyisocyanates having 2 to 18 carbon atoms, and alicyclic polyisocyanates having 4 to 15 carbon atoms can be mentioned. In addition, mixtures and modified products of these polyisocyanates (for example, prepolymers obtained by partially reacting with polyols) can be mentioned.
[0074] In order to reduce the universal hardness of the coating layer, the mixing ratio of the polyisocyanate may be reduced.
[0075] The urethane resin may be a one-component or two-component urethane raw material containing a polyhydroxy compound and a polyisocyanate, and may use an epoxy resin or a melamine resin as a crosslinking agent as necessary.
[0076] (2.1.2) Polyamide The polyamide is not particularly limited, but is preferably soluble in alcohol when preparing a coating solution. Examples of such polyamides include polyamide 6, 6·6, 6·10, 6·12, 11, 12, 12·12, and polyamides obtained by polycondensation of different monomers of these polyamides. Other examples include polyamide terpolymers and quaternary copolymers with adjusted molecular weights, and polyamide 6 and polyamide 12 methoxymethylated to make them soluble in alcohol or water.
[0077] (2.1.3) Acrylic resin Examples of the acrylic resin include polyacrylate, polymethyl methacrylate, polymethyl ethacrylate, those in which the side chain terminals of these are substituted with hydroxyalkyl groups or the like, and copolymers of these.
[0078] Examples of monomers constituting the acrylic resin include methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, cyclohexyl acrylate, phenyl acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, hexyl methacrylate, 2-ethylhexyl methacrylate, β-ethyl hydroxyacrylate, γ-propyl aminoacrylate, stearyl methacrylate, dimethylaminoethyl methacrylate, and diethylaminoethyl methacrylate.
[0079] (2.1.4) Silicone copolymer polyurethane Silicone copolymer polyurethane can be synthesized from a compound having a silicone skeleton with a di- or higher functional polyisocyanate and a di- or higher functional hydroxyl group in the molecule.
[0080] The silicone copolymer polyurethane is not particularly limited, and for example, those disclosed in JP-B-7-33427 can be used.
[0081] (2.1.5) Siloxane-modified polyurethane The siloxane-modified polyurethane is not particularly limited, and examples thereof include alkoxy group-containing siloxane-modified polyurethanes. The alkoxy group-containing siloxane-modified polyurethane is obtained by reacting polyurethane (1), which is obtained from a polyol, an isocyanate, and a chain extender and has a functional group reactive with an epoxy group, with an epoxy group-containing alkoxysilane partial condensate (2). The epoxy group-containing alkoxysilane partial condensate (2) is obtained by a dealcoholization reaction between an epoxy compound (A) (hereinafter simply referred to as epoxy compound (A)) having one hydroxy group per molecule and an alkoxysilane partial condensate (B).
[0082] The functional group in polyurethane (1) that is reactive with an epoxy group may be present either at the terminal or in the main chain of polyurethane (1). Examples of such functional groups include acidic groups such as carboxylic acid groups, sulfonic acid groups, and phosphoric acid groups, amino groups, hydroxyl groups, and mercapto groups. From the viewpoint of reactivity with epoxy groups and ease of imparting functional groups, acidic groups or amino groups are preferred. The method of imparting an acidic group to polyurethane (1) is not particularly limited. For example, the functional group can be imparted by using a compound having the above-mentioned functional group as the above-mentioned chain extender or polymerization terminator.
[0083] Methods for synthesizing polyurethane (1) include a one-stage method and a two-stage method. In the one-stage method, a high molecular weight polyol and a diisocyanate compound, and if necessary, a chain extender or a polymerization terminator, are reacted at once in a suitable solvent. In the two-stage method, a polymer polyol and a diisocyanate compound are reacted under the condition of an excess of isocyanate groups to prepare a prepolymer having an isocyanate group at the end of the polymer polyol. Then, this is reacted with a chain extender and, if necessary, a polymerization terminator in a suitable solvent. From the viewpoint of obtaining a uniform polymer solution, the two-stage method is preferable.
[0084] In these synthesis methods, examples of solvents used include aromatic solvents such as benzene, toluene, and xylene; ester-based solvents such as ethyl acetate and butyl acetate; alcohol-based solvents such as methanol, ethanol, isopropanol, n-butanol, and diacetone alcohol; ketone-based solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; and other solvents such as dimethylformamide, dimethylacetamide, ethylene glycol dimethyl ether, tetrahydrofuran, and cyclohexanone.
[0085] The method for imparting amino groups to the polyurethane (1) is not particularly limited, and may be, for example, a method in which polyamines are reacted with the terminal isocyanate groups of the prepolymer so that the amino groups are in excess.
[0086] The amount of epoxy-reactive functional groups in polyurethane (1) is not particularly limited, but is preferably within the range of 0.1 to 20 KOHmg / g. When it is 0.1 KOHmg / g or more, the flexibility and heat resistance of the resulting polyurethane-silica hybrid are good. Also, when it is 20 KOHmg / g or less, the water resistance of the polyurethane-silica hybrid is good. From the viewpoint of adhesion between the metal part and the coating layer, it is preferable that the polyurethane contains a urea bond.
[0087] As described above, the epoxy group-containing alkoxysilane partial condensate (2) can be obtained by the dealcoholization reaction between the epoxy compound (A) and the alkoxysilane partial condensate (B).
[0088] The number of epoxy groups in the epoxy compound (A) is not particularly limited as long as the epoxy compound has one hydroxyl group in one molecule. In addition, the smaller the molecular weight, the better the compatibility with the alkoxysilane partial condensate (B) and the higher the heat resistance and adhesion imparting effect, so that the epoxy compound (A) preferably has 15 or less carbon atoms.
[0089] Examples of such glycidyl ethers include monoglycidyl ethers obtained by reacting epichlorohydrin with water and a dihydric alcohol or a phenol and having one hydroxyl group at the molecular terminal; polyglycidyl ethers obtained by reacting epichlorohydrin with a trihydric or higher polyhydric alcohol such as glycerin or pentaerythritol and having one hydroxyl group at the molecular terminal; epoxy compounds obtained by reacting epichlorohydrin with an amino monoalcohol and having one hydroxyl group at the molecular terminal; and alicyclic hydrocarbon monoepoxides having one hydroxyl group in the molecule (e.g., epoxidized tetrahydrobenzyl alcohol). Among these, glycidol is preferred from the viewpoints of its excellent effect of imparting heat resistance and its high reactivity with the alkoxysilane partial condensate (B).
[0090] Examples of the alkoxysilane partial condensate (B) include those obtained by hydrolyzing a hydrolyzable alkoxysilane monomer represented by the following general formula (a) in the presence of an acid or alkaline water and then partially condensing it.
[0091] General formula (a):R 1 p Si(OR 2 ) 4-p (In the formula, p represents 0 or 1. 1 R represents a lower alkyl group, an aryl group, or an unsaturated aliphatic residue, which may have a functional group directly bonded to a carbon atom. 2 represents a methyl group or an ethyl group, and R 2 They may be the same or different.)
[0092] Examples of such hydrolyzable alkoxysilane monomers include tetraalkoxysilanes such as tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, and tetraisopropoxysilane; and trialkoxysilanes such as methyltrimethoxysilane, methyltriethoxysilane, methyltripoxysilane, methyltributoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, isopropyltrimethoxysilane, and isopropyltriethoxysilane.
[0093] When two or more alkoxysilane monomers are used in combination, it is preferable to mix 70 mol % or more of tetramethoxysilane. From the viewpoint of adhesion between the metal part and the coating layer, the proportion of the silane skeleton contained in the polyurethane-silica hybrid material is preferably within the range of 1.0 to 30.0 mass %.
[0094] Examples of the alkoxysilane partial condensate (B) include compounds represented by the following general formula (b) or (c).
[0095] [ka]
[0096] (In the formula, R 1 R represents a lower alkyl group, an aryl group, or an unsaturated aliphatic residue, which may have a functional group directly bonded to a carbon atom. 2 represents a methyl group or an ethyl group, and R 2 may be the same or different, and n is an integer.
[0097] [ka]
[0098] (In the formula, R 1 , R 2 is R in general formula (b)1 , R 2 where n is an integer.)
[0099] (2.2) Conductive agent The coating layer can be made conductive by containing a conductive agent. Examples of the conductive agent include an electronic conductive agent and an ionic conductive agent.
[0100] (2.2.1) Electronic Conductive Agent Examples of the electronic conductive agent include various conductive metals or alloys such as carbon black, graphite, aluminum, copper, tin, stainless steel, etc. Also included are various conductive metal oxides such as tin oxide, zinc oxide, indium oxide, titanium oxide, tin oxide antimony oxide solid solution, tin oxide indium oxide solid solution, etc. Other examples include fine powders of insulating substances coated with these conductive materials. Among these, carbon black is preferred from the viewpoints of being relatively easily available and providing good electrostatic properties.
[0101] The type of carbon black is not particularly limited, and examples thereof include various conventionally known carbon blacks such as Ketjen black, channel black, and furnace black.
[0102] The carbon black content varies depending on the type of carbon black used, and is not particularly limited, and is appropriately adjusted according to the electrical conductivity and universal hardness required for the coating layer. In general, the carbon black content is preferably within a range of 5 to 50% by mass, more preferably within a range of 10 to 40% by mass, based on the total mass of the resin.
[0103] (2.2.2) Ionic Conductive Agent As the ionic conductive agent, a conventionally known inorganic ionic salt or organic ionic salt can be used.
[0104] Specific examples of the salt include inorganic ion salts such as alkali metal halides such as Li, LiCl, NaI, NaBr, and KI, perchlorates such as LiClO4, KClO4, and CuCl2Mg(ClO4)2, and thiocyanates such as LiSCN, NaSCN, and CsSCN, etc. In addition, examples of the salt include organic ion salts such as aliphatic sulfonates, higher alcohol sulfate salts, higher alcohol phosphate salts, higher alcohol ethylene oxide adduct sulfate salts, higher alcohol ethylene oxide adduct phosphate salts, quaternary ammonium salts, and betaine. Among these, quaternary ammonium salts such as trimethyloctadecylammonium perchlorate, tetramethylammonium chloride, and benzyltrimethylammonium chloride are preferred. These may be used alone or in combination of two or more.
[0105] The content of the ion conductive agent is not particularly limited and is adjusted appropriately according to various conditions. In general, the content is preferably within a range of 0.001 to 5 mass %, and more preferably within a range of 0.05 to 2 mass %, based on the total mass of the resin.
[0106] By using these conductive agents, the resistance value of the coating layer can be increased to 1×10 4 ~1×10 10 It is possible to keep the resistance within the range of Ω·cm. In addition, there is little variation in resistance value depending on the position of the coating layer, and the voltage dependency of the resistance value is small. Furthermore, it is possible to obtain a coating layer with conductivity that has little fluctuation in resistance value due to environmental changes such as temperature and humidity.
[0107] (2.3) Other additives The coating layer may further contain additives, if necessary. Examples of additives include plasticizers, fillers, extenders, vulcanizing agents, vulcanization aids, crosslinking aids, curing inhibitors, antioxidants, antiaging agents, processing aids, etc. Examples of fillers include silica, quartz powder, calcium carbonate, etc. These additives are contained to the extent that they do not inhibit the function of the coating layer.
[0108] 4. Manufacturing method of developing sleeve The method for producing the developing sleeve is not particularly limited. For example, it is preferable to form a coating layer on the outer circumferential surface of the metal part of the developing sleeve. In addition, it is preferable to attach a flange or a shaft to the developing sleeve to form a developing roller.
[0109] (1) Fabrication of metal parts The metal part is made of an aluminum alloy with a silicon content of more than 0.6% by mass, and may be made by mixing other metal materials into the aluminum alloy so that the silicon content is more than 0.6% by mass.
[0110] From the viewpoint of making the image forming apparatus small, lightweight, and low cost, it is preferable that the metal part be a hollow cylindrical metal part with a small diameter (for example, an outer diameter in the range of 5 to 30 mm) and a thin wall thickness (for example, in the range of 0.5 to 2.0 mm) and that the shaft is attached via a flange. The material and shape of the flange are not particularly limited, and any conventionally known material may be used. The flange does not have to be made of the same material as the metal portion.
[0111] The method for producing the metal part is not particularly limited, and any conventionally known method can be used. Examples of methods for forming the metal part into a columnar or cylindrical shape include cutting, extrusion, and drawing.
[0112] (2) Formation of the coating layer The method for forming the coating layer is not particularly limited, but may be, for example, a method in which a coating liquid is applied to the outer circumferential surface of the metal part, dried, and, if desired, heated and cured to form the coating layer, as described above.
[0113] Other methods include, for example, fixing pieces to hold the shaft in the cylindrical mold at both ends, and injecting the material for the coating layer through an injection port formed in the pieces. The material is then heated at a temperature at which the resin hardens, demolded, and the coating layer is formed. Another method includes extruding the material for the coating layer into a cylindrical shape, hardening it, forming a tube, and inserting a metal part into it to form the coating layer. Still another method includes extruding a metal part together with the material for the coating layer, hardening it, and forming the coating layer around the shaft.
[0114] Hereinafter, a method for forming a coating layer by applying a coating liquid to the outer peripheral surface of a metal part, drying it, and, if desired, heating and curing it, will be described.
[0115] A preferred method for forming a coating layer directly on the outer peripheral surface of a metal part is to apply a coating liquid in which the materials for the coating layer (resin, conductive agent, and if necessary, non-conductive filler, etc.) are dissolved or dispersed in a solvent onto the shaft, and then dry the coating liquid. The content of the resin in the coating liquid is not particularly limited, and is preferably adjusted appropriately depending on the required layer thickness. However, from the viewpoint of dispersibility and stability of solid matter in the coating liquid, the content of the resin is preferably 10% by mass or more with respect to the total mass of the coating liquid.
[0116] The solvent is not particularly limited as long as it can dissolve the resin, and examples of the solvent include lower alcohols such as methanol, ethanol, and isopropanol, ketones such as methyl ethyl ketone, cyclohexane, toluene, and xylene.
[0117] From the viewpoint of the viscosity of the resin, examples of the method for forming the coating layer include dipping, spraying, roll coating, brush coating, etc. Among them, from the viewpoint of facilitating the formation of a uniform coating layer, the dipping or spraying method is preferred.
[0118] The thickness of the coating layer is preferably within a range of 1 to 30 μm, and more preferably within a range of 5 to 20 μm. The thickness of the coating layer can be measured by taking a cross-sectional sample including the coating layer from the developing sleeve and taking a micrograph of the cross-sectional sample.
[0119] 5. Structure of the developing roller The developing roller of the present invention has the above-mentioned developing sleeve. As mentioned above, the "developing roller" refers to a developing sleeve with a flange or a shaft attached, as necessary. The developing sleeve is preferably attached to the developing unit as a developing roller.
[0120] 6. Structure of Electrophotographic Image Forming Apparatus The electrophotographic image forming apparatus of the present invention has at least a means for transporting a developer, and the means for transporting a developer includes the developing sleeve having the above-mentioned metal portion. Hereinafter, a developing device as a means for transporting a developer and an image forming apparatus having the developing device will be described.
[0121] (1) Developing device 4 is a schematic cross-sectional view showing an example of a developing device, although the developing device is not limited to this. Further, the developing device shown in FIG. 4 is a developing device that is applied to a non-magnetic one-component developer, but the developer is not limited to the non-magnetic one-component developer.
[0122] 4 has a buffer chamber 26 adjacent to the developing roller 25, and a hopper 27 adjacent to the buffer chamber 26. The developing roller 25 has a developing sleeve.
[0123] In the buffer chamber 26, a blade 28, which is a toner regulating member, is disposed in a state of being pressed against the developing roller 25. The blade 28 regulates the charge amount and adhesion amount of the toner on the developing roller 25. In addition, an auxiliary blade 29 for assisting in regulating the charge amount and adhesion amount of the toner on the developing roller 25 can also be provided downstream of the blade 28 with respect to the rotation direction of the developing roller 25.
[0124] A transport roller 30 is pressed against the developing roller 25. The transport roller 30 is driven to rotate in the same direction as the developing roller 25 (counterclockwise in the figure) by a motor (not shown). The transport roller 30 has a conductive cylindrical base and a foam layer formed of urethane foam or the like on the outer periphery of the base.
[0125] The hopper 27 contains toner T, which is a non-magnetic one-component developer. The hopper 27 is also provided with a rotor 34 that stirs the toner T. A film-shaped transport blade is attached to the rotor 34, and the toner T is transported by the rotation of the rotor 34 in the direction of the arrow. The toner T transported by the transport blade is transported to the buffer chamber 26 through a passage 32 provided in a partition wall separating the hopper 27 from the buffer chamber 26. The shape of the transport blade is such that it bends while transporting the toner T in the forward direction of the blade as the rotor 34 rotates, and returns to a straight state when it reaches the left end of the passage 32. In this way, the transport blade transports the toner T to the passage 32 by changing its shape from a curved state to a straight state.
[0126] Further, the passage 32 is provided with a valve 321 for closing the passage 32. This valve is a film-like member, and one end is fixed to the upper right side of the passage 32 of the partition. When the toner T is transported from the hopper 27 to the passage 32, the valve is pushed to the right by the pressing force of the toner T, thereby opening the passage 32. As a result, the toner T is transported into the buffer chamber 26.
[0127] In addition, a regulating member 322 is attached to the other end of the valve 321. The regulating member 322 and the transport roller 30 are arranged so that a small gap is formed between them even when the valve 321 closes the passage 32. The regulating member 322 adjusts the amount of toner that accumulates at the bottom of the buffer chamber 26 so that it does not become excessive. The regulating member 322 adjusts the amount of toner T that is collected by the transport roller 30 from the developing roller 25 so that it does not fall in large amounts to the bottom of the buffer chamber 26.
[0128] In the developing device 20, the developing roller 25 rotates in the direction of the arrow during image formation. At the same time, the toner in the buffer chamber 26 is transported onto the developing roller 25 by the rotation of the transport roller 30. The toner T transported onto the developing roller 25 is charged and thinned by the blade 28 and the auxiliary blade 29, and then transported to an area facing the photoconductor (image carrier). The toner is then used to develop the electrostatic image on the photoconductor. The toner not used for development returns to the buffer chamber 26 as the developing roller 25 rotates, and is scraped off the developing roller 25 and collected by the transport roller 30.
[0129] (2) An image forming apparatus having a developing device 5 is a schematic cross-sectional view showing an example of a full-color image forming apparatus, although the image forming apparatus is not limited to this. Further, the image forming apparatus shown in FIG. 5 is an image forming apparatus that uses a non-magnetic one-component developer, but the developer is not limited to the non-magnetic one-component developer.
[0130] In the full-color image forming apparatus shown in FIG. 5, a charging brush 111 for uniformly charging the surface of the photosensitive drum 10 to a predetermined potential is provided around the photosensitive drum 10 which is driven to rotate.
[0131] Also provided is a laser scanning optical system 35 that scans and exposes the photoconductor drum 10, which has been charged by the charging brush 111, with a laser beam. This laser scanning optical system 35 is a well-known system that incorporates a laser diode, a polygon mirror, and an fθ optical element. Print data for each of yellow, magenta, cyan, and black is transferred to the control unit from a host computer. Then, based on the print data for each color, this laser scanning optical system 35 sequentially outputs a laser beam and scans and exposes the photoconductor drum 10. As a result, electrostatic charge images of each color are formed sequentially on the photoconductor drum 10.
[0132] The full-color developing device 36 conveys toner of each color to the photoconductor drum 10 on which the electrostatic image has been formed, thereby performing full-color development. Four developing devices 31Y, 31M, 31C, and 31Bk, each containing a non-magnetic single-component toner of yellow, magenta, cyan, and black, are provided around the shaft 33. By rotating around the shaft 33, each of the developing devices 31Y, 31M, 31C, and 31Bk is guided to a position facing the photoconductor drum 10.
[0133] 5, in each of the developing devices 31Y, 31M, 31C, and 31Bk, a toner regulating member is pressed against the outer circumferential surface of the developing roller 25 that rotates to transport the toner. This toner regulating member regulates the amount of toner transported by the developing roller 25 and charges the transported toner. Note that, from the viewpoint of appropriately regulating the amount of toner transported by the developing roller and charging it, two toner regulating members may be provided.
[0134] In this way, every time an electrostatic image of each color is formed on the photoconductor drum 10 by the laser scanning optical system 35, the full-color developing device 36 is rotated around the support shaft 33. The developing devices 31Y, 31M, 31C, and 31Bk containing toner of the corresponding color are sequentially guided to a position facing the photoconductor drum 10. Then, using the developing rollers 25 of the developing devices 31Y, 31M, 31C, and 31Bk, the charged toner of each color is transported in sequence toward the photoconductor drum 10 on which the electrostatic images of each color have been formed in sequence, thereby performing development.
[0135] Further, at a position downstream of the full-color developing device 36 in the rotation direction of the photosensitive drum 10, an endless intermediate transfer belt 40 that is rotated is provided as an intermediate transfer body 40. The intermediate transfer belt 40 is rotated in synchronization with the photosensitive drum 10. The intermediate transfer belt 40 is pressed by a rotatable primary transfer roller 41 and comes into contact with the photosensitive drum 10. Further, a rotatable secondary transfer roller 43 is provided at a portion of a support roller 42 that supports the intermediate transfer belt 40. The secondary transfer roller 43 presses a recording material S, such as recording paper, against the intermediate transfer belt 40.
[0136] Furthermore, a cleaner 50 for scraping off residual toner on the intermediate transfer belt 40 is provided between the full-color developing device 36 and the intermediate transfer belt 40 so as to be movable toward and away from the intermediate transfer belt 40 .
[0137] The paper feed means 60, which guides the recording material S, such as plain paper, to the intermediate transfer belt 40, is composed of a paper feed tray 61, a paper feed roller 62, and a timing roller 63. The paper feed tray 61 stores the recording material S. The paper feed roller 62 feeds the recording material S stored in the paper feed tray 61 one by one. The timing roller 63 sends the fed recording material S between the intermediate transfer belt 40 and the secondary transfer roller 43 in synchronization with the image formed on the intermediate transfer belt 40. In this way, the recording material S sent between the intermediate transfer belt 40 and the secondary transfer roller 43 is pressed against the intermediate transfer belt 40 by the secondary transfer roller 43. Then, the toner image is pressed and transferred from the intermediate transfer belt 40 to the recording material S.
[0138] Meanwhile, the recording material S onto which the toner image has been pressure-transferred is guided to a fixing device 70 by a conveying means 66 constituted by an air suction belt or the like. In the fixing device 70, the transferred toner image is fixed onto the recording material S, and thereafter, the recording material S is discharged onto the top surface of the apparatus main body 100 through a vertical conveying path 80.
[0139] 7. Configuration of Electrophotographic Image Forming System The electrophotographic image forming system of the present invention is an electrophotographic image forming system including a developing sleeve that transports a developer, the developing sleeve containing an aluminum alloy containing more than 0.6% by mass of silicon, the developer including a toner for developing an electrostatic image having an external additive, and the external additive being charged with a polarity opposite to that of the toner for developing an electrostatic image.
[0140] That is, the electrophotographic image forming system of the present invention is characterized in that it has a means for transporting a developer, which comprises a developing sleeve having the above-mentioned metal portion, and the developer contains a specific toner for developing an electrostatic image. The toner for developing electrostatic images will now be described. The developer may be a one-component developer or a two-component developer.
[0141] (1) Overview of toner for developing electrostatic images The toner for developing electrostatic images according to the present invention contains at least toner particles having an external additive attached to the surface of the toner base particles. The external additive and the Image Society of Japan standard carrier N-01 are shaken at a rotation speed of 200 rpm for 10 minutes and frictionally charged, and the charge polarity sign (±) of the external additive is opposite to the charge polarity sign (±) of the electrostatic image developing toner when the Image Society of Japan standard carrier N-01 is shaken at a rotation speed of 200 rpm for 10 minutes and frictionally charged.
[0142] The “toner for developing electrostatic images” according to the present invention may also be simply referred to as “toner.” The toner according to the present invention includes toner particles having toner base particles and an external additive attached to the surfaces of the toner base particles. In this specification, the term "toner base particles" refers to a base of "toner particles." The "toner base particles" are called "toner particles" when an external additive is added. And, "toner" refers to an aggregate of toner particles.
[0143] As described above, the toner is charged in the developing device and transported to the photoconductor, other developing rollers, etc. The mechanism by which the toner is charged is mainly considered to be frictional charging with a blade that is a toner regulating member (single-component developer) or frictional charging with a carrier (two-component developer). In addition to this, frictional charging within the toner is also considered. In order to obtain a toner having a desired charge amount during development, it is necessary to increase the charge amount itself during charging in addition to maintaining the charge amount of the toner. One method for changing the charge amount during charging is to select an external additive.
[0144] Since the toner contains external additives, it is believed that microscopic friction within the toner occurs in the form of friction between toner base particles, friction between external additives, and friction between the toner base particles and the external additives.
[0145] When two or more kinds of external additives are used, those with relatively small particle diameters are easily fixed to the surface of the toner base particle, and those with relatively large particle diameters are not easily fixed to the surface of the toner base particle. Therefore, it is considered that the toner exists in a state of a mixture of toner base particles with small-diameter external additive particles fixed to the surface and large-diameter external additive particles. In the friction within the toner, it is considered that microscopically, friction occurs between toner base particles with small-diameter external additive particles fixed to the surface, and friction occurs between large-diameter external additive particles. It is also considered that friction occurs between toner base particles with small-diameter external additive particles fixed to the surface and large-diameter external additive particles. In the friction between toner base particles with small-diameter external additive particles fixed to the surface and large-diameter external additive particles, friction occurs between the small-diameter external additive particles and the large-diameter external additive particles, and friction occurs between the toner base particles and the large-diameter external additive particles.
[0146] In triboelectric charging, when two objects are rubbed together, negatively charged electrons move to one of the objects, resulting in charging. Therefore, triboelectric charging is difficult to occur between objects made of the same material, but is most likely to occur when objects made of different materials, that is, when toner base particles and external additives are rubbed together. Therefore, by combining toner base particles and external additives, which allow electrons to move easily, the amount of charge generated can be increased.
[0147] When two or more types of external additives are used, triboelectric charging is most likely to occur due to friction between toner base particles having small external additive particles fixed to their surfaces and large external additive particles. Therefore, by combining toner base particles having small external additive particles fixed to their surfaces, through which electrons can easily move, with large external additive particles, the amount of charge generated can be increased.
[0148] In the present invention, the ease with which electrons move when biased to one side is determined using the Image Society of Japan standard carrier N-01 (hereinafter, also simply referred to as the "standard carrier"), which serves as a reference.
[0149] In measuring the charge amount, it is relatively difficult to remove the external additive from a toner to which the external additive has already been added to obtain an aggregate of only the toner base particles, and therefore in the present invention, the polarity sign of the charge of the external additive when the external additive and the standard carrier are triboelectrically charged is compared with the polarity sign of the charge of the toner when the toner and the standard carrier are triboelectrically charged.
[0150] When two or more types of external additives are used, the polarity of the charge of each external additive when it is triboelectrically charged with a standard carrier is compared with the polarity of the charge of the toner when it is triboelectrically charged with a standard carrier. When there is at least one external additive whose polarity of charge is opposite to that of the toner, the present invention applies. When there is no external additive whose polarity of charge is opposite to that of the toner, the present invention does not apply. When two or more types of external additives are used, the external additive whose polarity of charge is opposite to that of the toner according to the present invention is preferably contained in an amount of 10% by mass or more, more preferably 50% by mass or more, of the total amount of external additives. In addition, when the external additive having a charge polarity opposite to that of the toner has a large diameter, the effect of the present invention is more easily obtained.
[0151] For example, if the polarity of the charge of the toner when the toner and the standard carrier are triboelectrically charged is negative (-), it can be seen that the electrons in the standard carrier tend to move into the toner base particles. Also, if the polarity of the charge of the external additive when the external additive and the standard carrier are triboelectrically charged is positive (+), it can be seen that the electrons in the external additive tend to move into the standard carrier. In other words, in this case, it can be inferred that the electrons in the external additive tend to move into the toner base particles when the external additive and the toner are triboelectrically charged.
[0152] On the other hand, if the polarity sign of the charge of the toner when the toner and standard carrier are frictionally charged is the same as the polarity sign of the charge of the external additive when the external additive and standard carrier are frictionally charged, it is not possible to predict the movement of electrons when the external additive and toner are frictionally charged, and even if electrons move and frictional charging occurs, it can be predicted that the amount of charge will be smaller than when the polarity sign is opposite.
[0153] The amount of charge when triboelectrically charged can be measured by the following method. 1.2g of external additive and 18.8g of Image Society of Japan standard carrier "N-01" are shaken at 200 rpm for 10 minutes, triboelectrically charged, and the charge is measured, for example, by a blow-off charge meter. Similarly, 1.2g of toner and 18.8g of Image Society of Japan standard carrier "N-01" are shaken at 200 rpm for 10 minutes, triboelectrically charged, and the charge is measured, for example, by a blow-off charge meter.
[0154] The toner may be either a so-called pulverized toner produced through a pulverization and classification process, or a so-called polymerized toner produced directly from a polymerization process for producing resin particles. Among them, polymerized toner is convenient for producing small-particle toner with a uniform shape, since it can be produced while controlling the toner particle size and shape.
[0155] By using a toner having a uniform shape and small particle diameter, it is easy to form high-resolution and high-definition images as required in digital image formation. For example, it is preferably used for forming pictorial full-color images with high gradation. It is expected that by combining with an image forming apparatus equipped with the developing sleeve of the present invention, high-definition full-color images can be stably formed.
[0156] (2) Composition of toner for developing electrostatic images The toner according to the present invention is composed of toner base particles and an external additive. The toner may be either a magnetic toner or a non-magnetic toner, but from the viewpoint of forming a full-color image, it is preferable that the color toner other than black be a non-magnetic toner. The toner base particles and external additives constituting the polymerized toner, which is an applicable example, will be described below.
[0157] (2.1) Toner base particles The composition of the toner base particles is not particularly limited, but preferably contains a binder resin and a colorant, and may further contain various additives such as a release agent (wax) and a charge control agent, if necessary.
[0158] (2.1.1) Binder resin In the present invention, the term "binding resin" (also referred to as "binder resin") refers to a medium or matrix (parent body) for dispersing internal additives (colorants, release agents, charge control agents, etc.) and external additives (silica, titanium oxide, etc.) contained in toner particles. By including a binder resin in the toner base particles, the toner image can be adhered to a recording medium (for example, paper) during fixing processing of the toner image.
[0159] The binder resin is obtained by adding a chain transfer agent, a polymerization initiator, and a surfactant to a monomer, if necessary, and polymerizing the monomer.
[0160] (2.1.1.1) Monomer The polymerizable monomer is essentially a radical polymerizable monomer, and a crosslinking agent may be used as necessary. It is preferable to contain at least one of the following radical polymerizable monomers having an acidic group or a radical polymerizable monomer having a basic group.
[0161] (Radical polymerizable monomer) The radical polymerizable monomer is not particularly limited, and any conventionally known radical polymerizable monomer can be used. The radical polymerizable monomers may be used alone or in combination of two or more kinds.
[0162] Examples of the radically polymerizable monomer include aromatic vinyl monomers, (meth)acrylic acid ester monomers, vinyl ester monomers, vinyl ether monomers, monoolefin monomers, diolefin monomers, and halogenated olefin monomers.
[0163] Examples of aromatic vinyl monomers include styrene monomers and derivatives thereof, such as styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, p-methoxystyrene, p-phenylstyrene, p-chlorostyrene, p-ethylstyrene, pn-butylstyrene, p-tert-butylstyrene, pn-hexylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decylstyrene, pn-dodecylstyrene, 2,4-dimethylstyrene, and 3,4-dichlorostyrene.
[0164] Examples of (meth)acrylic acid ester monomers include methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, cyclohexyl acrylate, phenyl acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, hexyl methacrylate, 2-ethylhexyl methacrylate, β-hydroxyacrylate, γ-aminopropyl acrylate, stearyl methacrylate, dimethylaminoethyl methacrylate, and diethylaminoethyl methacrylate.
[0165] Examples of the vinyl ester monomer include vinyl acetate, vinyl propionate, and vinyl benzoate.
[0166] Examples of the vinyl ether monomer include vinyl methyl ether, vinyl ethyl ether, vinyl isobutyl ether, and vinyl phenyl ether.
[0167] Examples of monoolefin monomers include ethylene, propylene, isobutylene, 1-butene, 1-pentene, and 4-methyl-1-pentene.
[0168] Examples of the diolefin monomer include butadiene, isoprene, and chloroprene.
[0169] Examples of halogenated olefin monomers include vinyl chloride, vinylidene chloride, and vinyl bromide.
[0170] (Crosslinking agent) From the viewpoint of improving the properties of the binder resin, a radically polymerizable crosslinking agent may be added. Examples of the radically polymerizable crosslinking agent include those having two or more unsaturated bonds, such as divinylbenzene, divinylnaphthalene, divinyl ether, diethylene glycol methacrylate, ethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, and diallyl phthalate.
[0171] (Radical polymerizable monomer having an acidic or basic group) Examples of radical polymerizable monomers having an acidic group include carboxylic acid group-containing monomers, sulfonic acid group-containing monomers, etc. Examples of radical polymerizable monomers having a basic group include amine-based compounds such as primary amines, secondary amines, tertiary amines, and quaternary ammonium salts.
[0172] Examples of the carboxylic acid group-containing monomer include acrylic acid, methacrylic acid, fumaric acid, maleic acid, itaconic acid, cinnamic acid, maleic acid monobutyl ester, and maleic acid monooctyl ester.
[0173] Examples of the sulfonic acid group-containing monomer include styrene sulfonic acid, allyl sulfosuccinic acid, and octyl allyl sulfosuccinate.
[0174] These may be in the form of an alkali metal salt, such as sodium or potassium, or an alkaline earth metal salt, such as calcium.
[0175] Examples of amine compounds include dimethylaminoethyl acrylate, dimethylaminoethyl methacrylate, diethylaminoethyl acrylate, diethylaminoethyl methacrylate, and quaternary ammonium salts of the above four compounds.Other examples include 3-dimethylaminophenyl acrylate, 2-hydroxy-3-methacryloxypropyl trimethyl ammonium salt, acrylamide, N-butylacrylamide, N,N-dibutylacrylamide, piperidyl acrylamide, methacrylamide, N-butyl methacrylamide, N-octadecylacrylamide, vinylpyridine, vinylpyrrolidone, vinyl-N-methylpyridinium chloride, vinyl-N-ethylpyridinium chloride, N,N-diallylmethyl ammonium chloride, and N,N-diallylethyl ammonium chloride.
[0176] The radical polymerizable monomer having an acidic group or the radical polymerizable monomer having a basic group is preferably used in an amount of 0.1 to 15% by mass based on the total mass of the polymerizable monomers. The radical polymerizable crosslinking agent is preferably used in an amount of 0.1 to 10% by mass based on the total mass of the polymerizable monomers, although this depends on the properties of the agent.
[0177] (2.1.1.2) Chain transfer agents From the viewpoint of adjusting the molecular weight, a general chain transfer agent may be used.
[0178] The chain transfer agent is not particularly limited, and examples thereof include octyl mercaptan, dodecyl mercaptan, tert-dodecyl mercaptan, n-octyl-3-mercaptopropionic acid ester, carbon tetrabromide, and styrene dimer.
[0179] (2.1.1.3) Polymerization initiator Any water-soluble radical polymerization initiator can be used. Examples of such initiators include persulfates (potassium persulfate, ammonium persulfate, etc.), azo compounds (4,4'-azobis-4-cyanovaleric acid and its salts, 2,2'-azobis(2-amidinopropane) salts, etc.), and peroxide compounds.
[0180] Furthermore, the radical polymerization initiator may be combined with a reducing agent as necessary to form a redox initiator, which is expected to increase the polymerization activity and lower the polymerization temperature, thereby shortening the polymerization time.
[0181] The polymerization temperature may be any temperature as long as it is equal to or higher than the minimum radical generating temperature of the polymerization initiator, but is preferably within the range of, for example, 50 to 90° C. However, by using a polymerization initiator that starts at room temperature, such as a combination of hydrogen peroxide and a reducing agent (such as ascorbic acid), it is also possible to carry out the polymerization at room temperature or a slightly higher temperature.
[0182] (2.1.1.4) Surfactants In order to carry out polymerization using a radically polymerizable monomer, it is necessary to disperse oil droplets in an aqueous medium using a surfactant.
[0183] Examples of ionic surfactants include sulfonates (sodium dodecylbenzenesulfonate, sodium arylalkyl polyether sulfonate, sodium 3,3-disulfonediphenylurea-4,4-diazo-bis-amino-8-naphthol-6-sulfonate, ortho-carboxybenzene-azo-dimethylaniline, sodium 2,2,5,5-tetramethyl-triphenylmethane-4,4-diazo-bis-β-naphthol-6-sulfonate, etc.), sulfates (sodium dodecyl sulfate, sodium tetradecyl sulfate, sodium pentadecyl sulfate, sodium octyl sulfate, etc.), and fatty acid salts (sodium oleate, sodium laurate, sodium caprate, sodium caprylate, sodium caproate, potassium stearate, calcium oleate, etc.).
[0184] Nonionic surfactants can also be used. Examples include polyethylene oxide, polypropylene oxide, a combination of polypropylene oxide and polyethylene oxide, esters of polyethylene glycol and higher fatty acids, alkylphenol polyethylene oxide, esters of higher fatty acids and polyethylene glycol, esters of higher fatty acids and polypropylene oxide, sorbitan esters, etc. These are mainly used as emulsifiers during emulsion polymerization, but may also be used for other steps or purposes.
[0185] (2.1.2) Colorants The toner base particles can contain a colorant to produce a colored toner. Colorants include inorganic pigments, organic pigments, and dyes.
[0186] As the inorganic pigment, a conventionally known inorganic pigment can be used. Specific examples of the inorganic pigment are shown below.
[0187] Examples of black pigments include carbon black such as furnace black, channel black, acetylene black, thermal black, lamp black, etc. Also included are magnetic powders such as magnetite and ferrite. These may be used alone or in combination of two or more.
[0188] The content of the black pigment is preferably within a range of 2 to 20% by mass, and more preferably within a range of 3 to 15% by mass, based on the total mass of the binder resin.
[0189] As the organic pigment and dye, conventionally known organic pigments and dyes can be used. Specific examples of the organic pigment and dye are shown below.
[0190] Examples of pigments for magenta or red include CI Pigment Red 2, CI Pigment Red 3, CI Pigment Red 5, CI Pigment Red 6, CI Pigment Red 7, CI Pigment Red 15, CI Pigment Red 16, CI Pigment Red 48:1, CI Pigment Red 53:1, CI Pigment Red 57:1, CI Pigment Red 122, CI Pigment Red 123, CI Pigment Red 139, CI Pigment Red 144, CI Pigment Red 149, CI Pigment Red 166, CI Pigment Red 177, CI Pigment Red 178, and CI Pigment Red 222.
[0191] Examples of pigments for orange or yellow include CI Pigment Orange 31, CI Pigment Orange 43, CI Pigment Yellow 12, CI Pigment Yellow 13, CI Pigment Yellow 14, CI Pigment Yellow 15, CI Pigment Yellow 17, CI Pigment Yellow 93, CI Pigment Yellow 94, CI Pigment Yellow 138, CI Pigment Yellow 180, CI Pigment Yellow 185, CI Pigment Yellow 155, and CI Pigment Yellow 156.
[0192] Examples of pigments for green or cyan include CI Pigment Blue 15, CI Pigment Blue 15:2, CI Pigment Blue 15:3, CI Pigment Blue 16, CI Pigment Blue 60, CI Pigment Green 7, and the like.
[0193] Examples of the dye include CI Solvent Red 1, CI Solvent Red 49, CI Solvent Red 52, CI Solvent Red 58, CI Solvent Red 63, CI Solvent Red 111, CI Solvent Red 122, CI Solvent Yellow 19, CI Solvent Yellow 44, CI Solvent Yellow 77, CI Solvent Yellow 79, CI Solvent Yellow 81, CI Solvent Yellow 82, CI Solvent Yellow 93, CI Solvent Yellow 98, CI Solvent Yellow 103, CI Solvent Yellow 104, CI Solvent Yellow 112, CI Solvent Yellow 162, CI Solvent Blue 25, CI Solvent Blue 36, CI Solvent Blue 60, CI Solvent Blue 70, CI Solvent Blue 93, and CI Solvent Blue 95. Mixtures of these can also be used.
[0194] These may be used alone or in combination of two or more. The content of the organic pigment or dye is preferably within a range of 2 to 20% by mass, and more preferably within a range of 3 to 15% by mass, based on the total mass of the binder resin.
[0195] (2.1.3) Release agents In the case of a polymerized toner, a release agent (wax) may be contained in the toner base particles. By including a release agent in the toner base particles, the releasability from the fixing belt can be improved during the fixing process of the toner image.
[0196] The structure and composition of the release agent itself are not particularly limited, and examples thereof include low molecular weight polyolefin waxes such as polypropylene and polyethylene, paraffin wax, Fischer-Tropsch wax, and ester wax.
[0197] The content of the release agent is preferably within a range of 1 to 30% by mass, more preferably within a range of 2 to 20% by mass, and further preferably within a range of 3 to 15% by mass, based on the total mass of the binder resin.
[0198] As a toner applicable to the present invention, first, a releasing agent is dissolved in a monomer, which is dispersed in water and polymerized to form particles in which the releasing agent is encapsulated in resin particles, and then, it is preferable to salt out / fuse the particles together with a colorant to form toner base particles.
[0199] (2.1.4) Charge control agents In the case of a polymerized toner, a charge control agent may be contained in the toner base particles. By including a charge control agent in the toner base particles, the charging performance of the toner can be adjusted. The charge control agent can be added in various ways, such as by adding the charge control agent simultaneously with the resin particles and colorant particles at the salting out / fusion stage, so as to be incorporated into the toner base particles, or by adding the charge control agent to the resin particles themselves.
[0200] The charge control agent is not particularly limited, and may be any conventionally known agent that can be dispersed in water, such as nigrosine dyes, metal salts of naphthenic acid or higher fatty acids, alkoxylated amines, quaternary ammonium salt compounds, azo metal complexes, salicylic acid metal salts or metal complexes thereof, etc.
[0201] (2.2) External additives The toner according to the present invention contains at least toner particles having an external additive attached to the surface of the toner base particles, which can improve the flowability, chargeability, cleaning properties, etc. of the toner.
[0202] As described above, the external additive is not particularly limited as long as the polarity of the charge when triboelectrically charged is opposite to that of the toner. From the viewpoint of toner chargeability, it is preferable to use two or more types of external additives, and it is more preferable that the external additives have different particle sizes.
[0203] Preferred external additives will now be described. When two or more types of external additives are used, it is preferable to apply the following external additives to at least one type of external additive. When two or more types of external additives are used, the following external additives are used to at least one type of external additive, so long as the other external additives are used, there are no particular limitations. However, it is preferable to appropriately select the material, shape, particle size, surface treatment agent, etc. of the particles so that the polarity of the charge when triboelectrically charged is reversed in relation to the toner.
[0204] Examples of the material include inorganic particles, organic particles, and lubricants. Among these, inorganic particles are preferred from the viewpoint of easily satisfying the relationship of polarity of charge when triboelectrically charged.
[0205] As the inorganic particles, conventionally known ones can be used. Among them, silica, titanium, alumina particles, etc., having a number average primary particle size in the range of 5 to 500 nm are preferable, and these are preferably hydrophobic. Furthermore, from the viewpoint of chargeability, titanic acid compounds having a size in the range of 50 to 500 nm are preferable.
[0206] Titanic acid compounds have an irregular shape, i.e., an irregular shape, and therefore have an extremely small contact area with the toner base particles, resulting in a small adhesive force. As a result, it is believed that frictional charging occurs efficiently, resulting in good chargeability.
[0207] Examples of titanate compounds include strontium titanate, calcium titanate, barium titanate, zinc titanate, magnesium titanate, etc. Among these, strontium titanate or calcium titanate is preferred from the viewpoint of positive charging properties.
[0208] Commercially available silica particles include, for example, "AEROSIL (registered trademark) R-805, R-976, R-974, R-972, R-812, R-809" (manufactured by Nippon Aerosil Co., Ltd.), "HVK-2150, H-200" (manufactured by Hoechst Ltd.), and "CAB-O-SIL (registered trademark) TS-720, TS-530, TS-610, H-5, MS-5" (manufactured by Cabot Corporation).
[0209] Commercially available titanium particles include, for example, "AEROSIL (registered trademark) T-805, T-604" (manufactured by Nippon Aerosil Co., Ltd.), "MT-100S, MT-100B, MT-500BS, MT-600, MT-600SS, JA-1" (manufactured by Teika Corporation), "TA-300SI, TA-500, TAF-130, TAF-510, TAF-510T" (manufactured by Fuji Titanium Co., Ltd.), and "IT-S, IT-OA, IT-OB, IT-OC" (manufactured by Idemitsu Kosan Co., Ltd.).
[0210] Commercially available alumina particles include, for example, "RFY-C, C-604" (manufactured by Nippon Aerosil Co., Ltd.) and "TTO-55" (manufactured by Ishihara Sangyo Kaisha, Ltd.).
[0211] As the organic particles, spherical organic particles having a number average primary particle diameter within the range of 10 to 2000 nm can be used. For example, homopolymers such as styrene and methyl methacrylate, and copolymers thereof can be mentioned.
[0212] Examples of lubricants include metal salts of higher fatty acids such as zinc, aluminum, copper, magnesium, calcium, etc., stearic acid salts; zinc, manganese, iron, copper, magnesium, etc., oleic acid salts; zinc, copper, magnesium, calcium, etc., palmitic acid salts; zinc, calcium, etc., linoleic acid salts; zinc, calcium, etc., ricinoleic acid salts; and the like.
[0213] The external additive may be surface-treated so as to satisfy the relationship of the polarity sign of the charge when triboelectrically charged. The surface treatment agent is not particularly limited, and examples thereof include known alkoxysilane compounds, silazane compounds, silicone oils, silane coupling agents, and the like.
[0214] Examples of treatment agents used to impart positive charging properties include silane coupling agents such as γ-(2-aminoethyl)aminopropyltrimethoxysilane, γ-(2-aminoethyl)aminopropylmethyldimethoxysilane, aminosilane, γ-aminopropyltriethoxysilane, N-(2-aminoethyl)3-aminopropyltrimethoxysilane, and N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane, and silicone oils such as amino-modified silicone oils. For titanic acid compounds with strong positive charging properties, silicone oils such as methylhydrogenpolysiloxane and methylphenylpolysiloxane are used for the purpose of hydrophobization.
[0215] On the other hand, examples of the treatment agent used to impart negative chargeability include silane coupling agents such as hexamethyldisilazane, trimethylsilane, trimethylchlorosilane, dimethyldichlorosilane, methyltrichlorosilane, allyldimethylchlorosilane, benzyldimethylchlorosilane, methyltrimethoxysilane, methyltriethoxysilane, isobutyltrimethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, trimethylmethoxysilane, hydroxypropyltrimethoxysilane, phenyltrimethoxysilane, n-butyltrimethoxysilane, n-hexadecyltrimethoxysilane, n-octadecyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, and vinyltriacetoxysilane. Examples of silicone oils include dimethylpolysiloxane, methylhydrogenpolysiloxane, and methylphenylpolysiloxane. In addition, when it is desired to further strengthen the negative chargeability, fluorine-based silane coupling agents and silicone oils can be used.
[0216] The content of the external additive is preferably within a range of 0.1 to 5% by mass with respect to the total mass of the toner. When two or more kinds of external additives are used, the total content of the external additives is preferably within a range of 0.1 to 5% by mass relative to the total mass of the toner. Among them, the content of the suitable external additive is preferably within a range of 0.05 to 3% by mass relative to the total mass of the toner.
[0217] (3) Method for producing toner for developing electrostatic images The method for producing the toner according to the present invention is not particularly limited, but is preferably a polymerization method including the following steps. 1) A process of dispersing a monomer solution in which a release agent is dissolved in an aqueous medium, and then forming resin particles containing the release agent by a polymerization method to prepare a resin particle dispersion liquid. 2) A process of fusing resin particles in an aqueous medium using a resin particle dispersion liquid. 3) A washing process in which the obtained particles are filtered from the aqueous medium and surfactants and other substances are removed. 4) A step of drying the obtained particles 5) A process of adding external additives to the particles obtained by drying.
[0218] Step 1) First, a release agent is dissolved in a monomer to prepare a monomer solution. Next, this monomer solution is dispersed into oil droplets by mechanical energy in an aqueous medium in which a surfactant is dissolved at a critical micelle concentration or less to prepare a dispersion. Then, a water-soluble polymerization initiator is added to this dispersion to cause radical polymerization, thereby forming resin particles containing the release agent. An oil-soluble polymerization initiator may be added to the monomer.
[0219] The dispersing machine for dispersing the oil droplets is not particularly limited, and examples thereof include a Clearmix, an ultrasonic dispersing machine, a mechanical homogenizer, a Manton-Gaulin, and a pressure homogenizer.
[0220] Here, the term "aqueous medium" refers to a medium whose main component is water, and the water content is 50% by mass or more based on the total mass of the aqueous medium. Examples of components other than water include organic solvents that dissolve in water. Examples include methanol, ethanol, isopropanol, butanol, acetone, methyl ethyl ketone, and tetrahydrofuran.
[0221] The resin particles may be colored or non-colored. When the resin particles are non-colored, they can be made into colored particles by adding a colorant particle dispersion or the like to a dispersion of the resin particles, and then fusing them in an aqueous medium.
[0222] Step 2) The fusion method is preferably a method of salting out / fusion using resin particles produced by a polymerization process. In addition, when the resin particles are non-colored, it is preferable to salt out / fusion the resin particles and a colorant in an aqueous medium. In addition to the colorant, a charge control agent and the like can also be added as particles in this step.
[0223] The colorant may be surface-treated (modified) before use. For example, the colorant may be dispersed in a solvent, a surface treatment agent may be added thereto, and the temperature may be raised to carry out a reaction. After the reaction is completed, the mixture is filtered, washed and filtered repeatedly with the same solvent, and dried to obtain a colorant treated with the surface treatment agent.
[0224] When the colorant is a pigment, it is preferable to prepare a colorant particle dispersion by dispersing colorant particles in an aqueous medium, in which the surfactant concentration is set to the critical micelle concentration (CMC) or higher in water.
[0225] The dispersing machine for dispersing the pigment is not particularly limited, and examples thereof include pressure dispersing machines such as Clearmix, ultrasonic dispersing machines, mechanical homogenizers, Manton-Gaulin and pressure homogenizers, and media-type dispersing machines such as sand grinders, Getzmann mills and diamond fine mills.
[0226] The surfactant may be any of the surfactants described above.
[0227] In the salting out / fusion process, a salting out agent made of an alkali metal salt or an alkaline earth metal salt is added as a flocculating agent to the water containing the resin particles and colorant at a concentration equal to or higher than the critical flocculation concentration.Then, the mixture is heated to a temperature equal to or higher than the glass transition point of the resin particles to promote salting out and simultaneously fuse the resin particles.
[0228] In the alkali metal salt and alkaline earth metal salt that are salting-out agents, examples of the alkali metal include lithium, potassium, sodium, etc. Examples of the alkaline earth metal include magnesium, calcium, strontium, barium, etc. Among them, potassium, sodium, magnesium, calcium, or barium is preferable. Examples of salts that constitute the salt include chloride salts, bromide salts, iodide salts, carbonates, sulfates, etc.
[0229] From the viewpoint of obtaining a high-quality toner image, the median diameter (D 50 ) is preferably within the range of 3 to 9 μm. Therefore, it is preferable to adjust the degree of progress of salting out / fusion so that it is within the above range.
[0230] For steps 3) and 4), a conventionally known method can be used.
[0231] 5) Process Examples of the method for adding the external additive include a method using a conventionally known mixer such as a Turbula mixer, a Henschel mixer, a Nauta mixer, or a V-type mixer.
[0232] 8. Electrophotographic Image Forming Method An electrophotographic image forming method using the toner according to the present invention and the full-color image forming apparatus shown in FIG. 5 will be described.
[0233] First, the photosensitive drum 10 and the intermediate transfer belt 40 are rotated in their respective directions at the same peripheral speed, and the photosensitive drum 10 is charged to a predetermined potential by the charging brush 111 .
[0234] The charged photoconductor drum 10 is exposed to a yellow image by the laser scanning optical system 35, and an electrostatic charge image of the yellow image is formed on the photoconductor drum 10. Next, yellow toner charged by a toner regulating member is conveyed from the developing unit 31Y containing yellow toner to the photoconductor drum 10 to develop the yellow image. The intermediate transfer belt 40 is pressed against the photoconductor drum 10 on which the yellow toner image has been formed by the primary transfer roller 41. Then, the yellow toner image formed on the photoconductor drum 10 is primarily transferred to the intermediate transfer belt 40.
[0235] The full-color developing device 36 is rotated around the support shaft 33, and the developing unit 31M containing magenta toner is guided to a position facing the photoconductor drum 10. As in the case of the yellow image, the magenta image is exposed to the photoconductor drum 10 charged by the laser scanning optical system 35 to form an electrostatic image. This electrostatic image is developed by the developing unit 31M containing magenta toner. The developed magenta toner image is primarily transferred from the photoconductor drum 10 to the intermediate transfer belt 40. Similarly, the exposure, development and primary transfer of the cyan and black images are performed in sequence, and the yellow, magenta, cyan and black toner images are layered in sequence on the intermediate transfer belt 40 to form a full-color toner image.
[0236] The recording material S is sent between the secondary transfer roller 43 and the intermediate transfer belt 40 by the timing roller 63. The recording material S is pressed against the intermediate transfer belt 40 by the secondary transfer roller 43, and the full-color toner image formed on the intermediate transfer belt 40 is secondarily transferred onto the recording material S.
[0237] After the full-color toner image is secondarily transferred onto the recording material S, the recording material S is guided to a fixing device 70 by a conveying means 66. The transferred full-color toner image is fixed onto the recording material S by the fixing device 70. Thereafter, the recording material S is discharged onto the top surface of the apparatus main body 100 through a vertical conveying path 80. Reference numeral 112 denotes a cleaning device. EXAMPLES
[0238] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. In the examples, the terms "parts" and "%" are used, but they represent "parts by mass" or "% by mass" unless otherwise specified. In the following examples, operations were carried out at room temperature (25° C.) unless otherwise specified.
[0239] 1. Preparation of the developing sleeve The developing sleeve was prepared according to the following procedure.
[0240] (1) Preparation of developing sleeve (1.1) Preparation of metal parts A hollow cylindrical tube having an outer diameter of 16 mm and a thickness of 1 mm was prepared from an aluminum alloy containing Si (silicon) and Cu (copper) to serve as the metal part 1. A flange and a shaft were attached to the end of the hollow cylindrical tube.
[0241] (1.2) Preparation of the coating layer (1.2.1) Preparation of coating solution for forming coating layer The following components were dissolved to obtain a solution. The alkoxy group-containing siloxane-modified polyurethane was obtained by the method described in JP-A No. 2002-220431, paragraph 0036. The Si content was 6.0% by mass calculated as the silica mass. Alkoxy group-containing siloxane modified polyurethane (urethane resin) 100.0 parts by mass Methyl ethyl ketone 400.0 parts by mass Isopropyl alcohol 300.0 parts by mass
[0242] The following components were mixed and dispersed in the obtained solution to prepare a coating solution for forming a covering layer. Carbon black (volume resistivity: 1×10 -1 Ωcm, number average primary particle diameter: 50nm) 30.0 parts by mass Tetramethylammonium chloride 1.0 parts by mass Cross-linked urethane resin particles (number average median diameter (D 50 ):20μm) 20.0 parts by mass
[0243] (1.2.2) Formation of the coating layer The coating layer forming coating liquid was sprayed onto the outer peripheral surface of the metal part 1, and then dried at 120° C. for 1 hour to form a coating layer having a thickness of 15 μm after drying. A developing roller 1 was produced by attaching a flange and a shaft to the end of the developing sleeve 1.
[0244] (2) Preparation of developing sleeves 2 to 12 Metal parts 2 to 12 were produced in the same manner as in producing metal part 1, except that the type of aluminum alloy was changed. The contents of Si (silicon) and Cu (copper) in the aluminum alloys used for metal parts 1 to 12 are as shown in Table I. In the preparation of the developing sleeve 1, the type of the metal portion was changed to that shown in Table I. Otherwise, the developing rollers 1 to 12 were prepared in the same manner as the developing sleeves 2 to 12, in which flanges and shafts were attached to the ends of the developing sleeves 2 to 12.
[0245] Table I shows the alloy compositions used for the metallic parts of the developing sleeve.
[0246] [Table 1]
[0247] 2. Toner production (non-magnetic single-component developer) The toner was prepared according to the following procedure.
[0248] (1) Preparation of colored particles (toner base particles) (1.1) Preparation of colored particles 1Bk (1.1.1) Preparation of resin particle dispersion 1 A monomer mixture consisting of the following components was prepared. Styrene 115.1 parts by mass n-Butyl acrylate 42.0 parts by mass Methacrylic acid 10.9 parts by mass
[0249] The resulting monomer mixture was placed in a flask equipped with a stirrer, and the following components were added and dissolved by heating to 80°C. Pentaerythritol tetrastearate 72.0 parts by mass Styrene 115.1 parts by mass n-Butyl acrylate 42.0 parts by mass Methacrylic acid 10.9 parts by mass
[0250] Meanwhile, a surfactant solution obtained by dissolving the following components was placed in a separable flask equipped with a stirrer, a temperature sensor, a cooling tube, and a nitrogen introducing device, and the temperature was raised to 80°C while stirring at a stirring speed of 230 rpm under a nitrogen stream. Anionic surfactant (sodium dodecylbenzenesulfonate (SDS)) 7.1 parts by mass Ion-exchanged water 2760.0 parts by mass
[0251] Next, the monomer solution (80°C) was mixed and dispersed into the surfactant solution (80°C) using a mechanical disperser "Clearmix" (manufactured by M Technique Co., Ltd.) with a circulation path to prepare an emulsion in which emulsified particles (oil droplets) with uniform dispersed particle size were dispersed.
[0252] To this dispersion was added an initiator solution obtained by dissolving the following components, and the system was heated and stirred at 80° C. for 3 hours to carry out a polymerization reaction. Polymerization initiator (potassium persulfate (KPS)) 0.8 parts by mass Ion-exchanged water 200.0 parts by mass
[0253] To the resulting reaction solution, a solution obtained by dissolving the following components was added, and after 15 minutes, the temperature was raised to 80°C. Polymerization initiator (potassium persulfate (KPS)) 7.7 parts by mass Ion-exchanged water 240.0 parts by mass
[0254] A mixed liquid consisting of the following components was added dropwise over 100 minutes, and the system was heated and stirred at 80° C. for 60 minutes. Thereafter, the system was cooled to 40° C. to prepare a wax-containing resin particle dispersion 1 (hereinafter referred to as "latex (1)"). Styrene 383.6 parts by mass n-Butyl acrylate 140.0 parts by mass Methacrylic acid 36.4 parts by mass n-Octyl mercaptan 12.0 parts by mass
[0255] (1.1.2) Preparation of colorant dispersion Bk The following components were dissolved to obtain a solution. Sodium n-dodecyl sulfate 9.2 parts by mass Ion-exchanged water 160.0 parts by mass
[0256] While stirring this solution, the following coloring agents were added: Carbon black "Mogul L" (Cabot Corporation) 20.0 parts by mass Next, a dispersion process was carried out using a mechanical disperser "Clearmix" (manufactured by M Technique Co., Ltd.) to prepare colorant dispersion liquid Bk. The particle size of the colorant particles in colorant dispersion liquid Bk was measured using an electrophoretic light scattering spectrometer "ELS-800" (manufactured by Otsuka Electronics Co., Ltd.) and found to be 120 nm in mass average particle size.
[0257] (1.1.3) Preparation of colored particles 1Bk The following components were placed in a reaction vessel (four-neck flask) equipped with a temperature sensor, a cooling tube, a stirring device (having two stirring blades with a crossing angle of 20°), and a shape monitoring device, and the internal temperature was adjusted to 25°C. Then, a 5 mol / L aqueous sodium hydroxide solution was added to this dispersion mixture to adjust the pH to 10.0. Resin particle dispersion liquid 1 (solid content equivalent) 1250.0 parts by mass Ion-exchanged water 2000.0 parts by mass Colorant dispersion Bk total amount
[0258] Next, a solution obtained by dissolving the following components was added over 10 minutes with stirring at 25° C. Then, heating was immediately started, and the system was heated to 95° C. over 5 minutes (heating rate: 14° C. / min). Magnesium chloride hexahydrate 52.6 parts by mass Ion-exchanged water 72.0 parts by mass
[0259] In this state, the particle size of the aggregated particles was measured using a "Multisizer 3" (Beckman Coulter), and the volume-based median diameter (D 50 When the particle size reached 6.5 μm, a solution obtained by dissolving the following components was added to stop particle growth. Sodium chloride 115.0 parts by mass Ion-exchanged water 700.0 parts by mass
[0260] Furthermore, the liquid was heated and stirred (stirring speed: 120 rpm) at a liquid temperature of 90°C for 8 hours to continue fusion and maturation, after which the system was cooled to 30°C at a rate of 10°C / min, hydrochloric acid was added to adjust the pH to 3.0, and stirring was stopped.
[0261] The produced particles were filtered, washed repeatedly with ion-exchanged water, and subjected to submerged classification treatment using a centrifugal separator, and then dried using a flash jet dryer to produce colored particles 1Bk with a moisture content of 1.0% by mass.
[0262] (1.2) Preparation of colored particles 1Y, 1M, and 1C (1.2.1) Preparation of colorant dispersion (1.2.1.1) Preparation of Colorant Dispersion Y Colorant dispersion Y was prepared in the same manner as in preparation of colorant dispersion Bk, except that the following pigment was used instead of 20 parts by mass of carbon black. The particle size of the colorant particles in colorant dispersion Y was measured using an electrophoretic light scattering photometer "ELS-800" (manufactured by Otsuka Electronics Co., Ltd.) and found to be 120 nm in mass average particle size. CI Pigment Yellow 74 20.0 parts by weight
[0263] (1.2.1.2) Preparation of Colorant Dispersion M Colorant dispersion M was prepared in the same manner as in preparation of colorant dispersion Bk, except that the following quinacridone magenta pigment was used instead of 20 parts by mass of carbon black. The particle size of the colorant particles in colorant dispersion M was measured using an electrophoretic light scattering photometer "ELS-800" (manufactured by Otsuka Electronics Co., Ltd.) and found to be 120 nm in mass average particle size. CI Pigment Red 122 20.0 parts by weight
[0264] (1.2.1.3) Preparation of Colorant Dispersion C Colorant dispersion C was prepared in the same manner as in preparation of colorant dispersion Bk, except that the following phthalocyanine cyan pigment was used instead of 20 parts by mass of carbon black. The particle size of the colorant particles in colorant dispersion C was measured using an electrophoretic light scattering photometer "ELS-800" (manufactured by Otsuka Electronics Co., Ltd.) and found to be 120 nm in mass average particle size. CI Pigment Blue 15:3 20.0 parts by weight
[0265] (1.2.2) Preparation of colored particles (1.2.2.1) Preparation of colored particles 1Y Colored particles 1Y were prepared in the same manner as in preparation of colored particles 1Bk, except that the entire amount of colorant dispersion Y was used instead of the entire amount of colorant dispersion Bk.
[0266] (1.2.2.2) Preparation of 1M colored particles Colored particles 1M were prepared in the same manner as in preparation of colored particles 1Bk, except that the entire amount of colorant dispersion M was used instead of the entire amount of colorant dispersion Bk.
[0267] (1.2.2.3) Preparation of colored particles 1C Colored particles 1C were prepared in the same manner as in preparation of colored particles 1Bk, except that the entire amount of colorant dispersion C was used instead of the entire amount of colorant dispersion Bk.
[0268] (2) Toner production (2.1) Preparation of Toner 1 The following components were added to each of the above colored particles and mixed in a Henschel mixer to prepare Toner 1. Specifically, Toner 1 was prepared, which is composed of Toner 1Bk, Toner 1Y, Toner 1M and Toner 1C. The external additive 1 was strontium titanate that had been surface-treated with dimethylpolysiloxane, and had a particle size of 380 nm. Colored particles 100.0 parts by mass Hydrophobic silica (number average primary particle size: 12 nm, hydrophobicity: 65) 0.8 parts by mass External additive 1 (strontium titanate) 1.0 part by mass
[0269] (2.2) Preparation of Toners 2 to 7 Toners 2 to 7 were prepared in the same manner as in the preparation of Toner 1, except that the external additive 1 used in the preparation of Toner 1 was changed to any of the external additives 2 to 7 shown in Table II. The external additives 2 to 7 were treated with the surface treatment agents shown in Table II.
[0270] 3. Evaluation The following measurements and evaluations were carried out.
[0271] (1) Measurement of charge amount of external additives and toner (determination of charge polarity) (1.1) Measurement of the charge amount of external additives 1 to 7 1.2 g of the external additive and 18.8 g of the Imaging Society of Japan standard carrier "N-01" were shaken at 200 rpm for 10 minutes to be charged by friction, and the charge amount was measured using a blow-off charge amount measuring device. The charge amounts of external additives 1 to 7 are shown in Table II. Two types of external additives were used in toners 1 to 7. The other external additive, hydrophobic silica (number average primary particle diameter: 12 nm), had a charge amount sign of (-).
[0272] (1.2) Measurement of Charge Amount of Toners 1 to 7 1.2 g of the toner prepared above and 18.8 g of the Imaging Society standard carrier "N-01" were shaken at a rotation speed of 200 rpm for 10 minutes to be triboelectrically charged, and the charge amount was measured using a blow-off charge amount measuring device. The charge polarity sign of Toners 1 to 7 was all (-).
[0273] (1.3) Identification of the polarity of charge of external additives and toner The polarity signs of the charge of the external additives 1 to 7 measured in the above (1.1) were compared with the polarity sign (-) of the charge of the toner measured in the above (1.2). Toners 1 to 4 were charged with opposite polarities, whereas toners 5 to 7 were charged with the same polarity. The sign of the charge amount of the hydrophobic silica used in combination as an external additive was (-), which was the same as the polarity sign (-) of the charge of the toner measured in (1.2) above.
[0274] (2) Measurement of the charge amount of the toner on the developing sleeve The developing sleeve and toner 1 (toner 1Bk, toner 1Y, toner 1M, toner 1C) prepared above were incorporated into a non-contact non-magnetic single-component development type electrophotographic printer "Magicolor (registered trademark) 3730DN". Then, printing was performed in a high temperature and high humidity environment (30°C, 85% RH). Printing was performed on 10,000 A4 size sheets with a pixel ratio of 20% (full color mode with 5% for each of yellow, magenta, cyan, and black). After printing, the toner on the developing sleeve was sucked at 20 points using a suction nozzle unit attached to a Q / m meter "MODEL 210HS" (manufactured by Trek). Next, the total charge [μC] of the sucked toner and the mass [g] of the sucked toner were measured using the Q / m meter. Then, q / m (charge amount per unit mass [μC / g]) was calculated based on the following formula. Formula: Toner charge [μC / g] = total charge of attracted toner [μC] / mass of attracted toner [g]
[0275] (3) Fog evaluation The developing sleeve and toner prepared above were incorporated into a non-contact non-magnetic one-component developing electrophotographic printer "Magicolor (registered trademark) 3730DN" in the combination shown in Table III below. Then, printing was performed in a high temperature and high humidity environment (30°C, 85% RH). 50,000 sheets of A4 size were printed at a pixel rate of 20% (full color mode with 5% of each of yellow, magenta, cyan, and black). After printing 10,000 sheets, 20 solid white images were printed, and the 20th image was scanned with a scanner. This scanned image was imported into image editing software "Photoshop (registered trademark) CS6" (manufactured by Adobe Systems Inc.) and converted into a monochrome image. Then, the black ratio was calculated at 10 points in the monochrome image using the same software, and the arithmetic average value of this black ratio was taken as the blackening ratio, which was evaluated according to the following criteria.
[0276] In a monochrome image, the areas where toner is applied to the white background are recognized as black. The "blackening rate" here refers to the area ratio of the black dots in the image. For example, the blackening rate for a solid black image is 100%, and for white paper it is 0%. The 10 points in the scanned image were selected by vertically dividing the A4 size paper into two rectangles, and selecting 5 points in each rectangle, for a total of 10 points, as shown in Figure 6. In addition, the intersection of the diagonals of each rectangle was set as the center point, and a total of 5 points were selected: the center point and the midpoints between the center point and the four corners.
[0277] AA: The blackening rate is less than 0.05%, and is practically acceptable. A: The blackening rate is 0.05% or more and less than 0.15%, and there is no problem in practical use. B: The blackening rate is 0.15% or more and less than 0.3%, and is problematic in practical use. C: The blackening rate is 0.3% or more, and is problematic in practical use.
[0278] (4) Toner spill evaluation The developing sleeve and toner prepared above were incorporated in a non-contact non-magnetic one-component developing electrophotographic printer "Magicolor (registered trademark) 3730DN" in the combination shown in Table III below. Then, printing was performed in a high temperature and high humidity environment (30°C, 85% RH). Printing was performed on 20,000 sheets of A4 size with a pixel ratio of 5% using cyan toner with good visibility. After printing 20,000 sheets, the developing machine was removed and visually confirmed whether toner spillage occurred near the transfer unit and whether toner had accumulated under the developing roller, and was evaluated according to the following criteria. Note that "toner spillage" refers to the toner remaining on the developing sleeve without adhering to the photoconductor overflowing from a collection container and spilling into the printer during the developing process.
[0279] AA: No toner accumulates under the developing roller of the developing machine, and no stains caused by toner spilled from the developing machine are observed on the transfer belt, so there are no problems in practical use. A: Toner was accumulated under the developing roller of the developing machine, but no stains caused by toner spilled from the developing machine were observed on the transfer belt, so there was no problem in practical use. B: Toner was accumulated under the developing roller of the developing machine, and stains due to toner spilled from the developing machine were observed on both ends of the transfer belt. Image defects occurred due to toner spillage, which was problematic for practical use. C: Toner accumulated under the developing roller of the developing machine, toner spilled from the developing machine was found to be stained all over the transfer belt, and image defects occurred due to toner spillage, which was problematic in practical use.
[0280] Table II shows the details of the external additives of each toner. In the table, "charge amount" is the charge amount [μC / g] of the external additive measured in the above evaluation, and "polarity sign" is the polarity sign of the charge amount. Table III shows the above evaluation results for each combination of developing sleeve and toner.
[0281] [Table 2]
[0282] [Table 3]
[0283] From the Examples and Comparative Examples, it is understood that the electrophotographic image forming system of the present invention can suppress fogging and toner spillage.
[0284] Comparison of Examples 1, 5, 6, 8 and 10 shows that fog and toner spillage can be further suppressed by setting the silicon content within the range of 0.8 to 12.6 mass % with respect to the total mass of the aluminum alloy.
[0285] Comparison of Examples 11, 12 and 14 shows that by controlling the copper content to 2.0 mass % or less with respect to the total mass of the aluminum alloy, fogging and toner spillage can be further suppressed.
[0286] From a comparison of Examples 1 to 4, it is seen that by using a titanic acid compound as inorganic particles, fogging and toner spillage can be further suppressed. [Explanation of symbols]
[0287] 10 Photoconductor drum 11 Developing sleeve 12 Metal Part 13 Covering layer 14 Lower layer 15 Upper layer 16 Flange 17 Shaft 18 Developing roller 20 Developing device 25 Developing roller 26 Buffer Room 27 Hopper 28 Regulatory Blade 29 Auxiliary Blade 30 Transport roller 32 Passage 321 Valve 322 Regulatory Materials 34 Rotating Body T Toner
Claims
1. 1. An electrophotographic imaging system including a developing sleeve for transporting a developer, the developing sleeve contains an aluminum alloy containing more than 0.6% by weight of silicon, the developer contains a toner for developing an electrostatic image having an external additive, The external additive is charged with a polarity opposite to that of the toner for developing an electrostatic image.
23. An electrophotographic imaging system comprising:
2. The developer is a one-component developer.
2. An electrophotographic imaging system according to claim 1.
3. The silicon content is within a range of 0.8 to 12.6 mass% based on the total mass of the aluminum alloy.
2. An electrophotographic imaging system according to claim 1.
4. The copper content is 2.0 mass% or less based on the total mass of the aluminum alloy.
2. An electrophotographic imaging system according to claim 1.
5. The external additive is an inorganic particle.
2. An electrophotographic imaging system according to claim 1.
6. The inorganic particles are titanate compounds.
6. An electrophotographic imaging system according to claim 5.
7. 1. An electrophotographic imaging system including a developing sleeve for transporting a developer, the developing sleeve contains an aluminum alloy containing more than 0.6% by weight of silicon, the developer contains a toner for developing an electrostatic image having an external additive, The external additive is titanium strontium oxide.
23. An electrophotographic imaging system comprising:
8. An electrophotographic image forming apparatus including at least a developing sleeve for transporting the developer, The electrophotographic imaging system according to any one of claims 1 to 7, 2. An electrophotographic image forming apparatus comprising:
9. The electrophotographic image forming apparatus according to claim 8, The developing sleeve is characterized by the above.
10. The developing sleeve according to claim 9 . A developing roller characterized by:
11. The electrophotographic image forming system according to any one of claims 1 to 7 is used.
1. An image forming method comprising:
Citation Information
Patent Citations
Developing method
JP1993188652A
Developing roller
JP1996179620A
Developer for electrostatic charge image development and image forming method
JP2007034164A